Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery containing same
The addition of specific additives in the non-aqueous electrolyte of lithium-ion batteries forms stable films on electrodes, addressing thermal instability issues and improving high-temperature durability by preventing decomposition and resistance increase.
Patent Information
- Application Number
- JP2024526702
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-07
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-12-08
AI Technical Summary
Lithium-ion secondary batteries face issues with decomposition of non-aqueous electrolytes due to thermal instability, leading to the formation of Lewis acids that cause electrode degradation, increased resistance, and reduced capacity, particularly at high temperatures.
Incorporation of specific additives such as compounds with propargyl groups and cyclic carbonates in the non-aqueous electrolyte to form stable films on the electrode surfaces, preventing decomposition products and enhancing the Solid Electrolyte Interphase (SEI) film, thereby improving high-temperature durability.
The proposed electrolyte composition effectively suppresses side reactions, reduces resistance, and enhances the battery's high-temperature performance by stabilizing the electrode interface and maintaining capacity.
Smart Images

Figure 2024540328000001 
Figure 2024540328000002 
Figure 2024540328000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0180099 filed December 15, 2021 and Korean Patent Application No. 10-2022-0169868 filed December 7, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.
[0002] The present invention relates to a nonaqueous electrolyte for lithium secondary batteries containing an additive that is excellent in removing decomposition products generated from lithium salts and in strengthening the SEI, and to a lithium secondary battery that contains the same and thereby has improved high-temperature durability. [Background technology]
[0003] In recent years, with the development of personal IT devices and computer networks due to the advancement of the information society, society as a whole has become more dependent on electrical energy, and this has created a demand for technological development to efficiently store and utilize electrical energy.
[0004] In particular, with the growing interest in solving environmental problems and realizing a sustainable recycling-based society, extensive research is being conducted on lithium-ion secondary batteries, which are in the spotlight as a clean energy source with low carbon dioxide emissions.
[0005] Lithium-ion secondary batteries can be miniaturized to a degree that makes them suitable for use in personal IT devices, and they have the advantages of having high energy density and operating voltage. They are therefore used not only as power sources for laptops and mobile phones, but also for power storage and electric vehicles.
[0006] On the other hand, a lithium-ion secondary battery includes a positive electrode mainly composed of a lithium-containing transition metal oxide, a negative electrode using a lithium alloy or a carbonaceous material such as graphite, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. The non-aqueous electrolyte is a medium through which Li ions move, and is made by dissolving an electrolyte such as lithium hexafluorophosphate (LiPF6) in an organic solvent with a high dielectric constant such as ethylene carbonate or dimethyl carbonate.
[0007] However, the electrolyte such as lithium hexafluorophosphate (LiPF6) is vulnerable to heat and moisture, and reacts with moisture present in the cell or is thermally decomposed to generate Lewis acids such as PF5. Such Lewis acids not only cause decomposition reactions of organic solvents such as ethylene carbonate, but also erode the passivation film formed at the electrode-electrolyte interface, which can induce additional decomposition of the electrolyte and elution of transition metal ions from the positive electrode.
[0008] The dissolved transition metal ions accelerate the decomposition of the electrolyte and accelerate gas generation, or are re-deposited on the positive electrode, increasing the resistance of the positive electrode. They also migrate to the negative electrode through the electrolyte and are deposited on the negative electrode, causing self-discharge of the negative electrode, destruction and regeneration of the solid electrolyte interphase (SEI), which results in the consumption of additional lithium ions and an increase in resistance.
[0009] Therefore, there is a demand for a non-aqueous electrolyte composition that can remove by-products (such as HF and PF5) generated by the thermal decomposition of lithium salts, and form a stable coating on the surface of the electrode to suppress the elution of transition metals, or suppress the electrodeposition of the eluted transition metal ions onto the negative electrode, thereby improving not only safety but also battery performance such as high-rate charge / discharge characteristics. Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention aims to solve the above problems and provides a non-aqueous electrolyte for a lithium secondary battery, which includes an additive capable of improving the effect of removing decomposition products generated from a lithium salt and the effect of strengthening the SEI.
[0011] The present invention also provides a lithium secondary battery that contains the nonaqueous electrolyte for lithium secondary batteries and thus has improved high-temperature durability. [Means for solving the problem]
[0012] According to one embodiment, the present invention comprises: A lithium salt; A non-aqueous organic solvent; A first additive containing a compound represented by the following chemical formula 1; a second additive comprising vinyl ethylene carbonate (VEC), ethyl di(prop-2-yn-1-yl) phosphate (EDP), or a mixture thereof; The present invention provides a non-aqueous electrolyte solution for a lithium secondary battery, comprising: a cyclic carbonate compound other than vinyl ethylene carbonate (VEC), a compound represented by the following chemical formula 2, or a third additive including a mixture thereof:
[0013] [Chemical formula 1] [ka]
[0014] In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms; R1 to R3 are each independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or -CN.
[0015] [Chemical formula 2] [ka]
[0016] In the above Chemical Formula 2, n is an integer of 1 or 2.
[0017] According to another embodiment, the present invention comprises: A negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and A lithium secondary battery is provided, which contains the nonaqueous electrolyte solution for lithium secondary batteries of the present invention. Effect of the Invention
[0018] The compound represented by Chemical Formula 1 contained in the nonaqueous electrolyte for a lithium secondary battery of the present invention is a Lewis base compound containing a propargyl group (-C≡C-) and a nitrogen element having an unshared electron pair in its structure, and can easily remove Lewis acid generated as a decomposition product of the electrolyte inside the battery during charging and discharging, and can form a strong coating on the surface of the positive electrode to suppress side reactions between the positive electrode and the electrolyte at high temperatures.
[0019] In addition, the non-aqueous electrolyte of the present invention contains the first additive and the second and third additives capable of forming a stable coating on the surface of the electrode, thereby forming a stronger passivation coating on the surface of the electrode, preventing side reactions between the electrode and the electrolyte, and suppressing an increase in resistance. By containing such a non-aqueous electrolyte of the present invention, a lithium secondary battery with improved high-temperature durability can be realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will now be described in more detail. The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0021] In this specification, when words such as "including," "comprises," "consists of," or "has," other parts may be added unless "only" is used. When a component is expressed in the singular, it includes the plural unless otherwise expressly stated. In this specification, "%" means % by weight, unless expressly indicated otherwise.
[0022] In addition, in this specification, the term "alkylene group" refers to a branched or unbranched divalent unsaturated hydrocarbon group. In one embodiment, the alkylene group may be substituted or unsubstituted. The alkylene group includes, but is not limited to, a methylene group, an ethylene group, a propylene group, an isopropylene group, a butylene group, an isobutylene group, a tert-butylene group, a pentylene group, a 3-pentylene group, and the like, each of which may be selectively substituted in other embodiments.
[0023] In general, in lithium secondary batteries, the non-aqueous electrolyte is decomposed during initial charging and discharging to form a coating having passivation ability on the surfaces of the positive and negative electrodes, thereby ensuring high-temperature storage characteristics. However, the coating can be deteriorated by Lewis acid substances such as HF and PF5, which are generated by thermal decomposition of lithium salts (such as LiPF6) widely used in lithium-ion secondary batteries. That is, when a transition metal element is dissolved from the positive electrode due to the attack of the Lewis acid substance, the surface structure changes, the surface resistance of the electrode increases, and the theoretical capacity decreases due to the disappearance of the metal element, which is the redox center, and the expressed capacity may decrease. In addition, the transition metal ions thus dissolved are electrodeposited on the negative electrode, which reacts in a strong reduction potential band, and not only consume electrons, but also destroy the coating during electrodeposition, exposing the surface of the negative electrode, which may cause an additional electrolyte decomposition reaction. As a result, there is a problem that the negative electrode resistance and irreversible capacity increase, and the cell capacity decreases continuously.
[0024] Therefore, the present invention provides a non-aqueous electrolyte solution containing an additive that is excellent in the effect of removing decomposition products generated from lithium salts and in the effect of strengthening the SEI, and a lithium secondary battery containing the same.
[0025] Nonaqueous electrolyte for lithium secondary batteries According to one embodiment, the present invention comprises: A lithium salt; A non-aqueous organic solvent; A first additive containing a compound represented by the following chemical formula 1; a second additive comprising vinyl ethylene carbonate (VEC), ethyl di(prop-2-yn-1-yl) phosphate (EDP), or a mixture thereof; The present invention provides a non-aqueous electrolyte solution for a lithium secondary battery, comprising: a cyclic carbonate compound other than vinyl ethylene carbonate (VEC), a compound represented by the following chemical formula 2, or a third additive comprising a mixture thereof:
[0026] [Chemical formula 1] [ka]
[0027] In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms; R1 to R3 are each independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or -CN.
[0028] [Chemical formula 2] [ka]
[0029] In the above Chemical Formula 2, n is an integer of 1 or 2.
[0030] (1) Lithium salt First, the lithium salt will be described. The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries without any limitations. For example, the cation may be Li + The anion is F. - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - , and SCN - At least one selected from the group consisting of:
[0031] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10, LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2 (lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2 (lithium bis(perfluoroethanesulfonyl)imide, LiBETI), and LiN(SO2CF3)2 (lithium bis(trifluoromethanesulfonyl)imide, LiTFSI), or a mixture of two or more selected from the group consisting of LiPF6 or LiBF4, which have particularly high ionic conductivity.
[0032] Meanwhile, when the organic solvent of the non-aqueous electrolyte is decomposed under high temperature conditions, the decomposition product of the organic solvent reacts with the anion of the lithium salt to generate a Lewis acid by-product. For example, as shown in the following reaction formula, when LiPF6 is used as the lithium salt, a Lewis acid by-product such as PF5 is generated. Such Lewis acid by-product generates by-products including HF through a chain chemical reaction as shown below, which promotes the spontaneous decomposition reaction of the organic solvent and leads to a side reaction that destroys the SEI film formed on the electrode interface.
[0033] [Reaction scheme] [ka]
[0034] On the other hand, the content of the lithium salt may be changed as appropriate within a range that is generally usable, but in order to obtain an optimal effect of forming a coating for preventing corrosion of the electrode surface, the lithium salt may be contained in the electrolyte at a concentration of 0.8 M to 3.0 M, specifically, at a concentration of 1.0 M to 3.0 M.
[0035] When the concentration of the lithium salt satisfies the above range, the viscosity of the nonaqueous electrolyte can be controlled to achieve optimal impregnation, and the mobility of lithium ions can be improved, thereby improving the capacity characteristics and cycle characteristics of the lithium secondary battery.
[0036] (2) Non-aqueous organic solvent The non-aqueous organic solvent is described as follows. As the non-aqueous organic solvent, various organic solvents commonly used in non-aqueous electrolytes may be used without limitation, and there is no limitation on the type of the organic solvent as long as it can minimize decomposition due to an oxidation reaction or the like during the charge / discharge process of the secondary battery and can exhibit the desired properties together with the additives.
[0037] Specifically, the non-aqueous organic solvent may include a cyclic carbonate organic solvent, a linear carbonate organic solvent, a linear ester organic solvent, or a mixture thereof.
[0038] The cyclic carbonate organic solvent is a high-viscosity organic solvent that has a high dielectric constant and effectively dissociates the lithium salt in the non-aqueous electrolyte solution. Specific examples of the cyclic carbonate organic solvent include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and among these, ethylene carbonate may be included.
[0039] The linear carbonate-based organic solvent is an organic solvent having low viscosity and low dielectric constant, and specific examples thereof may include at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically may include ethyl methyl carbonate (EMC).
[0040] The linear ester-based organic solvent is a solvent that is relatively more stable at high temperatures and high voltages than cyclic carbonate-based organic solvents, and can improve the disadvantage of cyclic carbonate-based organic solvents, which cause gas generation when operated at high temperatures, and can achieve high ionic conductivity.
[0041] Specific examples of the linear ester organic solvent include at least one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and specifically, at least one of ethyl propionate and propyl propionate.
[0042] The non-aqueous electrolyte of the present invention may further contain a cyclic ester organic solvent, if necessary. The cyclic ester organic solvent may contain at least one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone. On the other hand, the remainder, excluding the lithium salt and the first to third additives, in the nonaqueous electrolyte solution of the present invention may be a nonaqueous organic solvent, unless otherwise specified.
[0043] (3) First additive The nonaqueous electrolyte for a lithium secondary battery of the present invention may contain a compound represented by the following Chemical Formula 1 as a first additive.
[0044] [Chemical formula 1] [ka]
[0045] In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms; R1 to R3 are each independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or -CN.
[0046] Specifically, the unshared electron pair of the nitrogen element contained in the compound represented by Chemical Formula 1 stabilizes the anion of the lithium salt and suppresses the generation of Lewis acids such as HF and PF5, which are decomposition products of the anion, and the nitrogen element acts as a Lewis base to remove the Lewis acid generated in the electrolyte, thereby suppressing the deterioration behavior of the coating on the surface of the positive electrode or negative electrode caused by the Lewis acid and preventing further decomposition of the electrolyte due to this. As a result, the self-discharge of the secondary battery can be mitigated and the high-temperature storage characteristics can be improved.
[0047] In addition, the compound represented by Formula 1 contains a propargyl functional group in its structure that is easily reduced on the surface of the negative electrode, and forms an SEI film with high passivation ability on the surface of the negative electrode, thereby preventing additional reduction and decomposition reactions of the electrolyte caused by the instability of the SEI film, and improving the high-temperature durability of the negative electrode itself, thereby suppressing the self-discharge reaction of the negative electrode. In particular, the propargyl group contained in the compound represented by Formula 1 can adsorb to the surface of metallic impurities contained in the positive electrode to suppress the elution of the impurities, thereby suppressing the electrodeposition of metal ions on the surface of the negative electrode, thereby preventing internal short circuits.
[0048] Specifically, in the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 or 2 carbon atoms, and R1 to R3 may each independently be a hydrogen atom or an alkyl group having 1 or 2 carbon atoms. In addition, in the above chemical formula 1, R is a substituted or unsubstituted alkylene group having 1 or 2 carbon atoms, and R1 to R3 may each be hydrogen.
[0049] Preferably, the compound represented by Chemical Formula 1 may be a compound represented by Chemical Formula 1a below.
[0050] [Chemical formula 1a] [ka]
[0051] The first additive may be included in an amount of 0.05% by weight to 5% by weight based on the total weight of the nonaqueous electrolyte. When the first additive is contained in the above content range, it is possible to manufacture a secondary battery having improved performance by minimizing disadvantages such as additive-induced side reactions, capacity reduction, and resistance increase while having excellent effect of removing decomposition products of lithium salt.
[0052] Specifically, when the first additive is contained in an amount of 0.05 wt % or more, the HF or PF5 removal effect can be maintained during repeated charging and discharging. Also, when the first additive is contained in an amount of 5.0 wt % or less, side reactions caused by the additive can be prevented, and an increase in the viscosity of the electrolyte can be prevented, thereby suppressing a decrease in ion conductivity due to the increase, and therefore a decrease in rate characteristics during high-temperature storage and low-temperature life characteristics can be prevented. Specifically, the first additive may be included in an amount of 0.05% by weight to 3% by weight based on the total weight of the nonaqueous electrolyte.
[0053] (4) Second additive The nonaqueous electrolyte for a lithium secondary battery of the present invention may further contain a second additive.
[0054] The second additive may include at least one selected from vinyl ethylene carbonate (VEC) represented by the following Chemical Formula 3, ethyl di(prop-2-yn-1-yl)phosphate (EDP) represented by the following Chemical Formula 4, or a mixture thereof.
[0055] [Chemical formula 3] [ka]
[0056] [Chemical formula 4] [ka]
[0057] Vinyl ethylene carbonate (VEC) represented by Chemical Formula 3 can form a robust SEI film containing inorganic components such as Li2CO3 by being reductively decomposed on the surface of the negative electrode. In particular, vinyl ethylene carbonate has the advantage that it is more thermally stable than vinylene carbonate (VC) and therefore undergoes relatively little chemical decomposition even when exposed to high temperatures. Therefore, when used in combination with vinylene carbonate as an additional additive, it can form a stable polymer-type coating (CEI, etc.) by being oxidatively decomposed on the surface of the positive electrode, thereby further enhancing the stabilization of the positive electrode interface. This effect is more evident when a high-content Ni material positive electrode material with a Ni content of 80 atm% or more is used.
[0058] In addition, ethyldi(prop-2-yn-1-yl)phosphate (EDP) represented by the above formula 4, which contains two or more propargyl functional groups and a phosphate functional group in its structure, can be easily reductively decomposed by converting the functional groups into radicals, and can form a high-density stable coating on the surface of the negative electrode. In addition, it can form a stable PO-based coating with excellent Li-ion permeability on the surface of the positive electrode, thereby suppressing an increase in interface resistance.
[0059] Specifically, the second additive of the present invention may contain vinyl ethylene carbonate (VEC) or ethyl di(prop-2-yn-1-yl) phosphate (EDP) represented by the above formula 4, or may contain both vinyl ethylene carbonate (VEC) and ethyl di(prop-2-yn-1-yl) phosphate (EDP).
[0060] When both vinyl ethylene carbonate (VEC) and ethyl di(prop-2-yn-1-yl) phosphate (EDP) are included as the second additive, the vinyl ethylene carbonate (VEC) and ethyl di(prop-2-yn-1-yl) phosphate (EDP) may be included in a weight ratio of 1:1 or 1:3.
[0061] When vinyl ethylene carbonate (VEC) and ethyl di(prop-2-yn-1-yl) phosphate (EDP) are included in the above ratio, the initial film formation effect can be further improved compared to when each additive is used alone, and an SEI film can be sequentially formed depending on the voltage due to the reduction potential difference, thereby forming a more stable and robust multi-layered film.
[0062] In the non-aqueous electrolyte of the present invention, the first additive and the second additive may be contained in a weight ratio of 1:0.5 to 1:60. When the first additive and the second additive are included in the above ratio, the surface tension can be reduced to improve the wettability of the electrolyte, and a stable SEI film can be formed without increasing resistance, thereby suppressing side reactions between the electrode and the electrolyte during charging at high temperatures. Specifically, when the second additive is included in the first additive in a weight ratio of 0.5 or more, a stable SEI film can be formed to suppress side reactions between the electrode and the electrolyte, thereby suppressing the volume increase rate. When the second additive is included in the first additive in a weight ratio of 60 or less, an excessively thick coating can be prevented from being formed on the surface of the electrode, thereby effectively suppressing an increase in initial interface resistance, and preventing a decrease in output. Specifically, the first additive and the second additive may be mixed and used in a weight ratio of 1:0.5 to 1:30, preferably a weight ratio of 1:0.5 to 1:15, and more preferably a weight ratio of 1:1 to 1:10.
[0063] (5) Third additive The nonaqueous electrolyte for a lithium secondary battery of the present invention may further contain a third additive in order to impart a more stable coating formation effect to the surface of the electrode.
[0064] The third additive may include a cyclic carbonate compound other than vinyl ethylene carbonate, a compound represented by the following Chemical Formula 2, or a mixture thereof.
[0065] [Chemical formula 2] [ka]
[0066] In the above Chemical Formula 2, n is an integer of 1 or 2.
[0067] The cyclic carbonate compound may, for example, be vinylene carbonate (VC). The vinylene carbonate can form a stable polymeric coating when the propargyl group, which is a substituent of the first additive, reacts with the first additive to form a radical, and therefore, when the third additive is used, a more stable coating can be formed on the surface of the negative electrode.
[0068] In addition, in the above chemical formula 2, n may be 1. Specifically, the compound represented by Chemical Formula 2 may be 1,3-propane sultone (PS) or 1,4-butane sultone, and preferably 1,3-propane sultone.
[0069] The inclusion of the third additive can stabilize the bulk properties of the electrolyte, improve the film formation effect at the electrode interface, and further improve the strength of the film components, thereby achieving the effect of suppressing lithium precipitation. Therefore, when the third additive is used together with the first and second additives, the durability of the film can be effectively improved.
[0070] The third additive may be included in an amount of 0.01 to 15 wt %, specifically 0.1 to 10 wt %, based on the total weight of the nonaqueous electrolyte. When the third additive is contained in the above range, a secondary battery with further improved performance can be manufactured. For example, when the third additive is contained in an amount of 0.01 wt % or more, the durability of the SEI film can be improved while suppressing the increase in resistance to the maximum extent. When the third additive is contained in an amount of 10 wt % or less, the SEI film can be maintained for a long period of time, excessive side reactions in the electrolyte during charging and discharging of the battery can be prevented, and the presence of unreacted substances in the electrolyte can be prevented, thereby suppressing the increase in resistance due to the unreacted substances.
[0071] (6) Fourth Additive In addition, the non-aqueous electrolyte of the present invention may further contain a fourth additive as necessary to prevent the collapse of the negative electrode caused by decomposition of the non-aqueous electrolyte in a high-power environment, and to further improve low-temperature high-rate discharge characteristics, high-temperature stability, prevention of overcharging, and effect of suppressing battery expansion at high temperatures.
[0072] Examples of the fourth additive include at least one selected from the group consisting of halogen-substituted carbonate compounds, sulfate compounds, phosphate or phosphite compounds, borate compounds, benzene compounds, amine compounds, silane compounds, and lithium salt compounds.
[0073] The halogen-substituted carbonate compounds include fluoroethylene carbonate (FEC). The sulfate compound may be, for example, ethylene sulfate (Esa), trimethylene sulfate (TMS), methyl trimethylene sulfate (MTMS), or the like.
[0074] The phosphate or phosphite compound may be, for example, one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.
[0075] Examples of the borate-based compound include tetraphenylborate, lithium oxalyldifluoroborate (LiODFB) capable of forming a coating on the surface of the negative electrode, and lithium bisoxalateborate (LiB(C2O4)2, LiBOB).
[0076] The benzene-based compound may be fluorobenzene, the amine-based compound may be triethanolamine or ethylenediamine, and the silane-based compound may be tetravinylsilane.
[0077] The lithium salt-based compound is a compound different from the lithium salt contained in the nonaqueous electrolyte, and examples of the lithium salt-based compound include lithium difluorophosphate (LiPO2F2, LiDFP) and LiBF4.
[0078] Among these other additives, in order to form a stronger SEI film on the surface of the negative electrode during the initial activation step, at least one selected from the group consisting of ethylene sulfate, fluoroethylene carbonate (FEC), LiBF4, and lithium oxalyl difluoroborate (LiODFB), which have excellent film-forming effects on the surface of the negative electrode, may be included.
[0079] The fourth additive may be a mixture of two or more compounds, and may be included in an amount of 10 wt % or less based on the total weight of the nonaqueous electrolyte in order to prevent side reactions caused by an excessive amount of the additive.
[0080] Lithium secondary battery In another embodiment of the present invention, there is provided a lithium secondary battery including a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and the nonaqueous electrolyte solution of the present invention.
[0081] The lithium secondary battery of the present invention may be manufactured by forming an electrode assembly in which a positive electrode, a negative electrode, and a separator are sequentially stacked between the positive electrode and the negative electrode, housing the electrode assembly in a battery case, and then introducing the nonaqueous electrolyte of the present invention into the battery case.
[0082] The method for manufacturing the lithium secondary battery of the present invention may be a method for manufacturing a conventional lithium secondary battery well known in the art, and will be described in detail below.
[0083] (1) Positive electrode The positive electrode according to the present invention may include a positive electrode active material layer containing a positive electrode active material, and if necessary, the positive electrode active material layer may further include a conductive material and / or a binder.
[0084] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically may include a lithium composite metal oxide containing lithium and one or more metals such as cobalt, manganese, nickel, and aluminum.
[0085] Specifically, the positive electrode active material may include at least one of lithium-cobalt-based oxides, lithium-manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), and lithium-nickel-manganese-cobalt-based oxides, which have high capacity characteristics and safety of the battery. Specifically, the positive electrode active material may include lithium-cobalt-based oxides, or lithium-nickel-manganese-cobalt-based oxides or lithium-nickel-cobalt-transition metal (M) oxides represented by the following Chemical Formula 5.
[0086] [Chemical formula 5] Li x [Ni y Co z Mnw M 1 v ]O2
[0087] In the above Chemical Formula 5, Said M 1 is a doping element substituted at the transition metal site, and may be one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo.
[0088] The above x means the atomic ratio of lithium to all transition metals in the lithium nickel cobalt manganese oxide, and may be 0.8 to 1.2, preferably 1 to 1.2.
[0089] The y means the atomic ratio of nickel among the transition metals in the lithium nickel cobalt manganese oxide, and is 0.5 or more and less than 1, preferably 0.7 to less than 1, and more preferably 0.75 to 0.98. Since the higher the content of nickel among the transition metals, the higher the capacity that can be achieved, it is more advantageous for realizing a high capacity to have a nickel content of 0.5 or more.
[0090] The above z means the atomic ratio of cobalt among the transition metals in the lithium nickel cobalt manganese oxide, and is more than 0 and less than 0.5, preferably 0.01 to 0.3, and more preferably 0.01 to 0.25.
[0091] The w means the atomic ratio of manganese among the transition metals in the lithium nickel cobalt manganese-based oxide, and is more than 0 and less than 0.5, preferably 0.01 to 0.3, and more preferably 0.01 to 0.25.
[0092] The v is a doping element M doped into the transition metal site in the lithium nickel cobalt manganese oxide. 1This means the atomic ratio of the doping element M, which may be 0 to 0.2, preferably 0 to 0.1. 1 When added, it has the effect of improving the structural stability of the lithium nickel cobalt manganese oxide, but if the content of the doping element increases, the capacity may decrease, so v is preferably contained in an amount of 0.2 or less. Meanwhile, in the above Chemical Formula 1, y+z+w+v=1 may also be satisfied.
[0093] Specific examples of the lithium-nickel-manganese-cobalt-based oxide include Li(Ni 0.5 Co 0.2 Mn 0.3 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.7 Mn 0.1 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, or Li(Ni 0.86 Mn 0.05 Co 0.07 Al 0.02 )O2, and more specifically, Li(Ni 0.7 Mn 0.1 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, or Li(Ni 0.86 Mn 0.05 Co 0.07 Al 0.02 )O2 is more preferred.
[0094] The positive electrode active material may be included in an amount of 80 wt% to 99 wt%, specifically 90 wt% to 99 wt%, based on the total weight of the solid content in the positive electrode slurry. In this case, if the content of the positive electrode active material is 80 wt% or less, the energy density may be reduced, and the capacity may be reduced.
[0095] Furthermore, the conductive material is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and examples of the conductive material that can be used include carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite with highly developed crystal structures; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. The conductive material is usually added in an amount of 1 to 30% by weight based on the total weight of the solid content in the positive electrode active material layer.
[0096] The binder is a component that plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector, and is usually added in an amount of 1 to 30% by weight based on the total weight of the solid content in the positive electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.
[0097] The positive electrode of the present invention as described above may be manufactured by a method for manufacturing a positive electrode well known in the art. For example, the positive electrode may be manufactured by a method of dissolving or dispersing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, which is then coated on a positive electrode current collector, and then dried and rolled to form a positive electrode active material layer, or by a method of casting the positive electrode active material layer on another support, peeling off the support, and laminating the resulting film on the positive electrode current collector.
[0098] The positive electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like may be used.
[0099] The solvent may contain an organic solvent such as N-methyl-2-pyrrolidone (NMP), and may be used in an amount that results in a preferred viscosity when the positive electrode active material, and optionally a binder, a conductive material, etc. are included. For example, it may be included such that the solid content concentration in the active material slurry containing the positive electrode active material, and optionally a binder and a conductive material, is 10% by weight to 90% by weight, preferably 30% by weight to 80% by weight.
[0100] (2) Negative electrode Next, the negative electrode will be described. The negative electrode according to the present invention includes a negative electrode active material layer containing a negative electrode active material, and the negative electrode active material layer may further contain a conductive material and / or a binder, if necessary.
[0101] The negative electrode active material may include a silicon-based active material capable of doping and undoping lithium. Typical examples of the silicon-based active material include Si, SiO x (0 < x < 2), Si-Y alloy (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and combinations thereof, and is not Si), etc. Examples of the element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof. The Si-Y alloy is an alloy in which the content of silicon is the largest among all metal elements with respect to the total amount of the alloy.
[0102] Further, the silicon-based active material may be used as a mixture with a carbon material capable of reversibly intercalating / deintercalating lithium ions.
[0103] As the carbon material capable of reversibly intercalating / deintercalating the lithium ions, any carbonaceous negative electrode active material generally used in lithium ion secondary batteries may be used without particular limitation. Representative examples thereof include crystalline carbon, amorphous carbon, or a combination of these. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite. Examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0104] In addition to this, the negative electrode active material may contain at least one selected from the group consisting of lithium metal, a metal or an alloy of these metals with lithium, and a metal composite oxide.
[0105] As the metal, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals with lithium may be used.
[0106] Examples of the metal composite oxide include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3(0≦x≦1), Li x WO2(0≦x≦1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0<x≦1; 1≦y≦3; 1≦z≦8) selected from the group consisting of may be used. The negative electrode active material may be contained in an amount of 80% to 99% by weight based on the total weight of the solid content in the negative electrode slurry.
[0107] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1 to 20% by weight based on the total weight of the solid content in the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives may be used.
[0108] The binder is a component that aids in bonding between the conductive material, the active material, and the current collector, and is usually added in an amount of 1 to 30% by weight based on the total weight of the solid content in the negative electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.
[0109] The negative electrode may be manufactured by a method for manufacturing a negative electrode well known in the art. For example, the negative electrode may be manufactured by applying a negative electrode active material slurry, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, onto a negative electrode current collector, rolling and drying the slurry to form a negative electrode active material layer, or by casting the negative electrode active material layer onto another support, peeling off the support, and laminating the resulting film onto the negative electrode current collector.
[0110] The negative electrode current collector generally has a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, like the positive electrode current collector, fine irregularities may be formed on the surface to strengthen the binding force of the negative electrode active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0111] The solvent may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a preferred viscosity when the negative electrode active material, and optionally a binder and a conductive material, etc. are contained. For example, the solvent may be contained so that the solid content concentration in the active material slurry containing the negative electrode active material, and optionally a binder and a conductive material, is 50% by weight to 75% by weight, preferably 40% by weight to 70% by weight.
[0112] (3) Separator The separator included in the lithium secondary battery of the present invention may be a commonly used conventional porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, either alone or in a laminated state, or a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, but is not limited thereto.
[0113] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.
[0114] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples of the present invention may be modified in various different forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those having ordinary skill in the art.
[0115] Working Example Example 1. (Manufacture of non-aqueous electrolyte for lithium secondary batteries) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0M, and then 0.1 wt% of the compound represented by formula 1a as a first additive, 0.3 wt% of vinyl ethylene carbonate (hereinafter referred to as "VEC") as a second additive, 3.0 wt% of vinylene carbonate (hereinafter referred to as "VC") and 0.5 wt% of 1,3-propane sultone (hereinafter referred to as "PS") as a third additive, and 1.0 wt% of ethylene sulfate (hereinafter referred to as "Esa") as a fourth additive were added to prepare a non-aqueous electrolyte (see Table 1 below).
[0116] (Secondary battery manufacturing) N-methyl-2-pyrrolidone (NMP) with positive electrode active material Li(Ni 0.86 Mn 0.05 Co 0.07 Al 0.02 A positive electrode slurry (solid content: 50 wt%) was prepared by adding 02, a conductive material (carbon black), and a binder (polyvinylidene fluoride) in a weight ratio of 97.5:1:1.5. The positive electrode slurry was applied to a 12 μm-thick aluminum (Al) thin film, which is a positive electrode current collector, and dried, followed by roll pressing to prepare a positive electrode.
[0117] Anode active material (graphite), binder (SBR-CMC), and conductive material (carbon black) were added to water as a solvent in a weight ratio of 97.5:1.5:1.0 to prepare anode slurry (solid content: 60 wt%). The anode slurry was applied to a copper (Cu) thin film as anode current collector with a thickness of 6 μm, dried, and then roll pressed to prepare anode.
[0118] The positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and a negative electrode were sequentially stacked to prepare an electrode assembly, which was then wound into a jelly-roll shape and housed in a cylindrical battery case. The non-aqueous electrolyte for lithium secondary batteries was then poured into the case to prepare a cylindrical lithium secondary battery having a driving voltage of 4.2 V or more.
[0119] Example 2. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 0.3 wt % of ethyl di(prop-2-yn-1-yl)phosphate (hereinafter referred to as "EDP") as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0120] Example 3. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 0.1 wt % of EDP as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0121] Example 4. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 0.5 wt % of EDP as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0122] Example 5. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 1.0 wt % of EDP as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0123] Example 6. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 3.0 wt % of EDP as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0124] Example 7. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 6.0 wt % of EDP as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0125] Example 8. LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70 to give a concentration of 1.0 M, and then 0.1 wt % of the compound represented by Formula 1a as a first additive, 0.04 wt % of EDP as a second additive, 3.0 wt % of VC and 0.5 wt % of PS as a third additive, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte. A lithium secondary battery was manufactured in the same manner as in Example 1 (see Table 1 below).
[0126] Example 9. Li(Ni) 0.7 Mn 0.1 Co 0.2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used as a positive electrode active material (see Table 1 below).
[0127] Example 10. Li(Ni) 0.6 Mn 0.2 Co 0.2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used as a positive electrode active material (see Table 1 below).
[0128] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and then 0.3 wt % of VEC, 3.0 wt % of VC, 0.5 wt % of PS, and 1.0 wt % of Esa were added to prepare a non-aqueous electrolyte (see Table 2 below).
[0129] Comparative Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and then 0.3 wt % EDP, 3.0 wt % VC, 0.5 wt % PS, and 1.0 wt % Esa were added to prepare a non-aqueous electrolyte (see Table 2 below).
[0130] Comparative Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and then 0.1 wt % of the compound represented by Formula 1a, 3.0 wt % of VC, 0.5 wt % of PS, and 1.0 wt % of Esa as a fourth additive were added to prepare a non-aqueous electrolyte (see Table 2 below).
[0131] Comparative Example 4. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and then 3.0 wt % of VC, 0.5 wt % of PS, and 1.0 wt % of Esa were added to prepare a non-aqueous electrolyte (see Table 2 below).
[0132] Comparative Example 5. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and then 3.0 wt % of VC, 0.5 wt % of PS, 1.0 wt % of Esa, and 1.0 wt % of lithium difluorophosphate (LiDFP) were added to prepare a non-aqueous electrolyte (see Table 2 below).
[0133] Comparative Example 6. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and then 3.0 wt % of VC, 0.5 wt % of PS, 1.0 wt % of Esa, and 5.0 wt % of fluoroethylene carbonate (FEC) were added to prepare a non-aqueous electrolyte (see Table 2 below).
[0134] Comparative Example 7. Li(Ni) 0.7 Mn 0.1 Co 0.2 A lithium secondary battery was manufactured in the same manner as in Comparative Example 1, except that O2 was used as a positive electrode active material (see Table 2 below).
[0135] Comparative Example 8. Li(Ni) 0.6 Mn 0.2 Co 0.2 A lithium secondary battery was manufactured in the same manner as in Comparative Example 1, except that O2 was used as a positive electrode active material (see Table 2 below).
[0136] [Table 1] [Table 1]
[0137] [Table 2] [Table 2]
[0138] In Tables 1 and 2, the abbreviations of the respective compounds have the following meanings. VEC: Vinyl ethylene carbonate EDP: Ethyl di(prop-2-yn-1-yl) phosphate VC: Vinylene carbonate PS: 1,3-propane sultone Esa: Ethylene sulfate LiDFP: Lithium difluorophosphate FEC: Fluoroethylene carbonate NCM 712:Li(Ni 0.7 Mn 0.1 Co 0.2 )O2 NCM 622:Li(Ni 0.6 Mn 0.2 Co 0.2 )O2
[0139] Experimental Example Experimental example 1: Evaluation experiment of volume increase rate The lithium secondary batteries prepared in Examples 1 to 10 and the lithium secondary batteries prepared in Comparative Examples 1 to 8 were each charged to 4.2 V at 0.33 C, and then the initial volume was measured by Archimedes' method using distilled water after charging was completed.
[0140] Next, each of the lithium secondary batteries was stored at 60° C. for 12 weeks under 100% SOC, and the volume increase rate of the lithium secondary battery after high temperature storage relative to the initial volume was measured by Archimedes' method, and the measured volume change was calculated in percentage (%) and shown in Table 3 below.
[0141] [Table 3] [Table 3]
[0142] Referring to Table 3, the volume increase rate of the lithium secondary batteries prepared in Examples 1 to 10 including the nonaqueous electrolyte of the present invention after high temperature storage was 3.5% or less, which was significantly reduced compared to the lithium secondary batteries of Comparative Examples 1 to 8.
[0143] Meanwhile, the volume increase rate of the lithium secondary battery of Example 8, which contained a slightly smaller amount of the second additive, after high temperature storage was 3.5%, which was slightly increased compared to the lithium secondary batteries prepared in Examples 1 to 7.
[0144] Meanwhile, referring to Table 3, the positive electrode active material is Li(Ni 0.7 Mn 0.1 Co 0.2 In the case of the lithium secondary battery of Example 9 including the positive electrode containing Li(Ni)O2 and the nonaqueous electrolyte of the present invention, the volume increase rate after high-temperature storage was reduced by about 65% compared to the lithium secondary battery of Comparative Example 7. 0.6 Mn 0.2 Co 0.2 In the case of the lithium secondary battery of Example 10 including the positive electrode containing Li(Ni)O2 and the nonaqueous electrolyte of the present invention, the volume increase rate after high-temperature storage was reduced by about 75% compared to the lithium secondary battery of Comparative Example 8. 0.86 Mn 0.05 Co 0.07 Al 0.02 In the case of the lithium secondary battery of Example 1, which uses a positive electrode containing O2 in combination with the nonaqueous electrolyte of the present invention, the volume increase rate after high temperature storage is reduced by about 80% or more compared to the lithium secondary battery of Comparative Example 1, which uses a nonaqueous electrolyte containing only the second and third additives, excluding the first additive. Based on this result, it can be seen that the effect of suppressing the volume increase rate is further improved when a positive electrode containing a positive electrode active material with a nickel content of 80 atm% or more is used in combination with the nonaqueous electrolyte of the present invention.
[0145] Experimental Example 2. Resistance increase rate during high temperature storage The secondary batteries manufactured in Examples 1 to 7, 9, and 10 and the secondary batteries manufactured in Comparative Examples 1 to 8 were activated at 0.1 C CC and then degassed.
[0146] Next, the battery was charged at 0.33 C CC up to 4.20 V under constant current-constant voltage (CC-CV) charging conditions at 25°C, and then pulse discharged at a 2.5 C rate with an SOC of 50%. The voltage drop over 10 seconds was measured to determine the initial resistance.
[0147] Next, after storing at a high temperature of 60° C. for 12 weeks, the battery was charged to 50% SOC and then pulse discharged at a rate of 2.5 C to measure the voltage drop for 10 seconds to obtain the resistance value after high temperature storage, and the resistance increase rate (%) relative to the initial resistance was calculated and shown in Table 4. The voltage drop was measured using a PNE-0506 charger / discharger (manufacturer: PNE solution Co., Ltd., 5V, 6A).
[0148] [Table 4] [Table 4]
[0149] Referring to Table 4, it can be seen that the resistance increase rate after high-temperature storage of the lithium secondary batteries prepared in Examples 1 to 7, 9, and 10 including the nonaqueous electrolyte of the present invention is about 7.1% or less, which is significantly improved compared to the lithium secondary batteries of Comparative Examples 1 to 8. That is, the secondary batteries of the Examples including the nonaqueous electrolyte of the present invention form a stable SEI film on the surface of the electrode, and can suppress film destruction at high temperatures even when the battery is exposed to high temperatures. Therefore, it is believed that the secondary batteries of the Examples including the nonaqueous electrolyte of the present invention have an excellent effect of suppressing resistance increase even after high-temperature storage because there is little decomposition of the additional electrolyte due to film destruction.
[0150] Meanwhile, referring to Table 4, the positive electrode active material is Li(Ni 0.7 Mn 0.1 Co 0.2 In the case of the lithium secondary battery of Example 9 containing a positive electrode containing Li(Ni)O2 and the nonaqueous electrolyte of the present invention, the resistance increase rate was reduced by about 54% compared to the lithium secondary battery of Comparative Example 7. 0.6 Mn 0.2 Co 0.2In the case of the lithium secondary battery of Example 10 containing a positive electrode containing Li(Ni)O2 and the nonaqueous electrolyte of the present invention, the resistance increase rate was reduced by about 58% compared to the lithium secondary battery of Comparative Example 8. 0.86 Mn 0.05 Co 0.07 Al 0.02 In the case of the lithium secondary battery of Example 1, which uses a positive electrode containing O2 in combination with the nonaqueous electrolyte of the present invention, the resistance increase rate was reduced by about 59% or more compared to the lithium secondary battery of Comparative Example 1, which uses a nonaqueous electrolyte containing only the second and third additives, excluding the first additive. From this result, it can be seen that the effect of suppressing the resistance increase rate is further improved when a positive electrode containing a positive electrode active material with a nickel content of 80 atm% or more is used in combination with the nonaqueous electrolyte of the present invention.
[0151] Experimental Example 3. Evaluation of initial resistance The lithium secondary batteries prepared in Examples 1 to 7 and Comparative Example 6 were each activated at 0.1 CCC and then degassed.
[0152] Next, the battery was charged at 0.33 C CC up to 4.20 V under constant current-constant voltage (CC-CV) charging conditions at 25° C., and then pulse discharged at a 2.5 C rate under 50% SOC conditions to measure the voltage drop for 10 seconds to obtain the initial resistance. The measured initial resistance values are shown in Table 5 below.
[0153] [Table 5] [Table 5]
[0154] Referring to Table 5, the initial resistance value of the lithium secondary batteries prepared in Examples 1 to 5 using the nonaqueous electrolyte of the present invention is 17.5% or less. In contrast, the initial resistance value of the lithium secondary battery of Comparative Example 6, which did not contain any of the first and second additives of the present invention, was 21.4%, which was significantly increased compared to the lithium secondary batteries manufactured in Examples 1 to 5.
[0155] On the other hand, the initial resistance values of the lithium secondary batteries of Examples 6 and 7, which contained a slightly larger amount of the second additive, were 20.3% and 27.7%, respectively, which was significantly increased compared to the lithium secondary batteries prepared in Examples 1 to 5.
Claims
1. A lithium salt; A non-aqueous organic solvent; A first additive including a compound represented by the following chemical formula 1: a second additive comprising vinyl ethylene carbonate (VEC), ethyl di(prop-2-yn-1-yl) phosphate (EDP), or a mixture thereof; a third additive including a cyclic carbonate compound other than vinyl ethylene carbonate (VEC), a compound represented by the following chemical formula 2, or a mixture thereof; A non-aqueous electrolyte for a lithium secondary battery, comprising: [Chemical formula 1] 【Chemistry 1】 In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms; R 1 ~R 3 are each independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or -CN; [Chemical formula 2] 【Chemistry 2】 In the above Chemical Formula 2, n is an integer of 1 or 2.
2. R is a substituted or unsubstituted alkylene group having 1 or 2 carbon atoms, R 1 ~R 3 and each independently represent a hydrogen atom or an alkyl group having 1 or 2 carbon atoms.
3. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Chemical Formula 1 is a compound represented by the following Chemical Formula 1a: [Chemical formula 1a] 【Chemistry 3】
4. 2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the first additive is included in an amount of 0.05 to 5 wt % based on the total weight of the non-aqueous electrolyte.
5. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the first additive and the second additive are contained in a weight ratio of 1:0.5 to 1:
60.
6. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the first additive and the second additive are contained in a weight ratio of 1:0.5 to 1:
30.
7. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the first additive and the second additive are contained in a weight ratio of 1:0.5 to 1:
15.
8. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the second additive is ethyldi(prop-2-yn-1-yl)phosphate (EDP).
9. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the cyclic carbonate compound is vinylene carbonate (VC).
10. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Formula 2 is 1,3-propane sultone (PS) or 1,4-butane sultone.
11. 2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the third additive is a mixture containing vinylene carbonate (VC) and a compound represented by Chemical Formula 2:
12. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, further comprising at least one fourth additive selected from the group consisting of halogen-substituted carbonate-based compounds, sulfate-based compounds, phosphate-based or phosphite-based compounds, borate-based compounds, benzene-based compounds, amine-based compounds, silane-based compounds, and lithium salt-based compounds.
13. A negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and A non-aqueous electrolyte for a lithium secondary battery is included, The nonaqueous electrolyte solution is A lithium salt; A non-aqueous organic solvent; A first additive including a compound represented by the following chemical formula 1: a second additive comprising vinyl ethylene carbonate (VEC), ethyl di(prop-2-yn-1-yl) phosphate (EDP), or a mixture thereof; a third additive including a cyclic carbonate compound other than vinyl ethylene carbonate (VEC), a compound represented by the following chemical formula 2, or a mixture thereof; Lithium secondary batteries, including: [Chemical formula 1] 【Chemistry 4】 In the above Chemical Formula 1, R is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms; R 1 ~R 3 are each independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or -CN; [Chemical formula 2] 【Chemistry 5】 In the above Chemical Formula 2, n is an integer of 1 or 2.
14. 14. The lithium secondary battery according to claim 13, wherein the positive electrode comprises a positive electrode active material made of a lithium transition metal oxide containing lithium and one or more metals selected from cobalt, manganese, nickel, and aluminum.
15. The lithium secondary battery according to claim 13, wherein the first additive and the second additive are contained in a weight ratio of 1:0.5 to 1:60.
Citation Information
Patent Citations
Nonaqueous electrolyte for lithium ion batteries and lithium ion batteries
JP2019537814A
Double pipe for transferring plating chemicals with joint type external pipe