Chamber dry cleaning of photoresist film

The chamber dry cleaning method using etching gases addresses the challenges of EUV lithography by efficiently removing unwanted photoresist material from processing chambers, ensuring reliable and reproducible semiconductor manufacturing.

JP7553489B2Active Publication Date: 2024-09-18LAM RES CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021576240
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2020-06-25
Publication Date
2024-09-18
Estimated Expiration
2040-06-25

AI Technical Summary

Technical Problem

Current photolithography processes face challenges in achieving reliable and reproducible resolution for features smaller than the wavelength of light, particularly with EUV lithography, due to low power output, light loss during patterning, and issues with conventional organic chemically amplified resists leading to blurring and pattern collapse.

Method used

A method and apparatus for chamber dry cleaning using etching gases like hydrogen halides to remove unwanted photoresist material from processing chambers, followed by purging and conditioning to restore the chamber surfaces, ensuring efficient removal of residual gases and preventing contamination.

Benefits of technology

The method effectively cleans EUV resist material from chamber surfaces, reducing contamination and enhancing tool availability by minimizing manual scrubbing and downtime, while maintaining chamber integrity for precise semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553489000004
    Figure 0007553489000004
  • Figure 0007553489000017
    Figure 0007553489000017
  • Figure 0007553489000025
    Figure 0007553489000025
Patent Text Reader

Abstract

Metal-containing photoresist films may be deposited on semiconductor substrates using dry deposition techniques. During deposition, bevel and backside cleaning, baking, developing, or etching operations, unintentional metal-containing photoresist material may form on the interior surfaces of the processing chamber. An in-situ chamber dry clean may be performed to remove the unintentional metal-containing photoresist material by exposing it to an etching gas. The chamber dry clean may be performed at high temperatures without striking a plasma. In some embodiments, the chamber dry clean may include pumping / purging and conditioning operations.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (Incorporated by reference) A PCT application form is being filed contemporaneously herewith as a part of this application. Each application to which this application claims priority or the benefit of priority as set forth in the contemporaneously filed PCT application form is hereby incorporated by reference in its entirety for all purposes. [Background technology]

[0002] The fabrication of semiconductor devices, such as integrated circuits, is a multi-step process that involves photolithography. Typically, the process involves the deposition of material onto a wafer and patterning the material by lithographic techniques to form structural features (e.g., transistors and circuits) of the semiconductor device. Typical photolithography process steps known in the prior art include: preparing a substrate; applying a photoresist, such as by spin coating; exposing the photoresist to light in a desired pattern and dissolving to some extent the exposed areas of the photoresist with a developer; applying and developing a developer to remove either the exposed or unexposed areas of the photoresist; and subsequent processing to create features in the areas of the substrate from which the photoresist has been removed, such as by etching or material deposition.

[0003] Advances in semiconductor design have been driven by the need and ability to create ever-smaller features in semiconductor substrate materials. This technological advance is characterized by "Moore's Law," which states that the density of transistors in dense integrated circuits will double every two years. In fact, advances in chip design and manufacturing mean that modern microprocessors may contain billions of transistors and other circuit features on a single chip. Individual features on such chips may be on the order of 22 nanometers (nm) or smaller, and in some cases may be less than 10 nm.

[0004] One challenge in manufacturing devices with such fine features is the ability to reliably and reproducibly create photolithography masks with sufficient resolution. Current photolithography processes expose photoresist using ultraviolet (UV) light, typically at 193 nm. The fact that the wavelength of this light is significantly larger than the desired size of the features to be created on the semiconductor substrate creates inherent problems. Achieving feature sizes smaller than the wavelength of light requires complex resolution enhancement techniques such as multiple patterning. As a result, there has been great interest and research effort in developing photolithography techniques that use shorter wavelength light, such as extreme ultraviolet (EUV) light, which has a wavelength between 10 nm and 15 nm, e.g., 13.5 nm.

[0005] However, EUV photolithography processes can be subject to challenges such as low power output and light loss during patterning. Typical organic chemically amplified resists (CARs), similar to those used in 193 nm UV lithography, have potential drawbacks when used in EUV lithography, especially due to their low absorption coefficient in the EUV region, which can lead to blurring and rough line edges due to diffusion of photoactivated chemical species. Furthermore, to provide the etch resistance required to pattern the underlying device layers, fine features patterned in conventional CAR materials can run the risk of causing high aspect ratios and pattern collapse. Thus, there remains a demand for improved EUV photoresist materials with the properties of low thickness, excellent absorbance, and excellent etch resistance.

[0006] The background discussion provided herein is intended to provide an overall presentation of the state of the art. To the extent that it is provided in this background section, aspects of the inventors' work as currently set forth, and of the discussion that may not qualify as prior art at the time of filing, are not admitted, expressly or impliedly, to be prior art against the present technology. Summary of the Invention

[0007] A chamber dry clean may be performed in the context of photoresist patterning. After a photoresist material is dry deposited in a process chamber, unwanted photoresist material may accumulate on the interior surfaces of the process chamber. The photoresist material may be, for example, a metal-containing EUV resist material. A chamber dry clean may be performed to remove the unwanted photoresist material by exposing it to an etching gas. In some embodiments, the etching gas may be a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a combination thereof. A purge may then be performed to remove residual etching gas from the process chamber. In some embodiments, the process chamber may then be conditioned or seasoned to restore the interior surfaces by depositing a coating of a film (e.g., a photoresist material) thereon.

[0008] Disclosed herein are methods and systems for cleaning a processing chamber, the method including providing a semiconductor substrate having a metal-containing resist film dry-deposited on a substrate layer of the semiconductor substrate in a processing chamber, and introducing an etching gas into the processing chamber, where a first thickness of dry-deposited metal-containing resist material is formed on one or more surfaces of the processing chamber, and the etching gas removes the first thickness of dry-deposited metal-containing resist material.

[0009] In some embodiments, the method further includes conditioning one or more surfaces of the processing chamber by forming a second thickness of a dry-deposited metal-containing resist material on the one or more surfaces of the processing chamber. In some embodiments, the method further includes purging the processing chamber after introducing the etching gas to remove residual etching gas from the processing chamber. In some embodiments, purging the processing chamber includes flowing an inert gas and / or a reactive gas into the processing chamber, the processing chamber being heated to an elevated temperature of about 20° C. to about 140° C., and the processing chamber being pumped such that the chamber pressure is about 13.3322 Pascals to about 799.934 Pascals (about 0.1 Torr to about 6 Torr). In some embodiments, purging the processing chamber includes subjecting one or more surfaces of the processing chamber to a remote plasma-based treatment to remove residual etching gas, the remote plasma-based treatment including a fluorine-based chemistry. In some embodiments, purging the processing chamber includes exposing one or more surfaces of the processing chamber to ozone and / or oxygen gas to remove residual etching gas. In some embodiments, the method further comprises heating one or more surfaces of the process chamber to an elevated temperature between about 20° C. and about 140° C. prior to introducing the etching gas. In some embodiments, the etching gas comprises a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a combination thereof. In some embodiments, the removal of the first thickness of the dry-deposited metal-containing resist material occurs without exposure to a plasma. In some embodiments, the method further comprises pumping the process chamber until the chamber pressure is between about 13.3322 Pascals and 799.934 Pascals (about 0.1 Torr and 6 Torr), heating one or more surfaces of the process chamber to an elevated temperature between about 20° C. and about 140° C., and introducing a dummy wafer into the process chamber prior to introducing the etching gas. In some embodiments, the dry-deposited metal-containing resist material is an organometallic oxide or organometallic-containing thin film.

[0010] Disclosed herein is an apparatus for depositing resist. The apparatus includes a process chamber including a substrate support, a vacuum line coupled to the process chamber, and an etching gas line coupled to the process chamber. The apparatus further includes a controller configured with instructions for cleaning the process chamber, the instructions including code for depositing a metal-containing resist film on a substrate layer of a semiconductor substrate in the process chamber, and cleaning the process chamber by flowing an etching gas into the process chamber, the etching gas removing a first thickness of the dry-deposited metal-containing resist material formed on one or more surfaces of the process chamber.

[0011] In some embodiments, the apparatus further includes one or more heaters coupled to one or more surfaces of the processing chamber, and the controller further includes instructions including code for heating the one or more surfaces of the processing chamber to an elevated temperature, the elevated temperature being between about 20° C. and about 140° C. In some embodiments, the controller includes instructions including code for conditioning the one or more surfaces of the processing chamber by forming a second thickness of a dry deposited metal-containing resist material on the one or more surfaces of the processing chamber. In some embodiments, the controller includes instructions including code for purging the processing chamber after introducing the etching gas to remove residual etching gas from the processing chamber.

[0012] These and other features of the disclosed embodiments are described in detail below with reference to the accompanying drawings. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a flow diagram of an example method for performing chamber dry cleaning while depositing and developing photoresist, according to some embodiments.

[0014] [Diagram 2] FIG. 2 is a flow diagram of an exemplary method for performing a chamber dry clean, according to some embodiments.

[0015] [Figure 3A] 3A-3D are cross-sectional schematic diagrams of various process stages of chamber dry cleaning according to some embodiments. [Figure 3B] 3A-3B are cross-sectional schematic diagrams of various processing stages of chamber dry cleaning according to some embodiments. [Figure 3C] 3A-3C are cross-sectional schematic diagrams of various processing stages of chamber dry cleaning according to some embodiments. [Figure 3D] 3A-3D are cross-sectional schematic diagrams of various processing stages of chamber dry cleaning according to some embodiments.

[0016] [Figure 4] FIG. 4 illustrates an exemplary chamber dry clean mechanism involving a chemical reaction between hydrogen chloride or hydrogen bromide and an organotin oxide / hydroxide resist material coated on the interior surface of a process chamber, according to some embodiments.

[0017] [Diagram 5] FIG. 5 is a graph contrasting HCl, HBr, and BCl3 in etching a metal-containing EUV resist versus time of the cleaning operation.

[0018] [Figure 6] FIG. 6 is a graph comparing the etch rates of various metal-containing EUV resist materials when HBr is used as the etching gas.

[0019] [Figure 7] FIG. 7 is a graph showing the effect of temperature on etch selectivity for removing exposed and unexposed areas of a photopatterned metal-containing EUV resist.

[0020] [Figure 8A] FIG. 8A is a graph showing the effect of temperature on EUV resist removal selectivity.

[0021] [Figure 8B] FIG. 8B is a bar graph showing the effect of temperature on the etch rate for removing EUV resist.

[0022] [Figure 9] FIG. 9 is a graph showing the effect of pressure on etch selectivity for removing exposed and unexposed areas of a photopatterned metal-containing EUV resist.

[0023] [Figure 10A] FIG. 10A is a graph showing the effect of pressure on EUV resist removal selectivity.

[0024] [Figure 10B] FIG. 10B is a bar graph showing the effect of pressure on etch rate for removing EUV resist.

[0025] [Figure 11A] FIG. 11A is a graph showing the performance of HCl as an etching gas at various pressures and temperatures. [Figure 11B] FIG. 11B is a graph showing the performance of HCl as an etching gas at various pressures and temperatures. [Figure 11C] FIG. 11C is a graph showing the performance of HCl as an etching gas at various pressures and temperatures. [Figure 11D] FIG. 11D is a graph showing the performance of HCl as an etching gas at various pressures and temperatures. [Figure 11E] FIG. 11E is a graph showing the performance of HCl as an etching gas at various pressures and temperatures.

[0026] [Figure 12] FIG. 12 is a graph showing the amount of bromine versus time in the process chamber when purging.

[0027] [Figure 13]FIG. 13 is a schematic diagram of an exemplary processing station for maintaining a low pressure environment suitable for performing chamber dry cleaning according to some embodiments.

[0028] [Figure 14] FIG. 14 is a schematic diagram of an exemplary multi-station processing tool suitable for performing the various developing, dry cleaning, rework, descum, and smoothing operations described herein.

[0029] [Figure 15] FIG. 15 is a schematic cross-sectional view of an exemplary inductively coupled plasma apparatus for carrying out certain embodiments and operations described herein.

[0030] [Figure 16] FIG. 16 illustrates a semiconductor processing cluster tool architecture with a patterning module interfaced with a vacuum integrated deposition and vacuum transfer module suitable for carrying out the processes described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The present disclosure relates generally to the field of semiconductor processing. In certain aspects, the present disclosure is directed to a process and apparatus for processing an EUV photoresist (e.g., an EUV-sensitive metal and / or metal oxide-containing photoresist film) in the context of EUV patterning and developing the EUV patterned film to form a patterning mask.

[0032] In this specification, we will look at specific embodiments of the present disclosure in detail. Examples of specific embodiments are shown in the accompanying drawings. Although the present disclosure will be described in conjunction with these specific embodiments, it will be understood that it is not intended to limit the present disclosure to such specific embodiments. Rather, it is intended to cover alternatives, modifications, and equivalents that may be included within the spirit and scope of the present disclosure. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the present disclosure. The present disclosure may be practiced without some or all of these specific details. In other instances, well-known processing operations have not been described in detail in order not to unnecessarily obscure the present disclosure.

[0033] Overview Patterning of thin films in semiconductor processing is often a critical step in semiconductor manufacturing. Patterning involves lithography. In traditional photolithography, such as 193 nm photolithography, patterns are printed by emitting photons from a photon source onto a mask to print the pattern onto a light-sensitive photoresist, which causes a chemical reaction in the photoresist that, after development, removes certain portions of the photoresist to form the pattern.

[0034] Advanced technology nodes (defined by the International Technology Roadmap for Semiconductors) include 22 nm, 16 nm, and beyond. For example, at the 16 nm node, the width of a typical via or line in a damascene structure usually does not exceed about 30 nm. Scaling of features in advanced semiconductor integrated circuits (ICs) and other devices employs lithography to improve resolution.

[0035] Extreme ultraviolet (EUV) lithography can extend lithography techniques by shortening the wavelength of the imaging source beyond what can be achieved with traditional photolithography methods. EUV sources with wavelengths of approximately 10-20 nm, or 11-14 nm, for example 13.5 nm, are available for state-of-the-art lithography tools, also called scanners. EUV radiation is strongly absorbed by a wide range of solid and fluid materials, such as quartz and water vapor, and therefore operates in a vacuum.

[0036] EUV lithography utilizes an EUV resist that is patterned to form a mask for use in etching an underlying layer. The EUV resist may be a polymeric chemically amplified resist (CAR) made by liquid-based spin-on techniques. An alternative to CAR is a directly photopatternable metal oxide-containing film, such as those available from Inpria, Inc., Corvallis, Oregon, and described, for example, in U.S. Patent Publication Nos. 2017 / 0102612, 2016 / 021660, and 2016 / 0116839, which are incorporated herein by reference for their disclosure of directly photopatternable metal oxide-containing films at least. Such films are made by spin-on techniques or dry deposition. Metal oxide-containing films can be directly patterned (i.e., without the use of a separate photoresist) by exposure to EUV in a vacuum environment to achieve patterning resolution below 30 nm, as described, for example, in U.S. Pat. No. 9,996,004, issued June 12, 2018, entitled EUV PHOTOPATTERNING OF VAPOR-DEPOSITED METAL OXIDE-CONTAINING HARDMASKS, and / or PCT / US19 / 31618, filed May 9, 2019, entitled METHODS FOR MAKING EUV PATTERNABLE HARD MASKS, which are incorporated herein by reference for at least their disclosures regarding the composition, deposition, and patterning of directly photopatternable metal oxide films to form EUV resist masks. Generally, patterning involves exposing an EUV resist to EUV radiation to form a photopattern in the resist, followed by development to remove portions of the resist according to the photopattern to form the mask.

[0037] It should also be understood that the present disclosure relates to lithographic patterning techniques and materials exemplified using EUV lithography, but is applicable to other next generation lithographic techniques. Besides EUV, which includes the standard 13.5 nm EUV wavelength currently in use and under development, the most relevant radiation source for such lithography is DUV (deep UV), which generally refers to the use of 248 nm or 193 nm excimer laser sources, X-rays (which formally include EUV in the lower energy range of the X-ray range), and electron beams that can cover a wide energy range. Specific methods may vary depending on the specific materials and applications used in the semiconductor substrate and the ultimate semiconductor device. As such, the methods described herein are merely exemplary of methods and materials that may be used in current technology.

[0038] Direct photopatternable EUV resists may consist of or contain metals and / or metal oxides mixed in an organic component. Metals / metal oxides hold great promise due to their ability to enhance EUV photon absorption, generate secondary electrons, and / or provide improved etch selectivity relative to the underlying film stack and device layers.

[0039] When manufacturing semiconductor devices, it is important that the manufacturing process is accurate and repeatable. Unfortunately, as a semiconductor manufacturing reaction chamber processes multiple substrates over time, the processing conditions and chemicals within the reaction chamber change. During deposition and application of a metal-containing EUV resist film onto a semiconductor substrate, for example, the dry deposition described herein, some unintended deposition of metal-containing EUV resist material on the chamber surfaces may occur. After performing several processing operations in the processing chamber, the unintended formation of metal-containing EUV resist material on the chamber surfaces may reach a level that makes the EUV resist material more susceptible to flaking and peeling. In some cases, particles and film impurities coming from the EUV resist material in the processing chamber may fall onto the substrate surface during processing. For example, particles and film impurities may come from the inner surfaces of the chamber walls, ceiling, showerhead, substrate support, lift pins, gas lines, nozzles, etc. Such particles and film impurities that peel or flake off from the inner surfaces of the processing chamber may cause contamination and defect issues in the semiconductor substrate. This contamination can not only cause contamination of the semiconductor substrate itself, but also downstream processing tools such as patterning (scanner) and development tools.

[0040] Traditionally, removal of unintentional deposits on the interior surfaces of a processing chamber can be accomplished by manually opening the processing chamber and mechanically scrubbing and wiping the interior surfaces with one or more cleaning agents. In some cases, these methods can require replacement of parts and can take two or more days to perform maintenance on the chamber. Such methods can be time-consuming, costly, and inefficient.

[0041] Dry cleaning of EUV resist in processing chamber The present disclosure proposes dry cleaning EUV resist material from the interior surfaces of a processing chamber. The dry cleaning can be performed using a halide-containing chemistry. In some embodiments, the halide-containing chemistry may include a hydrogen halide, such as HCl, HBr, or HI. For example, the hydrogen halide may be HCl. In some embodiments, the halide-containing chemistry may include hydrogen gas and a halogen gas. The dry cleaning may be a non-plasma thermal based cleaning operation. For example, the temperature of the chamber walls may be between about 20° C. and about 140° C. The dry cleaning may be followed by a dehalogenation step to remove excess halide from the processing chamber and / or a conditioning step to protect the interior surfaces of the processing chamber. Although dry cleaning is particularly useful in processing chambers used for EUV dry deposition, dry cleaning may be performed in any processing chamber used for bevel edge and / or backside cleaning, baking, developing, or etching operations. Current in situ dry cleaning can reduce the frequency of cleaning operations, improve particle performance, and increase tool availability.

[0042] FIG. 1 illustrates a flow diagram of an example method of performing a chamber dry clean when depositing and developing photoresist, according to some embodiments. The operations of process 100 may be performed in a different order and / or with different, fewer, or additional operations. Aspects of process 100 may be described with reference to FIG. 2 and FIGS. 3A-3D. One or more operations of process 100 may be performed using an apparatus as described in any one of FIGS. 13-16. In some embodiments, the operations of process 100 may be performed, at least in part, in accordance with software stored on one or more non-transitory computer-readable media.

[0043] In block 102 of process 100, a layer of photoresist is deposited, which can be either a dry deposition process, such as an evaporation process, or a wet process, such as a spin-on deposition process.

[0044] The photoresist may be a metal-containing EUV resist. The EUV-sensitive metal or metal oxide-containing film may be deposited on the semiconductor substrate by any suitable technique, including wet (e.g., spin-on) or dry (e.g., CVD) deposition techniques. For example, the described process has been demonstrated for organotin oxide-based EUV photoresist compositions, and is applicable to both commercially spin-coatable formulations (e.g., those available from Inpria, Inc., Corvallis, Oregon) and formulations applied using dry vacuum deposition techniques, as further described below.

[0045] The semiconductor substrate may include any material structure suitable for photolithographic processing, particularly for fabricating integrated circuits and other semiconductor devices. In some embodiments, the semiconductor substrate is a silicon wafer. The semiconductor substrate may be a silicon wafer having features formed thereon ("base features") and having an irregular surface topology. As described herein, a "surface" is a surface onto which a film of the present disclosure is deposited or which is exposed to EUV during processing. The base features may include areas from which material has been removed (e.g., by etching) or to which material has been added (e.g., by deposition) during processing prior to performing the method of the present disclosure. Such prior processing may include the method of the present disclosure or other processing methods in an iterative process in which two or more layers of features are formed on the substrate.

[0046] EUV-sensitive thin films may be deposited on semiconductor substrates, and such films may act as resists for subsequent EUV lithography and processing. Such EUV-sensitive thin films include materials that undergo changes upon exposure to EUV, such as loss of bulky pendant substituents bonded to metal atoms in low-density, M-OH-rich materials, allowing crosslinking to dense, MOM-bonded metal oxide materials. EUV patterning results in regions of the film that have altered physical or chemical properties compared to unexposed regions. These properties may be exploited in subsequent processing, such as to dissolve either unexposed or exposed regions, or to selectively deposit material in either exposed or unexposed regions. In some embodiments, the unexposed film has a more hydrophobic surface than the exposed film under conditions under which such subsequent processing is performed. For example, removal of material may be performed by exploiting differences in chemical composition, density, and crosslinking of the film. Removal may be by wet or dry processing, as further described below.

[0047] The thin film, in various embodiments, is an organometallic material, such as an organotin material including tin oxide, or other metal oxide material / moiety. The organometallic compound may be produced in a gas phase reaction of an organometallic precursor with a counter reactant. In various embodiments, the organometallic compound is formed by mixing a specific combination of an organometallic precursor having a bulky alkyl or fluoroalkyl group with a counter reactant and polymerizing the mixture in the gas phase to create a low density EUV sensitive material that is deposited on the semiconductor substrate.

[0048] In various embodiments, the organometallic precursors contain at least one alkyl group for each metal atom that is capable of undergoing gas phase reaction, while other ligands or ions coordinated to the metal atom can be displaced by counter reactants. M a R b L c (Formula 1) where M is a metal with a large EUV absorption cross section and R is C nH 2n+1 and the like, preferably n>2; L is a ligand, ion or other moiety that reacts with the counter reactant; a>1, b>1, and c>1.

[0049] In various embodiments, M is 1x10 7 cm 2 / mol or more. M may be, for example, selected from the group consisting of tin, hafnium, tellurium, bismuth, indium, antimony, germanium, and combinations thereof. In some embodiments, M is tin. R may be fluorinated, for example, as represented by the formula C n F x H (2n+1) In various embodiments, R has at least one beta hydrogen or beta fluorine. For example, R may be selected from the group consisting of ethyl, i-propyl, n-propyl, t-butyl, i-butyl, n-butyl, sec-butyl, n-pentyl, i-pentyl, t-pentyl, sec-pentyl, and mixtures thereof. L can be readily displaced by a reverse reactant to generate the M-OH moiety, such as a moiety selected from the group consisting of amines (dialkylamino, monoalkylamino, etc.), alkoxy, carboxylate, halogen, and mixtures thereof.

[0050] The organometallic precursor may be any of a wide variety of potential metal organic precursors. For example, when M is tin, such precursors include t-butyltris(dimethylamino)tin, i-butyltris(dimethylamino)tin, n-butyltris(dimethylamino)tin, sec-butyltris(dimethylamino)tin, i-propyl(tris)dimethylaminotin, n-propyltris(dimethylamino)tin, ethyltris(dimethylamino)tin, and the related alkyl(tris)(t-butoxy)tin compound t-butyltris(t-butoxy)tin. In some embodiments, the organometallic precursor is partially fluorinated.

[0051] The counter reactant has the ability to replace a reactive moiety, ligand or ion (e.g., L in Formula 1 above) to link at least two metal atoms via a chemical bond. The counter reactant can include water, peroxides (e.g., hydrogen peroxide), di- or polyhydroxy alcohols, fluorinated di- or polyhydroxy alcohols, fluorinated glycols, and other sources of hydroxyl moieties. In various embodiments, the counter reactant reacts with the organometallic precursor by forming an oxygen bridge between adjacent metal atoms.

[0052] Other possible counter reactants are hydrogen sulfide and hydrogen disulfide, which can bridge metal atoms via sulfur bridges. In some cases, Te-containing precursors can be used as counter reactants with or instead of water, for example to form Te-Sn-Te-Sn bridge bonds. Tellurium coreactants suitable for use with Sn(NMe2)x type precursors are RTeH or RTeD (D=deuterium) and R2Te precursors, where R=alkyl group, especially t-butyl or isopropyl, such as t-butylTeD. For use with M(OR)x type precursors, for example, Bis(trimethylsilyl)Te can be used.

[0053] The thin film may include optional materials in addition to the organometallic precursors and counter reactants to modify the chemical or physical properties of the film, such as to modify the film's sensitivity to EUV or to increase its etch resistance. Such optional materials may be introduced, such as by doping, during vapor formation prior to deposition on the semiconductor substrate, or after the thin film is deposited, or both. In some embodiments, a gentle remote H2 plasma may be introduced to replace some Sn-L bonds with Sn-H, which can increase the reactivity of the resist under EUV.

[0054] In various embodiments, the EUV patternable film is prepared and deposited on the semiconductor substrate using deposition equipment and deposition processes known in the prior art. In such processes, polymerized organometallic materials are formed in the gas phase or in situ on the surface of the semiconductor substrate. Suitable processes include, for example, chemical vapor deposition (CVD), atomic layer deposition (ALD), and discontinuous ALD-like processes in which the metal precursor and counter reactant are separated in either time or space, with ALD including components of CVD.

[0055] Generally, the method includes mixing a vapor flow of an organometallic precursor with a vapor flow of a counter reactant to form a polymerized organometallic material, and depositing the organometallic material on a surface of a semiconductor substrate. In some embodiments, the vapor flow includes two or more organometallic precursors. In some embodiments, the vapor flow includes two or more counter reactants. As will be appreciated by one of ordinary skill in the art, the mixing and deposition aspects of the process may be simultaneous in a substantially continuous process.

[0056] In an exemplary sequential CVD process, two or more gas streams with separate inlet paths for the organometallic precursor and the reverse reactant sources are introduced into a deposition chamber of a CVD apparatus, where the gas streams are mixed in the gas phase and react to form an aggregated polymeric material (e.g., via the formation of metal-oxygen-metal bonds). The streams may be introduced, for example, using separate inlets or a dual plenum showerhead. The apparatus is configured such that the organometallic precursor and reverse reactant streams are mixed in the chamber, allowing the organometallic precursor and reverse reactant to react to form a polymerized organometallic material. Without limiting the mechanism, function, or utility of the present technology, it is believed that the products resulting from such gas phase reactions have a high molecular weight because the metal atoms are bridged by the reverse reactant and then condensed or otherwise deposited on the semiconductor substrate. In various embodiments, bulky alkyl groups provide steric hindrance to prevent the formation of a tightly packed network, producing smooth, amorphous, low density films.

[0057] CVD processes are typically carried out at low pressures, such as between 10 millitorr and 10 torr. In some embodiments, the processes are carried out between 0.5 and 2 torr. In some embodiments, the temperature of the semiconductor substrate is at or below the reactant flow temperature. For example, the substrate temperature may be between 0° C. and 250° C., or between ambient temperature (e.g., 23° C.) and 150° C. In various processes, deposition of polymerized organometallic material on the substrate occurs at a rate inversely proportional to the surface temperature.

[0058] The thickness of the EUV patternable film formed on the surface of the semiconductor substrate may vary depending on the surface features, the materials used, and the processing conditions. In various embodiments, the thickness of the film may range from 0.5 nm to 100 nm, and may be thick enough to absorb most of the EUV light under the conditions of EUV patterning. The EUV patternable film may be capable of 30% or more absorption, which results in significantly fewer EUV photons available toward the bottom of the EUV patternable film. Higher absorption of EUV results in more cross-linking and densification near the top of the EUV exposed film than the bottom of the EUV exposed film. It will be appreciated that while effective utilization of EUV photons can occur with EUV patternable films with higher overall absorption, in some cases, the EUV patternable film is less than about 30%. By comparison, most other resist films have a maximum overall absorption less than 30% (e.g., 10% or less, or 5% or less), so that the resist material at the bottom of the resist film is fully exposed. In some embodiments, the thickness of the film is 5 nm to 40 nm or 10 nm to 20 nm. Without limiting the mechanism, function, or utility of the present disclosure, it is believed that the process of the present disclosure, unlike prior art wet spin-coating processes, is applicable to a wide variety of substrates because it has fewer limitations regarding the surface adhesion properties of the substrate. Furthermore, as discussed above, the deposited film may closely conform to surface features, providing the advantage of forming a mask on a substrate, such as a substrate having basic features, without "filling" or planarizing such features.

[0059] In addition to depositing a metal-containing EUV resist thin film on a semiconductor substrate in block 102 of process 100, the metal-containing EUV resist material may be formed on the interior surfaces of the processing chamber. The interior surfaces may include the chamber walls, bottom, and ceiling of the processing chamber. Other interior surfaces may include the showerhead, nozzle, and surfaces of the substrate support. The metal-containing EUV resist material may be formed as a result of a dry deposition process, such as a CVD or ALD process. The thickness of the metal-containing EUV resist material formed on the interior surfaces may increase over time as a result of additional processing (e.g., deposition) operations being performed in the processing chamber. The metal-containing EUV resist material has a tendency to flake off, shed particles, or peel off from the interior surfaces of the processing chamber during processing, thereby contaminating subsequent semiconductor substrates.

[0060] In block 150 of process 100, a chamber dry clean operation of the present disclosure may be performed after depositing a metal-containing EUV resist film on a semiconductor substrate in block 102 of process 100. This allows the deposition and dry clean to be performed in the same processing chamber, although it will be understood that the chamber dry clean may be performed in a different processing chamber than the deposition operation in embodiments. Indeed, the chamber dry clean may be performed following bevel and / or backside clean, bake, develop, or etch operations.

[0061] The dry-deposited EUV photoresist films that are removed are typically composed of Sn, O, and C, but the same cleaning techniques can be extended to films of other metal oxide resists and materials. The technique can also be used for film stripping and PR rework.

[0062] In block 104 of process 100, an optional cleaning process is performed to clean the backside and / or bevel edge of the semiconductor substrate. In cleaning the backside and / or bevel edge, the EUV resist film may be non-selectively etched to evenly remove films with various levels of oxidation or crosslinking on the substrate backside and bevel edge. During the application of EUV patternable films, either by wet or dry deposition processes, some unintentional deposition of resist material may occur on the bevel edge and / or backside of the substrate. Unintentional deposition may result in unwanted particles that may subsequently migrate to the upper surface of the semiconductor substrate and become particle defects. Furthermore, this bevel edge and backside deposition may cause downstream processing issues, such as contamination of patterning (scanner) and development tools. Traditionally, this bevel edge and backside deposition is removed by wet cleaning techniques. For spin-coated photoresist materials, this process is called edge bead removal (EBR) and is performed by directing a flow of solvent from above and below the bevel edge while the substrate is rotating. The same process can be applied to resists based on soluble organotin oxides deposited by evaporation techniques.

[0063] Cleaning the bevel edge and / or backside of the substrate may be a dry cleaning process. In some embodiments, the dry cleaning process involves a vapor and / or plasma containing one or more of the following gases: HBr, HCl, BCl3, SOCl2, Cl2, BBr3, H2, O2, PCl3, CH4, methanol, ammonia, formic acid, NF3, HF. In some embodiments, the dry cleaning process may use the same chemistry as the dry developing process described herein. For example, cleaning the bevel edge and backside may use a hydrogen halide developing chemistry. In the backside and bevel edge cleaning process, the vapor and / or plasma must be limited to certain areas of the substrate to ensure that only the backside and bevel are removed without degrading the film on the frontside of the substrate.

[0064] The process conditions may be optimized to clean the bevel edge and backside. In some embodiments, higher temperatures, higher pressures, and / or faster reactant flows may lead to increased etch rates. Suitable process conditions for dry cleaning of the bevel edge and backside are: reactant flows of 100-500 sccm (e.g., 500 sccm HCl, HBr or H2, and Cl2 or Br2, BCl3 or H2), temperatures of -10-120°C (e.g., 20°C), pressures of 20-500 mTorr (e.g., 300 mTorr), plasma powers of 0-500 W at radio frequency (e.g., 13.56 MHz), and times of about 10-20 seconds, depending on the photoresist film and composition and properties. These conditions are suitable for some processing reactors, such as the Kiyo etch tool available from Lam Research Corporation, Fremont, Calif., but it should be understood that a wider range of processing conditions may be used depending on the capabilities of the processing reactor.

[0065] Alternatively, the dry cleaning operation may be extended to full photoresist removal or photoresist "rework" to remove applied EUV photoresist and prepare the semiconductor substrate for reapplication of photoresist, such as when the original photoresist is damaged or defective. Photoresist rework must be accomplished without damaging the underlying semiconductor substrate, and therefore oxygen-based etches should be avoided. Alternately, variations of the halide-containing chemistries described herein may be used. It will be appreciated that the photoresist rework operation may be applied at any stage of the process 100. Thus, the photoresist rework operation may be applied after photoresist deposition, after bevel edge and backside cleaning, after PAB processing, after EUV exposure, after PEB processing, or after development. In some embodiments, the photoresist rework may be performed to selectively remove the underlying layer without selectively exposing and unexposing areas of the photoresist.

[0066] In some embodiments, the photoresist rework process involves vapors and / or plasmas containing one or more of the following gases: HBr, HCl, BCl3, Cl2, BBr3, H2, PCl3, CH4, methanol, ammonia, formic acid, NF3, HF. In some embodiments, the photoresist rework process may use the same chemistry as the dry development process described herein. For example, the photoresist rework may use a hydrogen halide development chemistry.

[0067] Process conditions may be optimized for photoresist rework. In some embodiments, higher temperatures, higher pressures, and / or faster reactant flows may lead to increased etch rates. Suitable process conditions for photoresist rework include: reactant flows of 100-500 sccm (e.g., 500 sccm HCl, HBr, BCl3 or H2 and Cl2 or Br2), temperatures of -10-120°C (e.g., 20°C), pressures of 20-500 mTorr (e.g., 300 mTorr), plasma power of 300-800 W (e.g., 500 W) at high frequency (e.g., 13.56 MHz), and wafer bias of 0-200 V. b (higher bias may be used if the underlying substrate material is harder) and the time is about 20 seconds to 3 minutes, sufficient to completely remove the EUV photoresist, but will vary depending on the photoresist film and composition and properties. These conditions are suitable for some process reactors, e.g., the Kiyo etch tool available from Lam Research Corporation, Fremont, Calif., but it will be understood that a wider range of process conditions may be used depending on the capabilities of the process reactor.

[0068] In block 150 of process 100, a chamber dry clean operation of the present disclosure may be performed after a bevel edge and / or backside cleaning operation, which allows the bevel and / or backside cleaning and the chamber dry clean to be performed in the same processing chamber, although it will be understood that the chamber dry clean may be performed in a different processing chamber than the bevel edge and / or backside cleaning operation in some embodiments.

[0069] In block 106 of process 100, an optional post-application bake (PAB) is performed after deposition of the EUV patternable film and before exposure to EUV. The PAB process may require a combination of thermal treatment, chemical exposure, and moisture to increase the EUV sensitivity of the EUV patternable film and reduce the EUV dose to develop a pattern in the EUV patternable film. The process temperature of the PAB may be adjusted to optimize the sensitivity of the EUV patternable film. For example, the process temperature may be about 90° C. to about 250° C. or about 100° C. to about 200° C. In some embodiments, the PAB process may be performed at a pressure between atmospheric pressure and vacuum for a process time of about 1 to 15 minutes, for example about 2 minutes. In some embodiments, the PAB process is performed at a temperature of about 100° C. to about 200° C. for about 1 to 2 minutes.

[0070] In block 150 of process 100, a chamber dry clean operation of the present disclosure may be performed after the PAB treatment, allowing the bake and chamber dry clean to be performed in the same processing chamber, although it will be understood that the chamber dry clean may be performed in a different processing chamber than the PAB treatment operation in some embodiments.

[0071] In block 108 of the process 100, the metal-containing EUV resist film is exposed to EUV radiation to develop the pattern. Generally, the EUV exposure causes changes in the chemical composition and cross-linking of the metal-containing EUV resist film, creating a contrast in etch selectivity that can be utilized for subsequent development.

[0072] The metal-containing EUV resist film may then be patterned by exposing a region of the film to EUV light, typically under a relatively high vacuum. Among those useful herein, EUV devices and imaging methods include those known in the prior art. In particular, as previously described, the exposed regions of the film are created by EUV patterning and have altered physical or chemical properties compared to the unexposed regions. For example, the exposed regions may undergo metal-carbon bond cleavage, such as by beta hydride elimination, leaving reactive and accessible metal hydride functionality that may be converted to hydroxide and cross-linked metal oxide moieties via metal-oxygen cross-linking in a subsequent post-exposure bake (PEB) step. This process can be used to create chemical contrast for development as a negative tone resist. In general, the higher the number of beta Hs in the alkyl group, the higher the sensitivity of the film. Following exposure, the metal-containing EUV resist film may be baked to induce additional cross-linking in the metal oxide film. The difference in properties between exposed and unexposed areas may be exploited in subsequent processing to dissolve the unexposed areas or deposit material in the exposed areas, for example the pattern can be developed using a dry method to form a metal oxide-containing mask.

[0073] In particular, in various embodiments, hydrocarbyl-terminated tin oxide present at the surface is converted to hydrogen-terminated tin oxide in the exposed regions of the imaging layer, particularly when the exposure is performed in a vacuum with EUV. However, upon removal of the exposed imaging layer from vacuum to air or the controlled introduction of oxygen, ozone, H2O2, or water, the surface Sn-H can oxidize to Sn-OH. The difference in properties between the exposed and unexposed regions may be exploited in subsequent processing, such as by reacting the irradiated regions, the unirradiated regions, or both, with one or more reagents to selectively add or remove materials from the imaging layer.

[0074] Without limiting the mechanism, function, or utility of the present technology, the EUV exposure may be, for example, 10 mJ / cm 2 ~100mJ / cm 2At doses of 100 nm to 100 nm, cleavage of Sn-C bonds occurs, resulting in loss of alkyl substituents, and the reduction of steric hindrance allows the collapse of low-density films. Also, reactive metal-H bonds resulting from the beta-hydride elimination reaction can react with adjacent active groups, such as hydroxyl groups, in the film, resulting in further cross-linking and densification, and creating chemical contrast between exposed and unexposed regions.

[0075] After exposing the metal-containing EUV resist film to EUV light, a photo-patterned metal-containing EUV resist is prepared. The photo-patterned metal-containing EUV resist includes EUV exposed areas and non-exposed areas.

[0076] In block 110 of process 100, an optional post-exposure bake (PEB) is performed to further enhance the contrast of the etch selectivity of the photo-patterned metal-containing EUV resist. The photo-patterned metal-containing EUV resist can be heat treated in the presence of various chemical species to promote cross-linking of the EUV-exposed regions of the photo-patterned metal-containing EUV resist, or can simply be baked on a hotplate in ambient air, for example, at 150° C.-250° C. for 1-5 minutes (e.g., 190° C. for 2 minutes).

[0077] In various embodiments, the bake strategy involves carefully controlling the bake environment, introducing reactive gases, and / or carefully controlling the ramp rate of the bake temperature. Examples of useful reactive gases include, for example, air, H2O, H2O2 vapor, CO2, CO, O2, O3, CH4, CH3OH, N2, H2, NH3, N2O, NO, alcohol, acetylacetone, formic acid, Ar, He, or mixtures thereof. The PEB process is designed to (1) completely vaporize organic fragments generated during EUV exposure, (2) oxidize any Sn-H, Sn-Sn, or Sn radical species generated by EUV exposure to metal hydroxides, and (3) promote cross-linking between adjacent Sn-OH groups to form a more tightly cross-linked SnO2-like network. The bake temperature is carefully selected to achieve optimal EUV lithography performance. Too low a PEB temperature will result in insufficient cross-linking, which will result in poor chemical contrast development at a given dose. Too high a PEB temperature can have deleterious effects such as severe oxidation and shrinkage of the unexposed areas (in this example, the areas that are removed by developing the patterned film to form the mask), as well as undesirable interdiffusion at the interface between the photopatterned metal-containing EUV resist and the underlayer, both of which can lead to loss of chemical contrast and increased defect density due to insoluble scum. The PEB treatment temperature can be from about 100°C to about 300°C, from about 170°C to about 290°C, or from about 220°C to about 250°C. In some embodiments, the PEB treatment can be performed at a pressure between atmospheric pressure and vacuum, and for a treatment time of about 1 to 15 minutes, e.g., about 2 minutes. In some embodiments, the PEB heat treatment can be repeated to further increase the etch selectivity.

[0078] In block 150 of process 100, a chamber dry clean operation of the present disclosure may be performed after the PEB process, which allows the bake and chamber dry clean to be performed in the same processing chamber, although it will be understood that the chamber dry clean may be performed in a different processing chamber than the PEB processing operation in some embodiments.

[0079] In block 112 of process 100, the photo-patterned metal-containing resist is developed to form a resist mask. In various embodiments, the exposed regions are removed (positive tone) or the unexposed regions are removed (negative tone). In some embodiments, the development may include selectively depositing a metal on either the exposed or unexposed regions of the photo-patterned metal-containing resist, followed by an etching operation. In various embodiments, these processes may be dry or wet processes. An example of a development process involves subjecting an EUV-sensitive photoresist film (e.g., 10-30 nm thick, such as 20 nm thick) containing an organotin oxide to a dose of EUV exposure and a post-exposure bake, followed by development. The photoresist film may be deposited based on a gas-phase reaction of an organotin precursor, such as isopropyl(tris)(dimethylamino)tin, with water vapor, or may be a spin-on film containing tin clusters in an organic matrix. The photo-patterned metal-containing resist is developed by exposure to a development chemical. In some embodiments, the development chemical comprises a halide-containing chemical.

[0080] In block 150 of process 100, a chamber dry clean operation of the present disclosure may be performed after development. This allows development and chamber dry clean to be performed in the same processing chamber. However, it will be understood that in some embodiments, the chamber dry clean may be performed in a different processing chamber than the development operation. Furthermore, it will be understood that in some embodiments, the chamber dry clean may be performed in the same processing chamber as the etch operation or in a different processing chamber. The etch operation may be applied to etch an underlying substrate layer of a semiconductor substrate.

[0081] FIG. 2 illustrates a flow diagram of an exemplary method of performing a chamber dry clean according to some embodiments. The chamber dry clean may be performed after a deposition, bevel and / or backside clean, bake, develop, or etch operation. In some embodiments, the chamber dry clean may be performed after deposition of a photoresist material in the same processing chamber as the deposition of the photoresist material. Aspects of process 200 may be described with reference to FIGS. 3A-3D. One or more operations of process 200 may be performed using an apparatus described in any one of FIGS. 13-16. In some embodiments, operations of process 200 may be performed, at least in part, in accordance with software stored on one or more non-transitory computer readable media.

[0082] In block 202 of process 200, a semiconductor substrate is provided in a processing chamber having a metal-containing resist film dry deposited on a substrate layer of the semiconductor substrate. The composition and deposition of such dry deposited metal-containing resist films may be described, for example, in PCT / US19 / 31618, filed May 9, 2019, which is incorporated by reference herein to disclose such methods and materials as may be applicable to the present disclosure. Methods include a method of vapor-phase preparation and deposition of polymerized metal-organic materials on a semiconductor substrate. In particular, a method of making an EUV-patternable thin film on a surface of a semiconductor substrate includes mixing a vapor flow of a metal-organic precursor with a vapor flow of a counter reactant to form a polymerized metal-organic material, and depositing the metal-organic polymer-like material on a surface of the semiconductor substrate. In some embodiments, the vapor flow includes two or more metal-organic precursors. In some embodiments, the vapor flow includes two or more counter reactants. In some embodiments, the mixing and deposition operations are performed in a continuous CVD process, an ALD process, or an ALD with CVD component, such as a discontinuous ALD-like process in which the metal precursor and the counter reactant are separated in either time or space. In some embodiments, the dry-deposited metal-containing resist film is a metal oxide-containing EUV resist film. For example, the elements in the metal-containing resist film are selected from the group consisting of tin, hafnium, tellurium, bismuth, indium, antimony, iodine, germanium, and combinations thereof. In some embodiments, the metal-containing resist film comprises an organometallic oxide, such as an organotin oxide.

[0083] In some embodiments, the processing chamber in which the semiconductor substrate is prepared may be a dry deposition chamber. In other embodiments, the processing chamber in which the semiconductor substrate is prepared may be a bevel edge and / or backside cleaning chamber, a PAB processing chamber, a PEB processing chamber, a development chamber, or an etch chamber. In any of the aforementioned processing chambers, metal-containing resist material may accumulate on the interior surfaces over time. As more and more semiconductor substrates are processed in the processing chamber, unintentional metal-containing resist material may grow on the interior surfaces. Periodic cleaning is required to remove unintentional deposits of metal-containing resist material. Cleaning is performed "in situ," where the chamber dry cleaning is performed in the same processing chamber in which the unintentional metal-containing resist material was formed.

[0084] FIG. 3A shows a schematic cross-sectional view of a metal-containing EUV resist material 302 formed on a chamber wall 304 of a processing chamber. The metal-containing EUV resist material 302 may include metal oxide 306 particles or clusters. The metal oxide 306 particles or clusters are generally difficult to remove. In some embodiments, the metal-containing EUV resist material 302 is formed by a deposition method such as CVD or ALD. Over time, the metal-containing EUV resist material may build up and thicken on the chamber wall 304 of the processing chamber. The metal-containing EUV resist material 302 may be an organotin oxide. The metal oxide 306 particles or clusters may include tin oxide.

[0085] Referring to FIG. 2, in block 204 of process 200, an etching gas is introduced into the process chamber, a first thickness of dry-deposited metal-containing resist material is formed on one or more surfaces of the process chamber, and the etching gas removes the first thickness of dry-deposited metal-containing resist material. In some embodiments, the etching gas includes a halide-containing chemical. In some embodiments, the etching gas includes a hydrogen halide, a hydrogen and halogen gas, boron trichloride, or a combination thereof. For example, the etching gas can be HCl. In some embodiments, the etching gas can remove the dry-deposited metal-containing resist material without striking a plasma. In some embodiments, the etching gas can remove the dry-deposited metal-containing resist material by heating the process chamber to an elevated temperature. The first thickness of the dry-deposited metal-containing resist material can be about 2 nm or more, about 3 nm or more, about 5 nm or more, or about 10 nm or more. The first thickness can correspond to an average thickness of the film material formed on one or more surfaces of the process chamber.

[0086] Prior to the introduction of the etching gas, the process chamber may be prepared in the desired conditions to dry clean the chamber, which may achieve specific pressure conditions, levels of coarse particles or film impurities, moisture levels, temperature conditions, or protection of the process chamber surfaces or components (e.g., the substrate support) from the etching gas.

[0087] In some embodiments, preparing the process chamber may include purging and / or pumping the process chamber to remove unwanted particles in the process chamber. A vacuum or purge line may be coupled to the process chamber. The vacuum line may include a vacuum pumping system, which may include a one-stage or two-stage mechanical dry pump and / or a turbomolecular pump. A purge gas may be flowed into the process chamber to facilitate removal of unwanted particles in the process chamber. Such unwanted particles may include particles or fragments from metal-containing resist materials. The vacuum pumping system may reduce the pressure of the chamber and / or remove the unwanted particles from the process chamber. The vacuum pumping system may be configured to generate a vacuum pressure within a relatively low range (e.g., from about 799.934 Pascals (about 6 Torr) to atmospheric pressure) or within a relatively high range (e.g., from about 133.322 millipascals to about 799.934 Pascals (about 1 mTorr to about 6 Torr)). In some embodiments, preparing the process chamber may include a combination of pumping and purging operations.

[0088] Purging of the metal organic precursors can be useful to avoid undesired by-products and ensure sufficient removal of the metallic and organic CVD precursors before dry cleaning. To promote complete reaction, sufficient pumping / purging and / or water injection may be performed before dry cleaning. In some embodiments, the chamber walls and other components may be heated to release unreacted precursors.

[0089] In some embodiments, preparing the processing chamber may include increasing the temperature of one or more surfaces of the processing chamber. The one or more surfaces of the processing chamber may include at least a chamber wall of the processing chamber. The increased temperature may facilitate removal of moisture from the processing chamber. Without being limited to any theory, the presence of water vapor retards the reaction of the etching gas with the metal-containing resist material to remove the metal-containing resist material. Additionally, increasing the temperature of the processing chamber may increase the etching rate to remove the metal-containing resist material. One or more heaters may be thermally coupled to the one or more surfaces of the processing chamber to heat the one or more surfaces to an elevated temperature. In some embodiments, the elevated temperature may be from about 20° C. to about 140° C., from about 40° C. to about 120° C., or from about 80° C. to about 120° C.

[0090] In some embodiments, preparing the processing chamber may include preparing a dummy substrate on a substrate support in the processing chamber. Thus, the semiconductor substrate with the dry-deposited metal-containing resist film may be removed from the processing chamber prior to the dry cleaning. In this manner, the semiconductor substrate prepared earlier in the processing chamber is not exposed to the etching gas when removing the first thickness of the dry-deposited metal-containing resist material. The dummy substrate may be prepared on the substrate support to protect the substrate support (e.g., an electrostatic chuck) from exposure to the etching gas during the dry cleaning. Alternatively, the substrate support may be protected by placing a protective cover on the substrate support during the dry cleaning.

[0091] The etching gas may be introduced through a showerhead or a separate chamber inlet connected to the process chamber. The etching gas may flow into the process chamber and react with the dry-deposited metal-containing resist material to form volatile products. Without being limited to any theory, organometallic oxide resist materials may have a tetrahedral coordinated structure, and etching gases containing halide-based chemicals (e.g., HBr or HCl) may protonate oxygen lone pairs to form volatile by-products such as R-Sn-Br. Water is also a by-product. The rate of the reaction may be increased by removing the water and increasing the temperature of the process chamber. After the volatile products are formed, the process chamber may be pumped and purged to remove the volatile products. The process chamber may also be pumped and purged to remove residual etching gas. Such residual etching gas may cause undesired etching of the semiconductor substrate in the future.

[0092] The dry cleaning may be optimized to reduce the etch selectivity or increase the etch rate of the resist material deposited in the process chamber. In this way, the unwanted resist material may be removed quickly and efficiently. A low etch selectivity may be achieved to selectively remove photoresist materials and metal oxide materials (e.g., tin oxide). A low etch selectivity may be achieved to selectively remove exposed and unexposed EUV resist materials. In some embodiments, a higher temperature and / or a higher pressure may result in a lower etch selectivity of the etching gas. During exposure to the etching gas, the metal-containing resist material on one or more surfaces may be subjected to an elevated temperature. The elevated temperature may be about 20° C. to about 140° C., about 40° C. to about 120° C., or about 80° C. to about 120° C. During exposure to the etching gas, the pressure of the process chamber may be high. In some embodiments, the chamber pressure is about 0.01 Torr to atmospheric pressure, about 0.1 Torr to 100 Torr, or about 0.1 Torr to 6 Torr. In some embodiments, the chamber pressure is cycled between high and low pressure during exposure to the etching gas. The flow rate of the etching gas may be adjusted to control the etching selectivity. In some embodiments, the flow rate of the etching gas is about 50 sccm to about 10,000 sccm, about 100 sccm to about 10,000 sccm, or about 100 sccm to about 2,000 sccm.

[0093] The etching gas serves to remove resist material from the interior surfaces of the chamber, and the etch rate may be adjusted by adjusting the temperature of one or more surfaces of the process chamber. Resist material can be removed at an etch rate of up to 1 nm / sec. Higher temperatures and / or pressures may increase the etch rate. Resist material can be removed using steam at various temperatures (e.g., HCl or HBr at temperatures above 10° C., or BCl3 at temperatures above 80° C.), but plasma can be used to further accelerate or promote the reaction. Thus, in some embodiments, the etching gas can be activated by heating or by a remote plasma source. This may further accelerate the etch or make it more reactive.

[0094] In a non-plasma thermal process for dry cleaning, the etching gas may be a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a mixture thereof. In some embodiments, the hydrogen halide includes HCl, HBr, or HI. For example, the hydrogen halide may be HCl. In some embodiments, the halogen gas is Cl2, Br2, or I2. In some embodiments, the etching gas flows with or without an inert / carrier gas, such as He, Ne, Ar, Xe, or N2. The first thickness of the metal-containing resist material is removed by the etching gas without impingement of the plasma, while residual carbon, contaminants, or other residual materials may be removed by exposure to the plasma. In some embodiments, after introducing the etching gas, the one or more surfaces may be exposed to an oxidizing gas, such as oxygen (O2), ozone (O3), carbon dioxide (CO2), or carbon monoxide (CO). The one or more surfaces may be exposed to radicals and / or ions of the oxidizing gas in the plasma.

[0095] In some embodiments, the dry cleaning may be a plasma-based dry cleaning. Thus, the dry cleaning may be performed directly with in situ plasma or remote plasma. The processing chamber may be a plasma generation chamber or may be coupled to a plasma generation chamber that is separate from the processing chamber. The plasma generation chamber may be an inductively coupled plasma (ICP) reactor, a transformer coupled plasma (TCP) reactor, or a capacitively coupled plasma (CPC) reactor, using equipment and techniques among those known in the prior art. In a plasma-based dry cleaning, the metal-containing resist material in the processing chamber is exposed to radicals of a particular gas. The gas may be selected from the group consisting of HBr, HCl, BCl3, SOCl2, Cl2, BBr3, H2, PCl3, CH4, methanol, ammonia, formic acid, NF3, HF, and HI. In a plasma-based dry cleaning, chemicals other than halogens may be used. In a non-plasma thermal dry cleaning, chemicals based on halogens may be used.

[0096] The ability to thermally clean as-deposited films (not exposed or cross-linked), without the need to use plasma, allows the techniques described herein to also clean downstream and upstream components of the tool beyond the process chamber (e.g., exhaust lines from the process chamber to the vacuum pump).More generally, this dry cleaning method can be used to clean other contaminated parts and components with similar composition to metals, including -Cl, -Br, -F, -H, -CH4, and volatile products with oxides and / or R groups.

[0097] It is important to note that in some embodiments, unexposed, uncrosslinked resist films can be cleaned and removed according to the techniques described herein without plasma: exposed films have a much slower etch rate and can utilize either higher temperatures, pressures, or plasmas for removal and cleaning.

[0098] In some embodiments, coatings compatible with halogen cleaning chemistries may be used on chamber walls and other components exposed to the cleaning agents, such as PTFE, anodized aluminum, yttrium oxide (YO), or organic polymer coatings. In some embodiments, the processing chamber may include a chamber component temperature control device coupled to one or more surfaces (e.g., chamber walls) to control the temperature. In some embodiments, the processing chamber may have a gas inlet other than a showerhead to deliver the etching gas. The gas inlet may be located in an area of ​​the processing chamber that has a higher concentration of metal-containing resist material. Alternatively, the gas inlet may be located in an area of ​​the processing chamber that is unlikely to be reached by delivery via a showerhead. In some embodiments, the gas inlet may be located below the substrate support, in a wall of the processing chamber, and / or near the exhaust of the processing chamber. Multiple gas inlets may be used to deliver the etching gas to the processing chamber. This can ensure dry cleaning of the entire processing chamber.

[0099] To prevent corrosion of chamber components, the etching gases may be separated from the deposition gases / precursors. In various embodiments, the etching gases may be delivered to the processing chamber through one or more gas inlets separate from the showerhead, and the deposition gases may be delivered to the processing chamber through the showerhead. In some embodiments, the showerhead may deliver the separate gases by keeping the gases largely separated in the showerhead. The showerhead may include multiple plenum spaces. To ensure separation of the gases downstream of the processing chamber, multiple exhaust lines may be used. Switches may be operably coupled to the multiple exhaust lines to allow separation of the etching gas chemistry from the deposition gases / precursors. For example, hydrogen halide chemistry may be separated from organotin precursors and water vapor. The halides may be exhausted from a first exhaust line during pumping / purging operations, and the deposition precursors and water vapor may be exhausted from a second exhaust line during pumping / purging operations.

[0100] To protect the showerhead, a pressure differential may be used to prevent the etching gas from entering the showerhead (e.g., backflowing). In some embodiments, the etching gas may clean the interior surface of the showerhead by flowing the etching gas through the showerhead. However, residual halides or moisture may remain inside the showerhead channels. In some embodiments, the showerhead may be made of a transparent material and heated with a suitable light source. For example, a radiation source tuned to a suitable wavelength (e.g., IR or blue wavelength) can directly heat the residual halides and / or moisture to remove the residual halides and / or moisture. Alternatively, the residual halides and / or moisture may be removed by a gas purge.

[0101] In some embodiments, periodic dry cleaning may be performed upon detection. A detection source may trigger chamber cleaning and / or cleaning end point. The detection source may be a sensor located in the process chamber, and may be a color-based sensor, an intensity-based sensor, a vision-based camera / sensor, etc., or a combination thereof. The sensor may trigger chamber dry cleaning by monitoring particle count or uniformity, wafer count, or thickness count. Alternatively, the sensor may trigger chamber dry cleaning by an insitu measurement device for chamber wall deposition. For example, the sensor may detect the presence of photoresist material using infrared (IR) measurements. A chamber dry cleaning may be triggered after a certain amount of photoresist material is formed or after a threshold particle, uniformity, wafer, or thickness count is reached. In some embodiments, a sensor may be located downstream of the foreline. Such a sensor may detect what gases / byproducts are being exhausted. The chamber dry cleaning may be terminated when volatile byproducts are no longer detected in the foreline.

[0102] FIG. 3B is a schematic cross-sectional view of the chamber walls 304 after the etching gas removes the metal-containing EUV resist material 302 from the chamber walls 304. The etching gas may be a hydrogen halide, hydrogen gas and a halogen gas, or boron trichloride. The chamber walls 304 may be heated to an elevated temperature to promote low etch selectivity. The processing chamber may be elevated to a high pressure to promote low etch selectivity. The removal of the metal-containing EUV resist material 302 may be performed without the use of a plasma. Residual particles or clusters of metal oxide 306 may remain on the chamber walls 304 after exposure to the etching gas. Also, residual etching gas 308 may remain in the processing chamber.

[0103] 4 illustrates an exemplary chamber dry clean mechanism involving a chemical reaction of hydrogen chloride or hydrogen bromide with an organotin oxide / hydroxide resist material coated on the interior surfaces of a process chamber, according to some embodiments. Hydrogen halide (HCl or HBr) reacts with an EUV resist, such as an organotin oxide / hydroxide resist material, coating the interior surfaces of the chamber and downstream components. The hydrogen halide cleaves Sn-OH and Sn-O-Sn bonds to produce HO and volatile organotin halide and tin halide products, which can then be pumped away.

[0104] Returning to FIG. 2, in block 206 of process 200, the process chamber is optionally purged to remove residual etching gas from the process chamber. Purging may include flowing a purge gas into the process chamber or flowing a purge gas in combination with pumping the process chamber to a desired chamber pressure. The purge gas may be an inert gas and / or a reactive gas. The reactive gas may react with the residual etching gas to facilitate its removal. The reactive gas may be, for example, a tin-based precursor, such as an organotin precursor. The inert gas may be Ar, He, Xe, or N2. The chamber pressure may be from about 13.3322 Pa to about 799.934 Pa (about 0.1 Torr to about 6 Torr).

[0105] Residual etching gas may be evacuated from the process chamber. In some embodiments, the purging operation may be referred to as dehalogenation. Halides may easily adhere to the chamber walls, chamber components, or wafer. If halides adhere to the wafer, it increases the risk that the halides (e.g., bromine) will be released from the wafer during EUV scanning, thereby corroding or damaging the scanner. Furthermore, if halides adhere to the chamber walls or chamber components, the halides may be more susceptible to forming organic salts with subsequent precursors during dry deposition operations. The purging of residual etching gas may be evacuated through a separate exhaust line from the deposition precursors and counter reactants (e.g., water vapor).

[0106] In some embodiments, the purging operation may proceed at an elevated temperature. The elevated temperature may aid in removing halides from the processing chamber. In one example, one or more heaters coupled to one or more surfaces of the processing chamber may heat the processing chamber to an elevated temperature. In another example, one or more IR sources or LEDs may be installed in the processing chamber to heat the processing chamber to an elevated temperature. The elevated temperature may be from about 20° C. to about 140° C. or from about 80° C. to about 120° C.

[0107] A variety of direct or remote plasma-based processes are useful for accelerating the removal of residual etching gas (e.g., Cl- or Br-containing chemicals) that may coat the interior surfaces of the process chamber after removing the metal-containing resist material. Such processes may be used individually or in combination to restore the interior surfaces of the process chamber. The interior surfaces of the process chamber may be, for example, aluminum oxide-based ceramics, anodized aluminum, and stainless steel hardware components (typically downstream). A restored interior surface may imply no or substantially no residual etching gas (e.g., no Cl and / or Br). In one approach, the remote plasma-based process is a remote NF3 plasma process, since both F radicals and F2 gas are generated and may be effective in converting residual halide-containing chemicals to volatile halogens. The volatile halogens are then pumped out, leaving behind a passivated surface, such as an Al-F passivated surface. The reactive gases used in the remote plasma process may include, but are not limited to, NF3, SF6, CF4, or ClF3. Another approach that may be considered less aggressive but also effective is oxygen-based plasma treatment. For example, oxygen-based plasma treatment may target the oxidation of bromide surface residues to form volatile bromine gas (Br2). Oxygen-based reactants may include, but are not limited to, O2, O3, a mixture of H2 and O2, and N2O. For example, after a fluorine-based clean, a H2 / O2 plasma with a low pressure N2O plasma may be utilized to restore the interior surface. In some embodiments, it may be advantageous to repeat cycles of fluorine-based and oxygen-based plasma treatments or to utilize a mixture of fluorine-based and oxygen-based chemistries. In some embodiments, it may be advantageous to interrupt the sequence with a hydrogen-containing plasma treatment (e.g., H plasma) that may target the formation of volatile hydrogen halide (e.g., HBr, HCl)-based by-products. This may leave a passivated surface.In some embodiments, a plasma-based process or series of plasma-based processes may end with an oxygen-based plasma conditioning step in which the interior surface may be exposed to an oxygen-based plasma to form a passivation layer of metal oxide (e.g., aluminum oxide) for recovery. As described below, the recovered interior surface may then be coated / seasoned with a photoresist film (to avoid undesirable first wafer effects) before resuming deposition operations on the semiconductor substrate.

[0108] In other embodiments, the non-plasma process may be useful for accelerating the removal of residual etching gas (e.g., Cl- or Br-containing chemicals) that may coat the interior surfaces of the process chamber after removing the metal-containing resist material. An oxidizing gas may be introduced to oxidize residual halides, such as Cl or Br, on the interior chamber surfaces. Thus, the non-plasma process may include providing a flow of ozone gas (O3) and / or oxygen gas (O2). For example, the non-plasma process may include providing a flow of ozone gas and oxygen gas (e.g., 0.1% to 30% ozone in oxygen). The non-plasma process may have the additional benefit of oxidizing and removing residual organic materials, such as carbon-containing and hydrogen-containing residues, remaining on the interior surfaces.

[0109] 3C shows a schematic cross-sectional view of the chamber walls 304 after dehalogenation to remove the residual etching gas 308 from the processing chamber. A pumping / purging operation may be performed to evacuate the residual etching gas 308 from the processing chamber. In some embodiments, the chamber walls 304 or other components of the processing chamber may be heated to facilitate the release of the residual etching gas 308. In some embodiments, a direct or remote plasma-based treatment may be applied to remove the residual etching gas 308, which may include a fluorine-based plasma treatment, an oxygen-based plasma treatment, or a combination thereof. Metal oxide 306 particles or clusters may remain on the chamber walls 304.

[0110] Returning to FIG. 2, in block 208 of process 200, one or more surfaces of the processing chamber are optionally conditioned by forming a second thickness of dry-deposited metal-containing resist material on one or more surfaces of the processing chamber. The second thickness is less than the first thickness of dry-deposited metal-containing resist material. In some embodiments, the second thickness is about 1 nm or more, about 2 nm or more, about 3 nm or more, or between about 1 nm and about 5 nm. Alternatively, one or more surfaces of the processing chamber are optionally conditioned by forming a protective film that is different from the dry-deposited metal-containing resist material. Such a protective film may be formed of SnO x C y After exposure to the etching gas, one or more surfaces remain exposed. Surfaces exposed in the processing chamber may be vulnerable to attack, particularly by halogen-based species. The conditioning operation may provide protection to the one or more surfaces. The conditioning operation may also cover residual metal oxide particles or clusters adhering to the one or more surfaces, reducing the likelihood that the metal oxide particles or clusters will contaminate the wafer during subsequent processing.

[0111] The conditioning of one or more surfaces of the process chamber may be performed by a vapor-based deposition technique, such as a CVD or ALD technique. An organometallic material is prepared in the vapor phase and deposited on one or more surfaces of the process chamber. The organometallic material may be deposited based on a vapor-phase reaction of an organotin precursor, such as isopropyl(tris)(dimethylamino)tin, with water vapor. The flow of water vapor may be relatively low. During the conditioning process, the substrate support may be protected or covered with a dummy wafer or other protective cover. A second thickness of metal-containing resist material may be formed on the chamber walls, bottom, and ceiling. A second thickness of metal-containing resist material may also be formed on chamber components such as gas inlets, showerheads, and exhaust lines. After the second thickness of metal-containing resist material is deposited, a pumping / purging operation is subsequently performed to remove excess precursors and / or back reactants. The conditioning of one or more surfaces of the process chamber may trap residual metal oxide particles to limit particle contamination.

[0112] FIG. 3D shows a schematic cross-sectional view of a metal-containing resist material 310 formed on the chamber walls 304 of a processing chamber. The metal-containing EUV resist material 310 may be redeposited during a conditioning operation to protect the chamber walls 304 and capture metal oxide 306 particles or clusters from contaminating wafers during processing. This is sometimes referred to as seasoning the chamber. The metal-containing EUV resist material 310 is formed by a deposition method such as CVD or ALD. In some embodiments, the metal-containing EUV resist material 310 may be an organotin oxide. Conditioning / seasoning the chamber walls 304 and other interior surfaces of the processing chamber reduces undesirable initial effects on the wafer when resuming deposition operations on a semiconductor substrate.

[0113] Although this disclosure frequently refers to cleaning of exposed and / or developed EUV-sensitive films, the cleaning processes described may also be used to clean EUV films that are similar in composition (e.g., other MO x R yThe method can be extended to other films containing metal oxides, such as EUV resist films that have not been exposed to light, as described herein, and other volatile products including -Cl, -Br, -F, -H, -CH4, etc. Also, in some embodiments, films other than EUV resists can be cleaned in this manner, such as hard masks, UV resists, or films of similar composition having other uses, in which the cleaning process described is related to the chemical composition of the film and not its function.

[0114] Also, in some embodiments, cleaning according to the present disclosure may be combined with a thermal treatment to remove most of the contaminating residues, followed by a plasma treatment to remove any remaining residues. This may be applicable to all applications including chamber cleaning, backside, bevel, stripping, and rework. In some embodiments, this approach may be particularly advantageously applied to chamber cleaning, where the plasma can provide a high degree of control to thoroughly clean the surface. Downstream, where cleaning may be performed primarily to prevent clogging, cleaning quality may be less important and some residue remaining after cleaning may be acceptable.

[0115] Figure 5 shows a graph contrasting HCl, HBr, and BCl3 in etching metal-containing EUV resist with the time of the cleaning operation. As shown in Figure 5, the target metal-containing EUV resist material can be thermally removed by each of HCl, HBr, and BCl3 at high temperatures and with fast etch rates.

[0116] Figure 6 shows a graph comparing the etch rates of various metal-containing EUV resist materials when using HBr as the etching gas. Each line represents a different concentration of tin oxide in the metal-containing EUV resist. Each material has a slightly different etch rate, but each material can be etched quickly using HBr as the etching gas. The higher the concentration of tin oxide, the slower the etch rate.

[0117] FIG. 7 is a graph showing the effect of temperature on the etch selectivity for removing exposed and unexposed regions of the photopatterned metal-containing EUV resist. The dashed line corresponds to the exposed regions of the metal-containing EUV resist, and the solid line corresponds to the unexposed regions of the metal-containing EUV resist. At low temperatures of 0° C. or 10° C., low etch rates were observed for both exposed and unexposed regions of the metal-containing EUV resist. However, at high temperatures of 80° C., high etch rates were observed for both exposed and unexposed regions of the metal-containing EUV resist. Thus, low temperatures result in high etch selectivity and high temperatures result in low etch selectivity. FIG. 8A is a graph showing the effect of temperature on the selectivity for removing the EUV resist. As shown in FIG. 8A, the etch selectivity decreases nonlinearly with increasing temperature. FIG. 8B is a bar graph showing the effect of temperature on the etch rate for removing the EUV resist. As shown in FIG. 8B, the etch rate increases with increasing temperature.

[0118] FIG. 9 is a graph showing the effect of pressure on the etch selectivity for removing exposed and unexposed regions of the photopatterned metal-containing EUV resist. The dashed line corresponds to the exposed regions of the metal-containing EUV resist, and the solid line corresponds to the unexposed regions of the metal-containing EUV resist. At a low pressure of 20 mTorr, a low etch rate was observed in the exposed regions of the metal-containing EUV resist, and a moderately high etch rate was observed in the unexposed regions of the metal-containing EUV resist. However, at a high pressure of 300 mTorr, a high etch rate was observed in both exposed and unexposed regions of the metal-containing EUV resist. Higher etch selectivity is observed at higher pressures, and higher etch rates are observed at higher pressures. FIG. 10A is a graph showing the effect of pressure on the selectivity for removal of the EUV resist. In FIG. 10A, the etch selectivity increases with increasing pressure. FIG. 10B is a bar graph showing the effect of pressure on the etch rate for removal of the EUV resist. In FIG. 10B, the etch rate increases with increasing pressure.

[0119] 11A-11E are graphs showing the performance of HCl as an etching gas at various pressures and temperatures. FIG. 11A is a graph showing the etch amount of EUV resist material versus time when HCl is used as an etching gas at various temperatures of -10°C, 20°C, and 40°C, and a fixed pressure of 20 mTorr. FIG. 11B is a graph showing the etch amount of EUV resist material versus time when HCl is used as an etching gas at various temperatures of -10°C and 20°C, and a fixed pressure of 100 mTorr. FIG. 11C is a graph showing the etch amount of EUV resist material versus time comparing HCl to HBr. FIG. 11D is a bar graph showing the etch rate of EUV resist material at various temperatures when HCl is used as an etching gas. FIG. 11E is a bar graph showing the etch rate of EUV resist material at various pressures when HCl is used as an etching gas.

[0120] FIG. 12 is a graph showing the amount of bromine versus time in a process chamber when purging. As shown in FIG. 12, purging can reduce the HBr on the chamber walls over time. The purge gas is Ar and the chamber walls are heated to 60° C. After 60 minutes, the amount of HBr in the process chamber is 200×10 atoms. 12 pieces / cm 2 is less than.

[0121] Device The disclosed apparatus is configured to perform chamber dry cleaning in situ. The apparatus may be configured to perform other processing operations such as deposition, bevel and backside cleaning, post apply bake, post exposure bake, photoresist rework, descum, smoothing, curing, etching, and other operations. In some embodiments, the apparatus is configured to perform all dry operations. For example, the apparatus is configured to perform dry deposition of EUV resist in the processing chamber as well as dry cleaning of the EUV resist formed on the interior surfaces of the processing chamber. This increases throughput and reduces the chance of contamination by exposing the substrate to a vacuum break between wet and dry operations.

[0122] The apparatus configured for chamber dry cleaning includes a process chamber having a substrate support. The apparatus may include one or more vacuum lines coupled to the process chamber to control pressure, and one or more etching gas lines coupled to the process chamber to deliver etching gas. In some embodiments, there may be multiple vacuum lines to separate the etching gas chemicals from the deposition precursors and counter reactants. In some embodiments, there may be multiple gas inlets positioned inside the process chamber to flow the etching gas near areas where unintended EUV resist material tends to form. In some embodiments, the etching gas includes a halide-containing chemical, such as a hydrogen halide (e.g., HBr or HCl). The apparatus may include one or more heaters for temperature control. Such heaters may be provided in the process chamber and / or the substrate support. In some embodiments, the one or more heaters may include an IR source. The apparatus may further include one or more sensors to sense particle count, wafer count, thickness count, or other parameters to trigger the chamber dry cleaning and / or the chamber dry cleaning endpoint.

[0123] 13 is a schematic diagram of an embodiment of a processing station 1300 having a processing chamber body 1302 for maintaining a low pressure environment suitable for performing the described dry cleaning embodiments. Multiple processing stations 1300 may be included in a common low pressure processing tool environment. For example, FIG. 14 shows an embodiment of a multi-station processing tool 1400, such as a VECTOR® processing tool available from Lam Research Corporation of Fremont, Calif. In some embodiments, one or more hardware parameters of the processing station 1300, such as those discussed in detail below, may be adjusted programmatically by one or more computer controllers 1350.

[0124] The processing stations may be configured as modules within a cluster tool. Figure 16 illustrates a semiconductor processing cluster tool architecture with a vacuum integrated deposition and patterning module suitable for carrying out the embodiments described herein. Such a cluster processing tool architecture may include resist deposition, resist exposure (EUV scanner), resist dry development and etching modules, as previously described and further described below with reference to Figures 15 and 16.

[0125] In some embodiments, certain processing functions, such as dry development and etching, can be performed sequentially in the same module. Additionally, embodiments of the present disclosure are directed to methods and apparatus for receiving a wafer including a photo-patterned EUV resist thin film layer disposed in a layer or layer stack to be etched after photo-patterning with an EUV scanner, as described herein, into a dry development / etch chamber, dry developing the photo-patterned EUV resist thin film layer, and then etching an underlying layer using the patterned EUV resist as a mask.

[0126] Returning to FIG. 13, the processing station 1300 is in fluid communication with a reactant delivery system 1301a that delivers process gases to a distribution showerhead 1306. The reactant delivery system 1301a optionally includes a mixing vessel 1304 for formulating and / or conditioning process gases for delivery to the showerhead 1306. One or more inlet valves 1320 in the mixing vessel may control the introduction of process gases to the mixing vessel 1304. If plasma exposure is used, the plasma may also be delivered to the showerhead 1306 or may be generated in the processing station 1300. As previously mentioned, in at least some embodiments, a non-plasma thermal exposure is preferred.

[0127] 13 includes an optional vaporization point 1303 for vaporizing a liquid reactant provided to the mixing vessel 1304. In some embodiments, a liquid flow controller (LFC) upstream of the vaporization point 1303 may be provided to control the mass flow rate of the liquid for vaporization and delivery to the processing station 1300. For example, the LFC may include a thermal mass flow meter (MFM) located downstream of the LFC. A plunger valve of the LFC may then be adjusted in response to a feedback control signal provided by a proportional differential and integral (PID) controller in electrical communication with the MFM.

[0128] The showerhead 1306 distributes process gases to the substrate 1312. In the embodiment depicted in Figure 13, the substrate 1312 is shown positioned below the showerhead 1306 and resting on a pedestal 1308. The showerhead 1306 may be of any suitable shape and may have any suitable number and arrangement of ports for distributing process gases to the substrate 1312.

[0129] In some embodiments, the pedestal 1308 may be raised or lowered to expose the substrate 1312 to the volume between the substrate 1312 and the showerhead 1306. It will be appreciated that in some embodiments, the height of the pedestal may be programmatically adjusted by a suitable computer controller 1350.

[0130] In some embodiments, the pedestal 1308 may be temperature controlled via a heater 1310. In some embodiments, the pedestal 1308 may be heated to temperatures above 0° C. up to 300° C. or more in the course of exposing the photo-patterned resist to clean chemical reactant gases (e.g., HCl, HBr, HI, and BCl3) as described in the disclosed embodiments.

[0131] Additionally, in some embodiments, pressure control of the processing station 1300 may be provided by a butterfly valve 1318. As shown in the embodiment of FIG. 13, the butterfly valve 1318 throttles the vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, pressure control of the processing station 1300 may be adjusted by varying the flow rate of one or more gases introduced to the processing station 1300.

[0132] In some embodiments, the position of the showerhead 1306 may be adjusted relative to the pedestal 1308 to change the volume between the substrate 1312 and the showerhead 1306. Further, it will be understood that the vertical position of the pedestal 1308 and / or the showerhead 1306 may be changed by any suitable mechanism within the scope of the present disclosure. In some embodiments, the pedestal 1308 may have a rotation axis to rotate the orientation of the substrate 1312. It will be understood that in some embodiments, one or more of these exemplary adjustments may be programmatically implemented by one or more suitable computer controllers 1350.

[0133] For example, in embodiments of mild plasma-based dry development and / or where a plasma may be used with an etching operation performed in the same chamber, the showerhead 1306 and pedestal 1308 are in electrical communication with a radio frequency (RF) power source 1314 and matching network 1316 to power the plasma. In some embodiments, the plasma energy may be controlled by controlling one or more of the process station pressure, gas concentration, RF source power, RF source frequency, and pulse timing of the plasma power. For example, the RF power source 1314 and matching network 1316 may be operated at any suitable power to form a plasma having a desired composition of radical species. An example of a suitable power is up to about 500 W.

[0134] In some embodiments, instructions to the controller 1350 may be provided via input / output control (IOC) sequencing instructions. In one example, instructions for setting conditions for a process step may be included in the appropriate recipe step of a process recipe. In some cases, the steps of a process recipe may be arranged in sequence such that all instructions for a process step are executed simultaneously with that process step. In some embodiments, instructions for setting one or more reactor parameters may be included in a recipe step. For example, a recipe step may include instructions for setting flow rates of clean chemical reactant gases (e.g., HCl, HBr, HI, and BCl3) and time delay instructions for that recipe step. In some embodiments, the controller 1350 may include any of the features described below with respect to the system controller 1450 of FIG. 14.

[0135] As previously mentioned, a multi-station processing tool may include one or more processing stations. FIG. 14 is a schematic diagram of an embodiment of a multi-station processing tool 1400 including an inbound load lock 1402 and an outbound load lock 1404, either or both of which may include a remote plasma source. An atmospheric pressure robot 1406 is configured to move a wafer from a cassette loaded via a pod 1408 to the inbound load lock 1402 via an atmospheric pressure port 1410. The wafer is placed on a pedestal 1412 in the inbound load lock 1402 by the robot 1406, the atmospheric pressure port 1410 is closed, and the load lock is pumped down. If the inbound load lock 1402 includes a remote plasma source, the wafer may be subjected to a remote plasma treatment to treat the silicon nitride surface in the load lock before being introduced into the processing chamber 1414. Additionally, the wafer may also be heated in the inbound load lock 1402, for example to remove moisture and absorbed gases. A chamber transport port 1416 to the processing chamber 1414 then opens and another robot (not shown) places the wafer into the reactor and onto the pedestal of the first station shown in the reactor for processing. Although the embodiment depicted in Figure 14 includes a load lock, it will be understood that in some embodiments the wafer may be placed directly into the processing station.

[0136] The illustrated processing chamber 1414 includes four processing stations, numbered 1-4 in the embodiment shown in FIG. 14. Each station includes a heated pedestal (shown at 1418 in station 1) and a gas line inlet. It will be appreciated that in some embodiments, each processing station may have different or multiple purposes. For example, in some embodiments, a processing station may be switchable between a dry development mode and an etch processing mode. Additionally or alternatively, in some embodiments, the processing chamber 1414 may include one or more combined pairs of dry development and etch processing stations. While the illustrated processing chamber 1414 includes four stations, it will be appreciated that a processing chamber according to the present disclosure may include any suitable number of stations. For example, in some embodiments, a processing chamber may include five or more stations, while in other embodiments, a processing chamber may include three or fewer stations.

[0137] FIG. 14 illustrates an embodiment of a wafer handling system 1490 that transports wafers inside the processing chamber 1414. In some embodiments, the wafer handling system 1490 may transport wafers between various processing stations and / or between processing stations and load locks. It will be understood that any suitable wafer handling system may be used. Non-limiting examples include wafer conveyors and wafer handling robots. FIG. 14 also illustrates an embodiment of a system controller 1450 that is used to control the processing conditions and hardware states of the processing tool 1400. The system controller 1450 may include one or more memory devices 1456, one or more mass storage devices 1454, and one or more processors 1452. The processor 1452 may include a CPU or computer, analog and / or digital input / output connections, stepper motor controller boards, etc.

[0138] In some embodiments, the system controller 1450 controls all activity of the processing tool 1400. The system controller 1450 executes system control software 1458, which is stored in the mass storage device 1454, loaded into the memory device 1456, and executed by the processor 1452. Alternatively, the control logic may be hard-coded into the controller 1450. For these purposes, application specific integrated circuits, programmable logic devices (e.g., field programmable gate arrays, or FPGAs), and the like may be used. In the following discussion, whenever "software" or "code" is used, functionally equivalent hard-coded logic may be used instead. The system control software 1458 may include instructions for controlling the timing, mixture of gases, gas flow rates, chamber and / or station pressure, chamber and / or station temperature, wafer temperature, target power levels, RF power levels, substrate pedestal, chuck and / or susceptor position, and other parameters of a particular process performed by the processing tool 1400. The system control software 1458 may be configured in any suitable manner. For example, various processing tool component subroutines or control objects may be written to control the operation of the processing tool components used to perform the various processing tool processes. The system control software 1458 may be coded in any suitable computer readable programming language.

[0139] In some embodiments, the system control software 1458 may include input / output control (IOC) sequencing instructions for controlling the various parameters previously described. In some embodiments, other computer software and / or programs stored on the mass storage device 1454 and / or memory device 1456 connected to the system controller 1450 may be used. Examples of programs or sections of programs for this purpose include a substrate positioning program, a process gas control program, a pressure control program, a heater control program, and a plasma control program.

[0140] The substrate positioning program may include program code for the processing tool components used to load the substrate onto the pedestal 1418 and control the spacing between the substrate and other parts of the processing tool 1400 .

[0141] The process gas control program may include code for controlling gas composition (e.g., HBr, HCl, or BCl3 gas as described herein) and flow rates, and optionally flowing gases to one or more process stations prior to deposition to stabilize the pressure in the process stations. The pressure control program may include code for controlling the pressure in the process stations, for example, by adjusting throttle valves in the exhaust systems of the process stations, gases flowing to the process stations, etc.

[0142] The heater control program may include code for controlling the current to a heating unit used to heat the substrate, or the heater control program may control the delivery of a heat transfer gas (such as helium) to the substrate.

[0143] A plasma control program may include code for setting RF power levels applied to process electrodes of one or more process stations according to embodiments herein.

[0144] The pressure control program may include code for maintaining pressure in a reaction chamber according to embodiments herein.

[0145] In some embodiments, there may be a user interface connected to the system controller 1450. The user interface may include a display screen, a graphical software display of equipment and / or processing conditions, and a user input device such as a pointing device, keyboard, touch screen, microphone, etc.

[0146] In some embodiments, the parameters adjusted by the system controller 1450 may relate to process conditions. Non-limiting examples include process gas composition and flow rates, temperature, pressure, plasma conditions (such as RF bias power levels), etc. These parameters may be provided to a user in the form of a recipe or may be entered using a user interface.

[0147] Signals to monitor the process may be provided from various process tool sensors by analog and / or digital input connections of the system controller 1450. Signals to control the process may be output at analog and digital output connections of the process tool 1400. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (such as pressure gauges), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used in conjunction with data from these sensors to maintain process conditions.

[0148] The system controller 1450 may issue program instructions for carrying out the deposition processes described above. The program instructions may control various process parameters such as DC power levels, RF bias power levels, pressure, temperature, etc. The instructions may control parameters for operating the dry development process and / or the etching process according to various embodiments described herein.

[0149] The system controller 1450 typically includes one or more memory devices and one or more processors configured to execute instructions such that the device performs methods according to the disclosed embodiments. The system controller 1450 may be coupled to a machine-readable medium that includes instructions that control processing operations according to the disclosed embodiments.

[0150] In some embodiments, the system controller 1450 is part of a system, which may be part of the examples described above. Such systems may include semiconductor processing equipment, including one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems may incorporate electronics that control the operation of the system before, during, and after processing of a semiconductor wafer or substrate. The electronics may be referred to as a "controller" and may control various components or subparts of one or more systems. The system controller 1450 may be programmed to control any of the processes disclosed herein, including delivery of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow settings, fluid delivery settings, position and operation settings, wafer transfer between tools and other transfer tools and / or load locks connected or interfaced to a particular system, depending on the processing conditions and / or type of system.

[0151] In general, the system controller 1450 may be defined as electronic equipment having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips in firmware form that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute the program instructions (e.g., software). The program instructions may be instructions communicated to the system controller 1450 in the form of various individual settings (or program files) that define the operating parameters for performing a particular process on or to a semiconductor wafer or to a system. The operating parameters may, in some embodiments, be part of a recipe defined by a process engineer to accomplish one or more process steps in the course of manufacturing one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.

[0152] The system controller 1450 may, in some embodiments, be part of or coupled to a computer that is integrated, coupled, or otherwise networked to the system. For example, the system controller 1450 may be in the "cloud" or may be all or part of a fab host computer system, thereby enabling remote access of wafer processing. The computer may enable remote access of the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance metrics from multiple manufacturing operations, modify parameters of a current process, set up process steps following a current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows for entry or programming of parameters and / or settings, which are then communicated from the remote computer to the system. In some examples, the system controller 1450 receives instructions in the form of data, where the instructions specify parameters for each of the process steps to be performed in one or more operational steps. It should be understood that the parameters may be specific to the type of process being performed and the type of tool that the system controller 1450 is configured to interface with or control. Thus, as previously discussed, the system controller 1450 may be distributed, such as by including one or more individual controllers that are networked together and function toward a common purpose, such as the processing and control described herein. One example of a distributed controller for such purposes is one or more integrated circuits located in the chamber that are in communication with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer) that combine to control the process in the chamber.

[0153] Exemplary systems may include, but are not limited to, a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an ALD chamber or module, an atomic layer etch (ALE) chamber or module, an ion introduction chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry development chamber or module, and any other semiconductor processing system that may be associated with or used for the manufacturing and / or production of semiconductor wafers.

[0154] As described above, depending on the process step or steps being performed by the tool, the system controller 1450 may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, nearby tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport to carry containers of wafers to and from tool locations and / or load ports in the semiconductor manufacturing factory.

[0155] In certain embodiments, an inductively coupled plasma (ICP) reactor that may be suitable for etching operations suitable for carrying out some embodiments is now described. Although an ICP reactor is described herein, it should be understood that in some embodiments, a capacitively coupled plasma reactor may also be used.

[0156] FIG. 15 illustrates generally a cross-sectional view of an inductively coupled plasma apparatus 1500 suitable for carrying out certain embodiments or aspects of embodiments, such as dry development and / or etching, an example of which is the Kiyo® Reactor manufactured by Lam Research Corporation of Fremont, California.

[0157] The inductively coupled plasma apparatus 1500 includes a processing chamber 1524 defined by a chamber wall 1501 and a window 1511. The chamber wall 1501 may be fabricated from stainless steel or aluminum. The window 1511 may be fabricated from quartz or other dielectric materials. An optional inner plasma grid 1550 divides the overall processing chamber into an upper sub-chamber 1502 and a lower sub-chamber 1503. In most embodiments, the plasma grid 1550 may be removed, thereby utilizing the chamber space created by the sub-chambers 1502 and 1503. A chuck 1517 is disposed within the lower sub-chamber 1503 near a bottom inner surface. The chuck 1517 is configured to receive and hold a semiconductor wafer 1519 on which the etching and deposition processes are performed. The chuck 1517 may be an electrostatic chuck that supports the wafer 1519 in some cases. In some embodiments, an edge ring (not shown) surrounds the chuck 1517 and, when on the chuck 1517, has a top surface that is approximately flush with the top surface of the wafer 1519. The chuck 1517 also includes an electrostatic electrode for securing and unclamping the wafer 1519 to the chuck. For this purpose, a filter and DC clamp power supply (not shown) may be provided. Other control systems may also be provided for lifting the wafer 1519 from the chuck 1517. The chuck 1517 can be charged using an RF power supply 1523. The RF power supply 1523 is connected to a matching circuit 1521 via connection 1527. The matching circuit 1521 is connected to the chuck 1517 via connection 1525. In this manner, the RF power supply 1523 is connected to the chuck 1517. In various embodiments, the bias power of the electrostatic chuck may be approximately 50V or may be set to a different bias power depending on the process being performed according to the disclosed embodiments. For example, the bias power can be from about 20Vb to about 100V, or from about 30V to about 150V.

[0158] The plasma generating element includes a coil 1533, which is disposed over the window 1511. In some embodiments, no coil is used in the disclosed embodiments. The coil 1533 is fabricated from a conductive material and includes at least one complete turn. The example coil 1533 shown in FIG. 15 includes three turns. A cross section of the coil 1533 is symbolically shown, with the coils marked with an "X" extending into the page and the coils marked with a "●" extending out of the page. The plasma generating element also includes an RF power source 1541 configured to provide RF power to the coil 1533. Generally, the RF power source 1541 is connected to a matching circuit 1539 via a connection 1545. The matching circuit 1539 is connected to the coil 1533 via a connection 1543. In this manner, the RF power source 1541 is connected to the coil 1533. An optional Faraday shield 1549a is disposed between the coil 1533 and the window 1511. The Faraday shield 1549a may be maintained in a spaced relationship relative to the coil 1533. In some embodiments, the Faraday shield 1549a is disposed directly above the window 1511. In some embodiments, the Faraday shield 1549b is between the window 1511 and the chuck 1517. In some embodiments, the Faraday shield 1549b is not maintained in a spaced relationship relative to the coil 1533. For example, the Faraday shield 1549b may be directly below the window 1511 with no gap. The coil 1533, the Faraday shield 1549a, and the window 1511 are configured to be substantially parallel to each other. The Faraday shield 1549a may prevent metals or other species from depositing on the window 1511 of the processing chamber 1524.

[0159] Processing gases may enter the processing chamber through one or more main gas inlets 1560 located in the upper subchamber 1502 and / or through one or more side gas inlets 1570. In a similar manner, but not explicitly shown, similar gas inlets may be used to supply processing gases to the capacitively coupled plasma processing chamber. A vacuum pump, such as a one or two stage mechanical dry pump and / or turbomolecular pump 1540, may be used to draw processing gases from the processing chamber 1524 and maintain pressure within the processing chamber 1524. For example, the vacuum pump may be used to evacuate the lower subchamber 1503 during an ALD purge operation. A valve-controlled conduit may be used to fluidly connect the vacuum pump to the processing chamber 1524 and selectively control the application of a vacuum environment provided by the vacuum pump. This may be done using a closed-loop controlled flow restriction device, such as a throttle valve (not shown) or a pendulum valve (not shown), during an active plasma processing process. Similarly, a vacuum pump and valve-controlled fluid connections to a capacitively coupled plasma processing chamber may also be used.

[0160] During operation of the apparatus 1500, one or more process gases may be provided through the gas inlets 1560 and / or 1570. In certain embodiments, process gases may be provided only through the main gas inlet 1560 or only through the side gas inlet 1570. In some cases, the illustrated gas inlets may be replaced with more complex gas inlets, such as one or more showerheads. The Faraday shield 1549a and / or the optional grid 1550 may have internal channels and holes that allow process gases to be delivered to the process chamber 1524. Either or both of the Faraday shield 1549a and the optional grid 1550 may function as showerheads to deliver process gases. In some embodiments, a liquid vaporization and delivery system may be located upstream of the process chamber 1524 such that when liquid reactants or precursors are vaporized, the vaporized reactants or precursors are introduced into the process chamber 1524 through the gas inlets 1560 and / or 1570.

[0161] Radio frequency power is supplied from an RF power source 1541 to the coil 1533, causing an RF current to flow through the coil 1533. The RF current flowing through the coil 1533 generates an electromagnetic field around the coil 1533. The electromagnetic field generates an induced current in the upper subchamber 1502. Various ions and radicals are generated that physically and chemically interact with the wafer 1519 to etch features in the wafer 1519 and selectively deposit layers on the wafer 1519.

[0162] When a plasma grid 1550 is used to provide both an upper subchamber 1502 and a lower subchamber 1503, induced currents act on the gas present in the upper subchamber 1502 to generate an electron ion plasma in the upper subchamber 1502. The optional inner plasma grid 1550 limits the amount of hot electrons in the lower subchamber 1503. In some embodiments, the apparatus 1500 is designed and operated such that the plasma present in the lower subchamber 1503 is an ionic plasma.

[0163] Both the upper electron ion plasma and the lower ionic plasma may contain positive and negative ions, but the ratio of negative ions to positive ions is greater in the ionic plasma. Volatile etching and / or deposition byproducts may be removed from the lower subchamber 1503 through port 1522. The chuck 1517 disclosed herein may operate at elevated temperatures ranging from about 10° C. to about 250° C. The temperature will vary depending on the process operation and the specific recipe.

[0164] The tool 1500 may be coupled to equipment (not shown) when installed in a cleaning room or manufacturing facility. The equipment includes plumbing to provide process gases, vacuum, temperature control, and environmental particle control. These equipment will be coupled to the tool 1500 when installed in the target manufacturing facility. The tool 1500 may also be coupled to a transfer chamber that allows a robot to transfer semiconductor wafers in and out of the tool 1500 using typical automation.

[0165] In some embodiments, a system controller 1530 (which may include one or more physical or logical controllers) controls some or all of the operation of the process chamber 1524. The system controller 1530 may include one or more memory devices and one or more processors. In some embodiments, the apparatus 1500 includes a switching system for controlling flow rates and durations when performing the disclosed embodiments. In some embodiments, the apparatus 1500 may have a switching time of up to about 500 ms, or up to about 750 ms. Switching times may vary depending on the flow chemistry, the selected recipe, the reactor architecture, and other factors.

[0166] In some implementations, the system controller 1530 is part of a system, which may be part of the examples above. Such a system may include semiconductor processing equipment with one or more processing tools, one or more chambers, one or more platforms for processing, and / or specific processing components (wafer pedestal, gas flow system, etc.). These systems may be integrated with electronics that control the operation of the system before, during, and after processing of a semiconductor wafer or substrate. The electronics may be integrated into the system controller 1530 and may control various components or subparts of one or more systems. The system controller may be programmed to control any of the processes disclosed herein, such as supply of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generating tool settings, RF matching circuit settings, frequency settings, flow settings, fluid delivery settings, potential and operation settings, wafer transfer into or out of the tool and other transfer tools and / or load locks connected to or interfaced with the particular system, depending on the process parameters and / or type of system.

[0167] In general, the system controller 1530 may be defined as electronic equipment having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips in firmware form that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute the program instructions (e.g., software). The program instructions may be instructions communicated to the controller in the form of various individual settings (or program files) that define the operating parameters for performing a particular process on or to a semiconductor wafer or to a system. The operating parameters may, in some embodiments, be part of a recipe defined by a process engineer to accomplish one or more process steps in the course of manufacturing or removing one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.

[0168] The system controller 1530 may, in some embodiments, be part of or coupled to a computer that is integrated, coupled, or otherwise networked to the system. For example, the controller may be in the "cloud" or may be all or part of a fab host computer system, which may enable remote access of the wafer processing. The computer may enable remote access of the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance metrics from multiple manufacturing operations, modify parameters of a current process, set up process steps following a current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows for entry or programming of parameters and / or settings, which are then communicated from the remote computer to the system. In some examples, the system controller 1530 receives instructions in the form of data, which specify parameters for each of the process steps to be performed in one or more operational steps. It should be understood that the parameters may be specific to the type of process being performed and the type of tool the controller is configured to interface with or control. Thus, as discussed above, the system controller 1530 may be distributed, such as by including one or more individual controllers networked together and functioning toward a common purpose, such as the processing and control described herein. One example of a distributed controller for such purposes is one or more integrated circuits located in the chamber, which are in communication with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer) that combine to control the process in the chamber.

[0169] Exemplary systems may include, but are not limited to, a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an ALD chamber or module, an ALE chamber or module, an ion introduction chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry development chamber or module, and any other semiconductor processing system that may be associated with or used for the manufacturing and / or production of semiconductor wafers.

[0170] As described above, depending on the process step or steps being performed by the tool, the controller may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, nearby tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport to carry containers of wafers to and from tool locations and / or load ports in a semiconductor manufacturing factory.

[0171] EUVL patterning may be performed using any suitable tool, often referred to as a scanner, such as the TWINSCAN NXE:3300B platform from ASML, Veldhoven, The Netherlands. The EUVL patterning tool may be a standalone device into which the substrate moves for deposition and etching, as described herein. Alternatively, as described below, the EUVL patterning tool may be a module of a larger multi-component tool. FIG. 16 illustrates the architecture of a semiconductor processing cluster tool including a vacuum integrated deposition module, an EUV patterning module, and a dry develop / etch module interfaced with a vacuum transfer module suitable for carrying out the processes described herein. The processes may be performed without such vacuum integrated equipment, although such equipment may be advantageous in some embodiments.

[0172] FIG. 16 illustrates a semiconductor processing cluster tool architecture including vacuum integrated deposition and patterning modules interfaced with a vacuum transfer module suitable for carrying out the processes described herein. The arrangement of transfer and processing modules for "transferring" wafers between multiple storage facilities is sometimes referred to as a "cluster tool architecture" system. The deposition and patterning modules are vacuum integrated according to the requirements of a particular process. Other modules, such as for etching, may also be included in the cluster.

[0173] A vacuum transport module (VTM) 1638 interfaces with four processing modules 1620a-1620d, which may be individually optimized to perform various manufacturing processes. By way of example, processing modules 1620a-1620d may be implemented to perform deposition, vaporization, ELD, dry development, etching, stripping, and / or other semiconductor processes. For example, module 1620a may be an ALD reactor that may be operable to perform non-plasma thermal atomic layer deposition as described herein, such as a Vector tool available from Lam Research Corporation, Fremont, Calif., and module 1620b may be a PECVD tool, such as a Lam Vector®. It should be understood that the figures are not necessarily drawn to scale.

[0174] Airlocks 1642 and 1646, also known as load locks or transfer modules, interface with the VTM 1638 and the patterning module 1640. For example, as previously mentioned, a suitable patterning module may be a TWINSCAN NXE:3300B platform from ASML, Veldhoven, The Netherlands. This tool architecture allows workpieces such as semiconductor substrates or wafers to be transferred under vacuum to make them non-reactive prior to exposure. The integration of deposition modules with lithography tools is facilitated by the fact that EUVL also requires significantly lower pressures, given that there is strong optical absorption of incident photons by surrounding gases such as H2O, O2, etc.

[0175] As mentioned above, this integrated architecture is just one possible embodiment of a tool for carrying out the described process. The process may be carried out using a more conventional stand-alone EUVL scanner and deposition reactor such as a Lam Vector tool, which may be stand-alone or integrated into a cluster architecture that includes other tools such as etch, strip, etc. (e.g., a Lam Kiyo or Gamma tool) as modules, as described, for example, with reference to FIG. 16, although this figure does not have an integrated patterning module.

[0176] Airlock 1642 may be an "outgoing" load lock, referring to transferring substrates from the VTM 1638 serving deposition module 1620a to the patterning module 1640, and airlock 1646 may be an "incoming" load lock, referring to transferring substrates from the patterning module 1640 back to the VTM 1638. The incoming load lock 1646 may provide a boundary to the outside of the tool for transferring substrates in and out. Each processing module has a face that interfaces the module to the VTM 1638. For example, deposition processing module 1620a has face 1636. Within each face, sensors, such as sensors 1-18 as shown, are used to detect the passage of wafer 1626 as it moves between the respective stations. Patterning module 1640 and airlocks 1642 and 1646 may similarly include additional faces and sensors not shown.

[0177] A main VTM robot 1622 transports wafers 1626 between modules including airlocks 1642 and 1646. In one embodiment, the robot 1622 has one arm, and in another embodiment, the robot 1622 has two arms, each arm having an end effector 1624 for picking up and transporting wafers such as wafer 1626. A front-end robot 1644 is used to transport wafers 1626 from the exit airlock 1642 to the patterning module 1640 and from the patterning module 1640 to the entry airlock 1646. The front-end robot 1644 may transport wafers 1626 between the entry loadlock and the exterior of the tool where substrates are loaded and unloaded. The entry airlock module 1646 has the ability to match environments between atmospheric pressure and vacuum, allowing the wafer 1626 to move between the two pressure environments without damage.

[0178] It should be noted that EUVL tools typically operate at a higher vacuum than deposition tools. In this case, it is desirable to elevate the vacuum environment of the substrate during transfer between the deposition and EUVL tools to degas the substrate before entering the patterning tool. The exit airlock 1642 may accomplish this function by holding the transferred wafer at a lower pressure than the pressure of the patterning module 1640 for a period of time and evacuating the off-gassing, so that the optics of the patterning tool 1640 are not contaminated by outgassing from the substrate. A suitable pressure for the outgassing exit airlock is (1E-8) x 133.322 Pascals (1E-8 Torr) or less.

[0179] In some embodiments, a system controller 1650 (which may include one or more physical or logical controllers) controls some or all of the operation of the cluster tool and / or its separate modules. Note that the controller may be local to the cluster architecture, located outside the cluster architecture on the manufacturing floor, or connected to the cluster architecture at a remote location via a network. The system controller 1650 may include one or more memory devices and one or more processors. The processor may include components such as a central processing unit (CPU) or computer, analog and / or digital input / output connections, stepper motor controller boards, etc. Instructions for performing appropriate control operations are executed by the processor. These instructions may be stored in a memory device associated with the controller or provided over a network. In certain embodiments, the system controller executes system control software.

[0180] The system control software may include instructions for controlling the timing of application of any aspect of the operation of a tool or module and / or the magnitude of that aspect. The system control software may be configured in any suitable manner. For example, subroutines or control objects for various processing tool components may be written to control the operation of the processing tool components necessary to perform the processes of the various processing tools. The system control software may be coded in any suitable computer readable program language. In some embodiments, the system control software includes input / output control (IOC) sequencing instructions for controlling the various parameters mentioned above. For example, each stage of a semiconductor manufacturing process may include one or more instructions for execution by the system controller. Instructions for setting process conditions for condensation, deposition, vaporization, patterning and / or etching stages may be included in the corresponding recipe stages, for example.

[0181] In various embodiments, an apparatus for forming a negative pattern mask is provided. The apparatus may include process chambers for patterning, deposition, and etching, and a controller including instructions for forming a negative pattern mask. The instructions may include code for patterning features in a chemically amplified resist (CAR) on a semiconductor substrate by EUV exposure in the process chamber to expose a surface of the substrate, dry developing the photo-patterned resist, and etching an underlying layer or layer stack using the patterned resist as a mask.

[0182] It should be noted that the computer controlling the wafer movement may be local to the cluster architecture, may be located outside the cluster architecture on the manufacturing floor, or may be networked to the cluster architecture at a remote location. The controller described above with respect to any of Figures 13, 14 or 15 may be implemented using the tools of Figure 16.

[0183] conclusion A process and apparatus are disclosed for chamber dry cleaning of metal and / or metal oxide photoresist to remove EUV resist material from interior surfaces of a processing chamber, for example in the context of EUV patterning.

[0184] It is understood that the examples and embodiments described herein are for illustrative purposes only, and various modifications or changes will be suggested to those skilled in the art in light thereof. Various details have been omitted for clarity, and various design alternatives may be implemented. Therefore, the examples should be considered as illustrative and not restrictive, and the present disclosure should not be limited to the details given herein, but may be modified within the scope of the present disclosure. The present disclosure can be realized in the following forms. [Form 1] 1. A method for cleaning a processing chamber, comprising: providing a semiconductor substrate in a process chamber having a metal-containing resist film dry-deposited onto a substrate layer of the semiconductor substrate; introducing an etching gas into the process chamber such that a first thickness of dry-deposited metal-containing resist material is formed on one or more surfaces of the process chamber, the etching gas removing the first thickness of dry-deposited metal-containing resist material; A method comprising: [Form 2] 2. The method of claim 1, further comprising: conditioning one or more surfaces of the processing chamber by forming a second thickness of the dry-deposited metal-containing resist material on one or more surfaces of the processing chamber. A method comprising: [Form 3] 2. The method of claim 1, further comprising: purging the processing chamber after introducing the etching gas to remove residual etching gas from the processing chamber. A method comprising: [Form 4] 4. The method of claim 3, further comprising: The method, wherein purging the processing chamber includes flowing an inert gas and / or a reactive gas into the processing chamber, the processing chamber being heated to an elevated temperature of about 20° C. to about 140° C., and the processing chamber being pumped to a chamber pressure of about 13.3322 Pascals to about 799.934 Pascals (about 0.1 Torr to about 6 Torr). [Form 5] 4. The method of claim 3, further comprising: purging the processing chamber includes subjecting the one or more surfaces of the processing chamber to a remote plasma-based treatment to remove the residual etching gas; The method, wherein the remote plasma-based treatment comprises a fluorine-based chemistry. [Form 6] 4. The method of claim 3, further comprising: The method, wherein purging the processing chamber comprises exposing the one or more surfaces of the processing chamber to a flow of ozone and / or oxygen gas to remove the residual etching gas. [Form 7] 2. The method of claim 1, further comprising: heating the one or more surfaces of the processing chamber to an elevated temperature prior to introducing the etching gas, the elevated temperature being between about 20° C. and about 140° C. method. [Form 8] 8. The method of claim 7, further comprising: The high temperature is from about 80°C to about 120°C. [Form 9] 8. The method of claim 7, further comprising: The method, wherein the etching gas comprises a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a combination thereof. [Form 10] 10. The method of claim 9, further comprising: The hydrogen halide comprises HCl. [Form 11] 2. The method of claim 1, further comprising: The etching gas is hydrogen bromide (HBr), hydrogen chloride (HCl), hydrogen iodide (HI), boron trichloride (BCl 3 ), thionyl chloride (SOCl 2 ), Chlorine (Cl 2 ), Bromine (Br 2 ), iodine (I 2 ), boron tribromide (BBr 3 ), hydrogen (H 2 ), phosphorus trichloride (PCl 3 ), methane (CH 4 ), methanol (CH 3 OH), ammonia (NH 3 ), formic acid (CH 2 O 2 ), nitrogen trifluoride (NF 3 ), hydrogen fluoride (HF), and combinations thereof. [Form 12] 2. The method of claim 1, further comprising: The method, wherein removing the first thickness of the dry-deposited metal-containing resist material occurs without exposure to a plasma. [Form 13] The method according to any one of aspects 1 to 12, further comprising: pumping the process chamber until the chamber pressure is between about 13.3322 Pascals and 799.934 Pascals (between about 0.1 Torr and 6 Torr); heating the one or more surfaces of the processing chamber to an elevated temperature of about 20° C. to about 140° C.; introducing a dummy wafer into the processing chamber prior to introducing the etching gas; A method comprising: [Form 14] 13. The method according to any one of aspects 1 to 12, The method, wherein preparing the semiconductor substrate comprises forming the dry deposited metal-containing resist film on the substrate layer in the process chamber. [Form 15] 13. The method according to any one of aspects 1 to 12, The method, wherein preparing the semiconductor substrate comprises baking the dry deposited metal-containing resist film in the processing chamber. [Form 16] 13. The method according to any one of aspects 1 to 12, The method, wherein preparing the semiconductor substrate comprises dry developing the dry deposited metal-containing resist film in the processing chamber. [Form 17] 13. The method according to any one of aspects 1 to 12, The method, wherein the one or more surfaces of the processing chamber include a chamber wall of the processing chamber. [Form 18] The method according to any one of aspects 1 to 12, further comprising: exposing said one or more surfaces of said processing chamber to an oxidizing gas or oxidizing plasma to remove residual carbon or other contaminants. A method comprising: [Form 19] 13. The method according to any one of aspects 1 to 12, The method wherein the etching gas is introduced through a showerhead or one or more separate chamber inlets to react with the dry-deposited metal-containing resist material and form volatile products. [Form 20] 13. The method according to any one of aspects 1 to 12, The method, wherein said dry-deposited metal-containing resist material is an organometallic oxide or organometallic-containing thin film. [Form 21] 21. The method of claim 20, further comprising: The method, wherein the dry deposited metal-containing resist material comprises an organotin oxide. [Form 22] 1. An apparatus for depositing resist, comprising: a processing chamber including a substrate support; a vacuum line coupled to the processing chamber; an etching gas line coupled to the processing chamber; a controller configured with instructions for cleaning the processing chamber, the instructions comprising: depositing a metal-containing resist film on a substrate layer of a semiconductor substrate in the processing chamber; Cleaning the process chamber by flowing an etching gas into the process chamber, the etching gas removing a first thickness of dry-deposited metal-containing resist material formed on the one or more surfaces of the process chamber. A controller that contains code for 13. An apparatus comprising: [Form 23] 23. The apparatus of claim 22, further comprising: one or more heaters coupled to the one or more surfaces of the processing chamber; The controller further comprises: an apparatus comprising instructions including code for heating the one or more surfaces of the processing chamber to an elevated temperature, the elevated temperature being between about 20° C. and about 140° C. [Form 24] 23. The apparatus of claim 22, The controller further comprises: an apparatus comprising instructions including code for conditioning the one or more surfaces of the processing chamber by forming a second thickness of the dry deposited metal-containing resist material on the one or more surfaces of the processing chamber. [Form 25] 23. The apparatus of claim 22, The apparatus, wherein the controller is further configured with instructions including code for purging the process chamber after introducing the etching gas to remove residual etching gas from the process chamber. [Form 26] 23. The apparatus of claim 22, The apparatus, wherein the etching gas comprises a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a combination thereof. [Form 27] 23. The apparatus of claim 22, further comprising: a remote plasma source coupled to the processing chamber; The remote plasma source can be hydrogen bromide (HBr), hydrogen chloride (HCl), hydrogen iodide (HI), boron trichloride (BCl 3 ), thionyl chloride (SOCl 2 ), Chlorine (Cl 2 ), Bromine (Br 2 ), iodine (I 2 ), boron tribromide (BBr 3 ), hydrogen (H 2 ), phosphorus trichloride (PCl 3 ), methane (CH 4 ), methanol (CH 3 OH), ammonia (NH 3 ), formic acid (CH 2 O 2 ), nitrogen trifluoride (NF 3 ), hydrogen fluoride (HF), and combinations thereof. [Form 28] The device according to any one of aspects 22 to 27, further comprising: a showerhead coupled to the processing chamber, the showerhead being disposed above the substrate support, the etching gas lines being disposed on a wall of the processing chamber and / or below the substrate support, the etching gas being delivered through the etching gas lines, and precursors for depositing the metal-containing resist film being delivered through the showerhead. 13. An apparatus comprising:

Claims

1. 1. A method for cleaning a processing chamber, comprising: providing a semiconductor substrate having a metal-containing resist film dry-deposited on a substrate layer of the semiconductor substrate in a process chamber, wherein a first thickness of dry-deposited metal-containing resist material is formed on one or more surfaces of the process chamber; introducing an etching gas into the process chamber, the etching gas removing the first thickness of the dry-deposited metal-containing resist material; A method comprising:

2. 10. The method of claim 1 further comprising: conditioning one or more surfaces of the processing chamber by forming a second thickness of the dry-deposited metal-containing resist material on one or more surfaces of the processing chamber. A method comprising:

3. 10. The method of claim 1 further comprising: purging the processing chamber after introducing the etching gas to remove residual etching gas from the processing chamber. A method comprising:

4. 4. The method of claim 3, 13. The method of claim 12, wherein purging the processing chamber comprises flowing an inert gas and / or a reactive gas into the processing chamber, the processing chamber being heated to an elevated temperature of about 20° C. to about 140° C., and the processing chamber being pumped to a chamber pressure of about 0.1 Torr to about 6 Torr.

5. 4. The method of claim 3, purging the processing chamber includes subjecting the one or more surfaces of the processing chamber to a remote plasma-based treatment to remove the residual etching gas; The method, wherein the remote plasma-based treatment comprises a fluorine-based chemistry.

6. 4. The method of claim 3, The method, wherein purging the processing chamber comprises exposing the one or more surfaces of the processing chamber to a flow of ozone and / or oxygen gas to remove the residual etching gas.

7. 10. The method of claim 1 further comprising: heating the one or more surfaces of the processing chamber to an elevated temperature prior to introducing the etching gas, the elevated temperature being between about 20° C. and about 140° C.; method.

8. 8. The method of claim 7, The elevated temperature is from about 80°C to about 120°C.

9. 8. The method of claim 7, The method, wherein the etching gas comprises a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a combination thereof.

10. 10. The method of claim 9, The hydrogen halide comprises HCl.

11. 2. The method of claim 1 , The etching gas is hydrogen bromide (HBr), hydrogen chloride (HCl), hydrogen iodide (HI), boron trichloride (BCl 3 ), thionyl chloride (SOCl 2 ), Chlorine (Cl 2 ), bromine (Br 2 ), iodine (I 2 ), boron tribromide (BBr 3 ), hydrogen (H 2 ), phosphorus trichloride (PCl 3 ), methane (CH 4 ), methanol (CH 3 OH), ammonia (NH 3 ), formic acid (CH 2 O 2 ), nitrogen trifluoride (NF 3), hydrogen fluoride (HF), and combinations thereof.

12. 2. The method of claim 1 , The method of claim 1, wherein removing the first thickness of the dry-deposited metal-containing resist material occurs without exposure to a plasma.

13. The method according to any one of claims 1 to 12, further comprising: pumping the process chamber until the chamber pressure is between about 0.1 Torr and 6 Torr; heating the one or more surfaces of the processing chamber to an elevated temperature of about 20° C. to about 140° C.; introducing a dummy wafer into the processing chamber prior to introducing the etching gas; A method comprising:

14. The method according to any one of claims 1 to 12, The method, wherein preparing the semiconductor substrate comprises forming the dry deposited metal-containing resist film on the substrate layer in the process chamber.

15. The method according to any one of claims 1 to 12, The method, wherein preparing the semiconductor substrate comprises baking the dry deposited metal-containing resist film in the processing chamber.

16. The method according to any one of claims 1 to 12, The method, wherein preparing the semiconductor substrate comprises dry developing the dry deposited metal-containing resist film in the processing chamber.

17. The method according to any one of claims 1 to 12, The method, wherein the one or more surfaces of the processing chamber include a chamber wall of the processing chamber.

18. The method according to any one of claims 1 to 12, further comprising: exposing the one or more surfaces of the processing chamber to an oxidizing gas or oxidizing plasma to remove residual carbon or other contaminants. A method comprising:

19. The method according to any one of claims 1 to 12, The method wherein the etching gas is introduced through a showerhead or one or more separate chamber inlets to react with the dry-deposited metal-containing resist material and form volatile products.

20. The method according to any one of claims 1 to 12, The method, wherein said dry-deposited metal-containing resist material is an organometallic oxide or organometallic-containing thin film.

21. 21. The method of claim 20, The method, wherein the dry deposited metal-containing resist material comprises an organotin oxide.

22. 1. An apparatus for depositing resist, comprising: a processing chamber including a substrate support; a vacuum line coupled to the processing chamber; an etching gas line coupled to the processing chamber; a controller configured with instructions for cleaning the processing chamber, the instructions comprising: depositing a metal-containing resist film on a substrate layer of a semiconductor substrate in the processing chamber; Cleaning the process chamber by flowing an etching gas into the process chamber, the etching gas removing a first thickness of dry-deposited metal-containing resist material formed on one or more surfaces of the process chamber. A controller that contains code for 13. An apparatus comprising:

23. 23. The apparatus of claim 22, further comprising: one or more heaters coupled to the one or more surfaces of the processing chamber; The controller further comprises: An apparatus comprising instructions including code for heating the one or more surfaces of the processing chamber to an elevated temperature, the elevated temperature being between about 20°C and about 140°C.

24. 23. The apparatus of claim 22, The controller further comprises:

23. An apparatus comprising: an apparatus comprising: instructions including code for conditioning the one or more surfaces of the processing chamber by forming a second thickness of the dry deposited metal-containing resist material on the one or more surfaces of the processing chamber.

25. 23. The apparatus of claim 22, The apparatus, wherein the controller is further configured with instructions including code for purging the process chamber after introducing the etching gas to remove residual etching gas from the process chamber.

26. 23. The apparatus of claim 22, The apparatus, wherein the etching gas comprises a hydrogen halide, hydrogen gas and a halogen gas, boron trichloride, or a combination thereof.

27. 23. The apparatus of claim 22, further comprising: a remote plasma source coupled to the processing chamber; The remote plasma source may be hydrogen bromide (HBr), hydrogen chloride (HCl), hydrogen iodide (HI), boron trichloride (BCl 3 ), thionyl chloride (SOCl 2 ), Chlorine (Cl 2 ), bromine (Br 2 ), iodine (I 2 ), boron tribromide (BBr 3 ), hydrogen (H 2 ), phosphorus trichloride (PCl 3 ), methane (CH 4 ), methanol (CH 3 OH), ammonia (NH 3 ), formic acid (CH 2 O 2 ), nitrogen trifluoride (NF 3 ), hydrogen fluoride (HF), and combinations thereof.

28. The device according to any one of claims 22 to 27, further comprising: a showerhead coupled to the processing chamber, the showerhead being disposed above the substrate support, the etching gas lines being disposed on a wall of the processing chamber and / or below the substrate support, the etching gas being delivered through the etching gas lines, and precursors for depositing the metal-containing resist film being delivered through the showerhead.

13. An apparatus comprising:

Citation Information

Patent Citations

  • Improved dry photolithography process for exposure with deep ultraviolet ray

    JP2000347421A

  • Device and method for dry-cleaning of treating chamber

    JP2001089860A

  • Method and apparatus for enhanced chamber cleaning

    JP2001308019A

  • Manufacturing method of semiconductor device, and cleaning method of semiconductor manufacturing method

    JP2004247678A

  • Method and apparatus for dry cleaning of a chamber by in situ during photomask plasma etching.