Anti-glare film
The anti-glare film with a biaxially stretched base film and optimized anti-glare layer effectively suppresses rainbow unevenness and maintains mechanical strength at a lower cost by adhering to specific thickness-retardation and surface parameter criteria.
Patent Information
- Application Number
- JP2023193926
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-14
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2043-11-14
AI Technical Summary
Existing anti-glare films using biaxially stretched polyethylene terephthalate (PET) films suffer from rainbow unevenness due to retardation effects, and adjusting the degree of stretching in different directions to mitigate this issue increases production costs and reduces mechanical strength.
An anti-glare film with a biaxially stretched base film that satisfies a specific thickness-retardation relationship and an anti-glare layer with a fractal parameter Safc of 0.02 or more and Smr1 of 14% or more, scattering incident light to suppress rainbow unevenness while maintaining mechanical strength.
The film achieves sufficient mechanical strength and effective suppression of rainbow unevenness at a lower cost by optimizing the base film's thickness and anti-glare layer's surface characteristics.
Smart Images

Figure 0007557601000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an antiglare film that is attached to a display device, a polarizing plate, or the like. [Background technology]
[0002] Antiglare films are attached to various display devices and polarizing plates. For example, antiglare films scatter incident light from the outside and protect the surface on which the antiglare film is attached from the outside. Antiglare films include a base film and an antiglare layer disposed over the base film. The antiglare layer has a roughened surface on which fine irregularities are formed. Patent Document 1 describes an antiglare film that uses a biaxially stretched polyethylene terephthalate (hereinafter also referred to as PET) film as the base film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-156938 A [Patent Document 2] Patent No. 5051328 Summary of the Invention [Problem to be solved by the invention]
[0004] Anti-glare films using biaxially stretched films, such as the anti-glare film of Patent Document 1, have sufficient mechanical strength, but may cause unnecessary rainbow unevenness (also called color unevenness or interference unevenness) due to the influence of phase difference. Patent Document 2 describes a method of preventing rainbow unevenness by using a polyester film with enhanced anisotropy by differentiating the degree of stretching in each stretching direction. However, in this case, the mechanical strength of the anti-glare film is reduced due to the insufficient degree of stretching compared to normal biaxially stretched films. In addition, additional processing and equipment are required to adjust the degree of stretching in each stretching direction to be different, which increases production costs.
[0005] Therefore, an object of the present disclosure is to provide an antiglare film that has sufficient mechanical strength and can suppress rainbow unevenness at low cost. [Means for solving the problem]
[0006] An antiglare film according to one embodiment of the present disclosure comprises a substrate film which is a biaxially stretched film having in-plane birefringence and which satisfies the relationship shown in Formula 1, and an antiglare layer disposed on the substrate film, wherein the surface of the antiglare layer opposite to the substrate film has an uneven shape in which a fractal parameter Safc is a value in the range of 0.02 or more when a short wavelength cutoff value λs is set to 50 μm, and Smr1 is a value in the range of 14% or more when a long wavelength cutoff value λc is set to 25 μm and a short wavelength cutoff value λs is set to 2.6 μm. [Formula 1] Substrate film thickness D(m) × retardation Re(m) ≧ 1.0 × 10 -10 (m 2 ) Effect of the Invention
[0007] According to the above-described aspects of the present disclosure, an antiglare film that has sufficient mechanical strength and can suppress rainbow unevenness can be provided at low cost. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view of the display device according to the first embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of the surface of the antiglare layer of the antiglare film of FIG. [Diagram 3] FIG. 3 is an enlarged cross-sectional view of the surface of the antiglare layer of the antiglare film according to the second embodiment. [Figure 4] FIG. 4 is a partial cross-sectional view of an antiglare film having an antireflection layer of the first structure according to the third embodiment. [Diagram 5] FIG. 5 is a partial cross-sectional view of an antiglare film having an antireflection layer of the second structure according to the third embodiment. [Figure 6] FIG. 6 is a partial cross-sectional view of an antiglare film including an antireflection layer of a third structure according to the third embodiment. [Figure 7] FIG. 7 is a cross-sectional view of an optical member according to a fourth embodiment. [Figure 8] FIG. 8 is a cross-sectional view of a display device according to a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Through the study of the present inventors, it has been confirmed that, in an antiglare film, when the thickness D of the substrate film and the integrated value (D×Re) of the retardation Re are set to values in a range equal to or greater than a predetermined value, and the Safc value and the Smr1 value of the uneven shape on the surface of the antiglare layer opposite to the substrate film side are set to values in a predetermined range, respectively, by using a biaxially stretched film as the substrate film, it is possible to obtain an excellent antiglare effect and an anti-rainbow unevenness effect while maintaining sufficient mechanical strength of the antiglare film. The antiglare film of the present disclosure has been made based on such findings.
[0010] Hereinafter, each embodiment of the present disclosure will be described with reference to the drawings. The cutoff value referred to in this specification refers to a predetermined wavelength that is removed from a cross-sectional curve defined in accordance with JIS B 0601:2001. Also, glare refers to a phenomenon defined in JIS C 1006:2019.
[0011] (First embodiment) [Anti-glare film and display device] FIG. 1 is a cross-sectional view of a display device 1 according to a first embodiment. FIG. 2 is an enlarged cross-sectional view of a surface 4a of an anti-glare layer 4 of an anti-glare film 2 in FIG. 1. As shown in FIG. 1, the display device 1 includes a display element 16 and an anti-glare film 2. As an example, the anti-glare film 2 is attached to a display surface 16a of the display element 16. The anti-glare film 2 has multiple functions. The anti-glare film 2 scatters incident light incident on the display surface 16a to provide anti-glare. The anti-glare film 2 also protects the display surface 16a from the outside.
[0012] There is no limitation on the type of the display element 16. For example, the display element 16 includes displays such as a liquid crystal display (LCD), an organic electroluminescence display (OLED), an inorganic electroluminescence display, and a plasma display panel (PDP). Examples of the display device 1 include a personal computer (PC), a monitor, a television, and a smartphone.
[0013] The antiglare film 2 includes a base film 3, an antiglare layer 4, and an adhesive layer 5. The adhesive layer 5 contains a material that does not easily affect the optical properties of the antiglare film 2, such as an optical glue. Another layer may be disposed between the base film 3 and the antiglare layer 4. The base film 3 is disposed so as to cover the display surface 16a and supports the antiglare layer 4. The base film 3 of this embodiment covers the entire surface of the display surface 16a. The base film 3 is a biaxially stretched film that satisfies the relationship shown in the following formula 1 and has an in-plane birefringence. [Formula 1] Substrate film thickness D(m) × retardation Re(m) ≧ 1.0 × 10 -10 (m 2 )
[0014] The retardation Re refers to a birefringence phase difference. That is, the retardation Re is calculated by the following formula 2 based on the refractive index (nx) in the direction (slow axis direction) with the largest refractive index in the plane of the base film 3, the refractive index (ny) in the direction perpendicular to the slow axis direction (fast axis direction), and the thickness D of the base film 3. [Formula 2] Retardation Re(m) = (nx-ny) x substrate film thickness D(m)
[0015] As an example, the substrate film thickness D×retardation Re (hereinafter also referred to simply as “integrated value (D×Re)”) is 1.5×10 -10 (m 2 ) or more is preferable, and 2.0×10 -10 (m 2) or more is even more preferable. By setting the integrated value (D×Re) to a value equal to or greater than the lower limit value shown in formula 1, it is possible to prevent problems such as rainbow unevenness becoming too strong and being unable to be suppressed by the scattering of transmitted light due to the unevenness of the surface of the antiglare layer alone. The upper limit value of the integrated value (D×Re) is not particularly limited, but is preferably 6.0×10 -10 (m 2 ), 5.0×10 -10 (m 2 ), or 4.0×10 -10 (m 2 ) can be exemplified. In the case of the antiglare film 2, the integrated value is 1.0×10 -10 (m 2 ) or more, and as described later, the surface 4a of the antiglare layer 4 opposite to the base film 3 has an uneven shape in which the fractal parameter Safc is a value in the range of 0.02 or more when the short wavelength cutoff value λs is set to 50 μm, and Smr1 is a value in the range of 14% or more when the long wavelength cutoff value λc is set to 25 μm and the short wavelength cutoff value λs is set to 2.6 μm, so that rainbow unevenness can be appropriately suppressed. As an example, the base film 3 has a retardation Re in the range of 1000 nm or more and 4000 nm or less. The value of the retardation Re of the base film 3 is not limited to this.
[0016] The base film 3, which is a biaxially stretched film, is sufficiently stretched in the slow axis direction and the fast axis direction during production, unlike the film of Patent Document 2, for example. For this reason, for example, one of the two directions is less stretched than the other, so that damage such as cracks is less likely to occur in the base film 3 when an external force is applied. As a result, the base film 3 has good mechanical strength. Specifically, for example, the difference in breaking strength (MPa) between the slow axis direction and the fast axis direction of the base film 3 is suppressed to a value in the range of less than 30%. In addition, for example, the difference in breaking elongation (%) between the slow axis direction and the fast axis direction of the base film 3 is suppressed to a value in the range of less than 60%. The breaking strength and breaking elongation referred to here refer to values measured by a method conforming to JIS-C-2151:2019 and ASTM-D-882.
[0017] The antiglare layer 4 is disposed on the base film 3. As shown in FIG. 2, the surface 4a of the antiglare layer 4 opposite to the base film 3 has a predetermined uneven shape. As an example, the surface 4a of the antiglare layer 4 is exposed to the outside. The antiglare layer 4 imparts antiglare properties to the antiglare film 2 and scatters and reflects incident light from the outside to prevent unnecessary reflection on the display surface 16a. The antiglare layer 4 also functions as a hard coat (HC) layer that protects the display surface 16a. The surface 4a of the antiglare layer 4 has an uneven shape in which the fractal parameter Safc is a value in the range of 0.02 or more when the short wavelength cutoff value λs is set to 50 μm, and the Smr1 is a value in the range of 14% or more when the long wavelength cutoff value λc is set to 25 μm and the short wavelength cutoff value λs is set to 2.6 μm.
[0018] Here, Safc (areal fractal complexity) is a parameter described in item 4.4.9.5 of ISO25178-2:2012, the international standard for surface roughness. Safc is equal to -1000 times the slope of the approximation line when the relationship between specific surface area and scale is plotted on a double logarithmic graph, and is related to the fractal dimension. The larger Safc is (in other words, the steeper the slope of the approximation line is), the larger the fractal dimension is, and the more complex the surface shape is evaluated to be.
[0019] By setting the short wavelength cutoff value λs at 50 μm when measuring the Safc, for example, uneven shapes that do not affect the rainbow unevenness on the surface 4a of the antiglare layer 4 can be removed. Also, for example, the higher the value of Safc when the short wavelength cutoff value λs is set to 50 μm, the higher the self-similarity and finer the structure of the uneven shape on the surface 4a of the antiglare layer 4. This makes it easier to scatter transmitted light on the surface 4a of the antiglare layer 4 and suppress rainbow unevenness. The Safc is preferably, for example, in the range of 0.02 to 1.00, and more preferably in the range of 0.03 to 0.50. The upper limit of the Safc can be set appropriately. Also, for example, by setting the upper limit of the Safc to 1.00, even small characters displayed on the display surface 16a to which the antiglare film 2 is attached can be easily viewed.
[0020] Smr1 is a functional parameter described in ISO25178-2:2012. In a graph showing a load curve, the line with the smallest slope among the lines where the difference in the areal load ratio Smr value at two points at a certain height is 40% is defined as the equivalent line. When the height difference of this equivalent line at the areal load ratios of 0% and 100% is defined as the core part Sk, the areal load ratio (%) that separates the core part from the protruding peak parts that are equal to or higher than the height of the core part is defined as Smr1.
[0021] By setting the cutoff value λc of the long wavelength when measuring the Smr1 to 25 μm, for example, large uneven shapes that do not affect the rainbow unevenness on the surface 4a of the antiglare layer 4 can be removed. In addition, for example, the higher the value of Smr1 when the cutoff value λc of the long wavelength is set to 25 μm, the easier it is to scatter transmitted light on the surface 4a of the antiglare layer 4 and suppress the rainbow unevenness. For example, the Smr1 is preferably a value in the range of 14% to 50%, and more preferably a value in the range of 15% to 30%. The upper limit of the Smr1 can be appropriately set. For example, by setting the upper limit of the Smr1 to 50%, for example, the ratio of convex parts of the uneven shape on the surface 4a of the antiglare layer 4 can be suppressed, and the mechanical strength of the antiglare film 2 can be easily maintained.
[0022] According to the antiglare film 2 having the above-mentioned configuration, the uneven shape of the surface 4a of the antiglare layer 4 is set to the above-mentioned values of Safc and Smr1, so that the uneven shape is formed to have a distribution structure of unevenness that is steep and has a high number density. This scatters the light incident on the surface 4a of the antiglare layer 4, and appropriately suppresses the reflection of external light on the surface 4a of the antiglare layer 4. Therefore, the image display performance of the display device 1 is prevented from being deteriorated.
[0023] Furthermore, by constructing the anti-glare film 2 to include an anti-glare layer 4 having the uneven surface 4a and a base film 3 satisfying formula 1, the base film 3 is made of a biaxially oriented film, maintaining sufficient mechanical strength, and the anti-glare film 2 having excellent anti-glare effect and anti-iridescent effect can be realized at low cost.
[0024] [Example of base film composition] The base film 3 contains a resin material. Examples of the resin material of the base film 3 include a transparent polymer. Specific examples of resin materials for the base film 3 include cellulose derivatives (cellulose acetates such as cellulose triacetate (TAC) and cellulose diacetate), polyester resins (polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polyarylate resins, etc.), polysulfone resins (polysulfone, polyethersulfone (PES), etc.), polyetherketone resins (polyetherketone (PEK), polyetheretherketone (PEEK), etc.), polycarbonate resins (PC), polyolefin resins (polyethylene, polypropylene, etc.), cyclic polyolefin resins (films such as "ARTON" (registered trademark) manufactured by JSR Corporation and "ZEONEX" (registered trademark) manufactured by Zeon Corporation), halogen-containing resins (polyvinylidene chloride, etc.), (meth)acrylic resins, styrene resins (polystyrene, etc.), vinyl acetate or vinyl alcohol resins (polyvinyl alcohol (PVA), etc.).
[0025] The thickness D of the base film 3 can be appropriately set within a range that satisfies Formula 1. The thickness D of the base film 3 is preferably, for example, from 20 μm to 500 μm, more preferably from 50 μm to 200 μm, and even more preferably from 75 μm to 150 μm.
[0026] [Example of anti-glare layer configuration] The antiglare layer 4 of the first embodiment contains a plurality of resin components and has a phase-separated structure of the plurality of resin components. The antiglare layer 4 has, as an example, a surface 4a on which a plurality of convex portions are distributed. As a result, the surface 4a of the antiglare layer 4 of the present embodiment has a sea-island structure formed by a plurality of convex portions and concave portions therebetween. The antiglare layer 4 exhibits antiglare properties due to the concave-convex shape formed by a plurality of convex portions and concave portions therebetween. By including such an antiglare layer 4, the antiglare film 2 has an excellent balance between the haze value and the transmitted image clarity (image clarity). The surface 4a of the antiglare layer 4 may have a bicontinuous phase structure in which a plurality of convex portions are densely arranged.
[0027] Furthermore, the anti-glare film 2 prevents light from the display surface 16a passing through the anti-glare layer 4 from being refracted due to the unevenness of the surface of the anti-glare layer 4, and prevents the pixels of the display surface 16a from appearing enlarged due to the lens effect of the uneven shape of the surface 4a of the anti-glare layer 4, thereby suppressing glare on the display surface 16a. As a result, even if the anti-glare film 2 is attached to a display surface 16a having high-definition pixels, glare on the display surface 16a can be suppressed to a high degree while maintaining anti-glare properties, and blurring of characters and images can also be suppressed.
[0028] As described later, the phase-separated structure of the antiglare layer 4 is formed by spinodal decomposition (wet spinodal decomposition) from a liquid phase using a solution that is a material for the antiglare layer 4. For details of the antiglare layer 4, see, for example, the description of Japanese Patent Application No. 2012-231496.
[0029] Examples of the polymer contained in the antiglare layer 4 include thermoplastic resins. Examples of the thermoplastic resins include styrene-based resins, (meth)acrylic-based resins, organic acid vinyl ester-based resins, vinyl ether-based resins, halogen-containing resins, olefin-based resins (including alicyclic olefin-based resins), polycarbonate-based resins, polyester-based resins, polyamide-based resins, thermoplastic polyurethane resins, polysulfone-based resins (polyethersulfone, polysulfone, etc.), polyphenylene ether-based resins (polymers of 2,6-xylenol, etc.), cellulose derivatives (cellulose esters, cellulose carbamates, cellulose ethers, etc.), silicone resins (polydimethylsiloxane, polymethylphenylsiloxane, etc.), rubber or elastomers (diene-based rubbers such as polybutadiene and polyisoprene, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic rubbers, urethane rubbers, silicone rubbers, etc.), etc. These thermoplastic resins can be used alone or in combination of two or more.
[0030] Further, the polymer may have a functional group involved in a curing reaction or a functional group that reacts with a curable compound. The polymer may have the functional group in the main chain or in a side chain.
[0031] The functional group may be a condensable group, a reactive group (e.g., a hydroxyl group, an acid anhydride group, a carboxyl group, an amino group or an imino group, an epoxy group, a glycidyl group, an isocyanate group), a polymerizable group (e.g., a C group such as vinyl, propenyl, isopropenyl, butenyl, or allyl group), or a condensable group (e.g., a C group such as vinyl, propenyl, isopropenyl, butenyl, or allyl group). 2-6 Alkenyl groups, ethynyl, propynyl, butynyl groups, etc. 2-6 Alkynyl group, vinylidene group, etc. 2-6 Examples of the functional groups include alkenylidene groups and groups having such polymerizable groups (e.g., (meth)acryloyl groups). Of these functional groups, the polymerizable groups are preferred.
[0032] The antiglare layer 4 may contain multiple types of polymers. These polymers may be phase-separable by spinodal decomposition from a liquid phase, or may be incompatible with each other. The combination of the first polymer and the second polymer contained in the multiple types of polymers is not particularly limited, but polymers that are incompatible with each other near the processing temperature may be used.
[0033] For example, when the first polymer is a styrene-based resin (polystyrene, styrene-acrylonitrile copolymer, etc.), the second polymer may be a cellulose derivative (e.g., cellulose esters such as cellulose acetate propionate), a (meth)acrylic resin (polymethyl methacrylate, etc.), an alicyclic olefin-based resin (polymers having norbornene as a monomer, etc.), a polycarbonate-based resin, a polyester-based resin (polyC 2-4 Alkylene arylate copolyesters, etc. can be mentioned as examples.
[0034] For example, when the first polymer is a cellulose derivative (e.g., cellulose esters such as cellulose acetate propionate), the second polymer may be a styrene-based resin (polystyrene, styrene-acrylonitrile copolymer, etc.), a (meth)acrylic-based resin, an alicyclic olefin-based resin (polymers having norbornene as a monomer, etc.), a polycarbonate-based resin, a polyester-based resin (polyC 2-4 Alkylene arylate copolyesters, etc. can be mentioned as examples.
[0035] The multiple types of polymers include at least cellulose esters (e.g., cellulose C such as cellulose diacetate, cellulose triacetate, cellulose acetate propionate, and cellulose acetate butyrate). 2-4 Alkyl carboxylates) may be included.
[0036] Here, the phase-separated structure of the antiglare layer 4 is fixed by curing a precursor of a curable resin contained in the multiple resin components with active energy rays (ultraviolet rays, electron beams, etc.), heat, etc. during the production of the antiglare layer 4. In addition, such a curable resin imparts scratch resistance and durability to the antiglare layer 4.
[0037] From the viewpoint of obtaining scratch resistance of the antiglare layer 4, it is desirable that at least one of the polymers included in the plurality of types of polymers is a polymer having a functional group in a side chain capable of reacting with a curable resin precursor. The polymer forming the phase separation structure may include a thermoplastic resin or other polymers in addition to the above-mentioned two mutually incompatible polymers. The weight ratio M1 / M2 of the weight M1 of the first polymer to the weight M2 of the second polymer, and the glass transition temperature of the polymers can be appropriately set.
[0038] Examples of the curable resin precursor include a curable compound that has a functional group that reacts with active energy rays (ultraviolet rays or electron beams, etc.) or heat, and that is cured or crosslinked by this functional group to form a resin (particularly a cured resin or a crosslinked resin).
[0039] Examples of such compounds include thermosetting compounds or thermosetting resins (low molecular weight compounds having an epoxy group, a polymerizable group, an isocyanate group, an alkoxysilyl group, a silanol group, or the like (for example, epoxy-based resins, unsaturated polyester-based resins, urethane-based resins, silicone-based resins, and the like)), and photocurable (ionizing radiation-curable) compounds that are cured by ultraviolet light, electron beams, or the like (ultraviolet light-curable compounds such as photocurable monomers and oligomers, and the like).
[0040] A preferable curable resin precursor is a photocurable compound that is cured in a short time by ultraviolet light or an electron beam. Among these, an ultraviolet curable compound is particularly practical. In order to improve resistance such as scratch resistance, the photocurable compound preferably has two or more (preferably 2 to 15, more preferably about 4 to 10) polymerizable unsaturated bonds in the molecule. Specifically, the photocurable compound is preferably an epoxy (meth)acrylate, a urethane (meth)acrylate, a polyester (meth)acrylate, a silicone (meth)acrylate, or a polyfunctional monomer having at least two polymerizable unsaturated bonds.
[0041] The curable resin precursor may contain a curing agent according to its type. For example, the thermosetting resin precursor may contain a curing agent such as amines or polyvalent carboxylic acids, and the photocurable resin precursor may contain a photopolymerization initiator. Examples of the photopolymerization initiator include conventional components such as acetophenones or propiophenones, benzils, benzoins, benzophenones, thioxanthones, and acylphosphine oxides.
[0042] The curable resin precursor may contain a curing accelerator. For example, the photocurable resin precursor may contain a photocuring accelerator, such as a tertiary amine (dialkylaminobenzoic acid ester, etc.) or a phosphine-based photopolymerization accelerator.
[0043] In the manufacturing process of the antiglare layer 4, at least two of the polymers and the curable resin precursors contained in the solution that is the material of the antiglare layer 4 are used in a combination that causes phase separation from each other near the processing temperature. Examples of combinations that cause phase separation include (a) a combination in which multiple types of polymers are phase-separated due to their mutual incompatibility, (b) a combination in which a polymer and a curable resin precursor are phase-separated due to their mutual incompatibility, and (c) a combination in which multiple curable resin precursors are phase-separated due to their mutual incompatibility. Among these combinations, typically, (a) a combination of multiple types of polymers and (b) a combination of a polymer and a curable resin precursor are included. In particular, (a) a combination of multiple types of polymers is desirable.
[0044] Here, the polymer and the cured resin or crosslinked resin generated by curing the curable resin precursor usually have different refractive indices. Also, the refractive indices of the multiple types of polymers (first polymer and second polymer) usually differ from each other. The refractive index difference between the polymer and the cured resin or crosslinked resin, and the refractive index difference between the multiple types of polymers (first polymer and second polymer) are preferably, for example, in the range of 0 to 0.04, more preferably in the range of 0 to 0.02.
[0045] The antiglare layer 4 may contain a matrix resin having a phase separation structure and a plurality of fine particles (fillers) dispersed in the matrix resin. The fine particles may be either organic fine particles or inorganic fine particles. The antiglare layer 4 may contain a plurality of types of fine particles having different materials or average particle sizes.
[0046] Examples of organic fine particles include crosslinked acrylic particles and crosslinked styrene particles. Examples of inorganic fine particles include silica (SiO2), zirconia (ZrO2), titania (TiO2), and other fine particles of various metal oxides. Examples of metal oxides include indium tin oxide, tin oxide, indium oxide, germanium oxide, zinc oxide, and aluminum oxide. Examples of inorganic fine particles include metal fluoride particles, metal sulfide particles, metal nitride particles, and metal particles. For example, fine particles contained in the antiglare layer 4 are preferably those having good transparency. For example, when the fine particles contain silica, for example, it is easy to improve the hardness of the antiglare film 2. For example, the refractive index difference between the fine particles contained in the antiglare layer 4 and the matrix resin can be set to a value in the range of 0 to 0.5. For example, this refractive index difference is preferably a value in the range of 0 to 0.3, and more preferably a value in the range of 0 to 0.2.
[0047] The average particle size of the fine particles is not particularly limited and can be set to a value in the range of 0.5 μm to 10 μm, for example. The average particle size is preferably in the range of 0.5 μm to 8.0 μm, and more preferably in the range of 1.0 μm to 6.0 μm.
[0048] The average particle size referred to in this specification is, for example, the volume average particle size (MV value) measured by a laser diffraction scattering method (the same applies to the average particle size mentioned below). The fine particles may be solid or hollow. For example, by setting the average particle size of the fine particles to a value that is not too small, anti-glare properties can be easily obtained. Also, for example, by setting the average particle size of the fine particles to a value that is not too large, glare can be easily suppressed.
[0049] The thickness dimension of the antiglare layer 4 can be appropriately set, but is, for example, a value in the range of 0.3 μm to 20 μm. The thickness dimension is, for example, preferably, a value in the range of 1 μm to 15 μm, and more preferably, a value in the range of 1 μm to 10 μm. The thickness dimension can usually be set, for example, to a value in the range of 2 μm to 10 μm (particularly, a value in the range of 3 μm to 7 μm).
[0050] The antiglare layer 4 may contain conventional additives, such as organic or inorganic particles, stabilizers (antioxidants, ultraviolet absorbers, etc.), surfactants, water-soluble polymers, fillers, crosslinking agents, coupling agents, colorants, flame retardants, lubricants, waxes, preservatives, viscosity adjusters, thickeners, leveling agents, and defoamers, within limits that do not impair the optical properties.
[0051] [Anti-glare film manufacturing method example] As an example, a manufacturing method of the antiglare film 2 includes a preparation step of preparing a solution (hereinafter simply referred to as the solution) that will be the material of the antiglare layer 4, a formation step of applying the solution prepared in the preparation step to the surface of a specified support (in this embodiment, the base film 3) to evaporate the solvent in the solution and form a phase separation structure by spinodal decomposition from the liquid phase, and a curing step of curing the curable resin precursor after the formation step.
[0052] In the preparation step, a solution is prepared that contains a solvent and a resin composition for forming the antiglare layer 4. The solvent can be selected depending on the types and solubility of the polymers and curable resin precursors contained in the antiglare layer 4. Any solvent can be used as long as it can uniformly dissolve at least the solid contents (multiple types of polymers and curable resin precursors, reaction initiator, and other additives).
[0053] Examples of the solvent include ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), ethers (dioxane, tetrahydrofuran, etc.), aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), halogenated carbons (dichloromethane, dichloroethane, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), water, alcohols (ethanol, isopropanol, butanol, cyclohexanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates, sulfoxides (dimethyl sulfoxide, etc.), amides (dimethylformamide, dimethylacetamide, etc.), etc. The solvent may be a mixed solvent.
[0054] The resin composition is preferably a composition containing the thermoplastic resin, a photocurable compound, a photopolymerization initiator, the thermoplastic resin, and a photocurable compound, or a composition containing the multiple types of mutually incompatible polymers, a photocurable compound, and a photopolymerization initiator.
[0055] The concentration of solutes (polymer and curable resin precursor, reaction initiator, and other additives) in the solution can be adjusted within a range in which phase separation of multiple resin components occurs and within a range in which the flowability, coatability, etc. of the solution are not impaired.
[0056] Here, the external haze value, internal haze value, antiglare properties, etc. of the antiglare layer 4 can vary depending on the combination and weight ratio of the resin compositions in the solution, or the working conditions of the preparation step, formation step, and curing step, etc. Therefore, an antiglare film 2 having the desired physical properties can be manufactured by forming an antiglare layer while changing each condition and measuring and understanding the physical properties of the obtained antiglare layer in advance.
[0057] In the forming step, the solution prepared in the preparing step is cast or applied onto the surface of a support (here, as an example, the base film 3). Examples of the method for casting or applying the solution include conventional methods such as spray, spinner, roll coater, air knife coater, blade coater, rod coater, reverse coater, bar coater, comma coater, dip, dip squeeze coater, die coater, gravure coater, microgravure coater, and silk screen coater.
[0058] The solvent is removed by evaporation from the solution cast or applied onto the surface of the support by drying. As the solution is concentrated during this evaporation process, phase separation occurs due to spinodal decomposition from the liquid phase of multiple resin components, forming a phase-separated structure. The uneven shape of the surface 4a due to the phase-separated structure can be formed by setting the drying conditions and recipe so that the melt fluidity of the resin components after the solvent evaporation is somewhat high.
[0059] For example, the evaporation of the solvent is desirably performed by heat drying, since this facilitates the formation of convex portions on the surface 4a of the antiglare layer 4. By adjusting the drying temperature so that it is not too low, and also adjusting the drying time so that it is not too short, it is possible to impart a sufficient amount of heat to the resin component, prevent a decrease in the melt fluidity of the resin component, and facilitate the formation of convex portions.
[0060] On the other hand, if the drying temperature is too high or the drying time is too long, the convex portions once formed may flow and lose their height, but the structure of the convex portions is maintained. Therefore, the drying temperature and drying time can be used as a means for adjusting the antiglare property and slipperiness of the antiglare layer 4 by changing the height of the convex portions.
[0061] As phase separation from the liquid phase of multiple resin components by spinodal decomposition progresses, a co-continuous phase structure is formed and coarsens, and the continuous phase becomes discontinuous, forming a droplet phase structure (an island structure of independent phases, such as spherical, true spherical, discoidal, or ellipsoidal). Depending on the degree of phase separation, an intermediate structure between the co-continuous phase structure and the droplet phase structure (a phase structure in the process of transitioning from the co-continuous phase to the droplet phase) can also be formed. After the solvent is removed, a layer with fine irregularities is formed on the surface.
[0062] In this way, by forming fine irregularities on the surface of the layer by phase separation, for example, the external haze value of the antiglare layer 4 can be adjusted without dispersing fine particles in the antiglare layer 4. Moreover, by omitting the fine particles, it is possible to easily adjust the haze value of the antiglare layer 4 while suppressing the internal haze value compared to the external haze value. Note that an antiglare layer 4 containing fine particles can also be formed by adding fine particles to the solution in the preparation process.
[0063] In the curing step, the phase separation structure formed in the forming step is fixed by curing the curable resin precursor in the solution, thereby forming the antiglare layer 4. The curable resin precursor is cured by heating or irradiating with active energy rays, or a combination of these methods, depending on the type of the curable resin precursor. The type of active energy rays to be irradiated is selected depending on the type of photocurable component, etc.
[0064] The irradiation of the active energy rays may be performed in an inert gas atmosphere. When the active energy rays are ultraviolet rays, a far ultraviolet lamp, a low pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a halogen lamp, a laser light source (a light source such as a helium-cadmium laser or an excimer laser) or the like can be used as the light source.
[0065] When forming the adhesive layer 5, a solution containing an adhesive component is prepared, and then the solution is applied to the other surface of the base film 3 by a conventional method, for example, the casting method or coating method described above in the formation step, and dried to form the adhesive layer 5. The antiglare film 2 is manufactured through the above steps.
[0066] Here, for example, by not only reducing the unevenness of the surface 4a of the anti-glare layer 4 but also increasing the slope of the unevenness to make the unevenness steeper and by increasing the number of unevennesses, it is possible to improve the anti-glare properties of the anti-glare film 2 as well as suppressing glare.
[0067] The basic method for forming the antiglare layer of the present disclosure is not particularly limited to the above-mentioned method, and any known method can be used. Examples of the known method include the above-mentioned formation method based on the phase separation structure of multiple resin components, as well as a formation method based on a microparticle dispersion method in which the antiglare layer 104 is formed using a matrix resin 40 and multiple microparticles 41, as described in the second embodiment. Another example is a transfer formation method in which a previously prepared mold (mother mold) is used to transfer the uneven shape of the surface to form the antiglare layer. In this case, for example, a mold in which a metal film is formed by electrochemical coating or the like on a previously manufactured antiglare film or the like can be used.
[0068] As a basic method for forming the antiglare layer, a method of forming an uneven shape on the surface of the antiglare layer by cutting the surface of the antiglare layer material using a laser or the like can be exemplified. Another example is a method of polishing the antiglare layer material by a shot blasting method using a projectile such as sand or beads to form an uneven shape on the surface of the antiglare layer. Another example is a method of etching the antiglare layer material to form an uneven shape on the surface of the antiglare layer. Hereinafter, the other embodiments will be described, focusing on the differences from the first embodiment.
[0069] Second embodiment [Anti-glare film] Fig. 3 is an enlarged cross-sectional view of a surface 104a of an anti-glare layer 104 of an anti-glare film 102 according to the second embodiment. As shown in Fig. 3, the anti-glare film 102 according to the second embodiment includes an anti-glare layer 104. The anti-glare film 102 includes a base film 3, similar to the anti-glare film 2. The surface 104a of the anti-glare layer 104 opposite to the base film 3 side has an uneven shape similar to the surface 4a of the anti-glare layer 4.
[0070] The antiglare layer 104 includes a matrix resin 40 and a plurality of fine particles 41 dispersed in the matrix resin 40. This gives the antiglare layer 104 a fine particle dispersion structure. Some of the fine particles 41 dispersed in the matrix resin 40 in the antiglare layer 104 are arranged so as to protrude outward from the surface of the matrix resin 40, forming an uneven shape on the surface 104a of the antiglare layer 104.
[0071] Even when multiple microparticles 41 are used to form an uneven shape on surface 104a of anti-glare layer 104 as in this embodiment, by selecting a material that strengthens the repulsive interaction between microparticles 41 and other resins or solvents when forming anti-glare layer 104, it is possible to induce moderate aggregation of microparticles 41 and form a steep, number-dense uneven distribution structure on surface 104a of anti-glare layer 104.
[0072] The shape of the fine particles 41 is not limited, and may be spherical or ellipsoidal. The fine particles 41 are formed to be solid, but may be hollow. When the fine particles 41 are formed to be hollow, the hollow portion of the fine particles 41 may be filled with air or other gas. In the antiglare layer 104, each fine particle 41 may be dispersed as a primary particle, or a plurality of secondary particles formed by aggregation of a plurality of fine particles 41 may be dispersed.
[0073] The refractive index difference between the matrix resin 40 and the fine particles 41 is set to a value in the range of, for example, 0 to 0.5. This refractive index difference is preferably, for example, a value in the range of 0 to 0.3, and more preferably, a value in the range of 0 to 0.2.
[0074] The average particle diameter of the particles 41 is set to, for example, a value in the range of 0.5 μm to 10 μm. The average particle diameter of the particles 41 is preferably, for example, a value in the range of 0.5 μm to 8.0 μm, and more preferably, a value in the range of 1.0 μm to 6.0 μm.
[0075] Also, for example, it is desirable that there is small variation in the particle size of the fine particles 41. In this case, for example, in the particle size distribution of the fine particles 41 contained in the antiglare layer 104, it is desirable that the average particle size of 50% by weight or more of the fine particles 41 contained in the antiglare layer 104 has a variation within 1.0 μm.
[0076] In this way, the particles 41, whose particle diameters are relatively uniform and whose average particle diameters are set within the above range, form uniform and appropriate unevenness on the surface of the antiglare layer 104. The ratio of the weight of the matrix resin 40 in the antiglare layer 104 to the total weight of the particles 41 can be set appropriately. In this embodiment, the ratio G2 / G1 of the weight G1 of the matrix resin 40 in the antiglare layer 104 to the total weight G2 of the particles 41 is set to a value in the range of 0.01 to 2.0, for example. The ratio G2 / G1 is preferably, for example, a value in the range of 0.02 to 1.5, and more preferably a value in the range of 0.03 to 1.0.
[0077] The fine particles 41 dispersed in the matrix resin 40 may be either inorganic or organic. For example, the fine particles 41 are preferably those having good transparency. An example of the organic fine particles is plastic beads. Examples of the plastic beads include styrene beads (refractive index 1.59), melamine beads (refractive index 1.57), acrylic beads (refractive index 1.49), acrylic-styrene beads (refractive index 1.54), polycarbonate beads, polyethylene beads, and the like. The styrene beads may be cross-linked styrene beads, and the acrylic beads may be cross-linked acrylic beads. It is preferable that the plastic beads have a hydrophobic group on the surface. An example of such plastic beads is styrene beads.
[0078] Examples of the matrix resin 40 include at least one of a photocurable resin that is cured by active energy rays, a solvent drying type resin that is cured by drying a solvent added during coating, and a thermosetting resin.
[0079] Examples of photocurable resins include those having an acrylate-based functional group, such as relatively low molecular weight polyester resins, polyether resins, acrylic resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, and oligomers such as (meth)acrylates of polyfunctional compounds such as polyhydric alcohols, prepolymers, and reactive diluents.
[0080] Specific examples of these include monofunctional monomers such as ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, and N-vinylpyrrolidone, as well as polyfunctional monomers such as polymethylolpropane tri(meth)acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate.
[0081] When the photocurable resin is an ultraviolet-curable resin, it is preferable to use a photopolymerization initiator. Examples of photopolymerization initiators include acetophenones, benzophenones, Michler's benzoyl benzoate, α-amyloxime ester, tetramethylthiuram monosulfide, and thioxanthones. It is also preferable to mix a photosensitizer with the photocurable resin. Examples of photosensitizers include n-butylamine, triethylamine, and poly-n-butylphosphine.
[0082] Examples of the solvent-drying type resin include known thermoplastic resins. Examples of the thermoplastic resin include styrene-based resins such as polystyrene resins, acrylic resins, (meth)acrylic resins, vinyl-based resins such as vinyl acetate resins, vinyl ether resins, acetal resins, halogen-containing resins, alicyclic olefin-based resins, polycarbonate resins, polyester resins, polyamide resins, cellulose resins, cellulose derivatives, silicone resins, and rubber or elastomers. As the solvent-drying type resin, a resin that is soluble in an organic solvent and is particularly excellent in moldability, film-forming properties, transparency, and weather resistance is desirable. Examples of such solvent-drying type resins include styrene-based resins, (meth)acrylic resins, alicyclic olefin-based resins, polyester resins, and cellulose derivatives (cellulose esters, etc.).
[0083] Examples of the thermosetting resin include phenol resin, urea resin, diallyl phthalate resin, melamine resin, guanamine resin, unsaturated polyester resin, polyurethane resin, epoxy resin, aminoalkyd resin, melamine-urea co-condensation resin, silicon resin, polysiloxane resin, etc. When a thermosetting resin is used as the matrix resin 40, at least one of a crosslinking agent, a curing agent such as a polymerization initiator, a polymerization accelerator, a solvent, and a viscosity adjuster may be used in combination.
[0084] [Anti-glare film manufacturing method example] As an example, a manufacturing method of the antiglare film 102 includes a preparation step of preparing a solution that will be the material of the antiglare layer 104, a coating step of coating the solution prepared in the preparation step onto the surface of a specified support (in this embodiment, the base film 3), and a curing step of curing the resin in the applied solution.
[0085] In the preparation step, a solution containing a solvent, a resin composition for forming the antiglare layer 104, and fine particles 41 is prepared. Examples of the solvent include at least one of alcohols (isopropyl alcohol, methanol, ethanol, etc.), ketones (methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclohexanone, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), halogenated hydrocarbons, and aromatic hydrocarbons (toluene, xylene, etc.). A known leveling agent may be further added to the solution. For example, the use of a fluorine-based or silicone-based leveling agent can impart good scratch resistance to the antiglare layer 104.
[0086] In the coating step, the solution prepared in the preparation step is cast or coated on the surface of a support (here, as an example, the base film 3) in the same manner as in the first embodiment. The solvent is removed from the solution cast or coated on the surface of the support by evaporation through drying.
[0087] When the matrix resin 40 is a photocurable resin, a curing step using, for example, ultraviolet light or electron beams is performed after the coating step. Examples of ultraviolet light sources include various mercury lamps, ultraviolet carbon arc lamps, black lights, and metal halide lamps. Examples of the wavelength range of ultraviolet light include a wavelength range of 190 nm to 380 nm.
[0088] Examples of the electron beam source include known electron beam accelerators, such as Van de Graaff type, Cockcroft-Walton type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type electron beam accelerators.
[0089] The matrix resin 40 contained in the solution is cured, thereby fixing the positions of the particles 41 in the matrix resin 40. As a result, a plurality of particles 41 are dispersed in the matrix resin 40, and an antiglare layer 104 having a structure in which the particles 41 form an uneven shape on the surface 104a.
[0090] Third embodiment Fig. 4 is a partial cross-sectional view of an antiglare film 202 having an antireflection layer 9 of a first structure according to the third embodiment. Fig. 5 is a partial cross-sectional view of an antiglare film 302 having an antireflection layer 9 of a second structure according to the third embodiment. Fig. 6 is a partial cross-sectional view of an antiglare film 402 having an antireflection layer 9 of a third structure according to the third embodiment. Fig. 6 shows an antireflection layer 9 of a four-layer structure as an example.
[0091] As shown in FIG. 4 to FIG. 6, the anti-glare films 202, 302, and 402 of the present embodiment have an anti-reflection layer 9 disposed on the surface 4a of the anti-glare layer 4 opposite to the substrate film 3 side. The anti-reflection layer 9 prevents reflection of external light. As shown in FIG. 4, the anti-reflection layer 9 has, for example, a first structure including only a single low refractive index layer 90. Alternatively, as shown in FIG. 5, the anti-reflection layer 9 has a second structure including a laminated structure of a single low refractive index layer 90 and a single high refractive index layer 91 having a higher refractive index than the low refractive index layer 90. Alternatively, as shown in FIG. 6, the anti-reflection layer 9 has a third structure that is a laminated structure of three or more layers including a low refractive index layer 90 and a high refractive index layer 91 arranged alternately. The low refractive index layer 90 has, for example, a refractive index lower than that of the anti-glare layer 4. The low refractive index layer 90 may have antifouling properties. In this case, the low refractive index layer 90 may include an antifouling agent such as a silicone-based compound or a fluorine-based compound.
[0092] The method for forming the low refractive index layer 90 and the high refractive index layer 91 is not particularly limited, and may be, for example, a known wet method or dry method. When the antireflection layer 9 has the first or second structure, for example, a wet method is preferable. When the antireflection layer 9 has the third structure, for example, a dry method is preferable.
[0093] The refractive index of the antireflection layer 9 is not particularly limited. The thickness of the antireflection layer 9 can be set within a range that ensures the antiglare properties of the antiglare film 202. For example, the thickness of the antireflection layer 9 can be set so that the spectral reflectance in the vicinity of 550 nm is the lowest when the spectral reflectance spectrum of the antiglare film 202 is measured.
[0094] When the antireflection layer 9 has the first structure or the second structure, the refractive index of the low refractive index layer 90 is, for example, a value in the range of 1.34 or more. In this case, the refractive index of the low refractive index layer 90 is desirably, for example, from 1.34 to 1.45, more desirably, from 1.34 to 1.4, even more desirably, from 1.34 to 1.39, and even more desirably, from 1.34 to 1.38. For example, by setting the refractive index of the low refractive index layer 90 not too high, it is possible to suppress a decrease in the antireflection properties of the antireflection layer 9.
[0095] When the antireflection layer 9 has the first structure or the second structure, the thickness of the low refractive index layer 90 is desirably, for example, in the range of 50 nm or more and 300 nm or less, more desirably, in the range of 60 nm or more and 150 nm or less, even more desirably, in the range of 80 nm or more and 120 nm or less, and even more desirably, in the range of 90 nm or more and 110 nm or less.
[0096] The configuration of the low refractive index layer 90 can be referred to, for example, in the configurations of low refractive index layers described in JP 2001-100006 A, JP 2008-58723 A, and WO 2016 / 039125. The low refractive index layer 90 is, for example, made of a composition containing a low refractive index resin. The low refractive index layer 90 may also be, for example, made of a cured product of a composition containing a curable resin and a fluorine-containing compound or a low refractive index inorganic filler.
[0097] Examples of the low refractive index resin include fluororesins such as methylpentene resin, diethylene glycol bis(allyl carbonate) resin, polyvinylidene fluoride (PVDF), and polyvinyl fluoride (PVF). Examples of the curable resin include fluorine-free photocurable resins used as materials for the antiglare layer 4. Examples of the fluorine-containing compound include fluorine-containing photocurable resins used as materials for the antiglare layer 4.
[0098] The ratio of the fluorine-containing compound in the composition constituting the low refractive index layer 90 is, for example, a value in the range of 1% by mass or more with respect to the entire composition. The ratio may be, for example, a value in the range of 5% by mass or more and 90% by mass or less. Examples of inorganic fillers with a low refractive index include fillers described in JP-A-2001-100006. As the inorganic filler, for example, fillers with a low refractive index such as silica and magnesium fluoride are preferable, and silica is particularly preferable. Examples of silica include hollow silica described in JP-A-2001-233611 or JP-A-2003-192994. Among these, hollow silica is preferable from the viewpoint of suppressing an increase in haze and improving transparency.
[0099] The number average particle size (number average primary particle size) of the inorganic filler (particularly, hollow silica) measured by an electron microscope is, for example, a value in the range of 100 nm or less. As an example, the number average particle size is preferably a value in the range of 80 nm or less. As another example, the number average particle size is preferably a value in the range of 10 nm to 80 nm, and more preferably a value in the range of 20 nm to 70 nm.
[0100] The proportion of the low refractive index inorganic filler (particularly, hollow silica) in the composition constituting the low refractive index layer 90 is, for example, a value in the range of 1 mass % or more with respect to the entire composition. The proportion may be, for example, a value in the range of 5 mass % or more and 90 mass % or less. The low refractive index inorganic filler may be surface-modified with a coupling agent (titanium coupling agent, silane coupling agent). Furthermore, the composition containing the low refractive index inorganic filler may contain other inorganic fillers in order to improve the coating strength.
[0101] The composition of the low refractive index layer 90 may contain a curing agent or known additives used as materials for the antiglare layer 4. The antiglare layer of this embodiment may be formed by any of the formation methods described in the first and second embodiments.
[0102] As shown in FIG. 5, when the anti-reflection layer 9 has the second structure, the high refractive index layer 91 is preferably disposed closer to the anti-glare layer 4 than the low refractive index layer 90. The refractive index of the high refractive index layer 91 can be appropriately set within a range higher than the refractive index of the low refractive index layer 90. In this case, the refractive index of the high refractive index layer 91 is, for example, a value in the range of 1.53 or more. In this case, the refractive index of the high refractive index layer 91 is preferably, for example, a value in the range of 1.54 or more, more preferably a value in the range of 1.55 or more, and even more preferably a value in the range of 1.56 or more. In this case, the refractive index of the high refractive index layer 91 is preferably, for example, a value in the range of 1.85 or less, more preferably a value in the range of 1.80 or less, and even more preferably a value in the range of 1.75 or less.
[0103] When the antireflection layer 9 has the second structure, the thickness of the high refractive index layer 91 is, for example, a value in the range of 200 nm or less. In this case, the thickness of the high refractive index layer 91 is preferably, for example, a value in the range of 180 nm or less, and more preferably a value in the range of 150 nm or less. In this case, the thickness of the high refractive index layer 91 is preferably, for example, a value in the range of 50 nm or more, and more preferably a value in the range of 70 nm or more.
[0104] The configuration of the high refractive index layer 91 can be referred to, for example, the configuration of the high refractive index layer described in JP 2016-097529 A. The high refractive index layer 91 is, for example, composed of a composition containing a high refractive index resin. The high refractive index layer 91 may also be, for example, composed of a cured product of a composition containing inorganic fine particles. The particle size of the inorganic fine particles can be, for example, a nanometer size. The number average particle size (number average primary particle size) of the inorganic fine particles is, for example, a value in the range of 1 nm to 100 nm. The number average particle size of the inorganic fine particles is, for example, desirably, a value in the range of 2 nm to 50 nm, more desirably, a value in the range of 3 nm to 40 nm, and even more desirably, a value in the range of 5 nm to 30 nm. The number average particle size of the inorganic fine particles can be measured by a conventional method using a particle size distribution meter. The number average particle size of the inorganic fine particles can be measured, for example, using a particle size measuring device (laser particle size analyzer "PAR-III" manufactured by Otsuka Electronics Co., Ltd.) based on a dynamic light scattering method.
[0105] The shape of inorganic fine particles is not particularly limited. Examples of the shape of inorganic fine particles include spherical, ellipsoidal, polygonal (polygonal pyramid, cuboid, rectangular, etc.), plate, rod, or amorphous. The shape of inorganic fine particles is preferably an isotropic shape such as a substantially spherical shape, because it can isotropically scatter light and improve visibility.
[0106] Examples of inorganic compounds constituting the inorganic fine particles include simple metals and metal oxides. For example, metal oxides are desirable because they can increase the refractive index of the high refractive index layer 91. Examples of metal oxides include periodic table Group 4A metal oxides (e.g., titanium oxide, zirconium oxide, etc.), periodic table Group 5A metal oxides (vanadium oxide, etc.), periodic table Group 6A metal oxides (molybdenum oxide, tungsten oxide, etc.), periodic table Group 7A metal oxides (manganese oxide, etc.), periodic table Group 8 metal oxides (nickel oxide, iron oxide, etc.), periodic table Group 1B metal oxides (copper oxide, etc.), periodic table Group 2B metal oxides (zinc oxide, etc.), periodic table Group 3B metal oxides (aluminum oxide, indium oxide, etc.), periodic table Group 4B metal oxides (silicon oxide, tin oxide, etc.), periodic table Group 5B metal oxides (antimony oxide, etc.), etc. These metal oxides can be used alone or in combination of two or more. Among these metal oxides, for example, the periodic table Group 4A metal oxides such as titanium oxide and zirconium oxide are desirable because they can increase the refractive index of the high refractive index layer 91 with a small proportion and can suppress an increase in haze even if the amount added is increased, and zirconium oxide is particularly desirable.
[0107] The high refractive index resin includes, for example, a curable resin. An example of the curable resin is an ultraviolet curable resin. As the ultraviolet curable resin, for example, a polyfunctional (meth)acrylate such as pentaerythritol tri(meth)acrylate or dipentaerythritol hexa(meth)acrylate is preferable.
[0108] 6, when the antireflection layer 9 has the third structure, the third structure preferably includes, for example, a low refractive index layer 90 disposed on the outermost surface of the antiglare film 202. When the antireflection layer 9 has the third structure, the thickness of each high refractive index layer 91 preferably has a value in the range of, for example, 10 nm to 200 nm, and more preferably has a value in the range of, for example, 20 nm to 70 nm. In this case, the refractive index of each high refractive index layer 91 preferably has a value in the range of, for example, 2.00 to 2.60.
[0109] When the antireflection layer 9 has the third structure, the thickness of each low refractive index layer 90 is preferably, for example, from 5 nm to 200 nm, and more preferably from 20 nm to 120 nm. In this case, the refractive index of each low refractive index layer 90 is preferably, for example, from 1.20 to 1.60.
[0110] The antireflection layer 9 is not limited to having any one of the first to third structures. The antireflection layer 9 may have a structure including another layer, such as at least one medium refractive index layer having a refractive index higher than that of the low refractive index layer 90 and lower than that of the high refractive index layer 91. In this case, the medium refractive index layer may be combined with at least one of the low refractive index layer 90 and the high refractive index layer 91, for example.
[0111] (Fourth embodiment) FIG. 7 is a schematic cross-sectional view of an optical member 10 according to a fourth embodiment. As shown in FIG. 7, the optical member 10 is an application example of an antiglare film 2. The optical member 10 includes an antiglare film 2 and a polarizing plate 6 arranged so as to be superimposed on the antiglare film 2. The polarizing plate 6 polarizes incident light from the outside. The polarizing plate 6 of this embodiment includes a retardation film 8 and a plate-shaped polarizing element 7 arranged so as to be superimposed on the retardation film 8. Examples of materials for the polarizing element 7 include polyvinyl alcohol (PVA), polyvinyl formal, polyvinyl acetal, and ethylene-vinyl acetate copolymer-based saponified products dyed with iodine or the like and stretched. Examples of materials for the retardation film 8 include triacetyl cellulose and cycloolefin polymer. According to this embodiment, the incident light to the retardation film 8 is incident on the polarizing element 7 and polarized, and then passes through the antiglare film 2 in a direction from the base film 3 to the antiglare layer 4.
[0112] The optical member 10 may include, for example, any of the antiglare films 102, 202, 302, and 402 of the other embodiments, instead of the antiglare film 2 of the first embodiment. The configuration of the polarizing plate 6 is not limited, and a known configuration can be adopted. For example, the polarizing plate 6 may include a protective film containing polyethylene terephthalate (PET) or the like.
[0113] Fifth embodiment FIG. 8 is a schematic cross-sectional view of a display device 20 according to a fifth embodiment. As shown in FIG. 8, the display device 20 is an application example of the optical member 10. The display device 20 includes a light source 17, a polarizing plate 18 arranged on the optical path of the light source 17, a panel-shaped display element 15 arranged on the polarizing plate 18 with the surface opposite to the image display side facing the polarizing plate 18, and an optical member 10 arranged on the image display side of the display element 15. As an example, the display element 15 includes an LCD. The light source 17 is a backlight. The surface 4a of the antiglare layer 4 in the optical member 10 is located at the top in the thickness direction of the display device 20. The polarizing plate 18 is a polarizing plate different from the polarizing plate 6 provided in the optical member 10.
[0114] When the display device 20 is driven, the light emitted from the light source 17 is polarized by the polarizing plate 18, and then sequentially enters the display element 15 and the optical member 10. Accordingly, an image on the display element 16 is visually recognized by the light emitted to the outside from the surface 4a of the antiglare layer 4 of the optical member 10.
[0115] (Confirmation test) Next, the performance confirmation test of the present disclosure will be described, but the present disclosure is not limited to each of the examples shown below. Antiglare films of Examples 1 to 13 and Comparative Examples 1 to 7 were manufactured based on the procedure shown below. Examples 1, 3, 5, 7 to 13 have an antiglare layer 4 having a phase separation structure, and correspond to the antiglare film 2. Examples 2 and 4 have an antiglare layer 104 having a fine particle dispersion structure, and correspond to the antiglare film 102. Example 6 has an antiglare layer 4 and an antireflection layer 9, and corresponds to the antiglare film 202. The antiglare layer 4 of Example 6 has a phase separation structure. Comparative Examples 1, 3 to 6 have an antiglare layer having a fine particle dispersion structure. Comparative Examples 2 and 7 have an antiglare layer having a phase separation structure. Examples 7 to 13 and Comparative Example 7 have the same antiglare layer 4 as Example 1, and are different from Example 1 in the thickness D, retardation Re, and integrated value (D×Re) of the substrate film 3. As materials for the antiglare films according to Examples 1 to 13 and Comparative Examples 1 to 7, the materials in the following items (M1) to (M29) were used.
[0116] [material] (M1) Acrylic polymer having a polymerizable group: "ACA Z322M" manufactured by Daicel Corporation, solid content 40% by weight, solvent: 1-methoxy-2-propanol (MMPG) (boiling point 119°C) (M2) Cellulose acetate propionate: Eastman Chemical Company "CAP-482-20" acetylation degree = 2.5%, propionylation degree = 46%, polystyrene equivalent number average molecular weight 75,000 (M3) Silicone acrylate: "EB1360" manufactured by Daicel Allnex Co., Ltd. (M4) Silicone-based hard coating material: "AS-201S" manufactured by TOKUSHIKI Co., Ltd. (M5) Urethane acrylate: "DCL-002" manufactured by Negami Chemical Industries, Ltd. (M6) Dipentaerythritol hexaacrylate: "DPHA" manufactured by Daicel Allnex Co., Ltd. (M7) Pentaerythritol tetraacrylate: "PETRA" manufactured by Daicel Allnex Co., Ltd. (M8) PMMA (polymethyl methacrylate) beads A: Sekisui Chemical Co., Ltd. "SSX-105" average particle size 5 μm, refractive index 1.49 (M9) PMMA beads B: "SSX-103" manufactured by Sekisui Plastics Co., Ltd. Average particle size 3 μm, refractive index 1.49 (M10) PMMA beads C: “SSX-115HXE” manufactured by Sekisui Plastics Co., Ltd. Average particle size 3 μm, refractive index 1.49 (M11) Silica microparticle A: "KE-P250" manufactured by Nippon Shokubai Co., Ltd., average particle size 2.5 μm, refractive index 1.43 (M12) Silica microparticles B: "Silysia 310P" manufactured by Fuji Silysia Chemical Co., Ltd., average particle size 2.7 μm (M13) Silica microparticle C: "Silohorbic 100" manufactured by Fuji Silysia Chemical Co., Ltd., average particle size 2.7 μm
[0117] (M14) Hollow silica dispersion acrylic hard coat liquid: "P-5063" manufactured by JGC Catalysts and Chemicals Co., Ltd., solid content 3% by weight (M15) Acrylic hard coat agent: Kyoeisha Chemical Co., Ltd. "HX-MR4" (M16) Styrene beads: "SX-350H" manufactured by Soken Chemical Industries, Ltd. (M17) Fluorine-based compound A having a polymerizable group: "Ftergent 602A" manufactured by Neos Co., Ltd. Solvent: ethyl acetate, solid content: 50% by mass (M18) Fluorine-based compound B having a polymerizable group: "KY-1203" manufactured by Shin-Etsu Chemical Co., Ltd., solid content concentration 20% by mass (M19) Photoinitiator A: "Omnirad184" manufactured by IGM Resin BV (M20) Photoinitiator B: "Omnirad907" manufactured by IGM Resin BV (M21) Polyethylene terephthalate (PET) film A: "Diafoil O321" manufactured by Mitsubishi Plastics, Inc., film thickness 75 μm (M22) Polyethylene terephthalate (PET) film B: "Diafoil O321" manufactured by Mitsubishi Plastics, Inc., film thickness 50 μm (M23) Polyethylene terephthalate (PET) film C: "Diafoil O321" manufactured by Mitsubishi Plastics, Inc., film thickness 100 μm (M24) Polyethylene terephthalate (PET) film D: "Diafoil O321" manufactured by Mitsubishi Plastics, Inc., film thickness 125 μm (M25) Polyethylene terephthalate (PET) film E: "Cosmoshine A4360" manufactured by Toyobo Co., Ltd., film thickness 50 μm (M26) Polyethylene terephthalate (PET) film F: "Cosmoshine A4360" manufactured by Toyobo Co., Ltd., film thickness 75 μm (M27) Polyethylene terephthalate (PET) film G: Toray Industries, Inc.'s "Lumirror U-403", film thickness 23 μm (M28) Polyethylene terephthalate (PET) film H: Toray Industries, Inc.'s "Lumirror U-403", film thickness 50 μm (M29) Polyethylene terephthalate (PET) film I: Toray Industries, Inc.'s "Lumirror U-403", film thickness 100 μm
[0118] [Example 1] A solution was prepared by dissolving 46 parts by weight of (M1) acrylic polymer having a polymerizable group, 5 parts by weight of (M2) cellulose acetate propionate, 77 parts by weight of (M5) urethane acrylate, 1.5 parts by weight of (M19) photoinitiator A, 1.5 parts by weight of (M20) photoinitiator B, and 0.5 parts by weight of (M17) fluorine-based compound A having a polymerizable group in a mixed solvent of 62 parts by weight of methyl ethyl ketone, 12 parts by weight of 1-butanol, 13 parts by weight of 1-methoxy-2-propanol, and 13 parts by weight of cyclohexanone.
[0119] This solution was cast onto the base film (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 8 μm. Then, a high-pressure mercury lamp was used to apply an integrated light dose of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer 4. In this way, an antiglare film 2 of Example 1 was produced.
[0120] [Example 2] A solution was prepared by dissolving 50 parts by weight of (M6) dipentaerythritol hexaacrylate, 50 parts by weight of (M7) pentaerythritol tetraacrylate, 6.0 parts by weight of (M8) PMMA beads A, 2.0 parts by weight of (M19) photoinitiator A, 2.0 parts by weight of (M20) photoinitiator B, and 1.0 part by weight of (M17) fluorine-based compound A having a polymerizable group in a mixed solvent of 146 parts by weight of methyl ethyl ketone and 59 parts by weight of 1-methoxy-2-propanol.
[0121] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 5 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer 104. In this way, an antiglare film 102 of Example 2 was produced.
[0122] [Example 3] A solution was prepared by dissolving 46 parts by weight of (M1) acrylic polymer having a polymerizable group, 5 parts by weight of (M2) cellulose acetate propionate, 62 parts by weight of (M5) urethane acrylate, 15 parts by weight of (M6) dipentaerythritol hexaacrylate, 1.5 parts by weight of (M19) photoinitiator A, 1.5 parts by weight of (M20) photoinitiator B, and 0.5 parts by weight of (M17) fluorine-based compound A having a polymerizable group in a mixed solvent of 62 parts by weight of methyl ethyl ketone, 12 parts by weight of 1-butanol, 13 parts by weight of 1-methoxy-2-propanol, and 13 parts by weight of cyclohexanone.
[0123] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 8 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer 4. In this way, an antiglare film 2 of Example 3 was produced.
[0124] [Example 4] A mixture of 100 parts by weight of (M15) acrylic hard coat agent A and 10 parts by weight of (M16) styrene beads A was dissolved in 30 parts by weight of methyl ethyl ketone to prepare a solution.
[0125] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 3 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer 104. In this way, an antiglare film 102 of Example 4 was produced.
[0126] [Example 5] A solution was prepared by dissolving 50 parts by weight of (M1) an acrylic polymer having a polymerizable group, 4 parts by weight of (M2) cellulose acetate propionate, 76 parts by weight of (M5) urethane acrylate, 1 part by weight of (M3) silicone acrylate, 1.5 parts by weight of (M19) photoinitiator A, and 1.5 parts by weight of (M20) photoinitiator B in a mixed solvent of 176 parts by weight of methyl ethyl ketone and 28 parts by weight of 1-butanol.
[0127] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 7 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer 4. In this way, an antiglare film 2 of Example 5 was produced.
[0128] [Example 6] A solution was prepared by dissolving 46 parts by weight of (M1) acrylic polymer having a polymerizable group, 5 parts by weight of (M2) cellulose acetate propionate, 77 parts by weight of (M5) urethane acrylate, 1.5 parts by weight of (M19) photoinitiator A, 1.5 parts by weight of (M20) photoinitiator B, and 0.5 parts by weight of (M17) fluorine-based compound A having a polymerizable group in a mixed solvent of 62 parts by weight of methyl ethyl ketone, 12 parts by weight of 1-butanol, 13 parts by weight of 1-methoxy-2-propanol, and 13 parts by weight of cyclohexanone.
[0129] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 8 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer 4. In this way, an intermediate film was obtained.
[0130] On the surface of the intermediate film on which the antiglare layer 4 was formed, the hollow silica-dispersed acrylic hard coat solution (M14) was cast using a wire bar, and the film was left in an oven at 70°C for 30 seconds to evaporate the solvent. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 100 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light of wavelength 365 nm (measured value of 365 nm line) to obtain a film in which a single-layer low refractive index layer 90 was formed as an antireflection layer 9 having a first structure on the surface of the antiglare layer 4. The type of wire bar was selected to set the thickness of the antireflection layer 9 so that the spectral reflectance in the vicinity of 550 nm would be the lowest when the spectral reflectance spectrum of the film was measured. In this way, the antiglare film 202 of Example 6 was produced.
[0131] [Example 7] Antiglare film 2 of Example 7 was produced in the same manner as in Example 1, except that (M21) PET film A was changed to (M22) PET film B. [Example 8] Antiglare film 2 of Example 8 was produced in the same manner as in Example 1, except that (M21) PET film A was changed to (M23) PET film C. [Example 9] Antiglare film 2 of Example 9 was produced in the same manner as in Example 1, except that (M21) PET film A was changed to (M24) PET film D. [Example 10] An antiglare film 2 of Example 10 was produced in the same manner as in Example 1, except that the (M21) PET film A was changed to the (M25) PET film E.
[0132] [Example 11] An antiglare film 2 of Example 11 was produced in the same manner as in Example 1, except that the (M21) PET film A was changed to the (M26) PET film F. [Example 12] (M21) PET film A (M2 8) PET Film H Except for the above change, the antiglare film 2 of Example 12 was produced in the same manner as in Example 1. [Example 13] An antiglare film of Example 13 was produced in the same manner as in Example 1, except that (M21) PET film A was changed to (M29) PET film I.
[0133] [Comparative Example 1] A solution was prepared by dissolving 50 parts by weight of (M6) dipentaerythritol hexaacrylate, 50 parts by weight of (M7) pentaerythritol tetraacrylate, 6.0 parts by weight of (M9) PMMA beads B, 2.0 parts by weight of (M19) photoinitiator A, 2.0 parts by weight of (M20) photoinitiator B, and 1.0 part by weight of (M17) fluorine-based compound A having a polymerizable group in a mixed solvent of 146 parts by weight of methyl ethyl ketone and 59 parts by weight of 1-methoxy-2-propanol.
[0134] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 5 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer. In this way, the antiglare film of Comparative Example 1 was produced.
[0135] [Comparative Example 2] A solution was prepared by dissolving 50 parts by weight of (M1) an acrylic polymer having a polymerizable group, 7 parts by weight of (M2) cellulose acetate propionate, 76 parts by weight of (M5) urethane acrylate, 1 part by weight of (M3) silicone acrylate, 1.5 parts by weight of (M19) photoinitiator A, and 1.5 parts by weight of (M20) photoinitiator B in a mixed solvent of 176 parts by weight of methyl ethyl ketone and 28 parts by weight of 1-butanol.
[0136] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 7 μm. Then, a high-pressure mercury lamp was used to apply the coating to the film, with an integrated light quantity of 200 mJ / cm2 and a peak illuminance of 400 mW / cm2.2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer. Thus, the antiglare film of Comparative Example 2 was produced.
[0137] [Comparative Example 3] A solution was prepared by dissolving 100 parts by weight of (M7) pentaerythritol tetraacrylate, 14.0 parts by weight of (M11) silica microparticles, 2.0 parts by weight of (M19) photoinitiator A, 2.0 parts by weight of (M20) photoinitiator B, and 1.0 part by weight of (M18) fluorine-based compound B having a polymerizable group in a mixed solvent of 146 parts by weight of methyl ethyl ketone and 59 parts by weight of 1-methoxy-2-propanol.
[0138] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 5 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2 and a peak illuminance of 400 mW / cm2. 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer. In this way, the antiglare film of Comparative Example 3 was produced.
[0139] [Comparative Example 4] A mixture of 100 parts by weight of (M15) acrylic hard coat agent A and 10 parts by weight of (M12) silica fine particles B was dissolved in 30 parts by weight of methyl ethyl ketone to prepare a solution.
[0140] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 4 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer. Thus, an antiglare film of Comparative Example 4 was produced.
[0141] [Comparative Example 5] A mixture of 100 parts by weight of (M15) acrylic hard coat agent A and 10 parts by weight of (M13) silica fine particles C was dissolved in 30 parts by weight of methyl ethyl ketone to prepare a solution.
[0142] This solution was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of about 3 μm. Then, a high-pressure mercury lamp was used to apply an integrated light amount of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer. Thus, the antiglare film of Comparative Example 5 was produced.
[0143] [Comparative Example 6] A liquid was prepared by mixing 260 parts by weight of (M4) silicone-based hard-coating material and 1.5 parts by weight of (M10) PMMA beads C. This liquid was cast onto (M21) PET film A using a wire bar, and then left in an oven at 80°C for 1 minute to evaporate the solvent and form a coating layer with a thickness of approximately 8 μm. Then, a high-pressure mercury lamp was used to apply an integrated light dose of 200 mJ / cm2. 2 , peak irradiance 400mW / cm 2 The coating layer was irradiated with ultraviolet light (measured value of 365 nm line) to cure the coating layer, thereby forming an antiglare layer. Thus, the antiglare film of Comparative Example 6 was produced.
[0144] Next, for each of the antiglare films of Examples 1 to 5 and Comparative Examples 1 to 6, Safc and Smr1 were measured under the following conditions, and the state of rainbow unevenness was evaluated. In addition, for Examples 1, 7 to 13, and Comparative Example 7, retardation Re was measured, and an integrated value (D×Re) was calculated, and the state of rainbow unevenness was evaluated.
[0145] Using an optical surface roughness meter "Vartscan R5500G" manufactured by Hitachi High-Tech Science Corporation, the fractal parameter Safc of the surface of the anti-glare layer of each anti-glare film opposite the substrate film side, and the load area ratio Smr1 separating the core portion and the protruding peak portion were measured according to the following procedure based on a method conforming to ISO 25178.
[0146] [Optical surface roughness meter setting conditions] Vibration isolation table: ON Objective lens: Nikon Corporation "5x / 0.13 OFN25 WD 9.3" Light source: Nikon Corporation "MODEL TE2-PS100W" Camera: Sony Corporation full pixel readout black and white camera module "XC-HR-57" 1 / 2'' CCD Upright microscope: Nikon Corporation "ECLIPSE LV150" Fiber light source: Nikon Corporation "LV-UEPI2"
[0147] [Setting conditions on the measurement screen] Camera: Sony Corporation full pixel readout black and white camera module "XC-HR-57" 1 / 2'' CCD Objective lens: 5X Lens tube: 0.5X Body Zoom Lens: No Relay Wavelength filter: 530white
[0148] [Measurement conditions] Measurement mode: Wave Field of view size: 640 x 480 Scan range: Start 5μm, Stop -10μm Average number of times: 1 After auto ramp, measurement begins
[0149] [Analysis conditions] Complement:Complete Surface correction: 4th order [Safc measurement conditions] Filter: Gaussian (short wavelength cutoff value λs: 50 [μm]) Parsing - ISOParam
[0150] [Smr1 measurement conditions] Filter: Gaussian (short wavelength cutoff value λs: 2.6 [μm]) Filter: Gaussian (long wavelength cutoff value λc: 25 [μm]) High-pass image was set as the main. Parsing - ISOParam
[0151] [Retardation Re] The retardation Re of the base film of each antiglare film was measured using a two-dimensional birefringence evaluation system, "Photonic Lattice WPA-200" manufactured by Ryoko Co., Ltd.
[0152] [Rainbow unevenness] Each anti-glare film was attached to the display surface of an LCD, "JN-T280UHD-NS" (4K resolution (28 inches, 3840 dots x 2160 dots)) manufactured by JAPANNEXT Co., Ltd. The LCD was driven to display a white screen, and the rainbow unevenness was visually confirmed when the screen was viewed through a polarizing plate "PZ-2" manufactured by KENIS Co., Ltd. The rainbow unevenness at this time was evaluated according to the following 5-point scale. The higher the evaluation value, the higher the evaluation. 5: No rainbow unevenness is visible no matter what angle you look at the surface from. 4: Faint rainbow irregularities can only be seen when viewing the surface from a specific angle. 3: The rainbow pattern is visible only when the surface is viewed from a specific angle. 2: A faint rainbow pattern can be seen across the entire surface. 1: Rainbow unevenness can be confirmed to the same extent as when there is no antiglare layer. The test results are shown in Tables 1 and 2.
[0153] [Table 1]
[0154] [Table 2]
[0155] As shown in Table 1, it was confirmed that the surfaces 4a, 104a of the antiglare layers 4, 104 in Examples 1 to 6 have an uneven shape in which Safc is a value in the range of 0.02 or more when the short wavelength cutoff value λs is set to 50 μm, and Smr1 is a value in the range of 14% or more when the long wavelength cutoff value λc is set to 25 μm and the short wavelength cutoff value λs is set to 2.6 μm. It was also confirmed that the rainbow unevenness was well improved in Examples 1 to 6. On the other hand, it was confirmed that the Safc of the surface of the antiglare layer in Comparative Examples 1 to 5 is not a value in the range of 0.02 or more, and the Smr1 of the surface of the antiglare layer in Comparative Example 6 is not a value in the range of 14% or more. It was also confirmed that the rainbow unevenness is easily generated in Comparative Examples 1 to 6 compared to Examples 1 to 6.
[0156] Furthermore, as shown in Table 2, it was confirmed that in Examples 1, 7 to 13, the integrated value (D×Re) was within the range of the formula 1. It was also confirmed that in Examples 1, 7 to 13, the rainbow unevenness was relatively well improved. In contrast, it was confirmed that in Comparative Example 7, although the antiglare layer is equivalent to that in Example 1, the integrated value (D×Re) was not within the range of the formula 1. It was also confirmed that in Comparative Example 7, the rainbow unevenness is more likely to occur than in Examples 1, 7 to 13.
[0157] (Disclosure items) Each of the following sections is a disclosure of a preferred embodiment. [Item 1] A substrate film which is a biaxially stretched film that satisfies the relationship shown in Formula 1 and has in-plane birefringence; An antiglare layer disposed on the base film, The surface of the antiglare layer opposite to the substrate film side is The fractal parameter Safc when the short wavelength cutoff value λs is set to 50 μm is a value in the range of 0.02 or more, and An antiglare film having an uneven shape in which Smr1 is a value in the range of 14% or more when the long wavelength cutoff value λc is set to 25 μm and the short wavelength cutoff value λs is set to 2.6 μm. [Formula 1] Substrate film thickness D(m) × retardation Re(m) ≧ 1.0 × 10 -10 (m 2 )
[0158] According to the above configuration, the uneven shape of the surface of the antiglare layer is set to the above-mentioned values of Safc and Smr1, so that the uneven shape is formed to have a distribution structure of steep unevenness with high number density. This scatters the light incident on the surface of the antiglare layer, and appropriately suppresses the reflection of external light on the surface of the antiglare layer. In addition, an excellent antiglare effect is obtained.
[0159] Furthermore, by constructing an antiglare film to include an antiglare layer having the uneven surface and a base film satisfying formula 1, the base film is made of a biaxially oriented film, which maintains sufficient mechanical strength, and an antiglare film that exhibits excellent antiglare effect and rainbow unevenness prevention effect can be realized at low cost.
[0160] [Item 2] 2. The antiglare film according to item 1, wherein the base film comprises a polyester film.
[0161] According to the above-mentioned configuration, an antiglare film having sufficient mechanical strength can be produced at a relatively low cost.
[0162] [Item 3] 3. The antiglare film according to item 1 or 2, wherein the Smr1 of the surface of the antiglare layer opposite to the substrate film side is a value in the range of 50% or less.
[0163] According to the above-mentioned configuration, for example, the ratio of convex portions in the uneven shape of the surface of the antiglare layer can be suppressed, and the mechanical strength of the antiglare film can be easily maintained.
[0164] [Item 4] 4. The antiglare film according to any one of items 1 to 3, wherein the Safc is a value in the range of 1.0 or less.
[0165] According to the above-mentioned configuration, even small characters displayed on the display surface to which the anti-glare film is attached can be easily viewed, thereby achieving excellent anti-glare effect and image display performance.
[0166] [Item 5] 5. The antiglare film according to any one of items 1 to 4, wherein the substrate film thickness D is a value in the range of 50 μm or more and 125 μm or less.
[0167] According to the above configuration, by using a base film having a certain degree of base film thickness D, it is possible to facilitate the handling of materials during the production of the antiglare film, and also to facilitate the realization of an antiglare film having excellent mechanical strength.
[0168] [Item 6] 6. The antiglare film according to any one of items 1 to 5, wherein the antiglare layer contains a plurality of resin components and has a phase-separated structure of the plurality of resin components.
[0169] According to the above-mentioned configuration, the phase separation structure can be used to form the uneven shape of the surface of the anti-glare layer so as to have a structure with steep projections and recesses and a high number density, thereby obtaining an excellent anti-glare effect.
[0170] [Item 7] 7. The antiglare film according to any one of items 1 to 6, wherein the antiglare layer has a microparticle dispersion structure containing a matrix resin and a plurality of microparticles dispersed in the matrix resin.
[0171] According to the above-mentioned configuration, the surface of the anti-glare layer can be formed to have a sharp uneven shape with a high number density by using a fine particle dispersion structure, thereby obtaining an excellent anti-glare effect.
[0172] [Item 8] 8. The antiglare film according to any one of items 1 to 7, further comprising an antireflection layer disposed on the antiglare layer opposite to the substrate film side.
[0173] According to the above-mentioned configuration, the optical characteristics of the antiglare film can be easily adjusted by using the low refractive index layer disposed so as to be superimposed on the antiglare layer.
[0174] [Item 9] An antiglare film according to any one of items 1 to 8, and a polarizing plate disposed so as to be superimposed on the antiglare film.
[0175] [Item 10] An antiglare film according to any one of items 1 to 8, a polarizing plate disposed on the film; a display element disposed on the antiglare film and the polarizing plate.
[0176] Each configuration in each embodiment and their combinations are examples. Addition, omission, substitution, and other modifications of the configuration are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited by the embodiments, but is limited only by the claims. In addition, each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. [Explanation of symbols]
[0177] 1, 20 display device 2, 102, 202, 302, 402 Anti-glare film 3. Base film 4, 104 Anti-glare layer 4a, 104a: Surface of the antiglare layer opposite to the substrate film side 6 Polarizing Plate 9 Anti-reflection layer 10 Optical components 15 Display element 40 Matrix Resin 41 Fine particles
Claims
1. A substrate film which is a biaxially stretched film that satisfies the relationship shown in Formula 1 and has an in-plane birefringence; An antiglare layer disposed on the base film, The surface of the antiglare layer opposite to the substrate film side is The fractal parameter Safc when the short wavelength cutoff value λs is set to 50 μm is a value in the range of 0.02 to 1.00, and An antiglare film having an uneven shape in which Smr1 is a value in the range of 14% or more and 50% or less when the long wavelength cutoff value λc is set to 25 μm and the short wavelength cutoff value λs is set to 2.6 μm. [Formula 1] Substrate film thickness D (m) × retardation Re (m) ≧ 1.0 × 10 -10 (m 2 )
2. The antiglare film according to claim 1 , wherein the substrate film comprises a polyester film.
3. The antiglare film according to claim 1 , wherein the Smr1 of the surface of the antiglare layer opposite to the substrate film side is a value in the range of 30% or less.
4. 2. The antiglare film according to claim 1, wherein the Safc is a value in the range of 0.50 or less.
5. The antiglare film according to claim 1 , wherein the substrate film thickness D is in the range of 50 μm or more and 125 μm or less.
6. The antiglare film according to claim 1 , wherein the antiglare layer contains a plurality of resin components and has a phase-separated structure of the plurality of resin components.
7. The antiglare film according to claim 1 , wherein the antiglare layer has a fine particle dispersion structure containing a matrix resin and a plurality of fine particles dispersed in the matrix resin.
8. The antiglare film according to claim 1 , further comprising an antireflection layer disposed on the antiglare layer opposite to the substrate film side.
9. The antiglare film according to any one of claims 1 to 8, and a polarizing plate disposed so as to be superimposed on the antiglare film.
10. The antiglare film according to any one of claims 1 to 8, a polarizing plate disposed on the antiglare film; a display element disposed on the antiglare film and the polarizing plate.
Citation Information
Patent Citations
JP1975051328A
Antiglare film and method for manufacturing the same
JP2007187746A
Antiglare film, antiglare polarizing plate and image display device
JP2009156938A
Anti-glare film, polarizer, liquid-crystal panel, and image display device