Isocyanate-based electrolyte additives based on imidazole structural groups and uses thereof

Isocyanate-based electrolyte additives with imidazole structural groups address the degradation issues in lithium-ion batteries by forming a protective film, enhancing high-temperature stability and cycle life.

JP7559254B2Active Publication Date: 2024-10-01VALIANT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023546344
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-03-02
Publication Date
2024-10-01
Estimated Expiration
2042-03-02

AI Technical Summary

Technical Problem

Lithium-ion batteries suffer from performance degradation due to oxidative decomposition of the electrolyte at high temperatures, leading to gas generation and reduced cycle life, which existing isocyanate-based additives fail to adequately address.

Method used

The use of isocyanate-based electrolyte additives containing imidazole structural groups, which interact with the electrolyte and electrode surfaces to form a protective film, reducing decomposition and enhancing stability.

Benefits of technology

The imidazole-containing additives effectively suppress gas generation and extend battery life by improving high-temperature storage characteristics and cycle performance, while maintaining electrolyte stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559254000001
    Figure 0007559254000001
  • Figure 0007559254000002
    Figure 0007559254000002
  • Figure 0007559254000003
    Figure 0007559254000003
Patent Text Reader

Abstract

The present invention relates to an isocyanate-based electrolyte additive based on an imidazole structural group, the structural formula of which is as shown in Formula I, and belongs to the technical field of non-aqueous electrolyte additives for lithium batteries. JPEG2024505954000019.jpg67160, wherein R1, R2, and R3 are the same or different, and R1, R2, and R3 are independently selected from hydrogen, methyl, ethyl, propyl, tert-butyl, trifluoromethyl, trifluoroethyl, pentafluoroethyl, perfluoropropyl, cyanoethyl, phenyl, fluorophenyl, cyano-containing fluorophenyl, alkoxy-containing phenyl, and alkyl-containing phenyl. After being used in a lithium ion battery, the electrolyte additive effectively inhibits the capacity loss of the battery during high-temperature cycles and high-temperature storage, inhibits gas generation caused by electrolyte decomposition, and greatly extends the service life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an isocyanate-based electrolyte additive based on an imidazole structural group and its use, which belongs to the technical field of non-aqueous electrolyte additives for lithium batteries. [Background technology]

[0002] Since their commercialization, lithium secondary batteries have been widely used in the fields of digital, energy storage, power, military aerospace and communication devices due to their high specific energy and excellent cycle performance. Compared with other secondary batteries, lithium secondary batteries have the advantages of high operating voltage, long cycle life, low self-discharge rate, environmental friendliness, no memory effect, etc.

[0003] In lithium-ion batteries, the battery performance is deteriorated due to the oxidative decomposition of the electrolyte, and the elution of metal ions occurs during cycles and high-temperature storage, which leads to a significant decrease in battery performance. With the continuous increase in the demand for lithium-ion batteries from the market, higher requirements are imposed on the overall performance of the battery, and the use of additives is one of the effective ways to improve the overall performance of lithium-ion batteries. There are many types of additives, which can be divided into film-forming additives, overcharge protection additives, conductive additives, flame retardant additives, electrolyte stabilizers, etc. according to the role of the additives in the electrolyte. Although the proportion of each additive in the electrolyte is very small, it has been widely researched and developed due to its remarkable function.

[0004] In recent years, known materials for the positive electrode include LiCoO2, LiMn2O4, LiNiO2, and LiFePO4. When a lithium-ion battery using these materials becomes hot while in a charged state, the non-aqueous solvent in the non-aqueous electrolyte partially decomposes due to oxidation at the interface between the positive electrode material and the non-aqueous electrolyte. The decomposition products and gases generated by this interfere with the original electrochemical reaction of the battery, reducing the performance of the battery, such as its cycle characteristics.

[0005] Patent document WO2010 / 021236 attempts to improve the long-term stability of batteries by using a compound containing an isocyanate group in the molecule, but due to the type of isocyanate compound, the type of additive combined therewith, or the amount of additives used, sufficient durability performance cannot be obtained, and the battery characteristics are still unsatisfactory.

[0006] Patent documents JP2010225522, JP2006164759 and CN10153329 disclose that adding an isocyanate compound to a non-aqueous electrolyte can improve the cycle characteristics of a battery and improve battery stability. However, the materials or electrolyte compositions described in these patents cannot solve the problems of high temperature stability of the battery and the tendency of discoloration and acidity increase when used in combination with other sulfonate additives. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the shortcomings of the prior art, the present invention provides an isocyanate-based electrolyte additive based on an imidazole structural group and its use, which, after being used in a lithium ion battery, can effectively inhibit the capacity loss of the battery during high temperature cycling and high temperature storage, inhibit the gas generation caused by the decomposition of the electrolyte, and greatly extend the service life of the battery. [Means for solving the problem]

[0008] An isocyanate-based electrolyte additive based on an imidazole structural group is disclosed, the structural formula of which is as shown in Formula I.

[0009] JPEG0007559254000001.jpg67160

[0010] In the formula, R1, R2, and R3 are the same or different, and R1, R2, and R3 are each independently selected from hydrogen, a methyl group, an ethyl group, a propyl group, a tert-butyl group, a trifluoromethyl group, a trifluoroethyl group, a pentafluoroethyl group, a perfluoropropyl group, a cyanoethyl group, a phenyl group, a fluorophenyl group, a cyano group-containing fluorophenyl group, an alkoxy group-containing phenyl group, and an alkyl group-containing phenyl group.

[0011] Furthermore, the electrolyte additive is any one or a mixture of two or more of the following structural formulas:

[0012] JPEG0007559254000002.jpg217170JPEG0007559254000003.jpg255153

[0013] The present invention further discloses a method for preparing the isocyanate-based electrolyte additive based on the imidazole structural group, the method comprising the steps of: The method includes a step of uniformly dispersing raw materials 1 and 2 in a solvent under the protection of an inert gas, controlling the reaction temperature to 10° C. to 120° C., and reacting for 1 to 48 hours to obtain an isocyanate-based additive reaction liquid containing an imidazole structural group; The solvent is one or a mixture of two or more selected from ether, THF, cyclopentyl methyl ether, acetonitrile, and ethyl acetate, or no solvent is used; Regarding the amount of the solvent used, the ratio of the mass amount of the raw material 1 to the mass amount of the solvent used is 1.0:1.0 to 10.0; The molar ratio of the amount of the raw material 1 to the amount of the raw material 2 is raw material 1:raw material 2=1.0:1.0 to 10.0, JPEG0007559254000004.jpg52168 wherein R1, R2 and R3 are the same or different, and R1, R2 and R3 are each independently selected from hydrogen, a methyl group, an ethyl group, a propyl group, a tert-butyl group, a trifluoromethyl group, a trifluoroethyl group, a pentafluoroethyl group, a perfluoropropyl group, a cyanoethyl group, a phenyl group, a fluorophenyl group, a cyano group-containing fluorophenyl group, an alkoxy group-containing phenyl group and an alkyl group-containing phenyl group; In the formula, M is one selected from Li, Na, K, and Ca.

[0014] In the imidazole structural group-based isocyanate additive and its preparation method, the raw materials are inexpensive and easily available, the reaction conditions are mild, the operation is simple and safe, environmentally friendly and effective.

[0015] The present invention further discloses the use of the isocyanate-based electrolyte additive based on the imidazole structural group, which is used in a lithium ion battery including a negative electrode, a positive electrode, a separator disposed between the negative electrode and the positive electrode, and an electrolyte, wherein the negative electrode is a single material selected from the group consisting of a carbon-based active material, a silicon-based active material, a metal-based active material, or a lithium-containing nitride, or a mixture of two or more of them.

[0016] By preparing a non-aqueous electrolyte solution for lithium ion batteries using the isocyanate-based electrolyte additive containing an imidazole structural group described in the present invention and using the non-aqueous electrolyte solution in a lithium ion battery, it is possible to effectively improve high-temperature storage characteristics and effectively suppress gas generation during high-temperature storage.

[0017] Further, the electrolyte solution includes a solvent, an electrolyte lithium salt, and an isocyanate-based electrolyte additive based on the imidazole structural group.

[0018] Furthermore, the mass content of the isocyanate-based electrolyte additive based on the imidazole structural group is 0.01 to 5%, and preferably 0.1 to 2%, based on the total mass of the electrolyte.

[0019] Furthermore, the electrolyte lithium salt is at least one selected from LiPF6, LiClO4, LiBF4, LiBOB, LiODFB, LiTDI, LiTFSI and LiFSI, and is preferably LiPF6, and the content of the electrolyte lithium salt is 10 to 20 wt% of the total mass of the electrolyte.

[0020] Furthermore, the solvent includes one or a mixture of two or more selected from the group consisting of ester-based solvents and amide-based solvents, and the ester-based solvent is at least one compound selected from the group consisting of cyclic carbonate ester compounds, linear carbonate ester compounds, linear ester compounds, and cyclic ester compounds.

[0021] Furthermore, the solvent is one or a combination of a plurality of solvents selected from ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, dimethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl propargyl carbonate, 1,4-butanolide, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate, and ethyl butyrate. Effect of the Invention

[0022] (1) The present invention provides an isocyanate-based electrolyte additive based on an imidazole structural group, and a method for synthesizing such a compound, in which the raw materials are inexpensive and easily available, the reaction conditions of the process are mild, the operation is simple and safe, environmentally friendly, and effective.

[0023] (2) In the isocyanate-based electrolyte additive based on the imidazole structural group provided by the present invention, the isocyanate group has strong electrophilicity and can react with the moisture in the electrolyte system and the active hydrogen contained in the positive and negative electrodes, thereby reducing the decomposition of LiPF6 caused by active hydrogen.

[0024] (3) In the isocyanate-based electrolyte additive based on the imidazole structural group provided by the present invention, the imidazole structure contained contains a nitrogen atom having a lone pair of electrons and imparts weak alkalinity to the electrolyte, thereby removing HF caused by the decomposition of LiPF6 (particularly in an electrolyte system containing ethylene sulfate (DTD) or methylenemethane disulfonate (MMDS), which is likely to lead to an increase in the acidity and color of the electrolyte), and further effectively suppressing the increase in acidity of the electrolyte, as well as suppressing the increase in color caused by the reaction of PF5 with trace impurities in the electrolyte.

[0025] (4) In the isocyanate-based electrolyte additive based on the imidazole structural group provided by the present invention, the sulfonyl group has good film-forming performance, and after being added to the electrolyte, it can react with the electrode surface to form a film, and can introduce S element into the SEI film and increase the ionic conductivity, thereby effectively improving the cycle performance of lithium-ion batteries.

[0026] (5) The isocyanate-based electrolyte additive based on the imidazole structural group provided by the present invention has high compatibility with the graphite negative electrode by organically bonding a sulfonyl group, a nitrogen-containing heterocyclic imidazole, and an isocyanate structural group. At the same time, the isocyanate group removes water, the imidazole group removes HF, and the sulfonyl group has good film-forming performance, which prevents the decomposition and fragmentation of the SEI caused by hydrogen fluoride decomposed from LiPF6, improves high-temperature cycle and high-temperature storage performance, and effectively suppresses gas generation due to electrolyte decomposition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In order to make the above objects, features and advantages of the present invention clearer and more understandable, the following describes in detail the specific embodiments of the present invention. In the following description, many specific details are set forth in order to fully understand the present invention. However, the present invention can be implemented in many other ways different from the way described herein, and those skilled in the art can make similar improvements without departing from the spirit of the present invention, so the present invention is not limited to the specific embodiments disclosed below.

[0028] Unless otherwise defined, all technical and scientific terms used in this document have the same meaning as commonly understood by those skilled in the art. In this document, the terms used in the specification of the present invention are only for describing specific embodiments and are not intended to limit the present invention.

[0029] This example provides a method for producing some of the compounds ZN01 to ZN27.

[0030] Synthesis embodiment 1 Preparation of compound ZN-01 JPEG0007559254000005.jpg40170

[0031] 33.6g (0.15mol) of KTDI, 42.4g (0.30mol) of sulfonyl chloride isocyanate and 150g of anhydrous acetonitrile were added to a 500mL three-neck flask, and the temperature was gradually raised to 75-80°C and the reaction was stirred for 26.0hrs. The temperature was lowered, filtered, and the filtrate was subjected to solvent removal under reduced pressure until no distillate remained to obtain a yellow-brown viscous material, which was purified by column chromatography using heptane + dichloromethane to obtain 24.0g of white solid ZN-01, with a yield of 55.00%.

[0032] GC-MS: 291, 13 C NMR (100 MHz): solvent deuterated chloroform, δ (ppm): 115.7 ppm (s, -CN), 119.8 (q, -CF3), 121.6 (q, C=C), 122.4 (s, N=C=O) 147.8 (q, C-CF3).

[0033] Synthesis embodiment 2 Preparation of compound ZN-12 JPEG0007559254000006.jpg61170

[0034] 32.2g (0.10mol) of pentafluorophenylimidazole potassium salt, 31.1g (0.22mol) of sulfonyl chloride isocyanate and 150g of anhydrous acetonitrile were added to a 500mL three-neck flask, and the temperature was gradually raised to 75-80°C and the reaction was stirred for 36.0hrs. The temperature was lowered, filtered, and the filtrate was subjected to solvent removal under reduced pressure until no distillate remained to obtain a yellow-brown viscous material, which was purified by column chromatography using heptane + dichloromethane to obtain 16.4g of white solid ZN-12, with a yield of 42.10%.

[0035] GC-MS: 389, 13 C NMR (100 MHz): solvent deuterated chloroform, δ (ppm): 113.4 (m, CC5F5), 116.1 ppm (s, -CN), 122.3 (q, C=C), 122.6 (s, N=C=O), 137.8 (dm), 140.4 (dm), 144.2 (dm), 146.7 (q, C-PhF5).

[0036] Synthesis embodiment 3 Preparation of compound ZN-19 JPEG0007559254000007.jpg31170

[0037] Add 13.6g (0.2mol) of imidazole, 10g (0.25mol, 60% content) of sodium hydride and 100g of anhydrous cyclopentyl methyl ether to a 500mL three-neck flask, stir for 1.0hr, gradually add 46.7g (0.33mol) of sulfonyl chloride isocyanate, gradually raise the temperature to 100-105℃, stir and react for 22.0hr, lower the temperature, filter, remove the solvent from the filtrate under reduced pressure until no distillate remains, and further distill under reduced pressure to obtain 16.2g of colorless viscous oil ZN-19, with a yield of 46.82%.

[0038] GC-MS: 173, 1 H NMR (400 MHz): solvent deuterated chloroform, δ (ppm): 7.155-7.173 ppm (d, 1H), 7.313-7.331 ppm (d, 1H), 7.912 ppm (s, 1H); 13 C NMR (100 MHz): solvent deuterated chloroform, δ (ppm): 121.8 (s, N=C=O), 125.4, 134.5 (s, NCH=CHN), 136.8 ppm (s, NCHN).

[0039] Battery Example The blend compositions of the nonaqueous electrolyte solutions for lithium ion batteries listed in Battery Examples 1 to 9 and Comparative Examples 1 to 6 are as shown in Table 1.

[0040] Table 1. Compositions of non-aqueous electrolytes for lithium ion batteries in battery examples 1 to 9 and comparative examples 1 to 6 JPEG0007559254000008.jpg214170JPEG0007559254000009.jpg83170

[0041] For the stability test of the electrolyte, the electrolyte for lithium ion batteries prepared in the above Examples 1 to 9 and Comparative Examples 1 to 6 were put into sealed aluminum bottles, and the aluminum bottles were vacuum-packed with aluminum plastic film. The electrolyte samples were simultaneously stored in a thermostatic box set at 45°C. Samples were taken in a glove box before and after 60 days of storage to measure the acidity and color value of the electrolyte. The acidity was tested with a potentiometric titrator, and the acidity value was converted to HF and expressed in ppm. The color value was measured using the platinum-cobalt colorimetric method and expressed in Hazen. Some test results are shown in Table 2.

[0042] Table 2. Effect of additives on the acidity and color of electrolyte JPEG0007559254000010.jpg205170

[0043] As can be seen from Table 2, after storing the electrolytes of Examples 1 to 6 at a high temperature of 45°C for 60 days, the acidity and color of the electrolytes are both lower than those of the comparative example. By adding propanedisulfonic anhydride and 1,8-octyldiisocyanate to the electrolyte system of Comparative Example 5, the change in acidity and color is suppressed, but the effect is far lower than that of the material provided by the present invention patent.

[0044] The electrolyte additive provided by the present invention has a more pronounced effect of inhibiting discoloration and an increase in acidity value in electrolyte systems containing ethylene sulfate or methylenemethane disulfonate, and the novel additive provided by the present invention can effectively inhibit the acidity and color increase of the electrolyte and improve the stability of the electrolyte under high temperature conditions.

[0045] The method for producing lithium ion button batteries using the nonaqueous electrolyte solutions for lithium ion batteries in Battery Examples 1 to 9 and Comparative Examples 1 to 6 is as follows.

[0046] (1) Manufacturing of positive electrodes For example, the positive electrode material LiCoO2 is 0.8 Co 0.1 Mn 0.1 O2 powder, carbon black (particle size 1000 nm), polyvinylidene fluoride (PVDF) and N,N-methylpyrrolidone (NMP) were mixed to form a uniform slurry, which was then uniformly applied to an aluminum foil (15 μm) current collector, dried, rolled, and coated with LiNi 0.8 Co 0.1 Mn 0.1 O2 positive electrode material was obtained. It was dried at 120°C for 12 hours, and the LiNi 0.8 Co 0.1 Mn 0.1 O2 accounts for 94% of the total coating, adhesive accounts for 4%, and carbon black accounts for 2%. The resulting plate was then cut into a circle with a diameter of 8 mm to form the positive electrode. The other positive electrode material LiFePO4 was produced in the same manner.

[0047] (2) Manufacturing of negative electrodes For example, artificial graphite anode material was prepared by mixing artificial graphite, polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) to form a uniform slurry, which was then uniformly applied to a copper foil (15μm) current collector, dried and rolled to obtain a carbon anode material. After drying at 120℃ for 12 hours, the graphite accounted for 96.4% of the total coating and the adhesive accounted for 3.6% of the dried plate. The resulting plate was then cut into a circle with a diameter of 8mm to form the anode.

[0048] (3) Electrolyte production In an argon atmosphere glove box with a water content of <1 ppm, the lithium salt was dissolved in the solvent, and then the novel phosphine-containing isocyanate system was added and mixed uniformly to obtain the electrolyte solution.

[0049] (4) Manufacture of lithium-ion batteries The materials described in steps (1) and (2) above were used as the working electrodes, and Celgard 2400 membrane (Tianjin) was used as the separator to assemble a CR2430 button battery. The assembly order was from negative to positive, and consisted of the negative electrode case, spring plate, gasket, negative electrode plate, electrolyte, separator, positive electrode plate, and positive electrode case, and then sealed with a sealing machine. All of these operations were completed in a glove box with a pure argon atmosphere, and after leaving it to stand for 6 h, it was taken out and subjected to an electrochemical reaction performance test.

[0050] Lithium-ion battery performance testing Test 1: High temperature cycle performance test The following tests were carried out on the manufactured batteries.

[0051] (1) At 45℃, the battery is charged at 0.1C constant current to 4.3V, then discharged at the corresponding constant current to 2.7V, which is the first cycle. (2) After the first cycle is completed, the battery is charged at a constant current of 1.0C to 4.3V, and then discharged at a constant current of the corresponding rate to 2.7V, and cycle tests are performed 100 times and 500 times according to the cycle conditions, and the capacity retention rate of the battery after 100 times and 500 times is calculated, and the capacity retention rate after cycling is calculated by the following formula. The related test data of each battery obtained is as shown in Table 2, among which the battery numbers of Examples 1 to 9 are Battery 1 to Battery 9, respectively, and the battery numbers of Comparative Examples 1 to 6 are Battery 1# to Battery 6#, respectively. Capacity retention rate after cycling = (discharge capacity after corresponding number of cycles / discharge capacity of first cycle) x 100%

[0052] Table 3. Battery cycle performance test results at 45°C JPEG0007559254000011.jpg204170

[0053] As can be seen from the data of different batteries in Table 3, in different positive electrode material systems, the lithium batteries prepared using the additives provided by the present invention have much higher cycle stability and capacity retention at 45°C than batteries 1# and 2# without additives.

[0054] For batteries 4# and 5# containing ethylene sulfate or methylenemethane disulfonate, the battery performance deteriorates after high temperature cycling due to the low thermal stability of such materials.

[0055] The data shows that for batteries 5# and 6#, by adding sulfonic acid anhydride + isocyanate-based material as a stabilizer, the capacity retention rate is improved after 100 cycles, but the capacity retention rate after 500 cycles is much lower than that of the battery containing the additive provided by the present invention. This shows that the novel additive provided by the present invention can obviously improve the high temperature cycle performance of the battery after being used in lithium ion batteries, and the electrolyte additive provided by the present invention can also show good effect in electrolyte systems containing ethylene sulfate or methylenemethane disulfonate, which have low thermal stability.

[0056] Test 2: After 100 cycles were performed on the batteries produced in Examples 1 to 9 and Comparative Examples 1 to 6, a thermal stability test after the cycles was performed.

[0057] Under the condition of 25℃, the battery was charged at a constant current of 0.5C up to 4.3V, then charged at a constant voltage of 4.3V until the current reached 0.025C, and then fully charged to 4.3V. The battery was then stored in a high-temperature oven at 50℃ for 15 days, and the voltage drop of the battery in the high-temperature oven and the volume change of the battery after the test were tested. The test data are shown in Table 4.

[0058] Among them, the voltage drop change rate (%) of the lithium-ion battery after high-temperature storage = (the voltage of the lithium-ion battery before high-temperature storage - the voltage of the lithium-ion battery after high-temperature storage) / the voltage of the lithium-ion battery before high-temperature storage × 100%, Volume change rate (%) of lithium-ion battery after high-temperature storage = (volume of lithium-ion battery after high-temperature storage - volume of lithium-ion battery before high-temperature storage) / volume of lithium-ion battery before high-temperature storage x 100%.

[0059] Table 4 JPEG0007559254000012.jpg196170

[0060] As can be seen from Table 4, compared with the state shown by batteries 1#~6# which underwent thermal stability testing after 100 cycles, the voltage drop change rates of batteries 1~9 containing the novel additive provided by the present invention patent which underwent thermal stability testing at high temperature after 100 cycles were only 9.18~12.42%, which is much lower than the voltage drop change rates of batteries 1#~6#.

[0061] At the same time, there is a large difference in the volume change rate, and the volume expansion of batteries 1#~6# is significant. By adding sulfonic anhydride + isocyanate-based material as a stabilizer to batteries 5~6#, the volume change is improved, but the effect is much lower than that of the battery containing the additive provided by the present invention. As can be seen, the novel imidazole phosphine-containing isocyanate-based electrolyte additive prepared by the present invention can greatly improve the thermal stability of lithium ion batteries after multiple cycles after being used in lithium ion batteries, and can inhibit gas generation caused by the decomposition of electrolyte, and has good prospects for use.

[0062] The technical features of the embodiments described above can be combined in any manner. For the sake of simplicity, not all possible combinations of the technical features in the embodiments described above have been described. However, as long as there are no contradictions in the combinations of these technical features, they should be considered within the scope of the present specification.

[0063] The above-described examples specifically and in detail describe some embodiments of the present invention, but this should not be understood as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the spirit of the present invention, which also belong to the protection scope of the present invention. Therefore, the protection scope of the invention patent is governed by the appended claims.

Claims

1. An isocyanate-based electrolyte additive based on an imidazole structural group, characterized in that it is any one or a mixture of two or more of the following structural formulas:

2. A method for producing an isocyanate-based electrolyte additive based on the imidazole structural group according to claim 1, comprising: The method includes the steps of: uniformly dispersing raw materials 1 and 2 in a solvent under the protection of an inert gas; controlling the reaction temperature to 10° C. to 120° C.; and reacting for 1 to 48 hours to obtain an isocyanate-based additive reaction liquid containing an imidazole structural group; The solvent is one or a mixture of two or more selected from ether, THF, cyclopentyl methyl ether, acetonitrile, and ethyl acetate, or no solvent is used; Regarding the amount of the solvent used, the ratio of the mass amount of the raw material 1 to the mass amount of the solvent used is 1.0:1.0 to 10.0; The molar ratio of the amount of the raw material 1 to the amount of the raw material 2 is raw material 1: raw material 2=1.0:1.0 to 10.0, The raw material 1 is A method for producing an isocyanate-based electrolyte additive based on an imidazole structural group, the additive being any one selected from the following:

3. The use of the isocyanate-based electrolyte additive based on an imidazole structural group according to claim 1, characterized in that the imidazole-based isocyanate-based electrolyte additive is used in a lithium ion battery comprising a negative electrode, a positive electrode, a separator disposed between the negative electrode and the positive electrode, and an electrolyte.

4. The use of the isocyanate-based electrolyte additive based on imidazole structural group according to claim 3, characterized in that the electrolyte comprises a solvent, an electrolyte lithium salt and the isocyanate-based electrolyte additive based on imidazole structural group.

5. The use of the isocyanate-based electrolyte additive based on imidazole structural group according to claim 4, characterized in that, in the total mass of the electrolyte, the mass content of the isocyanate-based electrolyte additive based on imidazole structural group is 0.01-5%.

6. The electrolyte lithium salt is LiPF 6 , LiClO 4 , LiBF 4 5. The use of the isocyanate-based electrolyte additive based on imidazole structural group according to claim 4, characterized in that the electrolyte lithium salt is one or more selected from the group consisting of LiBOB, LiODFB, LiTDI, LiTFSI and LiFSI, and the content of the electrolyte lithium salt is 10-20 wt% in the total mass of the electrolyte.

7. The use of the isocyanate-based electrolyte additive based on the imidazole structural group according to claim 4, characterized in that the solvent is selected from ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, dimethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl propargyl carbonate, 1,4-butanolide, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate or ethyl butyrate.

Citation Information

Patent Citations

  • Anti-overcharge electrolyte and lithium ion battery using same

    CN111244545A

  • Nonaqueous electrolyte secondary battery

    JP1997139233A

  • Lithium secondary battery, electrolyte for lithium secondary battery, power tool, electric vehicle, and power storage system

    JP2011198508A

  • Salts used in electrolyte compositions or as electrode additives

    JP2020515558A

  • Nonaqueous electrolyte solution and nonaqueous electrolyte battery using same

    WO2014157591A1