Monomer composition for contact lenses, polymer for contact lenses and method for producing same, and contact lenses and method for producing same

A monomer composition for contact lenses, including specific polysiloxane and methacrylic monomers, addresses the need for improved modulus and elongation in silicone hydrogels, achieving stable shape and high oxygen permeability for extended wear.

JP7551059B2Active Publication Date: 2024-09-17NOF CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021516091
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-25
Filing Date
2020-04-17
Publication Date
2024-09-17
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

Silicone hydrogel contact lenses require improvement in modulus and elongation at break to maintain shape stability during repeated use, while maintaining high oxygen permeability and surface hydrophilicity.

Method used

A monomer composition containing a phosphorylcholine group-containing polysiloxane monomer, a phosphorylcholine group-containing methacrylic monomer, a trimethylsiloxylyl group-containing silicone monomer, a monovinyl ether monomer, hydroxyl group-containing monomers, and a crosslinking agent, with specific mass ratios, to form a polymer that enhances surface hydrophilicity, modulus, and elongation at break.

Benefits of technology

The resulting contact lenses exhibit excellent surface hydrophilicity, modulus, and oxygen permeability, allowing for longer wear without significant shape change, with a break elongation of 250% or more and oxygen permeability coefficient of 75 or more.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551059000005
    Figure 0007551059000005
  • Figure 0007551059000011
    Figure 0007551059000011
  • Figure 0007551059000013
    Figure 0007551059000013
Patent Text Reader

Abstract

The present invention provides a monomer composition for contact lenses that exhibit good surface hydrophilicity, good oxygen permeability, while having excellent modulus and excellent elongation at break, said monomer composition producing a polymer using a polysiloxane monomer. It is found that the above objective is able to be achieved by a monomer composition which contains a phosphorylcholine group-containing polysiloxane monomer, a monovinyl ether monomer or the like.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a monomer composition for contact lenses, a polymer of said composition and a method for producing the same, and a contact lens comprising a hydrate of said polymer and a method for producing the same. This application claims priority to Japanese Patent Application No. 2019-083615, which is incorporated herein by reference. [Background technology]

[0002] Silicone hydrogel contact lenses have high oxygen permeability and therefore place less strain on the eyes. On the other hand, silicone hydrogels tend to lack wettability and lubricity due to the inclusion of hydrophobic silicone. Therefore, surface hydrophilization by surface modification methods and by mixing a hydrophilic polymer into the lens composition before curing have been considered. Currently, there are various methods for providing silicone hydrogel lenses that have optical transparency, desired lubricity, and high oxygen permeability.

[0003] Patent Document 1 discloses a silicone hydrogel produced by random copolymerization of MPC and a polysiloxane monomer SiGMA having a hydroxyl group.

[0004] Generally, when MPC is used for copolymerization to introduce phosphorylcholine groups into silicone hydrogel lenses, it is necessary to overcome phase separation between the highly hydrophilic MPC moiety and the hydrophobic silicone moiety in the silicone hydrogel skeleton, so there is still room for improvement in order to stably manufacture silicone hydrogel lenses.

[0005] Patent Document 2 discloses a polysiloxane monomer in which phosphorylcholine-like groups are introduced to both ends of the silicone chain. Patent Documents 3 and 4 disclose polysiloxane monomers in which phosphoryl groups are introduced to both ends. In polysiloxane monomers having these structures, the polydimethylsiloxane portion of the main chain is not modified, so it cannot be said that sufficient performance is necessarily obtained in terms of compatibility with hydrophilic monomers and transparency of the obtained lens. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2007-197513 A [Patent Document 2] WO2010 / 147779 [Patent Document 3] WO2001 / 057047 [Patent Document 4] WO2012 / 104349 Summary of the Invention [Problem to be solved by the invention]

[0007] Currently, silicone hydrogel contact lenses in widespread use must be replaced at regular intervals, which can range from every other day to every two weeks or months, etc. For contact lenses with longer replacement intervals, the same lenses are worn repeatedly, so it is important that the shape of the lenses does not change when used repeatedly.

[0008] The shape stability of a contact lens is closely related to the modulus and breaking elongation of the contact lens. Although contact lenses using polysiloxane monomers are excellent in terms of the surface hydrophilicity and oxygen permeability of the lens surface, there is room for improvement in the modulus and breaking elongation.

[0009] Therefore, an object of the present invention is to provide a monomer composition for contact lenses which is produced by using a polysiloxane monomer to produce a polymer and which exhibits good surface hydrophilicity and oxygen permeability, as well as excellent modulus and breaking elongation. [Means for solving the problem]

[0010] As a result of intensive research into solving the above problems, the inventors have discovered that the above object can be achieved by a monomer composition containing a phosphorylcholine group-containing polysiloxane monomer, a monovinyl ether monomer, and the like, and have thus completed the present invention.

[0011] According to one embodiment of the present invention, there is provided a polymerizable composition comprising: (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1); (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2); (C) a trimethylsiloxyl group-containing silicone monomer having at least one hydroxyl group in the molecule; (D) a monovinyl ether monomer having at least one hydroxyl group in the molecule; and (E) a hydroxyethyl (meth)acrylate, a hydroxypropyl (meth)acrylate, a hydroxybutyl (meth)acrylate, a hydroxyethyl ... and (F) a crosslinking agent, wherein, relative to 100% by mass of the total of all monomer components in the composition, the content of component (A) is 10 to 50% by mass, the content of component (B) is 5 to 20% by mass, the content of component (C) is 5 to 40% by mass, the content of component (D) is 5 to 40% by mass, the content of component (E) is 5 to 30% by mass, and the content of component (F) is 0.1 to 15% by mass. According to one embodiment of the present invention, there is provided a composition comprising: (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1); (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2); (C) a trimethylsiloxyl group-containing silicone monomer having at least one hydroxyl group in the molecule; (D) a monovinyl ether monomer having at least one hydroxyl group in the molecule; and (E) one or more hydroxyl groups selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide. Provided is a monomer composition for contact lenses comprising a monomer containing (A) and (F) a crosslinking agent, and (G) a monomer other than the above components (A) to (F), wherein, relative to 100% by mass as the total of all monomer components in the composition, the content of component (A) is 10 to 50% by mass, the content of component (B) is 5 to 20% by mass, the content of component (C) is 5 to 40% by mass, the content of component (D) is 5 to 40% by mass, the content of component (E) is 5 to 30% by mass, the content of component (F) is 0.1 to 15% by mass, and the content of component (G) is 0 to 50% by mass. In addition, the content ratio (mass ratio) of the components (A), (B), (C), (D), (E), (F) and (G) may be 100:10-200:10-400:10-400:10-300:1-150:0-500.

[0012] [ka]

[0013] In formula (1), a represents an integer of 20 to 500. b represents an integer of 1 to 70. c represents 0 or 1. p and q each represent 0 or 1. X represents -CH2- or -CH2CH2-.

[0014] [ka]

[0015] According to another aspect of the present invention, there is provided a polymer for contact lenses comprising a polymer of the above-mentioned monomer composition for contact lenses.

[0016] According to a further aspect of the present invention, there are provided a contact lens comprising the above-mentioned hydrate of the contact lens polymer, and a method for producing the same.

[0017] That is, the present invention is as follows. 1. (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1), (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2), (C) a trimethylsiloxylyl group-containing silicone monomer having at least one hydroxyl group in the molecule; (D) a monovinyl ether monomer having at least one hydroxyl group in the molecule; (E) one or more hydroxyl group-containing monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide; (F) a crosslinking agent; (G) a monomer other than the components (A) to (F), the content of the (A) component is 10 to 50 mass%, the content of the (B) component is 5 to 20 mass%, the content of the (C) component is 5 to 40 mass%, the content of the (D) component is 5 to 40 mass%, the content of the (E) component is 5 to 30 mass%, the content of the (F) component is 0.1 to 15 mass%, and the content of the (G) component is 0 to 50 mass%, relative to 100 mass% in total of all monomer components in the composition; A monomer composition for contact lenses. [ka] [In formula (1), a represents an integer of 20 to 500. b represents an integer of 1 to 70. c represents 0 or 1. p and q each represent 0 or 1. X represents -CH2- or -CH2CH2-.] [ka] 2. The composition further contains (H) a solvent having a hydroxyl group, and the content of the component (H) is 30 parts by mass or less per 100 parts by mass of the total of all monomer components in the composition. 2. The monomer composition for contact lenses according to item 1 above. 3. A polymer of the monomer composition for contact lenses according to the preceding item 1 or 2. Polymers for contact lenses. 4. A contact lens composition comprising the hydrate of the polymer for contact lenses according to the preceding item 3. Contact lenses. 5. A step of mixing the polymer for contact lenses according to the preceding item 3 with one or more solvents selected from water, methanol, ethanol, 1-propanol, and 2-propanol, and washing the polymer; and hydrating the polymer by immersing it in physiological saline. A method for manufacturing contact lenses. 6. A method for producing a polymer for contact lenses, comprising the step of polymerizing the following monomer composition: (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1), (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2), (C) a trimethylsiloxylyl group-containing silicone monomer having at least one hydroxyl group in the molecule; (D) a monovinyl ether monomer having at least one hydroxyl group in the molecule; (E) one or more hydroxyl group-containing monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide; (F) a crosslinking agent; (G) a monomer other than the components (A) to (F), Here, relative to 100% by mass of the total of all monomer components in the composition, the content of component (A) is 10 to 50% by mass, the content of component (B) is 5 to 20% by mass, the content of component (C) is 5 to 40% by mass, the content of component (D) is 5 to 40% by mass, the content of component (E) is 5 to 30% by mass, the content of component (F) is 0.1 to 15% by mass, and the content of component (G) is 0 to 50% by mass. [ka] [In formula (1), a represents an integer of 20 to 500. b represents an integer of 1 to 70. c represents 0 or 1. p and q each represent 0 or 1. X represents -CH2- or -CH2CH2-.] [ka] 7. The method for producing a polymer for contact lenses according to item 6 above, wherein the composition further contains (H) a solvent having a hydroxyl group, and the content of component (H) is 30 parts by mass or less per 100 parts by mass of the total of all monomer components in the composition. 8. Use of the following monomer composition in the manufacture of a polymer for contact lenses: (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1), (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2), (C) a trimethylsiloxylyl group-containing silicone monomer having at least one hydroxyl group in the molecule; (D) a monovinyl ether monomer having at least one hydroxyl group in the molecule; (E) one or more hydroxyl group-containing monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide; (F) a crosslinking agent; (G) a monomer other than the components (A) to (F), Here, relative to 100% by mass of the total of all monomer components in the composition, the content of component (A) is 10 to 50% by mass, the content of component (B) is 5 to 20% by mass, the content of component (C) is 5 to 40% by mass, the content of component (D) is 5 to 40% by mass, the content of component (E) is 5 to 30% by mass, the content of component (F) is 0.1 to 15% by mass, and the content of component (G) is 0 to 50% by mass. [ka] [In formula (1), a represents an integer of 20 to 500. b represents an integer of 1 to 70. c represents 0 or 1. p and q each represent 0 or 1. X represents -CH2- or -CH2CH2-.] [ka] 9. Use for producing a polymer for contact lenses according to the preceding item 8, wherein the composition further contains (H) a solvent having a hydroxyl group, and the content of component (H) is 30 parts by mass or less per 100 parts by mass of the total of all monomer components in the composition. 10. Use of the following monomer composition as a polymer for contact lenses: (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1), (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2), (C) a trimethylsiloxylyl group-containing silicone monomer having at least one hydroxyl group in the molecule; (D) a monovinyl ether monomer having at least one hydroxyl group in the molecule; (E) one or more hydroxyl group-containing monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide; (F) a crosslinking agent; (G) a monomer other than the components (A) to (F), Here, relative to 100% by mass of the total of all monomer components in the composition, the content of component (A) is 10 to 50% by mass, the content of component (B) is 5 to 20% by mass, the content of component (C) is 5 to 40% by mass, the content of component (D) is 5 to 40% by mass, the content of component (E) is 5 to 30% by mass, the content of component (F) is 0.1 to 15% by mass, and the content of component (G) is 0 to 50% by mass. [ka] [In formula (1), a represents an integer of 20 to 500. b represents an integer of 1 to 70. c represents 0 or 1. p and q each represent 0 or 1. X represents -CH2- or -CH2CH2-.] [ka] 11. The use as a polymer for contact lenses according to the preceding item 10, wherein the composition further contains (H) a solvent having a hydroxyl group, and the content of component (H) is 30 parts by mass or less per 100 parts by mass of the total of all monomer components in the composition. Effect of the Invention

[0018] The contact lens of the present invention is produced using the monomer composition for contact lenses of the present invention, and therefore can simultaneously exhibit excellent surface hydrophilicity, modulus, breaking elongation and oxygen permeability coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The monomer composition for contact lenses of the present invention contains the below-described components (A) to (F) as essential monomer components, and may further contain a component (G) as an optional monomer component, and may further contain a component (H) as an optional solvent component. The polymer for contact lenses of the present invention is obtained from a polymer of the monomer composition for contact lenses of the present invention. Also, the contact lens of the present invention is obtained from the polymer for contact lenses of the present invention. In addition, the contact lens of the present invention may be a hydrate of the polymer for contact lenses of the present invention. Hereinafter, the monomer composition for contact lenses of the present invention will be referred to simply as a composition. Also, the polymer for contact lenses of the present invention will be referred to simply as a polymer. In the present invention, "excellent breaking elongation" means, without any particular limitation on the numerical value, a breaking elongation of 250% or more in the mechanical strength measurement detailed in the Examples. "Excellent hydrophilicity" means, without any particular limitation on the numerical value, a water film break up time (WBUT) of 30 seconds or more in the evaluation detailed in the Examples. "Excellent oxygen permeability" means, without any particular limitation on the numerical value, a oxygen permeability coefficient of 75 or more in the oxygen permeability measurement detailed in the Examples.

[0020] Component (A) is a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1). Component (A) is a component that contributes to improving the oxygen permeability and surface hydrophilicity of the contact lens produced. The number average molecular weight of the phosphorylcholine group-containing polysiloxane monomer of the present invention may be 2,000 to 50,000, and preferably 4,600 to 42,000.

[0021] [ka]

[0022] In the formula, a represents an integer of 20 to 500. b represents an integer of 1 to 70. c represents 0 or 1. p and q each represent 0 or 1. X represents -CH2- or -CH2CH2-. Although a and b are not particularly limited as long as they are within the above ranges, a is 20-500, preferably 50-300, more preferably 80-200, and b is 1-70, preferably 2-40, more preferably 3-15.

[0023] In the composition of the present invention, when the total of all monomer components is taken as 100% by mass, the content of component (A) is 10 to 50% by mass, preferably 15 to 50% by mass, and more preferably 25 to 40% by mass. If the content of component (A) is less than 10% by mass, there is a concern that the oxygen permeability of the contact lens produced will be insufficient. On the other hand, if it exceeds 50% by mass, the contact lens may become cloudy. In the present invention, the term "monomer component" refers to a component having one or more polymerizable unsaturated groups in the molecule. That is, the term "monomer component" includes components (A) to (F) and (G), but does not include component (H).

[0024] Component (B) is a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2), specifically 2-methacryloyloxyethyl phosphorylcholine (MPC). Component (B) is a component that contributes to improving the surface hydrophilicity and lubricity of the contact lens to be manufactured.

[0025] [ka]

[0026] In the composition of the present invention, when the total of all monomer components is taken as 100% by mass, the content of component (B) is 5 to 20% by mass, preferably 8 to 15% by mass. If the content of component (B) is less than 5% by mass, sufficient surface hydrophilicity cannot be obtained. On the other hand, if it exceeds 20% by mass, it becomes difficult to dissolve component (B) in the composition, and there is a concern that the modulus (tensile stress) of the contact lens may increase.

[0027] Component (C) is a trimethylsiloxylyl group-containing silicone monomer having at least one hydroxyl group in the molecule. Component (C) is a component that contributes to improving the oxygen permeability and transparency of the contact lens produced. Specific examples of the (C) component include 4-(2-hydroxyethyl)=1-[3-tris(trimethylsiloxy)silylpropyl]=2-methylidenesuccinate, 2-hydroxy-3-[tris(trimethylsiloxy)silyl]propyl methacrylate, 2-hydroxy-3-[bis(trimethylsiloxy)methylsilyl]propyl methacrylate, etc., with 4-(2-hydroxyethyl)=1-[3-tris(trimethylsiloxy)silylpropyl]=2-methylidenesuccinate and 2-hydroxy-3-[bis(trimethylsiloxy)methylsilyl]propyl methacrylate being preferred, and 4-(2-hydroxyethyl)=1-[3-tris(trimethylsiloxy)silylpropyl]=2-methylidenesuccinate being more preferred.

[0028] In the composition of the present invention, when the total of all monomer components is taken as 100% by mass, the content of component (C) is 5 to 40% by mass, preferably 10 to 20% by mass. If the content of component (C) is less than 5% by mass, it may be difficult to dissolve component (B) or the polymer for contact lenses produced may become cloudy. On the other hand, if it exceeds 40% by mass, there is a concern that the surface hydrophilicity of the contact lens may be insufficient.

[0029] Component (D) is a monovinyl ether monomer having at least one hydroxyl group in the molecule, and is a component that contributes to improving the surface hydrophilicity and breaking elongation of the contact lens produced.

[0030] Specific examples of the component (D) include ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, tetramethylene glycol monovinyl ether, and the like. Of these, ethylene glycol monovinyl ether and diethylene glycol monovinyl ether are preferred, and ethylene glycol monovinyl ether is more preferred.

[0031] In the composition of the present invention, when the total of all monomer components is taken as 100% by mass, the content of component (D) is 5 to 40% by mass, preferably 10 to 20% by mass. If the content of component (D) is less than 5% by mass, there is a concern that the breaking elongation will be insufficient. The polymer for contact lenses produced may become cloudy. On the other hand, if it exceeds 40% by mass, there is a concern that the polymerizability will deteriorate, and the effects of the present invention will not be fully obtained.

[0032] The component (E) is one or more hydroxyl group-containing monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide. Hydroxyethyl methacrylate, hydroxypropyl methacrylate, and / or hydroxybutyl methacrylate are preferred, and hydroxypropyl methacrylate and / or hydroxybutyl methacrylate are more preferred. By including a predetermined amount of the component (E), the dissolution of the component (B) in the composition of the present invention is improved. In terms of the solubility of the component (B), the hydroxyl group of the component (E) is preferably a primary hydroxyl group. In the present invention, "(meth)acrylate" means "acrylate and / or methacrylate", and "(meth)acrylic" means "acrylic and / or methacrylic".

[0033] In the composition of the present invention, when the total of all monomer components is taken as 100% by mass, the content of component (E) is 5 to 30% by mass, and preferably 5 to 15% by mass. If the content of component (E) is less than 5% by mass, the composition of the present invention will not be a uniform transparent liquid, and there is a concern that the effects of the present invention will not be fully achieved. On the other hand, if it exceeds 30% by mass, there is a concern that the oxygen permeability of the contact lens will decrease.

[0034] Component (F) acts as a crosslinking agent during the polymerization reaction of the monomers (A) to (E). Component (F) usually has two or more polymerizable unsaturated groups. Since the composition of the present invention contains a predetermined amount of component (F), the polymer of the present invention has a crosslinked structure, and therefore the contact lens of the present invention exhibits excellent modulus.

[0035] Specific examples of the component (F) include silicone dimethacrylate represented by the following formula (3), ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, methylene bisacrylamide, alkylene glycol di(meth)acrylate (alkylene having 2 to 6 carbon atoms), polyalkylene glycol di(meth)acrylate (alkylene having 2 to 4 carbon atoms), divinyl sulfone, divinylbenzene, trivinylbenzene, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, allyl methacrylate, (2-allyloxy)ethyl methacrylate, 2-(2-vinyloxyethoxy)ethyl acrylate, and 2-(2-vinyloxyethoxy)ethyl methacrylate. Among these, silicone dimethacrylate, triethylene glycol divinyl ether, and tetraethylene glycol di(meth)acrylate represented by formula (3) are preferred, and triethylene glycol divinyl ether and tetraethylene glycol di(meth)acrylate are more preferred. The (F) component may be any one of these crosslinking agents or a mixture of two or more of them, but a mixture of two or more of them is preferred, and a mixture of triethylene glycol divinyl ether and tetraethylene glycol di(meth)acrylate in a mass ratio of 1 / 4 to 4 / 1 (1:4 to 4:1) is more preferred, and a mixture of 1 / 2 to 2 / 1 (1:2 to 2:1) is particularly preferred.

[0036] [ka]

[0037] In formula (3), p and r are equal to each other and are 0 or 1. q represents the number of repetitions of the dimethylsiloxane portion and is 10 to 70. The silicone dimethacrylate represented by formula (3) may be a mixture of multiple compounds having different repetition numbers q. In this case, q is the average value in the number average molecular weight, and is within the range of 10 to 70 from the viewpoint of availability.

[0038] In the composition of the present invention, when the total of all monomer components is 100% by mass, the content of component (F) is 0.1 to 15% by mass, preferably 0.5 to 5% by mass, and more preferably 1 to 3% by mass. If the content of component (F) is less than 0.1% by mass, the solvent resistance of the polymer decreases, and the polymer may be damaged when washed. If it exceeds 15% by mass, the contact lens may become brittle and may be damaged, and the modulus may become too high, resulting in a poor wearing comfort.

[0039] Component (G) is a monomer other than components (A) to (F). Component (G) is an optional component that can be blended for the purpose of adjusting the water content in the contact lens. Specific examples of the (G) component include alkyl methacrylates such as methyl (meth)acrylate, (meth)acrylic acid, 2-methacryloyloxyethyl succinate, methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, as well as amide group-containing monomers such as methoxypolyethylene glycol methacrylate, N-vinylpyrrolidone, N,N-dimethylacrylamide, N-vinyl-N-methylacetamide, and N-methylacetamide. The component (G) may be any one of these monomers, or a mixture of two or more of them.

[0040] When the component (G) is contained, its content is 50% by mass or less based on the total amount of all monomer components in the composition of the present invention, and may be 0 to 50% by mass, 0.01 to 50% by mass, 0.1 to 50% by mass, 1 to 50% by mass, or 10 to 50% by mass. If it is 50% by mass or less, the solubility of the component (A) in the composition of the present invention is good, and the effects of the present invention can be obtained in a well-balanced manner.

[0041] Component (H) is a solvent having a hydroxyl group, and may be a carboxylic acid or an alcohol. Component (H) can be blended for the purpose of stabilizing the modulus and shape of the contact lens. Specific examples of component (H) include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, 1-pentanol, 2-pentanol, tert-amyl alcohol, 1-hexanol, 1-octanol, 1-decanol, 1-dodecanol, glycolic acid, lactic acid, and acetic acid. Component (H) may be any one of these solvents or a mixture of two or more of them. In terms of availability and pH stability, component (H) is preferably one or more selected from ethanol, 1-propanol, 2-propanol, and 1-hexanol.

[0042] When the composition of the present invention contains component (H), the content of component (H) is 30 parts by mass or less, and preferably 20 parts by mass or less, when the total amount of all monomer components in the composition is 100 parts by mass. If it is 30 parts by mass or less, the modulus and shape of the contact lens can be maintained in a well-balanced manner.

[0043] The composition of the present invention may contain a polymerization initiator in addition to the above components (A) to (H). The polymerization initiator may be a known one, and is preferably a thermal polymerization initiator. When a thermal polymerization initiator is used, the copolymerizability of each monomer component can be easily changed by temperature change during polymerization. Examples of the thermal polymerization initiator include 2,2'-azobisisobutyronitrile, dimethyl 2,2-azobis(2-methylpropionate), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]dihydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(1-imino-1-pyrrolidino-2-methyl)propane, Examples of the polymerization initiator include azo-based polymerization initiators such as 2,2'-azobis[2-methyl-N-{1,1-bis(hydroxymethyl)-2-hydroxyethyl}propionamide], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis(2-methylpropionamidine)dihydrochloride, and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and peroxide-based polymerization initiators such as benzoyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, lauroyl peroxide, t-butyl peroxyhexanoate, and 3,5,5-trimethylhexanoyl peroxide. These polymerization initiators may be used alone or in combination of two or more. Among these, azo-based polymerization initiators are preferred in terms of safety and availability, and 2,2'-azobisisobutyronitrile, dimethyl 2,2-azobis(2-methylpropionate), and 2,2'-azobis(2,4-dimethylvaleronitrile) are particularly preferred in terms of reactivity.

[0044] The amount of the polymerization initiator to be added is 0.1 to 3 parts by mass, preferably 0.1 to 2 parts by mass, and more preferably 0.2 to 1 part by mass, when the total amount of all monomer components in the composition is 100 parts by mass. If the amount is within the range of 0.1 to 3 parts by mass, a polymer of the monomer composition of the present invention can be easily obtained.

[0045] In addition to the above components (A) to (H) and the polymerization initiator, the composition of the present invention may contain additives such as a polymerizable ultraviolet absorber and a polymerizable dye (colorant) within the scope of not impairing the object of the present invention. By incorporating an ultraviolet absorber, the burden on the eyes caused by ultraviolet rays such as sunlight can be reduced. Furthermore, by incorporating a dye, a colored contact lens can be made.

[0046] The amounts of these additives used vary depending on the thickness of the contact lens, etc., but usually, when the total amount of all monomer components is 100 parts by mass, the content of each of the polymerizable ultraviolet absorber and the polymerizable dye is preferably 5 parts by mass or less, and more preferably 0.02 to 3 parts by mass.

[0047] The method for producing the composition of the present invention is not particularly limited, and the composition can be produced, for example, by putting each component into a stirring (mixing) device in any order or all at once, and stirring (mixing) until it becomes uniform at a temperature of 10° C. to 50° C. However, if the composition contains a polymerization initiator, care must be taken not to start a polymerization reaction during mixing, and mixing is preferably performed at 40° C. or less. In terms of improving the solubility of component (A), it is preferable to mix and dissolve the three components (A), (B), and (C) and then add and mix the other components.

[0048] The polymer of the present invention is a polymer of the composition of the present invention. A method for producing the polymer of the present invention will be described below. The production method shown below is merely one embodiment of a method for obtaining the polymer, and the polymer of the present invention is not limited to the one obtained by this production method.

[0049] The polymer of the present invention can be produced by filling the composition of the present invention into a mold and carrying out a polymerization reaction. As the mold, a mold having a hydrophobic surface made of polypropylene or the like can be used.

[0050] The polymerization reaction can be carried out in one polymerization step or two or more polymerization steps. The polymerization reaction may be carried out in one polymerization step in which the composition is maintained at a temperature of 45°C to 140°C for one hour or more according to the decomposition temperature of the polymerization initiator used, but is preferably carried out in one polymerization step consisting of the polymerization step 2 shown below, or in two or more polymerization steps including the polymerization step 1 and the polymerization step 2. After the polymerization is completed, the polymer may be removed from the mold by cooling to, for example, 60°C or less.

[0051] (Polymerization step 1) In the polymerization step 1, the above-mentioned polymerization initiator is added to the composition as necessary, and polymerization is carried out at a temperature of 45° C. to 140° C. for 1 hour or longer.

[0052] The polymerization temperature in the polymerization step 1 is preferably 50° C. to 70° C., and more preferably 55° C. to 70° C. When the polymerization temperature in the polymerization step 1 is 45° C. to 75° C., a polymer having good physical properties such as surface hydrophilicity can be stably obtained.

[0053] The polymerization time in the polymerization step 1 is preferably 2 hours or more and 12 hours or less. If the polymerization time in the polymerization step 1 is 1 to 12 hours, a polymer having good physical properties such as surface hydrophilicity can be efficiently obtained.

[0054] (Polymerization step 2) The polymerization step 2 is a step in which a polymerization reaction is carried out at 90° C. to 140° C. When the polymerization step 1 is not carried out, the polymerization step 2 is carried out by adding the above-mentioned polymerization initiator to the composition as necessary.

[0055] The polymerization temperature in the polymerization step 2 is preferably 100° C. to 120° C. If the polymerization temperature in the polymerization step 2 is 90° C. to 140° C., a polymer having good physical properties such as surface hydrophilicity can be stably obtained, and the polymer can be efficiently obtained without deforming a mold made of polypropylene or the like.

[0056] The polymerization time in the polymerization step 2 is preferably 1 hour or more and 10 hours or less. If the polymerization time in the polymerization step 2 is 1 to 10 hours, a polymer having good physical properties such as surface hydrophilicity can be efficiently obtained.

[0057] The atmosphere in which the polymerization steps 1 and 2 are carried out is not particularly limited, but in terms of improving the polymerization rate, it is preferable to carry out both the polymerization steps 1 and 2 in an inert gas atmosphere such as nitrogen or argon. In this case, the inert gas may be passed through the composition, or the composition filling location in the mold may be in an inert gas atmosphere.

[0058] The pressure inside the mold can be atmospheric pressure to slight pressure. When polymerizing in an inert gas atmosphere, the gauge pressure should be 1kgf / cm. 2 It is preferable that:

[0059] The contact lens of the present invention may be a silicone hydrogel contact lens made of a hydrate of the above polymer. That is, the contact lens of the present invention can be obtained by hydrating and absorbing water into the polymer of the present invention to form a hydrogel. In this specification, the term "silicone hydrogel" refers to a hydrogel having a silicone moiety in the polymer. Since the composition of the present invention contains the silicone-containing monomers (A) and (C), the polymer has a silicone moiety and can form a silicone hydrogel by hydrating (absorbing water).

[0060] The water content of the contact lens (the ratio of water to the total mass of the contact lens) is 35% by mass to 60% by mass, and preferably 35% by mass to 50% by mass. If the water content is 35 to 60% by mass, it can be well balanced with oxygen permeability.

[0061] Next, a method for producing the contact lens of the present invention will be described. The production method described below is merely one embodiment of a method for obtaining the contact lens of the present invention, and the contact lens of the present invention is not limited to those obtained by this production method.

[0062] After the polymerization reaction, the polymer may be in a state of a mixture with unreacted monomer components (unreacted materials), residues of each component, by-products, remaining solvent, etc. Although such a mixture can be subjected to the hydration treatment as it is, it is preferable to purify the polymer using a purification solvent before the hydration treatment.

[0063] Examples of the purification solvent include water, methanol, ethanol, 1-propanol, 2-propanol, and mixtures thereof. The purification can be carried out, for example, by immersing the polymer in an alcohol solvent at a temperature of 10°C to 40°C for 10 minutes to 5 hours, and then immersing it in water for 10 minutes to 5 hours. After immersion in the alcohol solvent, the polymer may be immersed in a water-containing alcohol having an alcohol concentration of 20 to 50% by weight for 10 minutes to 5 hours, and then immersed in water. As the water, pure water, ion-exchanged water, etc. are preferable.

[0064] The contact lens of the present invention can be obtained by immersing the polymer in physiological saline and hydrating it to a predetermined water content. The physiological saline may be borate buffered physiological saline, phosphate buffered physiological saline, or the like. The polymer may also be immersed in a storage solution for soft contact lenses containing physiological saline. From the viewpoint of hydration, it is preferable that the osmotic pressure of the physiological saline is 250 to 400 mOms / kg.

[0065] The contact lenses of the present invention have high surface hydrophilicity and oxygen permeability, and also have appropriate mechanical strength and excellent wearing comfort, so that they can be used for about one month under normal usage conditions. That is, the contact lenses of the present invention may be replaced at most once a month. Of course, they may be replaced at shorter intervals. EXAMPLES

[0066] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. First, the components used in the examples and comparative examples are shown below.

[0067] Component (A) The compound represented by formula (1) was synthesized by the following method: (A-1) In a 1L four-neck flask, 97.26g (0.68 mol) of 2-chloro-2-oxo-1,3,2-dioxaphospholane (COP) was dissolved in 389.03g of acetonitrile and cooled to 5°C or less in an ice bath. In a 500mL beaker, 66.38g (0.65 mol) of ethylene glycol monoallyl ether (Tokyo Chemical Industry Co., Ltd.) and 69.07g (0.68 mol) of triethylamine (Kishida Chemical Co., Ltd.) were dissolved in 135.45g of acetonitrile, transferred to a 300mL dropping funnel, and dropped into the COP solution over 1 hour. The reaction was further carried out for 4 hours in an ice bath. After filtering out the triethylamine hydrochloride produced by the reaction, 61.46g (1.04 mol) of trimethylamine was charged and reacted at 75°C for 8 hours. After cooling, the target product produced was filtered out and washed twice with 140g of acetone. The solvent was removed under reduced pressure to obtain 104.1 g of an allyl group-containing phosphorylcholine compound. In a 500mL light-shielding bottle, 17.24g of FM-7711 (JNC, both-terminated methacryloyloxypropyl polydimethylsiloxane (molecular weight ≒ 1,000)), 150.0g of octamethylcyclotetrasiloxane, 6.74g of 1,3,5,7-tetramethylcyclotetrasiloxane, and 173.99g of chloroform were mixed, and 1.50g of trifluoromethanesulfonic acid was added. After reacting for 8 hours at 25°C, the mixture was washed five times with about 1500g of ion-exchanged water. Then, low boiling points were removed by reducing the pressure, and 24.2g of acetone and 120.1g of methanol were added and stirred. After standing, the upper layer was discarded, and the lower layer was reduced in pressure to distill off the low boiling points, yielding 127.09g of a transparent liquid hydrosilyl-containing both-terminated methacrylic silicone. In a 100 mL three-neck flask, 10.00 g of the hydrosilyl group-containing both-terminated methacrylic silicone and 0.2140 g of the allyl group-containing phosphorylcholine compound were dissolved in 10.00 g of 2-propanol and heated to 80° C. using an oil bath, and then 40 μL of a 4 wt % hexachloroplatinic acid hexahydrate 2-propanol solution was added. A solution prepared by dissolving 1.93 g of the allyl group-containing phosphorylcholine compound represented by formula (5) in 5.78 g of 2-propanol was placed in a 10 mL dropping funnel and attached to the top of the three-neck flask. The liquid in the dropping funnel was added dropwise over 30 minutes while maintaining the temperature at 80°C. After the addition, the reaction was continued for another hour under reflux conditions. After the low boiling point components were distilled off under reduced pressure, 33.18g of ion-exchanged water, 11.05g of ethanol, and 44.21g of ethyl acetate were mixed and stirred. After standing, the mixture separated into three layers. The upper and lower layers were discarded, and 7.31g of a transparent gel was obtained by distilling off the middle layer under reduced pressure. 1 H NMR analysis confirmed that the compound was represented by formula (1). For the component (A-1) used this time, the molar ratio of the structural units in formula (1) and the number average molecular weight are shown in Table 1.

[0068] 1 H NMR analysis Peak area value of 2H of terminal double bond at 5.54 and 6.10 ppm (1.00 + 1.00 = 2.00) Area value of 9H from choline group at 3.34 ppm (46.89) Peak area value (646.15) derived from siloxane at 0.16 ppm From the above, it was calculated that in the structural formula (1), a≈108, b=5, c=1, p=q=0, and X is -CH2CH2-. The number average molecular weight was measured by gel permeation chromatography (GPC) and calculated under the following measurement conditions using PMMA (polymethyl methacrylate) as the standard. The number average molecular weight Mn was calculated to be approximately 10,000. Eluent: Tetrahydrofuran Flow rate: 0.8mL / min Column: PLgelmixed-E x 3 (connected in series) Column temperature: 40℃ Detector: Differential refractometer

[0069] (A-2~A-6) A-2 to A-6 were carried out in the same manner as A-1, except that the molecular weight and hydrosilyl group content of the hydrosilyl group-containing double-terminated methacrylic silicone were changed, and the amount of the allyl group-containing phosphorylcholine compound was changed in proportion to the concentration of the hydrosilyl group. A-5 and A-6 are components similar to (A) in which a in formula (1) does not satisfy the range of 20 to 500. The molar ratio of the constituent units of formula (1) and the number average molecular weight of A-2 to A-6 are calculated as shown in Table 1.

[0070] [Table 1]

[0071] (B) Component MPC: a compound represented by formula (2)

[0072] (C) Component ES: 4-(2-hydroxyethyl) = 1-[3-tris(trimethylsiloxy)silylpropyl] = 2-methylidenesuccinate SiGMA: 2-hydroxy-3-[bis(trimethylsiloxy)methylsilyl]propyl methacrylate

[0073] (D) Component EGMV: Ethylene glycol monovinyl ether DEGMV: Diethylene glycol monovinyl ether

[0074] (E) Component HEMA: 2-hydroxyethyl methacrylate HPMA: 2-hydroxypropyl methacrylate HBMA: 2-Hydroxybutyl methacrylate

[0075] Ingredient (F) FM-7711: Compound represented by formula (3) (p=r=0, q=10, number average molecular weight Mn≒1000) TEGDV: Triethylene glycol divinyl ether TEGDMA: Tetraethylene glycol dimethacrylate

[0076] (G) Component MMA: Methyl methacrylate NVP: N-vinylpyrrolidone DMAA: N,N-Dimethylacrylamide

[0077] (H) Component HeOH: 1-Hexanol

[0078] Polymerization initiator AIBN: 2,2'-azobis(isobutyronitrile)

[0079] The compositions, polymers, and contact lenses of the Examples and Comparative Examples were evaluated for the following items.

[0080] Contact lens modulus (tensile stress) The modulus [MPa] of the contact lens was measured according to JIS-K7127 using a Yamaden BAS-3305(W) breaking strength analyzer. In detail, the modulus was measured using a sample with a width of 2 mm, a 200gf load cell, and a clamp distance of 6 mm at a pulling speed of 1 mm / sec. When the modulus was 0.3 MPa or more but less than 0.7 MPa, the modulus (tensile stress) was judged to be good.

[0081] Contact lens breaking elongation The breaking elongation [%] of the contact lenses was measured according to JIS-K7127 using a Yamaden BAS-3305(W) breaking strength analyzer. In detail, a sample with a width of 2 mm was used, and the breaking elongation was measured by pulling at a speed of 1 mm / sec with a clamp distance of 6 mm using a 200 gf load cell. A breaking elongation of 250% or more was judged to be good.

[0082] Contact lens surface hydrophilicity (WBUT) The surface hydrophilicity of contact lenses was evaluated by WBUT (water film break up time). In detail, a sample was immersed in ISO physiological saline overnight, and the outer periphery was pinched with tweezers and pulled out from the water surface, and the time from when it was pulled out until the water film on the lens surface broke (water film retention time) was measured. The state of the water film breaking was judged by visual inspection. This measurement was carried out three times, and the average value was calculated. A time of 30 seconds or more was judged to be good for surface hydrophilicity.

[0083] Water content of contact lenses The moisture content was measured according to the method described in ISO-18369-4.

[0084] Oxygen permeability of contact lenses The oxygen permeability coefficient of samples in which one to four contact lenses were stacked was measured according to the polarographic measurement method described in ISO 18369-4. The measurement was performed using an O2 Permeometer Model 201T manufactured by Rehder Development Company. The lens thickness was plotted on the x-axis and the t / Dk value obtained by measurement was plotted on the y-axis, and the reciprocal of the slope of the regression line was calculated as the oxygen permeability coefficient {(cm 2 / sec) / (mLO 2 / (mL×mmHg)}. The higher the oxygen permeability coefficient, the better the oxygen permeability. When the oxygen permeability coefficient was 75 or more, the oxygen permeability was judged to be particularly good.

[0085] [Example 1] Under a temperature condition of 25°C, 11.8% by mass of A-1, 11.8% by mass of MPC and 31.5% by mass of ES were mixed and dissolved, and then 7.9 parts by mass of EGMV, 7.9% by mass of HBMA, 0.8% by mass of TEGDMA, 0.8% by mass of TEGDV, 11.8% by mass of MMA, 15.7% by mass of NVP, and 15.0 parts by mass of HeOH were mixed and dissolved uniformly to obtain a composition. The content ratio of each component is shown in Table 2.

[0086] 0.5 parts by mass of AIBN was added to the above composition, and the mixture was poured into a cell sandwiched between two polypropylene plates using a 0.1 mm thick polyethylene terephthalate sheet as a spacer, and then placed in an oven. After replacing the inside of the oven with nitrogen, the temperature was raised to 100°C and maintained for 2 hours, and the pressure was reduced to 0 kgf / cm. 2 The composition was polymerized at (gauge pressure) to obtain the polymer of Example 1. The polymer was removed from the cell.

[0087] Physiological saline was prepared with reference to the literature (ISO 18369-3:2006, Ophthalmic Optics-Contact Lenses Part 3: Measurement Methods.) 8.3 g of sodium chloride, 5.993 g of sodium hydrogen phosphate dodecahydrate, and 0.528 g of sodium dihydrogen phosphate dihydrate were weighed out, dissolved in water to make 1000 mL, and filtered to make physiological saline. The polymer was immersed in 2-propanol for 4 hours, then immersed in ion-exchanged water for 4 hours, and further immersed in physiological saline according to ISO 18369-3 to produce a hydrate of the polymer. The hydrate was processed into a shape suitable for each evaluation test to obtain a contact lens sample. The results of each evaluation are shown in Table 2. The breaking elongation was 250%, the oxygen permeability coefficient was 80, the WBUT was 30 seconds or more, and the modulus was 0.5 MPa, confirming that the contact lens of Example 1 exhibited good hydrophilicity, oxygen permeability, and modulus, and was excellent in terms of breaking elongation.

[0088] [Examples 2 to 15 and Comparative Examples 1 and 2] The compositions, polymers, and contact lenses of Examples 2 to 15 and Comparative Examples 1 and 2 were prepared and evaluated in the same manner as in Example 1, except that the content ratio of each component and the polymerization conditions were changed as shown in Tables 2, 3, and 4. The results are shown in Tables 2, 3, and 4.

[0089] [Table 2]

[0090] [Table 3]

[0091] [Table 4]

[0092] From the results in Tables 2 and 3, in Examples 1 to 15, the WBUT evaluation was greater than 30 seconds, indicating good surface hydrophilicity, the modulus was in the range of 0.3 MPa or more and less than 0.7 MPa, indicating good modulus, the oxygen permeability coefficient was 75 or more, indicating particularly good oxygen permeability, and the breaking elongation was 250% or more, indicating good breaking elongation. On the other hand, as can be seen from Table 4, in Comparative Example 1, since it did not contain component (D), the breaking elongation was less than 250%, which was poor, and further the modulus was 0.7 MPa or more, which was unsuitable for contact lenses. In Comparative Example 2, A-6 was used in place of the component (A), and since a in formula (1) was smaller than 20, the modulus was 0.7 MPa or more, which was unsuitable for contact lenses. Therefore, it was confirmed that the polymer obtained by polymerizing the monomer composition of the present invention can be used to produce contact lenses having excellent surface hydrophilicity, modulus, breaking elongation and oxygen permeability coefficient.

[0093] From the above, it was confirmed that the contact lens obtained by polymerizing the monomer composition for contact lenses of the present invention simultaneously satisfies the requirements for surface hydrophilicity, modulus, breaking elongation and oxygen permeability coefficient. [Industrial Applicability]

[0094] It is possible to provide a contact lens that simultaneously satisfies the requirements for surface hydrophilicity, modulus, breaking elongation and oxygen permeability coefficient.

Claims

1. (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1), (B) a phosphorylcholine group-containing methacrylic monomer represented by the following formula (2), (C) a trimethylsiloxylyl group-containing silicone monomer having one or more hydroxyl groups; (D) a monovinyl ether monomer having one or more hydroxyl groups; (E) one or more hydroxyl group-containing monomers selected from hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide; (F) a monomer that acts as a crosslinker; (G) a monomer other than the components (A) to (F), the content of the (A) component is 10 to 50 mass%, the content of the (B) component is 5 to 20 mass%, the content of the (C) component is 5 to 40 mass%, the content of the (D) component is 5 to 40 mass%, the content of the (E) component is 5 to 30 mass%, the content of the (F) component is 0.1 to 15 mass%, and the content of the (G) component is 0 to 50 mass%, relative to the total of all monomer components in the composition (100 mass%); A monomer composition for contact lenses. 【Chemistry 1】 [In formula (1), a represents an integer of 20 to 500; b represents an integer of 1 to 70; c represents 0 or 1; p and q each represent 0 or 1; X represents -CH 2 -or-CH 2 CH 2 - represents.] 【Chemistry 2】

2. the composition further contains (H) a solvent having a hydroxyl group, and the content of the component (H) is 30 parts by mass or less per 100 parts by mass of the total of all monomer components in the composition; The monomer composition for contact lenses according to claim 1 .

3. A polymer, which is a polymerization reaction product of polymerizable unsaturated groups of the following structural units: (A) a phosphorylcholine group-containing polysiloxane monomer represented by the following formula (1): (B) A phosphorylcholine group-containing methacrylic monomer represented by the following formula (2): (C) Trimethylsiloxylyl group-containing silicone monomer having one or more hydroxyl groups (D) Monovinyl ether monomer having one or more hydroxyl groups (E) One or more hydroxyl group-containing monomers selected from the group consisting of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl acrylamide. (F) A monomer that acts as a cross-linking agent. 【Chemistry 3】 [In formula (1), a represents an integer of 20 to 500; b represents an integer of 1 to 70; c represents 0 or 1; p and q each represent 0 or 1; X represents -CH 2 -or-CH 2 CH 2 - represents.] 【Chemistry 4】

4. The polymer according to claim 3 , further comprising (H) a solvent having a hydroxyl group as a constituent unit.

5. the content of (A) is 10 to 50 mass%, the content of (B) is 5 to 20 mass%, the content of (C) is 5 to 40 mass%, the content of (D) is 5 to 40 mass%, the content of (E) is 5 to 30 mass%, and the content of (F) is 0.1 to 15 mass%, relative to 100 mass% in total of the structural units of the polymer before polymerization; The polymer according to claim 4.

6. The polymer according to claim 3, Contact lenses.

7. A process for washing the polymer by mixing the polymer according to any one of claims 3 to 5 with one or more solvents selected from water, methanol, ethanol, 1-propanol, and 2-propanol; and hydrating the polymer by immersing it in physiological saline. A method for manufacturing contact lenses.

Citation Information

Patent Citations

  • Copolymer with phosphorylcholine group or its derivative group, its production, and antithrombotic material

    JP1995268038A

  • Polysiloxane having phosphorylcholine group and method for producing the same

    JP2004175830A

  • Transparent liquid composition and polymer

    JP2007197513A

  • Phoslorylcholine-based medical amphiphilic silicone

    JP2012530052A

  • Method for manufacturing hydrophilic silicone macromer

    JP2013139567A