Silicide-based alloy thin film and its manufacturing method
A silicide-based alloy thin film with specific composition and crystal phases addresses the limitations of toxic Bi-Te materials by providing high Seebeck coefficient and low thermal conductivity, enabling efficient thermoelectric conversion.
Patent Information
- Application Number
- JP2020157537
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-09-18
AI Technical Summary
Existing thermoelectric materials, such as Bi-Te-based materials, are toxic and unsuitable for high-temperature applications, lacking desirable thermoelectric properties like high Seebeck coefficients and power factors, and there is a need for non-toxic, lightweight materials with improved performance for waste heat recovery.
A silicide-based alloy thin film composed of alkaline earth metals and silicon, with specific atomic ratios and crystal phases, is produced using a sputtering method with a strontium silicide target, achieving a high Seebeck coefficient and low thermal conductivity.
The silicide-based alloy thin film exhibits low electrical resistivity, high Seebeck coefficient, and low thermal conductivity, enabling efficient thermoelectric conversion at room temperature.
Smart Images

Figure 0007562093000001 
Figure 0007562093000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicide-based alloy thin film having excellent thermoelectric conversion properties and a method for producing the same. [Background technology]
[0002] Thermoelectric conversion elements are known as elements capable of mutual conversion between thermal energy and electrical energy. These thermoelectric conversion elements are constructed using two types of thermoelectric conversion materials, p-type and n-type, which are electrically connected in series and thermally arranged in parallel. When a voltage is applied between the two terminals of this thermoelectric conversion element, holes and electrons move, generating a temperature difference between the two sides (Peltier effect). When a temperature difference is applied between the two sides of this thermoelectric conversion element, holes and electrons also move, generating an electromotive force between the two terminals (Seebeck effect).
[0003] For this reason, studies are being conducted on its use as a cooling element for personal computer CPUs, refrigerators, car air conditioners, etc., which utilize the Peltier effect, and as an element for power generation equipment that utilizes waste heat from waste incinerators, etc., which utilize the Seebeck effect. In particular, since the amount of waste heat from automobile engines is too large to be ignored, it is being considered to generate electricity using the engine waste heat, and the temperature range is said to be several hundred degrees.
[0004] Conventionally, Bi2Te3 has been mainly used as a thermoelectric material for thermoelectric conversion elements, and Se is generally added when forming n-type thermoelectric materials with Bi-Te-based materials. However, the elements Bi, Te, and Se that make up these thermoelectric materials are highly toxic and may cause environmental pollution. Therefore, thermoelectric materials that have little environmental impact, i.e., are non-toxic, are desired. In addition, Bi-Te-based materials are mainly used at around 100°C and are not suitable for use in the utilization of exhaust heat from automobiles. Furthermore, lightweight and resource-rich materials are desired for use in automobile waste heat recovery.
[0005] Mg2Si is known as a silicide-based thermoelectric material (see, for example, Patent Document 1). As a method for producing a thin film using a homologous element, a BaSi2-based material (see, for example, Patent Document 2) has been proposed, but there has been no research on a thin film having multiple SrSi2 crystal polytypes, and it has been unclear what kind of thermoelectric properties it has. Although the SrSi2 system (see, for example, Patent Document 3) has been reported, there is a demand for better thermoelectric properties, in particular a higher Seebeck coefficient. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-368291 A [Patent Document 2] JP 2016-008316 A [Patent Document 3] JP 2019-149523 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a silicide-based alloy thin film having high thermoelectric conversion properties (particularly high Seebeck coefficient and power factor) and a method for producing the same. [Means for solving the problem]
[0008] In view of the above background, the present inventors have conducted extensive research and have found that a silicide-based alloy thin film containing an alkaline earth metal and silicon as main components, which has a specific composition and in which the cubic and trigonal phases satisfy specific requirements, has excellent thermoelectric conversion properties, and have also found a method for producing the thin film, thereby completing the present invention.
[0009] The aspects of the present invention are as follows. (1) A silicide-based alloy thin film mainly composed of alkaline earth metal and silicon, in which the atomic ratio of the elements constituting the alloy thin film is: 20at%≦X / (X+Si)≦45at% 55at%≦Si / (X+Si)≦80at% and A silicide alloy thin film in which the crystal phases present within the thin film are primarily cubic and trigonal. When the peak intensity due to the cubic (210) plane in X-ray diffraction is C and the peak intensity due to the trigonal (101) plane is T, the following relationship is satisfied: 0.1≦T / (C+T)≦0.3 (2) The silicide alloy thin film according to (1), wherein the alkaline earth metal is strontium. (3) A thermoelectric conversion element using the silicide alloy thin film according to (1) or (2). (4) A method for producing a silicide alloy thin film according to (1) or (2) above, which comprises forming the silicide alloy thin film on a substrate by a sputtering method using strontium silicide as a target. (5) The method for producing a silicide alloy thin film according to (4) above, wherein the strontium silicide sputtering target is a strontium silicide bulk polycrystalline body having an oxygen content of 1.5 wt % or less. (6) The discharge power during sputtering is given to the target with a power density of 3.0 W / cm 2 More than 10W / cm 2 The method for producing a silicide alloy thin film according to (4) or (5) above, which is as follows: (7) The method for producing a silicide alloy thin film according to any one of (4) to (6) above, wherein the substrate temperature during sputtering is 590°C to 690°C. Effect of the Invention
[0010] According to the present invention, it is possible to provide a silicide-based alloy thin film having excellent thermoelectric conversion properties, such as a low electrical resistivity of 10 mΩ·cm or less, a high Seebeck coefficient of 100 μV / K or more, and a low thermal conductivity of 5 W / mK or less. Moreover, by using the silicide alloy thin film of the present invention, a highly efficient thermoelectric conversion element can be fabricated in the room temperature range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The contents of the present invention are as follows. The silicide alloy thin film of the present invention is mainly composed of an alkaline earth metal and silicon, of which the alkaline earth metal is preferably selected from calcium, strontium, and barium, and more preferably strontium, and may contain a plurality of alkaline earth metals.
[0012] The silicide alloy thin film in the present invention is defined by the composition shown below, where X is an alkaline earth metal and Si is silicon. 20at%≦X / (X+Si)≦45at% 55at%≦Si / (X+Si)≦80at% Preferably 25at%≦X / (X+Si)≦40at% 60at%≦Si / (X+Si)≦75at% More preferably 30at%≦X / (X+Si)≦37at% 63at%≦Si / (X+Si)≦70at% It is.
[0013] By satisfying the above specific composition, it becomes possible to have a high Seebeck coefficient, low thermal conductivity, and high power factor, and to achieve high thermoelectric conversion efficiency.
[0014] The silicide alloy thin film of the present invention contains a cubic phase and a trigonal phase within the thin film and satisfies the following specific formula: In other words, the abundance ratio of the cubic phase and the trigonal phase is defined by the following formula, where C is the peak intensity due to the cubic (210) plane in X-ray diffraction and T is the peak intensity due to the trigonal (101) plane. 0.1≦T / (C+T)≦0.3 Preferably 0.1≦T / (C+T)≦0.25 It is. By satisfying this specific formula, it becomes possible to have a high Seebeck coefficient, low thermal conductivity, and a high power factor, and to achieve high thermoelectric conversion efficiency.
[0015] The presence of an excessive amount of trigonal phase (i.e., when T / (C+T)>0.3) leads to a decrease in the Seebeck coefficient and an increase in thermal conductivity, resulting in a decrease in thermoelectric conversion performance.On the other hand, when the proportion of trigonal phase is low (i.e., when T / (C+T)<0.1), the electrical resistance increases and the thermoelectric conversion performance deteriorates.
[0016] The thickness of the silicide alloy thin film of the present invention is preferably 50 nm or more, and more preferably 500 nm or more. By having a thickness of 50 nm or more, the thin film exhibits sufficient crystallinity and conductivity, and can obtain better thermoelectric properties. There is no particular upper limit to the thickness of the thin film, but the thickness of the thin film is usually 100 nm or less.
[0017] The surface roughness (Ra) of the silicide alloy thin film of the present invention is preferably 20 nm or less, more preferably 15 nm or less. A flat surface reduces the surface area, making it possible to suppress surface oxidation. The surface roughness (Ra) is measured according to JIS R 1683.
[0018] The silicide alloy thin film of the present invention is preferably formed on a substrate. Examples of the substrate material include sapphire, inorganic glass, silicon, and the like. Among them, in order to prepare a film with good crystallinity, a sapphire substrate is preferable, and the substrate is preferably oriented in the (0001) plane. This improves the crystallinity of the thin film in accordance with the crystallinity of the substrate, thereby further improving the thermoelectric properties.
[0019] The power factor PF=S is an index used to evaluate the performance of thermoelectric conversion materials. 2 σ, dimensionless figure of merit: ZT=(S 2 / (ρ κ))T is used, where S is the Seebeck coefficient, ρ is resistivity, κ is thermal conductivity, and T is absolute temperature. In other words, to obtain good thermoelectric properties in a thermoelectric conversion material, it is necessary that the Seebeck coefficient S and electrical resistivity ρ are low, and that the thermal conductivity κ is low.
[0020] The silicide-based alloy thin film of the present invention has a resistivity of 10 Ω·cm or less, particularly 1.0×10 -2 It can have an electrical resistivity of Ω·cm or less. This increases the index as a thermoelectric conversion material, and it shows good thermoelectric conversion characteristics. It can also have a Seebeck coefficient of 100 μV / K or more, particularly 120 μV / K or more. This increases the index as a thermoelectric conversion material, and it shows good thermoelectric conversion characteristics. It can also have a thermal conductivity of 5 w / mK or less, particularly 3 w / mK or less. This increases the index as a thermoelectric conversion material, and it shows good thermoelectric conversion characteristics.
[0021] Next, an example of a method for producing a silicide-based alloy thin film according to the present invention will be described, but the present invention is not limited to this method. The method for producing the silicide-based alloy thin film of the present invention is preferably a method for forming a film on a substrate by a sputtering method. In the sputtering method, in order to obtain stable discharge characteristics and reduce the inclusion of impurities, it is preferable to use a strontium silicide sputtering target in the present invention, since it has low reactivity with air and can suppress the amount of oxygen.
[0022] The strontium silicide sputtering target preferably used in the present invention is preferably a bulk polycrystalline body having an oxygen content of preferably 1.5 wt % or less, more preferably 1.0 wt % or less, more preferably 0.7 wt % or less, and more preferably 0.5 wt % or less.
[0023] Here, the method for measuring the oxygen content can be a method of pyrolyzing the polycrystalline body and measuring the oxygen content by a thermal conductivity method using a carbon / nitrogen / hydrogen analyzer. In addition, there can also be a method of measuring the oxygen content by elemental analysis such as XPS (X-ray photoelectron spectroscopy) and EPMA.
[0024] The bulk polycrystalline strontium silicide sputtering target has a density of 3.0 g / cm 3 It is preferable that the content is 3.2 g / cm or more. 3 The above is more preferable. This reduces open pores in the bulk body, making it difficult for oxidation of the surface to progress. The density here refers to bulk density, which can be measured by a method of measuring dimensions, such as the Archimedes method.
[0025] The method of adjusting the composition of the silicide-based alloy thin film is not particularly limited, and includes a method of preparing each element as a separate sputtering target and sputtering them together. In addition, a fragment of a strontium element source may be placed on a base sputtering target, for example, a silicon target, and sputtered. When each element is prepared as a separate sputtering target, the amount of strontium element and silicon element can be adjusted, for example, by adjusting the discharge power during sputtering, the gas pressure during sputtering, and the gas composition. When fragments of each element target are used, the size, number, and installation position of the fragments can be selected to adjust the amount. In addition, when preparing an integrated sputtering target, JP 2015-221744 and the like can be referred to.
[0026] In the method for producing a silicide-based alloy thin film, in order to make the cubic SrSi2 phase and the trigonal SrSi2 phase coexist, the substrate temperature during sputtering is preferably 590° C. to 690° C., and more preferably 590° C. to 650° C. By setting the temperature in the above range, it is possible to set the abundance ratio T / (C+T) of the cubic phase with high thermoelectric properties and the trigonal phase with high electrical conductivity in the above range, resulting in a silicide-based alloy thin film having a crystal phase with good thermoelectric properties.
[0027] In the method for producing a silicide-based alloy thin film of the present invention, the gas pressure during film formation is preferably 10 mtorr or more, more preferably 20 mtorr or more. The gas pressure during film formation is preferably 500 mtorr or less, more preferably 400 mtorr or less. By setting the pressure within this range, it is possible to maintain a stable discharge during film formation, appropriately adjust the energy when the particles reach the substrate, and obtain a film with good crystallinity.
[0028] In the method for producing a silicide-based alloy thin film of the present invention, the power density applied to the target as the discharge power during sputtering is 10 W / cm 2 It is preferable that the value is less than 5 W / cm. 2 This allows the energy given to the particles to be suppressed, resulting in a film with less distortion. The power density is 3.0 W / cm 2 More preferably, 3.5 W / cm 2 This enables stable discharge, and makes it possible to set the abundance ratio T / (C+T) of cubic crystals with high thermoelectric properties and trigonal crystals with high electrical conductivity within the above-mentioned range.
[0029] Gases such as argon and nitrogen can be used for film formation, but it is preferable to contain hydrogen in order to suppress the influence of oxygen. By containing hydrogen, it becomes possible to react with oxygen in the sputtering target and reduce the amount of oxygen in the film. Next, a preferred method for producing a bulk polycrystalline material preferably used for a strontium silicide sputtering target will be described.
[0030] (Alloying process) This is a process for alloying raw materials including a strontium source and a silicon source. Although the alloying method is not particularly limited, a method that minimizes the inclusion of oxygen is preferable, and for this purpose, an arc melting method is preferable, which is an apparatus that uses as few oxygen-containing materials as possible in containers, etc. The arc melting method is a technique in which the material to be treated is locally heated and melted by discharging electricity from an electrode. This method allows high-temperature treatment easily and is an excellent alloying treatment method. In addition, since the atmosphere can be controlled, treatment can be performed in an inert gas atmosphere, etc., and the oxygen content of the obtained alloy can be reduced.
[0031] For example, when metallic strontium is used as the strontium source and silicon is used as the silicon source, the melting point of strontium is approximately 780°C, the boiling point of strontium is approximately 1400°C, and the melting point of silicon is approximately 1400°C. Therefore, an arc melting furnace, which is capable of raising the temperature rapidly, is effective in melting both materials uniformly.
[0032] The strontium source is preferably at least one of strontium metal and a strontium alloy, and a particularly preferred strontium alloy is a strontium silicide alloy. The silicon source is preferably at least one of silicon metal and a silicon alloy, and a particularly preferred silicon alloy is a strontium silicide alloy.
[0033] Here, when the raw material contains a strontium silicide alloy, the strontium silicide alloy can also be used as a strontium source and a silicon source.
[0034] The average particle size of the strontium source is preferably greater than 1 mm, and more preferably greater than 8 mm, which suppresses oxidation and provides the effect of stably reducing the amount of oxygen in the bulk polycrystalline body.
[0035] In the alloying process, either a single-stage arc melting process in which a strontium source and a silicon source are mixed and then subjected to an arc melting process, or a two-stage arc melting process in which a strontium source and a silicon source are subjected to an arc melting process, the melt is then inverted, and then subjected to an arc melting process again, may be used, but the two-stage arc melting process described above is preferred. This allows silicon to be sufficiently diffused in the bulk polycrystalline body, i.e., to be sufficiently dissolved in strontium silicide, and therefore the problem of the strength of the sintered body decreasing due to the presence of silicon that is not dissolved in the body can be solved. As a specific melting method, the raw materials are placed so that strontium is dissolved first.
[0036] For example, by placing silicon at the bottom of a water-cooled mold and then placing metallic strontium on top of it, the strontium is exposed to the arc discharge at the beginning of the arc melting process. This allows the strontium to melt at the beginning and then be alloyed with silicon. However, because the temperature at the bottom of the water-cooled mold is low, some ingenuity is required, such as extending the melting time.
[0037] When using the arc melting method in alloying processing, the strength of the arc output per material weight affects the alloying of materials with large differences in melting points. For example, in the case of alloying barium and silicon, the melting point of barium is about 730°C, the boiling point is about 1640°C, and there is a certain range of temperatures from melting to volatilization, so melting is possible with an initial output of 100-200A and an output during melting of 10-30A / g (amount of discharge current per amount of molten metal input), making it relatively easy to melt, but metal strontium has a melting point of about 780°C and a boiling point of 1400°C, so strontium volatilizes in the melting temperature range of silicon, making it difficult to obtain a strontium silicide alloy with the desired composition ratio.
[0038] In particular, when metal strontium is used as the strontium source, the initial discharge current is preferably less than 100A, more preferably 70A or less, and even more preferably 50A or less. The initial discharge current is preferably 20A or more, and even more preferably 30A or more. This makes it possible to start synthesis while dissolving metal strontium and suppressing volatilization. A discharge current of 5 to 10A / Sr-g (discharge current value per input amount of strontium) is applied to the alloy after dissolution. By carrying out the reaction for 3 minutes or more, alloying to strontium silicide proceeds at a temperature lower than the melting temperature of silicon, suppressing volatilization, and making it possible to proceed with alloying of silicon and strontium without leaving silicon.
[0039] In addition, by using the arc melting method to perform heating locally, it is possible to heat only the interface between strontium and silicon preferentially, thereby accelerating the reaction.
[0040] When metallic strontium is used as the strontium source, it is preferably in the form of a lump. In the form of a powder, surface oxidation progresses, oxygen is easily taken into the alloy, and the oxide film volatilizes when strontium is dissolved, reducing the amount of strontium added. The diameter of the lump is preferably 1 mm or more, more preferably 5 mm or more, and even more preferably 10 mm or more. This reduces the surface layer, suppresses oxidation, and enables stable addition of strontium.
[0041] The silicon source is preferably a powder, and the average particle size of the powder is preferably 10 mm or less, more preferably 5 mm or less. The average particle size refers to the average particle size of the powder or the crushed material after pulverization, and refers to the D50 average particle size measured by a particle size distribution meter, particle size measurement, etc.
[0042] If the average particle size is larger than 10 mm, the silicon powder will be left undissolved or unreacted during melting, resulting in cracks caused by the coarse silicon particles generated in the strontium silicide alloy body, making it difficult to manufacture a strontium silicide bulk polycrystalline body. Also, if the average particle size is small, the silicon powder will scatter before melting due to the energy of the discharge when using the arc melting method, and will float in the solution due to surface tension, making it difficult to dissolve stably and in the required composition ratio, so the average particle size of the silicon powder is preferably 0.1 mm or more.
[0043] In addition, it is desirable that the oxygen content of the raw materials, strontium source and silicon source, is as low as possible, specifically, 20 atm% or less is preferable, and 10 atm% or less is more preferable. By reducing the oxygen content in the raw materials, the amount of oxygen remaining in the polycrystalline body is reduced, and the amount of oxygen in the formed strontium silicide film is also reduced, thereby improving the purity. For example, when metallic strontium is used as the strontium source, strontium is oxidized quickly when exposed to air, so in order to reduce the amount of oxygen, it is preferable to install it in a melting device so that it does not come into contact with air.
[0044] (Crushing process) This is a process for pulverizing the strontium alloy obtained in the alloying process. In order not to increase the oxygen content of the obtained alloy, it is preferable to carry out the strontium silicide alloy in an inert gas or dry gas atmosphere between the alloying process and the pulverization process, and it is also preferable to carry out the pulverization in an inert gas or dry gas atmosphere. This is because it is possible to prevent oxidation of the powder surface of the alloy containing the doping element and to keep the oxygen content low. Examples of the pulverization method include a method using a mortar, a method using a ball mill, and a method using a bead mill.
[0045] (Hot press process) This is a process in which strontium silicide alloy powder is hot pressed at 600°C to 1100°C. This process makes the resulting bulk polycrystal more uniform, and stabilizes its thermoelectric conversion properties. The hot press method is a device that advances sintering by applying heat while pressing the powder. Uniaxial pressure is applied during heating to assist the diffusion of elements within the workpiece during sintering, so this is a sintering method that can sinter even materials that are difficult to sinter, such as those that contain elements with low diffusion coefficients or those that process powders with large particle sizes, such as metals. Sintering using the hot press method improves density, for example, to 3.0 g / cm. 3 It is possible to obtain a strontium silicide polycrystalline body having a density as high as or higher than that mentioned above.
[0046] The powder of strontium silicide alloy to be subjected to the hot pressing step is preferably a strontium silicide alloy obtained by treating raw materials including a strontium source and a silicon source by the above-mentioned arc melting.
[0047] The particle size (D50%, sieve type particle size distribution analyzer) of the strontium silicide alloy to be subjected to the hot pressing process is preferably 10 μm to 200 μm, more preferably 30 μm to 150 μm. This makes the powder finer, improves the sinterability, and increases the density of the bulk polycrystalline body. However, if the particle size is less than 10 μm, the oxidation of the powder is likely to proceed, and the density during powder packing decreases, making it difficult to obtain a low-oxygen, high-density sintered body.
[0048] The firing temperature in the hot press treatment is 600° C. to 1000° C., and preferably 700° C. to 1000° C. At temperatures lower than 600° C., sintering does not proceed, and the density increases only to the same extent as the density of the compact. Furthermore, if firing is performed at a temperature higher than 1000° C., there is a possibility that strontium silicide will melt because the melting point is close to that of the strontium silicide.
[0049] The pressure in the hot press treatment is preferably 10 MPa to 100 MPa, because this can further improve the density of the polycrystalline body and ensure that it can withstand use in a commonly used carbon mold.
[0050] The hot press treatment is preferably carried out in an atmosphere that does not contain oxygen, and is preferably either a vacuum, nitrogen, or argon atmosphere. The holding time at the firing temperature in the hot press treatment is preferably 30 minutes or more, and more preferably 1 hour or more. If the holding time is too short, the inside cannot be heated uniformly, making it difficult to maintain the shape as a polycrystalline body.
[0051] The bulk polycrystalline body may be processed to a predetermined size. The processing method is not particularly limited, but a surface grinding method, a rotary grinding method, a cylindrical grinding method, or the like may be used. Since it reacts with water, care must be taken when handling water during processing. If necessary, it may be processed into a shape suitable for use as a thermoelectric conversion element. EXAMPLES
[0052] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0053] (Method of confirming crystallinity) An XRD device (device name: Bruker AXS D8 Discover) was used to scan from 20° to 50°, and the data measured in the tilt angle range of 0° to 90° was integrated to obtain a diffraction pattern, from which the crystalline phases contained were identified from the peak positions. The JCPDS card for the crystal phase used as reference was 00-020-1215 for the cubic crystal, and the trigonal phase was identified with Phys.Rev.B 84, 184503 (2011) as the point group P-3m1, 164, a = 3.89 Å, c = 5.01 Å, with the (101) peak at 31.35° and the (102) peak at 44.05°. From the obtained diffraction pattern, the peak intensity C due to the cubic (210) plane and the peak intensity T due to the trigonal (101) plane were obtained, and T / (C+T) was calculated.
[0054] (Method for checking the amount of added elements in the film) Elemental analysis was carried out using a wavelength dispersive X-ray fluorescence analyzer (instrument name: PW2404, PANalytical Corporation), and the contents of the added elements were calculated. (Method of measuring the electrical resistivity of the film) The film was heated from room temperature to 400° C. using a Seebeck coefficient measuring device (device name: ULVAC ZEM-3) and the film resistivity was measured at each temperature.
[0055] (Method of distinguishing semiconductor type) The Seebeck coefficient was determined from the absolute value of the Seebeck coefficient when heated from room temperature to 400° C. using a Seebeck coefficient measuring device (device name: ULVAC ZEM-3). Positive value: p-type, negative value: n-type. (Method of measuring Seebeck coefficient) Using a Seebeck coefficient measuring device (device name: ULVAC ZEM-3), the sample was heated from room temperature to 400° C., and the Seebeck coefficient at each temperature was calculated. (Method of measuring the thermal conductivity of a film) The measurements were carried out by the picosecond thermoreflectance method using a thin film thermal property measuring device (Picotherm PicоTR). (Performance evaluation of thermoelectric conversion materials) The performance was evaluated based on the dimensionless figure of merit: ZT = (S2 / (ρ κ))T, where S is the Seebeck coefficient, ρ is resistivity, κ is thermal conductivity, and T is absolute temperature.
[0056] [Example 1] Under the conditions shown below, the target discharge power: 50 W (3.8 W / cm 2 ) a sputtering deposition test was carried out on a (0001) sapphire substrate (manufactured by Kyocera Corporation, 5 mm square, 0.5 mm thick) at a substrate temperature of 600°C. (Sputtering conditions) Discharge method: RF sputtering Film forming equipment: Magnetron sputtering equipment Target: 2 inch φ strontium silicide target Distance between target and board: 60mm Deposition pressure: 20mTorr Inlet gas: Argon 100sccm
[0057] [Example 2] Film formation was carried out in the same manner as in Example 1, except that the substrate temperature was set to 680°C. [Example 3] Film formation was carried out in the same manner as in Example 1, except that the substrate temperature was set to 650°C. [Example 4] Film formation was carried out in the same manner as in Example 1, except that the substrate temperature was set to 630°C. [Example 5] Film formation was carried out in the same manner as in Example 1, except that the substrate temperature was set to 620°C. [Example 6] Film formation was carried out in the same manner as in Example 1, except that the substrate temperature was set to 590°C.
[0058] [Comparative Example 1] Discharge power of target: 30W (2.3W / cm 2 ) and the substrate temperature was 520° C., and film formation was carried out in the same manner as in Example 1. [Comparative Example 2] Discharge power of target: 30W (2.3W / cm 2 ) and the substrate temperature was 490° C., and film formation was carried out in the same manner as in Example 1. [Comparative Example 3] Discharge power of target: 50W (3.8W / cm 2 ) and the substrate temperature was 530° C., and film formation was carried out in the same manner as in Example 1.
[0059] [Comparative Example 4] Discharge power of target: 50W (3.8W / cm 2 ) and the substrate temperature was 520° C., and film formation was carried out in the same manner as in Example 1. [Comparative Example 5] Target discharge power: 20 W (1.5 W / cm 2 ) and the substrate temperature was 500° C., and film formation was carried out in the same manner as in Example 1. [Comparative Example 6] Discharge power of target: 30W (2.3W / cm 2 ) and the substrate temperature was 760° C., and film formation was carried out in the same manner as in Example 1. The physical properties at 50° C. of the thin films obtained in Examples 1 to 6 and Comparative Examples 1 to 6 are shown in Tables 1 and 2.
[0060] [Table 1]
[0061] [Table 2] [Industrial Applicability]
[0062] By using the present invention, it is possible to fabricate a high-performance thermoelectric conversion element, and to efficiently utilize waste heat over a wide temperature range.
Claims
1. The silicide-based alloy thin film is mainly composed of alkaline earth metal and silicon, and the atomic ratio of the elements constituting the alloy thin film is as follows: 20at%≦X / (X+Si)≦45at% 55at%≦Si / (X+Si)≦80at% and A method for producing a silicide alloy thin film, in which the crystal phases present in the thin film are mainly composed of a cubic phase and a trigonal phase, and the peak intensity due to a cubic (210) plane in X-ray diffraction is defined as C and the peak intensity due to a trigonal (101) plane is defined as T, the following relational expression is satisfied: 0.1≦T / (C+T)≦0.3 A method for producing a silicide alloy thin film, in which the film is formed on a substrate by a sputtering method, the substrate temperature during sputtering being 590°C to 630°C.
2. 2. The method for producing a silicide alloy thin film according to claim 1, wherein the alkaline earth metal is strontium.
3. 3. The method for producing a silicide alloy thin film according to claim 1, wherein the silicide alloy thin film is formed on a substrate by a sputtering method using strontium silicide as a target.
4. 4. The method for producing a silicide alloy thin film according to claim 3, wherein the strontium silicide sputtering target is a strontium silicide bulk polycrystalline body having an oxygen content of 1.5 wt % or less.
5. The discharge power during sputtering was 3.0 W / cm 2 More than 10W / cm 2 The method for producing a silicide alloy thin film according to any one of claims 1 to 4, wherein:
Citation Information
Patent Citations
Thermoelectric material
JP2002368291A
Hydrogen storage material
JP2005232583A
PRODUCTION METHOD OF MSi2 (M IS AT LEAST ONE KIND OF ALKALINE EARTH METAL SELECTED FROM Mg, Ca, Sr, Ba AND Ra) FILM
JP2016008316A
Barium-silicide-based laminate material, and production therefor
JP2016044326A
Bulk body containing strontium and producing method of the same
JP2019147728A