Photocurable resin compositions, photocurable resin articles, and methods for making such articles
The photocurable resin composition with tailored mechanical properties and microstructures addresses the stress relaxation issue in orthodontic aligners, enhancing treatment efficacy and patient comfort by maintaining force application over time.
Patent Information
- Application Number
- JP2021521408
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-19
- Filing Date
- 2019-10-18
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-10-18
AI Technical Summary
Current orthodontic aligners made from thermoplastic materials experience significant stress relaxation, leading to reduced mechanical force over time, limiting their effectiveness in treating orthodontic cases and requiring interim corrections or conversions to fixed appliances due to uniform thickness and mechanical strength, which fails to account for the varying force needs of individual teeth.
A photocurable resin composition comprising urethane (meth)acrylate, di(meth)acrylate, and photoinitiator, with specific diisocyanates and hydroxy(meth)acrylates, is used to create 3D printed aligners with internal microstructures and varying mechanical strengths, allowing for stress recovery and tailored force application.
The photocurable resin composition maintains mechanical strength and reduces stress relaxation, enabling more effective and comfortable orthodontic treatment by providing aligners with controlled force distribution and improved clinical outcomes.
Smart Images

Figure 0007560129000004 
Figure 0007560129000005 
Figure 0007560129000006
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 747,694, filed October 19, 2018, which is incorporated by reference in its entirety. [Background technology]
[0002] 2. Background of the Invention Dental malocclusion affects approximately 60%-75% of the world's population (4.6-5.7 billion people). As a result, there is a tremendous global demand for orthodontic treatment to correct malocclusion. Roughly, 15% of these cases are treated with orthodontic clear aligners (690-855 million patients per year), representing a market size of $1.5 billion. This market segment is expected to reach $2.7 billion by 2021, with a projected annual compound growth rate of 12.16% from 2018 to 2021. The aligners are manufactured through the following steps: 1) scanning the patient's dental impression with a 3D scanner; 2) digitizing the dental impression and converting it into a stereolithography CAD software-compliant STL file; 3) creating an orthodontic treatment plan with the software resulting in a 3D model of the patient's teeth representing different stages of treatment, from the current teeth to a perfect smile; 4) 3D printing the model by stereolithography; 5) heating and vacuum-adhering a sheet of thermoplastic material onto the 3D printed model, resulting in an aligner similar to the designed treatment plan; 6) preparing the aligner using milling and then smoothing it; 7) packaging and delivering the aligner to the orthodontist or directly to the patient.
[0003] The use of current orthodontic dental aligners is limited to mild / moderate orthodontic cases, in part due to limited mechanical properties and the inherent thermoplastic materials utilized in the manufacture of the aligners. Unlike traditional metal appliances that exert a constant force to induce tooth movement (Zhang et al., 2011, Dent. Mater. J., 30: 954-959; Lombardo et al., 2017, Angle. Orthod., 87: 11-18), the force exerted by clear orthodontic aligners decreases significantly (15%-45%) throughout the first 8 hours of application until any tooth movement is achieved. This is caused by a phenomenon known as stress relaxation, which is commonly seen among thermoplastic materials. In studies, the mechanical degradation of these materials has led to their limited case application and poor clinical efficiency compared to fixed orthodontic treatments. Furthermore, 70% to 80% of orthodontists report that their patients have asked for mid-course correction, narrowing of the case, or conversion to fixed orthodontic appliances before the end of treatment.
[0004] Furthermore, thickness and mechanical strength are uniform properties in clear orthodontic aligners because they are made by heat pressing a piece of plastic sheet onto a preformed mold similar to the shape of the desired aligner. However, in an ideal orthodontic treatment, each tooth to be moved would require a different amount of force to be repositioned into its natural position. To achieve this, the aligner would have to feature different local strengths to manipulate each individual tooth with the force required for its repositioning. This is not achieved with current thermoplastic aligners due to the homogeneity of the material.
[0005] There is a need in the art for a light curable material that recovers stress in its corresponding plastic after an initial stress relaxation period and also allows for an assembly process, as well as a method for making an orthodontic aligner involving a one-step system. The present invention fulfills this unmet need. Summary of the Invention
[0006] SUMMARY OF THE PRESENT APPLICATION In one aspect, the present invention relates to a photocurable resin comprising 75 to 85 weight percent of a urethane (meth)acrylate, 10 to 25 weight percent of a di(meth)acrylate, and less than 5 weight percent of a photoinitiator. In one embodiment, the urethane (meth)acrylate comprises a diisocyanate and a hydroxy (meth)acrylate. In one embodiment, the diisocyanate is selected from the group consisting of 2,4-toluene diisocyanate, 2,5-toluene diisocyanate, 2,6-toluene diisocyanate, and 4,4'-methylenebis(phenylisocyanate); and the hydroxy(meth)acrylate is selected from the group consisting of poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, poly(propylene glycol) methacrylate, poly(propylene glycol) acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate. In one embodiment, the di(meth)acrylate is selected from the group consisting of triethylene glycol dimethacrylate, di(ethylene glycol) dimethacrylate, propylene glycol dimethacrylate, and di(propylene glycol) dimethacrylate. In one embodiment, the photoinitiator is selected from the group consisting of: diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide; bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide. In one embodiment, the composition further comprises a stabilizer selected from the group consisting of: bis(2,2,6,6-tetramethyl-1-octyloxy-4-piperidyl)sebacate; bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate; methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate; dimethylsebacate; and bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate.
[0007] In one embodiment, the composition further comprises a second photocurable resin composition comprising a second urethane (meth)acrylate, a second di(meth)acrylate, a triacrylate, and a second photoinitiator. In one embodiment, the second urethane (meth)acrylate of the second photocurable resin comprises a diisocyanate and a hydroxy (meth)acrylate, wherein the diisocyanate is selected from the group consisting of 2,4-toluene diisocyanate, 2,5-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-methylenebis(phenylisocyanate), and combinations thereof; and wherein the hydroxy (meth)acrylate is selected from the group consisting of poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, poly(propylene glycol) methacrylate, poly(propylene glycol) acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, and combinations thereof. In one embodiment, the second di(meth)acrylate of the second photocurable resin is selected from the group consisting of: triethylene glycol dimethacrylate, di(ethylene glycol) dimethacrylate, propylene glycol dimethacrylate, and di(propylene glycol) dimethacrylate. In one embodiment, the triacrylate is 1,1-trimethylolpropane triacrylate. In one embodiment, the second photoinitiator of the second photocurable resin is selected from the group consisting of: diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide; bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide.
[0008] The invention also relates, in part, to a method of making an article comprising the steps of: providing a photocurable resin comprising 75-85 weight percent of a urethane (meth)acrylate, 10-25 weight percent of a di(meth)acrylate, and less than 5 weight percent of a photoinitiator; 3D printing the photocurable resin to form an article; and curing the article. In one embodiment, providing a photocurable resin comprises providing a second photocurable resin comprising a second urethane (meth)acrylate, a second di(meth)acrylate, a triacrylate, and a second photoinitiator, and 3D printing the photocurable resin comprises 3D printing the second photocurable resin.
[0009] The invention further relates, in part, to a 3D printed resin article, wherein the article comprises an inner microarchitecture comprising a photocured resin and a solid coating comprising a second photocured resin; wherein the solid coating encapsulates the inner microarchitecture. In one embodiment, the microarchitecture comprises pores having an inner diameter of 0.5 mm to 5 mm. In one embodiment, the microarchitecture comprises a photocured resin having a thickness of 0.1 mm to 3 mm. In one embodiment, the article has an initial stress of 0.45 MPa to 1.6 MPa when tested with a preload of 0.01 N. In one embodiment, the article has a stress relaxation of 50% to 65% after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article is a tooth aligner.
[0010] BRIEF DESCRIPTION OF THE DRAWINGS The following detailed description of various embodiments of the invention will be better understood when read in conjunction with the accompanying drawings. For the purpose of illustrating the invention, illustrative embodiments are shown in the drawings. It should be understood, however, that the invention is not limited to the precise arrangements and instrumentalities of the embodiments shown in the drawings. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a flow chart of an exemplary method for making a photocurable resin composition. [Diagram 2] Figure 2 shows the synthesis of MDI-PEGMA from 4,4'-methylenebis(phenylisocyanate) (MDI) and poly(ethylene glycol) methacrylate (PEGMA). The methacrylate groups susceptible to photoreactivity are shown in red. [Diagram 3] FIG. 3 shows the 1H NMR spectrum of MDI-PEGMA in DMSO. [Figure 4] Figure 4, comprising Figures 4A and 4B, shows the characterization of MDI-PEGMA using Fourier Transform Infrared Spectroscopy (FTIR) analysis. Figure 4A shows the FTIR spectrum of MDI-PEGMA resin with free isocyanate groups. Figure 4B shows the FTIR spectrum of MDI-PEGMA resin when the isocyanate groups have been reacted. [Diagram 5] FIG. 5 shows the squares designed for the top and bottom layers of plastic. [Figure 6] Figure 6, which includes Figures 6A and 6B, shows a beehive microstructure. Figure 6A shows a beehive microstructure with an inner diameter of 3.0 mm. Figure 6B shows a beehive microstructure with an inner diameter of 1.5 mm. [Figure 7] Figure 7, including Figures 7A, 7B, 7C, and 7D, shows the printed parts and post-cure process. Figure 7A shows a beehive with an inner diameter of 3.0 mm. Figure 7B shows a beehive with an inner diameter of 1.5 mm. Figure 7C shows a square structure placed between glass slides prepared for post-cure under UV light. Figure 7D shows UV light exposure to the printed pieces for strength enhancement. [Figure 8]Figure 8, comprising Figures 8A, 8B, and 8C, shows the assembly of plastic sheets for the preparation of a microstructured plastic sheet. Figure 8A shows a square piece with a thin layer of Bioink2 on the top layer. Figure 8B shows a 3.0 mm beehive structure combined with a bottom square layer. Figure 8C shows the addition of additional Bioink2 to combine the top and bottom layers with the microstructures upon light exposure. [Figure 9] FIG. 9 shows the sample preparation for dynamic mechanical analysis (DMA). [Figure 10] Figure 10, including Figures 10A, 10B, 10C, and 10D, shows 3D models of an aligner and support. Figure 10A shows a top view of the 3D model of the aligner with support. Figure 10B shows a bottom view of the 3D model of the aligner with support. Figure 10C shows a side view of the 3D model of the aligner with support. Figure 10D shows a front view of the 3D model of the aligner with support. [Figure 11] Figure 11, including Figures 11A, 11B, 11C, and 11D, shows a 3D printed aligner with supports. Figure 11A shows a 3D printed aligner with supports coupled to a 3D printer platform. Figure 11B shows a top view of the 3D printed aligner with supports. Figure 11C shows a front view of the 3D printed aligner with supports. Figure 11D shows a side view of the 3D printed aligner with supports. [Figure 12] FIG. 12, including FIG. 12A, FIG. 12B, FIG. 12C, FIG. 12D, FIG. 12E, and FIG. 12F, shows a 3D printed aligner with the supports removed. FIG. 12A shows a side view of the 3D printed aligner with the supports removed. FIG. 12B shows a top view of the 3D printed aligner with the supports removed and a cross-sectional view of the aligner. FIG. 12C shows the cross-sectional location of the 3D printed aligner with the supports removed. FIG. 12D shows a cross-sectional view of the 3D printed aligner with the supports removed. FIG. 12E shows a top view of the 3D printed aligner with the supports removed. FIG. 12F shows a close-up top view of the 3D printed aligner with the supports removed. [Figure 13] Figure 13, which includes Figures 13A, 13B, 13C, and 13D, shows the polymerization of Bioinks for mechanical property analysis. Figure 13A shows the deposition of Bioink onto a mold. Figure 13B shows the Bioink material exposed to 415 nm light for 1 minute. Figure 13C shows the photopolymerizable Bioink plastic sheet removed from the mold. Figure 13D shows the transparency of the photopolymerizable Bioink plastic when placed on a white surface with black lines drawn on it. The lines are clearly visible on both the front and back of the material. [Figure 14] FIG. 14 shows stress relaxation of orthodontic aligner material. [Figure 15] FIG. 15 includes FIG. 15A, FIG. 15B, FIG. 15C, FIG. 15D, FIG. 15E, and FIG. 15F and shows the preparation of a microstructured plastic sheet. FIG. 15A shows a pattern B mold for the preparation of a microstructured plastic sheet. FIG. 15B shows a pattern A mold for the preparation of a microstructured plastic sheet. FIG. 15C shows Bioink2 dispensed into a pattern A mold. Red dye was added to the formulation for visualization purposes in the final product. FIG. 15D shows the photopolymerization of Bioink2 in a pattern A mold. FIG. 15E shows the addition of a layer of Bioink1 to one side of the mesh. This layer was polymerized, the piece was flipped over, a second layer was dispensed, and polymerized to completely embed the mesh of Bioink2 within the two Bioink1 layers. FIG. 15F shows a photopolymerized plastic sheet of Bioink1 with embedded pattern A microstructures composed of Bioink2. [Figure 16] FIG. 16 shows the mesh design and stress relaxation of SmartTrack. [Figure 17] Figure 17, which includes Figures 17A and 17B, shows layering patterns. Figure 17A shows a photopolymerizable plastic sheet of pattern C, which is composed of three layers of Bioink 1. Figure 17B shows a photopolymerizable plastic sheet of pattern D, which is composed of one layer of Bioink 2 sandwiched between two layers of Bioink 1. [Figure 18] FIG. 18 shows the stress relief of the mesh and layering design. [Figure 19] FIG. 19 includes FIG. 19A, FIG. 19B, FIG. 19C, FIG. 19D, FIG. 19E, and FIG. 19F and shows the results of DMA. FIG. 19A shows the stress of 3.0mm Beehive compared to Invisalign. FIG. 19B shows the stress of 1.5mm Beehive compared to Invisalign. FIG. 19C shows the stress comparison of Microstructure to Invisalign. FIG. 19D shows the residual stress percentage of 3.0mm Beehive compared to Invisalign. FIG. 19E shows the residual stress percentage of 1.5mm Beehive compared to Invisalign. FIG. 19F shows the residual stress percentage comparison of Microstructure to Invisalign. [Figure 20] FIG. 20 shows stereolithographic polymerization of photocurable resins using a bottom-up approach using a scanning laser (left) or a top-down deposition using digital light projection (right) (Chia et al., 2015, J. Biomed. Mater. Res.-Part B Appl. Biomater., 103: 1415-1423). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Detailed Description of the Invention It should be understood that the drawings and description of the present invention have been simplified to illustrative elements that are pertinent for a clear understanding of the present invention, while many other elements found in photocurable resin compositions, and methods of making and using such materials, have been omitted for purposes of clarity. Those skilled in the art may recognize that other elements and / or steps are desirable and / or necessary in the practice of the present invention. However, such elements and / or steps are not described herein because they are well known in the art and would not contribute to a thorough understanding of the present invention. The disclosure herein is intended to include all variations and modifications of such elements and methods known to those skilled in the art.
[0013] As used herein, each of the following terms has the meaning associated with it in this section. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0014] The articles "a" and "an" are used herein to refer to one or to more than one (i.e., to at least one) of the grammatical object of the article. For example, "an element" means one element or more than one element.
[0015] The term "about" as used herein will be understood by those of ordinary skill in the art and will vary to some extent depending on the context in which it is used. When used herein with respect to measurable values, such as amounts, durations, etc., the term "about" is intended to encompass variations of ±20% or ±10%, more preferably ±5%, even more preferably ±1%, and even more preferably ±0.1% from the specified value, as such variations are appropriate for the practice of the methods disclosed herein.
[0016] Throughout this disclosure, various aspects of the invention may be expressed in a range format. It should be understood that the description in range format is merely for convenience and brevity and should not be construed as an inflexible limitation on the scope of the invention. Thus, the description of a range should be considered to include all the specifically disclosed possible subranges and individual numerical values within that range. For example, the description of a range such as 1-6 should be considered to include the specifically disclosed subranges, such as 1-3, 1-4, 1-5, 2-4, 2-6, 3-6, etc., and individual numerical values within that range, such as 1, 2, 2.7, 3, 4, 5, 5.3, and 6. This applies regardless of the breadth of the range.
[0017] explanation In one aspect, the present invention relates to a photocurable resin composition. In a second aspect, the present invention relates to a method of making the photocurable resin composition. In another aspect, the present invention relates to a method of making an article comprising a photocurable resin. In a fourth aspect, the present invention relates to a method of assembling 3D printed photocurable resin to form an article.
[0018] Photocurable resin composition In one aspect, the present invention relates to a photocurable resin composition. In one embodiment, the photocurable resin composition comprises a first compound comprising one or more double bonds susceptible to polymerization. In one embodiment, the first compound comprises the reaction product of one or more isocyanate-reactive compounds comprising a double bond and one or more diisocyanates.Exemplary diisocyanates include, but are not limited to, 2,2,4-trimethylhexamethylene-1,6-diisocyanate; hexamethylene-1,6-diisocyanate (FIDI); cyclohexyl-1,4-diisocyanate; 4,4'-methylene-bis(cyclohexyl isocyanate); 1,1'-methylenebis(4-isocyanato)cyclohexane; isophorone diisocyanate; 4,4'-methylenediphenyl diisocyanate (MDI). );1,4-Tetramethylene diisocyanate;meta- and para-tetramethylxylene diisocyanate;1,4-Phenylene diisocyanate;2,4' and 4,4'-Diphenylmethane diisocyanate;3-Methylhexane-1,6-diisocyanate;3-Ethyl-1,6-hexane diisocyanate;5-Methyl-1,9-nonane diisocyanate;5-Ethyl-1,10-decane diisocyanate;10-Hexyl-1,2,4-tetracosane diisocyanate ;2,3-Dimethyl-1,6-hexane diisocyanate;2,4-Dimethyl-1,8-octane diisocyanate;2,4,6-Trimethyl-1,7-heptane diisocyanate;2,3-Dimethyl-5-ethyl-1,8-octane diisocyanate;2-Methyl-4,6,8,10-tetrapropyl-1,12-dodecane diisocyanate;1,6-Hexane diisocyanate (HDI);1,8-Octamethylene diisocyanate, Tetramethylxylene diisocyanate (TMXDI); 4,4'-dicyclohexylmethane diisocyanate (HMDI); 3,3'-dimethyl-4,4'biphenylene diisocyanate; 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate; 4-bromo-6-methyl-1,3-phenylene diisocyanate; 2,4-toluene diisocyanate; 2,5-toluene diisocyanate; 2,6-toluene diisocyanate; 1,5-naphthalene diisocyanate; and combinations thereof.
[0019] In one embodiment, the isocyanate-reactive compound containing a double bond comprises a hydroxyacrylate or a hydroxymethacrylate (ie, a hydroxy(meth)acrylate).Exemplary hydroxy(meth)acrylates include, but are not limited to, 2-hydroxyethyl(meth)acrylate; 2-hydroxypropyl(meth)acrylate; 3-hydroxypropyl(meth)acrylate; 4-hydroxybutyl(meth)acrylate; 8-hydroxyoctyl(meth)acrylate; 12-hydroxydodecanoyl(meth)acrylate; 2-hydroxy-3-chloropropyl(meth)acrylate; 2-hydroxy-3-acryloxypropyl(meth)acrylate; 2-hydroxy-B-methacryloxypropyl(meth)acrylate; 2-hydroxy-3-allyloxypropyl(meth)acrylate; 2-hydroxy-3-cinnamylpropyl(meth)acrylate; 2-hydroxy-3-phenoxypropyl(meth)acrylate; 2-hydroxy-3-(o-chlorophenoxy)propyl(meth)acrylate; 2-hydroxy-3-(p-chlorophenoxy)propyl(meth)acrylate. 2-Hydroxy-3-(2,4-dichlorophenoxy)propyl(meth)acrylate;2-Hydroxy-3-acetoxypropyl acrylate;2-Hydroxy-3-propionoxypropyl(meth)acrylate;2-Hydroxy-3-chloroacetoxypropyl acrylate;2-Hydroxy-3-dichloroacetoxypropyl(meth)acrylate;2-Hydroxy-3-trichloroacetoxypropyl(meth)acrylate;2-Hydroxy-3-benzoyl acrylate 2-hydroxy-3-(o-chlorobenzoxy)propyl (meth)acrylate; 2-hydroxy-3-(p-chlorobenzoxy)propyl (meth)acrylate; 2-hydroxy-3-(2,4-dichlorobenzoxy)propyl (meth)acrylate; 2-hydroxy-3-(3,4-dichlorobenzoxy)propyl (meth)acrylate; 2-hydroxy-3-(2,4,6-trichlorophenoxy)propyl (meth)acrylate; 2-hydroxy-3-(2,4,5-trichlorophenoxy)propyl (meth)acrylate; 2-hydroxy-3-(o-chlorophenoxyacetoxy)propyl (meth)acrylate; poly(propylene glycol) (meth)acrylate; poly(ethylene glycol) (meth)acrylate and combinations thereof.
[0020] In one embodiment, the isocyanate-reactive compound containing a double bond comprises an unsaturated carboxylic acid. Exemplary unsaturated carboxylic acids include, but are not limited to, maleic acid, fumaric acid, citraconic acid, mesaconic acid, itanconic acid, glutaconic acid, muconic acid, aconitic acid, crotonic acid, alpha-linolenic acid, stearidonic acid, eicosapentaenoic acid, docosahexaenoic acid, linoleic acid, gamma-linolenic acid, dihomo-gamma-linolenic acid, arachidonic acid, docosatetraenoic acid, palmitoleic acid, vaccenic acid, paulic acid, oleic acid, elaidic acid, gondoic acid, erucic acid, nervonic acid, mead acid, and combinations thereof.
[0021] In one embodiment, the isocyanate-reactive compound containing a double bond comprises an unsaturated anhydride. Exemplary unsaturated anhydrides include, but are not limited to, maleic anhydride, fumaric anhydride, citraconic anhydride, itaconic anhydride, chloromaleic anhydride, methoxymaleic anhydride, ethylmaleic anhydride, and combinations thereof.
[0022] In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 20:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 18:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 16:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 14:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 12:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 10:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 8:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 6:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 1:1 and 4:1. In one embodiment, the molar ratio of the isocyanate-reactive compound containing a double bond to the diisocyanate is between 2:1 and 3:1.
[0023] In one embodiment, the photocurable resin composition includes a second compound that includes one or more double bonds susceptible to polymerization. In one embodiment, the second compound includes a diacrylate or dimethacrylate (i.e., a di(meth)acrylate). Exemplary di(meth)acrylates include, but are not limited to, triethylene glycol di(meth)acrylate (TEG DMA), di(ethylene glycol) di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, di(propylene glycol) di(meth)acrylate, butane glycol di(meth)acrylate, glycerol di(meth)acrylate, bisphenol A di(meth)acrylate, 1,4-phenylene di(meth)acrylate, butane diol di(meth)acrylate, hexane diol dimethacrylate, and combinations thereof.
[0024] In one embodiment, the second compound comprises a triacrylate or a trimethacrylate (ie, a tri(meth)acrylate). Exemplary tri(meth)acrylates include, but are not limited to, 1,1-trimethylolpropane tri(meth)acrylate; ethoxylated or propoxylated 1,1,1-trimethylolpropane tri(meth)acrylate; ethoxylated or propoxylated glycerol tri(meth)acrylate; pentaerythritol monohydroxy tri(meth)acrylate; ethoxylated trimethylolpropane tri(meth)acrylate; ethoxylated (9) trimethylolpropane tri(meth)acrylate; pentaerythritol tri(meth)acrylate, propoxylated (3) glyceryl tri(meth)acrylate; propoxylated (3) trimethylolpropane tri(meth)acrylate; tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate; and combinations thereof.
[0025] In one embodiment, the second compound comprises an unsaturated carboxylic acid. Exemplary unsaturated carboxylic acids are described elsewhere herein. In one embodiment, the second compound comprises an unsaturated anhydride. Exemplary unsaturated anhydrides are described elsewhere herein.
[0026] In one embodiment, the photocurable resin composition includes an additional compound that includes one or more double bonds susceptible to polymerization. Exemplary additional compounds include unsaturated carboxylic acids, unsaturated acid anhydrides, di(meth)acrylates, tri(meth)acrylates, and combinations thereof. Exemplary unsaturated carboxylic acids, unsaturated acid anhydrides, di(meth)acrylates, and tri(meth)acrylates are described elsewhere herein.
[0027] In one embodiment, the photocurable resin composition includes one or more photoinitiators. Exemplary photoinitiators include, but are not limited to, 1-hydroxy-cyclohexyl-phenyl-ketone; diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide; bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide and other acylphosphines; phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO); 2-methyl-1-( 4-Methylthio)phenyl-2-(4-morpholinyl)-1-propanone;1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methylpropan-1-one;2-Benzyl 2-dimethylamino 1-(4-morpholinophenyl)-butanone-1;2-Hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)-phenyl)-2-methylpropan-1-one;2-Dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl- phenyl)-butan-1-one;Titanocene;Isopropylthioxanthone;1-Hydroxy-cyclohexyl phenyl ketone;Benzophenone;2,4,6-Trimethylbenzophenone;4-Methylbenzophenone;Diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide;2,4,6-Trimethylbenzoylphenylphosphinic acid ethyl ester;Oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone);2-Hydroxy-2-methyl 1-phenyl-1-propanone;Benzil dimethyl ketal;Benzil;2,3-boranedione (camphorquinone);9-fluorene;2-methylanthraquinone;Diacetyl;Benzanthrone;Thioxanthen-9-one;Benzoin isobutyl ether;2-Hydroxy-2,2-dimethyl-acetophenone;2,4,5,7-tetrabromofluorescein (eosin Y);4,5-dibromo-2,7-dinitrofluorescein disodium salt;Riboflavin;Fluorescein;n 5-2,4-Cyclopentadien-1-yl)((1,2,3,4,5,6-n)-(1-methylethyl)benzene)-iron(+)-hexafluorophosphate(-1);2-Benzyl-2-n-dimethylamino-1-(4-morpholinophenyl)-1-butanone;Bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide (DMBAPO);2-Hydroxy-2-methyl-1-phenylpropan-1-one (HMMP);4-(2-hydroxyethoxy)phenyl-(2-hydro 2,2-dimethoxy-2-phenylacetophenone (BDK); 2-methyl-1-(4-(methylthio)phenyl)-2-morpholinopropan-1-one (MMMP); 2-hydroxy-2-methyl-1-phenyl-propan-1-one (HMPP); 5,7-diiodo-3-butoxy-6-fluorene; 2,4,5,7-tetraiodo-3-hydroxy-6-fluorene; 2,4,5,7-tetraiodo-9-cyano-3-hydroxy-6-fluorene; and combinations thereof.
[0028] In one embodiment, the photocurable resin composition includes one or more stabilizers. Exemplary stabilizers include, but are not limited to, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, hexadecylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, diaminopentane, diaminohexane, diaminoheptane, diaminooctane, diaminononane, diaminodecane, diaminooctane, dipropylamine, dibutylamine, dipentylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, methylpropylamine, ethylpropylamine, propylbutylamine, ethylbutylamine, ethylpentylamine, propylpentylamine, butylpentylamine, tributylamine, trihexylamine, polyethylene glycol, polyvinylpyridine, polyvinylpyrrolidone, butanethiol, pentanethiol, hexadecylamine ... thiol, heptanethiol, octanethiol, decanethiol, dodecanethiol, 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, O-methyl xanthate, O-ethyl xanthate, O-propyl xanthate, O-butyl xanthate, O-pentyl xanthate, O-hexyl xanthate, O-heptyl xanthate, O-octyl xanthate, O-nonyl xanthate, O-decyl xanthate, hexanthic acid, O-undecylxanthic acid, O-dodecylxanthic acid, bis(2,2,6,6-tetramethyl-1-octyloxy-4-piperidyl)sebacate; bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate; methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate; dimethylsebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, and combinations thereof.
[0029] In one embodiment, the photocurable resin composition includes one or more dyes. Exemplary dyes include, but are not limited to, chromium-cobalt-aluminum oxide; ferric ammonium citrate; pyrogallol; logwood extract; 1,4-bis[(2-hydroxy-ethyl)amino]-9,10-anthracenedione bis(2-propenoic) ester copolymer; 1,4-bis[(2-methylphenyl)amino]-9,10-anthracenedione; 1,4-bis[4-(2-methacryloxyethyl)phenylamino]anthraquinone copolymer; carbazole violet; chlorophyllin-copper complex; chromium oxide green; CI Vat Orange 1; 2-[[2,5-diethoxy-4-[(4-methylphenyl)thiol]phenyl]azo]-1,3,5-benzenetriol; 7,16-dichloro-6,15-dihydro-5,9,14,18-anthrazinetetrone; Reactive Black 5; Reactive Blue 21; Reactive Orange 78; Reactive Yellow 15; Reactive Blue No. 19; Reactive Blue No. 4; CI Reactive Red 11; CI Reactive Yellow 86; CI Reactive Blue 163; CI Reactive Red 180; 4-[(2,4-dimethylphenyl)azo]-2,4-dihydro-5-methyl-2-phenyl-3H-pyrazol-3-one; 6-ethoxy-2-(6-ethoxy-3-oxobenzo[b]thien-2(3H)-ylidene)benzo[b]thiophen-3(2H)-one; Phthalocyanine Green; iron oxide; titanium dioxide; and combinations thereof.
[0030] In one embodiment, the photocurable resin composition includes a first photocurable resin composition and a second photocurable resin composition. In one embodiment, the first photocurable resin composition includes 100 wt% to 50 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the first photocurable resin composition includes 100 wt% to 60 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the first photocurable resin composition includes 100 wt% to 70 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the first photocurable resin composition includes 90 wt% to 70 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the first photocurable resin composition comprises 85 wt% to 75 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the first photocurable resin comprises a compound formed from the reaction of one or more hydroxy(meth)acrylates with one or more diisocyanates. Exemplary hydroxy(meth)acrylates are described elsewhere herein. In one embodiment, the compound formed from the reaction of one or more hydroxy(meth)acrylates with one or more diisocyanates comprises a urethane(meth)acrylate.
[0031] In one embodiment, the first photocurable resin composition contains 5 wt% to 50 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition contains 5 wt% to 45 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition contains 5 wt% to 40 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition contains 5 wt% to 35 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition contains 5 wt% to 30 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition contains 5 wt% to 25 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition contains 10 wt% to 25 wt% of the second compound containing one or more double bonds. In one embodiment, the first photocurable resin composition includes a second compound that includes a di(meth)acrylate. Exemplary di(meth)acrylates are described elsewhere herein.
[0032] In one embodiment, the first photocurable resin composition comprises less than 30 wt.% photoinitiator. In one embodiment, the first photocurable resin composition comprises less than 25 wt.% photoinitiator. In one embodiment, the first photocurable resin composition comprises less than 20 wt.% photoinitiator. In one embodiment, the first photocurable resin composition comprises less than 15 wt.% photoinitiator. In one embodiment, the first photocurable resin composition comprises less than 10 wt.% photoinitiator. In one embodiment, the first photocurable resin composition comprises less than 5 wt.% photoinitiator.
[0033] In one embodiment, the first photocurable resin composition comprises less than 30 wt.% of a stabilizer. In one embodiment, the first photocurable resin composition comprises less than 25 wt.% of a stabilizer. In one embodiment, the first photocurable resin composition comprises less than 20 wt.% of a stabilizer. In one embodiment, the first photocurable resin composition comprises less than 15 wt.% of a stabilizer. In one embodiment, the first photocurable resin composition comprises less than 10 wt.% of a stabilizer. In one embodiment, the first photocurable resin composition comprises less than 5 wt.% of a stabilizer.
[0034] In one embodiment, the second photocurable resin composition contains 10 wt% to 60 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the second photocurable resin composition contains 20 wt% to 60 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the second photocurable resin composition contains 30 wt% to 60 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the second photocurable resin composition contains 40 wt% to 60 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the second photocurable resin composition comprises 45 wt% to 55 wt% of a compound formed from the reaction of one or more isocyanate-reactive compounds containing a double bond with one or more diisocyanates. In one embodiment, the second photocurable resin comprises a compound formed from the reaction of one or more hydroxy(meth)acrylates with one or more diisocyanates. Exemplary hydroxy(meth)acrylates are described elsewhere herein. In one embodiment, the compound formed from the reaction of one or more hydroxy(meth)acrylates with one or more diisocyanates comprises a urethane(meth)acrylate.
[0035] In one embodiment, the second photocurable resin composition contains 5 wt% to 50 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition contains 5 wt% to 45 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition contains 5 wt% to 40 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition contains 5 wt% to 35 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition contains 5 wt% to 30 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition contains 5 wt% to 25 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition contains 10 wt% to 25 wt% of the second compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 12 wt% to 22 wt% of a second compound including one or more double bonds. In one embodiment, the second photocurable resin composition includes a second compound including a di(meth)acrylate. Exemplary di(meth)acrylates are described elsewhere herein.
[0036] In one embodiment, the second photocurable resin composition includes an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 5 wt% to 50 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 10 wt% to 50 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 15 wt% to 50 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 20 wt% to 50 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 25 wt% to 50 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 25 wt% to 45 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 25 wt% to 40 wt% of an additional compound containing one or more double bonds. In one embodiment, the second photocurable resin composition includes 25 wt% to 35 wt% of an additional compound that includes one or more double bonds. In one embodiment, the second photocurable resin composition includes an additional compound that includes a tri(meth)acrylate. Exemplary tri(meth)acrylates are described elsewhere herein.
[0037] In one embodiment, the second photocurable resin composition comprises less than 30 wt.% photoinitiator. In one embodiment, the second photocurable resin composition comprises less than 25 wt.% photoinitiator. In one embodiment, the second photocurable resin composition comprises less than 20 wt.% photoinitiator. In one embodiment, the second photocurable resin composition comprises less than 15 wt.% photoinitiator. In one embodiment, the second photocurable resin composition comprises less than 10 wt.% photoinitiator. In one embodiment, the second photocurable resin composition comprises less than 5 wt.% photoinitiator.
[0038] In one embodiment, the second photocurable resin composition comprises less than 30 wt.% of a stabilizer. In one embodiment, the second photocurable resin composition comprises less than 25 wt.% of a stabilizer. In one embodiment, the second photocurable resin composition comprises less than 20 wt.% of a stabilizer. In one embodiment, the second photocurable resin composition comprises less than 15 wt.% of a stabilizer. In one embodiment, the second photocurable resin composition comprises less than 10 wt.% of a stabilizer. In one embodiment, the second photocurable resin composition comprises less than 5 wt.% of a stabilizer.
[0039] Method for preparing a photocurable resin composition In one aspect, the present invention relates to a method of making a photocurable resin composition. An exemplary process 100 is shown in FIG. 1. In step 110, a diisocyanate is provided. In step 120, an isocyanate-reactive compound containing a double bond is provided. In step 130, the diisocyanate and the isocyanate-reactive compound are combined and reacted to form a first compound containing one or more double bonds susceptible to polymerization. In step 140, the first compound is mixed with a second compound containing one or more double bonds susceptible to polymerization to form a mixture. In step 150, a photoinitiator is added to the mixture.
[0040] In step 110, the diisocyanate may be any diisocyanate known to one of skill in the art. Exemplary diisocyanates are described elsewhere herein. In one embodiment, the diisocyanate is a solid. In one embodiment, the diisocyanate is mixed with a solvent. In one embodiment, the diisocyanate is mixed with an organic solvent. Exemplary organic solvents include, but are not limited to, pentane, hexane, diethyl ether, tetrahydrofuran, acetone, benzene, toluene, methanol, ethanol, isopropanol, ethyl acetate, DMF, dichloromethane, chloroform, and combinations thereof. In one embodiment, the diisocyanate is heated. In one embodiment, the diisocyanate is heated to melt. In one embodiment, the diisocyanate is heated between 10° C. and 100° C. In one embodiment, the diisocyanate is heated between 10° C. and 90° C. In one embodiment, the diisocyanate is heated between 10° C. and 80° C. In one embodiment, the diisocyanate is heated between 10° C. and 70° C. In one embodiment, the diisocyanate is heated at between 20°C and 70°C. In one embodiment, the diisocyanate is heated at between 30°C and 70°C. In one embodiment, the diisocyanate is heated at between 40°C and 70°C. In one embodiment, the diisocyanate is heated at between 50°C and 70°C. In one embodiment, the diisocyanate is heated at between 55°C and 65°C.
[0041] In step 120, the isocyanate-reactive compound containing a double bond may be any isocyanate-reactive compound containing a double bond known to one of skill in the art. Exemplary isocyanate-reactive compounds are described elsewhere herein. In one embodiment, the isocyanate-reactive compound is mixed with a solvent. In one embodiment, the isocyanate-reactive compound is mixed with an organic solvent. Exemplary organic solvents are described elsewhere herein.
[0042] In step 130, the diisocyanate and the isocyanate-reactive compound containing a double bond may be combined using any method known to one of skill in the art. In one embodiment, the isocyanate-reactive compound is added dropwise to the diisocyanate. In one embodiment, the isocyanate-reactive compound is added all at once to the diisocyanate. In one embodiment, the diisocyanate is stirred as the isocyanate-reactive compound is being added. In one embodiment, the diisocyanate and the isocyanate-reactive compound are reacted at room temperature. In one embodiment, the diisocyanate and the isocyanate-reactive compound are reacted at an elevated temperature. In one embodiment, the reaction occurs at a temperature between 10°C and 100°C. In one embodiment, the reaction occurs at a temperature between 10°C and 90°C. In one embodiment, the reaction occurs at a temperature between 10°C and 80°C. In one embodiment, the reaction occurs at a temperature between 10°C and 70°C. In one embodiment, the reaction occurs at a temperature between 20°C and 70°C. In one embodiment, the reaction occurs at a temperature between 30°C and 70°C. In one embodiment, the reaction occurs at a temperature between 40°C and 70°C. In one embodiment, the reaction occurs at a temperature between 50° C. and 70° C. In one embodiment, the reaction occurs at a temperature between 55° C. and 65° C. In one embodiment, the solvent present during the reaction between the diisocyanate and the isocyanate-reactive compound is removed. The solvent is removed using any method known to one of skill in the art. In one embodiment, the solvent is removed using filtration. In one embodiment, the solvent is removed by rotary evaporation.
[0043] In step 140, the second compound comprising one or more double bonds susceptible to polymerization may be any compound comprising one or more double bonds susceptible to polymerization known to one of skill in the art. Exemplary compounds comprising one or more double bonds susceptible to polymerization are described elsewhere herein. In one embodiment, the second compound is mixed with a solvent. In one embodiment, the second compound is mixed with an organic solvent. Exemplary organic solvents are described elsewhere herein.
[0044] In some embodiments, the step of mixing the first compound with the second compound comprising one or more double bonds susceptible to polymerization to form a mixture further comprises step 142, where an additional compound comprising one or more double bonds susceptible to polymerization is added to the mixture. The additional compound comprising one or more double bonds susceptible to polymerization may be any compound comprising one or more double bonds susceptible to polymerization known to one of skill in the art. Exemplary additional compounds are described elsewhere herein. In one embodiment, the additional compound is mixed with a solvent. In one embodiment, the additional compound is mixed with an organic solvent. Exemplary organic solvents are described elsewhere herein.
[0045] In step 150, the photoinitiator may be any photoinitiator known to one of skill in the art. Exemplary photoinitiators are described elsewhere herein. In one embodiment, the photoinitiator is mixed with a solvent. In one embodiment, the photoinitiator is mixed with an organic solvent. Exemplary organic solvents are described elsewhere herein.
[0046] In some embodiments, adding a photoinitiator to the mixture further comprises step 152, where a stabilizing agent is added to the mixture. The stabilizing agent may be any stabilizing agent known to one of skill in the art. Exemplary stabilizing agents are described elsewhere herein. In one embodiment, the stabilizing agent is mixed with a solvent. In one embodiment, the stabilizing agent is mixed with an organic solvent. Exemplary organic solvents are described elsewhere herein.
[0047] In some embodiments, adding a photoinitiator to the mixture further comprises step 154, where a dye is added to the mixture. The dye may be any dye known to one of skill in the art. Exemplary dyes are described elsewhere herein. In one embodiment, the dye is mixed with a solvent. In one embodiment, the dye is mixed with an organic solvent. Exemplary organic solvents are described elsewhere herein. In one embodiment, the dye is mixed with an aqueous solvent. Exemplary aqueous solvents include, but are not limited to, water, distilled water, deionized water, salt water, and combinations thereof.
[0048] Method for 3D printing photocurable resin composition In one aspect, the present invention relates to a method for 3D printing a photocurable resin composition. The 3D printing technique may be any known to one of skill in the art. Exemplary 3D printing techniques include, but are not limited to, continuous liquid interface manufacturing (CLIP), stereolithography, digital light processing, fused deposition modeling, selective laser sintering, selective laser melting, thin film additive manufacturing, digital beam melting, carbon printing, and material jetting (such as Polyjet 3D printing). In one embodiment, the photocurable resin is printed using stereolithography. In one embodiment, the stereolithography printer is a bottom-up method that includes a scanning laser. In one embodiment, the stereolithography printer is a top-down method that includes digital light projection. In one embodiment, the photocurable resin is printed using material jetting.
[0049] In one embodiment, the 3D printer uses STL format software. In one embodiment, the 3D printer uses ML format software. In one embodiment, the 3D printer prints impressions taken using a 3D scanner that are then digitized and converted into an STL or ML file.
[0050] In one embodiment, the print speed is between 1 mm / hour and 100 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 90 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 80 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 70 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 60 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 50 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 40 mm / hour. In one embodiment, the print speed is between 1 mm / hour and 30 mm / hour. In one embodiment, the print speed is between 10 mm / hour and 30 mm / hour. In one embodiment, the print speed is between 12 mm / hour and 25 mm / hour.
[0051] In one embodiment, the photocurable resin is printed or deposited onto a support. The support may be any support known to one of skill in the art. In one embodiment, the photocurable resin is printed to form a support structure before the desired photocurable resin structure is printed onto the support structure. In one embodiment, the desired printed photocurable resin structure is held to the support structure using supports. In one embodiment, the support structure is attached to a 3D printing platform.
[0052] In one embodiment, the photocurable resin is irradiated during the printing process. In one embodiment, the photocurable resin is irradiated with UV light. In one embodiment, the photocurable resin is irradiated with visible light. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 750 nm. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 700 nm. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 650 nm. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 600 nm. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 550 nm. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 500 nm. In one embodiment, the photocurable resin is irradiated with light between 380 nm and 450 nm. In one embodiment, the photocurable resin is irradiated with light between 395 nm and 415 nm. In one embodiment, the irradiation is provided by a laser. In one embodiment, the photocurable resin composition is irradiated continuously during printing. In one embodiment, the photocurable resin composition is irradiated discontinuously during printing. In one embodiment, the irradiation photopolymerizes the photocurable composition. In one embodiment, the irradiation cures the photocurable composition.
[0053] In one embodiment, when the composition is irradiated, the photocurable composition forms a thin layer. In one embodiment, the layer is 5 μm to 500 μm in height. In one embodiment, the layer is 5 μm to 450 μm in height. In one embodiment, the layer is 5 μm to 400 μm in height. In one embodiment, the layer is 5 μm to 350 μm in height. In one embodiment, the layer is 5 μm to 300 μm in height. In one embodiment, the layer is 5 μm to 250 μm in height. In one embodiment, the layer is 5 μm to 200 μm in height. In one embodiment, the layer is 5 μm to 150 μm in height. In one embodiment, the layer is 5 μm to 100 μm in height. In one embodiment, the layer is 40 μm to 100 μm in height. In one embodiment, the layer is 40 μm to 60 μm in height.
[0054] In one embodiment, the length of irradiation of each layer of photocurable resin depends on the desired height of the resin layer. In one embodiment, layers with a height of 40 μm to 60 μm are irradiated for 1 second to 1 minute. In one embodiment, layers with a height of 40 μm to 60 μm are irradiated for 1 second to 50 minutes. In one embodiment, layers with a height of 40 μm to 60 μm are irradiated for 1 second to 40 minutes. In one embodiment, layers with a height of 40 μm to 60 μm are irradiated for 1 second to 30 minutes. In one embodiment, layers with a height of 40 μm to 60 μm are irradiated for 1 second to 20 minutes. In one embodiment, layers with a height of 40 μm to 60 μm are irradiated for 5 seconds to 15 minutes.
[0055] In one embodiment, the photocurable resin is printed to form a solid structure. In one embodiment, the photocurable resin is printed to form a solid coating. In one embodiment, both the solid structure and the solid coating are printed. In one embodiment, the photocurable resin used to print the solid coating has a different composition than the photocurable resin used to print the solid structure. In one embodiment, the photocurable resin used to print the solid structure comprises a mixture of two or more photocurable resins having different compositions. In one embodiment, the photocurable resin used to print the solid coating comprises a mixture of two or more photocurable resins having different compositions. In one embodiment, the photocurable resin used to print the solid coating comprises a gradient of two or more photocurable resins having different compositions. In one embodiment, the photocurable resin used to print the solid coating comprises a gradient of two or more photocurable resins having different compositions. In one embodiment, the solid coating and the solid structure are 3D printed separately and then assembled after printing. In one embodiment, a solid structure is printed to form an internal structure and then a solid coating is printed in the form of a coating / covering on one or more surfaces of the internal structure.
[0056] In one embodiment, the photocurable resin composition is printed to form a structure that includes a particular microstructure. In one embodiment, the microstructure is continuous throughout the 3D printed structure. In one embodiment, the microstructure is discontinuous throughout the 3D printed structure. In one embodiment, the microstructure includes areas of the particular microstructure connected to areas lacking the particular microstructure. In one embodiment, the microstructure includes pores or holes. In one embodiment, the microstructure includes a network structure. In one embodiment, both the solid coating and the microstructure are printed. The solid coating is described elsewhere herein. In one embodiment, the photocurable resin used to print the microstructure has a different composition than the photocurable resin used to print the solid coating. In one embodiment, the photocurable resin used to print the microstructure includes a mixture of two or more photocurable resins having different compositions. In one embodiment, the photocurable resin used to print the microstructure includes a gradient of two or more photocurable resins having different compositions. In one embodiment, the solid coating and the microstructure are 3D printed separately and then assembled after printing. In one embodiment, the microstructure is printed to form an internal structure and then a solid coating is printed in the form of a coating / covering on one or more surfaces of the internal structure.
[0057] The microstructures may be created during the 3D printing process. In one embodiment, the microstructures may be created by physical means, chemical means, biological means, and combinations thereof. In one embodiment, the microstructures are formed during the 3D printing process. In one embodiment, the solid portions of the microstructures are formed by irradiating certain areas of the photocurable resin. In one embodiment, the pores or holes of the microstructures are formed by not irradiating certain areas of the photocurable resin. In one embodiment, the microstructures are created by chemical means. In one embodiment, the chemical means includes voxel level printing. In one embodiment, the chemical means includes sub-level printing. In one embodiment, the microstructures are created by physical means. Exemplary physical means include, but are not limited to, mechanical means, optical means, thermal means, electrical means, electromagnetic manipulation, and combinations thereof. In one embodiment, the microstructures are created by biological means. Exemplary biological means include, but are not limited to, biochemical reactions, enzymatic reactions, living biological cells, synthetic biological cells, viruses, vesicles, and combinations thereof. In one embodiment, the biological means responds to an external stimulus. In one embodiment, the biological means is responsive to a local stimulus.
[0058] In one embodiment, an internal structure is printed and a solid coating covering one or more sides of the internal structure is simultaneously printed. In one embodiment, the internal structure includes a microstructure. In one embodiment, the internal structure includes a solid structure. In one embodiment, the internal structure includes a mixture of microstructured regions and solid regions. In one embodiment, the internal structure and the solid coating are printed using stereolithography. In one embodiment, the internal structure and the solid coating include different photocurable resin compositions. In one embodiment, the different photocurable resin compositions are placed in the same 3D printing bath. In one embodiment, the different photocurable resins include different photoinitiators that polymerize the photocurable resins at different wavelengths. In one embodiment, the different photocurable resins include different photoinitiators that cure the photocurable resins at different wavelengths. In one embodiment, the different photocurable resin compositions are placed in separate 3D printing baths. In one embodiment, a layer of the internal structure is 3D printed from one bath of photocurable resin and then a layer of the coating is 3D printed from a second, separate bath.
[0059] In one embodiment, the internal features and solid coating are printed using material jetting. In one embodiment, the internal features and solid coating can be printed using material jetting as described elsewhere herein. In one embodiment, the internal features and solid coating can be printed using materials jetted simultaneously using one or more printheads. In one embodiment, the material jetting deposits small droplets of one or more photocurable resins that are then polymerized and / or cured immediately after depositing them. In one embodiment, the material jetting deposits small droplets of one or more photocurable resins that are then polymerized and / or cured as they are deposited.
[0060] In one embodiment, the internal structure and solid coating are printed using carbon printing. In one embodiment, the internal structure and solid coating can be printed using carbon printing as described elsewhere herein. In one embodiment, the photocurable resin is printed using carbon printing from a bath of a first photocurable resin. In one embodiment, the photocurable resin is printed using carbon printing from a bath of a first photocurable resin, where the bath includes one or more print heads. In one embodiment, the one or more print heads dispense one or more additional photocurable resins into the bath. In one embodiment, the additional photocurable resin(s) have a different composition than the first photocurable resin, but are miscible with the first photocurable resin. In one embodiment, the one or more print heads dispense different amounts of the one or more additional photocurable resins into the bath throughout the printing process, such that a gradient of the first photocurable resin relative to the additional photocurable resin(s) is formed throughout the resulting 3D printed article.
[0061] In one embodiment, the photocurable resin is printed using 3D printing to form an article including a microstructure, a solid coating structure, or a combination of the two structures. In one embodiment, the photocurable resin is printed using 3D printing to form an article including a solid structure, a solid coating structure, or a combination of the two structures. In one embodiment, the article is washed with a solvent to remove excess resin after printing is completed. The solvent can be any solvent known to those skilled in the art. Exemplary solvents include, but are not limited to, water, distilled water, water, deionized water, hexane, diethyl ether, acetone, methanol, ethanol, isopropanol, dichloromethane, toluene, THF, benzene, ethyl acetate, and combinations thereof.
[0062] In one embodiment, the 3D printed article is removed from the support by cutting the struts. In one embodiment, after the struts are cut, the surface of the 3D printed article is smoothed. In one embodiment, the surface of the 3D printed article is smoothed by grinding. In one embodiment, the surface of the 3D printed article is smoothed using a dental drill. In one embodiment, the dental drill includes a rubber point. In one embodiment, the dental drill includes one or more disk attachments. In one embodiment, the support is dissolved. In one embodiment, the support is dissolved with an acidic solution. Exemplary acids include, but are not limited to, hydrochloric acid, sulfuric acid, acetic acid, nitric acid, citric acid, phosphoric acid, carbonic acid, boric acid, and combinations thereof. In one embodiment, the support is dissolved with a basic solution including a base. Exemplary bases include, but are not limited to, sodium hydroxide, potassium hydroxide, sodium bicarbonate, lithium hydroxide, calcium hydroxide, ammonia, and combinations thereof. In one embodiment, the basic solution includes 0.1 wt % to 50 wt % sodium hydroxide. In one embodiment, the basic solution comprises 0.1 wt% to 40 wt% sodium hydroxide. In one embodiment, the basic solution comprises 0.1 wt% to 30 wt% sodium hydroxide. In one embodiment, the basic solution comprises 0.1 wt% to 20 wt% sodium hydroxide. In one embodiment, the basic solution comprises 0.1 wt% to 10 wt% sodium hydroxide. In one embodiment, the basic solution comprises 1 wt% to 5 wt% sodium hydroxide. In one embodiment, the basic solution further comprises a silicate. In one embodiment, the basic solution comprises 0.1 wt% to 50 wt% sodium silicate. In one embodiment, the basic solution comprises 0.1 wt% to 40 wt% sodium silicate. In one embodiment, the basic solution comprises 0.1 wt% to 30 wt% sodium silicate. In one embodiment, the basic solution comprises 0.1 wt% to 20 wt% sodium silicate. In one embodiment, the basic solution comprises 0.1 wt% to 10 wt% sodium silicate. In one embodiment, the basic solution comprises 0.1 wt% to 3 wt% sodium silicate.
[0063] In one embodiment, the 3D printed article is post-cured. In one embodiment, the 3D printed article is post-cured for 10 seconds to 60 minutes. In one embodiment, the 3D printed article is post-cured for 10 seconds to 50 minutes. In one embodiment, the 3D printed article is post-cured for 10 seconds to 40 minutes. In one embodiment, the 3D printed article is post-cured for 10 seconds to 30 minutes. In one embodiment, the 3D printed article is post-cured for 10 seconds to 20 minutes. In one embodiment, the 3D printed article is post-cured for 10 seconds to 10 minutes. In one embodiment, the 3D printed article is post-cured for 30 seconds to 2 minutes. In one embodiment, the 3D printed article is post-cured by irradiation with UV light. In one embodiment, the 3D printed article is post-cured by irradiation with visible light. In one embodiment, the 3D printed article is post-cured by irradiation with UV light and visible light. In one embodiment, the wavelength of light used for post-curing is determined by the absorption capacity of the photoinitiator used.
[0064] Method for assembling 3D printed light curable resins to form an article In some embodiments, the 3D printed and photocured resin structures are assembled after printing to form an article. In one embodiment, the solid coating structure is connected to the microstructure after 3D printing such that it covers the microstructure on one or more sides to form the desired 3D printed article. In one embodiment, the solid coating structure is connected to the solid structure after 3D printing such that it covers the solid structure on one or more sides to form the desired 3D printed article. In one embodiment, the desired 3D printed article includes an internal structure that includes a particular microstructure or includes a solid structure that is covered on one or more sides by a solid coating.
[0065] In one embodiment, the solid coating structure is held to the internal structure using additional photocurable resin. In one embodiment, additional photocurable resin is applied to the solid coating structure and then the internal structure is placed on top to form the bilayer article. In one embodiment, the bilayer article is irradiated to adhere the internal structure to the solid coating. In one embodiment, the bilayer article is irradiated for 10 seconds to 60 minutes. In one embodiment, the bilayer article is irradiated for 10 seconds to 50 minutes. In one embodiment, the bilayer article is irradiated for 10 seconds to 40 minutes. In one embodiment, the bilayer article is irradiated for 10 seconds to 30 minutes. In one embodiment, the bilayer article is irradiated for 10 seconds to 20 minutes. In one embodiment, the bilayer article is irradiated for 10 seconds to 10 minutes. In one embodiment, the bilayer article is irradiated for 10 seconds to 1 minute. In one embodiment, the bilayer article is irradiated with UV light. In one embodiment, the bilayer article is irradiated with visible light. In one embodiment, the bilayer article is irradiated with UV light. In one embodiment, the bilayer article is irradiated with both UV and visible light. The wavelengths of UV and / or visible light that may be used to irradiate the bilayer article may be any of the wavelengths disclosed elsewhere herein.
[0066] In one embodiment, the side of the internal structure not covered with the solid coating is covered with a second layer solid coating structure to form a three-layer article. In one embodiment, the second layer solid coating structure is held to the internal structure using additional photocurable resin. In one embodiment, the internal structure includes a microstructure, pores within the microstructure are filled with additional photocurable resin, and then a second solid coating structure is placed over the microstructure to form a three-layer article. In one embodiment, the three-layer article is irradiated to adhere the internal structure to the second solid coating structure. In one embodiment, the irradiation further enhances the adhesion of the first solid coating structure to the internal structure. In one embodiment, the three-layer article is irradiated for 10 seconds to 60 minutes. In one embodiment, the three-layer article is irradiated for 10 seconds to 50 minutes. In one embodiment, the three-layer article is irradiated for 10 seconds to 40 minutes. In one embodiment, the three-layer article is irradiated for 10 seconds to 30 minutes. In one embodiment, the three-layer article is irradiated for 10 seconds to 20 minutes. In one embodiment, the tri-layer article is irradiated for between 10 seconds and 10 minutes. In one embodiment, the tri-layer article is irradiated for between 30 seconds and 2 minutes.
[0067] In one embodiment, the three layer article is irradiated with UV light. In one embodiment, the three layer article is irradiated with visible light. In one embodiment, the three layer article is irradiated with UV light. In one embodiment, the three layer article is irradiated with both UV and visible light. The wavelengths of UV and / or visible light that may be used to irradiate the three layer article may be any of the wavelengths disclosed elsewhere herein.
[0068] 3D printed resin items In one aspect, the present invention relates to a 3D printed article. The 3D printed article may include any shape known to one of skill in the art. In one embodiment, the 3D printed article is a medical device. In one embodiment, the 3D printed article is a dental article. In one embodiment, the 3D printed article is a dental aligner. In one embodiment, the 3D printed article is transparent. In one embodiment, the 3D printed article is colored.
[0069] In one embodiment, the 3D printed article includes two or more photocurable resin compositions that have been irradiated or photocured. Exemplary photocurable resin compositions are described elsewhere herein. In one embodiment, the article includes an inner layer including a first resin composition. In one embodiment, the inner layer has a thickness of 0.1 mm to 1.5 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 1.4 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 1.3 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 1.2 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 1.1 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 1.0 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 0.9 mm. In one embodiment, the inner layer has a thickness of 0.1 mm to 0.8 mm. In one embodiment, the inner layer has a thickness of 0.2 mm to 0.8 mm. In one embodiment, the inner layer has a thickness of 0.3 mm to 0.8 mm.
[0070] In one embodiment, the inner layer comprising the first resin composition comprises a microstructure. In one embodiment, the inner layer comprises regions of a microstructure and regions lacking a microstructure. In one embodiment, the microstructure comprises pores or holes. In one embodiment, the pores are uniform in size. In one embodiment, the pores are variable in size. In one embodiment, the pores are 0.1 mm to 50 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 45 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 40 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 35 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 30 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 25 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 20 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 15 mm in inner diameter. In one embodiment, the pores are 0.1 mm to 10 mm in inner diameter. In one embodiment, the pores are between 0.1 mm and 5 mm in inner diameter. In one embodiment, the pores are not regularly spaced. In one embodiment, the pores are regularly spaced. In one embodiment, the microstructure comprises a honeycomb / beehive structure. In one embodiment, the microstructure comprises a mesh structure.
[0071] In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 50 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 45 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 40 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 35 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 30 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 25 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 20 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 15 mm. In one embodiment, the microstructure includes a photocurable resin having an inter-pore thickness of 0.1 mm to 10 mm. In one embodiment, the microstructure comprises a photocurable resin having an inter-pore thickness of 0.1 mm to 3 mm.
[0072] In one embodiment, the inner layer is coated with a second photocurable resin that has been irradiated or photocured. In one embodiment, the second photocurable resin is coated on both sides of the inner layer. In one embodiment, the second photocurable resin is coated on one side of the inner layer. In one embodiment, the photocurable resin coating comprises a solid coating that does not have any pores or holes. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 1 mm. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 0.9 mm. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 0.8 mm. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 0.7 mm. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 0.6 mm. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 0.5 mm. In one embodiment, the photocurable resin coating has a thickness of 0.01 mm to 0.4 mm.
[0073] In one embodiment, the photocurable resin coating is the same resin used for the inner layer. In one embodiment, the photocurable resin coating is a different resin than the first photocurable resin used for the inner layer. In one embodiment, the photocurable resin coating comprises a gradient of photocurable resin compositions. In one embodiment, the inner layer comprises a gradient of photocurable resin compositions. In one embodiment, the photocurable resin coating has a different mechanical strength than the photocurable resin used to form the inner layer. In one embodiment, the photocurable resin used to coat the inner layer has a lower mechanical strength than the photocurable resin used to form the inner layer. In one embodiment, the photocurable resin used to coat the inner layer has a higher mechanical strength than the photocurable resin used to form the inner layer. In one embodiment, the inner layer has varying local mechanical strength at different locations of the article. In one embodiment, the coating has varying local mechanical strength at different locations of the article.
[0074] In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 50 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 45 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 40 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 35 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 30 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 25 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 20 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.1 MPa to 15 MPa when tested with a preload of 0.01 N. In one embodiment, the 3D printed article has an initial stress of 0.45 MPa to 10 MPa when tested with a preload of 0.01 N.
[0075] In one embodiment, the article exhibits 5% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits 10% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits 15% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits 20% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits 25% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits 30% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits 35% to 95% stress relaxation after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits a stress relaxation of 40% to 95% after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits a stress relaxation of 45% to 95% after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits a stress relaxation of 45% to 90% after 2 hours when tested with a preload of 0.01 N. In one embodiment, the article exhibits a stress relaxation of 45% to 85% after 2 hours when tested with a preload of 0.01 N. EXAMPLES
[0076] Experimental Example The invention will now be described with reference to the following examples, which are provided for illustrative purposes only, and the invention is not limited to these examples, but rather encompasses all variations that become evident as a result of the teachings provided herein.
[0077] Materials and Methods Synthesis of photocurable MDI-PEGMA MDI-PEGMA was synthesized using 4,4'-methylenebis(phenylisocyanate) (MDI) (10.00 g, 40.00 mmol) (added in an inert atmosphere, round bottom flask containing a stir bar and heated to 60 °C). Upon dissolution of the MDI reagent, poly(ethylene glycol) methacrylate (PEGMA) (32.55 mL, 100.00 mmol) was added dropwise and reacted at 60 °C for 8 hours. The reaction was then allowed to proceed overnight at room temperature. The synthesized compound (MDI-PEGMA) was collected using a positive displacement pipette and analyzed by proton magnetic resonance spectroscopy ( 1 The compounds were characterized by 1 H NMR (H NMR) and by Fourier Transform Infrared Spectroscopy (FTIR) on a PerkinElmer Spectrum Two FT-IR Spectrometer (Waltham, MA, USA).
[0078] Characterization of MDI-PEGMA Photocurable resins (commonly known as Bioinks) contain urethane-containing compounds that are synthesized in the reaction between the diisocyanate and hydroxyl groups of hydroxy (meth)acrylates. Figure 2 shows a reaction scheme depicting how the synthesis was carried out. MDI was utilized as the diisocyanate agent and PEGMA was chosen as the hydroxyl group-containing reagent due to its acrylate groups that add photoreactivity to the final product, MDI-PEGMA. 1 Examination by H NMR confirms the reaction between the isocyanate and the hydroxyl group (Figure 3). The appearance of an aromatic peak at δ 7.32 ppm (C), representing four aromatic protons, confirms the reaction of MDI with PEGMA. FTIR analysis is performed to confirm the complete reaction of the isocyanate (Figures 4A and 4B). -1 The absence of a peak in this region indicates the disappearance of the isocyanate group, thus further confirming its reaction with the hydroxyl groups in the PEGMA.
[0079] Synthesis of Photocurable Bioinks Bioinks containing MDI-PEGMA: Synthesis of Bioinks 1 and 2 During the synthesis of urethane-containing compounds, the photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and stabilizer bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate were added to MDI-PEGMA at final concentrations of 2% and 1%, respectively. Additionally, the compounds triethylene glycol dimethacrylate and trimethylolpropane triacrylate were mixed in different ratios to form a Bioink that resulted in a softer material (Bioink1) and a tougher plastic (Bioink2). All chemicals were purchased from Sigma-Aldrich.
[0080] Two Bioinks were made using MDI-PEGMA as the main component of the resin: the first (Bioink1), designed to have low mechanical strength, contained 80% MDI-PEGMA, 17% triethylene glycol dimethacrylate, 2% diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide as a photoinitiator, and 1% bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate as a stabilizer.
[0081] A more robust Bioink (Bioink2) was designed containing 50% MDI-PEGMA, 17% triethylene glycol dimethacrylate, 30% trimethylolpropane triacrylate, 2% diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide as a photoinitiator, and 1% bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate as a stabilizer.
[0082] Synthesis of Bioink3 A more robust resin (Bioink3) was synthesized utilizing tolylene-2,4-diisocyanate (TDI) as the diisocyanate and a combination of poly(ethylene glycol) methacrylate and 2-hydroxyethyl acrylate as the hydroxyl groups to form an acrylated urethane-containing compound. Tolylene-2,4-diisocyanate (25.00 g, 143.5 mmol) was added to an inert atmosphere, round-bottom flask containing a stir bar and heated to 60°C. Subsequently, poly(ethylene glycol) methacrylate (PEGMA) (23.38 mL, 71.8 mmol) and acrylate-2-hydroxyethyl (32.97 mL, 287.1 mmol) were added dropwise and reacted at 60°C for 4 hours. The reaction was then allowed to proceed overnight at room temperature. 77% of the final photocurable Bioink3 resin contained the product of this reaction. The remainder of the Bioink3 resin was made from triethylene glycol dimethacrylate (20%), diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (2%) as the photoinitiator, and bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (1%) as the stabilizer.
[0083] Bioink polymerization and mechanical properties To test the polymerization ability of these Bioinks, 1.50 mL was pipetted onto a mold similar to a flat sheet size (53 mm long, 29 mm wide) fabricated by a computer numerically controlled (CNC) milling machine. The resin was then exposed to 25 mW / cm for 10 seconds to confirm its polymerization ability. 2The specimens were exposed to blue light (415 nm) (Polylight® PL500, Rofin Forensic) at an intensity of 0.15 μm for 1 s, 10 s, and 1 min. The plastic sheets obtained after 1 min of light exposure were cut into 10 mm lengths and 2.5 mm widths with a thickness of 0.8 mm. The resulting pieces were tested by DMA analysis with a preload of 0.01 N for 120 min and their initial stress and stress relaxation were evaluated. This test was performed with samples of Bioink1, Bioink2, and materials utilized in Invisalign aligners (SmartTrack).
[0084] Designing material microstructures for low stress relaxation Two molds containing mesh patterns (Pattern A and Pattern B) were fabricated using a CNC machine. The mold patterns were filled with 160 μL of Bioink2 (the tougher material) and exposed to light to induce its polymerization. Additionally, 320 μL of Bioink1 was added on top of the mesh still placed in the mold and allowed to photopolymerize. Subsequently, the piece was turned over, 320 μL of Bioink1 was added, and the other side of the mesh was allowed to polymerize. The product plastic sheet containing the inner scaffold composed of the tougher material was cut to the dimensions specified in the previous section and tested by DMA analysis with a preload of 0.01 N for 120 min.
[0085] Additionally, to test the effect of layering materials on stress relaxation and to compare it with the meshwork embedded in the material, plastic sheets were made by photopolymerizing layers with a combination of Bioink1 and Bioink2 layers. Two layering combinations were evaluated for this analysis. In the first, 600 μL of Bioink1 was pipetted onto the mold used in section 2 and photopolymerized. This layer was then added with two more layers of Bioink1 for a total thickness of 0.8 mm and a plastic sheet composed of three layers of Bioink1 stacked together. To make the second sample, 600 μL of Bioink1 was pipetted onto the mold utilized in section 2 and polymerized. Subsequently, 600 μL of Bioink2 was added and polymerized on top of the polymerized Bioink1. Finally, a third layer of Bioink1 (600 μL) was added on top of the previous two layers and polymerized to form a plastic sheet composed of two soft layers above and below it and a tougher middle layer. The bilayered samples were tested by DMA analysis with a preload of 0.01 N for 20 minutes.
[0086] Several parts were 3D printed using Bioink2 (the tougher MDI-PEGMA resin) and TDI resin (Bioink3) and assembled together to form a plastic sheet composed of three layers. The top and bottom sheets were 3D printed in square shapes using the two softer resins (Bioink2) and a stereolithography 3D printing machine (Figure 5). The middle layer was a sheet with a beehive structure made from Bioink3 by 3D printing. Two versions of this layer were made, one with a beehive inner diameter of 3.0 mm (Figure 6A) and the other with an inner diameter of 1.5 mm (Figure 6B). Additionally, the lines used were of thickness 1.0 mm and 0.5 mm, respectively.
[0087] The printed parts were cleaned and excess resin was removed. Each part was post-cured under UV light for 1 minute to fully polymerize the resin to its higher strength capacity. Figures 7A-7D show the three printed parts and demonstrate how each of them was placed between glass slides before the post-curing process to maintain their flat structure and avoid bending the material.
[0088] After printing the parts, the three layers were bonded together by light exposure and the addition of more Bioink2 to act as an adhesive between the layers (Figures 8A-8C). The square sheet and the beehive were bonded together by first adding a thin layer of Bioink2 on top of the square sheet, placing the beehive structure on top, and combining the sheets under light for 30 seconds. Additional Bioink2 was added on top of the beehive to cover any open gaps before placing the top square layer on top and a 1-minute light exposure to complete the process. This additional Bioink2 ensured that the top and bottom layers were combined together.
[0089] Following assembly of the plastic sheet, samples were prepared for DMA testing. A straight handpiece and cutting disk were utilized to create small pieces (Figure 9).
[0090] Stereolithography 3D printing of clear orthodontic aligners A transparent orthodontic aligner was constructed using Bioink2 and a stereolithography 3D printer (Wanhao Duplicator 7 Plus Touch Screen UV DLP Resin 3D Printer). A 10 second light exposure time was used at a wavelength of 405 nm for a layer thickness of 50 μm. Under these conditions, the process was carried out at a print speed of 18 mm / hour. The STL file containing the 3D drawing of the aligner was loaded into the printer (FIGS. 10A-10D), and the support structure required for printing due to the nature of stereolithography was added to the element. When this additional print is taken into account, the print time of the aligner ranges from 2 to 3 hours. After printing, the aligner and the support scaffold used in the 3D printing process were attached to the surface of the printing platform (FIG. 11A). The polymerized material of the present invention was ready for post-processing, as it resulted in a transparent solid with good strength immediately after removal from the 3D printer. The part was then removed from the platform, and the excess resin was removed with an ethanol wash (FIG. 11B). The supports were removed by trimming the scaffolding attached to the aligner and / or by using a dental drill. The struts attaching the aligner to the support scaffolding can be seen in FIG. 11C, while FIG. 11D shows the aligner with some struts trimmed. The aligner was then placed in an ethanol bath overnight and dried under compressed air the next day. No post-curing was required.
[0091] Various images of the aligner after trimming of its support material show the quality of the finished product, including an image of the entire aligner after post-processing (FIGS. 12A and 12B), a sectioned image (FIG. 12C), a cross-section (FIG. 12D), the bottom (FIG. 12E), and the finish of the area after trimming of the support (FIG. 12F). These figures demonstrate that polished products can be obtained by stereolithographic 3D printing.
[0092] Results and Discussion The present invention relates in part to novel light-curable materials formed using the methods described herein and the use of these light-curable materials as superior plastics for the manufacture of orthodontic aligners. The invention is based in part on the creation of light-curable resins Bioink1, Bioink2, and Bioink3, and the use of these resins to form plastics with controlled patterns. The microstructure and plastic composition of the novel materials provide stress relief.
[0093] Bioink polymerization and mechanical properties To prepare the samples for mechanical testing, 1.50 mL of Bioink1 was pipetted onto a mold and exposed to blue light for 1 min (Figures 13A and 13B). The polymerized part was removed from the mold resulting in a transparent plastic that was analyzed by DMA testing to evaluate its mechanical properties (Figures 13C and 13D). The same procedure was followed with Bioink2.
[0094] A thermoplastic material commonly used by companies that manufacture commercial orthodontic aligners (Invisalign and Align Technologies (MC)) and an aligner made of poly(ethylene terephthalate) (PETG) were tested by DMA (Figure 14) and compared to the bioink of the present invention. The DMA results showed a difference in initial stress and stress relaxation between Bioink1 and Bioink2, where Bioink2 had a higher initial stress (3.62 MPa) and lower stress relaxation (91.18%) when compared to Bioink1 (1.11 MPa, 98.36%) (Table 1). SmartTrack, the Invisalign material, was also tested by the same DMA analysis and conditions and showed an initial stress of 5.05 MPa and a stress relaxation of 88.95%. These results show a similar 120 minute stress relaxation with SmartTrack having a slightly higher initial stress (1.43 MPa difference) than Bioink2, with only a difference of 2.23%. A slightly higher initial stress and maintaining the same stress relaxation would place Bioink2 in the same category as the market leaders in terms of mechanical properties, however the significant improvement to stress relaxation may allow the use of softer and more comfortable materials while at the same time maintaining the relevant mechanical strength for clinical orthodontic treatment.
[0095] [Table 1]
[0096] Microstructural design of materials for low stress relaxation The present invention relates to the use of defined microstructures of polymeric sheets targeted at reducing stress relaxation in materials for orthodontic transparent aligner applications. To prove this methodology, two approaches were tested. Two molds with patterns A and B were made (FIGS. 15A-15F) and filled with Bioink2 for the formation of a polymerized structure. The polymerized structure was then sandwiched between two layers of softer Bioink1 to complete the plastic sheet. This was done by pipetting a layer of Bioink1 and polymerizing it on each side of the structure. The resulting plastic sheet was tested by DMA for 120 minutes at a preload of 0.01 N.
[0097] The data show that scaffolds with defined microstructures within the photopolymerized plastic significantly reduce the stress relaxation experienced by the material. Comparison of the stress relaxation curves of Pattern A, Pattern B, and SmartTrack samples shows that after 2 hours, the residual stresses were very similar between the SmartTrack and mesh samples, even though SmartTrack had a significantly higher initial stress (Figure 16). In particular, Patterns A and B had a stress relaxation of 56.57% and 60.51%, respectively, which are significantly lower values when compared to the current market standard SmartTrack (Align Technologies), which showed a stress relaxation of 88.95% after 2 hours (Table 2).
[0098] [Table 2]
[0099] Considering the initial stress (5.05 MPa) and the large stress relaxation (88.95%) obtained by the SmartTrack material, it is concluded that after 2 hours the residual stress of the aligner is 0.5580 MPa. When performing the same analysis with the mesh of pattern A, a residual stress of 0.4777 MPa was obtained, which differs by 0.0803 MPa when compared to SmartTrack. Two main conclusions can be obtained from these results: 1) By controlling the microstructure and spatial material composition of plastics designed for orthodontic transparent aligner applications, the stress relaxation obtained by these devices is significantly reduced; 2) It is possible to design materials that are softer, and therefore more comfortable, to be worn by the patient and at the same time apply the mechanical stresses required to achieve a successful clinical outcome. This microstructuring concept can be applied both in 3D printing and in conventional thermoforming of plastic sheets currently used on the market. In the latter case, sheets of different plastics stacked together with different patterns will achieve the desired initial stress and stress relaxation properties.
[0100] In addition to this mesh approach, a layering setup was performed to test whether the microstructure design was indeed important to the stress relaxation effect seen, or whether simply creating layers with materials having the same or different mechanical strengths was sufficient to obtain the observed results. The first layering pattern (Pattern C) (Figure 17A) consisted of three layers of Bioink1 to test the pure effect of layering. The second pattern (Pattern D) (Figure 17B) involved a layer of Bioink2 between two layers of Bioink1. This pattern was designed to test whether simply having a stronger material in the plastic sheet was sufficient to reduce stress relaxation, or whether the microstructure was actually necessary to obtain the desired results.
[0101] The results of the DMA analysis (20 min) show stress relaxation of 75.69% and 74.23% for patterns C and D, respectively (Figure 18 and Table 3). These data suggest that microstructure is indeed necessary to obtain lower stress relaxation, as these values were significantly higher than those obtained for the samples containing mesh (51.92% and 56.16%). This advancement in orthodontic clear aligner technology represents a major innovation in the field.
[0102] [Table 3]
[0103] DMA analysis was performed on various mesh samples and compared with Invisalign aligner material, which is partially composed of urethane groups. Samples containing the material(s) of the present invention with 1.5mm or 3.0mm beehive microstructure reached the same stress as Invisalign after 2 hours (Figures 19A-C), and stress gain after initial loss was observed in all samples. The material and plastic structure design of the present invention enhance the stress exerted over time after the initial deformation. Invisalign ended up with 14% of the initial stress, while the product of the present invention with 3.0mm beehive microstructure maintained 36% of the initial stress (Figures 19D and 19F). Similar behavior was observed with the smaller 1.5mm beehive microstructure, resulting in a residual stress of 32% (Figures 19E and 19F). The combination of the material(s) of the present invention with the microstructure design results in a recovery stress after the initial stress relaxation time. This results in a product that applies the same stress as Invisalign over an extended period of time at lower initial stress values, and allows for the potential design of aligners that are more comfortable for the patient (Figures 19C and 19F).
[0104] Stereolithography 3D printing of clear orthodontic aligners Current dental aligners are manufactured by thermoforming procedures utilizing thermoplastic resins composed mainly of polyurethane groups. In the present invention, aligners were fabricated by 3D printing utilizing the curability of Bioinks upon blue light exposure. Stereolithography, an energy application technique in which light is exposed layer by layer onto a light-curable resin to form a 3D object (Wang et al., 2016, Int. J. Pharm., 503: 207-212) (Figure 20), was the 3D printing technique utilized to fabricate dental aligners. Bioinks of the present invention contain urethane compounds modified with acrylated groups. The urethane groups provide the elastic properties of the material, while the acrylate groups provide the polymerization ability and fine tuning of the strength of the formed solid material. In general, isocyanates have been successfully used in the field of orthodontic transparent aligners and have met strict biocompatibility criteria.
[0105] Although stereolithography is the printing technique used recently, other one-step printing methods are also of interest. Modification of the Bioinks of the present invention, directed to material jetting techniques (PolyJet 3D Printing) or continuous liquid interface manufacturing (CLIP), would allow faster polymerization and reduced aligner printing times with constant light exposure. Moreover, the support removal process would be simpler compared to the extraction of the support under stereolithography, where the excess material is trimmed. Under material jetting techniques, the support can be dissolved with a solution with a basic pH. Under CLIP, printing of the support is not necessary. Finally, material jetting allows the incorporation of multiple materials into the aligner, allowing us to create products with advanced mechanical properties, as well as potential additional applications in the transparent aligner field.
[0106] This one-step fabrication process, in which the entire aligner is printed at once using 3D printing, contrasts with other techniques in which a lattice of cavities is 3D printed and then filled by other conventional methods in a multi-step fabrication process. This difference in fabrication allows for the substitution of multiple inks with different mechanical properties to be controlled, which results in both unique results in terms of mechanical properties and aligners that can be customized for each patient. Moreover, this process allows for the fabrication of structures with features smaller than 1 mm, which can result in further efficiency improvements.
[0107] The present invention relates to an improvement to current orthodontic aligners and their manufacturing methods. One improvement is reduced cost per aligner set: direct 3D printing of aligners results in a cost reduction in the formulation process due to the elimination of 3D printing of tooth molds before thermoforming of the aligners. Another improvement is wider case coverage and enhanced treatment outcomes: 3D printing aligners allows for more complex features as well as the incorporation of additives for precise and advanced force delivery. In addition, various regions of the aligner can now be printed with different thicknesses or materials to provide the desired mechanical properties tailored to a single tooth, thereby greatly enhancing treatment efficacy by eliminating treatment failures. Furthermore, this allows for the treatment of more complex cases that cannot be treated with current aligner products on the market.
[0108] The third improvement is the introduction of microstructures for low stress relaxation: this technology will allow the creation of aligners using softer, more comfortable materials that still exhibit the necessary mechanical strength for the treatment of dental malocclusion. The fourth improvement is that the process is environmentally friendly: 3D printing is an integral step used to create a resin model, into which a thermoplastic material is pressed to form the aligner tray. In a typical treatment, 25-50 aligners are delivered to the patient. Thus, 25-50 sets of corresponding resin models are created, each with slight differences in stages that are geared toward the final tooth movement outcome. Once the aligners are delivered, these models become disposable waste. Different countries impose different rates of environmental taxes or fees on the disposal waste of resin models, which further increases the manufacturing costs. In addition to lowering the manufacturing costs, the technology of the present invention will also reduce the cost of waste disposal for these 3D printed molds, at the same time resulting in a more environmentally friendly manufacturing process.
[0109] The disclosures of each patent, patent application, and publication cited herein are hereby incorporated by reference in their entirety. Although the present invention has been disclosed with respect to specific embodiments, it is apparent that other embodiments and variations of the present invention may be devised by others skilled in the art without departing from the true spirit and scope of the present invention. It is intended that the appended claims be construed to include all such embodiments and equivalent variations. Some aspects of the invention are described below. A photocurable resin comprising 1.75 to 85 weight percent of a urethane (meth)acrylate, 10 to 25 weight percent of a di(meth)acrylate, and less than 5 weight percent of a photoinitiator. 2. The resin of claim 1, wherein the urethane (meth)acrylate comprises a diisocyanate and a hydroxy (meth)acrylate. 3. The resin of claim 2, wherein the diisocyanate is selected from the group consisting of 2,4-toluene diisocyanate, 2,5-toluene diisocyanate, 2,6-toluene diisocyanate, and 4,4'-methylenebis(phenylisocyanate); and the hydroxy(meth)acrylate is selected from the group consisting of poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, poly(propylene glycol) methacrylate, poly(propylene glycol) acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate. 4. The resin of claim 1, wherein the di(meth)acrylate is selected from the group consisting of: triethylene glycol dimethacrylate, di(ethylene glycol) dimethacrylate, propylene glycol dimethacrylate, and di(propylene glycol) dimethacrylate. 5. The resin of claim 1, wherein the photoinitiator is selected from the group consisting of: diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide; and bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide. 6. The resin of claim 1, further comprising a stabilizer selected from the group consisting of: bis(2,2,6,6-tetramethyl-1-octyloxy-4-piperidyl)sebacate; bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate; methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate; dimethylsebacate; and bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate. 7. The resin of claim 1, further comprising a second photocurable resin comprising a second urethane (meth)acrylate, a second di(meth)acrylate, a triacrylate, and a second photoinitiator. 8. The resin of claim 7, wherein the second urethane (meth)acrylate of the second photocurable resin comprises a diisocyanate and a hydroxy (meth)acrylate, wherein the diisocyanate is selected from the group consisting of 2,4-toluene diisocyanate, 2,5-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-methylene bis(phenyl isocyanate), and combinations thereof; and wherein the hydroxy (meth)acrylate is selected from the group consisting of poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, poly(propylene glycol) methacrylate, poly(propylene glycol) acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, and combinations thereof. 9. The resin of claim 7, wherein the second di(meth)acrylate of the second photocurable resin is selected from the group consisting of: triethylene glycol dimethacrylate, di(ethylene glycol) dimethacrylate, propylene glycol dimethacrylate, and di(propylene glycol) dimethacrylate. 10. The resin according to claim 7, wherein the triacrylate is 1,1-trimethylolpropane triacrylate. 11. The resin according to claim 7, wherein the second photoinitiator of the second photocurable resin is selected from the group consisting of: diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide; and bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide. 12. A method of making an article, comprising the steps of: providing a photocurable resin comprising 75 to 85 weight percent of a urethane (meth)acrylate, 10 to 25 weight percent of a di(meth)acrylate, and less than 5 weight percent of a photoinitiator; 3D printing the photocurable resin to form an article; and curing the article; The method includes: 13. The method of claim 12, wherein the step of providing a photocurable resin comprises providing a second photocurable resin comprising a second urethane (meth)acrylate, a second di(meth)acrylate, a triacrylate, and a second photoinitiator, and the step of 3D printing the photocurable resin comprises 3D printing the second photocurable resin. 14. A 3D printed resin article produced by the method according to item 13. 15. The resin article of claim 14, wherein the article comprises an inner microstructure comprising a photocurable resin and a solid coating comprising a second photocurable resin; wherein the solid coating encapsulates the inner microstructure. 16. The resin article according to item 15, wherein the microstructure comprises pores having an inner diameter of 0.5 mm to 5 mm. 17. The resin article according to item 15, wherein the microstructure comprises a photocurable resin having a thickness of 0.1 mm to 3 mm. 18. The resin article according to item 15, wherein the article has an initial stress of 0.45 MPa to 1.6 MPa when tested with a preload of 0.01 N. 19. The resin article according to item 15, wherein the article has a stress relaxation of 50% to 65% after 2 hours when tested with a preload of 0.01 N. 20. The resin article of item 15, wherein the article is a dental aligner.
Claims
1. The steps of: providing a first photocurable resin and a second photocurable resin; 3D printing the first photocurable resin and the second photocurable resin to form an article; and curing the article; 1. A 3D printed resin article produced by a method comprising: the first photocurable resin comprises 75 to 85 weight percent of a first urethane (meth)acrylate, 10 to 25 weight percent of a first di(meth)acrylate, and less than 5 weight percent of a first photoinitiator; the second photocurable resin includes a second urethane (meth)acrylate, a second di(meth)acrylate, and a second photoinitiator, and 1,1-trimethylolpropane triacrylate; the first and second urethane (meth)acrylates independently comprise a diisocyanate selected from the group consisting of 2,4-toluene diisocyanate, 2,5-toluene diisocyanate, 2,6-toluene diisocyanate, and 4,4'-methylenebis(phenylisocyanate); and a hydroxy (meth)acrylate selected from the group consisting of poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, poly(propylene glycol) methacrylate, poly(propylene glycol) acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate; the first and second di(meth)acrylates are independently selected from the group consisting of triethylene glycol dimethacrylate, di(ethylene glycol) dimethacrylate, propylene glycol dimethacrylate, and di(propylene glycol) dimethacrylate; the first and second photoinitiators are independently selected from the group consisting of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide; and The article comprises an interior microstructure comprising the first photocurable resin and a solid coating comprising the second photocurable resin, wherein the solid coating encapsulates the interior microstructure. 3D printed resin items.
2. 2. The 3D printed resin article of claim 1, wherein the first photocurable resin further comprises a stabilizer selected from the group consisting of: bis(2,2,6,6-tetramethyl-1-octyloxy-4-piperidyl)sebacate; bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate; methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate; dimethylsebacate; and bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate.
3. 10. The 3D printed resin article of claim 1, wherein the microstructure comprises pores having an inner diameter between 0.5 mm and 5 mm.
4. 10. The 3D printed resin article of claim 1, wherein the microstructure comprises a photocured resin having a thickness of 0.1 mm to 3 mm.
5. 10. The 3D printed resin article of claim 1, wherein the article has an initial stress of 0.45 MPa to 1.6 MPa when tested with a preload of 0.01 N.
6. 10. The 3D printed resin article of claim 1, wherein the article has a stress relaxation of 50% to 65% after 2 hours when tested with a preload of 0.01 N.
7. 13. The 3D printed resin article of claim 1, wherein the article is a dental aligner.
Citation Information
Patent Citations
Halogen-free radiation-curable flame-retardant composition
JP1996512346A
Compositions that crosslink using visible light and their uses
JP2003507499A
Active energy ray curing composition and use thereof
JP2004244426A
Method for manufacturing artificial teeth
JP2015043793A
Three-dimensional fabrication material systems and methods for producing layered dental products
JP2019521188A