Airless tires
The application of a polyamide resin adhesive layer between the metal hub and resin spokes in airless tires enhances adhesive strength, addressing durability issues and maintaining ride comfort.
Patent Information
- Application Number
- JP2020138474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-08-19
AI Technical Summary
The durability of airless tires is limited by the adhesive strength between the hub and spokes, which are made of different materials.
An adhesive reinforcing layer containing a polyamide resin is applied between the metal hub and resin or elastomer spokes to enhance adhesion, with a thickness of 1 to 10 mm and a flexural modulus of 50 to 300 MPa, ensuring the layer is uniformly applied over the hub's outer peripheral surface.
The adhesive reinforcing layer significantly increases the adhesive strength between the hub and spokes, improving the durability and maintaining ride comfort by preventing separation and distortion during vehicle operation.
Smart Images

Figure 0007552140000004 
Figure 0007552140000011 
Figure 0007552140000010
Abstract
Description
[Technical field]
[0001] The present invention relates to an airless tire. [Background technology]
[0002] Patent Document 1 below describes an airless tire. This airless tire includes a cylindrical tread ring, a metal hub disposed radially inside the tread ring, and spokes made of resin or elastomer that connect the tread ring and the hub. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-153932 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the above-mentioned airless tire, the hub and the spokes are formed from different materials, and therefore, in order to improve the durability of this type of airless tire, it is important to increase the adhesive strength between the hub and the spokes.
[0005] The present invention has been devised in view of the above circumstances, and has as its main object to provide an airless tire that can improve durability. [Means for solving the problem]
[0006] The present invention is an airless tire comprising an annular tread ring having a contact surface, a hub disposed radially inward of the tread ring, and spoke portions connecting the tread ring and the hub, wherein the hub is made of a metal material, the spoke portions are made of a resin or elastomer material, and an adhesive reinforcement layer containing a polyamide resin is provided between the hub and the spoke portions.
[0007] In the airless tire according to the present invention, the adhesive reinforcing layer may have a thickness of 1 to 10 (mm).
[0008] In the airless tire according to the present invention, the adhesive reinforcing layer may have a flexural modulus of 50 to 300 (MPa).
[0009] In the airless tire according to the present invention, the adhesive reinforcing layer may be formed over the entire outer circumferential surface of the hub.
[0010] In the airless tire according to the present invention, the polyamide resin may be a polyamide elastomer having polyamide 6 or polyamide 12 as a hard segment portion.
[0011] In the airless tire according to the present invention, the spoke portion may be made of a thermoplastic resin or an elastomer.
[0012] In the airless tire according to the present invention, the thermoplastic resin may be a polyurethane resin or a polyurethane elastomer. Effect of the Invention
[0013] The airless tire of the present invention has an adhesive reinforcing layer between the hub and the spoke portion, the adhesive reinforcing layer containing a polyamide resin having excellent adhesion to both metals and resins, thereby increasing the adhesive strength between the hub and the spoke portion, and thereby improving durability. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a side view illustrating an example of an airless tire. [Diagram 2] FIG. 2 is a perspective view of FIG. [Diagram 3] FIG. 2 is an enlarged cross-sectional view of a main portion of FIG. [Figure 4]FIG. 2 is a plan view of an example hub composite. [Diagram 5] FIG. 2 is a plan view showing an example of a first mold. [Figure 6] FIG. 2 is a plan view showing an example of a hub arranged in a first mold. [Figure 7] FIG. 4 is a plan view showing an example of a second mold. [Figure 8] FIG. 2 is a top view of an example of a tread ring and hub composite disposed in a second mold; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. It should be understood that the drawings include exaggerated expressions and expressions different from the dimensional ratio of the actual structure in order to facilitate understanding of the present invention. In addition, when there are multiple embodiments, the same or common elements are given the same reference numerals throughout the specification, and duplicated explanations are omitted. Furthermore, the specific configurations shown in the embodiments and drawings are for understanding the contents of the present invention, and the present invention is not limited to the specific configurations shown in the drawings.
[0016] [Basic structure of airless tires] The basic structure of the airless tire of this embodiment will be described. Fig. 1 is a side view showing an example of an airless tire 1. Fig. 2 is a perspective view thereof. Fig. 3 is an enlarged cross-sectional view of a main part of Fig. 1. As shown in Figs. 1 to 3, the airless tire 1 includes a tread ring 2, a hub 3 disposed radially inward of the tread ring 2, and spoke portions 4 connecting the tread ring 2 and the hub 3.
[0017] [Tread Ring] The tread ring 2 is an annular rubber member. The tread ring 2 is formed of, for example, vulcanized rubber. The outer surface of the tread ring 2 in the tire radial direction is formed as a contact surface 2a for contacting the ground (road surface). Various drainage grooves (not shown) may be formed in this contact surface 2a. In addition, spoke portions 4 are joined to an inner peripheral surface 2b of the tread ring 2 in the tire radial direction.
[0018] In a preferred embodiment, a reinforcing cord layer 2c (shown in FIG. 3) is disposed inside the tread ring 2. The reinforcing cord layer 2c is, for example, made of a layer in which a plurality of organic fiber cords or steel cords are oriented in a predetermined direction. Such a reinforcing cord layer 2c increases the rigidity of the tread ring 2 in the tire circumferential direction and / or the tire axial direction, and helps to improve steering stability. Furthermore, a resin material may be added to or compounded with a part of the tread ring 2.
[0019] [Hub] The hub 3 is for fixing an axle (not shown). The hub 3 in this embodiment is made of a metal material. The hub 3 is integrally provided with, for example, a disk portion 3a and a cylindrical portion 3b formed on the outer side in the tire radial direction. The disk portion 3a is disposed concentrically with the tread ring 2. For example, a center bore 3c and a mounting hole 3d are formed in the disk portion 3a.
[0020] [Spokes] The spoke portion 4 is formed between the tread ring 2 and the hub 3 and connects them together.
[0021] The spoke portions 4 have the function of absorbing vibrations during tire running and improving ride comfort. For this reason, the spoke portions 4 are desirably formed of a material having sufficient strength to fully exert its load support capability. The spoke portions 4 of this embodiment are formed of a resin or elastomer material 8. It is desirable to select a resin for the resin or elastomer material 8 that is different from the polyamide resin 9 of the adhesive reinforcement layer 5 described below.
[0022] The resin or elastomer material 8 can be appropriately selected. The resin or elastomer material 8 of this embodiment is made of a thermoplastic resin or elastomer. Such a thermoplastic resin or elastomer material 8 can shorten the curing time (molding time) of the spoke portion 4 in the manufacturing process of the airless tire 1 compared to a thermosetting material. Therefore, the productivity of the airless tire 1 can be improved.
[0023] The thermoplastic resin can be appropriately selected. It is preferable to adopt a polyurethane resin or a polyurethane elastomer as the thermoplastic resin in this embodiment. Such a thermoplastic resin has the strength and elastic modulus required for the spoke portion 4, and is useful for improving the durability of the airless tire 1.
[0024] The spoke portion 4 of the present embodiment integrally includes, for example, an outer ring portion 4a on the outer side in the tire radial direction, an inner ring portion 4b on the inner side in the tire radial direction, and a plurality of spoke elements 4c.
[0025] The outer ring portion 4a is, for example, an annular body joined to the inner circumferential surface 2b of the tread ring 2.
[0026] The inner ring portion 4b is an annular body joined to the outer circumferential surface 3e side of the hub 3 (more specifically, the outer circumferential surface of the cylindrical portion 3b).
[0027] Each spoke element 4c extends in the tire radial direction and connects the outer ring portion 4a and the inner ring portion 4b to each other. Each spoke element 4c can, for example, flex during running to absorb an impact input to the tread ring 2. The shape, etc. of the spoke elements 4c are not limited to the illustrated embodiment, and various embodiments can be adopted, such as those extending in a zigzag shape in the tire radial or circumferential direction, or those extending in a mesh-like shape in a tire circumferential cross section.
[0028] [Adhesive reinforcing layer] As shown in Fig. 3, the airless tire 1 of this embodiment has an adhesive reinforcement layer 5 containing a polyamide resin 9 between the hub 3 and the spoke portion 4. The polyamide resin 9 has excellent adhesive properties with both metal and resin (or elastomer material). Therefore, the adhesive reinforcement layer 5 can increase the adhesive strength between the hub 3 made of a metal material and the spoke portion 4 made of a resin or elastomer material 8. As a result, the airless tire 1 of this embodiment can effectively prevent peeling between the hub 3 and the spoke portion 4 compared to a conventional airless tire (not shown) that does not have the adhesive reinforcement layer 5, thereby improving durability.
[0029] Polyamide resin 9 has particularly good adhesion to polyurethane resin and polyurethane elastomer among resins that can be used for the spoke portion 4. Therefore, when the spoke portion 4 is made of polyurethane resin or polyurethane elastomer as in this embodiment, the adhesive reinforcing layer 5 can exhibit excellent adhesive strength.
[0030] Any polyamide resin having excellent adhesive properties to both metals and resins (or elastomer materials) can be used as the polyamide resin 9. For the polyamide resin 9 of this embodiment, it is preferable to use a polyamide elastomer having polyamide 6 or polyamide 12 as a hard segment portion. Such a polyamide elastomer not only has excellent adhesive properties to both metals and resins (or elastomer materials), but also has excellent heat resistance and durability.
[0031] The thickness W1 (shown in FIG. 3) of the adhesive reinforcement layer 5 is desirably set to 1 to 10 mm. By setting the thickness W1 to 1 mm or more, the adhesive strength between the hub 3 and the spoke portion 4 can be effectively increased. On the other hand, by setting the thickness W1 to 10 mm or less, the adhesive reinforcement layer 5 can be prevented from being broken due to distortion between the hub 3 and the spoke portion 4 that occurs while the vehicle equipped with the airless tire 1 is traveling. Furthermore, the adhesive reinforcement layer 5 can be prevented from moving too much while traveling, thereby improving the ride comfort performance. In order to effectively exert such an effect, the thickness W1 is preferably 3 mm or more and preferably 8 mm or less.
[0032] The flexural modulus of the adhesive reinforcement layer 5 is desirably 50 to 300 MPa. By setting the flexural modulus to 50 MPa or more, the adhesive strength between the hub 3 and the spoke portion 4 can be effectively increased. Furthermore, the movement of the adhesive reinforcement layer 5 during running can be prevented from becoming large, and the ride comfort performance can be improved. On the other hand, by setting the flexural modulus to 300 MPa or less, the adhesive reinforcement layer 5 can follow the deformation of the spoke portion 4 during running, and therefore the ride comfort performance can be improved while preventing the adhesive reinforcement layer 5 from being broken. In order to effectively exert such an action, the flexural modulus is preferably 100 MPa or more and preferably 250 MPa or less.
[0033] In this specification, the "flexural modulus" is a value measured in accordance with ISO178 on a test piece (length 80 mm x width 10 mm x thickness 4 mm) made of the same polyamide resin as the adhesive reinforcing layer 5.
[0034] 1, the adhesive reinforcing layer 5 is desirably formed over the entire circumference of the outer circumferential surface 3e of the hub 3. In this way, the adhesive reinforcing layer 5 can effectively increase the adhesive strength between the hub 3 and the spoke portion 4, and can improve the durability of the airless tire 1.
[0035] [Manufacturing method of airless tires] Next, a method for manufacturing the airless tire 1 will be described.
[0036] [Preparing the tread ring and hub] This embodiment includes a process of preparing a tread ring 2 (shown in FIG. 8) and a hub 3 (shown in FIG. 6). The tread ring 2 is obtained, for example, according to a conventional method, by molding an unvulcanized rubber material, a cord material, or the like into a predetermined shape and vulcanizing the molded product. Meanwhile, the hub 3 is manufactured by various methods such as casting, forging, cutting, and the like. The outer peripheral surface 3e of the hub 3 may be subjected to a surface treatment such as shot blasting and / or an adhesive may be applied thereto. This helps to increase the adhesive strength between the hub 3 and the adhesive reinforcing layer 5.
[0037] [Formation of adhesive reinforcement layer] This embodiment includes a step of forming an adhesive reinforcement layer 5 containing a polyamide resin 9 on the outer peripheral surface 3e of the hub 3. This results in a hub composite 21 (shown in FIG. 4) in which the adhesive reinforcement layer 5 is formed on the outer peripheral surface 3e of the hub 3. A first mold 10 (shown in FIG. 5) is used to form the adhesive reinforcement layer 5. FIG. 4 is a plan view showing an example of the hub composite 21. FIG. 5 is a plan view showing an example of the first mold 10.
[0038] As shown in Fig. 5, the first mold 10 includes, for example, a lower mold 10A and an upper mold (not shown) that is vertically movable relative to the lower mold 10A. Fig. 5 shows the lower side of a mating surface 20 of the lower mold 10A and the upper mold in a closed state.
[0039] A cavity 11 consisting of a cylindrical recess is formed in the lower mold 10A of the first mold 10. The cavity 11 essentially includes a circular bottom surface 13 and an inner circumferential surface 14 rising from the bottom surface 13, and its upper portion is closed by an upper mold (not shown).
[0040] The cavity 11 includes a first cavity 16 and a second cavity 17. In order to facilitate understanding of these, a first boundary 15 between the first cavity 16 and the second cavity 17 is shown by a virtual line in Fig. 5 .
[0041] The first cavity 16 is a space for placing a hub 3 (shown by an imaginary line in FIG. 5) that has been prepared in advance. The first cavity 16 is provided with protruding shafts 18 and 19 that extend upward from the bottom surface 13. The hub 3 is placed in the first cavity 16 with its axis aligned in the up-down direction, and substantially fills the first cavity 16. In other words, the outer circumferential surface 3e of the hub 3 essentially defines the first boundary 15 between the first cavity 16 and the second cavity 17.
[0042] The center bore 3c and the mounting hole 3d (shown in FIG. 4) of the hub 3 are inserted into the protruding shafts 18 and 19 of the first cavity 16, respectively. This helps to accurately align the hub 3 in the first cavity 16.
[0043] The second cavity 17 is a space for molding an adhesive reinforcing layer 5 (shown in FIG. 4) on the outer peripheral surface 3e of the hub 3 placed in the first cavity 16. The second cavity 17 is connected to the outside of the first cavity 16 and extends in an annular shape. The second cavity 17 in this embodiment is defined by the bottom surface 13 of the lower mold 10A, the inner peripheral surface 14 of the cavity 11, the outer peripheral surface 3e of the hub 3 placed in the first cavity 16, and the upper mold (not shown). A gate (not shown) for injecting polyamide resin 9 therein is connected to the second cavity 17.
[0044] A preferable procedure for molding the adhesive reinforcing layer 5 using the first mold 10 configured as above is as follows. Figure 6 is a plan view showing an example of the hub 3 placed in the first mold 10.
[0045] Next, the hub 3 is placed in the first mold 10. Specifically, the first mold 10 is opened, and the hub 3 is placed in the first cavity 16 of the lower mold 10A. Then, an upper mold (not shown) is fitted into the lower mold 10A, and the first mold 10 is closed.
[0046] Next, molten polyamide resin 9 is injected (pressurized injection) through a gate (not shown) into second cavity 17. This fills second cavity 17 with polyamide resin 9. For example, an injection molding machine (not shown) is used to inject polyamide resin 9 according to conventional practices.
[0047] Next, the polyamide resin 9 is cooled and hardened in the first mold 10. As a result, a hub composite 21 in which the adhesive reinforcing layer 5 is formed on the outer circumferential surface 3e of the hub 3 is obtained, as shown in FIG.
[0048] [Removal of the hub complex] This embodiment includes the step of removing the hub composite 21 from the first mold 10. Specifically, the first mold 10 is opened and the hub composite 21 (shown in FIG. 4) is removed.
[0049] [Placement of tread ring and hub composite in second mold] Fig. 7 is a plan view showing an example of the second mold 22. Fig. 8 is a plan view showing an example of the tread ring 2 and the hub composite body 21 arranged in the second mold 22.
[0050] 8, this embodiment includes a step of placing the tread ring 2 and the hub composite 21 in a second mold 22. The second mold 22 is used to mold the spoke portion 4 that connects the tread ring 2 and the hub 3 (hub composite 21) to integrally mold the airless tire 1.
[0051] 7, the second mold 22 includes, for example, a lower mold 22A and an upper mold 22B that is movable in the vertical direction relative to the lower mold 22A. In FIG. 7, the lower side of a mating surface 31 of the upper mold 22B and the lower mold 22A is shown in a closed state, and the upper mold 22B is shown in cross section.
[0052] A cavity 23 consisting of a cylindrical recess is formed in the lower mold 22A of the second mold 22. The cavity 23 essentially includes a circular bottom surface 24 and an inner circumferential surface 25 rising from the bottom surface 24, and its upper portion is closed by the upper mold 22B.
[0053] The cavity 23 includes a third cavity portion 26, a fourth cavity portion 27, and a fifth cavity portion 28. In order to facilitate understanding of these, a second boundary 29 between the third cavity portion 26 and the fifth cavity portion 28, and a third boundary 30 between the fourth cavity portion 27 and the fifth cavity portion 28 are each indicated by a two-dot chain line (phantom line) in Fig. 7.
[0054] The third cavity portion 26 is a space for accommodating a tread ring 2 (shown in FIG. 8) that has been prepared in advance. In this embodiment, the outer peripheral surface of the tread ring 2 is disposed so as to be substantially aligned with the inner peripheral surface 25 of the cavity 23. Therefore, in this state, a position corresponding to the inner peripheral surface 2b (shown in FIG. 8) of the tread ring 2 essentially defines a second boundary 29 (shown by a two-dot chain line) between the third cavity portion 26 and the fifth cavity portion 28.
[0055] The fourth cavity portion 27 is a space for accommodating the hub composite portion 21. The fourth cavity portion 27 is provided with protruding shafts 32 and 33 extending upward from the bottom surface 24. The hub composite portion 21 is disposed in the fourth cavity portion 27 with its axis in the up-down direction, and substantially fills the fourth cavity portion 27. In other words, the outer peripheral surface 21a (shown in FIG. 8 ) of the hub composite portion 21 (the adhesive reinforcement layer 5) essentially defines a third boundary 30 (shown by a two-dot chain line) between the fourth cavity portion 27 and the fifth cavity portion 28.
[0056] 8, the center bore 3c and the mounting hole 3d of the hub 3 are inserted into the protruding shafts 32 and 33 of the fourth cavity portion 27, respectively. This helps to accurately align the hub 3 (hub composite body 21) with the fourth cavity portion 27.
[0057] As shown in FIG. 7, the fifth cavity portion 28 is a space for molding the spoke portion 4 (shown in FIG. 8) between the tread ring 2 arranged in the third cavity portion 26 and the hub 3 (hub composite body 21) arranged in the fourth cavity portion 27. The fifth cavity portion 28 communicates between the third cavity portion 26 and the fourth cavity portion 27. The fifth cavity portion 28 in this embodiment is defined by the bottom surface 24 of the lower mold 22A, the multiple protrusions 34, the multiple protrusions 35, the second boundary 29 (the inner peripheral surface 2b shown in FIG. 8), the third boundary 30 (the outer peripheral surface 21a shown in FIG. 8), and the upper mold 22B.
[0058] The multiple protrusions 34 extend upward from the bottom surface 24 of the lower die 22A. Meanwhile, the multiple protrusions 35 extend downward from the upper die 22B. When the lower die 22A and the upper die 22B are closed, these protrusions 35 enter between the protrusions 34, 34 of the lower die 22A to define the fifth cavity portion 28. In this embodiment, the fifth cavity portion 28 on the hub composite 21 side is connected to an injection gate (not shown) for injecting the thermoplastic resin or elastomer material 8 into the fifth cavity portion 28.
[0059] As shown in FIG. 8, an annular first gap 36 for forming the outer ring portion 4a (shown in FIG. 1) of the spoke portion 4 is formed between each of the protrusions 34, 35 and the inner peripheral surface 2b of the tread ring 2. Similarly, an annular second gap 37 for forming the inner ring portion 4b (shown in FIG. 1) of the spoke portion 4 is formed between each of the protrusions 34, 35 and the outer peripheral surface 21a of the hub composite body 21. In this embodiment, an injection gate (not shown) communicates with the second gap 37. Furthermore, a third gap 38 for forming the spoke element 4c (shown in FIG. 1) is formed between each of the protrusions 34, 35 adjacent to each other in the circumferential direction.
[0060] The first gap 36 to the third gap 38 are connected to each other. Therefore, by injecting the molten thermoplastic resin or elastomer material 8 into the second gap 37 through an injection gate (not shown), the first gap 36 can be filled from the second gap 37 through the third gap 38.
[0061] The tread ring 2 and the hub composite 21 are placed in the second mold 22 configured as above. Specifically, the second mold 22 is opened, and the tread ring 2 is placed in the third cavity portion 26 of the lower mold 22A, and the hub composite 21 is placed in the fourth cavity portion 27, as shown in Fig. 8. Then, the upper mold 22B is fitted into the lower mold 22A, and the second mold 22 is closed. As a result, in this embodiment, the tread ring 2 and the hub composite 21 are placed in the second mold 22.
[0062] Prior to the arrangement of the tread ring 2, the inner circumferential surface 2b of the tread ring 2 may be surface-treated and / or coated with an adhesive, for example, in order to increase the adhesive strength between the tread ring 2 and the spoke portions 4. Furthermore, prior to the arrangement of the hub composite 21, the outer circumferential surface 21a of the hub composite 21 (adhesive reinforcement layer 5) may be surface-treated and / or coated with an adhesive in order to increase the adhesive strength between the adhesive reinforcement layer 5 and the spoke portions 4.
[0063] [Molding of spokes] This embodiment includes a step of molding the spoke portions 4 that connect the tread ring 2 and the hub 3 (hub composite 21) by injecting a molten thermoplastic resin or elastomer material 8 between the tread ring 2 and the hub composite 21 arranged in the second mold 22. By molding the spoke portions 4, the airless tire 1 is integrally molded.
[0064] In this embodiment, a molten thermoplastic resin or elastomer material 8 is injected (pressurized and injected) into the fifth cavity portion 28 (first gap 36 to third gap 38) through an injection gate (not shown). This causes the thermoplastic resin or elastomer material 8 to fill the space between the tread ring 2 and the hub composite 21 arranged in the second mold 22. For example, an injection molding machine (not shown) is used to inject the thermoplastic resin or elastomer material 8 according to conventional practices.
[0065] Next, the thermoplastic resin or elastomer material 8 is cooled and hardened in the second mold 22. This forms the spoke portions 4 that connect the tread ring 2 and the hub 3 (hub complex 21), thereby obtaining the airless tire 1 in which they are integrally molded.
[0066] [Removing airless tires] This embodiment includes a step of removing the airless tire 1 from the second mold 22. Specifically, the second mold 22 is opened, and the airless tire 1 is removed.
[0067] In the manufacturing method of this embodiment, an adhesive reinforcing layer 5 containing polyamide resin 9 (shown in FIG. 4) can be formed between the hub 3 and the spoke portions 4. This makes it possible to reliably manufacture an airless tire 1 that can increase the adhesive strength between the hub 3 and the spoke portions 4 and thereby improve durability.
[0068] Although a particularly preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the illustrated embodiment and can be modified and carried out in various forms. EXAMPLES
[0069] More specific, non-limiting examples of the present invention will now be described.
[0070] [Example A] An airless tire (corresponding to a tire size of 145 / 70R12) having the basic structure shown in Figs. 1 to 3 was produced as a prototype (Example 1). The airless tire of Example 1 was produced by the following method.
[0071] In the manufacturing method of Example 1, a tread ring made of vulcanized rubber and a hub made of an aluminum alloy were prepared. The tread ring was vulcanized under the conditions of 170°C x 20 minutes. An outer reinforcing cord layer and an inner reinforcing cord layer were disposed inside the tread ring. The details of these are as follows. <Outer reinforcement cord layer> Number of plies: 2 Reinforcement cord: Steel cord Cord angle: +21 degrees / -21 degrees <Inner reinforcing cord layer> Number of plies: 2 Reinforcement cord: Steel cord Cord angle: +21 degrees / -21 degrees
[0072] Next, in Example 1, an adhesive (trade name "Chemlock" manufactured by Lord Far East Corporation) was applied to the outer circumferential surface of the hub. The thickness of the adhesive layer was set to 20 μm.
[0073] Next, in Example 1, the hub coated with the adhesive was placed in a first mold. Then, polyamide resin (manufactured by Ube Industries, Ltd. under the trade name "UBESTA (registered trademark)") was injected onto the outer circumferential surface of the hub to form an adhesive reinforcement layer (thickness W1: 3 mm, flexural modulus: 150 MPa). In this way, a hub composite was molded. The polyamide resin was a polyamide elastomer with PA12 (polyamide 12) as the hard segment portion.
[0074] Next, in Example 1, the above-mentioned adhesive was applied to the inner peripheral surface of the tread ring. Next, in Example 1, the tread ring and the hub composite were placed in a second mold. Then, in Example 1, a thermoplastic polyurethane resin was injected between the tread ring and the hub of the second mold. In this way, spoke portions connecting the tread ring and the hub (hub composite) were formed, and an airless tire was manufactured.
[0075] For comparison, an airless tire without an adhesive reinforcing layer was manufactured (Comparative Example). The Comparative Example airless tire had the same structure as Example 1, except for the adhesive reinforcing layer. The durability of the Example 1 and Comparative Example airless tires was evaluated. The test method was as follows.
[0076] <Durability> The adhesive strength between the hub and spokes of the evaluated airless tires was evaluated by a peel test (T-peel) conducted in accordance with JIS K6854. The results are shown as an index with the adhesive strength of Example 1 set at 100. The larger the value, the higher and better the adhesive strength. A value of 60 or higher indicates good durability. The results of the tests are shown in Table 1.
[0077] [Table 1]
[0078] As a result of the test, it was found that Example 1 was able to increase the adhesive strength between the hub and the spokes, and was able to improve the durability of the airless tire, compared to the comparative example.
[0079] [Example B] Airless tires (having the same tire size as in Example A) having the basic structure shown in Figs. 1 to 3 were produced as prototypes (Examples 1 to 6). The configurations of Examples 2 to 6 are substantially the same as the configuration of Example 1 (described in Example A) except for the thickness W1 of the adhesive reinforcing layer.
[0080] The durability and ride comfort were evaluated for the airless tires of Examples 1 to 6. The durability was evaluated in the same manner as in Example A. The ride comfort was tested in the following manner.
[0081] <Ride comfort performance> The tires to be evaluated were attached to the four wheels of a vehicle (small EV: product name COMS), and the vehicle was driven on a tire test course with a dry asphalt road surface with one person aboard, and the ride comfort performance was evaluated by a sensory evaluation by the driver. The results are shown as an index with Example 1 being 100, and the larger the value, the better the performance. The test results are shown in Table 2.
[0082] [Table 2]
[0083] As a result of the tests, Examples 1 and 3 to 5, in which the thickness W1 of the adhesive reinforcement layer was set within a preferred range, were able to maintain ride comfort performance while increasing the adhesive strength between the hub and the spoke portion, compared to Examples 2 and 6.
[0084] [Example C] Airless tires (having the same tire size as in Example A) having the basic structure shown in Figs. 1 to 3 were produced as prototypes (Example 1 and Examples 7 to 11). The configurations of Examples 7 to 11 are substantially the same as the configuration of Example 1 (described in Example A) except for the flexural modulus of the adhesive reinforcing layer.
[0085] The airless tires of Example 1 and Examples 7 to 11 were evaluated for durability and ride comfort. The durability test method was as described in Example A. The ride comfort test method was as described in Example C. The test results are shown in Table 3.
[0086] [Table 3]
[0087] As a result of the tests, Examples 1 and 7 to 10, in which the flexural modulus of the adhesive reinforcement layer is within a preferable range, were able to maintain ride comfort performance while increasing the adhesive strength between the hub and the spoke portion compared to Example 11. [Explanation of symbols]
[0088] 1. Airless tires 2 Tread Ring 3. Hub 4 Spoke section 5 Adhesive reinforcement layer
Claims
1. An airless tire comprising an annular tread ring having a ground contact surface, a hub disposed radially inward of the tread ring, and a spoke portion connecting the tread ring and the hub, The hub is made of a metal material. The spoke portion is made of a resin or an elastomer material, an adhesive reinforcing layer containing a polyamide resin between the hub and the spoke portions; The thickness of the adhesive reinforcing layer is 1 to 10 (mm); Airless tires.
2. An airless tire as described in claim 1, wherein the flexural modulus of the adhesive reinforcement layer is 50 to 300 (MPa).
3. An airless tire as described in claim 1 or 2, wherein the adhesive reinforcement layer is formed around the entire outer circumferential surface of the hub.
4. An airless tire as described in any one of claims 1 to 3, wherein the polyamide resin is a polyamide elastomer having polyamide 6 or polyamide 12 as a hard segment portion.
5. An airless tire as described in any one of claims 1 to 4, wherein the spoke portion is made of a thermoplastic resin or elastomer.
6. An airless tire as described in claim 5, wherein the thermoplastic resin is a polyurethane resin or a polyurethane elastomer.
Citation Information
Patent Citations
Laminate and manufacture thereof
JP1986152443A
Airless tire
JP2017081199A
Non-pneumatic tire
JP2018002142A
Method for producing airless tire, and airless tire
JP2018153932A
Non-pneumatic tire
JP2019218002A