Toner manufacturing method

The method of using a water-insoluble grinding agent and binder to crush pigments for toner production addresses the productivity issues of solvent salt milling by eliminating the need for solvent removal and drying, while maintaining performance properties.

JP7558790B2Active Publication Date: 2024-10-01CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020209350
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-17
Publication Date
2024-10-01
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Conventional solvent salt milling methods for reducing pigment particle size in toner production require additional processes to remove water-soluble inorganic salts and solvents, leading to decreased productivity.

Method used

A method involving the use of a water-insoluble grinding agent and binder to crush pigments, followed by melt-kneading and optional polymerization or aggregation steps to produce toner particles without the need for solvent removal and drying processes.

Benefits of technology

This approach allows for the reduction of pigment particle size without the need for additional cleaning and drying steps, maintaining charge retention, low-temperature fixing properties, and improving coloring power.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558790000001
    Figure 0007558790000001
  • Figure 0007558790000002
    Figure 0007558790000002
  • Figure 0007558790000003
    Figure 0007558790000003
Patent Text Reader

Abstract

To provide a toner manufacturing method which does not require removal of a grinding agent and binder and allows for reducing the particle size of a pigment dispersed in a toner.SOLUTION: A toner manufacturing method provided herein comprises a pigment crushing step for kneading a pigment, binder and grinding agent to obtain a pigment dispersion having the grinding agent and the crushed pigment dispersed in the binder, and a step for obtaining toner particles by a predetermined method using the pigment dispersion, where the obtained toner particles contain the binder and the grinding agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, and a toner jet system. [Background technology]

[0002] In recent years, full-color electrophotographic copiers have become widespread and have begun to be applied to the printing market. In the printing market, high speed, high image quality, and high productivity are required while handling a wide range of media (paper types). In order to achieve high image quality, further expansion of coloring power is required, and for this purpose, reducing the particle size of the pigment is effective (Patent Document 1). Thus, as a method for reducing the particle size of the pigment, the solvent salt milling method has been conventionally known (Patent Document 2). The solvent salt milling method is a method in which a pigment having a large particle size is kneaded with a water-soluble inorganic salt as a grinding agent and a water-soluble organic solvent as a binder to disintegrate the pigment and obtain a pigment having a small particle size. However, when applied to the production of toner, a washing process for removing the water-soluble inorganic salt and the water-soluble organic solvent, and an accompanying drying process are also required, which significantly deteriorates productivity. Therefore, a milling method that does not use an organic solvent as a binder is required. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-20244 A [Patent Document 2] Japanese Patent Application Publication No. 3-84067 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to solve the above problems, that is, to provide a method for producing a toner which does not require the removal of a grinding agent and a binder and can reduce the particle size of a pigment dispersed in the toner. [Means for solving the problem]

[0005] The present invention includes a pigment disintegration step of kneading a pigment, a binder, and a grinding agent to obtain a pigment dispersion in which the grinding agent and the disintegrated pigment are dispersed in the binder; A step of obtaining toner particles using the pigment dispersion by at least one of the following methods (i) to (v): A method for producing a toner comprising the steps of: The binder is a water-insoluble thermoplastic component that is solid at 25° C. The grinding agent is water-insoluble and has a number-average particle size of 0.1 to 5 μm; The proportion of the binder is 5 to 50 mass% based on the mass of the pigment dispersion, a mass ratio of the pigment to the grinding agent in the pigment dispersion is 0.2 to 1.5; In the pigment crushing step, kneading is carried out at a temperature at which the melt viscosity of the binder is 6000 Pa sec or less, The toner particles contain the binder and the grinding agent.

[0006] (i) A method of obtaining toner particles through a step of melt-kneading the pigment dispersion and a resin A, and a step of pulverizing the obtained kneaded product.

[0007] (ii) A method for obtaining toner particles through a step of preparing a resin solution in which the pigment dispersion and resin A are dissolved in an organic solvent, a step of dispersing the obtained resin solution in an aqueous medium and granulating it to form droplet particles A, and a step of removing the organic solvent contained in the droplet particles A.

[0008] (iii) A method for obtaining toner particles containing resin A formed by polymerization of the polymerizable monomer, through a step of mixing the pigment dispersion with a polymerizable monomer to prepare a polymerizable monomer composition, a step of dispersing the polymerizable monomer composition in an aqueous medium and granulating it to form droplet particles B, and a step of polymerizing the polymerizable monomer contained in the droplet particles B.

[0009] (iv) A method of obtaining toner particles through a step of mixing a dispersion liquid containing fine particles of the pigment dispersion with a dispersion liquid containing fine particles containing resin A, aggregating the fine particles to form aggregate particles, and heating the aggregate particles to fuse them.

[0010] (v) A method for obtaining toner particles through a step of preparing a resin composition containing the pigment dispersion and resin A, a step of preparing a dispersion containing fine particles of the resin composition, aggregating the fine particles to form aggregate particles, and a step of heating and fusing the aggregate particles. Effect of the Invention

[0011] According to the present invention, it is possible to provide a method for producing a toner which does not require the removal of a grinding agent and a binder and which is capable of reducing the particle size of a pigment dispersed in the toner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In order to improve coloring power, it is necessary to reduce the particle size of pigments, but in the conventional solvent salt milling method, it is necessary to remove the grinding agent and binder, and the additional washing process for removing them and the accompanying drying process reduce productivity. As a result of the inventors' further investigation, they have succeeded in producing a toner without adding any additional process by crushing the pigment using a water-insoluble grinding agent and a water-insoluble binder to obtain a pigment dispersant, and using this to produce toner particles.

[0013] In the present invention, it is important to use water-insoluble particles having a number-average particle size of 0.1 μm to 5.0 μm as the grinding agent. By setting the above range, even if the grinding agent is contained in the toner, the charge retention, low-temperature fixability, and coloring power are not impaired. Furthermore, the binder is a thermoplastic component that is water-insoluble and solid at 25° C. Using such a binder, kneading is performed in a state where the melt viscosity is 6000 Pa·sec or less. In this case, since it is solid before kneading, it is easy to handle, and by reducing the viscosity during kneading, it functions as a binder, and even if it is contained in the toner, blocking resistance and charge retention are not impaired.

[0014] Furthermore, by setting the proportion of the binder to 5 to 50 mass % based on the mass of the pigment dispersion, a uniform dispersion state is obtained for disintegrating the pigment with the grinding agent, and a strong shear force is applied to the pigment by the grinding agent, so that the pigment is efficiently disintegrated.

[0015] In addition, by setting the mass ratio of pigment to grinding agent in the pigment dispersion to 0.2 to 1.5, the amount of grinding agent contained in the toner is reduced without impairing the pigment grindability, and the charge retention, low-temperature fixability, and coloring power are not impaired.

[0016] <Manufacturing method for pigment crushing process> Next, the procedure of the pigment crushing step for obtaining a pigment dispersion in the production method of the present invention will be described, but the present invention is not limited to this, and the details are not particularly important as long as it is a melt-kneading method in which a heating mechanism for melting the binder is provided, the pigment is crushed, and a pigment dispersion is obtained.

[0017] It is preferable to first mix the pigment, grinding agent, and binder uniformly and then perform kneading. As a process for uniformly mixing, the raw material mixing process will be described. In the raw material mixing process, at least the pigment, grinding agent, and binder are weighed in predetermined amounts, mixed, and mixed. Examples of mixing devices include double con mixers, V-type mixers, drum mixers, super mixers, Henschel mixers, and Nauta mixers.

[0018] The mixed raw materials are then fed into a melt kneader and melt kneaded at a temperature at which the melt viscosity of the binder is 6000 Pa·sec or less. In this melt kneading process, the pigment is disintegrated by the grinding agent in the melt kneader to obtain a pigment dispersion. In the melt kneading process, for example, a batch kneader such as a kneader, a pressure kneader, or a Banbury mixer, or a continuous kneader can be used, but it is preferable to use a twin-screw kneading extruder.

[0019] <Raw materials for pigment dispersions> Next, the raw materials used in preparing the pigment dispersant will be described. The raw materials include at least a pigment, a water-insoluble grinding agent, and a water-insoluble binder.

[0020] <Pigments> Examples of pigments that can be contained in the pigment dispersion include the following.

[0021] Examples of the pigment include known organic pigments and carbon black.

[0022] Examples of cyan pigments include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds.

[0023] Examples of magenta pigments include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds.

[0024] Examples of yellow pigments include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds.

[0025] Examples of black pigments include carbon black and pigments toned to black using the above-mentioned yellow pigments, magenta pigments, and cyan pigments.

[0026] The pigments may be used alone or in combination of two or more.

[0027] The pigment before the pigment crushing step is a coarsely crushed pigment, and has a number-average particle size of about 80 nm to 150 nm. After the pigment crushing step, the number-average particle size of the pigment dispersed in the pigment dispersion is preferably 30 nm to 65 nm, since this improves coloring power. The number-average particle size of the pigment is measured by the method described below.

[0028] <Grinding agent> The grinding agent that can be contained in the pigment dispersion may be water-insoluble, and examples of the grinding agent include known water-insoluble inorganic salt particles, inorganic oxide particles, mineral particles, etc. Specific examples include the following.

[0029] Examples of inorganic salts include carbonates, sulfates, and chromates.

[0030] Examples of inorganic oxides include silica, alumina, titania, and strontium titanate.

[0031] Minerals include kaolinite, talc, barium sulfate, and the like.

[0032] Among the above, the grinding agent is preferably a particle that does not affect the color tone even if it is contained in the toner. Specifically, carbonates and the minerals exemplified above are preferable, and among them, calcium carbonate particles, which have a refractive index close to that of the toner binder resin, are particularly preferable.

[0033] The non-water-soluble grinding agent is required to exhibit good pigment disintegration properties and not to affect the toner even when contained therein, and from this viewpoint, the number-average particle size is preferably 0.1 μm to 5.0 μm, and more preferably 0.2 to 1.0 μm. The method for measuring the number-average particle size of the non-water-soluble grinding agent will be described later.

[0034] It is more preferable to keep the content of the non-water-soluble grinding agent in the toner particles to 20% by mass or less, since this does not affect the color tone.

[0035] <Binding agent> The binder that can be included in the pigment dispersion is a thermoplastic component that is water-insoluble and solid at 25°C.

[0036] The binder in the present invention is a component that is solid at 25° C., but has a melt viscosity of 6000 Pa·sec or less at the temperature during heating, melting and kneading.

[0037] The binder is not particularly limited as long as it has little effect on color, charge retention, and blocking resistance, but is preferably a material that is generally used as a material for constituting a toner. Examples of the binder include amorphous resins and crystalline resins used as binder resins for toners, thermoplastic elastomers, and low-molecular-weight crystalline compounds used as release agents and plasticizers.

[0038] (amorphous resin) First, the amorphous resin will be described. By using an amorphous resin as a binder, a pigment dispersion in which the crushed pigment is dispersed in the amorphous resin can be obtained. By producing toner particles using such a pigment dispersion, the pigment is well dispersed, and a toner with excellent coloring power can be obtained.

[0039] The amorphous resin is not particularly limited as long as it is a general resin used in toners, and examples thereof include polyester, styrene-acrylic acid copolymer, polyolefin resin, vinyl resin, fluororesin, phenol resin, silicone resin, epoxy resin, hybrid resin thereof, etc. Among these, it is preferable to use amorphous polyester, styrene-acrylic acid copolymer, and hybrid resin thereof, which have good charge retention and low-temperature fixing properties, and amorphous polyester is particularly preferable.

[0040] The content of the amorphous resin in the binder is preferably 20% by mass or more in order to disperse the pigment in the toner, and more preferably 50% by mass or more.

[0041] The glass transition temperature of the amorphous resin is preferably 30° C. to 80° C., and more preferably 50° C. to 70° C. When the glass transition temperature is 30° C. or higher, the resin can be handled as a solid before the pigment crushing step. When the glass transition temperature is 80° C. or lower, the effect on the low-temperature fixability of the toner can be suppressed.

[0042] The softening point (Tm) of the amorphous resin is preferably 80° C. to 200° C., and more preferably 100° C. to 150° C. If the softening point (Tm) is within the above range, the effect on the blocking resistance and offset resistance of the toner can be reduced.

[0043] In addition, the SP value of the amorphous resin is 21.0 (J / cm 3 ) 0.5 ~24.0(J / cm 3 ) 0.5 Within the above range, adhesion to paper and charge retention can be maintained well.

[0044] It is more preferable that the binder contains a crystalline resin together with the amorphous resin, since the viscosity of the pigment dispersion is appropriately reduced by containing the crystalline resin, and the dispersibility of the grinding agent and the pigment is improved, thereby improving the crushability of the pigment.

[0045] (Low molecular crystal compound) The low molecular weight crystalline compound is a compound having a number average molecular weight (Mn) of 250 or more and 1,000 or less.

[0046] By making the number average molecular weight (Mn) of the low molecular weight crystalline compound fall within the above range, the melting point can be lowered, and the component becomes one that crystallizes immediately upon cooling after kneading, which results in the pigment movement being restricted and pigment aggregation being suppressed, thereby achieving good pigment dispersion.

[0047] The number average molecular weight (Mn) of the low molecular weight crystalline compound can be easily controlled by various known production conditions of the low molecular weight crystalline compound.

[0048] The number average molecular weight (Mn) of a low molecular weight crystalline compound is measured by gel permeation chromatography (GPC) as follows.

[0049] Add 2,6-di-t-butyl-4-methylphenol (BHT) to o-dichlorobenzene for gel chromatography to a concentration of 0.10% by mass and dissolve at room temperature. Place the low molecular weight crystalline compound and the o-dichlorobenzene with BHT added in a sample bottle and heat on a hot plate set at 150°C to dissolve the low molecular weight crystalline compound.

[0050] Once the low molecular weight crystalline compound has melted, it is placed in a preheated filter unit and placed in the main unit. The sample that passes through the filter unit is the GPC sample.

[0051] The sample solution is adjusted to have a concentration of about 0.15% by mass.

[0052] Using this sample solution, measurements are performed under the following conditions. Equipment: HLC-8121GPC / HT (Tosoh Corporation) Detector: High temperature RI Column: TSKgel GMHHR-H HT 2-unit (Tosoh Corporation) Temperature: 135.0℃ Solvent: o-Dichlorobenzene for gel chromatography (BHT 0.10% by mass added) Flow rate: 1.0ml / min Injection volume: 0.4ml In calculating the molecular weight of low molecular weight crystalline compounds, a molecular weight calibration curve prepared using standard polystyrene resins (product names: "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.

[0053] The melting point of the low molecular weight crystalline compound is preferably 60° C. to 120° C., more preferably 70° C. to 100° C. In this case, since the crushability is excellent, the effect of reducing the hardness of the crushed pigment product after kneading and cooling can be obtained. As a result, the crushing energy can be reduced, and the productivity can be improved.

[0054] Examples of low molecular weight crystalline compounds include hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax, which are used as release agents for toners; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes containing fatty acid esters as the main component such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax.

[0055] Other examples include crystalline long-chain alkyl carboxylic acids such as stearic acid and behenic acid, and crystalline alkyl alcohols such as 1-docosanol and 1-octacosanol.

[0056] The content of the low molecular weight crystalline compound in the water-insoluble binder is preferably 20% by mass or more in order to disperse the pigment in the toner, and more preferably 50% by mass or more.

[0057] (Crystalline Resin) The crystalline resin is not particularly limited as long as it is a typical crystalline resin used in toner, and examples of the crystalline resin include polyester, polyamide, polyimide, polyolefin, polyethylene, polybutylene, polyisobutyrate, polyvinyl, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, polypropylene, acrylic resin, etc. Among them, crystalline polyester and crystalline acrylic resin are preferable.

[0058] In addition, the crystalline acrylic resin preferably has a monomer unit represented by the following formula: The monomer unit represented by the following formula is formed by copolymerization with a (meth)acrylic acid ester having an alkyl group having 18 to 36 carbon atoms.

[0059] [ka]

[0060] [In the formula, R Z1 represents a hydrogen atom or a methyl group, and R represents an alkyl group having 18 to 36 carbon atoms. Examples of (meth)acrylic acid esters having an alkyl group having 18 to 36 carbon atoms include stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosanyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, octacosyl (meth)acrylate, myrisyl (meth)acrylate, dotriacontane (meth)acrylate, and 2-decyltetradecyl (meth)acrylate.

[0061] Among these, from the viewpoint of low-temperature fixability, at least one selected from the group consisting of (meth)acrylic acid esters having a linear alkyl group with 18 to 36 carbon atoms is preferred, at least one selected from the group consisting of (meth)acrylic acid esters having a linear alkyl group with 18 to 30 carbon atoms is more preferred, and at least one of linear stearyl (meth)acrylate and behenyl (meth)acrylate is even more preferred.

[0062] The melting point of the crystalline resin is preferably 60° C. to 120° C., more preferably 70° C. to 100° C., and particularly preferably 70° C. to 90° C. In this case, the excellent crushability can reduce the hardness of the crushed pigment product after kneading and cooling, thereby reducing the crushing energy and improving productivity.

[0063] (SP value of binder) In the process of obtaining toner particles, the amorphous resin, crystalline low molecular weight compound or crystalline resin used as a binder coexists with another resin (resin A). The SP value difference between the binder component and the other resin (resin A) is 3.0 (J / cm 3 ) 0.5 It is preferable that:

[0064] The SP value can be calculated using the Fedors formula, where Δei and Δvi values ​​are based on the evaporation energies and molar volumes (25°C) of atoms and atomic groups in Tables 3-9 of "Basic Science of Coatings" (Maki Shoten, 1986), pp. 54-57. Formula: δi = [Ev / V] (1 / 2) = [Δei / Δvi] (1 / 2) Ev: Evaporation energy V: Molar volume Δei: Evaporation energy of the atom or atomic group of the i component Δvi: Molar volume of the atom or atomic group of the i component <Toner raw materials> Next, the components contained in the toner particles will be described.

[0065] The toner produced by the production method of the present invention contains the same components as those contained in general toner, specifically, a binder resin, a release agent, a charge control agent, and the like.

[0066] <Binding resin> In the process of obtaining toner particles, the pigment dispersion and the resin (resin A) coexist. When the pigment dispersion contains a resin component that acts as a binder resin, the resin component contained in the pigment dispersion and the mixed resin (resin A) act as a binder resin in the toner particles. On the other hand, when the pigment dispersant does not contain a resin component, the mixed resin (resin A) acts as a binder resin in the toner particles. The mixing ratio of the pigment dispersion and the resin may be in the range of 3 to 20% by mass of the pigment in the toner particles.

[0067] In the toner particle manufacturing process, the resin (resin A) to be mixed / synthesized can be a resin generally used as a binder resin for toner. Specific examples include polyester, polyolefin resin, vinyl resin (styrene-(meth)acrylic acid ester copolymer), fluororesin, phenol resin, silicone resin, and epoxy resin. Among these, from the viewpoint of improving low-temperature fixability, amorphous polyester is preferred. As the amorphous polyester, a low molecular weight polyester and a high molecular weight polyester may be used in combination from the viewpoint of achieving both low-temperature fixability and hot offset resistance. In addition, a crystalline polyester may be contained from the viewpoint of further improving low-temperature fixability and blocking resistance during storage.

[0068] <Method of manufacturing toner particles> Methods for obtaining toner particles using the pigment dispersion obtained in the pigment crushing step include a kneading and pulverizing method, a dissolution suspension method, a suspension polymerization method, and an emulsion aggregation method. The toner particles may be produced by any one of the production methods alone or by a combination of the methods.

[0069] If necessary, inorganic fine particles such as silica, alumina, titania, and calcium carbonate, and resin fine particles such as vinyl resin, polyester resin, and silicone resin may be added to the produced toner particles by applying a shear force in a dry state. These inorganic fine particles and resin fine particles function as external additives such as a flowability aid and a cleaning aid.

[0070] The methods for producing toner particles, including the kneading and pulverizing method, the dissolution suspension method, the suspension polymerization method, and the emulsion aggregation method, will be specifically described below.

[0071] <Kneading and grinding method> In the kneading and grinding method, first, the pigment dispersion and resin A, and optionally the release agent, colorant, and other additives are thoroughly mixed using a mixer. Next, the resulting mixture is melt-kneaded using a thermal kneader (kneading step). Thereafter, the resulting kneaded product is pulverized to a desired toner particle size (pulverizing step), and if necessary, classified to obtain a desired particle size distribution (classifying step) to obtain toner particles.

[0072] Examples of mixers include Henschel mixer (manufactured by Mitsui Mining Co., Ltd.); Super mixer (manufactured by Kawata Co., Ltd.); Ribocone (manufactured by Okawara Manufacturing Co., Ltd.); Nauta mixer, Turbulizer, Cyclomix (manufactured by Hosokawa Micron Corporation); Spiral pin mixer (manufactured by Pacific Machinery Co., Ltd.); and Loedige mixer (manufactured by Matsubo Co., Ltd.).

[0073] Examples of thermal kneaders include the KRC kneader (manufactured by Kurimoto Iron Works); the Buss-Co kneader (manufactured by Buss); the TEM type extruder (manufactured by Toshiba Machine Co., Ltd.); the TEX twin-screw kneader (manufactured by Japan Steel Works); the PCM kneader (manufactured by Ikegai Iron Works); the three-roll mill, mixing roll mill, kneader (manufactured by Inoue Seisakusho Co., Ltd.); the Kneadex (manufactured by Mitsui Mining Co., Ltd.); the MS-type pressure kneader, Niderruder (manufactured by Moriyama Seisakusho Co., Ltd.); and the Banbury mixer (manufactured by Kobe Steel, Ltd.).

[0074] In the pulverization step, known pulverizers such as a collision plate type jet mill, a fluidized bed type jet mill, and a rotary mechanical mill can be used. Specifically, counter jet mills, micron jets, and innomizers (manufactured by Hosokawa Micron Corporation); IDS type mills, PJM jet pulverizers (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); cross jet mills (manufactured by Kurimoto Iron Works Co., Ltd.); Urumax (manufactured by Nisso Engineering Co., Ltd.); SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.); Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.); Turbo Mill (manufactured by Turbo Kogyo Co., Ltd.); and Super Rotor (manufactured by Nisshin Engineering Co., Ltd.).

[0075] Examples of classifiers used in the classification step include known devices such as wind classifiers, inertial classifiers, and sieve classifiers.Specific examples include Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turbo Flex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).

[0076] <Dissolution suspension method> In the solution suspension method, the toner is manufactured through a resin dissolving step, a granulating step, a solvent removing step, and a washing and drying step.

[0077] (Resin melting process) The resin dissolving step is a step of preparing a resin solution by dissolving the pigment dispersion and the resin A in an organic solvent. If necessary, other resins, plasticizers, colorants, release agents, etc. may be dissolved or dispersed in the organic solvent.

[0078] As the organic solvent, any organic solvent capable of dissolving the binder in the pigment dispersion and the resin A can be used. Specific examples include toluene and xylene.

[0079] The amount of the organic solvent used is not limited, but may be an amount that provides a viscosity that allows the resin composition to be dispersed and granulated in an aqueous medium. Specifically, the mass ratio of the resin composition containing the pigment dispersion, resin A, other resins, plasticizers, colorants, etc. as necessary, to the organic solvent is preferably 10 / 90 to 50 / 50 in terms of granulation properties and toner production efficiency.

[0080] On the other hand, the pigment and grinding agent in the pigment dispersion, and the colorant and release agent added as necessary, do not need to be dissolved in an organic solvent, and may be dispersed. When the colorant and release agent are used in a dispersed state, they are preferably dispersed using a dispersing machine such as a bead mill.

[0081] (granulation process) The granulation process is a process in which the obtained resin solution is dispersed in an aqueous medium containing a dispersant, and granulated to a predetermined toner particle size, to prepare a dispersion (granulated product) in which droplet particles A are dispersed. Water is mainly used as the aqueous medium. In addition, the aqueous medium preferably contains 1% by mass or more and 30% by mass or less of a monovalent metal salt. By containing the monovalent metal salt, the organic solvent in the resin solution is prevented from diffusing into the aqueous medium, and the particle size distribution of the toner tends to become sharp.

[0082] Examples of monovalent metal salts include sodium chloride, potassium chloride, lithium chloride, and potassium bromide, and among these, sodium chloride and potassium chloride are preferred.

[0083] The mixing ratio (mass ratio) of the aqueous medium to the resin solution is preferably aqueous medium / resin solution=90 / 10 to 50 / 50.

[0084] The dispersant is not particularly limited, but cationic, anionic and nonionic surfactants are used as organic dispersants, with anionic surfactants being preferred. Examples include sodium alkylbenzenesulfonate, sodium α-olefinsulfonate, sodium alkylsulfonate, sodium alkyldiphenyletherdisulfonate, etc. On the other hand, inorganic dispersants include tricalcium phosphate, hydroxyapatite, calcium carbonate, titanium oxide and silica powder. Among these, the inorganic dispersant tricalcium phosphate is particularly preferred from the viewpoint of granulation stability.

[0085] The amount of dispersant added is determined according to the particle diameter of the granulated product, and the particle diameter decreases as the amount of dispersant added increases. Therefore, the amount of dispersant added varies depending on the desired particle diameter, but is preferably 0.1 to 15 parts by mass per 100 parts by mass of the resin solution. If the amount is 0.1 part by mass or more, coarse powder is unlikely to be generated, and if it is 15 parts by mass or less, unnecessary fine particles are unlikely to be generated.

[0086] In addition, when preparing a dispersion of the resin solution in an aqueous medium, it is preferable to carry out the preparation under high speed shearing. The dispersion of the resin solution dispersed in the aqueous medium is preferably granulated to a volume average particle size of 10 μm or less, more preferably about 4 to 9 μm.

[0087] Devices for imparting high-speed shear include various high-speed dispersers and ultrasonic dispersers.

[0088] (Solvent removal process) The desolvation step is a step of removing the organic solvent from the droplet particles A. The organic solvent is preferably removed while stirring. In addition, the removal rate of the organic solvent can be controlled by heating or reducing pressure as necessary.

[0089] (Washing and drying process) After the solvent removal step, a washing and drying step may be carried out in which the toner particles are washed multiple times with water or the like, and then filtered and dried. When a dispersant that dissolves under acidic conditions, such as tricalcium phosphate, is used as the dispersant, it is preferable to wash with water after washing with hydrochloric acid or the like. By carrying out washing, the dispersant used for granulation can be removed, and the toner properties can be improved.

[0090] <Suspension polymerization method> First, the polymerizable monomer is mixed with the pigment dispersion and other necessary components (e.g., a release agent, a crosslinking agent, a charge control agent, a chain transfer agent, a plasticizer, a pigment dispersant, a release agent dispersant) and dissolved or dispersed to prepare a polymerizable monomer composition. At this time, a dispersing machine such as a homogenizer, a ball mill, a colloid mill, or an ultrasonic dispersing machine can be used. Next, the polymerizable monomer composition is put into an aqueous medium, and dispersed (suspended) using a high-speed dispersing machine such as a high-speed agitator or an ultrasonic dispersing machine to form droplet particles B. It is preferable that a dispersion stabilizer is contained in the aqueous medium. The polymerization initiator may be mixed with other additives when preparing the polymerizable monomer composition, or may be added to the aqueous medium immediately before dispersion. In addition, the polymerization initiator may be added in a state dissolved in the polymerizable monomer or another solvent during or after granulation is completed, i.e., immediately before starting the polymerization reaction, if necessary. Thereafter, a polymerization reaction is carried out while stirring so that the droplet particles of the polymerizable monomer composition in the suspension maintain a particle state and do not float or settle, and resin particles are formed by polymerizing the polymerizable monomer contained in the droplet particles B. Thereafter, the suspension is cooled, washed as necessary, and dried and classified by various methods to obtain toner particles. The obtained toner particles contain resin A produced by polymerization of the polymerizable monomer.

[0091] <Emulsification aggregation method> In the emulsion aggregation method, a toner is produced through a step of preparing a fine particle dispersion, a step of aggregating, a step of fusing, a step of cooling, and a step of washing. A specific method for producing a toner using the emulsion aggregation method will be described below, but the method is not limited thereto.

[0092] (Step of preparing a fine particle dispersion) First, the preparation of the dispersion of resin fine particles will be described. The resin fine particles can be produced by a known method, but it is preferable to produce them by the following method.

[0093] A resin (e.g., polyester resin) is dissolved in an organic solvent to form a uniform solution. Then, a basic compound and a surfactant are added as necessary. Furthermore, fine particles are formed by slowly adding an aqueous medium while applying shear using a homogenizer or the like, or by applying shear using a homogenizer after adding the aqueous medium. Then, the solvent is removed to obtain a resin fine particle dispersion in which the resin fine particles are dispersed.

[0094] The concentration of the resin when dissolved in the organic solvent is preferably 10% by mass or more and 50% by mass or less, more preferably 30% by mass or more and 50% by mass or less. Any organic solvent can be used as long as it can dissolve the resin, but toluene, xylene, tetrahydrofuran, etc. are preferred.

[0095] The surfactant is not particularly limited, and examples thereof include anionic surfactants such as sulfate salts, sulfonates, carboxylates, phosphates, and soaps, cationic surfactants such as amine salts and quaternary ammonium salts, and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols.

[0096] Examples of the base include inorganic bases such as sodium hydroxide and potassium hydroxide, and organic bases such as triethylamine, trimethylamine, dimethylaminoethanol, diethylaminoethanol, etc. The base may be used alone or in combination of two or more kinds.

[0097] The volume-based median diameter of the resin fine particles is preferably 0.05 to 1.0 μm, more preferably 0.1 to 0.6 μm. When the median diameter is within the above range, toner particles having a desired particle size are easily obtained. The volume-based median diameter can be measured using a dynamic light scattering particle size distribution meter (Nanotrac UPA-EX150: manufactured by Nikkiso).

[0098] Next, the preparation of a fine particle dispersion of a pigment dispersion will be described. When preparing a dispersion (emulsion) containing fine particles of the pigment dispersion alone, the pigment dispersion, a surfactant, and an aqueous medium are mixed, and then the temperature is raised to a temperature at which the binder in the pigment dispersion melts, and shear is applied using a homogenizer or the like, followed by cooling to obtain a dispersion of the pigment dispersion in which the pigment dispersion is dispersed in the aqueous medium.

[0099] It is also possible to prepare a fine particle dispersion containing the pigment dispersion and the resin A, without separately preparing a dispersion of the resin fine particles and a dispersion of the pigment dispersion. In this case, in the step of preparing the fine particle dispersion, the pigment dispersion is added when dissolving the resin in the organic solvent, thereby obtaining a fine particle dispersion containing the resin A and the pigment dispersion.

[0100] (agglomeration process) A dispersion of a releasing agent particle or the like is mixed into the dispersion of a resin particle and the dispersion of a pigment, if necessary, to prepare a mixed liquid. Instead of using the dispersion of a resin particle and the dispersion of a pigment, a dispersion of a particle containing a resin and a pigment may be used. Then, the particles contained in the prepared mixed liquid are aggregated to form aggregate particles. Suitable examples of the method for forming aggregate particles include a method of adding and mixing an aggregating agent into the mixed liquid, and raising the temperature or applying mechanical power appropriately.

[0101] The dispersion of the release agent particles used as necessary in the aggregation step is prepared by dispersing the above-mentioned release agent. The release agent particles are dispersed by a known method, for example, by mixing the release agent with an aqueous medium, heating the mixture to a temperature at which the release agent melts, shearing the mixture using a media-type dispersing machine such as a rotary shearing homogenizer, a ball mill, a sand mill, or an attritor, or a high-pressure counter-collision type dispersing machine, and then cooling the mixture to obtain a release agent dispersion dispersed in an aqueous medium. In addition, a surfactant or a polymer dispersing agent that provides dispersion stability can be added as necessary.

[0102] Examples of the flocculant used in the flocculation step include metal salts of monovalent metals such as sodium and potassium, metal salts of divalent metals such as calcium and magnesium, metal salts of trivalent metals such as iron and aluminum, and polyvalent metal salts such as polyaluminum chloride. From the viewpoint of particle size controllability in the flocculation step, divalent metal salts such as calcium chloride and magnesium sulfate are preferred.

[0103] The mixing of the flocculant is preferably carried out in the temperature range of room temperature (25° C.) to 75° C. When the mixing is carried out under these temperature conditions, the flocculation proceeds in a stable state. The mixing can be carried out using a known mixing device, homogenizer, mixer, etc.

[0104] The average particle size of the aggregate particles formed in the aggregation step is not particularly limited, but it is usually preferable to control the weight average particle size to 4.0 to 7.0 μm so that it is approximately the same as the average particle size of the toner particles to be obtained. The control can be easily performed, for example, by appropriately setting and changing the temperature during addition and mixing of the aggregating agent and the like and the stirring and mixing conditions. The particle size distribution of the aggregate particles can be measured using a particle size distribution analyzer (Coulter Multisizer III, manufactured by Coulter) using the Coulter method.

[0105] (fusion process) The fusion process is a process in which aggregate particles are heated and fused to form toner particles with smooth surfaces. Prior to the fusion process, a chelating agent, a pH adjuster, a surfactant, etc. may be appropriately added to prevent fusion between particles.

[0106] Examples of chelating agents include ethylenediaminetetraacetic acid (EDTA) and its alkali metal salts such as the Na salt, sodium gluconate, sodium tartrate, potassium and sodium citrate, nitrilotriacetate (NTA) salts, and many water-soluble polymers containing both COOH and OH functionality (polyelectrolytes).

[0107] The heating temperature should be equal to or higher than the glass transition temperature of the resin contained in the aggregate and lower than the temperature at which the resin thermally decomposes. The heating time is shorter if the heating temperature is high, and longer if the heating temperature is low. That is, the heating / fusion time depends on the heating temperature and cannot be generally specified, but is generally 10 minutes to 10 hours.

[0108] (cooling process) The cooling step is a step of cooling the temperature of the aqueous medium containing the particles obtained in the fusion step to a temperature lower than the glass transition temperature of the resin. By cooling to a temperature lower than the glass transition temperature, the generation of coarse particles can be suppressed. The specific cooling rate is 0.1 to 50°C / min.

[0109] (Cleaning process) The particles produced through the above steps can be washed, filtered, and then repeatedly washed to remove impurities from the toner particles. Specifically, it is preferable to wash the toner particles using an aqueous solution containing a chelating agent such as ethylenediaminetetraacetic acid (EDTA) and its Na salt, and then further wash the particles with ion-exchanged water. By repeatedly filtering the washed particles with ion-exchanged water multiple times, metal salts, surfactants, and the like can be removed from the toner particles. From the viewpoint of production efficiency, the number of filtrations is preferably 3 to 20, and more preferably 3 to 10.

[0110] (drying process) The particles obtained in the above step are dried to obtain toner particles.

[0111] The methods for measuring various physical properties of the toner and raw materials are described below.

[0112] <Measurement of number-average particle size of pigments and grinding agents> The number-average particle size of the pigment and the grinding agent is measured using a transmission electron microscope (TEM) "JEM2800" (manufactured by JEOL Ltd.).

[0113] First, a measurement sample is prepared. 1 ml of ion-exchanged water containing a dispersible surfactant is added to approximately 5 mg of pigment or grinding agent, and the mixture is dispersed for 5 minutes using an ultrasonic disperser (ultrasonic cleaner). Next, a drop of the above dispersion liquid is placed on a microgrid (150 mesh) with a support membrane for TEM, and the mixture is dried to prepare a measurement sample.

[0114] Next, images are taken using a transmission electron microscope (TEM) at an accelerating voltage of 200 kV at a magnification (e.g., 20k to 100k) that allows the pigment or grinding agent in the field of view to be measured sufficiently, and the particle size of 100 randomly selected primary particles of the pigment or grinding agent is measured to determine the number-average particle size. The particle size of the primary particles may be measured manually or using a measuring tool.

[0115] In order to measure the number-average particle size of the pigment contained in the pigment dispersion after the pigment crushing step, it is necessary to extract the pigment from the pigment dispersion. An example is shown below.

[0116] In order to dissolve the binder in the pigment dispersion with a solvent, a solvent is selected according to the type of binder, and the binder is melted using a swing roll mixer or the like. For example, if the binder is an amorphous polyester resin, tetrahydrofuran or methyl ethyl ketone can be used. Thereafter, the binder is separated from the pigment dispersion by filtration and washing, and a mixture of the pigment and grinding agent is extracted. The mixture of the extracted pigment and grinding agent is observed in the same manner as above, and only the pigment is extracted based on the shape of the pigment and grinding agent, and the number-average particle size is measured manually or with a measuring tool.

[0117] <Measurement of resin glass transition temperature (Tg)> The glass transition temperature of the resin is measured using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments) in accordance with ASTM D3418-82.

[0118] The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction.

[0119] Specifically, approximately 5 mg of resin is weighed out and placed in an aluminum pan. An empty aluminum pan is used as a reference, and measurements are performed in the measurement range of 30°C to 180°C at a heating rate of 10°C / min.

[0120] The temperature is first raised to 180°C and held there for 10 minutes, then lowered to 30°C, and then raised again. During this second heating process, a specific heat change is obtained in the temperature range of 30°C to 100°C. The glass transition temperature (Tg:°C) of the resin is determined by the temperature at the point where a line equidistant in the vertical direction from a line extending the baseline before and after the specific heat change occurs intersects with the curve of the stepwise change in the glass transition in the DSC curve.

[0121] <Measurement of the peak temperature (melting point) of the endothermic peak> The peak top temperature (melting point) of the maximum endothermic peak of the crystalline resin, release agent, etc. is measured using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments) in accordance with ASTM D3418-82.

[0122] The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction.

[0123] Specifically, about 5 mg of the sample is weighed out precisely, placed in a silver pan, and measured once. An empty silver pan is used as a reference. The measurement conditions are as follows: Heating rate: 10℃ / min Measurement start temperature: 20℃ End of measurement temperature: 180℃ The maximum endothermic peak means the peak with the largest amount of endothermic heat when there are multiple peaks. The peak temperature of the maximum endothermic peak is defined as the melting point.

[0124] <Measurement of resin melt viscosity and softening point (Tm)> The melt viscosity and softening point (Tm) of the resin can be measured using a constant load extrusion type capillary rheometer "Flow characteristic evaluation device Flow Tester CFT-500D" (manufactured by Shimadzu Corporation).

[0125] The CFT-500D is an instrument that applies a constant load from above using a piston while heating and melting the measurement sample filled in a cylinder and pushing it out through a capillary hole at the bottom of the cylinder, and can graph a flow curve from the amount of descent of the piston (mm) and the temperature (℃) during this process.

[0126] In the present invention, the melt viscosity is measured by measuring a sample using a "Flow characteristic evaluation device, Flow Tester CFT-500D" and is expressed as a function of shear stress (Pa) and shear rate (sec sec) at each heating temperature. -1 ) to calculate the "shear stress / shear rate at each heating temperature," and the value obtained is the melt viscosity (Pa sec).

[0127] In the present invention, the softening point (Tm) is defined as the "melting temperature in the 1 / 2 method" described in the manual attached to the "flow property evaluation device, flow tester CFT-500D."

[0128] The melting temperature in the 1 / 2 method is calculated as follows.

[0129] First, calculate half the difference between the amount of piston descent when the outflow ends (end of outflow, Smax) and the amount of piston descent when the outflow starts (minimum point, Smin) (this is X; X=(Smax-Smin) / 2). Then, the temperature on the flow curve when the amount of piston descent is the sum of X and Smin is the melting temperature in the 1 / 2 method.

[0130] The measurement sample is prepared by compressing 1.2 g of resin at 10 MPa for 60 seconds using a tablet press (e.g., a standard manual Newton press NT-100H, manufactured by NPA Systems) in an environment of 25°C to form a cylindrical shape with a diameter of 8 mm.

[0131] The specific operations for the measurement are performed according to the manual that comes with the device.

[0132] The measurement conditions for the CFT-500D are as follows. Test mode: Temperature rise method Starting temperature: 40℃ Achieved temperature: 200℃ Measurement interval: 1.0℃ Heating rate: 4.0℃ / min Piston cross-sectional area: 1.000cm 2 Test load (piston load): 5.0kgf Preheat time: 300 seconds Die hole diameter: 1.0mm Die length: 1.0mm <Method of measuring weight average particle size (D4) of toner particles> The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 50 μm aperture tube, and the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), for setting measurement conditions and analyzing measurement data, and is calculated by analyzing the measurement data.

[0133] The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).

[0134] Before carrying out the measurements and analyses, the dedicated software is set up as follows.

[0135] In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement.

[0136] In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 1 μm or more and 30 μm or less.

[0137] The specific measurement method is as follows. (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube. (2) Approximately 30 ml of the above-mentioned aqueous electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and approximately 0.3 ml of a solution prepared by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, with a pH of 7, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water is added as a dispersant. (3) A specified amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispension System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 ml of the Conaminon N is added to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, add the electrolyte solution (5) in which the toner is dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4). EXAMPLES

[0138] In the following examples, unless otherwise specified, parts are by weight.

[0139] <Production of Pigment Dispersion A-1> Pigment 35 parts (Cyan pigment: Pigment Blue 15:3, number average particle size 102nm) Grinding agent 35 parts (Light calcium carbonate, number average particle size 0.4μm) Binding agent 30 parts (Resin 1; amorphous polyester: composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: isophthalic acid: terephthalic acid = 100:50:50], softening point (Tm) = 122°C, glass transition temperature (Tg) = 70°C, SP value = 22.6 (J / cm 3 ) 0.5 ) The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1After mixing for 5 minutes at 120°C, the mixture was kneaded in a twin-screw kneader (PCM-30, Ikegai Corporation). The resulting kneaded mixture was cooled and coarsely pulverized in a pin mill to a particle size of 100μm or less to obtain coarsely pulverized pigment dispersion A-1. The melt viscosity of resin 1 at 120°C was 2080 Pa sec. The number average particle size of the pigment in the resulting pigment dispersion A-1 was 55nm.

[0140] <Production of Pigment Dispersion A-2> A coarsely ground pigment dispersion A-2 was obtained in the same manner as for pigment dispersion A-1, except that the binder was changed to the following resin 2. The melt viscosity of resin 2 at 120°C was 1490 Pa sec. The number average particle size of the pigment in the obtained pigment dispersion A-2 was 57 nm. Resin 2: Styrene-butyl acrylate copolymer: composition (mol%) [styrene:butyl acrylate=72.5:27.5], softening point (Tm) = 118°C, glass transition temperature (Tg) = 55°C, SP value = 21.1 (J / cm 3 ) 0.5 <Production of Pigment Dispersions A-3 to A-35> Pigment dispersions A-3 to A-35 were obtained in the same manner as pigment dispersion A-1, except that the binder, grinding agent, and pigment shown in Table 1 below were used and kneaded under the conditions shown in Table 2. The number average particle size of the pigments in the obtained pigment dispersions A-3 to A-35 is shown in Table 2.

[0141] Resins 3 and 5 to 9 are amorphous polyesters having the physical properties shown in Table 1, and resin 4 is a styrene-acrylic resin having the physical properties shown in Table 1.

[0142] The crystalline resin in pigment dispersion A-18 is the following resin. Crystalline polyester: composition (mol%) [1,6-hexanediol:dodecanedioic acid=100:100], melting point=72°C Furthermore, the synthetic wax in pigment dispersion A-19 is the following wax. Synthetic wax (Nippon Seiro FNP0090, melting point = 90℃) In the production of pigment dispersion A-5, a single-screw extruder was used instead of the twin-screw extruder.

[0143] <Production of Pigment Dispersion A-36> A coarsely ground pigment dispersion A-36 was obtained in the same manner as for pigment dispersion A-1, except that the binder was changed to a polyester thermoplastic elastomer (block copolymer of polybutylene terephthalate and polytetramethylene ether glycol, melting point = 163°C) and the kneading temperature was changed to 200°C. The melt viscosity of the polyester thermoplastic elastomer at 200°C was 5040 Pa sec. The number average particle size of the pigment in the obtained pigment dispersion A-36 was 65 nm.

[0144] [Table 1]

[0145] [Table 2]

[0146] <Production Example of Toner A-1> Amorphous polyester 77.7 parts (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 ) Pigment Dispersion A-1 14.3 parts Hydrocarbon wax (maximum endothermic peak temperature 90℃) 8.0 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1After mixing for 5 minutes at 100° C., the mixture was melted and kneaded in a twin-screw kneader (PCM-30, Ikegai Corporation). The kneaded mixture was cooled and coarsely pulverized to a particle size of 100 μm or less in a pin mill to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (T-250, Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes to obtain the target particle size. Classification was then performed using a rotary classifier (200TSP, Hosokawa Micron Corporation) to obtain toner particles with a weight average particle size of 6.5 μm. The operating conditions of the rotary classifier (200TSP, Hosokawa Micron Corporation) were such that the rotation speed was adjusted to obtain the target particle size and particle size distribution.

[0147] 100 parts of the obtained toner particles were mixed with silica fine particles (BET specific surface area 200 m) that had been hydrophobized with silicone oil. 2 The mixture was mixed with 1.8 parts of 1.0 parts of 1 / g of 100 ml of water and mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for a rotation time of 10 minutes to obtain Toner A-1.

[0148] <Production Examples of Toners A-2 to A-20 and A-24 to A-40> Except for changing the materials and conditions shown in Table 3, the same production method as for toner 1 was used to obtain toners A-2 to A-20 and A-24 to A-40.

[0149] In addition, in the toner A-11, the SP value of the amorphous polyester is 23.9 (J / cm 3 ) 0.5 The resin used was

[0150] Additionally, toners A-32 to A-39 produced using pigment dispersions A-28 to A-35 are described as comparative examples.

[0151] <Production Example of Toner A-21> Pigment Dispersion A-1 160 parts Organic solvent (toluene) 150 parts Glass beads (diameter 1 mm) 130 pieces The above materials were mixed and dispersed for 3 hours using an attritor (manufactured by Nippon Coke & Engineering Co., Ltd.) to obtain a pigment dispersion.

[0152] Next, Amorphous polyester used in the production of toner A-1: ​​75.7 parts Pigment dispersion 50 parts Hydrocarbon wax (maximum endothermic peak temperature 90℃) 10 parts Toluene 350 parts The above ingredients were mixed and heated to 80° C. with stirring to dissolve and disperse each ingredient, thereby preparing a resin solution.

[0153] Next, 11.7 parts of trisodium phosphate dodecahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) and 1200 parts of ion-exchanged water were added to a beaker set in a water bath to dissolve the trisodium phosphate dodecahydrate. Then, the temperature of the water bath was raised to 60°C. After reaching 60°C, an aqueous solution in which 5.15 parts of calcium chloride (manufactured by Kishida Chemical Industries, Ltd.) was dissolved in 100 parts of ion-exchanged water was added. After the addition, the mixture was stirred for 30 minutes to obtain an aqueous medium containing tricalcium phosphate.

[0154] Meanwhile, 600 parts of the above aqueous medium was heated to 80°C while stirring with Clearmix (manufactured by M Technique Co., Ltd.). A resin solution was added to this aqueous medium, and the mixture was granulated by stirring at 10,000 rpm for 10 minutes to obtain a dispersion in which droplet particles were dispersed. While maintaining the temperature at 80°C, stirring was continued for 5 hours using a stirring blade to remove the toluene contained in the droplet particles. The mixture was then cooled to 25°C for 10 minutes to obtain a dispersion in which toner particles were dispersed.

[0155] Dilute hydrochloric acid was added to the dispersion liquid of the toner particles while stirring, and the mixture was stirred for 2 hours at pH 1.5 to dissolve tricalcium phosphate, and then the mixture was subjected to solid-liquid separation using a filter to obtain resin particles.

[0156] The mixture was poured into water and stirred to prepare a dispersion again, which was then subjected to solid-liquid separation using a filter. This procedure was repeated until the tricalcium phosphate was sufficiently removed, and the resulting particles were thoroughly dried in a dryer to obtain toner particles.

[0157] The obtained toner particles were subjected to external addition in the same manner as in Toner A-1, to obtain Toner A-21.

[0158] <Production Example of Toner A-22> Styrene 47.6 parts n-Butyl acrylate 15.1 parts Pigment Dispersion A-2 14.3 parts Hydrocarbon wax (maximum endothermic peak temperature 90℃) 20.0 parts Amorphous polyester used in the production of toner A-1: ​​3.0 parts The above materials were mixed and placed in an attritor (manufactured by Nippon Coke Corporation), and dispersed using zirconia beads having a diameter of 5 mm at 200 rpm for 2 hours to obtain a polymerizable monomer composition.

[0159] On the other hand, 735.0 parts of ion-exchanged water and 16.0 parts of trisodium phosphate (12-hydrate) were added to a container equipped with a high-speed stirring device homomixer (manufactured by Primix Corporation) and a thermometer, and the temperature was raised to 60°C while stirring at 12000 rpm. An aqueous calcium chloride solution in which 9.0 parts of calcium chloride (2-hydrate) was dissolved in 65.0 parts of ion-exchanged water was added thereto, and the mixture was stirred at 12000 rpm for 30 minutes while maintaining the temperature at 60°C. 10% hydrochloric acid was added thereto to adjust the pH to 6.0, and an aqueous medium containing a dispersion stabilizer was obtained.

[0160] Next, the polymerizable monomer composition was transferred to a vessel equipped with a stirrer and a thermometer, and heated to 60° C. while stirring at 100 rpm. 8.0 parts of t-butyl peroxypivalate (Perbutyl PV, manufactured by NOF Corp.) was added thereto as a polymerization initiator, and stirred at 100 rpm for 5 minutes while maintaining 60° C. Then, the polymerizable monomer composition to which the polymerization initiator was added was put into the aqueous medium being stirred at 12000 rpm by the high-speed stirrer. While maintaining 60° C., stirring was continued at 12000 rpm by the high-speed stirrer for 20 minutes to perform granulation, and a dispersion in which droplet particles were dispersed was obtained. The dispersion was transferred to a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube, and heated to 70° C. while stirring at 150 rpm under a nitrogen atmosphere. Polymerization of the polymerizable monomer contained in the droplet particles was carried out at 150 rpm for 10 hours while maintaining 70° C. Thereafter, the reflux condenser was removed from the reaction vessel, and the reaction liquid was heated to 95° C., and then stirred at 150 rpm for 5 hours while maintaining the temperature at 95° C., thereby obtaining a toner particle dispersion liquid.

[0161] The resulting toner particle dispersion was cooled to 20°C while stirring at 150 rpm, and then diluted hydrochloric acid was added with stirring until the pH reached 1.5 to dissolve the dispersion stabilizer. The solid content was filtered and thoroughly washed with ion-exchanged water, and then vacuum-dried at 40°C for 24 hours to obtain toner particles.

[0162] The obtained toner particles were subjected to external addition in the same manner as in Toner A-1, to obtain Toner A-22.

[0163] <Production Example of Toner A-23> -Production of dispersion of resin particles- Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) 200 parts 120 parts of amorphous polyester used in the production of toner A-1 Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 0.6 parts The above materials were mixed and then stirred for 12 hours to dissolve the resin in tetrahydrofuran.

[0164] Next, 2.7 parts of N,N-dimethylaminoethanol was added, and the mixture was stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation).

[0165] Further, 359.4 parts of ion-exchanged water was added at a rate of 1 g / min to precipitate resin particles, after which tetrahydrofuran was removed using an evaporator to obtain a dispersion liquid in which amorphous resin particles were dispersed. -Production of dispersion liquid of pigment fine particles- Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) 200 parts Pigment Dispersion A-1 42.9 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.5 parts The above materials were mixed and then stirred for 12 hours to dissolve the binder in the pigment dispersion in tetrahydrofuran.

[0166] Next, 0.3 parts of N,N-dimethylaminoethanol and 255.6 parts of ion-exchanged water were added, and the mixture was stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation).

[0167] The mixture was then dispersed for about 1 hour using a high-pressure impact disperser Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) After that, tetrahydrofuran was removed using an evaporator to prepare a dispersion in which the pigment dispersion was dispersed. -Production of dispersion of release agent particles- Hydrocarbon wax (maximum endothermic peak temperature 90℃) 20.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.0 part 79.0 parts of ion-exchanged water The above ingredients were placed in a mixing vessel equipped with an agitator, heated to 90°C, and circulated through a Clearmix W Motion (manufactured by M Technique) while being stirred at a shear mixing section with a rotor outer diameter of 3 cm and clearance of 0.3 mm at a rotor rotation speed of 19,000 rpm and a screen rotation speed of 19,000 rpm for 60 minutes for dispersion processing.

[0168] Thereafter, the mixture was cooled to 40° C. under cooling treatment conditions of a rotor rotation speed of 1000 rpm, a screen rotation speed of 0 rpm, and a cooling rate of 10° C. / min, to obtain a dispersion liquid of release agent fine particles. -Agglutination- Dispersion of resin particles 310.8 parts Pigment dispersion fine particle dispersion liquid 100 parts Dispersion of release agent particles 50 parts -Ion-exchanged water 400 parts The above materials were placed in a round stainless steel flask and mixed, after which an aqueous solution of 2 parts magnesium sulfate dissolved in 98 parts ion-exchanged water was added thereto, and the mixture was dispersed at 5,000 rpm for 10 minutes using a homogenizer (IKA Ultra Turrax T50).

[0169] Thereafter, the mixture was heated to 58° C. in a heating water bath while appropriately adjusting the rotation speed using a stirring blade so that the mixture was stirred. The mixture was kept at 58° C. for 1 hour to obtain aggregate particles. -fusion- To the dispersion liquid containing the aggregate particles, an aqueous solution in which 20 parts of trisodium citrate was dissolved in 380 parts of ion-exchanged water was added, and the mixture was then heated to 95°C.

[0170] The mixture was kept at 95° C. for 2 hours to fuse the aggregated particles, and then cooled to 25° C. while continuing to stir, to obtain a toner particle dispersion.

[0171] Thereafter, after filtration and solid-liquid separation, the filter cake was thoroughly washed with ion-exchanged water and dried using a vacuum dryer to obtain toner particles.

[0172] The obtained toner particles were subjected to external addition in the same manner as in Toner A-1, to obtain Toner A-23.

[0173] [Table 3]

[0174] <Production Example of Two-Component Developer A-1> A magnetic carrier having a volume distribution-based 50% particle size (D50) of 38.2 μm was prepared by forming a coating layer of a copolymer of cyclohexyl methacrylate, methyl methacrylate, and methyl methacrylate macromonomer on the surface of a Mn-Mg-Sr ferrite carrier core.

[0175] 92.0 parts of this magnetic carrier and 8.0 parts of toner A-1 were mixed in a V-type mixer (V-20, manufactured by Seishin Enterprises) to obtain two-component developer A-1.

[0176] <Production Examples of Two-Component Developers A-2 to A-40> Two-component developers A-2 to A-40 were obtained in the same manner as in the production example of two-component developer A-1, except that toner A-1 was changed to toners A-2 to A-40.

[0177] <Evaluation of preservation> Each toner was left to stand in a thermo-hygrostat for 3 days, and then sieved using a sieve with a 75 μm mesh size at a shaking width of 1 mm for 300 seconds. The amount of toner remaining on the sieve was evaluated according to the following criteria. The results are shown in Table 4.

[0178] (Evaluation Criteria) A: After leaving the toner in a constant temperature and humidity chamber at a temperature of 55°C and a humidity of 10% RH for 3 days, the toner amount remaining on the sieve is 10% by mass or less. B: When left for 3 days in a thermostatic chamber at a temperature of 55°C and a humidity of 10% RH and then sieved, the amount of toner remaining on the sieve is 10% by mass or more, but when left for 3 days in a thermostatic chamber at a temperature of 50°C and a humidity of 10% RH and then sieved, the amount of toner remaining on the sieve is 10% by mass or less C: After being left to stand for 3 days in a constant temperature and humidity chamber at a temperature of 50° C. and a humidity of 10% RH, the amount of toner remaining on the sieve is 10% by mass or more. <Method for evaluating toner coloring power> A modified Canon imageRUNNER ADVANCE C5255 full-color copying machine was used as the image forming apparatus, and each two-component developer was charged into the developing device of the cyan station to perform the evaluation.

[0179] The evaluation environment was normal temperature and humidity (23°C, 50% RH), and the evaluation paper was GFC-081 plain copy paper (A4, basis weight 81.4 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0180] First, in the evaluation environment, the amount of toner applied on the paper was changed to examine the relationship between image density and the amount of toner applied on the paper.

[0181] Next, the image density of the FFH image (solid portion) was adjusted to 1.40, and the toner amount when the image density reached 1.40 was determined.

[0182] An FFH image is a value obtained by expressing 256 gradations in hexadecimal, with 00H being the first gradation (white area) and FFH being the 256th gradation (solid area).

[0183] The image density was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite).

[0184] Toner load (mg / cm 2 The coloring power of the toner was evaluated based on the following criteria. The evaluation results are shown in Table 4.

[0185] (Evaluation Criteria) A: Less than 0.35 B: 0.35 or more, less than 0.50 C: 0.50 or more, less than 0.65 D:0.65 or more <Evaluation of charge retention> The triboelectric charge amount of the toner was measured using each two-component developer with an Espart analyzer manufactured by Hosokawa Micron Corp. The chargeability of the toner was evaluated according to the following criteria.

[0186] After measuring the initial triboelectric charge amount of the toner, the two-component developer was left to stand in a thermo-hygrostat (temperature 30° C., humidity 80% RH) for one week, and the triboelectric charge amount was measured again using the developer.

[0187] The measurement results were substituted into the following formula to calculate the triboelectric charge retention rate, and the rate was evaluated according to the following criteria. The evaluation results are shown in Table 4. Toner triboelectric charge retention rate (%) = [Toner triboelectric charge after one week] / [Initial toner triboelectric charge] x 100 (Evaluation Criteria) A: Triboelectric charge retention rate is 80% or more B: Triboelectric charge retention rate is 60% or more and less than 80% C: Triboelectric charge retention rate is less than 60%

[0188] [Table 4]

[0189] Toner A-32 is a toner produced using sodium chloride, which is water-soluble, without going through the filtering, washing, and drying processes. As a result, the toner contains sodium chloride, which results in unacceptable storage stability and charge retention.

[0190] Toner A-33 was produced using conditions in which the amount of grinding agent relative to the pigment was too high, resulting in unacceptable low charge retention and low color strength.

[0191] Toner A-34 was produced under conditions where the amount of grinding agent relative to the pigment was too small, resulting in insufficient disintegration, large pigment particle size, and unacceptable color strength.

[0192] Toner A-35 was manufactured under conditions where the amount of binder in the pigment dispersion was too small, resulting in insufficient mixing of the pigment and grinding agent, resulting in large pigment particle size and unacceptable color strength.

[0193] Toner A-36 was produced under conditions in which the amount of binder in the pigment dispersion was too high, resulting in a low degree of pigment disintegration by the grinding agent, large pigment particle size, and unacceptable color strength.

[0194] Toner A-37 was produced under conditions where the grinding agent particle size was too small, resulting in insufficient pigment disintegration by the grinding agent, resulting in large pigment particle size and unacceptable tinting strength.

[0195] Toner A-38 was produced under conditions where the grinding agent particle size was too large, resulting in unacceptably low charge retention and low color strength.

[0196] In toner A-39, the viscosity of the binder during pigment grinding was too high, so the pigment and grinding agent could not be mixed sufficiently, resulting in large pigment particle size and unacceptable coloring power.

[0197] <Production of Pigment Dispersion B-1> Pigment 35 parts (Cyan pigment: Pigment Blue 15:3, volume average particle size 102nm) Grinding agent 35 parts (Light calcium carbonate, number average particle size 0.4μm) Binder B-1 30 parts (Synthetic wax; Nippon Seiro FNP0090, melting point = 90°C, number average molecular weight 578) The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100°C, the mixture was kneaded in a twin-screw kneader (PCM-30, Ikegai Corporation). The resulting kneaded product was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100μm or less, obtaining coarsely pulverized pigment dispersion B-1. The melt viscosity of binder B-1 at 100°C was less than 1000 Pa·sec. The number average particle size of the pigment in the resulting pigment dispersion B-1 was 59nm.

[0198] <Production of Pigment Dispersion B-2> A coarsely ground pigment dispersion B-2 was obtained in the same manner as for pigment dispersion B-1, except that binder B-2 [stearic acid (Tokyo Chemical Industry Co., Ltd., melting point = 70 ° C, number average molecular weight 286)] was used instead of binder B-1 and the kneading temperature was 80 ° C. The melt viscosity of binder B-2 at 80 ° C was less than 1000 Pa sec. The number average particle size of the pigment in the obtained pigment dispersion B-2 was 58 nm.

[0199] <Production of Pigment Dispersion B-3> A coarsely ground pigment dispersion B-3 was obtained in the same manner as for pigment dispersion B-1, except that binder B-3 [hydrocarbon wax (HNP-51 manufactured by Nippon Seiro, melting point = 77°C, number average molecular weight 522)] was used instead of binder B-1 and the kneading temperature was 90°C. The melt viscosity of binder B-3 at 90°C was less than 1000 Pa sec. The number average particle size of the pigment in the obtained pigment dispersion B-3 was 55 nm.

[0200] <Production of Pigment Dispersion B-4> A coarsely ground pigment dispersion B-4 was obtained in the same manner as for pigment dispersion B-1, except that binder B-1 was replaced with binder B-4 [carnauba wax (carnauba wax manufactured by Yamakei Sangyo Co., Ltd., melting point = 83°C, number average molecular weight 396)]. The melt viscosity of binder B-4 at 100°C was less than 1000 Pa·sec. The number average particle size of the pigment in the obtained pigment dispersion B-4 was 56 nm.

[0201] <Production of Pigment Dispersion B-5> A coarsely ground pigment dispersion B-5 was obtained in the same manner as for pigment dispersion B-1, except that binder B-5 [hydrocarbon wax (Paraffin Wax-135, manufactured by Nippon Seiro, melting point = 58°C, number average molecular weight 370)] was used instead of binder B-1 and the kneading temperature was 70°C. The melt viscosity of binder B-5 at 70°C was less than 1000 Pa sec. The number average particle size of the pigment in the obtained pigment dispersion B-5 was 58 nm.

[0202] <Production of Pigment Dispersion B-6> A coarsely ground pigment dispersion B-6 was obtained in the same manner as for pigment dispersion B-1, except that binder B-1 was replaced with binder B-6 [hydrocarbon wax (SX-105 manufactured by Nippon Seiro, melting point = 117°C, 912)] and the kneading temperature was changed to 130°C. The melt viscosity of binder B-6 at 130°C was less than 1000 Pa·sec. The number average particle size of the pigment in the obtained pigment dispersion B-6 was 59 nm.

[0203] <Production of Pigment Dispersion B-7> A coarsely ground pigment dispersion B-7 was obtained in the same manner as for pigment dispersion B-1, except that binder B-1 was replaced with binder B-7 [polyolefin wax (Mitsui Chemicals NP-056, melting point = 129°C, number average molecular weight 7000)] and the kneading temperature was 140°C. The melt viscosity of binder B-7 at 140°C was less than 1000 Pa sec. The number average particle size of the pigment in the obtained pigment dispersion B-7 was 58 nm.

[0204] <Production of Pigment Dispersions B-8 to B-15 and B-18 to B-28> Pigment dispersions B-8 to B-15 and B-18 to B-28 were obtained in the same manner as pigment dispersion B-1, except that binder B-3 was used instead of binder B-1, and the grinding agents and pigments shown in Table 5 below were used and kneaded under the conditions shown in Table 6. The number average particle size of the pigment in each of the obtained pigment dispersions is shown in Table 6.

[0205] <Production of pigment dispersions B-16 and B-17> Coarsely ground pigment dispersions B-16 and B-17 were obtained in the same manner as for pigment dispersion B-3, except that binder B-1 was replaced with a mixture of binder B-3 and crystalline polyester in the ratio shown in Table 5. The melt viscosity at 90°C of the binder and the number average particle size of the obtained pigment dispersions are shown in Table 6.

[0206] The crystalline polyester in pigment dispersions B-16 and B-17 is as follows. Crystalline polyester: Composition (mol%) [1,6-hexanediol:dodecanedioic acid = 100:100], melting point = 72°C In addition, in the case of pigment dispersion B-8, a single screw extruder was used instead of the twin screw extruder.

[0207] [Table 5]

[0208] [Table 6]

[0209] <Production Example of Toner B-1> Amorphous polyester I 77.7 parts (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 ) Pigment Dispersion B-1 14.3 parts Hydrocarbon wax 8.0 parts (Maximum endothermic peak temperature 90℃) The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100° C., the mixture was melted and kneaded in a twin-screw kneader (PCM-30, Ikegai Corporation). The kneaded mixture was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (T-250, Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes to obtain the target particle size. Classification was then performed using a rotary classifier (200TSP, Hosokawa Micron Corporation) to obtain toner particles with a weight average particle size of 6.5 μm. The operating conditions of the rotary classifier (200TSP, Hosokawa Micron Corporation) were such that the rotation speed was adjusted to obtain the target particle size and particle size distribution.

[0210] 100 parts of the obtained toner particles were mixed with silica fine particles (BET specific surface area 200 m) that had been hydrophobized with silicone oil.2 The mixture was mixed with 1.8 parts of 1.0 parts of 1 / g of 100 ml of water and mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for a rotation time of 10 minutes to obtain Toner B-1.

[0211] <Production Examples of Toners B-2 to B-7, B-9 to B-18, and B-21 to B-32> Except for changing the materials and conditions shown in Table 7, the toners were produced in the same manner as Toner B-1, toners B-2 to B-7, B-9 to B-18, and B-21 to B-32.

[0212] Additionally, toners B-26 to B-32 produced using pigment dispersions B-22 to B-28 are described as comparative examples.

[0213] <Production Example of Toner B-8> Toner B-8 was obtained in the same manner as in the production of Toner B-1, except that the following amorphous polyester II was used instead of the amorphous polyester I. Amorphous polyester II: Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:fumaric acid:terephthalic acid=100:76:24], softening point (Tm)=106°C, glass transition temperature (Tg)=59°C, SP value=21.7 (J / cm 3 ) 0.5 <Production Example of Toner B-19> 60 parts of Pigment Dispersion B-3, 150 parts of toluene as a solvent, and 130 parts of glass beads (diameter 1 mm) were mixed and dispersed for 3 hours using an attritor (manufactured by Nippon Coke & Co., Ltd.) to obtain a pigment dispersion.

[0214] Next, 11.7 parts of trisodium phosphate dodecahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) and 1200 parts of ion-exchanged water were added to a beaker set in a water bath to dissolve the trisodium phosphate dodecahydrate. Then, the temperature of the water bath was raised to 60°C. After reaching 60°C, an aqueous solution in which 5.15 parts of calcium chloride (manufactured by Kishida Chemical Industries, Ltd.) was dissolved in 100 parts of ion-exchanged water was added. After the addition, the mixture was stirred for 30 minutes to obtain an aqueous medium containing tricalcium phosphate. Amorphous polyester I 80.0 parts Pigment dispersion 50.0 parts Hydrocarbon wax (maximum endothermic peak temperature 90°C) 5.7 parts Toluene 350.0 parts The above materials were mixed and heated to 80° C. with stirring to dissolve and disperse each material, thereby preparing a resin composition.

[0215] Meanwhile, 600 parts of the aqueous medium containing the above-mentioned tricalcium phosphate was heated to 80°C while stirring with Clearmix (manufactured by M Technique Co., Ltd.). A resin composition was added to the aqueous medium containing the tricalcium phosphate, and the mixture was stirred at 10,000 rpm for 10 minutes to obtain a dispersion. The obtained dispersion was stirred with a stirring blade for 5 hours at 80°C to remove toluene. The mixture was then cooled to 25°C for 10 minutes to obtain an aqueous dispersion of toner particles.

[0216] Dilute hydrochloric acid was added to the obtained aqueous dispersion of toner particles while stirring, and the mixture was stirred for 2 hours at pH 1.5 to dissolve tricalcium phosphate, and then the mixture was subjected to solid-liquid separation using a filter to obtain toner particles.

[0217] The mixture was poured into water and stirred to prepare a dispersion again, and then the mixture was subjected to solid-liquid separation using a filter. This operation was repeated until the tricalcium phosphate was sufficiently removed, and the obtained toner particles were sufficiently dried using a dryer to obtain toner particles.

[0218] The obtained toner particles were subjected to external addition in the same manner as in Toner B-1 to obtain Toner B-19.

[0219] <Production Example of Toner B-20> Styrene 50.9 parts n-Butyl acrylate 16.1 parts Pigment Dispersion B-7 14.3 parts Hydrocarbon wax (maximum endothermic peak temperature 90℃) 15.7 parts Amorphous polyester I 3.0 parts A mixture consisting of the above was prepared. The mixture was placed in an attritor (manufactured by Nippon Coke Corporation) and dispersed at 200 rpm for 2 hours using zirconia beads having a diameter of 5 mm to obtain a raw material dispersion.

[0220] On the other hand, 735.0 parts of ion-exchanged water and 16.0 parts of trisodium phosphate (12-hydrate) were added to a container equipped with a high-speed stirring device homomixer (manufactured by Primix Corporation) and a thermometer, and the temperature was raised to 60°C while stirring at 12000 rpm. An aqueous calcium chloride solution in which 9.0 parts of calcium chloride (2-hydrate) was dissolved in 65.0 parts of ion-exchanged water was added thereto, and the mixture was stirred at 12000 rpm for 30 minutes while maintaining the temperature at 60°C. 10% hydrochloric acid was added thereto to adjust the pH to 6.0, and an aqueous medium containing a dispersion stabilizer was obtained.

[0221] Next, the raw material dispersion liquid was transferred to a vessel equipped with a stirrer and a thermometer, and heated to 60° C. while stirring at 100 rpm. 8.0 parts of t-butyl peroxypivalate (Perbutyl PV, manufactured by NOF Corp.) was added thereto as a polymerization initiator, and after stirring at 100 rpm for 5 minutes while maintaining 60° C., it was poured into the aqueous medium being stirred at 12000 rpm by the high-speed stirrer. Stirring was continued for 20 minutes at 12000 rpm by the high-speed stirrer while maintaining 60° C., to obtain a granulation liquid. The granulation liquid was transferred to a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube, and heated to 70° C. while stirring at 150 rpm under a nitrogen atmosphere. A polymerization reaction was carried out at 150 rpm for 10 hours while maintaining 70° C. Thereafter, the reflux condenser was removed from the reaction vessel, and the reaction liquid was heated to 95° C., and then stirred at 150 rpm for 5 hours while maintaining 95° C., to obtain a toner particle dispersion liquid.

[0222] The resulting toner particle dispersion was cooled to 20°C while stirring at 150 rpm, and then diluted hydrochloric acid was added with stirring until the pH reached 1.5 to dissolve the dispersion stabilizer. The solid content was filtered and thoroughly washed with ion-exchanged water, and then vacuum-dried at 40°C for 24 hours to obtain toner particles.

[0223] The obtained toner particles were subjected to external addition in the same manner as in Toner B-1 to obtain Toner B-20.

[0224] <Production Example of Toner B-21> - Manufacturing of amorphous resin particles Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) 200 parts Amorphous polyester I 120 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 0.6 parts After mixing the above, the mixture was stirred for 12 hours to dissolve the resin.

[0225] Next, 2.7 g of N,N-dimethylaminoethanol was added, and the mixture was stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation).

[0226] Further, 359.4 parts of ion-exchanged water was added at a rate of 1 g / min to precipitate resin fine particles, after which tetrahydrofuran was removed using an evaporator to obtain amorphous resin fine particles and a dispersion thereof. - Manufacturing of pigment dispersion fine particles Pigment Dispersion B-3 10.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 0.5 parts Ion-exchanged water 89.5 parts The above ingredients were mixed, heated to 90°C for dissolution, and dispersed for approximately 1 hour using a high-pressure impact disperser Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a dispersion of pigment dispersion fine particles in water. - Manufacturing of release agent particles Hydrocarbon wax (maximum endothermic peak temperature 90°C) 20.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.0 part Ion-exchanged water 79.0 parts The above ingredients were placed in a mixing vessel equipped with an agitator, heated to 90°C, and circulated through a Clearmix W Motion (manufactured by M Technique) while being stirred at a shear mixing section with a rotor outer diameter of 3 cm and clearance of 0.3 mm at a rotor rotation speed of 19,000 rpm and a screen rotation speed of 19,000 rpm for 60 minutes for dispersion processing.

[0227] Thereafter, the mixture was cooled to 40° C. under cooling treatment conditions of a rotor rotation speed of 1000 rpm, a screen rotation speed of 0 rpm, and a cooling rate of 10° C. / min, to obtain a dispersion liquid of release agent fine particles.

[0228] A method for producing a toner using the above dispersion liquid will be exemplified below. Dispersion of amorphous polyester I 320 parts Pigment dispersion fine particle dispersion liquid 143 parts Dispersion of release agent particles 28.5 parts -Ion-exchanged water 400 parts The above materials were placed in a round stainless steel flask and mixed, after which an aqueous solution of 2 parts magnesium sulfate dissolved in 98 parts ion-exchanged water was added thereto, and the mixture was dispersed at 5,000 rpm for 10 minutes using a homogenizer (IKA Ultra Turrax T50).

[0229] Thereafter, the mixture was heated to 58° C. in a heating water bath while appropriately adjusting the rotation speed using a stirring blade so that the mixture was stirred. The mixture was kept at 58° C. for 1 hour to obtain aggregated particles.

[0230] To the dispersion liquid containing the aggregated particles, an aqueous solution in which 20 parts of trisodium citrate was dissolved in 380 parts of ion-exchanged water was added, and the mixture was then heated to 95°C.

[0231] After keeping the temperature at 95° C. for 2 hours, the mixture was cooled to 25° C. while continuing to stir, thereby obtaining a toner particle dispersion liquid.

[0232] Thereafter, after filtration and solid-liquid separation, the filter cake was thoroughly washed with ion-exchanged water and dried using a vacuum dryer to obtain toner particles.

[0233] The obtained toner particles were subjected to external addition in the same manner as in Toner B-1 to obtain Toner B-21.

[0234] [Table 7]

[0235] <Production Example of Two-Component Developer B-1> A magnetic carrier having a volume distribution-based 50% particle size (D50) of 38.2 μm was prepared by forming a coating layer of a copolymer of cyclohexyl methacrylate, methyl methacrylate, and methyl methacrylate macromonomer on the surface of a Mn-Mg-Sr ferrite carrier core.

[0236] 92.0 parts of this magnetic carrier and 8.0 parts of toner B-1 were mixed in a V-type mixer (V-20, manufactured by Seishin Enterprises) to obtain two-component developer B-1.

[0237] <Production Examples of Two-Component Developers B-2 to B-32> Two-component developers B-2 to B-32 were obtained in the same manner as in the production example of two-component developer B-1, except that toner B-1 was changed to toners B-2 to B-32.

[0238] <Evaluation of grindability> In the manufacturing process of each toner, 1000 kg of the coarsely ground material was pulverized using a mechanical pulverizer (T-250, manufactured by Turbo Kogyo Co., Ltd.) to produce a finely ground product with a weight average particle size of 6.2 μm. The power consumption of the mechanical pulverizer was measured at this time, and this value was used as an index of grindability. The power consumption of toner B-27 was used as the reference power consumption, and evaluation was performed according to the following criteria. The smaller the power consumption, the better the grindability and the more productive it is. The results are shown in Table 8.

[0239] (Evaluation Criteria) A: Less than 90% of standard power consumption B: 90% to 110% of standard power consumption C: 110% or more of standard power consumption <Method for evaluating toner coloring power> A modified Canon imageRUNNER ADVANCE C5255 full-color copying machine was used as the image forming apparatus, and each two-component developer was charged into the developing device of the cyan station to perform the evaluation.

[0240] The evaluation environment was normal temperature and humidity (23°C, 50% RH), and the evaluation paper was GFC-081 plain copy paper (A4, basis weight 81.4 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0241] First, in the evaluation environment, the amount of toner applied on the paper was changed to examine the relationship between image density and the amount of toner applied on the paper.

[0242] Next, the image density of the FFH image (solid portion) was adjusted to 1.40, and the toner amount when the image density reached 1.40 was determined.

[0243] An FFH image is a value obtained by expressing 256 gradations in hexadecimal, with 00H being the first gradation (white area) and FFH being the 256th gradation (solid area).

[0244] The image density was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite).

[0245] The toner load (mg / cm 2 The coloring power of the toner was evaluated based on the following criteria. The evaluation results are shown in Table 8.

[0246] (Evaluation Criteria) A: Less than 0.35 B: 0.35 or more, less than 0.50 C: 0.50 or more, less than 0.65 D:0.65 or more <Evaluation of charge retention> Each two-component developer was used, and the amount of triboelectric charge of the toner was measured, and the chargeability of the toner was evaluated according to the following criteria.

[0247] The triboelectric charge of the toner was measured using an Espart analyzer manufactured by Hosokawa Micron Corporation.

[0248] After measuring the initial triboelectric charge amount of the toner, each two-component developer was left to stand in a thermo-hygrostat (temperature 30° C., humidity 80% RH) for one week, and then the triboelectric charge amount was measured again using the toner.

[0249] The measurement results were substituted into the following formula to calculate the triboelectric charge retention rate, and the results were evaluated according to the following criteria. The evaluation results are shown in Table 8. Toner triboelectric charge retention rate (%) = [Toner triboelectric charge after one week] / [Initial toner triboelectric charge] x 100 (Evaluation Criteria) A: Triboelectric charge retention rate is 80% or more B: Triboelectric charge retention rate is 60% or more and less than 80% C: Triboelectric charge retention rate is less than 60%

[0250] [Table 8]

[0251] Toner B-26 was not subjected to the filtering, washing, and drying processes, so salt was contained in the toner, resulting in unacceptable charging properties. In addition, the salt reduced the grindability during grinding.

[0252] In toner B-27, the amount of grinding agent relative to the pigment is small, so sufficient disintegration is not achieved, and the pigment particle size is large, resulting in unacceptable coloring power.

[0253] Toner B-28 has an unacceptable result in that the amount of grinding agent relative to the pigment is too high, resulting in reduced charge retention and coloring power when made into a toner.

[0254] In toner B-29, the amount of binder in the pigment dispersion is small, so the pigment and grinding agent cannot be mixed sufficiently, and the pigment particle size is large, resulting in unacceptable color strength.

[0255] In toner B-30, the amount of binder in the pigment dispersion is too high, which reduces the pigment disintegration ability of the grinding agent and results in unacceptable coloring power due to the large pigment particle size.

[0256] In toner B-31, the small particle size of the grinding agent reduces the pigment disintegration by the grinding agent, and the large particle size of the pigment results in unacceptable color strength.

[0257] Toner B-32 has unacceptable results because the particle size of the grinding agent is large, resulting in a decrease in the charge retention and coloring power when made into a toner.

[0258] <Preparation of Pigment Dispersion C-1> Pigment 35 parts (Cyan pigment: Pigment Blue 15:3, volume average particle size 102nm) Grinding agent 35 parts (Light calcium carbonate, number average particle size 0.4μm) Binder C-1 30 parts (Crystalline polyester: composition (mol%) [sebacic acid:nonanediol = 50:50], melting point (Tp) = 72°C, SP value = 19.8 (J / cm 3 ) 0.5 ) The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100°C, the mixture was kneaded at 85°C in a twin-screw kneader (PCM-30, Ikegai Corporation). The resulting kneaded mixture was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less, obtaining coarsely pulverized pigment dispersion C-1. The melt viscosity of binder C-1 at 85°C was less than 1000 Pa sec. The number average particle size of the pigment in the resulting pigment dispersion C-1 was 52 nm.

[0259] <Preparation of Pigment Dispersion C-2> Binder C-1 was replaced with binder C-2 [crystalline vinyl resin (composition (mol%) [behenyl acrylate: acrylonitrile: styrene = 25.3: 59.5: 15.2], melting point (Tp) = 62 °C, SP value = 20.7 (J / cm 3 )0.5 )] and kneaded at 75°C in the same manner as for Pigment Dispersion C-1, to obtain a coarsely ground product of Pigment Dispersion C-2. The melt viscosity of Binder C-2 at 75°C was 2200 Pa sec. The number-average particle size of the pigment in the obtained Pigment Dispersion C-2 was 49 nm.

[0260] <Production of Pigment Dispersion C-3> Binder C-1 was replaced with binder C-3 [crystalline polyester (composition (mol%) [decanedicarboxylic acid:hexanediol = 50:50], melting point (Tp) = 75 °C, SP value = 19.9 (J / cm 3 ) 0.5 A coarsely ground pigment dispersion C-3 was obtained in the same manner as for pigment dispersion C-1, except that the binder C-3 had a melt viscosity of less than 1000 Pa·sec at 85°C. The number-average particle size of the pigment in the obtained pigment dispersion C-3 was 51 nm.

[0261] <Production of Pigment Dispersions C-4 to C-11 and C-14 to C-28> The number average particle diameters of the pigments in pigment dispersions C-4 to C-11 and C-14 to C-28 obtained by kneading the binders, grinding agents, and pigments shown in Table 9 below under the conditions shown in Table 10 are shown in Table 10.

[0262] The amorphous polyester in pigment dispersions C-14 and C-15 is as follows. Amorphous polyester: composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 In addition, in the case of pigment dispersion C-4, a single screw extruder was used instead of the twin screw extruder.

[0263] <Preparation of Pigment Dispersion C-12> Binder C-1 was replaced with binder C-4 [crystalline polyester; number average molecular weight about 6000, melting point (Tp) = 71°C, SP value = 18.8 (J / cm 3) 0.5 A coarsely ground pigment dispersion C-12 was obtained in the same manner as for Pigment Dispersion C-1, except that the mixing temperature was changed to 75°C and the binder C-4 had a melt viscosity of less than 1000 Pa sec at 75°C. The number-average particle size of the pigment in the obtained Pigment Dispersion C-12 was 52 nm.

[0264] <Production of Pigment Dispersion C-13> Binder C-1 was replaced with binder C-5 [crystalline polyester; number average molecular weight about 2000, melting point (Tp) = 69°C, SP value = 18.3 (J / cm 3 ) 0.5 A coarsely ground pigment dispersion C-13 was obtained in the same manner as for pigment dispersion C-1, except that the mixing temperature was changed to 75°C and the binder C-5 had a melt viscosity of less than 1000 Pa·sec at 75°C. The number-average particle size of the pigment in the obtained pigment dispersion C-13 was 53 nm.

[0265] [Table 9]

[0266] [Table 10]

[0267] <Production Example of Toner C-1> Amorphous polyester 77.7 parts (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 ) Pigment Dispersion C-1 14.3 parts Hydrocarbon wax 8.0 parts (Maximum endothermic peak temperature 90℃) The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1After mixing for 5 minutes at 100° C., the mixture was kneaded in a twin-screw kneader (PCM-30 type, manufactured by Ikegai Corporation). The kneaded product was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (T-250, manufactured by Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes so as to obtain the target particle size. Classification was further performed using a rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) to obtain toner particles with a weight average particle size of 6.5 μm. The operating conditions of the rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) were such that the rotation speed was adjusted so as to obtain the target particle size and particle size distribution, and classification was performed.

[0268] 100 parts of the obtained toner particles were mixed with silica fine particles (BET specific surface area 200 m) that had been hydrophobized with silicone oil. 2 The mixture was mixed with 1.8 parts of 1.0 parts of 1 / g of 100 ml of water and mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for 10 minutes to obtain Toner C-1.

[0269] <Production Examples of Toners C-2 to C-12, C-14 to C-19, and C-23 to C-32> Except for changing the materials and conditions shown in Table 11, the same production method as for toner C-1 was used to obtain toners C-2 to C-12, C-14 to C-19, and C-23 to C-32.

[0270] In the toner C-12, the amorphous polyester was changed to the following crystalline vinyl resin. Crystalline vinyl resin (composition (mol%) [behenyl acrylate: acrylonitrile: styrene = 25.3: 59.5: 15.2], melting point (Tp) = 62 °C, SP value = 20.7 (J / cm 3 ) 0.5 ) In addition, in toner C-14, the amorphous polyester was changed to the following amorphous polyester. Amorphous polyester: composition (mol%) [polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: terephthalic acid: trimellitic acid = 100:80:20], softening point (Tm) = 135°C, glass transition temperature (Tg) = 69°C, SP value = 23.6 (J / cm 3 ) 0.5 Additionally, toners C-26 to C-32 produced using pigment dispersions C-22 to C-28 are described as comparative examples.

[0271] <Production Example of Toner C-13> Toner C-13 was obtained in the same manner as in toner C-1, except that the amorphous polyester was changed to the following amorphous polyester. Amorphous polyester; composition (mol%) [polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: terephthalic acid: trimellitic acid = 100: 80: 20], softening point (Tm) = 135°C, glass transition temperature (Tg) = 69°C, SP value = 23.6 (J / cm 3 ) 0.5 <Production Example of Toner C-21> 60 parts of pigment dispersion C-1, 150 parts of toluene as a solvent, and 130 parts of glass beads (diameter 1 mm) were mixed and dispersed for 3 hours using an attritor (manufactured by Nippon Coke & Co., Ltd.) to obtain a pigment dispersion.

[0272] Next, 11.7 parts of trisodium phosphate dodecahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) and 1200 parts of ion-exchanged water were added to a beaker set in a water bath to dissolve the trisodium phosphate dodecahydrate. Then, the temperature of the water bath was raised to 60°C. After reaching 60°C, an aqueous solution in which 5.15 parts of calcium chloride (manufactured by Kishida Chemical Industries, Ltd.) was dissolved in 100 parts of ion-exchanged water was added. After the addition, the mixture was stirred for 30 minutes to obtain an aqueous medium containing tricalcium phosphate. Amorphous polyester 75.7 parts (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 ) 50.0 parts of the above pigment dispersion Hydrocarbon wax (maximum endothermic peak temperature 90℃) 10.0 parts Toluene 350.0 parts The above materials were mixed and heated to 80° C. with stirring to dissolve and disperse each material, thereby preparing a resin composition.

[0273] Meanwhile, 600 parts of the aqueous medium containing the above-mentioned tricalcium phosphate was heated to 80°C while stirring with Clearmix (manufactured by M Technique Co., Ltd.). A resin composition was added to the aqueous medium containing the tricalcium phosphate, and the mixture was stirred at 10,000 rpm for 10 minutes to obtain a dispersion. The obtained dispersion was stirred with a stirring blade for 5 hours at 80°C to remove toluene. The mixture was then cooled to 25°C for 10 minutes to obtain an aqueous dispersion of toner particles.

[0274] Dilute hydrochloric acid was added to the obtained aqueous dispersion of toner particles while stirring, and the mixture was stirred for 2 hours at pH 1.5 to dissolve tricalcium phosphate, and then the mixture was subjected to solid-liquid separation using a filter to obtain toner particles.

[0275] The mixture was poured into water and stirred to prepare a dispersion again, and then the mixture was subjected to solid-liquid separation using a filter. This operation was repeated until the tricalcium phosphate was sufficiently removed, and the obtained toner particles were sufficiently dried using a dryer to obtain toner particles.

[0276] The obtained toner particles were subjected to external addition in the same manner as in Toner C-1 to obtain Toner C-21.

[0277] <Production Example of Toner C-22> Styrene 47.6 parts n-Butyl acrylate 15.1 parts Pigment Dispersion C-1 14.3 parts Hydrocarbon wax (maximum endothermic peak temperature 90℃) 20.0 parts Amorphous polyester 3.0 parts (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 ) A mixture consisting of the above was prepared. The mixture was placed in an attritor (manufactured by Nippon Coke Corporation) and dispersed at 200 rpm for 2 hours using zirconia beads having a diameter of 5 mm to obtain a raw material dispersion.

[0278] On the other hand, 735.0 parts of ion-exchanged water and 16.0 parts of trisodium phosphate (12-hydrate) were added to a container equipped with a high-speed stirring device homomixer (manufactured by Primix Corporation) and a thermometer, and the temperature was raised to 60°C while stirring at 12000 rpm. An aqueous calcium chloride solution in which 9.0 parts of calcium chloride (2-hydrate) was dissolved in 65.0 parts of ion-exchanged water was added thereto, and the mixture was stirred at 12000 rpm for 30 minutes while maintaining the temperature at 60°C. 10% hydrochloric acid was added thereto to adjust the pH to 6.0, and an aqueous medium containing a dispersion stabilizer was obtained.

[0279] Next, the raw material dispersion liquid was transferred to a vessel equipped with a stirrer and a thermometer, and heated to 60° C. while stirring at 100 rpm. 8.0 parts of t-butyl peroxypivalate (Perbutyl PV, manufactured by NOF Corp.) was added thereto as a polymerization initiator, and after stirring at 100 rpm for 5 minutes while maintaining 60° C., it was poured into the aqueous medium being stirred at 12000 rpm by the high-speed stirrer. Stirring was continued for 20 minutes at 12000 rpm by the high-speed stirrer while maintaining 60° C., to obtain a granulation liquid. The granulation liquid was transferred to a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube, and heated to 70° C. while stirring at 150 rpm under a nitrogen atmosphere. A polymerization reaction was carried out at 150 rpm for 10 hours while maintaining 70° C. Thereafter, the reflux condenser was removed from the reaction vessel, and the reaction liquid was heated to 95° C., and then stirred at 150 rpm for 5 hours while maintaining 95° C., to obtain a toner particle dispersion liquid.

[0280] The resulting toner particle dispersion was cooled to 20°C while stirring at 150 rpm, and then diluted hydrochloric acid was added with stirring until the pH reached 1.5 to dissolve the dispersion stabilizer. The solid content was filtered and thoroughly washed with ion-exchanged water, and then vacuum-dried at 40°C for 24 hours to obtain toner particles.

[0281] The obtained toner particles were subjected to external addition in the same manner as in Toner C-1 to obtain Toner C-22.

[0282] <Production Example of Toner C-23> - Manufacturing of amorphous resin particles Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) 200 parts Amorphous polyester 120 parts (Composition (mol%) [polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid=100:50:50], softening point (Tm)=122°C, glass transition temperature (Tg)=70°C, SP value=22.6 (J / cm 3 ) 0.5 ) Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 0.6 parts After mixing the above, the mixture was stirred for 12 hours to dissolve the resin.

[0283] Next, 2.7 parts of N,N-dimethylaminoethanol was added, and the mixture was stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation).

[0284] Further, 359.4 parts of ion-exchanged water was added at a rate of 1 part / min to precipitate resin fine particles, after which tetrahydrofuran was removed using an evaporator to obtain amorphous resin fine particles and a dispersion thereof. - Manufacturing of pigment dispersion fine particles Pigment Dispersion C-1 24.0 parts Methyl ethyl ketone 76.0 parts The above materials were gradually added to a container, stirred, and completely dissolved, then the temperature was set to 40°C. 0.1 parts of N,N-dimethylaminoethanol was added while stirring, and then an aqueous solution of 1.5 parts of Nergen RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) mixed with 74.5 parts of ion-exchanged water was gradually added dropwise to cause phase inversion emulsification. After further reducing the pressure to remove the solvent, the mixture was dispersed for about 1 hour using a high-pressure impact disperser Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a dispersion of pigment dispersion fine particles in which the pigment dispersion was dispersed in water. - Manufacturing of release agent particles Hydrocarbon wax (maximum endothermic peak temperature 90°C) 10.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.0 part Ion-exchanged water 89.0 parts The above ingredients were placed in a mixing vessel equipped with an agitator, heated to 90°C, and circulated through a Clearmix W Motion (manufactured by M Technique) while being stirred at a shear mixing section with a rotor outer diameter of 3 cm and clearance of 0.3 mm at a rotor rotation speed of 19,000 rpm and a screen rotation speed of 19,000 rpm for 60 minutes for dispersion processing.

[0285] Thereafter, the mixture was cooled to 40° C. under cooling treatment conditions of a rotor rotation speed of 1000 rpm, a screen rotation speed of 0 rpm, and a cooling rate of 10° C. / min, to obtain a dispersion liquid of release agent fine particles.

[0286] A method for producing a toner using the above dispersion liquid will be exemplified below. Amorphous polyester dispersion 302.8 parts Pigment dispersion fine particle dispersion liquid 59.6 parts Dispersion of release agent particles 100.0 parts Ion-exchanged water 400.0 parts The above materials were placed in a round stainless steel flask and mixed, after which an aqueous solution of 2 parts magnesium sulfate dissolved in 98 parts ion-exchanged water was added thereto, and the mixture was dispersed at 5,000 rpm for 10 minutes using a homogenizer (IKA Ultra Turrax T50).

[0287] Thereafter, the mixture was heated to 58° C. in a heating water bath while appropriately adjusting the rotation speed using a stirring blade so that the mixture was stirred. The mixture was kept at 58° C. for 1 hour to obtain aggregated particles.

[0288] To the dispersion liquid containing the aggregated particles, an aqueous solution in which 20 parts of trisodium citrate was dissolved in 380 parts of ion-exchanged water was added, and the mixture was then heated to 95°C.

[0289] After keeping the temperature at 95° C. for 2 hours, the mixture was cooled to 25° C. while continuing to stir, thereby obtaining a toner particle dispersion liquid.

[0290] Thereafter, after filtration and solid-liquid separation, the filter cake was thoroughly washed with ion-exchanged water and dried using a vacuum dryer to obtain toner particles.

[0291] The obtained toner particles were subjected to external addition in the same manner as in Toner C-1 to obtain Toner C-23.

[0292] [Table 11]

[0293] <Production example of two-component developer C-1> A magnetic carrier having a volume distribution-based 50% particle size (D50) of 38.2 μm was prepared by forming a coating layer of a copolymer of cyclohexyl methacrylate, methyl methacrylate, and methyl methacrylate macromonomer on the surface of a Mn-Mg-Sr ferrite carrier core.

[0294] 92.0 parts of this magnetic carrier and 8.0 parts of toner C-1 were mixed in a V-type mixer (V-20, manufactured by Seishin Enterprises) to obtain two-component developer C-1.

[0295] <Production Examples of Two-Component Developers C-2 to C-32> Two-component developers C-2 to C-32 were obtained in the same manner as in the production example of two-component developer C-1, except that toner C-1 was changed to toners C-2 to C-32.

[0296] <Method for evaluating toner coloring power> A modified Canon imageRUNNER ADVANCE C5255 full-color copying machine was used as the image forming apparatus, and each two-component developer was charged into the developing device of the cyan station to perform the evaluation.

[0297] The evaluation environment was normal temperature and humidity (23°C, 50% RH), and the evaluation paper was GFC-081 plain copy paper (A4, basis weight 81.4 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0298] First, in the evaluation environment, the amount of toner applied on the paper was changed to examine the relationship between image density and the amount of toner applied on the paper.

[0299] Next, the image density of the FFH image (solid portion) was adjusted to 1.40, and the toner amount when the image density reached 1.40 was determined.

[0300] An FFH image is a value obtained by expressing 256 gradations in hexadecimal, with 00H being the first gradation (white area) and FFH being the 256th gradation (solid area).

[0301] The image density was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite).

[0302] The toner load (mg / cm 2 The coloring power of the toner was evaluated based on the following criteria. The evaluation results are shown in Table 12.

[0303] (Evaluation Criteria) A: Less than 0.35 B: 0.35 or more, less than 0.50 C: 0.50 or more, less than 0.65 D:0.65 or more <Evaluation of low-temperature fixing ability of toner> Paper: GFC-081 (81.0g / m 2 ) (Sold by Canon Marketing Japan Inc.) Toner load on paper: 0.50mg / cm 2 (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Evaluation image: A 2cm x 5cm image placed in the center of the A4 paper. Test environment: Low temperature and low humidity environment: Temperature 15℃ / Humidity 10%RH (hereinafter referred to as "L / L") Fixing temperature: 130℃ Process speed: 377mm / sec The above evaluation image was output, and the low-temperature fixability was evaluated. The value of the image density reduction rate was used as an evaluation index for low-temperature fixability. The image density reduction rate was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite Corporation), and first, the image density in the center was measured. Next, the part where the image density was measured was subjected to pressure of 4.9 kPa (50 g / cm 2 The fixed image was rubbed (five times back and forth) with Silbon paper under a load of 1000 g / m2, and the image density was measured again. The image density reduction rate before and after rubbing was calculated using the following formula. The obtained image density reduction rate was evaluated according to the following evaluation criteria. Image density decrease rate = (image density before rubbing - image density after rubbing) / image density before rubbing x 100 (Evaluation Criteria) A: Image density reduction rate is less than 3.0% B: Image density reduction rate: 3.0% or more and less than 10.0% C: Image density reduction rate: 10.0% or more and less than 15.0% D: Image density reduction rate of 15.0% or more <Evaluation of Toner Charge Retention> Each two-component developer was used, and the amount of triboelectric charge of the toner was measured, and the chargeability of the toner was evaluated according to the following criteria.

[0304] The triboelectric charge of the toner was measured using an Espart analyzer manufactured by Hosokawa Micron Corporation.

[0305] After measuring the initial triboelectric charge amount of the toner, the two-component developer was left to stand in a thermo-hygrostat (temperature 30° C., humidity 80% RH) for one week, and the triboelectric charge amount was measured again using the developer.

[0306] The measurement results were substituted into the following formula to calculate the triboelectric charge retention rate, and the results were evaluated according to the following criteria. The evaluation results are shown in Table 12. Toner triboelectric charge retention rate (%) = [Toner triboelectric charge after one week] / [Initial toner triboelectric charge] x 100 (Evaluation Criteria) A: Triboelectric charge retention rate is 80% or more B: Triboelectric charge retention rate is 60% or more and less than 80% C: Triboelectric charge retention rate is less than 60%

[0307] [Table 12]

Claims

1. a pigment disintegration step of kneading a pigment, a binder, and a grinding agent to obtain a pigment dispersion in which the grinding agent and the disintegrated pigment are dispersed in the binder; and A step of obtaining toner particles using the pigment dispersion by at least one of the following methods (i) to (v): A method for producing a toner comprising the steps of: The binder is a water-insoluble thermoplastic component that is solid at 25° C. the grinding agent is water-insoluble and has a number-average particle size of 0.1 μm to 5.0 μm; The proportion of the binder is 5 to 50% by mass based on the mass of the pigment dispersion, a mass ratio of the pigment to the grinding agent in the pigment dispersion is from 0.2 to 1.5; In the pigment crushing step, kneading is carried out at a temperature at which the melt viscosity of the binder is 6000 Pa sec or less, The method for producing a toner, wherein the toner particles contain the binder and the grinding agent. (i) A method of obtaining toner particles through a step of melt-kneading the pigment dispersion and a resin A, and a step of pulverizing the obtained kneaded product. (ii) A method for obtaining toner particles through a step of preparing a resin solution in which the pigment dispersion and resin A are dissolved in an organic solvent, a step of dispersing the obtained resin solution in an aqueous medium and granulating it to form droplet particles A, and a step of removing the organic solvent contained in the droplet particles A. (iii) A method for obtaining toner particles containing resin A formed by polymerization of the polymerizable monomer, through a step of mixing the pigment dispersion with a polymerizable monomer to prepare a polymerizable monomer composition, a step of dispersing the polymerizable monomer composition in an aqueous medium and granulating it to form droplet particles B, and a step of polymerizing the polymerizable monomer contained in the droplet particles B. (iv) A method of obtaining toner particles through a step of mixing a dispersion liquid containing fine particles of the pigment dispersion with a dispersion liquid containing fine particles containing resin A, aggregating the fine particles to form aggregate particles, and heating the aggregate particles to fuse them. (v) A method for obtaining toner particles through a step of preparing a resin composition containing the pigment dispersion and resin A, a step of preparing a dispersion containing fine particles of the resin composition, aggregating the fine particles to form aggregate particles, and a step of heating and fusing the aggregate particles.

2. 2. The method for producing a toner according to claim 1, wherein the grinding agent is contained in the toner particles in an amount of 20% by mass or less based on the mass of the toner particles.

3. 3. The method for producing a toner according to claim 1, wherein the grinding agent contains any one particle selected from the group consisting of inorganic salt particles, inorganic oxide particles, and mineral particles.

4. The binder contains 20% by mass or more of an amorphous resin, 4. The method for producing a toner according to claim 1, wherein the amorphous resin has a glass transition temperature of 30°C to 80°C and a softening point Tm of 80°C to 200°C.

5. The method for producing a toner according to claim 4 , wherein the binder contains the amorphous resin in an amount of 50% by mass or more.

6. 6. The method for producing a toner according to claim 4, wherein the amorphous resin has a glass transition temperature Tg of 50° C. to 70° C.

7. 7. The method for producing a toner according to claim 4, wherein the softening point Tm of the amorphous resin is 100° C. to 150° C.

8. The difference in SP value between the amorphous resin and the resin A is 3.0 (J / cm 3 ) 0.5 The method for producing a toner according to any one of claims 4 to 7, wherein the toner is:

9. The SP value of the amorphous resin is 21.0 (J / cm 3 ) 0.5 ~24.0 (J / cm 3 ) 0.5 The method for producing a toner according to any one of claims 4 to 8, wherein

10. 10. The method for producing a toner according to claim 4, wherein the amorphous resin is an amorphous polyester.

11. 4. The method for producing a toner according to claim 1, wherein the binder contains 20% by mass or more of a low-molecular-weight crystalline compound having a number-average molecular weight of 250 or more and 1,000 or less.

12. The method for producing a toner according to claim 11, wherein the binder contains the low molecular weight crystalline compound in an amount of 50% by mass or more.

13. 13. The method for producing a toner according to claim 11, wherein the low molecular weight crystalline compound has a melting point of 60° C. to 120° C.

14. 4. The method for producing a toner according to claim 1, wherein the binder contains 20% by mass or more of a crystalline resin having a melting point of 60° C. to 120° C.

15. The method for producing a toner according to any one of claims 1 to 14, wherein the number average particle size of the grinding agent is 0.2 to 1.0 µm.

16. The method for producing a toner according to any one of claims 1 to 15, wherein the grinding agent is calcium carbonate particles.

17. 17. The method for producing a toner according to claim 1, wherein the kneading machine used in the pigment crushing step is a twin-screw kneading extruder.

18. The method for producing a toner according to any one of claims 1 to 17, wherein the step of producing the toner particles is the step (i).

Citation Information

Patent Citations

  • Preparation of beta type copper phtalocyanine pigment

    JP1991084067A

  • Electrostatic charge image developing color toner and its production

    JP1999007159A

  • Cyan pigment, method for manufacturing the same, and color composition for image recording

    JP2009173800A

  • Powder particle thermal treatment apparatus and toner manufacturing method

    JP2013020244A