Photoresponsive material, adhesive, photoswitching material, toner and image forming method
A composition of isomerized polymer and low-molecular compound in photoresponsive materials addresses the inefficiency of energy use in azobenzene derivatives by enabling efficient fluidization and non-fluidization with reduced energy through photothermal conversion and cis-trans photoisomerization.
Patent Information
- Application Number
- JP2020135373
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-24
- Filing Date
- 2020-08-07
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-08-07
AI Technical Summary
Existing photoresponsive materials, such as azobenzene derivatives, require a significant amount of light energy for efficient fluidization due to inefficient propagation of structural changes during photoisomerization.
A composition comprising an isomerized polymer containing a structural unit and an isomerized low-molecular compound, which becomes fluidized by light irradiation and reversibly non-fluidized, utilizing photothermal conversion and cis-trans photoisomerization to induce phase transitions.
The composition achieves more efficient fluidization and non-fluidization with less energy, allowing for reversible transitions between solid and fluid states.
Smart Images

Figure 0007556229000042 
Figure 0007556229000044 
Figure 0007556229000043
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition as a photoresponsive material that becomes fluid and reversibly non-fluid upon irradiation with light, an adhesive, a photoswitching material and a toner each using the composition, and an image forming method using the toner. [Background technology]
[0002] Photoresponsive liquid crystal materials are known as materials whose fluidity changes when irradiated with light. For example, Patent Documents 1 and 2 propose polymer liquid crystal materials using azobenzene derivatives. These undergo a cis-trans isomerization reaction at the azobenzene moiety in response to light. It is believed that the resulting change in molecular structure induces a phase transition from a solid state to a fluid state. In addition, if the material is irradiated with light at a different wavelength again, heated, or left at room temperature in the dark, a reverse reaction will occur and the material will solidify again. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-256155 A [Patent Document 2] JP 2011-256291 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, a sufficient amount of light energy is required to break the ordered structure in the phase change from a highly ordered solid state to a fluid state of the azobenzene derivatives described in the above Patent Documents 1 and 2. Since the propagation of the structural change caused by photoisomerization is inefficient in these azobenzene derivatives, a large amount of energy is required by light irradiation to fluidize them.
[0005] Therefore, the present invention aims to provide a photoresponsive material that is fluidized and reversibly non-fluidized upon irradiation with light, which exhibits more efficient fluidization / non-fluidization, i.e., requires less energy. [Means for solving the problem]
[0006] The present inventors have conducted extensive research in view of the above problems, and as a result have found that the above problems can be solved by using a solid composition in which a polymer containing a structural unit derived from an isomerized structure and an isomerized low molecular weight compound are mixed, thereby completing the present invention.
[0007] That is, the present invention provides a composition which contains an isomerized polymer including a structural unit having an isomerized structure and an isomerized low molecular weight compound, and which is fluidized from a solid state by irradiation with light and reversibly becomes non-fluid. Effect of the Invention
[0008] According to the present invention, in a photoresponsive material that is fluidized and reversibly non-fluidized by irradiation with light, it is possible to obtain a material that exhibits more efficient fluidization / non-fluidization, that is, a material that requires less energy. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. [Diagram 2] 2 is a schematic configuration diagram of an irradiation unit 40 in the image forming apparatus 100. FIG. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus for measuring the change in adhesiveness of a composition with light irradiation used in the photoresponsive adhesion test of the Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention relates to a composition which contains an isomerized polymer including a structural unit having an isomerized structure and an isomerized low molecular weight compound, and which is rendered fluid from a solid state by irradiation with light and reversibly rendered non-fluid.
[0011] According to the present invention, it is possible to obtain a composition that exhibits efficient fluidization / non-fluidization by photoisomerization, that is, a composition that requires less energy.
[0012] Although the details of why the composition of the present invention provides the above-mentioned effects are unclear, the following mechanism is considered to be the cause. Note that the following mechanism is based on speculation, and the present invention is not limited to the following mechanism in any way.
[0013] Polymers containing structural units containing isomerized structures can induce reversible fluidization / immobilization phenomena when the isomerized structures absorb light, and the heat energy released during the photoexcitation / deactivation process is transferred to the repeating units (structural units) that bond (photothermal conversion). In particular, if the isomerized structures in the polymer are derived from the trans form of a molecule that exhibits cis-trans photoisomerization, in addition to the above-mentioned photothermal conversion, trans-cis photoisomerization is more likely to occur upon light irradiation, and a cis form with a low Tg is more likely to be produced. It is believed that photoisomerization destroys the ordered structure and causes a phase transition, which can induce more efficient fluidization / immobilization phenomena.
[0014] When an isomerized low molecular weight compound is mixed with a polymer containing the above-mentioned isomerized structure, if the polymer contains an isomerized structure as a polymer side chain, the isomerized low molecular weight compound is thought to enter the gap space of the isomerized structure as a side chain and form a π-π stack. When light is irradiated, the isomerized low molecular weight compound that formed a π-π stack is released from the ordered structure due to a structural change accompanying the isomerization of the isomerized structure of the polymer, and the free space generated by this makes it easier for the isomerized structure to be isomerized, and it is thought that a more efficient collapse of the ordered structure, i.e., a fluidization phenomenon, can be induced.
[0015] Furthermore, if the isomerized low molecular weight compound is a compound that exhibits cis-trans photoisomerization and is a trans isomer, it is likely to undergo photoisomerization upon light irradiation, and by changing to a cis isomer, it is likely to deviate from the regular structure of π-π stacking. This creates free space in the polymer side chain, making it easier to induce structural changes in the isomerized structure of the polymer side chain, and it is thought that a more efficient fluidization phenomenon can be induced. In addition, by mixing an isomerized polymer with an isomerized low molecular weight compound, a material with superior toughness can be obtained compared to the case of using only an isomerized low molecular weight compound.
[0016] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, in this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0017] [Composition that becomes fluid and reversibly non-fluid upon irradiation with light] In this specification, the term "fluidized by light irradiation and reversibly non-fluidized" refers to a state in which the composition changes from a non-fluid state to a fluid state by light irradiation and then returns to a non-fluid state. That is, the composition of the present invention is in a non-fluid solid state at room temperature and normal pressure when not irradiated with light, and softens and changes to a fluid state by light irradiation. When the light irradiation is stopped and the composition is left in a dark place at room temperature or under visible light irradiation, or is heated, the composition returns to a non-fluid solid state. In this specification, the term "fluid state" refers to a state in which the composition is deformed by a small external force.
[0018] Specific forms of the isomerized polymer and isomerized low molecular weight compound that can be used in the composition of the present invention will be described later, but it is preferable that the isomerized polymer used in the composition of the present invention contains a polymer containing a structural unit derived from an azobenzene derivative or a structural unit derived from an azomethine derivative, and the isomerized low molecular weight compound contains an azobenzene compound or an azomethine compound.
[0019] Azobenzene derivatives and azomethine derivatives undergo a cis-trans isomerization reaction upon irradiation with light, and this change in molecular structure induces a phase transition from a solid state to a fluid state. After the light irradiation is stopped, they are reversibly rendered non-fluid (resolidified) by leaving them in the dark at room temperature or under visible light irradiation, or by heating. Therefore, by using azobenzene derivatives (azobenzene compounds) or azomethine derivatives (azomethine compounds) and polymers containing structural units derived from them, it is possible to more effectively induce fluidization and reversible fluidization upon irradiation with light.
[0020] The composition of the present invention may be a combination of a polymer containing a structural unit derived from an azobenzene derivative and an azobenzene compound, or a combination of a polymer containing a structural unit derived from an azomethine derivative and an azomethine compound. In this case, the azobenzene derivative and the azobenzene compound contained in the structural unit of the polymer may have the same structure or different structures. In addition, the azomethine derivative and the azomethine compound contained in the structural unit of the polymer may have the same structure or different structures.
[0021] In addition, the composition of the present invention may use a combination of a polymer containing a structural unit derived from an azobenzene derivative and an azomethine compound, or may use a combination of a polymer containing a structural unit derived from an azomethine derivative and an azobenzene compound.
[0022] Furthermore, a polymer having a structural unit derived from an azobenzene derivative and a polymer having a structural unit derived from an azomethine derivative may be used in combination, or a polymer having a structural unit derived from an azobenzene derivative and a structural unit derived from an azomethine derivative may be used.
[0023] The proportion of the polymer having a structural unit derived from an azobenzene derivative or a structural unit derived from an azomethine derivative relative to the total mass of the isomerized polymer contained in the composition of the present invention is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more. The total amount of the azobenzene compound and the azomethine compound relative to the total mass of the isomerized low molecular weight compound contained in the composition of the present invention is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more.
[0024] [Isomerized low molecular weight compound] The isomerizable low molecular weight compound used in the composition of the present invention is a compound that is fluidized and reversibly non-fluidized upon irradiation with light, and has a molecular weight of less than 1,000.
[0025] The isomerized low molecular weight compound preferably has a molecular weight of 100 or more and less than 1000, more preferably 100 or more and 800 or less. The isomerized low molecular weight compound does not include a polymer. In a preferred embodiment, the isomerized low molecular weight compound is configured without including a repeating unit. In a preferred embodiment, the isomerized low molecular weight compound is not obtained by polymerizing a monomer containing a polymerizable group.
[0026] The isomerizable low molecular weight compound is preferably a compound that exhibits photoisomerization. For example, a compound that exhibits cis-trans isomerization upon light irradiation may be mentioned. As such a compound that exhibits cis-trans isomerization upon light irradiation, an azobenzene derivative (azobenzene compound) or an azomethine derivative (azomethine compound) is preferable. In this specification, the azobenzene derivative (azobenzene compound) includes azobenzene.
[0027] (azobenzene derivatives) The azobenzene derivative (azobenzene compound) used in the present invention is not particularly limited, but a preferred embodiment of the azobenzene derivative is an azobenzene derivative represented by the following chemical formula (1), since it has a high softening speed when irradiated with light and has excellent image fixing properties when used in a toner.
[0028] [ka]
[0029] In the above chemical formula (1), R to R 10 are each independently a group selected from the group consisting of a hydrogen atom, an alkyl group, an alkoxy group, a halogen group, a hydroxyl group, and a carboxyl group, and R to R 10 At least two of R1 to R5 are groups selected from the group consisting of an alkyl group, an alkoxy group, a halogen group, a hydroxy group, and a carboxy group, and preferably, at least one of R1 to R5 is an alkyl group or an alkoxy group having 1 to 18 carbon atoms, and 10 At least one of them is an alkyl group or an alkoxy group having 1 to 18 carbon atoms.
[0030] In the above chemical formula (1), at least one of R3 and R8 is preferably an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms. That is, a preferred embodiment of the azobenzene derivative used in the present invention is an azobenzene derivative having a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position relative to the nitrogen-nitrogen double bond. If at least one of R3 and R8 is an alkyl group or an alkoxy group within the above carbon number range, in the trans form, intermolecular packing (π-π interaction) is expressed by the aromatic ring, while high thermal mobility is exhibited when isomerized from the trans form to the cis form, and it is considered that the fluidization phenomenon is easily induced.
[0031] Among them, from the viewpoint of further improving the fixability of the image when used in the toner, R3 and R8 are preferably each independently an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms. In this way, by having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position of the two benzene rings, the thermal mobility of the molecule is increased, and as described above, isotropic melting is likely to occur in a chain manner in the entire system. In this case, R3 and R8 may be the same or different, but from the viewpoint of ease of synthesis, it is preferable that they are the same. In addition, the alkyl group or alkoxy group having 1 to 18 carbon atoms used in R3 and R8 may be linear or branched, but from the viewpoint of forming a rod-shaped molecular structure that is likely to undergo photophase transition, it is preferable that they are linear.
[0032] Among them, R3 and R8 are preferably each independently an alkyl group or an alkoxy group having 6 to 12 carbon atoms. If R3 and R8 are an alkyl group or an alkoxy group having the above carbon number, the compound has high thermal mobility, but the alkyl-alkyl interaction between molecules is relatively weak. Therefore, the crystals are easily broken, cis-trans isomerization is more likely to proceed, and the softening speed by light irradiation and the fixability of the image when used in a toner are further improved.
[0033] In the above chemical formula (1), R1, R2, R4, R5, R6, R7, R9, R 10 At least one of the groups is preferably a group (hereinafter also simply referred to as a substituent) selected from the group consisting of an alkyl group, an alkoxy group, a halogen group, a hydroxy group, and a carboxy group. By having such a structure, lattice defects that act favorably on cis-trans isomerization, free volume is generated, and π-π interactions are reduced. Therefore, cis-trans isomerization proceeds more easily, and the softening speed and image fixability due to light irradiation are further improved. Among them, from the viewpoint of ensuring the free volume necessary for cis-trans isomerization, R1, R2, R4, R5, R6, R7, R9, R 10At least one of these is more preferably an alkyl group or alkoxy group having 1 to 4 carbon atoms, which may be branched, or a halogen group, and from the viewpoint of further improving the fixability of the image, it is even more preferably an alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group.
[0034] In the above chemical formula (1), R1, R2, R4, R5, R6, R7, R9, R 10 The number of the substituents in is preferably 1 to 8, more preferably 1 to 6. Among them, from the viewpoint of not lowering the melting point of the azobenzene derivative too much and further enhancing the heat-resistant storage stability of the toner, it is even more preferably 1 to 4, and particularly preferably 1 to 3.
[0035] R1, R2, R4, R5, R6, R7, R9, R 10 The position where the substituent is present in is not particularly limited, but it is preferable that at least one of R2, R4, R7 and R9 in the above chemical formula (1) has a substituent, and it is more preferable that at least one of R2, R4, R7 and R9 in the above chemical formula (1) has a methyl group. An azobenzene derivative having such a structure has an improved softening speed by light irradiation, thereby improving the fixing property of an image, and also has an appropriately high melting point, thereby improving the heat-resistant storage stability of a toner.
[0036] Examples of the azobenzene derivative include 4,4'-dialkylazobenzenes, such as 4,4'-dihexylazobenzene, 4,4'-dioctylazobenzene, 4,4'-didecylazobenzene, 4,4'-didodecylazobenzene, and 4,4'-dihexadecylazobenzene, in which R3 and R8 in the chemical formula (1) are each an alkyl group having 1 to 18 carbon atoms; or 4,4'-bis(hexyloxy)azobenzene, 4,4'-bis(octyloxy)azobenzene, In 4,4'-bis(alkoxy)azobenzenes such as 4,4'-bis(dodecyloxy)azobenzene and 4,4'-bis(hexadecyloxy)azobenzene, in which R3 and R8 in the chemical formula (1) are each an alkoxy group having 1 to 18 carbon atoms, the hydrogen atoms added to the benzene ring are preferably mono-, di- or tri-substituted with a group selected from the group consisting of an alkyl group, an alkoxy group, a halogen group, a hydroxyl group and a carboxyl group. More specifically, the following azobenzene derivatives (1) to (12) can be mentioned.
[0037] [ka]
[0038] [ka]
[0039] The method for synthesizing the azobenzene derivative is not particularly limited, and any conventionally known synthesis method can be applied.
[0040] For example, as shown in the following reaction formula A, 4-aminophenol is reacted with sodium nitrite under cooling to produce a diazonium salt, which is then reacted with o-cresol to synthesize intermediate A (first step), and intermediate A is then reacted with n-bromohexane to obtain the above-mentioned azobenzene derivative (1).
[0041] [ka]
[0042] In the above reaction formula A, the desired azobenzene derivative can be obtained by changing the raw materials (4-aminophenol, o-cresol and / or n-bromohexane) to other compounds. In addition, the above production method makes it easy to obtain an azobenzene derivative having an asymmetric structure.
[0043] For example, as shown in the following reaction scheme B, by replacing o-cresol and n-bromohexane with 2-bromophenol and n-bromododecane, respectively, the azobenzene derivative (4) can be obtained.
[0044] [ka]
[0045] Moreover, as shown in the following reaction formula C, the azobenzene derivative (4) can be reacted with methanol in the presence of a Pd catalyst and a base to obtain the azobenzene derivative (5).
[0046] [ka]
[0047] Alternatively, for example, as shown in the following reaction formula D, p-hexylaniline can be reacted with manganese dioxide, which is an oxidizing agent, to synthesize 4,4'-dihexylazobenzene, which can then be reacted with N-bromosuccinimide and methylboronic acid in the presence of a Pd catalyst and a base to obtain the azobenzene derivative (6).
[0048] [ka]
[0049] In the above reaction formula D, the desired azobenzene derivative can be synthesized by changing the raw materials (p-hexylaniline and / or methylboronic acid) to other compounds.
[0050] The azobenzene derivatives can be used alone or in combination of two or more kinds.
[0051] (Azomethine derivatives) An azomethine derivative (azomethine compound) that is preferably used as an isomerizable low molecular weight compound is a compound having an aromatic hydrocarbon group or an aromatic heterocyclic group at each end of a C=N bond, and has an activation energy Ea of cis-trans isomerization of 60 kJ / mol or more.
[0052] The activation energy of cis-trans isomerization is the difference between the total energy of the transition state represented by the following general formula (2) and the total energy of the cis isomer represented by the following general formula (3) in a photoresponsive compound represented by the following general formula (1).
[0053] [ka]
[0054] [ka]
[0055] In general formula (1), Z1 and Z2 are each independently N or CH, and Z1 ≠ Z2; and A and B are each independently a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group.
[0056] If the activation energy Ea of cis-trans isomerization is 60 kJ / mol or more, the barrier to the isomerization reaction from cis to trans isomers is sufficiently high, and the rapid reversion to the trans isomer after isomerization to the cis isomer by light irradiation can be suppressed, thereby inducing a fluidization phenomenon by light irradiation and further realizing reversible immobilization.
[0057] The activation energy Ea is more preferably 63 kJ / mol or more, even more preferably 64 kJ / mol or more, and even more preferably 65 kJ / mol or more. In view of the ease of reversion to the trans isomer, the activation energy Ea is preferably 100 kJ / mol or less, more preferably 95 kJ / mol or less, and even more preferably 90 kJ / mol or less.
[0058] This is the snowflake range of snowflakes This is the best dressing room for you The intrinsic wavelength is the Gaussian wavelength of the gaussian waveguide 16 (Revision B.01, Frisch MJ, GW Trucks, HB Schlegel, Scuseria GE, Robb MA, Cheeseman JR, Scalmani G, Barone V, Petersson GA, Nakatsuji H, Li X, Caricato M, Marenich AV, Bloino J, Janesko BG, Gomperts R, Mennucci, HP Hratchian, JV Ortiz, AF Izmaylov, JL Sonnenberg, D. Williams-Young, F. Ding, F. Lipparini, F. Egidi, J. Goings, B. Peng, A. Petrone, T. Henderson, D. Ranasinghe, VG Zakrzewski, J. Gao, N. Rega, G. Zheng, W. Liang, M. Hada, M. Ehara, K. Toyota, R.K. Fukuda , Hasegawa J , Ishida M , Nakajima T , Honda Y , Kitao O , Nakai H , Vreven T , Throssell K , Montgomery JA , Peralta JE , Ogliaro F MJ , Bearpark MJ , Heyd EN Brothers , Kudin KN , Staroverov VN , Keith TA , Kobayashi R , Normand J, Raghavachari K, Rendell AP, Burant JC, Iyengar SS, Tomasi J, Cossi M, Millam JM, Klene M, Adamo C, Cammi R, JWOchterski, RL Martin, K. Morokuma, O. Farkas, JB Foresman, and DJ Fox, Gaussian, Inc., Wallingford CT, 2016.) software can be used, and the density functional theory (B3LYP / 6-31G(d)) can be used as the calculation method. For the molecular structure of the cis isomer, the most stable molecular structure of the isomer represented by general formula (3), i.e., the molecular structure with the lowest total energy, is calculated, and this total energy is the total energy of the cis isomer. For the molecular structure of the transition state (TS), the saddle point of the corresponding molecular structure is calculated for the transition state represented by general formula (2), and the total energy obtained at this time is the total energy of the transition state. There is no particular limitation on the software or calculation method, and similar values can be obtained using any of them. From the calculated value obtained in this way, the value of the activation energy Ea can be calculated using formula (1): Ea (kJ / mol) = (total energy of TS (kJ / mol)) - (total energy of cis isomer (kJ / mol)). .
[0059] By appropriately selecting the structures of A and B in the above general formula (1), the activation energy Ea represented by formula (1) can be controlled to 60 kJ / mol or more.
[0060] Specifically, by introducing an electron-donating structure into a compound having an azomethine moiety, the electron density of the azomethine moiety can be increased, and the activation energy Ea can be increased. For example, by making at least one of A and B an aromatic heterocyclic group with high electron-donating properties, the activation energy Ea can be increased. In addition, by introducing a substituent with high electron-donating properties into the aromatic hydrocarbon group or aromatic heterocyclic group as A and B, the activation energy Ea can be increased.
[0061] Here, the aromatic hydrocarbon group is not particularly limited, but is preferably an aryl group having 6 to 30 carbon atoms, such as a phenyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, a pyrenyl group, etc. Among these, a phenyl group is preferred because it effectively produces fluidity and non-fluidity.
[0062] The aromatic heterocyclic group is not particularly limited, but preferably has 2 to 30 carbon atoms. In addition, those with high electron donating properties are preferred, and examples thereof include, but are not limited to, thienyl, pyrrolyl, furanyl, pyrazolyl, imidazolyl, pyridyl, pyrimidinyl, pyrazinyl, triazinyl, benzothienyl, benzimidazolyl, indolyl, isoindolyl, quinolinyl, isoquinolinyl, quinazolinyl, quinoxalinyl, naphthyridinyl, acridinyl, carbazolyl, and dibenzothienyl groups. Among these, thienyl, pyrrolyl, furanyl, pyrazolyl, imidazolyl, indolyl, and carbazolyl groups are preferred because they have high activation energy and effectively fluidize and defluidize.
[0063] The above aromatic hydrocarbon group or aromatic heterocyclic group may each have a substituent. The substituent is not particularly limited, but examples thereof include a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. Preferred are a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0064] As described above, the photoinduced phase transition of azomethine derivatives is believed to occur due to the collapse of the crystal structure caused by cis-trans isomerization, as in the case of azobenzene compounds. In general, the π-π interaction between molecules is strong, so the photoinduced phase transition occurs only at the very outermost surface of the crystal structure. Here, when the aromatic hydrocarbon group or aromatic heterocyclic group represented by A or B in the above general formula (1) has a substituent, the azomethine derivative forms a specific crystal structure in which an isotropically disordered structure caused by the thermal motion of these substituents coexists in a periodic structure dominated by π-π interactions. Therefore, when the cis-trans isomerization reaction proceeds locally and the π-π interaction of the azomethine moiety is reduced, isotropic melting occurs in a chain reaction throughout the system. Therefore, it is believed that the cis-trans isomerization proceeds more easily, and fluidization is more likely to occur.
[0065] Preferably, in the general formula (1), A and B are each independently a substituted or unsubstituted phenyl group or a substituted or unsubstituted aromatic heterocyclic group. By adopting such a structure, fluidization and non-fluidization can occur more effectively.
[0066] Another preferred embodiment of the present invention is a compound in which, in the general formula (1), at least one of A and B is a phenyl group substituted with at least one substituent selected from an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms. Preferably, one of A and B is a phenyl group substituted with at least one substituent selected from an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, and a dialkylamino group having 2 to 10 carbon atoms, and the other is a substituted or unsubstituted aromatic heterocyclic group. With the above configuration, the electron density of the azomethine moiety can be increased to control the activation energy, and fluidization and reversible non-fluidization phenomena can be effectively induced. In addition, lattice defects that act favorably on cis-trans isomerization, free volume, and π-π interaction are generated. Therefore, it is considered that cis-trans isomerization is more likely to proceed and fluidization is more likely to occur. Here, the specific forms of the aromatic heterocyclic group and each of the substituents are the same as those described above.
[0067] In particular, in the general formula (1), at least one of A and B is preferably a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position to Z1 or Z2. This is believed to facilitate collapse of the crystals and facilitate fluidization by light irradiation.
[0068] In a preferred embodiment, in the above general formula (1), one of A and B is a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position to Z1 or Z2, and the other is a substituted or unsubstituted thienyl group, pyrrolyl group, pyrazolyl group, furanyl group, imidazolyl group, or indolyl group. This allows fluidization to be achieved with a lower irradiation light intensity. Among them, the above effect can be more significantly obtained in a compound in which B is a substituted or unsubstituted thienyl group, pyrrolyl group, pyrazolyl group, furanyl group, imidazolyl group, or indolyl group, Z1 is N, and Z2 is CH.
[0069] As described above, it is believed that the azomethine derivative as an isomerizable low molecular weight compound can effectively achieve fluidization and reversible non-fluidization by setting the activation energy of photoisomerization within a predetermined range. Furthermore, in the above general formula (1), it is believed that the magnitude of intermolecular interaction can be controlled by appropriately selecting A, Z1, Z2, and B, and the photomeltability can be controlled, so that the effect of the present invention can be more significantly obtained.
[0070] Examples of the azomethine derivative as the isomerizable low molecular weight compound used in the present invention include compounds 1 to 5 and 7 to 10 in which A, Z1, Z2, and B are appropriately selected in general formula (1) shown in Table 1 below.
[0071] [Table 1-1]
[0072] [Table 1-2]
[0073] [Table 1-3]
[0074] [Table 1-4]
[0075] [Table 1-5]
[0076] The synthesis method of the azomethine derivative is not particularly limited, and a conventionally known synthesis method can be applied. For example, a compound represented by the general formula (1) in which Z1 is N, Z2 is CH, A is a 4-hexyloxyphenyl group, and B is a 5-methyl-2-thienyl group can be synthesized according to the following scheme 1.
[0077] In ethanol (EtOH), 4-(hexyloxy)aniline and 5-methylthiophene-2-carboxaldehyde are reacted with each other by heating and stirring, the reaction liquid is filtered, the resulting powder is washed with cooled ethanol, and recrystallized with methanol / ethanol to obtain the target azomethine compound (see Scheme 1 below). The temperature during heating and stirring is preferably within the range of 0°C to 100°C, more preferably within the range of 30°C to 70°C, and even more preferably within the range of 40°C to 60°C.
[0078] [ka]
[0079] For example, a compound in which Z1 is N, Z2 is CH, A is a 4-hexyloxyphenyl group, and B is an N-methyl-2-pyrrolyl group in general formula (1) can be synthesized according to the following scheme 2. For example, compounds in which Z1 and Z2 are interchanged in these compounds can also be appropriately synthesized with reference to the above scheme 1 and the following scheme 2.
[0080] In ethanol (EtOH), 4-(hexyloxy)aniline and N-methyl-pyrrole-2-carboxaldehyde are reacted with each other by heating and stirring, the reaction liquid is filtered, the resulting powder is washed with cooled ethanol, and recrystallized with methanol / ethanol to obtain the target azomethine compound (see Scheme 2 below). The temperature during heating and stirring is preferably within the range of 0°C to 100°C, more preferably within the range of 30°C to 70°C, and even more preferably within the range of 40°C to 60°C.
[0081] [ka]
[0082] Azomethine derivatives other than those mentioned above can also be synthesized in a similar manner by referring to Schemes 1 and 2 above and appropriately changing the starting materials.
[0083] The above azomethine derivatives can be used alone or in combination of two or more kinds.
[0084] [Isomerized polymer] The isomerized polymer used in the composition of the present invention is a polymer that is fluidized and reversibly non-fluidized by light irradiation, and is not particularly limited as long as it has a structural unit containing an isomerized structure. In a preferred embodiment, the isomerized polymer has a structural unit containing an isomerized structure as a repeating unit. In a preferred embodiment, the isomerized polymer has a number average molecular weight of 1000 or more.
[0085] The isomerization structure is preferably a molecular structure derived from a compound that exhibits photoisomerization. For example, a molecular structure derived from a compound that exhibits cis-trans isomerization reaction upon photoirradiation can be mentioned. Examples of such compounds that exhibit cis-trans isomerization upon photoirradiation include azobenzene derivatives and azomethine derivatives, which can be introduced into the isomerization polymer as the isomerization structure. That is, as the isomerization polymer in the composition of the present invention, a polymer containing a structural unit derived from an azobenzene derivative or a structural unit derived from an azomethine derivative can be used.
[0086] (Polymers containing structural units derived from azobenzene derivatives or structural units derived from azomethine derivatives) A polymer containing a structural unit derived from an azobenzene derivative or a structural unit derived from an azomethine derivative preferably has a group represented by any one of the following formulas (i) to (iii) as a group having a polymerizable group. The polymer preferably contains a group having the following polymerizable group, since it is suitable for synthesis of a block copolymer by a living radical polymerization method. Among them, from the viewpoint of ease of softening and melting, it is preferable to contain a group having a polymerizable group of (ii) or (iii), and it is more preferable to contain a group having a polymerizable group of (iii).
[0087] [ka]
[0088] In the formulae (i) to (iii), r1 is independently a hydrogen atom or a methyl group. r2 is independently an alkylene group having 1 to 18 carbon atoms. Preferably, r2 is an alkylene group having 3 to 10 carbon atoms. The alkylene group may be linear or branched, and is preferably linear. A part of the alkylene group may be substituted with a substituent. Examples of the substituent include a halogen group, a nitro group, a hydroxy group, and a carboxy group.
[0089] As the structural unit derived from an azobenzene derivative, one having a phenylene group having a linker moiety to the polymer main chain at the para position to the nitrogen-nitrogen double bond is preferred. By introducing the above-mentioned substituent at the para position to the nitrogen-nitrogen double bond, the crystal is easily broken down and photoisomerization occurs easily, and the compound can be melted or softened by irradiation with light of lower energy. More preferred is a structure in which R3 of the compound of chemical formula (1) as the above-mentioned isomerizable low molecular weight compound is substituted with a group having a polymerizable group represented by any one of the above formulas (i) to (iii). In formula (1), R1, R2, R4 to R 10 The preferred form of the isomerized low molecular weight compound is the same as that of the compound of formula (1).
[0090] In this case, it is preferable to use a polymer containing a structural unit derived from an azobenzene derivative containing a phenylene group having a linker moiety to the polymer main chain at the para position to the nitrogen-nitrogen double bond as the isomerized polymer, and to use an azobenzene derivative or an azomethine derivative having a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position to the nitrogen-nitrogen double bond or the carbon-nitrogen double bond as the isomerized low molecular weight compound. By doing so, the crystals are easily broken, and the effect of improving the light melting property can be more significantly obtained. Therefore, the fluidization by light irradiation can be performed more efficiently.
[0091] In the polymer used in the present invention, the structural unit derived from an azomethine derivative preferably has a structure in which, in a polymer represented by the following general formula (1a), A is represented by the following general formula (2a), and a hydrogen atom is bonded in place of the oxygen atom bonded to A, and the activation energy Ea represented by the following formula (1a) is 60 kJ / mol or more.
[0092] [ka]
[0093] In the general formula (1a), r1 is a hydrogen atom or a methyl group. A is a group having an azomethine structure represented by the following general formula (2a):
[0094] [ka]
[0095] In the general formula (2a), Z1 and Z2 are each independently N or CH, and Z1≠Z2; B1 is a substituted or unsubstituted divalent aromatic hydrocarbon group or a substituted or unsubstituted divalent aromatic heterocyclic group; B2 is a substituted or unsubstituted monovalent aromatic hydrocarbon group or a substituted or unsubstituted monovalent aromatic heterocyclic group; r2 is an alkylene group having 1 to 18 carbon atoms. Equation (1a): Ea (kJ / mol) = (total energy of TS (kJ / mol)) - (total energy of cis isomer (kJ / mol)) In the above formula (1a), TS indicates a transition state represented by general formula (3a), and the cis form indicates an isomer represented by general formula (4a).
[0096] [ka]
[0097] When the energy barrier (activation energy Ea) in the isomerization reaction from cis to trans of a compound having a hydrogen atom bonded to the structure represented by the above general formula (2a) is 60 kJ / mol or more, the reaction rate of the isomerization reaction from cis to trans decreases, the amount of cis upon light irradiation increases, and fluidization accompanying the photoisomerization reaction can be induced more effectively.
[0098] In addition, while the azomethine group exhibits intermolecular packing (π-π interactions), it exhibits high thermal mobility when isomerized from the trans isomer to the cis isomer, which is thought to increase the strength of the material and make it easier to induce fluidization.
[0099] Preferably, the activation energy Ea is 63 kJ / mol or more, more preferably 65 kJ / mol or more, and even more preferably 67 kJ / mol or more. In addition, the activation energy Ea is preferably 100 kJ / mol or less, more preferably 95 kJ / mol or less, and even more preferably 90 kJ / mol or less, in view of the ease of reversion to the trans isomer. In this way, the above-mentioned effect can be more easily obtained.
[0100] In calculating the activation energy Ea of formula (1a), the structure of the transition state can be represented by general formula (3a), and the cis structure can be represented by general formula (4a). General formulas (3a) and (4a) show the arrangement (position) of B1 and B2 relative to the Z1=Z2 bond, and the positions of H, r2-H, and O-r2-H depend on the structure of group A having an azomethine structure including the B1 structure.
[0101] Here, the molecular structure and total energy of the cis isomer of the compound and the molecular structure and total energy of the transition state can be calculated using Gaussian 16 software manufactured by Gaussian, USA, and the density functional theory (B3LYP / 6-31G(d)) can be used as the calculation method. As the molecular structure of the cis isomer, the most stable molecular structure of the isomer represented by general formula (4a), i.e., the molecular structure with the lowest total energy, is calculated, and this total energy is taken as the total energy of the cis isomer. As the molecular structure of the transition state, the saddle point of the corresponding molecular structure is calculated for the transition state represented by general formula (3a), and the total energy obtained at this time is taken as the total energy of the transition state. There is no particular limitation on the software or calculation method, and similar values can be obtained using any of them. From the calculated value obtained in this way, the value of the activation energy Ea can be obtained according to the above formula (1a).
[0102] By appropriately selecting the structures of Z1, Z2, B1 and B2 in the above general formula (1a), the activation energy Ea represented by the above formula (1a) can be controlled to 60 kJ / mol or more.
[0103] Specifically, by introducing an electron-donating structure into group A having an azomethine structure, the electron density of the azomethine moiety can be increased, and the activation energy Ea can be increased. For example, by making at least one of B1 and B2 an aromatic heterocyclic group with high electron-donating properties, the activation energy Ea can be increased. In addition, by introducing a substituent with high electron-donating properties into the aromatic hydrocarbon group or aromatic heterocyclic group as B1 and B2, the activation energy Ea can be increased.
[0104] Here, preferred forms of the aromatic hydrocarbon group and aromatic heterocyclic group, and examples of substituents that can be introduced into the aromatic hydrocarbon group and aromatic heterocyclic group are the same as those of the azomethine derivatives as the above-mentioned isomerizable low molecular weight compounds.
[0105] In the structural unit represented by the above general formula (1a), one polymerizable group is provided for each group having an azomethine moiety, which makes it easy to obtain a polymer that is easily melted even with a low amount of light irradiation energy.
[0106] The group having a polymerizable group of the monomer constituting the structural unit of the general formula (1a) preferably has a group represented by any one of the above (i) to (iii). The polymers having the group having a polymerizable group correspond to the polymers in which A in the general formula (1a) is represented by the general formulas (2a-a), (2a-b), and (2a-c), respectively.
[0107] The polymer represented by the above general formula (1a) is not particularly limited and can be prepared by any method, but for example, a polymer in which A in the above general formula (1a) is represented by the above general formula (2a-a), (2a-b), or (2a-c) can be obtained by polymerizing a monomer represented by the following formula (i-2), (ii-2), or (iii-2). In the following formulas (i-2), (ii-2), and (iii-2), Z1, Z2, B1, and B2 are the same as in the above general formula (1a), and r1 and r2 are the same as in the above general formula (1a) and the above formulas (i), (ii), and (iii). That is, in one embodiment of the present invention, the polymer contains a structural unit derived from an azomethine derivative having a polymerizable group represented by the following formula (i-2), (ii-2), or (iii-2).
[0108] [ka]
[0109] In a preferred embodiment, in the general formula (1a), B1 is a phenylene group bonded to an oxygen atom (in the case of (2a-a) or (2a-c)) or r2 (in the case of (2a-b)) at the para position relative to Z1. That is, a preferred embodiment of the structural unit derived from an azomethine derivative contains a phenylene group having a linker moiety to the polymer main chain at the para position relative to the carbon-nitrogen double bond. This is thought to make the crystal more likely to collapse and more likely to become fluidized by light irradiation.
[0110] In this case, it is preferable to use a polymer containing a structural unit derived from an azomethine derivative containing a phenylene group having a linker moiety to the polymer main chain at the para position to the carbon-nitrogen double bond as the isomerized polymer, and to use an azobenzene derivative or an azomethine derivative having a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position to the nitrogen-nitrogen double bond or the carbon-nitrogen double bond as the isomerized low molecular weight compound. By doing so, the crystals are easily broken, and the effect of improving the light melting property can be more significantly obtained. Therefore, the fluidization by light irradiation can be performed more efficiently.
[0111] Another preferred embodiment of the present invention is a polymer wherein, in said general formula (1a), B1 is a phenylene group bonded to an oxygen atom (in the case of (2a-a) or (2a-c)) or r2 (in the case of (2a-b)) at the para position relative to Z1, and B2 is an aromatic heterocyclic group which is unsubstituted or substituted with any one of a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, or an alkoxycarbonyl group having 2 to 19 carbon atoms.
[0112] The above-mentioned structure can effectively induce the phenomenon of fluidization and reversible non-fluidization by light irradiation by increasing the electron density of the azomethine moiety. In addition, lattice defects that act favorably on cis-trans isomerization, free volume, and reduced π-π interactions are generated. Therefore, it is believed that cis-trans isomerization proceeds more easily and fluidization occurs more easily.
[0113] Here, in this embodiment where B1 is a phenylene group and B2 is an aromatic heterocyclic group, it is preferable that Z1 is N and Z2 is CH. In this embodiment, the aromatic heterocyclic group of B2 is preferably a substituted or unsubstituted thienyl group, pyrrolyl group, pyrazolyl group, furanyl group, imidazolyl group, or indolyl group, and particularly preferably a substituted or unsubstituted thienyl group, furanyl group, pyrazolyl group, or pyrrolyl group.
[0114] In the polymer, the structural unit represented by formula (1a) may be used alone or in combination of two or more kinds.
[0115] Specific examples of the structural unit represented by general formula (1a) include structural units 1 to 4, 6, 7, and 18 shown in Table 2 below.
[0116] [Table 2-1]
[0117] [Table 2-2]
[0118] [Table 2-3]
[0119] [Table 2-4]
[0120] [Table 2-5]
[0121] [Table 2-6]
[0122] <Method for preparing an azobenzene derivative having a polymerizable group or an azomethine derivative having a polymerizable group> The method for preparing the azobenzene derivative having a polymerizable group or the azomethine derivative having a polymerizable group is not particularly limited. For example, the desired azobenzene derivative or azomethine derivative is first prepared, and a group having a polymerizable group is introduced into the obtained azobenzene derivative or azomethine derivative to prepare the azobenzene derivative or the azomethine derivative. Hereinafter, an example of the method for preparing the azomethine derivative having a polymerizable group will be described. The azobenzene derivative having a polymerizable group can also be appropriately prepared with reference to the following scheme.
[0123] For example, in the case of preparing an azomethine derivative containing a thiophene ring, in the first step, an aniline derivative is reacted with a thiophene carboxaldehyde derivative as a compound having a thiophene ring. In this case, if either the raw material aniline derivative or the thiophene carboxaldehyde derivative has an OH group as a substituent, a polymerizable group can be easily introduced at the position of the OH group.
[0124] For example, in the case of an azomethine derivative in which Z1 in the above general formula (1a) is N, Z2 is CH, X is S, and B1 is a phenylene group, in which a group having a polymerizable group is introduced at the para-position to Z1 in the phenylene group, and B2 is a 2-methylthienyl group that is bonded to Z2 at the 5-position, intermediate A can be obtained by the following reaction formula.
[0125] Specifically, the target compound can be obtained by treating 4-hydroxyaniline and 5-methylthiophene-2-carboxaldehyde in a solvent such as ethanol (EtOH) or methanol (MeOH) (heating to reflux to cause reaction), filtering the reaction liquid, washing the resulting powder with cooled ethanol, and recrystallizing it from methanol / ethanol.
[0126] [ka]
[0127] Then, in the second step, a polymerizable group is introduced into the intermediate A. The method for introducing the polymerizable group is not particularly limited. For example, 12 When introducing -, use a halogenated alcohol compound, such as Cl-CH 12 By reacting with -OH, intermediate B shown below is obtained.
[0128] The reaction conditions are not particularly limited, but for example, the reaction is carried out in a solvent such as dimethylformamide (DMF) in the presence of potassium carbonate and potassium iodide at a temperature preferably within the range of 0°C to 100°C, more preferably within the range of 0°C to 60°C, and even more preferably within the range of 0°C to 40°C.
[0129] [ka]
[0130] Then, in the third step, the intermediate B is reacted with a compound for constituting a group having a polymerizable group, for example, acrylic acid chloride or methacrylic acid chloride. The reaction conditions are not particularly limited. For example, it is preferable to carry out the reaction in a known organic solvent in the presence of tertiary amines such as triethylamine and triethanolamine. Preferably, while keeping the mixed liquid containing the intermediate B, tertiary amines, and solvent at 0 to 10°C, a compound for constituting a group having a polymerizable group, such as acrylic acid chloride or methacrylic acid chloride, is dropped into the mixed liquid and mixed. Then, the mixed liquid is reacted at room temperature for about 5 to 10 hours, for example, to obtain an azomethine derivative having a polymerizable group.
[0131] [ka]
[0132] In addition, by changing the raw material used in the first step to another compound, an azomethine derivative having a desired substituent can be obtained. For example, by reacting a benzaldehyde derivative with an aminothiophene derivative, an azomethine derivative in which Z1 in the general formula (1a) is CH, Z2 is N, B1 is a phenylene group, and B2 is a thienyl group can be obtained. In addition, by using another aromatic hydrocarbon compound or aromatic heterocyclic compound (carboxaldehyde derivative) instead of a compound having a thiophene ring (thiophenecarboxaldehyde derivative) as a raw material, an azomethine derivative having a different structure of B2 can be obtained. Similarly, by changing the raw material aniline derivative to another aromatic hydrocarbon compound or aromatic heterocyclic compound having an amino group, an azomethine derivative having a different structure of B1 can be obtained.
[0133] In addition, groups having polymerizable groups with different structures can be introduced by changing the compounds added in the second and third steps. A person skilled in the art can synthesize an azomethine derivative having a desired polymerizable group by appropriately making the above changes and selecting appropriate reaction conditions.
[0134] In addition, by appropriately selecting the raw materials to be used in the first step, it is also possible to introduce a group having a polymerizable group into intermediate A without carrying out the second step.
[0135] <Structural units other than those containing isomerized structures> The polymer used in the present invention may contain structural units (other structural units) other than the structural units containing the isomerized structure. When the copolymer contains other structural units, the arrangement of the repeating units of the copolymer is not particularly limited, and may be any of a random copolymer, a block copolymer, and an alternating copolymer.
[0136] The other structural units are not particularly limited as long as they do not contain an isomerized structure, but are more preferably structural units that constitute a thermoplastic resin that is softened by heating.
[0137] As the other structural unit, it is preferable that it has a vinyl-based polymerizable group because it is easy to synthesize the copolymer.Specifically, for example, a styrene derivative, a (meth)acrylic acid derivative, an olefin derivative, a vinyl ester derivative, a vinyl ether derivative, a vinyl ketone derivative, etc. are used, and it is preferable that it is a structural unit derived from a styrene derivative, a (meth)acrylic acid derivative, or an olefin derivative.
[0138] Examples of styrene derivatives include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pt-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.
[0139] Examples of (meth)acrylic acid derivatives include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.
[0140] Examples of the olefin derivative include ethylene, propylene, n-butylene, isobutylene, n-pentene, 3-methyl-1-pentene, etc. The olefin derivative may be linear or branched, and the number of carbon chains is not particularly limited.
[0141] Examples of the vinyl ester derivatives include vinyl propionate, vinyl acetate, vinyl benzoate, etc. Examples of the vinyl ether derivatives include vinyl methyl ether, vinyl ethyl ether, etc. Examples of the vinyl ketone derivatives include vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc.
[0142] The content of the other structural units in the polymer is not particularly limited and can be selected as appropriate, but is preferably 70% by mass or less, and more preferably 40% by mass or less, relative to 100% by mass of the total amount of all structural units constituting the polymer.
[0143] The number average molecular weight Mn of the polymer is not particularly limited, but is preferably 1000 or more, more preferably 3500 or more, even more preferably 3500 to 100000, even more preferably 3500 to 70000, even more preferably 3500 to 50000, and particularly preferably 5000 to 50000. If the number average molecular weight of the polymer is 3500 or more, it is preferable because it is excellent in toughness and when used as a toner, a toner image with excellent fixability can be more easily obtained. In addition, if the number average molecular weight is 100000 or less, it is preferable because the efficiency of isomerization and softening and melting is high.
[0144] The number average molecular weight of the polymer can be measured by gel permeation chromatography (GPC), specifically, by the method described in the examples below.
[0145] <Method of preparing polymer> The method for synthesizing the polymer is not particularly limited, and may be a method of polymerizing a monomer such as an azomethine derivative or an azobenzene derivative having a polymerizable group by using a known polymerization initiator, such as anionic polymerization, cationic polymerization, or living radical polymerization. If necessary, a known chain transfer agent may be used.
[0146] As the polymerization initiator, for example, the following azo-based or diazo-based polymerization initiators and peroxide-based polymerization initiators can be used.
[0147] Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile.
[0148] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.
[0149] Examples of the chain transfer agent include benzyl dithiobenzoate, 1-phenylethyl dithiobenzoate, 2-phenylprop-2-yl dithiobenzoate, 1-acetoxyethyl dithiobenzoate, hexakis(thiobenzoylthiomethyl)benzene, 1,4-bis(thiobenzoylthiomethyl)benzene, 1,2,4,5-tetrakis(thiobenzoylthiomethyl)benzene, 1,4-bis-(2-(thiobenzoylthio)prop-2-yl)benzene, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate; ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)prop-2-yl dithiobenzoate, 2-cyano prop-2-yl dithiobenzoate, t-butyl dithiobenzoate, 2,4,4-trimethylpent-2-yl dithiobenzoate, 2-(4-chlorophenyl)prop-2-yl dithiobenzoate, 3- and 4-vinylbenzyl dithiobenzoate, S-benzyl diethoxyphosphinyl dithioformate, t-butyl trithioperbenzoate, 2-phenylprop-2-yl 4-chlorodithiobenzoate, 2-phenylprop-2-yl 1-dithionaphthalate, 4-cyanopentanoic acid dithiobenzoate, dibenzyl tetrathioterephthalate, dibenzyl trithiocarbonate, carboxymethyl dithiobenzoate, and the like.
[0150] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 60 hours.
[0151] Regarding the copolymer containing structural units (other structural units) other than the structural unit containing the isomerized structure, the preparation method thereof is not particularly limited.
[0152] For example, when preparing a random copolymer, the monomers for constituting the structural units including the isomerized structure as the raw material monomers, as well as the monomers for constituting the other structural units, are mixed with a chain transfer agent, a polymerization initiator, etc., and a polymerization reaction is carried out to obtain a desired copolymer. The specific form of the monomers for constituting the other structural units is as described above.
[0153] A preferred embodiment of the polymer used in the composition of the present invention is a polymer (block copolymer) represented by the following general formula (5).
[0154] [ka]
[0155] In the above general formula (5), α is a polymer block containing a structural unit containing an isomerized structure, and β is a polymer block not containing a structural unit containing an isomerized structure.
[0156] The thermal energy released during the photoexcitation and deactivation process of the isomerized structure is transferred to the repeating units (structural units) that are bonded by polymerization, and melting or softening may proceed in the polymer. In addition, by forming a block copolymer, the isomerized structure portion is likely to form a domain in the polymer, which is thought to efficiently induce softening and melting. Therefore, the effect of the present invention can be obtained even more significantly.
[0157] Of the above block copolymer structures, from the viewpoints of ease of softening and melting and image strength when used as a toner, an α-β-α (also represented as 2α-β) or β-α-β (also represented as 2β-α) block copolymer structure is preferred, and an α-β-α block copolymer structure is more preferred.
[0158] The specific form of the structural unit containing the isomerized structure constituting the polymer block α is as described above.
[0159] The structural unit constituting the polymer block β does not include an isomerized structure. Specifically, the forms described as other structural units can be preferably used. In particular, from the viewpoint of application to the synthesis of block copolymers by living radical polymerization methods such as ATRP, ARGET-ATRP, or RAFT, it is preferable that the structural unit has a vinyl-based polymerizable group. Specifically, for example, styrene derivatives, (meth)acrylic acid derivatives, olefin derivatives, vinyl ester derivatives, vinyl ether derivatives, vinyl ketone derivatives, etc. are used, and styrene derivatives, (meth)acrylic acid derivatives, or olefin derivatives are preferable. The specific forms of these are the same as those described above.
[0160] The number average molecular weight (total number average molecular weight) of the polymer block α contained in the polymer represented by the general formula (5) is not particularly limited, but is preferably 1000 or more, more preferably 1000 to 100,000, even more preferably 1000 to 70,000, even more preferably 1000 to 50,000, and particularly preferably 3000 to 50,000. If the total number average molecular weight of the polymer blocks α is 1000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. In addition, if the total number average molecular weight of the polymer blocks α is 100,000 or less, it is preferable because the efficiency of softening and melting is high. Here, the total number average molecular weight of the polymer blocks α refers to the number average molecular weight of the polymer block α when the polymer represented by the general formula (5) contains a single polymer block α, and refers to the sum of the number average molecular weights of the polymer blocks α when the polymer represented by the general formula (5) contains multiple polymer blocks α.
[0161] The number average molecular weight (total number average molecular weight) of the polymer block β contained in the polymer represented by the general formula (5) is not particularly limited, but is preferably 1000 or more, more preferably 1000 to 100,000, even more preferably 1000 to 70,000, even more preferably 1000 to 50,000, and particularly preferably 3000 to 50,000. If the total number average molecular weight of the polymer blocks β is 1000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. In addition, if the total number average molecular weight of the polymer blocks β is 100,000 or less, it is preferable because the efficiency of softening and melting is high. Here, the total number average molecular weight of the polymer blocks β refers to the number average molecular weight of the polymer block β when the polymer represented by the general formula (5) contains a single polymer block β, and refers to the sum of the number average molecular weights of the polymer blocks β when the polymer represented by the general formula (5) contains multiple polymer blocks β.
[0162] The total number average molecular weight Mn of the polymer represented by formula (5) is preferably 3500 or more, more preferably 3500 to 100000, even more preferably 3500 to 70000, even more preferably 3500 to 50000, and particularly preferably 5000 to 50000. If the total number average molecular weight of the polymer represented by formula (5) is 3500 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. If the total number average molecular weight is 100000 or less, it is preferable because the efficiency of softening and melting is high.
[0163] Therefore, according to a preferred embodiment of the present invention, the total number average molecular weight of the polymer blocks α contained in the polymer represented by general formula (5) is 1000 or more, the total number average molecular weight of the polymer blocks β is 1000 or more, and the total number average molecular weight Mn of the polymer represented by general formula (5) is 3500 or more.
[0164] In the polymer represented by general formula (5), the ratio of the total number average molecular weight of the polymer blocks α to the total number average molecular weight of the polymer blocks β is not particularly limited, but from the viewpoints of ease of softening and melting and image strength, the ratio of the total number average molecular weight of the polymer blocks α to the total number average molecular weight of the polymer blocks β is preferably 1:20 to 20:1, and more preferably 1:15 to 15:1.
[0165] The total number average molecular weight of the polymer represented by formula (5) and the total number average molecular weight of the polymer blocks α and β can be measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples below.
[0166] The method for synthesizing the block copolymer represented by the general formula (5) is not particularly limited, and known methods such as anionic polymerization, cationic polymerization, living radical polymerization, etc. can be used. Among them, as a simple synthesis method, a living radical polymerization method such as an atom transfer radical polymerization method (ATRP method), an ARGET-ATRP method, or a RAFT method can be preferably used.
[0167] Taking the ATRP method as an example, the method can be carried out by using a monofunctional, difunctional, trifunctional, or tetrafunctional compound containing a halogen element as an initiator as a starting material, and polymerizing a monomer that becomes a structural unit of the polymer block α or β in the presence of a catalyst.
[0168] In the step of polymerizing the monomer, for example, a macroinitiator is produced by polymerizing a monomer that will be a structural unit of either one of the polymer blocks α or β (the block that will be the core part of the block copolymer) in the presence of an initiator, a catalyst, and a ligand.
[0169] Examples of the initiator include, but are not limited to, 2-bromoisobutyrate butyl, 2-bromoisobutyrate ethyl, ethylene bis(2-bromoisobutyrate), 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane, pentaerythritol tetrakis(2-bromoisobutyrate), α,α'-dibromo-p-xylene, ethyl bromoacetate, 2-bromoisobutyryl bromide, and mixtures thereof.
[0170] Examples of the catalyst include copper (I) catalysts and iron (II) catalysts, such as Cu(I)Cl, Cu(I)Br, Fe(II)Cl, Fe(II)Br, and mixtures thereof.
[0171] As the ligand, known ligands can be used, but one or more selected from the group consisting of 2,2'-bipyridyl, 4,4'-dimethyl-2,2'-bipyridyl, 4,4'-di-tert-butyl-2,2'-bipyridyl, 1,1,4,7,10,10-hexamethyltriethylenetetramine, N,N,N',N",N"-pentamethyldiethylenetriamine, cyclam (1,4,8,11-tetraazacyclotetradecane), 1,4,8,11-tetramethylcyclam (1,4,8,11-tetramethyl-1,4,8,11-tetraazacyclotetradecane), tris[2-(dimethylamino)ethyl]amine, and the like are preferred.
[0172] The amounts of the catalyst and ligand used are not particularly limited, and can be appropriately determined with reference to conventionally known knowledge.
[0173] Next, the macroinitiator obtained by the above polymerization is isolated and used as an initiator, and the monomer that is to become the structural unit of the polymer block α or β, which is not used in the synthesis of the macroinitiator, is polymerized again in the presence of a catalyst and a ligand. Alternatively, when the monomers have been almost completely consumed in the synthesis of the macroinitiator, the macroinitiator may be left as it is without isolating it, and the monomer that was not used in the synthesis of the macroinitiator may be added to continue the polymerization. By these operations, the desired block copolymer can be obtained.
[0174] Each of the above reactions is preferably carried out in an inert atmosphere, such as nitrogen or a rare gas such as argon. Each of the above reactions can be carried out at a temperature of, for example, 25 to 160° C., preferably 35 to 130° C. Each of the above reactions may be carried out without using a solvent, or in a solvent such as an organic solvent.
[0175] In the reaction for obtaining a macroinitiator by polymerizing a monomer that will become a structural unit of either one of the polymer blocks α or β, and the reaction for obtaining a block copolymer by reacting the macroinitiator with a monomer that will become a structural unit of the other polymer block, the conditions such as the type and amount of catalyst and ligand used, and the reaction temperature may be the same or different.
[0176] [Mixing ratio of isomerized polymer to isomerized low molecular weight compound] In the composition of the present invention, the mixing ratio of the isomerized polymer and the isomerized low molecular weight compound is not particularly limited, but is preferably in the range of isomerized polymer:isomerized low molecular weight compound=99:1 to 10:90 in terms of mass ratio. When the isomerized polymer is 99% by mass or less with respect to 100% by mass of the total amount of the isomerized polymer and the isomerized low molecular weight compound, the effect of suppressing the amount of light irradiation required for fluidization is excellent. In addition, when it is 10% by mass or more, a composition with excellent adhesiveness can be more easily obtained. Among them, isomerized polymer:isomerized low molecular weight compound=30:70 to 90:10 is more preferable, and 40:60 to 80:20 is even more preferable.
[0177] The composition of the present invention may contain components other than the isomerized polymer and the isomerized low molecular weight compound. The specific form and content of the components other than the isomerized polymer and the isomerized low molecular weight compound are not particularly limited as long as the composition is fluidized from a solid state by light irradiation and reversibly non-fluidized.
[0178] In one embodiment, the total amount of the isomerized polymer and the isomerized low molecular weight compound is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more in the entire composition. The composition according to the present embodiment can be used as an adhesive as it is, or after adding an appropriate amount of any known additive. Similarly, the composition according to the present embodiment can be used as an optical switching material as it is, or after adding an appropriate amount of any known additive. In addition, as described later, a toner can be produced by using the composition according to the present embodiment and further using a binder resin, a colorant, etc. as necessary.
[0179] [Combination of isomerized polymer and isomerized low molecular weight compound] As the isomerized polymer and isomerized low molecular weight compound that can be used in the composition of the present invention, a polymer and a compound that are fluidized and reversibly non-fluidized by light irradiation can be used in appropriate combination. However, particularly when used in a toner, it is preferable to combine a polymer containing a structural unit derived from an azomethine derivative with an azomethine compound.
[0180] Among them, it is preferable to use a combination of a polymer containing a structural unit derived from an azomethine derivative containing a phenylene group having a linker moiety to the polymer main chain at the para position to the carbon-nitrogen double bond, and an azomethine compound containing a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position to the nitrogen-carbon double bond. This allows fluidization by light irradiation to proceed more efficiently.
[0181] In addition, it is preferable that both the structural unit derived from the azomethine derivative in the polymer and the azomethine compound contain a thiophene ring or a pyrrole ring, which allows the fluidization by light irradiation to proceed more efficiently.
[0182] [Method of preparing the composition] The method for preparing the composition of the present invention is not particularly limited. For example, an isomerized polymer and an isomerized low molecular weight compound are prepared, and then dissolved in a solvent capable of dissolving the isomerized polymer and the isomerized low molecular weight compound at a desired mixing ratio, and then the solvent is removed to dryness.
[0183] <Fluidization and reversible non-fluidization by light irradiation> The wavelength of the irradiated light when the composition of the present invention is fluidized by light irradiation is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. Within the above range, the crystals are easily broken (improved light melting property), and the fixability is improved. In addition, when fluidizing, heat or pressure may be applied in addition to light irradiation to promote fluidization. By irradiating with light of the above wavelength, even when heat or pressure is applied, it is possible to fluidize with less heat or pressure. Therefore, by introducing the composition of the present invention into a toner, fixation at the above wavelength is possible, and a toner with excellent fixability and high color reproducibility can be obtained.
[0184] The above wavelength range includes a part of visible light. Therefore, it is desirable that the composition of the present invention does not become fluid only by being exposed to sunlight (natural light) or light from a fluorescent lamp, and that the composition is made more fluid under low-cost conditions with as low an irradiation amount and irradiation time as possible. From this viewpoint, the irradiation conditions for the above-mentioned composition to become fluid include an irradiation amount of, for example, 0.1 J / cm. 2 More than 200J / cm 2 Within the following range, preferably 0.1 J / cm 2 More than 100J / cm 2 Within the range of 0.1 J / cm2 More than 50J / cm 2 Within the range below, more preferably 0.1 J / cm 2 More than 30J / cm 2 It is within the following range.
[0185] When the composition is fluidized, the composition may be heated in addition to the light irradiation. This allows the composition to be fluidized with a lower irradiation dose. The heating temperature in this case is, for example, in the range of 20°C to 200°C, preferably in the range of 20°C to 150°C.
[0186] On the other hand, the conditions for imfluidizing (resolidifying) the composition of the present invention are preferably leaving (under natural environment) at room temperature (within the range of 25±15° C.), heating, or irradiating with visible light. The wavelength and irradiation conditions of visible light when imfluidizing the composition of the present invention by irradiating with visible light are not particularly limited, but light with a longer wavelength than the wavelength of the irradiated light when fluidizing the composition of the present invention is preferred.
[0187] When the composition is heated to make it non-fluid, the heating temperature is preferably in the range of 0°C or more and 200°C or less, more preferably in the range of 20°C or more and 150°C or less, and even more preferably in the range of 20°C or more and 100°C or less.
[0188] [Toner composition] One embodiment of the present invention is a toner containing the composition of the present invention. By introducing the composition of the present invention into a toner, a toner that can be fixed by light irradiation with less energy and has excellent fixability can be obtained. The term "toner" refers to toner base particles or an aggregate of toner particles. The toner particles are preferably toner base particles to which an external additive has been added, but the toner base particles can also be used as they are as toner particles. In the present invention, when there is no particular need to distinguish between toner base particles, toner particles, and toner, they are also simply referred to as "toner".
[0189] The content of the above-mentioned composition in the toner depends on the type of the isomerized polymer and the isomerized low molecular weight compound, but from the viewpoint of efficient fluidization and image strength, it is preferable that the total amount of the isomerized polymer and the isomerized low molecular weight compound is in the range of 5 to 95 mass % with respect to the total amount of the binder resin, colorant, release agent, isomerized polymer, and isomerized low molecular weight compound constituting the toner.
[0190] When the composition of the present invention is used for a toner, the isomerized polymer is preferably a polymer containing a structural unit derived from an azomethine derivative, and the isomerized low molecular weight compound is preferably an azomethine derivative. Since the azomethine derivative does not cause significant coloring, a toner having high color reproducibility of the colorant can be obtained.
[0191] <Binding resin> The toner of the present invention may further include a binder resin. The binder resin is a resin that does not include a structure derived from an isomerized structure or a structure derived from an isomerized low molecular weight compound, and any resin generally used as a binder resin constituting a toner can be used without limitation. As the binder resin, for example, a styrene resin, an acrylic resin, a styrene-acrylic resin, a polyester resin, a silicone resin, an olefin resin, an amide resin, and an epoxy resin can be used. These binder resins can be used alone or in combination of two or more kinds.
[0192] Among these, from the viewpoint of having a low viscosity when melted and having high sharp melting properties, the binder resin preferably contains at least one selected from the group consisting of a styrene resin, an acrylic resin, a styrene-acrylic resin, and a polyester resin, and more preferably contains at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.
[0193] (styrene acrylic resin) The styrene-acrylic resin in the present invention is a polymer containing at least a structural unit derived from a styrene monomer and a structural unit derived from a (meth)acrylic acid ester monomer. Here, the styrene monomer includes not only styrene represented by the structural formula CH2=CH-C6H5, but also structures having a known side chain or functional group in the styrene structure.
[0194] Examples of the styrene monomer include the same styrene monomers capable of forming the above-mentioned polymer.
[0195] Moreover, the (meth)acrylic acid ester monomer has a functional group having an ester bond in the side chain. Specifically, in addition to the acrylic acid ester monomer represented by CH2=CHCOOR (R is an alkyl group), it includes vinyl ester compounds such as the methacrylic acid ester monomer represented by CH2=C(CH3)COOR (R is an alkyl group). Note that (meth)acrylic acid in the (meth)acrylic acid ester monomer means acrylic acid and methacrylic acid.
[0196] Examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.
[0197] The styrene monomer and the (meth)acrylic acid ester monomer can be used either alone or in combination of two or more kinds.
[0198] The content of the structural unit derived from the styrene monomer and the structural unit derived from the (meth)acrylic acid ester monomer in the styrene-acrylic resin is not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point and glass transition temperature of the binder resin. Specifically, the content of the structural unit derived from the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total structural units constituting the styrene-acrylic resin. In addition, the content of the structural unit derived from the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total structural units constituting the styrene-acrylic resin.
[0199] The styrene-acrylic resin may further contain structural units derived from other monomers than the styrene monomer and the (meth)acrylic acid ester monomer, if necessary. Examples of other monomers include vinyl monomers. Below, examples of vinyl monomers that can be used in combination when forming the styrene-acrylic copolymer of the present invention are shown, but the vinyl monomers that can be used in combination are not limited to those shown below.
[0200] (1) Olefins Ethylene, propylene, isobutylene, etc. (2) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (3) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (4) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (5) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (6)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile and acrylamide, and the like.
[0201] It is also possible to prepare a resin having a crosslinked structure by using a polyfunctional vinyl monomer. Furthermore, it is also possible to use a vinyl monomer having an ionic dissociation group in the side chain. Specific examples of the ionic dissociation group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group. Specific examples of the vinyl monomer having these ionic dissociation groups are shown below.
[0202] Specific examples of vinyl monomers having a carboxyl group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.
[0203] The preparation method of the styrene-acrylic resin is not particularly limited, and may be a method of polymerizing a monomer using a known oil-soluble or water-soluble polymerization initiator. If necessary, a known chain transfer agent such as n-octyl mercaptan or n-octyl-3-mercaptopropionate may be used. As the oil-soluble polymerization initiator, for example, an azo-based or diazo-based polymerization initiator or a peroxide-based polymerization initiator is used. The specific form of the azo-based or diazo-based polymerization initiator and the peroxide-based polymerization initiator are the same as those described in the preparation method of the polymer above.
[0204] In addition, when forming styrene-acrylic resin particles by emulsion polymerization, a water-soluble radical polymerization initiator can be used. Examples of the water-soluble radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, and hydrogen peroxide.
[0205] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 12 hours.
[0206] The styrene-acrylic resin particles formed by emulsion polymerization can be made to have two or more layers made of resins with different compositions. In this case, the manufacturing method can be a multi-stage polymerization method in which a polymerization initiator and a polymerizable monomer are added to a dispersion of resin particles prepared by emulsion polymerization treatment (first stage polymerization) according to a conventional method, and this system is polymerized (second stage, third stage polymerization).
[0207] (polyester resin) The polyester resin is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (a polyvalent carboxylic acid component) and a divalent or higher alcohol (a polyhydric alcohol component). The polyester resin may be amorphous or crystalline.
[0208] The valence of each of the polyvalent carboxylic acid component and the polyhydric alcohol component is preferably 2 to 3, and more preferably 2. That is, the polyvalent carboxylic acid component preferably contains a dicarboxylic acid component, and the polyhydric alcohol component preferably contains a dialcohol component.
[0209] Examples of the dicarboxylic acid component include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; methylenesuccinic acid, Examples of the dicarboxylic acid include unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid; unsaturated aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylenediacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and anthracenedicarboxylic acid; and lower alkyl esters and acid anhydrides of these compounds can also be used. The dicarboxylic acid component can be used alone or in combination of two or more kinds.
[0210] In addition, trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid, and their anhydrides or alkyl esters having 1 to 3 carbon atoms can also be used.
[0211] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, and neopentane. Examples of the diol component include saturated aliphatic diols such as ethyl glycol; unsaturated aliphatic diols such as 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, and 9-octadecene-7,12-diol; and aromatic diols such as bisphenols such as bisphenol A and bisphenol F, and alkylene oxide adducts of bisphenols such as ethylene oxide adducts and propylene oxide adducts thereof, and derivatives thereof can also be used. The diol component may be used alone or in combination of two or more kinds.
[0212] The method for producing the polyester resin is not particularly limited, and the polyester resin can be produced by polycondensing (esterifying) the polyvalent carboxylic acid component and the polyhydric alcohol component using a known esterification catalyst.
[0213] Examples of catalysts that can be used in the production of polyester resins include alkali metal compounds such as sodium and lithium; compounds containing group 2 elements such as magnesium and calcium; compounds of metals such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds. Specifically, examples of tin compounds include dibutyltin oxide (dibutyltin oxide), tin octoate, tin dioctoate, and salts thereof. Examples of titanium compounds include titanium alkoxides such as tetra-normal-butyl titanate (Ti(On-Bu)4), tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanolamine. Examples of germanium compounds include germanium dioxide. Examples of aluminum compounds include polyaluminum hydroxide, aluminum alkoxide, and tributylaluminate. These may be used alone or in combination of two or more.
[0214] The polymerization temperature is not particularly limited, but is preferably 70 to 250° C. The polymerization time is also not particularly limited, but is preferably 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0215] When the toner of the present invention contains a binder resin in addition to the composition of the present invention, the content ratio of the composition to the binder resin is not particularly limited.
[0216] The toner of the present invention may be particles having a single layer structure or particles having a core-shell structure. The types of binder resins used for the core particles and shell part of the core-shell structure are not particularly limited.
[0217] <Coloring agent> The toner of the present invention may further contain a colorant. As the colorant, generally known dyes and pigments can be used.
[0218] Examples of colorants for obtaining black toner include carbon black, magnetic materials, iron-titanium composite oxide black, etc. Examples of carbon black include channel black, furnace black, acetylene black, thermal black, and lamp black, and examples of magnetic materials include ferrite and magnetite.
[0219] Colorants for obtaining yellow toners include dyes such as CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; and pigments such as CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, and 185.
[0220] Colorants for obtaining magenta toner include dyes such as CI Solvent Red 1, 49, 52, 58, 63, 111, and 122; and pigments such as CI Pigment Red 5, 48:1, 53:1, 57:1, 122, 139, 144, 149, 166, 177, 178, and 222.
[0221] Colorants for obtaining cyan toner include dyes such as CI Solvent Blue 25, 36, 60, 70, 93, and 95; and pigments such as CI Pigment Blue 1, 7, 15, 15:3, 60, 62, 66, and 76.
[0222] The colorants for obtaining the toner of each color may be used alone or in combination of two or more kinds for each color.
[0223] The content of the colorant in the toner particles (toner base particles) before addition of external additives is preferably 0.5 to 20% by mass, and more preferably 2 to 10% by mass.
[0224] <Release agent> The toner according to the present invention may further contain a release agent. By incorporating a release agent into the toner, a toner having superior fixability and color reproducibility can be obtained when thermal fixing is performed together with light irradiation.
[0225] The release agent used is not particularly limited, and various known waxes can be used. Examples of the wax include polyolefins such as low molecular weight polypropylene, polyethylene, or oxidized low molecular weight polypropylene, polyethylene, paraffin wax, and synthetic ester wax. Among them, it is preferable to use paraffin wax from the viewpoint of improving the storage stability of the toner.
[0226] The content of the release agent in the toner base particles is preferably 1 to 30% by mass, and more preferably 3 to 15% by mass.
[0227] <Charge control agent> The toner according to the present invention may contain a charge control agent. The charge control agent used is a substance capable of imparting positive or negative charge by frictional charging, and is colorless, and is not particularly limited. Any of various known positively and negatively chargeable charge control agents can be used.
[0228] The content of the charge control agent in the toner base particles is preferably 0.01 to 30% by mass, and more preferably 0.1 to 10% by mass.
[0229] <External additives> In order to improve the fluidity, chargeability, cleaning properties, etc. of the toner, external additives such as a fluidizing agent, a cleaning aid, etc., which are so-called post-treatment agents, may be added to the toner base particles to form the toner according to the present invention.
[0230] Examples of the external additive include inorganic oxide particles such as silica particles, alumina particles, and titanium oxide particles, inorganic stearic acid compound particles such as aluminum stearate particles and zinc stearate particles, and inorganic titanic acid compound particles such as strontium titanate particles and zinc titanate particles. If necessary, these inorganic particles may be hydrophobized. These may be used alone or in combination of two or more.
[0231] Among these, preferred external additives are, for example, sol-gel silica particles, silica particles whose surfaces have been hydrophobized (hydrophobic silica particles), or titanium oxide particles (hydrophobic titania particles), and it is more preferred to use at least two or more types of external additives among these.
[0232] The number average primary particle size of the external additive is preferably within the range of 1 to 200 nm, and more preferably 10 to 180 nm.
[0233] The amount of these external additives added is preferably 0.05 to 5% by mass, and more preferably 0.1 to 3% by mass, in the toner.
[0234] <Average particle size of toner> The average particle size of the toner (and the average particle size of the toner base particles) is preferably 4 to 20 μm, more preferably 5 to 15 μm, in terms of volume-based median diameter (D50). When the volume-based median diameter (D50) is within the above range, the transfer efficiency is increased, and the image quality of halftones and fine lines, dots, etc. is improved.
[0235] The volume-based median diameter (D50) can be measured and calculated using a measuring device consisting of a "Coulter Counter 3" (Beckman Coulter, Inc.) connected to a computer system (Beckman Coulter, Inc.) equipped with the data processing software "Software V3.51."
[0236] Specifically, 0.02 g of the measurement sample (toner or toner base particles) is added to 20 mL of surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing surfactant components 10 times with pure water in order to disperse toner particles), and after mixing, ultrasonic dispersion is performed for 1 minute to prepare a dispersion liquid. This dispersion liquid is then pipetted into a beaker containing an "ISOTON II" (manufactured by Beckman Coulter, Inc.) in the sample stand until the concentration indicated on the measuring device reaches 8%.
[0237] Here, by setting the display concentration to the above value, a reproducible measurement value can be obtained. In the measurement device, the number of measured particles is set to 25,000, the aperture diameter is set to 50 μm, the measurement range of 1 to 30 μm is divided into 256 parts to calculate the frequency value, and the particle size of the largest volume cumulative fraction, which is 50%, is set as the volume-based median diameter (D50).
[0238] [Toner manufacturing method] The method for producing the toner of the present invention is not particularly limited. For example, when the toner is made from only the composition of the present invention, a production method including pulverizing the composition using an apparatus such as a hammer mill, a feather mill, or a counter jet mill, and then classifying the particles to a desired particle size using a dry classifier such as a spin air sieve, a classifier, or a micron classifier can be used. When a toner further containing a colorant is produced, the composition and the colorant are dissolved in a solvent in which both the composition and the colorant are soluble to obtain a solution, the solvent is removed, and the solution is then pulverized and classified in the same manner as above.
[0239] In particular, the toner containing the composition of the present invention and, if necessary, a binder resin and a colorant is preferably produced by a production method utilizing an emulsion aggregation method, which allows easy control of particle size and shape.
[0240] Such a manufacturing method is as follows: (1A) A binder resin particle dispersion preparation step of preparing a binder resin particle dispersion as required. (1B) A composition particle dispersion preparation step for preparing a dispersion of particles of the composition of the present invention (1C) A colorant particle dispersion preparation step of preparing a colorant particle dispersion as required. (2) An association step in which a flocculant is added to an aqueous medium in which composition particles, and optionally binder resin particles and colorant particles, are present, and salting out is promoted while simultaneously flocculation and fusion are carried out to form associated particles. (3) Aging process to form toner base particles by controlling the shape of aggregated particles (4) A filtering and washing process for filtering the toner base particles from the aqueous medium and removing surfactants and the like from the toner base particles. (5) A drying process for drying the washed toner base particles. (6) Additive addition step of adding additives to the dried toner base particles It is preferable that the method includes each of the steps of:
[0241] The steps (1A) to (1C) are described below.
[0242] (1A) Binder resin particle dispersion preparation process In this process, resin particles are formed by a conventional emulsion polymerization or the like, and the resin particles are aggregated and fused to form binder resin particles. As an example, polymerizable monomers constituting the binder resin are introduced into an aqueous medium, dispersed therein, and polymerized by a polymerization initiator to prepare a dispersion of binder resin particles.
[0243] As a method for obtaining a binder resin particle dispersion, in addition to the above-mentioned method of polymerizing a polymerizable monomer in an aqueous medium by a polymerization initiator, for example, a method of performing a dispersion treatment in an aqueous medium, or a method of dissolving a crystalline resin in a solvent such as ethyl acetate to prepare a solution, emulsifying and dispersing the solution in an aqueous medium using a disperser, and then performing a solvent removal treatment, can be mentioned.
[0244] In this case, if necessary, a release agent may be added to the binder resin in advance. For dispersion, it is also preferable to carry out the polymerization in the presence of a known surfactant (e.g., anionic surfactants such as polyoxyethylene (2) dodecyl ether sodium sulfate, sodium dodecyl sulfate, and dodecylbenzenesulfonic acid).
[0245] The volume-based median diameter of the binder resin particles in the dispersion is preferably 50 to 300 nm. The volume-based median diameter of the binder resin particles in the dispersion can be measured by a dynamic light scattering method using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).
[0246] (1B) Composition particle dispersion preparation process The composition particle dispersion preparation step is a step of dispersing the composition of the present invention in the form of fine particles in an aqueous medium to prepare a dispersion of particles of the composition.
[0247] In preparing a dispersion of particles of the composition, first, an emulsion of the composition is prepared. For example, the emulsion of the composition can be prepared by dissolving the composition in an organic solvent and then emulsifying the obtained solution in an aqueous medium.
[0248] The method of dissolving the composition in an organic solvent is not particularly limited, and examples thereof include a method of adding the composition to an organic solvent and stirring and mixing the composition so that the composition is dissolved. The amount of the composition added is preferably 5 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the organic solvent.
[0249] Next, the obtained solution of the composition is mixed with an aqueous medium and stirred using a known dispersing machine such as a homogenizer, whereby the composition becomes droplets and is emulsified in the aqueous medium, thereby preparing an emulsion of the composition.
[0250] The amount of the solution of the composition added is preferably 10 parts by mass or more and 110 parts by mass or less with respect to 100 parts by mass of the aqueous medium.
[0251] The temperatures of the composition solution and the aqueous medium when the composition solution and the aqueous medium are in a temperature range below the boiling point of the organic solvent, and are preferably from 20° C. to 80° C., more preferably from 30° C. to 75° C. When the composition solution and the aqueous medium are mixed, the temperatures of the composition solution and the aqueous medium may be the same or different, and are preferably the same.
[0252] Regarding the stirring conditions of the dispersing machine, when the capacity of the stirring vessel is 1 to 3 L, for example, the rotation speed is preferably 7000 rpm or more and 20000 rpm or less, and the stirring time is preferably 10 minutes or more and 30 minutes or less.
[0253] The dispersion of the particles of the composition is prepared by removing the organic solvent from the emulsion of the composition. Examples of the method for removing the organic solvent from the emulsion of the composition include known methods such as blowing air, heating, reducing pressure, or a combination of these.
[0254] As an example, the emulsion of the composition is heated, for example, in an inert gas atmosphere such as nitrogen, preferably at 25° C. to 90° C., more preferably at 30° C. to 80° C., until, for example, about 80% by mass to 95% by mass of the initial amount of organic solvent is removed, thereby removing the organic solvent. As a result, the organic solvent is removed from the aqueous medium, and a dispersion of particles of the composition in which particles of the composition are dispersed in the aqueous medium is prepared.
[0255] The mass average particle diameter of the particles of the composition in the dispersion of the particles of the composition is preferably 90 nm or more and 1200 nm or less. The mass average particle diameter can be set within the above range by appropriately adjusting the viscosity when the composition is mixed with an organic solvent, the mixing ratio of the solution of the composition to the aqueous medium, the stirring speed of a dispersing machine when preparing an emulsion of the composition, etc. The mass average particle diameter of the particles of the composition in the dispersion of the particles of the polymer can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0256] <Organic solvent> The organic solvent used in this step is not particularly limited as long as it can dissolve the polymer and the compound in the composition.Specific examples include esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, diisopropyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, saturated hydrocarbons such as hexane and heptane, and halogenated hydrocarbons such as dichloromethane, dichloroethane, and carbon tetrachloride.
[0257] Such organic solvents can be used alone or in combination of two or more kinds. Among these organic solvents, ketones and halogenated hydrocarbons are preferred, and methyl ethyl ketone and dichloromethane are more preferred.
[0258] <Aqueous medium> The aqueous medium used in this step may be water, or an aqueous medium containing water as the main component and water-soluble solvents such as alcohols and glycols, and optional components such as surfactants and dispersants. The aqueous medium used is preferably a mixture of water and a surfactant.
[0259] Examples of the surfactant include cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of the cationic surfactant include dodecyl ammonium chloride, dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, and hexadecyl trimethyl ammonium bromide. Examples of the anionic surfactant include fatty acid soaps such as sodium stearate and sodium dodecanoate, sodium dodecyl benzene sulfonate, and sodium dodecyl sulfate. Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl ether, polyoxyethylene sorbitan monooleate ether, and monodecanoyl sucrose.
[0260] Such surfactants can be used alone or in combination of two or more. Among the surfactants, anionic surfactants are preferred, and sodium dodecylbenzenesulfonate is more preferred.
[0261] The amount of the surfactant added is preferably from 0.01 to 10 parts by mass, more preferably from 0.04 to 1 part by mass, based on 100 parts by mass of the aqueous medium.
[0262] (1C) Colorant particle dispersion preparation process The colorant particle dispersion preparation step is a step of dispersing a colorant in the form of fine particles in an aqueous medium to prepare a colorant particle dispersion.
[0263] The colorant can be dispersed by utilizing mechanical energy. The median diameter based on the number of colorant particles in the dispersion is preferably 10 to 300 nm, and more preferably 50 to 200 nm. The median diameter based on the number of colorant particles can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0264] The steps from (2) association step to (6) external additive addition step can be carried out according to various conventionally known methods.
[0265] The flocculant used in the (2) association step is not particularly limited, but is preferably selected from metal salts. Examples of metal salts include monovalent metal salts such as salts of alkali metals such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum. Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, and manganese sulfate. Among these, it is particularly preferable to use divalent metal salts because they can promote flocculation with a smaller amount. These can be used alone or in combination of two or more.
[0266] [Developer] The toner according to the present invention can be suitably used, for example, when it contains a magnetic material and is used as a one-component magnetic toner, when it is mixed with a so-called carrier and is used as a two-component developer, or when it is used alone as a non-magnetic toner.
[0267] As the magnetic material, for example, magnetite, γ-hematite, or various ferrites can be used.
[0268] The carrier contained in the two-component developer may be magnetic particles made of conventionally known materials such as metals such as iron, steel, nickel, cobalt, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead.
[0269] The carrier may be a coated carrier in which the surface of a magnetic particle is coated with a coating agent such as a resin, or a resin-dispersed carrier in which a magnetic powder is dispersed in a binder resin. The resin for coating is not particularly limited, but for example, an olefin resin, an acrylic resin, a styrene resin, a styrene-acrylic resin, a silicone resin, a polyester resin, or a fluororesin is used. The resin for constituting the resin-dispersed carrier particles is not particularly limited, and a known resin can be used, for example, an acrylic resin, a styrene-acrylic resin, a polyester resin, a fluororesin, or a phenolic resin can be used.
[0270] The volume-based median diameter of the carrier is preferably 20 to 100 μm, and more preferably 25 to 80 μm. The volume-based median diameter of the carrier can be measured typically by a laser diffraction particle size distribution measuring device "HELOS" (manufactured by SYMPATEC) equipped with a wet disperser.
[0271] The mixed amount of the toner is preferably 2 to 10% by mass, with the total mass of the toner and carrier being 100% by mass.
[0272] [Image forming method] The toner of the present invention can be used in various known electrophotographic image forming methods. For example, it can be used in monochrome image forming methods and full-color image forming methods. In the full-color image forming method, it can be applied to any image forming method, such as a four-cycle image forming method that is composed of four types of color developing devices for yellow, magenta, cyan, and black, and one photoconductor, and a tandem image forming method that is equipped with image forming units having color developing devices and photoconductors for each color, respectively.
[0273] An image forming method according to one embodiment of the present invention includes the steps of 1) forming a toner image made of the toner of the present invention on a recording medium, and 2) irradiating the toner image with light to soften the toner image. This embodiment provides excellent fixability and high image quality.
[0274] Regarding step 1) In this process, a toner image made of the toner of the present invention is formed on a recording medium.
[0275] (Recording medium) The recording medium is a member for holding a toner image. Examples of the recording medium include plain paper, high-quality paper, art paper, coated printing paper such as coated paper, commercially available Japanese paper and postcard paper, resin films for overhead projectors or packaging materials, and cloth.
[0276] The recording medium may be in the form of a sheet (foliage) having a predetermined size, or may be in the form of a long piece that is wound up in a roll after the toner image is fixed thereon.
[0277] As described later, the toner image can be formed, for example, by transferring the toner image on the photoconductor onto a recording medium.
[0278] Regarding step 2) In this process, the formed toner image is irradiated with light to soften the toner image, which allows the toner image to adhere to a recording medium.
[0279] The wavelength of the light to be irradiated is not particularly limited as long as it can sufficiently soften the toner image by photothermal conversion of the compounds and polymers contained in the composition in the toner, but is preferably 280 nm or more and 480 nm or less. If it is within the above range, the toner image can be softened more efficiently. From the same viewpoint, the amount of light irradiation is preferably 0.1 to 200 J / cm. 2 , more preferably 0.1 to 100 J / cm 2 , and more preferably 0.1 to 50 J / cm 2 It is.
[0280] As described later, the light irradiation can be performed using a light source such as a light emitting diode (LED) or a laser light source. In addition, as described later, heating may be further performed in addition to the light irradiation.
[0281] After the step 2), if necessary, a step 3) of pressing the softened toner image may be further carried out. This embodiment improves the fixing property.
[0282] Regarding step 3) In this process, the softened toner image is pressed.
[0283] The pressure when pressing the toner image on the recording medium is not particularly limited, but is preferably 0.01 to 5.0 MPa, and more preferably 0.05 to 1.0 MPa. By setting the pressure to 0.01 MPa or more, the deformation amount of the toner image can be increased, so that the contact area between the toner image and the recording paper S increases, and it is easy to further improve the fixability of the image. In addition, by setting the pressure to 5.0 MPa or less, shock noise during pressing can be suppressed.
[0284] The pressurizing step may be carried out before or simultaneously with the step of irradiating light and softening the toner image (step 2) described above), but it is preferable to carry it out after the light irradiation, since this allows pressure to be applied to the toner image that has already been softened, thereby further improving the fixability of the image.
[0285] In addition, in the pressurizing step, the softened toner image may be further heated. That is, the pressurizing step may be performed while heating the toner image. The temperature at that time (for example, the temperature of the pressing member) is preferably 15°C or higher, more preferably 20°C or higher, even more preferably more than 20°C, even more preferably 30°C or higher, and even more preferably 40°C or higher. This embodiment significantly improves the fixability. There is no particular upper limit, but it is, for example, 200°C or lower, 150°C or lower, or 100°C or lower.
[0286] The heating temperature of the toner image (the surface temperature of the toner image during heating) is preferably (Tg+20) to (Tg+100)° C., and more preferably (Tg+25) to (Tg+80)° C., where Tg is the glass transition temperature of the toner. If the surface temperature of the toner image is (Tg+20)° C. or higher, the toner image is easily deformed by pressure, and if it is (Tg+100)° C. or lower, hot offset is easily suppressed. Note that hot offset refers to a phenomenon in which part of the toner is transferred to a pressure member such as a roller during the fixing process, causing the toner layer to break up.
[0287] In addition, before the step 2), a step 4) of heating the toner image in advance may be further carried out as necessary. In this way, by further carrying out the step 4) of heating the toner image in advance before the step 2), the sensitivity of the compound of the present invention to light can be further increased. As a result, even if the compound is a polymer, the sensitivity to light is unlikely to be impaired, and therefore, the melting or softening of the toner image by light irradiation can be easily promoted.
[0288] Fig. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. However, the image forming apparatus used in the present invention is not limited to the following form and illustrated example. Fig. 1 shows an example of a monochrome image forming apparatus 100, but the present invention can also be applied to a color image forming apparatus.
[0289] The image forming apparatus 100 is an apparatus for forming an image on a recording paper S as a recording medium, and is equipped with an image reading device 71 and an automatic document feeder 72, and performs image formation on the recording paper S transported by a paper transport system 7 using an image forming unit 10, an irradiation unit 40, and a pressing unit 9.
[0290] Furthermore, while image forming apparatus 100 uses recording paper S as a recording medium, the medium on which an image is formed may be something other than paper, as described above.
[0291] An original d placed on the platen of the automatic document feeder 72 is scanned and exposed by the optical system of the scanning exposure device of the image reading device 71 and read into the image sensor CCD. An analog signal photoelectrically converted by the image sensor CCD is subjected to analog processing, A / D conversion, shading correction, image compression processing, etc. in the image processing unit 20, and then input to the exposure device 3 of the image forming unit 10.
[0292] The paper transport system 7 includes a plurality of trays 16, a plurality of paper feed units 11, transport rollers 12, a transport belt 13, etc. The trays 16 each store recording paper S of a predetermined size, and operate the paper feed unit 11 of the specified tray 16 in response to an instruction from the control unit 90 to supply the recording paper S. The transport rollers 12 transport the recording paper S sent out from the tray 16 by the paper feed unit 11 or the recording paper S brought in from the manual paper feed unit 15 to the image forming unit 10.
[0293] The image forming unit 10 is configured with a charger 2, an exposure unit 3, a developing unit 4, a transfer unit 5, a charge removal unit (not shown) and a cleaning unit 8 arranged in this order around the photoconductor 1 along the direction of rotation of the photoconductor 1.
[0294] The photoconductor 1, which is an image carrier, is an image carrier having a photoconductive layer formed on its surface, and is configured to be rotatable in the direction of the arrow in Fig. 1 by a driving device (not shown). A thermo-hygrometer 17 that detects the temperature and humidity inside the image forming apparatus 100 is provided near the photoconductor 1.
[0295] The charger 2 uniformly charges the surface of the photoreceptor 1, thereby uniformly charging the surface of the photoreceptor 1. The exposure unit 3 is equipped with a beam emission source such as a laser diode, and irradiates the charged surface of the photoreceptor 1 with a beam of light, thereby dissipating the charge in the irradiated area and forming an electrostatic latent image on the photoreceptor 1 according to the image data. The development unit 4 supplies the toner contained therein to the photoreceptor 1, and creates a toner image on the surface of the photoreceptor 1 based on the electrostatic latent image.
[0296] The transfer unit 5 faces the photoreceptor 1 via the recording paper S, and transfers the toner image onto the recording paper S. The charge removing unit removes charge from the photoreceptor 1 after the toner image has been transferred. The cleaning unit 8 includes a blade 85. The blade 85 cleans the surface of the photoreceptor 1 to remove any developer remaining on the surface of the photoreceptor 1.
[0297] The recording paper S onto which the toner image has been transferred is transported by a transport belt 13 to a pressing unit 9. The pressing unit 9 may be installed arbitrarily, and performs a fixing process on the recording paper S onto which the toner image has been transferred by applying pressure alone or heat and pressure with pressure members 91 and 92, thereby fixing the image onto the recording paper S. The recording paper S onto which the image has been fixed is transported by transport rollers to a paper discharge unit 14, and is discharged from the paper discharge unit 14 to the outside of the machine.
[0298] In addition, the image forming apparatus 100 is equipped with a paper inversion section 24, so that the recording paper S that has been subjected to the heat fixing process is transported to the paper inversion section 24 just before the paper discharge section 14, and the recording paper S is either inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10, so that images can be formed on both sides of the recording paper S.
[0299] <Irradiation unit> FIG. 2 is a schematic diagram of the irradiation unit 40 in the image forming apparatus 100. As shown in FIG.
[0300] An image forming apparatus 100 according to an embodiment of the present invention includes an irradiation section 40. The irradiation section 40 includes a light source 41 and a heating member 93. Examples of devices constituting the light source 41 include a light emitting diode (LED) and a laser light source.
[0301] The light source 41 irradiates the toner image formed on the recording medium with light to soften the toner image. The conditions of the light irradiation are not particularly limited as long as they melt and fluidize the composition of the present invention contained in the toner of the developer. The wavelength of the light irradiated to the toner image may be sufficient to sufficiently fluidize the composition, and is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. The amount of light irradiated by the light source 41 may also be sufficient to sufficiently fluidize the composition, and is, for example, 0.1 J / cm. 2 More than 200J / cm 2 Within the range below, preferably 0.1 J / cm 2 More than 100J / cm 2 Within the range of 0.1 J / cm 2 More than 50J / cm 2 Within the range below, more preferably 0.1 J / cm 2 More than 30J / cm 2 It is within the following range.
[0302] When the toner image is softened by irradiating the toner image with light from the light source 41, the toner image may be heated by the heating member 93 in addition to the light irradiation. This allows the toner image to be softened and melted more efficiently. The heating temperature at this time is, for example, in the range of 20° C. to 200° C., and preferably in the range of 20° C. to 150° C.
[0303] The softened toner image can be solidified and fixed to the recording medium by leaving it at room temperature (within the range of 25±15° C.), heating it, or irradiating it with visible light. As described below, the fixing step preferably further includes a step of applying pressure to the softened toner image. In the pressurizing step, it is preferable to further heat the softened toner image.
[0304] Light source 41 irradiates light toward a first surface of recording paper S holding a toner image, which is on the photoreceptor side, and is disposed on the photoreceptor side with respect to the surface of recording paper S nipped between photoreceptor 1 and transfer roller 5, which is a transfer section. A heating member 93 is disposed on the opposite side of light source 41 with respect to the surface of recording paper S. Light source 41 and heating member 93 are disposed along the transport direction of recording paper S (paper transport direction).
[0305] The light source 41 and the heating member 93 are disposed downstream of the nip position between the photoconductor 1 and the transfer roller 5 in the paper transport direction and upstream of the pressure bonding unit 9 in the paper transport direction.
[0306] According to an image forming method according to an embodiment of the present invention, the photoconductor 1 is charged by applying a uniform potential to it using the charger 2, and then the photoconductor 1 is scanned with a light beam irradiated by the exposure device 3 based on original image data to form an electrostatic latent image. Next, the developing unit 4 supplies a developer having a toner containing the composition of the present invention onto the photoconductor 1.
[0307] When the recording paper S is transported from the tray 16 to the image forming unit 10 in time with the rotation of the photoconductor 1 causing the toner image carried on the surface of the photoconductor 1 to reach the position of the transfer roller 5, which is the transfer unit, the toner image on the photoconductor 1 is transferred onto the recording paper S, which is nipped between the transfer roller 5 and the photoconductor 1, by the transfer bias applied to the transfer roller 5.
[0308] The transfer unit 5 also functions as a pressure member, and can reliably bring the toner image into close contact with the recording paper S while transferring the toner image from the photoconductor 1 to the recording paper S.
[0309] After the toner image is transferred onto the recording paper S, the blade 85 of the cleaning unit 8 removes the developer remaining on the surface of the photoconductor 1 .
[0310] In the process in which the recording paper S onto which the toner image has been transferred is transported by the transport belt 13 to the pressing unit 9, the light source 41 irradiates light onto the toner image transferred onto the recording paper S. By irradiating light onto the toner image on the first side of the recording paper S from the light source 41, the toner image can be melted more reliably, and the fixability of the toner image to the recording paper S can be improved.
[0311] When the recording paper S carrying the toner image reaches the pressing unit 9 by the conveyor belt 13, the pressure members 91 and 92 press the toner image onto the first side of the recording paper S. Before the toner image is fixed by the pressing unit 9, the toner image is softened by being irradiated with light by the light source 41, so that it is possible to save energy in pressing the image onto the recording paper S. Furthermore, in the process of solidifying the toner image and fixing it to the recording medium, the toner image is pressed by the pressure members 91 and 92, so that the fixability of the toner image onto the recording paper S is further improved.
[0312] The pressure when pressing the toner image on the recording medium is not particularly limited, but is preferably 0.01 to 5.0 MPa, and more preferably 0.05 to 1.0 MPa. By setting the pressure to 0.01 MPa or more, the deformation amount of the toner image can be increased, so that the contact area between the toner image and the recording paper S increases, and it is easy to further improve the fixability of the image. In addition, by setting the pressure to 5.0 MPa or less, shock noise during pressing can be suppressed.
[0313] In the pressurizing step, it is preferable to further heat the toner image. By applying pressure and heat by pressure members 91 and 92, the fixability of the toner image to the recording paper S is further improved. Specifically, when the recording paper S passes between the pressure members 91 and 92, the toner image softened by light irradiation is pressurized by pressure member 91 in a state further softened by heating, thereby further improving the fixability of the toner image to the recording paper S.
[0314] The heating temperature during the further heating in the pressurizing step is preferably 15° C. or higher, more preferably 20° C. or higher, even more preferably more than 20° C., even more preferably 30° C. or higher, and even more preferably 40° C. or higher. This embodiment significantly improves the fixability. There is no particular upper limit, but it is, for example, 200° C. or lower, 150° C. or lower, or 100° C. or lower.
[0315] The toner image pressed by the pressure members 91 and 92 is solidified and fixed onto the recording paper S.
[0316] That is, in one embodiment of the present invention, the fixing device has a pressure bonding section equipped with a pressure member. Also, in one embodiment of the present invention, the pressure member has a heating means.
[0317] In one embodiment of the present invention, the temperature of the pressure member is preferably 15° C. or higher, more preferably 20° C. or higher, even more preferably more than 20° C., even more preferably 30° C. or higher, and even more preferably 40° C. or higher. There is no particular upper limit, but it is, for example, 200° C. or lower, 150° C. or lower, or 100° C. or lower.
[0318] When forming images on both sides of the recording paper S, the recording paper S that has been subjected to the pressure bonding process is transported to the paper inversion section 24 just before the paper discharge section 14, and either inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10.
[0319] (Photoresponsive adhesive) The composition of the present invention becomes fluid when irradiated with light and becomes non-fluid reversibly, so that a photoresponsive adhesive (photosensitive adhesive) that can be used repeatedly can be produced using the composition of the present invention. For example, it can be applied to various adhesion techniques as a photoresponsive adhesive that can be repeatedly attached and detached by light in response to changes in viscosity (friction coefficient). That is, one embodiment of the present invention is a photoresponsive adhesive that includes the composition of the present invention.
[0320] The light-responsive adhesive of the present invention can be used for temporary fixing that allows repeated use, and is also suitable for recycling, but is not limited thereto.
[0321] (Photoswitching Materials) The composition of the present invention is fluidized by light irradiation and reversibly non-fluidized, so that a light-switching material can be prepared using the composition of the present invention. For example, a light-switching material can be prepared by utilizing the change in color or polarity, mass transfer, change in orientation, change in viscosity, or change in surface tension that accompanies photoisomerization. For example, in liquid crystal materials, it is possible to apply the composition to patterning drawings that can be repeatedly rewritten in response to the change in molecular orientation that accompanies photoisomerization. In addition, for example, the change in surface tension that accompanies light irradiation and the resulting mass transfer can be utilized to perform microfabrication of the surface of a polymer film. That is, one embodiment of the present invention is a light-switching material that includes the composition of the present invention.
[0322] The optical switching material of the present invention can be used for liquid crystal display materials and surface processing of polymer films, but is not limited thereto. EXAMPLES
[0323] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0324] First, compounds 1, 2, 6 and 10 shown in Table 1 above and polymers 1 to 3 and 5 to 18 shown in Table 3 below, which contain structural units 1 to 3, 5 and 18 shown in Table 2 above, were prepared.
[0325] [Synthesis of compound 1] 4-Hexyloxyaniline (7.7mmol), 5-methylthiophene-2-carboxaldehyde (7.7mmol), and 20ml of ethanol were added to a 100ml four-neck flask equipped with a cooling tube, nitrogen inlet tube, and thermometer, and heated and stirred. The reaction solution was suction filtered, and the resulting powder was washed with cooled ethanol. Further, recrystallization was performed with methanol / ethanol to obtain the target compound 1 in a yield of 42%.
[0326] [ka]
[0327] 1 The formation of compound 1 was confirmed by 1 H NMR. 1 H NMR (400MHz, CDCl3); 8.35ppm(s,1H,CH=N), 7.39ppm(d,2H,aryl), 7.08ppm(d,1H,thiophene), 6.96ppm(d,2H,aryl), 6.67ppm(d,2H,thiophene), 4.11ppm (t,2H,methylene), 2.44ppm(s,3H,methyl), 1.80ppm(m,2H,methylene), 1.47ppm(m,2H,methylene), 1.37ppm(m,4H,methylene), 0.89ppm(t,3H,methyl).
[0328] [Synthesis of compound 2] Compound 2 was synthesized in the same manner as in the synthesis of compound 1, except that 5-methylthiophene-2-carboxaldehyde (7.7 mmol) was replaced with N-methylpyrrole-2-carboxaldehyde (7.7 mmol). 1 The production of the compound was confirmed by 1 H NMR, and it was found that the target compound was obtained.
[0329] [Synthesis of compound 10] Compound 10 was synthesized in the same manner as in the synthesis of compound 1, except that 5-methylthiophene-2-carboxaldehyde (7.7 mmol) was replaced with 1-methyl-1H-pyrazole-4-carboxaldehyde (7.7 mmol). 1 The production of the compound was confirmed by 1 H NMR, and it was found that the target compound was obtained.
[0330] [Synthesis of compound 6] 75 mL of 2.4N hydrochloric acid was added to 4-aminophenol (6.54 g, 60 mmol), and then a solution of sodium nitrite (4.98 g, 72 mmol) dissolved in 6 mL of distilled water was added while cooling and stirring at 0 ° C., and stirring was continued at 0 ° C. for 60 minutes. A mixed solution of o-cresol (6.48 g, 60 mmol) and 24 mL of 20% aqueous sodium hydroxide solution was added to this solution and stirred for 20 hours. The precipitate was filtered, and the solid was washed with water. The obtained solid was purified by silica gel column chromatography using a mixture of ethyl acetate and hexane as a developing solvent, and recrystallized with a mixture of acetone and hexane to obtain intermediate A. 100 mL of DMF, 1-bromohexane (9.9 g, 60 mmol), and potassium carbonate (6.9 g, 50 mmol) were added to this intermediate A (2.28 g, 10 mmol), and the mixture was stirred at 80 ° C. for 2 hours, and then stirred at room temperature for 20 hours. After the solvent was removed under reduced pressure, the mixture was extracted with ethyl acetate, the organic layer was washed with saturated saline and then dried over anhydrous magnesium sulfate, filtered, the solvent was removed under reduced pressure, and the resulting solid was purified by silica gel column chromatography using a mixture of ethyl acetate and hexane as a developing solvent to obtain compound 6, an azobenzene derivative.
[0331] [ka]
[0332] [Synthesis of polymer 1] (Synthesis of azomethine derivative monomer 1) 4-Aminophenol (5 g, 0.046 mol), 5-methylthiophene-2-carboxaldehyde (5.8 g, 0.046 mol), and 100 ml of ethanol were added to a 100 ml four-neck flask and heated and stirred. The reaction solution was suction filtered, and the resulting powder was washed with cooled ethanol. Further, recrystallization was performed with methanol / ethanol to obtain target product 1.
[0333] [ka]
[0334] Next, in a 200 ml four-neck flask, the target product 1 (5 g, 0.023 mol) obtained above was dissolved in 25 ml of dimethylformamide (DMF). To this, 4.88 g (0.035 mol) of potassium carbonate was added, and the mixture was stirred while maintaining the temperature at 30°C. To this, 10.2 mg (0.06 mmol) of potassium iodide and 6-chloro-1-hexanol (3.54 g, 0.026 mol) were added, and the mixture was reacted at 110°C. This was cooled to room temperature, added to 650 g of ice, and then filtered. The crystals were dispersed in 400 ml of water, stirred overnight, washed, filtered, and dried. Furthermore, recrystallization was performed with ethanol to obtain target product 2.
[0335] [ka]
[0336] Next, the target product 2 (3 g, 0.001 mol) obtained above, 1.34 ml (0.001 mol) of triethylamine, and 30 ml of dichloromethane were added to a 100 ml four-neck flask. At this time, the raw materials were in a dispersed state. While maintaining the internal temperature at 0°C, a solution of 1.04 g (0.011 mol) of acrylic acid chloride dissolved in 10 ml of dichloromethane was added dropwise while maintaining the internal temperature at 0 to 5°C. As the mixture was added dropwise, the raw materials dissolved.
[0337] After the dropwise addition, the reaction solution was returned to room temperature and stirred. After the reaction was completed, dichloromethane was removed by concentration, and the solution was dissolved in ethyl acetate and washed with dilute hydrochloric acid, aqueous sodium bicarbonate solution, and saturated saline. The organic layer was dried over magnesium sulfate and then concentrated. The orange crystals obtained were purified using a silica gel column (ethyl acetate / heptane=1 / 5) to obtain azomethine derivative monomer 1 having structural unit 1.
[0338] [ka]
[0339] (Synthesis of Polymer 1) In a 100 ml four-neck flask, 1.5 g (4.096 mmol) of the azomethine derivative monomer 1 obtained above, 5 mg (0.023 mmol) of 4-cyanopentanoic acid dithiobenzoate, and 1 mg (0.006 mmol) of AIBN were dissolved in 4 ml of anisole. Then, after creating an argon gas atmosphere by freeze degassing, the mixture was heated to 75°C and polymerized by stirring. 40 ml of methanol was gradually added dropwise to the obtained polymer solution, and then THF was added to remove unreacted azomethine derivative monomer 1. The separated polymer solution was dried in a vacuum drying oven at 40°C for 24 hours to obtain polymer 1. The number average molecular weight Mn of the obtained polymer 1 was measured by GPC method and found to be 12,000.
[0340] [ka]
[0341] [Synthesis of polymers 2, 3, and 18] Polymers 2, 3, and 18 having structural units 2, 3, and 18 were obtained using the same synthesis method as for polymer 1 using the corresponding raw materials.
[0342] Specifically, polymer 2 was synthesized in the same manner as polymer 1, except that in the synthesis of azomethine derivative monomer 1, 4-aminophenol was changed to 3-aminophenol.
[0343] Polymer 3 was synthesized in the same manner as polymer 1, except that in the synthesis of azomethine derivative monomer 1, 5-methylthiophene-2-carboxaldehyde was changed to N-hexylpyrrole-3-carboxaldehyde.
[0344] Polymer 18 was synthesized in the same manner as polymer 1, except that in the synthesis of azomethine derivative monomer 1, 5-methylthiophene-2-carboxaldehyde was changed to 1-methyl-1H-pyrazole-4-carboxaldehyde and 6-chloro-1-hexanol was changed to 10-chloro-1-decanol.
[0345] In the preparation of Polymers 2, 3, 18 and the following polymers, the amount of each raw material added and the reaction conditions were appropriately adjusted as necessary.
[0346] [Synthesis of polymer 5] In a dark room under an argon stream, 4-hexylaniline (11 g, 0.0643 mol) and 100 ml of acetone were added, and 26 ml of HCl aq. was added dropwise while cooling. NaNO2 aq. (NaNO2 4.6 g / H2O 10 ml) was further added dropwise, and the mixture was stirred at 0°C or less for 30 minutes. 26 ml of 20% NaOH aq. and 6 g of phenol were added dropwise to this preparation solution, and the mixture was stirred at room temperature. Then, 64 ml of HCl aq. was added dropwise, and the mixture was separated into toluene and water. The obtained organic layer was purified using a silica gel column (toluene) to obtain the target product 1'.
[0347] [ka]
[0348] Next, azobenzene derivative monomer 5 was obtained in the same manner as in the synthesis of azomethine derivative monomer 1, except that target substance 1' prepared above was used instead of target substance 1 and 10-chloro-1-decanol was used instead of 6-chloro-1-hexanol. Polymer 5 was obtained in the same manner as in the synthesis of polymer 1, except that azobenzene derivative monomer 5 was used instead of azomethine derivative monomer 1.
[0349] [Synthesis of polymers 6-9] Polymers 6 to 8 were prepared in the same manner as in the synthesis of polymer 1, except that the amount of azomethine derivative monomer 1 was changed from 1.5 g to 1.2 g, and 0.3 g each of styrene, ethyl acrylate, and n-butyl methacrylate were added. Polymer 9 was prepared in the same manner as in the synthesis of polymer 1, except that the amount of azomethine derivative monomer 1 was changed from 1.5 g to 1.2 g, and 0.15 g of styrene and 0.15 g of methyl acrylate were added.
[0350] [Synthesis of polymer 10] <Synthesis of macroinitiator 10> In a 100 ml eggplant flask, 2,2'-bipyridyl (230 mg, 1.47 mmol) was added, and in a glove box under a nitrogen atmosphere, Cu(I)Br (95 mg, 0.66 mmol), styrene (15 g, 144 mmol), and ethyl 2-bromoisobutyrate (35 mg, 0.18 mmol) were added and sealed. This was heated and stirred in an oil bath at 100°C. Then, an appropriate amount of tetrahydrofuran was added, and the mixture was passed through a neutral alumina column. This was purified by reprecipitation with methanol and centrifugation to obtain macroinitiator 10. The number average molecular weight (β Mn) of the obtained macroinitiator 10 was measured by GPC method and found to be 1100.
[0351] <Synthesis of polymer 10> In a 100 ml eggplant flask, the above-obtained azomethine derivative monomer 1 (16 g, 38 mmol) and the above-mentioned macroinitiator 10 (0.92 g, 0.18 mmol) were placed, and in a glove box under a nitrogen atmosphere, Cu(I)Cl (29 mg, 0.29 mmol), 1,1,4,7,10,10-hexamethyltriethylenetetramine (136 mg, 0.59 mmol), and anisole (4.9 g, 41.1 mmol) as a solvent were added and sealed. Then, the mixture was heated and stirred in an oil bath at 80°C. Then, an appropriate amount of chloroform was added, and the mixture was passed through a basic alumina column. The mixture was purified by reprecipitation with methanol and centrifugation to obtain polymer 10. The total number-average molecular weight Mn of the obtained polymer 10 was 5600 when measured by the GPC method. From this, the number-average molecular weight (α Mn) of the structural unit derived from the azomethine derivative was determined to be 4500.
[0352] [Synthesis of polymer 11] <Synthesis of macroinitiator 11> Macroinitiator 11 was obtained in the same manner as in the synthesis of macroinitiator 10, except that ethyl 2-bromoisobutyrate was changed to α,α'-dibromo-p-xylene.
[0353] <Synthesis of Polymer 11> Polymer 11 was obtained in the same manner as in the synthesis of Polymer 10, except that macroinitiator 10 was changed to macroinitiator 11.
[0354] [Synthesis of polymer 12] <Synthesis of macroinitiator 12> Macroinitiator 12 was obtained in the same manner as in the synthesis of macroinitiator 10, except that ethyl 2-bromoisobutyrate was changed to ethylene bis(2-bromoisobutyrate), 2,2'-bipyridyl was changed to 1,1,4,7,10,10-hexamethyltriethylenetetramine, styrene was changed to azomethine derivative monomer 1, and anisole was further added.
[0355] <Synthesis of polymer 12> Polymer 12 was obtained in the same manner as in the synthesis of polymer 10, except that macroinitiator 10 was changed to macroinitiator 12, 1,1,4,7,10,10-hexamethyltriethylenetetramine was changed to 2,2'-bipyridyl, azomethine derivative monomer 1 was changed to styrene, and anisole was omitted.
[0356] [Synthesis of polymer 13] <Synthesis of macroinitiator 13> In the synthesis of macroinitiator 10, by appropriately adjusting the time of heating and stirring in a 100°C oil bath, macroinitiator 13 was obtained which has the same structure as macroinitiator 10 and a number average molecular weight (β Mn) of 7000.
[0357] <Synthesis of polymer 13> In the synthesis of polymer 10, the time of heating and stirring in an 80°C oil bath was appropriately adjusted to obtain polymer 13, which is composed of structural units similar to those of polymer 10 and has a total number average molecular weight Mn of 7500. In polymer 13, the number average molecular weight (α Mn) of the structural units derived from the azomethine derivative was 500.
[0358] [Synthesis of polymer 14] <Synthesis of macroinitiator 14> Macroinitiator 14 was obtained in the same manner as in the synthesis of macroinitiator 11, except that styrene was changed to methyl acrylate.
[0359] <Synthesis of polymer 14> Polymer 14 was obtained in the same manner as in the synthesis of Polymer 11, except that Macroinitiator 11 was changed to Macroinitiator 14.
[0360] [Synthesis of polymer 15] <Synthesis of macroinitiator 15> Macroinitiator 15 was obtained in the same manner as in the synthesis of macroinitiator 11, except that styrene was changed to n-hexyl methacrylate.
[0361] <Synthesis of polymer 15> Polymer 15 was obtained in the same manner as in the synthesis of Polymer 11, except that Macroinitiator 11 was changed to Macroinitiator 15.
[0362] [Synthesis of polymer 16] <Synthesis of macroinitiator 16> Macroinitiator 16 was obtained in the same manner as in the synthesis of macroinitiator 11, except that styrene was changed to 3-methyl-1-pentene.
[0363] <Synthesis of polymer 16> Polymer 16 was obtained in the same manner as in the synthesis of Polymer 11, except that Macroinitiator 11 was changed to Macroinitiator 16.
[0364] [Synthesis of polymer 17] <Synthesis of macroinitiator 17> Macroinitiator 17 was obtained in the same manner as in the synthesis of macroinitiator 11, except that styrene was changed to a mixture of styrene:methyl acrylate in a molar ratio of 5:5.
[0365] <Synthesis of polymer 17> Polymer 17 was obtained in the same manner as in the synthesis of Polymer 11, except that Macroinitiator 11 was changed to Macroinitiator 17.
[0366] [Preparation of Compositions 1 to 25] The compounds 1, 2, 6, and 10 and polymers 1 to 3 and 5 to 18 prepared above were dissolved in an appropriate amount of THF in the ratios (mass ratios) in Table 3 below, and dried to obtain compositions 1 to 25.
[0367] The following Table 3 shows the compounds and polymers constituting compositions 1 to 25. In Table 3, compounds 1, 2, 6, and 10 are compounds 1, 2, 6, and 10 in the above-mentioned Table 1. Furthermore, the structural unit numbers constituting polymers 1 to 3 and 5 to 18 correspond to the structural unit numbers in the above-mentioned Table 2.
[0368] [Preparation of Toner 1] <Preparation of Composition Particle Dispersion 1> 80 parts by mass of dichloromethane and 20 parts by mass of the composition 1 obtained above were mixed and stirred while being heated at 50°C to obtain a solution containing composition 1. A mixed liquid of 99.5 parts by mass of distilled water heated to 50°C and 0.5 parts by mass of a 20% by mass aqueous solution of sodium dodecylbenzenesulfonate was added to 100 parts by mass of the obtained solution. Thereafter, the mixture was emulsified by stirring at 16000 rpm for 20 minutes using a homogenizer (manufactured by Heidolph) equipped with a shaft generator 18F, to obtain an emulsion of composition 1.
[0369] The obtained emulsion was placed in a separable flask, and the organic solvent was removed by heating and stirring at 40° C. for 90 minutes while supplying nitrogen into the gas phase, to obtain composition particle dispersion 1. The particle size of the composition particles in composition particle dispersion 1 was measured using an electrophoretic light scattering photometer “ELS-800” (manufactured by Otsuka Electronics Co., Ltd.) and found to be 155 nm in mass average particle size.
[0370] (Preparation of Black Colorant Particle Dispersion (Bk-1)) 11.5 parts by mass of sodium n-dodecyl sulfate was dissolved in 160 parts by mass of pure water, 25 parts by mass of carbon black "Mogul L (manufactured by Cabot Corporation)" was gradually added, and then the mixture was dispersed using "Clearmix (registered trademark) W Motion CLM-0.8 (manufactured by M Technique Co., Ltd.)" to prepare a black colorant particle dispersion (Bk-1). The volume-based median diameter of the colorant particles in the black colorant particle dispersion (Bk-1) was 110 nm.
[0371] <Preparation of Toner 1> The above-prepared composition particle dispersion 1 (602 parts by mass in terms of solid content), black colorant particle dispersion (Bk-1) (52 parts by mass in terms of solid content), and ion-exchanged water (900 parts by mass) were charged into a reaction device equipped with a stirrer, a temperature sensor, and a cooling tube. The temperature inside the container was kept at 30° C., and a 5 mol / L aqueous solution of sodium hydroxide was added to adjust the pH to 10.
[0372] Next, an aqueous solution of 2 parts by mass of magnesium chloride hexahydrate dissolved in 1000 parts by mass of ion-exchanged water was added dropwise under stirring over a period of 10 minutes, and then heating was started. The temperature of this system was raised to 70°C over a period of 60 minutes, and the particle growth reaction was continued while maintaining the temperature at 70°C. In this state, the particle size of the associated particles was measured using a "Multisizer 3" (manufactured by Beckman Coulter, Inc.), and when the volume-based median diameter (D50) reached 6.5 μm, an aqueous solution of 190 parts by mass of sodium chloride dissolved in 760 parts by mass of ion-exchanged water was added to stop the particle growth. After stirring at 70°C for 1 hour, the temperature was further raised, and the particles were heated and stirred at 75°C to promote fusion of the particles. The mixture was then cooled to 30°C to obtain a dispersion of toner base particles.
[0373] The obtained dispersion liquid of the toner base particles was subjected to solid-liquid separation using a centrifuge to form a wet cake of the toner base particles. The wet cake was washed with ion-exchanged water at 35°C until the electrical conductivity of the filtrate in the centrifuge reached 5 μS / cm, and then transferred to a "Flash Jet Dryer (manufactured by Seishin Enterprise Co., Ltd.)" and dried until the moisture content reached 0.5% by mass to produce the toner base particles.
[0374] To 100% by mass of the obtained toner base particles, 1% by mass of hydrophobic silica (number average primary particle size: 12 nm) and 0.3% by mass of hydrophobic titania (number average primary particle size: 20 nm) were added and mixed using a Henschel mixer (registered trademark), thereby obtaining toner 1.
[0375] [Preparation of Toners 2 to 23, 26, 27, and Comparative Examples 1 and 2] Toners 2 to 23, 26, and 27 were obtained in the same manner as in the preparation of Toner 1 above, except that composition 1 was changed to compositions 2 to 25. The toners of Comparative Examples 1 and 2 were prepared according to the compositions shown in Table 4 below.
[0376] [Preparation of Toner 24] Toner 24 was obtained in the same manner as in the preparation of Toner 1, except that the amount of polymer particle dispersion 1 was changed from 602 parts by mass to 421 parts by mass in terms of solid content, and 181 parts by mass of the following styrene-acrylic resin particle dispersion was added in terms of solid content.
[0377] <Preparation of styrene acrylic resin particle dispersion> (First stage polymerization) A solution of 8 parts by mass of sodium dodecyl sulfate dissolved in 3000 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirring device, a temperature sensor, a cooling tube, and a nitrogen introduction device, and the internal temperature was raised to 80 ° C. while stirring at a stirring speed of 230 rpm under a nitrogen gas flow. After the temperature was raised, a solution of 10 parts by mass of potassium persulfate dissolved in 200 parts by mass of ion-exchanged water was added, the liquid temperature was again raised to 80 ° C., and a polymerizable monomer solution consisting of 480 parts by mass of styrene, 250 parts by mass of n-butyl acrylate, 68.0 parts by mass of methacrylic acid, and 16.0 parts by mass of n-octyl-3-mercaptopropionate was dropped over 1 hour, and the mixture was heated and stirred at 80 ° C. for 2 hours to polymerize, thereby preparing a styrene acrylic resin particle dispersion liquid (1A) containing styrene acrylic resin particles (1a).
[0378] (Second stage polymerization) A solution of 7 parts by mass of sodium polyoxyethylene (2) dodecyl ether sulfate dissolved in 800 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98°C. After that, a polymerizable monomer solution of 260 parts by mass of the styrene acrylic resin particle dispersion (1A) obtained above, 245 parts by mass of styrene, 120 parts by mass of n-butyl acrylate, 1.5 parts by mass of n-octyl-3-mercaptopropionate, and 67 parts by mass of paraffin wax "HNP-11" (manufactured by Nippon Seiro Co., Ltd.) as a release agent was added at 90°C, and the mixture was mixed and dispersed for 1 hour using a mechanical disperser "CREARMIX (registered trademark)" (manufactured by M Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). Next, an initiator solution prepared by dissolving 6 parts by mass of potassium persulfate in 200 parts by mass of ion-exchanged water was added to this dispersion, and the system was heated and stirred at 82°C for 1 hour to carry out polymerization, thereby preparing a styrene-acrylic resin particle dispersion (1B) containing styrene-acrylic resin particles (1b).
[0379] (Third stage polymerization) A solution of 11 parts by mass of potassium persulfate dissolved in 400 parts by mass of ion-exchanged water was added to the obtained styrene-acrylic resin particle dispersion liquid (1B), and then a polymerizable monomer solution consisting of 435 parts by mass of styrene, 130 parts by mass of n-butyl acrylate, 33 parts by mass of methacrylic acid, and 8 parts by mass of n-octyl-3-mercaptopropionate was added dropwise over 1 hour at a temperature condition of 82° C. After the dropwise addition was completed, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28° C. to obtain a styrene-acrylic resin particle dispersion liquid containing styrene-acrylic resin 1.
[0380] [Preparation of Toner 25] Toner 25 was obtained in the same manner as in preparation of Toner 1, except that the amount of polymer particle dispersion 1 was changed from 602 parts by mass to 421 parts by mass in terms of solid content, and 181 parts by mass of the following polyester resin particle dispersion was added in terms of solid content.
[0381] (Preparation of polyester resin particle dispersion containing polyester resin) In a 10-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 524 parts by mass of bisphenol A propylene oxide 2-mol adduct, 105 parts by mass of terephthalic acid, 69 parts by mass of fumaric acid, and 2 parts by mass of tin octylate (esterification catalyst) were added, and a polycondensation reaction was carried out at a temperature of 230°C for 8 hours. The polycondensation reaction was further continued at 8 kPa for 1 hour, and then cooled to 160°C to obtain polyester resin 1. 100 parts by mass of polyester resin 1 was pulverized with a "Landermill Type: RM" (manufactured by Tokuju Machinery Co., Ltd.), mixed with 638 parts by mass of a 0.26% by mass aqueous solution of sodium lauryl sulfate prepared in advance, and ultrasonically dispersed for 30 minutes at V-LEVEL and 300 μA using an ultrasonic homogenizer "US-150T" (manufactured by Nippon Seiki Co., Ltd.) while stirring, to obtain a polyester resin particle dispersion. The particle size of the polyester resin particles in the polyester resin particle dispersion was measured by dynamic light scattering using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.), and the volume-based median diameter was 135 nm.
[0382] (Number average molecular weight Mn) The number average molecular weights Mn of the polymers 1 to 3 and 5 to 18 prepared above were measured by the GPC method. Specifically, an apparatus "HLC-8120GPC" (manufactured by Tosoh Corporation) and a column "TSKguardcolumn+TSKgelSuperHZ-M3 series" (manufactured by Tosoh Corporation) were used, and tetrahydrofuran (THF) was passed as a carrier solvent at a flow rate of 0.2 mL / min while maintaining the column temperature at 40°C. The measurement sample was dissolved in tetrahydrofuran to a concentration of 1 mg / ml. The solution was prepared by treating the solution at room temperature for 5 minutes using an ultrasonic disperser. Then, the sample solution was treated with a membrane filter having a pore size of 0.2 μm to obtain a sample solution, and 10 μL of this sample solution was injected into the apparatus together with the above carrier solvent and detected using a refractive index detector (RI detector). The molecular weight distribution of the measurement sample was calculated based on a calibration curve prepared using monodisperse polystyrene standard particles. Ten polystyrene points were used for the above calibration curve measurement.
[0383] In addition to the total number average molecular weight, the number average molecular weight of the macroinitiator was also measured by the above method for polymers 10 to 17. The number average molecular weight of the macroinitiator was taken as the number average molecular weight of polymer block α or β, and the total number average molecular weight of the other polymer block (number average molecular weight of the other polymer block × number of blocks) was obtained by subtracting (number average molecular weight of macroinitiator × number of blocks) from the total number average molecular weight of the polymer for each block structure. The results are shown in Table 3 below. In Table 3, Mn represents the total number average molecular weight of the polymer, αMn represents the total number average molecular weight of polymer block α, and βMn represents the total number average molecular weight of polymer block β.
[0384] [Evaluation: Photoresponsive adhesion test of composition] The change in adhesiveness of compositions 1 to 25 prepared in each example with light irradiation was evaluated by the following photoresponsive adhesive test using the apparatus shown in FIG. 3. As shown in FIG. 3, 2 mg of the composition was placed on a 18 mm square cover glass 1 within a radius of 6 mm from the center of the glass, and a cover glass 2 of the same size was placed at a position shifted about 4 mm in a parallel direction to the cover glass 1 so as to completely cover the composition. This was heated to melt the sample, and the cover glass 1 and the cover glass 2 were bonded together. Each of the obtained samples was subjected to the following non-fluidity → fluidity test, and then the following fluidity → non-fluidity test.
[0385] <Testing non-fluidity to fluidity (fluidity test)> Part (A) shown in Figure 3 was fixed to the stand with cellophane tape, and a 30 cm long vinyl string with a 100 g weight attached was fixed to part (C) with cellophane tape. Part (B) was irradiated with light of 365 nm wavelength at a dose of 30 J / cm. 2 It was confirmed whether cover glass 2 peeled off from cover glass 1, and the peeling was judged according to the following evaluation criteria.
[0386] - Evaluation criteria for testing non-liquidity to liquidity (fluidity test) - ○: Cover glass 2 was completely peeled off from cover glass 1 △: Cover glass 2 is displaced ×: The cover glass 2 did not move.
[0387] <Testing from liquidity to non-liquidity (non-liquidity test)> After the non-fluidity → fluidity test was completed, the following experiment was performed on the samples in which the cover glass 2 had been completely peeled off and on the samples in which it had shifted. For the shifted samples, the cover glasses 1 and 2 were peeled off by hand. Five minutes after the light irradiation in the non-fluidity → fluidity test had finished (the sample was left for five minutes at room temperature (within the range of 25±15°C) and exposed to visible light such as fluorescent light), a cover glass 3 (same size as cover glasses 1 and 2) was placed so as to cover the sample portion (part (B)) of the cover glass 1 used in the above test, and it was confirmed whether the cover glass 1 and the cover glass 3 were adhered to each other, and a judgment was made according to the following evaluation criteria.
[0388] -Evaluation criteria for liquidity to non-liquidity testing (non-liquidity testing)- 〇: Did not adhere (had become non-fluid) △: Partially adhered (partially maintained in a fluid state) ×: Adhered (fluid state was maintained).
[0389] All of compositions 1 to 25 containing an isomerized polymer and an isomerized low molecular weight compound were evaluated as having an excellent result in the fluidization test and the non-fluidization test, and it was confirmed that the compositions were fluidized and non-fluidized reversibly when irradiated with light.
[0390] [Evaluation: Fixation test] (Preparation of developer) For the toners 1 to 27 and the toners of Comparative Examples 1 and 2 prepared above, ferrite carrier particles with a volume average particle size of 30 μm coated with a copolymer resin of cyclohexane methacrylate and methyl methacrylate (monomer mass ratio 1:1) were mixed so that the toner particles were 6 mass %, thereby obtaining developers 1 to 27 and the developers of Comparative Examples 1 and 2. Mixing was performed for 30 minutes using a V-type mixer.
[0391] (Fixation test) The fixing property test was carried out under normal temperature and humidity conditions (temperature 20°C, relative humidity 50% RH) using the developers 1 to 27 obtained above and the developers of Comparative Examples 1 and 2. Specifically, the developer was placed on one side and plain paper (basis weight: 64 g / m 2 The developer is placed between a pair of parallel flat plate (aluminum) electrodes with a magnetic force, and the gap between the electrodes is 0.5 mm. The DC bias and AC bias are used to control the toner adhesion amount to 6 g / m. 2 The toner was developed under the above conditions, a toner image was formed on the surface of the plain paper, and the toner image was fixed by each fixing device to obtain a printed matter (image formation).
[0392] The printed matter was folded by a folding machine under a load, and then compressed air of 0.45 MPa was blown onto the image area. The folded area was ranked according to the following evaluation criteria, with rank 3 or higher being considered acceptable.
[0393] 6: No creases at all 5: Very slight peeling along the fold 4: Some peeling along the fold 3: Fine linear peeling along the fold 2: Thick linear peeling along the fold 1: Large peeling along the fold.
[0394] The fixing devices used were the following four types of fixing devices configured by appropriately modifying the device shown in FIG. 2: No. 1: There is no pressure bonding portion 9 in FIG. 2, the temperature of the heating member 93 is 20° C., the wavelength of the ultraviolet light irradiated from the light source 41 is 365 nm (light source: LED light source with an emission wavelength of 365 nm±10 nm), and the irradiation amount is 7 J / cm 2 and 11 J / cm 2 is; No. 2: The pressing unit 9 in FIG. 2 is included, the temperature of the heating member 93 is 20° C., the temperature of the pressure member 91 is 20° C., and the pressure during pressing is 0.2 MPa. The wavelength and irradiation amount of the light source 41 are the same as those of No. 1; No. 3: The pressing unit 9 in FIG. 2 is included, the temperature of the heating member 93 is 20° C., the temperature of the pressure member 91 is 80° C., and the pressure during pressing is 0.2 MPa. The wavelength and irradiation amount of the light source 41 are the same as those of No. 1; No. 4: There is no pressure bonding portion 9 in FIG. 2, the temperature of the heating member 93 is 80° C., and the wavelength and irradiation amount of the light source 41 are the same as those of No. 1.
[0395] [Color reproducibility evaluation] The color reproducibility of the images obtained in the above examples and comparative examples was evaluated by visual evaluation by 10 monitors according to the following evaluation criteria. Specifically, as a sample for evaluation comparison, a toner was prepared in which all of the polymer 1 in Example 1 was replaced with a styrene acrylic resin. Using this, a developer was prepared in the same manner as above, and development was performed in the same manner as in the image formation in the fixing property test above, and fixing was performed using the fixing device No. 5 described below: Fixing device No. 5: The pressing unit 9 in FIG. 2 was included, the temperature of the heating member 93 was 20° C., the temperature of the pressure member 91 was 150° C., the pressure during pressing was 0.2 MPa, and no light irradiation was performed.
[0396] The 10 monitors were shown the sample for evaluation and comparison, and the images obtained in the above-mentioned Examples and Comparative Examples in turn, and asked whether the colors of the two images were clearly different. The results of the judgment based on the following color reproducibility evaluation criteria are shown in Table 4 below: -Evaluation criteria for color reproducibility- ◎: Less than 2 people answered that it was clearly different ○: 3 to 4 people answered that it was clearly different △: 5 to 7 people answered that it was clearly different ×: Eight or more people answered that it was clearly different.
[0397] The results are shown in Tables 3 and 4 below.
[0398] [Table 3]
[0399] [Table 4-1]
[0400] [Table 4-2]
[0401] As shown in Table 4, all of the toners 1 to 27 using the composition of the present invention could be fixed by light irradiation and showed high fixability.
[0402] Toners 1 to 3, 26, and 27 using compositions 1 to 3, 24, and 25 containing a polymer having a structural unit derived from an azomethine derivative and an azomethine compound, toner 4 using composition 4 containing a polymer having a structural unit derived from an azobenzene derivative and an azobenzene compound, toner 5 using composition 5 containing a polymer having a structural unit derived from an azobenzene derivative and an azomethine compound, and toner 6 using composition 6 containing a polymer having a structural unit derived from an azomethine derivative and an azobenzene compound all showed high fixing ability when irradiated with light.
[0403] On the other hand, as in Comparative Examples 1 and 2, the toners prepared using only polymer 5 or only compound 6 had insufficient fixing properties. In particular, it was found that the fixing properties were poor when the light irradiation dose was low. From this, it was confirmed that the use of a combination of a polymer and a compound allows fixing at a low light irradiation dose compared to the use of each alone.
[0404] It has been found that toners 1 to 6 using compositions 1 to 6, in which the structural units in the polymer contain a phenylene group having a linker moiety to the polymer main chain at the para position to the nitrogen-nitrogen double bond or carbon-nitrogen double bond of an azobenzene derivative or the azomethine derivative, and the azobenzene compound or azomethine compound contains a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position to the nitrogen-nitrogen double bond or the nitrogen-carbon double bond, have superior fixing properties at a low irradiation dose compared to toner 11 using composition 11 containing polymer 2 containing a phenylene group having a linker moiety at the meta position.
[0405] As long as the mixing ratio of the polymer to the compound in the composition was within the range of polymer:compound=99:1 to 10:90 (mass ratio), good fixability was obtained (Examples 1, 7 to 10). In particular, it was found that the fixability was better when the polymer:compound was within the range of 30:70 to 90:10, and was even better when the polymer:compound was within the range of 40:60 to 80:20.
[0406] Good fixability was obtained when the polymer was a homopolymer, a random copolymer, or a block copolymer. In particular, toners 1 to 6, 16 to 18, 20 to 23, 26, and 27 using a composition using a homopolymer or a block copolymer as the polymer tend to have better fixability at a low irradiation dose than toners 12 to 15 using a random copolymer. If the number average molecular weight of the polymer is 3500 or more, and if the polymer is a block copolymer, the total number average molecular weight of each polymer block is 1000 or more, better fixability can be obtained.
[0407] In addition to the composition, a binder resin can be further contained in the toner. It was confirmed that when a binder resin was further used as in toners 24 and 25, good fixing properties were also obtained.
[0408] Comparing the fixing devices, it was found that the fixing performance was higher when the fixing device No. 2, which applied pressure with a pressure member, and the fixing device No. 3, which applied pressure while heating with a pressure member, were used than when the fixing device No. 1 was used, irradiated with ultraviolet light under the same conditions, and did not use a pressure member (Comparison of Examples 1, 26, and 27). Also, the fixing performance was higher when the fixing device No. 4, which heated with the heating member 93, was used than when the fixing device No. 1 was used, irradiated with ultraviolet light under the same conditions, and did not heat during ultraviolet light irradiation (Examples 1 and 28).
[0409] Moreover, it was found that the toners 1 to 3 and 7 to 27, which used the compositions 1 to 3 and 7 to 25 containing an azomethine compound and a polymer containing a structural unit derived from an azomethine derivative, were excellent in color reproducibility. [Explanation of symbols]
[0410] 1 photoreceptor, 2 Charger, 3 Exposure device, 4 Development section, 5 Transcription unit, 7 Paper transport system, 8 Cleaning section, 9 Crimping section, 10 Image forming unit, 11 Paper feed section, 12 Transport roller, 13 conveyor belt, 14 Paper ejection section, 15 Manual feed unit, 16 trays, 17 Thermohygrometer, 20 Image processing unit, 24 Paper reversing section, 40 Irradiation unit, 41 light source, 71 Image reading device, 72 Automatic document feeder, 85 blades, 90 control section, 91, 92 Pressurizing member, 93 Heating element, 100 Image forming apparatus, d manuscript, S Recording paper.
Claims
1. An isomerized polymer including a structural unit including an isomerized structure, and an isomerized low molecular weight compound, the isomerized polymer is a polymer containing a structural unit derived from an azomethine derivative, and the isomerized low molecular weight compound is an azomethine compound, The azomethine derivative comprises a phenylene group having a linker moiety to a polymer backbone at the para position relative to a carbon-nitrogen double bond; the azomethine compound contains a phenyl group having an alkyl group having 1 to 18 carbon atoms or an alkoxy group having 1 to 18 carbon atoms at the para position relative to the nitrogen-carbon double bond; A composition which becomes fluid from a solid state upon irradiation with light and then becomes reversibly non-fluid.
2. 2. The composition according to claim 1, wherein a mixing ratio of the isomerized polymer to the isomerized low molecular weight compound is, in terms of mass ratio, isomerized polymer:isomerized low molecular weight compound=99:1 to 10:
90.
3. The composition according to claim 1 or 2, wherein the wavelength of the light is not less than 280 nm and not more than 480 nm.
4. A toner comprising the composition according to any one of claims 1 to 3.
5. The toner according to claim 4 , further comprising a binder resin.
6. The toner according to claim 5 , wherein the binder resin comprises at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.
7. 7. An image forming method comprising: a step of forming a toner image made of the toner according to claim 4 on a recording medium; and a step of irradiating the toner image with light to soften the toner image.
8. The image forming method according to claim 7 , wherein the wavelength of the light is from 280 nm to 480 nm.
9. 9. The image forming method according to claim 7, further comprising a step of pressing the toner image.
10. The image forming method according to claim 9 , wherein the toner image is further heated in the pressurizing step.
11. 11. The image forming method according to claim 7, wherein in the step of irradiating the toner image with light to soften the toner image, the toner image is heated in addition to being irradiated with light.
12. A light-responsive adhesive comprising the composition according to any one of claims 1 to 3.
13. A light switching material comprising the composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Composition for nonlinear optical material, optical member, nonlinear optical material and manufacturing method of the same
JP2007017960A
Photoresponsive liquid crystal compound
JP2011256155A
Method for fluidizing / non-fluidizing compound with light
JP2011256291A
Toner and image forming method
JP2018124387A
Light-responsive adhesive agent
WO2013168712A1