Acrylic rubber with excellent storage stability

An acrylic rubber with specific compositional units and controlled processing methods achieves enhanced storage stability and water resistance, addressing the limitations of existing formulations.

JP7556353B2Active Publication Date: 2024-09-26ZEON CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021534587
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-19
Filing Date
2020-06-05
Publication Date
2024-09-26
Estimated Expiration
2040-06-05

AI Technical Summary

Technical Problem

Existing acrylic rubbers lack sufficient storage stability, particularly in harsh environments, necessitating improved formulations to enhance their durability and resistance to degradation.

Method used

The development of an acrylic rubber with specific compositional units, molecular weights, and anti-aging agents, combined with controlled coagulation and drying processes, to achieve enhanced storage stability and water resistance.

Benefits of technology

The resulting acrylic rubber exhibits superior storage stability, workability, and resistance to environmental factors, maintaining properties over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556353000009
    Figure 0007556353000009
  • Figure 0007556353000011
    Figure 0007556353000011
  • Figure 0007556353000010
    Figure 0007556353000010
Patent Text Reader

Abstract

Provided are: an acrylic rubber having excellent storage stability; a production method therefor; a rubber composition including the acrylic rubber; and a crosslinked rubber object obtained by crosslinking the rubber composition. The acrylic rubber comprises 50-99.9 wt% combined units derived from at least one (meth)acrylic ester selected from the group consisting of alkyl (meth)acrylates and alkoxyalkyl (meth)acrylates, 0.1-20 wt% combined units derived from a monomer having a reactive group, and 0-30 wt% combined units derived from other monomer(s). The acrylic rubber contains a phenolic antioxidant represented by general formula (1) (R1 represents an isopropyl group or a t-butyl group and R2 represents an alkyl group having 1-12 carbon atoms) and has a weight-average molecular weight (Mw) in the range of 100,000-5,000,000.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an acrylic rubber, a method for producing the same, a rubber composition, and a cross-linked rubber product, and more specifically to an acrylic rubber having excellent storage stability, a method for producing the same, a rubber composition containing the acrylic rubber, and a cross-linked rubber product obtained by cross-linking the acrylic rubber. [Background technology]

[0002] Acrylic rubber is a polymer whose main component is acrylic ester, and is generally known as a rubber having excellent heat resistance, oil resistance, and ozone resistance. It is widely used in fields such as automobiles, and is used with the addition of antioxidants as necessary.

[0003] For example, Patent Document 1 (International Publication No. WO 2018 / 139466) describes a method for obtaining a monomer emulsion by stirring monomer components including ethyl acrylate, n-butyl acrylate, monobutyl fumarate, and the like with pure water, sodium lauryl sulfate, and polyoxyethylene dodecyl ether, and then continuously adding dropwise an aqueous solution of ferrous sulfate, sodium ascorbate, and potassium persulfate over a period of 3 hours to obtain a monomer emulsion having a polymerization conversion rate of 95%. The emulsion is then mixed with 50 parts of an aqueous solution of 0.2% by weight of sodium lauryl sulfate and (3,5-di-tert-butyl-4-hydroxyphenyl)propionate to obtain a monomer emulsion. The method for producing crumb-like acrylic rubber, which can suppress contamination of a polymerization apparatus during polymerization and has excellent initial mechanical strength, is disclosed, in which a 50% by weight aqueous dispersion of 2,4-bis[(octylthio)methyl]-6-methylphenol (prepared by adding and mixing 50 parts by weight of 2,4-bis[(octylthio)methyl]-6-methylphenol to 50 parts by weight of an aqueous solution of 0.2% by weight of sodium lauryl sulfate) is added, the temperature is raised to 85°C, and the mixture is coagulated with sodium sulfate to produce hydrous crumbs, and the hydrous crumbs are washed four times with industrial water, washed once with an acid of pH 3, and washed once with pure water, and then dried at 160°C for 10 minutes in a hot air dryer. It is also disclosed that according to this method, the hydrous crumbs washed with a screw-type extrusion dryer can be dried at 150°C or higher. However, in addition to heat resistance, there is a demand for improving storage stability under severe environments. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 139466 Brochure Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an acrylic rubber having excellent storage stability, a production method thereof, a rubber composition containing the acrylic rubber, and a cross-linked rubber product obtained by cross-linking the acrylic rubber. [Means for solving the problem]

[0006] The present inventors have conducted extensive research in view of the above problems and have found that an acrylic rubber containing an antioxidant with a specific structure having a specific composition unit and a specific molecular weight has significantly superior storage stability. They have also found that the storage stability can be further improved by specifying the compound and content of the antioxidant with a specific structure, the molecular weight distribution in the high molecular weight region, the pH, the water content, the complex viscosity at a specific temperature, the ash content, the ash component content, and the component ratio.

[0007] The present inventors have also found that the storage stability can be further improved by forming the acrylic rubber of the present invention into a sheet or veil shape, and that the storage stability can be improved and processability can be improved by specifying the specific gravity and gel content.

[0008] The present inventors have also found that an acrylic rubber with excellent storage stability can be produced by adding an antioxidant with a specific structure to an emulsion polymerization liquid obtained by emulsion-polymerizing a specific monomer component, followed by coagulation and drying. They have also found that the storage stability and water resistance of the produced acrylic rubber can be further improved by using a specific coagulation method, washing with hot water after coagulation, and dehydrating the water-containing crumbs after washing.

[0009] Based on these findings, the present inventors have completed the present invention.

[0010] Thus, according to the present invention, there is provided a polymerizable composition comprising 50 to 99.9% by weight of bonding units derived from at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, 0.1 to 20% by weight of bonding units derived from reactive group-containing monomers, and 0 to 30% by weight of bonding units derived from other monomers, and represented by the general formula (1): [ka] (R1 represents an isopropyl group or a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms), and an acrylic rubber having a weight average molecular weight (Mw) in the range of 100,000 to 5,000,000 is provided.

[0011] In the acrylic rubber of the present invention, the phenol-based antioxidant represented by the general formula (1) is preferably octyl 3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate or octyl 3-(4-hydroxy-3,5-diisopropylphenyl)propionate.

[0012] In the acrylic rubber of the present invention, the content of the phenol-based antioxidant represented by the general formula (1) is preferably 0.001 to 15% by weight.

[0013] In the acrylic rubber of the present invention, the ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) is preferably 1.3 or more.

[0014] In the acrylic rubber of the present invention, the complex viscosity at 60° C. ([η]100° C.) is preferably 15,000 Pa·s or less.

[0015] In the acrylic rubber of the present invention, the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is preferably 0.5 or more.

[0016] In the acrylic rubber of the present invention, the pH is preferably 6 or less.

[0017] In the acrylic rubber of the present invention, the water content is preferably less than 1% by weight.

[0018] In the acrylic rubber of the present invention, the ash content is preferably 0.5% by weight or less.

[0019] In the acrylic rubber of the present invention, the total amount of magnesium and phosphorus in the ash is preferably 30% by weight or more.

[0020] In the acrylic rubber of the present invention, the ratio of magnesium to phosphorus in the ash ([Mg] / [P]) is preferably in the range of 0.4 to 2.5.

[0021] In the acrylic rubber of the present invention, the acrylic rubber is preferably in the form of a sheet or a veil.

[0022] The acrylic rubber of the present invention preferably has a specific gravity of 0.8 or more.

[0023] In the acrylic rubber of the present invention, the gel amount is preferably 50% by weight or less.

[0024] Thus, according to the present invention, a monomer component consisting of at least one (meth)acrylic acid ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and, if necessary, other copolymerizable monomers is emulsified with water and an emulsifier, and emulsion-polymerized in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid containing a compound represented by the general formula (1) [ka] (R1 represents an isopropyl group or a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms), and then the mixture is coagulated and dried.

[0025] In the method for producing an acrylic rubber of the present invention, it is preferable that the coagulation of the emulsion polymerization liquid to which the phenol-based antiaging agent represented by the general formula (1) has been added is carried out by adding the emulsion polymerization liquid to a coagulating liquid that is being stirred.

[0026] In the method for producing an acrylic rubber of the present invention, it is preferable that the water-containing crumbs produced during coagulation are washed with warm water.

[0027] In the method for producing acrylic rubber of the present invention, it is preferable to squeeze water out of the water-containing crumbs after washing using a dehydrator.

[0028] Thus, according to the present invention, there is also provided a rubber composition comprising a rubber component containing the above-mentioned acrylic rubber, a filler and a crosslinking agent.

[0029] Thus, according to the present invention, there is further provided a cross-linked rubber product obtained by cross-linking the above rubber composition. Effect of the Invention

[0030] According to the present invention, there are provided an acrylic rubber having excellent storage stability, a method for producing the same, a rubber composition containing the acrylic rubber, and a cross-linked rubber obtained by cross-linking the acrylic rubber. [Brief description of the drawings]

[0031] [Figure 1] FIG. 1 is a diagram illustrating an example of an acrylic rubber production system used for producing a sheet-like or veil-like acrylic rubber according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the configuration of the screw-type extruder in FIG. 1. [Diagram 3] FIG. 2 is a diagram showing the configuration of a transportable cooling device used as the cooling device in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] The acrylic rubber of the present invention comprises 50 to 99.9% by weight of bonding units derived from at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, 0.1 to 20% by weight of bonding units derived from reactive group-containing monomers, and 0 to 30% by weight of bonding units derived from other monomers, and is represented by the general formula (1): [ka] (R1 represents an isopropyl group or a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms), and has a weight average molecular weight (Mw) in the range of 100,000 to 5,000,000.

[0033] <Monomer components> The acrylic rubber of the present invention comprises at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and, if necessary, bond units derived from other copolymerizable monomers. In the present invention, the term "(meth)acrylic acid ester" is used as a general term for esters of acrylic acid and / or methacrylic acid.

[0034] The (meth)acrylic acid alkyl ester is not particularly limited, but is usually a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 12 carbon atoms, preferably a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms, and more preferably a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 6 carbon atoms.

[0035] Specific examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred.

[0036] The (meth)acrylic acid alkoxyalkyl ester is not particularly limited, but is usually a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 12, preferably a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 8, and more preferably a (meth)acrylic acid alkoxyalkyl ester having an alkoxyalkyl group of 2 to 6 carbon atoms.

[0037] Specific examples of the (meth)acrylic acid alkoxyalkyl ester include methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxymethyl (meth)acrylate, ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, etc. Among these, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, etc. are preferred, and methoxyethyl acrylate, ethoxyethyl acrylate, etc. are more preferred.

[0038] At least one (meth)acrylic acid ester selected from the group consisting of these (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters is used alone or in combination of two or more, and the proportion in the acrylic rubber is usually 50 to 99.9% by weight, preferably 70 to 99.9% by weight, more preferably 80 to 99.5% by weight, and most preferably 87 to 99% by weight. If the amount of the (meth)acrylic acid ester in the monomer component is excessively small, the weather resistance, heat resistance, and oil resistance of the resulting acrylic rubber may decrease, which is not preferable.

[0039] The reactive group-containing monomer is not particularly limited and may be appropriately selected depending on the intended use, but is preferably a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a halogen group, more preferably a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a chlorine atom, particularly preferably a monomer having a carboxyl group or an epoxy group, and most preferably a monomer having a carboxyl group, which can highly improve the crosslinked properties of the acrylic rubber. Also, a monomer having an ion-reactive group such as a carboxyl group or an epoxy group is preferable because it can improve the water resistance of the acrylic rubber.

[0040] The monomer having a carboxyl group is not particularly limited, but an ethylenically unsaturated carboxylic acid can be suitably used. Examples of the ethylenically unsaturated carboxylic acid include ethylenically unsaturated monocarboxylic acid, ethylenically unsaturated dicarboxylic acid, and ethylenically unsaturated dicarboxylic acid monoester, and among these, ethylenically unsaturated dicarboxylic acid monoester is particularly preferred because it can further improve the compression set resistance property when the acrylic rubber is made into a rubber cross-linked product.

[0041] The ethylenically unsaturated monocarboxylic acid is not particularly limited, but is preferably an ethylenically unsaturated monocarboxylic acid having 3 to 12 carbon atoms, and examples thereof include acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and cinnamic acid.

[0042] The ethylenically unsaturated dicarboxylic acid is not particularly limited, but is preferably an ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms, and examples thereof include butenedioic acids such as fumaric acid and maleic acid, itaconic acid, citraconic acid, etc. The ethylenically unsaturated dicarboxylic acid also includes those that exist as an anhydride.

[0043] The ethylenically unsaturated dicarboxylic acid monoester is not particularly limited, but is usually an ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms and an alkyl monoester having 1 to 12 carbon atoms, preferably an ethylenically unsaturated dicarboxylic acid having 4 to 6 carbon atoms and an alkyl monoester having 2 to 8 carbon atoms, and more preferably an alkyl monoester having 2 to 6 carbon atoms of butenedioic acid having 4 carbon atoms.

[0044] Specific examples of ethylenically unsaturated dicarboxylic acid monoesters include butenedioic acid monoalkyl esters such as monomethyl fumarate, monoethyl fumarate, mono-n-butyl fumarate, monomethyl maleate, monoethyl maleate, mono-n-butyl maleate, monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclohexenyl fumarate, monocyclopentyl maleate, and monocyclohexyl maleate; and itaconic acid monoalkyl esters such as monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, and monocyclohexyl itaconate; and among these, mono-n-butyl fumarate and mono-n-butyl maleate are preferred, and mono-n-butyl fumarate is particularly preferred.

[0045] Examples of the monomer having an epoxy group include epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate; epoxy group-containing vinyl ethers such as allyl glycidyl ether and vinyl glycidyl ether; and the like.

[0046] Examples of monomers having a halogen group include unsaturated alcohol esters of halogen-containing saturated carboxylic acids, (meth)acrylic acid haloalkyl esters, (meth)acrylic acid haloacyloxyalkyl esters, (meth)acrylic acid (haloacetylcarbamoyloxy)alkyl esters, halogen-containing unsaturated ethers, halogen-containing unsaturated ketones, halomethyl group-containing aromatic vinyl compounds, halogen-containing unsaturated amides, and haloacetyl group-containing unsaturated monomers.

[0047] Examples of unsaturated alcohol esters of halogen-containing saturated carboxylic acids include vinyl chloroacetate, vinyl 2-chloropropionate, and allyl chloroacetate. Examples of (meth)acrylic acid haloalkyl esters include chloromethyl (meth)acrylate, 1-chloroethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 1,2-dichloroethyl (meth)acrylate, 2-chloropropyl (meth)acrylate, 3-chloropropyl (meth)acrylate, and 2,3-dichloropropyl (meth)acrylate. Examples of (meth)acrylic acid haloacyloxyalkyl esters include 2-(chloroacetoxy)ethyl (meth)acrylate, 2-(chloroacetoxy)propyl (meth)acrylate, 3-(chloroacetoxy)propyl (meth)acrylate, and 3-(hydroxychloroacetoxy)propyl (meth)acrylate. Examples of (meth)acrylic acid (haloacetylcarbamoyloxy) alkyl esters include 2-(chloroacetylcarbamoyloxy) ethyl (meth)acrylate and 3-(chloroacetylcarbamoyloxy) propyl (meth)acrylate. Examples of halogen-containing unsaturated ethers include chloromethyl vinyl ether, 2-chloroethyl vinyl ether, 3-chloropropyl vinyl ether, 2-chloroethyl allyl ether, and 3-chloropropyl allyl ether. Examples of halogen-containing unsaturated ketones include 2-chloroethyl vinyl ketone, 3-chloropropyl vinyl ketone, and 2-chloroethyl allyl ketone. Examples of halomethyl group-containing aromatic vinyl compounds include p-chloromethylstyrene, m-chloromethylstyrene, o-chloromethylstyrene, and p-chloromethyl-α-methylstyrene. Examples of halogen-containing unsaturated amides include N-chloromethyl(meth)acrylamide. Examples of the haloacetyl group-containing unsaturated monomer include 3-(hydroxychloroacetoxy)propyl allyl ether, p-vinylbenzyl chloroacetic acid ester, and the like.

[0048] These reactive group-containing monomers may be used alone or in combination of two or more, and their proportion in the acrylic rubber is usually 0.1 to 20% by weight, preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and most preferably 1 to 3% by weight.

[0049] The other monomers used as necessary are not particularly limited as long as they are copolymerizable with the above-mentioned monomers, and examples thereof include aromatic vinyl, ethylenically unsaturated nitrile, acrylamide monomers, other olefin monomers, etc. Examples of aromatic vinyl include styrene, α-methylstyrene, divinylbenzene, etc. Examples of ethylenically unsaturated nitrile include acrylonitrile, methacrylonitrile, etc. Examples of acrylamide monomers include acrylamide, methacrylamide, etc. Examples of other olefin monomers include ethylene, propylene, vinyl acetate, ethyl vinyl ether, butyl vinyl ether, etc.

[0050] These other monomers may be used alone or in combination of two or more, and their proportion in the acrylic rubber is usually in the range of 0 to 30% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, and most preferably 0 to 10% by weight.

[0051] <Acrylic rubber> The acrylic rubber of the present invention comprises at least one (meth)acrylic acid ester selected from the group consisting of the above-mentioned (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and, if necessary, other copolymerizable monomers. The proportions of each in the acrylic rubber are as follows: the bonding units derived from at least one (meth)acrylic acid ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters are usually in the range of 50 to 99.9% by weight, preferably 70 to 99.9% by weight, more preferably 80 to 99.5% by weight, and particularly preferably 87 to 99% by weight; the bonding units derived from the reactive group-containing monomer are usually in the range of 0.1 to 20% by weight, preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and particularly preferably 1 to 3% by weight; and the bonding units derived from other monomers are usually in the range of 0 to 30% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, and particularly preferably 0 to 10% by weight. By setting the content of these monomers in the acrylic rubber within this range, the object of the present invention can be achieved to a high degree, and when the acrylic rubber is crosslinked, the water resistance and compression set resistance are improved significantly, which is preferable.

[0052] The weight average molecular weight (Mw) of the acrylic rubber of the present invention, in terms of absolute molecular weight measured by GPC-MALS, is in the range of 100,000 to 5,000,000, preferably 500,000 to 4,000,000, more preferably 700,000 to 3,000,000, and most preferably 1,000,000 to 2,500,000, which is suitable since the storage stability, processability, strength properties, and compression set resistance properties during mixing of the acrylic rubber are highly balanced.

[0053] The ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) of the acrylic rubber of the present invention is not particularly limited, but when the ratio is in the range of usually 1.3 or more, preferably 1.4 to 5, and more preferably 1.5 to 2, in terms of absolute molecular weight distribution with emphasis on the polymer region measured by GPC-MALS, the processability and strength characteristics of the acrylic rubber are highly balanced and changes in physical properties during storage can be alleviated, which is suitable.

[0054] The content of reactive groups in the acrylic rubber of the present invention may be appropriately selected depending on the purpose of use, but when the weight ratio of the reactive groups themselves is usually in the range of 0.001 to 5 wt%, preferably 0.01 to 3 wt%, more preferably 0.05 to 1 wt%, and particularly preferably 0.1 to 0.5 wt%, it is suitable in that properties such as processability, strength properties, compression set resistance, oil resistance, cold resistance, and water resistance are highly balanced.

[0055] The glass transition temperature (Tg) of the acrylic rubber of the present invention is not particularly limited, but is usually 20° C. or lower, preferably 10° C. or lower, and more preferably 0° C. or lower. The lower limit of the glass transition temperature (Tg) of the acrylic rubber is not particularly limited, but is usually −80° C. or higher, preferably −60° C. or higher, and more preferably −40° C. or higher. By setting the glass transition temperature to the lower limit or higher, the oil resistance and heat resistance can be improved, and by setting the glass transition temperature to the upper limit or lower, the cold resistance and processability can be improved.

[0056] The specific gravity of the acrylic rubber of the present invention is not particularly limited, but is usually 0.7 or more, preferably 0.8 to 1.4, more preferably 0.9 to 1.3, particularly preferably 0.95 to 1.25, and most preferably 1.0 to 1.2, and is therefore suitable since it has excellent storage stability.

[0057] The gel amount of the acrylic rubber of the present invention is not particularly limited, but when the gel amount is, in terms of the insoluble matter in methyl ethyl ketone, usually 50% by weight or less, preferably 30% by weight or less, more preferably 20% by weight or less, particularly preferably 10% by weight or less, and most preferably 5% by weight or less, storage stability and processability are highly improved, and this is suitable.

[0058] The pH of the acrylic rubber of the present invention is not particularly limited, but is usually 6 or less, preferably 2 to 6, more preferably 2.5 to 5.5, and particularly preferably 3 to 5, and is therefore suitable since storage stability is highly improved.

[0059] The water content of the acrylic rubber of the present invention is not particularly limited, but when it is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less, the crosslinking characteristics are optimized and the properties such as heat resistance and water resistance are highly excellent, which is preferable.

[0060] The ash content of the acrylic rubber of the present invention is not particularly limited, but is usually 0.5% by weight or less, preferably 0.3% by weight or less, more preferably 0.2% by weight or less, and particularly preferably 0.15% by weight or less, which is suitable in terms of excellent storage stability and water resistance.

[0061] The lower limit of the ash content of the acrylic rubber of the present invention is not particularly limited, but when it is usually 0.0001% by weight or more, preferably 0.0005% by weight or more, more preferably 0.001% by weight or more, particularly preferably 0.005% by weight or more, and most preferably 0.01% by weight or more, metal adhesion is suppressed and the workability is excellent, which is suitable.

[0062] The ash content, which provides a high balance between storage stability, water resistance, and workability of the acrylic rubber of the present invention, is usually in the range of 0.0001 to 0.5% by weight, preferably 0.0005 to 0.3% by weight, more preferably 0.001 to 0.2% by weight, particularly preferably 0.005 to 0.15% by weight, and most preferably 0.01 to 0.12% by weight.

[0063] The content (total amount) of at least one element selected from the group consisting of sodium, sulfur, calcium, magnesium and phosphorus in the ash of the acrylic rubber of the present invention is not particularly limited, but when the content is usually at least 30% by weight, preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 80% by weight or more, based on the total ash content, the storage stability and water resistance are highly excellent and suitable.

[0064] The total amount of sodium and sulfur in the ash of the acrylic rubber of the present invention is not particularly limited, but when the total amount of sodium and sulfur is 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 80% by weight or more, the storage stability and water resistance are highly excellent and suitable.

[0065] The ratio of sodium to sulfur in the ash of the acrylic rubber of the present invention ([Na] / [S]) is not particularly limited by weight, but when it is in the range of usually 0.4 to 2.5, preferably 0.6 to 2, preferably 0.8 to 1.7, more preferably 1 to 1.5, water resistance is highly excellent and it is suitable.

[0066] The total amount of magnesium and phosphorus in the ash of the acrylic rubber of the present invention is not particularly limited, but when the total amount of magnesium and phosphorus is, in terms of the ratio to the total ash content, usually 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 80% by weight or more, the storage stability and water resistance are highly excellent and suitable.

[0067] The ratio of magnesium to phosphorus in the ash of the acrylic rubber of the present invention ([Mg] / [P]) is not particularly limited by weight, but when it is in the range of usually 0.4 to 2.5, preferably 0.4 to 1.3, more preferably 0.4 to 1, particularly preferably 0.45 to 0.75, and most preferably 0.5 to 0.7, the storage stability and water resistance are highly excellent and it is suitable.

[0068] The complex viscosity of the acrylic rubber of the present invention at 60°C ([η]60°C) is not particularly limited, but when it is usually in the range of 15,000 Pa·s or less, preferably 2,000 to 10,000 Pa·s, more preferably 2,500 to 7,000 Pa·s, and most preferably 2,700 to 5,500 Pa·s, it is suitable in terms of excellent processability, oil resistance, and shape retention.

[0069] The complex viscosity of the acrylic rubber of the present invention at 100°C ([η]100°C) is not particularly limited, but when it is in the range of usually 1,500 to 6,000 Pa·s, preferably 2,000 to 5,000 Pa·s, more preferably 2,500 to 4,000 Pa·s, and most preferably 2,500 to 3,500 Pa·s, it is suitable in terms of excellent processability, oil resistance, and shape retention.

[0070] The ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) of the acrylic rubber of the present invention to the complex viscosity at 60°C ([η]60°C) is not particularly limited, but is usually 0.5 or more, preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.82 or more. In addition, when the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) of the acrylic rubber of the present invention to the complex viscosity at 60°C ([η]60°C) is usually 0.5 to 0.99, preferably 0.6 to 0.98, more preferably 0.75 to 0.95, particularly preferably 0.8 to 0.94, and most preferably 0.83 to 0.93, the processability, oil resistance, and shape retention are highly balanced and suitable.

[0071] The Mooney viscosity (ML1+4, 100°C) of the acrylic rubber of the present invention is not particularly limited, but when it is in the range of usually 10 to 150, preferably 20 to 100, more preferably 25 to 70, the processability and strength properties are highly balanced and it is suitable.

[0072] <Contains anti-aging agents> The acrylic rubber of the present invention is represented by the general formula (1) [ka] (R1 represents an isopropyl group or a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms).

[0073] In the formula, R1 represents an isopropyl group or a t-butyl group, and preferably a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms, preferably an alkyl group having 4 to 10 carbon atoms, and more preferably an alkyl group having 6 to 10 carbon atoms.

[0074] Specific examples of the phenol-based antiaging agent represented by the general formula (1) include butyl 3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate, hexyl 3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate, octyl 3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate, decyl 3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate, and 3-(4-hydroxy-3,5-diisopropylphenyl)propionate. Examples of the 3-(4-hydroxy-3,5-diisopropylphenyl)propionate include 3-(4-hydroxy-3,5-diisopropylphenyl)heptyl propionate, octyl 3-(4-hydroxy-3,5-diisopropylphenyl)propionate, and dodecyl 3-(4-hydroxy-3,5-diisopropylphenyl)propionate. Of these, 3-(4-hydroxy-3,5-di-tert-butylphenyl)octyl propionate or 3-(4-hydroxy-3,5-diisopropylphenyl)propionate is preferred, and 3-(4-hydroxy-3,5-di-tert-butylphenyl)octyl propionate is more preferred.

[0075] The melting point of the phenolic antioxidant represented by general formula (1) is not particularly limited, but is usually not more than 100° C., preferably not more than 70° C., more preferably not more than 50° C., particularly preferably not more than 40° C., and most preferably not more than 30° C. When the melting point of the phenolic antioxidant represented by general formula (1) is in this range, the storage stability and heat resistance of the acrylic rubber can be improved to a high level, which is suitable.

[0076] The lower limit of the melting point of the phenol-based antiaging agent represented by the general formula (1) is not particularly limited, but it is usually suitable to be −40° C. or higher, preferably −20° C. or higher, and more preferably 0° C. or higher, since the storage stability and heat resistance of the acrylic rubber can be highly improved.

[0077] These phenolic antioxidants represented by the general formula (1) can be used alone or in combination of two or more kinds. The content in the acrylic rubber is not particularly limited and may be appropriately selected within the range in which the effects of the present invention can be exhibited, but is usually in the range of 0.001 to 15% by weight, preferably 0.01 to 10% by weight, more preferably 0.1 to 5% by weight, and particularly preferably 0.5 to 3% by weight.

[0078] The acrylic rubber of the present invention must contain the phenol-based antioxidant represented by the above general formula (1), but may contain other antioxidants within the scope of the present invention.

[0079] <Manufacturing method> The method for producing the acrylic rubber of the present invention is not particularly limited, but for example, the acrylic rubber can be easily produced by emulsifying a monomer component consisting of at least one (meth)acrylic acid ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a reactive group-containing monomer, and, as necessary, other copolymerizable monomers, with water and an emulsifier, emulsion-polymerizing the emulsion in the presence of a polymerization catalyst, adding the phenol-based antiaging agent represented by the above general formula (1) to the emulsion polymerization liquid, and then coagulating and drying the mixture.

[0080] The monomer components used are the same as those described above in the monomer components, and the amount used may be appropriately selected so as to obtain the monomer composition of the acrylic rubber constituting the acrylic rubber, and is equivalent to the monomer composition of the acrylic rubber.

[0081] (emulsifier) The emulsifier used is not particularly limited, but examples thereof include anionic emulsifiers, cationic emulsifiers, and nonionic emulsifiers. Preferably, the emulsifier contains an anionic emulsifier, more preferably, the emulsifier contains a sulfate ester salt or a phosphate ester salt, and most preferably, the emulsifier contains a phosphate ester salt.

[0082] The anionic emulsifier is not particularly limited, and examples thereof include salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid; alkylbenzenesulfonates such as sodium dodecylbenzenesulfonate; sulfates such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium myristyl sulfate, sodium laureth sulfate, sodium polyoxyethylene alkyl sulfate, and sodium polyoxyethylene alkylaryl sulfate; phosphates such as sodium lauryl phosphate, potassium lauryl phosphate, and sodium polyoxyalkylene alkyl ether phosphate; and alkylsulfosuccinates. Among these anionic emulsifiers, phosphates and sulfates are preferred, and phosphates are particularly preferred. These anionic emulsifiers can be used alone or in combination of two or more.

[0083] Examples of the cationic emulsifier include alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride.

[0084] The nonionic emulsifier is not particularly limited, but examples thereof include polyoxyalkylene fatty acid esters such as polyoxyethylene stearate ester; polyoxyalkylene alkyl ethers such as polyoxyethylene dodecyl ether; polyoxyalkylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether; polyoxyethylene sorbitan alkyl esters; and the like. Polyoxyalkylene alkyl ethers and polyoxyalkylene alkylphenol ethers are preferred, and polyoxyethylene alkyl ethers and polyoxyethylene alkylphenol ethers are more preferred.

[0085] These emulsifiers can be used alone or in combination of two or more. The amount used is usually 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 1 to 3 parts by weight, per 100 parts by weight of the monomer component.

[0086] The method of mixing the monomer component, water, and an emulsifier to emulsify may be a conventional method, such as a method of stirring the monomer, emulsifier, and water using a stirrer such as a homogenizer or a disk turbine. The amount of water used is usually in the range of 10 to 750 parts by weight, preferably 50 to 500 parts by weight, and more preferably 100 to 400 parts by weight, based on 100 parts by weight of the monomer component.

[0087] (Polymerization catalyst) The polymerization catalyst used is not particularly limited as long as it is one that is usually used in emulsion polymerization. For example, a redox catalyst consisting of a radical generator and a reducing agent can be used.

[0088] Examples of the radical generator include peroxides and azo compounds, and preferably peroxides. As the peroxide, inorganic peroxides and organic peroxides can be used.

[0089] Examples of inorganic peroxides include sodium persulfate, potassium persulfate, hydrogen peroxide, and ammonium persulfate. Among these, potassium persulfate, hydrogen peroxide, and ammonium persulfate are preferred, and potassium persulfate is particularly preferred.

[0090] The organic peroxide is not particularly limited as long as it is a known peroxide used in emulsion polymerization, and examples thereof include 2,2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane, 1-di-(t-hexylperoxy)cyclohexane, 1,1-di-(t-butylperoxy)cyclohexane, 4,4-di-(t-butylperoxy)n-butyl valerate, 2,2-di-(t-butylperoxy)butane, t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, and paramenthane hydroperoxide. oxide, benzoyl peroxide, 1,1,3,3-tetraethylbutyl hydroperoxide, t-butylcumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide, dibenzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzyl) peroxydicarbonate, diisobutyryl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxyneodecanate, t-hexyl peroxypivalate, t-butyl peroxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethyl t-butylperoxy-2-ethylhexanate, t-hexylperoxy-2-ethylhexanate, t-butylperoxy-3,5,5-trimethylhexanate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxybenzoate, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and among these, diisopropylbenzene hydroperoxide, cumene hydroperoxide, paramenthane hydroperoxide, benzoyl peroxide, and the like are preferred.

[0091] Examples of azo compounds include azobisisoptylonitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane, 2,2'-azobis(propane-2-carboxamidine), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide], 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2,2'-azobis(1-imino-1-pyrrolidino-2-methylpropane), and 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide}.

[0092] These radical generators can be used alone or in combination of two or more kinds. The amount of the radical generator used is usually in the range of 0.0001 to 5 parts by weight, preferably 0.0005 to 1 part by weight, and more preferably 0.001 to 0.5 parts by weight, per 100 parts by weight of the monomer component.

[0093] The reducing agent can be any reducing agent that is used in a redox catalyst for emulsion polymerization, but in the present invention, it is particularly preferable to use at least two reducing agents. As the at least two reducing agents, for example, a combination of a metal ion compound in a reduced state and another reducing agent is preferable.

[0094] The reduced metal ion compound is not particularly limited, but examples thereof include ferrous sulfate, sodium iron hexamethylenediaminetetraacetate, and cuprous naphthenate, among which ferrous sulfate is preferred. These reduced metal ion compounds can be used alone or in combination of two or more, and the amount used is usually in the range of 0.000001 to 0.01 parts by weight, preferably 0.00001 to 0.001 parts by weight, and more preferably 0.00005 to 0.0005 parts by weight, relative to 100 parts by weight of the monomer component.

[0095] The reducing agent other than these metal ion compounds in a reduced state is not particularly limited, and examples thereof include ascorbic acid or a salt thereof, such as ascorbic acid, sodium ascorbate, and potassium ascorbate; erythorbic acid or a salt thereof, such as erythorbic acid, sodium erythorbate, and potassium erythorbate; sulfinates, such as sodium hydroxymethanesulfinate; sulfites, such as sodium sulfite, potassium sulfite, sodium hydrogen sulfite, aldehyde sodium hydrogen sulfite, and potassium hydrogen sulfite; Examples of suitable phosphorous acids include pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium hydrogen pyrosulfite, and potassium hydrogen pyrosulfite; thiosulfates such as sodium thiosulfate and potassium thiosulfate; phosphorous acid or a salt thereof such as phosphorous acid, sodium phosphite, potassium phosphite, sodium hydrogen phosphite, and potassium hydrogen phosphite; pyrophosphorous acid or a salt thereof such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite, and potassium hydrogen pyrophosphite; sodium formaldehyde sulfoxylate, etc. Among these, ascorbic acid or a salt thereof, sodium formaldehyde sulfoxylate, etc. are preferred, and ascorbic acid or a salt thereof is particularly preferred.

[0096] These reducing agents other than metal ion compounds in a reduced state can be used alone or in combination of two or more kinds, and the amount used is usually in the range of 0.001 to 1 part by weight, preferably 0.005 to 0.5 parts by weight, and more preferably 0.01 to 0.3 parts by weight, per 100 parts by weight of the monomer component.

[0097] A preferred combination of a metal ion compound in a reduced state and another reducing agent is ferrous sulfate and ascorbic acid or a salt thereof and / or sodium formaldehyde sulfoxylate, more preferably ferrous sulfate and an ascorbate and / or sodium formaldehyde sulfoxylate, and most preferably ferrous sulfate and an ascorbate. In this case, the amount of ferrous sulfate used is usually 0.000001 to 0.01 parts by weight, preferably 0.00001 to 0.001 parts by weight, more preferably 0.00005 to 0.0005 parts by weight, relative to 100 parts by weight of the monomer component, and the amount of ascorbic acid or a salt thereof and / or sodium formaldehyde sulfoxylate used is usually 0.001 to 1 part by weight, preferably 0.005 to 0.5 parts by weight, more preferably 0.01 to 0.3 parts by weight, relative to 100 parts by weight of the monomer component.

[0098] The amount of water used in the emulsion polymerization reaction may be only that used during emulsification of the monomer components, but is adjusted to be in the range of usually 10 to 1,000 parts by weight, preferably 50 to 500 parts by weight, more preferably 80 to 400 parts by weight, and most preferably 100 to 300 parts by weight, relative to 100 parts by weight of the monomer components used in the polymerization.

[0099] The emulsion polymerization reaction may be carried out according to a conventional method, and may be any of batch, semi-batch, and continuous. The polymerization temperature and polymerization time are not particularly limited and may be appropriately selected depending on the type of polymerization initiator used. The polymerization temperature is usually in the range of 0 to 100°C, preferably 5 to 80°C, and more preferably 10 to 50°C, and the polymerization time is usually 0.5 to 100 hours, and preferably 1 to 10 hours.

[0100] The polymerization conversion rate of the emulsion polymerization reaction is not particularly limited, but is usually 80% by weight or more, preferably 90% by weight or more, and more preferably 95% by weight or more, which is preferable because the acrylic rubber produced has excellent strength characteristics and is free of monomer odor. A polymerization terminator may be used to terminate the polymerization.

[0101] (Anti-aging agent added) The phenol-based antiaging agent represented by general formula (1) used is the same as that described for the antiaging agent contained above, and the amount used may be appropriately selected so as to be the content in the acrylic rubber, and is usually in the range of 0.001 to 15 parts by weight, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, particularly preferably 0.3 to 3 parts by weight, and most preferably 0.5 to 2 parts by weight, relative to 100 parts by weight of the monomer component.

[0102] The method of adding the phenol-based antiaging agent represented by the general formula (1) to the emulsion polymerization liquid is not particularly limited and may be a conventional method. The phenol-based antiaging agent represented by the general formula (1) may be added as it is, or may be added after being emulsified with water and an emulsifier.

[0103] (solidification process) The emulsion polymerization liquid to which the phenol-based antiaging agent represented by the above general formula (1) has been added may be solidified according to a conventional method, for example, by contacting the emulsion polymerization liquid with a coagulating liquid to produce water-containing crumbs.

[0104] The coagulant used is not particularly limited, but a metal salt is usually used. Examples of the metal salt include alkali metals, salts of metals in Group 2 of the periodic table, and other metal salts, and are preferably alkali metal salts and salts of metals in Group 2 of the periodic table, more preferably salts of metals in Group 2 of the periodic table, and particularly preferably magnesium salts.

[0105] Examples of alkali metal salts include sodium salts such as sodium chloride, sodium nitrate, and sodium sulfate; potassium salts such as potassium chloride, potassium nitrate, and potassium sulfate; and lithium salts such as lithium chloride, lithium nitrate, and lithium sulfate. Among these, sodium salts are preferred, and sodium chloride and sodium sulfate are particularly preferred.

[0106] Examples of the salt of a metal of Group 2 of the periodic table include magnesium chloride, calcium chloride, magnesium nitrate, calcium nitrate, magnesium sulfate, and calcium sulfate, and preferably calcium chloride and magnesium sulfate.

[0107] Examples of other metal salts include zinc chloride, titanium chloride, manganese chloride, iron chloride, cobalt chloride, nickel chloride, aluminum chloride, tin chloride, zinc nitrate, titanium nitrate, manganese nitrate, iron nitrate, cobalt nitrate, nickel nitrate, aluminum nitrate, tin nitrate, zinc sulfate, titanium sulfate, manganese sulfate, iron sulfate, cobalt sulfate, nickel sulfate, aluminum sulfate, and tin sulfate.

[0108] These coagulants can be used alone or in combination of two or more, and the amount used is usually 0.01 to 100 parts by weight, preferably 0.1 to 50 parts by weight, and more preferably 1 to 30 parts by weight, relative to 100 parts by weight of the monomer component. When the coagulant is in this range, it is preferable because it can sufficiently coagulate the acrylic rubber while highly improving the compression set resistance and water resistance when the acrylic rubber is crosslinked.

[0109] The coagulant concentration of the coagulation liquid used is usually in the range of 0.1 to 20% by weight, preferably 0.5 to 15% by weight, more preferably 1 to 10% by weight, and particularly preferably 1.5 to 5% by weight, which is suitable for concentrating the particle size of the generated hydrous crumbs uniformly in a specific region.

[0110] The temperature of the coagulation liquid is not particularly limited, but when it is usually 40°C or higher, preferably 40 to 90°C, more preferably in the range of 50 to 80°C, uniform water-containing crumbs are preferably formed.

[0111] The method for contacting the emulsion polymerization liquid containing the phenolic antioxidant represented by general formula (1) added with the coagulating liquid is not particularly limited, and any method may be used, such as a method of adding the coagulating liquid to the emulsion polymerization liquid, a method of adding the coagulating liquid to the emulsion polymerization liquid while it is being stirred, a method of adding the emulsion polymerization liquid to the coagulating liquid, or a method of adding the emulsion polymerization liquid to the coagulating liquid while it is being stirred. However, the method of adding the emulsion polymerization liquid to the coagulating liquid while being stirred is preferable because it provides excellent washing efficiency and dehydration efficiency for the generated water-containing crumbs and can significantly improve the water resistance and storage stability of the obtained acrylic rubber.

[0112] The stirring speed (rotation speed) of the stirred coagulation liquid, that is, the rotation speed of the stirring blade of the stirring device, is not particularly limited, but is usually 100 rpm or more, preferably 200 to 1,000 rpm, more preferably 300 to 900 rpm, and particularly preferably in the range of 400 to 800 rpm.

[0113] A rotation speed that provides a certain degree of vigorous stirring is preferable, as this allows the particle size of the hydrous crumbs to be small and uniform. By setting the rotation speed above the lower limit, the generation of crumbs with excessively large and small particle sizes can be prevented, and by setting the rotation speed below the upper limit, the coagulation reaction can be more easily controlled.

[0114] The peripheral speed of the stirred coagulation liquid, that is, the speed of the outer periphery of the stirring blade of the stirring device, is not particularly limited, but it is preferable to stir vigorously to a certain extent so that the particle size of the generated water-containing crumbs can be made small and uniform, and is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. On the other hand, the upper limit of the peripheral speed is not particularly limited, but it is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less, which is preferable because it makes it easier to control the coagulation reaction.

[0115] By setting the above conditions for the coagulation reaction in the coagulation step (such as the contact method, the solids concentration of the emulsion polymerization liquid, the concentration and temperature of the coagulation liquid, the number of rotations and peripheral speed when stirring the coagulation liquid) within specific ranges, the shape and diameter of the water-containing crumbs that are generated are uniform and focused, and removal of the emulsifier and coagulant during washing and dehydration is significantly improved, resulting in highly improved water resistance and storage stability of the acrylic rubber that is produced, which is therefore preferable.

[0116] (Cleaning process) The washing method of the produced water-containing crumbs is not particularly limited and may be performed according to a conventional method, but it is preferable to use warm water to increase the efficiency of removing the emulsifier and coagulant from the water-containing crumbs.

[0117] The amount of warm water used is not particularly limited, but when the amount per one water wash is usually 50 parts by weight or more, preferably 50 to 15,000 parts by weight, more preferably 100 to 10,000 parts by weight, and particularly preferably 150 to 5,000 parts by weight, relative to 100 parts by weight of the monomer component, it is suitable because the ash content in the acrylic rubber can be effectively reduced.

[0118] The temperature of the warm water used for washing is not particularly limited, but is usually 40° C. or higher, preferably 40 to 100° C., more preferably 50 to 90° C., and most preferably 60 to 80° C., which is suitable because it can remarkably improve the washing efficiency.

[0119] By setting the temperature of the washing water to the lower limit or higher, the emulsifier and coagulant are released from the water-containing crumbs, and the washing efficiency is further improved.

[0120] The washing time is not particularly limited, but is usually in the range of 1 to 120 minutes, preferably 2 to 60 minutes, and more preferably 3 to 30 minutes.

[0121] The number of washings is not particularly limited, and is usually 1 to 10 times, preferably multiple times, and more preferably 2 to 3 times. From the viewpoint of reducing the amount of residual coagulant in the finally obtained acrylic rubber, it is desirable to wash with water more frequently, but the number of washings can be significantly reduced by specifying the shape and diameter of the water-containing crumbs and / or setting the washing temperature within the above range.

[0122] (Dehydration process) In the present invention, it is preferable to squeeze out water from the above-mentioned washed wet crumbs using a dehydrator before drying the same, since this makes it possible to significantly reduce the ash content in the acrylic rubber.

[0123] The water-containing crumbs to be subjected to the dehydrator are preferably those from which free water has been separated using a drainer after washing. As the drainer, any known device can be used without particular limitation, for example, a wire mesh, a screen, an electric sieve, etc., and preferably a wire mesh or a screen. The water content of the water-containing crumbs after draining, i.e., the water content of the water-containing crumbs to be fed into the dehydration and drying process, is not particularly limited, but is usually in the range of 50 to 80% by weight, preferably 50 to 70% by weight, more preferably 50 to 60% by weight.

[0124] The dehydrator is not particularly limited and may be any ordinary method, for example, a centrifuge, a squeezer, a screw-type extruder, etc., and in particular, a screw-type extruder is suitable because it can efficiently remove water from the water-containing crumb and reduce the water content to a high level. In the case of a centrifuge, etc., the acrylic rubber adheres to the wall surface and between the slits, and the water content of the viscous acrylic rubber can only be dehydrated to about 45 to 55% by weight, so a mechanism that forcibly squeezes out the water, such as a screw-type extruder, is suitable.

[0125] The slit width of the dehydrator is not particularly limited, but is usually in the range of 0.1 to 1 mm, preferably 0.2 to 0.6 mm, which is suitable for achieving a high balance between the efficiency of removing the coagulant and emulsifier from the water-containing crumbs and the productivity.

[0126] The water content after dehydration, in which the water content of the hydrous crumbs is squeezed out, is not particularly limited, but is usually in the range of 1 to 50% by weight, preferably 1 to 40% by weight, more preferably 5 to 40% by weight, particularly preferably 10 to 35% by weight, and most preferably 15 to 35% by weight. By setting the water content after dehydration to the lower limit or more, the dehydration time can be shortened and deterioration of the acrylic rubber can be suppressed, and by setting it to the upper limit or less, the ash content can be sufficiently reduced.

[0127] (drying process) The drying method is not particularly limited and may be a conventional method, for example, using a dryer such as a hot air dryer, a reduced pressure dryer, an expander dryer, a kneader type dryer, or a screw type extruder.

[0128] The drying temperature may be appropriately selected, but is usually suitable within the range of 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C, since this allows efficient drying without discoloration or deterioration of the acrylic rubber and reduces the amount of gel insoluble in methyl ethyl ketone in the acrylic rubber sheet.

[0129] The drying time is not particularly limited and can be appropriately selected depending on the target moisture content and the drying method.

[0130] The acrylic rubber thus obtained has a remarkably excellent storage stability. The water content of the obtained acrylic rubber is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less. The shape of the acrylic rubber is not particularly limited, and may be, for example, any of crumb, powder, rod, sheet, etc.

[0131] <Sheet or veil-shaped acrylic rubber> The sheet-like or veil-like acrylic rubber of the present invention is one form of the above-mentioned acrylic rubber, and is overwhelmingly superior in workability compared to crumb-like forms, and is preferable because the specific surface area of ​​the acrylic rubber is small and the storage stability is remarkably excellent. The sheet-like or veil-like acrylic rubber of the present invention is in a raw rubber state and is uncrosslinked.

[0132] The thickness of the sheet-like acrylic rubber of the present invention is not particularly limited and is appropriately selected depending on the intended use, but is usually 1 to 40 mm, preferably 2 to 35 mm, more preferably 3 to 30 mm, and most preferably 5 to 25 mm, which is suitable for achieving a high balance of workability, storage stability, and productivity. The width of the sheet-like acrylic rubber of the present invention is appropriately selected depending on the intended use, but is particularly suitable for excellent handling properties when it is usually 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm. The length of the sheet-like acrylic rubber of the present invention is not particularly limited, but is particularly suitable for excellent handling properties when it is usually 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm.

[0133] The shape of the veil-shaped acrylic rubber of the present invention is not particularly limited and is appropriately selected depending on the intended use, but in many cases, a rectangular parallelepiped is suitable. The size of the veil-shaped acrylic rubber of the present invention is not particularly limited and is appropriately selected depending on the intended use, but the width is usually in the range of 100 to 800 mm, preferably 200 to 500 mm, more preferably 250 to 450 mm, the length is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, more preferably 500 to 800 mm, and the height (thickness) is usually in the range of 50 to 500 mm, preferably 100 to 300 mm, more preferably 150 to 250 mm.

[0134] The specific gravity of the sheet-like or veil-like acrylic rubber of the present invention is not particularly limited, but is preferably 0.7 or more, more preferably 0.8 or more, more preferably 0.9 or more, particularly preferably 0.95 or more, and most preferably 1 or more, since it contains almost no air and has excellent storage stability. The specific gravity of the sheet-like or veil-like acrylic rubber of the present invention is also preferably in the range of usually 0.7 to 1.6, preferably 0.8 to 1.5, more preferably 0.9 to 1.4, particularly preferably 0.95 to 1.3, and most preferably 1.0 to 1.2, since it is highly balanced between productivity, storage stability, and the stability of the crosslinking properties of the crosslinked product.

[0135] The gel content of the sheet-like or veil-like acrylic rubber of the present invention is not particularly limited, but when the gel content, in terms of the content insoluble in methyl ethyl ketone, is usually 50% by weight or less, preferably 30% by weight or less, more preferably 20% by weight or less, particularly preferably 10% by weight or less, and most preferably 5% by weight or less, storage stability and processability are highly improved, and this is suitable.

[0136] The sheet-like or veil-like acrylic rubber of the present invention is one form of the above-mentioned acrylic rubber, and includes characteristic values ​​other than the above-mentioned specific gravity and gel amount, such as monomer composition, reactive group amount, weight average molecular weight (Mw), ratio of z-average molecular weight (Mz) to weight average molecular weight (Mw) (Mz / Mw), glass transition temperature (Tg), ash content, ash component amount (total amount of sodium, magnesium, calcium, phosphorus and sulfur, total amount of magnesium and phosphorus, magnesium, The characteristic values ​​of the acrylic rubber, such as the amount of sodium or phosphorus, the ash content, the complex viscosity at 60°C ([η]60°C), the complex viscosity at 100°C ([η]100°C), the ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C), the water content, the pH, and the Mooney viscosity (ML1+4, 100°C), are the same as those exemplified and in the preferred range for the acrylic rubber.

[0137] The acrylic rubber component content in the sheet-like or veil-like acrylic rubber of the present invention is usually 85% by weight, preferably 90% by weight or more, more preferably 95% by weight or more, particularly preferably 97% by weight or more, and most preferably 98% by weight or more. The acrylic rubber component content in the sheet-like or veil-like acrylic rubber of the present invention excludes the amount of ash remaining after the emulsifier and coagulant used in the production of the acrylic rubber cannot be completely removed, and the amount of antioxidant added and dispersed in the acrylic rubber.

[0138] The sheet- or veil-like acrylic rubber of the present invention is excellent in operability and storage stability, and further, is excellent in strength properties, processability and resistance to compression set, and can be used as is or after cutting.

[0139] <Method for producing sheet or veil acrylic rubber> The method for producing the sheet-like or veil-like acrylic rubber is not particularly limited, but it is preferable to carry out molding processing subsequent to the above-mentioned method for producing the acrylic rubber.

[0140] Specific examples of the method for producing the sheet- or veil-shaped acrylic rubber include the following: an emulsion polymerization step of emulsifying a monomer component containing a (meth)acrylic acid ester, a reactive group-containing monomer, and, if necessary, other copolymerizable monomers with water and an emulsifier, and emulsion-polymerizing the monomer component in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid; an antioxidant addition step of adding a phenol-based antioxidant represented by the general formula (1) to the obtained emulsion polymerization liquid; a coagulation step of contacting the emulsion polymerization liquid containing the antioxidant with a coagulation liquid to produce water-containing crumbs; A washing step of washing the produced hydrous crumbs; a dehydration, drying and molding process in which the washed wet crumbs are dehydrated in the dehydration barrel using a screw-type extruder having a dehydration slit, a drying barrel under reduced pressure, and a die at the tip to a moisture content of 1 to 40% by weight, and then dried in the drying barrel to a moisture content of less than 1% by weight, and a sheet-like dried rubber is extruded through the die; The method for producing a sheet-shaped acrylic rubber includes the steps of:

[0141] Furthermore, there can be mentioned a method for producing a veiled acrylic rubber, which further includes a bale-forming step of laminating the extruded sheet-like dried rubber to form bales.

[0142] (emulsion polymerization process, coagulation process and washing process) The emulsion polymerization step, coagulation step and washing step in the method for producing sheet-like or veil-like acrylic rubber are the same as those described in the above-mentioned method for producing acrylic rubber.

[0143] (Dehydration, drying, molding process) The dehydrating, drying and molding steps in the manufacturing method for sheet-like or veil-like acrylic rubber are characterized in that the above-mentioned washed wet crumbs are dehydrated in the dehydrating barrel using a dehydrating barrel with a dehydration slit, a drying barrel under reduced pressure, and a screw-type extruder having a die at the tip to a moisture content of 1 to 40% by weight, and then dried in the drying barrel to a moisture content of less than 1% by weight, and sheet-like dried rubber is extruded through the die.

[0144] In the present invention, the water-containing crumbs to be supplied to the screw-type extruder are preferably those from which free water has been removed (drained) after washing.

[0145] Draining process In the method for producing the sheet-like or veil-like acrylic rubber of the present invention, it is preferable to provide a draining step in which free water is separated from the hydrous crumbs after washing with a drainer after the water-washing step and before the dehydrating, drying and molding steps, in order to increase the dehydration efficiency.

[0146] Any known draining machine can be used without any particular limitation, and examples thereof include wire mesh, screens, and electric sifters, with wire mesh and screens being preferred.

[0147] The opening of the drainer is not particularly limited, but is usually in the range of 0.01 to 5 mm, preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm, which is suitable for minimizing loss of water-containing crumb and enabling efficient draining.

[0148] The moisture content of the hydrous crumbs after draining, i.e., the moisture content of the hydrous crumbs fed into the dehydration and drying process, is not particularly limited, but is usually in the range of 50 to 80% by weight, preferably 50 to 70% by weight, and more preferably 50 to 60% by weight.

[0149] The temperature of the hydrous crumbs after draining, i.e., the temperature of the hydrous crumbs fed into the dehydration and drying step, is not particularly limited, but is usually in the range of 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, particularly preferably 55 to 85°C, and most preferably 60 to 80°C, which is suitable for efficiently dehydrating and drying hydrous crumbs such as the acrylic rubber of the present invention, which has a high specific heat of 1.5 to 2.5 KJ / kg K and is difficult to raise in temperature, using a screw-type extruder.

[0150] Dehydration of crumbs (dehydration barrel section) The dehydration of the hydrous crumb is carried out in a dehydration barrel having a dehydration slit. The opening of the dehydration slit may be appropriately selected depending on the conditions of use, but it is usually in the range of 0.01 to 5 mm, preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm, which is suitable for efficient dehydration of the hydrous crumb with little hydrous crumb loss.

[0151] The number of dehydration barrels in the screw-type extruder is not particularly limited, but it is generally suitable to have multiple barrels, preferably 2 to 10 barrels, and more preferably 3 to 6 barrels, in order to efficiently dehydrate the viscous acrylic rubber.

[0152] Water is removed from the wet crumb in the dewatering barrel in two ways: in liquid form (wastewater) through the dewatering slit, and in vapor form (exhaust steam). In the present invention, the wastewater is defined as dewatering, and the exhaust steam is defined as pre-drying, to distinguish between the two.

[0153] The water discharged from the dehydration slit in the dehydration of the water-containing crumbs may be in either a liquid state (wastewater) or a vapor state (exhaust steam), but when a screw-type extruder equipped with a plurality of dehydration barrels is used, it is preferable to combine the drainage and exhaust steam, since this allows efficient dehydration of the viscous acrylic rubber.Whether the drainage type dehydration barrel or the exhaust steam type dehydration barrel of a screw-type extruder equipped with three or more dehydration barrels can be selected appropriately depending on the intended use, but when the ash content of the sheet-like or bale-like acrylic rubber that is usually produced is to be reduced, the number of drainage type barrels is increased, and when the moisture content is to be reduced, the number of exhaust steam type barrels is increased.

[0154] The set temperature of the dehydration barrel is appropriately selected depending on the monomer composition, ash content, water content, and operating conditions of the acrylic rubber, but is usually in the range of 60 to 150° C., preferably 70 to 140° C., and more preferably 80 to 130° C. The set temperature of the dehydration barrel for dehydration in a drainage state is usually in the range of 60 to 120° C., preferably 70 to 110° C., and more preferably 80 to 100° C. The set temperature of the dehydration barrel for dehydration in an exhaust steam state is usually in the range of 100 to 150° C., preferably 105 to 140° C., and more preferably 110 to 130° C.

[0155] The moisture content after dehydration in the drainage type dehydration in which moisture is squeezed out from the hydrous crumb is not particularly limited, but a moisture content of 1 to 45% by weight, preferably 1 to 40% by weight, more preferably 5 to 35% by weight, and particularly preferably 10 to 35% by weight, is suitable because it provides a high balance between productivity and ash removal efficiency.

[0156] When dehydrating adhesive acrylic rubber having reactive groups using a centrifuge or the like, the acrylic rubber adheres to the dehydration slits and is barely dehydrated (water content is up to about 45 to 55% by weight); however, in the present invention, by using a screw-type extruder that has a dehydration slit and is forcibly squeezed by a screw, it is possible to reduce the water content to this extent.

[0157] In the case where a drainage type dehydration barrel and a steam exhaust type dehydration barrel are provided, the moisture content after drainage in the drainage type dehydration barrel is usually 5 to 40% by weight, preferably 10 to 40% by weight, and more preferably 15 to 35% by weight, and the moisture content after preliminary drying in the steam exhaust type dehydration barrel is usually 1 to 30% by weight, preferably 3 to 20% by weight, and more preferably 5 to 15% by weight.

[0158] By setting the water content after dehydration to above the lower limit, the dehydration time can be shortened and deterioration of the acrylic rubber can be suppressed, whereas by setting it to below the upper limit, the ash content can be sufficiently reduced.

[0159] Drying of moist crumbs (drying barrel section) The drying of the water-containing crumbs after the dehydration is carried out in a drying barrel under reduced pressure.

[0160] The degree of reduced pressure in the drying barrel may be appropriately selected, but is usually 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa, which is suitable for efficiently drying the water-containing crumbs.

[0161] The set temperature of the drying barrel may be appropriately selected, but a temperature in the range of usually 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C is suitable because it enables efficient drying without discoloration or deterioration of the acrylic rubber and also enables the amount of methyl ethyl ketone insoluble in the sheet-like or veil-like acrylic rubber to be reduced.

[0162] The number of drying barrels in the screw extruder is not particularly limited, but is usually more than one, preferably 2 to 10, more preferably 3 to 8. When there are more than one drying barrels, the degree of reduced pressure may be similar for all drying barrels or may be different. When there are more than one drying barrels, the set temperatures may be similar for all drying barrels or may be different, but it is preferable to make the temperature of the discharge part (closer to the die) higher than the temperature of the introduction part (closer to the dehydration barrel) in order to increase the drying efficiency.

[0163] The water content of the dried rubber after drying is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less. In the present invention, it is particularly preferable to melt-extrude the dried rubber in a screw-type extruder with the water content at this value (a state in which almost all water has been removed), since this reduces the amount of methyl ethyl ketone insolubles in the sheet-like or veil-like acrylic rubber.

[0164] In the present invention, the shear rate at which the acrylic rubber is subjected in the drying barrel of the screw extruder in a state in which it is substantially free of water is not particularly limited, but a rate within the range of usually 10 [1 / s] or more, preferably 10 to 400 [1 / s], and more preferably 50 to 250 [1 / s] is suitable because it provides a highly balanced storage stability, processability, strength properties and compression set resistance of the obtained sheet-like or veil-like acrylic rubber.

[0165] The shear viscosity of the acrylic rubber inside the screw-type extruder used in the present invention, particularly in the drying barrel, is not particularly limited, but when it is usually in the range of 12,000 Pa·s or less, preferably 1,000 to 12,000 Pa·s, more preferably 2,000 to 10,000 Pa·s, particularly preferably 3,000 to 7,000 Pa·s, and most preferably 4,000 to 6,000 Pa·s, the storage stability, processability and strength properties of the obtained sheet-like or veil-like acrylic rubber are highly balanced and suitable.

[0166] Drying rubber (die part) The dried rubber dehydrated and dried in the screw section of the dehydrating barrel and the drying barrel is sent to the screw-free straightening die section. A breaker plate or wire mesh may or may not be provided between the screw section and the die section.

[0167] The dried rubber to be extruded is preferably extruded in a sheet form using a die having a substantially rectangular shape, which results in less air entrapment, a high specific gravity, and excellent storage stability.

[0168] The resin pressure in the die section is not particularly limited, but when it is in the range of usually 0.1 to 10 MPa, preferably 0.5 to 5 MPa, and more preferably 1 to 3 MPa, it is suitable because it reduces air entrapment in the sheet-like or veil-like acrylic rubber (high specific gravity) and provides excellent productivity. Screw type extruder and operating conditions The screw length (L) of the screw type extruder used may be appropriately selected depending on the purpose of use, but is usually in the range of 3,000 to 15,000 mm, preferably 4,000 to 10,000 mm, and more preferably 4,500 to 8,000 mm.

[0169] The screw diameter (D) of the screw type extruder used may be appropriately selected depending on the purpose of use, but is usually in the range of 50 to 250 mm, preferably 100 to 200 mm, and more preferably 120 to 160 mm.

[0170] The ratio (L / D) of the screw length (L) to the screw diameter (D) of the screw extruder used is not particularly limited, but is usually in the range of 10 to 100, preferably 20 to 80, and more preferably 30 to 60, which is suitable since the moisture content can be reduced to less than 1% by weight without causing a decrease in the molecular weight of the dried rubber or scorching.

[0171] The rotation speed (N) of the screw-type extruder used may be appropriately selected depending on various conditions, but a rotation speed of usually 10 to 1,000 rpm, preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm is suitable because it enables the water content and methyl ethyl ketone insoluble content of the sheet-like or veil-like acrylic rubber to be efficiently reduced.

[0172] The extrusion rate (Q) of the screw extruder used is not particularly limited, but is usually in the range of 100 to 1,500 kg / hr, preferably 300 to 1,200 kg / hr, more preferably 400 to 1,000 kg / hr, and most preferably 500 to 800 kg / hr.

[0173] The ratio (Q / N) of the extrusion rate (Q) to the rotation speed (N) of the screw extruder used is not particularly limited, but is usually in the range of 2 to 10, preferably 3 to 8, and more preferably 4 to 6.

[0174] Dry rubber sheet The dried rubber extruded from the screw extruder is in the form of a sheet, which is preferable because it has a high specific gravity and highly improved storage stability without entraining air. The dried rubber sheet extruded from the screw extruder is usually cooled and cut into pieces for use as sheet acrylic rubber.

[0175] The thickness of the sheet-like dry rubber extruded from the screw extruder is not particularly limited, but is preferably in the range of usually 1 to 40 mm, preferably 2 to 35 mm, more preferably 3 to 30 mm, and most preferably 5 to 25 mm, which is excellent in workability and productivity. In particular, when the thermal conductivity of the sheet-like dry rubber is as low as 0.15 to 0.35 W / mK and the cooling efficiency is increased to significantly improve the productivity, the thickness of the sheet-like dry rubber is usually in the range of 1 to 30 mm, preferably 2 to 25 mm, more preferably 3 to 15 mm, and particularly preferably 4 to 12 mm.

[0176] The width of the sheet-like dry rubber extruded from the screw extruder is appropriately selected depending on the intended use, but is usually in the range of 300 to 1,200 mm, preferably 400 to 1,000 mm, and more preferably 500 to 800 mm.

[0177] The temperature of the dried rubber extruded from the screw extruder is not particularly limited, but is usually in the range of 100 to 200°C, preferably 110 to 180°C, and more preferably 120 to 160°C.

[0178] The moisture content of the dry rubber extruded from the screw-type extruder is not particularly limited, but is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less.

[0179] The complex viscosity at 100°C of the dry rubber sheet extruded from the screw extruder ([η]100°C) is not particularly limited, but is usually in the range of 1,500 to 6,000 Pa·s, preferably 2,000 to 5,000 Pa·s, more preferably 2,500 to 4,000 Pa·s, and most preferably 2,500 to 3,500 Pa·s, which is suitable for achieving a high balance between extrudability as a sheet and shape retention. That is, by setting the viscosity at or above the lower limit, the extrudability can be made superior, and by setting the viscosity at or below the upper limit, deformation or breakage of the dry rubber sheet can be suppressed.

[0180] The sheet-like dried rubber extruded from the screw-type extruder may be folded as it is for use, but is usually cut for use.

[0181] There is no particular limitation on the cutting of the sheet-like dry rubber, but since the acrylic rubber of the present invention has strong adhesiveness, it is preferable to cool the sheet-like dry rubber before cutting in order to cut it continuously without entraining air.

[0182] The cutting temperature of the dry rubber sheet is not particularly limited, but a temperature of usually 60° C. or less, preferably 55° C. or less, and more preferably 50° C. or less provides a high balance between cuttability and productivity, and is therefore suitable.

[0183] The complex viscosity of the dry rubber sheet at 60°C ([η]60°C) is not particularly limited, but is usually 15,000 Pa·s or less, preferably 2,000 to 10,000 Pa·s, more preferably 2,500 to 7,000 Pa·s, and most preferably 2,700 to 5,500 Pa·s, which allows continuous cutting without entraining air.

[0184] The ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) of the sheet-like dry rubber is not particularly limited and may be appropriately selected depending on the purpose of use, but is usually 0.5 or more, preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.85 or more. When the upper limit is usually 0.98 or less, preferably 0.97 or less, more preferably 0.96 or less, particularly preferably 0.95 or less, and most preferably 0.93 or less, air entrapment is reduced and cutting and productivity are highly balanced, which is suitable.

[0185] The cooling method for the dry rubber sheet is not particularly limited, and the sheet may be left at room temperature. However, since the thermal conductivity of the dry rubber sheet is very low at 0.15 to 0.35 W / mK, forced cooling such as air cooling using ventilation or cooling, water spraying by spraying water, or immersion in water is preferred in order to increase productivity, and air cooling using ventilation or cooling is particularly preferred.

[0186] In the air-cooling method of the sheet-like dry rubber, for example, the sheet-like dry rubber is extruded from a screw-type extruder onto a conveyor such as a belt conveyor, and conveyed and cooled while blowing cold air. The temperature of the cold air is not particularly limited, but is usually in the range of 0 to 25°C, preferably 5 to 25°C, and more preferably 10 to 20°C. The length to be cooled is not particularly limited, but is usually in the range of 5 to 500m, preferably 10 to 200m, and more preferably 20 to 100m. The cooling speed of the sheet-like dry rubber is not particularly limited, but is usually 50°C / hr or more, more preferably 100°C / hr or more, and more preferably 150°C / hr or more, which is particularly easy to cut and is therefore suitable.

[0187] The cut length of the dry rubber sheet is not particularly limited and may be appropriately selected depending on the intended use, but is usually in the range of 100 to 800 mm, preferably 200 to 500 mm, and more preferably 250 to 450 mm.

[0188] The sheet-like acrylic rubber thus obtained is superior in terms of handling, storage stability, processability, strength properties and resistance to compression set compared with crumb-like acrylic rubber, and can be used as is or after being laminated into bales.

[0189] Lamination process The method for producing the veil-shaped acrylic rubber of the present invention is not particularly limited, but it is preferable to laminate the above-mentioned sheet-shaped dry rubber (sheet-shaped acrylic rubber) to obtain a veil-shaped acrylic rubber bale with excellent storage stability and little air entrapment.

[0190] The lamination temperature of the sheet-like dry rubber is not particularly limited, but is usually 30° C. or higher, preferably 35° C. or higher, and more preferably 40° C. or higher, so that air entrapped during lamination can be released. The number of layers may be appropriately selected depending on the size or weight of the veil-like acrylic rubber. The veil-like acrylic rubber of the present invention is integrated by the weight of the laminated sheet-like dry rubber.

[0191] The veil-like acrylic rubber of the present invention thus obtained is superior in operability and storage stability as well as in processability, strength properties and compression set resistance compared with crumb-like acrylic rubber, and the veil-like acrylic rubber can be used as is or can be cut into a required amount and fed into a mixer such as a Banbury mixer or roll mixer.

[0192] <Rubber composition> The rubber composition of the present invention is characterized by comprising a rubber component containing the above-mentioned acrylic rubber (including sheet-like or veil-like acrylic rubber), a filler, and a crosslinking agent.

[0193] The content of the acrylic rubber of the present invention in the rubber component may be selected depending on the intended use and is, for example, usually 30% by weight or more, preferably 50% by weight or more, and more preferably 70% by weight or more.

[0194] As the rubber component, the acrylic rubber of the present invention may be used alone or in combination with other rubbers.

[0195] Examples of other rubbers include acrylic rubbers other than the acrylic rubber of the present invention, natural rubber, polybutadiene rubber, polyisoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, silicone rubber, fluororubber, olefin-based elastomers, styrene-based elastomers, vinyl chloride-based elastomers, polyester-based elastomers, polyamide-based elastomers, polyurethane-based elastomers, and polysiloxane-based elastomers.

[0196] These other rubbers can be used alone or in combination of two or more. The content of the other rubbers in the rubber component is appropriately selected within a range that does not impair the effects of the present invention, and is usually 70% by weight or less, preferably 50% by weight or less, and more preferably 30% by weight or less. The shape of the other rubbers may be any of crumb, sheet, veil, rod, etc.

[0197] The filler is not particularly limited, but examples thereof include reinforcing fillers and non-reinforcing fillers, with reinforcing fillers being preferred.

[0198] Examples of reinforcing fillers include carbon blacks such as furnace black, acetylene black, thermal black, channel black, and graphite; silicas such as wet silica, dry silica, and colloidal silica; etc. Examples of non-reinforcing fillers include quartz powder, diatomaceous earth, zinc oxide, basic magnesium carbonate, activated calcium carbonate, magnesium silicate, aluminum silicate, titanium dioxide, talc, aluminum sulfate, calcium sulfate, barium sulfate, etc.

[0199] These fillers can be used alone or in combination of two or more kinds. The amount of the fillers to be added is appropriately selected within a range that does not impair the effects of the present invention, and is usually in the range of 1 to 200 parts by weight, preferably 10 to 150 parts by weight, and more preferably 20 to 100 parts by weight, per 100 parts by weight of the rubber component.

[0200] The crosslinking agent is not particularly limited, and examples of crosslinking agents that can be used include polyamine compounds such as diamine compounds and carbonates thereof, sulfur compounds, sulfur donors, triazine thiol compounds, polyepoxy compounds, organic ammonium carboxylates, organic peroxides, polycarboxylic acids, quaternary onium salts, imidazole compounds, isocyanuric acid compounds, organic peroxides, and triazine compounds. Among these, polyamine compounds and triazine compounds are preferred, and polyamine compounds are particularly preferred.

[0201] Examples of the polyvalent amine compound include aliphatic polyvalent amine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine; and aromatic polyvalent amine compounds such as 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, and 1,3,5-benzenetriamine. Among these, preferred are hexamethylenediamine carbamate, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, etc. These polyamine compounds are particularly suitable for use in combination with carboxyl group-containing acrylic rubber.

[0202] Examples of triazine compounds include 6-trimercapto-s-triazine, 2-anilino-4,6-dithiol-s-triazine, 1-dibutylamino-3,5-dimercaptotriazine, 2-dibutylamino-4,6-dithiol-s-triazine, 1-phenylamino-3,5-dimercaptotriazine, 2,4,6-trimercapto-1,3,5-triazine, 1-hexylamino-3,5-dimercaptotriazine, etc. These triazine compounds are particularly suitable for use in combination with halogen-containing acrylic rubber.

[0203] These crosslinking agents can be used alone or in combination of two or more, and the amount of the crosslinking agent is usually 0.001 to 20 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the rubber component. By setting the amount of the crosslinking agent within this range, it is possible to obtain excellent mechanical strength as a crosslinked rubber product while ensuring sufficient rubber elasticity, which is preferable.

[0204] The rubber composition of the present invention may further contain other antioxidants in addition to the phenol-based antioxidant represented by the general formula (1). The other antioxidants are not particularly limited, but examples thereof include 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butylphenol, butylhydroxyanisole, 2,6-di-t-butyl-α-dimethylamino-p-cresol, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, styrenated phenol, 2,2'-methylene-bis(6-α-methyl-benzyl-p-cresol), 4,4'-methyl-p-cresol, 2,2 ... and other compounds such as ethylenebis(2,6-di-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, 2,2'-thiobis-(4-methyl-6-t-butylphenol), 4,4'-thiobis-(6-t-butyl-o-cresol), and 2,6-di-t-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol. Other phenol-based antioxidants; phosphorous ester-based antioxidants such as tris(nonylphenyl)phosphite, diphenylisodecylphosphite, and tetraphenyldipropylene glycol diphosphite; sulfur ester-based antioxidants such as dilauryl thiodipropionate; phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonylamido)-diphenylamine, and 4,4'-(α,α-dimethylbenzyl)diphenyl Examples of such antioxidants include amine-based antioxidants such as amines, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and butyraldehyde-aniline condensates; imidazole-based antioxidants such as 2-mercaptobenzimidazole; quinoline-based antioxidants such as 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline; and hydroquinone-based antioxidants such as 2,5-di-(t-amyl)hydroquinone. Among these, amine-based antioxidants are particularly preferred.

[0205] These other antioxidants can be used alone or in combination of two or more kinds. The amount of the antioxidant is in the range of 0.01 to 15 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 1 to 5 parts by weight, based on 100 parts by weight of the rubber component.

[0206] The rubber composition of the present invention comprises the above-mentioned rubber component, filler, crosslinking agent, and, if necessary, other antioxidants other than those represented by general formula (1). Furthermore, if necessary, other additives commonly used in the art, such as crosslinking aids, crosslinking accelerators, crosslinking retarders, silane coupling agents, plasticizers, processing aids, lubricants, pigments, colorants, antistatic agents, and foaming agents, may be optionally blended.

[0207] These other additives may be used alone or in combination of two or more kinds, and the amount of each additive is appropriately selected within a range that does not impair the effects of the present invention.

[0208] The rubber composition of the present invention can be mixed using any means conventionally used in the field of rubber processing, such as an open roll, a Banbury mixer, various kneaders, etc. As for the mixing procedure, it is preferable to thoroughly mix components that are unlikely to react or decompose due to heat, and then mix components that are likely to react or decompose due to heat, such as a crosslinking agent, for a short period of time at a temperature at which no reaction or decomposition occurs.

[0209] <Rubber cross-linked products> The cross-linked rubber product of the present invention is obtained by cross-linking the above-mentioned rubber composition. The cross-linked rubber product of the present invention can be produced by using the rubber composition of the present invention, molding it into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, and a roll, heating it to cause a cross-linking reaction, and fixing the shape as a cross-linked rubber product. In this case, cross-linking may be performed after molding in advance, or simultaneously with molding. The molding temperature is usually 10 to 200°C, preferably 25 to 150°C. The cross-linking temperature is usually 100 to 250°C, preferably 130 to 220°C, more preferably 150 to 200°C, and the cross-linking time is usually 0.1 minutes to 10 hours, preferably 1 minute to 5 hours. As the heating method, a method used for cross-linking rubber, such as press heating, steam heating, oven heating, and hot air heating, may be appropriately selected.

[0210] The cross-linked rubber of the present invention may be further heated to carry out secondary cross-linking depending on the shape, size, etc. of the cross-linked rubber. The secondary cross-linking is preferably carried out for 1 to 48 hours, although it varies depending on the heating method, cross-linking temperature, shape, etc. The heating method and heating temperature may be appropriately selected.

[0211] The cross-linked rubber product of the present invention is suitably used, for example, as sealing materials such as O-rings, packings, diaphragms, oil seals, shaft seals, bearing sheaths, mechanical seals, well head seals, seals for electric and electronic devices, and seals for air compressors; various gaskets such as a rocker cover gasket attached to the joint between a cylinder block and a cylinder head, an oil pan gasket attached to the joint between an oil pan and a cylinder head or a transmission case, a gasket for a fuel cell separator attached between a pair of housings sandwiching a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and a gasket for the top cover of a hard disk drive; cushioning materials, vibration-proof materials; wire covering materials; industrial belts; tubes and hoses; sheets; and the like.

[0212] The cross-linked rubber product of the present invention can also be suitably used as extrusion molded products and mold cross-linked products for automotive applications, for example, various hoses such as fuel hoses, filler neck hoses, vent hoses, paper hoses, fuel oil hoses such as fuel tank hoses, oil hoses, air hoses such as turbo air hoses and transmission control hoses, radiator hoses, heater hoses, brake hoses, and air conditioner hoses.

[0213] <Device configuration used in the production of acrylic rubber> Next, the configuration of the equipment used in the production of the sheet-like or veil-like acrylic rubber according to one embodiment of the present invention will be described. Fig. 1 is a schematic diagram showing an example of an acrylic rubber production system having an equipment configuration used in the production of the sheet-like or veil-like acrylic rubber according to one embodiment of the present invention. For example, the acrylic rubber production system 1 shown in Fig. 1 can be used to produce the acrylic rubber according to the present invention.

[0214] The acrylic rubber production system 1 shown in FIG. 1 is composed of an emulsion polymerization reactor, a coagulation device 3, a washing device 4, a draining machine 43, a screw-type extruder 5, a cooling device 6, and a baling device 7, all of which are not shown.

[0215] The emulsion polymerization reactor is configured to carry out the treatment related to the emulsion polymerization step described above. Although not shown in FIG. 1, the emulsion polymerization reactor has, for example, a polymerization reaction tank, a temperature control unit for controlling the reaction temperature, and a stirring device equipped with a motor and a stirring blade. In the emulsion polymerization reactor, the monomer components for forming the acrylic rubber are mixed with water and an emulsifier, emulsified while being appropriately stirred with a stirrer, and emulsion-polymerized in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid. The addition of the phenol-based antiaging agent represented by the general formula (1) to the emulsion polymerization liquid can be carried out directly in the emulsion polymerization reactor. The emulsion polymerization reactor may be any of a batch type, a semi-batch type, and a continuous type, and may be any of a tank type reactor and a tubular type reactor.

[0216] The solidification device 3 shown in Fig. 1 is configured to perform the above-mentioned solidification process. As shown in Fig. 1, the solidification device 3 has, for example, a stirring tank 30, a heating unit 31 for heating the inside of the stirring tank 30, a temperature control unit (not shown) for controlling the temperature inside the stirring tank 30, a stirring device 34 equipped with a motor 32 and a stirring blade 33, and a drive control unit (not shown) for controlling the number of revolutions and the rotation speed of the stirring blade 33. In the solidification device 3, the emulsion polymerization liquid obtained in the emulsion polymerization reactor is brought into contact with a coagulation liquid as a coagulant and solidified to produce water-containing crumbs.

[0217] In the coagulation device 3, for example, the emulsion polymerization liquid is brought into contact with the coagulation liquid by adding the emulsion polymerization liquid to the coagulation liquid being stirred. That is, the stirring tank 30 of the coagulation device 3 is filled with the coagulation liquid, and the emulsion polymerization liquid is added to and brought into contact with the coagulation liquid to coagulate the emulsion polymerization liquid, thereby generating water-containing crumbs.

[0218] The heating unit 31 of the solidification device 3 is configured to heat the solidification liquid filled in the stirring tank 30. The temperature control unit of the solidification device 3 is configured to control the heating operation by the heating unit 31 while monitoring the temperature in the stirring tank 30 measured by a thermometer, thereby controlling the temperature in the stirring tank 30. The temperature of the solidification liquid in the stirring tank 30 is controlled by the temperature control unit to be usually 40°C or higher, preferably in the range of 40 to 90°C, and more preferably 50 to 80°C.

[0219] The agitator 34 of the solidification device 3 is configured to agitate the solidification liquid filled in the agitation tank 30. Specifically, the agitator 34 includes a motor 32 that generates rotational power, and an agitator blade 33 that spreads in a direction perpendicular to the rotation axis of the motor 32. The agitator blade 33 can cause the solidification liquid filled in the agitation tank 30 to flow by rotating around the rotation axis by the rotational power of the motor 32. The shape, size, and number of the agitator blades 33 to be installed are not particularly limited.

[0220] The drive control unit of the solidification device 3 is configured to control the rotation drive of the motor 32 of the agitation device 34 to set the number of rotations and the rotation speed of the agitation blade 33 of the agitation device 34 to a predetermined value. The rotation of the agitation blade 33 is controlled by the drive control unit so that the agitation speed of the solidification liquid is, for example, usually 100 rpm or more, preferably 200 to 1,000 rpm, more preferably 300 to 900 rpm, and particularly preferably 400 to 800 rpm. The rotation of the agitation blade 33 is controlled by the drive control unit so that the peripheral speed of the solidification liquid is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. Furthermore, the rotation of the agitation blade 33 is controlled by the drive control unit so that the upper limit of the peripheral speed of the solidification liquid is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less.

[0221] The washing device 4 shown in Fig. 1 is configured to carry out the treatment related to the above-mentioned washing step. As shown in Fig. 1, the washing device 4 has, for example, a washing tank 40, a heating unit 41 for heating the inside of the washing tank 40, and a temperature control unit (not shown) for controlling the temperature inside the washing tank 40. In the washing device 4, the water-containing crumbs generated in the solidifying device 3 are mixed with a large amount of water and washed, thereby effectively reducing the amount of ash in the finally obtained sheet-like or veil-like acrylic rubber.

[0222] The heating unit 41 of the cleaning device 4 is configured to heat the inside of the cleaning tank 40. The temperature control unit of the cleaning device 4 is configured to control the heating operation by the heating unit 41 while monitoring the temperature inside the cleaning tank 40 measured by a thermometer, thereby controlling the temperature inside the cleaning tank 40. As described above, the temperature of the cleaning water inside the cleaning tank 40 is controlled to be usually in the range of 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, and most preferably 60 to 80°C.

[0223] The water-containing crumb washed in the washing device 4 is supplied to a screw-type extruder 5 which performs a dehydration step and a drying step. At this time, the water-containing crumb after washing is preferably supplied to the screw-type extruder 5 through a drainer 43 capable of separating free water. For the drainer 43, for example, a wire net, a screen, an electric sieve, or the like can be used.

[0224] In addition, when the washed wet crumbs are supplied to the screw-type extruder 5, the temperature of the wet crumbs is preferably 40° C. or higher, more preferably 60° C. or higher. For example, the temperature of the water used for washing in the washing device 4 may be set to 60° C. or higher (e.g., 70° C.) so that the temperature of the wet crumbs when supplied to the screw-type extruder 5 can be maintained at 60° C. or higher, or the wet crumbs may be heated to a temperature of 40° C. or higher, preferably 60° C. or higher, when conveyed from the washing device 4 to the screw-type extruder 5. This makes it possible to effectively perform the subsequent dehydration and drying steps, and to significantly reduce the moisture content of the finally obtained dried rubber.

[0225] The screw-type extruder 5 shown in Fig. 1 is configured to perform the processes related to the dehydration step and the drying step described above. Although the screw-type extruder 5 is shown in Fig. 1 as a suitable example, a centrifuge or a squeezer may be used as a dehydrator that performs the process related to the dehydration step, and a hot air dryer, a reduced pressure dryer, an expander dryer, a kneader dryer, etc. may be used as a dryer that performs the process related to the drying step.

[0226] The screw-type extruder 5 is configured to mold the dried rubber obtained through the dehydration process and the drying process into a predetermined shape and discharge it. Specifically, the screw-type extruder 5 is equipped with a dehydration barrel section 53 having a function as a dehydrator for dehydrating the wet crumbs washed in the washing device 4, and a drying barrel section 54 having a function as a dryer for drying the wet crumbs, and further equipped with a die 59 downstream of the screw-type extruder 5 having a molding function for molding the wet crumbs.

[0227] Hereinafter, the configuration of the screw-type extruder 5 will be described with reference to Fig. 2. Fig. 2 shows the configuration of a specific example suitable for the screw-type extruder 5 shown in Fig. 1. By using this screw-type extruder 5, the above-mentioned dehydration and drying process can be suitably carried out.

[0228] The screw-type extruder 5 shown in Fig. 2 is a twin-screw type extrusion dryer having a pair of screws (not shown) in a barrel unit 51. The screw-type extruder 5 has a drive unit 50 that rotates and drives the pair of screws in the barrel unit 51. The drive unit 50 is attached to the upstream end (left end in Fig. 2) of the barrel unit 51. The screw-type extruder 5 also has a die 59 at the downstream end (right end in Fig. 2) of the barrel unit 51.

[0229] The barrel unit 51 has, from the upstream side to the downstream side (from the left side to the right side in FIG. 2), a supply barrel section 52, a dewatering barrel section 53, and a drying barrel section .

[0230] The supply barrel section 52 is made up of two supply barrels, that is, a first supply barrel 52a and a second supply barrel 52b.

[0231] The dehydration barrel section 53 is made up of three dehydration barrels, that is, a first dehydration barrel 53a, a second dehydration barrel 53b, and a third dehydration barrel 53c.

[0232] The drying barrel section 54 is composed of eight drying barrels, namely, a first drying barrel 54a, a second drying barrel 54b, a third drying barrel 54c, a fourth drying barrel 54d, a fifth drying barrel 54e, a sixth drying barrel 54f, a seventh drying barrel 54g, and an eighth drying barrel 54h.

[0233] In this manner, the barrel unit 51 is configured by connecting the divided 13 barrels 52a to 52b, 53a to 53c, and 54a to 54h from the upstream side to the downstream side.

[0234] The screw-type extruder 5 also has heating means (not shown) for individually heating each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h to heat the water-containing crumbs in each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h to a predetermined temperature. The number of heating means corresponds to each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h. As such a heating means, for example, a configuration in which high-temperature steam is supplied from a steam supply means to a steam circulation jacket formed in each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h is adopted, but is not limited thereto. The screw-type extruder 5 also has temperature control means (not shown) for controlling the set temperature of each heating means corresponding to each of the barrels 52a to 52b, 53a to 53c, and 54a to 54h.

[0235] The number of supply barrels, dewatering barrels, and drying barrels constituting each of barrel portions 52, 53, and 54 in barrel unit 51 is not limited to the embodiment shown in FIG. 2, and can be set to a number depending on factors such as the moisture content of the moisture-containing acrylic rubber crumbs to be dried.

[0236] For example, the number of supply barrels installed in supply barrel section 52 is, for example, 1 to 3. The number of dehydration barrels installed in dehydration barrel section 53 is, for example, preferably 2 to 10, and more preferably 3 to 6, since this allows efficient dehydration of the water-containing crumbs of sticky acrylic rubber. The number of drying barrels installed in drying barrel section 54 is, for example, preferably 2 to 10, and more preferably 3 to 8.

[0237] The pair of screws in the barrel unit 51 are rotated by a driving means such as a motor housed in the drive unit 50. The pair of screws extend from the upstream side to the downstream side in the barrel unit 51, and are rotated to convey the wet crumb supplied to the supply barrel section 52 to the downstream side while mixing them. The pair of screws is preferably a twin-shaft intermeshing type in which the peaks and valleys are intermeshed with each other, which can increase the dewatering and drying efficiency of the wet crumb.

[0238] The rotation directions of the pair of screws may be the same or different, but from the viewpoint of self-cleaning performance, it is preferable that the screws rotate in the same direction. The screw shape of the pair of screws is not particularly limited as long as it is a shape required for each of the barrel portions 52, 53, and 54.

[0239] The supply barrel section 52 is a region for supplying the wet crumbs into the barrel unit 51. The first supply barrel 52a of the supply barrel section 52 has a feed port 55 for supplying the wet crumbs into the barrel unit 51.

[0240] The dewatering barrel section 53 is a region where liquid (serum water) containing a coagulant and the like is separated from the water-containing crumbs and discharged.

[0241] The first to third dewatering barrels 53a to 53c constituting the dewatering barrel section 53 each have a dewatering slit 56a, 56b, 56c for discharging moisture from the wet crumb to the outside. A plurality of dewatering slits 56a, 56b, 56c are formed in each of the dewatering barrels 53a to 53c.

[0242] The slit width, i.e., mesh size, of each dewatering slit 56a, 56b, 56c may be appropriately selected depending on the conditions of use, and is typically 0.01 to 5 mm. From the viewpoints of minimizing loss of moist crumb and enabling efficient dewatering of the moist crumb, the width is preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm.

[0243] The removal of moisture from the wet crumb in each of the dehydration barrels 53a to 53c of the dehydration barrel section 53 can be done in two ways: in liquid form through the dehydration slits 56a, 56b, and 56c, and in vapor form. In the dehydration barrel section 53 of this embodiment, the removal of moisture in liquid form is defined as drainage, and the removal of moisture in vapor form is defined as exhaust steam, and are distinguished between these.

[0244] In the dehydration barrel section 53, the combination of drainage and exhaust steam is suitable because it can efficiently reduce the moisture content of the viscous acrylic rubber. In the dehydration barrel section 53, which of the first to third dehydration barrels 53a to 53c is used for drainage or steam exhaust may be appropriately set according to the purpose of use, but when the amount of ash in the acrylic rubber to be produced is usually reduced, it is preferable to increase the number of dehydration barrels for drainage. In that case, for example, as shown in FIG. 2, drainage is performed in the first and second dehydration barrels 53a and 53b on the upstream side, and steam exhaust is performed in the third dehydration barrel 53c on the downstream side. In addition, for example, when the dehydration barrel section 53 has four dehydration barrels, it is possible to consider an embodiment in which drainage is performed in three dehydration barrels on the upstream side and steam exhaust is performed in one dehydration barrel on the downstream side. On the other hand, when the moisture content is reduced, it is preferable to increase the number of dehydration barrels for steam exhaust.

[0245] As described above in the dehydrating / drying process, the set temperature of the dehydrating barrel section 53 is usually in the range of 60 to 150°C, preferably 70 to 140°C, and more preferably 80 to 130°C. The set temperature of the dehydrating barrel for dehydrating in a drainage state is usually in the range of 60 to 120°C, preferably 70 to 110°C, and more preferably 80 to 100°C. The set temperature of the dehydrating barrel for dehydrating in an exhaust steam state is usually in the range of 100 to 150°C, preferably 105 to 140°C, and more preferably 110 to 130°C.

[0246] The drying barrel section 54 is a region where the dehydrated water-containing crumbs are dried under reduced pressure. Among the first to eighth drying barrels 54a to 54h constituting the drying barrel section 54, the second drying barrel 54b, the fourth drying barrel 54d, the sixth drying barrel 54f and the eighth drying barrel 54h each have a vent port 58a, 58b, 58c, 58d for degassing. The vent ports 58a, 58b, 58c, 58d are each connected to a vent pipe (not shown).

[0247] A vacuum pump (not shown) is connected to the end of each vent pipe, and the pressure inside the drying barrel portion 54 is reduced to a predetermined level by operation of the vacuum pumps. The screw-type extruder 5 has a pressure control means (not shown) that controls the operation of the vacuum pumps to control the degree of reduced pressure inside the drying barrel portion 54.

[0248] The degree of reduced pressure in the drying barrel section 54 may be appropriately selected, but as described above, it is usually set to 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa.

[0249] The temperature set within the drying barrel section 54 may be appropriately selected, but as described above, it is usually set to 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C.

[0250] In each of the drying barrels 54a to 54h that make up the drying barrel section 54, the set temperatures in all of the drying barrels 54a to 54h may be similar or different, but it is preferable to set the temperature on the downstream side (die 59 side) higher than the temperature on the upstream side (dehydration barrel section 53 side), as this improves drying efficiency.

[0251] The die 59 is a metal mold disposed at the downstream end of the barrel unit 51, and has an outlet of a predetermined nozzle shape. The acrylic rubber dried in the drying barrel section 54 passes through the outlet of the die 59, and is extruded into a shape corresponding to the predetermined nozzle shape. The acrylic rubber passing through the die 59 is molded into various shapes, such as granular, columnar, round rod, and sheet, depending on the nozzle shape of the die 59. For example, the acrylic rubber can be extruded into a sheet by forming the outlet of the die 59 into a substantially rectangular shape. A breaker plate or a wire mesh may or may not be provided between the screw and the die 59.

[0252] According to the screw-type extruder 5 of this embodiment, the water-containing crumbs of the raw acrylic rubber are extruded into a sheet-like dry rubber in the following manner.

[0253] The hydrous crumbs of the acrylic rubber obtained through the washing process are supplied to the supply barrel section 52 from the feed port 55. The hydrous crumbs supplied to the supply barrel section 52 are transferred from the supply barrel section 52 to the dehydration barrel section 53 by the rotation of the pair of screws in the barrel unit 51. In the dehydration barrel section 53, the hydrous crumbs are dehydrated by draining water contained in the hydrous crumbs and discharging steam from the dehydration slits 56a, 56b, and 56c provided in the first to third dehydration barrels 53a to 53c, respectively, as described above.

[0254] The water-containing crumbs dewatered in the dewatering barrel section 53 are sent to the drying barrel section 54 by the rotation of a pair of screws in the barrel unit 51. The water-containing crumbs sent to the drying barrel section 54 are plasticized and mixed to become a melt, and are transported downstream while generating heat and increasing in temperature. Then, the water contained in the acrylic rubber melt vaporizes, and the water (steam) is discharged to the outside through vent pipes (not shown) connected to each of the vent ports 58a, 58b, 58c, and 58d.

[0255] As described above, by passing through the drying barrel section 54, the water-containing crumb is dried and becomes a molten acrylic rubber. The acrylic rubber is supplied to the die 59 by the rotation of the pair of screws in the barrel unit 51 and is extruded from the die 59 as a sheet-like dried rubber.

[0256] Here, an example of operating conditions for the screw-type extruder 5 according to this embodiment will be given.

[0257] The rotation speed (N) of the pair of screws in barrel unit 51 may be appropriately selected depending on various conditions, and is usually set to 10 to 1,000 rpm. From the viewpoint of efficiently reducing the water content and gel amount in the acrylic rubber veil, it is preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm.

[0258] The extrusion rate (Q) of the acrylic rubber is not particularly limited, but is usually 100 to 1,500 kg / hr, preferably 300 to 1,200 kg / hr, more preferably 400 to 1,000 kg / hr, and most preferably 500 to 800 kg / hr.

[0259] In addition, the ratio (Q / N) of the extrusion amount (Q) of the acrylic rubber to the screw rotation speed (N) is not particularly limited, but is usually 1 to 20, preferably 2 to 10, more preferably 3 to 8, and particularly preferably 4 to 6.

[0260] The cooling device 6 shown in Fig. 1 is configured to cool the dried rubber obtained through the dehydration process using a dehydrator and the drying process using a dryer. As a cooling method using the cooling device 6, various methods can be adopted, including an air-cooling method using blowing air or air conditioning, a water-spraying method in which water is sprayed, and an immersion method in which the rubber is immersed in water. The dried rubber may also be cooled by leaving it at room temperature.

[0261] As described above, the dry rubber discharged from the screw-type extruder 5 is extruded and molded into various shapes such as granules, columns, round rods, sheets, etc., depending on the nozzle shape of the die 59. Hereinafter, as an example of the cooling device 6, a conveying type cooling device 60 that cools the sheet-shaped dry rubber (sheet-shaped acrylic rubber) 10 molded into a sheet will be described with reference to Fig. 3.

[0262] Fig. 3 shows the configuration of a conveyor-type cooling device 60 suitable for use as the cooling device 6 shown in Fig. 1. The conveyor-type cooling device 60 shown in Fig. 3 is configured to cool the sheet-like dry rubber 10 discharged from the discharge port of the die 59 of the screw-type extruder 5 by air cooling while conveying the sheet-like dry rubber 10. By using this conveyor-type cooling device 60, the sheet-like dry rubber discharged from the screw-type extruder 5 can be suitably cooled.

[0263] The conveying cooling device 60 shown in FIG. 3 is used by being directly connected to the die 59 of the screw-type extruder 5 shown in FIG.

[0264] The conveying type cooling device 60 has a conveyor 61 that conveys the sheet-like dried rubber 10 discharged from the die 59 of the screw-type extruder 5 in the direction of arrow A in Figure 3, and a cooling means 65 that blows cold air onto the sheet-like dried rubber 10 on the conveyor 61.

[0265] The conveyor 61 has rollers 62, 63, and a conveyor belt 64 that is wound around the rollers 62, 63 and on which the sheet-like dry rubber 10 is placed. The conveyor 61 is configured to continuously transport the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5 onto the conveyor belt 64 downstream (to the right in FIG. 3).

[0266] The cooling means 65 is not particularly limited, but may be, for example, a means configured to blow cooling air sent from a cooling air generating means (not shown) onto the surface of the sheet-like dried rubber 10 on the conveyor belt 64.

[0267] The length L1 of the conveyor 61 and the cooling means 65 of the transport-type cooling device 60 (the length of the part where cooling air can be blown) is not particularly limited, but is, for example, 10 to 100 m, and preferably 20 to 50 m. The transport speed of the sheet-like dry rubber 10 in the transport-type cooling device 60 may be appropriately adjusted depending on the length L1 of the conveyor 61 and the cooling means 65, the discharge speed of the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5, the target cooling speed and cooling time, and is, for example, 10 to 100 m / hr, and more preferably 15 to 70 m / hr.

[0268] According to the conveying type cooling device 60 shown in Figure 3, the sheet-like dry rubber 10 discharged from the die 59 of the screw-type extruder 5 is conveyed by a conveyor 61 while cooling air is blown from a cooling means 65 onto the sheet-like dry rubber 10, thereby cooling the sheet-like dry rubber 10.

[0269] 3, the transportable cooling device 60 is not particularly limited to a configuration including one conveyor 61 and one cooling means 65, but may be configured to include two or more conveyors 61 and two or more corresponding cooling means 65. In that case, the total length of each of the two or more conveyors 61 and the cooling means 65 may be within the above range.

[0270] The baling device 7 shown in Fig. 1 is configured to process the dry rubber extruded from the screw-type extruder 5 and cooled by the cooling device 6 to produce a bale, which is a block. As described above, the screw-type extruder 5 is capable of extruding the dry rubber into various shapes such as granules, columns, round bars, and sheets, and the baling device 7 is configured to bales the dry rubber thus formed into various shapes. The weight and shape of the baled acrylic rubber produced by the baling device 7 are not particularly limited, but for example, a roughly rectangular parallelepiped baled acrylic rubber weighing about 20 kg is produced.

[0271] The baling device 7 may include, for example, a baler, and the cooled, dried rubber may be compressed by the baler to produce baled acrylic rubber.

[0272] In addition, when the sheet-like dry rubber (sheet-like acrylic rubber) 10 is produced by the screw-type extruder 5, a bale-like acrylic rubber may be produced by stacking the sheet-like dry rubber 10. For example, a cutting mechanism for cutting the sheet-like dry rubber 10 may be provided in the baling device 7 arranged downstream of the conveying cooling device 60 shown in FIG. 3. Specifically, the cutting mechanism of the baling device 7 is configured to continuously cut the cooled sheet-like dry rubber 10 at predetermined intervals and process it into cut sheet-like dry rubber 16 of a predetermined size. A plurality of cut sheet-like dry rubber 16 cut to a predetermined size by the cutting mechanism are stacked to produce a bale-like acrylic rubber in which the cut sheet-like dry rubber 16 is stacked.

[0273] When manufacturing a veil-shaped acrylic rubber in which cut sheet-shaped dry rubber 16 is laminated, it is preferable to laminate the cut sheet-shaped dry rubber 16 at, for example, 40° C. or higher. By laminating the cut sheet-shaped dry rubber 16 at 40° C. or higher, good air release is achieved by further cooling and compression due to its own weight. EXAMPLES

[0274] The present invention will be described in more detail below with reference to examples and comparative examples. In each example, "parts", "%" and "ratio" are by weight unless otherwise specified. Various physical properties were evaluated according to the following methods.

[0275] [Monomer composition] Regarding the monomer composition of the acrylic rubber, the monomer composition of each monomer unit in the acrylic rubber was confirmed by H-NMR, and the remaining activity of reactive groups in the acrylic rubber and the content of each reactive group were confirmed by the following test methods.

[0276] The content ratio of each monomer unit in the acrylic rubber was calculated from the amount of each monomer used in the polymerization reaction and the polymerization conversion rate. Specifically, the polymerization reaction was an emulsion polymerization reaction, and the polymerization conversion rate was approximately 100%, with no unreacted monomers being confirmed, so the content ratio of each monomer unit was set to be the same as the amount of each monomer used.

[0277] [Reactive group content] The reactive group content of the acrylic rubber was measured by the following method. (1) The amount of carboxyl groups was calculated by dissolving the acrylic rubber in acetone and performing potentiometric titration with a potassium hydroxide solution. (2) The amount of epoxy groups was calculated by dissolving the acrylic rubber in methyl ethyl ketone, adding a specified amount of hydrochloric acid to react with the epoxy groups, and titrating the amount of residual hydrochloric acid with potassium hydroxide. (3) The amount of chlorine was calculated by completely burning acrylic rubber in a combustion flask, absorbing the chlorine generated in water, and titrating it with silver nitrate.

[0278] [Anti-aging agent content] The antioxidant content (%) in the acrylic rubber was calculated based on the calibration curve of the same antioxidant by dissolving the acrylic rubber sheet or acrylic rubber veil in tetrahydrofuran and measuring with gel permeation chromatography (GPC).

[0279] [Ash content] The ash content (%) in the acrylic rubber was measured in accordance with JIS K6228 Method A.

[0280] [Ash content] The amount (ppm) of each component in the acrylic rubber ash was measured by pressing the ash sampled during the above ash content measurement onto a titration filter paper of Φ20 mm and subjecting it to XRF measurement using ZSX Primus (manufactured by Rigaku Co., Ltd.).

[0281] [Glass transition temperature (Tg)] The glass transition temperature (Tg) of the acrylic rubber was measured using a differential scanning calorimeter (DSC, product name "X-DSC7000", manufactured by Hitachi High-Tech Science Corporation).

[0282] [pH] The pH of the acrylic rubber was measured with a pH electrode after dissolving 6 g (±0.05 g) of acrylic rubber in 100 g of tetrahydrofuran, adding 2.0 ml of distilled water, and confirming complete dissolution.

[0283] [Water content] The water content (%) of the acrylic rubber was measured in accordance with JIS K6238-1: Oven A (volatile matter measurement) method.

[0284] [Molecular weight and molecular weight distribution] The weight average molecular weight (Mw) and molecular weight distribution (Mz / Mw) of acrylic rubber are absolute molecular weight and absolute molecular weight distribution measured by GPC-MALS method using a solution of dimethylformamide with 0.05 mol / L lithium chloride and 0.01% 37% concentrated hydrochloric acid as a solvent. Specifically, a multi-angle laser light scattering photometer (MALS) and a differential refractometer (RI) were incorporated into a GPC (Gel Permeation Chromatography) device, and the light scattering intensity and refractive index difference of the molecular chain solution size-fractionated by the GPC device were measured over the elution time, and the molecular weight of the solute and its content were calculated sequentially. The measurement conditions and method using the GPC device are as follows. Column: 2 TSKgel α-M (φ7.8mm×30cm, Tosoh Corporation) Column temperature: 40℃ Flow rate: 0.8ml / mm Sample preparation: 5 ml of solvent was added to 10 mg of sample, and the mixture was gently stirred at room temperature (dissolution was visually confirmed).Then, the mixture was filtered using a 0.5 μm filter.

[0285] [Complex viscosity] The complex viscosity η of acrylic rubber was measured at 473% strain and 1 Hz using a dynamic viscoelasticity measuring device "Rubber Process Analyzer RPA-2000" (manufactured by Alpha Technology Co., Ltd.) to measure temperature dispersion (40 to 120°C) and obtain the complex viscosity η at each temperature. Here, the dynamic viscoelasticity at 60°C of the above-mentioned dynamic viscoelasticity was taken as the complex viscosity η(60°C), and the dynamic viscoelasticity at 100°C was taken as the complex viscosity η(100°C), and the values ​​of η(100°C) / η(60°C) and η(60°C) / η(100°C) were calculated.

[0286] [Gel amount] The gel content (%) of the acrylic rubber is the amount of the insoluble portion in methyl ethyl ketone, and was determined by the following method.

[0287] Approximately 0.2 g of acrylic rubber was weighed out (Xg), immersed in 100 ml of methyl ethyl ketone, and left to stand at room temperature for 24 hours. After that, the insoluble matter in methyl ethyl ketone was filtered off using an 80 mesh wire screen. The filtrate, i.e., the filtrate in which only the rubber components soluble in methyl ethyl ketone were dissolved, was evaporated, dried, and solidified. The dried solid content (Yg) was weighed and calculated using the following formula.

[0288] Gel volume (%) = 100 × (XY) / X

[0289] [specific gravity] The specific gravity of the acrylic rubber was measured in accordance with JIS 6268 Crosslinked Rubber - Density Measurement Method A.

[0290] [Storage stability evaluation] The storage stability of the rubber samples was evaluated by placing the rubber mixture of the rubber sample in a constant temperature and humidity chamber at 45°C x 80% RH for 7 days, and then using the rubber sample before and after the test as a rubber mixture, a crosslinking test was performed at 180°C for 10 minutes using a rubber vulcanization tester (Moving Die Rheometer MDR; manufactured by Alpha Technology Co., Ltd.) to calculate the rate of change in crosslink density, which is the difference between the maximum torque (MH) and the minimum torque (ML) (MH-ML), and evaluating it with an index of 100 for Comparative Example 1 (the smaller the index, the better the storage stability).

[0291] [Water resistance evaluation] The water resistance of the rubber sample was evaluated by performing an immersion test in accordance with JIS K6258, in which a crosslinked rubber sample was immersed in distilled water at a temperature of 85°C for 100 hours, and calculating the volume change rate before and after immersion according to the following formula, with Comparative Example 1 being 100 (the smaller the index, the better the water resistance). Volume change rate before and after immersion (%) = ((volume of test piece after immersion - volume of test piece before immersion) / volume of test piece before immersion) x 100

[0292] [Normal state physical property evaluation] The normal state physical properties of the rubber samples were evaluated according to the following criteria by measuring the breaking strength, 100% tensile stress and breaking elongation of the cross-linked rubber samples in accordance with JIS K6251. (1) The breaking strength was evaluated as ⊚ when it was 10 MPa or more, and x when it was less than 10 MPa. (2) The 100% tensile stress was evaluated as ⊚ when it was 5 MPa or more, and x when it was less than 5 MPa. (3) The breaking elongation was evaluated as ⊚ when it was 150% or more, and x when it was less than 150%.

[0293] [Example 1] A mixing vessel equipped with a homomixer was charged with 46 parts of pure water, 74.5 parts of ethyl acrylate, 17 parts of n-butyl acrylate, 7 parts of methoxyethyl acrylate, 1.5 parts of mono-n-butyl fumarate, and 1.8 parts of octyloxydioxyethylene phosphate sodium salt as an emulsifier, and the mixture was stirred to obtain a monomer emulsion.

[0294] Next, 170 parts of pure water and 3 parts of the monomer emulsion obtained above were put into a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to 12°C under a nitrogen stream. Next, the remainder of the monomer emulsion, 0.00033 parts of ferrous sulfate, 0.264 parts of sodium ascorbate, and 0.22 parts of potassium persulfate were continuously dropped into the polymerization reaction tank over 3 hours. Thereafter, the reaction was continued while maintaining the temperature inside the polymerization reaction at 23°C, and it was confirmed that the polymerization conversion rate reached approximately 100%, and the polymerization reaction was stopped by adding hydroquinone as a polymerization terminator, and 1 part of 3-(4-hydroxy-3,5-di-tert-butylphenyl)octyl propionate (Irganox 1135; manufactured by BASF) was added to obtain an emulsion polymerization liquid.

[0295] In a coagulation tank equipped with a thermometer and agitator, the emulsion polymerization liquid containing the antioxidant was heated to 80°C and continuously added to a 2% magnesium sulfate aqueous solution (coagulation liquid) that had been heated to 80°C and vigorously stirred (600 rpm: peripheral speed 3.1 m / s), to coagulate the polymer, which was then filtered off to obtain hydrous crumbs.

[0296] Next, 194 parts of hot water (70°C) was added to the coagulation tank and stirred for 15 minutes, after which the water was drained, and 194 parts of hot water (70°C) was added again and stirred for 15 minutes to wash the water-containing crumbs. The washed water-containing crumbs (water-containing crumb temperature 65°C) were dehydrated (drained) to a water content of 20% by weight using a screw-type extruder, and then dried to a water content of 0.4% by weight to obtain an acrylic rubber (A). The temperature of the drying barrel of the screw-type extruder was set to a gradient of 120 to 180°C.

[0297] The reactive group content, ash content, ash component content, glass transition temperature (Tg), pH, antioxidant content, water content, molecular weight, molecular weight distribution and complex viscosity of the obtained acrylic rubber (A) were measured, and the results are shown in Table 2.

[0298] Next, 100 parts of the acrylic rubber (A) and compounding agent A of "Compound 1" shown in Table 1 were added using a Banbury mixer, and mixed at 50°C for 5 minutes.

[0299] The resulting mixture was then transferred to a roll at 50°C, and compounding ingredient B of "Compound 1" in Table 1 was added and mixed to obtain a rubber mixture (composition). A crosslinking test was performed on the rubber mixture using acrylic rubber (A) before and after the storage stability test, and the change in crosslink density (MH-ML) was measured. The results are shown in Table 2.

[0300] [Table 1]

[0301] The obtained rubber mixture was placed in a mold 15 cm long, 15 cm wide, and 0.2 cm deep, and pressed at 180°C for 10 minutes while applying a pressure of 10 MPa to cause primary crosslinking, and then the obtained primary crosslinked product was further heated in a gear oven at 180°C for 2 hours to cause secondary crosslinking, thereby obtaining a sheet-like crosslinked rubber product. Then, a test piece measuring 3 cm x 2 cm x 0.2 cm was cut from the obtained sheet-like crosslinked rubber product, and the water resistance and normal physical properties were evaluated, and the results are shown in Table 2.

[0302] [Example 2] The same procedure as in Example 1 was carried out except that the monomer components were changed to 4.5 parts of ethyl acrylate, 64.5 parts of n-butyl acrylate, 29.5 parts of methoxyethyl acrylate, and 1.5 parts of mono n-butyl fumarate, and the emulsifier was changed to nonylphenyloxyhexaoxyethylene phosphate sodium salt, to obtain an acrylic rubber (B), and the properties were evaluated. The results are shown in Table 2.

[0303] [Example 3] The same procedure as in Example 1 was carried out except that the monomer components were changed to 48.25 parts of ethyl acrylate, 50 parts of n-butyl acrylate, and 1.75 parts of mono n-butyl fumarate, and the emulsifier was changed to tridecyloxyhexaoxyethylene phosphate sodium salt, to obtain an acrylic rubber (C), and the properties were evaluated (the compounding ingredients were changed to "Compound 2"). The results are shown in Table 2.

[0304] [Example 4] The same procedure as in Example 3 was carried out except that the water content of the dewatered (discharged) water in the screw-type extruder was changed to 30%, to obtain an acrylic rubber (D), and the properties thereof were evaluated. The results are shown in Table 2.

[0305] [Example 5] The same procedure as in Example 4 was carried out except that the monomer components were changed to 28 parts of ethyl acrylate, 38 parts of n-butyl acrylate, 27 parts of methoxyethyl acrylate, 5 parts of acrylonitrile, and 2 parts of allyl glycidyl ether, and an acrylic rubber (E) was obtained and each property was evaluated (the compounding agent was changed to "Compound 3"). The results are shown in Table 2.

[0306] [Example 6] The same procedure as in Example 4 was carried out except that the monomer components were changed to 42.5 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile, and 1.3 parts of vinyl chloroacetate, and an acrylic rubber (F) was obtained and each property was evaluated (the compounding agent was changed to "Compound 4"). The results are shown in Table 2.

[0307] [Comparative Example 1] A mixing vessel equipped with a homomixer was charged with 46 parts of pure water, 42.2 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile, 1.3 parts of vinyl chloroacetate, 0.709 parts of sodium lauryl sulfate as an emulsifier, and 1.82 parts of polyoxyethylene dodecyl ether (molecular weight 1500), and the mixture was stirred to obtain a monomer emulsion.

[0308] Next, 170 parts of pure water and 3 parts of the monomer emulsion obtained above were put into a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to 12°C under a nitrogen stream. Next, the remainder of the monomer emulsion, 0.00033 parts of ferrous sulfate, 0.264 parts of sodium ascorbate, and 0.22 parts of potassium persulfate were continuously dropped into the polymerization reaction tank over 3 hours. Thereafter, the reaction was continued while maintaining the temperature inside the polymerization reaction at 23°C, and it was confirmed that the polymerization conversion rate reached approximately 100%, and hydroquinone was added as a polymerization terminator to terminate the polymerization reaction, and an emulsion polymerization liquid was obtained in which 1 part of 3-(3,5-tert-butyl-4-hydroxyphenyl)stearyl propionate (Irganox 1076; manufactured by BASF) was added as a 50% by weight aqueous dispersion (0.1% by weight sodium lauryl sulfate dispersion).

[0309] Next, the emulsion polymerization liquid to which the antioxidant was added was heated to 80°C, and then a 0.7% aqueous sodium sulfate solution (coagulation liquid) was continuously added to the emulsion polymerization liquid (rotation speed 100 rpm, peripheral speed 0.5 m / s) to coagulate the polymer, which was then filtered to obtain hydrous crumbs. 194 parts of industrial water was added to 100 parts of the obtained hydrous crumbs, and the mixture was stirred at 25°C for 5 minutes, after which the hydrous crumbs were washed 4 times by draining water from the coagulation tank, and then 194 parts of a sulfuric acid solution at pH 3 was added and stirred at 25°C for 5 minutes, after which the water was drained from the coagulation tank and acid washed once, and then 194 parts of pure water was added and pure water washed once, and then the mixture was dried in a hot air dryer at 160°C to obtain an acrylic rubber (G) with a water content of 0.4% by weight. The properties of the obtained acrylic rubber (G) were evaluated and shown in Table 2.

[0310] [Comparative Example 2] Acrylic rubber (H) was obtained in the same manner as in Comparative Example 1, except that the antioxidant added to the emulsion polymerization liquid was changed to 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Nocrac CD; manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) The properties of the obtained acrylic rubber (H) were evaluated and are shown in Table 2.

[0311] [Table 2]

[0312] From Table 2, it can be seen that the acrylic rubbers (A) to (F) of the present invention, which are composed of 50 to 99.9% by weight of bonding units derived from at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, 0.1 to 20% by weight of bonding units derived from reactive group-containing monomers, and 0 to 30% by weight of bonding units derived from other monomers, contain a phenol-based antiaging agent represented by general formula (1), and have a weight average molecular weight (Mw) in the range of 100,000 to 5,000,000, are excellent in storage stability, normal state physical properties including strength characteristics, and water resistance (comparison between Examples 1 to 6 and Comparative Examples 1 and 2).

[0313] Regarding normal physical properties, the acrylic rubbers (A) to (G) produced under the conditions of the present examples and comparative examples have weight average molecular weights (Mw) of absolute molecular weights measured by GPC-MALS exceeding 100,000, and the ratio (Mz / Mw) of the z-average molecular weight (Mz) and weight average molecular weight (Mw) of absolute molecular weight distribution with emphasis on the high molecular weight region measured by GPC-MALS exceeds 1.3, which is quite large, so that all of the normal physical properties including breaking strength are excellent (Examples 1 to 6 and Comparative Examples 1 and 2). However, it can be seen from Table 2 that the acrylic rubbers (G) to (H) of Comparative Examples 1 and 2 have excellent strength characteristics but are extremely poor in storage stability and water resistance.

[0314] As for storage stability, since the antioxidant content of the acrylic rubbers (A) to (F) is the same as that of the acrylic rubber (G), it is found that the phenolic antioxidant represented by the general formula (1) has a far superior acrylic rubber storage stability effect than the phenolic antioxidant used in the acrylic rubber (G). This is because there is not much difference in the antioxidant effect against peroxide radicals between the two phenolic antioxidants, and it is believed that the difference in uniform fine dispersion in the acrylic rubbers (A) to (F) is the cause of the difference in storage stability (comparison between Examples 1 to 6 and Comparative Example 1). In addition, after the storage stability test, no change in color was observed in the acrylic rubbers (A) to (F), but the acrylic rubbers (G) to (H) were yellowed.

[0315] As for water resistance, it can be seen from Table 2 that the acrylic rubbers (A) to (F) of the present invention are overwhelmingly superior to the acrylic rubbers (G) to (H) (comparison of Examples 1 to 6 and Comparative Examples 1 and 2). This is because the amount of ash in the acrylic rubber is reduced by squeezing water from the water-containing crumbs to a specific water content in the dehydration process, and when a phosphate ester salt is used as an emulsifier and a magnesium salt is used as a coagulant, the ash remaining in the acrylic rubber has a high content of magnesium and phosphorus and the two are in a specific ratio, so that water resistance is hardly affected, and the water resistance of the acrylic rubbers (A) to (F) is significantly improved, and normal state physical properties including strength properties and storage stability are also highly balanced (Examples 1 to 6).

[0316] From Table 2, it can be seen that the acrylic rubbers (A) to (F) which contain the phenolic antioxidant represented by the general formula (1) of the present invention and have specific values ​​for the reactive group amount, glass transition temperature (Tg), pH, water content, weight average molecular weight (Mw), ratio (Mz / Mw) of z-average molecular weight (Mz) to weight average molecular weight (Mw), complex viscosity η (100°C) at 100°C, complex viscosity η (60°C) at 60°C, and ratio of complex viscosities at 100°C and 60°C (η100°C / η60°C) are excellent in storage stability, normal physical properties including strength characteristics, and water resistance (Examples 1 to 6).

[0317] [Example 7] Acrylic rubber (I) was obtained in the same manner as in Comparative Example 1, except that the antioxidant added to the emulsion polymerization liquid was changed to 3-(4-hydroxy-3,5-di-tert-butylphenyl)octyl propionate (Irganox 1135; manufactured by BASF). The storage stability, water resistance, and normal physical properties of the obtained acrylic rubber (I) were evaluated, and the results were storage stability of "45", water resistance of "100", breaking strength of "◎", 100% tensile stress of "◎", and breaking elongation of "◎". From these results, it can be seen that the effect of the phenol-based antioxidant represented by the above general formula (1) used in Example 7 on the storage stability of acrylic rubber is higher than that of the antioxidants used in Comparative Examples 1 and 2, and that the storage stability was further improved by specifying the ash content of the specific ash component (comparison between Example 7, Comparative Examples 1-2, and Examples 1-6).

[0318] [Examples 8 to 10] The hydrous crumbs (hydrous crumb temperature 65°C) which had been emulsion polymerized, coagulated and washed in the same manner as in Examples 1 to 3 were fed to a screw-type extruder, dehydrated and dried to extrude a sheet-like dry rubber having a width of 300 mm and a thickness of 10 mm. The sheet-like dry rubber was then cooled at a cooling rate of 200°C / hr using a conveying cooling device directly connected to the screw-type extruder.

[0319] The screw extruder used in Examples 8 to 10 is composed of one supply barrel, three dehydration barrels (first to third dehydration barrels), and five drying barrels (first to fifth drying barrels). The first and second dehydration barrels discharge water, and the third dehydration barrel discharges steam. The operating conditions of the screw extruder were as follows.

[0320] Water content: Moisture content of wet crumbs after draining in the second dewatering barrel: 20% Moisture content of wet crumb after steaming in the third dewatering barrel: 10% Moisture content of wet crumb after drying in the fifth drying barrel: 0.4% Rubber Temperature: Temperature of wet crumbs fed into the first feed barrel: 65℃ -Temperature of rubber discharged from screw extruder: 140℃ Temperature settings for each barrel: First dehydration barrel: 90℃ Second dehydration barrel: 100℃ ·Third dehydration barrel: 120℃ ·First drying barrel: 120℃ Second drying barrel: 130℃ ·Third drying barrel: 140℃ ·Fourth drying barrel: 160℃ · Fifth drying barrel: 180℃ Operating conditions: Diameter of the screw in the barrel unit (D): 132mm Total length of the screw in the barrel unit (L): 4620mm Length / Depth:35 - Rotation speed of the screw in the barrel unit: 135 rpm -Rubber extrusion rate from die: 700kg / hr Die resin pressure: 2MPa

[0321] The extruded dry rubber sheets (acrylic rubber sheets (J) to (L)) were cooled to 50°C and then cut with a cutter. The cut pieces were then laminated to 20 parts (20 kg) before the temperature dropped below 40°C, to obtain acrylic rubber veils (J) to (L).

[0322] When the specific gravity and the gel amount of the methyl ethyl ketone insoluble matter of the obtained sheet-like acrylic rubbers (J) to (L) and veil-like acrylic rubbers (J) to (L) were measured, the measured values ​​of each sheet-like acrylic rubber and the veil-like acrylic rubber were almost the same, with the sheet-like and veil-like acrylic rubbers (J) having a specific gravity of 1.107 and a gel amount of 1.7% by weight, the sheet-like and veil-like acrylic rubbers (K) having a specific gravity of 1.098 and a gel amount of 2.3% by weight, and the sheet-like and veil-like acrylic rubbers (L) having a specific gravity of 1.101 and a gel amount of 1.9% by weight, and all of the sheet-like and veil-like acrylic rubbers (J) to (L) having little air entrapment, having high specific gravity, and also having an extremely small amount of gel amount of the methyl ethyl ketone insoluble matter.

[0323] The reactive group content, ash content, ash component content, glass transition temperature (Tg), pH, antioxidant content, water content, molecular weight, molecular weight distribution and complex viscosity of the obtained sheet-like and veil-like acrylic rubbers (J) to (L) were measured, and the values ​​were almost the same as those of the corresponding acrylic rubbers (A) to (C).

[0324] The storage stability, water resistance and normal state physical properties of the obtained sheet-like and veil-like acrylic rubbers (J) to (L) were evaluated in the same manner as in Examples 1 to 3. The normal state physical properties and water resistance were excellent, just like the corresponding acrylic rubbers (A) to (C), and the storage stability was all "<30", which was superior to the corresponding acrylic rubbers (A) to (C). [Explanation of symbols]

[0325] 1 Acrylic rubber manufacturing system 3 Coagulation device 4. Cleaning equipment 5 Screw Extruder 6 Cooling device 7 Baling Equipment

Claims

1. comprising 50 to 99.9% by weight of bonding units derived from at least one (meth)acrylic ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, 0.1 to 20% by weight of bonding units derived from a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a halogen group, and 0 to 30% by weight of bonding units derived from other monomers; General formula (1) 【Chemistry 5】 (R1 represents an isopropyl group or a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms), the total amount of magnesium and phosphorus in the ash is 30% by weight or more, and the weight average molecular weight (Mw) is in the range of 100,000 to 5,000,000.

2. The acrylic rubber according to claim 1, wherein the phenol-based antioxidant represented by the general formula (1) is octyl 3-(4-hydroxy-3,5-di-tert-butylphenyl)propionate or octyl 3-(4-hydroxy-3,5-diisopropylphenyl)propionate.

3. 3. The acrylic rubber according to claim 1 or 2, wherein the content of the phenol-based antioxidant represented by the general formula (1) is 0.001 to 15% by weight.

4. The acrylic rubber according to any one of claims 1 to 3, wherein the ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) is 1.3 or more.

5. The acrylic rubber according to any one of claims 1 to 4, having a complex viscosity at 60 ° C. ([η]100 ° C.) of 15,000 Pa s or less.

6. The acrylic rubber according to any one of claims 1 to 5, wherein the ratio ([η]100°C / [η]60°C) of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is 0.5 or more.

7. The acrylic rubber according to any one of claims 1 to 6, which has a pH of 6 or less.

8. The acrylic rubber according to any one of claims 1 to 7, having a water content of less than 1% by weight.

9. The acrylic rubber according to any one of claims 1 to 8, having an ash content of 0.5% by weight or less.

10. The acrylic rubber according to any one of claims 1 to 9, wherein the ratio of magnesium to phosphorus in the ash ([Mg] / [P]) is in the range of 0.4 to 2.

5.

11. The acrylic rubber according to any one of claims 1 to 10, which is in the form of a sheet or a veil.

12. The acrylic rubber according to any one of claims 1 to 11, having a specific gravity of 0.8 or more.

13. The acrylic rubber according to any one of claims 1 to 12, wherein the gel content is 50% by weight or less.

14. A monomer component consisting of at least one (meth)acrylic acid ester selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters, a monomer having at least one functional group selected from the group consisting of a carboxyl group, an epoxy group, and a halogen group, and, if necessary, other copolymerizable monomers, is emulsified with water and an emulsifier, and emulsion-polymerized in the presence of a polymerization catalyst to obtain an emulsion polymerization liquid. General formula (1) 【Chemistry 6】 (R1 represents an isopropyl group or a t-butyl group, and R2 represents an alkyl group having 1 to 12 carbon atoms), and then the mixture is coagulated and dried.

15. The method for producing an acrylic rubber according to claim 14, wherein the coagulation of the emulsion polymerization liquid to which the phenol-based antiaging agent represented by the general formula (1) has been added is carried out by adding the emulsion polymerization liquid to a coagulation liquid that is being stirred.

16. The method for producing an acrylic rubber according to claim 14 or 15, wherein water-containing crumbs produced during solidification are washed with warm water.

17. The method for producing acrylic rubber according to claim 16, wherein water is squeezed out of the washed wet crumbs using a dehydrator.

18. A rubber composition comprising a rubber component containing the acrylic rubber according to any one of claims 1 to 13, a filler, and a crosslinking agent.

19. A cross-linked rubber product obtained by cross-linking the rubber composition according to claim 18.

Citation Information

Patent Citations

  • Copolymer, method for producing the same and composition

    JP2005060440A

  • Adhesive composition

    WO2009154205A1

  • Method for producing acrylic rubber

    WO2018139466A1