Pressure Sensitive Adhesive Tape

The pressure-sensitive adhesive tape with a specific nonwoven fabric and water-dispersed adhesive layer addresses peeling issues on curved surfaces, enhancing visibility and reliability by optimizing basis weight and thickness.

JP7558684B2Active Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020097020
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-03
Publication Date
2024-10-01
Estimated Expiration
2040-06-03

AI Technical Summary

Technical Problem

Pressure-sensitive adhesive tapes used to adhere objects to curved surfaces risk peeling off due to the elasticity of nonwoven fabrics, compromising visibility and reliability.

Method used

A pressure-sensitive adhesive tape with a nonwoven fabric base material containing a colorant and a pressure-sensitive adhesive layer without a colorant, where the nonwoven fabric has a basis weight of 10-30 g/m² and a thickness of 20-50 μm, and the adhesive layer is water-dispersed, enhancing visibility and reducing peeling.

Benefits of technology

The tape improves visibility and prevents peeling from curved surfaces by balancing the nonwoven fabric's elasticity and adhesive strength, ensuring reliable adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558684000002
    Figure 0007558684000002
  • Figure 0007558684000001
    Figure 0007558684000001
Patent Text Reader

Abstract

To provide an adhesive tape capable of preventing removal from an adherend while improving visibility.SOLUTION: A double-sided pressure-sensitive adhesive tape 1 includes a non-woven fabric substrate 2, and a first pressure-sensitive adhesive layer 3 arranged on one side in a thickness direction of the non-woven fabric substrate 2. The non-woven fabric substrate 2 contains a coloring agent, and the first pressure-sensitive adhesive layer 3 does not contain any coloring agent. A basis weight of the non-woven fabric substrate 2 is adjusted to 10 g / m2 or more and 30 g / m2 or less, and the thickness of the non-woven fabric substrate 2 is adjusted to 20 μm or more and 50 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive tape. [Background technology]

[0002] In various industrial fields, pressure-sensitive adhesive tapes are used to fix objects to adherends. For example, in the manufacture of various industrial products such as automobiles, multiple objects are adhered to the adherends by multiple pressure-sensitive adhesive tapes. However, if the pressure-sensitive adhesive tape is forgotten to be applied, the objects may fall off the adherends, which may reduce the reliability of the product. Therefore, there is a demand for improving the visibility of the pressure-sensitive adhesive tape.

[0003] As such a pressure-sensitive adhesive tape, for example, a pressure-sensitive adhesive sheet has been proposed which includes a nonwoven fabric and an adhesive layer disposed on the nonwoven fabric, the adhesive layer containing a colorant (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-40218 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when adhering an object to an adherend, the pressure-sensitive adhesive tape may be adhered to the curved surface of the adherend. However, when the pressure-sensitive adhesive sheet described in Patent Document 1 is adhered to a curved surface, there is a risk that the pressure-sensitive adhesive sheet will peel off from the curved surface of the adherend due to the elasticity of the nonwoven fabric.

[0006] The present invention provides a pressure-sensitive adhesive tape that can improve visibility while being inhibited from peeling off from an adherend. [Means for solving the problem]

[0007] The present invention [1] comprises a nonwoven fabric substrate and a pressure-sensitive adhesive layer disposed on one side of the nonwoven fabric substrate in a thickness direction, the nonwoven fabric substrate containing a colorant, and the nonwoven fabric substrate has a basis weight of 10 g / m 2 More than 30g / m 2 the thickness of the nonwoven fabric substrate is 20 μm or more and 50 μm or less, and the pressure-sensitive adhesive layer comprises a pressure-sensitive adhesive tape that does not contain a colorant.

[0008] The present invention [2] includes the pressure-sensitive adhesive tape according to the above [1], wherein the pressure-sensitive adhesive layer contains a water-dispersible pressure-sensitive adhesive composition.

[0009] The present invention [3] includes the pressure-sensitive adhesive tape according to [1] or [2] above, which is used for fixing a wire harness. Effect of the Invention

[0010] In the pressure-sensitive adhesive tape of the present invention, the pressure-sensitive adhesive layer does not contain a colorant, while the nonwoven fabric substrate contains a colorant. Since the basis weight of the nonwoven fabric substrate is equal to or greater than the above-mentioned lower limit, and the thickness of the nonwoven fabric substrate is equal to or greater than the above-mentioned lower limit, the visibility of the pressure-sensitive adhesive tape can be improved. Furthermore, since the basis weight of the nonwoven fabric substrate is equal to or less than the above-mentioned upper limit, and the thickness of the nonwoven fabric substrate is equal to or less than the above-mentioned upper limit, the elastic force of the nonwoven fabric substrate can be reduced, and peeling of the pressure-sensitive adhesive tape from the adherend can be suppressed. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing the configuration of a double-sided pressure-sensitive adhesive tape as one embodiment of the pressure-sensitive adhesive tape of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] 1. Double-sided pressure-sensitive adhesive tape A double-sided pressure-sensitive adhesive tape 1 as one embodiment of the pressure-sensitive adhesive tape of the present invention will be described with reference to FIG.

[0013] The double-sided pressure-sensitive adhesive tape 1 comprises a nonwoven fabric substrate 2, a first pressure-sensitive adhesive layer 3, a second pressure-sensitive adhesive layer 4, a first release liner 5, and a second release liner 6.

[0014] The nonwoven fabric substrate 2 is formed by intertwining fibers without weaving them. Examples of the fibers of the nonwoven fabric substrate 2 include natural fibers (e.g., plant fibers such as wood pulp, Manila hemp, and cotton, and animal fibers such as wool and silk), synthetic fibers (e.g., cellulose fibers such as acetate fibers and rayon fibers, polyester fibers, polyamide fibers, and polyvinyl alcohol fibers (vinylon fibers)), and inorganic fibers (e.g., glass fibers, carbon fibers). The fibers can be used alone or in combination of two or more types.

[0015] The fibers preferably include natural fibers and / or synthetic fibers, more preferably include at least one type of fiber selected from the group consisting of vegetable fibers, polyvinyl alcohol-based fibers, and cellulose-based fibers, and even more preferably include at least one type of fiber selected from the group consisting of wood pulp, rayon-based fibers, and polyvinyl alcohol-based fibers.

[0016] The nonwoven fabric substrate 2 includes a colorant. In other words, the nonwoven fabric substrate 2 includes fibers and a colorant.

[0017] Examples of colorants include inorganic pigments (e.g., black pigments such as carbon black, red pigments such as red lead and iron oxide red, yellow pigments such as yellow lead and zinc yellow, blue pigments such as ultramarine blue, Prussian blue, and YInMn blue, white pigments such as zinc oxide, white lead, lithopone, titanium dioxide, and baryte powder), organic pigments, polycyclic pigments, azo pigments, lake pigments, fluorescent pigments, direct dyes (e.g., black dyes such as azo and anthraquinone, red dyes such as azo and anthraquinone, yellow dyes such as azo and anthraquinone, blue dyes such as azo and anthraquinone), reactive dyes, sulfur dyes, basic dyes, acid dyes, metal-containing acid dyes, indigo dyes, threne dyes, disperse dyes, and cationic dyes. Colorants can be used alone or in combination of two or more types.

[0018] The colorant is appropriately selected depending on the color of the adherend. The colorant preferably has a color different from that of the adherend. For example, when the adherend is a ceiling material of a vehicle and has a light color such as white, the colorant preferably has a black color.

[0019] The colorant preferably includes an inorganic pigment, more preferably includes a black pigment, and further preferably includes carbon black. The colorant is preferably made of an inorganic pigment.

[0020] When the colorant contains an inorganic pigment, migration of the colorant from the nonwoven fabric substrate 2 to the first pressure-sensitive adhesive layer 3 and / or the second pressure-sensitive adhesive layer 4 can be prevented, and the colorant can be prevented from contaminating the manufacturing equipment (e.g., rolls, etc.) for the double-sided pressure-sensitive adhesive tape 1.

[0021] The content of the colorant is, for example, 0.05 parts by mass or more, preferably 0.5 parts by mass or more, for example, 2.0 parts by mass or less, preferably 1.5 parts by mass or less, per 100 parts by mass of the fiber (nonwoven fabric substrate before the addition of the colorant).

[0022] When the content of the colorant is equal to or greater than the above lower limit, the visibility of the double-sided pressure-sensitive adhesive tape 1 can be reliably improved.

[0023] The weight of the nonwoven fabric substrate 2 is 10 g / m 2 More than 14 g / m 2 More than 30g / m 2 Preferably, 20 g / m or less 2 The following is the result.

[0024] When the basis weight of the nonwoven fabric substrate 2 is equal to or greater than the above lower limit, it is possible to improve the visibility of the double-sided pressure-sensitive adhesive tape 1. When the basis weight of the nonwoven fabric substrate 2 is equal to or less than the above upper limit, it is possible to reduce the elastic force of the nonwoven fabric substrate 2, thereby improving the adhesion of the double-sided pressure-sensitive adhesive tape 1 to a curved surface. Therefore, it is possible to prevent the double-sided pressure-sensitive adhesive tape 1 from peeling off from a curved surface.

[0025] The thickness of the nonwoven fabric substrate 2 is 20 μm or more, preferably 25 μm or more, more preferably 32 μm or more, and is 50 μm or less, preferably 45 μm or less.

[0026] When the thickness of the nonwoven fabric substrate 2 is equal to or greater than the above lower limit, it is possible to reliably improve the visibility of the double-sided pressure-sensitive adhesive tape 1. When the thickness of the nonwoven fabric substrate 2 is equal to or less than the above upper limit, it is possible to reliably reduce the elastic force of the nonwoven fabric substrate 2, and to reliably improve the adhesion of the double-sided pressure-sensitive adhesive tape 1 to a curved surface. Therefore, it is possible to stably prevent the double-sided pressure-sensitive adhesive tape 1 from peeling off the curved surface.

[0027] The air permeability of the nonwoven fabric substrate 2 is, for example, 0.10 s or more, preferably 0.15 s or more, and for example, 1.00 or less, preferably 0.80 or less, more preferably 0.50 or less. The air permeability is the time it takes for 100 cc of air to pass through a sample in which four nonwoven fabric substrates are laminated, and can be measured in accordance with the method described in JIS P8177:2009 (hereinafter the same).

[0028] The total light transmittance of the nonwoven fabric substrate 2 is, for example, from 5% to 30%. The total light transmittance can be measured in accordance with the method described in JIS K7136 (the same applies below).

[0029] To manufacture such a nonwoven fabric substrate 2, for example, a nonwoven fabric substrate not containing a colorant is immersed in a colorant-containing liquid containing a colorant and then dried. Alternatively, fibers may be colored with a colorant, and then the nonwoven fabric substrate 2 may be formed from the fibers.

[0030] The first pressure-sensitive adhesive layer 3 is disposed on one side in the thickness direction of the nonwoven fabric substrate 2. More specifically, the first pressure-sensitive adhesive layer 3 is disposed on one surface in the thickness direction of the nonwoven fabric substrate 2. The first pressure-sensitive adhesive layer 3 has a flat plate shape (sheet shape). The thickness of the first pressure-sensitive adhesive layer 3 is, for example, 40 μm or more and 80 μm or less.

[0031] The first pressure-sensitive adhesive layer 3 does not contain the above-mentioned colorant. Therefore, the pressure-sensitive adhesive strength of the first pressure-sensitive adhesive layer 3 can be improved compared to when the first pressure-sensitive adhesive layer 3 contains a colorant.

[0032] The first pressure-sensitive adhesive layer 3 includes a pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition is not particularly limited as long as it does not contain a colorant. From the viewpoint of environmental load, the pressure-sensitive adhesive composition is preferably a water-dispersed pressure-sensitive adhesive composition. In other words, the first pressure-sensitive adhesive layer 3 includes a water-dispersed pressure-sensitive adhesive composition, and is preferably made of a water-dispersed pressure-sensitive adhesive composition.

[0033] An example of the water-dispersible pressure-sensitive adhesive composition is the water-dispersible pressure-sensitive adhesive composition described in JP-A-2011-16943.

[0034] The aqueous dispersion type pressure-sensitive adhesive composition contains at least a (meth)acrylic polymer. Here, (meth)acrylic is synonymous with methacrylic and / or acrylic.

[0035] The (meth)acrylic polymer is prepared, for example, by adding an emulsion containing a (meth)acrylic monomer, an emulsifier and water to an initiator solution (described later) containing a polymerization initiator, and emulsion-polymerizing the (meth)acrylic monomer.

[0036] The (meth)acrylic monomer contains an alkyl (meth)acrylate as a main component.

[0037] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having an alkyl group having 1 to 3 carbon atoms (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, etc.), and alkyl (meth)acrylates having an alkyl group having 4 to 12 carbon atoms (e.g., butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, o-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, etc.).

[0038] The alkyl (meth)acrylates can be used alone or in combination of two or more kinds. The alkyl(meth)acrylate includes at least an alkyl(meth)acrylate having an alkyl group having 4 to 12 carbon atoms, and preferably includes an alkyl(meth)acrylate having an alkyl group having 4 to 12 carbon atoms, and an alkyl(meth)acrylate having an alkyl group having 1 to 3 carbon atoms.

[0039] The content ratio of the alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms is, relative to 100 mass% of the (meth)acrylic monomer, for example, 60 mass% or more, preferably 80 mass% or more, for example, 100 mass% or less, preferably 90 mass% or less.

[0040] The content of the alkyl (meth)acrylate having an alkyl group having 1 to 3 carbon atoms is, for example, 0 mass% or more, preferably 5 mass% or more, for example, 35 mass% or less, preferably 15 mass% or less, relative to 100 mass% of the (meth)acrylic monomer.

[0041] The content of the alkyl (meth)acrylate relative to 100 mass% of the (meth)acrylic monomer is, for example, 60 mass% or more, preferably 85 mass% or more, for example, 100 mass% or less, preferably 98 mass% or less.

[0042] Moreover, the (meth)acrylic monomer preferably further contains (meth)acrylic acid and a (meth)acryloyl group-containing alkoxysilane compound.

[0043] The content of (meth)acrylic acid is, for example, 0 mass % or more, preferably 1 mass % or more, for example, 5 mass % or less, preferably 3 mass % or less, relative to 100 mass % of the (meth)acrylic monomer.

[0044] The (meth)acryloyl group-containing alkoxysilane compound contains a (meth)acryloyl group and an alkoxysilyl group.

[0045] Examples of (meth)acryloyl group-containing alkoxysilane compounds include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.

[0046] The (meth)acryloyl group-containing alkoxysilane compounds can be used alone or in combination of two or more kinds.

[0047] The (meth)acryloyl group-containing alkoxysilane compound preferably contains 3-(meth)acryloxypropyltriethoxysilane, and more preferably consists of 3-(meth)acryloxypropyltriethoxysilane.

[0048] The content ratio of the (meth)acryloyl group-containing alkoxysilane compound relative to 100 mass% of the (meth)acrylic monomer is, for example, 0 mass% or more, preferably 0.001 mass% or more, for example, 0.1 mass% or less, preferably 0.05 mass% or less.

[0049] The content of the (meth)acrylic monomer in the emulsion is, for example, 60 mass % or more, preferably 70 mass % or more, for example, 90 mass % or less, preferably 80 mass % or less.

[0050] Examples of emulsifiers include anionic emulsifiers (e.g., sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene alkyl phenyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, etc.), and nonionic emulsifiers (e.g., polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, etc.).

[0051] Furthermore, as the emulsifier, a radically polymerizable emulsifier in which a radically polymerizable group (for example, a propenyl group) has been introduced into the above-mentioned anionic emulsifier or the above-mentioned nonionic emulsifier can also be used.

[0052] The emulsifiers can be used alone or in combination of two or more kinds.

[0053] The emulsifier preferably comprises an anionic emulsifier, preferably sodium polyoxyethylene alkyl ether sulfate. The emulsifier preferably consists of an anionic emulsifier.

[0054] The content of the emulsifier in the emulsion is, for example, 0.01 mass % or more, preferably 0.5 mass % or more, for example, 5.0 mass % or less, preferably 3.0 mass % or less.

[0055] The content ratio of the emulsifier relative to 100 parts by mass of the (meth)acrylic monomer is, for example, 0.5 parts by mass or more, preferably 1.0 part by mass or more, for example, 5.0 parts by mass or less, preferably 3.0 parts by mass or less.

[0056] The water content in the emulsion is, for example, 5 mass % or more, preferably 10 mass % or more, for example, 35 mass % or less, preferably 25 mass % or less.

[0057] The water content is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, for example, 50 parts by mass or less, preferably 40 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic monomer.

[0058] The emulsion preferably further contains a chain transfer agent.

[0059] Examples of the chain transfer agent include mercaptans such as dodecyl mercaptan (dodecanethiol), glycidyl mercaptan, and 2-mercaptoethanol.

[0060] The chain transfer agents can be used alone or in combination of two or more kinds.

[0061] The chain transfer agent preferably comprises, and more preferably consists of, dodecanethiol.

[0062] The content of the chain transfer agent in the emulsion is, for example, from 0% by mass to 0.5% by mass.

[0063] The content ratio of the chain transfer agent relative to 100 parts by mass of the (meth)acrylic monomer is, for example, 0 part by mass or more, preferably 0.01 part by mass or more, for example, 0.5 parts by mass or less, preferably 0.05 parts by mass or less.

[0064] Examples of the polymerization initiator include an azo-based initiator, a peroxide-based initiator, and a redox-based initiator that combines a peroxide and a reducing agent.

[0065] Examples of azo initiators include 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate, 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylpropionamidine)disulfate, 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, and 2,2'-azobis(N,N'-dimethyleneisobutylamidine)dihydrochloride.

[0066] Examples of peroxide initiators include persulfates (eg, potassium persulfate, ammonium persulfate, etc.), benzoyl peroxide, t-butyl hydroperoxide, and hydrogen peroxide.

[0067] Examples of the redox initiator include a combination of a persulfate and sodium hydrogen sulfite, and a combination of hydrogen peroxide and sodium ascorbate.

[0068] The polymerization initiators can be used alone or in combination of two or more kinds.

[0069] As the polymerization initiator, an azo-based initiator and a redox-based initiator are preferably used in combination.

[0070] When an azo-based initiator and a redox-based initiator are used in combination, first, the above-mentioned emulsion is added to an initiator solution containing an azo-based initiator, and the (meth)acrylic monomer is emulsion-polymerized.

[0071] The mixing ratio of the azo-based initiator is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, for example, 0.5 parts by mass or less, preferably 0.2 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic monomer.

[0072] The polymerization temperature in the presence of an azo-based initiator is, for example, 20°C or more, preferably 40°C or more, for example, 100°C or less, preferably 80°C or less.

[0073] Next, a peroxide as a redox initiator is added to the emulsion polymerization reaction liquid. The mixing ratio of the peroxide is, for example, 0.03 parts by mass or more, preferably 0.05 parts by mass or more, for example, 0.2 parts by mass or less, preferably 0.1 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic monomer.

[0074] Next, a reducing agent for the redox initiator is added to the reaction solution to which the peroxide has been added, to carry out a redox treatment. The mixing ratio of the reducing agent is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, for example, 1.0 parts by mass or less, preferably 0.8 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic monomer.

[0075] The temperature range for the redox treatment is, for example, the same as the temperature range for polymerization in the presence of an azo-based initiator.

[0076] As a result, a (meth)acrylic polymer, which is a polymerization product of the (meth)acrylic monomer, is produced, and a (meth)acrylic polymer emulsion containing the (meth)acrylic polymer and water is prepared.

[0077] Also, a first pressure-sensitive adhesive layer 3 containing a pressure-sensitive adhesive composition is prepared from a (meth)acrylic polymer emulsion.

[0078] The acrylic polymer emulsion is cooled to room temperature (25° C.) as needed. A pH adjuster (e.g., ammonia water, etc.) is added to the acrylic polymer emulsion as needed. This adjusts the pH of the acrylic polymer emulsion to, for example, 5.0 or more and 8.0 or less.

[0079] The solid content concentration (NV) of the acrylic polymer emulsion is, for example, 30 mass % or more, preferably 40 mass % or more, for example, 70 mass % or less, preferably 60 mass % or less.

[0080] The average particle size of the acrylic polymer emulsion is, for example, 100 nm or more and 300 nm or less.

[0081] The (meth)acrylic polymer emulsion is then applied, for example, onto the nonwoven fabric substrate 2 or the first release liner 5, and then dried as necessary.

[0082] In this manner, the first pressure-sensitive adhesive layer 3 containing the water-dispersible pressure-sensitive adhesive composition is prepared.

[0083] The aqueous dispersion type pressure-sensitive adhesive composition preferably contains a tackifier in addition to the above-mentioned (meth)acrylic polymer. In this case, the tackifier is added to the (meth)acrylic polymer emulsion.

[0084] Examples of the tackifier include rosin-based resins, rosin derivative resins, petroleum-based resins, terpene-based resins, phenol-based resins, and ketone-based resins.

[0085] The tackifiers can be used alone or in combination of two or more kinds.

[0086] Of the tackifiers, preferably, a rosin-based resin is used.

[0087] The content ratio of the tackifier relative to 100 parts by mass of the (meth)acrylic polymer is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, for example, 40 parts by mass or less, preferably 30 parts by mass or less.

[0088] Furthermore, the aqueous dispersion type pressure-sensitive adhesive composition may contain known additives such as viscosity modifiers, leveling agents, plasticizers, fillers, stabilizers, preservatives, and antioxidants in appropriate proportions, as necessary.

[0089] The second pressure-sensitive adhesive layer 4 is disposed on the other side in the thickness direction of the nonwoven fabric substrate 2. More specifically, the second pressure-sensitive adhesive layer 4 is disposed on the other surface in the thickness direction of the nonwoven fabric substrate 2. The second pressure-sensitive adhesive layer 4 will be described in the same manner as the first pressure-sensitive adhesive layer 3. Therefore, a description of the second pressure-sensitive adhesive layer 4 will be omitted.

[0090] The first release liner 5 is located on the opposite side of the nonwoven fabric substrate 2 with respect to the first pressure-sensitive adhesive layer 3. Before use of the double-sided pressure-sensitive adhesive tape 1, the first release liner 5 is releasably attached to one surface in the thickness direction of the first pressure-sensitive adhesive layer 3 in order to protect the first pressure-sensitive adhesive layer 3. The first release liner 5 has a flat plate shape (sheet shape). The first release liner 5 is formed from a flexible resin film. Examples of the resin film include fluorine-based films such as polytetrafluoroethylene, polyolefin films such as polyethylene and polypropylene, and polyester films such as polyethylene terephthalate.

[0091] The adhesive surface of the first release liner 5 is, if necessary, surface-treated with a release treatment agent. Examples of the release treatment agent include silicone-based release treatment agents, long-chain alkyl-based release treatment agents, fluorine-based release treatment agents, molybdenum sulfide-based release treatment agents, etc. The release treatment agents can be used alone or in combination of two or more kinds.

[0092] When the double-sided pressure-sensitive adhesive tape 1 is used, the first release liner 5 is peeled off from the first pressure-sensitive adhesive layer 3. The exposed first pressure-sensitive adhesive layer 3 is then pressure-sensitively adhered to an adherend or object.

[0093] The second release liner 6 is located on the opposite side of the nonwoven fabric substrate 2 with respect to the second pressure-sensitive adhesive layer 4. The second pressure-sensitive adhesive layer 4 is releasably attached to the other surface in the thickness direction of the second pressure-sensitive adhesive layer 4 in order to protect the second pressure-sensitive adhesive layer 4 before use of the double-sided pressure-sensitive adhesive tape 1. The second release liner 6 will be described in the same manner as the first release liner 5. Therefore, a description of the second release liner 6 will be omitted. The second release liner 6 is peeled off from the second pressure-sensitive adhesive layer 4 when the double-sided pressure-sensitive adhesive tape 1 is used. The exposed second pressure-sensitive adhesive layer 4 is then pressure-sensitively adhered to an adherend or object.

[0094] To produce such a double-sided pressure-sensitive adhesive tape 1, for example, the above-mentioned (meth)acrylic polymer emulsion is applied onto a first release liner 5 by a known application method. Thereafter, the coating of the (meth)acrylic polymer emulsion is dried as necessary to form a first pressure-sensitive adhesive layer 3.

[0095] Next, the first pressure-sensitive adhesive layer 3 on the first release liner 5 is pressure-bonded to one surface in the thickness direction of the nonwoven fabric substrate 2 so that the first pressure-sensitive adhesive layer 3 is in direct contact with one surface in the thickness direction of the nonwoven fabric substrate 2.

[0096] Next, the above-mentioned (meth)acrylic polymer emulsion is directly applied by a known application method to the other surface in the thickness direction of the nonwoven fabric substrate 2. Thereafter, the coating film is dried as necessary to form a second pressure-sensitive adhesive layer 4.

[0097] A second release liner 6 is then pressed onto the opposite side of the nonwoven fabric substrate 2 from the second pressure-sensitive adhesive layer 4 .

[0098] In this manner, the double-sided adhesive tape 1 is manufactured.

[0099] The double-sided adhesive tape 1 comprises, in the thickness direction of the nonwoven fabric substrate 2, a second release liner 6, a second pressure-sensitive adhesive layer 4, the nonwoven fabric substrate 2, a first pressure-sensitive adhesive layer 3, and a first release liner 5 in that order.

[0100] Such a double-sided pressure-sensitive adhesive tape 1 is used, for example, in the manufacture of various industrial products, and is preferably used in the manufacture of automobiles. More specifically, the double-sided pressure-sensitive adhesive tape 1 is preferably used when fixing automobile parts (e.g., wire harnesses) to vehicle frames having curved surfaces. In other words, the double-sided adhesive tape 1 is used to fix automobile parts (wire harnesses).

[0101] When the double-sided pressure-sensitive adhesive tape 1 is used, as described above, the first release liner 5 is peeled off from the first pressure-sensitive adhesive layer 3, and the second release liner 6 is peeled off from the second pressure-sensitive adhesive layer 4. Therefore, when the double-sided adhesive tape 1 is in use, the tape body 1A comprising the nonwoven fabric substrate 2, the first pressure-sensitive adhesive layer 3, and the second pressure-sensitive adhesive layer 4, but not the first release liner 5 or the second release liner 6, is attached to an adherend.

[0102] In the double-sided pressure-sensitive adhesive tape 1, the first pressure-sensitive adhesive layer 3 and the second pressure-sensitive adhesive layer 4 do not contain a colorant, while the nonwoven fabric substrate 2 contains a colorant. The basis weight of the nonwoven fabric substrate 2 is equal to or greater than the above-mentioned lower limit, and the thickness of the nonwoven fabric substrate 2 is equal to or greater than the above-mentioned lower limit. Therefore, when the double-sided adhesive tape 1 (specifically, the tape body 1A) is attached to the curved surface of the adherend, the visibility of the tape body 1A can be improved. Furthermore, since the basis weight of the nonwoven fabric substrate 2 is equal to or less than the above-mentioned upper limit, and the thickness of the nonwoven fabric substrate 2 is equal to or less than the above-mentioned upper limit, even when the double-sided adhesive tape 1 (specifically, the tape body 1A) is attached to the curved surface of the adherend, the elastic force of the nonwoven fabric substrate 2 can be reduced, and the tape body 1A can be prevented from peeling off from the adherend.

[0103] 3. Variations As shown in FIG. 1, the double-sided pressure-sensitive adhesive tape 1 comprises a nonwoven fabric substrate 2, a first pressure-sensitive adhesive layer 3, a second pressure-sensitive adhesive layer 4, a first release liner 5, and a second release liner 6, but the pressure-sensitive adhesive tape of the present invention is not particularly limited as long as it comprises a nonwoven fabric substrate 2 and a first pressure-sensitive adhesive layer 3.

[0104] The pressure-sensitive adhesive tape may be comprised of a nonwoven fabric substrate 2 and a first pressure-sensitive adhesive layer 3. The pressure-sensitive adhesive tape may be comprised of a nonwoven fabric substrate 2, a first pressure-sensitive adhesive layer 3, and a first release liner 5. The pressure-sensitive adhesive tape may be comprised of a nonwoven fabric substrate 2, a first pressure-sensitive adhesive layer 3, and a second pressure-sensitive adhesive layer 4. The pressure-sensitive adhesive tape may be comprised of a nonwoven fabric substrate 2, a first pressure-sensitive adhesive layer 3, a second pressure-sensitive adhesive layer 4, and a first release liner 5.

[0105] Even with such a modification, the same effects as those of the above-described embodiment can be achieved. EXAMPLES

[0106] The present invention will be described in more detail below with reference to preparatory examples, examples, and comparative examples. The present invention is not limited to the preparatory examples, examples, and comparative examples. The specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".

[0107] <Preparation of nonwoven fabric substrate> <<Preparation Example 1>> Nonwoven fabric A (material: pulp / rayon / vinyl binder, product name: synthetic fiber paper, black, 14.0 g / m 2 The nonwoven fabric was dyed by adding 1 part by mass of black pigment (carbon black) to 100 parts by mass of the polyester fiberboard (manufactured by Nippon Paper Papylia Co., Ltd.). In this way, a nonwoven fabric substrate was obtained. The breathability, basis weight and thickness of the nonwoven fabric substrate are shown in Table 1.

[0108] <<Preparation Example 2>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2A nonwoven fabric base material was obtained in the same manner as in Preparation Example 1, except that Nonwoven Fabric B (material: pulp, product name: No. 4134, manufactured by Daifuku Paper Co., Ltd.) was used instead of Nonwoven Fabric A (material: pulp, product name: No. 4134, manufactured by Daifuku Paper Co., Ltd.).

[0109] <<Preparation Example 3>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that Nonwoven Fabric C (material: pulp, product name: NTO-16P-Black, manufactured by Daifuku Paper Co., Ltd.) was used instead of Nonwoven Fabric A (material: pulp, product name: NTO-16P-Black, manufactured by Daifuku Paper Co., Ltd.).

[0110] <<Preparation Example 4>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 (manufactured by Nippon Paper Papylia Co., Ltd.) was used. 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that the polyester fiber reinforced plastic (manufactured by Nippon Paper Papylia Co., Ltd.) was used.

[0111] <<Preparation Example 5>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that Nonwoven Fabric E (material: pulp, manufactured by Fujiko Co., Ltd.) was used instead of Nonwoven Fabric A (material: pulp, manufactured by Fujiko Co., Ltd.).

[0112] <<Preparation Example 6>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that nonwoven fabric F was used instead of nonwoven fabric 1 (manufactured by Nippon Paper Papylia Co., Ltd.).

[0113] <<Preparation Example 7>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 (manufactured by Nippon Paper Papylia Co., Ltd.) was placed on nonwoven fabric G (material: polyester, product name: PET paper 30 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that the polyester fiber reinforced plastic (manufactured by Nippon Paper Papylia Co., Ltd.) was used.

[0114] <<Preparation Example 8>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that nonwoven fabric H (material: pulp, product name: F-18 processed paper, manufactured by Nippon Paper Papylia Co., Ltd.) was changed to nonwoven fabric H (material: pulp, product name: F-18 processed paper, manufactured by Nippon Paper Papylia Co., Ltd.).

[0115] <<Preparation Example 9>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that Nonwoven Fabric I (material: pulp, product name: MM Base Paper, manufactured by Miki Tokushu Paper Co., Ltd.) was used instead of Nonwoven Fabric I (material: pulp, product name: MM Base Paper, manufactured by Miki Tokushu Paper Co., Ltd.).

[0116] <<Preparation Example 10>> Nonwoven fabric A (Product name: Chemical fiber paper, black, 14.0 g / m 2 A nonwoven fabric substrate was obtained in the same manner as in Preparation Example 1, except that Nonwoven Fabric J (material: pulp, product name: NTO-16P-Black, manufactured by Daifuku Paper Co., Ltd.) was used instead of Nonwoven Fabric 1 (material: pulp, product name: NTO-16P-Black, manufactured by Daifuku Paper Co., Ltd.).

[0117] <<Examples 1 to 5 and Comparative Examples 1 to 4>> 60 parts by mass of distilled water and 0.1 parts by mass of an emulsifier (polyoxyethylene alkyl ether sodium sulfate, product name: LATEMURU E-118B, manufactured by Kao Corporation) were added to a reaction vessel. The reaction vessel was equipped with a vessel body, a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube.

[0118] Next, 0.1 parts by mass of a polymerization initiator (2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate, product name: VA-057, manufactured by Wako Pure Chemical Industries, Ltd.) was added to the reaction vessel.

[0119] In addition, an emulsion was prepared by mixing and emulsifying 85 parts by mass of 2-ethylhexyl acrylate, 13 parts by mass of methyl acrylate, 1.5 parts by mass of acrylic acid, 0.5 parts by mass of methacrylic acid, 0.02 parts by mass of 3-methacryloxypropyltrimethoxysilane (product name: KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.), 0.033 parts by mass of a chain transfer agent (dodecanethiol), 1.9 parts by mass of the above emulsifier, and 28.6 parts by mass of distilled water.

[0120] Next, the temperature of the emulsion was adjusted to 60° C. Then, the emulsion was gradually added dropwise to the reaction vessel over 4 hours to carry out emulsion polymerization. Thereafter, the reaction solution was stirred at 60° C. for 3 hours, and heating of the reaction solution was stopped.

[0121] Next, 0.75 parts by mass of 10% by mass hydrogen peroxide solution was added to the reaction solution. After that, the reaction solution was stirred for 5 minutes. Then, 0.5 parts by mass of sodium ascorbate was added to the reaction solution to perform a redox treatment. Then, the reaction solution was cooled to room temperature (25°C). 10% by mass ammonia water was added to the reaction solution after cooling to adjust the pH of the reaction solution to 6.5.

[0122] This resulted in the production of a (meth)acrylic polymer emulsion. The solid content (NV) of the (meth)acrylic polymer emulsion was about 51% by mass. The average particle size of the emulsion was about 200 nm.

[0123] Next, 10 parts by mass (solid content equivalent) of a first water-dispersible rosin resin (product name: Super Ester KE-802, manufactured by Arakawa Chemical Industries, Ltd.) and 10 parts by mass of a second water-dispersible rosin resin (product name: Super Ester NS-100H, manufactured by Arakawa Chemical Industries, Ltd.) were added to the (meth)acrylic polymer emulsion.

[0124] Then, a pH adjuster (10% by mass ammonia water) and a thickener (polyacrylic acid) were added to the (meth)acrylic polymer emulsion. The pH of the (meth)acrylic polymer emulsion was 7.2. The viscosity of the (meth)acrylic polymer emulsion was 8 Pa s.

[0125] Next, the (meth)acrylic polymer emulsion was applied to the surface of a first release liner (product name: SLB-80WD(V2), manufactured by Kaito Chemical Industry Co., Ltd.) The front and back surfaces of the first release liner had been treated with a silicone-based release agent.

[0126] The (meth)acrylic polymer emulsion coating was then dried for 2 minutes at 100° C. This resulted in a first pressure-sensitive adhesive layer made of the water-dispersed acrylic pressure-sensitive adhesive composition. The thickness of the first pressure-sensitive adhesive layer was approximately 60 μm.

[0127] The first pressure-sensitive adhesive layer on the first release liner was then placed on the nonwoven fabric so that the first pressure-sensitive adhesive layer was in direct contact with the surface of the nonwoven fabric of each Preparation Example, so that the nonwoven fabric, the first pressure-sensitive adhesive layer, and the first release liner were laminated in order in the thickness direction of the nonwoven fabric.

[0128] Next, a (meth)acrylic polymer emulsion containing a water-dispersible rosin resin, a pH adjuster, and a thickener was directly applied to the back surface of the nonwoven fabric. The coating of the (meth)acrylic polymer emulsion was then dried at 100°C for 2 minutes. This resulted in the formation of a second pressure-sensitive adhesive layer made of a water-dispersible acrylic pressure-sensitive adhesive composition. The thickness of the second pressure-sensitive adhesive layer was approximately 60 μm.

[0129] A second release liner was then attached to the opposite side of the nonwoven fabric substrate from the second pressure-sensitive adhesive layer, thereby obtaining a laminate. 2 The laminate was provided with a release liner, a second pressure-sensitive adhesive layer, a nonwoven fabric, a first pressure-sensitive adhesive layer, and a first release liner in that order in the thickness direction of the nonwoven fabric. The laminate was then kept in an oven at 50° C. for 24 hours.

[0130] In this way, a double-sided pressure-sensitive adhesive tape was obtained.

[0131] <<Comparative Example 5>> A double-sided pressure-sensitive adhesive tape was obtained in the same manner as in Example 1, except that the water-dispersed acrylic pressure-sensitive adhesive composition contained a black pigment and the nonwoven fabric substrate of Preparatory Example 1 was changed to the nonwoven fabric substrate of Preparatory Example 5. The black pigment was added to the (meth)acrylic polymer emulsion. The proportion of the black pigment added was 10 parts by mass relative to 100 parts by mass of the (meth)acrylic monomer.

[0132] evaluation (Visibility) The double-sided pressure-sensitive adhesive tape of each Example and Comparative Example was cut to a size of 10 cm x 10 cm. The first release liner was then peeled off from the first pressure-sensitive adhesive layer. The first pressure-sensitive adhesive layer was then attached to a white polystyrene film. The white polystyrene film was L * :88.85,a * :0.45, b * :-5.76.

[0133] The second release liner was then peeled off from the second pressure-sensitive adhesive layer. The color of the double-sided pressure-sensitive adhesive tape (tape body) was measured from the opposite side of the nonwoven fabric substrate to the second pressure-sensitive adhesive layer. The color was measured using a multi-angle spectrophotometer (MA68II, manufactured by X-rite). The measurement angle was 45°.

[0134] The color of the double-sided pressure-sensitive adhesive tape was evaluated according to the following criteria. The results are shown in Table 1. 〇:L * is less than 40. ×:L * has exceeded 40.

[0135] (Adhesion (resilience)) The adhesion (repulsion resistance) of each of the double-sided pressure-sensitive adhesive tapes of the Examples and Comparative Examples was evaluated by the repulsion resistance test (foam repulsion resistance test) described in JP 2015-218283 A.

[0136] Specifically, in the double-sided pressure-sensitive adhesive tapes of each Example and Comparative Example, the first release liner was peeled off from the first pressure-sensitive adhesive layer. Then, a soft urethane foam (product name: ECS (gray)) was attached to the first pressure-sensitive adhesive layer. After that, a 1 kg roller was brought into contact with the soft urethane foam from the side opposite the first pressure-sensitive adhesive layer, and the 1 kg roller was moved back and forth once.

[0137] This resulted in a laminate, which in turn comprised a second release liner, a second pressure-sensitive adhesive layer, a nonwoven fabric substrate, a first pressure-sensitive adhesive layer, and a soft urethane foam.

[0138] The laminate was then held at 23° C. for 24 hours, and then cut to a size of 10 mm wide x 50 mm long to obtain a sample.

[0139] The second release liner was then peeled off from the second pressure-sensitive adhesive layer of the sample. An ABS plate was then attached to a first portion of the sample from one end of the second pressure-sensitive adhesive layer to 10 mm in the longitudinal direction. A 2 kg roller was then brought into contact with the ABS plate from the side opposite the second pressure-sensitive adhesive layer, and the 2 kg roller was moved back and forth once.

[0140] The sample was then folded back, and the second portion of the second pressure-sensitive adhesive layer other than the first portion was attached to the back surface of the ABS plate. The sample attached to the ABS plate was then left in an environment of 23°C and 50% RH for 24 hours.

[0141] The adhesion (resilience) of the double-sided pressure-sensitive adhesive tape was evaluated based on whether or not the first portion of the second pressure-sensitive adhesive layer peeled off from the ABS plate. If the first portion of the second pressure-sensitive adhesive layer peeled off from the ABS plate, the adhesion (resilience) of the double-sided pressure-sensitive adhesive tape was rated as ×. If the first portion of the second pressure-sensitive adhesive layer did not peel off from the ABS plate, the adhesion (resilience) of the double-sided pressure-sensitive adhesive tape was rated as ◯. The results are shown in Table 1.

[0142] [Table 1] [Explanation of symbols]

[0143] 1 Double-sided pressure-sensitive adhesive tape 2 Nonwoven fabric base material 3 First Pressure Sensitive Adhesive Layer 4 Second Pressure Sensitive Adhesive Layer 5 First release liner 6 Second release liner

Claims

1. A nonwoven fabric substrate; A pressure-sensitive adhesive layer is disposed on at least one side of the nonwoven fabric substrate in a thickness direction, The nonwoven fabric substrate includes a colorant, The weight of the nonwoven fabric substrate is 10 g / m 2 30g / m or more 2 is as follows: The thickness of the nonwoven fabric substrate is 20 μm or more and 50 μm or less, The content ratio of the colorant is 0.05 parts by mass or more and 2.0 parts by mass or less with respect to 100 parts by mass of the nonwoven fabric substrate before the addition of the colorant, The pressure-sensitive adhesive layer does not contain a colorant, The colorant includes an inorganic pigment, The pressure-sensitive adhesive layer comprises a water-dispersible pressure-sensitive adhesive composition, The aqueous dispersion type pressure-sensitive adhesive composition contains a (meth)acrylic polymer, The (meth)acrylic polymer is a polymer of a (meth)acrylic monomer, A pressure-sensitive adhesive tape, wherein the (meth)acrylic monomer contains an alkoxysilane compound containing a (meth)acryloyl group.

2. L * : 88.85, a * : 0.45, b * The color of the pressure-sensitive adhesive tape attached to a white polystyrene film having a color of -5.76 at a measurement angle of 45° is L * 2. The pressure-sensitive adhesive tape of claim 1, wherein the viscosity is 40 or less.

3. 3. The pressure-sensitive adhesive tape according to claim 1, wherein the pressure-sensitive adhesive layer comprises a water-dispersible pressure-sensitive adhesive composition.

4. The pressure-sensitive adhesive tape according to any one of claims 1 to 3, which is used for fixing a wire harness.

Citation Information

Patent Citations

  • Wire harnessing tape

    EP1932892A1

  • Adhesive sheet and speaker

    JP2015025041A

  • Adhesive sheet and speaker

    JP2015040218A

  • Adhesive sheet and loudspeaker

    JP2015105319A

  • Adhesive tape

    JP2015221846A