Rare earth aluminate sintered body and method for producing same
The rare earth aluminate sintered body addresses light scattering issues in wavelength conversion members by arranging crystal phases with different refractive indices, improving light extraction efficiency and maintaining luminous flux.
Patent Information
- Application Number
- JP2022075673
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-05-02
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2042-05-02
AI Technical Summary
The porosity of wavelength conversion members in light emitting devices leads to light scattering, resulting in decreased luminous flux and light extraction efficiency.
A rare earth aluminate sintered body is developed with crystal aggregate grains containing a rare earth aluminate phosphor crystal phase and a rare earth aluminate crystal phase of a different refractive index, arranged around the crystal aggregates to minimize light scattering.
The arrangement suppresses light spread, enhancing light extraction efficiency by maintaining high luminous flux and focused light emission.
Smart Images

Figure 0007560752000006 
Figure 0007560752000007 
Figure 0007560752000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a rare earth aluminate sintered body and a method for producing the same. [Background technology]
[0002] There is known a light emitting device that includes a light emitting diode (LED) or a laser diode (LD) and a wavelength conversion member containing a phosphor that converts the wavelength of light emitted from the LED or LD. Such a light emitting device is used as a light source for, for example, in-vehicle lighting, general lighting, backlights for liquid crystal display devices, projectors, etc.
[0003] As a wavelength conversion member provided in a light emitting device, for example, Patent Document 1 discloses a single-phase porous opto-ceramic having a density in a specific range with respect to the theoretical density. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-197774 A Summary of the Invention [Problem to be solved by the invention]
[0005] When the wavelength conversion member scatters light due to its porosity, the luminous flux tends to decrease when the density of the wavelength conversion member decreases due to porosity, and the light extraction efficiency of the wavelength conversion member may decrease. Therefore, an object of the present disclosure is to provide a rare earth aluminate sintered body capable of increasing light extraction efficiency, and a method for producing the same. [Means for solving the problem]
[0006] A first aspect is a rare earth aluminate sintered body including: crystal agglomerate grains containing a rare earth aluminate phosphor crystal phase; and a rare earth aluminate crystal phase having a refractive index different from that of the rare earth aluminate phosphor crystal phase, the rare earth aluminate crystal phase being disposed around the crystal agglomerate grains.
[0007] The second aspect is a method for producing a rare earth aluminate sintered body, the method including: preparing a first raw material mixture obtained by wet mixing and then drying; dry-mixing the first raw material mixture with rare earth aluminate particles; shaping the mixture obtained by dry-mixing the first raw material mixture with the rare earth aluminate particles; and firing the shaped body obtained by shaping the mixture. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a rare earth aluminate sintered body and a method for producing the same, which are capable of increasing light extraction efficiency. [Brief description of the drawings]
[0009] [Figure 1] 1 is a flowchart of a method for producing a rare earth aluminate sintered body. [Diagram 2] FIG. 1 is a diagram showing a schematic configuration of an example of a light emitting device. [Diagram 3] FIG. 1 is a plan view showing a schematic configuration of an example of a phosphor device including a rare earth aluminate sintered body. [Figure 4] FIG. 1 is a side view showing a schematic configuration of an example of a phosphor device including a rare earth aluminate sintered body. [Diagram 5] 1 is a SEM photograph of a rare earth aluminate sintered body according to Example 3. [Figure 6] FIG. 11 is an image showing a state in which crystal aggregate grains are separated at grain boundaries in an SEM photograph of the rare earth aluminate sintered body according to Example 3. [Figure 7] 1 is a SEM photograph of a rare earth aluminate sintered body according to Comparative Example 3. [Figure 8]FIG. 13 is an image showing a state in which an aluminum oxide crystal phase is separated at grain boundaries in an SEM photograph of a rare earth aluminate sintered body according to Comparative Example 3. [Figure 9] FIG. 2 is a diagram showing the transmission spectrum of the rare earth aluminate sintered body according to Examples 1 and 2, and the transmission spectrum of the rare earth aluminate sintered body according to Comparative Example 1. [Figure 10] FIG. 2 is a diagram showing the transmission spectrum of the rare earth aluminate sintered body according to Examples 3 and 4, and the transmission spectrum of the rare earth aluminate sintered body according to Comparative Example 1. [Figure 11] FIG. 13 is a diagram showing a transmission spectrum of a rare earth aluminate sintered body according to Example 5 and a transmission spectrum of a rare earth aluminate sintered body according to Comparative Example 1. [Figure 12] FIG. 2 is a diagram showing the transmission spectra of the rare earth aluminate sintered bodies according to Examples 6 and 7, and the transmission spectrum of the rare earth aluminate sintered body according to Comparative Example 1. [Figure 13] FIG. 1 is a diagram showing the transmission spectra of the rare earth aluminate sintered bodies according to Examples 8 and 9, and the transmission spectrum of the rare earth aluminate sintered body according to Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The rare earth aluminate sintered body and the manufacturing method thereof according to the present invention will be described below based on the embodiments. However, the embodiments shown below are merely examples for embodying the technical idea of the present invention, and the present invention is not limited to the rare earth aluminate sintered body and the manufacturing method thereof. The relationship between the color name and the chromaticity coordinate, and the relationship between the wavelength range of light and the color name of monochromatic light are in accordance with JIS Z8110.
[0011] The rare earth aluminate sintered body includes a crystal aggregate grain containing a rare earth aluminate phosphor crystal phase and a rare earth aluminate crystal phase having a different refractive index from the rare earth aluminate phosphor crystal phase, and the rare earth aluminate crystal phase is arranged around the crystal aggregate grain. In this specification, the rare earth aluminate sintered body may be referred to as a "sintered body". In addition, in this specification, the rare earth aluminate phosphor crystal phase may be referred to as a "phosphor crystal phase". When the rare earth aluminate crystal phase having a different refractive index from the phosphor crystal phase is arranged around the crystal aggregate grain containing the phosphor crystal phase, the excitation light incident on the sintered body and the wavelength-converted light obtained by absorbing the excitation light in the phosphor crystal phase and converting the wavelength are scattered at the interface between the phosphor crystal phase and the rare earth aluminate crystal phase having a different refractive index from the phosphor crystal phase, and the spread of the light emitted from the sintered body can be suppressed. The rare earth aluminate sintered body can increase the light extraction efficiency because the spread of light emitted from the rare earth aluminate sintered body is suppressed.
[0012] The rare earth aluminate sintered body preferably includes two or more crystal aggregate grains in a cross-sectional view, and the rare earth aluminate crystal phase is disposed between the two or more crystal aggregate grains. The cross-sectional view shows, for example, the surface or cross section of the rare earth aluminate sintered body in an SEM image measured using a scanning electron microscope (SEM). When the rare earth aluminate crystal phase is disposed between two or more crystal aggregate grains, the excitation light incident on the sintered body and the wavelength-converted light converted by the phosphor crystal phase are more likely to be scattered at the interface between the phosphor crystal phase and the rare earth aluminate crystal phase having a refractive index different from that of the phosphor crystal phase, and the spread of the light emitted from the sintered body can be more suppressed. The rare earth aluminate sintered body can increase the light extraction efficiency because the spread of the light emitted from the rare earth aluminate sintered body is more suppressed.
[0013] The rare earth aluminate crystal phase is preferably derived from primary particles of rare earth aluminate. When the rare earth aluminate crystal phase is derived from primary particles of rare earth aluminate, the rare earth aluminate crystal phase is easily arranged around the crystal aggregate particles. When the rare earth aluminate crystal phase is derived from primary particles of rare earth aluminate, the rare earth aluminate crystal phase is easily arranged between two or more crystal aggregate particles.
[0014] The rare earth aluminate sintered body preferably has an absolute maximum length of the crystal aggregate grains on the surface or cross section of the rare earth aluminate sintered body within the range of 10.0 μm to 150.0 μm. The absolute maximum length of the crystal aggregate grains on the surface or cross section of the rare earth aluminate sintered body is more preferably within the range of 80.0 μm to 148.0 μm, and even more preferably within the range of 100.0 μm to 145.0 μm. If the absolute maximum length of the crystal aggregate grains on the surface or cross section of the rare earth aluminate sintered body is within the range of 10.0 μm to 150.0 μm, the excitation light incident on the sintered body is easily absorbed and wavelength converted by the phosphor crystal phase contained in the crystal aggregate grains, and the decrease in the luminous flux emitted from the sintered body is suppressed, and light with a high luminous flux can be emitted from the sintered body. The absolute maximum length of a crystal agglomerate grain refers to the distance between the two most distant points of one crystal agglomerate grain that can be confirmed in the measurement range of the surface or cross section of the rare earth aluminate sintered body. If the absolute maximum length of the crystal agglomerate grain on the surface or cross section of the rare earth aluminate sintered body is in the range of 10.0 μm to 150.0 μm, the crystal agglomerate grain is larger than the rare earth aluminate crystal phase derived from the primary particles of the rare earth aluminate, and the rare earth aluminate crystal phase is easily arranged around the crystal agglomerate grain. If the crystal agglomerate grain is larger than the rare earth aluminate crystal phase, the rare earth aluminate crystal phase is easily arranged between two or more crystal agglomerate grains.
[0015] The area of measurement range of rare earth aluminate sintered body for measuring the absolute maximum length of crystal aggregate grains was measured using a scanning electron microscope (SEM). 2In the surface or cross section of the rare earth aluminate sintered body, the measurement range for measuring the absolute maximum length of the crystal aggregate grains is preferably 1,209,675 μm in the SEM image. 2 In the region of 0.1 mm, the absolute maximum length of the crystal aggregates can be accurately measured.
[0016] In the rare earth aluminate sintered body, the rare earth aluminate phosphor crystal phase is preferably the main phase, and the rare earth aluminate crystal phase is preferably the subphase. In this specification, the main phase refers to a crystal phase that exists in a range of 51 volume % to 100 volume % in a total of 100 volume % of the main phase and the subphase. In the rare earth aluminate sintered body, when the rare earth aluminate phosphor crystal phase is the main phase and the rare earth aluminate crystal phase is the subphase, the volume ratio of the crystal aggregate grains containing the rare earth aluminate phosphor crystal phase becomes larger than the volume ratio of the rare earth aluminate crystal phase, and the rare earth aluminate crystal phase is easily arranged around the crystal aggregate grains, and the rare earth aluminate crystal phase is easily arranged between two or more crystal aggregate grains.
[0017] In the rare earth aluminate sintered body, the rare earth aluminate crystal phase is preferably in the range of 1.0 volume % to 10.0 volume % relative to the total 100 volume % of the crystal aggregate grains and the rare earth aluminate crystal phase. More preferably, the rare earth aluminate crystal phase is in the range of 1.2 volume % to 8.0 volume % relative to the total 100 volume % of the crystal aggregate grains and the rare earth aluminate crystal phase, and even more preferably, in the range of 1.5 volume % to 5.0 volume %. In the rare earth aluminate sintered body, when the rare earth aluminate crystal phase is in the range of 1.0 volume % to 10.0 volume % the rare earth aluminate crystal phase is easily arranged around the crystal aggregate grains and is easily arranged between two or more crystal aggregate grains.
[0018] The rare earth aluminate phosphor crystal phase preferably contains at least one element selected from the group consisting of Y, La, Gd, Tb, and Lu. When the rare earth aluminate phosphor crystal phase contains at least one element selected from the group consisting of Y, La, Gd, Tb, and Lu, it becomes easier to obtain a rare earth aluminate phosphor crystal phase having a composition that absorbs incident excitation light and converts the wavelength to a desired wavelength.
[0019] The rare earth aluminate phosphor crystal phase preferably has a composition contained in the composition formula represented by the following formula (I): When the rare earth aluminate phosphor crystal phase has the composition represented by the following formula (I), it is possible to absorb excitation light and emit light whose wavelength has been converted to a desired wavelength. (R 1 1-n Ce n )3(Al 1-m M 1 m ) 5k O 12 (I) (In the above formula (I), R 1 is at least one element selected from the group consisting of Y, La, Lu, Gd and Tb, and M 1 is at least one element selected from the group consisting of Ga and Sc, and m, n, and k satisfy 0≦m≦0.02, 0.002≦n≦0.017, and 0.95≦k≦1.10, respectively.
[0020] In the composition represented by the above formula (I), R 1 may contain two or more rare earth elements. Ce is an activator element for the rare earth aluminate phosphor crystal phase, and the product of the variables n and 3 represents the molar ratio of Ce in the composition represented by formula (I). The variable n is more preferably 0.002 or more and 0.016 or less (0.002≦n≦0.016), and further preferably 0.003 or more and 0.015 or less (0.003≦n≦0.015). In the composition represented by formula (I), the product of the variables m, 5, and k represents the molar ratio of element M 1 The molar ratio of element M 1may not be included in the composition represented by formula (I), that is, m may be 0. In the composition represented by formula (I), in order to convert the wavelength to a desired color tone, the variable m may be 0.00001 or more and 0.02 or less (0.00001≦m≦0.02), or 0.00005 or more and 0.018 or less (0.00005≦m≦0.018). In the composition represented by formula (I), the product of the variable k and 5 is the sum of Al and the element M. 1 The variable k is more preferably 0.96 or more and 1.09 or less (0.96≦k≦1.09), and further preferably 0.97 or more and 1.08 or less (0.97≦k≦1.08).
[0021] The rare earth aluminate crystal phase preferably contains at least one element selected from the group consisting of Gd, Tb, and Lu. When the rare earth aluminate crystal phase contains at least one element selected from the group consisting of Gd, Tb, and Lu, it becomes easier to obtain a rare earth aluminate phosphor crystal phase having a composition that absorbs incident excitation light and converts the wavelength to a desired wavelength.
[0022] The rare earth aluminate crystal phase preferably has a composition represented by the following formula (II): When the rare earth aluminate crystal phase has a composition represented by the following formula (II), the rare earth aluminate crystal phase is likely to be disposed around the crystal aggregate grains, and is likely to be disposed between two or more crystal aggregate grains. R 2 Al 1-j M 2 j O3(II) (In the above formula (II), R 2 is at least one element selected from the group consisting of Gd, Tb and Lu, and M 2 is at least one element selected from the group consisting of Ga and Sc, and j satisfies 0≦j≦0.02.
[0023] The relative density of the rare earth aluminate sintered body is preferably 90% or more, more preferably 93% or more, and preferably 95% or more, and may be 100%, 99% or less, or 98% or less. When the relative density of the rare earth aluminate sintered body is within the range of 90% or more and 100% or less, the excitation light incident on the sintered body and the wavelength-converted light wavelength-converted in the phosphor crystal phase are scattered at the interface between the phosphor crystal phase and the rare earth aluminate crystal phase having a refractive index different from that of the phosphor crystal phase, and the spread of the light emitted from the sintered body is further suppressed.
[0024] The relative density of the rare earth aluminate sintered body can be calculated from the apparent density and true density of the rare earth aluminate sintered body by the following formula (1).
[0025]
number
[0026] The apparent density of the rare earth aluminate sintered body is the mass of the rare earth aluminate sintered body divided by the volume of the rare earth aluminate sintered body, and can be calculated by the following formula (2). The true density of the rare earth aluminate sintered body can be calculated by the following formula (3), using the true density of the rare earth aluminate phosphor and the true density of the rare earth aluminate. The porosity of the rare earth aluminate sintered body is the remainder obtained by subtracting the relative density of the rare earth aluminate sintered body from 100%.
[0027]
number
[0028]
number
[0029] The rare earth aluminate sintered body can be used as a reflective wavelength conversion member in which the incident surface (first main surface) into which the excitation light is incident and the exit surface (first main surface) from which the wavelength-changed light is emitted are the same surface. When the rare earth aluminate sintered body is used as a reflective wavelength conversion member, there is no limitation on the thickness of the rare earth aluminate sintered body, and when the rare earth aluminate sintered body is a plate-like body, the plate thickness is preferably within a range of 90 μm to 250 μm, more preferably within a range of 100 μm to 240 μm, in order to improve the light extraction efficiency.
[0030] When the rare earth aluminate sintered body has a plate shape and the incident surface on which the excitation light is incident and the exit surface from which the light is emitted are the same surface, the light diameter of the exiting light is preferably less than 100%, more preferably 95% or less, and even more preferably 94% or less, when the light diameter of the incident light is 100%. In this way, if the light diameter of the exiting light emitted from the same surface as the incident surface is less than 100% of the light diameter of the incident light, the spread of the exiting light is suppressed, and the light emitted from the rare earth aluminate sintered body can be focused at a target position. The light diameter of the incident light incident on one surface of the rare earth aluminate sintered body is the light diameter of the light emitted from the light source. The light diameter of the incident light can be measured, for example, by a color luminance meter. The light diameter of the incident light is preferably in the range of 0.1 mm to 5 mm, more preferably 0.5 mm to 4 mm. The beam diameter of the outgoing light emitted from the same surface of the rare earth aluminate sintered body as the surface to which the incident light was incident can be measured by measuring the emission luminance of the light emitted from the rare earth aluminate sintered body with a color luminance meter, taking the position showing the maximum luminance in the obtained emission spectrum as the center (measurement center), measuring the distance (mm) from the measurement center to two positions where the luminance is 10 / 100 of the maximum luminance in the emission spectrum (hereinafter sometimes referred to as "10 / 100 luminance") as absolute values, and measuring the sum of the absolute values of the distance (mm) from the measurement center to two positions where the luminance is from the maximum luminance to 10 / 100 of the maximum luminance in the emission spectrum as the beam diameter of the outgoing light.
[0031] A method for producing a rare earth aluminate sintered body includes the steps of preparing a first raw material mixture obtained by wet mixing and then drying, dry mixing the first raw material mixture with rare earth aluminate particles, molding the mixture obtained by dry mixing the first raw material mixture with the rare earth aluminate particles, and firing the molded body obtained by molding the mixture.
[0032] Fig. 1 is a flow chart showing an example of a method for producing a rare earth aluminate sintered body. The method for producing a rare earth aluminate sintered body will be described with reference to Fig. 1. The method for producing a rare earth aluminate sintered body includes steps of preparing a first raw material mixture and rare earth aluminate particles (S101), dry-mixing the first raw material mixture and the rare earth aluminate particles (S102), molding the mixture (S103), and firing the molded body (S104).
[0033] When preparing the first raw material mixture, the first raw material mixture contains at least one rare earth element R selected from the group consisting of Y, La, Lu, Gd, and Tb. 1 a first oxide particle containing Ce, a second oxide particle containing Al, and optionally at least one element M selected from Ga and Sc. 1 and, if necessary, rare earth aluminate phosphor particles.
[0034] Specifically, the first oxide particles include yttrium oxide particles, lanthanum oxide particles, lutetium oxide particles, gadolinium oxide particles, and terbium oxide particles. The second oxide particles include cerium oxide particles. The third oxide particles include aluminum oxide particles. The fourth oxide particles include gallium oxide particles and scandium oxide particles.
[0035] The oxide particles contained in the first raw material mixture are preferably mixed in a molar ratio that results in the composition represented by formula (I) above.
[0036] When the oxides contained in the first raw material mixture are blended, for example, in a molar ratio that results in the composition represented by formula (I), it is preferable that the rare earth aluminate phosphor particles contained in the first raw material mixture have the composition represented by formula (I).
[0037] When the first raw material mixture contains rare earth aluminate phosphor particles, the mass ratio of the rare earth aluminate phosphor particles is preferably in the range of 10% by mass to 90% by mass, more preferably in the range of 15% by mass to 80% by mass, and more preferably in the range of 30% by mass to 70% by mass, based on the total of 100% by mass of the first oxide particles, the second oxide particles, the third oxide particles, and, if necessary, the fourth oxide particles. When the first raw material mixture contains rare earth aluminate phosphor particles within the above mass ratio range, a sintered body containing crystal aggregate particles of a desired size can be obtained so that the rare earth aluminate crystal phase is arranged around the crystal aggregate particles containing the rare earth aluminate phosphor crystal phase. The rare earth aluminate phosphor particles contained in the first raw material mixture may be rare earth aluminate phosphor particles formed by a coprecipitation method. The rare earth aluminate phosphor particles formed by a coprecipitation method have a large specific surface area and are easy to form crystal aggregate particles containing the rare earth aluminate phosphor crystal phase.
[0038] The first raw material mixture is preferably wet-mixed. By wet-mixing the first raw material mixture, the first to fourth oxide particles, and, if necessary, rare earth aluminate phosphor particles, are uniformly dispersed in the liquid, and crystal aggregate particles containing a homogeneous rare earth aluminate phosphor crystal phase are formed. Examples of the liquid used when wet-mixing the first raw material mixture include deionized water, water, and ethanol. The liquid used when wet-mixing the first raw material mixture is preferably in the range of 10 parts by mass to 200 parts by mass, and may be in the range of 50 parts by mass to 150 parts by mass, relative to 100 parts by mass of the first raw material mixture.
[0039] The first raw material mixture to be wet-mixed may contain a dispersant. For example, an organic dispersant may be used as the dispersant, and a cationic dispersant, an anionic dispersant, a nonionic dispersant, or the like may be used. When a dispersant is added to the first raw material mixture, the amount of the dispersant is preferably such that the dispersant volatilizes upon thermal degreasing or baking, and is preferably 10% by mass or less, or may be 5% by mass or less, or may be 3% by mass or less, relative to 100% by mass of the first raw material mixture.
[0040] The first raw material mixture is wet-mixed and then dried to obtain a first raw material mixture. The drying temperature may be in the range of 50°C to 150°C, and the drying time may be 1 hour to 20 hours. By wet-mixing and drying the first raw material mixture, a first raw material mixture in which the first to fourth oxides and the raw materials of the rare earth aluminate phosphor particles, which are included as necessary, are uniformly mixed can be obtained.
[0041] When preparing the rare earth aluminate particles, at least one element R selected from the group consisting of Gd, Tb and Lu is added. 2 a fifth oxide particle containing Al, and a sixth oxide particle containing an element M selected from the group consisting of Ga and Sc, as required; 2 and firing the second raw material mixture obtained by the wet mixing at a temperature in the range of 1000° C. or more and 1600° C. or less. Second raw material By wet mixing the mixture, the fifth to seventh oxide particles are uniformly dispersed, and rare earth aluminate particles having a homogeneous rare earth aluminate crystal phase are formed. The liquid used for wet mixing the second raw material mixture can be the same liquid as that used for wet mixing the first raw material mixture. The liquid used for wet mixing the second raw material mixture is preferably in the range of 10 parts by mass to 200 parts by mass, and may be in the range of 50 parts by mass to 150 parts by mass, relative to 100 parts by mass of the second raw material mixture.
[0042] The oxide particles contained in the second raw material mixture are preferably mixed in a molar ratio that results in the composition represented by formula (II) above. Specific examples of the fifth oxide particles include gadolinium oxide particles, terbium oxide particles, and lutetium oxide particles. Examples of the sixth oxide particles include aluminum oxide particles. Examples of the seventh oxide particles include gallium oxide particles and scandium oxide particles.
[0043] The second raw material mixture is obtained by wet mixing and then drying. The drying temperature may be in the range of 50° C. to 150° C., and the drying time may be in the range of 1 hour to 20 hours.
[0044] The second raw material mixture is fired at a temperature in the range of 1000°C to 1600°C to obtain rare earth aluminate particles. The obtained rare earth aluminate particles preferably have a composition included in the composition formula represented by formula (II). The second raw material mixture is preferably fired in an oxygen-containing atmosphere. The oxygen content in the atmosphere is preferably 5% by volume or more. The second raw material mixture Is, large The calcination may be performed under a gas atmosphere (oxygen content of 20% by volume or more). In an atmosphere with an oxygen content of less than 1% by volume, the surface of each oxide is difficult to melt, and a crystal structure having a rare earth aluminate composition may be difficult to generate. The amount of oxygen in the atmosphere may be measured, for example, by the amount of oxygen flowing into a calcination device, and may be measured at a temperature of 20°C and atmospheric pressure (101.325 kPa). The pressure when the second raw material mixture is calcined may be atmospheric pressure (101.325 kPa).
[0045] The rare earth aluminate particles obtained by firing the second raw material mixture may be wet-disintegrated. The rare earth aluminate particles may be dry-disintegrated and mixed. The rare earth aluminate particles may be wet-disintegrated and then dry-disintegrated and mixed. The rare earth aluminate particles may be dispersed in a liquid and wet-disintegrated using, for example, a ball mill. The rare earth aluminate particles may be dried at a temperature of 50°C or more and 150°C or less and then pulverized and mixed using, for example, a ball mill.
[0046] The method for producing a rare earth aluminate sintered body includes dry-mixing a first raw material mixture obtained by drying after wet mixing with rare earth aluminate particles. The dry mixing is preferably performed, for example, in a ball mill for 10 minutes to 2 hours. After the dry mixing, the mixture may be passed through a sieve with an opening of 350 μm or less. When the first raw material mixture and the rare earth aluminate particles are dry-mixed, they are not mixed as evenly as when wet-mixed. By firing the dry-mixed first raw material mixture and the rare earth aluminate particles that are not mixed as evenly as when wet-mixed, crystal aggregate particles containing a rare earth aluminate phosphor crystal phase are formed from the first raw material mixture, and a sintered body containing rare earth aluminate particles arranged around the crystal aggregate particles is obtained. The mixture containing the first raw material mixture and the rare earth aluminate particles may be dry-powder mixed, with a portion of the mixture being pulverized.
[0047] The content of the rare earth aluminate particles is preferably in the range of 1.0% by mass to 20.0% by mass, more preferably in the range of 1.2% by mass to 19.0% by mass, and even more preferably in the range of 1.5% by mass to 18.0% by mass, based on 100% by mass of the total amount of the first raw material mixture and the rare earth aluminate particles. If the content of the rare earth aluminate particles is in the range of 1.0% by mass to 20.0% by mass, based on 100% by mass of the total amount of the first raw material mixture and the rare earth aluminate particles, a sintered body can be obtained in which the rare earth aluminate crystal phase is in the range of 1.0% by volume to 10.0% by volume, based on 100% by volume of the total of the crystal aggregate grains and the rare earth aluminate crystal phase.
[0048] The method for producing a rare earth aluminate sintered body includes molding the mixture obtained by dry mixing. The method for molding the mixture obtained by dry mixing can employ known methods such as press molding. Examples of press molding methods include die press molding and cold isostatic pressing (CIP) method, the term of which is defined in JIS Z2500:2000, No.2109. In addition, molding may be performed by uniaxial compression. As a molding method, two types of methods may be adopted to adjust the shape of the molded body, for example, CIP may be performed after die press molding, or CIP may be performed after uniaxial compression by the roller bench method. As for CIP, it is preferable to press the molded body by cold isostatic pressing using water as a medium.
[0049] The pressure during die press molding or uniaxial compression molding is preferably in the range of 5 MPa to 50 MPa, more preferably 5 MPa to 30 MPa. If the pressure during die press molding or uniaxial compression molding is in the above range, the molded body can be shaped into a desired shape.
[0050] The pressure in the CIP is preferably in the range of 50 MPa to 200 MPa, more preferably in the range of 50 MPa to 180 MPa. When the pressure in the CIP is in the range of 50 MPa to 200 MPa, a sintered body can be obtained that contains crystal agglomerates containing a rare earth aluminate phosphor crystal phase and a rare earth aluminate crystal phase arranged around the crystal agglomerates.
[0051] The molded body obtained by molding the mixture may be heated to remove the dispersant and the like and degrease the molded body. When the molded body is heated to degrease the molded body, it is preferable to heat the molded body in the air or nitrogen atmosphere at a temperature in the range of 500° C. to 1000° C. By heating the molded body in the air or nitrogen atmosphere at a temperature in the range of 500° C. to 1000° C., the amount of carbon contained in the molded body is reduced, and the decrease in luminous flux due to the inclusion of carbon can be suppressed.
[0052] The method for producing a rare earth aluminate sintered body includes firing the molded body obtained by molding. When firing the molded body, the firing temperature (temperature in the firing furnace) is preferably in the range of 1300°C to 1800°C, more preferably in the range of 1400°C to 1790°C, even more preferably in the range of 1450°C to 1780°C, may be in the range of 1500°C to 1700°C, or may be in the range of 1550°C to 1650°C. When firing the molded body, if the firing temperature is 1300°C or higher, a sintered body containing crystal aggregate grains containing a rare earth aluminate phosphor crystal phase and a rare earth aluminate crystal phase arranged around the crystal aggregate grains can be obtained. When firing the molded body, if the firing temperature is 1800°C or lower, a sintered body containing voids dispersed around each crystal phase in the cross section of the rare earth aluminate sintered body and in which the grain boundaries of each crystal phase can be distinguished can be obtained without dissolving the molded body so that the grain boundaries of each crystal phase disappear.
[0053] The molded body is preferably fired in an oxygen-containing atmosphere. The oxygen content in the atmosphere is preferably 5% by volume or more, more preferably 10% by volume or more, and even more preferably 15% by volume or more. The molded body may be fired in an air atmosphere (oxygen content of 20% by volume or more). In an atmosphere with an oxygen content of less than 1% by volume, the surface of the oxide is difficult to melt, crystal aggregate particles containing a rare earth aluminate phosphor crystal phase are difficult to form, and the rare earth aluminate crystal phase may be difficult to arrange around the crystal aggregate particles. The amount of oxygen in the atmosphere may be measured, for example, by the amount of oxygen flowing into a firing device, and may be measured at a temperature of 20°C and atmospheric pressure (101.325 kPa). The pressure when firing the molded body may be atmospheric pressure (101.325 kPa).
[0054] The obtained sintered body may be annealed in a reducing atmosphere. By annealing the obtained sintered body in a reducing atmosphere, cerium, which is an oxidized activation element contained in the rare earth aluminate phosphor crystal phase in the sintered body, is reduced, and the decrease in wavelength conversion efficiency and the decrease in luminous efficiency in each crystal phase can be suppressed. The reducing atmosphere may be an atmosphere containing at least one rare gas selected from the group consisting of helium, neon, and argon, or nitrogen gas, and hydrogen gas or carbon monoxide gas, and more preferably contains at least argon or nitrogen gas, and hydrogen gas or carbon monoxide gas. The annealing treatment may be performed after processing.
[0055] The annealing temperature is lower than the firing temperature and is preferably within the range of 1000° C. to 1600° C. The annealing temperature is more preferably within the range of 1100° C. to 1400° C. If the annealing temperature is lower than the firing temperature and within the range of 1000° C. to 1600° C., it is possible to reduce cerium, which is an oxidized activator element contained in the rare earth aluminate phosphor crystal phase in the sintered body, without reducing the voids in the sintered body, and to suppress a decrease in the efficiency of wavelength conversion and a decrease in luminous flux.
[0056] The obtained sintered body may be cut into a desired size or thickness by any known method, such as blade dicing, laser dicing, or a method using a wire saw.
[0057] The obtained sintered body may be surface-treated. In the surface treatment, the surface of the cut piece obtained by cutting the obtained sintered body is surface-treated. This surface treatment not only makes the surface of the sintered body suitable for increasing the light extraction efficiency of the rare earth aluminate sintered body, but also makes it possible to make the sintered body into a desired shape, size, or thickness by cutting the sintered body into a desired size or thickness or by surface treatment alone. The surface treatment may be performed before or after cutting the sintered body into a desired size or thickness and processing it. Examples of the surface treatment method include a sandblasting method, a mechanical grinding method, a dicing method, and a chemical etching method.
[0058] The above-mentioned manufacturing method provides a rare earth aluminate sintered body, which includes crystal aggregate grains containing a rare earth aluminate phosphor crystal phase and a rare earth aluminate crystal phase having a different refractive index from the rare earth aluminate phosphor crystal phase, and in which the rare earth aluminate crystal phase is disposed around the crystal aggregate grains. The rare earth aluminate phosphor crystal phase contained in the rare earth aluminate sintered body obtained by the above-mentioned manufacturing method preferably has a composition represented by the above formula (I).
[0059] The obtained rare earth aluminate sintered body can be used as a wavelength conversion member in a light emitting device such as a light source for a projector by combining it with a light source.
[0060] A light emitting device using the above-mentioned rare earth aluminate sintered body as a wavelength conversion member will be described below. The light emitting device includes a rare earth aluminate sintered body and an excitation light source.
[0061] The excitation light source is preferably a semiconductor light-emitting element made of an LED chip or an LD chip. The semiconductor light-emitting element can be a nitride-based semiconductor. By using a semiconductor light-emitting element as the excitation light source, a highly efficient light-emitting device with high linearity of output relative to input and high mechanical shock resistance can be obtained. The rare earth aluminate sintered body can convert the wavelength of light emitted from the semiconductor light-emitting element to form a light-emitting device that emits wavelength-converted mixed color light. The semiconductor light-emitting element is preferably one that emits light in a wavelength range of, for example, 350 nm or more and 500 nm or less. The rare earth aluminate sintered body preferably converts the wavelength of the excitation light from the semiconductor light-emitting element to emit an emission light having an emission peak wavelength in the range of 500 nm or more and less than 650 nm.
[0062] The light emitting element is more preferably a laser diode. The excitation light emitted from the laser diode as the excitation light source is made incident on the wavelength conversion member, and the light whose wavelength is converted by the phosphor contained in the ceramic composite of the wavelength conversion member is condensed, and separated into red light, green light, and blue light by a plurality of optical systems such as a lens array, a polarization conversion element, and a color separation optical system, and modulated according to image information to form color image light. The excitation light emitted from the laser diode as the excitation light source may be made incident on the wavelength conversion member through an optical system such as a dichroic mirror or a collimating optical system.
[0063] FIG. 2 is a schematic diagram showing an example of a configuration of a light emitting device 100. The arrows in FIG. 2 are schematic diagrams showing the optical paths of light. The light emitting device 100 preferably includes an excitation light source 101, which is a light emitting element, a collimating lens 102, three condenser lenses 103, 105, and 106, a dichroic mirror 104, a rod integrator 107, and a wavelength conversion device 120 including a wavelength conversion member. The excitation light source 101 preferably uses a laser diode. The excitation light source 101 may use a plurality of laser diodes, or may be one in which a plurality of laser diodes are arranged in an array or matrix. The collimating lens 102 may be a collimating lens array in which a plurality of collimating lenses are arranged in an array. The laser light emitted from the excitation light source 101 becomes approximately parallel light by the collimating lens 102, is collected by the condenser lens 103, passes through the dichroic mirror 104, and is further collected by the condenser lens 105. The laser light condensed by the condenser lens 105 is wavelength-converted by a wavelength conversion device 120 including a wavelength conversion member 110 and a light reflector 122, and light having an emission peak wavelength in a desired wavelength range is emitted from the wavelength conversion member 110 side of the wavelength conversion device 120. The wavelength-converted light emitted from the wavelength conversion device 120 is condensed by a condenser lens 106 and incident on the rod integrated radar 107, and light with improved uniformity of illuminance distribution in the illuminated area is emitted from the light emitting device 100.
[0064] Fig. 3 is a schematic diagram showing a planar configuration of an example of the wavelength conversion device 120. In Fig. 4, the wavelength conversion device 120 is shown in a side view as one of the members constituting the light emitting device 100. The wavelength conversion device 120 includes at least a wavelength conversion member 110. The wavelength conversion device 120 includes a disk-shaped wavelength conversion member 110, and may include a rotation mechanism 121 for rotating the wavelength conversion member 110. The rotation mechanism 121 is connected to a drive mechanism such as a motor, and can dissipate heat by rotating the wavelength conversion member 110.
[0065] FIG. 4 is a schematic diagram showing the configuration of a side of an example of the wavelength conversion device 120, which is shown in a side view in FIG. 2 as one of the members constituting the light emitting device 100. The wavelength conversion device 120 includes a rare earth aluminate sintered body 111 and a light-transmitting thin film 112 as the wavelength conversion member 110. The wavelength conversion device 120 includes a light reflector 122 on the side of the rare earth aluminate sintered body 111 of the wavelength conversion member 110 opposite to the side on which the light-transmitting thin film 112 is disposed. If the light from the rare earth aluminate sintered body 111 can be sufficiently emitted to the side on which the light-transmitting thin film 112 is disposed, the light reflector 122 can be omitted. The light reflector 122 may be used not only as a member that reflects the light from the rare earth aluminate sintered body 111 to the side on which the light-transmitting thin film 112 is disposed, but also as a heat dissipation member that transfers heat generated in the rare earth aluminate sintered body 111 and dissipates it to the outside. EXAMPLES
[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0067] Example of manufacturing raw material rare earth aluminate phosphor particles (YAG phosphor particles by coprecipitation method) Yttrium chloride (YCl3), cerium chloride (CeCl3), and aluminum chloride (AlCl3) are 2.99 Ce 0.01 AlO 12 The mixture was dissolved in deionized water to prepare a mixed solution. This mixed solution was poured into a (NH3)2CO3 solution, and Y was precipitated by coprecipitation. 2.99 Ce 0.01 AlO 12 This mixture was placed in an alumina crucible and fired in an air atmosphere at a temperature ranging from 1200°C to 1600°C for 10 hours to obtain a fired product. The fired product was classified by passing it through a dry sieve to obtain a mixture represented by the formula: 2.99 Ce 0.01 AlO 12 A raw material YAG phosphor particle (co-precipitated YAG phosphor particle) having a composition represented by the following formula was prepared.
[0068] As the first oxide particles, yttrium oxide particles having a purity of 98 mass % were used.
[0069] As the second oxide particles, cerium oxide particles having a purity of 92 mass % were used.
[0070] As the third oxide particles or the sixth oxide particles, aluminum oxide particles having an aluminum oxide purity of 99 mass % were used.
[0071] As the fifth oxide particles, gadolinium oxide particles having a gadolinium oxide purity of 98 mass %, terbium oxide particles having a terbium oxide purity of 98 mass %, and lutetium oxide particles having a lutetium oxide purity of 99 mass % were used.
[0072] Example 1 The molar ratio of each element of Y, Al, and Ce contained in each oxide particle is Y 2.988 Ce 0.012 Al 5.1 O 12 Yttrium oxide particles as the first oxide particles, cerium oxide particles as the second oxide particles, aluminum oxide particles as the third oxide particles, and rare earth aluminate phosphor particles as the raw material were weighed out so as to obtain a composition represented by the following formula: 6.0 parts by mass of a dispersant (Floren G-700, Kyoeisha Chemical Co., Ltd.) was added to 100 parts by mass of the total amount of the first oxide particles, the second oxide particles, the third oxide particles, and the obtained YAG phosphor particles as the raw material, and 50 parts by mass of ethanol was further added. The mixture was wet-mixed using a ball mill, dried at 130°C for 10 hours, and then dry-pulverized and mixed using a ball mill to prepare a first raw material mixture.
[0073] Gadolinium oxide particles were weighed as the fifth oxide particles and aluminum oxide particles were weighed as the sixth oxide particles so that the molar ratio of each element of Gd and Al contained in each oxide particle was a composition represented by GdAlO3. 3.0 parts by mass of a dispersant (ES-REAM C-2093I, NOF Corp.) was added to 100 parts by mass of the total amount of the fifth oxide particles and the sixth oxide particles, and 50 parts by mass of ethanol was further added, and the mixture was wet-mixed using a ball mill and dried at 130°C for 10 hours to prepare a second raw material mixture. This second raw material mixture was fired at 1400°C in an air atmosphere (oxygen content of 20% by volume or more, 101.325 kPa), and the fired product obtained by firing was dispersed in ethanol, wet-disintegrated using a ball mill, dried at 130°C, and dry-pulverized and mixed using a ball mill to prepare rare earth aluminate particles having a composition represented by GdAlO3.
[0074] The obtained first raw material mixture and the obtained rare earth aluminate particles were dry mixed for 20 minutes using a ball mill. 2.6 mass% of rare earth aluminate particles were added to 100 mass% of the total of the first raw material mixture and the rare earth aluminate particles, and the content of the rare earth aluminate crystal phase was the amount (volume %) shown in Table 1 with respect to 100 volume% of the total amount of the obtained sintered body, and a mixture was obtained by dry mixing. The content (volume %) of the rare earth aluminate crystal phase with respect to the total amount of the rare earth aluminate sintered body can be calculated from the content (mass %) of the rare earth aluminate particles with respect to 100 mass% of the total amount of the first raw material mixture and the rare earth aluminate particles, the true density of the rare earth aluminate phosphor and the true density of the rare earth aluminate, which will be described later.
[0075] The mixture obtained was filled into a mold and subjected to a pressure of 5 MPa (51 kgf / cm 2 A cylindrical molded body with a diameter of 26 mm and a thickness of 10 mm was formed at a pressure of 100 MPa. The obtained molded body was placed in a packaging container and vacuum-packed, and subjected to CIP at 176 MPa using a cold isostatic pressurizing device (manufactured by Kobe Steel, Ltd. (KOBELCO)) to obtain a molded body. The obtained molded body was heated and degreased at 700°C in a nitrogen atmosphere.
[0076] The compact obtained by molding was fired in a firing furnace (manufactured by Marusho Denki Co., Ltd.) to obtain a rare earth aluminate sintered body. The firing conditions were an air atmosphere (101.325 kPa, oxygen concentration: approximately 20% by volume), a temperature of 1605°C, and a firing time of 6 hours. The obtained rare earth aluminate sintered body was cut into an appropriate shape and size with a wire saw, and the surface of the cut piece was polished with a surface grinder. Finally, a rare earth aluminate sintered body according to Example 1 having a plate thickness of 230 μm was obtained. The rare earth aluminate sintered body according to Example 1 was a rare earth aluminate sintered body having a plate thickness of 230 μm. 2.988 Ce 0.012 Al 5.1 O 12 The phosphor crystal phase contained crystal aggregates containing a rare earth aluminate phosphor crystal phase having a composition represented by the formula: Y 2.988 Ce 0.012 Al 5.1 O 12 The refractive index of the rare earth aluminate phosphor crystal phase having the composition represented by the formula: is 1.83, and the refractive index of the rare earth aluminate crystal phase having the composition represented by the formula: GdAlO3 is 2.02.
[0077] Example 2 The rare earth aluminate sintered body of Example 2 was obtained in the same manner as in Example 1, except that the first raw material mixture and the rare earth aluminate particles were dry-mixed to obtain a mixture in which 3.8 mass% of the rare earth aluminate particles were added relative to 100 mass% of the total of the first raw material mixture and the rare earth aluminate particles, and the content of the rare earth aluminate crystal phase relative to 100 volume% of the total amount of the obtained sintered body was the amount (volume %) shown in Table 1. 2.988 Ce 0.012 Al 5.1 O 12 The phosphor crystal phase contained crystal aggregates having a rare earth aluminate phosphor crystal phase represented by the composition represented by GdAlO3.
[0078] Example 3 Terbium oxide particles were weighed as the fifth oxide particles and aluminum oxide particles were weighed as the sixth oxide particles so that the molar ratio of the Tb and Al elements contained in each oxide particle would be a composition represented by TbAlO3, and rare earth aluminate particles having a composition represented by TbAlO3 were prepared in the same manner as in Example 1. The rare earth aluminate sintered body of Example 3 was obtained in the same manner as in Example 1, except that the first raw material mixture and the rare earth aluminate particles were dry-mixed to obtain a mixture in which 2.6 mass% of the rare earth aluminate particles were added relative to 100 mass% of the total of the first raw material mixture and the rare earth aluminate particles, and the content of the rare earth aluminate crystal phase relative to 100 volume% of the total amount of the obtained sintered body was the amount (volume %) shown in Table 1. 2.988 Ce 0.012 Al 5.1 O 12 The rare earth aluminate phosphor crystal phase having a composition represented by TbAlO3 has a refractive index of 1.76.
[0079] Example 4 The rare earth aluminate sintered body of Example 4 was obtained in the same manner as in Example 3, except that the first raw material mixture and the rare earth aluminate particles were dry-mixed to obtain a mixture in which 3.0 mass% of the rare earth aluminate particles were added relative to 100 mass% of the total of the first raw material mixture and the rare earth aluminate particles, and the content of the rare earth aluminate crystal phase relative to 100 volume% of the total amount of the obtained sintered body was the amount (volume %) shown in Table 1. 2.988 Ce 0.012 Al 5.1 O 12 and a rare earth aluminate crystal phase having a composition represented by TbAlO3. The refractive index of the rare earth aluminate crystal phase having a composition represented by TbAlO3 is 1.95.
[0080] Example 5 Lutetium oxide particles were weighed as the fifth oxide particles and aluminum oxide particles were weighed as the sixth oxide particles so that the molar ratio of Lu and Al elements contained in each oxide particle would be a composition represented by LuAlO3, and rare earth aluminate particles having a composition represented by LuAlO3 were prepared in the same manner as in Example 1. The rare earth aluminate sintered body of Example 5 was obtained in the same manner as in Example 1, except that the first raw material mixture and the rare earth aluminate particles were dry-mixed to obtain a mixture in which 4.4 mass% of the rare earth aluminate particles were added relative to 100 mass% of the total of the first raw material mixture and the rare earth aluminate particles, and the content of the rare earth aluminate crystal phase relative to 100 volume% of the total amount of the obtained sintered body was the amount (volume %) shown in Table 1. 2.988 Ce 0.012 Al 5.1 O 12 and a rare earth aluminate phosphor crystal phase having a composition represented by LuAlO3.
[0081] Comparative Example 1 A rare earth aluminate sintered body of Comparative Example 1 was obtained in the same manner as in Example 1, except that rare earth aluminate particles were not used.
[0082] Example 6 A rare earth aluminate sintered body according to Example 6 was obtained in the same manner as in Example 2, except that 3.8 mass% of rare earth aluminate particles were added relative to 100 mass% of the total of the first raw material mixture and the rare earth aluminate particles, the content of the rare earth aluminate crystal phase was the amount (volume %) shown in Table 1 relative to 100 volume% of the total amount of the obtained sintered body, and the obtained molded body was fired at 1610°C. 2.988 Ce 0.012 Al 5.1 O 12The phosphor crystal phase contained crystal aggregates having a rare earth aluminate phosphor crystal phase represented by the composition represented by GdAlO3.
[0083] Example 7 The first raw material mixture and rare earth aluminate particles having a composition represented by TbAlO3 obtained in the same manner as in Example 4 were dry-mixed to obtain a mixture, and a rare earth aluminate sintered body according to Example 7 was obtained in the same manner as in Example 6. The rare earth aluminate sintered body according to Example 7 has a composition of Y 2.988 Ce 0.012 Al 5.1 O 12 The phosphor crystal phase contained crystal aggregates having a rare earth aluminate phosphor crystal phase having a composition represented by the formula:
[0084] Example 8 The first raw material mixture and rare earth aluminate particles having a composition represented by LuAlO3 obtained in the same manner as in Example 5 were dry-mixed to obtain a mixture such that 3.0 mass% of the rare earth aluminate particles were added relative to the total mass of the first raw material mixture and the rare earth aluminate particles (100 mass%), and the content of the rare earth aluminate crystal phase relative to the total volume of the obtained sintered body (100 volume%) was the amount (volume %) shown in Table 1. The rare earth aluminate sintered body of Example 8 was obtained in the same manner as in Example 6. The rare earth aluminate sintered body of Example 8 has a structure of Y 2.988 Ce 0.012 Al 5.1 O 12 and a rare earth aluminate phosphor crystal phase having a composition represented by LuAlO3.
[0085] Example 9 The first raw material mixture and rare earth aluminate particles having a composition represented by LuAlO3 obtained in the same manner as in Example 5 were dry-mixed to obtain a mixture, and a rare earth aluminate sintered body according to Example 9 was obtained in the same manner as in Example 6. The rare earth aluminate sintered body according to Example 9 has a composition of Y 2.988 Ce0.012 Al 5.1 O 12 and a rare earth aluminate phosphor crystal phase having a composition represented by LuAlO3.
[0086] Comparative Example 2 A rare earth aluminate sintered body of Comparative Example 2 was obtained in the same manner as in Example 6, except that rare earth aluminate particles were not used.
[0087] Comparative Example 3 A rare earth aluminate sintered body of Comparative Example 3 was obtained in the same manner as in Example 1, except that aluminum oxide particles having an aluminum oxide purity of 99 mass % were used instead of the rare earth aluminate particles.
[0088] The following evaluations were carried out for each rare earth aluminate sintered body, except for the rare earth aluminate sintered body of Comparative Example 3. The results are shown in Table 1. In Table 1, the symbol "-" indicates that there is no corresponding item or value.
[0089] Relative Density The relative density of each rare earth aluminate sintered body of the examples and comparative examples was measured. The relative density of the rare earth aluminate sintered body of the examples and comparative examples was calculated by the above-mentioned formula (1). The apparent density of the rare earth aluminate sintered body was calculated by the above-mentioned formula (2). The true density of the rare earth aluminate sintered body was calculated by the above-mentioned formula (3). The true density of the rare earth aluminate phosphor was 4.60 g / cm. 3 , the true density of GdAlO3 is 7.24g / cm 3 , the true density of TbAlO3 is 7.39g / cm 3 , the true density of LuAlO3 is 8.30g / cm 3 It is.
[0090] Relative luminous flux (%) The rare earth aluminate sintered bodies of each Example and Comparative Example were irradiated with a laser beam having a wavelength of 450 nm from a laser diode so that the diameter of the incident beam was 2.2 mm, and the radiant flux of the light emitted from the same surface as the surface on which the laser beam was incident was measured with an integrating sphere. The radiant flux of Comparative Example 1 was taken as 100%, and the radiant flux of the samples of each of the rare earth aluminate sintered bodies of Examples 1 to 9 and each of the rare earth aluminate sintered bodies of Comparative Example 2 relative to the radiant flux of Comparative Example 1 was expressed as relative luminous flux (%).
[0091] Beam diameter ratio (beam diameter of outgoing light / beam diameter of incoming light) Each rare earth aluminate sintered body of the examples and comparative examples was irradiated with a laser beam having a wavelength of 450 nm from a laser diode so that the diameter of the incident beam was 0.6 mm on the first main surface to which the laser beam was incident, and the diameter of the laser beam was defined as the diameter of the incident beam incident on the first main surface of the rare earth aluminate sintered body. The diameter of the outgoing beam emitted from the same surface as the first main surface to which the laser beam was incident was measured by measuring the emission luminance of the light emitted from the rare earth aluminate sintered body of each example and comparative example with a color luminance meter, setting the position showing the maximum luminance in the obtained emission spectrum as the center (measurement center), measuring the distance (mm) from the measurement center to two positions having a luminance of 10 / 100 of the maximum luminance in the emission spectrum as an absolute value, and measuring the sum of the absolute values of the distance (mm) from the measurement center to two positions having a luminance of 10 / 100 of the maximum luminance from the maximum luminance as the diameter of the outgoing beam emitted from the first main surface. The beam diameter ratio of the beam diameter of the outgoing light from the first main surface to the beam diameter of the incident light on the first main surface was calculated. The beam diameter ratio of Comparative Example 1 was set to 100%, and the beam diameter ratios of the samples of the rare earth aluminate sintered bodies of Examples 1 to 9 and the rare earth aluminate sintered body of Comparative Example 2 relative to the beam diameter ratio of Comparative Example 1 were measured and expressed as relative beam diameter ratios (%).
[0092] Light extraction efficiency (%) For each of the rare earth aluminate sintered bodies of the Examples and Comparative Examples, the measured relative luminous flux was divided by the relative beam diameter ratio to calculate the light extraction efficiency (%).
[0093] How to measure absolute maximum length In the SEM images obtained by photographing the surface or cross section of each rare earth aluminate sintered body of the examples and comparative examples with a scanning electron microscope (SEM), 2 The area where the measurement range was determined was the area where the data size of the SEM image was 640 × 480 pixels (vertical × horizontal), and one pixel was 1.984375 μm. Therefore, the area of the measurement range was calculated as 1270 μm × 952.5 μm, which is 1209675 μm. 2 The secondary agglomerates of one rare earth aluminate phosphor crystal phase included in this measurement range were taken as crystal agglomerates, and the distance between the two most distant points on the contour of the crystal agglomerates was taken as the absolute maximum length, and measurements were performed using Winroof2018 image analysis software (manufactured by Mitani Shoji Co., Ltd.). The absolute maximum lengths of 100 to 1000 crystal agglomerates on the measurement area were measured, and the largest absolute maximum length was taken as the absolute maximum length of the crystal agglomerates on the surface or cross section of each rare earth aluminate sintered body. When the content of rare earth aluminate particles was 1.7% by volume (Examples 1, 3, and 8), or when no rare earth aluminate particles were contained (Comparative Examples 1 and 2), the crystal agglomerates of the rare earth aluminate particles could not be separated, and the crystal agglomerates separated at the grain boundaries could not be measured.
[0094] SEM images Using a scanning electron microscope (SEM), SEM images of the surface of each rare earth aluminate sintered body of the examples and comparative examples were obtained. The SEM images shown in the figures were obtained at a magnification of 100 times, and the SEM images used for measuring the absolute maximum length were obtained at a magnification of 100 times in consideration of the accuracy of the analysis. Fig. 5 is an SEM photograph of the surface of the rare earth aluminate sintered body of Example 3. Fig. 7 is an SEM photograph of the surface of the rare earth aluminate sintered body of Comparative Example 3.
[0095] Transmittance (%) Using a spectrophotometer (Hitachi High-Tech Science Corporation), the light from the light source was converted to monochromatic light with a wavelength of 550 nm by a spectroscope, and the light intensity of the converted light with a wavelength of 550 nm was measured and used as the incident light intensity. The light with a wavelength of 550 nm was incident on each rare earth aluminate sintered body of the examples and comparative examples, and the light intensity of the light emitted from the rare earth aluminate sintered body on the opposite side to the incident side was measured and used as the transmitted light intensity. The ratio of the transmitted light intensity to the incident light intensity was measured as the transmittance for light with a wavelength of 550 nm based on the following formula (4). In the following formula (4), I0 is the incident light intensity, and I is the transmitted light intensity at each wavelength.
[0096]
number
[0097] Transmission spectrum Using a spectrophotometer (manufactured by Hitachi High-Tech Science Corporation), the light from the light source was converted into monochromatic light of each wavelength by a spectroscope, the light intensity of the converted wavelength was determined as the incident intensity, the light of each wavelength was incident on each rare earth aluminate sintered body of the examples and comparative examples, and the light intensity of the light emitted from the rare earth aluminate sintered body on the opposite side to the incident side was measured and determined as the transmitted light intensity, and the ratio of the transmitted light intensity to the incident intensity was calculated based on the above formula (4), and the transmittance of each wavelength was expressed as a transmission spectrum. Transparent The spectrum of the rare earth aluminate sintered body according to Comparative Example 1 is shown.
[0098] [Table 1]
[0099] In the rare earth aluminate sintered bodies according to Example 2, Examples 4 to 7, and Example 9, the absolute maximum length of the crystal aggregate grains containing the rare earth aluminate phosphor phase was in the range of 10.0 μm or more and 150.0 μm or less. The rare earth aluminate sintered bodies according to Examples 1 to 9 had a smaller relative beam diameter ratio and suppressed the spread of the emitted light than the rare earth aluminate sintered body of Comparative Example 1. The relative luminous flux of the rare earth aluminate sintered bodies according to Examples 1 to 9 was lower than that of Comparative Example 1, but the light extraction efficiency was higher than that of Comparative Example 1 because the relative beam diameter ratio was small and the spread of the emitted light was suppressed. The transmittance at 550 nm of the rare earth aluminate sintered bodies according to Examples 1 to 9 was lower than that of the rare earth aluminate sintered bodies according to Comparative Examples 1 and 2, and the light from the light source was effectively utilized in the rare earth aluminate phosphor phase.
[0100] The rare earth aluminate sintered body according to Comparative Example 2 had a higher relative luminous flux than the sintered body according to Comparative Example 1, but had a larger relative beam diameter ratio than the sintered body according to Comparative Example 1, and the emitted light was broadened, resulting in a decrease in the light extraction efficiency.
[0101] FIG. 5 is a SEM photograph of the surface of the rare earth aluminate sintered body according to Example 3. Example 3FIG. 1 is an image of grain boundary separation of crystal aggregate grains containing a rare earth aluminate phosphor phase on the surface of the rare earth aluminate sintered body according to Example 3. On the surface of the rare earth aluminate sintered body according to Example 3, a rare earth aluminate crystal phase 2 having a composition represented by TbAlO3 and having a refractive index different from that of the rare earth aluminate phosphor crystal phase was arranged around a crystal aggregate grain 1 containing a rare earth aluminate phosphor crystal phase. The rare earth aluminate sintered body according to Example 3 includes two or more crystal aggregate grains 1 in a cross-sectional view (SEM photograph of the surface of the rare earth aluminate sintered body), and a rare earth aluminate crystal 2 is arranged between the two crystal aggregate grains 1, 1. In the rare earth aluminate sintered body according to Example 3, the excitation light and the wavelength-converted light are scattered at the interface between the crystal aggregate grain 1 and the rare earth aluminate crystal phase 2, and the spread of the light emitted from the sintered body is suppressed, resulting in a small relative light diameter ratio. In the rare earth aluminate sintered body according to Example 3, the spread of the light emitted from the rare earth aluminate sintered body was suppressed, and therefore the light extraction efficiency was increased.
[0102] Fig. 7 is an SEM photograph of the surface of the rare earth aluminate sintered body according to Comparative Example 3. Fig. 8 is an image diagram of grain boundary separation of the aluminum oxide crystal phase on the surface of the rare earth aluminate sintered body according to Comparative Example 3. The rare earth aluminate sintered body according to Comparative Example 3 does not contain a rare earth aluminate crystal phase, and crystal aggregate grains containing a rare earth aluminate phosphor crystal phase are not formed. In the rare earth aluminate sintered body according to Comparative Example 3, an aluminum oxide crystal phase 3 is formed, and a rare earth aluminate phosphor crystal phase 4 is described between the aluminum oxide crystal phases.
[0103] 9 to 13 show the transmission spectra of the rare earth aluminate sintered bodies according to Examples 1 to 9 and the rare earth aluminate sintered body according to Comparative Example 1. FIG. Examples 1 to 9 The transmission spectrum of the rare earth aluminate sintered body is lower than that of the rare earth aluminate sintered body according to Comparative Example 1, and the incident light is absorbed and efficiently wavelength-converted in the rare earth aluminate phosphor crystal phase. As a result, the rare earth aluminate sintered bodies according to Examples 1 to 9 have high light extraction efficiency.
[0104] An embodiment of the present invention includes the following rare earth aluminate sintered body and a method for producing the same.
[0105] [Section 1] The present invention comprises: a crystal aggregate grain including a rare earth aluminate phosphor crystal phase; and a rare earth aluminate crystal phase having a refractive index different from that of the rare earth aluminate phosphor crystal phase, the rare earth aluminate crystal phase being disposed around the crystal aggregate grains. [Section 2] Item 2. The rare earth aluminate sintered body according to item 1, comprising two or more of the crystal agglomerates in one cross-sectional view, and the rare earth aluminate crystal phase is disposed between two of the crystal agglomerates. [Section 3] Item 3. The rare earth aluminate sintered body according to item 1 or 2, wherein the rare earth aluminate crystal phase is derived from primary particles of the rare earth aluminate. [Section 4] Item 4. The rare earth aluminate sintered body according to any one of items 1 to 3, wherein the absolute maximum length of the crystal aggregate grains on the surface or cross section of the rare earth aluminate sintered body is in the range of 10.0 μm to 150.0 μm. [Section 5] Item 5. The rare earth aluminate sintered body according to any one of items 1 to 4, wherein the rare earth aluminate phosphor crystal phase contains at least one element selected from the group consisting of Y, La, Gd, Tb and Lu. [Section 6] Item 6. The rare earth aluminate sintered body according to any one of items 1 to 5, wherein the rare earth aluminate crystal phase contains at least one element selected from the group consisting of Gd, Tb, and Lu. [Section 7] The region of the measurement range of the rare earth aluminate sintered body for measuring the absolute maximum length of the crystal aggregate grains is 1209675 μm in the SEM image measured using a scanning electron microscope. 2 Item 5. The rare earth aluminate sintered body according to item 4, wherein the rare earth aluminate sintered body is in the range of 0.1 to 0.5 μm. [Section 8] Item 8. The rare earth aluminate sintered body according to any one of Items 1 to 7, wherein the rare earth aluminate crystal phase is in the range of 1.0 vol. % to 10.0 vol. % relative to 100 vol. % in total of the crystal agglomerates and the rare earth aluminate crystal phase. [Section 9] Item 9. The rare earth aluminate sintered body according to any one of items 1 to 8, wherein the rare earth aluminate phosphor crystal phase has a composition represented by the following formula (I): (R 1 1-n Ce n )3(Al 1-m M 1 m ) 5k O 12 (I) (In the above formula (I), R 1 is at least one element selected from the group consisting of Y, La, Lu, Gd and Tb, and M 1 is at least one element selected from the group consisting of Ga and Sc, and m, n, and k satisfy 0≦m≦0.02, 0.002≦n≦0.017, and 0.95≦k≦1.10, respectively. [Section 10] Item 10. The rare earth aluminate sintered body according to any one of items 1 to 9, wherein the rare earth aluminate crystal phase has a composition represented by the following formula (II): R 2 Al 1-j M 2 j O3(II) (In the above formula (II), R 2 is at least one element selected from the group consisting of Gd, Tb and Lu, and M 2 is at least one element selected from the group consisting of Ga and Sc, and j satisfies 0≦j≦0.02. [Section 11] preparing a first raw material mixture obtained by wet mixing and then drying; dry mixing the first raw material mixture with rare earth aluminate particles; shaping a mixture obtained by dry-mixing the first raw material mixture and the rare earth aluminate particles; and sintering the resulting molded body obtained by molding the mixture. [Section 12] When preparing the first raw material mixture, the first raw material mixture contains at least one element R selected from the group consisting of Y, La, Lu, Gd, and Tb. 1 a first oxide particle containing Ce; a second oxide particle containing Al; and, if necessary, at least one element M selected from the group consisting of Ga and Sc. 1 Item 12. A method for producing a rare earth aluminate sintered body according to item 11, further comprising the step of: [Section 13] When preparing the rare earth aluminate particles, At least one element R selected from the group consisting of Gd, Tb and Lu 2 a fifth oxide particle containing Al, and a sixth oxide particle containing an element M selected from the group consisting of Ga and Sc, as required; 2 and a seventh oxide particle comprising: Item 13. The method for producing a rare earth aluminate sintered body according to item 11 or 12, wherein the rare earth aluminate particles are produced by firing the second raw material mixture obtained by the wet mixing at a temperature in the range of 1000° C. to 1600° C. [Section 14] Item 14. The method for producing a rare earth aluminate sintered body according to any one of items 11 to 13, wherein the sintering temperature is in the range of 1300° C. or more and 1800° C. or less when the molded body is sintered. [Industrial Applicability]
[0106] The rare earth aluminate sintered body according to the present disclosure can be used in combination with an excitation light source as a wavelength conversion member for vehicle-mounted or general lighting devices, backlights for liquid crystal display devices, and light sources for projectors. [Explanation of symbols]
[0107] 1: crystal agglomerate grains, 2: rare earth aluminate crystal phase, 3: aluminum oxide crystal phase, 4: rare earth aluminate phosphor crystal phase, 100: light emitting device, 101: excitation light source, 102: collimating lens, 103, 105 and 106: condenser lenses, 104: dichroic mirror, 107: rod integrator, 110: wavelength conversion member, 111: rare earth aluminate sintered body, 112: light-transmitting thin film, 120: wavelength conversion device, 121: rotation mechanism, 122: light reflector.
Claims
1. The present invention comprises: a crystal aggregate grain including a rare earth aluminate phosphor crystal phase; and a rare earth aluminate crystal phase having a refractive index different from that of the rare earth aluminate phosphor crystal phase, the rare earth aluminate crystal phase is disposed around the crystal aggregate grains; In one cross-sectional view, the rare earth aluminate crystal phase includes two or more of the crystal agglomerates, and the rare earth aluminate crystal phase is disposed between two of the crystal agglomerates; A rare earth aluminate sintered body, wherein the absolute maximum length of the crystal agglomerate grains on a surface or cross section of the rare earth aluminate sintered body is within the range of 10.0 μm or more and 150.0 μm or less, as measured by the following method. Measurement method In an SEM image obtained by photographing the surface or cross section of a rare earth aluminate sintered body with a scanning electron microscope (SEM), an area of 1,209,675 μm 2 is taken as the measurement range, secondary agglomerates of one rare earth aluminate phosphor crystal phase included in this measurement range are taken as crystal agglomerates, the distance between the two most distant points on the outline of the crystal agglomerates is taken as the absolute maximum length, and the absolute maximum lengths of 100 to 1,000 crystal agglomerates in the measurement area are measured, and the largest absolute maximum length is taken as the absolute maximum length of the crystal agglomerates on the surface or cross section of the rare earth aluminate sintered body.
2. 2. The rare earth aluminate sintered body according to claim 1, wherein the rare earth aluminate crystal phase is derived from primary particles of the rare earth aluminate.
3. 3. The rare earth aluminate sintered body according to claim 1, wherein the rare earth aluminate phosphor crystal phase contains at least one element selected from the group consisting of Y, La, Gd, Tb and Lu.
4. 3. The rare earth aluminate sintered body according to claim 1, wherein the rare earth aluminate crystal phase contains at least one element selected from the group consisting of Gd, Tb and Lu.
5. 3. The rare earth aluminate sintered body according to claim 1, wherein the rare earth aluminate crystal phase is in a range of 1.0 vol. % to 10.0 vol. % relative to 100 vol. % in total of the crystal agglomerates and the rare earth aluminate crystal phase.
6. 3. The rare earth aluminate sintered body according to claim 1, wherein the rare earth aluminate phosphor crystal phase has a composition represented by the following formula (I): (R) 1 1-n Yes n ) 3 (Al) 1-m M 1 m ) 5k O 12 (I) (In the above formula (I), R 1 is at least one element selected from the group consisting of Y, La, Lu, Gd and Tb, M 1 is at least one element selected from the group consisting of Ga and Sc, and m, n, and k satisfy 0≦m≦0.02, 0.002≦n≦0.017, and 0.95≦k≦1.10, respectively.
7. 3. The rare earth aluminate sintered body according to claim 1, wherein the rare earth aluminate crystal phase has a composition represented by the following formula (II): R 2 Al 1-j M 2 j O 3 (II) (In the above formula (II), R 2 is at least one element selected from the group consisting of Gd, Tb and Lu, M 2 is at least one element selected from the group consisting of Ga and Sc, and j satisfies 0≦j≦0.
02.
8. preparing a first raw material mixture obtained by wet mixing and then drying; dry mixing the first raw material mixture with rare earth aluminate particles; dry-mixing the first raw material mixture with the rare earth aluminate particles to obtain a mixture; and shaping the mixture. and calcining the molded body obtained by molding the mixture. a crystal agglomerate grains including a rare earth aluminate phosphor crystal phase formed from the first raw material mixture; and a rare earth aluminate crystal phase formed from the rare earth aluminate particles arranged around the crystal agglomerate grains, In one cross-sectional view, the rare earth aluminate crystal phase includes two or more of the crystal agglomerates, and the rare earth aluminate crystal phase is disposed between two of the crystal agglomerates; A method for producing a rare earth aluminate sintered body, comprising the steps of: obtaining a rare earth aluminate sintered body in which the rare earth aluminate crystal phase has a refractive index different from that of the rare earth aluminate phosphor crystal phase.
9. When preparing the first raw material mixture, the first raw material mixture contains at least one element R selected from the group consisting of Y, La, Lu, Gd, and Tb. 1 a first oxide particle containing Ce, a second oxide particle containing Al, and optionally at least one element M selected from the group consisting of Ga and Sc. 1 and optionally rare earth aluminate phosphor particles.
10. When preparing the rare earth aluminate particles, At least one element R selected from the group consisting of Gd, Tb and Lu 2 a fifth oxide particle containing Al, and an element M selected from the group consisting of Ga and Sc, as required. 2 and a seventh oxide particle comprising:
10. The method for producing a rare earth aluminate sintered body according to claim 8 or 9, further comprising firing the second raw material mixture obtained by the wet mixing at a temperature in the range of 1000° C. or more and 1600° C. or less, thereby producing the rare earth aluminate particles.
11. The method for producing a rare earth aluminate sintered body according to claim 8 or 9, wherein the sintering temperature when the molded body is sintered is within a range of 1300° C. or more and 1800° C. or less.
12. A method for producing a rare earth aluminate sintered body as described in claim 10, wherein the liquid used in the wet mixing is at least one selected from the group consisting of deionized water, water and ethanol, and the liquid is in the range of 10 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the first raw material mixture.
13. A method for producing a rare earth aluminate sintered body as described in claim 8, wherein the content of the rare earth aluminate particles is in the range of 1.0 mass% or more and 20.0 mass% or less relative to a total amount of 100 mass% of the first raw material mixture and the rare earth aluminate particles.
14. A method for producing a rare earth aluminate sintered body as described in claim 9, wherein the mass ratio of the rare earth aluminate phosphor particles contained in the first raw material mixture is within the range of 10 mass% or more and 90 mass% or less relative to a total of 100 mass% of the first oxide particles, the second oxide particles, the third oxide particles, and, if necessary, the fourth oxide particles.
Citation Information
Patent Citations
Wavelength conversion member, light-emitting device, and method of manufacturing wavelength conversion member
JP2011256371A
Strongly scattering ceramic converter and method for producing the same
JP2017197774A
Phosphor, wavelength conversion element, light source device, and projector
JP2019066880A
Ceramic composite
JP2021151933A
Ceramic complex and method for producing the same
JP2022030048A