Solid electrolyte material and battery using same
A sulfur-free solid electrolyte material of Li, Ca, Y, Sm, and O with X as F, Cl, or Br addresses the conductivity and safety issues of sulfide electrolytes, enabling high-performance all-solid-state batteries.
Patent Information
- Application Number
- JP2022511544
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2020-12-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Existing solid electrolytes, such as sulfide solid electrolytes, suffer from issues like hydrogen sulfide generation when exposed to the atmosphere and have lower lithium ion conductivity, limiting their safety and performance in batteries.
A solid electrolyte material composed of Li, Ca, Y, Sm, and O, with X being F, Cl, or Br, is developed, which does not contain sulfur and exhibits high lithium ion conductivity, achieving ionic conductivities of 1×10^-5 S/cm or more.
The new electrolyte material provides safe and efficient charge and discharge characteristics for all-solid-state batteries, with improved lithium ion conductivity and stability, avoiding hydrogen sulfide generation.
Smart Images

Figure 0007584107000003 
Figure 0007584107000004 
Figure 0007584107000005
Abstract
Description
Technical Field
[0001] The present disclosure relates to a solid electrolyte material and a battery using the same.
Background Art
[0002] Patent Document 1 discloses an all-solid-state battery using a sulfide solid electrolyte. Patent Document 2 discloses a solid electrolyte material represented by Li 6-3z Y z X6 (where 0 < z < 2 is satisfied and X is Cl or Br).
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0004] An object of the present disclosure is to provide a solid electrolyte material having high lithium ion conductivity.
Means for Solving the Problems
[0005] The solid electrolyte material of the present disclosure contains Li, Ca, Y, Sm, X, and O, where X is at least one selected from the group consisting of F, Cl, Br, and I.
Effects of the Invention
[0006] The present disclosure provides a solid electrolyte material having high lithium ion conductivity.
Brief Description of the Drawings
[0007] [Figure 1]FIG. 1 shows a cross-sectional view of a battery 1000 according to a second embodiment. [Diagram 2] FIG. 2 is a graph showing the X-ray diffraction patterns of the solid electrolyte materials according to Examples 1 to 4. [Diagram 3] FIG. 3 shows a schematic diagram of a pressing die 300 used to evaluate the ionic conductivity of a solid electrolyte material. [Figure 4] FIG. 4 is a graph showing a Cole-Cole plot obtained by impedance measurement of the solid electrolyte material according to Example 1. [Diagram 5] FIG. 5 is a graph showing the initial discharge characteristics of the batteries according to Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0009] (First embodiment) The solid electrolyte material according to the first embodiment contains Li, Ca, Y, Sm, X, and O, where X is at least one selected from the group consisting of F, Cl, Br, and I.
[0010] The solid electrolyte material according to the first embodiment has high lithium ion conductivity. Here, high lithium ion conductivity is, for example, 1×10 -5 That is, the solid electrolyte material according to the first embodiment has a dielectric constant of, for example, 1×10 -5 The ionic conductivity may be 1.0 S / cm or more.
[0011] The solid electrolyte material according to the first embodiment can be used to obtain an all-solid-state battery having excellent charge / discharge characteristics. The all-solid-state battery may be a primary battery or a secondary battery.
[0012] The solid electrolyte material according to the first embodiment desirably does not contain sulfur. A solid electrolyte material that does not contain sulfur is excellent in safety because it does not generate hydrogen sulfide even when exposed to the atmosphere. The sulfide solid electrolyte disclosed in Patent Document 1 may generate hydrogen sulfide when exposed to the atmosphere.
[0013] The solid electrolyte material according to the first embodiment may be substantially composed of Li, Ca, Y, Sm, X, and O. "The solid electrolyte material according to the first embodiment is substantially composed of Li, Ca, Y, Sm, X, and O" means that in the solid electrolyte material according to the first embodiment, the molar ratio (i.e., molar fraction) of the total amount of substance of Li, Ca, Y, Sm, X, and O to the total amount of substance of all elements constituting the solid electrolyte material is 90% or more. As an example, the molar ratio may be 95% or more. The solid electrolyte material according to the first embodiment may be composed only of Li, Ca, Y, Sm, X, and O.
[0014] To enhance the ionic conductivity of the solid electrolyte material, X may be Cl and Br.
[0015] In order to increase the ionic conductivity of the solid electrolyte material, the solid electrolyte material according to the first embodiment may further include at least one selected from the group consisting of Gd, Sr, Ba, Al, Sc, Ga, Bi, La, Zr, Hf, Ta, and Nb.
[0016] The transition metals contained in the solid electrolyte material according to the present embodiment may be only Y and Sm, excluding elements contained as unavoidable impurities.
[0017] The X-ray diffraction pattern of the solid electrolyte material according to the first embodiment can be obtained using Cu-Kα radiation. In the obtained X-ray diffraction pattern, peaks may be present in the range of diffraction angles 2θ of 14.9° to 16.0°, 16.2° to 17.4°, 22.3° to 23.5°, 28.1° to 29.2°, 30.0° to 31.2°, 32.1° to 33.3°, 39.2° to 40.3°, 47.0° to 48.1°, and 51.5° to 52.6°. Such a solid electrolyte material has high ionic conductivity.
[0018] In order to increase the ionic conductivity of the solid electrolyte material, the following four formulas may be satisfied: 2.6≦x≦3.4, 0.09≦y≦0.11, 1.2≦z≦2.1, and 2.7≦w≦4.4, Where: x represents the molar ratio of Li to the sum of Y and Sm; y represents the molar ratio of Ca to the sum of Y and Sm; z represents the molar ratio of Br to the sum of Y and Sm; w represents the molar ratio of Cl to the total of Y and Sm.
[0019] In order to further increase the ionic conductivity of the solid electrolyte material, the following four formulas may be satisfied: 2.9≦x≦3.1, 0.09≦y≦0.11, 1.3≦z≦1.9, and 3.0≦w≦4.0
[0020] In order to increase the ionic conductivity of the solid electrolyte material, the molar ratio of O to the sum of Y and Sm may be greater than 0 and less than or equal to 0.36.
[0021] In order to increase the ionic conductivity of the solid electrolyte material, in the solid electrolyte material according to the first embodiment, the molar ratio of O to the sum of Y and Sm may be greater than 0 and less than or equal to 0.08. The molar ratio of O to the sum of Y and Sm may be greater than 0 and less than or equal to 0.04. The molar ratio of O to the sum of Y and Sm may be greater than 0 and less than or equal to 0.01.
[0022] The shape of the solid electrolyte material according to the first embodiment is not limited. Examples of the shape are needle-like, spherical, or elliptical. The solid electrolyte material according to the first embodiment may be particles. The solid electrolyte material according to the first embodiment may be formed to have a pellet or plate shape.
[0023] When the solid electrolyte material according to the first embodiment has a particulate shape (e.g., spherical shape), the solid electrolyte material according to the first embodiment may have a median diameter of 0.1 μm or more and 100 μm or less. The median diameter means a particle diameter at which the cumulative volume in the volumetric particle size distribution is 50%. The volumetric particle size distribution is measured, for example, by a laser diffraction measuring device or an image analyzer.
[0024] In order to increase the ionic conductivity of the solid electrolyte material according to the first embodiment and to satisfactorily disperse the solid electrolyte material according to the first embodiment and the active material, the median diameter may be 0.5 μm or more and 10 μm or less.
[0025] <Method of manufacturing solid electrolyte material> The solid electrolyte material according to the first embodiment can be produced by the following method.
[0026] First, raw material powders are prepared and mixed to obtain a desired composition.
[0027] When preparing a solid electrolyte material consisting of Li, Ca, Y, Sm, Br, Cl, and O, LiCl raw material powder, LiBr raw material powder, YCl3 raw material powder, SmCl3 raw material powder, and CaBr2 are mixed. The obtained mixed powder is fired in an inert gas atmosphere (e.g., an argon atmosphere having a dew point of -60°C or less) in which the oxygen concentration and the moisture concentration are adjusted. The firing temperature may be, for example, 200°C or more and 650°C or less. The obtained fired product is left to stand in an atmosphere having a relatively high dew point (e.g., a dry atmosphere having a dew point of -30°C).
[0028] Then, for example, the solid electrolyte material is fired at a temperature equal to or higher than the melting point (for example, 500°C) in an inert gas atmosphere (for example, an argon atmosphere having a dew point of -60°C or lower) in which the oxygen concentration and moisture concentration are adjusted. By firing at a temperature equal to or higher than the melting point, O can be present throughout the solid electrolyte material. The raw material powders may be mixed in a pre-adjusted molar ratio to offset composition changes that may occur in the synthesis process. The amount of oxygen in the solid electrolyte material is determined by the selection of the raw material powder, the oxygen concentration in the atmosphere, the moisture concentration in the atmosphere, and the reaction time. In this manner, the solid electrolyte material according to the first embodiment is obtained.
[0029] The fired product obtained by the first firing may be used as the solid electrolyte material according to the first embodiment.
[0030] The raw material powders to be mixed may be oxides and halides. For example, Y2O3, Sm2O3, NH4Cl, NH4Br, LiCl, LiBr, CaCl2, and CaBr2 may be used as raw material powders.
[0031] It is believed that the oxygen constituting the solid electrolyte material according to the first embodiment is taken in from the atmosphere having the above-mentioned relatively high dew point.
[0032] Second embodiment The second embodiment will be described below. The matters described in the first embodiment may be omitted as appropriate.
[0033] The battery according to the second embodiment includes a positive electrode, a negative electrode, and an electrolyte layer. The electrolyte layer is disposed between the positive electrode and the negative electrode. At least one selected from the group consisting of the positive electrode, the electrolyte layer, and the negative electrode contains the solid electrolyte material according to the first embodiment.
[0034] The battery according to the second embodiment has excellent charge / discharge characteristics since it contains the solid electrolyte material according to the first embodiment.
[0035] FIG. 1 shows a cross-sectional view of a battery 1000 according to a second embodiment.
[0036] The battery 1000 includes a positive electrode 201, an electrolyte layer 202, and a negative electrode 203. The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203.
[0037] The positive electrode 201 contains positive electrode active material particles 204 and solid electrolyte particles 100 .
[0038] The electrolyte layer 202 contains an electrolyte material (eg, a solid electrolyte material).
[0039] The negative electrode 203 contains negative electrode active material particles 205 and solid electrolyte particles 100 .
[0040] The solid electrolyte particle 100 is a particle containing the solid electrolyte material according to the first embodiment as a main component. Here, the particle containing the solid electrolyte material according to the first embodiment as a main component means a particle in which the component contained most abundantly by mass ratio is the solid electrolyte material according to the first embodiment. The solid electrolyte particle 100 may be a particle made of the solid electrolyte material according to the first embodiment.
[0041] The positive electrode 201 contains a material capable of absorbing and releasing metal ions (for example, lithium ions). The material is, for example, a positive electrode active material (for example, positive electrode active material particles 204).
[0042] Examples of the positive electrode active material are lithium-containing transition metal oxides, transition metal fluorides, polyanion materials, fluorinated polyanion materials, transition metal sulfides, transition metal oxyfluorides, transition metal oxysulfides, or transition metal oxynitrides. Examples of lithium-containing transition metal oxides are LiNi 1-d-f Co d Al f O2 (where 0 <d、0<f、かつ0<(d+f)<1)またはLiCoO2である。
[0043] In order to disperse the positive electrode active material particles 204 and the solid electrolyte particles 100 well in the positive electrode 201, the positive electrode active material particles 204 may have a median diameter of 0.1 μm or more. This good dispersion improves the charge / discharge characteristics of the battery 1000. In order to rapidly diffuse lithium in the positive electrode active material particles 204, the positive electrode active material particles 204 may have a median diameter of 100 μm or less. Due to the rapid diffusion of lithium, the battery 1000 can operate at a high output. As described above, the positive electrode active material particles 204 may have a median diameter of 0.1 μm or more and 100 μm or less.
[0044] In order to disperse the positive electrode active material particles 204 and the solid electrolyte particles 100 well in the positive electrode 201 , the positive electrode active material particles 204 may have a larger median diameter than the solid electrolyte particles 100 .
[0045] To increase the energy density and output of the battery 1000, in the positive electrode 201, the ratio of the volume of the positive electrode active material particles 204 to the total volume of the positive electrode active material particles 204 and the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.
[0046] To increase the energy density and power output of the battery 1000, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.
[0047] The electrolyte layer 202 contains an electrolyte material. The electrolyte material may be the solid electrolyte material according to the first embodiment. The electrolyte layer 202 may be a solid electrolyte layer.
[0048] The electrolyte layer 202 may be made of only the solid electrolyte material according to the first embodiment, or may be made of only a solid electrolyte material different from the solid electrolyte material according to the first embodiment.
[0049] Examples of solid electrolyte materials different from the solid electrolyte material according to the first embodiment are Li2MgX'4, Li2FeX'4, Li(Al,Ga,In)X'4, Li3(Al,Ga,In)X'6, or LiI, where X' is at least one selected from the group consisting of F, Cl, Br, and I.
[0050] In this disclosure, "(A,B,C)" means "at least one selected from the group consisting of A, B, and C."
[0051] Hereinafter, the solid electrolyte material according to the first embodiment will be referred to as a first solid electrolyte material, and a solid electrolyte material different from the solid electrolyte material according to the first embodiment will be referred to as a second solid electrolyte material.
[0052] The electrolyte layer 202 may contain not only the first solid electrolyte material but also the second solid electrolyte material. The first solid electrolyte material and the second solid electrolyte material may be uniformly dispersed. A layer made of the first solid electrolyte material and a layer made of the second solid electrolyte material may be stacked along the stacking direction of the battery 1000.
[0053] In order to suppress short circuits between the positive electrode 201 and the negative electrode 203 and to increase the output of the battery, the electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less.
[0054] The negative electrode 203 contains a material capable of absorbing and releasing metal ions (for example, lithium ions). The material is, for example, a negative electrode active material (for example, negative electrode active material particles 205).
[0055] Examples of the negative electrode active material are metal materials, carbon materials, oxides, nitrides, tin compounds, or silicon compounds. The metal material may be a single metal or an alloy. Examples of the metal material are lithium metal or lithium alloys. Examples of the carbon material are natural graphite, coke, partially graphitized carbon, carbon fiber, spherical carbon, artificial graphite, or amorphous carbon. From the viewpoint of capacity density, suitable examples of the negative electrode active material are silicon (i.e., Si), tin (i.e., Sn), silicon compounds, or tin compounds.
[0056] In the negative electrode 203, in order to disperse the negative electrode active material particles 205 and the solid electrolyte particles 100 well, the negative electrode active material particles 205 may have a median diameter of 0.1 μm or more. This good dispersion improves the charge / discharge characteristics of the battery. In order to rapidly diffuse lithium in the negative electrode active material particles 205, the negative electrode active material particles 205 may have a median diameter of 100 μm or less. Due to the rapid diffusion of lithium, the battery can operate at a high output. As described above, the negative electrode active material particles 205 may have a median diameter of 0.1 μm or more and 100 μm or less.
[0057] In order to disperse the negative electrode active material particles 205 and the solid electrolyte particles 100 well in the negative electrode 203 , the negative electrode active material particles 205 may have a larger median diameter than the solid electrolyte particles 100 .
[0058] To increase the energy density and output of the battery 1000, in the negative electrode 203, the ratio of the volume of the negative electrode active material particles 205 to the total volume of the negative electrode active material particles 205 and the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.
[0059] To increase the energy density and power output of the battery 1000, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.
[0060] In order to enhance ionic conductivity, chemical stability, and electrochemical stability, at least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a second solid electrolyte material.
[0061] As mentioned above, the second solid electrolyte material may be a halide solid electrolyte. Examples of halide solid electrolytes are Li2MgX'4, Li2FeX'4, Li(Al,Ga,In)X'4, Li3(Al,Ga,In)X'6, or LiI, where X' is at least one selected from the group consisting of F, Cl, Br, and I.
[0062] The second solid electrolyte material may be a sulfide solid electrolyte.
[0063] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4, or Li 10 GeP2S 12 It is.
[0064] The second solid electrolyte material may be an oxide solid electrolyte.
[0065] Examples of oxide solid electrolytes include: (i) NASICON-type solid electrolytes such as LiTi2(PO4)3 or elemental substitutions thereof; (ii) Perovskite-type solid electrolytes such as (LaLi)TiO3; (iii) Li 14 ZnGeO 16 LISICON-type solid electrolytes such as Li4SiO4, LiGeO4, or elemental substitutions thereof; (iv) Li7La3Zr2O 12 or an element-substituted garnet-type solid electrolyte; or (v) Li3PO4 or its N-substituted derivatives It is.
[0066] The second solid electrolyte material may be an organic polymer solid electrolyte.
[0067] Examples of organic polymer solid electrolytes include polymer compounds and lithium salt compounds. The polymer compounds may have an ethylene oxide structure. Polymer compounds having an ethylene oxide structure can contain a large amount of lithium salt, and therefore can further increase ionic conductivity.
[0068] Examples of the lithium salt are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.
[0069] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a nonaqueous electrolyte, a gel electrolyte, or an ionic liquid for the purpose of facilitating the exchange of lithium ions and improving the output characteristics of the battery 1000.
[0070] The non-aqueous electrolyte contains a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent.
[0071] Examples of non-aqueous solvents are cyclic carbonate solvents, chain carbonate solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents, or fluorine solvents. Examples of cyclic carbonate solvents are ethylene carbonate, propylene carbonate, or butylene carbonate. Examples of chain carbonate solvents are dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dioxane, or 1,3-dioxolane. Examples of chain ether solvents are 1,2-dimethoxyethane or 1,2-diethoxyethane. Examples of cyclic ester solvents are γ-butyrolactone. Examples of chain ester solvents are methyl acetate. Examples of fluorine solvents are fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, or fluorodimethylene carbonate. One type of non-aqueous solvent selected from these may be used alone, or a mixture of two or more types of non-aqueous solvents selected from these may be used.
[0072] Examples of the lithium salt are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.
[0073] The concentration of the lithium salt is, for example, in the range of 0.5 mol / liter to 2 mol / liter.
[0074] The gel electrolyte may be a polymer material impregnated with a non-aqueous electrolyte, such as polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.
[0075] Examples of cations contained in ionic liquids are: (i) Aliphatic chain quaternary salts such as tetraalkylammonium or tetraalkylphosphonium salts, (ii) aliphatic cyclic ammonium such as pyrrolidiniums, morpholiniums, imidazoliniums, tetrahydropyrimidiniums, piperaziniums, or piperidiniums, or (iii) Nitrogen-containing heterocyclic aromatic cations such as pyridiniums or imidazoliums. An example of an anion contained in an ionic liquid is PF6 - , BF4 - , SbF6 - , AsF6 - , SO3CF3 - , N(SO2CF3)2 - , N(SO2C2F5)2 - , N(SO2CF3)(SO2C4F9) - , or C(SO2CF3)3 - It is.
[0076] The ionic liquid may contain a lithium salt.
[0077] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a binder for the purpose of improving adhesion between particles.
[0078] Examples of the binder are polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylic acid methyl ester, polyacrylic acid ethyl ester, polyacrylic acid hexyl ester, polymethacrylic acid, polymethacrylic acid methyl ester, polymethacrylic acid ethyl ester, polymethacrylic acid hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene butadiene rubber, or carboxymethylcellulose. Copolymers may also be used as binders. Examples of such binders are copolymers of two or more materials selected from the group consisting of tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. A mixture of two or more materials selected from these may be used as the binder.
[0079] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive assistant to enhance electronic conductivity.
[0080] Examples of the conductive additive include: (i) Graphites, such as natural or synthetic graphite; (ii) Carbon blacks such as acetylene black or ketjen black; (iii) conductive fibers, such as carbon or metal fibers; (iv) fluorocarbons, (v) Metal powders such as aluminum; (vi) conductive whiskers such as zinc oxide or potassium titanate; (vii) a conductive metal oxide, such as titanium dioxide; or (viii) Conductive polymers such as polyaniline, polypyrrole, or polythiophene In order to reduce costs, the above-mentioned conductive assistant (i) or (ii) may be used.
[0081] Examples of the shape of the battery according to the second embodiment are a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminate type.
[0082] The battery according to the second embodiment may be manufactured, for example, by preparing a material for forming a positive electrode, a material for forming an electrolyte layer, and a material for forming a negative electrode, and producing a laminate in which the positive electrode, the electrolyte layer, and the negative electrode are arranged in this order by a known method. EXAMPLES
[0083] Hereinafter, the present disclosure will be described in more detail with reference to examples.
[0084] Example 1 [Preparation of solid electrolyte materials] In an argon atmosphere having a dew point of -60°C or less and an oxygen concentration of 0.0001% by volume or less (hereinafter referred to as "dry argon atmosphere"), LiCl, LiBr, YCl3, SmCl3, and CaBr2 were prepared as raw material powders in a molar ratio of about LiCl:LiBr:YCl3:SmCl3:CaBr2=1:1.8:0.8:0.2:0.1. These materials were ground and mixed in a mortar. The resulting mixture was fired at 500°C for 1 hour in an alumina crucible, and then ground in the mortar. In this manner, a solid electrolyte material according to Example 1 was obtained.
[0085] [Composition analysis of solid electrolyte materials] The contents of Li, Ca, Sm and Y per unit weight of the solid electrolyte material according to Example 1 were measured by high-frequency inductively coupled plasma optical emission spectrometry using a high-frequency inductively coupled plasma optical emission spectrometry analyzer (iCAP7400, manufactured by Thermo Fisher Scientific). The contents of Br and Cl of the solid electrolyte material according to Example 1 were measured by ion chromatography using an ion chromatograph (ICS-2000, manufactured by Dionex). Based on the contents of Li, Ca, Y, Sm, Br and Cl obtained from these measurement results, the Li:Ca:Y:Sm:Br:Cl molar ratio was calculated. As a result, the solid electrolyte material according to Example 1 had a Li:Ca:Y:Sm:Br:Cl molar ratio of 3.07:0.10:0.80:0.20:1.80:3.75.
[0086] The mass of O relative to the total mass of the solid electrolyte material according to Example 1 was measured by a non-dispersive infrared absorption method using an oxygen / nitrogen / hydrogen analyzer (EMGA-930, manufactured by Horiba, Ltd.). As a result, the mass ratio of O was 0.03%. Based on this, the (Y+Sm):O molar ratio was calculated. As a result, the solid electrolyte material according to Example 1 had a (Y+Sm):O molar ratio of 1.00:0.01.
[0087] In the compositional analysis, elements with a mole fraction less than 0.01% relative to the sum of Y and Sm were considered as impurities.
[0088] [X-ray diffraction] The X-ray diffraction pattern of the solid electrolyte material according to Example 1 was measured using an X-ray diffractometer (MiniFlex600, manufactured by RIGAKU) in a dry environment with a dew point of -45°C or less. Cu-Kα radiation (wavelengths 1.5405 Å and 1.5444 Å) was used as the X-ray source.
[0089] As a result of X-ray diffraction measurement, peaks were present at 15.43°, 16.80°, 22.90°, 28.67°, 30.59°, 32.76°, 39.80°, 47.55°, and 52.05°. FIG. 2 is a graph showing the X-ray diffraction pattern of the solid electrolyte material according to Example 1.
[0090] [Evaluation of ionic conductivity] 3 is a schematic diagram of a pressure molding die 300 used to evaluate the ionic conductivity of a solid electrolyte material. The pressure molding die 300 had an upper punch 301, a frame 302, and a lower punch 303. The frame 302 was made of insulating polycarbonate. The upper punch 301 and the lower punch 303 were both made of electronically conductive stainless steel.
[0091] Using the pressure molding die 300 shown in FIG. 3, the ionic conductivity of the solid electrolyte material according to Example 1 was measured by the following method.
[0092] In a dry argon atmosphere, the powder of the solid electrolyte material according to Example 1 was filled into the inside of a pressure molding die 300. Inside the pressure molding die 300, a pressure of 400 MPa was applied to the solid electrolyte material according to Example 1 (i.e., the powder of the solid electrolyte material 101 in FIG. 3) using an upper punch 301 and a lower punch 303.
[0093] While the pressure was applied, the upper punch 301 and the lower punch 303 were connected to a potentiostat (VersaSTAT4, manufactured by Princeton Applied Research). The upper punch 301 was connected to a working electrode and a terminal for measuring potential. The lower punch 303 was connected to a counter electrode and a reference electrode. The impedance of the solid electrolyte material according to Example 1 was measured at room temperature by an electrochemical impedance measurement method.
[0094] FIG. 4 is a graph showing a Cole-Cole plot obtained by impedance measurement of the solid electrolyte material according to Example 1.
[0095] In Fig. 4, the real value of the impedance at the measurement point where the absolute value of the phase of the complex impedance is the smallest was considered to be the resistance value for the ion conduction of the solid electrolyte material according to Example 1. The real value is indicated by an arrow R SE Using the resistance value, the ionic conductivity was calculated based on the following formula (1). σ = (R SE ×S / t) -1 (1) Here, σ is the ionic conductivity. S is the contact area of the solid electrolyte material with the punch upper portion 301 (equal to the cross-sectional area of the hollow portion of the frame mold 302 in FIG. 3). R SE is the resistance value of the solid electrolyte material in the impedance measurement, and t is the thickness of the solid electrolyte material to which pressure is applied (equal to the thickness of the layer formed from the powder 101 of the solid electrolyte material in FIG. 3).
[0096] The ionic conductivity of the solid electrolyte material according to Example 1 measured at 25° C. was 3.0×10 -3 It was S / cm.
[0097] [Battery construction] In a dry argon atmosphere, the solid electrolyte material according to Example 1 and the active material LiCoO2 were prepared in a volume ratio of 70:30. These materials were mixed in an agate mortar. In this way, a mixture was obtained.
[0098] In an insulating cylinder having an inner diameter of 9.5 mm, the solid electrolyte material according to Example 1 (100 mg), the above mixture (12.0 mg), and aluminum powder (14.7 mg) were laminated in this order. A pressure of 300 MPa was applied to this laminate to form a first electrode and a solid electrolyte layer. The solid electrolyte layer had a thickness of about 500 μm.
[0099] Next, a metal In foil was laminated on the solid electrolyte layer. The solid electrolyte layer was sandwiched between the metal In foil and the first electrode. The metal In foil had a thickness of 200 μm. Next, a pressure of 80 MPa was applied to the metal In foil to form a second electrode.
[0100] A current collector made of stainless steel was attached to the first electrode and the second electrode, and then a current collector lead was attached to the current collector. Finally, the inside of the insulating cylinder was isolated from the outside atmosphere using an insulating ferrule, and the inside of the cylinder was sealed. In this way, the battery according to Example 1 was obtained.
[0101] [Charge / discharge test] 5 is a graph showing the initial discharge characteristics of the battery according to Example 1. A charge / discharge test was carried out as follows.
[0102] The battery according to Example 1 was placed in a thermostatic chamber at 25°C.
[0103] 86μA / cm 3 The battery according to Example 1 was charged until a voltage of 3.7 V was reached at a current density of 0.05 C, which corresponds to a 0.05 C rate.
[0104] Next, 86 μA / cm 3 The battery according to Example 1 was discharged at a current density of 0.1 V until a voltage of 1.9 V was reached.
[0105] As a result of the charge / discharge test, the battery according to Example 1 had an initial discharge capacity of 515 μAh.
[0106] (Examples 2 to 4) In Example 2, the solid electrolyte material according to Example 1 was left to stand for about 30 minutes in a dry atmosphere having a dew point of -30°C and an oxygen concentration of 20.9% by volume. It was then fired at 500°C for 1 hour in a dry argon atmosphere, and then crushed in a mortar. In this way, the solid electrolyte material according to Example 2 was obtained.
[0107] In Example 3, the solid electrolyte material according to Example 3 was obtained in the same manner as in Example 2, except that the time during which the material was left standing in a dry atmosphere having a dew point of -30°C and an oxygen concentration of 20.9% by volume was 2 hours instead of about 30 minutes.
[0108] In Example 4, the solid electrolyte material according to Example 4 was obtained in the same manner as in Example 2, except that the time during which the material was left standing in a dry atmosphere having a dew point of -30°C and an oxygen concentration of 20.9% by volume was 80 hours instead of about 30 minutes.
[0109] The element ratio (molar ratio), X-ray diffraction, and ionic conductivity of the solid electrolyte materials according to Examples 2 to 4 were measured in the same manner as in Example 1. The measurement results are shown in Tables 1 and 2. FIG. 2 is a graph showing the X-ray diffraction patterns of the solid electrolyte materials according to Examples 2 to 4.
[0110] The mass ratios of oxygen to the entire solid electrolyte material in Examples 2 to 4 were 0.13%, 0.31%, and 1.58%, respectively.
[0111] The solid electrolyte materials according to Examples 2 to 4 were used to obtain the batteries according to Examples 2 to 4 in the same manner as in Example 1.
[0112] Using the batteries according to Examples 2 to 4, charge / discharge tests were carried out in the same manner as in Example 1.
[0113] The cells according to Examples 2 to 4 charged and discharged as well as the cell according to Example 1.
[0114] Comparative Example 1 In a dry argon atmosphere, LiCl and FeCl2 were prepared as raw material powders in a molar ratio of LiCl:FeCl2=2:1. These materials were milled using a planetary ball mill at 600 rpm for 25 hours to cause a mechanochemical reaction. In this manner, a solid electrolyte material according to Comparative Example 1 was obtained. The solid electrolyte material according to Comparative Example 1 was a known halide solid electrolyte material having a composition represented by Li2FeCl4.
[0115] The ionic conductivity of the solid electrolyte material according to Comparative Example 1 was measured in the same manner as in Example 1. As a result, the ionic conductivity measured at 22° C. was 9.0×10 -6 It was S / cm.
[0116] The solid electrolyte material according to Comparative Example 1 was used to obtain a battery according to Comparative Example 1 in the same manner as in Example 1.
[0117] A charge / discharge test was carried out using the battery according to Comparative Example 1 in the same manner as in Example 1. The battery according to Comparative Example 1 only had an initial discharge capacity of 1 μAh or less. That is, the battery according to Comparative Example 1 was neither charged nor discharged.
[0118] [Table 1]
[0119] [Table 2]
[0120] <Consideration> As is clear from Table 1, the solid electrolyte materials according to Examples 1 to 4 have a melting point of 1×10 -5 It has high ionic conductivity of more than S / cm.
[0121] As is clear from Examples 1 to 4, when the molar ratio of O to the total of Y and Sm is greater than 0 and less than or equal to 0.36, the solid electrolyte material can be obtained at a concentration of 1×10 -5As is clear from a comparison of Examples 1 to 3 with Example 4, when the molar ratio is greater than 0 and less than or equal to 0.08, the solid electrolyte material has a high ionic conductivity of 1×10 -3 It has an even higher ionic conductivity of more than S / cm.
[0122] As is clear from the X-ray diffraction pattern shown in Figure 2 and Table 2, the crystal structure of the solid electrolyte material changes depending on the O content. As the O content increases, the Br and Cl contents decrease. Therefore, it is believed that O replaces Br and Cl and is incorporated into the crystal structure.
[0123] The batteries according to Examples 1 to 4 were charged and discharged at 25°C.
[0124] The solid electrolyte materials according to Examples 1 to 4 do not contain sulfur and therefore do not generate hydrogen sulfide.
[0125] As described above, the solid electrolyte material according to the present disclosure is suitable for providing a battery that has high lithium ion conductivity and can be charged and discharged well. [Industrial Applicability]
[0126] The solid electrolyte material of the present disclosure is used, for example, in an all-solid-state lithium ion secondary battery. [Explanation of symbols]
[0127] 100 solid electrolyte particles 101 Solid electrolyte material powder 201 Positive electrode 202 Electrolyte layer 203 Negative electrode 204 Positive electrode active material particles 205 Negative electrode active material particles 300 Pressure forming die 301 Punch top 302 Frame type 303 Punch bottom 1000 batteries
Claims
1. Li, Ca, Y, Sm, X, and O; wherein X is at least one selected from the group consisting of F, Cl, Br, and I; In an X-ray diffraction pattern obtained by X-ray diffraction measurement using Cu-Kα radiation, peaks are present in the following diffraction angle 2θ ranges: 14.9° to 16.0°, 16.2° to 17.4°, 22.3° to 23.5°, 28.1° to 29.2°, 30.0° to 31.2°, 32.1° to 33.3°, 39.2° to 40.3°, 47.0° to 48.1°, and 51.5° to 52.6°. Solid electrolyte material.
2. X is Cl and Br; The solid electrolyte material according to claim 1 .
3. Further comprising at least one selected from the group consisting of Gd, Sr, Ba, Al, Sc, Ga, Bi, La, Zr, Hf, Ta, and Nb; The solid electrolyte material according to claim 1 or 2.
4. The following four equations are satisfied: 2.6≦x≦3.4, 0.09≦y≦0.11, 1.2≦z≦2.1, and 2.7≦w≦4.4, Where: x represents the molar ratio of Li to the sum of Y and Sm; y represents the molar ratio of Ca to the sum of Y and Sm; z represents the molar ratio of Br to the sum of Y and Sm; w represents the molar ratio of Cl to the sum of Y and Sm; The solid electrolyte material according to claim 1 .
5. The molar ratio of O to the sum of Y and Sm is greater than 0 and less than or equal to 0.36; The solid electrolyte material according to claim 1 .
6. positive electrode, a negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode; Equipped with At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte layer contains the solid electrolyte material according to any one of claims 1 to 5. battery.
Citation Information
Patent Citations
Solid ionic conductor, solid electrolyte membrane, and all-solid lithium secondary battery
JP2011119158A
Method of manufacturing sulfide solid electrolyte material, sulfide solid electrolyte material, and lithium battery
JP2011129312A
Lithium ion conductor and lithium ion battery using the same
JP2017091955A
Stabilizing Coatings for Solid-State Batteries
JP2019530963A
Solid electrolyte material, and cell
WO2018025582A1