Waterproof sheet, resin composition for waterproof sheet, and method for producing waterproof sheet

A resin composition with polyvinyl chloride homopolymer, ethylene/carbon monoxide/vinyl acetate copolymer, and plasticizer, combined with a reinforcing layer, addresses the issue of deteriorating waterproof performance in outdoor sheets by maintaining flexibility and suppressing shrinkage.

JP7552068B2Active Publication Date: 2024-09-18SUMITOMO BAKELITE CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020082402
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-08
Publication Date
2024-09-18
Estimated Expiration
2040-05-08

Smart Images

  • Figure 0007552068000002
    Figure 0007552068000002
  • Figure 0007552068000001
    Figure 0007552068000001
Patent Text Reader

Abstract

To provide a waterproof sheet that can maintain its waterproof performance for a long period of time.SOLUTION: A waterproof sheet 10 contains: (A) polyvinyl chloride resin; (B) ethylene, carbon monoxide, and vinyl acetate copolymer; and (C) a plasticizer. The polyvinyl chloride resin (A) is a homopolymer of vinyl chloride.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a waterproof sheet, a resin composition for a waterproof sheet, and a method for producing a waterproof sheet. [Background technology]

[0002] Waterproof sheets are installed on roofs and balconies of buildings to prevent water from penetrating into the interior. Because waterproof sheets are used outdoors, they deteriorate and lose their waterproof performance when exposed to sunlight and heat for a long period of time. Therefore, waterproof sheets that can maintain their waterproof performance for a long period of time are being developed.

[0003] Patent Document 1 discloses a thermoplastic resin composition containing a vinyl chloride resin, an ethylene-carbon monoxide-vinyl acetate copolymer, and a thermoplastic urethane elastomer. The document states that the thermoplastic resin composition can be used as a wire covering material.

[0004] Patent Documents 2 to 6 disclose a resin composition and a waterproof sheet containing an acrylic-grafted vinyl chloride resin and an ethylene-carbon monoxide-vinyl acetate copolymer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 59-33345 [Patent Document 2] JP 2017-132996 A [Patent Document 3] JP 2017-132997 A [Patent Document 4] JP 2017-132998 A [Patent Document 5] JP 2017-132999 A [Patent Document 6] JP 2017-133000 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in Patent Document 1, it is not clear what structure the vinyl chloride resin actually used has.

[0007] Patent Documents 2 to 6 disclose waterproof sheets containing an acrylic-grafted vinyl chloride resin and an ethylene-carbon monoxide-vinyl acetate copolymer, but there is room for improvement in terms of long-term waterproof performance. [Means for solving the problem]

[0008] The present invention can be shown as follows. According to the present invention, (A) polyvinyl chloride resin; (B) ethylene-carbon monoxide-vinyl acetate copolymer; (C) a plasticizer; A waterproof sheet comprising the polyvinyl chloride resin (A) which is a homopolymer of vinyl chloride. is provided. According to the present invention, (A) polyvinyl chloride resin; (B) ethylene-carbon monoxide-vinyl acetate copolymer; (C) a plasticizer; wherein the polyvinyl chloride resin (A) is a homopolymer of vinyl chloride. According to the present invention, There is also provided a method for producing a waterproof sheet, which comprises a step of melt-extruding the resin composition for a waterproof sheet at a temperature of 130 to 210°C. Effect of the Invention

[0009] According to the present invention, it is possible to provide a waterproof sheet, a resin composition for a waterproof sheet, and a method for producing a waterproof sheet that are capable of maintaining waterproof performance for a long period of time. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of a waterproof sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference symbols and their description will be omitted as appropriate. In addition, "~" indicates "above" to "below" unless otherwise specified. FIG. 1 is a cross-sectional view showing the structure of the waterproof sheet of the present embodiment.

[0012] 1, the waterproof sheet 10 of this embodiment comprises, in this order, a back layer 12, a reinforcing material layer 14, and a front layer 16. The components contained in the back layer 12 and the components contained in the front layer 16 are substantially the same, and include (A) a polyvinyl chloride resin, (B) an ethylene-carbon monoxide-vinyl acetate copolymer, and (C) a plasticizer. First, these components will be described.

[0013] [Polyvinyl chloride resin (A)] The waterproof sheet of this embodiment contains a polyvinyl chloride resin (A). The polyvinyl chloride resin (A) is a homopolymer of vinyl chloride.

[0014] In this embodiment, by using a combination of polyvinyl chloride resin (A), which is a homopolymer of vinyl chloride, and ethylene-carbon monoxide-vinyl acetate copolymer (B), the volumetric shrinkage of the waterproof sheet is suppressed, and the waterproof performance can be maintained for a long period of time. The average degree of polymerization of the polyvinyl chloride resin (A) is 700 or more and 3,000 or less, and preferably 1,000 or more and 3,000 or less.

[0015] Examples of the polyvinyl chloride resin (A) include ZEST 1300Z (manufactured by Shin-Dai-Ichi Vinyl), S1003 (manufactured by Kaneka Corporation), and TK-1300 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0016] [Ethylene-carbon monoxide-vinyl acetate copolymer (B)] The waterproof sheet of the present embodiment contains ethylene-carbon monoxide-vinyl acetate copolymer (B) (hereinafter, also referred to as copolymer (B)).

[0017] From the viewpoint of the effects of the present invention, the copolymer (B) that can be preferably used has an ethylene content of 40 to 80% by weight, a carbon monoxide content of 5 to 20% by weight, and a vinyl acetate content of 15 to 50% by weight.

[0018] The melting point of the copolymer (B) is 30 to 80° C., preferably 40 to 75° C. If the melting point is within this range, it acts as a softener when used outdoors, effectively suppresses the volumetric shrinkage of the waterproof sheet, and can maintain the waterproof performance for a longer period of time.

[0019] Examples of the copolymer (B) include Elbaloy 741, 742, HP441, HP661, HP662, HP4051, AS, and AM (manufactured by Mitsui DuPont Polychemicals).

[0020] The copolymer (B) can be contained in an amount of 10 to 80 parts by weight, preferably 30 to 60 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin (A). By including the copolymer (B) in this range, the amount of the plasticizer (C) added can be reduced, and the influence of loss of the plasticizer due to volatilization, etc. can be reduced. Therefore, the waterproof sheet of this embodiment can maintain its flexibility and can maintain its waterproof performance for a longer period of time.

[0021] [Plasticizer (C)] The waterproof sheet of this embodiment contains a plasticizer (C). The plasticizer (C) may be any known plasticizer within the scope of the effects of the present invention, and specifically, it is at least one selected from the group consisting of phthalic acid plasticizers, adipic acid plasticizers, phosphoric acid plasticizers, trimellitic acid plasticizers, and polyester plasticizers. The plasticizer (C) can be contained in an amount of 10 to 100 parts by weight, preferably 20 to 70 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin (A).

[0022] Since the waterproof sheet of this embodiment contains the copolymer (B), the amount of plasticizer (C) added can be reduced to the above-mentioned range, and the effects of loss of the plasticizer due to volatilization, etc. (reduction in flexibility) can be mitigated.

[0023] [Other ingredients] The waterproof sheet of the present embodiment may contain ultraviolet absorbing agents, antioxidants, pigments, processing aids, stabilizers, fillers, and the like as main components in addition to the above-mentioned components.

[0024] The resin composition for waterproof sheets of this embodiment can be obtained by mixing polyvinyl chloride resin (A), ethylene-carbon monoxide-vinyl acetate copolymer (B), plasticizer (C), and, if necessary, other components as described above, by a conventionally known method. The amount of copolymer (B) added to polyvinyl chloride resin (A), the amount of plasticizer (C) added to copolymer (B), and the effects thereof are as described above.

[0025] <Waterproof sheet> The waterproof sheet 10 of this embodiment comprises, in this order, a back layer 12 located on the application surface side, a reinforcing material layer 14, and a front layer 16. The back layer 12 is about 0.1 to 2 mm thick, and the front layer is about 0.05 to 3 mm thick. The thickness of the reinforcing material layer 14 of the waterproof sheet is appropriately selected depending on the material constituting the reinforcing material layer 14 and the required strength, but is about 200 to 400 μm.

[0026] The back layer 12 and the front layer 16 can be formed from the resin composition for waterproof sheets of this embodiment, and the components may be the same or different. The back layer 12 and the front layer 16 may each be configured with a laminated structure of two or more layers. The front layer 16 preferably contains an ultraviolet absorbing agent to suppress deterioration due to sunlight. The back layer 12 may be an adhesive layer, and an adhesive layer may be provided separately on the application surface side of the back layer 12.

[0027] In the back layer 12 and the front layer 16 formed from the resin composition for waterproof sheet of this embodiment, the copolymer (B) is compatible with the polyvinyl chloride resin (A). Due to this compatible state, the volumetric shrinkage of the waterproof sheet is effectively suppressed, and the waterproof performance can be maintained for a long period of time.

[0028] The reinforcing layer 14 can efficiently improve the rigidity and strength of the waterproof sheet 10, can obtain good shape stability due to low shrinkage, and can also suppress the occurrence of cracks, breaks, etc. As the reinforcing layer 14, a woven or nonwoven fabric made of inorganic fibers such as glass fibers or organic synthetic fibers such as polyester fibers can be suitably used.

[0029] Since the volumetric shrinkage of the waterproof sheet of this embodiment is effectively suppressed, in the following weather resistance test, the change rate of the elongation after the weather resistance test relative to the elongation before the weather resistance test is within -15%, preferably within -12%. Metal halide lamp weather resistance test: Irradiation intensity 90mW / cm 2 , 2 minutes out of 120 minutes spray cycle, black panel temperature 80℃, exposure time 2700 hours

[0030] <Waterproof sheet manufacturing method> The waterproof sheet of the present embodiment includes a step of melting the resin composition for waterproof sheets at a temperature of 130 to 210° C., and a step of forming the molten composition into a sheet.

[0031] By heating and melting the resin composition for waterproof sheets of this embodiment within the above temperature range, the copolymer (B) becomes sufficiently compatible with the polyvinyl chloride resin (A), the volumetric shrinkage of the waterproof sheet is effectively suppressed, and the waterproof performance can be maintained for a longer period of time.

[0032] Examples of the method for forming into a sheet include a calendar method or an extrusion method. The waterproof sheet having a multilayer structure of this embodiment may be formed by forming a resin composition into a sheet by a calendar method, an extrusion method, or the like, and laminating and integrating the resin compositions constituting the other layers by a calendar method, or each resin composition may be formed into a sheet in advance separately by a calendar method or an extrusion method, and then laminated and integrated by a lamination method such as a lamination method. Also, each resin composition may be multilayered by coextrusion.

[0033] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention.

[0034] For example, the waterproof sheet may have a structure in which the back layer 12, the reinforcing material layer 14, and the surface layer 16 are laminated in this order as in the present embodiment, or may have a structure in which the reinforcing material layer 14 and the surface layer 16 are laminated, a structure in which only the surface layer 16 is formed, or a structure in which the back layer 12 and the surface layer 16 are laminated without providing the reinforcing material layer 14. In any layer structure, a functionality-imparting layer such as an antifouling layer or a hard coat layer may be formed on the surface of the surface layer 16. EXAMPLES

[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0036] (Examples 1 to 10, Comparative Examples 1 to 7) A resin composition was prepared by mixing each material listed in Table 1 in the compounding ratio, and the resin composition was melted at a temperature of 170°C and formed into a sheet by a calendar method. The sheet was then laminated and integrated onto a net to produce a waterproof sheet consisting of a surface layer and a reinforcing layer (net). The formulations of the resin compositions of the respective Examples and Comparative Examples are shown in Table 1.

[0037] <Evaluation of waterproof sheets> [Weather resistance evaluation] Using a metal halide lamp weather resistance tester (Metal Weather, manufactured by Daipla Wintes), light emitted from a metal halide lamp as a light source was irradiated continuously from the normal direction onto the surface of the waterproof sheet of each Example and Comparative Example for 2700 hours, after which the elongation of the waterproof sheet was measured, and the change from the elongation of the waterproof sheet before the test was calculated according to the following formula and evaluated according to the following criteria. The results are shown in Table 1. Formula: (Elongation rate of waterproof sheet after test / Elongation rate of waterproof sheet before test) x 100 (standard) 〇: 70% or more, △: Less than 70% 60% or more ×: Less than 60%

[0038] [Olsen bending stiffness test] According to JIS K7106 (cantilever beam), the Olsen bending stiffness modulus was measured at 23° C. and evaluated according to the following criteria. The results are shown in Table 1. (standard) ○: 1500N / cm 2 less than, ×:1500N / cm 2 End

[0039] [Table 1]

[0040] The ingredients listed in Table 1 are as follows. Polyvinyl chloride resin (A): ZEST 1300Z (manufactured by Shin-Daiichi Vinyl Co., Ltd.) Ethylene-carbon monoxide-vinyl acetate copolymer (B): Elvaloy 724 (manufactured by Mitsui DuPont Polychemicals) Plasticizer (C): Bis(2-ethylhexyl) phthalate (DOP) (manufactured by Mitsubishi Chemical Corporation)

[0041] As is clear from Table 1, it was presumed that the waterproof sheet of the present invention had excellent weather resistance and flexibility, and maintained its waterproof performance for a long period of time. In contrast, the comparative examples did not produce satisfactory results. [Explanation of symbols]

[0042] 10. Tarpaulin 12 Back layer 14 Reinforcement layer 16 Surface layer

Claims

1. A polyvinyl chloride resin (A), an ethylene-carbon monoxide-vinyl acetate copolymer (B); A plasticizer (C); Including, The polyvinyl chloride resin (A) is a homopolymer of vinyl chloride, A waterproof sheet comprising 100 parts by weight of polyvinyl chloride resin (A) and 10 to 80 parts by weight of ethylene-carbon monoxide-vinyl acetate copolymer (B).

2. 2. The waterproof sheet according to claim 1, wherein the polyvinyl chloride resin (A) is compatible with the ethylene-carbon monoxide-vinyl acetate copolymer (B).

3. 3. The waterproof sheet according to claim 1, comprising 30 to 60 parts by weight of an ethylene-carbon monoxide-vinyl acetate copolymer (B) per 100 parts by weight of the polyvinyl chloride resin (A).

4. The waterproof sheet according to any one of claims 1 to 3, comprising 10 to 100 parts by weight of a plasticizer (C) per 100 parts by weight of the polyvinyl chloride resin (A).

5. Irradiation intensity 90mW / cm 2 The waterproof sheet according to any one of claims 1 to 4, wherein when a metal halide lamp weather resistance test is conducted under the conditions of a spray cycle of 120 minutes for 2 minutes, a black panel temperature of 80°C, and an irradiation time of 2700 hours, the change in elongation after the weather resistance test relative to the elongation before the weather resistance test is within -15%.

6. The waterproof sheet according to any one of claims 1 to 5, wherein the plasticizer (C) is at least one selected from the group consisting of phthalic acid-based plasticizers, adipic acid-based plasticizers, phosphoric acid-based plasticizers, trimellitic acid-based plasticizers, and polyester-based plasticizers.

7. A waterproof sheet described in any one of claims 1 to 6, wherein the melting point of the ethylene-carbon monoxide-vinyl acetate copolymer (B) is 30 to 80°C.

8. A back layer, a reinforcing material layer, and a front layer are provided in this order, The waterproof sheet according to any one of claims 1 to 7, wherein the back layer and the front layer contain polyvinyl chloride resin (A), an ethylene-carbon monoxide-vinyl acetate copolymer (B), and a plasticizer (C).

9. A polyvinyl chloride resin (A), an ethylene-carbon monoxide-vinyl acetate copolymer (B); A plasticizer (C); Including, The polyvinyl chloride resin (A) is a homopolymer of vinyl chloride, A resin composition for waterproof sheets, comprising 100 parts by weight of a polyvinyl chloride resin (A) and 10 to 80 parts by weight of an ethylene-carbon monoxide-vinyl acetate copolymer (B).

10. The resin composition for waterproof sheets according to claim 9, which contains 30 to 60 parts by weight of ethylene-carbon monoxide-vinyl acetate copolymer (B) per 100 parts by weight of polyvinyl chloride resin (A).

11. A resin composition for waterproof sheets as described in claim 9 or 10, containing 10 to 100 parts by weight of a plasticizer (C) per 100 parts by weight of the ethylene-carbon monoxide-vinyl acetate copolymer (B).

12. A step of melting the waterproof sheet resin composition according to any one of claims 9 to 11 at a temperature of 130 to 210 ° C.; forming the molten composition into a sheet; A method for manufacturing a waterproof sheet, comprising:

Citation Information

Patent Citations

  • Thermoplastic resin composition

    JP1984033345A

  • Acrylic-vinyl chloride copolymer resin-laminated waterproof sheet

    JP2009270290A

  • Waterproof sheet

    JP2017081112A

  • Polyvinyl chloride resin composition and polyvinyl chloride resin sheet

    JP2017132996A

  • Polyvinyl chloride resin composition and polyvinyl chloride resin sheet

    JP2017132997A