Developing roller and image forming apparatus
The developing roller's coating layer composition with specific nitrogen content and elastic design addresses filming and fogging issues, enhancing image quality and durability under high humidity conditions.
Patent Information
- Application Number
- JP2021104459
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-23
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-06-23
AI Technical Summary
Conventional developing rollers face issues with filming and fogging under high temperature and high humidity conditions, leading to decreased image quality and durability, especially at high speeds and over long periods.
A developing roller design featuring a coating layer made of a resin containing carbon, nitrogen, and silicon, with a nitrogen content between 4 and 15 atomic%, combined with an elastic layer and intermediate layer, enhances flexibility and toner transportability, reducing filming and fogging.
The design improves image quality and durability by preventing filming and fogging under high humidity conditions, ensuring high-quality images over time.
Smart Images

Figure 0007557432000004 
Figure 0007557432000005 
Figure 0007557432000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a developing roller and an image forming apparatus. [Background technology]
[0002] The developing rollers used in electrophotographic image forming apparatuses such as copying machines, printers, and facsimiles have the function of applying a uniform triboelectric charge to the toner and transporting a predetermined amount of toner stably to the development area. In the process of responding to the recent demands for faster operation, longer life, and higher image quality in electrophotographic devices, the performance of the toner has improved, and therefore studies are being conducted on improving the developer transport performance of the developing roller by adjusting the electrical properties of various materials constituting the developing roller.
[0003] For example, Patent Documents 1 and 2 propose a semiconductive roll having excellent electrostatic properties, in which a silane coupling agent is laminated and coated on the outermost layer of a urethane resin film, thereby achieving both excellent durability, flexibility, and a low coefficient of friction.
[0004] When a developing roller is used for a long period of time, the developer may adhere to the surface of the developing roller (hereinafter, also referred to as "filming"). Filming is thought to occur due to deformation or destruction of the developer caused by sliding stress between the developing roller and the contacting object that is in pressure contact with the developing roller when the developer is charged or adhered, and further due to melting of the developer caused by frictional heat with a blade or the like. For these reasons, there is a demand for a developing roller that minimizes the occurrence of filming and has stable durable printing performance.
[0005] Furthermore, in image forming apparatuses that employ electrophotography, when a large amount of images are output from the beginning, the apparatus may be subjected to high temperature and humidity conditions, resulting in insufficient charging and image defects (hereinafter also referred to as "fogging") in which developer is developed into the white areas of the image. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-318249 [Patent Document 2] JP 2003-98782 A Summary of the Invention [Problem to be solved by the invention]
[0007] Although the conventional technology described in the above patent document has the effect of controlling the contact charge amount, in the recent situation where high speed and high durability are required, it is required to prevent filming and further improve fogging under high temperature and high humidity. In addition, the outermost coating of the conventional developing roller is hard, and there is a concern that it may crack when used at high speed and for a long time. Such a defect leads to a deterioration of image quality. The present invention has been made in consideration of the above circumstances, and has an object to provide a developing roller that is improved in terms of filming and fogging under high humidity conditions and that can produce high-quality images, and an image forming apparatus equipped with such a developing roller. [Means for solving the problem]
[0008] The coating layer, which is the outermost layer of the developing roller, is required to be flexible and have toner transport properties and properties against fogging and filming. The present inventors have found that by forming the coating layer of the developing roller with a multifunctional silane coupling agent and setting the nitrogen content within a certain range, filming and fogging under high humidity conditions can be improved and high quality images can be obtained, and have arrived at the present invention. That is, the present invention is a developing roller comprising a shaft body, an elastic layer provided on the outside of the shaft body, an intermediate layer provided on the outside of the elastic layer, and a coating layer provided on the outside of the intermediate layer, wherein the coating layer is made of a resin containing a polymeric compound containing at least carbon, nitrogen, oxygen, and silicon, and the nitrogen atom content on the surface of the coating layer is greater than 4 atomic % and less than 15 atomic %.
[0009] The intermediate layer is preferably a urethane elastic layer.
[0010] It is preferable that the resin constituting the coating layer is a resin based on a polyfunctional silane coupling agent, and is impregnated into the urethane elastic layer, so that the coating layer and the urethane elastic layer are in close contact with each other.
[0011] The surface roughness Rz of the developing roller is preferably 2 μm or more and 15 μm or less.
[0012] The resistance of the developing roller is 1 x 10 6 Ω or more 9×10 9 It is preferably Ω or less.
[0013] The elastic layer of the developing roller is preferably made of silicone rubber.
[0014] The image forming apparatus of the present invention is provided with the developing roller of the present invention. Effect of the Invention
[0015] According to the present invention, it is possible to provide a developing roller which is improved in terms of filming and fogging under high humidity conditions and which can provide high quality images, and an image forming apparatus equipped with the developing roller. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a perspective view illustrating an embodiment of a developing roller of the present invention. [Diagram 2] 1 is a cross-sectional view illustrating an embodiment of a developing roller of the present invention. [Diagram 3] 1 is a schematic cross-sectional view illustrating an embodiment of an image forming apparatus of the present invention. [Figure 4] FIG. 4 is a front view showing an apparatus for measuring the surface resistance of a developing roller. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. [Developing roller] 1, the developing roller 1 of the present invention includes a shaft 2, an elastic layer 3 provided on the outside of the shaft 2, an intermediate layer 4 provided on the outside of the elastic layer 3, and a coating layer 5 provided on the outside of the intermediate layer 4. The coating layer 5 is made of a resin containing a polymer compound containing at least carbon, nitrogen, oxygen, and silicon, and the nitrogen atom content of the surface of the coating layer 5 is more than 4 atomic % and not more than 15 atomic %. Each component will be described in detail below.
[0018] (Shaft body) The shaft 2 may preferably be a shaft having conductive properties and used in a conventionally known developing roller. The shaft 2 is preferably made of at least one metal selected from the group consisting of iron, aluminum, stainless steel, and brass. Such a shaft 2 is also generally known as a "core metal."
[0019] The shaft body 2 may contain an insulating resin. The insulating resin may be, for example, a thermoplastic resin or a thermosetting resin. The shaft body 2 may include, for example, a core body made of an insulating resin and a plating layer provided on the core body. Such a shaft body 2 can be obtained, for example, by plating a core body made of an insulating resin to make it conductive. The shaft body 2 is preferably a core bar in order to obtain good electrical conductivity.
[0020] The shape of the shaft body 2 is preferably, for example, rod-like, tubular, etc. The cross-sectional shape of the shaft body 2 may be, for example, circular, elliptical, or non-circular, such as polygonal. The outer peripheral surface of the shaft body 2 may be subjected to treatment such as cleaning treatment, degreasing treatment, and primer treatment.
[0021] The axial length of the shaft body 2 is not particularly limited, and may be adjusted as appropriate depending on the type of the image forming apparatus in which it is installed. The diameter (diameter of the circumscribing circle) of the shaft body 2 is also not particularly limited, and may be adjusted as appropriate depending on the type of the image forming apparatus in which it is installed.
[0022] (Elastic layer) The elastic layer 3 is provided to impart to the developing roller 1 hardness and elasticity that enables it to be pressed against the photosensitive member with an appropriate nip width and nip pressure so that the toner can be supplied to the electrostatic latent image formed on the surface of the photosensitive member without excess or deficiency. Various rubber materials can be used for the elastic layer 3. Examples of rubbers used for the rubber material include ethylene-propylene-diene copolymer rubber (EPDM), acrylonitrile-butadiene rubber (NBR), chloroprene rubber (CR), natural rubber (NR), isoprene rubber (IR), styrene-butadiene rubber (SBR), fluororubber, silicone rubber, epichlorohydrin rubber, NBR hydride, and urethane rubber. These can be used alone or in combination of two or more. Among these, silicone rubber is preferable from the viewpoint of reducing damage to the toner and compressive stress distortion due to pressing. Examples of silicone rubber include polydimethylsiloxane, polymethyltrifluoropropylsiloxane, polymethylvinylsiloxane, polyphenylvinylsiloxane, and copolymers of these siloxanes.
[0023] The rubber composition for forming the elastic layer may contain various additives, such as an auxiliary such as a conductivity imparting agent, a chain extender, and a crosslinking agent, a catalyst such as an addition reaction catalyst, a reaction control agent, a dispersant, an antiaging agent, an antioxidant, a filler, a pigment, a colorant, a processing aid, a softener, a plasticizer, an emulsifier, a heat resistance improver, a flame retardant improver, an acid acceptor, a thermal conductivity improver, a release agent, and a solvent.
[0024] When forming the elastic layer 3 made of silicone rubber, it may be formed by a liquid silicone rubber composition using a LIMS (Liquid Injection Molding System) method, or it may be formed by injection molding using a millable silicone rubber composition. When a millable silicone rubber composition is used, it is preferable that the surface of the elastic layer is polished.
[0025] The elastic layer 3 is preferably a solid layer, and preferably has no hollow space inside the layer. In this specification, "solid" means that the layer has a hollow space of 0.1 mm or less inside. 2 This means that the material does not have more than one hollow space.
[0026] The JIS A hardness (JIS K 6301) of the elastic layer 3 is preferably 20 or more and 55 or less. When the JIS A hardness of the elastic layer 3 is within the above range, the contact area (nip width) between the developing roller 1 and the contacted body (for example, an image carrier such as a photoconductor) becomes large, which tends to further improve the performance such as transfer efficiency, charging efficiency, and development efficiency. In addition, the possibility of mechanically damaging the contacted body is reduced.
[0027] The thickness of the elastic layer 3 is preferably 0.5 mm to 10 mm, more preferably 1 mm to 5 mm, from the viewpoint of ensuring a uniform nip width with the contacted body when in contact with the contacted body. In the present invention, the "thickness" refers to the thickness in the direction perpendicular to the axial direction of the developing roller 1. The outer diameter of the elastic layer 3 is not particularly limited. The outer diameter may be, for example, 5 mm or more and 20 mm or less. In this specification, the "outer diameter" refers to the outer diameter in a cross section perpendicular to the axial direction of the developing roller 1. The thickness and outer diameter of the elastic layer 3 can be adjusted by methods such as adjusting the amount of rubber composition used when forming the elastic layer 3, or polishing or grinding the outer peripheral surface of the elastic layer 3 after forming the elastic layer 3.
[0028] The outer peripheral surface of the elastic layer 3 may be subjected to a surface treatment such as a primer treatment, a corona treatment, a plasma treatment, an excimer treatment, a UV treatment, an ITO treatment, or a frame treatment.
[0029] (Middle class) The developing roller 1 of the present invention includes an intermediate layer 4 on the outside of the elastic layer 3. The intermediate layer 4 has the purpose of protecting the surface of the elastic layer 3 and adjusting the surface characteristics of the developing roller 1, i.e., the resistance value, toner transportability, antistatic properties, etc.
[0030] The intermediate layer 4 is preferably a urethane elastic layer from the viewpoint of adhesion to the covering layer 5. The urethane elastic layer has a urethane bond formed by a polyol and an isocyanate as a constituent unit. The polyol component is not particularly limited, but polyether polyol, polyester polyol, polycarbonate polyol, polybutadiene polyol, polyisoprene polyol, acrylic polyol, silicone modified polyol, and fluorine modified polyol can be used. The isocyanate compound to be reacted with these polyol components is not particularly limited, but examples of the isocyanate compound that can be used include aliphatic polyisocyanates such as ethylene diisocyanate and 1,6-hexamethylene diisocyanate (HDI), alicyclic polyisocyanates such as isophorone diisocyanate (IPDI), cyclohexane 1,3-diisocyanate and cyclohexane 1,4-diisocyanate, aromatic isocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI), and copolymers or blocks thereof.
[0031] -Conductive agent- The intermediate layer 4 may contain a conductive agent such as an electronic conductive material or an ionic conductive material to adjust the surface resistance of the developing roller 1. Examples of electronic conductive materials include conductive carbon such as Ketjen Black EC and acetylene black, rubber carbon such as SAF, ISAF, HAF, FEF, GPF, SRF, FT, and MT, color (ink) carbon that has been subjected to oxidation treatment, and metals such as copper, silver, and germanium, as well as their metal oxides. Among these, carbon black (conductive carbon, rubber carbon, and color (ink) carbon) is preferred because it is easy to control the conductivity with a small amount. Examples of ionic conductive materials include inorganic ionic conductive materials such as sodium perchlorate, lithium perchlorate, calcium perchlorate, lithium chloride, lithium bisimide, and potassium bisimide, and organic ionic conductive materials such as modified aliphatic dimethylammonium ethosulfate and stearyl ammonium acetate.
[0032] -Roughness agent- The intermediate layer 4 preferably contains a roughening agent in order to adjust the surface roughness of the developing roller 1. Examples of the roughening agent include inorganic particles such as silica (including surface-treated silica), metal oxides, organometallic compound particles, acrylic particles, urethane particles, nylon particles, acrylonitrile particles, styrene particles, silicone particles, silicone rubber particles, and benzoguanamine particles. The intermediate layer 4 may contain only one type of roughening agent, or two or more types.
[0033] The size of the roughening agent is preferably an average particle diameter of 2 μm or more and 15 μm or less. By setting the average particle diameter of the roughening agent within the above range, it is possible to set the surface roughness Rz of the developing roller 1 to 2 μm or more and 15 μm or less, as described below. By setting the surface roughness of the developing roller 1 within the above range, the surface roughness is appropriately maintained, and the developer transportability is kept good, while the resolution is maintained at a high level, and deterioration of image quality can be prevented. Note that when the average particle is about 2 μm, it is preferable to coat after confirming that the agent is easily aggregated and not completely dispersed. The average particle size (secondary particles) of the roughness agent can be measured using a particle size distribution analyzer (manufactured by Beckman Coulter).
[0034] The roughness agent used in the present invention preferably has heat resistance such that it does not deform or melt even at temperatures of 100° C. or higher, and more preferably has heat resistance at temperatures from 130° C. to 180° C. This makes it possible to prevent the roughness agent from deforming even at the crosslinking temperature of the intermediate layer 4. The heat resistance of the roughness agent can be evaluated by applying pressure and heat in a melt flow indexer to confirm that the roughness agent does not melt and flow out.
[0035] The roughness agent may be present (embedded) in the intermediate layer 4, may be dispersed unevenly in the intermediate layer 4, or may be unevenly distributed on the surface side of the intermediate layer 4.
[0036] The content of the roughening agent is preferably 1 part by mass or more and 40 parts by mass or less, and more preferably 3 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the composition for forming the intermediate layer. By setting the amount of the roughening agent used within the above range, the surface roughness of the developing roller 1 is appropriately maintained, and the developer transportability is kept good, while the resolution is maintained at a high level, and deterioration of the image quality can be prevented.
[0037] The thickness of the intermediate layer 4 is preferably 5 μm or more and 13 μm or less, and more preferably 6 μm or more and 11 μm or less.
[0038] To prevent siloxane from bleeding, a plasma coat of HMDSO (hexamethyldisiloxane) may be provided on the surface of the intermediate layer 4. The plasma coat of hexamethylsiloxane is a coat of hexamethyldisiloxane and plasma at the same time, which prevents siloxane from bleeding and also serves as a primer layer.
[0039] (covering layer) The coating layer 5 is composed of a resin containing a polymeric compound containing at least carbon, nitrogen, oxygen, and silicon. In particular, a compound having a structure containing a siloxane bond is preferable. By the coating layer 5 being composed of a resin containing a polymeric compound containing at least carbon, nitrogen, oxygen, and silicon, the adhesive force of the surface can be reduced, which results in the effect of suppressing filming. Note that it is preferable that the coating layer 5 does not contain fluorine atoms, since the potential is lowered in terms of the triboelectric series of the toner particles and the triboelectric charge.
[0040] The resin constituting the coating layer 5 is preferably a resin based on a polyfunctional silane coupling agent. "Based on" means that the coating layer 5 contains at least 80% polyfunctional silane coupling agent. Since the polyfunctional silane coupling agent has film-forming properties by itself, the coating layer 5 may be entirely composed of the polyfunctional silane coupling agent, but may also contain other additives. By using a polyfunctional silane coupling agent, the coating layer 5 has good film-forming properties by itself and can impart flexibility to the surface of the developing roller, so that the occurrence of cracks is suppressed, durability is ensured, and image quality is not deteriorated. In addition, when the polyfunctional silane coupling agent is applied and dried, condensation of alkoxysilane occurs, and since the film has siloxane bonds, the toner adhesion is small, so filming is suppressed. Furthermore, the polyfunctional silane coupling agent does not have functional groups that absorb moisture through reaction, so fogging can be effectively prevented. Furthermore, the polyfunctional silane coupling agent containing nitrogen also reacts with nitrogen compounds at the same time as condensation of alkoxysilane, and the proportion of nitrogen element increases, so the charging property is improved against negatively charged toner, and fogging is improved under high temperature and high humidity conditions.
[0041] Examples of the polyfunctional silane coupling agent include an amine-based silane coupling agent, a mercapto-based silane coupling agent, an isocyanate-based silane coupling agent, an epoxy-based silane coupling agent, and an acrylic-based silane coupling agent. An example of the amino-based silane coupling agent is X-12-972F (product name, manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of the isocyanate-based silane coupling agent include X-12-1234 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), X-12-1159L (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), X-12-1242 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), X-12-1248 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), and X-24-9750A (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of mercapto-based silane coupling agents include X-12-1154 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), X-12-1156 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), X-41-1805 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), and X-41-1810 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.). An example of the epoxy-based silane coupling agent is X-12-981S (product name, manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of the acrylic silane coupling agent include X-12-1048 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.) and X-12-1050 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.). Among the above, isocyanate-based polyfunctional silane coupling agents are preferred because of their flexibility. The polyfunctional silane coupling agents may be used alone or in combination of several kinds.
[0042] The polyfunctional silane coupling agent in the coating layer 5 is partially impregnated into the underlying intermediate layer 4, improving the adhesion between the intermediate layer 4 and the coating layer 5. In particular, when the intermediate layer 4 is a urethane elastic layer, the adhesion between the coating layer 5 and the intermediate layer 4 is better.
[0043] -Nitrogen atom content- The nitrogen atom content in the surface of the coating layer 5 is greater than 4 atomic % and equal to or less than 15 atomic %. When the nitrogen atom content in the surface of the coating layer 5 is 4 atomic % or more, triboelectric charging with respect to negative toner is improved, and fogging can be prevented. Furthermore, when the nitrogen atom content in the surface of the coating layer 5 is 15 atomic % or less, excessive charging can be prevented, and roughness in the image can be prevented. Furthermore, the nitrogen atom content in the surface of the coating layer 5 is more preferably equal to or more than 5 atomic % and equal to or less than 10 atomic %. The nitrogen atom content is a value measured by X-ray photoelectron spectroscopy (XPS), specifically as described in the Examples below.
[0044] The thickness of the coating layer 5 is preferably 0.1 μm or more and 3 μm or less, and more preferably 0.2 μm or more and 1.5 μm or less.
[0045] [Physical properties of developing roller] The developing roller 1 of the present invention has the following physical properties. (Resistance of the developing roller) The resistance of developing roller 1 is 1×10 6 Ω or more 9×10 9 It is preferable that the resistance value of the developing roller 1 is 1×10 6 By setting the resistance to 9×10 Ω or more, leakage can be prevented. 9 By keeping the resistance Ω or less, it is possible to prevent the image from becoming rough. The resistance value of the developing roller 1 is 9×10 9 If necessary, the resistance can be adjusted to 1×10 or less by selecting an ionic conductive material such as sodium perchlorate, lithium perchlorate, calcium perchlorate, lithium chloride, lithium bisimide, or potassium bisimide; an ionic liquid such as a pyridinium-based, imidazole-based, or quaternary ammonium-based; or an electronic conductive material such as carbon, carbon nanotubes, metals, metal oxides, or organic conductive materials. 6 Ω or more 1×10E9 It is possible to adjust it to Ω or less. However, the resistance value of the electronic conduction by carbon basically varies depending on the dispersion conditions and is in a range that is difficult to adjust, so it is preferable to use an ionic conductive mechanism. The resistance of developing roller 1 is 1 x 10 6 For resistances above 9×10 Ω, it is easy to adjust the resistance value using ionic conductive materials. 9 At Ω or less, the occurrence of fog can be effectively prevented. The resistance value of the developing roller 1 is measured by the measuring method in the examples described later.
[0046] (Surface roughness Rz) The surface roughness Rz of the developing roller 1 is preferably 2 μm or more and 15 μm or less, and more preferably 2 μm or more and 10 μm or less. By making the surface roughness Rz 2 μm or more, the minimum amount of toner transport can be ensured. Also, by making the surface roughness Rz 15 μm or less, the maximum amount of toner transport can be ensured. The surface roughness Rz of the developing roller 1 can be adjusted by selecting the size of the roughness agent contained in the intermediate layer 4, as described above. Here, the surface roughness Rz is a value determined using a contact type roughness meter based on the ten-point average roughness specified in JIS B0601:1994.
[0047] The developing roller 1 of the present invention has a coating layer 5 made of a resin containing a polymer compound containing at least carbon, nitrogen, oxygen, and silicon, which can solve the problems of filming and fogging under high temperature and high humidity conditions and provide high quality images. Furthermore, the outermost coating can be softened, preventing cracks from occurring due to high speed and long-term use.
[0048] [Developing device and image forming device] The developing roller 1 of the present invention can be suitably used as a developer carrier in a developing device and an image forming apparatus. In this embodiment, the configuration of the image forming apparatus other than the developing roller 1 is not particularly limited. An example of a developing device and an image forming apparatus 10 including the developing roller 1 of the present invention will be described with reference to FIG.
[0049] The image forming apparatus 10 is a tandem type color image forming apparatus in which a plurality of image carriers 11B, 11C, 11M, and 11Y equipped in developing units B, C, M, and Y of each color (black, cyan, magenta, and yellow) are arranged in series on a transfer transport belt 6, and the developing units B, C, M, and Y are arranged in series on the transfer transport belt 6. The developing unit B includes an image carrier 11B, for example a photosensitive member (also called a photosensitive drum), charging means 12B, for example a charging roller, exposure means 13B, a developing device 20B, transfer means 14B, for example a transfer roller, which contacts the image carrier 11B via the transfer transport belt 6, and cleaning means 15B.
[0050] The developing device 20B is an example of the developing device of the present invention, and includes the developing roller 1 and developer 22B of the present invention as shown in FIG. 3. Therefore, in this image forming apparatus 10, the developing roller 1 is mounted as developer carriers 23B, 23C, 23M, and 23Y. Specifically, the developing device 20B includes a housing 21B that contains one-component non-magnetic developer 22B, a developer carrier 23B that supplies the developer 22B to the image carrier 11B, a toner supply roller 25B that supplies the developer 22B to the developer carrier 23B, and a developer amount adjustment means 24B, such as a blade, that adjusts the thickness of the developer 22B. In the developing device 20B, the developer amount adjustment means 24B is in contact or pressure contact with the outer peripheral surface of the developer carrier 23B as shown in FIG. 3. That is, the developing device 20B is a "contact type developing device." The developing units C, M and Y are basically configured in the same manner as the developing unit B, and the same elements are given the same reference numerals and the symbols C, M or Y indicating each unit, and the description thereof will be omitted.
[0051] In image forming apparatus 10, developer carrier 23B of developing device 20B is arranged so that its surface is in contact or pressure contact with the surface of image carrier 11B. Similarly to developing device 20B, developing devices 20C, 20M, and 20Y are also arranged so that their surfaces, developer carriers 23C, 23M, and 23Y, are in contact or pressure contact with the surfaces of image carriers 11C, 11M, and 11Y. In other words, this image forming apparatus 10 is a "contact type image forming apparatus."
[0052] The fixing means 30 is disposed downstream of the developing unit Y. The fixing means 30 is a pressure heat fixing device that includes a fixing roller 31, an endless belt support roller 33 disposed near the fixing roller 31, an endless belt 36 wound around the fixing roller 31 and the endless belt support roller 33, and a pressure roller 32 disposed opposite the fixing roller 31, all of which are disposed in a housing 34 having an opening 35 through which the recording medium 16 passes, and is supported rotatably so that the fixing roller 31 and the pressure roller 32 come into contact with or are in pressure contact with each other via the endless belt 36. A cassette 41 that contains the recording medium 16 is disposed at the bottom of the image forming apparatus 10. The transfer and transport belt 6 is wound around a plurality of support rollers 42.
[0053] The developers 22B, 22C, 22M and 22Y used in the image forming apparatus 10 may be either dry or wet developers, and may be either non-magnetic or magnetic developers, so long as they are capable of being charged by friction. The housings 21B, 21C, 21M and 21Y of the developing units B, C, M and Y respectively contain one-component non-magnetic black developer 22B, cyan developer 22C, magenta developer 22M and yellow developer 22Y.
[0054] The image forming apparatus 10 forms a color image on the recording medium 16 as follows. First, in the developing unit B, an electrostatic latent image is formed by the exposure means 13B on the surface of the image carrier 11B charged by the charging means 12B, and a black electrostatic latent image is developed by the developer 22B supplied by the developer carrier 23B. Then, when the recording medium 16 passes between the transfer means 14B and the image carrier 11B, the black electrostatic latent image is transferred to the surface of the recording medium 16. Next, in the same manner as in the developing unit B, a cyan image, a magenta image, and a yellow image are superimposed on the recording medium 16, on which the electrostatic latent image has been visualized as a black image, by the developing units C, M, and Y, respectively, to visualize a color image. Next, the color image of the recording medium 16 on which the color image has been visualized is fixed to the recording medium 16 as a permanent image by the fixing means 30. In this manner, a color image can be formed on the recording medium 16.
[0055] The developing device 20B is equipped with a developing roller 1, and is excellent in developer transportability and suppresses the occurrence of toner filming, which contributes to forming high-density, high-quality images for a long period of time. Also, an image forming apparatus equipped with this developing device 20B can form high-density, high-quality images for a long period of time.
[0056] The developing device and image forming apparatus of the present invention are not limited to those described above, and various modifications are possible within the scope of the present invention.
[0057] In this invention, the image forming apparatus 10 is not limited to an electrophotographic type, and may be, for example, an electrostatic type image forming apparatus. In addition, the image forming apparatus 10 in which the developing roller 1 of the present invention is arranged is not limited to a tandem type color image forming apparatus in which a plurality of image carriers each having a developing unit of each color are arranged in series on a transfer conveyor belt, and may be, for example, a monochrome image forming apparatus having a single developing unit, or a four-cycle type color image forming apparatus in which a developer image carried on an image carrier is sequentially and repeatedly transferred to an endless belt. In addition, the developer used in the image forming apparatus is a one-component non-magnetic developer, but in this invention, it may be a one-component magnetic developer, a two-component non-magnetic developer, or a two-component magnetic developer.
[0058] The image forming apparatus is a contact type image forming apparatus in which the surface of the developing roller is placed in contact or pressure contact with the surface of the image carrier. The image forming apparatus of the present invention may be a non-contact type image forming apparatus.
[0059] Since the image forming apparatus 10 of the present invention is equipped with the developing roller 1 of the present invention, the occurrence of fogging under high temperature and high humidity conditions is suppressed, and high quality images can be provided.
[0060] Although the present invention has been described above using the embodiments, it goes without saying that the technical scope of the present invention is not limited to the scope of the invention described in the above embodiments, and it is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. Furthermore, it is clear from the description of the claims that inventions with such modifications or improvements can also be included in the technical scope of the present invention. EXAMPLES
[0061] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below.
[0062] [Example 1] The developing roller was produced according to the following procedure. (Formation of primer layer) The electroless nickel-plated shaft (made of SUM22, diameter 10 mm, length 274.2 mm) was washed with ethanol, and its surface was coated with a silicone primer (product name "Primer No. 16", made by Shin-Etsu Chemical Co., Ltd.). The primer-treated shaft was baked in a gear oven at 150°C for 10 minutes and then cooled at room temperature for 30 minutes or more to form a primer layer on the outer circumferential surface of the shaft.
[0063] (Formation of elastic layer) An elastic body made of a rubber material was molded on the outer circumferential surface of a shaft by extrusion molding using a millable type rubber composition containing silicone rubber (composition containing conductive carbon). In the extrusion molding, the millable type silicone rubber composition was heated at 270°C for 5 minutes using an infrared heating furnace (IR furnace), and further heated at 200°C for 4 hours using a gear oven to harden it. As a result, an elastic layer made of a hardened product of the rubber composition was formed on the outer circumferential surface of the shaft treated with a primer. The elastic layer was a solid layer and had a thickness of 3 mm.
[0064] (Formation of intermediate layer (urethane elastic layer)) Next, the outer peripheral surface of the elastic layer was UV-treated. After that, a primer (KBP-40, manufactured by Shin-Etsu Chemical) was applied onto the UV-treated elastic layer, and then the following urethane elastic layer composition was applied by spraying. The urethane elastic layer is provided to adjust the resistance and surface roughness of the developing roller. -Composition for forming elastic urethane layer- Polyester polyol 28 parts by weight Isocyanate 14 parts by weight Carbon 3 parts by weight Ion conductive material (EF-112N, manufactured by Mitsubishi Electronics Materials) 0.1 parts by mass Urethane particles (average particle diameter φ7μm) 10 parts by mass Thinner 130 parts by weight
[0065] The applied elastic urethane layer-forming composition was heated at 160° C. for 30 minutes and then cooled.
[0066] (Formation of coating layer) Next, the following composition for forming a covering layer was prepared, and the composition for forming a covering layer was applied to the outer periphery of the urethane elastic layer by a spray method, and then dried at 150° C. for 10 minutes and allowed to stand for one day to obtain a developing roller. The coating layer had a thickness of 0.5 μm after drying. -Composition for forming coating layer- Multifunctional silane coupling agent (X-12-1159L, Shin-Etsu Chemical Co., Ltd.) 10 parts by mass Butyl acetate 100 parts by mass
[0067] [Example 2] A developing roller was prepared in the same manner as in Example 1, except that a mixture of 8 parts by mass of a multifunctional silane coupling agent (X-12-1159L) and 2 parts by mass of a silane coupling agent (KBE-9007N, manufactured by Shin-Etsu Chemical Co., Ltd.) was used.
[0068] [Example 3] A developing roller was produced in the same manner as in Example 1, except that the surface of the urethane elastic layer was plasma-coated with HMDSO (hexamethyldisiloxane), and the surface was coated with a polyfunctional silane coupling agent.
[0069] [Comparative Example 1] The preparation was carried out in the same manner as in Example 1, except that the multifunctional silane coupling agent was changed to aminosilane (KBE-902, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0070] [Physical Properties] The resistivity, surface roughness Rz, and nitrogen atom content were measured for the above-mentioned examples and comparative examples.
[0071] (Resistance of the surface of the developing roller) The surface resistance of the developing rollers of the above-mentioned Examples and Comparative Examples was measured using a measuring device shown in FIG. As shown in FIG. 4, the developing roller 1 was placed on a gold-plated plate 51, and weights 52 weighing 500 g were attached to both ends. The resistance value between the shaft 53 and the gold-plated plate 51 was measured with an ultra-high resistance / microammeter "5450" (manufactured by ADC Corporation) 54 at an applied voltage of 100 V.
[0072] (Surface roughness Rz) The surface roughness Rz was determined by measuring the ten-point average roughness using a contact surface roughness measuring instrument Surfcom 1400G (manufactured by Tokyo Seimitsu) in accordance with JIS B 0601:1994, and this was taken as the surface roughness Rz.
[0073] (Nitrogen atom content of coating layer) The nitrogen atom content on the surface of the coating layer was measured by cutting out a sample of a measurable size after forming the coating layer, and measuring the nitrogen atom content of the sample at a depth of 1 to 10 nm from the surface of the coating layer using ESCA (Electron Spectroscopy for Chemical Analysis, product name "ESCA-1000", manufactured by Shimadzu Corporation) under the following measurement conditions. X-ray gun acceleration voltage: 10 kV X-ray gun emission current: 20mA X-ray diameter: 1mmφ
[0074] [evaluation] The printing performance of the above-mentioned Examples and Comparative Examples was evaluated.
[0075] (Fogging evaluation under high temperature and humidity conditions) The developing rollers of the above-mentioned Examples and Comparative Examples were mounted on a magenta cartridge in a color image forming apparatus (product name "C610dn2", manufactured by Oki Data Corporation), and fogging was evaluated under high temperature and high humidity conditions of 27° C. and 80% RH. 4000 sheets were printed at 0.3% duty, the solid white printing was stopped instantly, tape was attached to the photosensitive drum, and the image was transferred onto a white paper. The tape was attached to a reference paper, and the color difference ΔE between the reference value and the transferred part was measured. The color difference ΔE was measured using a color difference meter (product name "CR-241", manufactured by Konica Minolta, Inc.). The color difference Δ after printing 4000 sheets was evaluated according to the following evaluation criteria: Fog evaluation under high temperature and high humidity conditions is acceptable if it is A or higher. A: ΔE is less than 1 B: ΔE is 1 to 2 C:2 or more
[0076] (Filming evaluation) The developing rollers of the above examples and comparative examples were attached to a magenta cartridge in a color image forming apparatus (product name "C610dn2", manufactured by OKI Data Corporation), and the filming state after printing 4,000 sheets under environmental conditions of 0.3% duty printing at 23°C and 55% RH was evaluated. After sucking the developer adhering to the surface of the developing roller, the mass transferred to the filming weight measuring jig was measured. The mass of the transferred developer was evaluated according to the following evaluation criteria. A filming evaluation of A is acceptable. A: 0.00 mg / cm 2 More than 0.03mg / cm 2 below B: 0.03 mg / cm 2 More than 0.06mg / cm 2 below C: 0.06 mg / cm 2 More
[0077] The evaluation results are shown in Table 1.
[0078] [Table 1]
[0079] As shown in Table 1, in Examples 1 to 3, in which the nitrogen atom content on the surface of the coating layer is greater than 4 atomic % and less than 15 atomic %, fogging and filming at high temperature and high humidity are suppressed compared to Comparative Example 1, in which the nitrogen atom content is less than 4 atomic %. [Explanation of symbols]
[0080] 1 Developing roller 2-axis body 3 Elastic layer 4. Middle Tier 5 Covering layer 6 Transfer conveyor belt 7 Second Surface Roughening Agent 8. First surface roughening agent 10 Image forming device 11B, 11C, 11M, 11Y Image carrier 12B, 12C, 12M, 12Y Charging means 13B, 13C, 13M, 13Y Exposure means 14B, 14C, 14M, 14Y Transfer means 15B, 15C, 15M, 15Y Cleaning means 16 Records 20B, 20C, 20M, 20Y developing device 21B, 21C, 21M, 21Y housing 22B, 22C, 22M, 22Y Developer 23B, 23C, 23M, 23Y Developer carriers 24B, 24C, 24M, 24Y Developer amount adjusting means 25B, 25C, 25M, 25Y Toner supply roller 30 Fixing Method 31 Fuser roller 32 Pressure roller 33 Endless belt support roller 34 Case 35 Opening 36 Endless Belt 41 Cassette 42 Support roller B, C, M, Y developing units 51 Gold Plated Sheet 52 Weight 53 Shaft 54 Ultra high resistance / micro current meter
Claims
1. a shaft body, an elastic layer provided on the outside of the shaft body, and an intermediate layer provided on the outside of the elastic layer; a coating layer provided on the outer side of the intermediate layer, the intermediate layer is a urethane elastic layer, the coating layer is made of a resin containing a polymer compound containing at least carbon, nitrogen, oxygen, and silicon, The content of nitrogen atoms on the surface of the coating layer is greater than 4 atomic % and less than 15 atomic %, the resin constituting the coating layer is a resin based on a polyfunctional silane coupling agent, and is impregnated into the urethane elastic layer; The developing roller has the coating layer and the urethane elastic layer in close contact with each other.
2. 2. The developing roller according to claim 1, wherein the surface roughness Rz of the surface of the developing roller is 2 [mu]m or more and 15 [mu]m or less.
3. The resistance of the developing roller is 1×10 6 Ω or more 9×10 9 3. The developing roller according to claim 1, wherein the surface roughness is Ω or less.
4. 4. The developing roller according to claim 1, wherein the elastic layer of the developing roller is made of silicone rubber.
5. 5. An image forming apparatus comprising the developing roller according to claim 1.
Citation Information
Patent Citations
Semi-conductive roll and developing device
JP1998318249A
Electrophotographic developing device
JP2000258990A
Semiconductive roll
JP2003098782A
Conductive roller
JP2007033665A
Conductive roller and image forming apparatus
JP2008070420A