Polybutylene terephthalate resin composition, its manufacturing method and molded article manufactured therefrom

A polybutylene terephthalate resin composition with specific additives achieves a balance of mechanical strength and flame retardancy, addressing the limitations of existing compositions for automobile parts, particularly in electrical components, with enhanced processability and fluidity.

JP2024536666AActive Publication Date: 2024-10-08LG CHEM LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023580882
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-06
Filing Date
2023-07-07
Publication Date
2024-10-08
Estimated Expiration
2043-07-07

AI Technical Summary

Technical Problem

Existing polybutylene terephthalate resin compositions struggle to achieve a balance between mechanical strength and flame retardancy suitable for automobile parts, particularly in electrical components, while using non-halogen flame retardants.

Method used

A polybutylene terephthalate resin composition comprising polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent, with specific ratios and contents, to enhance mechanical strength and flame retardancy.

Benefits of technology

The composition provides an excellent balance of mechanical properties and flame retardancy, suitable for automobile electrical parts, with improved processability and fluidity, comparable to or exceeding that of polyester resin composites with halogenated flame retardants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536666000001
    Figure 2024536666000001
  • Figure 2024536666000002
    Figure 2024536666000002
  • Figure 2024536666000003
    Figure 2024536666000003
Patent Text Reader

Abstract

The present invention relates to a polybutylene terephthalate resin composition, a manufacturing method thereof, and a molded article manufactured from the same, which provides an excellent balance of physical properties, namely mechanical strength and flame retardancy, equivalent to or higher than that of polyester resin composite materials containing halogen-based flame retardants, and has excellent processability due to its excellent fluidity, and is particularly suitable as a material for automotive electrical components.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0117051 filed on September 16, 2022 and Korean Patent Application No. 10-2023-0087762 refiled on July 6, 2023 based thereon, and all contents disclosed in the documents of the Korean patent application are incorporated as part of this specification.

[0002] The present invention relates to a polybutylene terephthalate resin composition, a production method thereof, and a molded article produced therefrom. More specifically, the present invention relates to a polybutylene terephthalate resin composition that does not contain a halogen-based flame retardant but has an excellent balance between mechanical properties and flame retardancy, a production method thereof, and a molded article produced therefrom. [Background technology]

[0003] In the field of automobiles, research is being actively conducted into replacing materials used in automobile parts with plastics in order to reduce weight and manufacturing costs.

[0004] Among plastics, polyester resins are widely used as materials for automobile parts, and are evaluated as having the potential to replace aluminum and steel. As a result, polybutylene terephthalate resins, among polyester resins, are excellent in terms of high rigidity and heat resistance as materials for automobile parts, and research into their application to various automobile parts is being actively conducted.

[0005] However, in order to use polybutylene terephthalate resin as a material for electrical components, especially connector parts, it is necessary to develop a flame-retardant composite material that includes a non-halogen flame retardant.

[0006] Metal salt phosphorus-based flame retardants are mainly used as non-halogen flame retardants in polybutylene terephthalate resin composite materials, but it is difficult to achieve the same level of mechanical rigidity and flame retardancy as when halogen-based flame retardants are used. Therefore, there is a need to develop polybutylene terephthalate resin compositions that contain non-halogen flame retardants but have excellent mechanical rigidity and flame retardancy. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent Publication No. 10-2011-0072828 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a polybutylene terephthalate resin composition which achieves a balance between mechanical strength and flame retardancy at a level suitable for use as a material for automobile parts, and a method for producing the same.

[0009] Another object of the present invention is to provide a molded article produced from the polybutylene terephthalate resin composition.

[0010] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides I) a polybutylene terephthalate resin composition comprising polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent (reinforcing agent), and satisfying the following mathematical formula 1:

[0012] [Formula 1] 7.76≦a / b≦45 (In the above formula 1, a is the tensile strength (MPa) of the polybutylene terephthalate resin composition measured according to ISO 527, and b is the flow index (g / 10 min) of the polybutylene terephthalate resin composition measured according to ISO 1133 at 265° C. under a load of 2.16 kg.)

[0013] II) In I), the silica-containing reinforcing agent may contain 50% by weight or more of silica in the reinforcing agent, specifically 50 to 70% by weight, preferably 50 to 65% by weight, and more preferably 50 to 60% by weight.

[0014] III) In I) or II), when the content of the polybutylene terephthalate is c and the content of the silica-containing reinforcing agent is d, a correlation of 0.5d≦c≦2d can be satisfied.

[0015] Here, the content may refer to weight % based on a total of 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent, and if necessary, refers to weight % based on a total of 100% by weight, further including at least one selected from melamine cyanurate, polyethylene, processability improver, and heat resistance additive.

[0016] IV) In the above I) to III), the polybutylene terephthalate is contained in a range of 15 to 65% by weight relative to a total of 100% by weight of polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the polybutylene terephthalate is contained in a range of 15 to 65% by weight relative to a total of 100% by weight of polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent, a processability improver, and a heat resistance additive.

[0017] V) In the above I) to IV), the polybutylene terephthalate may have an intrinsic viscosity (η) of 0.5 to 1.25 dl / g as measured in accordance with ASTM D2857.

[0018] VI) In the above I) to V), the silica-containing reinforcing agent is contained in a range of 10 to 50% by weight relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the silica-containing reinforcing agent is contained in a range of 10 to 50% by weight relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

[0019] VII) In the above I) to VI), the aluminum salt of diethylphosphinic acid is contained in a range of 5 to 35 weight % relative to a total of 100 weight % of polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the aluminum salt of diethylphosphinic acid is contained in a range of 5 to 35 weight % relative to a total of 100 weight % of polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, melamine polyphosphate, and the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

[0020] VIII) In the above I) to VII), the melamine polyphosphate is contained in the range of 0.1 to 10% by weight relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the melamine polyphosphate is contained in the range of 0.1 to 10% by weight relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

[0021] IX) In the above I) to VIII), the resin composition may contain melamine cyanurate, and the melamine cyanurate may be contained in an amount within a range of 0.1 to 10% by weight relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, and the melamine cyanurate; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the polybutylene terephthalate resin composition may contain the processability improver and the heat resistance additive in an amount within a range of 0.1 to 10% by weight relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the melamine cyanurate, the processability improver, and the heat resistance additive.

[0022] X) In the above I) to IX), the resin composition may contain a processability improver, and may contain this in a range of 0.001 to 3 weight % based on a total of 100 weight % of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent plus the processability improver.

[0023] XI) In the above I) to X), the resin composition may contain a heat-resistant additive, and may contain this in a range of 0.001 to 3 weight % based on a total of 100 weight % of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, and the heat-resistant additive.

[0024] The present invention also provides a method for producing a polybutylene terephthalate resin composition, comprising the steps of kneading and extruding polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent, and satisfying the following mathematical formula 1:

[0025] [Formula 1] 7.76≦a / b≦45 (In the above formula 1, a is the tensile strength (MPa) of the polybutylene terephthalate resin composition measured according to ISO 527, and b is the flow index (g / 10 min) of the polybutylene terephthalate resin composition measured according to ISO 1133 at 265° C. under a load of 2.16 kg.)

[0026] The present invention also includes XIII) a molded article comprising the above-mentioned polybutylene terephthalate resin composition.

[0027] XIV) In the above-mentioned XIII), the molded article may be an automobile electrical component. Effect of the Invention

[0028] The polybutylene terephthalate resin composition according to the present invention provides an excellent balance of physical properties, namely mechanical strength and flame retardancy, which is equivalent to or exceeds the level of a polyester resin composite material containing a halogen-based flame retardant, and has excellent processability due to its excellent fluidity, and can be used as a material for automotive electrical components in particular.

[0029] That is, the molded article produced from the polybutylene terephthalate resin composition according to the present invention has an effect of realizing a high level of balance between mechanical properties such as tensile strength and flame retardancy.

[0030] Therefore, the polybutylene terephthalate resin composition according to the present invention and the molded article produced therefrom can be widely applied to the field of automobile parts where such is required. BEST MODE FOR CARRYING OUT THEINVENTION

[0031] In the following, the present invention will be described in more detail to facilitate understanding of the present invention.

[0032] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meaning, but should be interpreted in a meaning and concept that corresponds to the technical idea of ​​the present invention, taking into consideration that the inventor can appropriately define the concept of the term in order to explain the invention in the best possible manner.

[0033] The present inventors have confirmed that by adjusting the type and content of the non-halogenated flame retardant, it is possible to achieve a balance of mechanical strength and flame retardancy suitable for the material of automotive parts, and have thus completed the present invention.

[0034] The polybutylene terephthalate resin composition according to the present invention comprises polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent.

[0035] When the tensile strength (MPa) measured according to ISO 527 is a and the flow index (g / 10 min) measured according to ISO 1133 at 265° C. under a load of 2.16 kg is b, the polybutylene terephthalate resin composition can have a / b in the range of, for example, 7.76 to 45, specifically 7.76 to 40, and preferably 7.77 to 40. When the above-mentioned range is satisfied, a balance of physical properties such as rigidity, flame retardancy, and processability can be provided.

[0036] In one embodiment of the present invention, the a may be 130 or more, or 130-165, and the b may be 4-20, or 4-18.

[0037] Hereinafter, each component of the polybutylene terephthalate resin composition of the present invention will be described in detail.

[0038] <Polybutylene terephthalate> In one embodiment of the present invention, the polybutylene terephthalate may be polybutylene terephthalate obtained by direct esterification or transesterification of 1,4-butanediol with terephthalic acid or dimethyl terephthalate.

[0039] In one embodiment of the present invention, in order to increase the impact strength of the polybutylene terephthalate resin composition, the polybutylene terephthalate may be a copolymer copolymerized with an impact improving compound such as polytetramethylene glycol, polyethylene glycol, polypropylene glycol, aliphatic polyester, aliphatic polyamide, etc., or the polybutylene terephthalate may be a modified polybutylene terephthalate mixed with the impact improving compound.

[0040] In one embodiment of the present invention, the intrinsic viscosity η of the polybutylene terephthalate measured in accordance with ASTM D2857 may be, for example, 0.5 to 1.25 dl / g, preferably 0.5 to 1.2 dl / g, and more preferably 0.52 to 1 dl / g. When the intrinsic viscosity of the polybutylene terephthalate satisfies the above range, a polybutylene terephthalate resin composition having an excellent balance of physical properties between mechanical properties and moldability can be obtained.

[0041] In one embodiment of the present invention, the polybutylene terephthalate is contained in a range of 15 to 65 wt%, 25 to 58 wt%, preferably 40 to 58 wt%, more preferably 40 to 55 wt%, and even more preferably 45 to 55 wt%, based on a total of 100 wt% of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent; or the polybutylene terephthalate resin composition includes a processability improver and a heat resistance additive, and the polybutylene terephthalate is contained in a range of 15 to 65 wt%, 25 to 58 wt%, preferably 40 to 58 wt%, more preferably 40 to 55 wt%, and even more preferably 45 to 55 wt%, based on a total of 100 wt% of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent, processability improver, and heat resistance additive. When the polybutylene terephthalate is contained within the above range, a polybutylene terephthalate resin composition having an excellent balance of processability, specific gravity, and mechanical properties can be provided.

[0042] <Reinforcement agent> In one embodiment of the present invention, the reinforcing material may be glass fiber as an example, and the reinforcing material may be used together with other inorganic fibers.

[0043] In this case, the inorganic fiber may be, for example, one or more selected from carbon fiber, basalt fiber, and natural fiber such as kenaf or hemp.

[0044] In one embodiment of the present invention, the cross section of the reinforcing agent may have a shape such as a circle, a rectangle, an oval, a dumbbell, a diamond, etc., and may have an average diameter of 8 to 20 μm, or 10 to 15 μm, and an average length of 2 to 6 mm, or 2 to 4 mm.

[0045] Here, the average diameter and the average length of the reinforcing agent can be measured by a method commonly used in this technical field. For example, the reinforcing agent can be observed with a scanning electron microscope (SEM), and the average diameter and the average length of 10 to 30 strands can be measured.

[0046] The reinforcing agents may be treated with sizing compositions during fiber manufacture or in post-treatment steps, including process improvers, coupling agents, surfactants, and the like.

[0047] The processing improver is mainly used to form good strands, and the coupling agent enables good adhesion between the reinforcing agent and the polybutylene terephthalate resin. When appropriately selected and used in consideration of the types of polybutylene terephthalate resin and reinforcing agent, the coupling agent can impart excellent physical properties to the polybutylene terephthalate resin composition.

[0048] The coupling agent can be used in a variety of ways, including directly treating the reinforcing agent and adding the agent to an organic matrix. In order to fully utilize the performance of the coupling agent, the content of the coupling agent must be appropriately selected.

[0049] Examples of the coupling agent include amine-based, acrylic-based, and silane-based agents such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)γ-aminopropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and β(3,4-epoxyethyl)γ-aminopropyltrimethoxysilane.

[0050] In particular, the reinforcing agent described herein preferably contains silica, as this can provide rigidity and mechanical properties.

[0051] The silica may be contained in the reinforcing agent in an amount of, for example, 50% by weight or more, specifically, 50 to 70% by weight, preferably 50 to 65% by weight, and more preferably 50 to 60% by weight. When the amount of the silica in the reinforcing agent is within the above range, it is possible to provide an excellent balance between rigidity and mechanical properties.

[0052] Specifically, as can be seen from the following examples and comparative examples, when a reinforcement with an inappropriate content of silica, for example 48 wt%, was used instead, the flame retardancy was excellent, but the tensile strength and flow index were poor, and it was confirmed that a balance of physical properties could not be provided (see Comparative Example 4).

[0053] In the present invention, the silica content in the reinforcing agent can be measured or confirmed using XRF (X-Ray Fluorescence spectrometry).

[0054] In one embodiment of the present invention, the silica-containing reinforcing agent is contained in a range of 10 to 50% by weight, preferably 15 to 50% by weight, more preferably 20 to 50% by weight, based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition includes a processability improver and a heat resistance additive, and the silica-containing reinforcing agent is contained in a range of 10 to 50% by weight, preferably 15 to 50% by weight, more preferably 20 to 50% by weight, based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

[0055] <Non-halogen flame retardants> The non-halogen flame retardant according to the present invention may include an aluminum salt of diethylphosphinic acid and melamine polyphosphate, and not only provides a flame retardant effect during extrusion / injection processing of the polybutylene terephthalate resin composition, but also provides a sufficient flame retardant effect during long-term storage of the polybutylene terephthalate resin composition.

[0056] The aluminum salt of diethylphosphinic acid can form char on the surface of the polymer to improve the flame retardancy of the composition.

[0057] In one embodiment of the present invention, the aluminum salt of diethylphosphinic acid may be a commercially available product.

[0058] The aluminum salt of diethylphosphinic acid may be, for example, 5 to 35% by weight, 10 to 30% by weight, specifically 10 to 25% by weight, and preferably 10 to 20% by weight, based on the total 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the aluminum salt of diethylphosphinic acid may be, for example, 5 to 35% by weight, 10 to 30% by weight, specifically 10 to 25% by weight, and preferably 10 to 20% by weight, based on the total 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent, processability improver, and heat resistance additive. When the above-mentioned range is satisfied, char may be formed on the surface of the polymer to improve the flame retardancy of the composition.

[0059] When the melamine polyphosphate is used simultaneously with the aluminum salt of diethylphosphinic acid, it can form char on the surface of the polymer together with the aluminum salt of diethylphosphinic acid, thereby improving the effect of protecting the polymer from combustion.

[0060] In one embodiment of the present invention, the melamine polyphosphate may be a commercially available product.

[0061] The melamine polyphosphate may be, for example, 0.1 to 10% by weight, specifically 0.1 to 5% by weight, preferably 1 to 5% by weight, more preferably 2 to 4% by weight, based on the total 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and the melamine polyphosphate may be, for example, 0.1 to 10% by weight, specifically 0.1 to 5% by weight, preferably 1 to 5% by weight, more preferably 2 to 4% by weight, based on the total 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and silica-containing reinforcing agent, processability improver, and heat resistance additive. When the above-mentioned range is satisfied, char can be sufficiently formed on the surface of the polymer to improve the flame retardancy of the composition.

[0062] According to an embodiment of the present invention, melamine cyanurate may be included, in which case, an inert gas may be generated to improve flame retardancy.

[0063] The melamine cyanurate is, for example, contained in the range of 0.1 to 10% by weight, specifically 0.1 to 4.5% by weight, preferably 0.1 to 3.5% by weight, and more preferably 1 to 3.5% by weight, relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, and the melamine cyanurate; or the polybutylene terephthalate resin composition may contain a processability improver and a heat resistance additive, and may be contained in the range of 0.1 to 10% by weight, specifically 0.1 to 4.5% by weight, preferably 0.1 to 3.5% by weight, and more preferably 1 to 3.5% by weight, relative to a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the melamine cyanurate, the processability improver, and the heat resistance additive.

[0064] <Processability improver> The processability improver according to the present invention may be an olefin wax, and serves to maintain excellent mold releasability and injectability of the polybutylene terephthalate resin composition.

[0065] The olefin wax may be a polymer having a low melt viscosity and may be an oily phase solid having slipperiness and plasticity. For example, the wax may be one or more selected from polyethylene wax and polypropylene wax, and a commercially available product may be used.

[0066] For example, the processability improver may be polyethylene, and specific examples thereof include polyethylene having a drop point of 100 to 120° C., a melting point (mp) of 95 to 115° C., and a density (23° C.) of 0.9 to 1.0 g / cm. 3 The absolute viscosity (120°C) is 350 to 450 mm 2 In this case, it is possible to effectively provide mold release properties and injectability.

[0067] In this description, the drop point is indicated as the minimum temperature at which a lubricant changes into a liquid state due to an increase in temperature, by an experimental method in accordance with ASTM D566 and KS M 2033. More specifically, the drop point can be indicated by placing a sample in a specified cup with a diameter of 100 mm, heating it under the specified conditions, and measuring the temperature at which the grease drops.

[0068] In this description, the melting point can be measured using a differential scanning calorimeter (DSC: Differential Scanning Calorimeter 2920) manufactured by TA Co. As a specific measurement example, the melting point can be measured by a method in which the DSC is equilibrated at a temperature of 0°C, the temperature is increased by 20°C per minute to 180°C, the temperature is decreased by 20°C per minute to -60°C, and the temperature is increased by 10°C per minute to 180°C. Here, the melting point is obtained by taking the apex region of the endothermic curve during the second temperature increase.

[0069] In this description, density can be measured, for example, according to the measurement method ASTM D1505.

[0070] In this description, the absolute viscosity can be measured using an absolute viscometer manufactured by Brookfield Co., Ltd. As a specific measurement example, the absolute viscosity can be measured using an absolute viscometer LVT230 manufactured by Brookfield Co., Ltd. according to the method of ASTM D1986-14.

[0071] As a specific example, the processability improver has a drop point of 105 to 115°C, a melting point (mp) of 100 to 110°C, and a density (23°C) of 0.95 to 1.0 g / cm 3 The absolute viscosity (120°C) is 380 to 420 mm 2 Polyethylene having a molecular weight of 1000 or less can be used.

[0072] As a specific example, the processability improver has a drop point of 108 to 112°C, a melting point (mp) of 102 to 106°C, and a density (23°C) of 0.95 to 0.98 g / cm 3 The absolute viscosity (120°C) is 400 to 420 mm 2 A polyethylene wax having a molecular weight of 1000 to 15000 can be used.

[0073] In one embodiment of the present invention, the processability improver may be a commercially available product, such as LC102N.

[0074] In one embodiment of the present invention, the processability improver is contained within a range of, for example, 0.001 to 3 wt%, preferably 0.05 to 3 wt%, more preferably 0.01 to 3 wt%, and most preferably 0.01 to 1 wt%, based on the total 100 wt% of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, silica-containing reinforcing agent, and processability improver; or, the polybutylene terephthalate resin composition contains melamine cyanurate, and is contained within a range of, for example, 0.001 to 3 wt%, preferably 0.05 to 3 wt%, more preferably 0.01 to 3 wt%, and most preferably 0.01 to 1 wt%, based on the total 100 wt% of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, polyethylene, silica-containing reinforcing agent, melamine cyanurate, and processability improver. When the above-mentioned range is satisfied, excellent mold releasability and injectability can be sufficiently provided.

[0075] As a specific example, the resin composition contains polyethylene, and the polyethylene is contained within, for example, 0.001 to 3% by weight, preferably 0.05 to 3% by weight, more preferably 0.01 to 3% by weight, and most preferably 0.01 to 1% by weight, relative to a total of 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, silica-containing reinforcing agent, and polyethylene; or the polybutylene terephthalate resin composition contains polyethylene, melamine cyanurate, and a heat-resistant additive, and the polyethylene is contained within, for example, 0.001 to 3% by weight, preferably 0.05 to 3% by weight, more preferably 0.01 to 3% by weight, and most preferably 0.01 to 1% by weight, relative to a total of 100% by weight of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, polyethylene, and silica-containing reinforcing agent, polyethylene, melamine cyanurate, and heat-resistant additive.

[0076] <Heat-resistant additive> The heat resistance additive according to the present invention can provide the polybutylene terephthalate resin composition with an anti-oxidation effect at high temperatures during extrusion and injection processing.

[0077] The heat resistance additive may be, for example, two or more selected from a hindered phenol-based compound, a phosphite-based compound, and a phosphonite-based compound.

[0078] As the hindered phenol compound, a commercially available product may be used.

[0079] Examples of the hindered phenol compound include octadecyl-3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate, tetrabis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, and the like. Examples of suitable hydroxybenzyl compounds include 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. Of these, it is preferable to use pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0080] Examples of the phosphite-based compound include triphenyl phosphite, tris(nonyl phenyl)phosphite, triisodecyl phosphite, diphenyl-isooctyl-phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and tris(2,4-di-tert-butylphenyl)phosphite. It is preferable to use tris(2,4-di-tert-butylphenyl)phosphite.

[0081] As the phosphonite-based compound, a compound represented by the following Chemical Formula 1 may be used.

[0082] [ka]

[0083] In the above formula 1, R1 and R2 are each independently alkyl, aryl, or alkylaryl, specifically C1-C 30 Alkyl, C6-C 30 aryl or alkylaryl, where Ar is an aryl group such as phenyl, naphthyl, biphenyl, terphenyl, and the like.

[0084] As another example, the heat-resistant additive may be a mixture of a compound represented by the following Formula 2 and a compound represented by the following Formula 3:

[0085] When a compound represented by the following chemical formula 2 and a compound represented by the following chemical formula 3 are mixed, it is preferable that the density is, for example, 530 g / l or more, specifically, 530 to 630 g / l, in order to provide an antioxidant effect at high temperatures.

[0086] Here, the density may be a value measured using a method and equipment commonly used in this technical field.

[0087] In one embodiment of the present invention, a commercially available product may be used, for example, a product such as B-225.

[0088] [ka]

[0089] [ka]

[0090] In one embodiment of the present invention, the heat resistance additive may be contained within a range of, for example, 0.001 to 3 wt%, preferably 0.05 to 2 wt%, more preferably 0.01 to 2 wt%, and even more preferably 0.1 to 2 wt% based on a total of 100 wt% of the polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, silica-containing reinforcing agent, and heat resistance additive. When the above range is satisfied, thermal stability can be provided during high-temperature processing.

[0091] The heat-resistant additive may be contained in an amount of, for example, 0.001 to 3% by weight, preferably 0.05 to 2% by weight, more preferably 0.01 to 2% by weight, and even more preferably 0.1 to 2% by weight, based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the melamine cyanurate, and the heat-resistant additive.

[0092] The heat-resistant additive may be contained in an amount of, for example, 0.001 to 3% by weight, preferably 0.05 to 2% by weight, more preferably 0.01 to 2% by weight, and even more preferably 0.1 to 2% by weight, based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the melamine cyanurate, the polyethylene, and the heat-resistant additive.

[0093] <Polybutylene terephthalate resin composition> The polybutylene terephthalate resin composition according to the present invention includes polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent, and when the content of the polybutylene terephthalate is c and the content of the silica-containing reinforcing agent is d, the composition satisfies a correlation of 0.5d≦c≦2d, specifically, a correlation of d≦c≦2d, and preferably a correlation of 1.3d≦c≦1.8d. When the above range is satisfied, the composition can provide an excellent balance of physical properties between rigidity, mechanical properties, and flame retardancy.

[0094] The term "content" used in this description can refer to the unit of weight % unless otherwise specified. Specifically, the contents of c and d can be weight % contained in the total of 100 weight % of polybutylene terephthalate, aluminum salt of diethylphosphinic acid, melamine polyphosphate, silica-containing reinforcing agent, processability improver, and heat resistance additive.

[0095] Here, c may be, for example, an integer of 35 to 58, preferably an integer of 40 to 58, more preferably an integer of 40 to 55, and even more preferably an integer of 45 to 50. When the above-mentioned range is satisfied, an excellent balance of physical properties between rigidity, mechanical properties, and flame retardancy can be provided.

[0096] Moreover, the d may be, for example, an integer of 10 to 50, preferably an integer of 15 to 50, and more preferably an integer of 20 to 50. When the above-mentioned range is satisfied, an excellent balance of physical properties between rigidity, mechanical properties, and flame retardancy can be provided.

[0097] In one embodiment of the present invention, the polybutylene terephthalate resin composition may include 15-65 wt% polybutylene terephthalate; 10-50 wt% silica-containing reinforcing agent; 5-35 wt% aluminum salt of diethylphosphinic acid; 0.1-10 wt% melamine polyphosphate; 0-10 wt% melamine cyanurate; 0.001-3 wt% heat resistance additive; and 0.001-3 wt% processability improver.

[0098] As another example, the polybutylene terephthalate resin composition may comprise 35-58 wt% polybutylene terephthalate; 15-50 wt% silica-containing reinforcing agent; 10-25 wt% aluminum salt of diethylphosphinic acid; 0.1-5 wt% melamine polyphosphate; 0-4.5 wt% melamine cyanurate; 0.001-3 wt% heat resistance additive; and 0.001-3 wt% processability improver.

[0099] As another example, the polybutylene terephthalate resin composition may contain 40-58% by weight of polybutylene terephthalate, 20-50% by weight of a silica-containing reinforcing agent, 10-20% by weight of an aluminum salt of diethylphosphinic acid, 1-5% by weight of melamine polyphosphate, 0.1-10% by weight of melamine cyanurate, 0.05-2% by weight of a heat resistance additive, and 0.05-3% by weight of a processability improver. When the above ranges are satisfied, an excellent balance of physical properties between rigidity, mechanical properties, and flame retardancy can be provided.

[0100] The polybutylene terephthalate resin composition may contain, for example, one or more additives selected from a UV stabilizer, a pigment, and a colorant, for example, in an amount of 0.01 to 5 parts by weight, preferably 0.5 to 2 parts by weight, and more preferably 1 to 2 parts by weight, based on 100 parts by weight of the polybutylene terephthalate resin composition. Within the above range, there is an effect that the physical properties of the resin composition are not affected and the inherent properties of the additive are expressed.

[0101] <Method of producing polybutylene terephthalate resin composition> The polybutylene terephthalate resin composition according to the present invention may be prepared by a method known in the art. For example, the polybutylene terephthalate resin composition may be prepared in the form of pellets by melt-extruding a mixture of each component and other additives in an extruder, and the pellets may be used for injection and extrusion molding.

[0102] In one embodiment of the present invention, the pellets are extruded at a temperature of 240 to 280° C., and the temperature of the mold during extrusion is preferably in the range of 80 to 120° C. If the temperature of the mold is less than 80° C., the appearance characteristics may deteriorate, and if it exceeds 120° C., the pellets may stick to the mold, reducing the demoldability and increasing the cooling rate.

[0103] As an example, a method for producing the polybutylene terephthalate resin composition of the present invention may include a step of kneading and extruding polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent, and may optionally include the above-mentioned melamine cyanurate.

[0104] In the kneading and extruding steps, the screw rotation speed of the extruder may be, for example, 150 to 330 rpm, 150 to 300 rpm, or 200 to 250 rpm. As long as the above-mentioned range is satisfied, the lower the value, the more improved the rigidity and processability can be.

[0105] The transfer rate per hour (F / R) of the polybutylene terephthalate resin composition fed into the extruder is 70 kg / hr or less, preferably 60 kg / hr or less, more preferably 50 kg / hr or less, and even more preferably 45 to 55 kg / hr. In this case, a balance of physical properties including rigidity, processability, and specific gravity can be achieved.

[0106] <Molded products> According to another embodiment of the present invention, there is provided a molded article made from the polybutylene terephthalate resin composition described above.

[0107] The molded product may be, for example, an automobile electrical component.

[0108] The molded article may specifically be an automobile connector.

[0109] The molded article may have a tensile strength, measured in accordance with ISO 527, of 130 MPa or more, or 135 to 165 MPa.

[0110] The molded article may have a flow index, measured in accordance with ISO 1133 at 265° C. under a load of 2.16 kg, of 4 to 20 g / 10 min, or 4 to 18 g / min.

[0111] The molded article may have a flame retardancy (Burning time / 5 pieces) of 50 seconds or less for 0.8 mm test pieces measured in accordance with UL 94.

[0112] In describing the polybutylene terephthalate resin composition, its production method, and molded products described herein, it is clearly stated that other conditions, equipment, etc. not explicitly described can be appropriately selected within the range commonly used in the art and are not particularly limited.

[0113] The present invention may, however, be embodied in various different forms and should not be construed as being limited to the embodiments set forth herein.

[0114] [Example] In one embodiment of the present invention, the components used in the preparation of the polybutylene terephthalate resin composition are as follows: (A) Polybutylene terephthalate (PBT: intrinsic viscosity 0.5-1 dl / g) (B) Silica-containing reinforcing agent: glass fibers having an average diameter of 10 μm and an average length of 3 mm (B-1) Glass fiber 1: Contains 55% silica by weight (B-2) Glass fiber 2: Contains 48% silica by weight (C) Aluminum salt of diethylphosphinic acid (D) Melamine polyphosphate (E) Melamine cyanurate (F) Aromatic phosphate: Product name PX200 (G) Heat-resistant additive: Product name B-225 (H) Processability improver: Drop point is 110°C, melting point (mp) is 104°C, density (23°C) is 0.97g / cm 3 and the absolute viscosity (120°C) is 410mm 2 / s polyethylene (I) Anti-drop agent: Teflon (product name JF-4A)

[0115] <Examples 1 to 3 and Comparative Examples 1 to 6> The components were mixed in the amounts shown in Table 1 below. The properties of the prepared compositions were measured as follows and are shown in Table 1 below.

[0116] *Flow index (g / 10min): Measured in accordance with ISO 1133.

[0117] The mixture was then fed at 50 kg / hr and the screw speed of the extruder was 250 rpm. At this time, the mixture was extruded at a temperature of 250° C. using a twin-screw extruder with a screw diameter of 45 mm, and the extrudate was produced into pellets.

[0118] The pellets were dried at 100°C for 4 hours or more, and then extruded at 80°C to prepare test pieces with a size of 2.5mm x 50mm x 90mm. The physical properties of the test pieces were measured as follows, and are shown in Table 1 below.

[0119] *Tensile strength (Mpa): Measured in accordance with ISO 527.

[0120] * Flame retardancy (Burning time / 5ea): 0.8mm test pieces were prepared and the total time (sec) required for five test pieces to burn was measured in accordance with UL 94. If the grade was V-0, it was marked as OK and the required time was also recorded, and if the grade did not reach V-0, it was marked as NG.

[0121] *When the tensile strength value is a and the flow index value is b, the calculation value of a / b is shown in Table 1 below.

[0122] [Table 1]

[0123] As can be seen from Table 1, Examples 1 to 3, which include all of the configurations according to the present invention, have a flow index of 4 to 18 g / 10 min, a tensile strength of 135 to 160 MPa, a flame retardancy of V-0, and a total time required for burning of 13.9 to 34 seconds, confirming a good balance of physical properties such as stiffness, processability, and flame retardancy. At this time, the calculated value of a / b was 7.77 to 40, which was confirmed to be within an appropriate range.

[0124] On the other hand, in the case of Comparative Example 1, in which aromatic phosphate and Teflon were used together, it was confirmed that the tensile strength and flow index were decreased, and the calculated value of a / b was also less than 7.76.

[0125] It was confirmed that the tensile strength was poor, the flow index was not measurable, and the calculated a / b value could not be calculated.

[0126] In addition, in the case of Comparative Example 2 in which only the aluminum salt of diethylphosphinic acid was added, and neither melamine polyphosphate nor melamine cyanurate was added, it was confirmed that the tensile strength and flow index were decreased.

[0127] In addition, in the case of Comparative Example 3, in which the content of aluminum salt of diethylphosphinic acid was reduced in the composition of Example 1 and polybutylene terephthalate was added to compensate for this, the tensile strength and flow index were excellent, but the flame retardancy was not measurable.

[0128] In addition, in the case of Comparative Example 4, in which a reinforcing agent with a silica content below the appropriate range was used instead of the composition of Example 2, the flame retardancy was excellent, but the tensile strength and flow index were poor. In this case, the calculated value of a / b was also less than 7.76.

[0129] In addition, in the case of Comparative Example 5, in which the content of the reinforcing agent was reduced in the composition of Example 2 and polybutylene terephthalate was added, the flow index was excellent, but the tensile strength and flame retardancy were poor. In this case, the calculated value of a / b was also less than 7.76.

[0130] In addition, it was confirmed that the flame retardancy was poor in the case of Comparative Example 6, in which the content of aluminum salt of diethylphosphinic acid and the content of melamine cyanurate were changed in the composition of Example 2. In this case, the calculated value of a / b was also less than 7.76.

[0131] In conclusion, it has been confirmed that the polybutylene terephthalate disclosed in the present invention is suitable for use in the field of automotive parts as an alternative material to polyester resin composite materials containing halogen-based flame retardants, as it is reinforced with a silica-containing reinforcing agent and contains flame retardant and heat-resistant components of specific compositions, thereby achieving a balance of physical properties between processability, specific gravity, rigidity, and flame retardancy.

Claims

1. polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent; A polybutylene terephthalate resin composition, characterized by satisfying the following mathematical formula 1. [Formula 1] 7.76≦a / b≦45 (In the above formula 1, a is the tensile strength (MPa) of the polybutylene terephthalate resin composition measured according to ISO 527, and b is the flow index (g / 10 min) of the polybutylene terephthalate resin composition measured according to ISO 1133 at 265° C. under a load of 2.16 kg.)

2. 2. The polybutylene terephthalate resin composition of claim 1, wherein the silica-containing reinforcing agent comprises at least 50% by weight of silica in the reinforcing agent.

3. 2. The polybutylene terephthalate resin composition according to claim 1, wherein the polybutylene terephthalate content is c and the silica-containing reinforcing agent content is d, and the polybutylene terephthalate resin composition satisfies the correlation of 0.5d≦c≦2d.

4. The polybutylene terephthalate resin composition according to claim 1, wherein the polybutylene terephthalate is contained in an amount within a range of 15 to 65% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition includes a processability improver and a heat resistance additive, and the polybutylene terephthalate is contained in an amount within a range of 15 to 65% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

5. The polybutylene terephthalate resin composition according to claim 1, wherein the polybutylene terephthalate has an intrinsic viscosity (η) of 0.5 to 1.25 dl / g as measured in accordance with ASTM D2857.

6. The polybutylene terephthalate resin composition according to claim 1, wherein the silica-containing reinforcing agent is contained in a range of 10 to 50% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition comprises a processability improver and a heat resistance additive, and the silica-containing reinforcing agent is contained in a range of 10 to 50% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

7. The polybutylene terephthalate resin composition according to claim 1, wherein the aluminum salt of diethylphosphinic acid is contained in a range of 5 to 35% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition comprises a processability improver and a heat resistance additive, and the aluminum salt of diethylphosphinic acid is contained in a range of 5 to 35% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, melamine polyphosphate, and the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

8. The polybutylene terephthalate resin composition according to claim 1, wherein the melamine polyphosphate is contained in an amount within a range of 0.1 to 10% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent; or the polybutylene terephthalate resin composition includes a processability improver and a heat resistance additive, and the melamine polyphosphate is contained in an amount within a range of 0.1 to 10% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent, the processability improver, and the heat resistance additive.

9. The polybutylene terephthalate resin composition according to claim 1, wherein the resin composition comprises melamine cyanurate, and the melamine cyanurate is contained in an amount within a range of 0.1 to 10% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, and the melamine cyanurate; or the polybutylene terephthalate resin composition comprises a processability improver and a heat resistance additive, and the processability improver and the heat resistance additive are contained in an amount within a range of 0.1 to 10% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, the melamine cyanurate, the processability improver, and the heat resistance additive.

10. The polybutylene terephthalate resin composition according to claim 1, wherein the resin composition contains a processability improver, and the processability improver is contained in a range of 0.001 to 3 wt % relative to a total of 100 wt % of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, and the silica-containing reinforcing agent plus the processability improver.

11. The polybutylene terephthalate resin composition according to claim 1, wherein the resin composition contains a heat-resistant additive, and the heat-resistant additive is contained in an amount of 0.001 to 3% by weight based on a total of 100% by weight of the polybutylene terephthalate, the aluminum salt of diethylphosphinic acid, the melamine polyphosphate, the silica-containing reinforcing agent, and the heat-resistant additive.

12. A method for producing a polybutylene terephthalate resin composition, comprising the steps of kneading and extruding polybutylene terephthalate, an aluminum salt of diethylphosphinic acid, melamine polyphosphate, and a silica-containing reinforcing agent, wherein the polybutylene terephthalate resin composition satisfies the following mathematical formula 1. [Formula 1] 7.76≦a / b≦45 (In the above formula 1, a is the tensile strength (MPa) of the polybutylene terephthalate resin composition measured according to ISO 527, and b is the flow index (g / 10 min) of the polybutylene terephthalate resin composition measured according to ISO 1133 at 265° C. under a load of 2.16 kg.)

13. A molded article comprising the polybutylene terephthalate resin composition according to any one of claims 1 to 11.

14. The molded article according to claim 13, which is an automobile electrical component.

Citation Information

Patent Citations

  • Flame retardant thermoplastic resin composition

    JP2010024272A

  • Reinforced polyester composition, method for producing the same, and article

    JP2012514112A

  • Polymer composition containing polybutylene terephthalate and flame retardant additives

    JP2012522083A

  • Flame retardant-stabilizer formulations for thermoplastic polymers

    JP2013531117A

  • Flame-retardant thermoplastic molding material

    JP2014511926A