Toner for developing electrostatic images
A toner with a crystalline polyester resin and specific wax ratios addresses tacking and heat-resistant storage issues, ensuring effective low-temperature fixability and rapid crystallization during high-speed printing.
Patent Information
- Application Number
- JP2020131327
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-03
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-08-03
AI Technical Summary
Existing toners with improved low-temperature fixability suffer from tacking issues during high-speed continuous printing, and lack sufficient heat-resistant storage properties.
A toner formulation containing a crystalline polyester resin with specific ΔHc(Hi)/ΔHc and ΔH2/ΔH1 ratios, combined with a fatty acid ester wax and a linear hydrocarbon wax, promotes rapid crystallization and suppresses tacking while maintaining low-temperature fixability.
The toner effectively suppresses tacking and maintains excellent heat-resistant storage properties during high-speed continuous printing by ensuring rapid crystallization of the crystalline polyester resin.
Smart Images

Figure 0007559408000006 
Figure 0007559408000007 
Figure 0007559408000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing electrostatic images, and more particularly to a toner for developing electrostatic images which is excellent in low-temperature fixing property, suppresses tacking, and has excellent heat-resistant storage property. [Background technology]
[0002] In recent years, electrophotographic image forming apparatuses have been required to have a toner for developing electrostatic images that can be thermally fixed at low temperatures. To this end, a toner has been proposed that has improved low-temperature fixability by adding a crystalline substance or a wax with a high plasticizing effect as a fixing aid and lowering the melting temperature and melt viscosity of the binder resin (see, for example, Patent Document 1). Toners containing such fixing aids have good low-temperature fixing properties, but the toner itself and the fixed image are vulnerable to thermal stress. In particular, when images with a large amount of toner adhesion are continuously printed, the images are piled up while retaining latent heat, and there is a problem that the latent heat and pressure due to the weight of the paper cause the image area to adhere to the paper or image area to image area (hereinafter referred to as "tacking").
[0003] Patent Document 2 proposes a toner containing a crystalline polyester resin, in which the peak top temperature and half width of the heat generation peak during temperature drop measured by differential scanning calorimetry of the toner are within a certain range. In this technology, the crystallization temperature of the toner is increased to a certain extent, but the crystallized ratio to the total added amount of crystalline substances (specifically, crystalline polyester resin and release agent) in the toner is not taken into consideration. Even if the crystallization temperature of the toner is high, if the crystallized ratio to the total added amount of crystalline substances is low, the resin layer does not solidify sufficiently, and tacking occurs. Under conditions where tacking is likely to occur, such as high-speed continuous printing, the effect becomes more pronounced, and there is room for improvement. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-45850 A [Patent Document 2] JP 2018-87901 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide a toner for developing electrostatic images which maintains good low-temperature fixing properties, suppresses tacking, and has excellent heat-resistant storage properties, even when images are printed continuously at high speed. [Means for solving the problem]
[0006] In the course of investigating the causes of the above problems in order to solve the above problems, the present inventors discovered that in a toner using a crystalline polyester resin, the larger the ΔHc(Hi) and ΔH2 / ΔH1 values in DSC measurement of the toner, the more quickly the crystalline polyester resin in the image can be crystallized at high temperatures, and tacking can be suppressed while maintaining low-temperature fixing properties, thus arriving at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0007] 1. A toner for developing electrostatic images, comprising at least a binder resin and a release agent, The binder resin is at least a crystalline polyester resin. and amorphous vinyl resin Contains the crystalline polyester resin has a portion having a crystalline structure and a crystallization-promoting portion, The content of the amorphous vinyl resin in the binder resin is 40% by mass or more relative to the binder resin, and The release agent contains at least a fatty acid ester wax and a linear hydrocarbon wax, The heat generation amount of the exothermic peak during cooling of the electrostatic image developing toner measured by differential scanning calorimetry is defined as ΔHc (J / g), and the heat generation amount from the crystallization onset temperature to 68° C. at the exothermic peak is defined as ΔHc(Hi) (J / g), A toner for developing electrostatic images, characterized in that the following formulas (1) and (2) are satisfied, where ΔH1 (J / g) is the endothermic peak attributable to a crystalline substance during the first temperature rise measured by differential scanning calorimetry, and ΔH2 (J / g) is the endothermic peak during the second temperature rise. Equation (1): ΔHc(Hi) / ΔHc≧0.60 Equation (2): 0.65≦ΔH2 / ΔH1≦0.95 (In the differential scanning calorimetry, during the first and second heating, the temperature is raised from 0°C to 150°C at a heating rate of 10°C / min and held at 150°C for 1 minute, and during cooling, the temperature is lowered from 150°C to 0°C at a cooling rate of 10°C / min and held at 0°C for 1 minute.)
[0008] 2. The toner for developing electrostatic images according to item 1, wherein the softening point of the toner for developing electrostatic images is within the range of 90 to 105°C.
[0010] 3 The mass ratio of the fatty acid ester wax to the linear hydrocarbon wax is 1:9 to 9:1. Paragraph 1 or 2 2. The toner for developing electrostatic images according to claim 1 .
[0011] 4 The linear hydrocarbon wax contains a linear hydrocarbon wax having a crystallization temperature of 75° C. or higher. 1 term from No. 3 term Any one of the items up to 2. The toner for developing electrostatic images according to claim 1 .
[0012] 5 The linear hydrocarbon wax contains Fischer-Tropsch wax. 1 From item to item 4 Item 1. The toner for developing an electrostatic image according to any one of items 1 to 9.
[0013] 6 The crystalline polyester resin according to any one of claims 1 to 5, characterized in that the crystalline polyester resin has a portion having a crystalline structure and a crystallization promoting portion, and the crystallization promoting portion is a portion derived from a compound selected from the group consisting of an aliphatic monocarboxylic acid having 10 to 30 carbon atoms or an aliphatic monoalcohol having 10 to 30 carbon atoms. 5Item 1. The toner for developing an electrostatic image according to any one of items 1 to 9.
[0014] 7 The crystalline polyester resin is characterized in that the portion having the crystalline structure of the crystalline polyester resin contains a hybrid crystalline polyester resin formed by chemically bonding a crystalline polyester polymer segment and a vinyl resin polymer segment. 6 2. The toner for developing electrostatic images according to claim 1.
[0015] 8 The content of the amorphous vinyl resin in the binder resin is 50% by mass or more. 7 Item 1. The toner for developing an electrostatic image according to any one of items 1 to 9. Effect of the Invention
[0016] According to the above-mentioned means of the present invention, it is possible to provide a toner for developing electrostatic images which maintains good low-temperature fixing properties even when images are printed continuously at high speed, suppresses tacking, and has excellent heat-resistant storage properties. Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows. Tacking occurs when the crystalline substance in the toner image does not completely crystallize before images having latent heat after fixing are piled up, causing the viscosity of the resin layer to decrease, resulting in images adhering to each other. Therefore, when the crystallization temperature of the toner is higher than the temperature of the laminated images immediately after fixing and the toner crystallizes at a high rate relative to the total amount of the crystalline substance added, tacking can be suppressed. In the present invention, ΔHc(Hi) / ΔHc means the ratio of the amount of crystals crystallized at a high temperature to the total amount of crystals crystallized after fixing, and when ΔHc(Hi) / ΔHc is 0.60 or more, excellent tack resistance can be exhibited. On the other hand, ΔH2 / ΔH1 is the ratio of the heat of fusion ΔH2 of the crystalline material recrystallized after melting the toner to the heat of fusion ΔH1 of the crystalline material in a fully crystallized state in the toner. In other words, ΔH2 / ΔH1 corresponds to the ratio of the amount of crystals recrystallized after fixing to the amount of crystals in the toner, and is an index of the ease of crystallization after melting the toner. When ΔH2 / ΔH1 is 0.65 or more, the ratio of the amount of crystals recrystallized after fixing to the amount of crystals in the toner is sufficiently high, and excellent tackiness can be achieved. On the other hand, when ΔH2 / ΔH1 is 0.95 or less, the compatibility between the crystalline material and the binder resin during fixing is ensured, and therefore excellent low-temperature fixing property can be achieved. From the above, when ΔHc(Hi) and ΔH2 / ΔH1 satisfy the above-mentioned specific ranges, a toner having excellent heat-resistant storage stability and suppressing tacking can be obtained while maintaining good low-temperature fixability. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a diagram for explaining a method for calculating ΔHc and ΔHc(Hi) of exothermic peaks in the present invention. [Diagram 2] FIG. 1 is a diagram for explaining a method for calculating ΔHc and ΔHc(Hi) of exothermic peaks in the present invention. [Diagram 3] FIG. 1 is a diagram for explaining a method for calculating ΔH1 and ΔH2 in the present invention. [Figure 4] FIG. 1 is a diagram for explaining a method for calculating ΔH1 and ΔH2 in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The toner for developing electrostatic images of the present invention is a toner for developing electrostatic images containing at least a binder resin and a release agent, the binder resin containing at least a crystalline polyester resin, and is characterized in that, when the heat generation amount of the exothermic peak during cooling measured by differential scanning calorimetry of the toner for developing electrostatic images is ΔHc (J / g), the heat generation amount from the crystallization onset temperature to 68° C. at the exothermic peak is ΔHc(Hi) (J / g), the endothermic amount of the endothermic peak derived from a crystalline substance during a first heating measured by differential scanning calorimetry is ΔH1 (J / g), and the endothermic amount of the endothermic peak during a second heating measured by differential scanning calorimetry is ΔH2 (J / g), the following formulas (1) and (2) are satisfied. Equation (1): ΔHc(Hi) / ΔHc≧0.60 Equation (2): 0.65≦ΔH2 / ΔH1≦0.95 This feature is a technical feature common to or corresponding to each of the following embodiments.
[0019] In an embodiment of the present invention, the softening point of the toner for developing electrostatic images is preferably within a range of 90 to 105° C. When the softening point of the toner is 90° C. or higher, good heat-resistant storage stability is obtained. When the softening point is 105° C. or lower, good low-temperature fixability is obtained.
[0020] It is also preferred that the release agent contains at least a fatty acid ester wax and a linear hydrocarbon wax. The fatty acid ester wax and the linear hydrocarbon wax function as a crystal nucleating agent for the crystalline polyester resin, and can promote the crystallization of the crystalline polyester resin even in the presence of a binder resin. The fatty acid ester wax is easily compatible with the binder resin when molten, and plasticizes the binder resin, thereby obtaining good low-temperature fixability. On the other hand, the linear hydrocarbon wax has a higher crystallization temperature than the fatty acid ester wax, and can crystallize the crystalline polyester in the toner at a high temperature, thereby suppressing tacking. Therefore, by containing the fatty acid ester wax and the linear hydrocarbon wax, excellent low-temperature fixability and a tacking suppression effect can be obtained.
[0021] The content mass ratio of the fatty acid ester wax to the linear hydrocarbon wax is preferably 1:9 to 9:1. When the ratio of the fatty acid ester wax is 10% or more of the total of the fatty acid ester wax and the linear hydrocarbon wax, the plasticizing effect of the binder resin is exerted, and good fixability is obtained. When the ratio of the linear hydrocarbon wax is 10% or more of the total of the fatty acid ester wax and the linear hydrocarbon wax, the crystallization of the crystallized polyester can be promoted, and the crystallization temperature of the entire toner can be increased, so that tacking can be reliably suppressed.
[0022] The linear hydrocarbon wax preferably contains a linear hydrocarbon wax having a crystallization temperature of 75° C. or higher. When the crystallization temperature is 75° C. or higher, the release agent and the crystalline polyester resin in the toner can be crystallized at a sufficiently high temperature, and a more excellent tacking suppression effect can be obtained. Therefore, from the viewpoint of suppressing tacking, the crystallization temperature is more preferably 80° C. or higher, and even more preferably 85° C. or higher.
[0023] The linear hydrocarbon wax preferably contains a Fischer-Tropsch wax. Among linear hydrocarbon waxes, the Fischer-Tropsch wax is highly effective as a crystal nucleating agent for crystalline polyester resins and fatty acid esters, and has a high crystallization temperature within a range that does not impair fixability. Therefore, by containing the Fischer-Tropsch wax, further excellent tack resistance can be obtained.
[0024] The crystalline polyester resin preferably has a portion having a crystalline structure and a crystallization promoting portion, and the crystallization promoting portion is a portion derived from a compound selected from the group consisting of an aliphatic monocarboxylic acid having 10 to 30 carbon atoms or an aliphatic monoalcohol having 10 to 30 carbon atoms. When the portion having a crystalline structure is contained, it is preferable because it can impart sharp melting properties that quickly plasticize the binder resin at a desired temperature. When the crystallization promoting portion is contained, the portion having a crystalline structure is easily crystallized because it is incompatible with the binder resin starting from the crystallization promoting portion. Furthermore, the crystallization promoting portion and the release agent have lower polarity than the binder resin and are easily interacted with each other, so that the release agent is easily able to function as a crystal nucleating agent. Therefore, the crystallization of the crystalline polyester resin is further promoted, and an excellent tack suppression effect is obtained. When the number of carbon atoms of the crystallization promoting portion is 10 or more, it is easily incompatible with the binder resin and promotes crystallization, which is preferable from the viewpoint of tack suppression and heat-resistant storage stability. From the viewpoint of fixing property, it is preferable that the carbon number is 30 or less because the crystallization promoting portion does not inhibit the plasticizing effect of the crystalline polyester. From the viewpoint of tacking suppression, low-temperature fixing property, and heat-resistant storage property, it is more preferable that the carbon number is within the range of 15 to 25.
[0025] It is preferable that the portion of the crystalline polyester resin having the crystalline structure contains a hybrid crystalline polyester resin formed by chemically bonding a crystalline polyester polymer segment and a vinyl resin polymer segment. By having the crystalline polyester resin have a segment of vinyl resin, which is the main component of the binder resin, the crystalline polyester resin is partially compatible with the binder resin and finely dispersed in the toner, thereby obtaining excellent low-temperature fixability.
[0026] The content of the amorphous vinyl resin in the binder resin is preferably 50% by mass or more. The amorphous polyester resin, which is often used in general, is structurally similar to the crystalline polyester resin, and therefore is easily compatible with the crystalline polyester resin. Therefore, when the content of the amorphous polyester resin is 50% by mass or more, the amorphous polyester resin is compatible with the crystalline polyester resin, and the crystallization of the crystalline polyester resin is suppressed. On the other hand, since the vinyl resin has a structure different from that of the crystalline polyester resin, an excellent tacking suppression effect can be obtained without suppressing the crystallization of the crystalline polyester resin. From the viewpoint of suppressing tacking, the content of the amorphous vinyl resin is more preferably 60% by mass or more, and even more preferably 70% by mass or more.
[0027] The present invention, its components, and embodiments for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as lower and upper limits.
[0028] [Outline of the toner for developing electrostatic images of the present invention] The toner for developing electrostatic images of the present invention (hereinafter, also simply referred to as "toner") is a toner for developing electrostatic images containing at least a binder resin and a release agent, the binder resin containing at least a crystalline polyester resin, and is characterized in that, when the heat generation amount of the exothermic peak during cooling measured by differential scanning calorimetry of the toner for developing electrostatic images is ΔHc (J / g), the heat generation amount from the crystallization onset temperature to 68°C at the exothermic peak is ΔHc(Hi) (J / g), the endothermic amount of the endothermic peak derived from a crystalline substance during a first heating measured by differential scanning calorimetry is ΔH1 (J / g), and the endothermic amount of the endothermic peak during a second heating measured by differential scanning calorimetry is ΔH2 (J / g), the following formulas (1) and (2) are satisfied. Equation (1): ΔHc(Hi) / ΔHc≧0.60 Equation (2): 0.65≦ΔH2 / ΔH1≦0.95
[0029] [Differential scanning calorimetry measurement method] Differential scanning calorimetry (DSC measurement) was performed using a differential scanning calorimeter "DSC7000X" (manufactured by HITACHI) and a thermal analysis device controller "AS3 / DX" (manufactured by HITACHI). Specifically, 5 mg of sample is sealed in a sample container for AL autosampler φ6.8 H2.5 mm (manufactured by HITACHI) and an AL autosampler cover (manufactured by HITACHI), and set in the sample holder of the "AS3 / DX", and the temperature is changed in the order of heating, high temperature, and heating again. During the first and second heating, the temperature is raised from 0°C to 150°C at a heating rate of 10°C / min and held at 150°C for 1 minute, and during cooling, the temperature is lowered from 150°C to 0°C at a cooling rate of 10°C / min and held at 0°C for 1 minute.
[0030] <Calculation method of ΔHc and ΔHc(Hi) of exothermic peak> In the above measurement method, the area of the exothermic peak (amount of heat generation) in the exothermic curve obtained upon cooling is defined as ΔHc. Specifically, when the point where the exothermic peak rises is Point A and the end point of the exothermic peak is Point B with respect to the baseline, ΔHc is the area enclosed by the DSC curve from Point A to Point B and the baseline (see Figure 1). When there are multiple exothermic peaks, it is the area enclosed by the DSC curve from the rise point of the exothermic peak on the highest temperature side to the end point of the exothermic peak on the lowest temperature side and the baseline. ΔHc(Hi) is the amount of heat generated from the rise point of the exothermic peak (Point A) to 68.0°C, and is the area enclosed by the DSC curve from Point A to 68.0°C and the baseline (shaded area in Figure 2). For example, it can be calculated by analyzing using manual division integration. A specific method for manual division integration is to select manual division integration, click to select the rise point of the exothermic peak (point A) and the end point of the exothermic peak (point B), and then click to select the rise point of the exothermic peak (point A) and the point at 68.0°C to obtain ΔHc(Hi) (see Figure 2).
[0031] <Calculation method of ΔH1 and ΔH2> In the above measurement method, the area (endothermic amount) of the endothermic peak derived from the crystalline substance in the endothermic curve obtained during the first heating is defined as ΔH1, and the area (endothermic amount) of the endothermic peak derived from the crystalline substance in the endothermic curve obtained during the second heating is defined as ΔH2. In this case, if an exothermic peak derived from enthalpy relaxation seen in amorphous resin exists in ΔH1, it is analyzed as follows. When the peak top temperature Tm of the endothermic peak originating from the crystalline substance located at the lowest temperature side and the peak top temperature Te of the enthalpy relaxation peak are 15°C or more apart, ΔH1 is the area enclosed by the DSC curve from the end point of the exothermic peak of enthalpy relaxation (point C) to the end point of the exothermic peak of the crystalline substance (point D) and the baseline, as shown in Figure 3. When Tm and Te are less than 15°C, as shown in Figures 4(a) and (b), ΔH1' is the area ΔH1 (see Figure 4(a)) enclosed by the DSC curve from the rise point of the enthalpy relaxation peak (point E) to the end point of the endothermic peak of the crystalline substance (point F) and the baseline, minus the area ΔHe enclosed by the DSC curve and the line EG (the line connecting points E and G) from the rise point of the enthalpy relaxation peak (point E) to the end point of the exothermic peak of enthalpy relaxation (point G) (see Figure 4(b)). The enthalpy relaxation is observed near the Tg of the toner, and is observed as an endothermic peak only during the first temperature rise.
[0032] In the above formula (1), ΔHc(Hi) / ΔHc is preferably 0.65 or more, more preferably 0.70 or more, even more preferably 0.80 or more, and most preferably 0.90 or more from the viewpoint of tacking. In addition, in the formula (2), it is preferable that 0.70≦ΔH2 / ΔH1≦0.92, it is more preferable that 0.75≦ΔH2 / ΔH1≦0.90, and it is most preferable that 0.80≦ΔH2 / ΔH1≦0.87 from the viewpoint of tacking.
[0033] (Means for satisfying formula (1) and formula (2)) As a means for satisfying the above formulas (1) and (2), the following conditions can be mentioned. A toner for developing electrostatic images containing at least a binder resin and a release agent, the binder resin containing a crystalline polyester resin having a crystallization-promoting site and an amorphous vinyl resin, the amorphous vinyl resin being 40% by mass or more relative to the binder resin, and the release agent containing at least a fatty acid ester wax and a linear hydrocarbon wax.
[0034] The means for satisfying each formula are as follows. The following conditions can be mentioned as a means for achieving the formula (1): ΔHc(Hi) / ΔHc≧0.60. Contains a crystalline polyester resin with a crystallization-promoting site and a linear hydrocarbon wax as a release agent. In particular, as a means for setting the formula (1) in a more preferable range, it is preferable to satisfy the following conditions. -Contains linear hydrocarbon wax at 10% by mass or more of the total wax. The crystallization temperature of the linear hydrocarbon wax is 75°C or higher.
[0035] The following conditions can be used to achieve equation (2)-1: 0.65≦ΔH2 / ΔH1. The composition contains a crystalline polyester resin having a crystallization-promoting site and an amorphous vinyl resin, and the amount of the amorphous vinyl resin is 40% by mass or more relative to the binder resin. In particular, as a means for setting the formula (2)-1 in a more preferable range, it is preferable to satisfy the following conditions. The crystallization-promoting portion of the crystalline polyester resin has 10 or more carbon atoms. - The binder resin contains 50% or more by mass of amorphous vinyl resin.
[0036] The following conditions can be mentioned as a means for achieving formula (2)-2: ΔH2 / ΔH1≦0.95. The release agent contains 50% or more by mass of fatty acid ester wax. In particular, as a means for setting the formula (2)-2 in a more preferable range, it is preferable to satisfy the following requirements. The number of carbon atoms in the crystallization-promoting portion of the crystalline polyester resin is 30 or less. The crystalline polyester resin has vinyl resin segments.
[0037] <Softening point of toner> The softening point (Tsp) of the toner of the present invention is preferably within the range of 90 to 105° C. When the softening point of the toner is 90° C. or higher, good heat-resistant storage stability is obtained, and when the softening point is 105° C. or lower, good low-temperature fixability is obtained. Therefore, from the viewpoint of achieving both heat-resistant storage stability and low-temperature fixability, the softening point is more preferably within the range of 93 to 102° C., and even more preferably within the range of 96 to 99° C.
[0038] (Method of Measuring Toner Softening Point) The softening point (Tsp) of the toner is measured by using a "Flow Tester CFT-500" (manufactured by Shimadzu Corporation) to mold the toner into a cylindrical shape with a height of 10 mm, and applying a pressure of 1.96 x 106 Pa from the plunger while heating at a temperature increase rate of 6°C / min, so that the toner is extruded from a nozzle with a diameter of 1 mm and a length of 1 mm, thereby drawing a curve (softening flow curve) between the plunger descent amount and temperature of the flow tester, and the temperature at which the toner first flows out is the melting start temperature, and the temperature at which the toner descent amount reaches 5 mm is the softening point temperature.
[0039] (Means for setting the softening point of the toner within the range of 90 to 105°C) In order to make the softening point of the toner 90° C. or higher, it is necessary that the linear hydrocarbon wax accounts for 10% by mass or more of the total amount of wax. In order to make the softening point of the toner 105° C. or lower, the fatty acid ester wax must be present in an amount of 10% by mass or more based on the total amount of wax.
[0040] [Composition of toner for developing electrostatic images] The toner of the present invention contains toner base particles that contain at least a binder resin and a release agent. The toner base particles according to the present invention may contain various internal additives such as a colorant, a charge control agent, a surfactant, etc., in addition to a binder resin and a release agent, as required. In the present invention, the toner base particles to which an external additive has been added are referred to as toner particles, and an aggregate of toner particles is referred to as toner. Generally, the toner base particles can be used as they are as toner particles, but in the present invention, the toner base particles to which an external additive has been added are used as toner particles.
[0041] <Release agent> The release agent according to the present invention preferably contains at least a fatty acid ester wax and a linear hydrocarbon wax. The fatty acid ester wax and the linear hydrocarbon wax function as crystal nucleating agents for the crystalline polyester, and can promote the crystallization of the crystalline polyester even in the presence of a binder resin. The fatty acid ester wax is easily compatible with the binder resin when molten and plasticizes the binder resin, thereby obtaining good low-temperature fixability. On the other hand, the linear hydrocarbon wax has a higher crystallization temperature than the fatty acid ester wax, and therefore the release agent and crystalline polyester in the toner can be crystallized at a high temperature, obtaining excellent tackiness resistance. Therefore, by including the fatty acid ester wax and the linear hydrocarbon wax, excellent low-temperature fixability and tackiness resistance can be obtained.
[0042] Examples of the fatty acid ester wax include behenyl behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, tristearyl trimellitate, distearyl maleate, etc. Behenyl behenate is particularly preferred from the viewpoint of its high plasticizing effect on the binder resin and its effect as a crystal nucleating agent for crystalline polyester. Examples of the linear hydrocarbon wax include Fischer-Tropsch wax, polyolefin waxes such as polyethylene wax and polypropylene wax, and paraffin wax. Among such linear hydrocarbon waxes, Fischer-Tropsch wax is preferred because it is highly effective as a crystal nucleating agent for crystalline polyesters and has a high crystallization temperature within a range that does not impair fixability, and further excellent tack resistance can be obtained by including Fischer-Tropsch wax as a release agent. FNP-0090 is particularly preferred because it is highly effective as a crystal nucleating agent for crystalline polyesters and fatty acid ester waxes and has a high crystallization temperature within a range that does not impair fixability.
[0043] The release agent may contain a release agent other than the fatty acid ester wax and the linear hydrocarbon wax. Examples of such a release agent include branched hydrocarbon waxes such as microcrystalline wax, dialkyl ketone waxes such as distearyl ketone, carnauba wax, rice wax, montan wax, ethylenediamine behenylamide, and amide waxes such as trimellitic acid tristearylamide.
[0044] Examples of commercially available products include FNP-0090 and HNP-51 manufactured by Nippon Seiro Co., Ltd., C80 manufactured by Sasol Co., Ltd., and CERAFLOUR 991 manufactured by BYK.
[0045] The melting point or crystallization temperature of the release agent is preferably within a range of 65 to 100°C from the viewpoint of both suppressing tackiness and achieving low-temperature fixability, and more preferably within a range of 75 to 90°C. In particular, it is preferable that the linear hydrocarbon wax contains a linear hydrocarbon wax having a crystallization temperature of 75° C. or more. When the crystallization temperature is 75° C. or more, the release agent and the crystalline polyester resin in the toner can be crystallized at a higher temperature, and a more excellent tacking suppression effect can be obtained. From the viewpoint of suppressing tacking, it is more preferable that the crystallization temperature is 80° C. or more, and even more preferable that the crystallization temperature is 85° C. or more. Examples of the linear hydrocarbon wax having a crystallization temperature of 75° C. or higher include polyolefin waxes such as Fischer-Tropsch wax, polyethylene wax, and polypropylene wax.
[0046] The ratio of the fatty acid ester wax to the linear hydrocarbon wax is preferably within the range of 1:9 to 9:1, more preferably within the range of 2:8 to 8:2, and further preferably within the range of 4:6 to 6:4. When the ratio of the fatty acid ester wax to the total wax amount is 10% by mass or more, the plasticizing effect of the binder resin is exerted, and good fixability is obtained.When the ratio of the linear hydrocarbon wax to the total wax amount is 10% by mass or more, the crystallization of the crystallized polyester can be promoted, and the crystallization temperature of the entire toner can be increased, and good tack resistance can be obtained.
[0047] The content of the release agent is preferably within a range of 1 to 20 parts by mass, and more preferably within a range of 5 to 10 parts by mass, relative to 100 parts by mass of the binder resin.
[0048] <Binding resin> The binder resin according to the present invention refers to the entire resin excluding the release agent and colorant. The binder resin according to the present invention is only required to contain at least a crystalline polyester resin, and may be appropriately selected from various known thermoplastic resins. Examples of thermoplastic resins include vinyl resins such as styrene resins, (meth)acrylic resins, styrene-(meth)acrylic copolymer resins, and olefin resins, and amorphous polyester resins such as carbonate resins, polyethers, polyvinyl acetate resins, urea resins, and styrene-acrylic modified polyester resins. In particular, styrene resins and acrylic resins are preferred from the viewpoint of ease of crystallization of crystalline polyester resins and ease of control of thermoplasticity. Compared with amorphous polyester resins, styrene resins and acrylic resins have a moderately different polarity from crystalline polyester resins, so they are easily incompatible and easily crystallized. The above-mentioned thermoplastic resins may be used alone or in combination of two or more types.
[0049] In the present invention, it is particularly preferable that the binder resin contains an amorphous vinyl resin in addition to the crystalline polyester resin. It is preferable that the content of the amorphous vinyl resin in the binder resin is 50% by mass or more, and the amorphous vinyl resin is the main binder. The amorphous polyester resin, which is commonly used, is structurally similar to the crystalline polyester resin, and therefore tends to interact with the crystalline polyester resin. Therefore, if the content of the amorphous polyester resin is 50% by mass or more, the amorphous polyester resin is compatible with the crystalline polyester resin, and the crystallization of the crystalline polyester is suppressed. By containing 50% or more of the amorphous vinyl resin, which has a structure different from that of the crystalline polyester resin, the crystallization of the crystalline polyester resin is not easily suppressed, and excellent tack resistance is obtained. Furthermore, a non-crystalline polyester resin may be contained as a binder resin. Hereinafter, the crystalline polyester resin, the amorphous vinyl resin as the amorphous resin, and the amorphous polyester resin will be described in that order.
[0050] <Crystalline polyester resin> In the present invention, the crystalline polyester resin is not limited as long as it is a polyester resin exhibiting crystallinity, and any known crystalline polyester resin can be used. The term "crystallinity" means that the endothermic curve obtained by DSC has a clear endothermic peak rather than a step-like endothermic change at the melting point, i.e., when the temperature is increased. A clear endothermic peak means a peak with a half-width of 15°C or less in the endothermic curve when the temperature is increased at a rate of 10°C / min.
[0051] (Method of measuring melting point) The melting point (Tm) of the crystalline polyester resin is preferably within a range of 55 to 90°C, more preferably 70 to 85°C, from the viewpoint of obtaining sufficient low-temperature fixing property and excellent hot offset resistance. The melting point of the crystalline polyester resin can be controlled by the resin composition.
[0052] The melting point (Tm) is the temperature at the top of the endothermic peak, and can be measured by DSC. Specifically, the sample is sealed in an aluminum pan KIT NO. B0143013 and set in the sample holder of a thermal analysis device Diamond DSC (manufactured by PerkinElmer), and the temperature is changed in the order of heating, cooling, and heating. In the first heating, the temperature is raised from room temperature (25°C), and in the second heating, the temperature is raised from 0°C at a heating rate of 10°C / min to 150°C and held at 150°C for 5 minutes, and in the cooling, the temperature is lowered from 150°C to 0°C at a heating rate of 10°C / min and held at 0°C for 5 minutes. The temperature at the top of the endothermic peak in the endothermic curve obtained in the second heating is measured as the melting point.
[0053] The crystalline polyester resin is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyalcohol). As the crystalline polyester resin, any crystalline polyester resin known in the art may be used.
[0054] The polycarboxylic acid is a compound containing two or more carboxy groups in one molecule.Specific examples include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, n-dodecyl succinic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid (dodecanedioic acid), and tetradecanedicarboxylic acid (tetradecanedioic acid); alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid; trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid; and anhydrides or alkyl esters of these carboxylic acid compounds having 1 to 3 carbon atoms.These may be used alone or in combination of two or more.
[0055] The polyhydric alcohol is a compound containing two or more hydroxyl groups in one molecule.Specific examples include aliphatic diols such as 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, dodecanediol, neopentyl glycol, and 1,4-butenediol; and polyhydric alcohols having three or more hydric groups such as glycerin, pentaerythritol, trimethylolpropane, and sorbitol.These may be used alone or in combination of two or more.
[0056] The method for forming the crystalline polyester resin is not particularly limited, and the resin can be formed by polycondensing (esterifying) the polyhydric alcohol component and the polyvalent carboxylic acid component using a known esterification catalyst. The ratio of the polyhydric alcohol component to the polycarboxylic acid component used is preferably within a range of 1.5 / 1 to 1 / 1.5, more preferably 1.2 / 1 to 1 / 1.2, in terms of the equivalent ratio of the hydroxyl group of the polyhydric alcohol component to the carboxyl group of the polycarboxylic acid component.
[0057] Examples of catalysts that can be used in producing the crystalline polyester resin include alkali metal compounds such as sodium and lithium, alkaline earth metal compounds such as magnesium and calcium, metal compounds such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium, phosphorous compounds, phosphoric acid compounds, and amine compounds. Specific examples of the tin compound include dibutyltin oxide, tin octoate, tin dioctoate, and salts thereof. Examples of titanium compounds include titanium alkoxides such as tetra-n-butyl titanate, tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanolaminate.
[0058] The germanium compound may include germanium dioxide. Examples of the aluminum compound include oxides such as polyaluminum hydroxide, aluminum alkoxides, and tributylaluminate. These may be used alone or in combination of two or more. The polymerization temperature and polymerization time are not particularly limited, and the pressure in the reaction system may be reduced during the polymerization, if necessary.
[0059] The above-mentioned "crystalline polyester resin" refers not only to a polymer whose constituent components are 100% polyester structure, but also to a polymer (copolymer) obtained by polymerizing a polyester component together with another component, provided that in the latter case, the other constituent components than the polyester that constitute the polymer (copolymer) are 50 mass % or less.
[0060] In addition, the crystalline polyester resin according to the present invention has a portion having a crystalline structure and a crystallization-promoting portion, and it is preferable that the crystallization-promoting portion is a portion derived from a compound selected from the group consisting of an aliphatic monocarboxylic acid having 10 to 30 carbon atoms or an aliphatic monoalcohol having 10 to 30 carbon atoms.
[0061] Inclusion of a portion having a crystalline structure is preferable from the viewpoint of fixability, since it can impart a sharp melt property that quickly plasticizes the binder resin at a desired temperature. Inclusion of a crystallization promoting portion promotes crystallization of the portion having a crystalline structure, since the crystallization promoting portion is incompatible with the binder resin, and the crystallization of the portion having a crystalline structure is promoted. Furthermore, since the crystallization promoting portion and the release agent have a lower polarity than the binder resin and tend to interact with each other, the release agent, which has a higher crystallization temperature than the crystalline polyester, becomes a crystal nucleus, and the crystallization of the portion having a crystalline structure is further promoted. Therefore, inclusion of a crystallization promoting portion is preferable from the viewpoint of tack resistance. When the number of carbon atoms of the crystallization promoting portion is 10 or more, the crystallization promoting portion is easily incompatible with the binder resin, and the crystallization of the portion having a crystalline structure is promoted, which is preferable from the viewpoint of tack resistance. When the number of carbon atoms is 30 or less, the crystallization promoting portion does not inhibit the plasticization effect of the crystalline polyester, which is preferable from the viewpoint of fixability.
[0062] <Parts having a crystal structure> In the present invention, the "site having a crystalline structure" preferably contains at least a crystalline polyester polymer segment that forms a crystalline structure, and is a hybrid crystalline polyester resin formed by chemically bonding the crystalline polyester polymer segment and a vinyl resin polymer segment. By having the crystalline polyester resin have segments of vinyl resin, which is the main component of the binder resin, the crystalline polyester resin is finely dispersed in the toner, and excellent low-temperature fixing property is obtained.
[0063] The proportion of the aliphatic carboxylic acid monomer and / or aliphatic alcohol monomer constituting the crystallization-promoting site relative to all units derived from the monomers constituting the crystalline polyester polymerization segment is preferably within the range of 1 to 15 mass%, more preferably within the range of 3 to 10 mass%. When the ratio is 1% by mass or more, the crystallization promoting portion is easily incompatible with the binder resin, so that the crystallization of the portion having a crystalline structure is promoted, and the tackiness can be favorable.When the ratio is 15% by mass or less, the crystallization promoting portion does not inhibit the plasticizing effect of the crystalline polyester resin, so that the low-temperature fixability can be favorable.
[0064] <Crystalline polyester polymer segment> The crystalline polyester polymer segment is a portion derived from a crystalline polyester resin, and refers to a resin segment that shows a clear endothermic peak, not a stepwise endothermic change, in differential scanning calorimetry (DSC) of the toner.
[0065] The crystalline polyester polymerized segment is not particularly limited as long as it is as defined above. For example, for a resin having a structure in which other components are copolymerized in a main chain of a crystalline polyester polymerized segment, or a resin having a structure in which a crystalline polyester polymerized segment is copolymerized in a main chain made of other components, if a toner containing this resin shows a clear endothermic peak as described above, the resin corresponds to the hybrid crystalline polyester resin having a crystalline polyester polymerized segment as defined in the present invention.
[0066] The crystalline polyester polymer segment is produced by polycondensing (esterifying) a polyvalent carboxylic acid monomer and a polyhydric alcohol monomer. As the polybasic carboxylic acid monomer and the polyhydric alcohol monomer, the same monomers as the polybasic carboxylic acid monomer and the polyhydric alcohol monomer which are the raw materials of the above-mentioned crystalline polyester resin can be used.
[0067] The method for forming the crystalline polyester polymer segment is not particularly limited, and the segment can be formed by polycondensing (esterifying) a polyvalent carboxylic acid and a polyhydric alcohol using a known esterification catalyst.
[0068] <Number of carbon atoms in crystalline polyester polymer segment> The crystalline polyester polymer segment used in the present invention is preferably a polymer of a polyhydric alcohol monomer having 4 to 14 carbon atoms and a polycarboxylic acid monomer having 4 to 14 carbon atoms. If the carbon number is 4 or more, the melting point of the crystalline polyester resin is prevented from excessively increasing due to an increase in the number of hydrogen bonds derived from ester bonds, and the fixability can be improved. If the carbon number is 14 or less, the melting point of the crystalline polyester resin is prevented from excessively increasing due to an increase in the interaction between aliphatic groups, and the fixability can be improved.
[0069] <Polymerized segment of vinyl resin> A polymerized segment of a vinyl resin (also referred to as a vinyl polymerized segment) is synthesized from a vinyl monomer, which is a raw material of the vinyl resin.
[0070] In the present invention, the crystalline polyester resin preferably contains a vinyl-based polymerized segment in the range of 1 to 20% by mass, more preferably 3 to 10% by mass, which can improve low-temperature fixability. In particular, if it is 1% by mass or more, the vinyl resin as the main binder is plasticized and sharp melting properties are imparted, thereby making the low temperature fixability more suitable. In particular, if it is 20% by mass or less, the toner is not too incompatible with the vinyl resin as the main binder, making the heat-resistant storage property more suitable.
[0071] Examples of the synthesis method for the hybrid crystalline polyester resin include the following synthesis methods (a), (b) and (c). (a) A method in which a bireactive monomer is reacted with a crystalline polyester polymer segment prepared in advance, and then a vinyl monomer, which is a raw material for vinyl resin, is reacted to chemically bond the vinyl polymer segment to the crystalline polyester polymer segment. (b) A method in which a bireactive monomer is reacted with a vinyl resin prepared in advance, and then a polyvalent carboxylic acid monomer and a polyhydric alcohol monomer, which are the raw materials for a crystalline polyester resin, are reacted to chemically bond a crystalline polyester polymer segment to a vinyl polymer segment. (c) A method in which a crystalline polyester resin and a vinyl resin are reacted with a bireactive monomer to chemically bond the crystalline polyester polymer segment and the vinyl polymer segment to each other.
[0072] The bireactive monomer is a monomer that bonds a crystalline polyester resin and a vinyl resin, and has a substituent such as a hydroxy group, a carboxy group, an epoxy group, a primary amino group, a secondary amino group, etc., that can react with a crystalline polyester resin, and an ethylenically unsaturated group that can react with an amorphous resin in the molecule. Among them, vinyl carboxylic acid having a hydroxy group or a carboxy group and an ethylenically unsaturated group is preferred. As the bireactive monomer, for example, (meth)acrylic acid, fumaric acid, maleic acid, etc. can be used, and hydroxyalkyl (having 1 to 3 carbon atoms) esters of these acids may also be used. From the viewpoint of reactivity, acrylic acid, methacrylic acid, or fumaric acid is preferred.
[0073] From the viewpoint of improving the low-temperature fixing property, hot offset resistance and durability of the toner, the amount of the bireactive monomer used is preferably within a range of 1 to 10 parts by mass, and more preferably within a range of 4 to 8 parts by mass, relative to 100 parts by mass of the total amount of the monomers used to form the vinyl-based polymerization segment.
[0074] <Crystallization promoting site> In the present invention, the "crystallization promoting portion" is a portion that is more easily incompatible with the binder resin than the portion having a crystalline structure, and is not particularly limited as long as it is a compound that promotes the crystallization of the portion having a crystalline structure and can raise the crystallization temperature higher than that of a crystalline polyester resin having no crystallization promoting portion. Furthermore, in the presence of a release agent, the crystallization promoting portion interacts with the release agent, and the release agent having a high crystallization temperature becomes a crystal nucleus, thereby further raising the crystallization temperature of the crystallized polyester resin having the crystallization promoting portion.
[0075] The crystallization promoting portion is not particularly limited as long as it does not impair the low-temperature fixing property of the toner of the present invention and can increase the crystallization temperature more than a crystalline polyester resin without a crystallization promoting portion, but from the viewpoint of both crystallization promotion and low-temperature fixing, it is preferable that the portion has the following structure. Specifically, it is preferable that the portion is derived from a compound selected from the group consisting of an aliphatic monocarboxylic acid having 10 to 30 carbon atoms or an aliphatic monoalcohol having 10 to 30 carbon atoms, and further has one or more functional groups that can react with the end of the portion having a crystal structure. The hydrocarbon-based portion is not limited to being unsaturated, saturated, branched, or linear, but from the viewpoint of crystallization promotion, it is preferable that the hydrocarbon-based portion is saturated and linear, and is bonded to the molecular chain end of the portion having a crystal structure.
[0076] (Aliphatic monocarboxylic acid) Examples of the aliphatic monocarboxylic acid include octylic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, triacontanoic acid, and dotriacontanoic acid.
[0077] (Aliphatic monoalcohol) Examples of the aliphatic monoalcohol include octynol, decanol, lauryl alcohol, myristyl alcohol, palmityl alcohol, stearyl alcohol, arachidyl alcohol, behenyl alcohol, tetracosanol, hexacosanol, octacosanol, triacontanol, and dotriacontanol.
[0078] From the viewpoint of achieving both tack suppression effect and fixability, the proportion of the crystallization-promoting portion in the crystalline polyester resin is preferably within the range of 1 to 15 mass %, more preferably within the range of 2 to 12 mass %, and even more preferably within the range of 3 to 9 mass %.
[0079] The content of the crystalline polyester resin in the binder resin is preferably within a range of 4 to 15% by mass, more preferably within a range of 7 to 12% by mass, from the viewpoint of achieving both low-temperature fixability and suppression of tacking.
[0080] <Weight average molecular weight of crystalline polyester resin> The weight average molecular weight (Mw(C)) of the crystalline polyester resin in the present invention preferably satisfies the following formula (1), more preferably the following formula (2), and particularly preferably the following formula (3). Formula (1): 1000≦Mw(C)≦29000 Formula (2): 3000≦Mw(C)≦20000 Formula (3): 5000≦Mw(C)≦15000 When Mw(C) is 1000 or less, the crystalline polyester resin becomes incompatible with the binder resin after melting, and crystallization proceeds, which is preferable in terms of suppressing tacking.When Mw(C) is 29000 or less, the crystalline polyester resin becomes compatible with the binder resin when melting, which is preferable in terms of low-temperature fixability.
[0081] The weight average molecular weight of the crystalline polyester resin is measured by the following method. Gel permeation chromatography (HLC-8320GPC: Tosoh Corporation) The measurement can be performed using a column consisting of one "TSKgel guard column SuperHZ-L" and three "TSKgel SuperHZM-M" columns (all manufactured by Tosoh Corporation). The column (TSK-) is stabilized at 40°C, and tetrahydrofuran (THF) is passed through the column at this temperature as a carrier solvent at a flow rate of 0.35mL / min. The THF sample solution of the measurement sample (resin) adjusted to a sample concentration of 1mg / mL is treated with a roll mill at room temperature for 10 minutes, and then processed with a membrane filter with a pore size of 0.2μm to obtain a sample solution. 10μL of this sample solution is injected into the device together with the above carrier solvent, and detected using a refractive index detector (RI detector). The molecular weight distribution of the measured sample is calculated based on a calibration curve created using a polystyrene standard sample with a monodisperse molecular weight distribution. Standard samples: "TSK standard": "A-500", "F-1", "F-10", The samples are prepared from 10 samples: F-80, F-380, A-2500, F-4, F-40, F-128, and F-700. The data collection interval for sample analysis is 300 ms. The weight average molecular weight of the crystalline polyester resin can be calculated by the above-mentioned measuring method after separating the crystalline resin and the release agent in the toner as described below.
[0082] <Separation of crystalline polyester resin> First, the toner is dispersed in ethanol, which is a poor solvent for the toner, and the temperature is raised to a temperature exceeding the melting points of the crystalline polyester and the wax. At this time, pressure may be applied if necessary. At this point, the crystalline polyester and the wax, which have exceeded their melting points, are melted. Then, a mixture of the crystalline polyester and the wax can be collected from the toner by solid-liquid separation. The mixture can be classified according to molecular weight to separate the crystalline polyester and the wax from the toner.
[0083] <Acid value of crystalline polyester resin> The acid value of the crystalline polyester resin in the present invention is preferably within a range of 9 to 30 mgKOH / g, and more preferably within a range of 15 to 23 mgKOH / g, from the viewpoints of low temperature fixability and fixability.
[0084] The acid value of a crystalline polyester resin is the number of milligrams of potassium hydroxide required to neutralize the carboxyl groups present in 1 g of the resin (mgKOH / g). Specifically, it is determined by the following method in accordance with JIS K0070-1992.
[0085] (1) Preparation of reagents (a) Phenolphthalein solution Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95 vol%), and add ion-exchanged water to make 100 mL to obtain a phenolphthalein solution.
[0086] (b) Potassium hydroxide solution Dissolve 7 g of special grade potassium hydroxide in 5 mL of ion-exchanged water, and add ethyl alcohol (95 vol%) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container.
[0087] (c) Factor of potassium hydroxide solution The factor of the potassium hydroxide solution is determined by placing 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding a few drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution to determine the amount of the potassium hydroxide solution required for neutralization.
[0088] (d) Hydrochloric acid solution The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K8001-1998.
[0089] (2) Operation (a) Main Test 2.0 g of toner is accurately weighed into a 200 mL Erlenmeyer flask, and 100 mL of a mixed solution of toluene:ethanol (2:1) is added and dissolved over 5 hours. Next, several drops of the phenolphthalein solution were added as an indicator, and the solution was titrated with the potassium hydroxide solution. The end point of the titration was when the light red color of the indicator continued for about 30 seconds.
[0090] (b) Blank test No sample was used (i.e., only a mixture of toluene:ethanol (2:1) was used). Except for the above, the titration is carried out in the same manner.
[0091] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CD) × f × 5.611] / S Where: A: Acid value (mgKOH / g) C: Amount of potassium hydroxide solution added in this test (mL) D: Amount of potassium hydroxide solution added for blank test (mL) f: Factor of 0.1 mol / L potassium hydroxide ethanol solution 5.611: Molar mass of potassium hydroxide 56.11 (g / mol) x (1 / 10) S: mass of sample (g)
[0092] <Amorphous resin> Amorphous resins are one type of binder resin, and examples of amorphous resins include amorphous vinyl resins such as styrene-acrylic resins (hereinafter simply referred to as vinyl resins) and known amorphous polyester resins. The term "amorphous" means that the material has a glass transition point (Tg) in an endothermic curve obtained by differential scanning calorimetry (DSC), but does not have a melting point, i.e., a clear endothermic peak during heating. The clear endothermic peak means an endothermic peak with a half-width of 15°C or less in an endothermic curve obtained during the second heating when heating, lowering, and heating are continuously performed at a rate of 10°C / min, as in the above-mentioned differential scanning calorimetry measurement method.
[0093] <Amorphous vinyl resin> An amorphous vinyl resin (hereinafter also referred to as a "vinyl-based resin") refers to a polymer of a monomer having a vinyl group (hereinafter referred to as a vinyl monomer) that exhibits amorphous properties. Depending on the type of binder resin, the binder resin may be compatible with the crystalline polyester resin, which may inhibit the crystallization of the crystalline polyester resin. However, by using an amorphous vinyl resin that has a different composition and molecular structure from the crystalline polyester resin, the inhibition of the crystallization of the crystalline polyester resin can be prevented, and good tacking resistance can be obtained. Examples of resins having a different composition from the crystalline polyester resin include styrene-acrylic resin, styrene resin, and acrylic resin, and among these, styrene-acrylic resin is preferred from the viewpoint of achieving both meltability and heat resistance.
[0094] Examples of vinyl monomers that can be used include the following, and one of these can be used alone or two or more can be used in combination.
[0095] (1) Styrene-based monomers Monomers having a styrene structure, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, and derivatives thereof (2) (Meth)acrylic acid ester monomers Monomers having a (meth)acrylic group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and derivatives thereof. (3) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (4) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (5) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (6) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (7)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid derivatives such as acrylonitrile, methacrylonitrile, and acrylamide, and methacrylic acid derivatives, etc.
[0096] As the vinyl monomer, it is preferable to use a monomer having an ionically dissociable group such as a carboxy group, a sulfonic acid group, or a phosphoric acid group, since this makes it easier to control the compatibility with the crystalline resin. Examples of monomers having a carboxy group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters. Examples of the monomer having a sulfonic acid group include styrenesulfonic acid, allylsulfosuccinic acid, and 2-acrylamido-2-methylpropanesulfonic acid. An example of a monomer having a phosphoric acid group is acidophosphooxyethyl methacrylate.
[0097] Furthermore, it is also possible to obtain a polymer having a crosslinked structure by using polyfunctional vinyls as the vinyl monomer. Examples of polyfunctional vinyls include divinylbenzene, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, neopentyl glycol dimethacrylate, and neopentyl glycol diacrylate.
[0098] From the viewpoint of tackiness resistance, the content of the amorphous vinyl resin in the binder resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount of the toner.
[0099] <Crosslinking agent> The vinyl resin may have a crosslinked structure formed by a crosslinking agent having two or more vinyl groups. Examples of the crosslinking agent used in this case include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, divinylbenzene, divinylnaphthalene, silicone modified with acrylic at both ends, and silicone modified with methacrylic at both ends. Examples of polyfunctional crosslinking agents include pentaerythritol triacrylate, trimethylolethane triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylate, and compounds in which the acrylate in the above compounds is replaced with methacrylate, such as triallyl cyanurate and triallyl trimellitate. Among the above crosslinking agents, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethoxylated bisphenol A-di(meth)acrylate, etc. are preferred in that they can increase the internal cohesive force of the toner layer without deteriorating the low-temperature fixing property. The amount of the crosslinking agent added is preferably within a range of 0.01 to 10 parts by mass, and more preferably within a range of 0.10 to 5.0 parts by mass, based on 100 parts by mass of the polymerizable monomer.
[0100] <Amorphous polyester resin> The amorphous polyester resin is a resin exhibiting amorphousness among polyester resins obtained by a polymerization reaction between a divalent or higher carboxylic acid (polycarboxylic acid) monomer and a divalent or higher alcohol (polyhydric alcohol) monomer. The amorphous polyester resin can be formed by condensing (esterifying) the polyvalent carboxylic acid monomer and the polyhydric alcohol monomer using a known esterification catalyst. Since the amorphous polyester resin has excellent affinity with paper, it is preferable to include the amorphous polyester resin as a shell in the toner surface layer from the viewpoint of folding fixability.
[0101] The polycarboxylic acid monomer is a compound that contains two or more carboxy groups in one molecule. Examples of polyvalent carboxylic acid monomers that can be used in the synthesis of the amorphous polyester resin include phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, mesaconic acid, dimethyl isophthalate, fumaric acid, dodecenylsuccinic acid, 1,10-dodecanedicarboxylic acid, etc. Among these, dimethyl isophthalate, terephthalic acid, dodecenylsuccinic acid, and trimellitic acid are preferred.
[0102] A polyhydric alcohol monomer is a compound that contains two or more hydroxy groups in one molecule. Examples of polyhydric alcohol monomers that can be used in the synthesis of the amorphous polyester resin include dihydric or trihydric alcohols such as ethylene glycol, propylene glycol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, ethylene oxide adduct of bisphenol A (BPA-EO), propylene oxide adduct of bisphenol A (BPA-PO), glycerin, sorbitol, 1,4-sorbitan, trimethylolpropane, etc. Among these, ethylene oxide adduct of bisphenol A and propylene oxide adduct of bisphenol A are preferred.
[0103] Examples of the esterification catalyst that can be used include alkali metal compounds such as sodium and lithium; alkaline earth metal compounds such as magnesium and calcium; metal compounds such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds.
[0104] The polymerization temperature is not particularly limited, but is preferably within the range of 150 to 250° C. The polymerization time is not particularly limited, but is preferably within the range of 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0105] The content of the amorphous polyester resin in the binder resin is preferably within a range of 3 to 20% by mass, and more preferably within a range of 5 to 15% by mass, in terms of folding fixability.
[0106] (Preferable glass transition temperature of amorphous resin) The glass transition point (Tg) of the amorphous resin is preferably within a range of 50 to 65°C, more preferably within a range of 55 to 60°C, from the viewpoint of achieving both sufficient low-temperature fixability and heat-resistant storage stability.
[0107] The glass transition point (Tg) can be calculated by carrying out differential scanning calorimetry (DSC measurement) using a differential scanning calorimeter "DSC7000X" (manufactured by HITACHI) and a thermal analysis device controller "AS3 / DX" (manufactured by HITACHI). Specifically, 5 mg of sample is sealed in a sample container for AL autosampler φ6.8 H2.5 mm (manufactured by HITACHI) and an AL autosampler cover (manufactured by HITACHI), and set in the sample holder of the "AS3 / DX", and the temperature is changed in the order of heating, high temperature, and heating again. During the first and second heating, the temperature is raised from 0°C to 150°C at a heating rate of 10°C / min and held at 150°C for 1 minute, and during cooling, the temperature is lowered from 150°C to 0°C at a cooling rate of 10°C / min and held at 0°C for 1 minute.
[0108] (Weight average molecular weight of amorphous resin) The weight average molecular weight (Mw) of the amorphous resin is preferably within a range of 10,000 to 100,000 from the viewpoints of fixability and heat-resistant storage stability. The weight average molecular weight of the amorphous resin can be measured in the same manner as the weight average molecular weight of the crystalline resin described below.
[0109] <Coloring agent> The colorant contained in the toner base particles according to the present invention may be a known inorganic or organic colorant. As the colorant, carbon black, magnetic powder, various organic or inorganic pigments, dyes, etc. may be used. The amount of the colorant added is in the range of 1 to 30% by mass, preferably 2 to 20% by mass, based on the toner particles.
[0110] <Other internal and external additives> In addition to the above, the toner particles may contain internal additives such as a crosslinking agent and a charge control agent, external additives, and the like, if necessary.
[0111] <Charge control agent> Charge control agents include nigrosine dyes, metal salts of naphthenic acid or higher fatty acids, and alkoxides. Known compounds such as xylated amines, quaternary ammonium salts, azo-based metal complexes, salicylic acid metal salts, etc. The charge control agent makes it possible to obtain a toner having excellent charging properties. The content of the charge control agent can usually be within a range of 0.1 to 5.0 parts by mass with respect to 100 parts by mass of the binder resin.
[0112] <External additives> The toner particles can be used as they are, but may be treated with external additives such as a fluidizing agent and a cleaning aid in order to improve flowability, chargeability, cleaning properties, and the like.
[0113] Examples of the external additive include inorganic oxide fine particles such as silica fine particles, alumina fine particles, and titanium oxide fine particles, inorganic stearic acid compound fine particles such as aluminum stearate fine particles and zinc stearate fine particles, and inorganic titanic acid compound fine particles such as strontium titanate and zinc titanate. These may be used alone or in combination of two or more. From the viewpoint of improving heat-resistant storage stability and environmental stability, it is preferable that these inorganic particles are subjected to a gloss treatment using a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, or the like.
[0114] The amount of the external additive added (the total amount added when multiple external additives are used) is preferably within a range of 0.05 to 5 parts by mass, and more preferably within a range of 0.1 to 3 parts by mass, per 100 parts by mass of the toner.
[0115] <Core-shell structure> The toner particles can be used as they are as a toner, but may also be toner particles having a multilayer structure such as a core-shell structure comprising the toner particles as a core particle and a shell layer covering the surface of the core particle. The shell layer does not have to cover the entire surface of the core particle, and the core particle may be partially exposed. The cross section of the core-shell structure can be confirmed by known observation means such as a transmission electron microscope (TEM) or a scanning probe microscope (SPM).
[0116] In the case of a core-shell structure, the core particle and the shell layer can have different properties such as glass transition point, melting point, and hardness, making it possible to design toner particles according to the purpose. For example, a shell layer can be formed by aggregating and fusing a resin having a relatively high glass transition point (Tg) to the surface of a core particle containing a binder resin, a colorant, a release agent, etc., and having a relatively low glass transition point (Tg). The shell layer preferably contains an amorphous resin, and more preferably contains an amorphous polyester resin.
[0117] <Toner particle size> The average particle size of the toner particles is the volume-based median diameter (D 50 ) is preferably in the range of 3 to 10 μm, and more preferably in the range of 5 to 8 μm, from the viewpoints of low-temperature fixability and cleaning ability. The average particle size of the toner particles can be controlled by the concentration of the coagulant used during production, the amount of organic solvent added, the fusion time, the composition of the binder resin, and the like.
[0118] The volume-based median diameter of toner particles (D 50 For the measurement of , a measuring device consisting of a Multisizer 3 (Beckman Coulter) connected to a computer system equipped with data processing software Software V3.51 can be used. Specifically, the measurement sample (toner) is added to a surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing a surfactant component 10 times with pure water in order to disperse toner particles) and allowed to mix, after which ultrasonic dispersion is performed to prepare a toner particle dispersion. This toner particle dispersion is pipetted into a beaker containing an ISOTON II (manufactured by Beckman Coulter) in a sample stand until the concentration indicated on the measuring device is 8%. By achieving this concentration, reproducible measurement values can be obtained. Then, in the measuring device, the measurement particle count is set to 25,000 particles, the aperture diameter is set to 100 μm, and the measurement range of 2 to 60 μm is divided into 256 parts to calculate the frequency value, and the particle diameters of the 50% with the largest volume cumulative fraction are determined as the volume-based median diameter (D 50 ) is obtained.
[0119] <Average circularity of toner particles> From the viewpoint of improving the stability of the charging characteristics and low-temperature fixability, the toner particles preferably have an average circularity in the range of 0.930 to 1.000, and more preferably in the range of 0.940 to 0.995. If the average circularity is within the above range, individual toner particles are less likely to be crushed, contamination of the frictional charging member can be suppressed, the charging property of the toner can be stabilized, and the image quality of the formed image can be improved.
[0120] The average circularity of the toner particles can be measured using an FPIA-3000 (manufactured by Sysmex Corporation). Specifically, the measurement sample (toner) is soaked in an aqueous solution containing a surfactant, and dispersed by ultrasonic dispersion treatment for 1 minute. After that, an image is taken using an FPIA-3000 (manufactured by Sysmex) under the measurement condition HPF (high magnification imaging) mode at an appropriate concentration of 3,000 to 10,000 HPF detections. If the HPF detections are within the above range, reproducible measurement values can be obtained. From the captured particle images, the circularity of each toner particle is calculated according to the following formula (I), and the circularity of each toner particle is added and divided by the total number of toner particles to obtain an average circularity. Formula (I) Circularity = (perimeter of a circle with the same projected area as the particle image) / (perimeter of the projected particle image)
[0121] [Developer] The toner of the present invention can be used as a magnetic or non-magnetic one-component developer, but may also be mixed with a carrier to be used as a two-component developer. When the toner is used as a two-component developer, the carrier may be magnetic particles made of a conventionally known material such as a metal such as iron, ferrite, or magnetite, or an alloy of such a metal with a metal such as aluminum or lead, and ferrite particles are particularly preferred.
[0122] As the carrier, a coated carrier in which the surface of magnetic particles is coated with a coating agent such as resin, or a dispersion type carrier in which fine magnetic powder is dispersed in a binder resin may be used. The volumetric median diameter of the carrier (D 50 ) is preferably in the range of 20 to 100 μm, and more preferably in the range of 25 to 80 μm. The volumetric median diameter of the carrier (D 50 ) can be measured, for example, by a laser diffraction particle size distribution measuring device HELOS (manufactured by SYMPATEC) equipped with a wet disperser.
[0123] [Method of manufacturing toner for developing electrostatic images] The method for producing the toner according to the present invention is not particularly limited, and a known method can be adopted, but an emulsion polymerization aggregation method or an emulsion aggregation method can be preferably adopted. The emulsion polymerization aggregation method preferably used in the method for producing the toner according to the present invention is a method for producing toner particles by mixing a dispersion of fine particles of a binder resin (hereinafter also referred to as "binder resin fine particles") produced by an emulsion polymerization method with a dispersion of fine particles of a colorant (hereinafter also referred to as "colorant fine particles"), a release agent dispersion, a crystalline resin, etc., aggregating the toner base particles until they have a desired particle size, and further controlling the shape by fusing the fine particles of the binder resin together. It is preferable to use a hybrid crystalline polyester resin having a crystallization-promoting site as the crystalline resin. An example of a method for producing the hybrid crystalline polyester resin will be described below.
[0124] Step (1): A step of mixing a monomer serving as a raw material for the crystalline polyester polymerization segment, a raw material monomer for an addition polymerization resin (styrene-acrylic resin) unit (a monomer serving as a raw material for a vinyl-based polymerization segment), and an esterification catalyst in a reaction vessel, and subjecting the raw material monomer to a polycondensation reaction. Step (2): A step of forming a crystallization promotion site by adding a crystallization promoter to the reaction tank after the raw material monomer is polycondensed in the step (1) and reacting the raw material monomer.
[0125] <Process (1)> In step (1), the raw material monomers for the crystalline polyester polymer segment, the raw material monomers for the vinyl resin (styrene-acrylic resin) unit, and an esterification catalyst are mixed in a reaction tank, and the raw material monomers are subjected to a polycondensation reaction.
[0126] As the monomer serving as the raw material for the crystalline polyester polymer segment, known monomers such as the above-mentioned polyhydric alcohol monomers and polyvalent carboxylic acid monomers can be suitably used.
[0127] (Polycondensation reaction) The polycondensation reaction of the raw material monomers, that is, the method for synthesizing the crystalline polyester polymer segment is not limited, but the following methods (A) to (C) are preferable. (A) A method of subjecting a trivalent or higher polyvalent carboxylic acid or a trivalent or higher polyhydric alcohol to a polymerization reaction (B) Method of Addition Polymerization of Unsaturated Dicarboxylic Acids or Unsaturated Dialcohols (C) A method using a hybrid crystalline polyester resin in which a crystalline polyester and an amorphous resin unit are chemically bonded
[0128] In the polymerization in the above methods (A) and (B), known polymerization initiators and chain transfer agents can be used.
[0129] (Esterification catalyst) As the esterification catalyst, a known catalyst can be used, for example, tin compounds such as tin dioctylate, dibutyltin oxide, and tin(II) 2-ethylhexanoate, titanium compounds such as tetrabutyl orthotitanate (hereinafter also referred to as "Ti(OBu)4") and titanium diisopropylate bistriethanolamine, etc. Among them, Ti(OBu)4 can be preferably used.
[0130] <Process (2)> In step (2), after the raw material monomers are subjected to a polycondensation reaction in step (1), a crystallization promoter is added to the reaction tank and reacted to form a crystallization promotion site. That is, in step (1), after obtaining a crystalline polyester polymer segment by a polycondensation reaction, a crystallization promoter is added and reacted with the crystalline polyester polymer segment, whereby the crystallization promoter can be chemically bonded to the crystalline polyester polymer segment, and a crystallization promotion site can be formed. The reaction at this time may be any reaction that can chemically bond the crystalline polyester polymer segment and the crystallization promoter, and may be, for example, a method of carrying out the reaction by heating, such as at 200° C. under normal pressure, but is not limited thereto.
[0131] After steps (1) and (2), the crystalline polyester polymerization segment to which the crystallization promoter is chemically bonded can be chemically bonded to a vinyl-based polymerization segment by the above-mentioned hybrid crystalline polyester resin synthesis method, etc., to synthesize a hybrid crystalline polyester resin having a crystallization-promoting site in the crystalline polyester polymerization segment.
[0132] (Crystallization promoter) The crystallization promoter may be any compound capable of forming a crystallization promoting site as described above, and is preferably an aliphatic monocarboxylic acid having a carbon number in the range of 10 to 30 or an aliphatic monoalcohol having a carbon number in the range of 10 to 30. Specific examples include decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, triacontanoic acid, decanol, lauryl alcohol, myristyl alcohol, palmityl alcohol, stearyl alcohol, arachidyl alcohol, behenyl alcohol, tetracosanol, hexacosanol, octacosanol, triacontanol, and the like.
[0133] As a method for aggregating and fusing, for example, a known emulsion aggregation method can be suitably adopted.
[0134] (Emulsification aggregation method) The emulsion aggregation method is a method for producing toner particles by dropping a solution of an amorphous resin or a crystalline resin (hereinafter, these are also collectively referred to as "binder resin") dissolved in a solvent into a poor solvent to obtain a binder resin microparticle dispersion, mixing this binder resin microparticle dispersion with a colorant microparticle dispersion, aggregating the amorphous resin microparticles, crystalline resin microparticles, colorant microparticles, and release agent in an aqueous medium until the desired toner particle diameter is achieved, and further controlling the shape by fusing these microparticles together. As a method for adding the release agent according to the present invention, the release agent may be added when synthesizing vinyl-based resin microparticles, or a release agent dispersion in which the release agent is dispersed may be added when a resin microparticle dispersion is aggregated and fused. The former method is preferred in that the release agent can be finely dispersed in the toner and exposure of the release agent to the toner surface can be suppressed. In the former method, when the amount of the release agent is large relative to the vinyl resin, it is preferable to further add the release agent as a release agent dispersion in terms of solubility and viscosity.
[0135] (aqueous medium) In the present invention, the term "aqueous medium" refers to a medium containing at least 50% by mass of water, and examples of components other than water include organic solvents that dissolve in water, such as methanol, ethanol, isopropanol, butanol, acetone, methyl ethyl ketone, dimethylformamide, methyl cellosolve, and tetrahydrofuran. Of these, it is preferable to use alcohol-based organic solvents such as methanol, ethanol, isopropanol, and butanol, which are organic solvents that do not dissolve resins. It is preferable to use only water, such as ion-exchanged water, as the aqueous medium.
[0136] In addition, in the case of toner particles having a multilayer structure such as a core-shell structure, a manufacturing method thereof is such that core particles are produced by the above-mentioned aggregation and fusion process, and then shell binder resin fine particles for forming a shell layer are added to a dispersion of the core particles, and the shell binder resin fine particles are aggregated and fused to the surface of the core particles to form a shell layer that covers the surface of the core particles.
[0137] The embodiments to which the present invention can be applied are not limited to the above-described embodiments, and can be modified as appropriate without departing from the spirit of the present invention. EXAMPLES
[0138] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0139] [Preparation of toner base particles] <Preparation of vinyl resin particle dispersion X1> (1) First-stage polymerization A 5L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introduction device was charged with 8 parts by mass of sodium dodecyl sulfate and 3000 parts by mass of ion-exchanged water, and the internal temperature of the reaction vessel was raised to 80° C. while stirring at a stirring speed of 230 rpm under a nitrogen gas flow. After the temperature was raised, an aqueous solution in which 10 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added to the resulting mixture, and the temperature of the resulting mixture was again raised to 80° C. A monomer mixture 1 having the following composition was added dropwise to the mixture over 1 hour, and the mixture was heated and stirred at 80° C. for 2 hours to polymerize, thereby preparing a dispersion a1 of resin fine particles. (Monomer mixture 1) Styrene 480 parts by weight n-Butyl acrylate 250 parts by weight Methacrylic acid 68 parts by weight
[0140] (2) Second stage polymerization A solution of 7 parts by mass of sodium polyoxyethylene (2) dodecyl ether sulfate dissolved in 3,000 parts by mass of ion-exchanged water was charged into a 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and the solution was heated to 80°C. After that, 80 parts by mass of dispersion a1 of resin microparticles (solid content equivalent) and monomer mixture 2 in which monomers and a release agent having the composition shown below were dissolved at 90°C were added, and the mixture was mixed and dispersed for 1 hour using a mechanical disperser "CLEARMIX" (manufactured by M Technique Co., Ltd., "CLEARMIX" is a registered trademark of the company) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). (Monomer mixture 2) Styrene 285 parts by weight n-Butyl acrylate 95 parts by weight Methacrylic acid 20 parts by weight n-Octyl-3-mercaptopropionate 8 parts by mass Release agent 1 (see Table I below) 80 parts by weight Release agent 2 (see Table I below) 80 parts by weight Next, an initiator solution in which 6 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added to the dispersion, and the resulting dispersion was polymerized by heating and stirring at 86°C for 1 hour to prepare dispersion a2 of resin microparticles.
[0141] (3) Third-stage polymerization Further, 400 parts by mass of ion-exchanged water was added to the dispersion a2 of resin fine particles and mixed thoroughly, and then a solution in which 11 parts by mass of potassium persulfate was dissolved in 400 parts by mass of ion-exchanged water was added to the obtained dispersion, and monomer mixture 3 having the following composition was added dropwise over one hour at a temperature condition of 82° C. After completion of the dropwise addition, the dispersion was heated and stirred for two hours to polymerize, and then cooled to 25° C. to prepare vinyl resin particle dispersion X1 made of vinyl resin (styrene-acrylic resin). (Monomer mixture 3) Styrene 300 parts by mass n-Butyl acrylate 129 parts by weight Methacrylic acid 52 parts by weight n-Octyl-3-mercaptopropionate 8 parts by mass The physical properties of the obtained vinyl resin particle dispersion X1 were measured. The volume-based median diameter (D 50 The molecular weight (Mw) was 30,900, the glass transition temperature (Tg) was 43.0° C., and the average molecular weight (Mw) was 30,900.
[0142] <Preparation of vinyl resin particle dispersions X2 to X10> The type of release agent and the ratio of each release agent in the second polymerization stage were changed as shown in Tables I and II below, and vinyl resin particle dispersions X2 to X10 were obtained in the same manner as in the preparation of vinyl resin particle dispersion X1. In Table II below, "Release agent A + release agent B [mass %]" refers to the content (mass %) of "release agent A + release agent B" in the total amount of toner (binder resin + pigment + release agent A + release agent B).
[0143] [Table 1]
[0144] [Table 2]
[0145] <Preparation of Amorphous Polyester Resin Particle Dispersion A1> Bisphenol A ethylene oxide 2.2 mole adduct (BPA-EO) 15 mole parts Bisphenol A propylene oxide 2.2 mole adduct (BPA-PO) 85 mole parts Terephthalic acid (TPA) 55 mole parts Fumaric acid (FA) 40 mole parts Trimellitic acid (TMA) 5 mole parts The monomers other than fumaric acid and trimellitic acid were added to a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, and 0.5 mol parts of tin dioctylate were added as a catalyst. After reacting for 6 hours at 235°C under a nitrogen gas stream, the temperature was lowered to 200°C, and fumaric acid and trimellitic acid were added and reacted for 1 hour. The temperature was raised to 220°C over 5 hours, and polymerization was carried out under a pressure of 10 kPa until the desired molecular weight was reached, to obtain a pale yellow transparent amorphous polyester resin (a1). The amorphous polyester resin (a1) had a weight average molecular weight of 29000, an acid value of 18.1 KOHmg / g, and a glass transition temperature (Tg) of 44°C. Next, 200 parts by mass of the amorphous polyester resin (a1), 100 parts by mass of methyl ethyl ketone, 35 parts by mass of isopropyl alcohol, and 7.0 parts by mass of a 10% by mass aqueous ammonia solution were placed in a separable flask, thoroughly mixed and dissolved, and then ion-exchanged water was dropped at a liquid delivery rate of 8 g / min using a liquid delivery pump while heating and stirring at 40°C, and the dropping was stopped when the liquid delivery amount reached 580 parts by mass. The solvent was then removed under reduced pressure to obtain an amorphous polyester resin dispersion. Ion-exchanged water was added to the above dispersion to adjust the solid content to 25% by mass, and an amorphous polyester resin particle dispersion (A1) in which amorphous polyester resin (a1) particles were dispersed was prepared. The volume-based median diameter (D 50 ) was measured using a Microtrac UPA-150 (manufactured by Nikkiso Co., Ltd.) and found to be 156 nm.
[0146] <Preparation of Release Agent Dispersion W1> Behenyl behenate 22.5 parts by weight Fischer-Tropsch wax: 22.5 parts by mass Anionic surfactant (Neogen (registered trademark) RK, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 5 parts by mass Ion-exchanged water 200 parts by weight The above materials were mixed and heated to 90°C, and thoroughly dispersed using an Ultra-Turrax T50 manufactured by IKA. After that, dispersion processing was performed using a pressure discharge type Gaulin homogenizer, and ion-exchanged water was added to the dispersion to adjust the solid content to 15%, to prepare a dispersion (W1) of release agent particles. The volume-based median diameter of the release agent particles in this dispersion was measured using a laser diffraction type particle size distribution analyzer LA-750 (manufactured by HORIBA), and was found to be 198 nm.
[0147] <Preparation of Colorant Dispersion P1> 90 parts by mass of sodium dodecyl sulfate was dissolved in 1600 parts by mass of ion-exchanged water with stirring, and 420 parts by mass of CI Pigment Blue 18:3 was gradually added to this solution while stirring. The resulting dispersion was then subjected to a dispersion treatment using a stirring device "Clearmix" (manufactured by M Technique Co., Ltd.) to prepare a colorant particle dispersion (colorant dispersion) P1 in which the colorant particles were dispersed. The volume-based median diameter (D 50 ) was measured using a Microtrac particle size distribution analyzer "UPA-150" (manufactured by Nikkiso Co., Ltd.) and found to be 150 nm.
[0148] <Synthesis of shell resin s1> Monomer mixture 4 having the following composition including an amphoteric compound (acrylic acid) was placed in the dropping funnel. Note that di-t-butyl peroxide is a polymerization initiator. (Monomer mixture 4) Styrene 80 parts by weight n-Butyl acrylate 20 parts by weight Acrylic acid 10 parts by mass Di-t-butyl peroxide 16 parts by mass Furthermore, the raw material monomers for the polycondensation segment (amorphous polyester segment) described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and were heated to 170° C. to dissolve. Bisphenol A propylene oxide 2 mole adduct 285.7 parts by mass Terephthalic acid 66.9 parts by mass Fumaric acid 47.4 parts by mass Next, to the resulting solution, the monomer mixture 6 was added dropwise over a period of 90 minutes while stirring, and after maturing for 60 minutes, the unreacted monomers among the components of the monomer mixture 6 were removed from the four-neck flask under reduced pressure (8 kPa). Then, 0.4 parts by mass of Ti(OBu)4 was added as an esterification catalyst to the four-neck flask, and the mixture in the four-neck flask was heated to 235°C. The reaction was carried out under normal pressure (101.3 kPa) for 5 hours and then under reduced pressure (8 kPa) for 1 hour to obtain shell resin s1.
[0149] <Preparation of Shell Resin Particle Dispersion S1> 100 parts by mass of shell resin s1 was dissolved in 400 parts by mass of ethyl acetate (Kanto Chemical Co., Ltd.) and mixed with 638 parts by mass of a 0.26% by mass sodium lauryl sulfate solution prepared in advance. The resulting mixture was ultrasonically dispersed for 30 minutes with stirring using an ultrasonic homogenizer "US-150T" (Nihon Seiki Seisakusho Co., Ltd.) at a V-LEVEL of 300 μA. After that, the mixture was heated to 40°C and stirred under reduced pressure for 3 hours using a diaphragm vacuum pump "V-700" (manufactured by BUCHI) to completely remove ethyl acetate. In this way, a shell resin particle dispersion S1 having a solid content of 13.5 mass% was prepared. The volume-based median diameter (D 50 ) was 160 nm.
[0150] <Synthesis of crystalline polyester resin c1> The raw material monomers of the following addition polymerization resin (styrene acrylic resin: StAc) unit containing a bireactive monomer and a radical polymerization initiator were placed in a dropping funnel. Styrene 40 parts by weight n-Butyl acrylate 16 parts by weight Acrylic acid 3.5 parts by mass Polymerization initiator (di-t-butyl peroxide) 8 parts by mass Furthermore, the raw material monomers of the polycondensation resin (crystalline polyester resin: CPEs) unit described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and were heated to 170° C. to dissolve. Dodecanedioic acid 280 parts by mass 1,4-butanediol 105 parts by mass Next, the raw material monomer of the addition polymerization resin (StAc) was dropped over 90 minutes under stirring, and after aging for 60 minutes, the unreacted addition polymerization monomer was removed under reduced pressure (8 kPa). The amount of monomer removed at this time was very small compared to the raw material monomer ratio of the resin. Then, 0.4 parts by mass of Ti(On-Bu)4 was added, the temperature was raised to 235°C, and the reaction was carried out at normal pressure (101.3 kPa) for 5 hours and further at reduced pressure (8 kPa) for 1 hour. Next, the resulting reaction liquid was cooled to 200° C., and then the reaction was carried out under reduced pressure (20 kPa) for 1 hour. Next, the pressure in the reaction vessel was gradually released to return to normal pressure, and then 20.3 parts by mass of stearyl alcohol (5% by mass relative to the raw material monomers and crystallization promoter of the polycondensation resin unit of the crystalline polyester resin) was added as a crystallization accelerator, and the mixture was reacted at 200°C under normal pressure for 1.2 hours. Thereafter, the pressure in the reaction vessel was reduced to 5 kPa or less at 200°C, and the mixture was reacted until the acid value calculated by the above-mentioned measurement method reached 20 mgKOH / g, to obtain crystalline polyester resin c1. The crystalline resin c1 had a weight average molecular weight (Mw) of 9700 and a melting point of 72°C.
[0151] <Preparation of Crystalline Polyester Resin Particle Dispersion C1> Crystalline polyester resin c1 174.3 parts by mass The above was added to 102 parts by mass of methyl ethyl ketone and stirred at 75° C. for 30 minutes to dissolve. Next, 3.1 parts by mass of a 25% by mass aqueous solution of sodium hydroxide was added to this solution. This solution was placed in a reaction vessel equipped with a stirrer, and 375 parts by mass of water heated to 70°C was added dropwise to the solution over a period of 70 minutes while stirring. The liquid in the vessel became cloudy during the dropping, and after the entire amount was dropped, a uniform emulsion state was obtained. Next, while keeping this emulsion at 70°C, a diaphragm vacuum pump "V-700" (manufactured by BUCHI) was used to stir the emulsion under reduced pressure of 15 kPa (150 mbar) for 3 hours to distill off the methyl ethyl ketone, and the emulsion was then cooled at a cooling rate of 6°C / min to produce crystalline polyester resin particle dispersion C1 in which particles of crystalline polyester resin c1 were dispersed. Measurement with the particle size distribution measuring device showed that the volume average particle size of the crystalline polyester resin particles in crystalline polyester resin particle dispersion C1 was 197 nm.
[0152] <Synthesis of crystalline polyester resins c2 to c5> In the synthesis of crystalline polyester resin c1, the type of crystallization promoter was changed as shown in Table III below, and the reaction time and reaction temperature were appropriately changed so that the acid value of the crystalline polyester after the introduction of the crystallization promoter was 20 mgKOH / g, to obtain crystalline polyester resins c2 to c5. The weight average molecular weight (Mw) and melting point of crystalline polyester resins c2 to c5 are shown in Table III below.
[0153] <Synthesis of crystalline polyester resin c6> Dodecanedioic acid 280 parts by mass 1,4-butanediol 105 parts by mass The monomers were placed in a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, and the atmosphere in the reaction vessel was replaced with dry nitrogen gas. 0.4 parts by mass of Ti(On-Bu)4 was added to the resulting mixture, and the mixture was heated to 235°C and reacted at normal pressure (101.3 kPa) for 5 hours and then at reduced pressure (8 kPa) for 2 hours. Next, the resulting reaction liquid was cooled to 200° C., and then the reaction was carried out under reduced pressure (20 kPa) for 1 hour. Next, the pressure in the reaction vessel was gradually released to return to normal pressure, and then 20.3 parts by mass of stearyl alcohol was added as a crystallization promoter, and the mixture was reacted at normal pressure and at a temperature of 200°C for 1.5 hours. The pressure in the reaction vessel was then reduced to 5 kPa or less at 200°C, and the mixture was reacted until the acid value calculated by the above-mentioned measurement method reached 20.0 mgKOH / g, to obtain crystalline polyester resin c6. The crystalline polyester resin c6 had a weight average molecular weight (Mw) of 10900 and a melting point of 74°C.
[0154] <Synthesis of crystalline polyester resin c7> The raw material monomers of the following addition polymerization resin (styrene acrylic resin: StAc) unit containing a bireactive monomer and a radical polymerization initiator were placed in a dropping funnel. Styrene 40 parts by weight n-Butyl acrylate 16 parts by weight Acrylic acid 3.5 parts by mass Polymerization initiator (di-t-butyl peroxide) 8 parts by mass Furthermore, the raw material monomers of the polycondensation resin (crystalline polyester resin: CPEs) unit described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and were heated to 170° C. to dissolve. Dodecanedioic acid 280 parts by mass 1,4-butanediol 105 parts by mass Next, the monomer was placed in a reaction vessel equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen gas inlet tube, and the inside of the reaction vessel was replaced with dry nitrogen gas. 0.4 parts by mass of Ti(On-Bu)4 was added to the resulting mixture, and the mixture was heated to 235°C and reacted at normal pressure (101.3 kPa) for 5 hours and then at reduced pressure (8 kPa) for 1 hour. The reaction solution was then cooled to 200°C, and the reaction was continued under reduced pressure (20kPa) until the acid value calculated by the above-mentioned measurement method was 20mgKOH / g, to obtain crystalline polyester resin c7. The crystalline polyester resin c7 had a weight average molecular weight (Mw) of 10300 and a melting point of 73°C.
[0155] <Preparation of Crystalline Polyester Resin Particle Dispersions C2 to C7> Crystalline polyester resin particle dispersions C2 to C7 were obtained in the same manner as in the preparation of crystalline polyester resin particle dispersion C1, except that the crystalline polyester resin c1 was changed to crystalline polyester resins c2 to c7, respectively. In Table III, "content of crystallization accelerator [mass %]" refers to the content of the crystallization accelerator relative to the raw material monomers and crystallization accelerator of the polycondensation resin unit of the crystalline polyester resin.
[0156] [Table 3]
[0157] [Preparation of toner base particles B1] ≪Agglomeration / fusion process≫ 290 parts by mass of vinyl resin particle dispersion X1 (solid content equivalent) and 2000 parts by mass of ion-exchanged water were added to a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, and then a 5 mol / L aqueous sodium hydroxide solution was further added to adjust the pH of the dispersion in the reaction vessel to 10 (measurement temperature: 25° C.). 30 parts by mass of colorant dispersion P1 (solid content equivalent) was added to the dispersion. Next, an aqueous solution of 30 parts by mass of magnesium chloride as an aggregating agent dissolved in 60 parts by mass of ion-exchanged water was added to the dispersion liquid over 15 minutes under stirring at 30° C. The resulting dispersion liquid was allowed to stand for 5 minutes, and then heated to 80° C. over 60 minutes, and 40 parts by mass (solid content equivalent) of crystalline polyester resin particle dispersion liquid C1 was added over 20 minutes, and the stirring speed and temperature were adjusted so that the particle size growth rate was 0.01 μm / min to allow aggregation to proceed. The particle size of the particles associated in the mixture was measured using a Coulter Multisizer 3 (manufactured by Beckman Coulter), and when the volume-based median diameter d50 of the particles reached 6.0 μm, 40 parts by mass of shell resin particle dispersion S1 (solid content equivalent) was added to the mixture over 30 minutes. When the supernatant of the resulting reaction solution became transparent, an aqueous solution in which 190 parts by mass of sodium chloride was dissolved in 760 parts by mass of ion-exchanged water was added to the reaction solution to stop particle growth.
[0158] ≪Aging / cooling process≫ Furthermore, the reaction solution was heated to 86°C and stirred to promote fusion of the particles, and the particles in the reaction solution were measured (HPF detection number: 4,000 particles) using a measuring device "FPIA-3000" (manufactured by Sysmex Corporation). When the average circularity of the particles reached 0.960, the reaction solution was cooled to 25°C at a cooling rate of 10°C / min.
[0159] <Filtering, washing and drying processes> Next, the particles were separated from the cooled reaction liquid, dehydrated, and the resulting cake was washed by repeating redispersion in ion-exchanged water and solid-liquid separation three times, and then dried at room temperature until the toner moisture content was less than 2%, and then dried at 35°C until the toner moisture content was less than 1%, to obtain toner base particles B1.
[0160] [Preparation of toner base particles B2, B4 to B13, B15 to B17, and B19] Toner base particles B2, B4 to B13, B15 to B17, and B19 were prepared in the same manner as in the preparation of toner base particle B1, except that vinyl resin particle dispersion X1 was changed to vinyl resin particle dispersions X2 to X10 shown in Table IV, and crystalline polyester resin particle dispersion C1 was changed to crystalline polyester resin particle dispersions C2 to C7 shown in Table IV.
[0161] [Preparation of toner base particles B3] Vinyl resin particle dispersion X1 758 parts by mass Amorphous polyester resin particle dispersion A1 586 parts by mass Crystalline polyester resin particle dispersion C1 198 parts by mass Release agent dispersion W1 94 parts by weight Colorant dispersion P1 149 parts by weight Anionic surfactant (Dowfax2A1 20% aqueous solution) 40 parts by mass Ion-exchanged water 1500 parts by weight The above materials were placed in a 4-liter reaction vessel equipped with a thermometer, pH meter, and stirrer, and 1.0% nitric acid was added at 25°C to adjust the pH to 3.0. Then, 100 parts by mass of a 2% aluminum sulfate (flocculant) aqueous solution was added over 30 minutes while dispersing at 3000 rpm with a homogenizer (IKA Ultra Turrax (registered trademark) T50). After the dropwise addition, the mixture was stirred for 10 minutes to thoroughly mix the raw materials and flocculant. After that, a stirrer and mantle heater were installed in the reaction vessel, and while adjusting the rotation speed of the stirrer so that the slurry was sufficiently stirred, the temperature was increased at a rate of 0.2°C / min up to 40°C, and at a rate of 0.05°C / min after exceeding 40°C, and the particle size was measured every 10 minutes using a Coulter Multisizer 3 (aperture diameter 100μm, manufactured by Beckman Coulter, Inc.). When the volume-based median diameter reached 6.0μm, the temperature was maintained, and a mixture of the following additional raw materials, which had been mixed in advance, was added over a period of 20 minutes. Shell resin particle dispersion S1 198 parts by weight Anionic surfactant (Dowfax2A1 20% aqueous solution) 15 parts by mass Next, after maintaining at 50°C for 30 minutes, 8 parts by mass of 20% EDTA (ethylenediaminetetraacetic acid) solution was added to the reaction vessel, and then 1 mol / L aqueous sodium hydroxide solution was added to control the pH of the raw material dispersion at 9.0. Thereafter, the temperature was increased to 85°C at a rate of 1°C / min while adjusting the pH to 9.0 every 5°C, and the temperature was maintained at 85°C.
[0162] ≪Cooling process≫ Thereafter, when the shape factor measured using "FPIA-3000" reached 0.960, the solution was cooled to 30° C. at a temperature drop rate of 10° C. / min to obtain a dispersion of toner base particles B3.
[0163] <Filtering, washing and drying processes> The particles were then separated from the cooled dispersion and dehydrated, and the resulting cake was washed by repeating redispersion in ion-exchanged water and solid-liquid separation three times, and then dried at room temperature until the toner moisture content was less than 2%, and then dried at 35° C. until the toner moisture content was less than 1%, to obtain toner base particles B3.
[0164] [Preparation of toner base particles B14] Toner base particles B14 were prepared in the same manner as toner base particles B3, except that the initial raw materials used in the preparation of toner base particles B3 were changed as follows. Vinyl resin particle dispersion X1 948 parts by mass Amorphous polyester resin particle dispersion A1 423 parts by mass Crystalline polyester resin particle dispersion C1 198 parts by mass Release agent dispersion W1 67 parts by weight Colorant dispersion P1 49 parts by weight Anionic surfactant (Dowfax2A1 20% aqueous solution) 40 parts by mass Ion-exchanged water 1500 parts by weight
[0165] [Production of toner base particles B18] Toner base particles B18 were prepared in the same manner as toner base particles B3, except that the initial raw materials were changed as follows: Amorphous polyester resin particle dispersion A1 1240 parts by mass Crystalline polyester resin particle dispersion C1 198 parts by mass Release agent dispersion W1 198 parts by weight Colorant dispersion P1 148 parts by weight Anionic surfactant (Dowfax2A1 20% aqueous solution) 40 parts by mass Ion-exchanged water 1500 parts by weight
[0166] [Table 4]
[0167] [Production of Toner 1] ≪External addition process≫ To 100 parts by mass of toner base particles B1, 0.7 parts by mass of hydrophobic silica (number average primary particle diameter = 12 nm, hydrophobicity = 68), 1.0 part by mass of strontium titanate (1) (number average particle diameter = 40 nm), and 0.7 parts by mass of strontium titanate (2) (number average particle diameter = 1000 nm) were added, and these were mixed for 20 minutes at 32 ° C. with a rotor blade peripheral speed of 35 mm / sec using a "Henschel Mixer" (manufactured by Nippon Coke & Engineering Co., Ltd.), and then coarse particles were removed using a sieve with 45 μm openings. By carrying out such external additive treatment, toner 1, which is an aggregate of toner particles 1 for electrostatic charge image development, was produced.
[0168] [Manufacture of developer 1] Toner 1 and an acrylic resin-coated ferrite carrier having a volume average particle size of 32 μm were added and mixed so that the toner particle concentration was 6.5 mass %. In this way, developer 1, which is a two-component developer containing toner 1, was produced.
[0169] [Production of toner 2-19] Toners 2 to 19 were produced in the same manner as in the production of toner 1, except that toner base particle B1 was changed to toner base particle B2 to B19, respectively.
[0170] [Manufacture of developers 2 to 19] Developers 2 to 19 were produced in the same manner as in the production of developer 1, except that toner 1 was changed to toners 2 to 19, respectively.
[0171] [evaluation] <Low temperature fixability> The low temperature fixing properties of the toners 1 to 19 were evaluated using the developers 1 to 19, respectively. Specific results are as follows. The fixing device of the multifunction printer "bizhub PRESS (registered trademark) C1070" (manufactured by Konica Minolta, Inc.) was modified to be able to change the surface temperatures of the upper fixing belt and the lower fixing roller, and two-component developers were loaded in sequence. The above device was also modified to be able to freely set the fixing temperature, toner adhesion amount, and system speed. Under normal temperature and humidity conditions (temperature 20°C, humidity 50% RH), A4 size Mondi Color Copy 90g / m 2 (Mondi) unfixed solid image (adhesion amount 11.3 g / m 2 ) was formed. Next, in the heating roller of the fixing device, the nip width was set to 11.2 mm, the fixing time was set to 50 msec, the fixing pressure was set to 135 kPa, and the surface temperature was set to 100°C, and fixing was performed while changing the surface temperature of the heating roller in 1°C increments in the range of 110 to 160°C. The lowest fixing temperature at which image staining due to fixing offset was not visually confirmed was taken as the minimum fixing temperature, and was ranked according to the following evaluation criteria. Rank 2 or higher was considered to be acceptable. (Evaluation Criteria) Rank 5: Minimum fixing temperature is less than 125℃ Rank 4: Minimum fixing temperature is 125℃ or higher and less than 130℃ Rank 3: Minimum fixing temperature is 130℃ or higher and less than 135℃ Rank 2: Minimum fixing temperature is 135℃ or higher and less than 140℃ Rank 1: Minimum fixing temperature is 140℃ or higher
[0172] <Tacking resistance> The tackiness resistance of the toners 1 to 19 was evaluated using the developers 1 to 19, respectively. Specific results are as follows. A multifunction printer "bizhub PRESS (registered trademark) C1070" (manufactured by Konica Minolta, Inc.) was used that had been modified to allow the fixing temperature of the upper fixing belt and lower fixing roller, the amount of toner attached, the system speed, and the paper discharge air strength to be changed, and two-component developers were loaded in sequence. 2 )" (Oji Paper Co., Ltd.), a solid image with an image ratio of 70% (adhesion amount 11.3 g / m 2 ) was continuously printed on 1000 sheets at a fixing temperature of 170° C. The 1000 printed sheets were output onto the same output tray, and left in a stacked state for 5 hours to cool in air. Thereafter, the adhesive strength of the fixed images on the 400th and 401st sheets, the 500th and 501st sheets, and the 600th and 601st sheets, which are prone to image defects in terms of latent heat and pressure, was evaluated. First, the 400th and 401st fixed images were carefully removed. A glass plate was placed on a flat table, and the above fixed images were gently placed on top of it. The lower fixed image and the glass plate were fixed with vinyl tape so that the lower fixed image would not move. A tape connected to a spring scale was attached to the tip of the upper fixed image, and the spring scale was slowly slid horizontally at a constant speed, and the force required to slide the fixed images was measured with the spring scale. This measurement was also carried out for the 500th and 501st, 600th and 601st images in the same manner, and the average value of the force indicated by the spring balance was taken as the adhesion force. Rank 2 or higher was considered to be a pass. (Evaluation Criteria) Rank 5: Adhesive force less than 1.0N Rank 4: Adhesive force less than 2.0N Rank 3: Adhesive force less than 3.0N Rank 2: Adhesive strength less than 4.0N Rank 1: Adhesive strength of 4.0N or more
[0173] <Heat-resistant storage> The tackiness resistance of the toners 1 to 19 was evaluated using the developers 1 to 19, respectively. Specific results are as follows. 0.5 g of the toner was placed in a 10 mL glass bottle having an inner diameter of 21 mm, the bottle was capped, and the 0.5 g of the toner was shaken 600 times at room temperature using a shaker "Tap Denser KYT-2000" (manufactured by Seishin Enterprise Co., Ltd.). Thereafter, with the lid removed, the container was left to stand for 2 hours in an environment of a temperature of 55° C. and a humidity of 35% RH. Next, the toner was carefully placed on a 48 mesh (350 μm mesh) sieve so as not to break up the toner aggregates, and set in a "Powder Tester" (manufactured by Hosokawa Micron Corporation). The sieve was fixed with a presser bar and a knob nut, and vibration was applied for 10 seconds with the vibration intensity adjusted to provide a feed width of 1 mm. The ratio (mass%) of the toner amount remaining on the sieve was then measured, and the toner aggregation rate was calculated using the following formula. Toner cohesion rate (mass%) = (mass of toner remaining on sieve (g) / 0.5 (g)) x 100 The above test was repeated while increasing the test temperature by 0.1°C at a time, keeping the humidity at 35% RH, until the toner cohesion rate exceeded 50% by mass. The maximum test temperature at which the toner cohesion rate did not exceed 50% by mass (limit heat-resistant storage temperature) was used as an index of heat-resistant storage property. Rank 2 or higher was considered to be acceptable. (Evaluation Criteria) Rank 5: Heat-resistant storage temperature limit is 60°C or higher Rank 4: Heat-resistant storage temperature limit is 59°C or higher and less than 60°C Rank 3: Heat-resistant storage temperature limit is 58°C or higher and less than 59°C Rank 2: Heat-resistant storage temperature limit is 57℃ or higher but less than 58℃ Rank 1: Heat-resistant storage temperature limit is less than 57°C
[0174] [Table 5]
[0175] As shown by the above results, it is recognized that the toner of the present invention is superior in low-temperature fixing property, can suppress tackiness, and has excellent heat-resistant storage property, as compared with the toner of the comparative example.
Claims
1. A toner for developing an electrostatic image, comprising at least a binder resin and a release agent, The binder resin contains at least a crystalline polyester resin and an amorphous vinyl resin, the crystalline polyester resin has a portion having a crystalline structure and a crystallization-promoting portion, The content of the amorphous vinyl resin in the binder resin is 40% by mass or more relative to the binder resin, and The release agent contains at least a fatty acid ester wax and a linear hydrocarbon wax, The heat generation amount of the exothermic peak during cooling of the electrostatic image developing toner measured by differential scanning calorimetry is defined as ΔHc (J / g), and the heat generation amount from the crystallization onset temperature to 68° C. at the exothermic peak is defined as ΔHc(Hi) (J / g), A toner for developing electrostatic images, characterized in that, when the endothermic heat of the endothermic peak derived from a crystalline substance during the first temperature rise measured by differential scanning calorimetry is ΔH1 (J / g) and the endothermic heat of the endothermic peak during the second temperature rise is ΔH2 (J / g), the toner satisfies the following formulas (1) and (2). Formula (1): ΔHc(Hi) / ΔHc≧0.60 Formula (2): 0.65≦ΔH2 / ΔH1≦0.95 (In the differential scanning calorimetry, during the first and second temperature rises, the temperature is raised from 0° C. to 150° C. at a temperature rise rate of 10° C. / min and held at 150° C. for 1 minute, and during temperature drop, the temperature is lowered from 150° C. to 0° C. at a temperature drop rate of 10° C. / min and held at 0° C. for 1 minute.)
2. 2. The toner for developing an electrostatic image according to claim 1, wherein the softening point of the toner for developing an electrostatic image is within a range of 90 to 105°C.
3. 3. The toner for developing electrostatic images according to claim 1, wherein a mass ratio of the fatty acid ester wax to the linear hydrocarbon wax is from 1:9 to 9:
1.
4. 4. The toner for developing electrostatic images according to claim 1, wherein the linear hydrocarbon wax contains a linear hydrocarbon wax having a crystallization temperature of 75[deg.] C. or higher.
5. 5. The toner for developing electrostatic images according to claim 1, wherein the linear hydrocarbon wax contains a Fischer-Tropsch wax.
6. The toner for developing electrostatic images according to any one of claims 1 to 5, characterized in that the crystalline polyester resin has a portion having a crystalline structure and a crystallization promoting portion, and the crystallization promoting portion is a portion derived from a compound selected from the group consisting of an aliphatic monocarboxylic acid having 10 to 30 carbon atoms or an aliphatic monoalcohol having 10 to 30 carbon atoms.
7. 7. The toner for developing electrostatic images according to claim 6, wherein the portion having the crystal structure of the crystalline polyester resin contains a hybrid crystalline polyester resin formed by chemically bonding a crystalline polyester polymer segment and a vinyl resin polymer segment.
8. 8. The toner for developing electrostatic images according to claim 1, wherein the content of the amorphous vinyl resin in the binder resin is 50% by mass or more.
Citation Information
Patent Citations
Toner for electrostatic charge image development and heat-fixing method
JP1993197192A
toner
JP2015045850A
Electrostatic latent image developing toner and method for manufacturing the same
JP2018087901A