Magnetoresistance element, magnetic memory, and method of manufacturing magnetoresistance element

JP7555200B2Active Publication Date: 2024-09-24SAMSUNG ELECTRONICS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020097602
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-04
Publication Date
2024-09-24
Estimated Expiration
2040-06-04

AI Technical Summary

Benefits of technology

【0025】 本発明の磁気抵抗素子,磁気メモリ及び磁気抵抗素子の製造方法によれば,SOT層において書き込み電流を流すのに支障の無い厚さが確保されるとともに,オーバーエッチングによる金属の再堆積に起因するMTJのトンネルバリアのショートパス形成,及びMTJ形状が裾引き形状となることを抑制できる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555200000005
    Figure 0007555200000005
  • Figure 0007555200000004
    Figure 0007555200000004
  • Figure 0007555200000006
    Figure 0007555200000006
Patent Text Reader

Abstract

To secure such a thickness as to eliminate trouble in write current flowing in an SOT layer, and prevent a short path of a tunnel barrier from being formed and an MTJ shape from being trailed by re-deposition of a metal caused by over etching.SOLUTION: In a magnetoresistive element 100, an SOT electrode layer 102, an interface layer 103, a first magnetic layer 104, a first non-magnetic layer 105 and a second magnetic layer 106 are laminated successively. An etching stop layer 107 is further included for covering a portion where the first magnetic layer 104, the first non-magnetic layer 105 and the second magnetic layer 106 are not laminated, in one face of the SOT electrode layer 102. In the interface layer 103, a spin diffusion length is equal to or greater than a thickness of the interface layer 103, and the interface layer contains a metal of which the etch rate is reduced by a composition of at least one of the first magnetic layer 104, the first non-magnetic layer 105 and the second magnetic layer 106 by being oxidized or nitrided. The etching stop layer 107 contains an oxide or a nitride of the metal.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetoresistive element, a magnetic memory, and a method for manufacturing a magnetoresistive element. [Background technology]

[0002] Spin Transfer Torque - Magnetoresistive Random Access Memory (STT-MRAM), which is currently being widely researched and developed, is a type of MRAM that uses a two-terminal structure to perform write and read operations on magnetic tunnel junction (MTJ) elements. Due to this two-terminal structure, STT-MRAM has problems such as insufficient read margin when highly integrated, and insufficient write endurance. As a method that can solve these problems and enable high-speed and low-power writing, a three-terminal structure spin orbit torque - magnetoresistive random access memory (SOT-MRAM) that uses the spin Hall effect (SHE) to generate spin current from electric current and writes data is attracting attention.

[0003] For example, Non-Patent Document 1 describes the problem of etching damage to the SOT electrode layer during etching of the MTJ of SOT-MRAM and a technique for solving the problem.

[0004] This non-patent document 1 describes a method for reducing the etching damage of a thin SOT electrode layer by using highly selective etching (HSE) in the processing of an MTJ with a thin SOT electrode layer. In a normal etching process, the initial film thickness of the SOT electrode layer, 10 nm, is reduced to 6.8 nm due to etching damage. On the other hand, in the improved HSE process, the film thickness after etching remains at 8.9 nm, suppressing the etching damage to about 1 nm. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Y. Ohsawa et al., IEEE J. Electron Device Soc. 6 (2018) 1233. Summary of the Invention [Problem to be solved by the invention]

[0006] However, in an actual element, the thickness of the SOT electrode layer is about 5 nm, so that even etching damage of about 1 nm has a large effect on the SOT effect.

[0007] In addition, because the spin diffusion length is short in the SOT electrode layer, making the SOT electrode layer thicker than necessary in order to avoid the effects of etching damage would undesirably increase the operating current without increasing the SOT effect.

[0008] Furthermore, the spin Hall angle θ, which represents the efficiency of conversion from electric current to spin current, SH Pt is known to be a material with a large resistance, but when Pt is used as the SOT electrode layer and MTJ processing is performed, over-etching of the Pt layer causes redeposition of Pt on the sidewalls of the MTJ. At this time, there is a problem that the redeposited Pt on the sidewalls becomes a short path for the tunnel barrier of the MTJ, significantly degrading the tunneling magnetoresistance (TMR) characteristics of the MTJ.

[0009] Furthermore, since MTJ elements are made of materials that are difficult to etch, including magnetic materials, it is difficult to etch them well using conventional reactive ion etching (RIE). Even now, dry etching methods that use tilt and rotation, such as Ar ion beam etching (IBE), are used for MTJ elements. In this case, if the etching selectivity between the etching stop layer and the MTJ is not large enough, the MTJ shape will have a tail shape, which causes problems when fabricating small elements.

[0010] The objective of the present invention is to provide a magnetoresistive element, a magnetic memory, and a method for manufacturing a magnetoresistive element that ensures a thickness in the SOT layer that does not interfere with the flow of write current, and that can suppress the formation of a short path in the tunnel barrier of an MTJ caused by metal redeposition due to over-etching, and the formation of a footing shape in the MTJ shape. [Means for solving the problem]

[0011] In one embodiment, the magnetoresistance element has an SOT electrode layer, an interface layer, a first magnetic layer, a first non-magnetic layer, and a second magnetic layer stacked in that order, and further includes an etching stop layer formed by oxidizing or nitriding the interface layer, covering portions of one surface of the SOT electrode layer from which the first magnetic layer, the first non-magnetic layer, and the second magnetic layer have been removed, the interface layer having a spin diffusion length equal to or greater than the thickness of the interface layer and comprising a metal which, upon being oxidized or nitrided, has an etch rate lower than the composition of at least one of the first magnetic layer, the first non-magnetic layer, and the second magnetic layer, and the etching stop layer comprises an oxide or nitride of the metal.

[0012] In one embodiment of the magnetoresistive element, the interface layer may contain, in atomic composition ratio, 90% or more of a metal having a spin diffusion length equal to or greater than the thickness of the interface layer, and the etching stop layer may contain, in atomic composition ratio, 90% or more of an oxide or nitride of the metal.

[0013] According to the magnetoresistance element of one embodiment of this invention, a thickness that does not impede the flow of write current in the SOT layer is ensured, and the formation of a short path in the MTJ tunnel barrier caused by metal redeposition due to over-etching and the formation of a footing shape in the MTJ shape can be suppressed.

[0014] In one embodiment of the magnetoresistance element, the interface layer may contain a metal whose spin diffusion length is five times or more the thickness of the interface layer.

[0015] According to one embodiment of the magnetoresistive element, the spin signal is e -0.2 = The reduction can be limited to 0.82 times.

[0016] In one embodiment of the magnetoresistance element, the metal may be any of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, Ta, or a mixture of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta.

[0017] In one embodiment of the magnetoresistance element, the SOT electrode layer may be made of a material that produces the spin Hall effect as a bulk.

[0018] According to the magnetoresistance element of one embodiment, problems that were encountered during MTJ etching processing, such as damage to the SOT electrode layer, degradation of the TMR characteristics of the MTJ due to redeposition of the SOT electrode layer, and tailing of the MTJ shape, can be solved. Also, SOT-MRAM with a fine element structure can be manufactured with good yield.

[0019] In one embodiment of the magnetoresistance element, the SOT electrode layer may be made of a material that is a magnetic material and generates a spin current or accumulates a spin current at the interface with the adjacent interface layer.

[0020] According to the magnetoresistance element of one embodiment, damage to the SOT electrode layer during the etching process of the MTJ can be suppressed, and the spin current generated in the SOT electrode layer can be effectively injected into the first magnetic layer, which is the recording layer. In addition, the problem of redeposition on the MTJ sidewall during the MTJ etching process and the problem of tailing of the MTJ shape can be solved by using a Ti interface layer and Ar + O 2 This can be solved by using the IBE method.

[0021] The magnetic memory of one embodiment includes any one of the above-mentioned magnetoresistance elements, a first electrode and a second electrode connected to the SOT electrode layer, and a third electrode connected to the second magnetic layer.

[0022] According to the magnetic memory of one embodiment, it is possible to provide a magnetic memory in which a thickness that does not impede the flow of a write current in the SOT layer is ensured.

[0023] A manufacturing method of a magnetoresistive element in one embodiment includes a lamination process of sequentially laminating an SOT electrode layer, an interface layer, a first magnetic layer, a first non-magnetic layer, and a second magnetic layer, a mask formation process of forming a mask layer corresponding to a desired MTJ element on the second magnetic layer, and an etching process of performing etching using an etching gas containing nitrogen or oxygen and oxidizing or nitriding the unmasked interface layer to form an etching stop layer, wherein the interface layer contains a metal whose spin diffusion length is equal to or greater than the thickness of the interface layer and whose etch rate is lower when oxidized or nitridized than the composition of at least one of the layers of the first magnetic layer, the first non-magnetic layer, and the second magnetic layer.

[0024] The manufacturing method of the magnetoresistive element according to one embodiment can suppress etching damage, short paths in the tunnel barrier of the MTJ caused by overetching, and the MTJ shape becoming a footing shape. Effect of the Invention

[0025] According to the magnetoresistive element, magnetic memory, and magnetoresistive element manufacturing method of the present invention, a thickness that does not interfere with the flow of write current in the SOT layer is ensured, and the formation of a short path in the MTJ tunnel barrier caused by metal redeposition due to over-etching and the formation of a footing shape in the MTJ shape can be suppressed. [Brief description of the drawings]

[0026] [Figure 1] 1 is a perspective view showing a schematic configuration of a magnetoresistance element according to a first embodiment. [Diagram 2] 4 is a flowchart showing a method for manufacturing the magnetoresistive element according to the first embodiment. [Diagram 3] FIG. 2 is a perspective view of a step S201 of the method for manufacturing the magnetoresistive element according to the first embodiment. [Figure 4] FIG. 2 is a perspective view of a step S202 of the method for manufacturing the magnetoresistive element according to the first embodiment. [Diagram 5] 1 is a perspective view at step S203 of the manufacturing method of the magnetoresistive element according to the first embodiment. FIG. [Figure 6] FIG. 1 is a perspective view showing a schematic configuration of a conventional magnetoresistance element. [Figure 7] FIG. 11 is a perspective view showing a schematic configuration of a magnetoresistance element according to a fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] (Embodiment 1) Hereinafter, embodiments of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view showing a schematic configuration of a magnetoresistance element according to embodiment 1. In Fig. 1, the magnetoresistance element 100 includes an SOT electrode layer 102, an interface layer 103, a first magnetic layer 104, a first non-magnetic layer 105, a second magnetic layer 106, and an etching stop layer 107.

[0028] The SOT electrode layer 102 controls the magnetization direction of the first magnetic layer 104 by passing a current through it. The SOT electrode layer 102 can reverse the magnetization direction of the first magnetic layer 104 depending on the direction of the current flow. The SOT electrode layer 102 is also called a channel layer. The SOT electrode layer 102 may be made of a material that generates the spin Hall effect as a bulk. The SOT electrode layer 102 may also be made of a material that is a magnetic material and generates a spin current or spin accumulation at the interface with the adjacent interface layer 103.

[0029] The interface layer 103 is a layer containing a metal whose spin diffusion length is longer than the thickness of the interface layer 103. It is desirable that the oxide or nitride of the metal contained in the interface layer 103 has a lower etch rate than the composition (e.g., Co or Fe) of at least one of the layers of the first magnetic layer 104, the first non-magnetic layer 105, and the second magnetic layer 106 constituting the MTJ. For example, the metal contained in this interface layer 103 is preferably any one of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta, or a mixture of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta. It is preferable that the interface layer 103 contains this metal in an atomic composition ratio of 90% or more. The remaining atomic composition ratio of less than 10% may be an alloy to which other elements are added.

[0030] Furthermore, it is more preferable that the interface layer 103 is a layer containing a metal whose spin diffusion length is longer than five times the thickness of the interface layer 103. When the spin diffusion length is approximately the same as the thickness of the interface layer, the spin signal passes through the interface layer 103. -1 On the other hand, when the spin diffusion length is 5 times the thickness of the interface layer, the spin signal decreases by e -0.2 = Only a 0.82x decrease.

[0031] The first magnetic layer 104 is a layer made of a magnetic material. The first magnetic layer 104 functions as a free layer (also called a recording layer) of the SOT-MARM. In other words, information is stored according to the magnetization direction of the first magnetic layer 104.

[0032] The first nonmagnetic layer 105 is a layer made of a nonmagnetic material. The first nonmagnetic layer 105 functions as a tunnel barrier.

[0033] The second magnetic layer 106 is a layer made of a magnetic material. The second magnetic layer 106 functions as a reference layer (also called a fixed layer) of the SOT-MARM. Since the magnetization direction of the second magnetic layer 106 is constant, the read current differs depending on whether the magnetization direction of the first magnetic layer 104 and the magnetization direction of the second magnetic layer 106 are the same or opposite to each other.

[0034] The etching stop layer 107 is a layer containing an oxide or nitride of the metal contained in the interface layer 103. For example, this metal is preferably an oxide of any of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta, or a mixture of oxides of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta. The etching stop layer 107 preferably contains 90% or more of this metal oxide or nitride in atomic composition ratio. The remaining 10% or less in atomic composition ratio may be a compound to which other elements (or oxides or nitrides of other elements) have been added.

[0035] Next, a method for manufacturing the magnetoresistance element 100 will be described with reference to Figs. 2 to 5. Fig. 2 is a flowchart showing a method for manufacturing the magnetoresistance element according to the first embodiment. Fig. 3 is a perspective view showing step S201 of the method for manufacturing the magnetoresistance element according to the first embodiment. Fig. 4 is a perspective view showing step S202 of the method for manufacturing the magnetoresistance element according to the first embodiment. Fig. 5 is a perspective view showing step S203 of the method for manufacturing the magnetoresistance element according to the first embodiment.

[0036] First, in step S201, the SOT electrode layer 102, the interface layer 103, the first magnetic layer 104, the first non-magnetic layer 105, and the second magnetic layer 106 are laminated in this order. The state in which each layer is laminated is shown in Fig. 3. Then, the process proceeds to step S202.

[0037] In step S202, a mask layer 401 corresponding to a desired MTJ element is formed on the second magnetic layer 106. The masked state is shown in Fig. 4. Then, the process proceeds to step S203. The mask layer 401 is formed in a required shape by patterning using, for example, photolithography or the like.

[0038] In step S203, the entire MTJ layer is etched using the mask layer 401. This etching removes the first magnetic layer 104, the first non-magnetic layer 105, and the second magnetic layer 106 in the unmasked portions. In this etching, it is preferable to use a mixed gas of Ar and oxygen or nitrogen. As a result, the interface layer 103 in the unmasked portions is oxidized or nitrided to form an etching stop layer 107. This etching stop layer 107 prevents the SOT electrode layer 102 in the unmasked portions from being over-etched. This etching stop layer 107 contains an oxide obtained by oxidizing a metal contained in the interface layer 103 or a nitride obtained by nitriding the metal. This oxide or nitride has a lower etch rate than the composition of at least one layer of the first magnetic layer 104, the first non-magnetic layer 105, and the second magnetic layer 106. In the structure of the MTJ, more functional layers are generally stacked on the second magnetic layer 106. In that case, in the stage of etching the layers above the second magnetic layer 106, it is preferable to perform IBE using only Ar that does not contain oxygen or nitrogen. Thereafter, in the stage of etching the second magnetic layer 106, the first non-magnetic layer 105, and the first magnetic layer 104, it is preferable to perform etching using a mixed gas of Ar and oxygen or nitrogen. In addition, when etching the entire MTJ layer by RIE, the etching gas may be switched from one that does not contain oxygen or nitrogen to one that contains oxygen and nitrogen in the stage of etching the layer below the second magnetic layer 106, as in the case of IBE. Furthermore, when etching the entire MTJ layer by RIE, etching may be performed from the beginning using an etching gas that contains oxygen or nitrogen.

[0039] Therefore, the MTJ shape including the first magnetic layer, the first non-magnetic layer, and the second magnetic layer is formed into a substantially vertical shape as shown in Fig. 5. In addition, since the etching stop layer 107 is formed on the surface of the SOT electrode layer 102, redeposition of the metal of the SOT electrode layer 102 into the MTJ shape by etching is also suppressed.

[0040] In the conventional magnetoresistance element, the absence of this etching stop layer 107 caused various problems during etching of the MTJ. FIG. 6 is a perspective view showing a schematic configuration of a conventional magnetoresistance element. First, in the etching of the MTJ, ideally, the etching should be stopped at the interface between the MTJ and the SOT layer, but in reality, some over-etching is necessary in terms of the non-uniformity of the etching in the surface and the acquisition of an etching stop signal. In this case, if the etching stop layer 107 is not present, an etching damage layer 601 is formed on the upper surface of the SOT electrode layer 102. This etching damage layer 601 causes a decrease in the electrical conductivity in the SOT layer and the diffusion of the spin current, which causes deterioration of the element performance of the SOT-MRAM. Furthermore, during the etching of the MTJ, redeposition 602 of the metal contained in the SOT electrode layer 102 due to over-etching occurs on the side wall of the MTJ. In this case, the redeposited metal becomes a short path of the tunnel barrier of the MTJ, which significantly deteriorates the tunnel magnetoresistance characteristics of the MTJ. Furthermore, if the etching stop mechanism does not work sufficiently during over-etching, the shape of the MTJ after etching deteriorates. That is, a skirt shape 603 as shown in FIG. 6 occurs at the bottom of the MTJ, which becomes a problem when fabricating a very small element.

[0041] On the other hand, in the magnetoresistance element of the first embodiment, as described above, the etching stop layer 107 can suppress etching damage to the SOT electrode layer 102 due to overetching, thereby ensuring a thickness that does not interfere with the flow of a write current in the SOT layer. Furthermore, it is possible to suppress the formation of a short path in the tunnel barrier of the MTJ caused by redeposition of metal due to overetching, and the MTJ shape becoming a footing shape.

[0042] Note that a step of removing the mask layer may be added after step S203. Also, in step S201, another layer may be further laminated.

[0043] Furthermore, another layer may be further laminated on the second magnetic layer 106. In the second and third embodiments described below, a form in which another layer is further laminated on the second magnetic layer 106 will be described.

[0044] (Embodiment 2) In the second embodiment, the SOT electrode layer 102 is made of Au. 0.25 Pt 0.75 The SOT-MRAM using an MTJ having a recording layer with perpendicular magnetic anisotropy (PMA) using an alloy is described below. The magnetoresistance element of the second embodiment is obtained by laminating another layer on the magnetoresistance element 100 of the first embodiment. Specifically, the laminated structure of the magnetoresistance element of the second embodiment is SiO 2 On the interlayer insulating film such as Ta(1) / Au 0.25 Pt 0.75 (4) / Ti(2) / CoFeB(1) / MgO(1) / CoFeB(1.4) / Ta(0.3) / PMA multilayer / Ru(0.9) / PMA multilayer / Cap layer / Hard mask layer (thickness in nm) was deposited using a sputtering device. Here, Au 0.25 Pt 0.75 (4) layer acts as the SOT electrode layer 102, and the spin-Hall angle θ SH Since it has a very large spin current, it is a highly efficient source of spin current.

number

[0045] The Ta(1) layer is Au 0.25 Pt 0.75 (4) This is due to the adhesion and uniformity of the layer, and because of its high resistivity, almost no current flows through it, making it almost unhelpful in generating spin current.

[0046] As described below, the Ti(2) layer serving as the interface layer 103 is a material that, while it is oxidized outside the MTJ pillar and acts as an etching stop layer 107, inside the MTJ it does not hinder the flow of spin current from the SOT electrode layer 102 into the MTJ.

[0047] The stacked layer above the CoFeB(1) layer is an MTJ with a PMA, and the CoFeB(1) layer acts as a recording layer.

[0048] The method for forming the element structure is explained below. First, a mask layer in the shape of an MTJ is formed using resist on a hard mask layer. Next, the hard mask layer is processed by dry etching such as RIE.

[0049] Next, using this hard mask layer, the MTJ is processed into a pillar shape by dry etching such as IBE. In this MTJ etching, IBE is performed using only Ar gas until the Ta(0.3) layer is etched away. Then, for the layers below the CoFeB(1.4) layer, IBE is performed using Ar gas with a small amount of O. 2 The etching is stopped halfway through the Ti(2) layer.

[0050] At this time, Ar + O 2 When etching is performed with IBE, Ti is easily converted to TiO X The etch rate of TiO2 formed during etching is approximately 1 / 5 of that of Co and Fe. X This serves as an excellent etching stop layer, making it possible to suppress damage to the SOT electrode layer 102 during etching of the MTJ, which was a problem in the conventional technology.

[0051] On the other hand, the Ti(2) layer at the bottom of the MTJ is Ar + O 2 Since it is not exposed to gas ions, it remains Ti. Here, the spin diffusion length of Ti is sufficiently long at about 13 nm, and since the spin transmittance is improved by the insertion of Ti, the spin current generated in the SOT electrode layer 102 can be effectively injected into the CoFeB recording layer.

[0052] In addition, TiO X Even if the etching stop layer 107 adheres to the MTJ sidewall as a redeposition during etching, it will not adhere to the TiO X Since the MTJ has insulating properties, it does not form a short path in the MTJ. Therefore, it is possible to suppress the degradation of the TMR characteristics due to redeposition on the sidewall, which was one of the problems during MTJ etching.

[0053] Furthermore, TiO X The resulting etching stop layer 107 has an etching selectivity of 1 / 5 with respect to the MTJ, and is therefore fully resistant to over-etching. In other words, the footing of the MTJ shape, which was one of the problems when etching the MTJ, can be removed by over-etching. As a result, a good element shape can be formed, enabling uniform and stable element operation.

[0054] Thus, according to the magnetoresistance element of the second embodiment, by using an interface layer such as Ti, which has a sufficiently long spin diffusion length and high etching resistance during dry etching of the MTJ, it is possible to solve problems that occurred during MTJ etching processing, such as damage to the SOT electrode layer 102, deterioration of the TMR characteristics of the MTJ due to redeposition of the SOT electrode layer 102, and tailing of the MTJ shape. As a result, SOT-MRAM having a fine element structure can be manufactured with good yield.

[0055] (Embodiment 3) In the third embodiment, an SOT-MRAM using CoFeB for the SOT electrode layer 102 and an MTJ having a PMA recording layer will be described. The stacked structure of the magnetoresistive element in the third embodiment is SiO 2On the interlayer insulating film such as those described above, from the bottom, for example, Ta(1) / CoFeB(4) / Ti(3) / CoFeB(1) / MgO(1) / CoFeB(1.4) / Ta(0.3) / PMA multilayer film / Ru(0.9) / PMA multilayer film / Cap layer / hard mask layer (thickness in nm) are formed using a sputtering device. Here, the CoFeB(4) layer serves as the SOT electrode layer 102.

[0056] As described below, the Ti(3) layer serving as the interface layer 103 functions as an etching stop layer 107 outside the MTJ pillar, while inside the MTJ, it is a material that does not impede the flow of spin current from the SOT electrode layer 102 to the MTJ.

[0057] The stacked layers above the CoFeB(1) layer are MTJs with a PMA, and the CoFeB(1) layer acts as a recording layer. Here, in this element, the current is converted to a spin current at the CoFeB(4) / Ti(3) interface, not by the bulk SHE due to the SOT electrode layer 102 of the CoFeB(4) layer.

[0058] The current applied to the SOT electrode layer 102 flows through the CoFeB(4) / Ti(3) interface, but the difference in conductivity between the two materials creates carrier asymmetry, which generates a spin current that flows through the Ti interface layer to the MTJ. At this time, if a ferromagnetic layer such as CoFeB has in-plane magnetization parallel to the current direction, a spin current with a spin polarization perpendicular to the plane is injected into the CoFeB(1) layer, which is the MTJ recording layer.

[0059] Here, in the case of spin current generated by conventional SHE, since it only has in-plane spin polarization, it is necessary to apply an in-plane external magnetic field to reverse the magnetization of the PMA recording layer. However, since the spin current generated by the above mechanism has a perpendicular spin polarization, it is not necessary to apply an external magnetic field, making it a switching method more suitable for the manufacture of SOT-MRAM.

[0060] The method of forming the element structure is the same as in the second embodiment. First, a hard mask layer is processed using a resist mask. Then, the MTJ is processed into a pillar shape by dry etching such as IBE. In this MTJ etching, the layer below the CoFeB(1.4) layer is etched with Ar and a small amount of O 2 The etching is stopped halfway through the Ti(3) layer.

[0061] At this time, Ar + O 2 When etching was performed with IBE, TiO X This makes it possible to suppress damage to the SOT electrode layer 102 during etching of the MTJ, which was a problem in the conventional technology. On the other hand, the Ti(3) layer under the MTJ is formed by Ar + O 2 Since it is not exposed to gas ions, it remains Ti. Here, the spin diffusion length of Ti is sufficiently long at about 13 nm, and since the spin transmittance is improved by the insertion of Ti, the spin current generated in the SOT electrode layer 102 can be effectively injected into the CoFeB recording layer.

[0062] In addition, to address the problem of redeposition on the MTJ sidewall during MTJ etching and the problem of the tailing of the MTJ shape, the Ti interface layer and Ar + O 2 This can be solved by using the IBE method.

[0063] (Embodiment 4) In the fourth embodiment, an example in which the magnetoresistance element of the first embodiment is applied to a magnetic memory will be described. Fig. 7 is a perspective view showing a schematic configuration of the magnetoresistance element according to the fourth embodiment. Fig. 7 shows an example in which the magnetoresistance element is applied to a three-terminal element SOT-MARAM. In Fig. 7, the magnetic memory 700 includes the magnetoresistance element 100, a first electrode 701, a second electrode 702, and a third electrode 703.

[0064] The first electrode 701 is an electrode that is connected to the SOT electrode layer 102. For example, the first electrode 701 is provided at one end of the SOT electrode layer 102.

[0065] The second electrode 702 is an electrode that is connected to the SOT electrode layer 102. For example, the second electrode 702 is provided at the other end of the SOT electrode layer 102. Then, in the path through which a write current flows from the first electrode 701 to the second electrode 702 via the SOT electrode layer 102, by controlling the direction of the current, the magnetization direction of the first magnetic layer 104 is controlled, that is, a write operation to the MTJ is performed.

[0066] The third electrode 703 is an electrode connected to the second magnetic layer 106. The third electrode 703 can detect the magnitude of the resistance of the MTJ and detect the magnetization direction of the first magnetic layer 104 by measuring the current flowing between at least one of the first electrode 701 and the second electrode 702. As described above, the magnetization direction of the first magnetic layer 104 corresponds to the stored information, so that the stored information can be read. In addition, a functional layer or a hard mask as described in the second and third embodiments may be present between the third electrode 703 and the second magnetic layer 106.

[0067] Thus, according to the magnetic memory of embodiment 4, a magnetic memory can be provided in which a thickness that does not interfere with the flow of write current in the SOT layer is ensured, and which can suppress the formation of a short path in the MTJ tunnel barrier caused by metal redeposition due to over-etching, and the MTJ shape from becoming a footing shape.

[0068] The present invention is not limited to the above-described embodiments, and can be modified as appropriate without departing from the spirit and scope of the present invention. For example, the fourth embodiment may be combined with the second or third embodiment. [Explanation of symbols]

[0069] 100 Magnetoresistance element 102 SOT electrode layer 103 Interface layer 104 First magnetic layer 105 First non-magnetic layer 106 Second magnetic layer 107 Etch stop layer 401 Mask Layer 700 Magnetic Memory 701 First electrode 702 Second electrode 703 Third Electrode

Claims

1. an SOT electrode layer, an interface layer, a first magnetic layer, a first non-magnetic layer, and a second magnetic layer are laminated in this order; the SOT electrode layer further includes an etching stop layer formed by oxidizing or nitriding the interface layer, the etching stop layer covering a portion of one surface of the SOT electrode layer from which the first magnetic layer, the first non-magnetic layer, and the second magnetic layer have been removed; the interface layer includes a metal having a spin diffusion length longer than a thickness of the interface layer and having an etch rate lower than a composition of at least one of the first magnetic layer, the first nonmagnetic layer, and the second magnetic layer by being oxidized or nitrided; The etch stop layer comprises an oxide or nitride of the metal.

2. the interface layer contains, in atomic composition ratio, 90% or more of a metal whose spin diffusion length is longer than a thickness of the interface layer; 2. The magnetoresistive element according to claim 1, wherein said etching stop layer contains at least 90% of said metal oxide or nitride in atomic composition ratio.

3. 3. The magnetoresistance element according to claim 1, wherein the interface layer contains a metal whose spin diffusion length is at least five times the thickness of the interface layer.

4. 4. A magnetoresistance element according to claim 1, wherein the metal is any one of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta, or a mixture of Ti, Al, Si, Ge, Cu, Mo, V, Nb, Zn, and Ta.

5. 5. The magnetoresistance element according to claim 1, wherein the SOT electrode layer is made of a material that produces a spin Hall effect as a bulk.

6. 5. The magnetoresistance element according to claim 1, wherein the SOT electrode layer is made of a material that is magnetic and generates or accumulates a spin current at an interface with an adjacent interface layer.

7. 7. A magnetic memory comprising: a magnetoresistive element according to claim 1; a first electrode and a second electrode connected to said SOT electrode layer; and a third electrode connected to said second magnetic layer.

8. a lamination step of laminating an SOT electrode layer, an interface layer, a first magnetic layer, a first non-magnetic layer, and a second magnetic layer in this order; a mask forming step of forming a mask layer having a pattern corresponding to a desired MTJ element shape on the second magnetic layer; and an etching step of etching using an etching gas containing nitrogen or oxygen and oxidizing or nitriding the unmasked interface layer to form an etch stop layer, A method for manufacturing a magnetoresistive element, wherein the interface layer contains a metal that has a spin diffusion length longer than a thickness of the interface layer and that, when oxidized or nitrided, has an etch rate lower than a composition of at least one of the first magnetic layer, the first non-magnetic layer, and the second magnetic layer.

Citation Information

Patent Citations

  • Spin-orbit torque mrams and method for fabricating same

    CN109841726A

  • Magnetic memory

    JP2018022796A

  • Spin current magnetization rotation type magnetic element, spin current magnetization rotation type magnetoresistance effect element and magnetic memory

    JP2020035971A

  • Circuits and devices based on enhanced spin hall effect for efficient spin transfer torque

    KR1020170041749A

  • Magnetic random access memory, and its manufacturing method

    WO2008068967A1