Optical film and display device including same

The integration of a polymer resin and malonate ultraviolet absorber in optical films addresses the issue of light-induced yellowing and color change, ensuring excellent light resistance and visibility in display devices.

JP2024544282AActive Publication Date: 2024-11-28KOLON INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024535646
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-16
Filing Date
2022-09-19
Publication Date
2024-11-28
Estimated Expiration
2042-09-19

AI Technical Summary

Technical Problem

Optical films containing polymeric resins used as cover windows in display devices suffer from high initial yellowing and color change due to light exposure over time, lacking sufficient light resistance.

Method used

Incorporating a light-transmitting base material with a polymer resin and a malonate ultraviolet absorber, such as Tetraethyl 2,2'-(1,4-phenylenedimethyldiyne) bismalonate, to achieve a yellowness of 5.0 or less and a color change (ΔE* ab) of 3.5 or less, with a maximum absorbance of 0.45 or more in the UVA region (315 to 400 nm).

Benefits of technology

The optical film exhibits excellent light resistance, maintaining minimal color change and high visibility even after prolonged exposure to UV light, extending the lifespan of the display device cover window.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544282000001_ABST
    Figure 2024544282000001_ABST
Patent Text Reader

Abstract

The present invention relates to a light-transmitting substrate having a yellowness index of 5.0 or less before a lightfastness test and a color change (ΔE* ab The present invention provides an optical film and a display device including the same, in which the refractive index is 3.5 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film and a display device including the same. [Background technology]

[0002] In recent years, with the trend toward thinner, lighter, and more flexible display devices, the use of optical films containing polymer resins instead of glass as cover windows has been considered. In order for an optical film to be used as a cover window of a display device, it is necessary for it to have excellent optical and mechanical properties.

[0003] On the other hand, optical films containing polymer resins have problems in that they have a high initial yellowing degree or the color of the optical films changes over time when exposed to light.

[0004] Therefore, there is a demand for the development of films that have excellent mechanical properties such as insolubility, chemical resistance, and heat resistance, as well as excellent optical properties such as light resistance. Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, an object of one embodiment of the present invention is to provide an optical film having excellent light resistance.

[0006] Another embodiment of the present invention has an object to provide a display device including an optical film having excellent light resistance. [Means for solving the problem]

[0007] One embodiment of the present invention includes a light-transmitting substrate, and has a yellowness index of 5.0 or less before lightfastness testing and a color change (ΔE* ab ) is 3.5 or less.

[0008] The light resistance test was performed using a xenon lamp, a daylight filter, 12 kW, 0.8 W / m 2 @420nm, 30℃ / 30RH% Chamber, 55℃ Black Panel for 300 hours. ab ) is calculated using the following formula 1.

[0009] [Formula 1] ΔE* ab = [(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2

[0010] In the above formula 1, ΔL* is the difference in L* before and after the light fastness test, Δa* is the difference in a* before and after the light fastness test, and Δb* is the difference in b* before and after the light fastness test.

[0011] The light-transmitting substrate may include a polymer resin and a malonate-based ultraviolet absorbing agent.

[0012] The ultraviolet absorbing agent may have a maximum absorbance of 0.45 or more in the UVA region (315 to 400 nm) when dissolved in DAMc (dimethylacetamide) at a concentration of 0.001 wt %.

[0013] The ultraviolet absorber may include a compound represented by the following Chemical Formula 2.

[0014] [Chemical formula 2] JPEG2024544282000002.jpg3968

[0015] In the above formula 2, R 1 , R 2 , R 3 and R 4are each independently a hydrogen atom, a halogen element, a phenyl group, or a C1 to C10 linear, branched or alicyclic alkyl group; Y is a divalent aromatic or hetero organic group having 6 to 40 carbon atoms; and a hydrogen atom in the organic group included in Chemical Formula 2 may be substituted with (1) a halogen element, (2) a hydrocarbon group, (3) a halogen-substituted hydrocarbon group, or (4) a hydrocarbon group substituted with a halogen element, oxygen or nitrogen.

[0016] The ultraviolet absorber may include tetraethyl 2,2'-(1,4-phenylenedimethylidyne) bismalonate.

[0017] The light-transmitting substrate may contain 1 to 10 parts by weight of the ultraviolet absorbing agent relative to 100 parts by weight of the polymer resin.

[0018] The polymeric resin may include at least one of imide repeat units and amide repeat units.

[0019] The optical film may have a light transmittance of 88.5% or more after a light resistance test, and may have a haze of 1.0 or less after a light resistance test.

[0020] Another embodiment of the present invention provides a display device including a display panel and the optical film disposed on the display panel. Effect of the Invention

[0021] According to one embodiment of the present invention, an optical film having excellent light resistance in the UVA region (315 to 400 nm) can be provided.

[0022] According to another embodiment of the present invention, a display device including an optical film having excellent light resistance in the UVA region (315 to 400 nm) can be provided. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a cross-sectional view of an optical film (100) according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view of an optical film (101) further comprising a primer layer (120). [Diagram 3] FIG. 2 is a cross-sectional view of an optical film (102) further comprising a hardcoat layer (130). [Figure 4] FIG. 2 is a cross-sectional view showing a portion of a display device (200) according to another embodiment of the present invention. [Diagram 5] FIG. 5 is an enlarged cross-sectional view of part “P” in FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, the embodiments of the present invention will be described in detail. However, the examples described below are presented for illustrative purposes to help a clear understanding of the present invention, and are not intended to limit the scope of the present invention.

[0025] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining the embodiments of the present invention are merely illustrative, and the present invention is not limited to the matters shown in the drawings. The same components may be designated by the same reference symbols throughout the specification. In explaining the present invention, if a detailed description of related publicly known techniques is deemed to unnecessarily obscure the gist of the present invention, the detailed description will be omitted.

[0026] When the terms "including," "having," "performed," etc. are used in this specification, other parts may be added unless the expression "only" is used. When a constituent feature is expressed in the singular, it includes the plural unless otherwise expressly stated. In addition, when interpreting a constituent feature, it is interpreted as including a margin of error even if there is no other express description.

[0027] When describing a positional relationship between two parts, for example "on top of", "above", "below", "beside", etc., one or more other parts may be located between the two parts, unless the words "immediately" or "directly" are used.

[0028] Spatially relative terms such as "below," "beneath," "lower," "above," "upper," and the like, may be used to facilitate describing the relationship of one element or component to another element or component as depicted in the drawings. Spatially relative terms should be understood as terms that include different orientations of the elements in use or operation in addition to the orientation depicted in the drawings. For example, if an element depicted in the drawings is turned over, an element described as "below" or "beneath" another element may be disposed "above" the other element. Thus, the exemplary term "below" can include both an orientation of below and above. Similarly, the exemplary terms "above" or "upper" can include both an orientation of above and below.

[0029] When describing a temporal relationship, for example, when describing a temporal precedence / subsequence relationship such as "after", "following", "next to", or "before", it can also include cases where the relationship is not consecutive, unless the words "immediately" or "directly" are used.

[0030] Although the terms "first", "second" and the like are used to describe various constituent elements, these constituent elements are not limited by these terms. These terms are used merely to distinguish one constituent element from another. Thus, the first constituent element referred to below may be the second constituent element within the scope of the technical idea of ​​the present invention.

[0031] The term "at least one" should be understood to include all possible combinations of one or more of the associated items. For example, "at least one of a first item, a second item, and a third item" means not only each of the first item, the second item, or the third item, but also all possible combinations of items that can be present from two or more of the first item, the second item, and the third item.

[0032] The features of the various embodiments of the present invention may be partially or fully combined or combined with each other, may be technically linked and driven in various ways, and may be implemented independently of each other or may be implemented together in a linked relationship.

[0033] Before describing the present invention in detail below, it should be understood that the terms used herein are for the purpose of describing particular embodiments, and are not intended to be limited solely by the scope of the appended claims. All technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art, unless otherwise specified.

[0034] Furthermore, in interpreting the terms and words used in the present specification and claims hereinafter, in accordance with the principle that an inventor can appropriately define the concept of a term in order to best explain his / her invention, the terms and words should not necessarily be interpreted in a limited way to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that is consistent with the technical idea of ​​the present invention as described in this specification.

[0035] One embodiment of the present invention provides an optical film 100. Figure 1 is a cross-sectional view of an optical film 100 according to one embodiment of the present invention.

[0036] As shown in FIG. 1, an optical film (100) according to one embodiment of the present invention includes a light-transmitting substrate (110).

[0037] The optical film (100) according to one embodiment of the present invention has a yellowness index of 5.0 or less before the light resistance test and a color change (ΔE* ab ) is less than or equal to 3.5.

[0038] The yellowness before the light fastness test can be measured using a spectrophotometer. Specifically, the yellowness of the optical film can be measured using a spectrophotometer, such as a KONICA MINOLTA spectrophotometer (model name: CM-3700D) device, according to the standard ASTM E313.

[0039] The light resistance test is carried out using a xenon lamp, for example, a SUNTEST XXL+ instrument manufactured by ATLAS, with a daylight filter at 420 nm and a light output of 0.8 W / m 2 12kW (12kW0.8W / m 2 The test was carried out for 300 hours under the conditions of @420 nm, 30°C and 30% relative humidity (30°C / 30RH% Chamber), and 55°C black panel. ab ) is calculated using the following formula 1.

[0040] [Formula 1] ΔE* ab = [(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2

[0041] In the above formula 1, ΔL* is the difference in L* before and after the light fastness test, Δa* is the difference in a* before and after the light fastness test, and Δb* is the difference in b* before and after the light fastness test.

[0042] The L*, a*, and b* of the optical film (100) before the lightfastness test can be measured using a color difference meter. Specifically, the optical film (100) is measured three times for L*, a*, and b* using a color difference meter, for example, a KONICA MINOLTA color difference meter (model name: CM-3600A) device, with a D65 light source, a viewing angle of 2°, and transmission mode, and the average values ​​of the three measurements are calculated to be the L*, a*, and b* of the optical film (100). The L*, a*, and b* after the lightfastness test can be measured using the same method as the measurement method of L*, a*, and b* before the lightfastness test after the lightfastness test.

[0043] The yellowing index of the optical film (100) before the light resistance test is 5.0 or less, and the color change (ΔE* ab ) is 3.5 or less, the optical film (100) has excellent visibility and light resistance, especially UV light resistance, and is suitable for use as a cover window of a display device. Since the polymer resin contained in the light-transmitting substrate (110) of the optical film (100) has a large amount of aromatic rings, the optical film (100) changes color when exposed to ultraviolet (UV) wavelength light for a long period of time. As a result, the color reproducibility and clarity of the optical film (100) decrease over time, and the visibility decreases. On the other hand, an optical film (100) with excellent UV light resistance changes color little even when exposed to ultraviolet (UV) wavelength light, and therefore the life of the cover window of a display device can be extended.

[0044] The light-transmitting substrate (110) of one embodiment of the present invention may include a polymeric resin and an ultraviolet light absorber.

[0045] The polymer resin has excellent bending properties and impact resistance, and is therefore suitable for use as a cover window of a flexible display device. The polymer resin may be included in the film in various shapes and forms, such as a solid powder form, a form dissolved in a solution, or a matrix form solidified after dissolving in a solution, and any resin containing the same repeating unit as that of the present invention, regardless of its shape and form, can be regarded as the same as the polymer resin of the present invention. In general, the polymer resin in the film may be present in the form of a matrix formed by applying a polymer resin solution and then drying and solidifying it.

[0046] The polymer resin according to one embodiment of the present invention may be any light-transmitting resin. For example, it may include at least one selected from cycloolefin derivatives, cellulose polymers, ethylene vinyl acetate copolymers, polyester polymers, polystyrene polymers, polyamide polymers, polyamideimide polymers, polyetherimide polymers, polyacrylic polymers, polyimide polymers, polyethersulfone polymers, polysulfone polymers, polyethylene polymers, polypropylene polymers, polymethylpentene polymers, polyvinyl chloride polymers, polyvinylidene chloride polymers, polyvinyl alcohol polymers, polyvinyl acetal polymers, polyether ketone polymers, polyether ether ketone polymers, polymethyl methacrylate polymers, polyethylene terephthalate polymers, polybutylene terephthalate polymers, polyethylene naphthalate polymers, polycarbonate polymers, polyurethane polymers, and epoxy polymers. Preferably, the polymer resin according to one embodiment of the present invention may include at least one of polyimide polymers, polyamide polymers, and polyamideimide polymers. In particular, polyimide-based polymers, polyamide-based polymers, and polyamideimide-based polymers are excellent not only in physical properties such as thermal properties, hardness, abrasion resistance, and flexibility, but also in optical properties such as light transmittance and haze, and it is preferable that the light-transmitting substrate (110) of the optical film (100) used as the cover window of a display device contains at least one of polyimide-based polymers, polyamide-based polymers, and polyamideimide-based polymers, although the present invention is not limited thereto.

[0047] According to an embodiment of the present invention, the light-transmitting substrate (110) may include a polymer resin containing at least one of an imide repeating unit and an amide repeating unit. In the present invention, the imide repeating unit refers to a repeating unit generated by imidization of a diamine compound and a dianhydride compound, and the amide repeating unit refers to a repeating unit generated by reaction of a diamine compound and a dicarbonyl compound. The light-transmitting substrate (110) may be any one of a polyimide substrate, a polyamide substrate, and a polyamideimide substrate. However, the embodiment of the present invention is not limited thereto, and any substrate having light transmittance may be the light-transmitting substrate (110) according to the embodiment of the present invention.

[0048] According to one embodiment of the present invention, the light-transmitting substrate (110) may include an ultraviolet absorbing agent. The ultraviolet absorbing agent may include a malonate compound. That is, the light-transmitting substrate (110) according to one embodiment of the present invention may include a malonate ultraviolet absorbing agent.

[0049] The malonate compound of the present invention is a compound containing a malonate substituent, and the malonate substituent has a structure represented by the following chemical formula 1. That is, the malonate compound refers to a compound containing a structure represented by the following chemical formula 1.

[0050] [Chemical formula 1] JPEG2024544282000003.jpg3335

[0051] In the above formula 1, R 1 and R 2 are each independently a hydrogen atom, a halogen element, a phenyl group, or a C1 to C10 linear, branched, or alicyclic alkyl group.

[0052] Malonate compounds are excellent in minimizing an increase in initial yellowness of the optical film (100) and improving the light resistance of the optical film (100), and when included as an ultraviolet absorber, they can minimize color change when the optical film (100) is exposed to light.

[0053] According to one embodiment of the present invention, the ultraviolet absorbent may have a maximum absorbance of 0.45 or more in the UVA region (315 to 400 nm) when dissolved in DAMc at a concentration of 0.001 wt %.

[0054] The maximum absorbance of the ultraviolet absorbent in the UVA region (315-400 nm) can be measured using an ultraviolet spectrophotometer. Specifically, the ultraviolet absorbent is dissolved in DMAc (N,N-Dimethylacetamide) at a concentration of 0.001 wt%, and the absorbance in the UVA region (315-400 nm) is measured using an ultraviolet spectrophotometer, for example, a Shimadzu ultraviolet spectrophotometer (model name: UV-1800) device, and the maximum value of the absorbance measured in the UVA region (315-400 nm) is the maximum absorbance of the ultraviolet absorbent in the UVA region (315-400 nm).

[0055] When the maximum absorbance of the ultraviolet absorber in the UVA region (315-400 nm) is 0.45 or more, the increase in the initial yellowing of the optical film (100) is minimized and the light fastness is improved so that the initial yellowing is 5.0 or less, and the color change (ΔE* ab ) can be made to be 3.5 or less.

[0056] According to one embodiment of the present invention, the ultraviolet absorber may contain at least two or more structures represented by Chemical Formula 1. That is, the ultraviolet absorber may contain at least two or more malonate substituents.

[0057] When the UV absorber contains two or more malonate substituents, the absorbance of the UV absorber is increased and may have a maximum absorbance of 0.45 or greater in the UVA region (315-400 nm).

[0058] According to one embodiment of the present invention, the ultraviolet absorber may include a compound represented by the following Chemical Formula 2:

[0059] [Chemical formula 2] JPEG2024544282000004.jpg3968

[0060] In the above formula 2, R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, a halogen element, a phenyl group, or a C1 to C10 linear, branched or alicyclic alkyl group; Y is a divalent aromatic organic group or hetero organic group having 6 to 40 carbon atoms; and a hydrogen atom in the organic group included in Chemical Formula 2 may be substituted with (1) a halogen element, (2) a hydrocarbon group, (3) a halogen-substituted hydrocarbon group, or (4) a hydrocarbon group substituted with a halogen element, oxygen or nitrogen.

[0061] In the above Chemical Formula 2, Y may include, for example, a structure represented by any one of the structural formulas represented by Chemical Formula 3 below.

[0062] [Chemical formula 3] JPEG2024544282000005.jpg109119

[0063] In the structural formula of Chemical Formula 3, * indicates a bonding position. In the structural formula, Z may independently be any one of a single bond, O, S, SO2, CO, and (C=C)n, where n may be an integer of 1 to 5. The bonding position of Z to each ring is not particularly limited, but the bonding position of Z may be, for example, an ortho or para position to each ring. The hydrogen atom in the structural formula of Chemical Formula 3 may be substituted by (1) a halogen element, (2) a hydrocarbon group, (3) a halogen-substituted hydrocarbon group, or (4) a halogen element, oxygen, or nitrogen-substituted hydrocarbon group. In Chemical Formula 3, each structural formula may be a heterocyclic organic group in which one or more carbons in the structural formula are substituted by an element such as nitrogen (N), sulfur (S), or oxygen (O).

[0064] According to one embodiment of the present invention, the UV absorber may include Tetraethyl 2,2'-(1,4-phenylenedimethylidyne)bismalonate.

[0065] According to one embodiment of the present invention, the light-transmitting substrate may contain 1 to 10 parts by weight of an ultraviolet absorbing agent based on 100 parts by weight of the polymer resin.

[0066] When the UV absorber is less than 1 part by weight per 100 parts by weight of polymer resin, the effect of improving light resistance is negligible, so the color change (ΔE* ab On the other hand, if the UV absorber is contained in an amount of more than 10 parts by weight per 100 parts by weight of the polymer resin, the initial yellowness index before the light fastness test will exceed 5.0, and there is a possibility that the problem of elution will occur during long-term storage.

[0067] According to one embodiment of the present invention, the optical film (101) may further include a primer layer (120) above the light-transmitting substrate (110). Figure 2 is a cross-sectional view of the optical film (101) further including a primer layer (120).

[0068] As shown in FIG. 2, the optical film (101) further including a primer layer (120) may be laminated in the order of the light-transmitting substrate (110) and the primer layer (120).

[0069] The primer layer (120) of the present invention may include a curable resin. According to one embodiment of the present invention, the curable resin may include at least one selected from an acrylic resin, a urethane resin, and a siloxane resin.

[0070] According to one embodiment of the present invention, the primer layer (120) of the present invention may further include at least one of an ultraviolet absorber and a pigment.

[0071] According to one embodiment of the present invention, the primer layer (120) may contain the same malonate UV absorber as the light-transmitting substrate (110), or may contain other UV absorbers in addition to the malonate UV absorber. The present invention is not limited thereto.

[0072] According to one embodiment of the present invention, the pigment may include a copper phthalocyanine-based compound. However, the present invention is not limited thereto, and other pigments besides the copper phthalocyanine-based compound may be used.

[0073] According to one embodiment of the present invention, the primer layer (120) may have a thickness of 0.1 to 10 μm. Preferably, the primer layer (120) may have a thickness of 1 to 5 μm. However, the present invention is not limited thereto.

[0074] According to one embodiment of the present invention, the optical film (102) may further include a hard coat layer (130) on the light-transmitting substrate (110). Figure 3 is a cross-sectional view of the optical film (102) further including a hard coat layer (130).

[0075] As shown in FIG. 3, the optical film (102) further including a hard coat layer (130) may be laminated in the order of the light-transmitting substrate (110) and the hard coat layer (130).

[0076] The hard coat layer (130) is a layer that protects the optical film (102) or the adherend to which the optical film (101) is attached from the external environment, and according to one embodiment of the present invention, the hard coat layer (130) may contain at least one of a siloxane-based resin, an acrylic-based resin, a urethane-based resin, and an epoxy-based resin.

[0077] According to one embodiment of the present invention, the hard coat layer (130) may have a thickness of 1 to 10 μm, and preferably has a thickness of 1 to 5 μm, although the present invention is not limited thereto.

[0078] According to one embodiment of the present invention, the optical film may further include both a primer layer (120) and a hard coat layer (130) (not shown) on the light-transmitting substrate (110). The optical film further including the primer layer (120) and the hard coat layer (130) may be laminated in the order of the light-transmitting substrate (110), the primer layer (120), and the hard coat layer (130).

[0079] According to one embodiment of the present invention, the optical film 100 may have optical transparency and flexibility properties, for example, the optical film according to one embodiment of the present invention may have bending, folding and rollable properties.

[0080] According to one embodiment of the present invention, the optical film (100) may have a light transmittance of 88.5% or more before a light fastness test, and a haze of 0.4 or less before a light fastness test.

[0081] The light transmittance before the light resistance test can be measured in accordance with the standard ASTM E313 using a spectrophotometer, for example, a KONICA MINOLTA spectrophotometer (model name: CM-3700D) to measure the average light transmittance in the wavelength range of 360 to 740 nm.

[0082] The haze before the light resistance test can be measured by cutting the manufactured optical film (100) to a size of 50 mm x 50 mm, measuring it three times using a haze meter according to the ASTM D1003 standard, for example, a MURAKAMI haze meter (model name: HM-150), and taking the average of the three measurements as the haze value.

[0083] According to one embodiment of the present invention, the optical film (100) may have a light transmittance of 88.5% or more after a light fastness test, and a haze of 1.0 or less after a light fastness test.

[0084] The light transmittance and haze after the light fastness test can be measured after the light fastness test in the same manner as the light transmittance and haze before the light fastness test.

[0085] The optical film (100) according to an embodiment of the present invention can be applied to a display device to protect the display surface of a display panel. The optical film (100) according to an embodiment of the present invention may have a thickness sufficient to protect the display panel. For example, the optical film (100) may have a thickness of 20 to 120 μm. However, the present invention is not limited thereto.

[0086] Hereinafter, a display device using an optical film 100 according to an embodiment of the present invention will be described with reference to FIGS.

[0087] FIG. 4 is a cross-sectional view of a portion of a display device (200) according to another embodiment of the present invention, and FIG. 5 is an enlarged cross-sectional view of a portion "P" in FIG.

[0088] 4, a display device (200) according to another embodiment of the present invention includes a display panel (501) and an optical film (100) on the display panel (501). The optical film (100) in FIG. 4 may be the optical film (101) in FIG. 2 or the optical film (102) in FIG. 3.

[0089] 4 and 5, the display panel 501 includes a substrate 510, a thin film transistor (TFT) on the substrate 510, and an organic light emitting element 570 connected to the thin film transistor (TFT). The organic light emitting element 570 includes a first electrode 571, an organic light emitting layer 572 on the first electrode 571, and a second electrode 573 on the organic light emitting layer 572. The display device 200 disclosed in FIGS. 4 and 5 is an organic light emitting display device.

[0090] The substrate 510 may be made of glass or plastic. Specifically, the substrate 510 may be made of plastic such as polyimide resin. Although not shown, a buffer layer may be disposed on the substrate 510.

[0091] The thin film transistor (TFT) is disposed on the substrate 510. The thin film transistor (TFT) includes a semiconductor layer 520, a gate electrode 530 insulated from the semiconductor layer 520 and overlapping at least a portion of the semiconductor layer 520, a source electrode 541 connected to the semiconductor layer 520, and a drain electrode 542 spaced apart from the source electrode 541 and connected to the semiconductor layer 520.

[0092] 5, a gate insulating film 535 is disposed between a gate electrode 530 and a semiconductor layer 520. An interlayer insulating film 551 may be disposed on the gate electrode 530, and a source electrode 541 and a drain electrode 542 may be disposed on the interlayer insulating film 551.

[0093] The planarization film (552) is disposed on the thin film transistor (TFT) and planarizes the upper portion of the thin film transistor (TFT).

[0094] The first electrode 571 is disposed on the planarization film 552. The first electrode 571 is connected to the thin film transistor (TFT) through a contact hole provided in the planarization film 552.

[0095] The bank layer (580) is disposed on a part of the first electrode (571) and the planarization film (552) and defines a pixel region or a light-emitting region. For example, the bank layer (580) is disposed in a matrix structure in a boundary region between a plurality of pixels, whereby the pixel region can be defined by the bank layer (580).

[0096] The organic light-emitting layer (572) is disposed on the first electrode (571). The organic light-emitting layer (572) may be disposed on the bank layer (580). The organic light-emitting layer (572) may include one light-emitting layer, or may include two or more light-emitting layers stacked one above the other. From such an organic light-emitting layer (572), light having any one of red, green, and blue colors may be emitted, and white light may also be emitted.

[0097] A second electrode (573) is disposed on the organic light-emitting layer (572).

[0098] A first electrode (571), an organic light-emitting layer (572), and a second electrode (573) may be laminated to form an organic light-emitting element (570).

[0099] Although not shown, when the organic light emitting layer 572 emits white light, each pixel may include a color filter for filtering the white light emitted from the organic light emitting layer 572 by wavelength. The color filter is formed on the path of light travel.

[0100] A thin film encapsulation layer (590) may be disposed on the second electrode (573). The thin film encapsulation layer (590) may include at least one organic film and at least one inorganic film, or the at least one organic film and the at least one inorganic film may be alternated.

[0101] An optical film (100) is disposed on the display panel (501) having the above-described laminated structure.

[0102] The present invention will be described in more detail below with reference to illustrative examples and comparative examples. However, the present invention is not limited to the examples and comparative examples described below.

[0103] <Production example: Polymer resin production> A 1 L reactor equipped with a stirrer, a nitrogen injector, a dropping funnel, a temperature regulator, and a cooler was charged with 776.655 g of DMAc (N,N-Dimethylacetamide) while passing nitrogen through it, and the temperature of the reactor was adjusted to 25°C. Then, 54.439 g (0.17 mol) of TFDB (Bis(trifluoromethyl)benzidine) was dissolved in the solution, and the solution was maintained at 25°C. 15.005g (0.051mol) of BPDA (biphenyl-tetracarboxylic acid dianhydride) was added thereto, and the mixture was stirred for 3 hours to completely dissolve BPDA. Then, 22.657g (0.051mol) of 6FDA (4,4'-(Hexafluoroisopropylidene)diphthalic anhydride) was added and completely dissolved. After lowering the reactor temperature to 10°C, 13.805g (0.068mol) of TPC (Terephthaloyl chloride) was added, and the mixture was reacted at 25°C for 12 hours to obtain a polymer solution with a solid concentration of 12% by weight.

[0104] 17.75g of pyridine and 22.92g of acetic anhydride were added to the obtained polymer solution and stirred for 30 minutes, then stirred again at 70°C for 1 hour and cooled to room temperature, 20L of methanol was added to the obtained polymer solution to precipitate solids, and the precipitated solids were filtered and pulverized. After this, it was washed again with 2L of methanol and dried at 100°C in vacuum for 6 hours to obtain a powdered polyimide-based polymer solid. The polyimide-based polymer solid produced here was a polyamideimide polymer solid.

[0105] <Example 1> In a 500 mL reactor, 300 parts by weight of DMAc and 2 parts by weight of tetraethyl 2,2'-(1,4-phenylenedimethylidyne)bismalonate (UV absorber, Cas No.: 6337-43-5, Chempia's Eversorb 320) per 100 parts by weight of polyamideimide polymer solid content were added, and after sufficient dissolution at room temperature for 10 minutes, the temperature of the reactor was maintained at 5° C. and stirred. Then, 43.72 parts by weight of the polyimide polymer solid content powder produced in the Production Example was added, and after stirring for 1 hour, the temperature was raised to 25° C. to produce a liquid polyimide resin solution. The maximum absorbance of tetraethyl 2,2'-(1,4-phenylenedimethylidyne)bismalonate was 0.95 (@321 nm).

[0106] The obtained polyimide resin solution was applied to a casting substrate and cast, and then dried with hot air at 130°C for 30 minutes to produce a film, which was then peeled off from the casting substrate and fixed to a frame with pins. At this time, there is no particular limitation on the type of casting substrate. As the casting substrate, a glass substrate, a stainless steel (SUS) substrate, a Teflon (registered trademark) substrate, etc. may be used. In Example 1, an organic substrate was used as the casting substrate. The same applies below.

[0107] The frame with the film fixed on it was placed in a vacuum oven and slowly heated from 100°C to 280°C for 2 hours, then slowly cooled and separated from the frame to obtain a polyimide-based optical film. The polyimide-based optical film was then heat-treated again at 250°C for 5 minutes. As a result, a polyimide-based optical film with a thickness of 50 μm was completed.

[0108] <Example 2> An optical film of Example 2 was produced in the same manner as in Example 1, except that the content of the ultraviolet absorbing agent was changed.

[0109] The specific content of the ultraviolet absorbent in Example 2 is as shown in Table 1 below.

[0110] <Comparative Examples 1 to 4> In the same manner as in Example 1, optical films of Comparative Examples 1 to 4 were produced by changing the type and content of the ultraviolet absorbing agent.

[0111] Specific types and contents of ultraviolet absorbents in Comparative Examples 1 to 4 are shown in Table 1 below.

[0112] In this case, the maximum absorbance of the ultraviolet absorbent in the UVA region (315 to 400 nm) was determined by dissolving each ultraviolet absorbent in DMAc at 0.001 wt%, measuring the absorbance in the UVA region (315 to 400 nm) using a Shimadzu ultraviolet spectrophotometer (UV spectrophotometer UV-1800), and determining the maximum value of the absorbances measured in the UVA region (315 to 400 nm) as the maximum absorbance of the ultraviolet absorbent in the UVA region (315 to 400 nm).

[0113] [Table 1]

[0114] <Measurement Examples> The following measurements were carried out on the optical films produced in Examples 1 and 2 and Comparative Examples 1 to 4. In the following measurement examples, measurements were carried out before the light fastness test, and again after the light fastness test.

[0115] The light resistance test was performed using a xenon lamp, specifically, a SUNTEST XXL+ device from ATLAS, with a Daylight filter, 12 kW, 0.8 W / m 2 The experiment was carried out for 300 hours under the conditions of @420 nm, 30℃ / 30RH% Chamber, 55℃ Black Panel.

[0116] 1) Yellowness (YI) The yellowness index was measured using a spectrophotometer. Specifically, the yellowness index of the optical film was measured using a spectrophotometer in accordance with standard ASTM E313, for example, a spectrophotometer (model name: CM-3700D) manufactured by KONICA MINOLTA.

[0117] 2) L*, a*, b* and color change (ΔE* ab ) Color change (ΔE*) of the optical films manufactured in the examples and comparative examples ab ) was calculated using the following formula 1.

[0118] [Formula 1] ΔE* ab = [(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2

[0119] In the above formula 1, ΔL* is the difference in L* before and after the light fastness test, Δa* is the difference in a* before and after the light fastness test, and Δb* is the difference in b* before and after the light fastness test.

[0120] The L*, a*, and b* of the optical film (100) before the lightfastness test were measured using a color difference meter. Specifically, the optical film (100) was measured three times for L*, a*, and b* using a color difference meter, for example, a KONICA MINOLTA color difference meter (model name: CM-3600A), with a D65 light source, a viewing angle of 2°, and transmission mode, and the average values ​​of the three measurements of L*, a*, and b* were calculated to obtain the L*, a*, and b* of the optical film (100). The L*, a*, and b* after the lightfastness test were measured using the same method as the measurement method of L*, a*, and b* before the lightfastness test after the lightfastness test.

[0121] 3) Light transmittance The optical films produced in the examples and comparative examples were measured for average light transmittance in the wavelength range of 360 to 740 nm using a spectrophotometer, for example a KONICA MINOLTA spectrophotometer (model name: CM-3700D) in accordance with standard ASTM E313.

[0122] 4) Hayes The optical films produced in the examples and comparative examples were cut to a size of 50 mm x 50 mm, and measured five times using a haze meter in accordance with standard ASTM D1003, for example, a MURAKAMI haze meter (model name: HM-150). The average of the five measurements was taken as the haze value of the optical film.

[0123] The measurement results are shown in Tables 2 and 3 below.

[0124] [Table 2]

[0125] [Table 3]

[0126] As shown in the measurement results in Tables 2 and 3, the optical films of Examples 1 and 2 of the present invention all have a yellowing index of 5.0 or less before the light fastness test, a yellowing index of 7.8 or less after the light fastness test, a light transmittance of 88.5% or more, a haze of 1.0 or less, and a ΔE* ab However, looking at the optical films of Comparative Examples 1 to 4, the ΔE* ab In Comparative Example 4, the initial yellowing index before the light fastness test exceeded 5.0, the haze after the light fastness test exceeded 1.0, and ΔE* ab was more than 3.5, the initial yellowing of the optical film was high, and the color reproducibility and clarity of the optical film after the light resistance test were deteriorated, and the visibility was deteriorated.

[0127] The features, structures, effects, etc. exemplified in each of the above-mentioned embodiments may be combined or modified to other embodiments by a person having ordinary skill in the art to which the embodiments belong. Therefore, the contents related to such combinations and modifications should be interpreted as being included in the scope of the present invention. [Explanation of symbols]

[0128] 100 Optical Film 101 Optical film 102 Optical film 110 Light-transmitting substrate 120 Primer layer 130 Hard coat layer 200 Display device 501 Display Panel 510 Substrate 520 Semiconductor layer 530 Gate electrode 535 Gate insulating film 541 Source Electrode 542 Drain electrode 551 Interlayer insulating film 552 Planarization film 570 Organic light-emitting devices 571 First Electrode 572 Organic light-emitting layer 573 Second Electrode 580 Bank Layer 590 Thin Film Encapsulating Layer

Claims

1. a light-transmitting substrate; The yellowness index before the light fastness test is 5.0 or less, Color change after light resistance test (ΔE* ab ) is 3.5 or less, Optical film: The light resistance test was carried out using a xenon lamp with a daylight filter at 420 nm and 0.8 W / m 2 12kW (12kW 0.8W / m 2 @420nm), 30℃ / 30% relative humidity chamber (30℃ / 30RH% Chamber), 55℃ black panel (Black Panel) conditions for 300 hours, The color change (ΔE* ab ) is calculated using the following formula 1. [Formula 1] ΔE* ab =[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2 In the above formula 1, ΔL* is the difference in L* before and after the light fastness test, Δa* is the difference in a* before and after the light fastness test, and Δb* is the difference in b* before and after the light fastness test.

2. The light-transmitting substrate is Polymer resins and Contains malonate UV absorbers, 2. The optical film according to claim 1.

3. The ultraviolet absorber has a maximum absorbance of 0.45 or more in the UVA region (315 to 400 nm) when dissolved in dimethylacetamide (DAMc) at a concentration of 0.001 wt %.

3. The optical film according to claim 2.

4. The ultraviolet absorber includes a compound represented by the following chemical formula 2: The optical film according to claim 2: [Chemical formula 2] In the above formula 2, R 1 , R 2 , R 3 and R 4 are each independently hydrogen, a halogen atom, a phenyl group, or a C1-C10 linear, branched, or alicyclic alkyl group; Y is a divalent aromatic or heteroorganic group having 6 to 40 carbon atoms; and the hydrogen atoms in the organic group included in Chemical Formula 2 may be substituted with (1) a halogen atom, (2) a hydrocarbon group, (3) a halogen-substituted hydrocarbon group, or (4) a hydrocarbon group substituted with a halogen element, oxygen, or nitrogen.

5. The ultraviolet absorber includes tetraethyl 2,2'-(1,4-phenylenedimethylidyne) bismalonate.

3. The optical film according to claim 2.

6. The light-transmitting substrate contains 1 to 10 parts by weight of the ultraviolet absorber relative to 100 parts by weight of the polymer resin.

3. The optical film according to claim 2.

7. The polymer resin comprises at least one of an imide repeat unit and an amide repeat unit.

3. The optical film according to claim 2.

8. The light transmittance after the light resistance test is 88.5% or more, The haze after the light resistance test is 1.0 or less.

2. The optical film according to claim 1.

9. A display panel; The optical film according to any one of claims 1 to 8 is disposed on the display panel. Display device.

Citation Information

Patent Citations

  • fluorescent pigment composition

    JP2005504159A

  • Stabilizer composition for improved protection against degradation of organic substrates due to light

    JP2010501705A

  • Polycarbonate resin composition and molded article thereof

    JP2014051558A

  • Polyamide resin composition

    JP2015028155A

  • Polyimide film, layered body, surface material for display, touch panel member, liquid crystal display device, and organic electroluminescent display device

    JP2020002196A