Thermoelectric conversion materials and thermoelectric conversion elements

A carbon nanotube-based thermoelectric conversion material with a cycloaliphatic hydrocarbon tackifier addresses the limitations of inorganic materials by providing high performance and stability, enabling flexible and efficient energy conversion.

JP7559428B2Active Publication Date: 2024-10-02TOYO INK MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020141057
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-24
Publication Date
2024-10-02
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Thermoelectric conversion materials using inorganic materials face challenges such as high cost, complexity in manufacturing, poor workability, rigidity, and difficulty in forming flexible shapes due to their composition, which limits their widespread application.

Method used

A thermoelectric conversion material comprising a conductive material with a carbon nanotube and a tackifier having a cycloaliphatic hydrocarbon structure, optimized in specific proportions, enhances both thermoelectric performance and stability under high temperature and humidity conditions.

Benefits of technology

The material achieves high thermoelectric conversion performance and stability under harsh conditions, offering flexibility and reduced manufacturing complexity, making it suitable for diverse applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559428000001
    Figure 0007559428000001
Patent Text Reader

Abstract

To provide a thermoelectric conversion material that can achieve both thermoelectric conversion performance and stability under high temperature and high humidity.SOLUTION: A thermoelectric conversion material contains a conductive material (A) and an adhesive agent (B) having a cyclic aliphatic hydrocarbon structure. Preferably, the conductive material (A) contains a carbon material and the amount of the adhesive agent (B) having a cyclic aliphatic hydrocarbon structure is 1 to 200 pts.mass per 100 pts.mass of the conductive material (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric conversion material and a thermoelectric conversion element. [Background technology]

[0002] Thermoelectric conversion technology, which converts heat into electricity using thermoelectric conversion materials, has been attracting attention as a clean energy source that can effectively utilize minute thermal energy such as body heat and exhaust heat from factories, cars, and homes, as well as various types of heat in nature, as electricity. There are various thermoelectric effects that are used in thermoelectric conversion technology, but the mainstream system uses the Seebeck effect, in which an electromotive force is generated by an electron gradient that occurs within a material in response to the temperature difference when two different temperatures are applied to both ends of the material, which is made up of a combination of semiconductors and metals.

[0003] Thermoelectric materials that can convert thermal energy to electrical energy and vice versa are used in thermoelectric conversion elements such as thermoelectric power generation elements and Peltier elements. Thermoelectric conversion elements are elements that convert heat into electrical power and are made up of a combination of semiconductors and metals. Representative thermoelectric conversion elements are classified into p-type semiconductors alone, n-type semiconductors alone, and combinations of p-type and n-type semiconductors. To obtain a larger potential difference, thermoelectric conversion elements generally use a combination of p-type and n-type semiconductors as materials.

[0004] Thermoelectric conversion elements, such as Peltier elements, are used as thermoelectric modules that are made by combining a number of elements in a plate or cylinder shape. Since they can directly convert thermal energy into electricity, they can be used, for example, as a power source for wristwatches that are powered by body heat, and for power generation on the ground and in artificial satellites. The performance of a thermoelectric conversion element depends on the performance of the thermoelectric conversion material, etc.

[0005] As described in Non-Patent Document 1, the dimensionless thermoelectric figure of merit ZT is used as an index representing the performance of a thermoelectric conversion material. In addition, the power factor PF (=S 2 ·σ) may also be used. The dimensionless thermoelectric figure of merit ZT is expressed by the following formula (1). ZT=((S 2 ·σ) / к)·T Equation (1) Here, S is the Seebeck coefficient (V / K), σ is the electrical conductivity (S / m), T is the absolute temperature (K), and κ is the thermal conductivity (W / (m K)). Thermal conductivity κ is expressed by the following formula (2). к=α·ρ·C Equation (2) where α is the thermal diffusivity (m 2 / s), ρ is density (kg / m 3 ), and C is the specific heat capacity (J / (kg K)). That is, in order to improve the thermoelectric conversion performance (hereinafter also referred to as thermoelectric properties), it is important to improve the Seebeck coefficient or electrical conductivity while decreasing the thermal conductivity.

[0006] Representative thermoelectric conversion materials include inorganic materials such as bismuth-tellurium (Bi-Te) for temperatures from room temperature to 500 K, lead-tellurium (Pb-Te) for temperatures from room temperature to 800 K, and silicon-germanium (Si-Ge) for temperatures from room temperature to 1000 K.

[0007] However, thermoelectric conversion materials containing these inorganic materials often contain rare elements and are expensive, or may contain harmful substances. In addition, inorganic materials are poorly processable, making the manufacturing process complicated. Therefore, thermoelectric conversion materials containing inorganic materials require high manufacturing energy and manufacturing costs, making it difficult to generalize them. Furthermore, since thermoelectric conversion materials containing inorganic materials are rigid, it is difficult to process them into shapes that are not flat or to manufacture thermoelectric conversion elements that have flexibility. In addition, thermoelectric conversion materials containing inorganic materials generally have a high specific gravity, which makes them prone to becoming heavy, which is also a problem.

[0008] In response to this, research is being conducted into thermoelectric conversion elements that use organic materials instead of conventional inorganic materials. Organic materials are lightweight, have excellent moldability, and are more flexible than inorganic materials, so they are versatile within the temperature range in which they do not decompose. In addition, because organic materials can be manufactured using printing technology, they are more advantageous than inorganic materials in terms of manufacturing energy and costs.

[0009] For example, Patent Document 1 discloses a thermoelectric conversion material containing a polymer dispersant having an organic dye skeleton and carbon nanotubes (CNTs) and a thermoelectric conversion element using the same. However, the thermoelectric conversion element disclosed in the invention of Patent Document 1 does not have sufficient thermoelectric conversion performance and has a problem of lacking stability under high temperature and high humidity conditions. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2015 / 050113 [Non-patent literature]

[0011] [Non-Patent Document 1] Takenobu Kajikawa, "Thermoelectric Conversion Technology Handbook (First Edition)", NTS Publishing, p. 19 Summary of the Invention [Problem to be solved by the invention]

[0012] An object of the present invention is to provide a thermoelectric conversion material that can achieve both thermoelectric conversion performance and stability under high temperature and high humidity conditions. [Means for solving the problem]

[0013] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to a thermoelectric conversion material comprising a conductive material (A) and a tackifier (B) having a cyclic aliphatic hydrocarbon structure.

[0014] The present invention also relates to the above thermoelectric conversion material, wherein the conductive material (A) comprises a carbon material.

[0015] The present invention also relates to the above thermoelectric conversion material, wherein the content of the tackifier (B) having a cyclic aliphatic hydrocarbon structure is from 1 part by mass to 200 parts by mass per 100 parts by mass of the conductive material (A).

[0016] The present invention also relates to a thermoelectric conversion element having a thermoelectric conversion film containing the above-mentioned thermoelectric conversion material and electrodes, in which the thermoelectric conversion film and the electrodes are electrically connected to each other. Effect of the Invention

[0017] The present invention makes it possible to provide a thermoelectric conversion material that is capable of achieving both thermoelectric conversion performance and stability under high temperature and high humidity conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] <Conductive material (A)> Conductive material (A) refers to a material that conducts electricity. The conductive material (A) is not particularly limited as long as it is a material having electrical conductivity (carbon material, metal material, conductive polymer, etc.), and examples of the carbon material include graphite, carbon nanotubes, carbon black, graphene (including graphene nanoplates), etc. Examples of the metal material include metals such as gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, silicon, aluminum, tungsten, molybdenum, germanium, gallium, and platinum. Examples of the metal material include alloys of these metals, and metal-containing particles in which a core material is coated with a material different from the core material, such as silver-coated copper powder particles in which the core material is copper and the surface is coated with silver. Examples of the metal oxide include metal oxides such as silver oxide, indium oxide, tin oxide, zinc oxide, ruthenium oxide, ITO (tin-doped indium oxide), AZO (aluminum-doped zinc oxide), and GZO (gallium-doped zinc oxide), and metal compounds other than metal oxides such as ZnSe, CdS, InP, GaN, SiC, and SiGe. Examples of conductive polymers include PEDOT / PSS (a composite of poly(3,4-ethylenedioxythiophene) and polystyrenesulfonic acid), polyaniline, polyacetylene, polypyrrole, polythiophene, and polyparaphenylene.

[0019] Graphite includes flaky graphite such as CMX, UP-5, UP-10, UP-20, UP-35N, CSSP, CSPE, CSP, CP, CB-150, CB-100, ACP, ACP-1000, ACB-50, ACB-100, ACB-150, SP-10, SP-20, J-SP, SP-270, HOP, GR-60, LEP, F#1, F#2, manufactured by Nippon Graphite Industries Co., Ltd. Examples of the graphite include F#3, BF-3AK, FBF, BF-15AK, CBR, CPB-6S, CPB-3, 96L, 96L-3, K-3, SC-120, SC-60, HLP, CP-150, and SB-1 manufactured by Chuetsu Graphite Industry Co., Ltd., EC1500, EC1000, EC500, EC300, EC100, and EC50 manufactured by Ito Graphite Industry Co., Ltd., and 10099M and PB-99 manufactured by Nishimura Graphite Co., Ltd. Examples of the spherical natural graphite include CGC-20, CGC-50, CGB-20, and CGB-50 manufactured by Nippon Graphite Industry Co., Ltd. Examples of the amorphous graphite include Ao-P, AP, AOP, and P#1 manufactured by Nippon Graphite Industry Co., Ltd., and APR, K-5, AP-2000, AP-6, 300F, and 150F manufactured by Chuetsu Graphite Co., Ltd. Examples of artificial graphite include PAG-60, PAG-80, PAG-120, PAG-5, HAG-10W, and HAG-150 manufactured by Nippon Graphite Industries Co., Ltd.; G-4AK, G-6S, G-3G-150, G-30, G-80, G-50, SMF, EMF, SFF, SFF-80B, SS-100, BSP-15AK, BSP-100AK, and WF-15C manufactured by Chuetsu Graphite Co., Ltd.; and SGP-100, SGP-50, SGP-25, SGP-15, SGP-5, SGP-1, SGO-100, SGO-50, SGO-25, SGO-15, SGO-5, SGO-1, SGX-100, SGX-50, SGX-25, SGX-15, SGX-5, and SGX-1 manufactured by SEC Carbon Co., Ltd.

[0020] Examples of conductive carbon fibers and carbon nanotubes include vapor grown carbon fibers such as VGCF manufactured by Showa Denko K.K.; single-walled carbon nanotubes such as EC1.5 and EC1.5-P manufactured by Meijo Nano Carbon Co., Ltd., TUBALL manufactured by OCSiAl Corporation, and ZEONANO manufactured by Zeon Nano Technology Inc.; FloTube9000, FloTube7000, and FloTube2000 manufactured by CNano Corporation; NC7000 manufactured by Nanocyl Corporation; and 100T and 200P manufactured by Knano Corporation.

[0021] Carbon black includes Tokai Carbon's Toka Black #4300, #4400, #4500, and #5500, Degussa's Printex L, and Colombian's Raven 7000, 5750, 5250, 5000ULTRAIII, 5000ULTRA, Conductex SC ULTRA, and Conductex 975. Examples of furnace blacks include ULTRA, PUERBLACK 100, 115, and 205; #2350, #2400B, #2600B, #3050B, #3030B, #3230B, #3350B, #3400B, and #5400B manufactured by Mitsubishi Chemical Corporation; MONARCH 1400, 1300, 900, Vulcan XC-72R, and Black Pearls 2000 manufactured by Cabot Corporation; Ensaco 250G, Ensaco 260G, Ensaco 350G, and Super P-Li manufactured by TIMCAL Corporation; Ketjen blacks such as EC-300J and EC-600JD manufactured by Lion Corporation; and acetylene blacks such as Denka Black, Denka Black HS-100, and FX-35 manufactured by Denki Kagaku Kogyo Co., Ltd.

[0022] Of the above-mentioned conductive materials (A), from the viewpoint of achieving both a Seebeck coefficient and electrical conductivity, the conductive material (A) preferably comprises a carbon material. The carbon material preferably comprises carbon nanotubes, carbon black, and graphene, and more preferably comprises carbon nanotubes. The carbon nanotubes preferably comprise single-walled carbon nanotubes.

[0023] The shape of the conductive material (A) is not particularly limited, and may be amorphous, aggregated, scaly, microcrystalline, spherical, flake, wire, etc. The conductive material (A) may be one type or may contain two or more types.

[0024] <Tackifier (B) Having a Cyclic Aliphatic Hydrocarbon Structure> The tackifier (B) having a cyclic aliphatic hydrocarbon structure (hereinafter sometimes abbreviated as tackifier (B)) is not particularly limited as long as it is a tackifier containing a cyclic aliphatic hydrocarbon structure, and examples thereof include petroleum resins such as aromatic modified rosin resins, aromatic modified terpene resins, C5 petroleum resins, C9 petroleum resins, and C5C9 petroleum resins. Further examples include hydrogenated petroleum resins in which the unsaturated bonds and aromatic rings of these petroleum resins are hydrogenated. Examples of hydrogenated petroleum resins include partially hydrogenated petroleum resins in which some of the unsaturated bonds and aromatic rings of the petroleum resins are hydrogenated, and fully hydrogenated petroleum resins in which the unsaturated bonds and aromatic rings of the petroleum resins are all hydrogenated and have no unsaturated bonds. Among the above tackifiers (B), C5 petroleum resins, C9 petroleum resins, and C5C9 petroleum resins, as well as these hydrogenated petroleum resins, are preferred.

[0025] Furthermore, tackifiers are often referred to as "tackifiers", and therefore, among tackifiers, those having a cyclic aliphatic hydrocarbon structure are also included in the tackifier (B).

[0026] C5 petroleum resin refers to petroleum resin made from the C5 fraction of petroleum (naphtha), C9 petroleum resin refers to petroleum resin made from the C9 fraction of petroleum, and C5C9 petroleum resin refers to petroleum resin made from the C5 and C9 fractions of petroleum. Examples of C5 fractions include isoprene, cyclopentadiene, pentane, etc. Examples of C9 fractions include styrene, vinyltoluene, indene, etc. Examples of C5C9 fractions include dicyclopentadiene (DCPD), which is a dimerization of cyclopentadiene, which is a type of C5 fraction. For example, C5 petroleum resin may be a copolymer of an olefin and a diolefin from a C5 fraction. The same applies to C9 petroleum resin and C5C9 petroleum resin.

[0027] Examples of commercially available tackifiers (B) include Clearon K110 and YS Polystar UH115 manufactured by Yasuhara Chemical Co., Ltd., Escorez 5300 and Escorez 5600 manufactured by Exxon Corporation, Quintone 1325 and Quintone 1345 manufactured by Zeon Corporation, Alcon P-90, Alcon P-100, Alcon P-125, Alcon P-140, Alcon M-90, Alcon M-100, Alcon M-115, and Alcon M135 manufactured by Arakawa Chemical Industries Co., Ltd., and SUKOREZ SU-100, SUKOREZ SU-120, SUKOREZ SU-130, SUKOREZ SU-210, SUKOREZ SU-420, SUKOREZ SU-500, and SUKOREZ SU-135 manufactured by KOLON Corporation. Examples of such antibacterial agents include SU-640, and Idemitsu Kosan's Imave S-100, Imave S-110, Imave P-100, and Imave P125.

[0028] The hydrogenation rate of the tackifier (B) is preferably 20% or more, more preferably 35% or more, and even more preferably 50% or more, from the viewpoint of weather resistance.

[0029] The softening point of the tackifier (B) is preferably 80° C. or higher, more preferably 90° C. or higher, and particularly preferably 100° C. or higher, in terms of providing even better thermal stability. Also, in terms of maintaining the flexibility of the thermoelectric conversion film, the softening point is preferably 200° C. or lower. In this specification, the softening point of the tackifier resin is a value measured by the ring and ball method in accordance with JIS K2207.

[0030] The weight average molecular weight (Mw) of the tackifier (B) having a cyclic aliphatic hydrocarbon structure is preferably from 100 to 200,000, more preferably from 200 to 20,000, and even more preferably from 300 to 5,000.

[0031] The content of the tackifier (B) having a cyclic aliphatic hydrocarbon structure is preferably 1 part by mass or more and 200 parts by mass or less, more preferably 10 parts by mass or more and 200 parts by mass or less, and particularly preferably 20 parts by mass or more and 200 parts by mass or less, per 100 parts by mass of the conductive material (A).

[0032] (solvent) The solvent can be used as a medium when mixing the conductive material (A) and the tackifier (B). The solvent that can be used is not particularly limited as long as it can dissolve or disperse the conductive material (A) and the tackifier (B), and examples of the solvent that can be used include organic solvents and water, and two or more of them may be used in combination. Examples of organic solvents include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol methyl ether, diethylene glycol methyl ether, terpineol, dihydroterpineol, 2,4-diethyl-1,5-pentanediol, 1,3-butylene glycol, isobornylcyclohexanol, ethylene glycol, 1,3-propanediol, 1,4-butanediol, diethylene glycol, triethylene glycol, glycerin, polyethylene glycol, polypropylene glycol, trifluoroethanol, m-cresol, and thiodiglycol, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, ethers such as tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether, hydrocarbons such as hexane, heptane, and octane, aromatics such as benzene, toluene, xylene, and cumene, esters such as ethyl acetate and butyl acetate, and N-methylpyrrolidone. These can be appropriately selected as needed. The solvent is preferably N-methylpyrrolidone.

[0033] The thermoelectric conversion material of the present invention preferably contains an inorganic base, an inorganic metal salt, or an organic base. This improves dispersibility when the conductive material (A) and the tackifier (B) are mixed. The inorganic base and inorganic metal salt preferably contain an alkali metal or an alkaline earth metal. For example, chlorides, hydroxides, carbonates, nitrates, sulfates, phosphates, tungstates, vanadates, molybdates, niobates, borates, etc. of alkali metals or alkaline earth metals are included. Among these, chlorides, hydroxides, and carbonates of alkali metals and alkaline earth metals are preferred in terms of being able to easily supply cations.

[0034] Examples of the hydroxides of alkali metals include lithium hydroxide, sodium hydroxide, potassium hydroxide, etc. Examples of the hydroxides of alkaline earth metals include calcium hydroxide, magnesium hydroxide, etc. Examples of the carbonates of alkali metals include lithium carbonate, lithium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, potassium hydrogen carbonate, etc. Examples of the carbonates of alkaline earth metals include calcium carbonate, magnesium carbonate, etc. Among these, lithium hydroxide, sodium hydroxide, lithium carbonate, and sodium carbonate are preferred. The metal in the inorganic base or inorganic metal salt may be a transition metal.

[0035] Examples of the organic base include primary, secondary or tertiary alkylamines and compounds containing a basic nitrogen atom, as shown below. Examples of primary alkylamines include propylamine, butylamine, isobutylamine, octylamine, 2-ethylhexylamine, laurylamine, stearylamine, oleylamine, 2-aminoethanol, 3-aminopropanol, 3-ethoxypropylamine, and 3-lauryloxypropylamine. Examples of secondary alkylamines include dibutylamine, diisobutylamine, N-methylhexylamine, dioctylamine, distearylamine, and 2-methylaminoethanol.

[0036] Examples of the tertiary alkylamine include triethylamine, tributylamine, N,N-dimethylbutylamine, N,N-diisopropylethylamine, dimethyloctylamine, trioctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dilaurylmonomethylamine, triethanolamine, 2-(dimethylamino)ethanol, etc. The number of carbon atoms in the alkylamine is preferably 1 to 30, more preferably 1 to 20.

[0037] Further, examples of the organic base include compounds containing a basic nitrogen atom, such as 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), 1,5-diazabicyclo[4.3.0]nonene-5 (DBN), 1,4-diazabicyclo[2.2.2]octane (DABCO), tri-n-butylamine, dimethylbenzylamine, monoethanolamine, imidazole, 1-methylimidazole, tetramethylammonium hydroxide, and tetraethylammonium hydroxide.

[0038] The blending amount of the inorganic base, inorganic metal salt, and organic base is preferably 1 to 50 parts by mass per 100 parts by mass of the conductive material (A), which further improves dispersibility.

[0039] When producing a dispersion liquid containing a thermoelectric conversion material, for example, the thermoelectric conversion material, the solvent, and other components as necessary are mixed, and then the mixture is dispersed using a dispersing machine or ultrasonic waves. The dispersing machine is not particularly limited, and for example, a kneader, an attritor, a ball mill, a sand mill using glass beads or zirconia beads, a media dispersing machine such as a scandex, an Eiger mill, a paint conditioner, or a paint shaker, or a colloid mill can be used.

[0040] <Thermoelectric conversion element> The thermoelectric conversion element of the present invention has a thermoelectric conversion film containing the above-mentioned thermoelectric conversion material and electrodes, and the thermoelectric conversion film and the electrodes are electrically connected to each other. The thermoelectric conversion film is excellent in heat resistance and flexibility in addition to electrical conductivity and thermoelectric properties. Therefore, a high-quality thermoelectric conversion element can be easily produced.

[0041] The thermoelectric conversion film may be a film obtained by applying a thermoelectric conversion material onto a substrate. Since the thermoelectric conversion material has excellent moldability, it is easy to obtain a good film by the application method. A wet film formation method is mainly used for forming the thermoelectric conversion film. Specifically, a method using various means such as a spin coating method, a spray method, a roller coating method, a gravure coating method, a die coating method, a comma coating method, a roll coating method, a curtain coating method, a bar coating method, an inkjet method, a dispenser method, silk screen printing, and flexographic printing can be mentioned. The above methods can be appropriately selected according to the thickness to be applied and the viscosity of the material.

[0042] The thickness of the thermoelectric conversion film is not particularly limited, but it is preferable that the film has a certain thickness or more so that a temperature difference can be generated and transmitted in the thickness direction or surface direction of the thermoelectric conversion film, as described later. From the viewpoint of thermoelectric properties, the film thickness of the thermoelectric conversion film is preferably in the range of 0.1 to 500 μm, more preferably in the range of 1 to 300 μm, and further preferably in the range of 1 to 200 μm.

[0043] The material of the substrate is not particularly limited, and examples of the substrate that can be used include nonwoven fabric, paper, plastic films such as polyethylene, polyethylene terephthalate (PET), polyethylene naphthalate, polyethersulfone, polypropylene, polyimide, polycarbonate, and cellulose triacetate, and glass, etc. These substrates may have an aluminum deposition layer or a barrier layer on the substrate surface to prevent deterioration of the thermoelectric conversion material due to the effects of water and oxygen.

[0044] In order to improve the adhesion between the substrate and the thermoelectric conversion film, various treatments can be performed on the substrate surface. Specifically, prior to application of the thermoelectric conversion material, UV ozone treatment, corona treatment, plasma treatment, or adhesion enhancing treatment may be performed.

[0045] The thermoelectric conversion film may be laminated with a substrate, or may be a free-standing film without a substrate. When preparing a free-standing film, there is no particular limitation, but for example, the film can be obtained by forming the thermoelectric conversion film on a release sheet and then removing the release coat.

[0046] Examples of the release sheet include release-treated plastic films such as polyester film, polyethylene film, polypropylene film, and polyimide film.

[0047] The thermoelectric conversion element can be constructed by applying techniques well known in the art, except that it is constructed using the above-mentioned thermoelectric conversion material. A more specific configuration of the thermoelectric conversion element and a manufacturing method thereof will be described below.

[0048] In the thermoelectric conversion element, the thermoelectric conversion film and the electrodes are electrically connected. Here, "electrically connected" means that they are joined to each other or can be electrically connected via other components such as wires.

[0049] The material of the electrode is not particularly limited as long as it functions as an electrode, and can be selected from metals, alloys, semiconductors, etc. In one embodiment, a metal or alloy is preferred because it has a high electrical conductivity and a low contact resistance of the thermoelectric conversion film. For example, it is preferred that the material contains at least one selected from the group consisting of gold, silver, copper, platinum, nickel, and aluminum, and more preferably contains silver.

[0050] The method for forming the electrodes is not particularly limited, and the electrodes can be formed by a method such as vacuum deposition, thermocompression bonding of an electrode material foil or a film having an electrode material film, application of a paste in which fine particles of the electrode material are dispersed, etc. From the viewpoint of process simplicity, a method using thermocompression bonding of an electrode material foil or a film having an electrode material film, or application of a paste in which the electrode material is dispersed is preferred.

[0051] Typical examples of the structure of a thermoelectric conversion element can be broadly classified into (1) a structure in which electrodes are formed on both ends of the thermoelectric conversion film of the present invention, and (2) a structure in which the thermoelectric conversion film of the present invention is sandwiched between two electrodes, based on the positional relationship between the thermoelectric conversion film and a pair of electrodes. The thermoelectric conversion element having the structure (1) above can be obtained, for example, by forming a thermoelectric conversion film on a substrate, and then applying silver paste to both ends of the film to form first and second electrodes. In a thermoelectric conversion element in which electrodes are formed on both ends of the thermoelectric conversion film in this way, it is easy to increase the distance between the two electrodes. Therefore, it is easy to generate a large temperature difference between the two electrodes and perform efficient thermoelectric conversion.

[0052] The thermoelectric conversion element having the structure of (2) above can be obtained, for example, by applying silver paste onto a substrate to form a first electrode, forming the thermoelectric conversion film of the present invention thereon, and further applying silver paste onto the first electrode to form a second electrode. In this way, a thermoelectric conversion element having the thermoelectric conversion film of the present invention sandwiched between two electrodes can utilize the temperature difference in the film thickness direction of the thermoelectric conversion film, that is, in the direction perpendicular to the substrate, and can be used in a form attached to a heat source. Therefore, it is preferable because it has the advantage of being able to extract heat from a wide range from the heat source. In the thermoelectric conversion element having the structure of (2) above, it is also possible to ensure a temperature difference by increasing the film thickness to widen the distance between the two electrodes.

[0053] Thermoelectric conversion elements can generate a high voltage by connecting them in series, and can generate a large current by connecting them in parallel. The thermoelectric conversion element may be one in which two or more thermoelectric conversion elements are connected. According to the present invention, since the thermoelectric conversion element has excellent flexibility, it can be well installed so as to conform to a heat source having a shape that is not flat.

[0054] The thermoelectric conversion element may have a heat absorption layer or a heat storage layer for efficient heat transfer from a heat source, and may also have a heat insulation layer or a heat dissipation layer for ensuring a temperature difference. Furthermore, depending on the application and the amount of power required, the extracted electricity can be boosted using a boost circuit, or the extracted electric energy can be temporarily stored in a condenser, a capacitor, a secondary battery, or the like for use. EXAMPLES

[0055] The present invention will be described in more detail below with reference to experimental examples, but the present invention is not limited thereto. In the examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". In addition, "NMP" refers to N-methylpyrrolidone.

[0056] <Production of Dispersion Containing Thermoelectric Conversion Material> [Example 1] (Dispersion 1) 0.3 parts of SU-100 (tackifier resin "SUKOREZ SU-100" manufactured by KOLON) as tackifier (B), 0.4 parts of SWCNT (single-walled carbon nanotube "TUBALL" manufactured by OCSiAl) as conductive material (A), 0.03 parts of sodium hydroxide as inorganic base, and 79.3 parts of NMP as solvent were weighed and mixed. Beads were further added and the mixture was shaken with Scandex for 4 hours, after which the beads were removed by filtration to obtain dispersion liquid 1 of thermoelectric conversion material.

[0057] [Examples 2 to 17, Comparative Example 1] (Dispersion 2~17, 101) Dispersions 2 to 17 of thermoelectric conversion material were obtained in the same manner as in Dispersion 1, except that the types and amounts of materials were changed as shown in Table 1. Dispersion 101 was obtained by weighing and mixing 0.4 parts of SWCNT (single-walled carbon nanotubes "TUBALL" manufactured by OCSiAl) as the conductive material (A), 0.03 parts of sodium hydroxide as the inorganic base, and 79.3 parts of NMP as the solvent, and then adding beads. The mixture was shaken with a Scandex for 4 hours, and then filtered to remove the beads, thereby obtaining Dispersion 101 of thermoelectric conversion material.

[0058] The abbreviations for the materials listed in Table 1 are as follows. (Conductive material (A)) A1: OCSiAl's single-walled carbon nanotube "TUBALL" A2: Multi-walled carbon nanotubes "Knanos100P" manufactured by Kumho Petrochemical Co., Ltd. A3: Graphene nanoplatelets "xGNP M5" manufactured by XG Sciences

[0059] (Tackifier (B) Having a Cycloaliphatic Hydrocarbon Structure) B1: KOLON tackifier resin "SUKOREZ SU-100" (softening point 105°C, hydrogenated petroleum resin including C5 petroleum resin, Mw400) B2: Tackifying resin "SUKOREZ SU-210" manufactured by KOLON (softening point 110°C, hydrogenated petroleum resin including C5 petroleum resin, Mw620) B3: KOLON tackifier resin "SUKOREZ SU-420" (softening point 120°C, hydrogenated petroleum resin containing C5 petroleum resin and C9 petroleum resin, Mw680) B4: KOLON tackifier resin "SUKOREZ SU-640" (softening point 136°C, hydrogenated petroleum resin including C5 petroleum resin, Mw550) B5: Arakawa Chemical Industries Co., Ltd. tackifier resin "Alcon P-125" (softening point 125°C, hydrogenated petroleum resin including C9 petroleum resin, Mw 700-900) B6: Arakawa Chemical Industries Co., Ltd. tackifier resin "Arcon P-140" (softening point 140°C, hydrogenated petroleum resin including C9 petroleum resin, Mw900) B7: Arakawa Chemical Industries Co., Ltd. tackifier resin "Alcon M-135" (softening point 135°C, partially hydrogenated petroleum resin including C9 petroleum resin, Mw 700-900)

[0060] <Evaluation of Thermoelectric Conversion Materials> The obtained dispersions 1 to 17 and 101 were each applied to a 75 μm thick PET film, which was a sheet-like substrate, using an applicator, and then dried at 120° C. for 30 minutes to obtain a laminate having a thermoelectric conversion film with a thickness of 2 μm. The Seebeck coefficient, which is one of the characteristics that indicate thermoelectric conversion performance, and the stability under high temperature and high humidity were evaluated for the laminate having the obtained thermoelectric conversion film (hereinafter also referred to as coating film) according to the following method. The results are shown in Table 1.

[0061] (Seebeck coefficient) The obtained laminate was cut into a size of 25 mm × 50 mm, and the Seebeck coefficient (μV / K) at 80° C. was measured using a ZEM-3LW manufactured by Advance Riko Co., Ltd. Table 1 shows the relative absolute values ​​of the Seebeck coefficient of each laminate to Comparative Example 1, where the absolute value of the Seebeck coefficient of Comparative Example 1 was set to 1.0.

[0062] (stability) The laminate immediately after preparation was left to stand for one day under conditions of 85°C and 85% humidity, and then the Seebeck coefficient was measured. The rate of change in the Seebeck coefficient relative to the Seebeck coefficient of the laminate immediately after preparation (the absolute value of the Seebeck coefficient listed in Table 1) was determined and evaluated based on the following criteria. A: The change in the Seebeck coefficient is within 10%. (Very good) B: The rate of change in the Seebeck coefficient is greater than 10% and less than 20% (good). C: The rate of change in the Seebeck coefficient is greater than 20% and less than 50%. (Usable) D: The change in the Seebeck coefficient is greater than 50% (poor).

[0063] As shown in Table 1, the thermoelectric conversion material of the present invention exhibited a high Seebeck coefficient. Furthermore, it was confirmed that the material had high stability under high temperature and high humidity conditions (85°C, 85%). This is presumably because the inclusion of the tackifier (B) prevents deterioration due to moisture in the air.

[0064] <Manufacturing of thermoelectric conversion elements> The above dispersions were applied onto a PET film having a thickness of 50 μm, and five thermoelectric conversion layers each having a thickness of 20 μm and a shape of 5 mm×30 mm were prepared at intervals of 10 mm. Next, four silver circuits (electrodes) having a thickness of 10 μm and a shape of 5 mm×33 mm were prepared using silver paste so that each thermoelectric conversion layer was connected in series, and thermoelectric conversion elements were manufactured. As the above silver paste, REXALPHA RA-FS 074 manufactured by Toyo Ink Co., Ltd. was used. When the electromotive force of each thermoelectric conversion element was measured, it was confirmed that the thermoelectric conversion elements manufactured using the dispersions manufactured in Examples 1 to 17 had a superior electromotive force to the thermoelectric conversion element manufactured using the dispersion manufactured in Comparative Example 101.

[0065] [Table 1]

Claims

1. A thermoelectric conversion material comprising a conductive material (A) and a tackifier (B) having a cyclic aliphatic hydrocarbon structure, wherein the conductive material (A) comprises carbon nanotubes, carbon black or graphene, and the tackifier (B) having a cyclic aliphatic hydrocarbon structure comprises a C5 petroleum resin, a C9 petroleum resin, a C5C9 petroleum resin, or a hydrogenated petroleum resin thereof.

2. A thermoelectric conversion material as described in claim 1, wherein the softening point of the tackifier (B) is 80°C or higher and 200°C or lower.

3. 3. The thermoelectric conversion material according to claim 1, wherein the content of the tackifier (B) having a cyclic aliphatic hydrocarbon structure is 1 part by mass or more and 200 parts by mass or less per 100 parts by mass of the conductive material (A).

4. A thermoelectric conversion element comprising a thermoelectric conversion film comprising the thermoelectric conversion material according to any one of claims 1 to 3 and electrodes, the thermoelectric conversion film and the electrodes being electrically connected to each other.

Citation Information

Patent Citations

  • Impact-resistant poly(arylene ether) resin with improved transparency

    JP2014515433A

  • Carbon nanotube dispersion, manufacturing method therefor, carbon nanotube-containing thermoelectric transducer and manufacturing method therefor

    JP2016153367A

  • Pressure sensitive adhesive sheet

    JP2017002292A

  • Thermoelectric conversion material and method for manufacturing same

    WO2013141065A1

  • Thermoelectric conversion material and thermoelectric conversion element

    WO2015050113A1