AI Technical Summary
Synthesizing multi-element compound nanoparticles is challenging due to the difficulty in mixing multiple elements at the nanoscale, leading to phase separation and agglomeration, and conventional high-temperature methods are energy-intensive and difficult to control.
A method involving the decomposition of precursors on a substrate using controlled high-temperature heating and rapid cooling to form multi-element compound nanoparticles, such as MEO, ME-carbide, and MEI nanoparticles, with precise temperature and time controls to avoid structural degradation and agglomeration.
Enables the formation of nanoparticles with a single homogeneous phase and high structural stability, allowing for improved catalytic and electrochemical applications by maintaining uniform composition and preventing particle growth.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit of U.S. Provisional Application No. 63 / 125,918, entitled "Multi-element compound nanoparticles and methods for making same," filed December 15, 2020, and is incorporated by reference in its entirety herein.
[0002] FIELD OF THE DISCLOSURE This disclosure relates generally to engineered multi-element particles, and more particularly to multi-element compound nanoparticles, and methods of making and using such nanoparticles. [Background technology]
[0003] Multi-element compound (MEC) nanoparticles can provide synergistic interactions between different elements, which are often superior to their single counterparts. However, synthesizing MEC nanoparticles remains a significant challenge, in part due to the difficulty of mixing multiple different elements at the nanoscale. Traditional wet-chemistry approaches (e.g., hydrothermal and co-precipitation), which are performed at relatively low temperatures (e.g., 300-673 K), may lack the activation energy to overcome the kinetic barriers to mix multiple elements and drive compound formation. As a result, traditional approaches tend to result in end products with phase separation. High-temperature thermal treatments (e.g., >700 K) provide higher activation energies and faster kinetics, thereby facilitating multi-element mixing into a single phase. However, traditional high-temperature strategies (e.g., sintering) are energy intensive and difficult to control for the synthesis of nanomaterials. For example, traditional approaches can require significant times to heat to the desired high temperatures, resulting in relatively long reaction times (e.g., on the order of minutes), which can lead to extensive overgrowth and agglomeration of particles. Summary of the Invention [Problem to be solved by the invention]
[0004] Embodiments of the disclosed subject matter may address, among other things, one or more of the problems and shortcomings set forth above.
[0005] System embodiments of the disclosed subject matter provide multi-element compound (MEC) nanoparticles, as well as systems and methods of making and using same. [Means for solving the problem]
[0006] The high temperature fabrication strategies disclosed herein can be used, alone or in combination, to drive the decomposition of precursors on a substrate and the subsequent mixing of multiple elements (e.g., 3 or more different elements, such as 5-10 different elements) and the formation of compounds of diverse compositions, such as, but not limited to, multi-element oxide (MEO) nanoparticles, multi-element carbide (ME-carbide) nanoparticles, and multi-element intermetallic (MEI) nanoparticles. Heating can be precisely controlled to achieve desired composition, structure, and / or other properties. For example, in some embodiments, exposure to high temperatures can be short enough to avoid structural degradation and / or particle aggregation. In some embodiments, additional heating at the same or different temperatures (e.g., higher) and / or for longer durations (e.g., 1-10 min) can be subsequently administered, for example, to convert MEO nanoparticles to ME-carbide nanoparticles or to convert disordered multimetallic particles to MEI nanoparticles.
[0007] In one or more embodiments, the structure can include one or more MEC nanoparticles. Each MEC nanoparticle can have a plurality of sites that include one or more elements. Each site can form a compound bond with at least one other site of the compound nanoparticle. The one or more compound bonds can include covalent bonds, ionic bonds, and / or metallic bonds. Each MEC nanoparticle can be formed from at least three different elements.
[0008] In one or more embodiments, the method can include providing a substrate having a plurality of metal salt precursors thereon. At least one of the metal salt precursors can include oxygen (O), and the plurality of metal salt precursors can include at least three different metal elements. The method can include cooling the substrate for at least 10 minutes from an initial temperature. 4 The method can further include heating the substrate to a first temperature at a first heating rate of 10 K / s and maintaining the substrate at the first temperature for a first period of time. The method can also include maintaining the substrate at the first temperature for a first period of time. 5 The method can include cooling the substrate from a first temperature to a second temperature at a first cooling rate of 100 K / s. The initial temperature and the second temperature can be less than 500 K. The heating, maintaining, and cooling can be such that the metal salt precursor on the substrate is converted to one or more MEO nanoparticles. Each MEO nanoparticle can include O and at least three metal elements in a single homogenous phase.
[0009] In some embodiments, the method can further include providing a coating on the one or more MEO nanoparticles and at least partially surrounding the one or more MEO nanoparticles. The method can also include heating the substrate from the third temperature to a fourth temperature at a second heating rate slower than the first heating rate. The method can include maintaining the substrate at the fourth temperature for a second period of time and, at the end of the second period of time, maintaining the substrate at the fourth temperature for at least 10 5 and cooling the substrate from the fourth temperature to a fifth temperature at a second cooling rate of 100 K / s. The third and fifth temperatures may be less than 500 K. Heating to the fourth temperature, maintaining at the fourth temperature, and cooling from the fourth temperature may cause the one or more MEO nanoparticles and coating to be converted to one or more ME-carbide nanoparticles. Each multi-element carbide nanoparticle may include carbon (C) and at least three metallic elements in a single homogenous phase.
[0010] In one or more embodiments, another method can include providing a substrate having one or more high entropy alloy (HEA) nanoparticles thereon. Each HEA nanoparticle can include at least three different metal elements. The method can include providing the substrate with at least 10 4 The method may further include heating the substrate to a first temperature at a first heating rate of 10 K / s and maintaining the substrate at the first temperature for a first period of time. The method may also include maintaining the substrate at the first temperature for a first period of time. 5 The method can include cooling the substrate from a first temperature to a second temperature at a first cooling rate of 100 K / s. The second temperature can be less than 500 K, the first temperature can be greater than 1000 K, and the first time period can be in the range of 1 minute to 10 minutes, inclusive. The heating, maintaining, and cooling can cause the one or more HEA nanoparticles to be converted into one or more multi-element intermetallic (MEI) nanoparticles. Each MEI nanoparticle can include at least five metallic elements in a single phase.
[0011] In some embodiments, providing one or more HEA nanoparticles on the substrate comprises providing a plurality of metal salt precursors on the substrate and cooling the substrate at least 10° C. from an initial temperature. 4 heating the substrate at a second heating rate of 10 K / s to a third temperature; maintaining the substrate at the third temperature for a second period of time; and at the end of the second period of time, heating the substrate at least 10 K / s from the third temperature. 5 and cooling to a fourth temperature at a second cooling rate of 100 K / s. The plurality of metal salt precursors can include at least five different metal elements. The initial temperature and the fourth temperature can be less than 500 K, the third temperature can be greater than 1000 K, and the second period of time can range from 10 ms to 100 ms. The heating to the third temperature, maintaining at the third temperature, and cooling from the third temperature can be such that the metal salt precursors on the substrate are converted to one or more HEA nanoparticles.
[0012] Any of the various innovations of the present disclosure can be used in combination or separately. This summary is provided to introduce in a simplified form a selection of concepts that are further described in the detailed description below. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter. The foregoing and other objects, features, and advantages of the disclosed technology will become more apparent from the following detailed description, which proceeds with reference to the accompanying drawings. [Brief description of the drawings]
[0013] Embodiments will now be described with reference to the accompanying drawings, which are not necessarily drawn to scale. Where applicable, some elements may be simplified or otherwise not shown to help illustrate and explain the underlying features. Like reference numbers refer to like elements throughout the drawings. [Figure 1A] FIG. 1A is a simplified schematic diagram illustrating an embodiment of a conventional multi-element nanoparticle having multiple phases. [Figure 1B] FIG. 1B is a simplified schematic diagram illustrating an embodiment of a multi-element oxide (MEO) nanoparticle having a single homogenous phase, according to one or more embodiments of the disclosed subject matter. [Figure 1C] FIG. 1C is a simplified schematic diagram of a carbon nanofiber (CNF) substrate having MEO nanoparticles according to one or more embodiments of the disclosed subject matter. [Fig. 1D-1E] 1D-1E are scanning electron microscope (SEM) images showing overview and close-up views of a CNF substrate on which MEO nanoparticles have been fabricated, in accordance with one or more embodiments of the disclosed subject matter. [Figure 2A] FIG. 2A is a simplified schematic diagram illustrating the behavior of a multi-element high entropy alloy (HEA) that forms a disordered solid solution phase. [Figure 2B]FIG. 2B is a simplified schematic diagram illustrating an embodiment of a multi-element intermetallic (MEI) nanoparticle having an ordered solid solution phase, in accordance with one or more embodiments of the disclosed subject matter. [Figure 2C] FIG. 2C shows an exemplary lattice structure of an octonary MEI nanoparticle in accordance with one or more embodiments of the disclosed subject matter. [Fig. 2D-2F] 2D-2F show high angle annular dark field imaging (HAADF) scanning transmission electron microscope (STEM) images of fabricated octanium (Pt0.8Pd0.1Au0.1)(Fe0.6Co0.1Ni0.1Cu0.1Sn0.1) MEI nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 2G] FIG. 2G is a simplified schematic diagram of a CNF substrate with MEI nanoparticles according to one or more embodiments of the disclosed subject matter. [Figure 3A] FIG. 3A is a process flow diagram of an exemplary method for forming MEO nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 3B] FIG. 3B is a graph illustrating aspects of an exemplary pulse heating profile that may be used to form MEO nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 3C] FIG. 3C is a schematic diagram illustrating an exemplary synthetic strategy for forming single-phase MEO nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 3D] FIG. 3D is a graph of the Gibbs free energy of formation of different oxides as a function of temperature showing the oxidation potential of different elements. [Figure 3E] FIG. 3E shows x-ray diffraction (x-ray diffractograms) patterns of (Zr,Ce,Hf,Ti)OX nanoparticles synthesized at 1000 K (showing phase separation), (Zr,Ce,Hf,Ti)O2 nanoparticles synthesized at 1550 K, and (Ca,Mg)(Ti,Nb,Mn)O3-X nanoparticles synthesized on a CNF substrate at 1150 K, in accordance with one or more embodiments of the disclosed subject matter. [Figure 3F]FIG. 3F shows x-ray diffraction patterns of (Fe,Co,Ni,Cu) nanoparticles made by low PO2 (~1 ppm) synthesis, (Fe,Co,Ni,Cu)Ox nanoparticles made by high PO2 (air) synthesis, and (Mn,Fe,Co,Ni)3O4-x nanoparticles made by high PO2 (air) synthesis, in accordance with one or more embodiments of the disclosed subject matter. [Figure 3G] FIG. 3G shows an x-ray diffraction diagram of (Zr,Ce,Hf)PdOx nanoparticles (showing phase separation) and (Zr,Ce,Hf,Ti,La,Y,Gd,Sm,Dy,Pd)O2-x nanoparticles (showing a single phase) in accordance with one or more embodiments of the disclosed subject matter. [Figure 4A] FIG. 4A is a process flow diagram of an exemplary method for forming multi-element carbide (ME-carbide) nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 4B] FIG. 4B is a schematic diagram illustrating an exemplary synthesis of single-phase ME-carbide nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 4C] FIG. 4C is a graph illustrating aspects of an exemplary heating profile for carbonization that may be used to form ME-carbide nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 4D] FIG. 4D is a graph showing an embodiment of another exemplary heating profile for carbonization that may be used to form ME-carbide nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 5A] FIG. 5A is a process flow diagram of an exemplary method for forming multi-element intermetallic (MEI) nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 5B] FIG. 5B is a graph illustrating aspects of an exemplary heating profile for forming MEI nanoparticles in accordance with one or more embodiments of the disclosed subject matter. [Figure 5C]FIG. 5C shows X-ray diffraction patterns of pentad Pt (Fe0.7Co0.1Ni0.1Cu0.1) MEI nanoparticles obtained from various annealing times at ∼1100 K in accordance with one or more embodiments of the disclosed subject matter. [Figure 5D] FIG. 5D is a graph of long-term ordering (LRO) as a function of pentagonal MEI nanoparticle size, in accordance with one or more embodiments of the disclosed subject matter. [Figure 6] FIG. 6 illustrates a generalized example of a computing environment in which the disclosed technology can be implemented. [Figure 7A] FIG. 7A is a graph of methane conversion in the experimental setup using a control sample of (Zr,Ce)0.6(Mg,La,Y,Hf,Ti,Cr,Mn)0.3 Pd0.1O2-x nanoparticles (10-MEO-PdO) and (Zr,Ce)0.6(Mg,Hf,Ti,Cr,Mn,Fe,Cu)0.3 Pd0.1Ox nanoparticles (10-MEO-FeCu). [Figure 7B] FIG. 7B shows the methane conversion versus reaction temperature in the experimental setup using PdOx, Pd-free 9-MEO ((Zr,Ce)0.66(Mg,La,Y,Hf,Ti,Cr,Mn)0.34O2-x), and 10-MEO-PdO as catalysts. [Figure 7C] FIG. 7C shows the change in methane conversion over time in the experimental setup using PdOx, 4-MEO-Pd((Zr,Ce)0.6Mg0.3Pd0.1Ox), and 10-MEO-PdO as catalysts. [Figure 7D] FIG. 7D shows the XRD patterns of rejected element particles with different Pd contents produced using the disclosed synthesis technique. [Figure 7E] FIG. 7E shows the XRD pattern of rejected element particles with 10 at.% Pd synthesized by annealing at 1273 K for 2 h in an Ar atmosphere. [Figure 8A] FIG. 8A is a graph comparing the hydrogen evolution reaction (HER) performance of various oxide and carbide nanoparticles using linear sweep voltammetry at a scan rate of 5 mV / s. [Figure 8B] FIG. 8B compares the HER performance of MoO2 and (TiZrVNbMo)Cx nanoparticles using chronoamperometry at 10 mA / cm2. [Figure 9A] FIG. 9A is a diagram of the LRO as a function of order heating time for pentad Pt(Fe0.7Co0.1Ni0.1Cu0.1) nanoparticles. [Figure 9B] FIG. 9B shows the X-ray diffraction patterns of pentogenous Pt(Fe0.7Co0.1Ni0.1Cu0.1) nanoparticles at various orders of heating time. [Fig. 9C-9E] 9C-9E are STEM images of pentogenous Pt(Fe0.7Co0.1Ni0.1Cu0.1) nanoparticles at heating times on the order of 0.5 seconds. [Figure 9F] FIG. 9F is a simplified schematic diagram of an ethanol fuel cell test apparatus using octanium (Pt0.8Pd0.1Au0.1)(Fe0.6Co0.1Ni0.1Cu0.1Sn0.1) intermetallic nanoparticles as the anode catalyst. [Figure 9G] FIG. 9G shows the ethanol electrooxidation (EOR) performance of octanium (Pt0.8Pd0.1Au0.1)(Fe0.6Co0.1Ni0.1Cu0.1Sn0.1) intermetallic nanoparticles, binary PtFe nanoparticles, and a commercial Pt / C catalyst in 1 M KOH and 1 M EtOH using cyclic voltammetry (CV). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] General Considerations For the purpose of this description, certain aspects, advantages, and novel features of the embodiments of the present disclosure are described herein. The disclosed methods and systems should not be construed as limiting in any way. Instead, the present disclosure is directed to all novel and non-obvious features and aspects of the various disclosed embodiments, both alone and in various combinations and subcombinations with each other. The methods and systems are not limited to any particular aspects, features, or combinations thereof, and the disclosed embodiments do not require that any one or more particular advantages exist or problems be solved. Techniques from any embodiment or example can be combined with techniques described in any one or more of the other embodiments or examples. In view of the many possible embodiments to which the principles of the disclosed technology may be applied, it should be recognized that the illustrated embodiments are merely illustrative and should not be construed as limiting the scope of the disclosed technology.
[0015] Although some operations of the disclosed methods are described in a particular order for convenient presentation, it should be understood that this method of description encompasses reordering, unless a particular ordering is required by the specific language described below. For example, operations described in sequence may be reordered or performed simultaneously in some cases. Furthermore, for simplicity, the accompanying drawings may not show the various ways in which the disclosed methods may be used in conjunction with other methods. Furthermore, the description may use terms such as "provide" or "achieve" to describe the disclosed methods. These terms are high-level abstractions of the actual operations that are performed. The actual operations that correspond to these terms may vary depending on the specific implementation and are readily discernible by those of ordinary skill in the art.
[0016] Disclosure of numerical ranges should be understood to refer to each discrete point within the range, including the endpoints, unless otherwise indicated. Unless otherwise indicated, all numbers expressing amounts of ingredients, molecular weights, percentages, temperatures, times, and the like used in this specification or claims should be understood to be modified by the term "about". Thus, unless otherwise implicitly or explicitly indicated, or unless the context is properly understood by those skilled in the art to have a clearer configuration, the numerical parameters described are approximations that may depend on the desired properties sought and / or the limits of detection under standard testing conditions / methods, as known to those skilled in the art. Whenever the embodiment numbers are directly and explicitly distinguished from the prior art discussed, the embodiment numbers are not approximations unless the word "about" is recited. Whenever "substantially", "approximately", "about", or similar language is explicitly used in conjunction with a particular value, a variation of up to 10% of that value is intended, unless explicitly stated otherwise.
[0017] Directions and other relative references may be used to facilitate the description of the figures and principles herein, but are not intended to be limiting. For example, terms such as "inner", "outer", "upper", "lower", "top", "bottom", "inner", "outer", "left", "right", "front", "rear", "rear", etc. may be used. Such terms are used, where applicable, to provide some clarity of description when dealing with relative relationships, particularly with respect to the illustrated embodiments. However, such terms are not intended to imply absolute relationships, positions, and / or orientations. For example, with respect to an object, an "upper" portion becomes a "lower" portion simply by flipping the object. Nevertheless, it is still the same portion and the object remains the same.
[0018] As used herein, the term "comprising" and the singular forms "a" or "an" or "the" include plural references unless the context clearly dictates otherwise. The term "or" refers to a single element or a combination of two or more of the listed alternative elements, unless the context clearly dictates otherwise.
[0019] The various components, parameters, operating conditions, and the like described herein may be alternatives, but these alternatives are not necessarily equivalent and / or will function equally well. Nor is it meant to imply that the options are listed in order of preference, unless otherwise indicated. Any of the groups defined below may be substituted or unsubstituted, unless otherwise indicated.
[0020] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this disclosure belongs.Methods and materials similar or equivalent to those described herein can be used in the practice or testing of this disclosure, but suitable methods and materials are described below.The materials, methods, and examples are illustrative only and are not intended to be limiting.The features of the subject matter of this disclosure will become apparent from the following detailed description and the appended claims.
[0021] Terminology Overview The following explanations of specific terms and abbreviations are provided to facilitate the description of various embodiments of the disclosed subject matter and to guide those of ordinary skill in the art in the practice of the disclosed subject matter.
[0022] Nanoparticle: An engineered particle formed from multiple elements (e.g., at least two elements, e.g., at least three elements, at least five elements, or at least eight elements) and having a maximum cross-sectional dimension (e.g., diameter when the particle is spherical, e.g., D1 in FIG. 1B or D2 in FIG. 2B) of 1 μm or less, e.g., about 100 nm or less. In some embodiments, each nanoparticle has a maximum cross-sectional dimension of about 20-25 nm. In other embodiments, each nanoparticle has a maximum cross-sectional dimension of 10 nm or less, e.g., about 3-6 nm.
[0023] Multi-element compound (MEC) nanoparticles: Nanoparticles having a plurality of sites containing one or more elements, each site forming a compound bond with at least one other site. In some embodiments, the compound bond is a covalent bond, an ionic bond, and / or a metallic bond. In some embodiments, the MEC nanoparticles are multi-element oxide (MEO) nanoparticles, multi-element carbide (ME-carbide) nanoparticles, multi-element intermediate (MEI) nanoparticles, multi-element nitride nanoparticles, multi-element amorphous glass nanoparticles, multi-element diboride nanoparticles, multi-element phosphide nanoparticles, multi-element sulfide nanoparticles, multi-element chalcogenide nanoparticles, or multi-element silicide nanoparticles.
[0024] Phase Separation: Nanoparticles or other structures in which two or more distinct phases arise from a single homogeneous phase or mixture.
[0025] Introduction Embodiments of the disclosed subject matter provide multi-element compound (MEC) nanoparticles having at least three different elements without phase separation (e.g., a single phase exhibiting a single crystal structure, e.g., a single solid solution) and high temperature techniques for their manufacture (also referred to herein as synthesis or fabrication). Each multi-element compound nanoparticle comprises at least three elements, e.g., A, B, C, D, E, E, F, H, I ... x ,B y ,C z where A, B, and C represent various elements in the molecular compound (e.g., one or more metals, one or more nonmetals, or any combination of the foregoing), and x, y, and z represent the number of atoms of each element in the molecular compound. In some embodiments, the MEC nanoparticles consist of multiple sites, with at least one atom of one of the elements in each site (e.g., site A, site B, site C, etc.). Each site can form a compound bond with at least one other site in the nanoparticle.
[0026] To produce MEC nanoparticles, high temperatures can be used to promote decomposition of the precursors and subsequent multi-element mixing and compound formation. However, temperature application can be precisely controlled to avoid structural degradation and particle aggregation, for example, by tailoring the heating profile to apply short pulses of high temperature. In some embodiments, the high temperature used to synthesize MEC nanoparticles can be, for example, in the range of 500 K to 4000 K (e.g., inclusive of 1000 to 2000 K), and the duration of the high temperature can be, for example, in the range of 1 millisecond (ms) to 1 second (s) (e.g., inclusive of 10 to 100 ms). The transition to / from high temperature can be, for example, at 10 K / min or more than 10 K / min. 7 This can be achieved relatively quickly, with heating and / or cooling rates of up to 1000 K / min. In some embodiments, additional heating at the same or different temperatures (e.g., 2000 K or higher) and / or for longer durations (e.g., 1-10 min) can be subsequently administered to achieve nanoparticles of different composition and / or material properties.
[0027] Such MEC nanoparticles can exhibit stable structures due at least in part to (1) compound-forming structures with strong covalent bonds, and / or (2) high mixing entropy, which can improve the structural stability thermodynamically and kinetically. In addition, the rapid synthesis capabilities enabled by the disclosed technology can allow high-throughput Pt screening of element combinations for suitability in specific applications. In some embodiments, artificial intelligence (AI) (e.g., machine learning) can be used in conjunction with the disclosed technology to fabricate and evaluate different MEC nanoparticle compositions for specific applications, as well as to optimize the properties of the MEC nanoparticles (e.g., by varying fabrication parameters such as heating temperature, temperature duration, heating ramp rate, cooling ramp rate, etc.).
[0028] In some embodiments, MEC nanoparticles may be particularly useful as catalysts for thermochemical and / or electrochemical reactions. For example, thermochemical reactions may include, but are not limited to, ammonia (NH3) synthesis or decomposition, methane (CH4) pyrolysis and conversion, carbon dioxide (CO2) methanation and conversion, coal gasification, water gas shift reaction, syngas conversion reaction, or any combination of the foregoing. For example, electrochemical reactions may include, but are not limited to, water splitting (e.g., hydrogen and oxygen generation), fuel cell applications (e.g., hydrogen oxidation and oxygen reduction reactions), CO2 reduction reactions, nitrogen (N2) reduction reactions, or any combination of the foregoing.
[0029] Multi-element oxide (MEO) nanoparticles and MEO nanoparticle structures As discussed above, conventional manufacturing techniques are unable to produce multi-element nanoparticles having a single phase. Rather, as shown in FIG. 1A, conventional nanoparticles 100 formed from at least two different elements 102, 104 result in a distinct phase separation. In contrast, MEC nanoparticles produced according to the disclosed techniques can combine multiple different elements into a compound nanoparticle having a single uniform oxide phase. For example, FIG. 1B shows an exemplary multi-element oxide (MEO) nanoparticle 110 formed from a combination of oxygen (O) 112 and at least three different cations 118a-118c. In some embodiments, one, some, or all of the cations 118a-118c can be selected from a group 116 of metals, e.g., alkali metals, alkaline earth metals, lanthanides, actinides, transition metals, or post-transition metals. For example, in some embodiments, at least one cation 118a-118c of group 116 can be a transition metal and at least another cation 118a-118c of group 116 can be a noble metal (e.g., Ru, Rh, Pd, Ag, Re, Os, Ir, Pt, and Au). In some embodiments, MEO nanoparticles 110 can have a maximum cross-sectional dimension (e.g., diameter) D1 of about 20-25 nm.
[0030] In some embodiments, the MEO nanoparticles 110 can have a configurational entropy that is greater than that of the conventional oxide nanoparticles 100. In general, the configurational entropy can increase with the number of cations, which may be limited to 5 or less due to limitations of conventional manufacturing processes. The configurational entropy ΔS config is represented by Equation 1 below for MEO materials (eg, fluoride oxides (MO2) where M is a cationic element):
[0031]
number
[0032] where R is the gas constant, xi represents the mole fraction of metal cations, M sites represent cationic sites, and n is the total number of cations. For example, the coordination entropy of conventional oxide nanoparticles can be less than 13.38 J / mol / K (e.g., for 5 cations), while MEO nanoparticles produced according to embodiments of the disclosed subject matter can demonstrate coordination entropy of more than 13.5 J / mol / K, e.g., about 19.14 J / mol / K for MEO nanoparticles with 10 cations. In some embodiments, such an increase in entropy can improve the structural stability of MEO nanoparticles, for example, when exposed to harsh environments in certain applications.
[0033] In some embodiments, the plurality of MEC nanoparticles 110 may be supported on and / or integrated with a substrate to form a structure (e.g., a catalyst structure). In some embodiments, the substrate may be the same structure used to initially form the nanoparticles from the plurality of precursors (e.g., metal salts) that are loaded thereon and then heated. For example, in some embodiments, the substrate may be a carbon-based structure and may function as a heating element for the disclosed precisely controlled heating (e.g., thermal shock process). Alternatively or additionally, the substrate may be placed in thermal communication (e.g., conductive, convective, or radiative) with a heating element that provides the desired thermal shock to convert the precursors into the plurality of separated nanoparticles (e.g., the minimum spacing between adjacent nanoparticles 110 varies from ∼10 nm to ∼100 nm).
[0034] Referring to FIG. 1C, a simplified diagram of an exemplary catalyst structure 120 is shown. In the illustrated example, the catalyst structure 120 has a substrate 122 (e.g., a carbon-based structure) having a random array of MEO nanoparticles 110 having substantially the same composition. For example, in some embodiments, the substrate 122 can be formed of a network of carbon nanofibers (CNFs) 124, as shown in FIG. 1C. The MEO nanoparticles 110 can be formed directly on the surface of the CNFs 124. Thus, some of the MEO nanoparticles 110 can be disposed within the CNF network, while others can be considered to be disposed on the exterior-facing surface of the CNF network (e.g., substrate 122). The resulting catalyst structure 120 can be considered to be porous such that the flow of reactants can be directed perpendicular to the substrate 122 (e.g., to allow reactants to contact the nanoparticles 110 within the CNF network). Alternatively or additionally, the reactants can be directed substantially parallel to the major or active exterior surface of the substrate 122.
[0035] In Figure 1C, the substrate 122 is generally shaped as a rectangular prism. However, in some embodiments, the substrate can have a different shape (e.g., a film, membrane, polyhedral prism, disordered shaped structures, particles, etc.) and / or an arrangement of the MEO nanoparticles 110 (e.g., an ordered array of MEO nanoparticles on an exposed surface of the substrate) than that shown in Figure 1C. For example, in some embodiments, the substrate used to form and / or subsequently support the MEO nanoparticles can include CNFs, carbon nanotubes (CNTs), mesoporous carbon molecular sieves (CMK), carbon paper, carbon felt, carbon black powder or particles, graphite powder or particles, graphene, carbonized wood, semiconductors, textiles, metals, dielectrics, oxides, or any combination of the foregoing.
[0036] In some embodiments, the use of the rapid non-equilibrium techniques described herein allows for the synthesis of MEO nanoparticles with single-phase structure and uniform dispersion. Non-equilibrium synthesis is characterized by rapid high-temperature heating that promotes multi-element mixing to form MEO, while short heating times effectively avoid particle aggregation and oxide reduction. In some embodiments, due to differences between elements for MEO nanoparticles (e.g., oxidation potential, cation radius, crystal structure, etc.), heating may be performed in the presence of oxygen partial pressure and / or additional elements may be added to increase entropy, allowing the synthesis of unique MEO nanoparticles with customized structures that are otherwise not possible with conventional techniques.
[0037] [Table 1A]
[0038] [Table 1B]
[0039] Tables 1A-1B provide exemplary compositions of MEO nanoparticles with different crystal structures. As an example, ten-dimensional MEO nanoparticles (e.g., Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O, denoted as 10-MEO-MgMn (where x represents oxygen vacancies), can be prepared by heating a precursor-coated substrate at about 1500-1550 K for about 50 ms. 2―x After fabrication, scanning electron microscope (SEM) imaging revealed that uniform and high density nanoparticles 110 were formed on the substrate CNF 124, as shown in Figures 1D to 1E.
[0040] In some embodiments, the produced MEO nanoparticles can be further processed to obtain nanoparticles with different compositions. For example, multi-element carbide (ME-carbide) nanoparticles can be derived from the reaction of MEO nanoparticles with carbon. In some embodiments, ME-carbide nanoparticles can be carbide compounds of three or more metal elements covalently bonded to carbon. The different elements in the ME-carbide nanoparticles can be randomly distributed with high entropy.
[0041] In some embodiments, ME-carbonized nanoparticles can be formed by encapsulating (partially or completely) MEO nanoparticles with a coating containing at least carbon (C), as described in more detail elsewhere herein, and then subjecting the coated MEO nanoparticles to further heating (e.g., carbonization). For example, the coating can be a polymer containing C, oxygen (O), and hydrogen (H), such as, but not limited to, polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyvinylidene difluoride (PVDF), polytetrafluoroethylene (PTFE), or any combination thereof. Because ME-carbonized nanoparticles are derived directly from the reaction of MEO nanoparticles with C, ME-carbonized nanoparticles have a similar compositional space as MEO nanoparticles. In addition to the examples set forth above in Tables 1A-1B, Table 2 shows further exemplary compositions for ME-carbonized nanoparticles.
[0042] [Table 2]
[0043] Multi-element intermetallic (MEI) nanoparticles and MEI nanoparticle structures In some embodiments, multi-metallic disordered (MMD) nanoparticles can be converted to multi-element intermetallic (MEI) nanoparticles with long-term ordering (LRO). MMD nanoparticles can include at least three different metals, for example, formed by applying a heating pulse (e.g., ≥1000 K for 10-100 ms) to a metal precursor on a substrate. In some embodiments, MMD nanoparticles can have five or more different metals and can therefore be considered high entropy alloy (HEA) nanoparticles. For example, FIG. 2A shows a HEA nanoparticle 200 formed from multiple metals 202, e.g., at least five different elements 204a-204e, that form a disordered solid solution alloy. To form MEI nanoparticles, the MMD nanoparticles can be subjected to a second heating (e.g., annealing or ordering heating period) for a longer duration than the heating pulse used to form the MMD nanoparticles. The second heating can be at the same temperature as the MMD-forming heating pulse, or at a different temperature (e.g., less than or greater than the MMD-forming heating pulse). In some embodiments, MMD nanoparticles can be converted to MEI nanoparticles by heating for a period of time at least two orders of magnitude greater than the MMD-forming heating pulse, for example, ≥1000 K for 1-10 min.
[0044] Annealing for a longer time allows the atoms in the MMD to rearrange into a more thermodynamically stable intermetallic structure (e.g., disorder-to-order transition), followed by rapid cooling (e.g., at least 10 4K / s) locks the final ordered structure in place. For example, FIG. 2B shows an exemplary MEI nanoparticle 210 formed by annealing an MMD-nanoparticle (e.g., HEA nanoparticle 200 of FIG. 2A). In the illustrated example, MEI nanoparticle 210 is formed from multiple metals 212, e.g., at least five different elements 214a-214e, that form a single solid solution phase with LRO. When formed from an MMD nanoparticle, metal 212 of MEI nanoparticle 210 can be the same as metal 202 of MMD nanoparticle (e.g., HEA nanoparticle 200). In some embodiments, one, some, or all of elements 214a-214e can be selected from any known metal, e.g., alkali metals, alkaline earth metals, lanthanides, actinides, transition metals, or post-transition metals. In some embodiments, MEI nanoparticle 210 can have a maximum cross-sectional dimension (e.g., diameter), D2, of 10 nm or less (e.g., 3-6 nm, e.g., 3.5-5 nm).
[0045] The MEI nanoparticles 210 can exhibit long-range ordering on two sublattices (e.g., superlattice and non-superlattice). In some embodiments, the MEI nanoparticles can exhibit an LRO of at least 70%, e.g., at least 90% (e.g., about 100%), as defined by Equation 2:
[0046]
number
[0047] where I110 and I111 are the peak intensities of the superlattice (110) and non-superlattice (111), respectively, and I* is the corresponding peak intensity of the fully ordered structure (e.g., LRO = 100%). In some embodiments, MEI nanoparticles can have geometrically close-packed or topologically close-packed phases, the formation of which can depend on the material selection and stoichiometry of the nanoparticles. For example, the lattice structure of the geometrically close-packed phase of MEI nanoparticles can include L10 (e.g., a tetragonal distortion of the face-centered cubic (fcc) structure), L11, L12, B2, etc., and the lattice structure of the topologically close-packed phase can include Laves phase, σ phase, μ phase, etc.
[0048] In binary intermetallic compounds, each sublattice may be occupied by a single element. However, in MEI phases with more constituents than available sublattices, at least one sublattice (or both sublattices) may have two or more elements occupying its sites. For example, an octagonal ABCDEFGH intermetallic compound 220 may have a random distribution of elements A, B, and C (e.g., Pt, Pd, and Au) on one sublattice 220a and a random distribution of elements D, E, F, G, and H (e.g., Fe, Co, Ni, Cu, and Sn) on a second sublattice 220b, as shown diagrammatically in FIG. 2C. In the example fabricated, (Pt 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 We synthesized octonary MEI nanoparticles with a composition of 1.2×100, 1.2×100, and 1.4×100. The octonary MEI nanoparticles formed L10 intermetallic compounds characterized by (001), (110), and (111) planes with spacings of 3.73, 2.76, and 2.34 Å, respectively, as shown in the STEM images in Figures 2D–2F.
[0049] In some embodiments, the plurality of MEI nanoparticles 210 may be supported on and / or integrated with a substrate to form a structure (e.g., a catalyst structure). In some embodiments, the substrate may be the same structure used to initially form the nanoparticles from the plurality of precursors (e.g., metal salts) loaded thereon (or from preformed MMD nanoparticles such as HEA nanoparticles 200) and then heat them. For example, in some embodiments, the substrate may be a carbon-based structure and may function as a heating element for the disclosed precisely controlled heating (e.g., thermal shock process) and / or subsequent annealing for ordering. Alternatively or additionally, the substrate may be placed in thermal communication (e.g., conductive, convective, or radiative) with a heating element that provides the desired thermal shock and / or annealing for ordering.
[0050] Referring to FIG. 2G, a simplified diagram of an exemplary catalyst structure 230 is shown. In the illustrated example, the catalyst structure 230 has a substrate 122 (e.g., a carbon-based structure) having a random array of MEI nanoparticles 210 having substantially the same composition. For example, in some embodiments, the substrate 122 can be formed of a network of carbon nanofibers (CNFs) 124, as shown in FIG. 2G. The MEI nanoparticles 210 can be formed directly on the surface of the CNFs 124. Thus, some of the MEI nanoparticles 210 can be disposed within the CNF network, while others can be considered to be disposed on the exterior-facing surface of the CNF network (e.g., substrate 122). The resulting catalyst structure 120 can be considered to be porous such that the flow of reactants can be directed perpendicular to the substrate 122 (e.g., to allow the reactants to contact the nanoparticles 210 within the CNF network). Alternatively or additionally, the reactants can be directed substantially parallel to the major or active exterior surface of the substrate 122.
[0051] In Figure 2G, the substrate 122 is generally shaped as a rectangular prism. However, in some embodiments, the substrate can have a different shape (e.g., a film, membrane, polyhedral prism, disordered shaped structures, particles, etc.) and / or an arrangement of MEI nanoparticles 210 (e.g., an ordered array of MEI nanoparticles on an exposed surface of the substrate) than that shown in Figure 2G. For example, in some embodiments, the substrate used to form and / or subsequently support the MEI nanoparticles can include CNFs, carbon nanotubes (CNTs), mesoporous carbon molecular sieves (CMK), carbon paper, carbon felt, carbon black powder or particles, graphite powder or particles, graphene, carbonized wood, semiconductors, textiles, metals, dielectrics, oxides, or any combination of the foregoing.
[0052] In some embodiments, the use of a two-step heating technique (e.g., rapid pulse heating to convert the precursors to disordered nanoparticles, followed by a longer duration annealing heat to induce a disorder-order transition of the nanoparticles) can yield ordered intermetallic nanoparticles with well-defined atomic arrangements, small particle sizes (e.g., <10 nm), and customized compositions and phase structures (e.g., binary PtFe, ternary PtCoNi, pentanary PtFeCoNiCu, octanary PtPdAuFeCoNiCuSn, etc.) that would otherwise be impossible with conventional techniques. Without being limiting, additional exemplary compositions for MEI nanoparticles according to embodiments of the disclosed subject matter are shown in Table 3.
[0053] [Table 3]
[0054] Other Multi-Element Compound (MEC) Nanoparticles and Structures The techniques disclosed herein can be used to produce various types of MEC nanoparticles, such as MEO nanoparticles (e.g., (Ce,Zr,Hf,Ti)O2), ME-carbide nanoparticles (e.g., Ti,Zr,Mo,V,Nb)C, and MEI nanoparticles (e.g., (FeCoNiCu)Pt). Although the discussion and specific examples presented herein focus on MEO, ME-carbide, and MEI nanoparticles, embodiments of the disclosed subject matter are not limited thereto. Rather, one of ordinary skill in the art will readily appreciate that the teachings presented herein can be extended to form other types of MEC nanoparticles, such as, but not limited to, multi-element nitride nanoparticles, multi-element diboride nanoparticles, multi-element phosphide nanoparticles, multi-element sulfide nanoparticles, multi-element chalcogenide nanoparticles, multi-element silicide nanoparticles, multi-element amorphous glass nanoparticles, and the like. For example, Tables 4A-4B provide exemplary compositions of various other MEC nanoparticles that may be formed according to embodiments of the disclosed subject matter.
[0055] Additionally, while the discussion above and elsewhere herein focuses on the specific example of substantially spherical MEC nanoparticles, the teachings presented herein can be readily extended to provide variations having different compositions (e.g., various compounds and / or different elements), different sizes (e.g., from atomic compounds down to 1 μm in a cross-sectional dimension (e.g., maximum or minimum cross-sectional dimension)), different shapes (e.g., triangular, cylindrical rod, rectangular, etc.), different microstructures, different configurations (e.g., hollow, heterogeneous mixture, core-shell, etc.), or any combination of the foregoing. In some embodiments, the size of the produced nanoparticles can be varied, for example, by changing the precursor loading, by changing the substrate type or configuration, by changing the synthesis conditions (e.g., pulse temperature and / or duration), or any combination of the foregoing. In some embodiments, the shape of the produced nanoparticles can be varied, for example, by altering the synthesis conditions (e.g., pulse temperature and / or cooling rate). In some embodiments, the microstructure of the produced nanoparticles can be varied, for example, by using a stepwise synthesis process (e.g., to form a core-shell structure). In some embodiments, the composition of the produced nanoparticles can be altered, for example, by combining them with different substrates and / or nanoparticles.
[0056] [Table 4A]
[0057] [Table 4B]
[0058] Manufacturing method of MEO nanoparticles FIG. 3A illustrates an exemplary method 300 for forming MEO nanoparticles, such as MEO nanoparticle 110 of FIG. 1B and / or MEO nanoparticle-incorporated structure 120 of FIG. 1C. Method 300 can begin with process step 302, where precursors of multiple elements in a desired MEO nanoparticle are selected. As described above, each MEO nanoparticle can be formed from O in combination with at least three different cations (e.g., metal elements). Thus, in some embodiments, the precursors can include metal salts (e.g., metal chloride salts, metal nitrate hydrate salts, etc.) in a solution (e.g., ethanol, water, or mixtures thereof). In some embodiments, at least one of the precursors can include O.
[0059] Method 300 can proceed to decision step 304, where it is determined whether one of the selected cations is a noble metal. As described in more detail below, the selection of a noble metal may require additional synthesis strategies to allow for proper formation of MEO nanoparticles. If a noble metal is selected, method 300 can proceed from decision step 304 to decision step 306, where it is further determined whether the number of selected components provides sufficient entropy to allow for the formation of MEO nanoparticles. For example, in some embodiments, the inclusion of a noble metal in MEO nanoparticles may require six or more other metal elements (e.g., at least 10 different metals total) for proper formation of the compound oxide. If an insufficient number of elements are selected, method 300 can return to process step 302 to include additional cations via the selection of additional precursors.
[0060] If it is determined in determining step 306 that a sufficient number of elements have been selected, or if it is determined in determining step 304 that the MEO nanoparticles do not include a precious metal, the method 300 proceeds to process step 308, where the selected precursors are loaded onto the substrate. In some embodiments, the loading can be provided by dip-coating the substrate in one or more solutions containing the selected precursors and then drying (e.g., at room temperature). Alternatively or additionally, the loading can be via any other application technique, such as, but not limited to, pouring, brushing, spraying, printing, or rolling the solution onto the substrate. The loading of the precursors can reflect a desired composition for the resulting nanoparticle mixture, such as, for example, that a desired atomic ratio of cations is achieved.
[0061] Method 300 can proceed to decision step 310, where it is determined whether any of the selected cations are readily reduced (e.g., when exposed to the high temperatures required for particle synthesis, such as 1400-1600 K). If one or more cations are readily reduced, method 300 can proceed to treatment step 312, where the substrate with the precursors is placed in an atmosphere having an oxygen partial pressure for subsequent heating. For example, the substrate can be placed in an atmosphere of ambient air. Alternatively or additionally, the substrate can be placed in an atmosphere containing at least 15 vol.% O (e.g., .about.20.95 vol.%) and / or having an oxygen partial pressure of at least 150 mbar (e.g., .about.212.3 mbar). Otherwise, if the cations are not readily reduced, method 300 can proceed from decision step 310 to treatment step 314, where the substrate is placed in an atmosphere having substantially no oxygen partial pressure (e.g., .ltoreq.1 ppm O) for subsequent heating. For example, the substrate can be placed in an atmosphere of a noble gas, such as argon (Ar).
[0062] The method 300 can proceed from either process step 312 or process step 314 to process step 316, where the substrate having the precursor thereon is heated to a high temperature T highThe method 300 may proceed to a determination step 318, where the substrate is heated for a predetermined pulse period or dwell time t dwell If the predetermined dwell time has not been met, the method 300 returns to process step 316 where heating continues to maintain the substrate at the elevated temperature. Otherwise, if the predetermined dwell time has been met, the method 300 may proceed from decision step 318 to process step 320 where the substrate is heated to a relatively low temperature T low It is cooled rapidly to
[0063] In some embodiments, steps 316-320 of method 300 may subject the substrate to a thermal shock process. The thermal shock process may be accomplished, for example, by a pulsed heating profile 330, as shown in FIG. 3B. The pulsed heating profile 330 may begin at a relatively low temperature (e.g., <500 K, e.g., room temperature (e.g., 290-300 K)) and include (i) a rapid heating lamp 332a (e.g., (T high -T low ) / (t1-t0)≧10 4 K / s), (ii) at or near the peak temperature, T high (e.g., ≧1200 K), and (iii) a short dwell period 332b (e.g., (t−t)≦200 ms or ≦100 ms) at t2−t1 (e.g., ≧1200 K), and (iv) a rapid cooling ramp 332c (e.g., (T high -T low ) / (t3-t2)≧10 4 For example, in some embodiments, the peep temperature T high can be in the range of 1400-1600 K (inclusive) (e.g., about 1500-1550 K) for about 50-55 ms. Alternatively, in some embodiments, the duration of dwell time 332b is longer than the peak temperature T when the peak temperature is lower, e.g., in the range of 1200-1400 K. high In some embodiments, the cooling ramp rate (e.g., about 10 5 K / s) is the heat ramp rate (e.g., about 10 4 K / s).
[0064] In some embodiments, the pulse heating profile may be provided by passing an electric current through the substrate to provide Joule heating. Alternatively or additionally, in some embodiments, the pulse heating profile may be provided by a separate heating mechanism (e.g., direct Joule heating, conductive heating, radiative heating, microwave heating, laser heating, plasma heating, or any combination of the foregoing) in thermal communication with the substrate and capable of providing the heating profile of FIG. 3B. Further details regarding the thermal shock process that may be used in embodiments of the disclosed subject matter may be found in U.S. Patent Application Publication No. 2019 / 0161840, published May 30, 2019, the details of which are incorporated herein by reference.
[0065] Returning to FIG. 3A, rapid heating of the substrate in process step 316 can induce rapid pyrolysis and mixing of the precursors thereon, and subsequent rapid cooling in process step 320 can form the mixed precursors into compound oxide nanoparticles without undergoing aggregation, agglomeration, elemental segregation, or phase separation. Method 300 can proceed to process step 322, where the resulting MEO nanoparticles can be used in certain applications. For example, in some embodiments, the MEO nanoparticles can be used as starting materials for the production of other MEC nanoparticles, such as ME-carbide nanoparticles. Alternatively or additionally, the MEO nanoparticles (with or without a substrate used for production) can be used as catalysts for thermochemical and / or electrochemical reactions.
[0066] Although some of steps 302-322 of method 300 have been described as being performed once, in some embodiments, multiple iterations of a particular processing step may be used before proceeding to the next decision or processing step. In addition, while steps 302-322 of method 300 have been illustrated and described separately, in some embodiments, the processing steps may be combined and performed together (concurrently or sequentially). Furthermore, while FIG. 3A illustrates a particular order for steps 302-322, embodiments of the disclosed subject matter are not limited thereto. Indeed, in certain embodiments, steps may occur in a different order than those illustrated, or simultaneously with other steps.
[0067] Metal elements can have a wide range of oxidation potentials at high temperatures (e.g., according to an Ellingham diagram) that may otherwise result in sequential phase separation or metal impurities (e.g., failure of homogeneous mixing) in multi-element systems. Thus, as described above, method 300 can employ different synthesis strategies based on the desired composition of the final MEO nanoparticles, for example, based on the Gibbs free energy (ΔG=ΔH-T×ΔS) of the system. Indeed, oxide materials feature more complex element combinations than pure metals, so the formation of single-phase MEO nanoparticles requires careful design and synthesis guidelines. The selection of elements for MEO nanoparticles can be important, since some, such as Ni, Cu, and Pd, can be reduced to metals at high temperatures or by reducing conditions (e.g., carbon and 5% H2 / Ar). The oxide formation potential of an element can be evaluated by an Ellingham diagram, which shows the Gibbs free energy (ΔG) of formation of oxides at high temperatures, as shown in FIG. 3D.
[0068] Using the Ellingham diagram as a guide, single-element nanoparticles were synthesized for 24 individual elements capable of forming stable oxide nanoparticles using the disclosed thermal shock method. After this initial single-element screening, the elements were separated into three categories: easily oxidized elements (e.g., Y, Ca, Ti, Zr), easily reducible elements (e.g., Ni, Cu, Fe), and rare elements (e.g., Pd). Figure 3C is a schematic diagram 340 illustrating an embodiment of an exemplary element classification 344a-344c and associated strategies for generating single-phase MEO nanoparticles 346 with various structures (e.g., phosphor 348a, perovskite 348b, spinel 348c, rock salt 348d) from elements with different oxidation potentials 342. By using these strategies (single or in combination based on the constituent elements of the nanoparticles), the Gibbs free energy ΔG can be reduced, thereby facilitating the formation of single-phase MEO nanoparticles.
[0069] The first classification 344a can be assigned to elements that are determined to be easily oxidized (e.g., through experimental testing of the individual elements) and that are easily oxidized (e.g., through temperature-driven mixing (e.g., synthesis temperature, T high , increasing) can be used to form MEO nanoparticles therefrom. For example, temperature-driven mixing can be produced by exposing the elements to thermal shock (e.g., 1200-1600 K, ≤200 ms, e.g., ~1500 K, 55 ms). For example, (Zr,Ce,Hf,Ti)O synthesized at ~1000 K is shown in Figure 3(e). X Although phase separation was observed in the X-ray powder diffraction (XRD) of the nanoparticles, a single-phase fluorite structure was successfully obtained by increasing the synthesis temperature to ~1550 K. Hexanyl oxide (Zr, Ce, Hf, Ti, La, Y)O 2-x , ten-element oxides (Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O 2-x (Fluorite), 10-element oxides (Zr, Ce, Hf, Ti, La, Y, V, Nb, Ca, Mn)O 2-x (fluorite), and the pentane oxide (Ca,Mg)(Ti,Nb,Mn)O 3-x(Perovskite) nanoparticles were also successfully synthesized by this method, and the XRD patterns in Figure 3E, STEM atomic imaging, and TEM mapping confirm the single-phase structure of these materials.
[0070] The second classification 344b can be assigned to elements that are determined to be easily reduced (e.g., via experimental testing of the individual elements) and from which MEO nanoparticles can be formed using oxidation-driven mixing (e.g., reducing the enthalpy of mixing, ΔH). For example, oxidation-driven mixing can be achieved by increasing the oxygen partial pressure (P O2 ) (e.g., from ~1 ppm oxygen to ~212.3 mbar oxygen partial pressure). For example, homogeneous oxides characterized by a rock salt structure, (Fe,Co,Ni,Cu)O x The nanoparticles can be synthesized in air (e.g., at high P o2 ) can be prepared from precursors containing Fe, Co, Ni, and Cu. In contrast, the synthesis can be performed in an argon-filled glove box (e.g., with low P content of ~1 ppm). o2 When a similar synthesis was carried out in 3000 cc (1000 cc) tetramer, a face-centered cubic (fcc) metal structure was observed, as shown in Figure 3F. 4-x (spinel structure) and single element oxide (Mg, Co, Ni, Zn, Cu)O nanoparticles (rock salt structure) were also successfully synthesized.
[0071] A third classification 344c can be assigned to elements that are noble metals (e.g., Ru, Rh, Pd, Ag, Re, Os, Ir, Pt, and Au) and from which MEO nanoparticles can be formed using entropy-driven mixing (e.g., increasing the entropy of mixing, ΔS). For example, entropy-driven mixing can be generated by increasing the number of elements (e.g., 10 cations) to allow for the inclusion and stabilization of noble metals in the MEO nanoparticles. For example, as shown in FIG. 3G, (Zr, Ce, Hf) synthesized at high temperature (~1500 K) in air.o。9 Pd o。1 O x Phase separation of Pd metal and oxide in the decadal MEO can be observed. However, by adding six more cations to the composition, the entropy is effectively increased, thereby allowing the formation of ten-component MEO nanoparticles containing Pd (~10 at%) in its oxidation state, as shown in Figure 3G. Such compositions would otherwise result in phase separation of metallic Pd when synthesized using conventional heating methods (e.g., as shown in Figures 7D-7E). Similar results were achieved for the stabilization of oxidized Rh in ten-component MEO.
[0072] ME-Carbide Nanoparticles Manufacturing Method FIG. 4A illustrates an exemplary method 400 for forming ME-carbide nanoparticles. Method 400 can begin with process step 402, in which MEO nanoparticles are provided on a substrate. For example, MEO nanoparticles can be formed on a substrate via method 300 of FIG. 3A and then provided for separate conversion to ME-carbide nanoparticles. Alternatively, in some embodiments, the methods of FIG. 3A and FIG. 4A can be combined, for example, by replacing process step 402 of method 400 of FIG. 4A with steps 302-320 of method 300 of FIG. 3A.
[0073] Method 400 can proceed to process step 404, where the carbon source is formed on the MEO nanoparticles as a thin layer or coating (e.g., having a thickness equal to or less than the maximum cross-sectional dimension of the MEO nanoparticles). For example, the carbon source coating can at least partially surround or surround the MEO nanoparticles (e.g., all exterior surfaces of the MEO nanoparticles exposed from the substrate). In some embodiments, the substrate can act as an additional carbon source (e.g., CNFs, carbon nanotubes (CNTs), mesoporous carbon molecular sieves (CMK), carbon paper, carbon felt, carbon black powder or particles, graphite powder or particles, graphene, carbonized wood, etc.), such that the combination of the coating and substrate completely surrounds each MEO nanoparticle and isolates it from adjacent MEO nanoparticles. In some embodiments, the carbon source coating can include at least carbon (C) and can also include, but is not limited to, oxygen (O) and / or hydrogen (H). For example, the coating can include a polymer such as polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyvinylidene difluoride (PVDF) and / or polytetrafluoroethylene (PTFE). In some embodiments, the coating can be applied by pouring a polymer-alcohol solution onto the substrate followed by drying (e.g., in air). Alternatively or additionally, the coating can be applied by any other application technique such as, but not limited to, dip coating, brushing, spraying, printing, rolling, deposition, in situ polymerization of a precursor, etc.
[0074] The method 400 can proceed to a decision step 406 where a heating profile for carbonization can be selected. For example, if shock wave heating is desired, the method 400 can proceed to a treatment step 408 where the substrate having the MEO nanoparticles thereon is heated to a high temperature T high A high temperature T that may be the same as or different from (e.g., higher or lower than) carbThe method 400 can proceed to a determination step 410, where the substrate is heated to a predetermined pulse period or dwell time t pulse It is then determined whether the substrate is maintained at the elevated temperature for a period of time equal to or greater than the predetermined pulse period. If the predetermined pulse period has not been met, the method 400 can return to process step 408, where heating continues to maintain the substrate at the carbonization temperature. Otherwise, if the predetermined pulse period has been met, the method 400 can proceed from determination step 410 to process step 412, where the substrate is maintained at the elevated temperature T used to form the MEO nanoparticles. low The method 400 can proceed to step 414, where the total heating time required for carbonization, t carb It is determined whether the total heating time has been met. If the total heating time has not been met, the method 400 may return to process step 408 for repeated application of the heating pulse.
[0075] In some embodiments, steps 408-414 of method 400 may subject the substrate to a thermal shock wave process. The thermal shock wave process may be accomplished, for example, by a multi-pulse heating profile 470, as shown in FIG. 4D. The multi-pulse heating profile 470 may be comprised of a number of individual pulses 472, each of which may be of substantially identical shape and / or duration. Each individual pulse 472 may begin at a relatively low temperature (e.g., <500K, e.g., room temperature (e.g., 290-300K)) and include (i) a rapid heating ramp 474a (e.g., ≧10 4 K / s), (ii) a short dwell period at or near the carbonization temperature (e.g., 10 ms to 1 s), T carb (e.g., 1500-3000K), and (iii) rapid cooling ramp 474c (e.g., ≥ 10 4 For example, in some embodiments, the carbonization temperature T carb is the maximum temperature T used to generate MEO nanoparticles high (For example, T carbSo about 2000K, T high In some embodiments, each pulse t pulse The period of time is, for example, about 50 to 55 ms, the residence time t used for the production of nanoparticles. dwell The heating profile 470 may be similar to the total time of carbonization t carb For example, the individual pulses 472 may be applied in sequence until a total time t carb may be about 1 to 2 minutes (eg, 10 to 100 repetitions of pulse 472, inclusive).
[0076] Returning to FIG. 4A, if shockwave heating is not desired in determining step 406, the method 400 can proceed to processing step 418, where the substrate having MEO nanoparticles thereon is heated to a high temperature T carb The method 400 can proceed to a determination step 420, where the total heating time required for carbonization, t carb It is determined whether the carbonization time has been met. If the carbonization time has not been met, the method 400 returns to process step 418 and heating continues to maintain the substrate at the carbonization temperature. Otherwise, if the carbonization time has been met, the method 400 proceeds from decision step 420 to process step 422 where the substrate is heated to a relatively low temperature, e.g., T low It is cooled rapidly to
[0077] In some embodiments, steps 418-422 of method 400 can subject the substrate to sequential annealing for carbonization. Sequential annealing can be accomplished, for example, by heating profile 460, as shown in FIG. 4C. Heating profile 460 can begin at a relatively low temperature (e.g., <500K, e.g., room temperature (e.g., 290-300K)), followed by (i) heating lamps 462a (e.g., <10 4 K / s), (ii) carbonization temperature, T carb (e.g., 1500-3000 K) or thereabouts (e.g., including 1-2 minutes), and (iii) a rapid cooling ramp 474c (e.g., ≥ 10 4For example, in some embodiments, the carbonization temperature T carb is the maximum temperature T used to generate MEO nanoparticles high (For example, T carb So about 2000K, T high In some embodiments, the heating ramp 462a rate can be at least an order of magnitude slower than the rate used for MEO nanoparticle formation, and / or the cooling ramp 462c rate can be substantially the same as the rate used for MEO nanoparticle formation.
[0078] Returning to FIG. 4A, in either process step 408 or 418, the respective heating profile may be provided by passing an electric current through the substrate to provide Joule heating. Alternatively or additionally, in some embodiments, the heating profile may be provided by a separate heating mechanism (e.g., direct Joule heating, conductive heating, radiative heating, microwave heating, laser heating, plasma heating, or any combination of the foregoing) that is in thermal communication with the substrate and can provide the heating profile of FIG. 4C or 4D. In some embodiments, during high temperature application, the coating can be converted to carbon (e.g., amorphous carbon), thereby acting as a carbon source for ME-carbide formation. Method 400 can proceed from process step 422 or from determining step 414 to process step 416, where the resulting MEC nanoparticles can be used in a particular application. For example, in some embodiments, the MEC nanoparticles (with or without a substrate used for fabrication) can be used as catalysts for thermochemical and / or electrochemical reactions.
[0079] Although some of steps 402-422 of method 400 have been described as being performed once, in some embodiments, multiple iterations of a particular processing step may be used before proceeding to the next decision or processing step. In addition, while steps 402-422 of method 400 have been illustrated and described separately, in some embodiments, the processing steps may be combined and performed together (concurrently or sequentially). Furthermore, while FIG. 4A illustrates a particular order for steps 402-422, embodiments of the disclosed subject matter are not limited thereto. Indeed, in certain embodiments, steps may occur in a different order than those illustrated, or simultaneously with other steps.
[0080] Referring to FIG. 4B, an exemplary two-step heating process for the fabrication of MEC nanoparticles is shown. Metal salt precursors 432 can be uniformly loaded onto a substrate 434 to form an initial assembly 430. For example, metal salts can be dissolved in an organic solvent (e.g., methanol, ethanol, dimethyl ether, methyl ether, etc.), and the resulting solution can be applied (e.g., poured, dropped, coated, etc.) onto a substrate, followed by drying. In some embodiments, the substrate 434 can have and / or be formed from carbon (e.g., CNF). Application 436 of a rapid thermal shock (e.g., pulsed heating profile 330 of FIG. 3B; 1000-2000 K; pulse duration of 10 ms-1 s) to the assembly 430 can convert the metal salt precursors 432 into MEO nanoparticles 440 (e.g., high entropy oxide nanoparticles), where the high temperature drives precursor decomposition, oxide formation, and further mixing into a high entropy homogeneous mixture.
[0081] To convert the oxide to carbide, the assembly 438 is subjected to a coating process 442, whereby a polymer layer 446 is provided on the MEO nanoparticles 440 to act as a carbon source. For example, a polymer (e.g., PVA, PVP, PVDF, PTFE, etc.) can be dissolved in alcohol and applied (e.g., poured, dripped, coated, etc.) onto the substrate and then dried to form the polymer layer 446. Application 448 of extended heat (e.g., carbonization annealing in FIG. 4C or shock wave heating in FIG. 4D) to the assembly 444 drives a carbide formation reaction from the MEO, thereby converting the MEO nanoparticles 440 into uniform ME-carbide nanoparticles 452 on the substrate 434 (e.g., thereby forming structure 450). During the high temperature conversion process, the MEO nanoparticles 440 were physically confined by the coated polymer layer 446, thus maintaining their size and distribution. The coated polymer layer 446 not only provided a carbon source but also limited undesired aggregation or ripening of the nanoparticles 440 during carbonization. In some embodiments, the substrate 434 (e.g., CNF) can also serve as another carbon source to ensure complete conversion such that the ME-carbide nanoparticles 452 are firmly anchored onto the etched substrate surface.
[0082] The formation of ME-carbide is a solid-state reaction (e.g., MEO+C converts to ME-carbide) and therefore may require additional time for diffusion and phase transformation. Thus, application of heat 448, whether via annealing or shockwave profiles, is provided for a relatively longer period of time (e.g., on the order of tens of seconds, such as 1-2 minutes) to allow for complete conversion of MEO 440 to ME-carbide 452. In some embodiments, continuous annealing may result in aggregation of nanoparticles due to diffusion over long periods of time. Thus, in some embodiments, shockwave heating may be preferred as it only results in short-term diffusion and therefore may be more controllable with respect to reaction time and particle size.
[0083] In some embodiments, the contribution to the overall stability of ME-carbide nanoparticles from their structural design and synthesis can be three-fold. First, the bond strength can be increased following the fabrication sequence from metal-metal (MM) to metal-oxygen (MO) (e.g., in MEO nanoparticles 440) to metal-carbon (MC) (e.g., in ME-carbide nanoparticles 452). Thus, the carbide structure can enable a certain chemical stability that is desirable when used as an electrocatalyst in harsh operating conditions. Second, the homogeneous mixing and high entropy stabilization effect can further improve the chemical and structural stability against parasitic reactions during electrocatalysis. Thermodynamically, the increase in the reaction temperature (T) and entropy (ΔS) of the system can lead to a decrease in the Gibbs free energy (ΔG), suggesting that high temperature and high entropy are both favorable for forming ME-carbide nanoparticles. Third, due to the etching mechanism during ME-carbide formation, these nanoparticles can be tightly embedded in and / or on the CNF substrate (rather than loosely attached), thereby improving the stability of the structure and avoiding nanoparticle detachment. In summary, embedded ME-carbide nanoparticles can combine the advantages of covalent bonding, high entropy stabilization, and surface structures toward ultrahigh stability.
[0084] Manufacturing method of MEI nanoparticles 5A illustrates an exemplary method 500 for forming MEI nanoparticles, such as MEI nanoparticles 210 of FIG. 2B and / or MEI nanoparticle-incorporated structure 230 of FIG. 2G. Method 500 can begin with a decision step 502, where it is determined whether a multi-element starting nanoparticle (e.g., high entropy alloy (HEA) or multi-metallic disorder (MMD)) is provided. If starting nanoparticles are provided, method 500 can proceed to process step 512; if not, method 500 can proceed to process step 504 to begin fabricating starting nanoparticles.
[0085] In process step 504, multiple metal precursors for the desired MEI nanoparticles are loaded onto the substrate. As discussed above, each MEI nanoparticle can be formed from at least three different metal elements (e.g., at least five different metal elements for high entropy configurations). Thus, in some embodiments, the precursors can include metal salts (e.g., metal chloride salts) in solution (e.g., ethanol, water, or mixtures thereof). In some embodiments, loading can be provided by dip-coating the substrate in one or more solutions containing the selected precursors and then drying (e.g., at room temperature). Alternatively or additionally, loading can be via any other application technique, such as, but not limited to, pouring, brushing, spraying, printing, or rolling the solution onto the substrate. The loading of the precursors can reflect the desired composition for the resulting mixture of nanoparticles, for example, such that a desired atomic ratio of metals is achieved.
[0086] The method 500 may proceed to process step 506, where the substrate having the precursor thereon is heated to a first high temperature T H1 The method 500 may proceed to a determination step 508, where the substrate is heated for a predetermined pulse or dwell time t dwell It is determined whether the substrate is maintained at the first elevated temperature for a predetermined dwell time. If the predetermined dwell time has not been met, the method 500 returns to process step 506 where heating continues to maintain the substrate at the first elevated temperature. Otherwise, if the predetermined dwell time has been met, the method 500 may proceed from determination step 508 to process step 510 where the substrate is heated to the first relatively low temperature T L1 The resulting mixture is then rapidly cooled to room temperature, thereby forming a plurality of MMD nanoparticles (e.g., HEA nanoparticles) on the substrate.
[0087] The method 500 can proceed to process step 512, where the substrate having MMD nanoparticles thereon is subjected to a second high temperature T H2The substrate is heated to a second elevated temperature, which may be the same or different (e.g., higher or lower) than the first elevated temperature. Method 500 may proceed to decision step 514, where it is determined whether the substrate has been maintained at the second elevated temperature for a predetermined period of time to induce long term ordering (e.g., LRO ≥ 90%) of the metal atoms within the nanoparticles. If the predetermined ordering period has not been met, method 500 returns to process step 512, where heating continues to maintain the substrate at the second elevated temperature. Otherwise, if the predetermined ordering period has been met, method 500 may proceed from decision step 514 to process step 516, where the substrate is heated to a second relatively lower temperature T L2 (For example, T L1 Same as or T L1 Higher, or T L1 The resulting MEI nanoparticles are then rapidly cooled to a temperature lower than 1000 K (lower than 1000 K), thereby forming a plurality of MEI nanoparticles on the substrate.
[0088] In some embodiments, steps 504-516 of method 500 can subject the substrate to a two-stage heating process. The two-stage heating process can be accomplished by a heating profile 520, for example, as shown in FIG. 5B. In some embodiments, in a first stage 522, the heating profile 520 can include, for example, a rapid heating pulse, similar in shape and / or timing to that used to produce MEO nanoparticles (e.g., as shown in FIG. 3B) and / or to produce ME-carbide nanoparticles (e.g., as shown by individual pulse 472 in FIG. 4D). For example, the heating in the first stage 522 can be performed at a relatively low temperature, T L (e.g., <500 K, such as at room temperature (e.g., 290-300 K)), (i) a rapid heating lamp 524a (e.g., ≥ 10 4 K / s), (ii) the first high temperature, T H (e.g., >1000K, e.g., about 1100K) or nearby short dwell times 524b (e.g., 10-100 ms, e.g., about 50-55 ms); (iii) a rapid cooling ramp 524c (e.g., ≥ 10 4 K / s).
[0089] After the first stage 522, the second stage 526 heating can be performed, for example, with a delay (e.g., (t2-t1) > 100 ms, e.g., 1 second) after completion of the rapid cooling ramp 524c. In some embodiments, in the second stage 526, the heating profile 520 can include an extended heating period, similar in shape and / or timing to that used to produce ME-carbide nanoparticles (e.g., as shown by profile 460 in FIG. 4C). For example, the second stage 526 heating can include a relatively low temperature, T L (e.g., <500 K, e.g., at room temperature (e.g., 290-300 K)), (i) a rapid heating lamp 528a (e.g., ≥ 10 4 K / s), (ii) a second high temperature, T H (e.g., >1000K, e.g., about 1100K) or thereabouts (e.g., 1-10 minutes, e.g., about 5 minutes); (iii) a rapid cooling ramp 528c (e.g., ≥10 4 K / s).
[0090] Returning to FIG. 5A, in either process step 506 or 512, the respective heating profile may be provided by passing an electric current through the substrate to provide Joule heating. Alternatively or additionally, in some embodiments, the heating profile may be provided by a separate heating mechanism (e.g., direct Joule heating, conductive heating, radiative heating, microwave heating, laser heating, plasma heating, or any combination of the foregoing) that is in thermal communication with the substrate and capable of providing the heating profile of FIG. 5B. From process step 516, method 500 may proceed to process step 518, where the resulting MEI nanoparticles may be used in a particular application. For example, in some embodiments, the MEI nanoparticles (with or without a substrate used for fabrication) may be used as catalysts for thermochemical and / or electrochemical reactions.
[0091] Although some of steps 502-518 of method 500 have been described as being performed once, in some embodiments, multiple iterations of a particular processing step may be used before proceeding to the next decision or processing step. In addition, while steps 502-518 of method 500 have been illustrated and described separately, in some embodiments, the processing steps may be combined and performed together (concurrently or sequentially). Furthermore, while FIG. 5A illustrates a particular order for steps 502-518, embodiments of the disclosed subject matter are not limited thereto. Indeed, in certain embodiments, steps may occur in a different order than those illustrated, or simultaneously with other steps.
[0092] Embodiments of the disclosed subject matter can provide MEI nanoparticles with multiple elements, for example, by using controllable synthesis of ordered intermetallic compounds driven by low enthalpy. In some embodiments, fabrication can rely on a multi-element disorder-order phase transition strategy (e.g., HEA to MEI) that results in a more thermodynamically stable configuration. The disclosed techniques can be used to synthesize MEI nanoparticles with sizes of, for example, about 4-5 nm and / or as many as eight different metal elements without the particle growth and / or phase separation commonly encountered in conventional intermetallic fabrication techniques. To investigate the disorder-order phase transition that enables MEI formation, pentanediol (Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 Arrays of Pt(Fe) samples were synthesized and their order was characterized via XRD, as shown in Figure 5C. According to the calculated hypothetical XRD pattern, the diffraction peaks of (001) at 24.2° and (110) at 33.4° are from Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) are the superlattice peaks of the ideal L10 intermetallic structure. Based on the intensities of these peaks, the degree of ordering of the different five-element samples was quantified using the LRO parameter (see equation (2) above).
[0093] In the sample prepared by heating for 0.05 s, no superlattice diffraction peaks were observed, and the short heating time was Pt1Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 As the heating time increased from 0.5 s to 5 min, the characteristic diffraction peaks of L10, (001) and (110) gradually enhanced, as shown in Figure 5C. As a result, the LO increased from 10% (0.5 s) to 60% (1 min) and finally to ~100% (5 min) (see Figure 9A), demonstrating the disordered to ordered phase transition process that was completed after 5 min of heating. 0.7 Co 0.1 Ni 0.1 Cu 0.1 The effect of heating temperature and time on the LRO of pentanediol (Fe ) could be achieved only by heating ~100% LRO at ~1100 K for ~5 min. This disorder-to-order transition process (0.5 s to 5 min) was also observed for pentanediol (Fe ) synthesized at ~1100 K for different heating times. 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) This is consistent with scanning transmission electron microscopy (STEM) imaging of the MEI nanoparticles (Figures 9C-9E). For example, Figures 9C-9E show that the disordered HEA nanoparticle structure is transformed into an MEI structure over the course of heating for ~5 min.
[0094] This disordered to ordered phase transition to a single-phase MEI of immiscible elements can only be achieved on the nanoscale. 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) For nanoparticles, a fully ordered L10 structure (LRO = 100%) could be obtained for particles with diameters between 4 and 5 nm. However, as shown in Figure 5D, the LRO decreases with particle size for particles larger than 5 nm, regardless of the particle synthesis method (e.g., slow cooling or longer heating time). As the particle size increases to approximately 60 nm or greater, the particles exhibit disordered or other phase-separated heterostructures, as confirmed by STEM and energy dispersive X-ray analysis (EDX).
[0095] System for nanoparticle production In some embodiments, a system for MEC nanoparticle fabrication can include a heating mechanism and a controller operably coupled to the heating mechanism and configured to control the heating mechanism, e.g., to achieve any of the heating profiles disclosed herein. For example, the heating mechanism can include a direct joule heater, a conductive heater, a radiative heater, a microwave heater, a laser, a plasma, or any combination thereof, or any other means for semi-continuous or pulsed heating. In some embodiments, the substrate to which the MEC nanoparticles are provided and / or bonded can be part of the heating mechanism (e.g., by passing a current through the substrate to provide joule heating).
[0096] In some embodiments, the manufacturing system can optionally include a rapid cooling mechanism. For example, the rapid cooling mechanism can be passive cooling by radiation, conduction, or both; active cooling by conduction, convection, or both; active cooling by endothermic induced phase or chemical transitions; any other means for rapid cooling (e.g., at least 10 4 K / s); or any combination of the foregoing. In some embodiments, the controller can be operatively coupled to and configured to control the rapid cooling mechanism, for example, to achieve any of the heating profiles disclosed herein.
[0097] The components of the nanoparticle production system and / or components of its configuration can be similar to the heating systems described in U.S. Patent Application Publication No. 11,193,191, published December 7, 2021, U.S. Patent Application Publication No. 2018 / 0369771, published December 27, 2019, International Publication No. WO2020 / 252435, published December 17, 2020, and / or International Publication No. WO2020 / 236767, published November 26, 2020, all of which are incorporated herein by reference.
[0098] 6 illustrates a generalized example of a suitable computing environment 631 in which the innovations described above may be implemented, such as aspects of the nanoparticle manufacturing system, method 300, method 400, and / or method 500 described above. The computing environment 631 is not intended to suggest any limitation as to scope of use or functionality, as the innovations may be implemented in a variety of general purpose or special purpose computing systems. For example, the computing environment 631 may be any of a variety of computing devices (e.g., a desktop computer, a laptop computer, a server computer, a tablet computer, etc.).
[0099] Referring to FIG. 6, a computing environment 631 includes one or more processing units 635, 637 and memory 639, 641. In FIG. 6, this basic configuration 651 is included within the dashed line. The processing units 635, 637 execute computer-executable instructions. The processing units may be general-purpose central processing units (CPUs), processors in application specific integrated circuits (ASICs), or any other type of processor. In a multi-processing system, multiple processing units execute computer-executable instructions to increase processing power. For example, FIG. 6 shows a central processing unit 635 and a graphics processing unit or co-processing unit 637. The tangible memory 639, 641 may be volatile memory (e.g., registers, cache, RAM), non-volatile memory (e.g., ROM, EEPROM, flash memory, etc.), or some combination of the two accessible by the processing units. The memories 639, 641 store software 633 implementing one or more innovations described herein in the form of computer-executable instructions suitable for execution by a processing unit(s).
[0100] A computing system may have additional features. For example, computing environment 631 includes storage 661, one or more input devices 671, one or more output devices 681, and one or more communication connections 691. An interconnection mechanism (not shown), such as a bus, controller, or network, interconnects the components of computing environment 631. Typically, operating system software (not shown) provides an operating environment for other software executing in computing environment 631 and coordinates the activities of the components of computing environment 631.
[0101] Tangible storage 661 may be removable or non-removable and includes magnetic disks, magnetic tapes or cassettes, CD-ROMs, DVDs, or any other medium that can be used to store information in a non-transitory manner and that can be accessed within computing environment 631. Storage 661 can store instructions for software 633 that implements one or more innovations described herein.
[0102] The input device(s) 671 may be a touch input device such as a keyboard, a mouse, a pen, or a trackball, a voice input device, a scanning device, or another device that provides input to the computing environment 631. The output device 671 may be a display, a printer, speakers, a CD-writer, or another device that provides output from the computing environment 631.
[0103] The communication connection(s) 691 enable communication over a communication medium to another computing entity. The communication medium conveys information such as computer-executable instructions, audio or video input or output, or other data in a modulated data signal. A modulated data signal is a signal that has one or more of its characteristics set or changed in such a manner as to encode information in the signal. By way of example, and not limitation, the communication medium may be electrical, optical, radio frequency (RF), or another carrier.
[0104] Any of the disclosed methods may be implemented as computer-executable instructions stored on one or more computer-readable storage media (e.g., one or more optical media disks, volatile memory components (such as DRAM or SRAM), or non-volatile memory components (such as flash memory or hard drives)) and executed on a computer (e.g., any commercially available computer, including a smartphone or other mobile device that includes computing hardware). The term computer-readable storage medium does not include communication connections such as signals and carrier waves. Any computer-executable instructions for implementing the disclosed techniques, as well as any data created and used during the implementation of the disclosed embodiments, may be stored on one or more computer-readable storage media. The computer-executable instructions may be a dedicated software application or part of a software application that is accessed or downloaded, for example, via a web browser or other software application (such as a remote computing application). Such software may be executed, for example, on a single local computer (e.g., any suitable commercially available computer) or in a networked environment using one or more networked computers (e.g., via the Internet, a wide area network, a local area network, a client-server network (such as a cloud computing network), or other such network).
[0105] For clarity, only some selected aspects of the software-based implementation are described. Other details well known in the art are omitted. For example, it should be understood that the disclosed technology is not limited to any particular computer language or program. For example, aspects of the disclosed technology can be implemented by software written in C++, Java, Perl, or any other suitable programming language. Similarly, the disclosed technology is not limited to any particular computer or hardware type. Specific details of suitable computers and hardware are well known and need not be described in detail in this disclosure.
[0106] It should also be appreciated that any functionality described herein may be performed, at least in part, by one or more hardware logic components instead of software. For example, and without limitation, exemplary types of hardware logic components that may be used include field programmable gate arrays (FPGAs), program specific integrated circuits (ASICs), program specific standard products (ASSPs), systems on a chip (SOCs), complex programmable logic devices (CPLDs), etc.
[0107] Additionally, any of the software-based embodiments (e.g., including computer-executable instructions for causing a computer to perform any of the disclosed methods) can be uploaded, downloaded, or remotely accessed via suitable communication means. Such suitable communication means include, for example, the Internet, the World Wide Web, an intranet, a software application, cable (including fiber optic cable), magnetic communication, electromagnetic communication (including radio frequency, microwave, and infrared communication), electronic communication, or other such communication means. In any of the above examples and embodiments, the provision of requests (e.g., data requests), instructions (e.g., data signals), commands (e.g., control signals), or any other communication between systems, components, devices, etc., can be by generation and transmission of appropriate electrical signals via wired or wireless connections.
[0108] Example of fabrication and experimental results MEO Nanoparticles Oxides (Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O 2-x (denoted as 10-MEO-MgMn (x represents oxygen vacancy)) nanoparticles were synthesized according to the disclosed fabrication technique. In particular, conductive carbon nanofibers (CNFs) were selected as the substrate and utilized for Joule heating to provide rapid high-temperature heating with controllable magnitude and duration. A solution of polyacrylonitrile with a concentration of 8 wt% in dimethylformamide was electrospun into polyacrylonitrile fibers at a voltage of 13 kV and a spinning distance of 15 cm. These as-spun films were first stabilized at 553 K in air for 6 h and then carbonized at 1273 K in argon for 2 h to prepare CNFs as substrates. Multiple salt precursors of each element were mixed in equimolar amounts in the solution phase (0.05 mol / L) and the mixed precursor salts were applied at 100 μL / cm. 2 The coating was uniformly performed on the CNF substrate with a loading of 100 μm. For example, CeN3O9·6H2O(99.0%), LaN3O9·6H2O(99.99%), YN3O9·6H2O(99.9%), CaN2O6·4H2O(99.0%), MgN2O6·6H2O(99.0%), GdN3O9·6H2O(99.9%), MnN2O6·4H2O(97.0%), FeN3O9·9H2O(98.0%), CoN2O6·6H2O(98.0%), CuN2O6·6H2O(98.0%), Different salt solutions (0.05 mol / L) were prepared by dissolving NiN2O6·6H2O (98.0%), InN3O9·xH2O (99.9%), CrN3O9·9H2O (99.0%), ZnN2O6·6H2O (98.0%), PdCl2 (99.0%), HfCl4 (99.9%), ZrCl4 (99.9%), TiCl4 (99.9%), VCl3 (97.0%), and NbCl5 (99.9%) in an ethanol / water mixture with a volume ratio of 9 / 1. The different salts were selected and mixed in equimolar amounts in a multi-element synthesis. These solutions were then pumped at 100 mL / cm. 2The mixture was loaded onto a CNF film at a loading amount of 0.01g / g and then dried at room temperature before being heated at high temperature.
[0109] High-temperature synthesis by electrical Joule heating was performed in an argon atmosphere (Po2: ~1 ppm) or in controlled oxygen partial pressure (high Po2: in air). CNFs or carbon paper films were cut to a size of 5 mm × 20 mm, which were attached to copper electrodes supported by glass slides using silver paste, then connected with a current supply. Different input currents were applied to the materials, and the resulting high temperatures produced emitted light, which was recorded using a high-speed camera to determine the sample temperature. After high-temperature heating (e.g., 1500 K, 50 ms), scanning electron microscope (SEM) imaging revealed the formation of uniform and dense nanoparticles on the CNFs. The particle size and distribution could be further tuned by adjusting the duration of the synthesis, e.g., shorter heating times yield smaller particle sizes with narrower particle size distributions (e.g., 8 nm for a 10 ms heating pulse), and longer heating times yield larger particle sizes with larger particle size distributions (e.g., 40 nm for a 500 ms heating pulse).
[0110] Scanning transmission electron microscopy (STEM) elemental mapping of the 10‐MEO‐MgMn nanoparticles revealed homogeneous mixing of the 10 different elements throughout the fabricated nanoparticles without obvious elemental segregation or phase separation. It is noted that the 10 cationic elements and their respective single-element oxides have very different physicochemical properties, including a range of cationic radii (0.74–1.16 Å) and crystal structures (e.g., phosphor, rutile, and rock salt), that would otherwise prevent single-phase homogeneous mixing in conventional fabrication techniques. In contrast, the disclosed technique uses high temperatures to promote multi-element mixing for MEO nanoparticle formation while ensuring that the heating duration is short enough to prevent particle coarsening and phase separation. Thus, with this unique rapid heating technique and the three MEO synthesis strategies described above, a library of oxide nanoparticles with tunable compositions (from single-element mixtures to ten-element mixtures) not observed and not necessarily stable in bulk materials was achieved.
[0111] Density functional theory (DFT) calculations were performed to evaluate each thermodynamic parameter in the formation of a series of oxide systems. For example, the formation temperature of binary (Zr,Ti)O2 from the corresponding single element oxides was predicted to be 2828 K, while quaternary (Zr,Ce,Hf,Ti)O2 could form a single phase structure at a temperature of 1075 K. This result indicates that high temperatures are required for single phase MEO formation (temperature-driven mixing), while the lower formation temperatures of high entropy systems with an increasing number of components indicate an entropy-driven mixing effect. The calculated Gibbs free energy of (Zr,Ce,Hf,Ti)O2 is P O2 It decreased with increasing , indicating the oxidation-driven stabilization of the material. Furthermore, the DFT calculation results predict reasonable structural and chemical stability by considering the lattice distortion and various decomposition pathways of the formed single-phase MEO. Thus, the DFT results confirm that temperature, oxidation, and entropy play important roles in driving the formation of single-phase MEO.
[0112] Kinetics-wise, high temperatures are important to overcome the kinetic barrier for multi-element mixing, but too high a temperature can adversely induce particle degradation such as coarsening, agglomeration, and phase separation (e.g., metal impurities). Experimentally, (Zr,Ce,Hf,Ti,Mn,Co)O 2-x For the low synthesis temperature of about 1200 K, the formation of uniform nanoparticles was not observed on the CNF substrate. Rather, terrace-shaped oxides were present due to insufficient reaction. Meanwhile, increasing the synthesis temperature to 1800 K accelerates particle growth and agglomeration (>80 nm) and introduces metal impurities (e.g., Co) due to carbothermal reduction. Thus, an optimized temperature (~1500 K) could be used to synthesize uniform MEO nanoparticles on CNFs, for example, by providing just enough energy to mix all elements while preventing the as-formed oxides from agglomerating and reacting with carbon.
[0113] Due to the high-temperature synthesis and entropy stabilization, MEO nanoparticles naturally have excellent thermal stability. Experimentally, the structural stability of MEO was confirmed by the ternary oxide (Ce, Gd, Y)O 2-x , quaternary oxide (Zr,Ce,Hf,Ti)O2, and 10‐MEO-MgMn nanoparticles were observed by heating in situ STEM from 298 K to 1073 K (samples were stabilized for 1 h at each temperature before imaging). At 1073 K, the 10‐MEO-MgMn nanoparticles showed excellent morphology and size stability and maintained a homogeneous mixture without phase separation. In contrast, changes in morphology and size of the ternary samples, as well as elemental segregation of both the ternary and quaternary oxides, were observed. These experimental results on the thermal stability of MEO were consistent with the force field simulations and revealed the excellent thermal stability of our ten-component MEO nanoparticles, which may be due to their high-entropy structure characterized by both thermodynamic and kinetic stability.
[0114] The disclosed high-throughput synthesis method can enable the theoretical design and rapid exploration of a large library of MEO nanoparticles, for example, by mixing most elements in the periodic table. Such MEO nanoparticles can be particularly advantageous for catalytic applications, for example, methane combustion. Compared with conventional flame combustion, catalytic combustion of methane can stabilize the complete oxidation of the fuel at low temperatures and, at the same time, reduce emissions (e.g., minimal NOx emissions). However, the PdOx catalysts typically used for such reactions suffer from deactivation due to sintering of the nanoparticles and conversion of PdOx to metallic Pd during the reaction. Thus, the development of Pd-based catalysts with improved performance and stability can effectively improve the energy efficiency of catalytic CH4 combustion processes.
[0115] When formulating MEO catalysts, elements from different groups can be included, e.g., alkali metals, 3d-5d transition metals, and the noble metal Pd, which provide distinct catalytic functions, e.g., facilitating the transfer of electrons during the redox step, improving redox capability, and creating more oxygen vacancies to activate CH4, respectively. MEO catalysts were prepared using the disclosed high-temperature synthesis method with an oxide loading of ~2 wt% in each catalyst. Single-element PdOx nanoparticles were also synthesized with similar Pd loadings to serve as controls in this study. In the first step, 4-MEO(XY) supported on carbon paper was synthesized. 0.6 Mg 0.3 Pd 0.1 O x (where X and Y represent different metal elements) nanoparticles were screened as catalysts for CH4 combustion and compared with a PdOx control sample. Gas hourly space velocity (GHSV) of 10,800 L / (g pd h) and catalytic activity was systematically measured at 573-973 K using a plug-flow reactor with 5 vol% CH4 and 20 vol% O2 in the feed gas balanced with N2. Thermogravimetric analysis (TGA) confirmed that below 973 K, the bare carbon paper substrate did not degrade in air and was inert to CH4 combustion. For 4-MEO, the reaction onset temperature was ~623 K and CH4 conversion increased with reaction temperature. Among the sieved 4-MEO catalysts, (Zr,Ce) 0.6 Mg 0.3 Pd 0.1 O x showed the best performance (100% conversion at ~823K), which was higher than the control PdO x (74% conversion at 823K) is much more active.
[0116] In the second step, 4-MEO (e.g., (Zr,Ce) 0.6 Mg 0.3 Pd 0.1 O x After screening between (Zr, Ce), eight different elements of the 3d-5d transition metals were 0.6 Mg 0.3 Pd 0.1 O x Addition to (Zr, Ce)0.6 (Z) 0.15 Mg 0.15 Pd 0.1 O x A series of 5-MEOs with compositions of (Z = La, Y, Hf, Ti, Cr, Mn, Fe, and Cu) were constructed. The catalytic activity of the 5-MEO samples was measured at 623 K, and that of the 4-MEO (Zr, Ce) 0.6 Mg 0.3 Pd 0.1 O x For Z = La, Y, Hf, Ti, Cr, Mn, these 5‐MEOs are (Zr,Ce) 0.6 Mg 0.3 Pd 0.1 O x However, poisoning effects were observed with the addition of Fe and Cu. Finally, six elements that were shielded from the second step (e.g., La, Y, Hf, Ti, Cr, and Mn) were eliminated from the best performing (Zr, Ce). 0.6 Mg 0.3 Pd 0.1 O x In combination with (4-MEO-Pd), the nonmetal oxides (Zr, Ce) have the highest entropy among these MEO catalysts. 0.6 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.3 Pd 0.1 O 2-x (10-MEO-PdO) was synthesized.
[0117] Catalytic methane combustion was carried out at atmospheric pressure in a fixed-bed flow reactor. Using the disclosed high-temperature strategy, non-metal oxide nanoparticles were formed on carbon paper or Al2O3-coated carbon paper at a loading of ~2 wt%. The carbon paper used was first activated in a carbon dioxide atmosphere at 1173 K for 180 min. Furthermore, the carbon paper and Al2O3-coated carbon paper were confirmed to be stable up to 973 K. For the control PdOx samples, particles were prepared with the same Pd loading by impregnation method (e.g., the precursor was first loaded onto carbon paper, and then the sample was heat treated in a furnace in air atmosphere (3 K / min, 773 K, 120 min). For example, 50 mg of catalyst (e.g., carbon paper with 2 wt. % oxide loading) was loaded into a microflow quartz reactor (7 mm inner diameter). The catalyst bed was placed between quartz wool plugs in the reactor. The catalyst was heated to 473 K, 523 K, or 573 K at a rate of 5 K / min in N2 (20 mL / min), and the gas flow was adjusted to the reactant feed (18 mL / min, space velocity = 10,800 L (g pd h) -1 or 180 mL / min, space velocity = 108,000 L (g pd h) -1 The reactants CH4 (99.99%) and O2 (99.999%) with N2 as the balance were co-fed to the reactor using calibrated mass flow controllers with a CH4:O2 molar ratio of 1:4.
[0118] To test the catalytic performance in the presence of water, about 4 vol% H2O was added to the gas feed using a steam generator maintained at 303 K. The reaction temperature was increased stepwise from 473 K, 523 K, or 573 K to 973 K, and the reaction was carried out at each temperature until the conversion was constant. A gas chromatograph equipped with a silica capillary column and a barrier ionization discharge (BID) detector was used to determine the conversion of reactants and the formation of products. All lines between the reactor outlet and the GC sampling loop inlet were heat traced up to 423 K to prevent condensation of products. The methane conversion was calculated as follows:
[0119]
number
[0120] 10-MEO-PdO is a catalyst that is more stable than other catalysts (single PdO x , 4-MEO, and 5-MEO), reaching full conversion at 673 K, as shown in Figure 7A. 0.66 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.34 O 2―x The sample (without Pd) was much less active towards CH combustion (e.g., as shown in FIG. 7B), indicating the importance of stabilizing Pd in the 10-MEO-PdO sample to improve the catalytic performance.
[0121] As shown in Figure 7C, PdO x The catalytic stability of the best performing 4-MEO-Pd and 10-MEO-PdO was also evaluated and compared continuously at 648 K (after catalytic reaction at 973 K). The high catalytic activity of the 10-MEO-PdO catalyst was extremely stable and did not decrease obviously after 100 h, while the CH4 conversion of 4-MEO-Pd decreased from 31% to 20% after 26 h. In contrast, PdO x The CH4 conversion of the control declined faster, resulting in deactivation after 22 h, which is consistent with the PdO2 catalysis during operation at high temperatures, as confirmed by XRD after extended stability testing. x The durability trend can be attributed to the entropy effect ((Zr, Ce) 0.6 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.3 Pd 0.1 O 2-x > Zr, Ce) 0.6 Mg 0.3 Pd 0.1 O x >PdO x), which can stabilize Pd in a cationic state in a high-entropy structure for substantially improved overall catalyst stability. The 10-MEO-PdO tennary oxide catalyst was also characterized after a 100-h durability test by elemental mapping, and little change in structural uniformity was observed.
[0122] To further stress the catalyst under harsh practical applications, the 10-MEO-PdO catalyst was evaluated for methane combustion in the presence of water (~4 vol%). To avoid accelerated carbon etching under humid conditions, the carbon paper substrate was protected by a thin layer of Al2O3 coating (deposited using atomic layer deposition). Despite these harsh conditions, the 10-MEO-PdO catalyst showed high activity for complete CH4 conversion at ~673 K. Notably, the 108,000 L(g pd h) -1 The high GHSV of the catalyst ensures stability evaluation in the kinetically controlled regime. In particular, the 10-MEO-PdO sample exhibited stable performance in both cases for 100 h of continuous operation, demonstrating the inherent stability of the catalyst.
[0123] ME-Carbide Nanoparticles Mo2C was initially selected as a model material to study the detailed mechanism during the two-step high-temperature transformation. First, CNF substrates were prepared using electrostatic spinning, which was uniformly coated with metal salt precursors. Polyaniline (Mw>15,000) was dissolved in N,N-dimethylformamide at 8 wt.%. The precursors of CNF were prepared by electrostatic spinning (e.g., 15 kV) with appropriate thickness. CNF membranes were prepared by activating the CNF precursors at 280 °C in air for 6 h, followed by carbonization at 1000 °C in Ar for 2 h. TiCl4, ZrCl4, VCl4, NbCl5 and MoCl5 were dissolved in alcohol at a concentration of 0.05 M, separately. The five equivalent solutions were mixed and 100 μL / cm 2 It was poured onto the CNF substrate at an areal density of
[0124] The loaded CNF substrate was then transferred to a Joule heating device (e.g., thermal shock device). For example, after drying, a 1 × 0.5 cm CNF substrate with mixed precursor salts thereon was glued between two copper tapes (fixed on a glass sheet) by using silver paste. The resulting device was then transferred to a glove box, and both ends of the copper tape were connected to a current source by wires. MEO nanoparticles (e.g., MoO2 intermediate nanoparticles) can be obtained after 55 ms of thermal shock treatment. A high-speed thermal sensing camera was used to determine the temperature profile (e.g., based on blackbody radiation) using the detected light spectrum emanating from the heating setup. The Joule heating setup was designed for rapid heating (e.g., ramp rate >10 4 K / s) and cooling (e.g., ramp rates >10 5 The synthesis was performed at a rate of 1000 s (1000 s / s), which ensured that ultra-small MoO2 nanoparticles with diameters of ~20 nm were uniformly distributed on the CNF substrate. The X-ray diffraction patterns of these nanoparticles were in good agreement with the MoO2 phase, suggesting successful synthesis.
[0125] In the second step, the obtained MoO nanoparticles on the CNF substrate are coated with a thin and uniform layer of polymer (e.g., 50 μL / cm 2 The CNF substrate was coated with a polyvinylpyrrolidone (PVP) / alcohol solution (0.05 g / mL). A second high-temperature treatment (e.g., carbonization) was then performed to obtain the final ME-carbonized nanoparticles supported on the CNF substrate. The system temperature was gradually increased to 2000 K by gradually increasing the current applied to the CNF substrate and maintained for 1 min, and then rapidly quenched to room temperature by cutting off the electric signal, thereby obtaining ME-carbonized nanoparticles on the CNF substrate.
[0126] Control experiments were performed in parallel using conventional furnace heating in Ar atmosphere for the same MEO to ME-carbide conversion process. Due to limitations of the furnace system, the highest heating rate achieved was 20 K / min and the highest temperature was 1273 K. Thus, the entire process was ~4-5 orders of magnitude longer compared to the disclosed Joule heating method. Due to the long heating time and slow cooling rate by furnace heating, the ME-carbide particles were found to severely agglomerate. In contrast, all ME-carbide nanoparticles formed using the disclosed Joule heating technique had a uniform size of ~15 nm and were firmly embedded on the CNF substrate. The uniform distribution of ME-carbide nanoparticles (e.g., Mo2C) on the substrate was confirmed by X-ray diffraction. In addition to Mo2C, other monometallic carbide nanoparticles such as TiC, ZrC, VC, and NbC were prepared with good material quality as well. High entropy carbide (HEC) nanoparticles (e.g., (TiZrVNbMo)C x ) were prepared in a similar manner to the monocarbides described above, e.g., by loading a mixture of metal salt precursors onto a CNF substrate followed by two-stage Joule heating (e.g., Figure 3B and Figure 4C or Figure 4D).
[0127] Among the selected carbide components, Mo2C showed good performance for hydrogen evolution reaction (HER) and oxygen evolution reaction (OER) processes as a catalytically active component, while the addition of TiC, ZrC, VC, and NbC can increase the entropy to enhance stability. Upon carbonization, uniformly distributed HEC nanoparticles with diameters of ~20 nm were formed on the CNF substrate, as confirmed by transmission electron microscopy (TEM). TEM images also showed HEC nanoparticles embedded within the CNF substrate by an etching mechanism (e.g., when CNFs serve as carbon sources in addition to polymer coating). X-ray diffraction patterns of high entropy oxide (HEO) nanoparticles and HEC nanoparticles were collected and compared to confirm the phase transition. Despite the short synthesis time (e.g., 55 ms), the obtained HEO nanoparticles were highly crystalline. After carbonization, (TiZrVNbMo)O x The nanoparticles are (TiZrVNbMo)C xIt was found that the nanoparticles were completely converted.
[0128] After each Joule heating step, Mo 3d and Zr 3d spectra were collected by X-ray photoelectron spectroscopy (XPS). x The peaks at 229.7, 232.9 and 235.9 eV in MoC correspond to Mo4+, Mo6+ / Mo4+ and Mo6+, respectively. x shows two distinct peaks at 228.8 and 231.9 eV corresponding to Mo2+ and Mo2+ / Mo5+, respectively, due to metal reduction by carbon. Similar results are obtained by XPS for Zr 3d, where the peak at 179.7 eV indicates partial reduction of Zr4+ to Zr2+ during carbonization in the second Joule heating step.
[0129] HER was used as a model reaction to evaluate the stability of the as-prepared HEC nanoparticles as electrocatalysts. Electrochemical tests were performed in 0.5 M H2SO4 with a carbon rod counter electrode and an Ag / AgCl reference electrode. The HEC nanoparticles immobilized on the CNF substrate can be directly used as the working electrode. Linear sweep voltammetry (LSV) curves were performed at a scan rate of 5 mV / s from 0.1 V until the peak appeared, and the potential was corrected to a reversible hydrogen electrode (RHE) at room temperature. The stability was evaluated at a constant potential (e.g., ~10 mA / cm 2 The current density of MoO, MoC, and (TiZrVNbMo)O supported on each CNF substrate was 100 s. x The results of nanoparticles are shown. Among the samples tested, (TiZrVNbMo)C x is 10mA / cm 2 The minimum overpotential was 140 mV at a current density of 100 mV. x , and compared with the single element carbides, single element oxides and HEO counterparts.
[0130] To evaluate the stability of the HEC nanoparticles, chronoamperometry was performed at extended operation times, as shown in Figure 8B. The current density of MoO2 was ∼0 mA / cm2 at 10 h. 2 In contrast, the (TiZrVNbMo)Cx nanoparticles decayed rapidly to about 10 mA / cm 2 The HECs remained stable for 250 h at a current density of 1000 nm. Such excellent stability can be attributed to the covalent bonds of carbides, the high entropy stabilizing effect, and the substrate etching process during synthesis. TEM images of the HECs after long-term HER operation further confirmed the excellent structural stability. The nanoparticles on the CNF substrate remain uniformly dispersed without observable aggregation or desorption even after 250 h of operation.
[0131] MEI nanoparticles To synthesize MEI nanoparticles, carbon substrates were loaded with the desired combination / ratio of metal salt precursors, heated, and the temperature and heating / cooling rates were precisely controlled by adjusting the power applied to the substrate. In particular, MEI nanoparticles were synthesized by Joule heating on carbonized wood substrates. For example, basswood (e.g., size 1.5cmx0.5cmx0.5cm) was treated at 533K in air for 6 hours with a heating rate of 5K / min, and then carbonized by maintaining at 1273K in argon flow for another 6 hours. The resulting substrate was further activated at 1023K in CO2 flow for 6 hours to introduce surface defects.
[0132] Metal salt precursors such as HPtCl, PdCl, HAuCl, FeCl, CoCl, NiCl, CuCl, and SnCl were provided in ethanol (0.05 mol / L). 0.7 Co 0.1 Ni 0.1 Cu 0.1 / Pt1Fe 0.25 Co 0.25 Ni 0.25 Cu 0.25 , and the octogenary Pt 0.8 Pd 0.1 Au 0.1 Fe 0.6 Co 0.1 Ni0.1 Cu 0.1 Sn 0.1 ) were mixed in a stoichiometric ratio and distributed onto the carbon substrate using a micropipette with a loading of ~800 μL / cm. The opposite ends of the carbon substrate were suspended on a glass slide and connected to two copper electrodes using silver paste. The precursor-loaded carbon substrate was then dried in a 353 K oven for 6 h and used directly for the Joule heating method. For example, an adjustable current source was connected to the precursor-loaded carbon substrate in an Ar-filled glove box. Electric pulses with different durations (0.05 s, 0.5 s, 1 min, and 5 min) were applied to the carbon substrate to generate the desired temperatures and heating times (e.g., as shown in Figure 5B) to synthesize MEI nanoparticles.
[0133] First, solid solution (HEA) nanoparticles are synthesized by heating the metal precursors for tens of milliseconds, e.g., at ~1100 K, to mix the different elements without phase separation. Then, the transition from the disordered to the ordered phase is achieved by rapidly reheating the material to ~1100 K for another ~5 min, with a limited amount of time sufficient to complete the desired transition from the disordered HEA structure to an ordered single-phase MEI structure, while simultaneously avoiding nanoparticle growth and / or aggregation. Finally, the material is quenched (~10 4 K / s) preserved the single-phase MEI structure and small grain size (~5 nm).
[0134] To demonstrate the versatility of the proposed synthesis, binary, pentanary, and octanary intermetallic nanoparticles were fabricated and characterized by scanning transmission electron microscopy (STEM), atomic resolution STEM, and energy dispersive X-ray spectroscopy (EDX). PtFe binary and Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1) The pentanary intermetallic nanoparticles exhibited small particle sizes and narrow particle size distributions of 5.4 ± 0.8 nm and 4.4 ± 0.5 nm, respectively. High-angle annular dark-field STEM (HAADF-STEM) images of the binary PtFe nanoparticles show alternating layers of Fe and Pt pillars typical of the L10 intermetallic structure. The ordered L10 structure of the binary PtFe samples was further confirmed by the lattice spacings of 3.71, 2.73 and 2.20 Å in the STEM images, which correspond to the (001), (110) and (111) facets of the ordered L10 structure along the [1-10] direction.
[0135] Similarly, the pentanediate Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) nanoparticles showed alternating dark rows of Fe, Co, Ni, and Cu atoms and bright rows of Pt atoms. Atomic resolution EDX mapping shows that well-defined Pt atoms are in one sublattice, while Fe, Co, Ni, and Cu atoms are uniformly distributed in the other sublattice, both in the L10 structure. According to fitted extended X-ray absorption fine structure (EXAFS), the coordination number of Fe-Pt(6) is much larger than those of Fe-Cu(1.2), Cu-Fe(1.0), Co-Ni(2.0), and Ni-Co(2). These results follow the L10 structure in which Fe-Pt bonds occur in a three-dimensional structure in intermetallic compounds, while Fe-Cu, Cu-Fe, Co-Ni, and Ni-Co bonds in static intermetallic compounds are localized and confined to two-dimensional layer bonds in ordered structures.
[0136] Pentanary MEI nanoparticles can also be synthesized with different element ratios as well as different intermetallic structures, e.g., (Pt 0.8 Au 0.1 Pd 0.1 )3(Fe 0.9 Co 0.1 ) in the L12 phase, demonstrating the potential of this rapid / limited heating method to broaden the range of possible intermetallic materials. 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn0.1 ) nanoparticles were also synthesized, featuring (001), (110), and (111) planes (e.g., as shown in the STEM images in Figures 2D-2F) with spacings of 3.73, 2.76, and 2.34 Å, respectively, and also forming the L10 intermetallic structure. Thus, the disclosed process based on the disorder-order transition allows the synthesis of nanoscale MEIs with multiple elements (e.g., up to 8), as well as different element ratios and various intermetallic structures.
[0137] In contrast, it is very difficult to synthesize nanoscale MEIs without phase separation by conventional methods. 0.8 Pd 0.1 Au 0.1 Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 Nanoparticles were prepared by conventional annealing (e.g., ∼1100 K, 3 h). These octanium nanoparticles were found to form phase-separated heterostructures without the desired atomic ordering according to STEM imaging and XRD. The slow heating / cooling rate of conventional annealing is different from that of MEI nanoparticles (∼5 nm) synthesized by the disclosed technique, which is consistent with the octanium Pt 0.8 Pd 0.1 Au 0.1 Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 Phase separation occurs, resulting in a large particle size and distribution of the nanoparticles (~76.2 ± 4.2 nm). Thus, phase separation can only be avoided by using the disclosed technique, which is made possible, at least in part, by starting the MEI nanoparticles with HEA nanoparticles, whose components are well mixed. The limited heating time of this technique also allows for the transition from disorder to order while preventing particle growth, in order to successfully produce MEI nanoparticles.
[0138] To further investigate the disorder-order phase transition that enables the MEI formation, the pentanediol Pt(Fe0.7 Co 0.1 Ni 0.1 Cu 0.1 Arrays of Pt(Fe) samples were synthesized by heating at ~1100 K for various times. XRD was then performed to characterize their degree of ordering. According to the calculated hypothetical XRD pattern, the diffraction peaks of (001) at 24.2° and (110) at 33.4° are due to Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) are superlattice peaks of the ideal LL10 intermetallic structure. Based on the intensities of these peaks, the LRO parameter, as defined by equation (2) above, can be used to quantify the degree of ordering of different pentane samples. No superlattice diffraction peaks were observed in the sample prepared by only 0.05 s of Joule heating, and the short heating time resulted in a large degree of ordering in the Pt1Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 This suggests that the disordered phase transition of the pentane (Fe) phase cannot be induced. As the heating time increased from 0.5 s to 5 min, the characteristic diffraction peaks of L10, (001) and (110) gradually enhanced. As a result, the LRO increased from 10% (0.5 s) to 60% (1 min) and finally to ∼100% (5 min), as shown in Figure 9A. As shown in Figure 9B, the pentane (Fe) phase 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) Rietveld refinement of the XRD results of the MEI also reveals the formation of a fully ordered L10 intermetallic structure in the sample heated for 5 min, where the elements Co, Ni, Cu, and Fe occupy one sublattice and Pt occupies the other sublattice.
[0139] This disorder-to-order transition process (0.5 s–5 min) was observed in pentogenous Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1This is consistent with STEM imaging of the pentad Pt(Fe) MEI nanoparticles, which indicates that the disordered HEA nanoparticle structure transforms into the MPEI structure over the course of ~5 min of heating. This disordered-to-ordered phase transition to a single-phase MPEI consisting of immiscible elements can only be achieved at the nanoscale. 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) For nanoparticles, a fully ordered L10 structure (LRO = 100%) was obtained for particles between 4 and 5 nm. However, for larger particles, the LRO decreases with particle size, regardless of the particle synthesis method (as shown in Figure 5D). As the particle size increases above about 60 nm, the particles exhibit disordered or other phase-separated heterostructures, as confirmed by STEM and EDX.
[0140] Monte Carlo (MC) simulations of nanoparticles of different sizes were performed to track the LRO change as a function of the MC stage (corresponding to the reaction time) at 1100 K to further understand the transition at the nanoscale. The LRO of particles with diameters of 3.1 and 4.6 nm increased with the MC stage, increasing by 3x10 7 Both particles completed the disorder-order phase transition at this point in the simulation, reaching ~100% within the step. However, for the 7.7 nm particle size, the 3x10 7 Only a partial disorder-order transition (LRO = 40%) can be achieved after 100 simulation steps. The largest particle simulated was 10.8 nm and showed an even lower LRO of 5% after the same number of MC simulation steps. These findings are consistent with experimental observations using XRD (e.g., Figure 5C) and STEM, where the complete disorder-order phase transition is achieved and stabilized mainly in ultrasmall nanoparticles (<5 nm).
[0141] Without being bound to any particular theory, the size effect on the disorder-order transition may be due to the difference in surface energy. For example, the MEI may have a lower surface energy than the HEA because the MEI forms stronger atom-atom interactions. Due to the large relative surface area of the small nanoparticles, the difference in surface energy between the MEI and the small nanoparticles (~5 nm) of the HEA may play a significant role in driving the disorder-to-order transition. It is also possible that larger particles (e.g., 10-20 nm) need to overcome a higher energy barrier to complete the disorder-order transition. For particles significantly larger than 5 nm (e.g., 150 nm), such a large energy barrier may prevent the formation of a fully ordered MEI. The disorder-order transition may be thermodynamically favored to form phase-stable MEI nanoparticles. The lower enthalpy of MEI nanoparticles with a size of 4-5 nm was verified by performing high-temperature oxide melt drop calorimetry on pentanary and octanary MEI and their corresponding disordered HEA starting materials. Calorimetric measurements show that the enthalpy change from the pentane HEA to the MEI is 0.7 Co 0.1 Ni 0.1 Cu 0.1 ) per equation, and the enthalpy change from the octanium HEA to the MEI is (Pt 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 ) per formula, indicating that the ordered MEI is thermodynamically favorable.
[0142] Pentanary Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1)The MC modeling of the atomic arrangement of the nanoparticles further simulated the transition from the disordered phase to the ordered phase. This indicated that, similar to the transition process of other intermetallic compounds, the atoms of the disordered HEA starting material diffused to form the ordered MEI. During the transition, driven by strong interactions via spin-orbit coupling and hybridization between the non-noble metal 3d and noble metal 5d states, the formation enthalpy (ΔHf) of the quinary MEI substantially decreased. According to the MC modeling, the decreased enthalpy led to a lower Gibbs free energy of the MEI (Go) than that of the HEA (Gd) sample (based on the same quinary composition PtFe 0.7 Co 0.1 Ni 0.1 Cu 0.1 over a wide temperature range (~273 - 1500K). At temperatures below 1500K (and above the decomposition temperature of the metal salt), the low enthalpy of the MEI dominated the Gibbs free energy, and thus Go < Gd. Therefore, at the synthesis temperature (~1100K), the transition from disorder to order is thermodynamically favorable (ΔGd→o = Go - Gd < 0), and at room temperature, the ordered MEI is the thermodynamically stable phase.
[0143] Upon completion of the transition from disorder to order, the ultrasmall MEI nanoparticles can exhibit excellent phase stability, as demonstrated by in situ heating of the static Pt(Fe 0.7 Co 0.1 Ni 0.1 Cu 0.1 )MEI nanoparticles and simultaneously monitoring their phase evolution by STEM. The quinary MEI nanoparticles synthesized by Joule heating showed a completely ordered structure even after heating at about 1100K for 13 minutes. The nanoparticles were maintained at ~1100K for an additional 47 minutes, but no phase change was observed, thereby indicating the thermal stability of the MEI nanoparticles. In contrast, the binary PtFe nanoparticles (~5nm) at about 1100K showed an ordered intermetallic structure (14 minutes), but gradually converted to a disordered alloy (60 minutes), indicating the excellent thermal stability of the MEI compared to the binary intermetallic compound.
[0144] For use as an electrocatalyst for ethanol oxidation (EOR), (Pt 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 ) octanium MEI nanoparticles were fabricated on a Ketjenblack carbon support (Figure S22). EOR is a key reaction in direct alcohol fuel cells, such as the fuel cell 900 of Figure 9F. In particular, the fuel cell 900 includes an anode 902 having a gas diffusion layer 904 thereon, a cathode 910, and a proton exchange membrane (PEM) 908 disposed between the anode 902 and the cathode 910. The PEM 908 can further include a catalyst layer 906 that includes, for example, a catalytic structure of octanium MEI nanoparticles. Ethanol is oxidized at the anode 902 via an inlet stream 912 on the anode side of the PEM 908 to form an outlet stream 914 of CO2. Concurrently, it is reduced at the cathode 910 via an inlet stream 916 on the cathode side of the PEM 908 to form an outlet stream 918 of HO. The protons are transported through the PEM 908 while the electrons are transported through an external circuit (not shown) from the anode 902 to the cathode 910, thereby providing power to a load.
[0145] However, EOR requires efficient catalysts with high surface area, tunable composition, and good stability, characteristics of which have been demonstrated in the development of octanium MEI nanoparticles ((Pt 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 )) can be used. FIG. 9G shows 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.19G shows the EOR constant voltage (CV) curves obtained for MEI nanoparticles, binary PtFe intermetallic nanoparticles, and a commercial Pt / C catalyst tested in 1 M KOH and 1 M EtOH. As shown by Figure 9G, the MEI nanoparticles exhibit improved EOR activity that is 8-fold and 12-fold higher than the binary PtFe intermetallic compound and the commercial Pt / C catalyst, respectively. Furthermore, the octanary MEI nanoparticles demonstrate superior durability during long-term catalytic operation, which can be attributed to the multi-element composition, ordered intermetallic structure, and nanosize of the materials.
[0146] Further additional examples of the disclosed technology In view of the above implementations of the disclosed subject matter, the present application discloses additional examples in the appended clauses listed below. It should be noted that any feature of the appended clause alone, or two or more features of the appended clauses listed in combination, and optionally combined with one or more features of one or more additional appended clauses, are also included within the scope of the disclosure of the present application.
[0147] Appendix 1. A structure comprising one or more multi-element compound (MEC) nanoparticles, A nanoparticle structure, wherein each MEC nanoparticle has a plurality of sites comprising one or more elements, each site forming a compound bond with at least one other site of the compound nanoparticle, one or more of the compound bonds comprising a covalent bond, an ionic bond, a metallic bond, or any combination of the foregoing, and each MEC nanoparticle is formed from at least three different elements.
[0148] Appendix 2. A structure as described in any section or example herein, particularly in Appendix 1, The structure, wherein each MEC nanoparticle has a maximum cross-sectional dimension of 25 nm or less.
[0149] Appendix 3. A structure according to any of the sections or examples herein, In particular, the one or more MEC nanoparticles comprise multi-element oxide nanoparticles, multi-element carbide nanoparticles, multi-element intermetallic nanoparticles, multi-element nitride nanoparticles, multi-element amorphous glass nanoparticles, multi-element diboride nanoparticles, multi-element phosphide nanoparticles, multi-element sulfide nanoparticles, multi-element chalcogenide nanoparticles, multi-element silicide nanoparticles, or any combination of the foregoing.
[0150] Appendix 4. A structure as described in any of the sections or examples herein, in particular any one of Appendices 1 to 3, A structure further comprising a substrate, the substrate having one or more MEC nanoparticles formed on one or more surfaces of the substrate, one or more MEC nanoparticles bonded to one or more surfaces of the substrate, or both.
[0151] Appendix 5. The structure of any clause or example in this specification, particularly in Appendix 4, The structure, wherein the substrate comprises carbon nanofibers (CNF), carbon nanotubes (CNT), mesoporous carbon molecular sieves (CMK), carbon paper, carbon felt, carbon black powder or carbon particles, graphite powder or graphite particles, graphene, carbonized wood, semiconductors, textiles, metals, dielectrics, oxides, or any combination thereof.
[0152] Appendix 6. A structure as described in any section or example herein, in particular any one of Appendices 1 to 5, A structure in which at least one of the one or more MEC nanoparticles comprises a multi-element oxide (MEO) nanoparticle, the MEO nanoparticle comprising oxygen and at least three cations in a single homogeneous phase.
[0153] Appendix 7. A structure as described in any section or example herein, particularly in Appendix 6, A structure in which the MEO nanoparticles contain more than five cations in a single homogeneous phase.
[0154] Appendix 8. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 6-7, The MEO nanoparticles have a crystal structure selected from the group consisting of rock salt, spinel, rutile, fluorite, tungsten bronze, and perovskite.
[0155] Appendix 9. A structure according to any of the sections or examples of this specification, particularly any one of Appendices 6 to 8, The at least three cations forming the MEO nanoparticles are selected from the group consisting of Ba, Ca, Ce, Co, Cr, Cu, Dy, Er, Eu, Fe, Gd, Hf, Ir, K, La, Li, Mg, Mn, Mo, Na, Nb, Nd, Ni, Pb, Pd, Pr, Sm, Sn, Sr, Ta, Ti, V, Y, Zn, and Zr.
[0156] Appendix 10. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 6 to 9, The structure, wherein the at least three cations include at least one transition metal and at least one noble metal.
[0157] Appendix 11. A structure according to any of the sections or examples of this specification, particularly any one of Appendices 6 to 10, The MEO nanoparticles contain Pd.
[0158] Appendix 12. A structure according to any of the sections or examples of this specification, particularly any one of Appendices 6 to 11, MEO nanoparticles are (Zr, Ce) 0.6 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.3 Pd 0.1 O 2-x where x represents an oxygen vacancy.
[0159] Appendix 13. A structure according to any of the sections or examples of this specification, particularly any one of Appendices 6 to 11, The nanoparticles are (Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O 2-x where x represents an oxygen vacancy.
[0160] Appendix 14. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 6 to 13, The structure in which the MEO nanoparticles have a coordination entropy of 13.5 J / mol / K or more.
[0161] Appendix 15. A structure as described in any of the sections or examples herein, particularly any one of Appendices 6 to 14, The structure further includes a coating formed on the MEO nanoparticles and surrounding at least a portion of the MEO nanoparticles.
[0162] Appendix 16. A structure as described in any of the sections or examples herein, particularly in Appendix 15, The coating comprises a polymer containing C, O, and H.
[0163] Appendix 17. A structure according to any of the sections or examples of this specification, particularly any one of Appendices 15-16, A structure wherein the coating comprises polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyvinylidene difluoride (PVDF), polytetrafluoroethylene (PTFE), or any combination of the foregoing.
[0164] Appendix 18. A structure as described in any of the sections or examples herein, in particular any one of Appendices 1 to 17, A structure in which at least one of the one or more MEC nanoparticles comprises a multi-element intermetallic (MEI) nanoparticle, the MEI nanoparticle comprising at least three metallic elements in a single phase.
[0165] Appendix 19. A structure as described in any section or example herein, particularly in Appendix 18, The structure, in which the MEI nanoparticles have a maximum cross-sectional dimension of about 4-6 nm.
[0166] Appendix 20. A structure according to any of the sections or examples of this specification, in particular any one of Appendices 18-19, A structure in which the MEI nanoparticles have a first and a second sublattice, one of the at least three metal elements being distributed in the first sublattice and another of the at least three metal elements being distributed in the second sublattice.
[0167] Appendix 21. A structure as described in any of the sections or examples herein, particularly in Appendix 20, A structure in which the first sublattice has a random distribution of precious metal atoms and the second sublattice has a random distribution of non-precious metal atoms.
[0168] Appendix 22. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 18 to 21, A structure in which the MEI nanoparticles have a geometrically close-packed phase or a topologically close-packed phase.
[0169] Appendix 23. A structure as described in any section or example herein, particularly in Appendix 22, A structure in which the geometrically closed-packed phase comprises an L10, L11, L12, or B2 lattice structure, and the topologically closed-packed phase comprises a Laves phase, a σ phase, or a μ phase.
[0170] Appendix 24. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 18 to 23, The MEI nanoparticles contain more than five metal elements, the structure.
[0171] Appendix 25. A structure as described in any of the sections or examples herein, particularly any one of appendices 18 to 24, The MEI nanoparticles are (Pt 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 ) structure.
[0172] Appendix 26. A structure as described in any of the sections or examples herein, in particular any one of Appendices 18 to 25, The structure in which the MEI nanoparticles exhibit at least 90% long-term ordering (LRO).
[0173] Appendix 27. A structure according to any of the sections or examples of this specification, particularly any one of Appendices 18 to 26, The MEI nanoparticles exhibit an LRO of approximately 100%.
[0174] Appendix 28. A structure as described in any of the sections or examples herein, in particular any one of Appendices 1 to 27, A structure wherein at least one of the one or more MEC nanoparticles comprises a multi-element carbide nanoparticle, the multi-element carbide nanoparticle comprising carbon and at least three metallic elements in a single homogenous phase.
[0175] Appendix 29. A structure as described in any section or example herein, particularly in Appendix 28, A structure in which multi-element carbide nanoparticles contain more than five metallic elements in a single homogeneous phase.
[0176] Appendix 30. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 28-29, The at least three metal elements forming the multi-element carbide nanoparticles are selected from the group consisting of Ba, Ca, Ce, Co, Cr, Cu, Dy, Er, Eu, Fe, Gd, Hf, Ir, K, La, Li, Mg, Mn, Mo, Na, Nb, Nd, Ni, Pb, Pd, Pr, Sm, Sn, Sr, Ta, Ti, V, Y, Zn, and Zr.
[0177] Appendix 31. A structure as described in any of the sections or examples of this specification, particularly any one of Appendices 28 to 30, Multi-element carbide nanoparticles are (TiZrVNbMo)C x . That is the structure.
[0178] Appendix 32. A structure as described in any of the sections or examples herein, in particular any one of Appendices 1 to 31, A structure constructed for use as a catalyst in a thermochemical or electrochemical reaction.
[0179] Appendix 33. (a) providing a substrate having a plurality of metal salt precursors thereon, at least one of the metal salt precursors comprising O, and the plurality of metal salt precursors comprising at least three different metal elements; (b) The substrate is cooled for at least 10 4 heating at a first heating rate of 10 K / s to a first temperature; (c) maintaining the substrate at a first temperature for a first period of time; (d) at the end of the first period, the substrate is cooled to at least 10° C. from the first temperature. 5 cooling at a first cooling rate of 10 K / s to a second temperature; the initial temperature and the second temperature are less than 500 K; (b) heating, (c) maintaining, and (d) cooling convert the metal salt precursor on the substrate into one or more multi-element oxide (MEO) nanoparticles, each MEO nanoparticle comprising oxygen and at least three metal elements in a single homogenous phase.
[0180] Appendix 34. The method according to any of the clauses or examples herein, particularly appendix 33, comprising: The method, wherein the initial temperature, the second temperature, or both, are about 290-300K.
[0181] Appendix 35. The method according to any of the clauses or examples of this specification, particularly any one of appendices 33 to 34, comprising: The method, wherein the first temperature is in the range of 1400K to 1600K, and the first time period is about 50 to 55 ms.
[0182] Appendix 36. The method according to any of the clauses or examples of this specification, particularly any one of appendices 33 to 34, comprising: The method, wherein the first temperature is in the range of 1200K to 1400K, inclusive, and the first period of time is about 200 ms.
[0183] Appendix 37. A method as described in any of the sections or examples herein, particularly any one of appendices 33 to 36, comprising: The method, wherein the heating of (b), the maintaining of (c), and the cooling of (d) are carried out in an atmosphere of a noble gas and / or atmosphere.
[0184] Appendix 38. A method as described in any section or example herein, particularly in Appendix 37, comprising: The method wherein the noble gas comprises Ar.
[0185] Appendix 39. The method according to any of the clauses or examples herein, particularly any one of appendices 33 to 38, comprising: the plurality of metal salt precursors comprises Ni, Cu, or Fe; The method, wherein the heating (b), the maintaining (c), and the cooling (d) are performed in an atmosphere having an oxygen partial pressure.
[0186] Appendix 40. A method as described in any of the clauses or examples herein, particularly in Appendix 39, comprising: A method wherein the atmosphere comprises ambient air, and / or the atmosphere comprises at least 15% O by volume (e.g., ∼20.95% by volume), and / or the atmosphere has an oxygen partial pressure of at least 150 mbar (e.g., ∼212.3 mbar).
[0187] Appendix 41. The method according to any of the sections or examples of this specification, particularly any one of appendices 33 to 40, The method of claim 1, wherein the at least three metallic elements are selected from the group consisting of Ba, Ca, Ce, Co, Cr, Cu, Dy, Er, Eu, Fe, Gd, Hf, Ir, K, La, Li, Mg, Mn, Mo, Na, Nb, Nd, Ni, Pb, Pd, Pr, Sm, Sn, Sr, Ta, Ti, V, Y, Zn, and Zr.
[0188] Appendix 42. A method as described in any of the sections or examples herein, particularly any one of appendices 33 to 41, comprising: The method, wherein the multiple metal salt precursor comprises ten different metal elements, at least one of which is a noble metal.
[0189] Appendix 43. A method as described in any of the clauses or examples herein, particularly in Appendix 42, comprising: The method wherein the noble metal is Pd.
[0190] Appendix 44. A method as described in any of the clauses or examples herein, particularly any one of appendices 33 to 43, comprising: MEO nanoparticles are (Zr,Ce) 0.6 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.3 Pd 0.1 O2-x where x represents an oxygen vacancy.
[0191] Appendix 45. A method as described in any of the clauses or examples herein, particularly any one of appendices 33 to 43, comprising: MEO nanoparticles are (Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O 2-x wherein x represents an oxygen vacancy.
[0192] Appendix 46. A method according to any of the clauses or examples herein, particularly any one of 33 to 45, comprising The method, wherein the substrate comprises carbon nanofibers (CNF), carbon nanotubes (CNT), mesoporous carbon molecular sieves (CMK), carbon paper, carbon felt, carbon black powder or particles, graphite powder or particles, graphene, carbonized wood, semiconductors, textiles, metals, dielectrics, oxides, or any combination of the foregoing.
[0193] Appendix 47. A method as described in any of the sections or examples herein, particularly any one of appendices 33 to 46, comprising: The method, wherein the heating comprises direct joule heating, conductive heating, radiative heating, microwave heating, laser heating, plasma heating, or any combination of the foregoing.
[0194] Appendix 48. A method as described in any of the sections or examples herein, particularly any one of appendices 33 to 47, comprising: The method, wherein the cooling comprises: (i) passive cooling by radiation, conduction, or both; (ii) active cooling by conduction, convection, or both; (iii) active cooling by phase or chemical transitions induced by heat absorption; or (iv) any combination of (i), (ii), and (iii).
[0195] Appendix 49. A method as described in any of the sections or examples herein, particularly any one of appendices 33 to 48, comprising: (d) After cooling, (e) providing a coating on the one or more MEO nanoparticles and at least partially surrounding the one or more MEO nanoparticles; (f) heating the substrate from the third temperature to a fourth temperature at a second heating rate slower than the first heating rate; (g) maintaining the substrate at a fourth temperature for a second period of time; (h) at least 10% below the fourth temperature at the end of the second period; 5 cooling the substrate from the fourth temperature to a fifth temperature at a second cooling rate of 10 K / s; Including, the third temperature and the fifth temperature are less than 500 K; The method, wherein (f) heating, (g) maintaining, and (h) cooling convert the one or more MEO nanoparticles and coating into one or more multi-element carbide nanoparticles, each multi-element carbide nanoparticle comprising carbon and at least three metallic elements in a single homogenous phase.
[0196] Note 50. A method as described in any of the sections or examples herein, particularly any one of appendices 33 to 48, comprising: (d) After cooling, (e) providing a coating on the one or more MEO nanoparticles and at least partially surrounding the one or more MEO nanoparticles; (f) The substrate is dried for at least 10 4 heating from the third temperature to a fourth temperature at a third heating rate of 10 K / s; (g) maintaining the substrate at a fourth temperature for a period of time; (h) at the end of that period, at least 10 5 cooling the substrate from the fourth temperature to a fifth temperature at a second cooling rate of 100 K / s; and (i) repeating the heating (f), maintaining (g), and cooling (h) one or more times to define a second period of time; Including, the third temperature and the fifth temperature are less than 500 K; The method, wherein by repeating (f) heating, (g) maintaining, (h) cooling, and (i), the one or more MEO nanoparticles and coatings are converted into one or more multi-element carbide nanoparticles, each multi-element carbide nanoparticle comprising carbon and at least three metallic elements in a single homogenous phase.
[0197] Note 51. The method according to any of the clauses or examples of this specification, particularly any one of appendices 49 to 50, comprising: The method, wherein the third temperature, the fifth temperature, or both, are about 290-300K.
[0198] Appendix 52. The method according to any of the clauses or examples herein, particularly any one of appendices 49 to 51, comprising: The method, wherein the fourth temperature is at least 200K higher than the first temperature and the second time period is at least 100 times higher than the first time period.
[0199] Note 53. A method as described in any of the clauses or examples herein, particularly any one of appendices 49 to 52, comprising: The method wherein the fourth temperature is about 2000K and the second period of time is about 60 seconds.
[0200] Note 54. The method according to any of the clauses or examples herein, particularly any one of appendices 49 to 53, comprising: The method of claim 1, wherein the coating comprises a polymer containing C, O, and H.
[0201] Note 55. A method as described in any of the clauses or examples herein, particularly any one of appendices 49 to 54, comprising: The method, wherein the coating comprises polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyvinylidene difluoride (PVDF), polytetrafluoroethylene (PTFE), or any combination of the foregoing.
[0202] Note 56. (a) providing a substrate having one or more high entropy alloy (HEA) nanoparticles thereon, each HEA nanoparticle comprising at least five different metal elements; (b) At least 10 4 heating the substrate to a first temperature at a first heating rate of 10 K / s; (c) maintaining the substrate at a first temperature for a first period of time; (d) at the end of the first period, removing the substrate from the first temperature by at least 10 5 cooling at a first cooling rate of 10 K / s to a second temperature; the second temperature is less than 500 K; the first temperature is greater than 1000K and the first time period is in the range of 1 minute to 10 minutes; The method, wherein (b) heating, (c) maintaining, and (d) cooling convert the one or more HEA nanoparticles into one or more multi-element intermetallic (MEI) nanoparticles, each MEI nanoparticle comprising at least five metallic elements in a single phase.
[0203] Note 57. The method according to any of the clauses or examples herein, particularly appendix 56, comprising: (a) The provision of (a1) providing a plurality of metal salt precursors on a substrate, the plurality of metal salt precursors comprising at least five different metal elements; (a2) At least 10 4 heating the substrate from the initial temperature to a third temperature at a second heating rate of 10 K / s; (a3) maintaining the substrate at a third temperature for a second period of time; (a4) At least 10 5 cooling the substrate from the third temperature to a fourth temperature at a second cooling rate of 10 K / s; Including, the initial temperature and the fourth temperature are less than 500 K; The third temperature is greater than 1000K, and the second time period is between 10 ms and 100 ms; The method, wherein (a2) heating, (a3) maintaining, and (a4) cooling convert the metal salt precursor on the substrate into one or more HEA nanoparticles.
[0204] Note 58. The method of any appendix or example herein, in particular the method of appendix 57, comprising: The method, wherein one, some, or all of the initial temperature, second temperature, and fourth temperature are about 290-300K.
[0205] Note 59. The method according to any of the clauses or examples herein, particularly any one of appendices 57-58, comprising: The method wherein the third temperature is about 1100K and the second time period is about 50-55 ms.
[0206] Note 60. (a) providing a substrate having one or more disordered nanoparticles thereon, the one or more disordered nanoparticles comprising at least three different metal elements and having a long term ordering (LRO) of less than 50%; (b) At least 10 4 heating the substrate to a first temperature at a first heating rate of 10 K / s; (c) maintaining the substrate at a first temperature for a first period of time; (d) at the end of the first period, the substrate is cooled to at least 10° C. from the first temperature. 5 cooling at a first cooling rate of 10 K / s to a second temperature; the second temperature is less than 500 K; the first temperature is greater than 1000K and the first time period is in the range of 1 minute to 10 minutes; The method, wherein (b) heating, (c) maintaining, and (d) cooling convert the one or more disordered nanoparticles into one or more multi-element intermetallic (MEI) nanoparticles, each MEI nanoparticle comprising at least three metallic elements in a single phase.
[0207] Appendix 61. The method according to any of the clauses or examples herein, particularly appendix 60, comprising: (a) The provision of (a1) providing a plurality of metal salt precursors on a substrate, the plurality of metal salt precursors comprising at least three different metal elements; (a2) At least 10 4 heating the substrate from the initial temperature to a third temperature at a second heating rate of 10 K / s; (a3) maintaining the substrate at a third temperature for a second period of time; (a4) At least 10 5 cooling the substrate from the third temperature to a fourth temperature at a second cooling rate of 10 K / s; Including, the initial temperature and the fourth temperature are less than 500 K; The third temperature is greater than 1000K, and the second time period is between 10 ms and 100 ms; The method, wherein (a2) heating, (a3) maintaining, and (a4) cooling convert the metal salt precursor on the substrate into one or more disordered nanoparticles.
[0208] Appendix 62. The method of any section or example herein, in particular the method of appendix 61, comprising: The method, wherein one, some, or all of the initial temperature, second temperature, and fourth temperature are about 290-300K.
[0209] Appendix 63. The method according to any of the clauses or examples of this specification, particularly any one of appendices 61 to 62, comprising: The method wherein the third temperature is about 1100K and the second time period is about 50-55 ms.
[0210] Note 64. A method as described in any of the sections or examples herein, in particular any one of appendices 56 to 63, comprising: The method, wherein the first temperature is about 1100K and the first time period is about 5 minutes.
[0211] Note 65. The method according to any of the clauses or examples herein, particularly any one of appendices 56 to 64, comprising: The method, wherein each MEI nanoparticle has a geometrically close-packed phase or a topologically close-packed phase.
[0212] Note 66. The method according to any of the clauses or examples herein, particularly appendix 65, comprising: The method, wherein the geometrically closed packed phase comprises a L10, L11, L12, or B2 lattice structure, and the topologically closed packed phase comprises a Laves phase, a σ phase, or a μ phase.
[0213] Note 67. A method as described in any of the clauses or examples herein, particularly any one of appendices 56 to 66, comprising: A method, wherein the one or more MEI nanoparticles comprise more than six metal elements, more than seven metal elements, or more than eight metal elements.
[0214] Note 68. The method according to any of the clauses or examples herein, particularly any one of appendices 56 to 67, comprising: Each MEI nanoparticle is (Pt 0.8 Pd 0.1 Au 0.1 )(Fe 0.6 Co 0.1 Ni 0.1 Cu 0.1 Sn 0.1 ) an octanium nanoparticle having a compound of
[0215] Note 69. The method according to any of the clauses or examples herein, in particular any one of appendices 56 to 68, comprising: A method, wherein each MEI nanoparticle exhibits at least 90% long-term ordering (LRO).
[0216] Appendix 70. The method according to any of the clauses or examples herein, in particular any one of appendices 56 to 69, comprising: The method wherein each MEI nanoparticle exhibits an LRO of about 100%.
[0217] Appendix 71. A system for producing multi-element compound nanoparticles according to any of the sections or examples of this specification, particularly any one of appendices 1 to 32, comprising: The system includes a pulsed or semi-continuous heating mechanism.
[0218] Appendix 72. A system as described in any of the clauses or examples herein, in particular in appendix 71, comprising: A system in which the pulsed or semi-continuous heating mechanism comprises one or more of a direct joule heater, a conductive heater, a radiative heater, a microwave heater, a laser, a plasma, or any combination of the foregoing, or any other means for heating.
[0219] Appendix 73. A system according to any of the clauses or examples of this specification, in particular any one of appendices 71-72, comprising: The system further comprises a rapid cooling mechanism.
[0220] Note 74. A system as described in any of the clauses or examples herein, particularly in appendix 73, comprising: A system wherein the rapid cooling mechanism includes: (i) passive cooling by radiation, conduction, or both; (ii) active cooling by conduction, convection, or both; (iii) active cooling by endothermic induced phase or chemical transitions; (iv) any other means for rapid cooling; or (v) any combination of (i), (ii), (iii), and (iv).
[0221] Appendix 75. A system according to any of the clauses or examples of this specification, in particular any one of appendices 71 to 74, comprising: The apparatus further comprises a controller operably coupled to and configured to control the pulse heating mechanism and / or the rapid cooling mechanism.
[0222] Appendix 76. A system as described in any clause or example herein, particularly in appendix 75, comprising: A system in which a controller comprises one or more processors and a computer-readable storage medium.
[0223] Appendix 77. A system according to any of the clauses or examples of this specification, particularly appendix 76, comprising: A computer-readable storage medium stores instructions that, when executed by one or more processors, cause a controller to perform one or more aspects of the methods described in any section or example herein, particularly any one of appendices 33-70, and / or issue control signals.
[0224] conclusion For example, any of the features shown or described herein with respect to Figures 1B-1E, 2B-2G, 3-7D, and 8A-9G and Appendices 1-77 can be combined with any other features shown or described herein with respect to Figures 1B-1E, 2B-2G, 3-7D, and 8A-9G and Appendices 1-77 to provide materials, structures, methods, and embodiments not otherwise shown or specifically described herein. All features described herein are independent of one another and can be used in combination with any other feature described herein, unless structurally impossible.
[0225] In view of the many possible embodiments to which the principles of the disclosed technology may be applied, it should be recognized that the illustrated embodiments are examples only and should not be construed as limiting the scope of the disclosed technology. Rather, the scope is defined by the following claims. We therefore claim all that comes within the scope and spirit of those claims.
Claims
1. 1. A structure comprising one or more multi-element compound (MEC) nanoparticles, each MEC nanoparticle has a plurality of sites containing one or more elements, each site forming a compound bond with at least one other site of the compound nanoparticle; one or more of the compound bonds comprises a covalent bond, an ionic bond, a metallic bond, or any combination of the foregoing; Each MEC nanoparticle is formed from at least three different elements, the structure.
2. The structure of claim 1 , further comprising a substrate, the substrate having one or more MEC nanoparticles formed on one or more surfaces of the substrate, one or more MEC nanoparticles bonded to one or more surfaces of the substrate, or both.
3. 3. The structure of claim 2, wherein the substrate comprises carbon nanofibers (CNF), carbon nanotubes (CNT), mesoporous carbon molecular sieves (CMK), carbon paper, carbon felt, carbon black powder or particles, graphite powder or particles, graphene, carbonized wood, semiconductors, textiles, metals, dielectrics, oxides, or any combination thereof.
4. 2. The structure of claim 1, wherein at least one of the one or more MEC nanoparticles comprises a multi-element oxide (MEO) nanoparticle, the MEO nanoparticle comprising oxygen and at least three cations in a single homogeneous phase.
5. 5. The structure of claim 4, wherein the at least three cations forming the MEO nanoparticles are Ba, Ca, Ce, Co, Cr, Cu, Dy, Er, Eu, Fe, Gd, Hf, Ir, K, La, Li, Mg, Mn, Mo, Na, Nb, Nd, Ni, Pb, Pd, Pr, Sm, Sn, Sr, Ta, Ti, V, Y, Zn, and Zr.
6. 5. The structure of claim 4, wherein the at least three cations include at least one transition metal and at least one noble metal.
7. The MEO nanoparticles are (Zr, Ce) 0.6 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.3 Pd 0.1 O 2-x 7. The structure of claim 6, wherein the oxide is a 10-nary oxide having the formula:
8. The MEO nanoparticles are (Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O 2-x 5. The structure of claim 4, wherein the oxide is a 10-nary oxide having the formula:
9. The structure of claim 4 , further comprising a coating formed on and surrounding at least a portion of said MEO nanoparticles.
10. 10. The structure of claim 9, wherein the coating comprises a polymer containing C, O and H.
11. 10. The structure of claim 1, wherein at least one of the one or more MEC nanoparticles comprises a multi-element intermetallic (MEI) nanoparticle, the MEI nanoparticle comprising at least three metallic elements in a single phase.
12. 10. The structure of claim 1, wherein at least one of the one or more MEC nanoparticles comprises a multi-element carbide nanoparticle, the multi-element carbide nanoparticle comprising carbon and at least three metallic elements in a single homogenous phase.
13. (a) providing a substrate having a plurality of metal salt precursors thereon, at least one of the metal salt precursors comprising O, and the plurality of metal salt precursors comprising at least three different metal elements; (b) cooling the substrate for at least 10 minutes from the initial temperature. 4 heating at a first heating rate of 10 K / s to a first temperature; (c) maintaining the substrate at the first temperature for a first period of time; (d) at the end of the first time, removing the substrate from the first temperature by at least 10 5 cooling at a first cooling rate of 100 K / s to a second temperature; the initial temperature and the second temperature are less than 500 K; (b) heating, (c) maintaining, and (d) cooling convert the metal salt precursor on the substrate into one or more multi-element oxide (MEO) nanoparticles, each MEO nanoparticle comprising O and at least three metal elements in a single homogenous phase.
14. 14. The method of claim 13, wherein the first temperature is in the range of 1400K to 1600K, and the first time period is about 50 to 55 ms.
15. 14. The method of claim 13, wherein the plurality of metal salt precursors comprises Ni, Cu, or Fe, and the heating of (b), the maintaining of (c), and the cooling of (d) are performed in an atmosphere having a partial pressure of oxygen.
16. 14. The method of claim 13, wherein the multiple metal salt precursors include ten different metal elements, at least one of which is a noble metal.
17. The MEO nanoparticles are (Zr, Ce) 0.6 (Mg, La, Y, Hf, Ti, Cr, Mn) 0.3 Pd 0.1 O 2-x 17. The method of claim 16, wherein the oxide is a 10-nary oxide having the formula:
18. The MEO nanoparticles are (Zr, Ce, Hf, Ti, La, Y, Gd, Ca, Mg, Mn)O 2-x 14. The method of claim 13, wherein the oxide is a 10-nary oxide having the formula:
19. 14. The method of claim 13, further comprising, after cooling in (d), (e) providing a coating on and at least partially surrounding the one or more MEO nanoparticles; (f) heating the substrate from the third temperature to a fourth temperature at a second heating rate slower than the first heating rate; (g) maintaining the substrate at the fourth temperature for a second period of time; (h) at least 10% below the fourth temperature at the end of the second period of time; 5 cooling the substrate from the fourth temperature to a fifth temperature at a second cooling rate of 100 K / s; Including, the third temperature and the fifth temperature are less than 500 K; The heating in (f), maintaining in (g), and cooling in (h) convert the one or more MEO nanoparticles and coating into one or more multi-element carbide nanoparticles, each multi-element carbide nanoparticle comprising carbon and at least three metallic elements in a single homogenous phase.
20. 14. The method of claim 13, further comprising after cooling in (d): (e) providing a coating on and at least partially surrounding the one or more MEO nanoparticles; (f) removing the substrate by at least 10 4 heating from the third temperature to a fourth temperature at a third heating rate of 100 K / s; (g) maintaining the substrate at a fourth temperature for a period of time; (h) at least 10 5 cooling the substrate from the fourth temperature to a fifth temperature at a second cooling rate of 100 K / s; (i) repeating the heating of (f), the maintaining of (g), and the cooling of (h) one or more times to define a second period of time; Including, the third temperature and the fifth temperature are less than 500 K; Repeating the heating of (f), maintaining of (g), cooling of (h), and (i) converts the one or more MEO nanoparticles and coatings into one or more multi-element carbide nanoparticles, each multi-element carbide nanoparticle comprising carbon and at least three metallic elements in a single homogenous phase.