How Lithium Batteries Work

By adjusting charging and discharging temperatures, the method enhances the cycling stability of LMP batteries, addressing issues of low ionic conductivity and mechanical stability, thereby improving their durability for electric vehicles and intermittent power storage.

JP2024536045APending Publication Date: 2024-10-04BLUE SOLUTIONS
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024518241
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-06
Filing Date
2022-10-05
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Lithium metal polymer (LMP) batteries face challenges with low ionic conductivity at room temperature and poor mechanical stability, leading to insufficient cycling stability, which is critical for applications in electric vehicles and intermittent power storage.

Method used

The method involves varying the charging and discharging temperatures to maintain ionic conductivity and mechanical properties, with a charging temperature strictly higher than the discharging temperature, enhancing cycling resistance.

Benefits of technology

This approach improves the cycling durability of LMP batteries by maintaining ionic conductivity and mechanical stability, enabling them to operate over a large number of cycles effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536045000001_ABST
    Figure 2024536045000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for operating a lithium battery selected from solid or quasi-solid electrolyte lithium batteries, comprising at least one positive electrode, at least one solid or quasi-solid electrolyte and at least one negative electrode, characterized in that by adjusting the charging and discharging temperatures a battery with improved performance in terms of cycle characteristics is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of lithium batteries, more particularly solid or quasi-solid electrolyte lithium batteries, in particular Lithium Metal Polymer (LMP) batteries, in particular those used in the manufacture of electric vehicles and / or for storing intermittent electricity such as wind and / or solar power. [Background technology]

[0002] The present invention more particularly relates to a method of operating a lithium battery in which the charge and discharge temperatures are adjusted to yield a battery with improved performance in terms of cycle durability.

[0003] Currently available lithium metal polymer batteries (or LMPs) are generally "all solid-state" batteries in the form of a thin film wound many times or a thin film stacked in many layers. The thickness of this wound or stacked thin film is of the order of 100 micrometers. It generally contains at least four functional films: a negative electrode (anode) that ensures the supply of lithium ions during discharge, a positive electrode (cathode) that acts as a receptor into which the lithium ions are inserted, a solid polymer electrolyte that is placed between the positive and negative electrodes to conduct the lithium ions, and a current collector that is connected to the positive electrode to ensure an electrical connection. The negative electrode generally consists of a sheet of lithium metal or a lithium alloy; the solid polymer electrolyte generally consists of a polymer based on poly(ethylene oxide) (PEO) and at least one lithium salt; the positive electrode generally consists of a metal oxide (e.g. V2O5, LiV3O8, LiCoO2, LiNiO2, LiMn2O4 or LiNi 0.5 Mn 0.5 O2) or phosphate (e.g., LiMPO4, where M represents a metal cation selected from Fe, Mn, Co, Ni, and Ti, or a combination thereof), and optionally carbon; and the current collector generally consists of a metal sheet.

[0004] Solid polymer electrolytes offer great advantages in terms of safety, since they avoid the use of potentially dangerous solvents when overheated. Such batteries can be operated at high temperatures without the risk of explosion. However, commonly used solid polymer electrolytes, for example high molecular weight PEO doped with lithium salts, have low ionic conductivity at room temperature, so their operating temperatures must be kept relatively high (usually between 70 and 100 °C). However, at these temperatures PEO becomes a viscous liquid and loses dimensional stability.

[0005] Therefore, a major area of ​​technology is aimed at modifying solid polymer electrolytes in order to obtain improved mechanical strength and ionic conductivity that is maintained at lower temperatures.

[0006] In particular, Porcarelli et al. (Electrochimica Acta, 2017, 241, 526-534) describe a polyurethane-type polymer electrolyte obtained by several polycondensation steps from isophorone diisocyanate, polyethylene glycol, and an anionic diol functionalized with ester groups and sulfonyl(trifluoromethylsulfonyl)imide anions. To improve the ionic conductivity and mechanical properties of the resulting polymer material, this polymer material is functionalized with crosslinkable functional groups of the methacrylate type and then crosslinked by UV irradiation to form a film, which is then impregnated with propylene carbonate to form a gelled polymer electrolyte (quasi-solid electrolyte). However, the cycling resistance of the resulting gelled polymer electrolyte is not entirely satisfactory, since a loss of capacity is observed after more than 10 cycles.

[0007] Therefore, the object of the present invention is to overcome the above-mentioned drawbacks of the prior art and to provide a lithium battery, in particular a lithium metal polymer (LMP) battery, having excellent cycle stability (i.e., operable over a large number of cycles). In fact, the widespread use of electric vehicles requires batteries with improved performance in terms of cycle characteristics. Summary of the Invention [Problem to be solved by the invention]

[0008] The object of the present invention is to overcome the above-mentioned drawbacks of the prior art and to provide a lithium battery, in particular a lithium metal polymer (LMP) battery, having excellent cycling stability (i.e., operable over a large number of cycles). [Means for solving the problem]

[0009] The present inventors have surprisingly found that it is possible to improve the cycle durability (also called cycle characteristics) of a lithium battery by varying the charge and discharge temperatures during its operation, while maintaining the excellent ionic conductivity and mechanical properties of the solid or quasi-solid electrolyte.

[0010] A first subject of the invention is a method for operating a lithium battery comprising at least one positive electrode, at least one solid or quasi-solid electrolyte, and at least one negative electrode, chosen from solid or quasi-solid electrolyte lithium batteries, comprising at least the following steps: i) Charging temperature T C charging the lithium battery at (°C); and ii) Discharge temperature T D Discharging a lithium battery at (℃) Including, Charging temperature T C (℃) is the discharge temperature T D (°C). Effect of the Invention

[0011] By operating a solid or quasi-solid electrolyte lithium battery with the method according to the invention, an improvement in cycle durability is observed. The method according to the invention is easy to implement, unlike the prior art solutions which aim at the new development of the positive electrode active material and / or the polymer electrolyte material. The charging temperature T C is the discharge temperature T D Higher than (TC > T D ) is implemented, the cycle characteristics of a solid or quasi-solid electrolyte lithium battery are improved. The solution of the present invention is easy to implement, unlike the prior art solutions that aim to develop new positive electrode active materials and / or new polymer electrolyte materials.

[0012] Steps i) and ii) In the present invention, the charging temperature T C (or discharge temperature T D ) is measured by means of an oven thermocouple, in particular that sold under the name UNE500 by the company MEMMERT.

[0013] Charging temperature T C (or discharge temperature T D ) represents the temperature to which the battery applies during operation when charging (or discharging).

[0014] When the battery is discharged, the negative electrode releases Li in the form of ions. + The lithium released at passes through a solid or quasi-solid electrolyte (e.g., an ion-conducting polymer) and is inserted into the active material of the positive electrode. + The passage of ions into the battery's internal circuit is exactly compensated by the passage of electrons into the external circuit, thereby generating an electric current.

[0015] During charging of the battery, the negative electrode inserts lithium into the material that constitutes it, and the positive electrode releases lithium. The method of the present invention promotes the deposition of lithium at the negative electrode during charging. Steps i) and ii) of the method of the present invention represent the charge-discharge process, i.e. the cycle of a lithium battery.

[0016] In a preferred embodiment, the charging temperature T C and the discharge temperature T in step ii) D (i.e., T C - T D ) is at least about 5° C., more preferably at least about 7° C., and even more preferably at least about 10° C. A difference of less than 5° C. will result in insufficient cycle resistance.

[0017] In a preferred embodiment, the charging temperature T C and the discharge temperature T D (i.e., T C - T D ) is at most about 50° C., more preferably at most about 40° C., even more preferably at most about 30° C., and even more preferably at most about 20° C. A difference of more than 50° C. makes the method more difficult to carry out (the battery heats up when charging and cools down when discharging).

[0018] In a particularly preferred embodiment, the charging temperature T C and the discharge temperature T in step ii) D (i.e., T C - T D ) is in the range of 20 to 35°C, more preferably about 25 to 30°C.

[0019] According to one embodiment of the present invention, the charging temperature T C The temperature is in the range of about 0 to 100°C, preferably about 10 to 95°C, and particularly preferably about 20 to 90°C.

[0020] Discharge temperature T in step ii) D The temperature may be in the range of about -10 to 90°C, preferably about 0 to 85°C, and particularly preferably about 10 to 80°C.

[0021] Needless to say, the charging temperature T C and discharge temperature T D is the charging temperature T C is the discharge temperature T D may be within the equivalent range of values, provided that it is strictly higher than

[0022] The method of operating a lithium battery according to the invention can be applied to any type of lithium battery selected from LMP batteries, regardless of the nature of the active material in the composition of the positive electrode and / or the nature of the solid or quasi-solid electrolyte.

[0023] In the present invention, the "solid or quasi-solid" electrolyte is in a solid or gel form at room temperature (ie, 18 to 25° C.), and is preferably in a solid form.

[0024] According to a preferred embodiment of the present invention, reducing the operating temperature of the battery between the charging step i) and the discharging step ii) reduces the charging potential U C and the discharge potential U in the discharge step ii) D (i.e., T C From T D U related to temperature change to C From U D (No potential change is observed to the

[0025] In step i), the battery is charged at a charging temperature T C and maintain this temperature T until a state of charge of about 95% is obtained. C This can be achieved by maintaining

[0026] temperature T C is preferably constant during step i).

[0027] The heating in step i) can be carried out using at least one of the following heating means, such as using heat-pulsed air, using a heated liquid circuit or using one or more heating plates, preferably using one or more heating plates.

[0028] In step ii), the battery is discharged at a temperature T D This can be achieved by cooling to

[0029] temperature T D is preferably variable during step ii). For example, the temperature T Dmax At temperature T Dmin However, the charging temperature T C (℃) is T Dmax and T Dmin It is understood that the temperature is strictly higher than (°C).

[0030] Cooling can be performed by stopping the heating implemented at the end of step i) (i.e. after a state of charge of about 95%) or by forced cooling, preferably by stopping the heating means implemented at the end of step i).

[0031] Cooling is typically performed at low current (a period commonly referred to as the "floating period").

[0032] Forced cooling can be achieved using at least one of the following cooling means: use of pulsed cold air or use of a liquid cooling circuit.

[0033] Other processes The method may further comprise repeating steps i) and ii) (ie, performing multiple charge-discharge cycles).

[0034] The method further comprises, before step i), increasing the discharge temperature T D (°C), and the charging temperature T C (℃) is the discharge temperature T D (° C.). This embodiment is used when the battery is being charged for the first time.

[0035] When the method of the present invention includes n charging steps and m discharging steps, n and m are integers greater than 1, and the charging temperature T Cn (or the discharge temperature T Dm ) may be the same or different, and are preferably the same.

[0036] Solid or semi-solid electrolyte The solid or semi-solid electrolyte of the battery used in the method of the present invention preferably comprises one or more polymeric materials.

[0037] The polymer material(s) of the solid or quasi-solid electrolyte preferably represents at least about 30% by weight, particularly preferably at least about 40% by weight, based on the total weight of the solid or quasi-solid electrolyte.

[0038] The solid or semi-solid electrolyte may be a polymer electrolyte: - comprising at least one lithium salt and at least one poly(ethylene oxide) (PEO) based polymeric material, or - those comprising at least one anionic polymer substituted with anions of a lithium salt.

[0039] The poly(ethylene oxide) (POE) based polymeric material can be selected from polystyrene-poly(ethylene oxide) (PS-b-PEO) block copolymers, polystyrene-poly(ethylene oxide)-polystyrene (PS-b-PEO-b-PS) block copolymers, random poly(ethylene oxide-co-propylene oxide) copolymers (i.e., PEO-ran-PPO), random poly(ethylene oxide-co-butylene oxide) copolymers (i.e., PEO-ran-PBO), poly(ethylene oxide), and mixtures thereof.

[0040] Lithium salts used in combination with poly(ethylene oxide)-based polymeric materials include lithium fluoride (LiFO3), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF6), lithium fluoroborate (LiBF4), lithium metaborate (LiBO2), lithium perchlorate (LiCIO4), lithium nitrate (LiNO3), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(pentafluoroethyl)imide (LiBETI), LiAsF6, LiCF3SO3, LiSbF6, LiSbCl6, Li2TiCl6, Li2SeCl6, Li2B 10 CI 10 , Li2B 12 CI 12, lithium bis(oxalato)borate (LiBOB), and mixtures thereof.

[0041] The lithium salt preferably represents between 5 and 30% by weight, even more preferably between 10 and 25% by weight relative to the total weight of the polymer electrolyte.

[0042] The poly(ethylene oxide) (POE) based polymeric materials can be combined with reinforcing agents, which allow the mechanical properties of the polymeric material to be tailored.

[0043] The reinforcing agents are preferably selected from cellulose nanofibrils, ceramic nanoparticles such as titanium oxide, aluminum oxide or silicon oxide nanoparticles, and fluorinated polymers and copolymers such as polyvinylidene fluoride (PVdF) or vinylidene fluoride-hexafluoropropylene copolymers (PVdF-co-HFP).

[0044] The anionic polymer substituted with an anion of a lithium salt may be a block copolymer comprising at least one first block based on poly(ethylene oxide) and at least one second block based on an anionic polymer preparable from one or more monomers substituted with an anion of a lithium salt, such as sulfonyl(trifluoromethylsulfonyl)imide (TFSILi).

[0045] The block copolymer, comprising at least one first block based on poly(ethylene oxide) and at least one second block based on an anionic polymer preparable from one or more monomers substituted with an anion of a lithium salt, already comprises anionic functional groups (anions of a lithium salt directly grafted into the structure of the polymer material). According to this embodiment, the polymer electrolyte does not comprise an additional lithium salt.

[0046] The monomers are preferably selected from vinylic and derivative monomers.

[0047] Examples of vinyl monomers include lithium sulfonyl(trifluoromethylsulfonyl)imide styrene and its derivatives, particularly derivatives in which the phenyl group of styrene is substituted with one or more groups selected from methyl, ethyl, tert-butyl, bromine atoms and chlorine atoms, lithium sulfonyl(trifluoromethylsulfonyl)imide, lithium sulfonyl(trifluoromethylsulfonyl)imide methacrylate, lithium sulfonyl(trifluoromethylsulfonyl)imide acrylamide, lithium-sulfonyl(trifluoromethylsulfonyl)imide methacrylamide, lithium ethylene-sulfonyl(trifluoromethylsulfonyl)imide, lithium propylene-sulfonyl(trifluoromethylsulfonyl)imide, and lithium diene-sulfonyl(trifluoromethylsulfonyl)imide diene or lithium maleimide-sulfonyl(trifluoromethylsulfonyl)imide.

[0048] The polymer electrolyte may further comprise at least one plasticizer or non-aqueous solvent, which allows for the formation of a gelled polymer electrolyte.

[0049] The solvent or plasticizer may be selected from linear and cyclic carbonates such as propylene carbonate, ethylene carbonate or dimethyl carbonate, fluorinated carbonates such as fluoroethylene carbonate, nitriles such as succinic acid dinitrile, lactones such as y-butyrolactone, linear or cyclic polyethers, fluorinated polyethers, sulfur-based solvents such as sulfolane and dimethyl sulfoxide.

[0050] Among such solvents or plasticizers are dimethyl ether, polyethylene glycol dimethyl ether (or PEGDME), such as tetraethylene glycol dimethyl ether (TEGDME), dioxolane, ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl isopropyl carbonate (MiPC), ethyl acetate, ethyl butyrate (EB), and mixtures thereof.

[0051] Preferably, the solvent or plasticizer is about 10-70% by weight, and even more preferably about 20-60% by weight, based on the total weight of the polymer electrolyte. The solid or quasi-solid electrolyte, the positive electrode, and the negative electrode are preferably in the form of a film.

[0052] In a lithium battery operated according to the method of the invention, the thickness of the films constituting the various elements of the battery is generally of the order of 1 to 100 micrometers.

[0053] Preferably, the solid or quasi-solid electrolyte membrane has a thickness of 1 to 50 μm, preferably 2 to 20 μm.

[0054] The solid or quasi-solid electrolyte can be prepared by any technique known to those skilled in the art, such as, for example, coating, extrusion or pressing (cold or hot).

[0055] positive electrode The positive electrode may include a positive electrode active material, optionally an electronic conductivity imparting agent, and optionally a polymeric material.

[0056] The active material of the positive electrode is a reversibly active material for lithium ions, in other words, capable of reversibly inserting and extracting lithium ions.

[0057] The positive electrode active material may be: - Vanadium oxide VO X (2≦x≦2.5), LiV3O8, Li y Ni 1-x Co x O2(0≦x≦1, 0≦y≦1), Manganese spinel Li y Mn 1-x M x O2 (M=Cr, Al, V, Ni, 0≦x≦0.5, 0≦y≦2), V2O5, LiCoO2, LiNiO2, LiMn2O4 and LiNi 0.5 Mn 0.5 Metal oxides such as O2, or - silicon phosphates or metal phosphates such as LiMPO4, where M represents a metal cation selected from Fe, Mn, Co, Ni and Ti or a combination thereof, such as LiFePO4, or - Metal sulfates such as ferrous sulfate Fe2(SO4)3.

[0058] The method of the present invention is particularly suitable for LMP batteries, most particularly LMP batteries in which the active material of the positive electrode is selected from iron phosphate and its derivatives, especially LiFePO4.

[0059] The electronic conductivity imparting agent can be selected from carbon black, SP carbon, acetylene black, carbon fibers and nanofibers, carbon nanotubes, graphene, graphite, metal particles and fibers of at least one conductive metal such as aluminum, platinum, iron, cobalt, and nickel, and mixtures thereof.

[0060] The active material of the positive electrode may represent about 60 to 95% by weight, preferably about 70 to 90% by weight, based on the total weight of the positive electrode.

[0061] The electronic conductivity imparting agent may represent about 0.1 to 10% by mass, preferably about 0.3 to 5% by mass, based on the total mass of the positive electrode.

[0062] The polymeric materials include homopolymers and copolymers of ethylene, homopolymers and copolymers of propylene, homopolymers and copolymers of ethylene oxide (e.g., PEO, copolymers of PEO), methylene oxide, propylene oxide, epichlorohydrin, homopolymers and copolymers of allyl glycidyl ether, and mixtures thereof, halogenated polymers such as vinyl chloride, vinylidene fluoride (PVdF), homopolymers and copolymers of vinylidene chloride, tetrafluoroethylene or chlorotrifluoroethylene, copolymers of vinylidene fluoride and hexafluoropropylene (PVdF-co-HFP) or mixtures thereof. The material may be a material selected from anionic polymers, electronically non-conductive anionic polymers such as poly(styrenesulfonic acid), poly(acrylic acid), poly(glutamic acid), alginic acid, pectin, gelatin or mixtures thereof, cationic polymers such as polyethyleneimine (PEI), polyaniline in the emeraldine salt (ES) form, quaternized poly(N-vinylimidazole), poly(acrylamide-diallyldimethylammonium chloride) (AMAC) or mixtures thereof, polyacrylates, lithium salt anion substituted anionic polymers, and mixtures thereof.

[0063] The anionic polymer substituted with an anion of a lithium salt is as defined in the present invention.

[0064] The polymeric material may in particular be a poly(ethylene oxide) (PEO) based polymeric material or an anionic polymer substituted with anions of lithium salts.

[0065] The active material of the positive electrode may represent about 1 to 20% by weight, preferably about 5 to 15% by weight, based on the total weight of the positive electrode.

[0066] According to a particularly preferred embodiment of the invention, the active material of the positive electrode is coated with a carbon layer, the presence of which makes it possible to improve the interface: active material-polymer material.

[0067] The amount of carbon coating the active material is preferably about 0.1 to 5% by mass based on the mass of the active material.

[0068] The carbon layer is preferably in the form of a layer having a thickness of about 1-4 nm.

[0069] The positive electrode may further include a lithium salt.

[0070] The lithium salt may be as defined herein.

[0071] Current collector The lithium battery may further include a current collector connected to the positive electrode.

[0072] The current collector generally consists of a metal sheet.

[0073] The current collector is preferably a stainless steel or aluminum current collector, optionally coated with a carbon-based layer (corrosion-resistant layer).

[0074] negative electrode The negative electrode preferably consists of lithium metal or one of its alloys, such as lithium alloys with silicon, tin, aluminum or germanium.

[0075] The battery is preferably an LMP battery.

[0076] A second subject of the invention is a lithium battery with a solid or quasi-solid electrolyte, the battery being charged at a temperature T C is the discharge temperature T D The charging temperature T C and discharge temperature T D and using a lithium battery selected from the group consisting of lithium batteries operating at 10000 volts (2000 volts) and 10000 volts (2000 volts) to improve its cycle durability.

[0077] Lithium battery, charging temperature T C , and discharge temperature T D is as defined in the first subject of the invention.

[0078] The lithium battery defined in the first subject of the present invention is charged at a temperature T C and discharge temperature T Dand the charging temperature T C is the discharge temperature T D The charging temperature T C and discharge temperature T D is as defined in the first subject of the invention. EXAMPLES

[0079] The following examples are given, but the present invention is not limited to these. [Brief description of the drawings]

[0080] [Figure 1] FIG. 1 shows the faradaic efficiency (percent) based on the number of cycles (number) for cells operated according to the method of the present invention and according to the prior art method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0081] The raw materials used in the examples are listed below. - Carbon black Ketjenblack EC600JD, manufactured by AkzoNobel - LiFePO4, manufactured by Pulead - PVDF-co-HFP, Solvay - Homo PEO, manufactured by Sumitomo Seika Chemicals - LiTFSI, manufactured by Solvay - Carbon-coated aluminum current collector, manufactured by Armor - Lithium metal sheet, Blue Solutions

[0082] Unless otherwise noted, all materials were used as received from the manufacturer.

[0083] Example 1: Preparation and operation of LMP batteries 1.1 Preparation of the positive electrode A positive electrode was prepared in the form of a film as follows: 46 g of LiFePO4, 1.2 g of carbon black, 17.5 g of homo-PEO polymer material, and 6.5 g of deionized water were placed in a mixer available from Brabender® as Plastograph. Mixing was performed at 60° C. and 80 rpm.

[0084] The resulting paste was rolled onto a carbon coated aluminum current collector at 60° C. The resulting film was dried at 100° C. for 10 minutes before use.

[0085] The obtained positive electrode contains 71% by mass of the active material LFP, 27% by mass of the homo-PEO polymer material, and 1.9% by mass of carbon black. The film thickness is about 45 μm.

[0086] 1.2 Preparation of LMP batteries An LMP cell was prepared in a controlled atmosphere (dew point -50°C) by assembling the following: - A 50 μm thick solid polymer electrolyte film containing 80 g of polymer material (a mixture of homo-PEO and PVDF-co-HFP) and 20 g of LiTFSI. - Lithium metal sheet, approximately 50μm thick - Positive electrode prepared in section 1.1

[0087] Therefore, the lithium sheet and the solid polymer electrolyte film were laminated at 70 °C and 5 bar to ensure a good Li / electrolyte interface. Then, finally, the cathode was laminated onto the Li / electrolyte assembly at 70 °C and 5 bar to form the battery. The electrolyte film was placed between the lithium metal film and the cathode film. A conductive wire was connected to the lithium and another conductive wire to the cathode current collector.

[0088] The resulting lithium battery has a sandwich construction and is sealed in a pouch (commonly known as a coffee bag) under vacuum to protect it from moisture.

[0089] A lithium battery under 1 atmosphere is obtained.

[0090] 1.3 LMP Battery Operation The cells obtained in section 1.2 were tested in an uncontrolled atmosphere.

[0091] The lithium battery is then subjected to a charging step i) at a charging temperature T c 90 °C, and discharge step ii) is performed at discharge temperature T D A multiple charge-discharge process (i.e., steps i) and ii) were repeated) was carried out at 50° C. (method according to the present invention).

[0092] Step i) was carried out using a Memmert UNE500 oven.

[0093] For comparison, a lithium battery having the same structure as that prepared in section 1.2 was subjected to multiple charge-discharge processes, with the charge and discharge steps being carried out at the same temperature of 80° C. (a method not according to the present invention).

[0094] FIG. 1 shows the Faradaic efficiency (in percent) versus cycle number (in number) for a lithium battery operated according to the method of the invention (curve with filled circles) and, by comparison, for a lithium battery operated according to a method not according to the invention (curve with filled squares).

[0095] The first cycle was performed at C / 10 (10 hour charge) and D / 10 (10 hour discharge), and the second cycle was performed at C / 4 (4 hour charge) and D / 20 (20 hour discharge).

[0096] For cells operated according to the method of the present invention, very good cycling durability of more than 20 cycles associated with a faradaic efficiency of 95% is obtained.

Claims

1. 1. A method of operating a lithium battery selected from a solid-state or quasi-solid-state electrolyte lithium battery, the lithium battery comprising at least one positive electrode, at least one solid-state or quasi-solid-state electrolyte, and at least one negative electrode, the method comprising at least the following steps: i) Charging temperature T C charging the lithium battery with ii) Discharge temperature T D discharging the lithium battery Including, The charging temperature T C is the discharge temperature T D 4. A method of operating a lithium battery, characterized in that:

2. The charging temperature T C and the discharge temperature T D The method of claim 1 , wherein the difference between the temperature and the temperature is at least 5° C.

3. The charging temperature T C and the discharge temperature T D The method according to claim 1 or 2, wherein the difference between the temperature and the temperature is 50° C. or less.

4. Charging temperature T in step i C A method according to any one of claims 1 to 3, wherein the temperature is in the range of 0 to 100°C.

5. Discharge temperature T in step ii) D The method of any one of claims 1 to 4, wherein the temperature is in the range of -10 to 90°C.

6. A method according to any one of claims 1 to 5, further comprising repeating steps i) and ii).

7. The solid or quasi-solid electrolyte is a polymer electrolyte, - comprising at least one lithium salt and at least one poly(ethylene oxide) (PEO) based polymeric material; or - comprises an anionic polymer substituted with the anion of at least one lithium salt, A method according to any one of claims 1 to 6.

8. The method of any one of claims 1 to 7, wherein the positive electrode comprises a positive electrode active material, optionally a conductivity imparting agent, and optionally a polymeric material.

9. The method of any one of claims 1 to 8, wherein the negative electrode comprises lithium metal or an amalgam thereof.

10. The method of any one of claims 1 to 9, wherein the battery further comprises a current collector connected to the positive electrode.

11. Use of a lithium battery selected from a solid-state or quasi-solid-state electrolyte lithium battery, the lithium battery comprising at least one positive electrode, at least one solid-state or quasi-solid-state electrolyte, and at least one negative electrode, the lithium battery being charged at a charging temperature T C and discharge temperature T D and the charging temperature T C is the discharge temperature T D The use of lithium batteries, thereby improving their cycle resistance, is strictly higher than that of conventional batteries.

Citation Information

Patent Citations

  • Lithium iron phosphate battery system

    CN103746150A

  • Solid-state electrolyte taking cyclodextrin as filler, preparation method and application thereof

    CN113471520A

  • Organic electrolyte secondary battery

    JP1983111265A

  • Negative electrode active material and nonaqueous electrolyte battery

    JP2003086177A

  • Slurry composition for lithium ion secondary battery negative electrode, secondary battery negative electrode, and secondary battery