Carbonate-containing epoxy resin, method for preparing the same, cured epoxy product prepared therefrom, and method for decomposing the cured epoxy product
By synthesizing a carbonate-containing epoxy resin through a catalytic reaction of polycarbonate with an epoxy group, the resin achieves chemical degradability and recyclability, addressing the challenges of crosslinked network decomposition and environmental impact.
Patent Information
- Application Number
- JP2022132934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-28
- Filing Date
- 2022-08-24
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2042-08-24
AI Technical Summary
Current epoxy resins face challenges in chemical recyclability due to their crosslinked network structure, making them difficult to decompose and reuse, and their production involves environmental concerns such as the use of phenol and formaldehyde, which limits the recovery of high molecular weight multifunctional epoxies.
A carbonate-containing epoxy resin is synthesized by reacting a polycarbonate or carbonate compound with an epoxy functional group under catalytic conditions, allowing for a curing reaction and subsequent decomposition for recovery and reuse.
The carbonate-containing epoxy resin enables chemical degradability and recyclability, reducing waste and environmental burden while maintaining excellent properties comparable to commercial epoxy resins.
Smart Images

Figure 0007555376000046 
Figure 0007555376000050 
Figure 0007555376000045
Abstract
Description
[Technical Field]
[0001] The present invention relates to an epoxy resin, a method for preparing the same, a cured epoxy product prepared by the same, and a method for decomposing the cured epoxy product, and more particularly to a carbonate-containing epoxy resin, a method for preparing the same, a cured epoxy product prepared by the same, and a method for decomposing the cured epoxy product. [Background technology]
[0002] Currently available epoxy resins are primarily bisphenol A difunctional and novolac multifunctional. Their synthesis involves reacting phenolic groups with epichlorohydrin to form epoxy groups. Multifunctional resins are based on phenolic resins, which require the use of formaldehyde to prepare the phenol, posing environmental concerns and making this method unsuitable for preparing high-molecular-weight multifunctional epoxies. The unique three-membered ring structure of epoxy resins allows for various ring-opening reactions and allows them to self-cure under the influence of a catalyst. However, the chain propagation is relatively difficult, resulting in poor performance of the final homopolymerized cured product. Therefore, epoxy resins must be combined with epoxy resin curing agents to undergo copolymerization reactions to improve the degree of crosslinking after curing. While the cured products currently available on the market have good physical properties, the crosslinked structure makes the products difficult to recover, resulting in a growing waste problem.
[0003] Generally, thermosetting materials have excellent thermal and chemical stability and a dense covalently crosslinked network structure, making them difficult to dissolve, decompose, and recover for reuse. However, the presence of unstable bonds in the crosslinked network can lead to decomposition of the cured product. In recent years, some studies have pointed out that ester groups are chemically degradable and are gradually being used in PET recovery. Therefore, if a similar concept can be introduced into epoxy resins, it is expected that the decomposition of waste materials can be improved and the goal of chemical recycling can be achieved.
[0004] However, since the preparation of ester groups is mainly produced by the reaction of carboxylic acid compounds with phenolic or alcoholic compounds, it is difficult to carry out epoxidation while leaving multifunctional alcohol or phenolic groups in the preparation process. Therefore, there are limitations on the preparation process of derived epoxy resins, and there are no related products to date.
[0005] In view of this, how to synthesize carbonate group-containing epoxy resins and how to make the cured products thereof chemically degradable has become a goal of efforts by those in the related art. Summary of the Invention
[0006] One object of the present invention is to provide a carbonate-containing epoxy resin and a method for preparing the same, which is obtained by reacting a polycarbonate or a carbonate compound with an epoxy functional group molecule under catalytic action to obtain a bifunctional or polyfunctional epoxy resin containing a carbonate group in its structure, and which epoxy resin may be used as is or in a subsequent reaction.
[0007] Another object of the present invention is to provide a cured epoxy product and a method for decomposing the cured epoxy product, which can be prepared by subjecting a carbonate-containing epoxy resin to a curing reaction, and then decomposing the cured epoxy product, thereby recovering and reusing the product and reducing the burden on the environment. [Means for solving the problem]
[0008] One embodiment of the present invention is a compound having the structure shown in formula (I) or formula (II): [ka] R1, R2, R7, and R8 each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; a and b each independently represent an integer of 0 to 4; e and f each independently represent an integer of 0 to 5; X represents a single bond, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an oxygen atom, a sulfur atom, a sulfonyl group, a sulfinyl group, an acyl group, an aryl group having 6 to 12 carbon atoms, a fluorenyl group, or a structure represented by formula (i) or formula (ii); [ka] X1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, Y is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, isocyanurate, or a structure represented by formula (iii) or formula (iv), [ka] R3 and R4 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R5 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, or an alkoxy group having 1 to 6 carbon atoms; R6 is a methylene group, an alkyl group having 5 to 12 carbon atoms, or a cycloalkyl group having 5 to 12 carbon atoms; c and d are each independently an integer of 0 to 4; Z is a single bond, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an oxygen atom, a sulfur atom, a sulfonyl group, a sulfinyl group, an acyl group, an aryl group having 6 to 12 carbon atoms, a fluorenyl group, or a structure represented by formula (i) or (ii); n represents the degree of polymerization, and 1≦n≦500; p is an integer of 1 to 11; q is an integer of 0 to 20; and r is an integer of 1 to 15.
[0009] Another embodiment of the present invention provides a method for preparing a carbonate-containing epoxy resin, comprising the steps of providing an aromatic carbonate group-containing structure having the structure shown in Formula (A1) or Formula (A2); providing an epoxy group-containing structure having the structure shown in Formula (B); and mixing the aromatic carbonate group-containing structure and the epoxy group-containing structure, followed by catalysis to obtain a carbonate-containing epoxy resin having the structure shown in Formula (I) or Formula (II). [ka] [ka] [ka] R1, R2, R7, and R8 each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; a and b each independently represent an integer of 0 to 4; e and f each independently represent an integer of 0 to 5; X represents a single bond, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an oxygen atom, a sulfur atom, a sulfonyl group, a sulfinyl group, an acyl group, an aryl group having 6 to 12 carbon atoms, a fluorenyl group, or a structure represented by formula (i) or formula (ii); [ka] X1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, Y is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, isocyanurate, or a structure represented by formula (iii) or formula (iv), [ka] R3 and R4 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R5 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, or an alkoxy group having 1 to 6 carbon atoms; R6 is a methylene group, an alkyl group having 5 to 12 carbon atoms, or a cycloalkyl group having 5 to 12 carbon atoms; c and d are each independently an integer of 0 to 4; Z is a single bond, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an oxygen atom, a sulfur atom, a sulfonyl group, a sulfinyl group, an acyl group, an aryl group having 6 to 12 carbon atoms, a fluorenyl group, or a structure represented by formula (i) or (ii); n represents the degree of polymerization and is 1≦n≦500; m is an integer of 2 to 12; p is an integer of 1 to 11; q is an integer of 0 to 20; and r is an integer of 1 to 15.
[0010] According to the method for preparing a carbonate-containing epoxy resin described in the preceding paragraph, the catalyst may be selected from the group consisting of 4-dimethylaminopyridine, imidazole, pyridine, 2-methylimidazole, 3-methylimidazole, and 2-ethyl-4-methylimidazole.
[0011] According to the method for preparing a carbonate-containing epoxy resin described in the preceding paragraph, the amount of catalyst added may be 0.1% by weight to 5% by weight of the content of the epoxy group-containing structure.
[0012] According to the method for preparing a carbonate-containing epoxy resin described in the preceding paragraph, the equivalent ratio of the epoxy groups in the epoxy group-containing structure to the carbonate groups in the aromatic carbonate group-containing structure may be 1.3 to 10.0.
[0013] A further embodiment of the present invention provides a cured epoxy product obtained by curing the carbonate-containing epoxy resin.
[0014] According to the epoxy cured product described in the previous paragraph, the curing reaction is completed by mixing the carbonate-containing epoxy resin and the curing agent and heating them.
[0015] According to the epoxy cured product described in the preceding paragraph, the curing agent may be a phenolic resin, an amine compound, an active ester compound, a carboxylic acid compound, a cyanate compound, an isocyanate compound, an acid anhydride compound, benzoxazine, a polycarbonate, or a mixture thereof.
[0016] According to the epoxy cured product described in the previous paragraph, the curing temperature of the curing reaction may be 180°C to 240°C.
[0017] Yet another embodiment of the present invention provides a method for decomposing a cured epoxy material, comprising: providing the cured epoxy material; and reacting the cured epoxy material with an amino group-containing compound so as to decompose the cured epoxy material. [Effects of the Invention]
[0018] Therefore, the carbonate-containing epoxy resin of the present invention is obtained by mixing a carbonate group-containing structure and an epoxy group-containing structure and then catalyzing the mixture. By adding a curing agent, an epoxy cured product with excellent properties is formed, which can be decomposed, recovered, and reused, which is consistent with environmental benefits. [Brief explanation of the drawings]
[0019] For a clearer understanding of the above and other objects, features, advantages and embodiments of the present invention, reference is made to the accompanying drawings, in which: [Figure 1] 1 is a step flow chart illustrating a method for preparing a carbonate-containing epoxy resin according to one embodiment of the present invention. [Figure 2] 1 is a step flowchart illustrating a method for preparing a cured epoxy material according to another embodiment of the present invention. [Figure 3] 1 is a step flowchart illustrating a method for decomposing a cured epoxy material according to a further embodiment of the present invention. [Figure 4] FIG. 1 is a diagram showing a 1H-NMR spectrum according to Example 1. [Figure 5] FIG. 1 shows 1H-NMR spectra according to Examples 2 to 4. [Figure 6] FIG. 1 shows the H-NMR spectrum of Example 19. DETAILED DESCRIPTION OF THE INVENTION
[0020] Each embodiment of the present invention will now be described in more detail. However, the embodiments may be applications of various inventive concepts and may be specifically implemented within a variety of different specific scopes. The specific embodiments are for illustrative purposes only and are not intended to be limiting in scope to the disclosure.
[0021] In the present invention, the structure of a compound may be represented by a skeleton formula, and in this representation, carbon atoms, hydrogen atoms, and carbon-hydrogen bonds may be omitted. If functional groups are clearly depicted in the structural formula, the depicted groups are used as the basis.
[0022] In the present invention, "a carbonate-containing epoxy resin having a structure shown in formula (I)" may be expressed as a carbonate-containing epoxy resin shown in formula (I) or carbonate-containing epoxy resin (I) for the sake of brevity and fluency, and the expression methods for other compounds or groups are inferred from this.
[0023] <Carbonate-containing epoxy resin>
[0024] The present invention relates to a compound having a structure shown in formula (I) or formula (II), [ka] R1, R2, R7, and R8 each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; a and b each independently represent an integer of 0 to 4; e and f each independently represent an integer of 0 to 5; X represents a single bond, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an oxygen atom, a sulfonyl group, a thionyl group, an acyl group, an aryl group having 6 to 12 carbon atoms, a fluorenyl group, or a structure represented by formula (i) or formula (ii); [ka] X1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, Y is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, isocyanurate, or a structure represented by formula (iii) or formula (iv), [ka] R3 and R4 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R5 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, or an alkoxy group having 1 to 6 carbon atoms; R6 is a methylene group, an alkyl group having 5 to 12 carbon atoms, or a cycloalkyl group having 5 to 12 carbon atoms; c and d are each independently an integer of 0 to 4; Z is a single bond, an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, an oxygen atom, a sulfur atom, a sulfonyl group, a sulfinyl group, an acyl group, an aryl group having 6 to 12 carbon atoms, a fluorenyl group, or a structure represented by formula (i) or (ii); n represents the degree of polymerization, and 1≦n≦500; p is an integer of 1 to 11; q is an integer of 0 to 20; and r is an integer of 1 to 15.
[0025] As a result, the carbonate-containing epoxy resin of the present invention has a carbonate structure, and therefore may be used as is or in a subsequent reaction, and the introduction of the carbonate structure improves its decomposability, thereby achieving the purpose of chemical recycling.
[0026] <Method for preparing carbonate-containing epoxy resin>
[0027] Reference is now made to Figure 1, which is a step flow chart illustrating a method 100 for preparing a carbonate-containing epoxy resin according to one embodiment of the present invention. In Figure 1, the method 100 for preparing a carbonate-containing epoxy resin includes steps 110, 120, and 130.
[0028] Step 110 is a step of providing an aromatic carbonate group-containing structure having the structure shown in formula (A1) or formula (A2). [ka] The definitions of R1, R2, R7, R8, X, a, b, e, f, and n refer to the above and will not be repeated here. In detail, the aromatic carbonate group-containing structure may be, but is not limited to, a carbonate compound, a new carbonate plastic, or a recycled polycarbonate material. The recycled polycarbonate material can be recovered from discarded optical discs, thereby reducing the burden on the environment.
[0029] Step 120 is a step of providing an epoxy group-containing structure having the structure shown in formula (B): [ka] The definition of Y is referred to above and will not be repeated here, but m is an integer from 2 to 12.
[0030] Step 130 is a catalytic step of mixing the aromatic carbonate group-containing structure and the epoxy group-containing structure, and then, under the action of a catalyst, obtaining a carbonate-containing epoxy resin having the structure shown in formula (I) or formula (II), [ka] The definitions of R1, R2, R7, R8, X, Y, a, b, e, f, p, and n refer to the above and will not be repeated here. The equivalent ratio of the epoxy groups in the epoxy group-containing structure to the carbonate groups in the aromatic carbonate group-containing structure may be 1.3 to 10.0, and preferably 2.0 to 10.0.
[0031] Specifically, when the aromatic carbonate group-containing structure is the structure shown in formula (A1), the synthesized carbonate-containing epoxy resin has the structure shown in formula (I), and the chemical reaction formula is shown in Table 1 below. [Table 1]
[0032] Furthermore, when the aromatic carbonate group-containing structure is the structure shown in formula (A2), the synthesized carbonate-containing epoxy resin has the structure shown in formula (II), and the chemical reaction formula is shown in Table 2 below. [Table 2]
[0033] The catalyst may contain an unshared electron pair and may be selected from the group consisting of 4-dimethylaminopyridine (DMAP), imidazole, pyridine, 2-methylimidazole, 3-methylimidazole, and 2-ethyl-4-methylimidazole. This allows the unshared electron pair of the catalyst to interact with the epoxy group in the epoxy group-containing structure, contributing to the subsequent curing reaction. Specifically, the amount of the catalyst added may be 0.1% by weight to 5% by weight of the content of the epoxy group-containing structure.
[0034] Specifically, the carbonate-containing epoxy resin of the present invention utilizes the carbonate group in the aromatic carbonate group-containing structure to react with the epoxy group in the epoxy group-containing structure. To demonstrate this concept, a model reaction was first performed according to Synthesis Example 1, in which diphenyl carbonate and bisphenol A epoxy resin (Diglycidyl ether of Bisphenol A, DGEBA) were reacted in the presence of pyridine as a catalyst. Specifically, 1.00 g (9.3 mmol) of diphenyl carbonate (107.1 g / eq) and 3.51 g (18.6 mmol) of bisphenol A epoxy resin (188 g / eq) were placed in a 100 mL three-neck flask, heated to 100°C, and after dissolution was confirmed, 0.0175 g of pyridine catalyst was added and the reaction was continued for 8 hours. Spectroscopic analysis was then performed on the product obtained in Synthesis Example 1, and the hydrogen spectrum data was: 1 H-NMR (CDCl), δ = 1.62 (12H, H d ), 2.73(2H,H a ), 2.88(2H,H a’ ), 3.33(2H,H b ), 3.92(2H,H c ), 4.12(2H,H j ), 4.16(2H,H c’), 4.25(4H,H l ,H l’ ), 4.35(2H,H j’ ), 5.36(2H,H k ), 6.80 (8H,H h ), 6.88(4H,H n ), 6.95 (2H,H p ), 7.12(8H,H g ), 7.27(4H,H o ) and the carbon spectrum data is 13 C-NMR (CDCl3), δ = 31.0 (C d ), 41.6(C e ), 44.7(C a ), 50.2(C b ), 67.0(C l ), 68.5(C c ), 68.7(C j ), 74.6(C k ), 113.9(C h ), 114.6(C n ), 121.2(C p ), 127.7(C g ), 129.5(C o ), 143.7(C f ), 154.1(C q ), 156.2(C i ), 158.1(C m ) and infrared spectral data is FTIR (KBr, cm -1 ): ν = 1750 (C = O stretch of carbonyl group), and high resolution mass spectral data was obtained by High resolution LC-MS (ESI-MS) m / z: [M + ]calcd.for C 55 H 58 O 11 The theoretical epoxy equivalent weight was 483.11 g / eq, and the actual epoxy equivalent weight was 476 g / eq. The chemical reaction formula of Synthesis Example 1 is shown in Table 3 below. As a result, it was found that carbonate groups can react with epoxy groups. [Table 3]
[0035] <Epoxy cured product>
[0036] The present invention further provides a cured epoxy product obtained by curing the carbonate-containing epoxy resin. The curing reaction is briefly described below with reference to Figure 2, which is a step flowchart illustrating a method 200 for preparing a cured epoxy product according to another embodiment of the present invention. In Figure 2, the method 200 for preparing a cured epoxy product includes steps 210 and 220.
[0037] Step 210 is a mixing step in which a carbonate-containing epoxy resin and a curing agent are mixed to obtain a curable composition. Specifically, in step 210, the carbonate-containing epoxy resin and the curing agent form a precursor solution containing the curable composition. The solvent used in the precursor solution is used to facilitate mixing of the carbonate-containing epoxy resin and the curing agent. Any solvent that can dissolve the carbonate-containing epoxy resin and the curing agent and does not react with them can be used as the solvent in step 210. Details of the carbonate-containing epoxy resin are described above and will not be repeated here. The curing agent of the present invention may be, but is not limited to, a phenolic resin, an amine-based compound, an active ester compound, a carboxylic acid compound, a cyanate ester, an isocyanate compound, an acid anhydride compound, benzoxazine, a polycarbonate, or a mixture thereof.
[0038] Step 220 is a curing step in which the carbonate-containing epoxy resin and the curing agent are crosslinked to form a cured epoxy product. Specifically, the curable composition can be directly pulverized into powder and heated to a molten state, or the precursor solution can be heated to crosslink the carbonate-containing epoxy resin and the curing agent. The final curing temperature can be 80°C to 240°C, preferably 180°C to 240°C, and the heating time can be 1 hour to 6 hours. More specifically, the heating method can be a multi-stage heating and curing method, for example, heating at 180°C, 200°C, and 220°C for 2 hours each. The curing temperature and heating time can be flexibly adjusted depending on the types of carbonate-containing epoxy resin and curing agent used, and the present invention is not limited thereto.
[0039] <Method for decomposing cured epoxy resin>
[0040] 3, which is a step flowchart illustrating a method 300 for decomposing a cured epoxy material according to yet another embodiment of the present invention. In FIG. 3, the method 300 for decomposing a cured epoxy material includes steps 310 and 320.
[0041] Step 310 is a step of providing the cured epoxy material, and step 320 is a decomposition step of reacting the cured epoxy material with an amino group-containing compound to decompose the cured epoxy material.
[0042] The present invention will be further illustrated by the following specific examples, which will serve to enable those skilled in the art to fully utilize and practice the present invention without the need for undue interpretation. These examples should not be construed as limiting the scope of the present invention, but are used to explain how to carry out the materials and methods of the present invention.
[0043] <Examples / Comparative Examples>
[0044] <Preparation of carbonate-containing epoxy resin>
[0045] In Example 1, 1.0 g of diphenyl carbonate and 3.51 g of bisphenol A epoxy resin (Changchun Artificial Resin, product number BE188) were heated to 100°C in an equivalent ratio of 1:2, and after confirming dissolution, 0.0175 g of pyridine was added and the reaction was carried out for 8 hours to obtain the carbonate-containing epoxy resin DPC-EP of Example 1, which had an epoxy equivalent of 476 g / eq (theoretical value 483 g / eq).
[0046] In Example 2, 1.50 g of polycarbonate and 4.44 g of bisphenol A epoxy resin (Changchun Artificial Resins, product number BE188) were melted in an equivalent ratio of 1:2 under a nitrogen atmosphere at 200°C, then the temperature was lowered to 100°C, 0.0133 g of pyridine (DGEBA 0.3 wt%) was added, and the mixture was allowed to react with mechanical stirring for 8 hours to produce a dark brown viscous liquid. After cooling to room temperature, the carbonate-containing epoxy resin WPC-EP2 of Example 2 was obtained, with an epoxy equivalent of 485 g / eq (theoretical value: 503 g / eq).
[0047] In Example 3, 1.50 g of polycarbonate and 6.66 g of bisphenol A epoxy resin (Changchun Artificial Resins, product number BE188) were melted in an equivalent ratio of 1:3 at 200°C under a nitrogen atmosphere, then the temperature was lowered to 100°C, and 0.0199 g of pyridine (DGEBA 0.3 wt%) was added. The carbonate-containing epoxy resin WPC-EP3 of Example 3 was obtained in the same manner as in Example 2, with an epoxy equivalent of 333 g / eq (theoretical value 345 g / eq).
[0048] In Example 4, 1.50 g of polycarbonate and 8.88 g of bisphenol A epoxy resin (Changchun Artificial Resins, product number BE188) were melted at 200°C in a nitrogen atmosphere in an equivalent ratio of 1:4, then the temperature was lowered to 100°C, and 0.0266 g of pyridine (DGEBA 0.3 wt%) was added. The carbonate-containing epoxy resin WPC-EP4 of Example 4 was obtained in the same manner as in Example 2, with an epoxy equivalent of 285 g / eq (theoretical value 293 g / eq).
[0049] To confirm the structures of Examples 1 to 4, 1 H-NMR analysis was carried out. 1 4 showing the H-NMR spectrum and the results of Examples 2 to 4 1 See Figure 5, which shows the H-NMR spectrum. From the results of Figures 4 and 5, it was found that the products of Examples 1 to 4 were all carbonate-containing epoxy resins.
[0050] <Preparation of cured epoxy product>
[0051] An equivalent amount of curing agent is added to the carbonate-containing epoxy resins synthesized in Examples 1 to 4, ground into powder, heated to 150°C to melt, and stirred uniformly.The mixture is then placed in an oven and heated to 160°C for 1 hour, 180°C for 2 hours, and then 200°C for 2 hours. Alternatively, the cured epoxy products of Examples 5 to 16 can be obtained by using the solvent method, where the carbonate-containing epoxy resins synthesized in Examples 1 to 4 and the curing agent are stirred in a solution with a solids content of 20 wt% until fully melted, and then poured into a mold and cured.
[0052] Specifically, the curing agent used in the present invention may be diaminodiphenylmethane (DDM), phenolic resin (PN), dicyandiamide (DICY), polycarbonate (PC), diphenyl ether tetracarboxylic dianhydride (ODPA), and phthalic anhydride (PAH). Taking Example 2 as an example, when different curing agents are selected, the cured epoxy products prepared are shown in Table 4 below. [Table 4]
[0053] Furthermore, an equivalent amount of curing agent was added to commercially available epoxy resin BE188 and epoxy resin BE501, and the same curing step as in Examples 5 to 16 was carried out to obtain the epoxy cured products of Comparative Examples 1 to 4.
[0054] In detail, when adding a curing agent that is diaminodiphenylmethane, adding an equal equivalent amount means that the number of epoxy equivalents is equal to the number of active hydrogen equivalents, and when adding a curing agent that is polycarbonate, adding an equal equivalent amount means that the number of epoxy equivalents is equal to the number of carbonate group equivalents.
[0055] The epoxy resins and curing agents used in Examples 5 to 16 and Comparative Examples 1 to 4 are shown in Table 5 below. [Table 5]
[0056] <Thermal characteristic evaluation>
[0057] For Examples 5 to 16 and Comparative Examples 1 to 4, the glass transition temperature (T g ), 5% thermogravimetric loss temperature (T d5% The thermal properties including the coke residual rate were evaluated as follows.
[0058] (1) Glass Transition Temperature: The storage modulus and tan delta curve vs. temperature, as well as the glass transition temperature, of the cured epoxy materials prepared in Examples 5 to 16 and Comparative Examples 1 to 4 were measured using a dynamic mechanical analyzer (DMA). Additionally, the glass transition temperature was measured using thermomechanical analysis (TMA) at a heating rate of 5°C / min.
[0059] (2) 5% Thermal Weight Loss Temperature and Coke Yield: The 5% thermal weight loss temperature and char yield at 800°C of the sample were measured using thermogravimetric analysis (TGA). The thermogravimetric analysis was performed under a nitrogen atmosphere at a heating rate of 20°C / min, with the weight change of the sample measured using a thermogravimetric analyzer. The 5% thermal weight loss temperature refers to the temperature at which the weight loss of the cured sample reaches 5%. A higher 5% thermal weight loss temperature indicates better thermal stability of the sample. The 800°C coke yield refers to the residual weight ratio of the sample when the heating temperature reaches 800°C. A higher residual weight ratio at 800°C indicates better thermal stability of the sample.
[0060] The measurement results of the glass transition temperature, storage modulus, thermal weight loss temperature, and coke residual rate for Examples 5 to 16 and Comparative Examples 1 to 4 are shown in Table 6 below. [Table 6]
[0061] As can be seen from the results in Table 6, the glass transition temperature of the cured epoxy resins prepared using DDM as the curing agent is higher than that of other curing agents. This is primarily due to the higher functionality of the DDM curing agent, which increases crosslink density and improves thermal properties. However, the 5% thermal weight loss temperature is primarily related to the bond after crosslinking. When PN is used as the curing agent, the energy required to decompose the ether group is greater than that required for ester and amine groups, resulting in a relatively excellent 5% thermal weight loss temperature. Furthermore, when PN and DDM are used as curing agents, the main chain often has a benzene ring structure, which allows for molecules that are more closely spaced from the epoxy resin, resulting in a relatively high coke residue rate. Furthermore, the carbonate-containing epoxy resins of Examples 5 to 16 of the present invention exhibited similar thermal properties after curing to the commercially available cured epoxy resins of Comparative Examples 1 to 4.
[0062] <Mechanical property evaluation>
[0063] For Examples 5 to 16 and Comparative Examples 1 to 4, mechanical properties were evaluated, and tensile strength and elongation at break were measured by tensile testing. Here, the tensile test was carried out at room temperature using test pieces having a length of 5 cm, a width of 1 cm, and a thickness of 0.04 to 0.10 mm. The measurement results of tensile strength and elongation at break for Examples 5 to 16 and Comparative Examples 1 to 4 are shown in Table 7 below. [Table 7]
[0064] As is clear from the results in Table 7, when PC is used as a curing agent, its main chain is long and the ester group of PC has a certain degree of steric hindrance, which gives the cured product high molecular motion and relatively excellent tensile performance. Furthermore, the carbonate-containing epoxy resins of Examples 5 to 16 of the present invention exhibit mechanical properties similar to those of the commercially available cured epoxy resins of Comparative Examples 1 to 4 after curing, and are therefore generally superior to the results of Comparative Examples 1 to 4.
[0065] <Decomposition of cured epoxy resin>
[0066] Examples 17 to 19 are the results obtained from the decomposition reaction of the epoxy cured products of Examples 8 to 10, respectively, and Comparative Examples 5 to 8 are the results obtained from the decomposition reaction of the epoxy cured products of Comparative Examples 1 to 4, respectively. First, the epoxy cured product films of Examples 8 to 10 and Comparative Examples 1 to 4 and 1-hexylamine were placed in a reactor, and after the reaction was completed, the 1-hexylamine was extracted directly using a vacuum concentrator to obtain Examples 17 to 19 and Comparative Examples 5 to 8 in which the decomposition was complete. The type of epoxy cured product, reaction temperature, reaction time, and residual weight required for Examples 17 to 19 and Comparative Examples 5 to 8 are all shown in Table 8 below. [Table 8]
[0067] According to Example 19 1 Please refer to Figure 6, which shows the H-NMR spectrum. In particular, Figure 6(a) shows the H-NMR spectrum of the product of Example 10 after the aminolysis reaction with 1-hexylamine and subsequent distillation of 1-hexylamine. 1 6(b) is a H-NMR spectrum of the precipitate obtained by distilling off 1-hexylamine after the aminolysis reaction of Example 10 with 1-hexylamine and pouring methanol into the precipitate. 1 1H-NMR spectrum.
[0068] From the results in Figure 6, the characteristic signals of 1,3-dihexylurea can be observed, with the amino signal (NH-CO-NH) of the urea structure at 7.3 ppm and the methylene signal at 2.9 ppm (H i ) and 1.2 to 1.4 ppm (H c-h ) and the methyl signal is located at 0.8 ppm (H d ), and among them, the characteristic signals of phenoxy resin can be observed, with a hydroxy signal at 5.3 ppm, benzene ring signals at 6.8 and 7.0 ppm, and methine and methylene signals at 4.1 ppm (H b ) and 3.9 ppm (H a ) and the methyl signal is located at 1.5 ppm (H c 6 and Table 8, it can be seen that the cured epoxy material of Example 10 of the present invention is decomposable after reaction with an amino group-containing compound, and the residual weight of the cured epoxy material was 0%.
[0069] Furthermore, in Examples 8 and 9, partial decomposition was observed even in the heat reaction of 1-hexylamine, with 85% and 77% remaining by weight, respectively. In Comparative Examples 1 to 4, the cured epoxy resins prepared from commercially available epoxy resins showed no decomposition even after 24 hours under the same conditions, with 100% remaining by weight in all cases. This proves that the carbonate-containing epoxy resins synthesized in the present invention have unique decomposition properties and can significantly contribute to the recovery of thermosetting materials and the reduction of waste.
[0070] As described above, the present invention provides a carbonate-containing bifunctional or polyfunctional epoxy resin through a simple one-step reaction. This preparation method can be particularly effective using recycled waste polycarbonate or carbonate compounds as the raw material, and its high atomic efficiency contributes to reducing polycarbonate waste. Furthermore, by curing the carbonate-containing epoxy resin of the present invention with a curing agent, a cured epoxy product with excellent properties can be obtained. The cured epoxy product is also chemically degradable, reducing the discharge of thermosetting plastic waste and achieving sustainability goals.
[0071] Although the present invention has been disclosed above in the form of embodiments, it is not intended to limit the present invention, and those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined based on the scope of the claims attached below. [Explanation of symbols]
[0072] 100. Method for preparing carbonate-containing epoxy resins 200 Method for preparing cured epoxy 300 Decomposition method for cured epoxy materials 110, 120, 130, 210, 220, 310, 320 steps
Claims
1. Having the structure shown in formula (II), [Formula 1] R 7 and R 8 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; e and f each independently represent an integer of 0 to 5; Y is an alkylene group having 1 to 12 carbon atoms, an alkoxylene group having 1 to 12 carbon atoms, or a structure represented by formula (iii) or formula (iv), [chemical 2] R 3 and R 4 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R 5 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, or an alkoxy group having 1 to 6 carbon atoms; R 6 teeth, [C3] an alkylene group having 5 to 12 carbon atoms or a cycloalkylene group having 5 to 12 carbon atoms, c and d each independently represent an integer of 0 to 4, Z is a single bond, an alkylene group having 1 to 12 carbon atoms, or a cycloalkylene group having 3 to 12 carbon atoms; [C4] [C5] [C6] [C7] [C8] an arylene group having 6 to 12 carbon atoms; [C9] or a structure as shown in formula (i) or (ii), [C10] X 1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms; A carbonate-containing epoxy resin, characterized in that p is an integer of 1 to 11, q is an integer of 0 to 20, and r is an integer of 1 to 15.
2. A method for producing an aromatic carbonate group-containing structure having a structure shown in formula (A2): [C11] Providing an epoxy group-containing structure having a structure shown in formula (B); [C12] a catalytic step of mixing the aromatic carbonate group-containing structure and the epoxy group-containing structure, followed by subjecting the mixture to the action of a catalyst to obtain a carbonate-containing epoxy resin having the structure shown in formula (II); Including, [C13] R 7 and R 8 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; e and f each independently represent an integer of 0 to 5; Y is an alkylene group having 1 to 12 carbon atoms, an alkoxylene group having 1 to 12 carbon atoms, or a structure represented by formula (iii) or formula (iv), [C14] R 3 and R 4 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R 5 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, or an alkoxy group having 1 to 6 carbon atoms; R 6 teeth, [C15] an alkylene group having 5 to 12 carbon atoms or a cycloalkylene group having 5 to 12 carbon atoms, c and d each independently represent an integer of 0 to 4, Z is a single bond, an alkylene group having 1 to 12 carbon atoms, or a cycloalkylene group having 3 to 12 carbon atoms; [C16] [C17] [C18] [C19] [C20] an arylene group having 6 to 12 carbon atoms; [C21] Or, a structure shown in formula (i) or formula (ii): [C22] X 1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms; m is an integer from 2 to 12, p is an integer from 1 to 11, q is an integer from 0 to 20, and r is an integer from 1 to 15; the catalyst is selected from the group consisting of 4-dimethylaminopyridine, imidazole, pyridine, 2-methylimidazole, 3-methylimidazole, and 2-ethyl-4-methylimidazole; a carbonate-containing epoxy resin preparation method, characterized in that an equivalent ratio of an epoxy group in the epoxy group-containing structure to a carbonate group in the aromatic carbonate group-containing structure is 1.3 to 10.
0.
3. The method for preparing a carbonate-containing epoxy resin according to claim 2, characterized in that the amount of the catalyst added is 0.1% by weight to 5% by weight of the content of the epoxy group-containing structure.
4. An epoxy cured product obtained by subjecting the carbonate-containing epoxy resin according to claim 1 to a curing reaction.
5. The epoxy cured product according to claim 4, wherein the curing reaction is completed by mixing the carbonate-containing epoxy resin and a curing agent and heating the mixture.
6. 6. The epoxy cured product according to claim 5, wherein the curing agent is a phenolic resin, an amine compound, an active ester compound, a carboxylic acid compound, a cyanate compound, an isocyanate compound, an acid anhydride compound, benzoxazine, polycarbonate, or a mixture thereof.
7. 6. The epoxy cured product according to claim 5, wherein the curing reaction is carried out at a curing temperature of 180° C. to 240° C.
8. Providing an epoxy cured product according to claim 4; a decomposition step of reacting an amino group-containing compound with the epoxy cured material so as to decompose the epoxy cured material; 1. A method for decomposing an epoxy cured material, comprising:
Citation Information
Patent Citations
JP1971021899B
Polyaddition copolymer and its production
JP1999302369A
Polycarbonate-epoxy polymer
US4943619A
Cited By
Modified epoxy resin, its manufacturing method, resin composition, cured product, and decomposition method.
JP2026144033A
Epoxy resin composition, cured product, etc., and decomposition method
JP2026151972A
MODIFIED EPOXY RESIN AND METHOD FOR PRODUCING SAME, RESIN COMPOSITION, CURED PRODUCT, etc., AND DECOMPOSITON METHOD
KR1020260133743A
Epoxy resin composition, cured product thereof, and decomposition method
KR1020260140167A