Separator for aluminum electrolytic capacitor and aluminum electrolytic capacitor

A separator made of fibrillated cellulose and synthetic fibers with controlled fiber content and diameter minimizes strength loss, enhancing heat resistance and reliability in conductive polymer capacitors.

JP7554812B2Active Publication Date: 2024-09-20NIPPON KODOSHI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022501730
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-21
Filing Date
2021-01-26
Publication Date
2024-09-20
Estimated Expiration
2041-01-26

AI Technical Summary

Technical Problem

Conventional separators for conductive polymer capacitors, primarily made of cellulose fibers, suffer from rapid deterioration and strength loss when exposed to high temperatures, leading to potential short-circuit defects and increased equivalent series resistance (ESR) due to thermal decomposition and uneven fiber distribution.

Method used

A separator composed of fibrillated cellulose fibers and fibrillated synthetic fibers, with a specific content ratio and average fiber diameter, is designed to minimize tensile strength reduction, maintaining integrity under high temperatures through controlled entanglement and fiber distribution.

Benefits of technology

The separator effectively maintains heat resistance and reduces short-circuit failures and ESR increases, ensuring reliability under both long-term high-temperature exposure and short-term rapid temperature changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554812000002
    Figure 0007554812000002
  • Figure 0007554812000003
    Figure 0007554812000003
  • Figure 0007554812000001
    Figure 0007554812000001
Patent Text Reader

Abstract

The present invention provides a separator for aluminum electrolytic capacitors, said separator being interposed between a pair of electrodes in an aluminum electrolytic capacitor that comprises a conductive polymer as a negative electrode material, wherein: the separator is composed of fibrillated cellulose fibers and fibrillated synthetic fibers; and the tensile strength decrease rate as expressed by formula (1) with use of the tensile strength after 30-minute humidity control at 20°C at 65% RH and the tensile strength after 20-minute heat treatment at 270°C is from 10% to 90%. Formula (1): (X1 – X2) / X1 × 100 X1: Tensile strength after 30-minute humidity control at 20°C at 65% RH X2: Tensile strength after 20-minute heat treatment at 270°C
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for an aluminum electrolytic capacitor and an aluminum electrolytic capacitor using the separator. [Background technology]

[0002] Aluminum electrolytic capacitors are used in many fields, including automotive electrical components and electronic devices. Among aluminum electrolytic capacitors, aluminum solid electrolytic capacitors (hereinafter referred to as "solid electrolytic capacitors") that use a conductive polymer as the cathode material have better frequency characteristics and a smaller equivalent series resistance (hereinafter referred to as "ESR") than regular aluminum electrolytic capacitors that use only an electrolyte as the cathode material, and are therefore used in personal computers and computer CPU peripheral circuits.

[0003] Furthermore, conductive polymer hybrid aluminum electrolytic capacitors (hereinafter referred to as "hybrid electrolytic capacitors"), which use both a conductive polymer and an electrolyte as the cathode material, have a lower ESR than regular aluminum electrolytic capacitors, which use only an electrolyte as the cathode material, and so are also being used in automotive electrical equipment.

[0004] In general, a solid electrolytic capacitor is produced by winding an anode aluminum foil and a cathode aluminum foil with a separator between them, impregnating the foil with a polymerization liquid containing a monomer of a conductive polymer and an oxidizer, polymerizing the monomer to obtain an element containing a conductive polymer, and then inserting the element into a case and sealing the case; alternatively, by winding an anode aluminum foil and a cathode aluminum foil with a separator between them, impregnating the foil with a dispersion of a conductive polymer, drying the foil to obtain an element containing a conductive polymer, and then inserting the element into a case and sealing the case.

[0005] A hybrid electrolytic capacitor is produced by further impregnating an element containing a conductive polymer with an electrolyte solution, inserting the element into a case and then sealing the case, or by injecting an electrolyte solution into the case, inserting the element into the case, impregnating the element with the electrolyte solution, and sealing the case.

[0006] The conduction mechanism of normal aluminum electrolytic capacitors that use only electrolyte is ionic conduction, but the conduction mechanism of solid electrolytic capacitors and hybrid electrolytic capacitors that contain conductive polymers is electronic conduction. For this reason, solid electrolytic capacitors and hybrid electrolytic capacitors have higher responsiveness than normal aluminum electrolytic capacitors, and because they have a low ESR, they can suppress heat generation, and are used in automotive electrical components that require high heat resistance.

[0007] As mentioned above, solid electrolytic capacitors or hybrid electrolytic capacitors containing conductive polymers (hereinafter, solid electrolytic capacitors and hybrid electrolytic capacitors are collectively referred to as "conductive polymer capacitors") are finding a wide range of applications, including personal computers, home game consoles, and automotive electrical components that require high heat resistance and long-term reliability. In particular, when used as automotive electrical components, there is a growing demand for capacitors to be able to withstand a guaranteed life of 150°C and 2,000 hours.

[0008] Additionally, in computer applications, there is an increasing demand for capacitors to be able to withstand temperatures of 270°C, higher than the conventional 260°C, when performing reflow soldering, which calls for separators to have even higher heat resistance.

[0009] As fibers constituting conventional separators for electrochemical elements, including separators for conductive polymer capacitors, cellulose fibers and synthetic fibers are used, and separators using cellulose fibers or synthetic fibers alone or mixtures of these fibers are used. Among them, cellulose fibers have high affinity not only for water but also for various liquids used in the capacitor manufacturing process, such as electrolyte solvents such as ethylene glycol and γ-butyrolactone, monomer liquids, and alcohol-based solvents, and do not dissolve in electrolyte solvents. Therefore, separators containing cellulose fibers have been used for separators for conductive polymer capacitors.

[0010] Patent Documents 1 to 4 and the like have proposed methods for improving the heat resistance of conductive polymer capacitor separators containing cellulose fibers. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent Publication 2017-119941 [Patent Document 2] Patent Publication No. 2019-176073 [Patent Document 3] Patent Publication No. 2006-245550 [Patent Document 4] Retable 2005 / 101432 Summary of the Invention [Problem to be solved by the invention]

[0012] Patent Document 1 proposes a separator made of cellulose fibers as a separator for electrochemical elements. It is said that the use of the separator described in Patent Document 1 can improve heat resistance. However, when a separator made only of cellulose fibers is exposed to high temperatures above the thermal decomposition temperature of cellulose, the decomposition of cellulose is gradually accelerated. This causes a concern that the strength of the separator will decrease and short circuit defects will occur. In other words, a separator with improved heat resistance is required.

[0013] Patent Document 2 describes a separator containing synthetic resin fibers, and controls the porosity, average pore size, and Clark stiffness to control the flexibility of the separator, improving the ESR characteristics and long-term reliability, and also discloses a technology containing cellulose fibers. In this way, a separator with controlled flexibility can suppress the contraction of the separator in a high-temperature environment. Therefore, even if an external force such as vibration is applied to the capacitor, the separator is moderately flexible, so that the element is less likely to shift, and long-term reliability can be improved. However, even such a separator may not have sufficient heat resistance when exposed to long-term high temperatures such as 150°C for 2,000 hours or when exposed to short-term, rapid high temperatures such as reflow soldering at 270°C, as is required in recent years, which may lead to an increase in short-circuit defects and an increase in ESR. In other words, there is a demand for further improving the heat resistance of the separator.

[0014] Patent Document 3 proposes a separator that is unlikely to expand or contract significantly or break when thermal expansion is measured, and describes that by using this separator, electronic components with good heat resistance and high reliability can be provided. The separator described in Patent Document 3 is highly stable in the case of gradual temperature changes. However, when a sudden temperature rise occurs in the element, such as reflow soldering at 270°C, the separator may expand or contract or break. This raises the concern that a short circuit may occur.

[0015] Patent Document 4 describes a separator with a low dimensional change rate after heat treatment. It is disclosed that the use of the separator described in Patent Document 4 can reduce the internal resistance of an electrochemical element even after exposure to high temperatures. This separator can maintain surface smoothness and suppress an increase in internal resistance by suppressing shrinkage when exposed to high temperatures. However, even with such a separator with small shrinkage, it is inevitable that the strength of the separator will decrease when exposed to high temperatures. Therefore, there was a concern that the shielding property of the separator would decrease.

[0016] Patent Documents 3 and 4 disclose a separator made of three components: fibrillated heat-resistant fiber, non-fibrillated fiber, and fibrillated cellulose fiber. It is said that by blending non-fibrillated fiber, the fibrillated heat-resistant fiber and the fibrillated cellulose fiber can be captured to form the basic skeleton of the separator. However, when non-fibrillated fibers are combined with fibrillated fibers, problems such as the tendency to form knotted fibers and poor fiber dispersion can occur, which can lead to poor formation of the separator. A separator containing non-fibrillated fibers is prone to poor formation, resulting in uneven fiber distribution in the paper layer. If the fiber distribution in the paper layer is uneven, strength is likely to decrease locally in areas with a large amount of cellulose fibers when heat is applied. If, as in Patent Document 3 and Patent Document 4, an attempt is made to increase the amount of cellulose fiber blended in order to suppress the expansion and contraction and deformation of the separator, the distribution of cellulose fibers becomes even more uneven, and the decrease in strength becomes more noticeable. Therefore, there is a concern that short circuit defects will occur due to the influence of the separator becoming brittle in parts and decreasing its strength. In addition, if the amount of fibrillated heat-resistant fiber blended is increased in order to increase resistance to high temperatures, there is a concern that the formation will also deteriorate and short circuit defects will occur.

[0017] Thus, separators containing cellulose fibers are widely used as separators for electrochemical elements, but conventional separators have problems with heat resistance when exposed to high temperatures for long periods of time, such as 150°C for 2,000 hours, or when exposed to high temperatures for short periods of time, such as reflow soldering at 270°C. When cellulose fibers are exposed to temperatures above their thermal decomposition temperature, changes in shape, such as shrinkage, are unlikely to occur, but thermal decomposition is unavoidable. Therefore, in order to improve the heat resistance of separators containing cellulose fibers, it is important to improve the resistance under conditions in which cellulose fibers actually decompose. Similarly, in order to improve the heat resistance of conductive polymer capacitors, it is necessary to further improve the heat resistance of separators when they are actually exposed to high temperatures.

[0018] Therefore, as a result of extensive research conducted by the present inventors, it was found that when a separator is exposed to high temperatures, various types of stepwise deterioration occur in the separator, and that it is particularly important to minimize the decrease in the tensile strength of the separator.

[0019] The present invention has been made in view of the above problems, and aims to provide a separator that has good heat resistance and high reliability, and a conductive polymer capacitor using the separator, by minimizing the gradual deterioration that occurs when the separator is exposed to high temperatures, particularly the decrease in tensile strength that occurs in the separator. [Means for solving the problem]

[0020] The present invention aims to solve the above-mentioned problems and to provide a separator that can minimize the gradual deterioration that occurs when the separator is exposed to high temperatures, particularly the decrease in tensile strength. As one means for achieving this aim, an embodiment of the present invention has, for example, the following configuration.

[0021] That is, a separator for an aluminum electrolytic capacitor, which is interposed between a pair of electrodes and has a conductive polymer as a cathode material, the separator being made of fibrillated cellulose fiber and fibrillated synthetic fiber, The content of fibrillated cellulose fibers in the entire separator is 40 to 60 mass%, and the content of fibrillated synthetic fibers is 40 to 60 mass%, and the separator contains, as the fibrillated cellulose fibers, fibers having an average fiber diameter of 6 to 12 μm, and as the fibrillated synthetic fibers, fibers having an average fiber diameter of 13 to 22 μm,The tensile strength reduction rate, expressed by the following formula (1), is determined by using the tensile strength after conditioning at 20°C and 65% RH for 30 minutes and the tensile strength after heat treatment at 270°C for 20 minutes. 80 %. Formula (1): (X1-X2) / X1×100 X1: Tensile strength after 30 minutes at 20℃ and 65% RH X2: Tensile strength after heat treatment at 270℃ for 20 minutes

[0022] Furthermore, the separator is characterized in that the tensile strength reduction rate is 20 to 80%.

[0023] Furthermore, the tensile strength after heat treatment at 270° C. for 20 minutes is 160 to 1600 N / m.

[0025] Alternatively, the present invention provides an aluminum electrolytic capacitor using a separator for an aluminum electrolytic capacitor having the above-mentioned configuration.

[0026] For example, the fibrillated synthetic fiber contains at least one type of fiber selected from the group consisting of wholly aromatic polyamide and wholly aromatic polyester.

[0028] In addition, for example, the aluminum electrolytic capacitor is characterized in that a conductive polymer is used as a cathode material in the pair of electrodes. Effect of the Invention

[0029] According to the present invention, by minimizing the decrease in tensile strength of the separator, which is one of the gradual deteriorations that occurs when the separator is exposed to high temperatures, it is possible to provide a highly reliable separator with good heat resistance, and a conductive polymer capacitor using the separator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] An embodiment of the present invention will be described in detail below. When heat treatment is performed under conditions that are more severe than the peak temperature and time of reflow soldering for general aluminum electrolytic capacitors, the separator deteriorates rapidly in a relatively short time. The deterioration progresses in stages, but the tensile strength of the separator in particular decreases rapidly. The inventors have discovered that if the sudden decrease in tensile strength that occurs in the separator can be suppressed, it is possible to ensure heat resistance not only during short-term, sudden exposure to high temperatures, such as in reflow soldering, but also during long-term exposure to high temperatures in the capacitor's usage environment.

[0031] In view of the above, the separator of the present embodiment is configured as follows, for example. The separator is for an aluminum electrolytic capacitor, and is interposed between a pair of electrodes and used in the aluminum electrolytic capacitor having a conductive polymer as a cathode material, the separator being made of fibrillated cellulose fibers and fibrillated synthetic fibers, and having a tensile strength reduction rate of 10 to 90%, as expressed by the following formula (1), using the tensile strength after humidity conditioning at 20°C and 65% RH for 30 minutes and the tensile strength after heat treatment at 270°C for 20 minutes:

[0032] Formula (1): (X1-X2) / X1×100 X1: Tensile strength after 30 minutes at 20℃ and 65% RH X2: Tensile strength after heat treatment at 270℃ for 20 minutes In the present invention, hereinafter, the tensile strength after conditioning at 20°C and 65% RH for 30 minutes (X1) will be referred to as "tensile strength after conditioning," and the tensile strength after heat treatment at 270°C for 20 minutes (X2) will be referred to as "tensile strength after heat treatment."

[0033] In the present invention, the tensile strength reduction rate was used as an index of the heat resistance of the separator. When the separator is subjected to excessive heat treatment such as heat treatment at 270°C for 20 minutes, changes such as thermal decomposition and melting of the fibers constituting the separator occur. These changes act in combination, and the tensile strength of the separator drops sharply. By determining the tensile strength reduction rate of the separator, it is possible to estimate the extent to which the separator has changed due to the heat treatment. In other words, if the tensile strength reduction rate is too high, it can be estimated that changes such as excessive thermal decomposition and melting have occurred in the fibers constituting the separator. Therefore, by determining the tensile strength reduction rate, the degree of change of the separator due to the heat treatment can be estimated and used as an index of the heat resistance of the separator. Note that the tensile strength reduction rate of the present invention assumes that the tensile strength value after humidity adjustment is greater than the tensile strength value after heat treatment, and the tensile strength reduction rate is a positive value.

[0034] The separator of this embodiment has a tensile strength reduction rate of 10 to 90%, as shown in the above formula (1). If the tensile strength reduction rate is 10 to 90%, the tensile strength will not decrease even if the separator is exposed to high temperatures for a long time or abruptly exposed to high temperatures for a short time. In other words, the changes due to thermal decomposition or melting of the fibers constituting the separator can be minimized, and the shielding properties of the separator and the continuity of the conductive polymer can be maintained even after heat treatment. If the changes such as thermal decomposition or melting of the fibers can be minimized, the fibers will not become brittle and easily crumble, and there will not be areas in the paper layer where there are few fibers. Therefore, a capacitor using this separator can reduce the short-circuit failure rate after reflow soldering and reduce the increase rate of ESR after a high-temperature load test assuming long-term reliability. Preferably, by setting the tensile strength reduction rate to 20 to 80% or less, the changes due to thermal decomposition or melting of the fibers constituting the separator can be further suppressed. Although a lower tensile strength reduction rate is preferable, the upper limit that can be achieved with the separator of the present invention is 10%. However, taking into consideration the strength of the separator required when fabricating the element winding, it is preferable to set the upper limit at 20%. In addition, it is preferable that the separator after the heat treatment does not have any deformation such as shrinkage or wrinkles.

[0035] If the tensile strength reduction rate exceeds 90%, the separator will decompose rapidly when exposed to high temperatures for a long time or suddenly exposed to high temperatures for a short time, causing the entanglement and bonding of the fibers that make up the separator to be damaged, and the separator will no longer be able to maintain its shielding properties. In other words, the fibers that make up the separator will be thermally decomposed or melted excessively, causing the fibers to become brittle and easily crumble, or causing areas in the paper layer with fewer fibers. Therefore, when reflow soldering or long-term reliability tests are performed on capacitors using this separator, problems such as short circuit failures caused by burrs on the electrode foil, etc. penetrating the separator, and cracks in the conductive polymer layer formed on the fiber surface or between the fibers may occur, causing the ESR to increase.

[0036] [Heat treatment] The heat treatment in this embodiment will be described below. In this embodiment, "heat treatment at 270°C for 20 minutes" means that the separator is placed in a device (such as a thermostatic bath or oven whose internal temperature is raised to 270°C) that has been heated to 270°C in advance, and then left for 20 minutes. A thermostatic bath or oven can be used as a device for heat treating the separator at 270°C. The atmosphere during the test can be air or in an inert gas, but it is preferable to carry out the test in air. In air, the fibers constituting the separator are also deteriorated by oxidation, and the evaluation can be carried out under severe conditions. If the tensile strength reduction rate can be kept to 90% or less under these conditions, the tensile strength reduction rate will also be 90% or less in an inert gas.

[0037] In the case of hybrid electrolytic capacitors, the separator exists inside the element in a wet state containing the electrolyte. Since the thermal decomposition of the fibers proceeds more slowly in a wet state, if the tensile strength reduction rate in air is 90% or less, the separator can maintain its tensile strength even in a wet state, resulting in a separator with excellent heat resistance.

[0038] The separator according to the embodiment of the present invention preferably has a tensile strength of 160 N / m or more after heat treatment. Even if the fibers constituting the separator undergo changes such as thermal decomposition or melting due to heat treatment, the separator can maintain its minimum functionality as long as the tensile strength after heat treatment is 160 N / m or more. More preferably, the tensile strength after heat treatment is 200 N / m or more, so that changes such as thermal decomposition or melting of the fibers constituting the separator can be further suppressed. The higher the tensile strength after heat treatment, the better, but considering the feasible range for the separator for aluminum electrolytic capacitors of the present invention, 1600 N / m is the upper limit.

[0039] In the separator according to the embodiment of the present invention, the tensile strength after humidity conditioning is preferably 330 N / m or more, and more preferably 520 N / m or more, in consideration of the workability when manufacturing the capacitor element winding. If the tensile strength after humidity conditioning is 520 N / m or more, the productivity when manufacturing the element winding is less likely to deteriorate.

[0040] The separator of the present invention contains fibrillated cellulose fibers. The cellulose fibers form hydrogen bonds between cellulose molecules, which serve as the skeleton of the separator and can increase the tensile strength after humidity conditioning. In addition, the cellulose fibers are not easily shrunk by heat, so the separator is likely to maintain its shape after heat treatment. In addition, by blending fibrillated cellulose fibers in which fibrils have been generated by beating, the strength and shielding properties of the separator can be controlled. Furthermore, by blending fibrillated cellulose fibers, the separator is likely to have good texture and the tensile strength after humidity conditioning is likely to be increased. Examples of cellulose fibers that can be used in the separator of the present invention include natural cellulose fibers and regenerated cellulose fibers. As natural cellulose fibers, vein fibers such as Manila hemp and sisal hemp from wood pulp, bast fibers such as jute and kenaf, grass plant fibers such as esparto, bamboo, rice straw, and sedge, and seed hair fibers such as cotton linters can be used. As regenerated cellulose fibers, solvent-spun cellulose fibers can be preferably used. Natural cellulose fibers are preferred because they have a higher degree of polymerization of cellulose than regenerated cellulose fibers and are less likely to cause a decrease in fiber strength even when exposed to high temperatures. Considering dispersibility when combined with synthetic fibers, it is preferable to include fibers such as sisal hemp, jute, kenaf, esparto, bamboo, rice straw, sedge, sedge, and bagasse among natural cellulose fibers. These fibers have short fiber lengths and small fiber diameters, so they have good dispersibility. Therefore, even when combined with synthetic fibers, they are easily dispersed uniformly to form a separator with good texture.

[0041] The separator of the present invention contains fibrillated synthetic fibers in addition to fibrillated cellulose fibers. By blending synthetic fibers, the rate of decrease in tensile strength can be suppressed compared to the case of using cellulose fibers alone. Although the details are unclear, it is thought that the uniform entanglement of synthetic fibers and cellulose fibers makes it difficult for localized areas of low strength to occur due to heat treatment, and thus the effect of suppressing the decrease in strength can be obtained. In addition, blending fibrillated synthetic fibers that have fibrils generated by beating treatment makes it easier to obtain a separator with good texture, and makes it easier to increase the tensile strength after heat treatment.

[0042] Among synthetic fibers, in consideration of stability at high temperatures and chemical resistance, it is preferable to contain aramid fibers, which are fully aromatic polyamide fibers, and polyarylate fibers, which are fully aromatic polyester fibers. Examples of aramid fibers include meta-aramid and para-aramid, and para-aramid is more preferable. These fully aromatic polyamide fibers and fully aromatic polyester fibers can be fibrillated by beating treatment because the molecules constituting the fibers have a high degree of orientation. Therefore, the strength and shielding properties of the separator can be controlled.

[0043] To achieve a tensile strength reduction rate of 10 to 90% using fibrillated cellulose fibers and fibrillated synthetic fibers, the balance of entanglement between the two fibers is important. In the present invention, the average fiber diameter is used as an index of entanglement. In the separator of the present invention, it is preferable that the average fiber diameter of the fibrillated cellulose fibers is 6 to 12 μm and the average fiber diameter of the fibrillated synthetic fibers is 13 to 22 μm. By setting the average fiber diameters of both fibers within the above ranges, the fibers are uniformly dispersed when the two fibers are combined, making it easy to obtain a separator with good texture.

[0044] If the average fiber diameter of the fibrillated cellulose fibers exceeds 12 μm, or if the average fiber diameter of the fibrillated synthetic fibers exceeds 22 μm, the entanglement of the two fibers is weak, which may cause the separator to have a poor texture or a low tensile strength after humidity control. If the average fiber diameter of the fibrillated cellulose fibers is less than 6 μm, or if the average fiber diameter of the fibrillated synthetic fibers is less than 13 μm, the amount of fine fibers increases too much, reducing the voids inside the separator and deteriorating the permeability of the conductive polymer. Furthermore, if the amount of fine fibers increases too much, dehydration in the papermaking machine becomes poor, resulting in reduced productivity. The average fiber diameter referred to here refers to the fiber diameter of the core portion, not the fibril portion generated by the beating treatment. The average fiber diameters of the fibrillated cellulose fibers and fibrillated synthetic fibers can be measured by observing the separator with a scanning electron microscope.

[0045] To obtain an average fiber diameter of fibrillated cellulose fibers of 6 to 12 μm, the CSF value of the cellulose fibers should be in the range of 300 ml to 0 ml. To obtain an average fiber diameter of fibrillated synthetic fibers of 13 to 22 μm, synthetic fibers having a fiber length of 0.5 to 5.0 mm and a fiber diameter of 15 to 24 μm should be used and the CSF value should be in the range of 700 ml to 50 ml. As the synthetic fibers, fibers having branched fibrils such as pulp may be used, and in that case, if the fiber length and fiber diameter are in the above ranges, the average fiber diameter can be obtained by setting the CSF value in the range of 700 ml to 50 ml. If the CSF values ​​of the fibrillated cellulose fibers and the fibrillated synthetic fibers are within this range, the average fiber diameters of both fibers can be within the above range, and the separator can have a uniform fiber distribution and good texture.

[0046] The equipment used for beating the cellulose fibers and synthetic fibers of the present invention may be any equipment used for preparing ordinary papermaking materials, generally including a beater, a conical refiner, a disc refiner, a high-pressure homogenizer, etc.

[0047] The content of fibrillated cellulose fibers in the entire separator of the present invention is preferably 30 to 70 mass%, more preferably 40 to 60 mass%, and the content of fibrillated synthetic fibers is preferably 30 to 70 mass%, more preferably 40 to 60 mass%. When the content of fibrillated cellulose fibers is less than 30% by mass, i.e., when the content of fibrillated synthetic fibers exceeds 70% by mass, it is difficult to increase the tensile strength of the separator after humidity adjustment. Furthermore, since fibrillated synthetic fibers are more likely to aggregate when dispersed in water than fibrillated cellulose fibers, the texture of the separator is likely to deteriorate. Furthermore, when the content of fibrillated cellulose fibers exceeds 70% by mass, i.e., when the content of fibrillated synthetic fibers is less than 30% by mass, the impregnation of the conductive polymer is likely to deteriorate.

[0048] In the embodiment of the present invention, the separator is a wet nonwoven fabric formed by a papermaking method. The separator is not particularly limited in the papermaking method, and may be formed by a papermaking method such as cylinder papermaking, short wire papermaking, or fourdrinier papermaking. The separator may also be formed by combining a plurality of layers formed by these papermaking methods. In addition, additives such as dispersants, defoamers, and paper strength enhancers may be added during the papermaking process, as long as the impurity content is not so high as to affect the capacitor separator. Furthermore, after the paper layer is formed, post-processing such as paper strength enhancement, lyophilic processing, calendaring, and embossing may be performed. However, the present invention is not limited to wet nonwoven fabrics formed by a papermaking method, and a method of forming a film by casting a fiber dispersion liquid, as used in a film-forming method, may also be used.

[0049] In the embodiment of the present invention, there is no particular limitation on the thickness and density of the separator. Taking into consideration the shielding property of the separator and the handling property during use such as strength, the thickness is preferably 25 to 80 μm and the density is preferably 0.250 to 0.550 g / cm. 3 The degree is common.

[0050] It was discovered that the above separator configuration can provide a separator for conductive polymer capacitors with good heat resistance by minimizing the gradual deterioration that occurs when the separator is exposed to high temperatures, particularly the decrease in strength that occurs in the separator. The aluminum electrolytic capacitor of this embodiment uses a separator having the above-described configuration as a separator made of fibrillated cellulose fibers and fibrillated synthetic fibers, interposes the separator between a pair of electrodes, and uses a conductive polymer as the cathode material.

[0051] [Method of measuring the characteristics of separators and aluminum electrolytic capacitors] Specific measurements of the characteristics of the separator and aluminum electrolytic capacitor of the present embodiment were performed under the following conditions and by the following method.

[0052] [Thickness] The thickness of the separator was measured using the micrometer specified in "JIS C 2300-2 'Cellulose paper for electrical purposes - Part 2: Test methods' 5.1 Thickness" in "5.1.1 Measuring instruments and measurement methods a When using an outside micrometer" and the method of folding the paper into 10 sheets in "5.1.3 When measuring thickness by folding the paper"

[0053] 〔density〕 The density of the separator in an absolute dry state was measured according to the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test method' 7.0A Density" Method B.

[0054] [CSF value] The CSF value was measured in accordance with JIS P8121-2 "Pulps-Determination of drainability-Part 2: Canadian Standard freeness method" (ISO5267-2 "Pulps-Determination of drainability-Part 2: "Canadian Standard" freeness method").

[0055] [Tensile strength reduction rate] The rate of decrease in tensile strength of the separator was calculated according to the following formula (1). Formula (1): (X1-X2) / X1×100 X1: Tensile strength after 30 minutes at 20℃ and 65% RH X2: Tensile strength after heat treatment at 270℃ for 20 minutes The preparation of the measurement sample and the measurement method were performed according to the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test methods' 8 Tensile strength and elongation", and the tensile strength in the longitudinal direction of the separator was measured. When measuring X1, the prepared separator test piece was conditioned at 20° C. and 65% RH for 30 minutes, and then the tensile strength of the separator was measured. When measuring X2, the prepared separator test piece was placed in a thermostatic chamber whose inside temperature had been raised to 270° C. in advance, and the tensile strength of the separator was measured after heat treatment for 20 minutes. Using the thus obtained X1 and X2, the tensile strength reduction rate was calculated according to the above formula (1).

[0056] [Average fiber diameter of fibrillated cellulose fibers and fibrillated synthetic fibers] The surface of the separator was observed at 1000 times magnification using a scanning electron microscope, and the lengths of the core portions of 100 fibers were measured and the average value was calculated.

[0057] [Fabrication process of solid electrolytic capacitor] Using the separators of the Example, Comparative Example, and Conventional Example, two types of solid electrolytic capacitors were fabricated: one with a rated voltage of 6.3 V, a diameter of 8.0 mm, and a height of 7.0 mm, and the other with a rated voltage of 50 V, a diameter of 8.0 mm, and a height of 10.0 mm.

[0058] A specific method for producing the solid electrolytic capacitor is as follows. The anode foil and cathode foil that had been etched and oxide film-formed were wound with a separator interposed therebetween so as not to come into contact with each other, to prepare a capacitor element. The prepared capacitor element was then subjected to a second chemical conversion treatment and then dried.

[0059] For the solid electrolytic capacitor with a rated voltage of 6.3V, the capacitor element was impregnated with a conductive polymer polymerization liquid, then heated and polymerized, and the solvent was dried to form a conductive polymer layer. For the solid electrolytic capacitor with a rated voltage of 50V, the capacitor element was impregnated with a conductive polymer dispersion liquid, then heated and dried to form a conductive polymer layer. The capacitor element was then placed in a specified case, the opening was sealed, and aging was performed to obtain each solid electrolytic capacitor.

[0060] [Production process of hybrid electrolytic capacitor] Using the separators of the working example, comparative example, and conventional example, two types of hybrid electrolytic capacitors were fabricated: one with a rated voltage of 16 V, a diameter of 10.0 mm, a height of 10.5 mm, and one with a rated voltage of 80 V, a diameter of 8.0 mm, and a height of 10.0 mm.

[0061] A specific method for producing the hybrid electrolytic capacitor is as follows. The anode foil and cathode foil that had been etched and oxide film-formed were wound with a separator interposed therebetween so as not to come into contact with each other, to prepare a capacitor element. The prepared capacitor element was then subjected to a re-chemical conversion treatment and then dried.

[0062] For the hybrid electrolytic capacitor with a rated voltage of 16V, a capacitor element was impregnated with a conductive polymer polymerization liquid, which was then heated and polymerized, and the solvent was dried to form a conductive polymer layer. For the hybrid electrolytic capacitor with a rated voltage of 80V, a capacitor element was impregnated with a conductive polymer dispersion liquid, which was then heated and dried to form a conductive polymer layer. The above capacitor elements were then impregnated with a driving electrolyte, the capacitor elements were placed in a specified case, the openings were sealed, and aging was performed to obtain the respective hybrid electrolytic capacitors.

[0063] [Initial ESR] The ESR of the fabricated capacitor was measured using an LCR meter at a temperature of 20°C and a frequency of 100 kHz.

[0064] [Short circuit failure rate after reflow soldering] The short circuit defect rate after reflow soldering was measured by first performing reflow soldering for 1 minute using the prepared capacitors, with the peak temperature at 270°C and the time over 230°C for 30 seconds. The rated voltage was then applied to the capacitors, and the number of short circuits that occurred was counted. The number of short circuits was divided by the total number of capacitors, and the percentage was calculated to determine the short circuit defect rate after reflow soldering.

[0065] [ESR increase rate after high temperature load test] After the high temperature load test, the ESR was measured using an LCR meter at a temperature of 20°C and a frequency of 100 kHz after heating at 150°C for 500 hours. The ESR after the high-temperature load test was divided by the ESR before the high-temperature load test to calculate the rate of increase in ESR after the high-temperature load test.

[0066] [Examples, Comparative Examples and Conventional Examples] Hereinafter, specific examples of the separator according to the embodiment of the present invention will be described.

[0067] The synthetic fibers used in each of the Examples, Comparative Examples, and Conventional Examples are listed in Table 1. Table 1 shows the fiber material, average fiber diameter, and fiber length of each of the synthetic fibers (Synthetic Fibers 1 to 6).

[0068] [Table 1]

[0069] Example 1 A raw material containing 60% by mass of fibrillated cellulose fiber beaten using jute fiber until the CSF value reached 200 ml, and 40% by mass of fibrillated synthetic fiber beaten using synthetic fiber 1 until the CSF value reached 100 ml was made into a cylinder net in one layer to obtain the separator of Example 1. The average fiber diameter of the fibrillated cellulose fiber was 11.5 μm, and the average fiber diameter of the fibrillated synthetic fiber was 13.4 μm. The completed separator of Example 1 had a thickness of 40 μm and a density of 0.453 g / cm 3 The tensile strength after humidity conditioning was 1020 N / m, the tensile strength after heat treatment was 410 N / m, and the tensile strength reduction rate was 60%.

[0070] Example 2 A raw material containing 70% by mass of fibrillated cellulose fiber beaten to a CSF value of 290 ml using cellulose fiber containing bamboo fiber and Manila hemp fiber in a 1:1 ratio, and 30% by mass of fibrillated synthetic fiber beaten to a CSF value of 50 ml using synthetic fiber 1 was made into a single layer using a cylinder net to obtain a separator of Example 2. The average fiber diameter of the fibrillated cellulose fiber was 11.8 μm, and the average fiber diameter of the fibrillated synthetic fiber was 13.2 μm. The completed separator of Example 2 had a thickness of 25 μm and a density of 0.545 g / cm 3 The tensile strength after humidity conditioning was 1500 N / m, the tensile strength after heat treatment was 170 N / m, and the tensile strength reduction rate was 89%.

[0071] Example 3 A raw material containing 30% by mass of fibrillated cellulose fiber beaten to a CSF value of 20 ml using dragonfly fiber and 70% by mass of fibrillated synthetic fiber beaten to a CSF value of 110 ml using synthetic fiber 2 was made into a cylinder net in one layer to obtain a separator of Example 3. The average fiber diameter of the fibrillated cellulose fiber was 6.3 μm, and the average fiber diameter of the fibrillated synthetic fiber was 14.2 μm. The completed separator of Example 3 had a thickness of 50 μm and a density of 0.260 g / cm 3 The tensile strength after humidity conditioning was 950 N / m, the tensile strength after heat treatment was 160 N / m, and the tensile strength reduction rate was 83%.

[0072] Example 4 A raw material containing 60% by mass of fibrillated cellulose fiber beaten using kenaf fiber until the CSF value reached 240 ml, and 40% by mass of fibrillated synthetic fiber beaten using synthetic fiber 3 until the CSF value reached 670 ml was made into a cylinder-type sheet to obtain a separator of Example 4. The average fiber diameter of the fibrillated cellulose fiber was 11.6 μm, and the average fiber diameter of the fibrillated synthetic fiber was 21.4 μm. The completed separator of Example 4 had a thickness of 35 μm and a density of 0.360 g / cm 3 The tensile strength after humidity conditioning was 940 N / m, the tensile strength after heat treatment was 210 N / m, and the tensile strength reduction rate was 78%.

[0073] Example 5 A raw material containing 50% by mass of fibrillated cellulose fiber obtained by beating cellulose fiber containing kenaf fiber and Manila hemp fiber in a 1:1 ratio until the CSF value was 0 ml, and 50% by mass of fibrillated synthetic fiber obtained by beating synthetic fiber 4 until the CSF value was 690 ml was made into a double layer paper using a cylinder net to obtain the separator of Example 5. The average fiber diameter of the fibrillated cellulose fiber was 6.7 μm, and the average fiber diameter of the fibrillated synthetic fiber was 21.7 μm. The completed separator of Example 5 had a thickness of 80 μm and a density of 0.472 g / cm 3The tensile strength after humidity conditioning was 2700 N / m, the tensile strength after heat treatment was 1500 N / m, and the tensile strength reduction rate was 44%.

[0074] Example 6 A raw material containing 40% by mass of fibrillated cellulose fiber beaten using sisal fiber until the CSF value reached 250 ml, and 60% by mass of fibrillated synthetic fiber beaten using synthetic fiber 5 until the CSF value reached 130 ml was made into a cylinder net in one layer to obtain the separator of Example 6. The average fiber diameter of the fibrillated cellulose fiber was 11.1 μm, and the average fiber diameter of the fibrillated synthetic fiber was 13.5 μm. The completed separator of Example 6 had a thickness of 40 μm and a density of 0.304 g / cm 3 The tensile strength after humidity conditioning was 350 N / m, the tensile strength after heat treatment was 290 N / m, and the tensile strength reduction rate was 17%.

[0075] Example 7 A raw material containing 55% by mass of fibrillated cellulose fiber beaten using jute fiber until the CSF value reached 50 ml, and 45% by mass of fibrillated synthetic fiber beaten using synthetic fiber 5 until the CSF value reached 480 ml was made into a cylinder net in one layer to obtain a separator of Example 7. The average fiber diameter of the fibrillated cellulose fiber was 8.6 μm, and the average fiber diameter of the fibrillated synthetic fiber was 17.0 μm. The completed separator of Example 7 had a thickness of 50 μm and a density of 0.420 g / cm 3 The tensile strength after humidity conditioning was 810 N / m, the tensile strength after heat treatment was 600 N / m, and the tensile strength reduction rate was 26%.

[0076] Comparative Example 1 A raw material containing 80% by mass of fibrillated cellulose fiber beaten using sisal fiber until the CSF value reached 280 ml, and 20% by mass of fibrillated synthetic fiber beaten using synthetic fiber 1 until the CSF value reached 20 ml was made into a cylinder net in one layer to obtain a separator of Comparative Example 1. The average fiber diameter of the fibrillated cellulose fiber was 11.3 μm, and the average fiber diameter of the fibrillated synthetic fiber was 12.0 μm. The completed separator of Comparative Example 1 had a thickness of 50 μm and a density of 0.470 g / cm 3 The tensile strength after humidity conditioning was 1820 N / m, the tensile strength after heat treatment was 150 N / m, and the tensile strength reduction rate was 92%.

[0077] Comparative Example 2 A raw material containing 70% by mass of fibrillated cellulose fiber beaten using kenaf fiber until the CSF value reached 330 ml, and 30% by mass of fibrillated synthetic fiber beaten using synthetic fiber 4 until the CSF value reached 460 ml was made into a cylinder-type sheet to obtain a separator of Comparative Example 2. The average fiber diameter of the fibrillated cellulose fiber was 12.8 μm, and the average fiber diameter of the fibrillated synthetic fiber was 19.0 μm. The completed separator of Comparative Example 2 had a thickness of 50 μm and a density of 0.378 g / cm 3 The tensile strength after humidity conditioning was 500 N / m, the tensile strength after heat treatment was 40 N / m, and the tensile strength reduction rate was 92%.

[0078] Comparative Example 3 A raw material containing 20% ​​by mass of fibrillated cellulose fiber beaten using bamboo fiber until the CSF value reached 210 ml, and 80% by mass of fibrillated synthetic fiber beaten using synthetic fiber 3 until the CSF value reached 740 ml was made into a single layer using a cylinder net to obtain a separator of Comparative Example 3. The average fiber diameter of the fibrillated cellulose fiber was 11.7 μm, and the average fiber diameter of the fibrillated synthetic fiber was 22.9 μm. The completed separator of Comparative Example 3 had a thickness of 30 μm and a density of 0.390 g / cm 3 The tensile strength after humidity conditioning was 320 N / m, the tensile strength after heat treatment was 20 N / m, and the tensile strength reduction rate was 94%.

[0079] Comparative Example 4 A raw material containing 70% by mass of fibrillated cellulose fiber beaten using jute fiber until the CSF value reached 0 ml, and 30% by mass of fibrillated synthetic fiber beaten using synthetic fiber 5 until the CSF value reached 360 ml was made into a cylinder net in one layer to obtain a separator of Comparative Example 4. The average fiber diameter of the fibrillated cellulose fiber was 5.3 μm, and the average fiber diameter of the fibrillated synthetic fiber was 17.0 μm. The completed separator of Comparative Example 4 had a thickness of 60 μm and a density of 0.460 g / cm 3 The tensile strength after humidity conditioning was 1600 N / m, the tensile strength after heat treatment was 120 N / m, and the tensile strength reduction rate was 93%.

[0080] Comparative Example 5 A raw material containing 30% by mass of fibrillated cellulose fiber beaten using esparto fiber until the CSF value reached 120 ml, and 70% by mass of fibrillated synthetic fiber beaten using synthetic fiber 6 until the CSF value reached 150 ml was made into a cylinder net in one layer to obtain a separator of Comparative Example 5. The average fiber diameter of the fibrillated cellulose fiber was 9.6 μm, and the average fiber diameter of the fibrillated synthetic fiber was 18.0 μm. The completed separator of Comparative Example 5 had a thickness of 40 μm and a density of 0.290 g / cm 3 The tensile strength after humidity conditioning was 530 N / m, the tensile strength after heat treatment was 20 N / m, and the tensile strength reduction rate was 96%. The separator of Comparative Example 5 had wrinkles after heat treatment.

[0081] [Conventional Example 1] A separator was produced by referring to the method described in Example 1 of Patent Document 1, and used as Conventional Example 1. Specifically, softwood pulp treated with a double disc refiner and a mass colloider was applied to a PET film using an applicator while containing a glycol ether-based pore-opening material and a hydrophilic polymer binder, and then dried and peeled off from the PET film to obtain the separator of Conventional Example 1. In the separator of Conventional Example 1, the average fiber diameter of the fibrillated cellulose fibers was unmeasurable. The separator of Conventional Example 1 obtained in this manner had a thickness of 30 μm and a density of 0.356 g / cm 3 The tensile strength after humidity conditioning was 2400 N / m, the tensile strength after heat treatment was 130 N / m, and the tensile strength reduction rate was 95%.

[0082] [Conventional Example 2] A separator was produced by referring to the method described in Example 8 of Patent Document 2, and used as Conventional Example 2. Specifically, a raw material containing 45% by mass of fibrillated cellulose fiber beaten using Manila hemp fiber until the CSF value reached 350 ml, 50% by mass of fibrillated synthetic fiber beaten using synthetic fiber 1 until the CSF value reached 0 ml, and 5% by mass of polyvinyl alcohol binder fiber was made into a single layer using a cylinder net to obtain a separator of Conventional Example 2. The average fiber diameter of the fibrillated cellulose fiber was 14.1 μm, and the average fiber diameter of the fibrillated synthetic fiber was 11.2 μm. The completed separator of Conventional Example 2 had a thickness of 50 μm and a density of 0.470 g / cm 3 The tensile strength after humidity conditioning was 1750 N / m, the tensile strength after heat treatment was 140 N / m, and the tensile strength reduction rate was 92%.

[0083] [Conventional Example 3] A raw material containing 70% by mass of non-fibrillated cellulose fiber made of bamboo fiber with a CSF value of 710 ml and 30% by mass of fibrillated synthetic fiber beaten using synthetic fiber 3 until the CSF value reached 600 ml was made into a single layer using a cylinder net to obtain a separator of Conventional Example 3. The average fiber diameter of the non-fibrillated cellulose fiber was 12.7 μm, and the average fiber diameter of the fibrillated synthetic fiber was 20.9 μm. The completed separator of Conventional Example 3 had a thickness of 40 μm and a density of 0.260 g / cm 3 The tensile strength after humidity conditioning was 320 N / m, the tensile strength after heat treatment was 20 N / m, and the tensile strength reduction rate was 94%.

[0084] [Conventional Example 4] A raw material containing 30% by mass of fibrillated cellulose fiber, which was beaten using jute fiber until the CSF value reached 190 ml, and 70% by mass of non-fibrillated synthetic fiber consisting of synthetic fiber 4, was made into a single layer using a cylinder net to obtain a separator of Conventional Example 4. The average fiber diameter of the fibrillated cellulose fiber was 11.0 μm, and the average fiber diameter of the fibrillated synthetic fiber was 23.5 μm. The completed separator of Conventional Example 4 had a thickness of 40 μm and a density of 0.340 g / cm 3 The tensile strength after humidity conditioning was 320 N / m, the tensile strength after heat treatment was 30 N / m, and the tensile strength reduction rate was 91%.

[0085] As aluminum electrolytic capacitors produced using the separators of each of the above Examples, Comparative Examples, and Conventional Examples, a low-voltage solid electrolytic capacitor with a rated voltage of 6.3 V and a high-voltage solid electrolytic capacitor with a rated voltage of 50 V were produced. In addition, as hybrid electrolytic capacitors, a low-voltage capacitor with a rated voltage of 16 V and a high-voltage capacitor with a rated voltage of 80 V were produced. Note that the separators of Comparative Example 3, Conventional Example 3, and Conventional Example 4 were broken during winding of the element, and the element could not be wound, so the characteristics of the capacitors using these separators were not measured.

[0086] For each capacitor, the initial ESR, the rate of short circuit defects after reflow soldering, and the rate of ESR increase after a high-temperature load test were measured.

[0087] Table 2 shows the raw materials and compositions of the separators of each Example, Comparative Example, and Conventional Example, and the evaluation results of each separator alone. Tables 3 and 4 show the performance evaluation results of the conductive polymer capacitors using the separators of each Example, Comparative Example, and Conventional Example.

[0088] [Table 2]

[0089] [Table 3]

[0090] [Table 4]

[0091] The separator properties of each Example, Comparative Example, and Conventional Example, and the evaluation results of the conductive polymer capacitor using each separator are described in detail below. In the following description, the short circuit defect rate after reflow soldering is referred to as the "short circuit defect rate," and the ESR increase rate after the high temperature load test is referred to as the "ESR increase rate."

[0092] The capacitors using the separators of Examples 1 to 7 had a lower short circuit failure rate and a lower ESR increase rate than the capacitors using the separators of each of the comparative examples and conventional examples. The reason why the short circuit failure rate and ESR increase rate of the capacitors using the separators of Examples 1 to 7 were low is thought to be because the tensile strength reduction rate was 17 to 89%, which is lower than the comparative examples and conventional examples, and changes such as fiber decomposition and melting due to heat treatment were suppressed. This shows that the heat resistance of conductive polymer capacitors can be improved by keeping the tensile strength reduction rate of the separator to 90% or less.

[0093] The separators of Example 1 and Example 4 to Example 7 had a lower short circuit defect rate than the capacitors using the separators of Example 2 and Example 3. The reason why the capacitors using the separators of Example 1 and Example 4 to Example 7 had a low short circuit defect rate is believed to be because the tensile strength reduction rate was low at 17 to 78%, and changes such as fiber decomposition and melting due to heat treatment were further suppressed. This shows that the heat resistance of conductive polymer capacitors can be further improved by keeping the tensile strength reduction rate of the separator to 80% or less. Furthermore, the separators of Examples 1 and 4 to 7 have a higher tensile strength of 210 to 1500 N / m after heat treatment than the separators of Examples 2 and 3. In other words, it is believed that the separator can maintain its shielding properties even when exposed to high temperatures. This shows that the heat resistance of the conductive polymer capacitor can be further improved by making the tensile strength of the separator after heat treatment 200 N / m or more. Furthermore, the separators of Examples 1 and 4 to 7 contain 40 to 60 mass% fibrillated cellulose fibers and 40 to 60 mass% fibrillated synthetic fibers. From the results of Examples 2 and 3 and Examples 1 and 4 to 7, it is found that in order to control the balance of entanglement between the fibrillated cellulose fibers and the fibrillated synthetic fibers, it is preferable to set the content of fibrillated cellulose fibers to 40 to 60 mass% and the content of fibrillated synthetic fibers to 40 to 60 mass%.

[0094] The separator of Example 6 has a low tensile strength reduction rate of 17%, but the tensile strength after humidity conditioning is low at 350 N / m. Therefore, although the element could be wound, the strength is low enough to further improve productivity. On the other hand, the separator of Example 7 has a tensile strength reduction rate of 26% and a tensile strength after humidity conditioning of 810 N / m, which is a higher tensile strength after humidity conditioning than that of Example 6. From this, it is considered that the upper limit of the tensile strength reduction rate is preferably set to 20% in order to obtain not only a tensile strength sufficient for winding the element but also a tensile strength necessary for improving productivity.

[0095] The separator of Comparative Example 1 has the same level of thickness, density, and tensile strength after humidity adjustment as the separator of the Example, but the tensile strength reduction rate is high at 92%, and the capacitor using the separator of Comparative Example 1 has a higher initial ESR, short circuit failure rate, and ESR increase rate than each Example. The short circuit failure rate and ESR increase rate are considered to be high because the tensile strength reduction rate is high at 92% and the tensile strength after heat treatment is also low at 150 N / m, which is caused by excessive changes in the fibers due to exposure to high temperatures. The separator of Comparative Example 1 has a fibrillated synthetic fiber with a small average fiber diameter of 12.0 μm, which is considered to be caused by a poor balance of entanglement between the fibrillated cellulose fiber and the fibrillated synthetic fiber, which is considered to have caused the tensile strength reduction rate and the tensile strength after heat treatment to be low. In addition, it is considered that the small average fiber diameter of the fibrillated synthetic fiber results in a large number of fine fibers, resulting in a high initial ESR. Furthermore, the separator of Comparative Example 1 has a low content of fibrillated synthetic fiber at 20 mass%. This is thought to be one of the reasons why the impregnation of the conductive polymer is easily deteriorated and the initial ESR is low. From the above, it was found that by setting the average fiber diameter of the fibrillated synthetic fibers to 13 μm or more, the balance of entanglement with the fibrillated cellulose fibers is good, and heat resistance during exposure to high temperatures can be improved. In addition, it was found that by setting the content of fibrillated synthetic fibers to 30 mass% or more, that is, the content of fibrillated cellulose fibers to 70 mass% or less, it becomes easier to control the entanglement of the two fibers, and it is easy to reduce the ESR when made into a capacitor while increasing the tensile strength after humidity conditioning.

[0096] The separator of Comparative Example 3 has the same thickness and density as the separator of the Example, but the tensile strength reduction rate is high at 94%, and the tensile strength after heat treatment is also low at 20 N / m. In the separator of Comparative Example 3, the average fiber diameter of the fibrillated synthetic fiber is large at 22.9 μm, so that the entanglement with the cellulose fiber is insufficient, and the distribution of the fibers in the separator is uneven. Therefore, it is considered that the stability when exposed to high temperatures is low. In addition, the separator of Comparative Example 3 has a low tensile strength of 320 N / m after humidity control, and the separator breaks during winding of the element, making it impossible to wind the element. The reason for the low tensile strength after humidity control is considered to be due to insufficient entanglement between the fibrillated cellulose fiber and the fibrillated synthetic fiber, as well as the fact that the blending ratio of the fibrillated synthetic fiber is high at 80 mass%. From the above, it was found that by setting the average fiber diameter of the fibrillated synthetic fibers to 22 μm or less, the balance of entanglement with the fibrillated cellulose fibers is good, and heat resistance during exposure to high temperatures can be improved. In addition, it was found that by setting the content of fibrillated synthetic fibers to 70 mass% or less, that is, the content of fibrillated cellulose fibers to 30 mass% or more, it becomes easier to control the entanglement of the two fibers, and it is easy to reduce the ESR when made into a capacitor while increasing the tensile strength after humidity conditioning.

[0097] The separator of Comparative Example 2 has the same thickness and density as the separator of the Example, but the tensile strength reduction rate is high at 92%, and the tensile strength after heat treatment is low at 40 N / m. The capacitor using the separator of Comparative Example 2 has the same initial ESR as the examples, but the short circuit failure rate and ESR increase rate are high. The short circuit failure rate and ESR increase rate are high because the tensile strength reduction rate is high at 92% and the tensile strength after heat treatment is low at 40 N / m, and excessive changes such as thermal decomposition and melting occur in the fibers due to exposure to high temperatures. The poor tensile strength reduction rate and tensile strength after heat treatment are likely due to the average fiber diameter of the fibrillated cellulose fibers being thicker at 12.8 μm than the examples, and the balance of entanglement between the fibrillated cellulose fibers and the fibrillated synthetic fibers being poor. In addition, although the element could be wound, the tensile strength after humidity adjustment was low at 500 N / m compared to the examples. From the above, it can be seen that by making the average fiber diameter of the fibrillated cellulose fibers 12 μm or less, a good balance of entanglement with the fibrillated synthetic fibers is achieved, thereby improving the tensile strength after humidity conditioning and the heat resistance when exposed to high temperatures.

[0098] The separator of Comparative Example 4 has the same thickness and density as the separator of the Examples, but the tensile strength reduction rate is high at 93%, and the tensile strength after heat treatment is low at 120 N / m. The capacitor using the separator of Comparative Example 4 has a higher initial ESR, short circuit failure rate, and ESR increase rate than the other Examples. The short circuit failure rate and ESR increase rate are considered to be high because the tensile strength reduction rate is high at 91% and the tensile strength after heat treatment is low at 120 N / m, which is considered to be the reason for the excessive changes in the fibers due to exposure to high temperatures. The separator of Comparative Example 4 has a smaller average fiber diameter of 5.3 μm than the Examples, which is considered to be due to the poor balance of entanglement between the fibrillated cellulose fibers and the fibrillated synthetic fibers, which is considered to have resulted in the lower tensile strength reduction rate and tensile strength after heat treatment. In addition, it is considered that the smaller average fiber diameter of the fibrillated cellulose fibers results in a larger number of fine fibers, which results in a higher initial ESR. From the above, it can be seen that by making the average fiber diameter of the fibrillated cellulose fiber 6μm or more, the balance of entanglement with the fibrillated synthetic fiber is improved, and the heat resistance when exposed to high temperatures can be improved. Furthermore, it can be seen that it is easy to reduce the ESR when used as a capacitor.

[0099] The separator of Comparative Example 5 has the same level of thickness, density, and tensile strength after humidity conditioning as the separator of the Examples, but contains fibrillated acrylic fiber as the fibrillated synthetic fiber. The capacitor using the separator of Comparative Example 5 has a higher short circuit defect rate and ESR increase rate than the other Examples. The high short circuit defect rate and ESR increase rate are thought to be due to the inclusion of acrylic fiber, which has low stability at high temperatures, as the fibrillated synthetic fiber. As a result, the tensile strength reduction rate was high at 96%, and it is thought that wrinkles were generated in the separator after heat treatment. From the above, it is understood that the fibrillated synthetic fibers must contain aramid fibers, which are wholly aromatic polyamide fibers, or polyarylate fibers, which are wholly aromatic polyester fibers.

[0100] The separator of Conventional Example 1 has the same level of thickness, density, and tensile strength after humidity conditioning as the Examples, but the capacitor using the separator of Conventional Example 1 had a high initial ESR, short circuit failure rate, and ESR increase rate. The short circuit failure rate and ESR increase rate are considered to be high because the separator is composed only of fibrillated cellulose fibers, and the thermal decomposition of the fibers cannot be suppressed. Furthermore, the initial ESR of the capacitor using the separator of Conventional Example 1 is considered to be high because the separator of Conventional Example 1 is composed only of fibrillated cellulose fibers, and the fibers are beaten to an extent that the average fiber diameter cannot be measured. This shows that a separator consisting only of fibrillated cellulose fibers cannot improve the heat resistance of a conductive polymer capacitor, but that the heat resistance of a conductive polymer capacitor can be improved by containing both fibrillated cellulose fibers and fibrillated synthetic fibers.

[0101] The separator of Conventional Example 2 had the same level of thickness, density, and tensile strength after humidity adjustment as the Example, but the capacitor using the separator of Conventional Example 2 had a high short-circuit defect rate and ESR increase rate. The high short-circuit defect rate and ESR increase rate of the capacitor using the separator of Conventional Example 2 is thought to be due to the inclusion of polyvinyl alcohol binder. Binder fibers such as polyvinyl alcohol may melt or decompose at a lower temperature than the main fiber. Therefore, it is difficult to suppress changes such as thermal decomposition and melting of the fibers in a separator using binder fibers. This shows that it is better not to include binder fibers in the separator. Furthermore, the separator of Conventional Example 2 contains only Manila hemp fiber as the fibrillated cellulose fiber, and has a larger average fiber diameter than the Examples. Since Manila hemp fiber is also long, when used alone, it is likely to have a non-uniform fiber distribution when combined with fibrillated synthetic fiber. From the results of Conventional Example 2 and Examples 2 and 5, it can be seen that when Manila hemp fiber is used, by combining it with a fiber with a small fiber diameter, the fiber distribution becomes uniform even when combined with fibrillated synthetic fiber, and a separator with improved heat resistance can be obtained.

[0102] The separators of Conventional Examples 3 and 4 had the same levels of thickness and density as those of the Examples, but had low tensile strength after humidity conditioning, and the separator broke when winding the element, making it impossible to wind the element. The reason for the low tensile strength after humidity conditioning is believed to be that the separators of Conventional Examples 3 and 4 consist of non-fibrillated fibers and fibrillated fibers. Since the non-fibrillated fibers do not have fibrils, they are unlikely to entangle with the fibrillated fibers, and it is believed that the tensile strength after humidity conditioning is reduced. Furthermore, the non-fibrillated fibers have a larger average fiber diameter than those of the Examples, and are therefore unlikely to entangle with the fibrillated fibers. From a comparison of Conventional Examples 3 and 4 with each of the Examples, it is apparent that it is preferable for the separator to be made of fibrillated cellulose fibers and fibrillated synthetic fibers.

[0103] As described above, according to the present embodiment, it is possible to provide a separator for an aluminum electrolytic capacitor, which is made of fibrillated cellulose fibers and fibrillated synthetic fibers and has stability against long-term exposure to high temperatures and against short-term and rapid exposure to high temperatures. Furthermore, by using this separator, it is possible to provide an aluminum electrolytic capacitor with a low short-circuit defect rate and a suppressed increase in ESR even after exposure to high temperatures.

Claims

1. A separator for an aluminum electrolytic capacitor, the separator being interposed between a pair of electrodes and used in an aluminum electrolytic capacitor having a conductive polymer as a cathode material, the separator comprising fibrillated cellulose fibers and fibrillated synthetic fibers, the content of the fibrillated cellulose fibers in the entire separator being 40 to 60 mass %, the content of the fibrillated synthetic fibers being 40 to 60 mass %, the separator comprising fibers having an average fiber diameter of 6 to 12 μm as the fibrillated cellulose fibers and fibers having an average fiber diameter of 13 to 22 μm as the fibrillated synthetic fibers, and a tensile strength reduction rate of 10 to 80%, as expressed by the following formula (1), using the tensile strength after humidity conditioning at 20°C and 65% RH for 30 minutes and the tensile strength after heat treatment at 270°C for 20 minutes: Formula (1): (X1-X2) / X1×100 X1: Tensile strength after conditioning at 20°C and 65% RH for 30 minutes X2: Tensile strength after heat treatment at 270°C for 20 minutes

2. 2. The separator for an aluminum electrolytic capacitor according to claim 1, wherein the rate of decrease in tensile strength is 20 to 80%.

3. 3. The separator for an aluminum electrolytic capacitor according to claim 1, wherein the separator has a tensile strength of 160 to 1600 N / m after heat treatment at 270° C. for 20 minutes.

4. 4. The separator for an aluminum electrolytic capacitor according to claim 1, wherein the separator contains, as the fibrillated synthetic fibers, at least one type of fiber selected from the group consisting of wholly aromatic polyamide and wholly aromatic polyester.

5. An aluminum electrolytic capacitor, comprising the separator for an aluminum electrolytic capacitor according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Separator sheet for alkaline battery and alkaline battery

    JP2006004844A

  • Separator for electronic components

    JP2006245550A

  • Separator for electric capacitor

    JP2014072361A

  • Microporous film, method for producing the same, and electrochemical element

    JP2017119941A

  • Separator for solid or hybrid electrolytic capacitor, and solid or hybrid electrolytic capacitor

    JP2019176073A