Luminescent compound or its salt, and polarized light emitting device, polarized light emitting plate, and display device each including the same

A novel luminescent compound-based polarized light-emitting element and plate address the issues of low transmittance and durability in conventional polarizing plates by providing high transmittance and durability, suitable for liquid crystal displays and other applications.

JP7556855B2Active Publication Date: 2024-09-26NIPPON KAYAKU CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021533043
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-10
Publication Date
2024-09-26
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Conventional polarizing plates used in displays suffer from low transmittance and high absorption in the visible light region, leading to reduced display brightness and durability issues, especially in harsh environments, and existing polarized light-emitting devices are expensive and difficult to manufacture.

Method used

A novel luminescent compound or its salt with a specific structure, capable of emitting polarized light in the visible light range when irradiated with ultraviolet to near ultraviolet light, is used to create a polarized light-emitting element and plate, which exhibits high transmittance and durability, avoiding the use of rare metals.

Benefits of technology

The compound achieves high transmittance and durability, enabling brighter and more durable displays with polarized light emission, suitable for liquid crystal displays and other applications requiring high transparency and stability under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556855000012
    Figure 0007556855000012
  • Figure 0007556855000021
    Figure 0007556855000021
  • Figure 0007556855000026
    Figure 0007556855000026
Patent Text Reader

Abstract

The present invention is a light-emitting compound represented by formula (1) or a salt thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel light-emitting compound or a salt thereof, and a polarized light-emitting device, a polarized light-emitting plate, and a display device each containing the same. [Background technology]

[0002] A polarizing plate having a light transmitting and / or blocking function is a basic component of a display device such as a liquid crystal display (LCD) together with a liquid crystal having a light switching function. The application field of this LCD is expanding from small devices such as calculators and clocks in the early days to notebook computers, word processors, liquid crystal projectors, liquid crystal televisions, car navigation systems, and indoor and outdoor measuring instruments. It can also be applied to lenses having a polarizing function, for example, sunglasses with improved visibility and polarized glasses compatible with 3D televisions in recent years. As described above, the applications of polarizing plates are expanding widely, and the environments in which they are used are also wide, such as low temperature to high temperature, low humidity to high humidity, and low light to high light, so that polarizing plates having high polarization performance and high durability are required.

[0003] In general, the polarizing film constituting the polarizing plate is produced by stretching and orienting a film of polyvinyl alcohol or its derivatives containing iodine or dichroic dye, or by dehydrochlorinating a polyvinyl chloride film or dehydrating a polyvinyl alcohol film to generate a polyene and orienting it. A polarizing plate composed of such a conventional polarizing film contains a dichroic dye that absorbs in the visible range, so the transmittance is reduced. For example, the transmittance of a typical polarizing plate available on the market is 35 to 45%.

[0004] To address the problem of conventional polarizing plates that transmittance in the visible range decreases, a technology for polarizing plates for ultraviolet rays that maintains a certain level of transmittance in the visible range while providing a polarizing function is described in Patent Document 1. However, this technology also uses a yellow dye that absorbs in the visible range, so the transmittance is insufficient and a strong yellow coloration is observed.

[0005] When a polarizing plate with low transmittance in the visible light region is used in a display or the like, the transmittance of the entire display decreases, so methods for obtaining polarized light without using a conventional polarizing plate are being researched. As such methods, elements that emit polarized light are described in Patent Documents 2 to 4.

[0006] However, the polarized light emitting elements described in Patent Documents 2 to 4 contain rare metals such as special metals, such as lanthanides and europium, and are therefore expensive, and are very difficult to manufacture and unsuitable for mass production. Furthermore, these polarized light emitting elements are difficult to use in displays because they emit weak polarized light, and linearly polarized light cannot be obtained. Therefore, it is desired to develop a new polarized light emitting plate and a material therefor that exhibits polarized light emission, has high transparency in the visible light range, and can be applied to liquid crystal displays and the like that require durability in harsh environments. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] WO2005 / 015275 [Patent Document 2] JP 2008-224854 A [Patent Document 3] JP 2013-121921 A [Patent Document 4] WO2011 / 111607 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present application is to provide a novel light-emitting compound, and a polarized light-emitting device, a polarized light-emitting plate, and a display device each containing the compound. [Means for solving the problem]

[0009] As a result of intensive research conducted by the present inventors to achieve this object, it has been found that a polarized light-emitting element and a polarized light-emitting plate containing a compound having a specific structure or a salt thereof have a high dichroic ratio in the ultraviolet region, a high transmittance in the visible light region, and excellent durability in harsh environments. It has also been found that such a compound having a specific structure or a salt thereof exhibits the action of emitting polarized light in the visible light region when irradiated with light in the ultraviolet region to the near ultraviolet-visible region, for example, light of 300 to 430 nm, and thus the present invention has been completed.

[0010] That is, the present invention relates to, but is not limited to, the following: [Invention 1] A luminescent compound represented by the following formula (1) or a salt thereof: [ka] (in formula (1), (i) X and Y each independently contain at least a group selected from the group consisting of a group represented by formula (2) above, a heterocyclic group containing a nitrogen atom or a sulfur atom, and a nitro group, except when both X and Y are nitro groups; or (ii) at least one of X and Y (independently in the case of both) is a nitro group, an amino group which may have a substituent, a C1-4 alkyl group which may have a substituent, a C1-4 alkoxy group which may have a substituent, an aromatic group which may have a substituent, an oxygen atom which may have a substituent, a heterocyclic group containing a nitrogen atom or a sulfur atom, or a group represented by formula (2), and when X or Y is not a group selected above, then said X or Y is selected from any substituent, Each M independently represents a hydrogen atom, a metal ion, or an ammonium ion; each m independently represents an integer of 0 to 2; and s is 0 or 1. In formula (2), * indicates the bonding position of X and / or Y in formula (1), Z is selected from the group consisting of an optionally substituted phenyl group, an optionally substituted naphthyl group, an optionally substituted stilbene group, an optionally substituted benzoyl group, and an optionally substituted heterocyclic group, and t represents an integer of 0 or 1. [Invention 2] The luminescent compound according to Invention 1, wherein at least one of X and Y in the above formula (1), and Z in the above formula (2) when at least one of X and Y is represented by the above formula (2), is selected from the group consisting of substituents represented by the following formulas (3) to (7). [ka] (In the above formula (3) and formula (4), each A is independently selected from the group consisting of a hydrogen atom, a halogen group, a nitro group, a hydroxy group, a C1-4 alkyl group, a C1-4 alkoxy group, a C1-4 alkyl group having a sulfo group, a C1-4 alkyl group having a hydroxy group, a C1-4 alkyl group having a carboxy group, a C1-4 alkoxy group having a sulfo group, a C1-4 alkoxy group having a hydroxy group, and a C1-4 alkoxy group having a carboxy group; q 1 represents an integer of 0 to 4, M in the above formulas (3) to (7) is as defined in the above formula (1), and n 1 and n 2 each independently represents an integer of 0 to 3, and * in the above formulas (3) to (7) respectively indicates the bonding position of X or Y in the above formula (1), or the bonding position of Z in the above formula (2). [Invention 3] The luminescent compound or salt thereof according to invention 1 or 2, wherein X and Y in the above formula (1) are each independently selected from the group consisting of substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of substituents represented by formulas (3) to (7). [Invention 4] The luminescent compound or salt thereof according to Invention 1 or 2, wherein, in the above formula (1), X and Y are both selected from the group consisting of the substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of the substituents represented by formulas (3) to (7). [Invention 5] 5. The luminescent compound or a salt thereof according to any one of Inventions 1 to 4, wherein each m in the above formula (1) is 0. [Invention 6] 6. The luminescent compound or a salt thereof according to any one of Inventions 1 to 5, wherein s is 0. [Invention 7] 6. The luminescent compound or a salt thereof according to any one of Inventions 1 to 5, wherein s is 1. [Invention 8] The luminescent compound or a salt thereof according to invention 7, wherein the above formula (1) is represented by the following formula (1'): [ka] (In the above formula (1'), X and Y are as defined in the above formula (1)). [Invention 9] 9. A polarized light emitting device having a polarized light emitting function, comprising the light emitting compound or a salt thereof according to any one of Inventions 1 to 8. [Invention 10] 10. The polarized light-emitting device according to claim 9, further comprising one or more organic dyes or fluorescent dyes other than the luminescent compound or the salt thereof. [Invention 11] 11. The polarized light-emitting element according to invention 9 or 10, further comprising a substrate. [Invention 12] 12. The polarized light-emitting element according to claim 11, wherein the substrate is a film containing a polyvinyl alcohol resin or a derivative thereof. [Invention 13] 13. A polarized light-emitting plate comprising a polarized light-emitting element according to any one of Inventions 9 to 12 and a transparent protective film on at least one surface of the element. [Invention 14] A display device comprising the polarized light-emitting element according to any one of Inventions 9 to 12 or the polarized light-emitting plate according to Invention 13. Effect of the Invention

[0011] The luminescent compound or its salt having a specific structure according to the present invention absorbs light in the ultraviolet to visible region, for example, light in the ultraviolet to near-ultraviolet visible region, specifically light of 300 to 430 nm, and exhibits polarized luminescence in the visible region by utilizing the energy of the absorbed light. In addition, a polarizing element and a polarizing plate prepared using the luminescent compound or its salt are novel polarized luminescent elements and polarized luminescent plates exhibiting polarized luminescence. In one aspect, the luminescent compound or its salt according to the present invention and the polarized luminescent element and polarized luminescent plate containing the same exhibit a high degree of polarization at the absorption wavelength. Therefore, by using such a compound represented by formula (1) or its salt, a novel polarized luminescent element and polarized luminescent plate having a high degree of polarization at the absorption wavelength and exhibiting polarized luminescence can be provided without using a highly rare lanthanoid metal or the like. In one aspect, the polarized luminescent element and polarized luminescent plate according to the present invention exhibit high transmittance in the visible region. In one aspect, the polarized luminescent element and polarized luminescent plate according to the present invention exhibit excellent durability against heat, humidity, and the like. Therefore, the polarized light emitting element and the polarized light emitting plate can be applied to display devices such as liquid crystal displays which require high transmittance in the visible light region and high durability in harsh environments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the present specification and claims, "substituents" includes hydrogen atoms for convenience. "May have a substituent" means that it also includes the case where it has no substituent. For example, "a phenyl group which may have a substituent" includes a simple unsubstituted phenyl group and a phenyl group which has a substituent.

[0013] [Luminescent compounds] The luminescent compound or a salt thereof according to the present invention is represented by the above formula (1). In this specification, the "luminescent compound or a salt thereof" may be abbreviated to simply "luminescent compound".

[0014] In formula (1), (i) X and Y each independently contain at least a group selected from the group consisting of the group represented by formula (2) above, a heterocyclic group containing a nitrogen atom or a sulfur atom, and a nitro group, except when both X and Y are nitro groups; or (ii) at least one of X and Y (each independently in the case of both) is a nitro group, an amino group which may have a substituent, an alkyl group having 1 to 4 carbon atoms which may have a substituent, an alkoxy group having 1 to 4 carbon atoms which may have a substituent, an aromatic group which may have a substituent, a heterocyclic group containing an oxygen atom, a nitrogen atom or a sulfur atom which may have a substituent, or a group represented by formula (2), and when X or Y is not a group selected above, said X or Y is selected from any substituent, Each M independently represents a hydrogen atom, a metal ion, or an ammonium ion; each m independently represents an integer of 0 to 2; and s is 0 or 1.

[0015] In formula (2), * indicates the bonding position of X and / or Y in formula (1), Z is selected from the group consisting of an optionally substituted phenyl group, an optionally substituted naphthyl group, an optionally substituted stilbene group, an optionally substituted benzoyl group, and an optionally substituted heterocyclic group, and t represents an integer of 0 or 1.

[0016] Examples of the "amino group which may have a substituent" in the definition of X and Y include amino groups; mono-substituted amino groups such as methylamino group, ethylamino group, n-butylamino group, phenylamino group, naphthylamino group, and acetylamino group (i.e., acetamide group); di-substituted amino groups such as dimethylamino group, diethylamino group, di-n-butylamino group, diphenylamino group, ethylmethylamino group, and ethylphenylamino group; etc. In addition, the above formula (2) described later is also included in the amino group which may have a substituent.

[0017] Examples of the "C1-4 alkyl group" in the "optionally substituted C1-4 alkyl group" in the definitions of X and Y include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and a cyclobutyl group.

[0018] Examples of the "C1 to 4 alkoxy group" in the "optionally substituted C1 to 4 alkoxy group" in the definitions of X and Y include a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, and a cyclobutoxy group.

[0019] Examples of the "aromatic group" in the "optionally substituted aromatic group" in the definitions of X and Y include a phenyl group, a naphthyl group, and anthracenyl group.

[0020] In the definition of X and Y, the term "heterocyclic group containing a nitrogen atom or a sulfur atom" refers to a heterocycle having at least one of a nitrogen atom and a sulfur atom as a ring component, and the term "heterocyclic group containing an oxygen atom, a nitrogen atom or a sulfur atom" in the above "heterocyclic group containing an oxygen atom, a nitrogen atom or a sulfur atom, which may have a substituent" refers to a heterocycle having at least one of an oxygen atom, a nitrogen atom and a sulfur atom as a ring component. These include not only monocyclic heterocycles, but also polycyclic heterocycles that further include an aromatic ring such as a benzene ring or a naphthalene ring in addition to the monocyclic heterocycle. Examples of the "heterocyclic group containing an oxygen atom, a nitrogen atom or a sulfur atom" include a pyrrole group, a benzopyrrole group, a thiophene group, a benzothiophene group, a thiazole group, a benzothiazole group, a naphthothiazole group, a triazole group, a benzotriazole group, a naphthotriazole group, a thiadiazole group, a benzothiadiazole group, a pyridine group, etc.

[0021] The substituents in the above-mentioned "optionally substituted amino group", "optionally substituted C1-4 alkyl group", "optionally substituted C1-4 alkoxy group", "optionally substituted aromatic group" and "optionally substituted heterocyclic group containing an oxygen atom, a nitrogen atom or a sulfur atom" are not particularly limited, and examples thereof include a hydroxy group, a cyano group, a phosphate group, a sulfo group, a carboxy group, an amino group, etc. The "optionally substituted amino group" may further have a substituent such as those exemplified here.

[0022] In the above formula (1), each M independently represents a hydrogen atom, a metal ion, or an ammonium ion. Examples of the metal ion include alkali metal ions such as lithium ion, sodium ion, and potassium ion, and alkaline earth metal ions such as calcium ion and magnesium ion. Examples of the ammonium ion include ammonium ion in the narrow sense (NH4 + ), methylammonium ion, dimethylammonium ion, triethylammonium ion, tetraethylammonium ion, tetra-n-propylammonium ion, tetra-n-butylammonium ion, monoethanolammonium ion, diethanolammonium ion, triethanolammonium ion, monoisopropanolammonium ion, diisopropanolammonium ion, triisopropanolammonium ion, triethanolammonium ion, etc. More specifically, for example, when M is a hydrogen atom, it represents sulfonic acid (-SO3H), when M is a sodium ion, it represents sodium sulfonate (-SO3Na), and when M is an ammonium ion, it represents ammonium sulfonate (-SO3NH4). Among these, preferred ones include lithium ion, ammonium ion, and sodium ion.

[0023] In the above formula (2), * indicates the bonding position of X and / or Y in formula (1), Z is selected from the group consisting of an optionally substituted phenyl group, an optionally substituted naphthyl group, an optionally substituted stilbene group, an optionally substituted benzoyl group, and an optionally substituted heterocyclic group, and t represents an integer of 0 or 1.

[0024] The "heterocyclic group which may have a substituent" in the definition of Z may be, for example, the same as the "heterocyclic group containing an oxygen atom, a nitrogen atom or a sulfur atom which may have a substituent" in the definition of X and Y in the above formula (1), and may further be a furan group, a benzofuran group, or the like which contains an oxygen atom as a ring component.

[0025] Preferred substituents of the "phenyl group which may have a substituent" in the definition of Z include a C1-4 alkoxy group, a nitro group, a sulfo group, and the substituents represented by the formulae (3) to (7). Preferred substituents of the "naphthyl group which may have a substituent" in the definition of Z include a hydroxy group, a sulfo group, a nitro group, and a C1-4 alkoxy group having a sulfo group. Preferred substituents of the "stilbene group which may have a substituent" in the definition of Z include a sulfo group, a nitro group, an amino group which may have a substituent, and the substituents represented by the formulae (3) to (7). Preferred substituents of the "optionally substituted benzoyl group" in the definition of Z include a sulfo group, a nitro group, and the like. Preferred substituents of the "optionally substituted heterocyclic group" in the definition of Z include a sulfo group, a halogen group, a hydroxy group, a C1-4 alkyl group, a C1-4 alkoxy group, a C1-4 alkyl group having a sulfo group, a C1-4 alkyl group having a hydroxy group, a C1-4 alkyl group having a carboxy group, a C1-4 alkoxy group having a sulfo group, a C1-4 alkoxy group having a hydroxy group, a C1-4 alkoxy group having a carboxy group, and the like.

[0026] Examples of the "halogen group" in the definition of Z include a fluorine group, a chlorine group, a bromine group, and an iodine group.

[0027] Examples of the "C1-4 alkyl group" in the definition of Z include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and a cyclobutyl group.

[0028] Examples of the "C1 to C4 alkoxy group" in the definition of Z include a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, and a cyclobutoxy group.

[0029] The above "C1-4 alkyl group having a sulfo group", "C1-4 alkyl group having a hydroxy group", and "C1-4 alkyl group having a carboxy group" in the definition of Z include the above "C1-4 alkyl group" having a sulfo group, a hydroxy group, or a carboxy group as a substituent at any position.

[0030] The above "C1-4 alkoxy group having a sulfo group", "C1-4 alkoxy group having a hydroxy group", and "C1-4 alkoxy group having a carboxy group" in the definition of Z include the above "C1-4 alkoxy group" having a sulfo group, a hydroxy group, or a carboxy group as a substituent at any position.

[0031] At least one of X, Y in the above formula (1), and Z in the above formula (2) when at least one of X and Y is represented by the above formula (2) is preferably selected from the group consisting of substituents represented by the above formulas (3) to (7).

[0032] In the above formula (3) and formula (4), each A is independently selected from the group consisting of a hydrogen atom, a halogen group, a nitro group, a hydroxy group, a C1-4 alkyl group, a C1-4 alkoxy group, a C1-4 alkyl group having a sulfo group, a C1-4 alkyl group having a hydroxy group, a C1-4 alkyl group having a carboxy group, a C1-4 alkoxy group having a sulfo group, a C1-4 alkoxy group having a hydroxy group, and a C1-4 alkoxy group having a carboxy group; 1 represents an integer of 0 to 4, M in the above formulas (3) to (7) is as defined in the above formula (1), and n 1 and n 2 each independently represents an integer of 0 to 3, and * in the above formulas (3) to (7) respectively indicates the bonding position of X or Y in the above formula (1), or the bonding position of Z in the above formula (2).

[0033] Examples of the "C1-4 alkyl group" in the definition of A include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and a cyclobutyl group.

[0034] Examples of the "C1-4 alkyl group having a sulfo group" in the definition of A include a sulfomethyl group, a sulfoethyl group, a sulfo-n-propyl group, a sulfo-n-butyl group, and a sulfo-sec-butyl group.

[0035] Examples of the "halogen group" in the definition of A include a fluorine group, a chlorine group, a bromine group, and an iodine group.

[0036] Examples of the "C1 to C4 alkoxy group" in the definition of A include a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, and a cyclobutoxy group.

[0037] Examples of the "C1-4 alkyl group having a hydroxy group" in the definition of A include a hydroxymethyl group, a hydroxyethyl group, a hydroxy-n-propyl group, a hydroxy-iso-propyl group, a hydroxy-n-butyl group, a hydroxy-sec-butyl group, a hydroxy-tert-butyl group, and a hydroxycyclobutyl group.

[0038] Examples of the "C1-4 alkyl group having a carboxy group" in the definition of A include a carboxymethyl group, a carboxyethyl group, a carboxy-n-propyl group, a carboxy-iso-propyl group, a carboxy-n-butyl group, a carboxy-sec-butyl group, a carboxy-tert-butyl group, and a carboxycyclobutyl group.

[0039] Examples of the "C1 to C4 alkoxy group having a sulfo group" in the definition of A include a sulfomethoxy group, a sulfoethoxy group, a sulfo-n-propoxy group, a sulfo-iso-propoxy group, a sulfo-n-butoxy group, a sulfo-sec-butoxy group, a sulfo-tert-butoxy group, and a sulfocyclobutoxy group.

[0040] Examples of the "C1-4 alkoxy group having a hydroxy group" in the definition of A include a hydroxymethoxy group, a hydroxyethoxy group, a hydroxy-n-propoxy group, a hydroxy-iso-propoxy group, a hydroxy-n-butoxy group, a hydroxy-sec-butoxy group, a hydroxy-tert-butoxy group, and a hydroxycyclobutoxy group.

[0041] Examples of the "C1-4 alkoxy group having a carboxy group" in the definition of A include a carboxymethoxy group, a carboxyethoxy group, a carboxy-n-propoxy group, a carboxy-iso-propoxy group, a carboxy-n-butoxy group, a carboxy-sec-butoxy group, a carboxy-tert-butoxy group, and a carboxycyclobutoxy group.

[0042] Preferably, at least one of X and Y in the above formula (1) is selected from the group consisting of the substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of the substituents represented by formulas (3) to (7). More preferably, X and Y in the above formula (1) are each independently selected from the group consisting of the substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of the substituents represented by formulas (3) to (7). Even more preferably, both X and Y in the above formula (1) are selected from the group consisting of the substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of the substituents represented by formulas (3) to (7).

[0043] In one embodiment of the invention, each m is 0.

[0044] In one embodiment of the invention, s is 0.

[0045] In one embodiment of the present invention, s is 1. In this embodiment, it is also preferable that the above formula (1) is represented by the above formula (1'). In formula (1'), X and Y are each as defined in the above formula (1).

[0046] A method for synthesizing the compound represented by formula (1) in which s is 0 will now be described.

[0047] For example, one equivalent each of the compound represented by formula (9) and the compound represented by formula (10) is heated in water, and caustic soda is added to dissolve them. One equivalent of commercially available terephthalic acid dichloride represented by formula (8) is added and reacted to obtain the target product.

[0048] [ka]

[0049] In the above formulas (8) to (10), X, Y, M, and m are each defined as in the above formula (1).

[0050] Next, specific examples of the luminescent compound or a salt thereof represented by the above formula (1) in which s is 0 are given below. Note that the sulfo group and the like in the formula are represented in the form of a free acid. [ka] [ka]

[0051] Next, a method for synthesizing the compound represented by formula (1) in which s is 1 will be described.

[0052] For example, one equivalent each of the compounds represented by the following formulae (8-A) and (8-B) is heated in water, and caustic soda is added to dissolve the mixture. One equivalent of commercially available terephthalic acid dichloride represented by formula (8) is added and reacted to obtain the target product.

[0053] [ka]

[0054] In formulas (8), (8-A), and (8-B), X, Y, M, and m are as defined in formula (1).

[0055] Next, specific examples of the luminescent compound or a salt thereof represented by the above formula (1) in which s is 1 are given below. Note that the sulfo group and the like in the formula are represented in the form of a free acid. [ka] [ka]

[0056] The compound represented by the above formula (1) or its salt is useful as a compound capable of polarized light emission. The compound represented by the formula (1) or its salt is combined with one or more organic dyes or fluorescent dyes other than the luminescent compound or its salt, if necessary, and is incorporated into a substrate, for example, a polymer film such as polyvinyl alcohol or its derivative, by a known method, and oriented to produce a polarized light-emitting device. The obtained polarized light-emitting device is provided with a transparent protective film to form a polarized light-emitting plate, and the polarized light-emitting plate is further provided with a hard coat layer (protective layer) or an AR (anti-reflection) layer and a support, if necessary, and is applied to liquid crystal projectors, calculators, clocks, notebook computers, word processors, liquid crystal televisions, car navigation systems, security displays, counterfeit prevention, and indoor and outdoor measuring instruments and displays, lenses, glasses, etc. In addition, in this specification, organic dyes or fluorescent dyes other than the luminescent compound or its salt according to the present invention may be abbreviated as "other organic dyes".

[0057] [Polarized light emitting element] The present invention also includes a polarized light-emitting device that contains the light-emitting compound represented by the above formula (1) or a salt thereof. The polarized light emitting element is preferably a polarized light emitting element comprising a luminescent compound represented by the above formula (1) or a salt thereof, and a substrate on which the polarized compound or the salt thereof is adsorbed and oriented. The polarized light emitting element may comprise one or more luminescent compounds represented by the above formula (1) or salts thereof.

[0058] The substrate is preferably a film obtained by forming a hydrophilic polymer capable of adsorbing the luminescent compound represented by the above formula (1) or a salt thereof. The hydrophilic polymer is not particularly limited, but examples thereof include polyvinyl alcohol resins, amylose resins, starch resins, cellulose resins, and polyacrylate resins. Among these resins, polyvinyl alcohol resins or derivatives thereof are preferred from the viewpoint of the adsorption, processability, and orientation of the luminescent compound represented by the above formula (1) or a salt thereof. As the polyvinyl alcohol resin derivative, any one generally known in this technical field can be used. Examples thereof include, but are not limited to, unsaturated carboxylic acids such as crotonic acid, acrylic acid, methacrylic acid, and maleic acid, unsaturated sulfonic acids such as vinyl sulfonic acid, acryl sulfonic acid, methacryloyl sulfonic acid, p-styrene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, and (meth)acryloyloxyethyl sulfonic acid, and modified polyvinyl alcohol resins obtained by copolymerizing olefins such as ethylene and propylene with vinyl alcohol. The shape of the substrate is not particularly limited, and the substrate can be prepared in any shape, for example, a film, a sheet, a flat plate, a curved plate, a hemisphere, etc. The thickness of the substrate is usually 10 to 100 μm, and preferably 20 to 80 μm.

[0059] The content of the luminescent compound represented by the formula (1) in the polarized light emitting element is not particularly limited, and the content can be designed based on any transmittance, and the content (content) may be set arbitrarily according to the transmittance required for the polarized light emitting element. The polarization performance of the polarized light emitting element varies not only depending on the content ratio of the luminescent compound represented by the formula (1) contained in the polarized light emitting element, but also on various factors such as the swelling degree of the substrate to which the luminescent compound is adsorbed, the stretching ratio, the dyeing time, the dyeing temperature, the pH during dyeing, and the influence of salt. For this reason, the content ratio of the luminescent compound represented by the formula (1) contained in the polarized light emitting element can be determined according to the swelling degree of the substrate, the dyeing temperature, the dyeing time, the pH during dyeing, the type of salt, the salt concentration, the stretching ratio, and the like. Such adjustment of the content ratio can be performed appropriately.

[0060] The polarized light emitting element may further contain one or more other organic dyes as necessary, within a range that does not impair the polarization performance or for the purpose of color adjustment. The other organic dyes used in combination are not particularly limited, but are preferably dyes with high dichroism and dyes that have little effect on the polarization performance in the absorption band of the light emitting compound represented by formula (1), for example, the ultraviolet region to the near ultraviolet visible region. Examples of the other organic dyes used in combination include CI Direct.Yellow 12, CI Direct.Yellow 28, CI Direct.Yellow 44, CI Direct.Orange 26, CI Direct.Orange 39, CI Direct.Orange 71, CI Direct.Orange 107, CI Direct.Red 2, CI Direct.Red 31, CI Direct.Red 79, CI Direct.Red 81, CI Direct.Red 247, CI Direct.Blue 69, CI Direct.Blue 78, CI Direct.Green 80, and CI Direct.Green 59. These other organic dyes may be in the form of free acids, alkali metal salts (eg, Na, K, and Li salts), ammonium salts, or salts of amines.

[0061] When the other organic dyes are used in combination as necessary, the type of the other organic dyes to be blended can be selected depending on the purpose such as adjusting the color of the polarized light emitting device to be manufactured. The content is not particularly limited, but generally, when the mass of the luminescent compound represented by the above formula (1) is taken as 1, the total mass of the other organic dyes to be used in combination is preferably in the range of 0.01 to 10.

[0062] <Method of manufacturing polarized light emitting device> Next, a method for producing the polarized light emitting device according to the present invention will be described. The production method is not limited to the following manufacturing method, but may include, for example, a step of preparing a substrate, a swelling step of immersing the substrate in a swelling liquid and stretching the substrate by swelling, a dyeing step of impregnating the swollen substrate with a dyeing solution containing at least one luminescent compound represented by the above formula (1) and adsorbing the luminescent compound represented by formula (1) to the substrate, a crosslinking step of immersing the substrate with the luminescent compound represented by formula (1) adsorbed in a solution containing a crosslinking agent such as boric acid and crosslinking the luminescent compound represented by formula (1) in the substrate, a stretching step of uniaxially stretching the substrate with the luminescent compound represented by formula (1) crosslinked in a certain direction to align the luminescent compound represented by formula (1) in a certain direction, a washing step of washing the stretched substrate with a washing liquid, and a drying step of drying the washed substrate.

[0063] (Preparation of the substrate) A substrate for containing the luminescent compound represented by the above formula (1) is prepared. For example, a film containing a commercially available polyvinyl alcohol resin or its derivative may be used as the substrate, or the substrate may be prepared by forming a film of the polyvinyl alcohol resin. The method for forming a film of the polyvinyl alcohol resin is not particularly limited, and known film forming methods can be adopted, such as a method of melt extruding water-containing polyvinyl alcohol, a casting film forming method, a wet film forming method, a gel film forming method (a polyvinyl alcohol aqueous solution is cooled to gel, and then the solvent is extracted and removed), a cast film forming method (a polyvinyl alcohol aqueous solution is cast on a substrate and dried), and a method by a combination of these. The degree of polymerization of the polyvinyl alcohol may be 1000 to 10000, and the degree of polymerization is preferably 1500 to 6000, and more preferably 2000 to 6000.

[0064] (Swelling process) Next, the above-mentioned substrate is subjected to a swelling treatment. The swelling treatment is preferably carried out by immersing the substrate in a swelling liquid at 20 to 50° C. for 30 seconds to 10 minutes, and the swelling liquid is preferably water. The stretching ratio of the substrate by the swelling liquid is preferably adjusted to 1.00 to 1.50 times, and more preferably adjusted to 1.10 to 1.35 times.

[0065] (dying process) Subsequently, at least one luminescent compound represented by formula (1) or a salt thereof is adsorbed and impregnated into the substrate obtained by the swelling treatment as described above. The dyeing step is not particularly limited as long as it is a method for adsorbing and impregnating the luminescent compound represented by formula (1) or a salt thereof into the substrate. For example, it is preferable to immerse the substrate in a dyeing solution containing the luminescent compound represented by formula (1) or a salt thereof, and it is also possible to adsorb the luminescent compound by applying the dyeing solution to the substrate. The concentration of the luminescent compound represented by formula (1) or a salt thereof in the dyeing solution is not particularly limited as long as the luminescent compound represented by formula (1) or a salt thereof is sufficiently adsorbed into the substrate. For example, it is preferable that the concentration of the luminescent compound represented by formula (1) or a salt thereof in the dyeing solution is 0.0001 to 3 mass %, and more preferably 0.001 to 1 mass %.

[0066] The temperature of the dyeing solution in the dyeing step is preferably 5 to 80° C., more preferably 20 to 50° C., and particularly preferably 40 to 50° C. The time for immersing the substrate in the dyeing solution can be appropriately adjusted, and is preferably adjusted between 30 seconds and 20 minutes, and more preferably between 1 to 10 minutes.

[0067] As the compound contained in the dyeing solution, the luminescent compound represented by the above formula (1) may be used alone or in combination of two or more. Since the luminescent compound represented by the above formula (1) has different emission colors due to differences in structure, the luminescent color generated can be appropriately adjusted to a desired color by containing two or more luminescent compounds represented by the above formula (1) or their salts, or the luminescent compound represented by the above formula (1) or its salts and one or more other luminescent compounds in the base material. In addition, the dyeing solution may further contain one or more of the other organic dyes as necessary. In the description of the manufacture of the polarized light-emitting element and the polarized light-emitting plate in this specification, the luminescent compound represented by formula (1) and the other organic dyes may be collectively referred to as "polarizing dyes".

[0068] The dyeing solution may further contain a dyeing assistant as necessary in addition to the polarizing dye. Examples of the dyeing assistant include sodium carbonate, sodium bicarbonate, sodium chloride, sodium sulfate (mirabilite), anhydrous sodium sulfate, and sodium tripolyphosphate, and sodium sulfate is preferred. The content of the dyeing assistant can be arbitrarily adjusted by the immersion time and the temperature of the dyeing solution based on the dyeability of the polarizing dye used, but it is preferably 0.1 to 10% by mass, and more preferably 0.1 to 2% by mass in the dyeing solution.

[0069] After the dyeing step, a preliminary cleaning step can be optionally performed to remove the dyeing solution attached to the surface of the substrate in the dyeing step. By performing the preliminary cleaning step, it is possible to prevent the luminescent compound represented by formula (1) or its salt remaining on the surface of the substrate from migrating into the treatment liquid in the next step. In the preliminary cleaning step, water is generally used as the cleaning liquid. As a cleaning method, it is preferable to immerse the dyed substrate in the cleaning liquid, and on the other hand, the substrate can also be cleaned by applying the cleaning liquid to the substrate. The cleaning time is not particularly limited, but is preferably 1 to 300 seconds, and more preferably 1 to 60 seconds. The temperature of the cleaning liquid in the preliminary cleaning step must be a temperature at which the material constituting the substrate does not dissolve, and the cleaning treatment is generally performed at 5 to 40°C. The preliminary cleaning step can be omitted because the performance of the polarized light emitting device is not significantly affected even if the preliminary cleaning step is not performed.

[0070] (Crosslinking process) After the dyeing step or the preliminary washing step, the crosslinking agent can be incorporated into the substrate. The method of incorporating the crosslinking agent into the substrate is preferably to immerse the substrate in a treatment solution containing the crosslinking agent, or the treatment solution may be applied or coated onto the substrate. As the crosslinking agent in the treatment solution, a solution containing boric acid is preferably used. The solvent in the treatment solution is not particularly limited, but water is preferred. The concentration of the crosslinking agent such as boric acid in the treatment solution is preferably 0.1 to 15 mass%, more preferably 0.1 to 10 mass%. The temperature of the treatment solution is preferably 30 to 80°C, more preferably 40 to 75°C. The treatment time of this crosslinking step is preferably 30 seconds to 10 minutes, more preferably 1 to 6 minutes. By including this crosslinking step in the method for producing a polarized light-emitting element according to the present invention, the obtained polarized light-emitting element can emit light having high brightness and a high degree of polarization. This is an excellent effect that is completely unexpected from the function of boric acid used in the prior art for the purpose of improving moisture resistance or light transmittance. In addition, in the crosslinking step, if necessary, a fixation treatment may be performed in combination with an aqueous solution containing a cationic polymer compound. The fixation treatment enables the fixation of the polarizing dye. In this case, as the cationic polymer compound, for example, a cation-releasing compound, a dicyan compound, a polyamine compound, a polycation compound, a dimethyldiallylammonium chloride-dioxide ion copolymer, a diallylamine salt polymer, a dimethyldiallylammonium chloride polymer, an allylamine salt polymer, or a dialkylaminoethyl acrylate quaternary salt polymer may be used. As the dicyan compound, for example, a dicyanamide-formaldehyde polymerized condensate may be used. As the polyamine compound, for example, a dicyandiamide-diethylenetriamine polycondensate may be used. As the polycation compound, for example, an epichlorohydrin-dimethylamine addition polymer may be used.

[0071] (Stretching process) After or simultaneously with the crosslinking step, a stretching step is carried out. The stretching step is carried out by uniaxially stretching the substrate in a certain direction. The stretching method may be either a wet stretching method or a dry stretching method. The stretching ratio is preferably 3 times or more, and more preferably 5 to 9 times.

[0072] In the dry stretching method, when the stretching heating medium is air, the substrate is preferably stretched at a temperature of the air medium ranging from room temperature to 180° C. The humidity is preferably 20 to 95% RH in the atmosphere. Examples of the method for heating the substrate include, but are not limited to, a zone stretching method between rolls, a roll heating stretching method, a hot rolling stretching method, and an infrared heating stretching method. The dry stretching process may be performed in one stage or in a multi-stage stretching method of two or more stages.

[0073] In the wet stretching method, it is preferable to stretch the substrate in water, a water-soluble organic solvent, or a mixed solution thereof. More preferably, the substrate is stretched while being immersed in a solution containing at least one crosslinking agent. The crosslinking agent may be, for example, boric acid in the crosslinking agent step, and the stretching may be preferably performed in the treatment solution used in the crosslinking step. The stretching temperature is preferably 40 to 70°C, more preferably 45 to 60°C. The stretching time is usually 30 seconds to 20 minutes, preferably 2 to 7 minutes. The wet stretching step may be performed in a single stretching step, or in a multi-stage stretching step of two or more stages. The stretching step may be optionally performed before the dyeing step, in which case the orientation of the luminescent compound represented by formula (1) or its salt can be performed at the same time as the dyeing step.

[0074] (Cleaning process) After the stretching step, the crosslinking agent may be precipitated or foreign matter may adhere to the surface of the substrate, so a washing step for washing the surface of the substrate may be performed. The washing time is preferably 1 second to 5 minutes. The washing method is preferably to immerse the substrate in a washing liquid, but the substrate may also be washed by applying or coating the washing liquid. The washing liquid is preferably water. The washing treatment may be performed in one stage or in a multi-stage treatment of two or more stages. The temperature of the washing solution in the washing step is not particularly limited, but is usually 5 to 50°C, preferably 10 to 40°C, and may be room temperature.

[0075] Examples of the solvent of the solution or treatment liquid used in each of the above-mentioned steps include, in addition to the above-mentioned water, alcohols, amines, etc. Examples of the alcohols include dimethyl sulfoxide, N-methylpyrrolidone, methanol, ethanol, propanol, isopropyl alcohol, glycerin, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, and trimethylolpropane, etc. Examples of the amines include ethylenediamine and diethylenetriamine, etc. The solvent of the solution or treatment liquid is not limited to these, but is most preferably water. Moreover, the solvent of these solutions or treatment liquids may be used alone or in a mixture of two or more.

[0076] (drying process) After the washing step, it is preferable to carry out a drying step of the substrate. The drying process can be carried out by natural drying, but in order to increase the drying efficiency, it is possible to carry out the drying process by compressing with a roll or removing moisture from the surface with an air knife or water absorbing roll, and further, it is also possible to carry out air drying. The temperature of the drying process is preferably 20 to 100°C, and more preferably 60 to 100°C. The drying time is preferably 30 seconds to 20 minutes, and more preferably 5 to 10 minutes.

[0077] The above description is an example of a polarized light-emitting device according to the present invention. The light-emitting compound represented by formula (1) in the present invention can be mixed with liquid crystal and aligned on a substrate, or aligned by a coating method in which the compound is sheared on a substrate, to produce a polarized light-emitting device having various colors or neutral gray.

[0078] [Polarizing plate] The present invention also includes a polarized light-emitting plate including the above-described polarized light-emitting element. The polarized light-emitting plate according to the present invention preferably has a transparent protective film on at least one surface of the polarized light-emitting element. The transparent protective film is used to improve the water resistance and handling properties of the polarized light-emitting element. Therefore, it is preferable that such a transparent protective film does not have any effect on the polarizing effect exhibited by the polarized light-emitting element according to the present invention.

[0079] The transparent protective film is preferably a transparent protective film excellent in optical transparency and mechanical strength. The transparent protective film is preferably a film having a layer shape capable of maintaining the shape of the polarized light emitting element, and is preferably a plastic film excellent in thermal stability, moisture shielding property, etc. in addition to transparency and mechanical strength. Examples of materials for forming such a transparent protective film include fluoro-based films such as cellulose acetate-based films, acrylic-based films, tetrafluoroethylene / hexafluoropropylene-based copolymers, and films made of polyester resins, polyolefin resins, or polyamide resins, and preferably triacetyl cellulose (TAC) films and cycloolefin-based films are used. The thickness of the transparent protective film is preferably in the range of 1 to 200 μm, more preferably in the range of 10 to 150 μm, and particularly preferably in the range of 40 to 100 μm. The method for producing the polarized light emitting plate according to the present invention is not particularly limited, but for example, the polarized light emitting plate can be produced by laminating the transparent protective film on the polarized light emitting element according to a known formula.

[0080] The polarized light-emitting plate may further include an adhesive layer between the transparent protective film and the polarized light-emitting element for bonding the transparent protective film to the polarized light-emitting element. The adhesive constituting the adhesive layer is not particularly limited, but examples thereof include polyvinyl alcohol-based adhesives, urethane emulsion-based adhesives, acrylic adhesives, polyester-isocyanate adhesives, etc., and preferably polyvinyl alcohol-based adhesives are used. After bonding the transparent protective film and the polarized light-emitting element with the adhesive, the polarized light-emitting plate can be produced by drying or heat treatment at an appropriate temperature.

[0081] In addition, the polarized light-emitting plate may be provided with various known functional layers such as an anti-reflection layer, an anti-glare layer, and a further transparent protective film on the exposed surface of the transparent protective film. When preparing such layers having various functions, a method of coating materials having various functions on the exposed surface of the transparent protective film is preferred, while a layer or film having such functions can also be attached to the exposed surface of the transparent protective film via an adhesive or pressure-sensitive adhesive.

[0082] Examples of the further transparent protective film include a hard coat layer of an acrylic type, a urethane type, a polysiloxane type, etc. In order to further improve the single-piece transmittance, an antireflection layer can be provided on the exposed surface of the transparent protective film. The antireflection layer can be formed, for example, by depositing or sputtering a material such as silicon dioxide or titanium oxide on the transparent protective film, or by thinly coating a fluorine-based material on the transparent protective film.

[0083] The polarized light-emitting plate may further include a transparent support such as glass, quartz, or sapphire, if necessary. Such a support preferably has a flat surface to which the polarized light-emitting plate is attached, and is preferably a transparent support from the viewpoint of optical applications. Transparent supports are divided into inorganic supports and organic supports. For example, supports made of inorganic materials include supports made of materials such as soda glass, borosilicate glass, quartz, sapphire, and spinel, and organic supports include supports made of acrylic, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, and cycloolefin polymer. The thickness and size of the transparent support are not particularly limited and can be determined appropriately. In addition, in order to further improve the single transmittance of the polarized light-emitting plate having such a transparent support, it is preferable to provide an anti-reflection layer on one or both surfaces of the support surface or the polarized light-emitting plate surface. In order to bond the polarized light-emitting plate to the flat surface of the support, a transparent adhesive (adhesive) agent is applied to the flat surface of the support, and then the polarized light-emitting plate according to the present invention is attached to the applied surface. The adhesive or pressure-sensitive adhesive to be used is not particularly limited, and commercially available adhesives or pressure-sensitive adhesives can be used, with acrylic ester-based adhesives or pressure-sensitive adhesives being preferred.

[0084] The polarized light-emitting plate can also be used as a circularly polarized light-emitting plate or an elliptically polarized light-emitting plate to which a retardation plate is attached. In this case, when a support or the like is further provided on the polarized light-emitting plate, the support may be a retardation plate. Retardation plates generally include those having a retardation value of 1 / 4λ or a retardation value of 1 / 2λ with respect to the absorption wavelength or emission wavelength of light, but are not limited thereto. By having a retardation value of 1 / 4λ, it functions as a circularly polarized light-emitting plate or a circularly polarized light-emitting plate with respect to that wavelength, and by using 1 / 2λ, it is possible to use it in such a way that the polarized light can be converted to a direction of 90°. In this way, the polarized light-emitting plate can be further provided with various functional layers, supports, etc., and such polarized light-emitting plates can be used in various products such as liquid crystal projectors, calculators, clocks, notebook computers, word processors, liquid crystal televisions, car navigation systems, and indoor and outdoor measuring instruments and displays, lenses, or glasses.

[0085] The polarized light emitting element and the polarized light emitting plate according to the present invention show a high degree of polarization in the ultraviolet to near ultraviolet visible region, for example, in the region of 300 to 430 nm, and further show polarized light emission action and high transmittance in the visible light region. In addition, the polarized light emitting element and the polarized light emitting plate according to the present invention show excellent durability against heat, humidity, light, etc., and can maintain their performance even in harsh environments, and have higher durability than conventional iodine-based polarizing plates. Therefore, the polarized light emitting element and the polarized light emitting plate according to the present invention can be applied to various display devices such as liquid crystal displays that require high transparency in the visible light region and high durability in harsh environments, such as televisions, wearable terminals, tablet terminals, smartphones, in-vehicle monitors, digital signage used outdoors or indoors, and smart windows.

[0086] [Display device] The present invention also includes a display device including the above-mentioned polarized light-emitting element or polarized light-emitting plate. The display device exhibits a polarized light emission effect by irradiating light in the ultraviolet to visible range, for example, light in the ultraviolet to near-ultraviolet visible range, specifically light of 300 to 430 nm, and this effect is utilized to enable display. The display device according to the present invention has a high transmittance in the visible light range, so there is no decrease in the transmittance in the visible light range as in conventional polarizing plates, or even if there is a decrease in the transmittance, the decrease in the transmittance is significantly smaller than that of conventional polarizing plates. For example, in conventional polarizing plates, such as iodine-based polarizing plates and dye-based polarizing plates using other dyes, the luminosity correction in the visible light range is about 35 to 45% in order to achieve a polarization degree of approximately 100%. The reason for this is that conventional polarizing plates have both a vertical axis and a horizontal axis as the light absorption axis, but in order to achieve a polarization degree of approximately 100%, the incident light is absorbed on one of the vertical axis or the horizontal axis, that is, light is absorbed on one axis and transmitted on the other axis, resulting in polarization. In such a case, the light on one axis is absorbed and not transmitted, so the transmittance inevitably becomes 50% or less. Conventionally, a polarizing plate is prepared by orienting a dichroic dye in a stretched film, but the dichroic dye is not necessarily 100% oriented, and the dichroic dye also has a small amount of absorption component with respect to the light transmission axis. Therefore, unless the transmittance is about 45% or less due to the surface reflection of the material, a polarization degree of almost 100% cannot be realized, that is, a high polarization degree cannot be realized unless the transmittance is reduced. In contrast, the polarized light emitting element and the polarized light emitting plate according to the present invention have an axis of light absorption (polarizing function) in the ultraviolet to near ultraviolet visible region, for example, 300 to 430 nm, that is, they have a light absorbing action in the ultraviolet to near ultraviolet visible region, for example, 300 to 430 nm, and exhibit a polarized light emitting action of emitting polarized light in the visible light region, while they hardly absorb light in the visible light region, so that the transmittance in the visible light region is very high. Furthermore, since they exhibit a polarized light emitting action in the visible light region, the loss of light is less than that of a conventional polarizing plate, that is, the decrease in transmittance as in the conventional polarizing plate is very small. Therefore, a display device, such as a liquid crystal display, using the polarized light-emitting element and polarized light-emitting plate according to the present invention can achieve higher brightness than a liquid crystal display equipped with a conventional polarizing plate.Furthermore, since the display device using the polarized light emitting element and the polarized light emitting plate according to the present invention has high transparency, it is possible to obtain a nearly transparent display, even though it is a liquid crystal display. Also, since it can be designed so that the polarized emitted light is transmitted when displaying characters and images, it is possible to obtain a display that is capable of displaying even though it is a transparent liquid crystal display, that is, a display that is capable of displaying characters and the like on a transparent display. Therefore, the display device according to the present invention can obtain a transparent liquid crystal display with no optical loss, in particular a see-through display.

[0087] In addition, the display device can polarize light in the ultraviolet to near ultraviolet visible range, for example, light of 300 to 430 nm, which is invisible or difficult to see with the human eye, and therefore can be applied to liquid crystal displays that can display images using ultraviolet light. For example, by recognizing an image or the like displayed in the ultraviolet to near ultraviolet visible range by a computer or the like, it is possible to fabricate a simple and highly secure liquid crystal display that is visible only when irradiated with light in the ultraviolet to near ultraviolet visible range, for example, light of 300 to 430 nm.

[0088] In addition, the display device exhibits polarized luminescence when irradiated with light in the ultraviolet to near-ultraviolet visible range, for example, light of 300 to 430 nm, and since a liquid crystal display utilizing this polarized luminescence can be produced, it is possible to realize a liquid crystal display utilizing light in the ultraviolet to near-ultraviolet visible range, rather than a normal liquid crystal display utilizing visible light. In other words, even in a dark space without visible light, as long as the space is irradiated with light in the ultraviolet to near-ultraviolet visible range, it is possible to produce an emissive liquid crystal display that displays characters, images, etc.

[0089] Furthermore, since the bands of light in the visible light region and the ultraviolet light region are different, it is possible to fabricate a display capable of two different displays, in which a liquid crystal display portion capable of displaying light in the visible light region and a liquid crystal display portion in light displayed by the polarized light emission action of ultraviolet light coexist. Displays capable of two different displays have existed up to now, but there is no display capable of displaying different images using separate light sources in the ultraviolet light region and the visible light region, even though it is the same liquid crystal panel. For this reason, the display device according to the present invention makes it possible to fabricate a novel display by using the above-mentioned polarized light emitting element or polarized light emitting plate.

[0090] The present invention also includes a liquid crystal display equipped with the above-mentioned polarized light-emitting element, polarized light-emitting plate, or display device. The liquid crystal cell used in the liquid crystal display is not limited to, for example, a TN liquid crystal cell, an STN liquid crystal cell, a VA liquid crystal cell, an IPS liquid crystal cell, etc., and can be used in any liquid crystal display mode. Since the liquid crystal display has high durability, it can be used as a liquid crystal display for in-vehicle or outdoor display.

[0091] The present invention also includes a neutral gray polarized light-emitting plate for vehicle installation or outdoor display, which is equipped with the above polarized light-emitting element, polarized light-emitting plate, or display device. The neutral gray polarized light-emitting plate for vehicle installation or outdoor display has the characteristic of being excellent in polarized light-emitting performance, and furthermore, not discoloring or decreasing in polarization performance even in high temperature and high humidity conditions inside a vehicle or outdoors. Note that the term "neutral gray" refers to a polarized light-emitting plate having a significantly low or constant transmittance for each wavelength in the orthogonal transmittance of the visible range. Specifically, the orthogonal transmittance is 0.3% or less, more preferably 0.1% or less, even more preferably 0.03% or less, and particularly preferably 0.01% or less, and the constant transmittance means that the difference in transmittance is within 1% with respect to the average transmittance of each wavelength. EXAMPLES

[0092] The present invention will be described in more detail below with reference to examples, which are merely illustrative and do not limit the present invention in any way. In addition, the "%" and "parts" described below are based on mass unless otherwise specified. In addition, in each structural formula of the compound used in each example and comparative example, acidic functional groups such as sulfo groups are described in the form of free acid.

[0093] [Example 1] (Synthesis example) 84 parts of the compound represented by formula (25) was added to 600 parts of water and heated to 60°C. 25% caustic soda was added while adjusting the pH to 6-7 to dissolve the compound. 20.2 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all the components were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was allowed to cool to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 67.4 parts of the compound represented by formula (15). [ka]

[0094] (Preparation of polarized light emitting element and polarized light emitting plate) A polyvinyl alcohol film (VF-PS#7500 manufactured by Kuraray Co., Ltd.) having a thickness of 75 μm was immersed in water at 40° C. for 3 minutes to swell the film. The swollen film was immersed in an aqueous solution at 45° C. containing 0.2 parts by mass of the compound represented by formula (15) obtained in Synthesis Example 1, 1.0 parts by mass of Glauber's salt, and 1000 parts by mass of water, for 4 minutes to allow the compound represented by formula (15) to be contained in the film. The film containing the compound represented by formula (15) was stretched 5 times in a 3% boric acid aqueous solution at 50° C. for 5 minutes. The stretched film was washed with water at room temperature for 20 seconds while maintaining tension, and dried at 70° C. to obtain a polarized light emitting element. A 60 μm-thick triacetyl cellulose film (ZRD-60, manufactured by Fuji Film Corporation) containing no ultraviolet absorber and having its surface saponified with 1.5 N sodium hydroxide was laminated on both sides of the obtained polarized light-emitting element using a 4 mass % aqueous solution of polyvinyl alcohol (NH-26, manufactured by Nippon Vacuum Acetate & Poval Corporation) as an adhesive to obtain a polarized light-emitting plate, which was used as the measurement sample for Example 1. In addition, even when a triacetyl cellulose film (ZRD-60 manufactured by Fujifilm Corporation) that does not contain an ultraviolet absorbing agent was attached to the polarized light emitting element, the optical properties of the polarized light emitting element were not affected at all. In the following examples and comparative examples, a triacetyl cellulose film that does not contain an ultraviolet absorbing agent was also attached to the polarized light emitting element, but similarly, the optical properties were not affected at all.

[0095] [Example 2] 60 parts of the compound represented by formula (26) was added to 600 parts of water and heated to 60°C. 25% caustic soda was added while adjusting the pH to 6 to 7 to dissolve the compound. 20 parts of terephthalic acid dichloride was gradually added over about 1 hour. After all of the components were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 51.5 parts of the compound represented by formula (14). A measurement sample of Example 2 was obtained in the same manner as in Example 1, except that the compound represented by formula (14) was used instead of the compound represented by formula (15). [ka]

[0096] [Example 3] 21.8 parts of the compound represented by formula (27) and 10.8 parts of the compound represented by formula (28) were added to 400 parts of water, and 25% caustic soda was added while adjusting the pH to 6-7 to dissolve the compound, and 15.6 parts of phenyl chloroformate was stirred at 50-70°C for 6 hours to form a ureido compound. Salting out with sodium chloride, filtering, and drying at 70°C obtained 24.6 parts of the ureido compound represented by formula (29). 24.6 parts of the obtained compound represented by formula (29) were added to 500 parts of water, heated to 60°C, and 25% caustic soda was added while adjusting the pH to 6-7 to dissolve the compound. 7.0 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all the mixture was added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70° C. to obtain 5.7 parts of a mixture of the compound represented by formula (16) and the compound represented by formula (30). A measurement sample of Example 3 was obtained in the same manner as in the preparation of the polarized light-emitting element and the polarized light-emitting plate of Example 1, except that the compound represented by formula (15) was replaced with a mixture of the compound represented by formula (16) and the compound represented by formula (30). [ka]

[0097] [Example 4] 21.8 parts of the compound represented by formula (28) was added to 400 parts of water, dissolved while adding sodium hydroxide, and 20.2 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, 80.0 parts of 4-nitro-4'-aminostilbene-2,2'-disulfonic acid was added, dissolved while adding sodium hydroxide, and 31.2 parts of phenyl chloroformate were added little by little over about 1 hour. After all were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 12.4 parts of a mixture of the compound represented by formula (18) and the compound represented by formula (31). In the preparation of the polarized light-emitting element and the polarized light-emitting plate of Example 1, a measurement sample of Example 4 was obtained in the same manner, except that a mixture of the compound represented by formula (18) and the compound represented by formula (31) was used instead of the compound represented by formula (15). [ka]

[0098] [Example 5] 40.0 parts of 4-nitro-4'-aminostilbene-2,2'-disulfonic acid and 10.8 parts of the compound represented by formula (28) were added to 400 parts of water, dissolved while adding sodium hydroxide, and 20.2 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, 40.0 parts of 4-nitro-4'-aminostilbene-2,2'-disulfonic acid were added, dissolved while adding sodium hydroxide, and 15.6 parts of phenyl chloroformate were added little by little over about 1 hour. After all were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was allowed to cool to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 8.9 parts of a mixture of the compound represented by formula (22) and the compound represented by formula (32). A measurement sample of Example 5 was obtained in the same manner as in the preparation of the polarized light-emitting element and polarized light-emitting plate of Example 1, except that a mixture of the compound represented by formula (22) and the compound represented by formula (32) was used instead of the compound represented by formula (15). [ka]

[0099] [Example s1] 120.4 parts of the compound represented by formula (s28) was added to 500 parts of water and heated to 60°C. 25% caustic soda was added while adjusting the pH to 6 to 7 to dissolve the compound. 20.2 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all the ingredients were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 93.4 parts of the compound represented by formula (s29). A measurement sample of Example s1 was obtained in the same manner as in Example 1, except that the compound represented by formula (s29) was used instead of the compound represented by formula (15). [ka]

[0100] [Example s2] 114 parts of the compound represented by formula (s30) was added to 500 parts of water and heated to 60°C, and 25% caustic soda was added while adjusting the pH to 6-7 to dissolve the compound. 20.2 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all of the components were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 103 parts of the compound represented by formula (s14). A measurement sample of Example s2 was obtained in the same manner as in Example 1, except that the compound represented by formula (s14) was used instead of the compound represented by formula (15). [ka]

[0101] [Example s3] 40 parts of 4-nitro-4'-aminostilbene-2,2'-disulfonic acid and 60.2 parts of the compound represented by formula (s28) were added to 500 parts of water and heated to 60°C. 25% caustic soda was added while adjusting the pH to 6-7 to dissolve the compound. 20.2 parts of terephthalic acid dichloride were added little by little over about 1 hour. After all of the ingredients were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 84.1 parts of the compound represented by formula (s31). A measurement sample of Example s3 was obtained in the same manner as in Example 1, except that the compound represented by formula (s31) was used instead of the compound represented by formula (15). [ka]

[0102] [Example s4] 21.8 parts by weight of the compound represented by formula (s32) and 37 parts by weight of 4,4'-diaminostilbene-2,2'-disulfonic acid were added to 500 parts of water, and the mixture was heated to 60°C. 25% caustic soda was added while adjusting the pH to 6 to 7 to dissolve the compound. 20.2 parts of terephthalic acid dichloride were gradually added over about 1 hour. After all the components were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 24.5 parts of a mixture of the compounds represented by formula (s15) and formula (s33). A measurement sample of Example s4 was obtained in the same manner as in Example 1, except that a mixture of the compounds represented by formula (s15) and formula (s33) was used instead of the compound represented by formula (15). [ka]

[0103] [Example s5] 40 parts of 4-nitro-4'-aminostilbene-2,2'-disulfonic acid was added to 500 parts of water and heated to 60°C. 25% caustic soda was added while adjusting the pH to 6-7 to dissolve the compound. 15.6 parts of phenyl chloroformate and 37 parts of 44'-diaminostilbene-2,2'-disulfonic acid were added little by little over about 1 hour. After all were added, the mixture was stirred at 60°C for 1 hour. 10.1 parts of terephthalic acid dichloride were added little by little over about 1 hour, and after all were added, the mixture was stirred at 60°C for 1 hour to react. After the reaction was completed, the mixture was cooled to room temperature and filtered, and the obtained solid was dried at 70°C to obtain 22.3 parts of a compound represented by formula (s19). A measurement sample of Example s5 was obtained in the same manner as in Example 1, except that the compound represented by formula (s19) was used instead of the compound represented by formula (15). [ka]

[0104] [Comparative Example 1] A measurement sample for Comparative Example 1 was obtained in the same manner as in the preparation of the polarized light-emitting element and polarized light-emitting plate of Example 1, except that the compound represented by formula (c1) described in JP-A-4-226162 was used instead of the compound represented by formula (15). [ka]

[0105] [Comparative Example 2] A measurement sample for Comparative Example 2 was obtained in the same manner as in Example 1 in producing the polarized light-emitting element and polarized light-emitting plate, except that CI Direct Yellow 4, a compound represented by formula (c2), was used instead of the compound represented by formula (15). [ka]

[0106] [Comparative Example 3] A measurement sample for Comparative Example 3 was obtained in the same manner as in Example 1 in producing the polarized light-emitting element and the polarized light-emitting plate, except that the compound represented by formula (c3) was used instead of the compound represented by formula (15). [ka]

[0107] [evaluation] Using the measurement samples obtained in Examples 1 to 5 and s1 to s5 and Comparative Examples 1 to 3, evaluations were carried out as follows.

[0108] (a) Measurement of single transmittance Ts, parallel transmittance Tp, and cross transmittance Tc The single transmittance Ts (%), parallel transmittance Tp (%), and orthogonal transmittance Tc (%) of each measurement sample were measured using a spectrophotometer (Hitachi's "U-4100"). Here, the single transmittance Ts (%) is the transmittance at each wavelength when one measurement sample is measured. The parallel transmittance Tp (%) is the spectral transmittance at each wavelength measured by overlapping two measurement samples so that their absorption axis directions are parallel. The orthogonal transmittance Tc (%) is the spectral transmittance measured by overlapping two measurement samples so that their absorption axes are orthogonal. The measurement of each transmittance was performed over a wavelength range of 220 to 780 nm.

[0109] (b) Calculation of the degree of polarization ρ The degree of polarization ρ (%) of each measurement sample was calculated by substituting the parallel transmittance Tp and the crossed transmittance Tc into the following formula (I).

number

[0110] (c) Calculation of the single transmittance Ys corrected for visual sensitivity The luminosity-corrected single transmittance Ys (%) of each measurement sample is the transmittance obtained by correcting the luminosity of the single transmittance Ts obtained at a predetermined wavelength interval dλ (here, 5 nm) in the wavelength region of 400 to 700 nm in the visible range according to JIS Z 8722:2009. Specifically, the luminosity-corrected single transmittance Ys was calculated by substituting the single transmittance Ts into formula (II). In the following formula (II), Pλ represents the spectral distribution of the standard light (C light source), and yλ represents the 2-degree visual field color matching function.

number

[0111] (d) Measurement of the emitted polarized light As a light source, an ultraviolet LED 375 nm hand light type black light (Nichia Corporation "PW-UV943H-04") was used, and an ultraviolet transmission and visible light cut filter (Isuzu Seiko Glass Co., Ltd. "IUV-340") was installed in the light source to cut visible light. When the measurement sample obtained in each example and comparative example was installed and the polarized light emitted by the measurement sample was measured using a spectroradiometer (Ushio Inc. "USR-40"), a polarizing plate having a polarizing function in the visible range and ultraviolet (Poratechno Inc. "SKN-18043P", thickness 180 μm, Ys is 43%) was installed in the light receiving part of the spectroradiometer, and the polarized emission light amount of the measurement sample obtained in each example and comparative example was measured. That is, the measurement was performed by arranging the light from the light source so that it passes through the ultraviolet transmission and visible light cut filter, the measurement sample, and the polarizing plate having polarization in the visible range and ultraviolet in that order, and is incident on the spectroradiometer. In this case, the absorption axis of the measurement sample with the maximum ultraviolet absorption was parallel to the absorption axis direction of a polarizing plate having polarization in the visible range and ultraviolet ("SKN-18043P" manufactured by Polatechno Co., Ltd.), and the spectral emission amount of each wavelength was measured by superposing the absorption axis of the measurement sample with the maximum ultraviolet absorption and the absorption axis direction of a polarizing plate having polarization in the visible range and ultraviolet ("SKN-18043P" manufactured by Polatechno Co., Ltd.) perpendicular to each other, and Lw and Ls were measured. By checking the amount of energy of light emitted in the visible range when the absorption axis of the measurement sample and a general polarizing plate are parallel and perpendicular to each other, the polarized emission light was evaluated in the visible range of 400 to 700 nm.

[0112] (e) Light fastness test A light resistance test was performed by irradiating the sample with light for 500 hours at an illuminance of 60 W, an environmental temperature of 50°C, and a relative humidity of 30% RH using a Suga Test Instruments SX-75. The changes in Ls and Lw at each wavelength were then confirmed.

[0113] Table 1 shows the wavelength at which each of the measurement samples obtained in Examples 1 to 5 and s1 to s5 and Comparative Examples 1 to 3 showed the maximum degree of polarization, as well as the single transmittance Ts (%), parallel transmittance Tp (%), orthogonal transmittance Tc (%), and degree of polarization ρ (%) at the wavelength at which each of the measurement samples showed the maximum degree of polarization, as well as the single transmittance Ys (%) corrected for luminous efficacy and the degree of polarization ρy (%) corrected for luminous efficacy. [Table 1]

[0114] Table 2 below shows Ls and Lw at each wavelength for each measurement sample obtained in Examples 1 to 5 and s1 to s5 and Comparative Examples 1 to 3. [Table 2]

[0115] Table 3 below shows Ls and Lw at each wavelength for each measurement sample obtained in Examples 1 to 5 and s1 to s5 and Comparative Example 1 after the light resistance test. [Table 3]

[0116] As shown in Table 1, it can be seen that the measurement samples of Examples 1 to 5 and s1 to s5 and Comparative Example 1 have absorption in the ultraviolet to near-ultraviolet visible range and function as polarizing light-emitting plates in that range. On the other hand, the transmittance in the visible range (luminosity-corrected transmittance Ys) was approximately 90%, indicating that the samples have high visible transparency while having a polarizing function in the ultraviolet to near-ultraviolet visible range. In contrast, Comparative Examples 2 and 3 showed a maximum polarization degree at wavelengths of 400 nm or more, and the luminosity-corrected transmittance Ys was reduced, indicating a reduction in visible transmittance.

[0117] Furthermore, as shown in Table 2, Lw and Ls were detected in Examples 1 to 5 and s1 to s5 and Comparative Example 1, which indicates that the samples emit polarized light when irradiated with ultraviolet light. On the other hand, Examples 1 to 5 and s1 to s5 had higher maximum emission luminance than Comparative Example 1, or emitted highly polarized light over a wide band of 400 to 700 nm.

[0118] Furthermore, as shown in Table 3, Examples 1 to 5 and s1 to s5 had higher light resistance than Comparative Example 1. Therefore, it was shown that the measurement samples of Examples 1 to 5 and s1 to s5 not only function as polarized light emitting elements that emit polarized light in the visible range when irradiated with ultraviolet light, but also have high light resistance.

[0119] (f) Durability test The polarized light-emitting plates obtained in Examples 1 to 5 and s1 to s5 were subjected to a durability test in an environment at 105°C for 1000 hours and an environment at 60°C and 90% relative humidity for 1000 hours, and no decrease in the degree of polarization or change in the emission of polarized light was observed. This demonstrates that the polarized light-emitting elements and polarized light-emitting plates of Examples 1 to 5 and s1 to s5 have high durability even in harsh environments. [Industrial Applicability]

[0120] By using the light-emitting compound according to the present invention contained in a base material, it is possible to obtain a polarized light-emitting element and a polarized light-emitting plate that not only have a high degree of polarization at the absorption wavelength but also exhibit a polarized light emission effect. In addition, such a polarized light-emitting element and a polarized light-emitting plate have high transmittance in the visible light range while having excellent durability. Therefore, a display device including the polarized light-emitting element or the polarized light-emitting plate according to the present invention has high transparency in the visible light range and can display images by polarized light emission for a long period of time, and is therefore applicable to a wide range of applications such as televisions, personal computers, tablet terminals, and even transparent displays (see-through displays). Furthermore, the polarized light-emitting element and the polarized light-emitting plate including the light-emitting compound according to the present invention can emit light with light in the ultraviolet range to the near-ultraviolet visible range, for example, light of 300 to 430 nm, and therefore can also be applied to displays and media that require high security.

Claims

1. A polarized light-emitting device comprising a light-emitting compound represented by the following formula (1) or a salt thereof: 【Chemistry 1】 (In formula (1), (i) X and Y each independently contain at least a group selected from the group consisting of a group represented by formula (2) above, a heterocyclic group containing a nitrogen atom or a sulfur atom, and a nitro group, except when both X and Y are nitro groups; or (ii) at least one of X and Y (independently in the case of both) is a nitro group, an amino group which may have a substituent, a C1-4 alkyl group which may have a substituent, a C1-4 alkoxy group which may have a substituent, an aromatic group which may have a substituent, an oxygen atom which may have a substituent, a heterocyclic group containing a nitrogen atom or a sulfur atom, or a group represented by formula (2), and when X or Y is not a group selected above, then said X or Y is selected from any substituent, Each M independently represents a hydrogen atom, a metal ion, or an ammonium ion; each m independently represents an integer of 0 to 2; and s is 0 or 1. In formula (2), * indicates a bonding position in X and / or Y in formula (1), Z is selected from the group consisting of an optionally substituted phenyl group, an optionally substituted naphthyl group, an optionally substituted stilbene group, an optionally substituted benzoyl group, and an optionally substituted heterocyclic group, and t represents an integer of 0 or 1).

2. The polarized light-emitting element according to claim 1, wherein at least one of X, Y in the formula (1), and Z in the formula (2) when at least one of X and Y is represented by the formula (2) is selected from the group consisting of substituents represented by the following formulas (3) to (7): 【Chemistry 2】 (In the above formula (3) and formula (4), each A is independently selected from the group consisting of a hydrogen atom, a halogen group, a nitro group, a hydroxy group, a C1-4 alkyl group, a C1-4 alkoxy group, a C1-4 alkyl group having a sulfo group, a C1-4 alkyl group having a hydroxy group, a C1-4 alkyl group having a carboxy group, a C1-4 alkoxy group having a sulfo group, a C1-4 alkoxy group having a hydroxy group, and a C1-4 alkoxy group having a carboxy group; q 1 represents an integer of 0 to 4, M in the above formulas (3) to (7) is as defined in the above formula (1), and n 1 and n 2 each independently represents an integer of 0 to 3, and * in the above formulas (3) to (7) represents the bonding position of X or Y in the above formula (1), or the bonding position of Z in the above formula (2).

3. The polarized light-emitting element according to claim 2, wherein X and Y in the formula (1) are each independently selected from the group consisting of substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of substituents represented by formulas (3) to (7).

4. The polarized light-emitting element according to claim 2, wherein X and Y in the above formula (1) are both selected from the group consisting of the substituents represented by formulas (2) to (7), and when formula (2) is selected, Z is selected from the group consisting of the substituents represented by formulas (3) to (7).

5. 5. The polarized light-emitting device according to claim 1, wherein each m in the formula (1) is 0.

6. 6. The polarized light-emitting element according to claim 1, wherein s is 0.

7. 6. The polarized light-emitting element according to claim 1, wherein s is 1.

8. 8. The polarized light emitting device according to claim 7, wherein the formula (1) is represented by the following formula (1'): 【Chemistry 3】 (In the above formula (1'), X and Y are as defined in the above formula (1)).

9. 9. The polarized light emitting device according to claim 1, further comprising at least one organic dye or fluorescent dye other than the luminescent compound or the salt thereof.

10. The polarized light-emitting device according to any one of claims 1 to 9, further comprising a substrate.

11. The polarized light-emitting element according to claim 10, wherein the substrate is a film containing a polyvinyl alcohol resin or a derivative thereof.

12. 12. A polarized light-emitting plate comprising the polarized light-emitting element according to claim 1 and a transparent protective film on at least one surface of the polarized light-emitting element.

13. A display device comprising the polarized light emitting element according to any one of claims 1 to 11 or the polarized light emitting plate according to claim 12.

Citation Information

Patent Citations

  • Photographic silver-dye-bleach material

    GB1254214A

  • Material for anisotropic film

    JP2008033275A

  • Polarizing light emitting element and polarizing element

    JP2008224854A

  • Circularly-polarized emission rare earth complex

    JP2013121921A