Composition for forming liquid crystal cured film and its use

The use of silicone and fluorine-based leveling agents in a specific ratio with polymerizable liquid crystal compounds addresses uneven film thickness and alignment issues, resulting in improved cured liquid crystal films for display devices.

JP7560940B2Active Publication Date: 2024-10-03SUMITOMO CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019085699
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-04-26
Publication Date
2024-10-03
Estimated Expiration
2039-04-26

AI Technical Summary

Technical Problem

Existing liquid crystal cured films suffer from uneven film thickness and alignment issues due to the addition of certain additives, which deteriorate the appearance and performance of display devices like organic EL displays.

Method used

A composition for forming a cured liquid crystal film is developed, containing silicone-based and fluorine-based leveling agents in a total amount of 3.0% by mass or less, along with a polymerizable liquid crystal compound, to achieve uniform film thickness and alignment, using a combination of acrylic leveling agents to address surface tension and local unevenness.

Benefits of technology

The composition results in a cured liquid crystal film with reduced unevenness, enhancing the appearance and performance of display devices by improving film thickness uniformity and maintaining alignment integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560940000001
    Figure 0007560940000001
  • Figure 0007560940000002
    Figure 0007560940000002
  • Figure 0007560940000003
    Figure 0007560940000003
Patent Text Reader

Abstract

To provide a liquid crystal cured film-forming composition for producing a liquid crystal cured film with less thickness unevenness.SOLUTION: A liquid crystal cured film-forming composition is provided, containing at least one type of silicon-based or fluorine-based leveling agent, at least one type of acrylic leveling agent, and at least one type of polymerizable liquid crystal compound, where the total leveling agent content is 3.0 wt.% or less with respect to a total amount of the polymerizable liquid crystal compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal cured film-forming composition, a liquid crystal cured film, an elliptically polarizing plate, and an organic EL display device. [Background technology]

[0002] An elliptical polarizing plate is an optical component in which a polarizing plate and a retardation plate are laminated, and is used, for example, in devices that display images in a flat state (such as organic EL display devices) to prevent light reflection at electrodes that constitute the device. In this elliptical polarizing plate, a so-called λ / 4 plate is used as the retardation plate.

[0003] As a retardation plate used in such an elliptically polarizing plate, one exhibiting reverse wavelength dispersion is suitable in that it exhibits equivalent retardation performance over a wide wavelength range of visible light. As a retardation plate exhibiting reverse wavelength dispersion, a retardation plate made of a horizontally aligned liquid crystal cured film obtained by polymerizing and curing a polymerizable liquid crystal compound exhibiting reverse wavelength dispersion in a state of being horizontally aligned is known.

[0004] It is also known that by forming a vertically aligned liquid crystal cured film and combining the vertically aligned liquid crystal cured film with the above-mentioned elliptically polarizing plate, it is possible to suppress oblique hue shift during black display when combined with an organic EL display device. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-163935 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, liquid crystal cured films such as horizontal alignment cured films and vertical alignment liquid crystal cured films are generally formed by producing a composition containing a polymerizable liquid crystal compound, applying the composition to a substrate or an alignment film, etc., and curing the composition to form a liquid crystal cured film, but the liquid crystal cured film formed is generally a thin film of 5 μm or less, and there has been a problem that unevenness in the film thickness significantly deteriorates the appearance of the product. In addition, when an additive is added to a composition containing a polymerizable liquid crystal compound, there has been a problem that the alignment of the polymerizable liquid crystal compound is deteriorated depending on the additive.

[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a composition for producing a liquid crystal cured film with little thickness unevenness. [Means for solving the problem]

[0008] The present inventors have conducted intensive research to solve the above problems and have completed the present invention. That is, the present invention provides the following preferred embodiments.

[0009] [1] At least one silicone-based or fluorine-based leveling agent, at least one acrylic-based leveling agent, and at least one polymerizable liquid crystal compound; A liquid crystal cured film-forming composition, wherein the total amount of a leveling agent is 3.0% by mass or less based on the total amount of a polymerizable liquid crystal compound. [2] The composition for forming a liquid crystal cured film according to [1], which comprises at least one silicone-based leveling agent, at least one acrylic-based leveling agent, and at least one polymerizable liquid crystal compound. [3] The composition for forming a liquid crystal cured film according to either [1] or [2], further comprising a dichroic dye. [4] The composition for forming a liquid crystal cured film according to any one of [1] to [3], wherein the polymerizable liquid crystal compound is a polymerizable liquid crystal compound exhibiting a smectic phase. [5] The composition for forming a liquid crystal cured film according to any one of [1] to [4], wherein the polymerizable liquid crystal compound is a liquid crystal compound having a T-shaped structure. [6] A liquid crystal cured film obtained by curing a polymerizable liquid crystal compound contained in the composition for forming a liquid crystal cured film according to any one of [1] to [5] in an aligned state. [7] The liquid crystal cured film according to [6], wherein the thickness of the liquid crystal cured film is 0.3 μm or more and 5.0 μm or less. [8] The liquid crystal cured film according to either [6] or [7], which is a horizontally aligned liquid crystal cured film in which the polymerizable liquid crystal compound is cured in a state where it is aligned in a direction parallel to the in-plane direction. [9] The liquid crystal cured film according to any one of [6] to [8], further satisfying the following formula (S1): 100nm≦ReA(550)≦180nm (S1) (In the formula, ReA(550) represents an in-plane retardation value at a wavelength of 550 nm.)

[10] The liquid crystal cured film according to any one of [6] to [9], further satisfying the following formula (S2): ReA(450) / ReA(550)<1.0 (S2) (In the formula, ReA(450) represents an in-plane retardation value at a wavelength of 450 nm.)

[11] The horizontally aligned liquid crystal cured film according to any one of [6] to

[10] , wherein the liquid crystal cured film is a horizontally aligned liquid crystal cured film, and shows a Bragg peak in X-ray diffraction measurement.

[12] The liquid crystal cured film according to either [6] or [7], which is a vertically aligned liquid crystal cured film in which the polymerizable liquid crystal compound is cured in a state where it is aligned in a direction perpendicular to the in-plane direction.

[13] The liquid crystal cured film according to

[12] , further satisfying the following relational formula (S3): -150≦RthC(550)≦-30 (S3) [In the formula (S3), RthC(550) represents the retardation value in the thickness direction of the liquid crystal cured film at a wavelength of 550 nm]

[14] The liquid crystal cured film according to either

[12] or

[13] , further satisfying the following relational formula (S4): RthC(450) / RthC(550)≦1.0 (S4) [In the formula (S4), RthC(450) represents the retardation value in the thickness direction of the cured liquid crystal film at a wavelength of 450 nm, and RthC(550) represents the retardation value in the thickness direction of the cured liquid crystal film at a wavelength of 550 nm]

[15] An elliptical polarizing plate including a horizontally aligned retardation film and a polarizing film, An elliptically polarizing plate, in which at least one of the horizontal alignment film and the polarizing film is the liquid crystal cured film according to any one of [6] to

[11] .

[16] An elliptical polarizing plate comprising a horizontally aligned retardation film, a vertically aligned liquid crystal cured film, and a polarizing film, An elliptically polarizing plate, wherein at least one of a horizontally aligned film, a vertically aligned liquid crystal cured film, and a polarizing film is the liquid crystal cured film according to any one of [6] to

[14] .

[17] The elliptical polarizing plate according to either

[15] or

[16] , wherein the angle between the slow axis of the horizontally aligned retardation film and the absorption axis of the polarizing plate is 45±5°.

[18] An organic electroluminescence display device comprising the elliptically polarizing plate according to any one of

[15] to

[17] . Effect of the Invention

[0010] According to the present invention, two types of leveling agents (i.e., a silicon-based or fluorine-based leveling agent and an acrylic-based leveling agent) are blended in a polymerizable liquid crystal composition in such a blending amount that the total amount of the leveling agents is 3.0 mass % or less based on the total amount of the polymerizable liquid crystal compound. These two types of leveling agents have different functions in the liquid crystal composition. The silicon-based or fluorine-based leveling agent has a tendency to segregate on the surface layer of the liquid crystal composition due to its low surface free energy, and is effective in flattening the surface layer of the coating film by reducing the surface tension of the composition, while the acrylic leveling agent has an effect of uniforming local unevenness in the liquid physical properties of the liquid crystal composition in the film, and by including a combination of the two in a specific blending amount, a liquid crystal cured film with less unevenness in film thickness can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0012] <Leveling agent> As described above, the present invention is characterized in that at least one type of silicone-based or fluorine-based leveling agent and at least one type of acrylic-based leveling agent are blended in the polymerizable liquid crystal composition in such a manner that the total amount of the leveling agents is 3.0 mass % or less relative to the total amount of the polymerizable liquid crystal compounds.

[0013] Examples of the silicon-based leveling agent include leveling agents having a polyorganosiloxane skeleton. Examples of the group bonded to the silicon atom (silicon atom forming a siloxane bond) in the polyorganosiloxane include a hydrocarbon group. Among them, an alkyl group or an aryl group having 1 to 10 carbon atoms is preferable, more preferably a methyl group or a phenyl group, and even more preferably a methyl group. The group bonded to the silicon atom may be of only one type or of two or more types. The number of repetitions of the siloxane unit (degree of polymerization) is not particularly limited, but is preferably 2 to 10,000, more preferably 3 to 5,000, and even more preferably 5 to 1,000.

[0014] As the silicon-based leveling agent, commercially available products can be used. For example, BYK-300, BYK-302, BYK-306, BYK-307, BYK-310, BYK-313, BYK-315N, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-342, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-370, BYK-377, BYK-378, BYK-3455, BYK-UV3510 (all manufactured by BYK Japan Co., Ltd.), KF-945, KF-6015, KF-6020 (all manufactured by Shin-Etsu Chemical Co., Ltd.) (manufactured by Degussa), TEGORad2300, TEGORad2200N, TEGORad2011 (manufactured by Degussa), and as those having a radical polymerizable group such as a (meth)acryloyl group added to the polyether chain, BYK-UV3500, BYK-UV3505, BYK-3510, BYK-UV3530, BYK-UV3570, BYK-UV3575, BYK-UV3576 (all manufactured by BYK-Chemie Japan K.K.), KP-422, KP-416, KP-418, KP-410, KP-411, KP-412, KP-413, KP-423, KP-414, KP-415, KP-420, KP-983 (all manufactured by Shin-Etsu Chemical Co., Ltd.), etc.

[0015] The content of the silicon-based leveling agent in the polymerizable liquid crystal composition is preferably 0.001 to 2 parts by mass, more preferably 0.01 to 1.5 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, relative to 100 parts by mass of the above-mentioned polymerizable liquid crystal compound.

[0016] The above-mentioned fluorine-based leveling agent is not particularly limited, but includes leveling agents having a fluoroaliphatic hydrocarbon skeleton. The above-mentioned fluoroaliphatic hydrocarbon skeleton is not particularly limited, but includes, for example, fluoroalkanes having 1 to 10 carbon atoms such as fluoromethane, fluoroethane, fluoropropane, fluoroisopropane, fluorobutane, fluoroisobutane, fluoro t-butane, fluoropentane, and fluorohexane. The fluoroaliphatic hydrocarbon skeleton may be such that at least a part of hydrogen atoms are substituted with fluorine atoms, but is preferably a perfluoroaliphatic hydrocarbon skeleton in which all hydrogen atoms are substituted with fluorine atoms.

[0017] The fluoroaliphatic hydrocarbon skeleton may form a polyfluoroalkylene ether skeleton, which is a repeating unit via an ether bond. The fluoroaliphatic hydrocarbon group as a repeating unit is not particularly limited, but examples thereof include fluoro C1-4 alkylene groups such as fluoromethylene, fluoroethylene, fluoropropylene, and fluoroisopropylene. The fluoroaliphatic hydrocarbon group may be of only one type, or of two or more types. The number of repeats (degree of polymerization) of the fluoroalkylene ether unit is not particularly limited, but is preferably 10 to 10,000, more preferably 30 to 5,000, and even more preferably 50 to 1,000.

[0018] Examples of fluorine-based leveling agents that can be used include commercially available products such as "Megafac (registered trademark) R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482", "F-483", "F-281", "F-253", "F-251", "F-114", "F-510", "F-551", "F-552", "F-553", "F-554", "F-555" and "F-556". , "F-557", "F-558", "F-559", "F-560", "F-561", "F-562", "F-563", "F-565", "F-568", "F-569", "F-570" , "F-572", "F-574", "F-575", "F-576", "R-40", "R-41", "R-94", "RS-56", "RS-72-K", "RS-75", "RS-76-E", "RS-76-NS" , “RS-78”, “RS-90” , "DS-21" (DIC Corporation); "Surflon (registered trademark) S-381", "S-382", "S-383", "S-393", "SC-101", "SC-105", "KH-40", and "SA-100" (AGC Seimi Chemical Co., Ltd.); "E1830", "E5844" (Daikin Fine Chemical Research Institute, Ltd.); "F-TOP EF301", "F-TOP EF303", "F-TOP EF351", and "F-TOP EF352" (Mitsubishi Materials Electronic Chemicals Co., Ltd.).

[0019] The content of the fluorine-based leveling agent in the polymerizable liquid crystal composition is preferably 0.001 to 2 parts by mass, more preferably 0.01 to 1.5 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, relative to 100 parts by mass of the above-mentioned polymerizable liquid crystal compound.

[0020] The acrylic leveling agent is produced, for example, by copolymerizing a monomer having a (meth)acryloyl group. The acrylic leveling agent can be produced by copolymerizing a monomer having a hydrophilic group, such as a (meth)acrylate having a hydroxyl group and a (meth)acrylate having an alkylene oxide, typically ethylene oxide and propylene oxide, as the monomer having a (meth)acryloyl group.

[0021] The acrylic leveling agent may be a commercially available product, such as "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-356", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381", "BYK-392", "BYK-394", or "BYK-3441" (BYK Japan Co., Ltd.).

[0022] The content of the acrylic leveling agent in the polymerizable liquid crystal composition is preferably 0.001 to 3 parts by mass, more preferably 0.01 to 2 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0023] As described above, the acrylic leveling agent is unlikely to cause segregation in the thickness direction in the liquid crystal cured film, and therefore tends to deteriorate the alignment of the liquid crystal cured film. The smaller the molecular weight of the acrylic leveling agent, the less likely it is to hinder the alignment of the polymerizable liquid crystal compound, so the molecular weight (weight average molecular weight) of the acrylic leveling agent is preferably 100 to 100,000, more preferably 500 to 50,000, even more preferably 500 to 10,000, and particularly preferably 500 to 5,000.

[0024] In the present invention, it is preferable to mix at least one type of silicon-based or fluorine-based leveling agent and at least one type of acrylic-based leveling agent in an amount where the total amount of the leveling agents is 3.0% by weight or less based on the total amount of the polymerizable liquid crystal compound. As described above, the action of the silicon-based or fluorine-based leveling agent in the polymerizable liquid crystal composition is different from that of the acrylic-based leveling agent in the polymerizable liquid crystal composition, so it is preferable to mix both leveling agents. As the silicon-based or fluorine-based leveling agent, the silicon-based leveling agent is more preferable. If the total amount of the leveling agent exceeds 3.0% by weight based on the total amount of the polymerizable liquid crystal composition, the alignment of the liquid crystal tends to deteriorate. The total amount of the leveling agent is preferably 0.001 to 3% by weight, more preferably 0.01 to 2.5% by weight. If the amount of the leveling agent added is less than the above range, the effect of adding the leveling agent tends to be less exhibited. The weight ratio of the silicon-based or fluorine-based leveling agent to the acrylic leveling agent, in terms of the weight ratio of silicon-based or fluorine-based leveling agent / acrylic leveling agent, is 0.01 to 30, and more preferably 0.05 to 10. If the amount of either leveling agent is too large, the balance of the effects is lost, resulting in uneven film thickness.

[0025] <Polymerizable liquid crystal composition> The polymerizable liquid crystal compound generally includes a polymerizable liquid crystal compound exhibiting normal wavelength dispersion and a polymerizable liquid crystal compound exhibiting reverse wavelength dispersion. Either one type of polymerizable liquid crystal compound can be used alone, or both types of polymerizable liquid crystal compounds can be used in combination. When used in a vertically aligned liquid crystal cured film, it is preferable to include a polymerizable liquid crystal compound exhibiting reverse wavelength dispersion from the viewpoint of a large effect of improving the oblique reflection hue during black display when the vertically aligned liquid crystal cured film is applied to a display device. When used in a horizontally aligned liquid crystal cured film, it is preferable to include a polymerizable liquid crystal compound exhibiting reverse wavelength dispersion from the viewpoint of improving the front reflection hue during black display when the horizontally aligned liquid crystal cured film is applied to a display device.

[0026] The polymerizable liquid crystal compound exhibiting reverse wavelength dispersion is preferably a compound having the following characteristics (A) to (D). (A) A compound capable of forming a nematic phase or a smectic phase. (B) The polymerizable liquid crystal compound has π electrons in the long axis direction (a). (C) It has π electrons in a direction intersecting with the long axis direction (a) [intersecting direction (b)]. (D) The total number of π electrons present in the long axis direction (a) is N(πa), and the total number of molecular weights present in the long axis direction is N(Aa), where N(πa) is the total number of π electrons present in the long axis direction, and N(Aa) is the total number of molecular weights present in the long axis direction. The π electron density in the long axis direction (a) of a polymerizable liquid crystal compound is defined by the following formula (i): D(πa)=N(πa) / N(Aa) (i) The total number of π electrons present in the cross direction (b) is N(πb), and the total number of molecular weights present in the cross direction (b) is N(Ab), where N(πb) is the total number of π electrons present in the cross direction (b), and the π electron density in the cross direction (b) of the polymerizable liquid crystal compound is defined by the following formula (ii): D(πb)=N(πb) / N(Ab) (ii) and the formula (iii) 0≦[D(πa) / D(πb)]<1 (iii) [That is, the π electron density in the intersecting direction (b) is greater than the π electron density in the long axis direction (a)]. As described above, the polymerizable liquid crystal compound having π electrons on the long axis and in the direction intersecting therewith has, for example, a T-shaped structure.

[0027] In the above features (A) to (D), the long axis direction (a) and the number of π electrons N are defined as follows. The long axis direction (a) is, for example, in the case of a compound having a rod-like structure, the long axis direction of the rod. The number of π electrons present in the long axis direction (a), N(πa), does not include the π electrons lost due to the polymerization reaction. The number of π electrons present along the long axis (a), N(πa), is the total number of π electrons on the long axis and those conjugated with it, and includes, for example, the number of π electrons present in rings present along the long axis (a) that satisfy Hückel's rule. The number of π electrons present in the intersecting direction (b), N(πb), does not include the π electrons lost due to the polymerization reaction. A polymerizable liquid crystal compound that satisfies the above conditions has a mesogenic structure in the long axis direction, and this mesogenic structure allows the compound to exhibit a liquid crystal phase (nematic phase, smectic phase).

[0028] The polymerizable liquid crystal compound satisfying the above (A) to (D) can form a nematic phase or a smectic phase by coating on a substrate or an alignment film and heating to a temperature equal to or higher than the phase transition temperature. In the nematic phase or smectic phase formed by the alignment of the polymerizable liquid crystal compound, the long axis directions of the polymerizable liquid crystal compound are usually aligned so that they are parallel to each other, and this long axis direction is the alignment direction of the nematic phase. When such a polymerizable liquid crystal compound is made into a film and polymerized in the nematic or smectic phase state, a polymer film can be formed that is made of a polymer that is polymerized in a state of being aligned in the long axis direction (a). This polymer film absorbs ultraviolet light by π electrons in the long axis direction (a) and π electrons in the cross direction (b). Here, the maximum absorption wavelength of ultraviolet light absorbed by π electrons in the cross direction (b) is defined as λbmax. λbmax is usually 300 nm to 400 nm. The π electron density satisfies the above formula (iii), and the π electron density in the cross direction (b) is greater than the π electron density in the long axis direction (a), resulting in a polymer film in which the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the cross direction (b) is greater than the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the long axis direction (a). The ratio (the ratio of the absorbance in the cross direction (b) of linearly polarized ultraviolet light / the absorbance in the long axis direction (a)) is, for example, greater than 1.0, preferably 1.2 or more, and usually 30 or less, for example 10 or less.

[0029] The polymerizable liquid crystal compound having the above characteristics generally exhibits reverse wavelength dispersion.Specifically, for example, the compound represented by the following formula (X) can be mentioned.In the present invention, the polymerizable liquid crystal compound represented by the following formula (X) may be called a polymerizable liquid crystal compound having a T-shaped structure. [ka]

[0030] In formula (X), Ar represents a divalent group having an aromatic group which may have a substituent. The aromatic group referred to here refers to a ring structure having a π electron number of [4n+2] according to the Huckel rule, and may have two or more Ar groups, such as those exemplified by (Ar-1) to (Ar-23) described later, via a divalent linking group. Here, n represents an integer. When a ring structure is formed by including heteroatoms such as -N= or -S-, the Huckel rule is satisfied including the non-covalent bond electron pairs on these heteroatoms, and aromaticity is also included. The aromatic group preferably contains at least one of a nitrogen atom, an oxygen atom, and a sulfur atom. The aromatic group contained in the divalent group Ar may have one or more aromatic groups. When there is one aromatic group, the divalent group Ar may be a divalent aromatic group which may have a substituent. When the divalent group Ar contains two or more aromatic groups, the two or more aromatic groups may be bonded to each other via a divalent bonding group such as a single bond, -CO-O-, or -O-. G 1 and G 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. L 1 , L 2 , B 1 and B. 2 each independently represents a single bond or a divalent linking group. k and l each independently represent an integer of 0 to 3, and satisfy the relationship of 1≦k+l. Here, when 2≦k+l, B 1 and B. 2 , G 1 and G 2 may be the same as or different from each other. E 1 and E 2each independently represents an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms. In addition, a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and -CH 2 - is -O-, -S-, -SiH 2 It may be substituted with - or -C(=O)-. P 1 and P 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.

[0031] G 1 and G 2 are each independently preferably a 1,4-phenylenediyl group optionally substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group optionally substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, more preferably a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group, and particularly preferably an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group. In addition, there are multiple G 1 and G 2 At least one of L is preferably a divalent alicyclic hydrocarbon group. 1 or L 2 G binds to 1 and G 2 It is more preferable that at least one of the groups is a divalent alicyclic hydrocarbon group.

[0032] L 1 and L 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -, -R a3 COOR a4 -, -Ra5 OCOR a6 -, R a7 OC=OOR a8 -, -N=N-, -CR c =CR d -, or C≡C-, where R a1 ~R a8 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms; R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 are each independently preferably a single bond, -OR a2-1 -, -CH 2 -, -CH 2 CH 2 -,-COOR a4-1 - or O.C.O.R. a6-1 -, where R a2-1 , R a4-1 , R a6-1 are each independently a single bond, -CH 2 -, -CH 2 CH 2 - represents either 1 and L 2 are each independently preferably a single bond, -O-, or -CH 2 CH 2 -, -COO-, -COOCH 2 CH 2 -, or OCO-.

[0033] B 1 and B. 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -, -R a11 COOR a12 -, -R a13 OCOR a14 - or R a15 OC=OOR a16 -, where R a9 ~R a16 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B.2 are each independently preferably a single bond, -OR a10-1 -, -CH 2 -, -CH 2 CH 2 -,-COOR a12-1 - or O.C.O.R. a14-1 -, where R a10-1 , R a12-1 , R a14-1 are each independently a single bond, -CH 2 -, -CH 2 CH 2 - represents either 1 and B. 2 are each independently preferably a single bond, -O-, or -CH 2 CH 2 -, -COO-, -COOCH 2 CH 2 -, -OCO-, or OCOCH 2 CH 2 -It is.

[0034] From the viewpoint of expressing reverse wavelength dispersion, k and l are preferably in the range of 2≦k+l≦6, preferably k+l=4, and more preferably k=2 and l=2. When k=2 and l=2, a symmetrical structure is obtained, which is preferable.

[0035] P 1 or P 2 Examples of the polymerizable group represented by the formula (I) include an epoxy group, a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred.

[0036] It is preferable that Ar has at least one selected from an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, and an electron-withdrawing group. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, and an anthracene ring, and the like, and the benzene ring and the naphthalene ring are preferable. Examples of the aromatic heterocycle include a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, and a phenanthroline ring. Among them, it is preferable that Ar has a thiazole ring, a benzothiazole ring, or a benzofuran ring, and it is more preferable that Ar has a benzothiazole group. In addition, when Ar contains a nitrogen atom, it is preferable that the nitrogen atom has π electrons.

[0037] In formula (X), the total number of π electrons contained in the divalent aromatic group represented by Ar is N π is preferably 8 or more, more preferably 10 or more, even more preferably 14 or more, and particularly preferably 16 or more. Also, it is preferably 30 or less, more preferably 26 or less, and even more preferably 24 or less.

[0038] Examples of the aromatic group represented by Ar include the following groups.

[0039] [ka]

[0040] In formulae (Ar-1) to (Ar-23), * represents a linking portion, Z 0 , Z 1 and Z 2each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms. 0 , Z 1 and Z 2 may contain a polymerizable group.

[0041] Q 1 and Q 2 are each independently -CR 2’ R 3’ -, -S-, -NH-, -NR 2’ -, -CO- or O-; R 2’ and R 3’ each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0042] J 1 , and J. 2 each independently represents a carbon atom or a nitrogen atom.

[0043] Y 1 , Y 2 and Y 3 each independently represents an optionally substituted aromatic hydrocarbon group or an optionally substituted aromatic heterocyclic group.

[0044] W 1 and W 2 each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom; and m represents an integer of 0 to 6.

[0045] Y 1 , Y 2 and Y 3Examples of the aromatic hydrocarbon group in the formula (I) include aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and a biphenyl group, of which a phenyl group and a naphthyl group are preferred, and a phenyl group is more preferred. Examples of the aromatic heterocyclic group in the formula (I) include aromatic heterocyclic groups having 4 to 20 carbon atoms and containing at least one heteroatom, such as a nitrogen atom, an oxygen atom, or a sulfur atom, such as a furyl group, a pyrrolyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group, of which a furyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group are preferred.

[0046] Y 1 , Y 2 and Y 3 may each independently be an optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring assembly. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring assembly.

[0047] Z 0 , Z 1 and Z 2 are each preferably independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms; Z 0 is more preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group; Z 1 and Z 2 is more preferably a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, or a cyano group. 0 , Z 1 and Z 2 may contain a polymerizable group.

[0048] Q 1 and Q 2 -NH-, -S-, -NR 2’ -, -O- are preferred, R 2’ is preferably a hydrogen atom, and among these, -S-, -O-, and -NH- are particularly preferable.

[0049] Among the formulae (Ar-1) to (Ar-23), the formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.

[0050] In formulas (Ar-16) to (Ar-23), Y 1 is the nitrogen atom to which it is bonded and Z 0 and may form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include those mentioned above as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. This aromatic heterocyclic group may have a substituent. In addition, Y 1 is the nitrogen atom to which it is bonded and Z 0 In addition, it may be the above-mentioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group, for example, a benzofuran ring, a benzothiazole ring, a benzoxazole ring, etc.

[0051] In addition, in the present invention, as the polymerizable liquid crystal compound forming the liquid crystal cured film, for example, a compound containing a group represented by the following formula (Y) (hereinafter, also referred to as "polymerizable liquid crystal compound (Y)") may be used. The polymerizable liquid crystal compound (Y) generally tends to exhibit positive wavelength dispersion. The polymerizable liquid crystal compound may be used alone or in combination of two or more kinds.

[0052] P11-B11-E11-B12-A11-B13- (Y) In formula (Y), P11 represents a polymerizable group. A11 represents a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. A hydrogen atom contained in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, or a nitro group, and a hydrogen atom contained in the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms may be substituted with a fluorine atom. B11 is -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -CO-NR 16 -, -NR 16 Represents -CO-, -CO-, -CS- or a single bond. R 16 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. B12 and B13 each independently represent -C≡C-, -CH=CH-, -CH 2 -CH 2 -, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -, -NR 16 -C(=O)-, -OCH 2 -, -OCF 2 -, -CH 2 O-, -CF 2 represents O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH- or a single bond. E11 represents an alkanediyl group having 1 to 12 carbon atoms, and a hydrogen atom contained in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and a hydrogen atom contained in the alkoxy group may be substituted with a halogen atom. 2 - may be replaced by -O- or -CO-.

[0053] The number of carbon atoms in the aromatic hydrocarbon group and alicyclic hydrocarbon group of A11 is preferably in the range of 3 to 18, more preferably in the range of 5 to 12, and particularly preferably 5 or 6. A11 is preferably a cyclohexane-1,4-diyl group or a 1,4-phenylene group.

[0054] E11 is preferably a linear alkanediyl group having 1 to 12 carbon atoms. 2 - may be replaced by -O-. Specific examples of such alkyl groups include linear alkanediyl groups having 1 to 12 carbon atoms, such as a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a nonane-1,9-diyl group, a decane-1,10-diyl group, an undecane-1,11-diyl group, and a dodecane-1,12-diyl group; 2 -CH 2 -O-CH 2 -CH 2 -, -CH 2 -CH 2 -O-CH 2 -CH 2 -O-CH 2 -CH 2 - and -CH 2 -CH 2 -O-CH 2 -CH 2 -O-CH 2 -CH 2 -O-CH 2 -CH 2 --etc. As B11, -O-, -S-, -CO-O-, and -O-CO- are preferable, and among them, -CO-O- is more preferable. As B12 and B13, each independently, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)- or -OC(=O)-O- is preferable, and among them, -O- or -OC(=O)-O- is more preferable.

[0055] As the polymerizable group represented by P11, a radically polymerizable group or a cationic polymerizable group is preferred from the viewpoint of high polymerization reactivity, particularly high photopolymerization reactivity. In addition, the polymerizable group is preferably a group represented by the following formulae (P-11) to (P-15), since it is easy to handle and the liquid crystal compound can be easily produced. [ka] [In formulas (P-11) to (P-15), R 17 ~R 21each independently represents an alkyl group having 1 to 6 carbon atoms or a hydrogen atom.

[0056] Specific examples of the groups represented by formulae (P-11) to (P-15) include groups represented by the following formulae (P-16) to (P-20). [ka]

[0057] P11 is preferably a group represented by formula (P-14) to formula (P-20), and more preferably a vinyl group, a p-stilbene group, an epoxy group or an oxetanyl group. The group represented by P11-B11- is more preferably an acryloyloxy group or a methacryloyloxy group.

[0058] Examples of the polymerizable liquid crystal compound (Y) include compounds represented by formula (I), formula (II), formula (III), formula (IV), formula (V) or formula (VI). P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12 (I) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11 (II) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12 (III) P11-B11-E11-B12-A11-B13-A12-B14-A13-F11 (IV) P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12 (V) P11-B11-E11-B12-A11-B13-A12-F11 (VI) (In the formula, A12 to A14 each independently have the same meaning as A11, B14 to B16 each independently have the same meaning as B12, B17 has the same meaning as B11, and E12 has the same meaning as E11. F11 is a hydrogen atom, an alkyl group having 1 to 13 carbon atoms, an alkoxy group having 1 to 13 carbon atoms, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxyl group, a methylol group, a formyl group, or a sulfo group (-SO 3 H), a carboxy group, an alkoxycarbonyl group having 1 to 10 carbon atoms, or a halogen atom, and -CH 2 - may be replaced with -O-.

[0059] Specific examples of the polymerizable liquid crystal compound (Y) include compounds having a polymerizable group among the compounds described in “3.8.6 Network (completely crosslinked type)” and “6.5.1 Liquid crystal materials b. Polymerizable nematic liquid crystal materials” in Liquid Crystal Handbook (edited by Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000), and the polymerizable liquid crystals described in JP-A Nos. 2010-31223, 2010-270108, 2011-6360, and 2011-207765.

[0060] Specific examples of the polymerizable liquid crystal compound (Y) include compounds represented by the following formulae (I-1) to (I-4), (II-1) to (II-4), (III-1) to (III-26), (IV-1) to (IV-26), (V-1) to (V-2), and (VI-1) to (VI-6). In the following formulae, k1 and k2 each independently represent an integer of 2 to 12. These polymerizable liquid crystal compounds (Y) are preferred in terms of ease of synthesis or availability.

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064]

change

[0065]

change

[0066]

change

[0067]

change

[0068]

change

[0069]

change

[0070] By using a polymerizable liquid crystal compound exhibiting smectic liquid crystal properties, it is preferable that a horizontally aligned liquid crystal cured film or a vertically aligned liquid crystal cured film having a high degree of alignment order can be formed. In the present invention, when a polymerizable liquid crystal compound exhibiting smectic liquid crystal properties is used as the polymerizable liquid crystal compound forming the liquid crystal cured film, it is more preferable that the polymerizable liquid crystal compound is a high-order smectic phase (high-order smectic liquid crystal state) from the viewpoint of realizing a higher degree of alignment order. Here, the high-order smectic phase means a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, and a smectic L phase, and among these, a smectic B phase, a smectic F phase, and a smectic I phase are more preferable. The liquid crystal property may be a thermotropic liquid crystal or a lyotropic liquid crystal, but a thermotropic liquid crystal is preferable from the viewpoint of enabling precise film thickness control. The polymerizable liquid crystal compound exhibiting smectic liquid crystallinity may be a monomer, or may be an oligomer or polymer in which a polymerizable group is polymerized.

[0071] The polymerizable liquid crystal compound exhibiting smectic liquid crystallinity is a liquid crystal compound having at least one polymerizable group, and from the viewpoint of improving the heat resistance of the liquid crystal cured film, it is preferable that the liquid crystal compound has two or more polymerizable groups. Examples of the polymerizable group include (meth)acryloyloxy group, vinyl group, vinyloxy group, 1-chlorovinyl group, isopropenyl group, 4-vinylphenyl group, oxiranyl group, oxetanyl group, etc., and among them, it is preferable to include (meth)acryloyloxy group because it is easy to manufacture, the heat resistance of the liquid crystal cured film is easily improved, and the adhesion between the liquid crystal cured film and the substrate is easily adjusted.

[0072] An example of the polymerizable liquid crystal compound exhibiting smectic liquid crystal properties is a compound represented by the following formula (Z) (hereinafter, sometimes referred to as "polymerizable liquid crystal compound (Z)"). U 1z -V 1z -W 1z -(X 1z -Y 1z -)nz -X 2z -W 2z -V 2z -U 2z (Z) [In formula (Z), X 1z and X 2z represent, independently of each other, a divalent aromatic group or a divalent alicyclic hydrocarbon group, in which a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. 1z and X 2z At least one of these is a 1,4-phenylene group which may have a substituent or a cyclohexane-1,4-diyl group which may have a substituent. Y 1z is a single bond or a divalent linking group. nz is 1 to 3. If nz is 2 or more, multiple X 1z may be the same or different. X 2z is multiple X 1z In addition, when nz is 2 or more, a plurality of Y 1z may be the same as or different from each other. From the viewpoint of liquid crystallinity, nz is preferably 2 or more. U 1z represents a hydrogen atom or a (meth)acryloyloxy group. U 2z represents a polymerizable group. W 1z and W 2z are each independently a single bond or a divalent linking group. V 1z and V 2z each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH 2 - may be replaced by -O-, -CO-, -S- or NH-.

[0073] In the polymerizable liquid crystal compound (Z), X 1z and X 2z are each independently preferably an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group; X 1z and X 2z At least one of the groups is a 1,4-phenylene group which may have a substituent, or a cyclohexane-1,4-diyl group which may have a substituent, and is preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent, or the cyclohexane-1,4-diyl group which may have a substituent, include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted.

[0074] The polymerizable liquid crystal compound (Z) is represented by the formula (Z1): -(X 1z -Y 1z -) nz -X 2z - (Z1) [In the formula, X 1z , Y 1z , X 2z and nz have the same meanings as above. [hereinafter referred to as partial structure (Z1)] is preferably an asymmetric structure, since this facilitates the development of smectic liquid crystal properties. The polymerizable liquid crystal compound (Z) in which the partial structure (Z1) is an asymmetric structure is, for example, a compound in which nz is 1 and one X 1z and X 2z In addition, the polymerizable liquid crystal compound (Z) may be a compound in which nz is 2 and two Y 1z A compound in which two Xs are the same structure. 1z are identical in structure to each other, and one X 2z These two X 1z A polymerizable liquid crystal compound (Z) with a structure different from that of the two X1z Of the W 1z X binds to 1z But the other X 1z and X 2z The structure is different from that of the other X 1z and X 2z Also included are polymerizable liquid crystal compounds (Z) having the same structure as each other. 1z are the same structure as each other, and three X 1z and 1 X 2z The polymerizable liquid crystal compound (Z) has a structure in which any one of the above is different from all of the other three.

[0075] Y 1z -CH 2 CH 2 -, -CH 2 O-, -CH 2 CH 2 O-, -COO-, -OCOO-, single bond, -N=N-, -CR az =CR bz -, -C≡C-, -CR az =N- or CO-NR az - is preferred. az and R bz each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1z is -CH 2 CH 2 More preferably, Y is -, -COO-, or a single bond. 1z If present, X 2z Y that binds to 1z is -CH 2 CH 2 - or CH 2 O- is more preferred. 1z and X 2z When all of Y are the same structure, two or more Y 1z It is preferable that there is a plurality of Y 1z When the compound has a structure of asymmetric structure, the compound tends to exhibit smectic liquid crystallinity.

[0076] U2z is the polymerizable group described above. 1z is a hydrogen atom or a polymerizable group. The polymerizable group is preferably a (meth)acryloyloxy group because it is easy to produce, the heat resistance of the liquid crystal cured film is easily improved, and the adhesion between the liquid crystal cured film and the substrate is easily adjusted. The polymerizable group may be in a polymerized state or an unpolymerized state, but is preferably in an unpolymerized state.

[0077] V 1z and V 2z Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1z and V 2z is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.

[0078] Examples of the substituent that the alkanediyl group may have include a cyano group and a halogen atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted linear alkanediyl group.

[0079] W 1z and W 2z are each independently preferably a single bond, -O-, -S-, -COO- or -OCOO-, more preferably a single bond or O-.

[0080] The polymerizable liquid crystal compound (Z) preferably has an asymmetric molecular structure in its molecular structure, and more specifically, is more preferably a polymerizable liquid crystal compound having the following partial structures (Aa) to (Ai). From the viewpoint of easily exhibiting high-order smectic liquid crystallinity, it is more preferably a polymerizable liquid crystal compound having the partial structure (Aa), (Ab) or (Ac). In the following (Aa) to (Ai), * represents a bond (single bond).

[0081] [ka]

[0082] Specific examples of the polymerizable liquid crystal compound (Z) include compounds represented by formulae (A-1) to (A-25). When the polymerizable liquid crystal compound (Z) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.

[0083] [ka]

[0084] [ka]

[0085] [ka]

[0086] [ka]

[0087] [ka]

[0088] Among these, at least one selected from the group consisting of compounds represented by formula (A-2), formula (A-3), formula (A-4), formula (A-5), formula (A-6), formula (A-7), formula (A-8), formula (A-13), formula (A-14), formula (A-15), formula (A-16) and formula (A-17) is preferred. As the polymerizable liquid crystal compound (Z), one type may be used alone, or two or more types may be used in combination.

[0089] The polymerizable liquid crystal compound (Z) can be produced by a known method, for example, as described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996), or Japanese Patent No. 4,719,156.

[0090] The polymerizable liquid crystal compound forming the liquid crystal cured film is preferably a polymerizable liquid crystal compound having a maximum absorption wavelength between 300 and 400 nm. When the polymerizable liquid crystal composition contains a photopolymerization initiator, the polymerization reaction and gelation of the polymerizable liquid crystal compound may proceed during long-term storage. However, if the maximum absorption wavelength of the polymerizable liquid crystal compound is 300 to 400 nm, even if the polymerizable liquid crystal composition is exposed to ultraviolet light during storage, the generation of reactive species from the photopolymerization initiator and the polymerization reaction and gelation of the polymerizable liquid crystal compound caused by the reactive species can be effectively suppressed. Therefore, it is advantageous in terms of long-term stability of the polymerizable liquid crystal composition, and the alignment property and the uniformity of the film thickness of the obtained liquid crystal cured film can be improved. The maximum absorption wavelength of the polymerizable liquid crystal compound can be measured using a UV-visible spectrophotometer in a solvent. The solvent is a solvent that can dissolve the polymerizable liquid crystal compound, and examples of the solvent include tetrahydrofuran and chloroform.

[0091] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition forming the liquid crystal cured film is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and even more preferably 90 to 95 parts by mass, based on 100 parts by mass of the solid content of the polymerizable liquid crystal composition. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous in terms of the alignment of the obtained liquid crystal cured film. In this specification, the solid content of the polymerizable liquid crystal composition means all components excluding volatile components such as organic solvents from the polymerizable liquid crystal composition.

[0092] <Polymerizable liquid crystal composition> The polymerizable liquid crystal composition used to form the liquid crystal cured film contains a polymerizable liquid crystal compound, a silicon-based or fluorine-based leveling agent, and an acrylic leveling agent. It may further contain additives such as a solvent, a photopolymerization initiator, a leveling agent, an antioxidant, a photosensitizer, and a dichroic dye. Each of these components may be used alone or in combination of two or more.

[0093] The polymerizable liquid crystal composition can be obtained by stirring the above components at a predetermined temperature.

[0094] The polymerizable liquid crystal composition for forming a liquid crystal cured film is preferably applied to a substrate or the like in a state of being dissolved in a solvent, and therefore preferably contains a solvent. The solvent is preferably a solvent capable of dissolving the polymerizable liquid crystal compound, and is preferably a solvent inactive to the polymerization reaction of the polymerizable liquid crystal compound. Examples of the solvent include alcohol solvents such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as ethylcyclohexane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone (NMP), and 1,3-dimethyl-2-imidazolidinone. These solvents can be used alone or in combination of two or more. Among these, alcohol solvents, ester solvents, ketone solvents, chlorine-containing solvents, amide solvents and aromatic hydrocarbon solvents are preferred.

[0095] The content of the solvent in the polymerizable liquid crystal composition is preferably 50 to 98 parts by weight, more preferably 70 to 95 parts by weight, relative to 100 parts by weight of the polymerizable liquid crystal composition. Therefore, the solid content per 100 parts by weight of the polymerizable liquid crystal composition is preferably 2 to 50 parts by weight. If the solid content is 50 parts by weight or less, the viscosity of the polymerizable liquid crystal composition is low, so that the thickness of the film becomes approximately uniform and unevenness tends to be less likely to occur. The solid content can be appropriately determined in consideration of the thickness of the liquid crystal cured film to be produced.

[0096] The polymerization initiator is a compound that generates reactive species by the contribution of heat or light and can initiate a polymerization reaction of a polymerizable liquid crystal compound, etc. Examples of the reactive species include active species such as radicals, cations, and anions. Among them, a photopolymerization initiator that generates radicals by light irradiation is preferred from the viewpoint of easy reaction control.

[0097] Examples of photopolymerization initiators include benzoin compounds, benzophenone compounds, benzyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, oxime compounds, triazine compounds, iodonium salts, and sulfonium salts.Specific examples include Irgacure (registered trademark) 907, Irgacure 184, Irgacure 651, Irgacure 819, Irgacure 250, Irgacure 369, Irgacure 379, Irgacure 127, Irgacure 2959, Irgacure 754, Irgacure 379EG (all manufactured by BASF Japan Ltd.), Seikuol BZ, Seikuol Z, Seikuol BEE (all manufactured by Seiko Chemical Co., Ltd.), Kayacure (registered trademark) Examples of suitable antibacterial agents include ADEKA CURE BP100 (manufactured by Nippon Kayaku Co., Ltd.), Kayacure UVI-6992 (manufactured by Dow), ADEKA OPTOMER SP-152, ADEKA OPTOMER SP-170, ADEKA OPTOMER N-1717, ADEKA OPTOMER N-1919, ADEKA ARCLES NCI-831, ADEKA ARCLES NCI-930 (all manufactured by ADEKA Corporation), TAZ-A, TAZ-PP (all manufactured by Nippon SiberHegner AG) and TAZ-104 (manufactured by Sanwa Chemical Co., Ltd.).

[0098] The photopolymerization initiator can fully utilize the energy emitted from the light source and has excellent productivity, so that the maximum absorption wavelength is preferably 300 nm to 400 nm, and more preferably 300 nm to 380 nm, and among them, an α-acetophenone-based polymerization initiator or an oxime-based photopolymerization initiator is preferable.

[0099] Examples of the α-acetophenone polymerization initiator include 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one, and 2-dimethylamino-1-(4-morpholinophenyl)-2-(4-methylphenylmethyl)butan-1-one, and more preferably 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one and 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one. Examples of commercially available α-acetophenone compounds include Irgacure 369, 379EG, and 907 (all manufactured by BASF Japan Co., Ltd.) and Seikuol BEE (manufactured by Seiko Chemical Co., Ltd.).

[0100] The oxime-based photopolymerization initiator generates radicals such as phenyl radicals and methyl radicals when irradiated with light. The polymerization of the polymerizable liquid crystal compound proceeds favorably by these radicals, and among them, the oxime-based photopolymerization initiator that generates methyl radicals is preferable because of its high initiation efficiency of the polymerization reaction. In addition, from the viewpoint of proceeding the polymerization reaction more efficiently, it is preferable to use a photopolymerization initiator that can efficiently utilize ultraviolet light with a wavelength of 350 nm or more. As the photopolymerization initiator that can efficiently utilize ultraviolet light with a wavelength of 350 nm or more, a triazine compound or a carbazole compound containing an oxime structure is preferable, and from the viewpoint of sensitivity, a carbazole compound containing an oxime ester structure is more preferable. Examples of the oxime-based photopolymerization initiator include 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime), and the like. Commercially available oxime ester photopolymerization initiators include Irgacure OXE-01, Irgacure OXE-02, Irgacure OXE-03 (all manufactured by BASF Japan Ltd.), ADEKA Optomer N-1919, ADEKA Arcles NCI-831 (all manufactured by ADEKA Corporation), and the like.

[0101] The content of the photopolymerization initiator is usually 0.1 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 1 to 15 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. Within the above range, the reaction of the polymerizable group proceeds sufficiently, and the alignment of the polymerizable liquid crystal compound is unlikely to be disturbed.

[0102] By blending an antioxidant, the polymerization reaction of the polymerizable liquid crystal compound can be controlled. The antioxidant may be a primary antioxidant selected from phenol-based antioxidants, amine-based antioxidants, quinone-based antioxidants, and nitroso-based antioxidants, or a secondary antioxidant selected from phosphorus-based antioxidants and sulfur-based antioxidants. In order to polymerize the polymerizable liquid crystal compound without disturbing the alignment of the polymerizable liquid crystal compound, the content of the antioxidant is usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. The antioxidant may be used alone or in combination of two or more kinds.

[0103] In addition, the photopolymerization initiator can be made highly sensitive by using a photosensitizer. Examples of the photosensitizer include xanthones such as xanthone and thioxanthone; anthracenes having a substituent such as anthracene and alkyl ether; phenothiazine; and rubrene. The photosensitizer can be used alone or in combination of two or more kinds. The content of the photosensitizer is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound.

[0104] <Dichroic dye> The polymerizable liquid crystal composition of the present invention may contain a dichroic dye. Here, the dichroic dye means a dye having different absorbance in the long axis direction and absorbance in the short axis direction of the molecule. The dichroic dye that can be used in the present invention is not particularly limited as long as it has the above-mentioned properties, and may be a dye or a pigment. In addition, two or more kinds of dyes or pigments may be used in combination, or a dye and a pigment may be used in combination. When such a dichroic dye is contained in a horizontally aligned liquid crystal cured film or a vertically aligned liquid crystal cured film, the dichroic dye may be aligned together with the polymerizable liquid crystal compound and exhibit absorption anisotropy. In particular, when the degree of orientation order is high, as represented by a smectic liquid crystal phase, the absorption anisotropy derived from the contained dichroic dye also tends to be significantly improved.

[0105] Dichroic dyes have a maximum absorption wavelength (λ MAX ) is preferable. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes.

[0106] Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes. Bisazo dyes and trisazo dyes are preferred, and examples thereof include a compound represented by formula (I) (hereinafter also referred to as "compound (I)"). K 1 (-N=NK 2 ) p -N=NK 3 (I) [In formula (I), K 1 and K. 3 each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2 represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of K2 may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.

[0107] Examples of monovalent heterocyclic groups include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of divalent heterocyclic groups include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.

[0108] K 1 and K. 3 Phenyl, naphthyl and monovalent heterocyclic groups in 2 In the above, examples of the substituents that the p-phenylene group, the naphthalene-1,4-diyl group, and the divalent heterocyclic group may optionally have include an alkyl group having 1 to 4 carbon atoms; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, or a pyrrolidino group (a substituted amino group means an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH 2 ) etc.

[0109] Among the compounds (I), compounds represented by any one of the following formulas (I-1) to (I-6) are preferred. [ka] [In the formulas (I-1) to (I-8), B 1 ~B 30each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the substituted amino group and the unsubstituted amino group are defined above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.]

[0110] The anthraquinone dye is preferably a compound represented by formula (I-9). [ka] [In formula (I-9), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH 2 , -NHR x , -NR x 2 , -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0111] The oxazone dye is preferably a compound represented by formula (I-10). [ka] [In formula (I-8), R 9 ~R 15 are each independently a hydrogen atom, -R x, -NH 2 , -NHR x , -NR x 2 , -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0112] The acridine dye is preferably a compound represented by formula (I-11). [ka] [In formula (I-11), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH 2 , -NHR x , -NR x 2 , -SR x Or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms. In formula (I-9), formula (I-10) and formula (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.

[0113] As the cyanine dye, the compounds represented by formula (I-12) and formula (I-13) are preferred. [ka] [In formula (I-12), D 1 and D. 2 represent, independently of each other, a group represented by any one of formulas (I-12a) to (I-12d). [ka] n5 represents an integer from 1 to 3. [ka] [In formula (I-13), D 3 and D. 4 each independently represents a group represented by any one of formulas (I-13a) to (1-13h). [ka] n6 represents an integer from 1 to 3.

[0114] Among these dichroic dyes, from the viewpoint of alignment, it is preferable that the vertically aligned liquid crystal cured film contains at least one azo dye as the dichroic dye. In the present invention, the weight average molecular weight of the dichroic dye is usually 300-2,000, and preferably 400-1,000.

[0115] The content of the dichroic dye in the polymerizable liquid crystal composition forming the liquid crystal cured film can be appropriately determined depending on the type of the dichroic dye used, and is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the dichroic dye is within the above range, the orientation of the polymerizable liquid crystal compound is unlikely to be disturbed, and a liquid crystal cured film having a high degree of orientation order can be obtained.

[0116] <Cured film of vertically aligned liquid crystal> The vertically aligned liquid crystal cured film is a liquid crystal cured film obtained by applying the polymerizable liquid crystal composition onto a substrate or an alignment film, and curing the polymerizable liquid crystal compound in a state where the polymerizable liquid crystal compound is aligned in a direction perpendicular to the substrate or the alignment film.

[0117] In the present invention, it is preferable that the uniformity of the horizontally aligned liquid crystal cured film satisfies the following formula (S4). RthC(450) / RthC(550)≦1.0 (S4) (In formula (S4), RthC(450) represents a retardation value in the thickness direction of the cured liquid crystal film at a wavelength of 450 nm, and RthC(550) represents a retardation value in the thickness direction of the cured liquid crystal film at a wavelength of 550 nm.)

[0118] When the horizontally aligned liquid crystal cured film satisfies the formula (S4), the vertically aligned liquid crystal cured film exhibits a so-called reverse wavelength dispersion, in which the retardation value in the thickness direction at a short wavelength is smaller than the retardation value in the thickness direction at a long wavelength. RthC(450) / RthC(550) is preferably 0.70 or more, more preferably 0.78 or more, and is preferably 0.95 or less, more preferably 0.92 or less.

[0119] The retardation value in the thickness direction can be adjusted by the thickness dC of the vertically aligned liquid crystal cured film. RthC(λ)=((nxC(λ)+nyC(λ)) / 2-nzC(λ))×dC Therefore, in order to obtain a desired retardation value in the thickness direction (RthC(λ): retardation value in the thickness direction of the vertically aligned liquid crystal cured film at a wavelength λ (nm)), the three-dimensional refractive index and the film thickness dC may be adjusted.

[0120] In addition, it is preferable that the vertically aligned liquid crystal cured film satisfies the following formula (S3). -150≦RthC(550)≦-30 (S3) [In formula (S3), RthC(550) represents a retardation value in the thickness direction of the liquid crystal cured film at a wavelength of 550 nm.] A more preferable range of the thickness direction retardation RthC(550) of the vertically aligned liquid crystal cured film is −110 nm≦RthC(550)≦−45 nm.

[0121] The vertically aligned liquid crystal cured film is, for example, A step of forming a coating film of a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film; drying the coating to form a dry coating; and A process of irradiating the dried coating with active energy rays to form a vertically aligned liquid crystal cured film. The composition can be produced by a method comprising the steps of:

[0122] The formation of a coating film of the polymerizable liquid crystal composition can be carried out, for example, by applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto a substrate, an alignment film, or a horizontally aligned liquid crystal cured film described later. Examples of the substrate include glass substrates and film substrates, but resin film substrates are preferred from the viewpoint of processability. Examples of the resin constituting the film substrate include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; plastics such as polyphenylene sulfide and polyphenylene oxide. Such resins can be formed into a film by known means such as solvent casting and melt extrusion to form a substrate. The substrate surface may have a protective layer formed from an acrylic resin, a methacrylic resin, an epoxy resin, an oxetane resin, a urethane resin, a melamine resin, or the like, and may be subjected to a surface treatment such as a release treatment such as silicone treatment, a corona treatment, or a plasma treatment.

[0123] Commercially available products may be used as the substrate. Examples of commercially available cellulose ester substrates include cellulose ester substrates manufactured by Fuji Photo Film Co., Ltd., such as Fujitac Film; cellulose ester substrates manufactured by Konica Minolta Opto Co., Ltd., such as "KC8UX2M", "KC8UY", and "KC4UY". Examples of commercially available cyclic olefin resins include cyclic olefin resins manufactured by Ticona (Germany), such as "Topas (registered trademark)", cyclic olefin resins manufactured by JSR Corporation, such as "Arton (registered trademark)", cyclic olefin resins manufactured by Zeon Corporation, such as "ZEONOR (registered trademark)" and "ZEONEX (registered trademark)", and cyclic olefin resins manufactured by Mitsui Chemicals, Inc., such as "Apel" (registered trademark). Commercially available cyclic olefin resin substrates may also be used. Commercially available cyclic olefin resin substrates include cyclic olefin resin substrates manufactured by Sekisui Chemical Co., Ltd., such as "S-Cina (registered trademark)" and "SCA40 (registered trademark)"; cyclic olefin resin substrates manufactured by Optes Inc., such as "ZEONORFILM (registered trademark)"; and cyclic olefin resin substrates manufactured by JSR Corporation, such as "ARTONFILM (registered trademark)."

[0124] From the viewpoints of thinning the laminate, ease of peeling the substrate, handleability of the substrate, and the like, the thickness of the substrate is usually 5 to 300 μm, and preferably 10 to 150 μm.

[0125] Examples of a method for applying the polymerizable liquid crystal composition to a substrate or the like include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.

[0126] Next, the solvent is removed by drying or the like to form a dried coating film. Examples of drying methods include natural drying, ventilation drying, heat drying, and reduced pressure drying. In this case, the coating film obtained from the polymerizable liquid crystal composition is heated to dry and remove the solvent from the coating film, and the polymerizable liquid crystal compound can be aligned in a direction perpendicular to the coating film plane. The heating temperature of the coating film can be appropriately determined in consideration of the materials of the polymerizable liquid crystal compound used and the substrate on which the coating film is formed, but it is necessary that the temperature is equal to or higher than the liquid crystal phase transition temperature in order to phase-transition the polymerizable liquid crystal compound to a liquid crystal layer state. In order to vertically align the polymerizable liquid crystal compound while removing the solvent contained in the polymerizable liquid crystal composition, the composition can be heated to a temperature equal to or higher than the liquid crystal phase transition temperature (smectic phase transition temperature or nematic phase transition temperature) of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition.

[0127] The liquid crystal phase transition temperature can be measured using, for example, a polarizing microscope equipped with a temperature control stage, a differential scanning calorimeter (DSC), a thermogravimetric differential thermal analyzer (TG-DTA), etc. When two or more polymerizable liquid crystal compounds are used in combination, the phase transition temperature means a temperature measured in the same manner as when one type of polymerizable liquid crystal compound is used, using a mixture of polymerizable liquid crystal compounds in which all polymerizable liquid crystal compounds constituting the polymerizable liquid crystal composition are mixed in the same ratio as the composition in the polymerizable liquid crystal composition. It is generally known that the liquid crystal phase transition temperature of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition may be lower than the liquid crystal phase transition temperature of the polymerizable liquid crystal compound alone.

[0128] The heating time can be appropriately determined depending on the heating temperature, the type of polymerizable liquid crystal compound used, the type and boiling point of the solvent, and the amount thereof, but is usually 15 seconds to 10 minutes, and preferably 0.5 to 5 minutes.

[0129] The removal of the solvent from the coating film may be performed simultaneously with or separately from the heating of the polymerizable liquid crystal compound to a temperature equal to or higher than the liquid crystal phase transition temperature, but is preferably performed simultaneously from the viewpoint of improving productivity. Before heating the polymerizable liquid crystal compound to a temperature equal to or higher than the liquid crystal phase transition temperature, a preliminary drying step may be provided to adequately remove the solvent in the coating film obtained from the polymerizable liquid crystal composition under conditions in which the polymerizable liquid crystal compound contained in the coating film is not polymerized. Examples of the drying method in the preliminary drying step include natural drying, ventilation drying, heat drying, and reduced pressure drying, and the drying temperature (heating temperature) in the drying step can be appropriately determined depending on the type of polymerizable liquid crystal compound used, the type of solvent, its boiling point, and its amount, etc.

[0130] Next, in the obtained dried coating film, the polymerizable liquid crystal compound is polymerized while maintaining the vertical alignment state of the polymerizable liquid crystal compound, thereby forming a vertically aligned liquid crystal cured film. Examples of polymerization methods include thermal polymerization and photopolymerization, but photopolymerization is preferred from the viewpoint of easy control of the polymerization reaction. In photopolymerization, the light irradiated to the dried coating film is appropriately selected according to the type of photopolymerization initiator contained in the dried coating film, the type of polymerizable liquid crystal compound (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof. Specific examples thereof include one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, and active electron beams. Among them, ultraviolet light is preferred in terms of easy control of the progress of the polymerization reaction and the ability to use photopolymerization devices that are widely used in this field, and it is preferable to select the types of polymerizable liquid crystal compound and photopolymerization initiator contained in the polymerizable liquid crystal composition so that they can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can also be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means during polymerization. By adopting such a cooling means, polymerization of the polymerizable liquid crystal compound can be performed at a lower temperature, and even if a substrate having a relatively low heat resistance is used, a vertically aligned liquid crystal cured film can be appropriately formed. In addition, it is also possible to promote the polymerization reaction by increasing the polymerization temperature within a range in which defects due to heat during light irradiation (such as deformation of the substrate due to heat) do not occur. During photopolymerization, a patterned cured film can also be obtained by performing masking and development.

[0131] Examples of the light source of the active energy rays include a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave excited mercury lamp, and a metal halide lamp.

[0132] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.

[0133] The thickness of the vertically aligned liquid crystal cured film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.2 to 3 μm, more preferably 0.2 to 2 μm. When the vertically aligned liquid crystal cured film has a positive wavelength dispersion, the thickness is more preferably 0.2 to 1 μm, and when the vertically aligned liquid crystal cured film has a reverse wavelength dispersion, the thickness is more preferably 0.4 to 2 μm. When the vertically aligned liquid crystal cured film has a reverse wavelength dispersion, the optical absorption in an oblique direction increases for the same dye concentration compared to when the vertically aligned liquid crystal cured film has a positive wavelength dispersion, and this is more preferable.

[0134] <Cured film of vertically aligned liquid crystal containing dichroic dye> As one aspect of the vertically aligned liquid crystal cured film in the present invention, the vertically aligned liquid crystal cured film may contain a dichroic dye. In particular, in the case of a vertically aligned liquid crystal cured film containing a dichroic dye, the higher the degree of alignment order of the liquid crystal, the more the absorption selectivity derived from the dichroic dye is improved, so it is preferable to use a polymerizable liquid crystal compound that shows the above-mentioned smectic phase, particularly a high-order smectic phase, and it is preferable to polymerize while maintaining the liquid crystal state of the smectic phase, preferably the high-order smectic phase, to form a vertically aligned liquid crystal cured film containing a dichroic dye.

[0135] The vertically aligned liquid crystal cured film containing the dichroic dye satisfies the following formulae (11) and (12). 0.001≦AxC≦0.3 (11) AxC(z=60) / AxC>2 (12)

[0136] In formulas (11) and (12), AxC and AxC (z=60) each represent the absorbance of the vertically aligned liquid crystal cured film at the maximum absorption wavelength of 400 to 750 nm. AxC represents the absorbance of linearly polarized light oscillating in the x-axis direction, and AxC (z=60) represents the absorbance of linearly polarized light oscillating in the x-axis direction when the vertically aligned liquid crystal cured film is rotated 60° around the y-axis as the rotation axis. The x-axis means any direction in the plane of the vertically aligned liquid crystal cured film, the y-axis means a direction perpendicular to the x-axis in the film plane, and the z-axis means the thickness direction of the vertically aligned liquid crystal cured film. In addition, all absorbances in this specification indicate absorbances measured in a state where the influence of interface reflection during measurement is removed. As a method for removing the influence of interface reflection, for example, a method is mentioned in which the absorbance at a long wavelength such as 800 nm where the absorption of the compound can be ignored is set to 0 using a spectrophotometer, and the absorbance at a wavelength in the range where the absorption of the compound exists in that state is measured.

[0137] The above AxC can be measured by applying linearly polarized light vibrating in the x-axis direction toward the film surface of the liquid crystal cured film from the z-axis direction. The above formula (11) means that the absorbance in the front direction in the vertically aligned liquid crystal cured film is 0.001 or more and 0.3 or less, and it can be said that the smaller the value of AxC, the more precisely the dichroic dye is aligned in the vertical direction relative to the plane of the obtained liquid crystal cured film. When the value of AxC exceeds 0.3, the coloring in the front direction of the vertically aligned liquid crystal cured film becomes strong, and the front hue tends to be inferior when combined with a horizontally aligned retardation film and applied to a display device, so the value of AxC is preferably 0.1 or less, more preferably 0.05 or less. The lower limit of the value of AxC is usually 0.001 or more, preferably 0.003 or more, and more preferably 0.005 or more.

[0138] The above AxC(z=60) can be measured by rotating the vertically aligned liquid crystal cured film by 60° around the y-axis as the rotation axis, and then applying the same linearly polarized light as that used to measure Ax. Here, the film is rotated by rotating the film in the state where Ax is measured by 60° around the y-axis as the rotation axis in the direction of incidence of the linearly polarized light. If the value of AxC(z=60) / AxC is 2 or less, it is difficult to obtain good light absorption anisotropy, so the value of AxC(z=60) / AxC is preferably 2.5 or more, more preferably 3 or more. On the other hand, if the value of AxC(z=60) / AxC is too large, the hue changes significantly only in the oblique hue, and the difference between the front hue and the oblique hue may become large, so the value of AxC(z=60) / AxC is preferably 50 or less, more preferably 30 or less, and even more preferably 20 or less. In addition, AxC(z=60) is preferably 0.01 or more, more preferably 0.03 or more, and even more preferably 0.05 or more, and is preferably 1.0 or less, more preferably 0.5 or less, and even more preferably 0.3 or less.

[0139] The absorbance of linearly polarized light vibrating in the y-axis direction is represented as AyC, and in the vertically aligned liquid crystal cured film described in the present invention, AxC and AyC are usually almost equal. When AxC and AyC are different, the film has in-plane dichroism, and in this case, the coloring of the vertically aligned liquid crystal cured film in the front hue tends to become large.

[0140] When the vertical liquid crystal cured film satisfies the above formulas (11) and (12), it can be said that the vertical liquid crystal alignment film has excellent polarization performance (absorption anisotropy), and thus can effectively transmit light from the front direction and effectively absorb light from an oblique direction.

[0141] AxC and AxC(Z=60) in the vertically aligned liquid crystal cured film containing the dichroic dye can be controlled, for example, by adjusting the film thickness, the conditions of the manufacturing process, the type and amount of the polymerizable liquid crystal compound and the dichroic dye constituting the vertically aligned liquid crystal cured film, etc. In addition, the value of AxC(z=60) / AxC is generally about 2 to 10 when the polymerizable liquid crystal compound is a nematic liquid crystal, and about 5 to 30 when the polymerizable liquid crystal compound is a smectic liquid crystal, and can be appropriately selected according to the desired optical properties.

[0142] <Alignment film> In one embodiment of the present invention, a coating film of the polymerizable liquid crystal composition is formed on an alignment film. The alignment film has an alignment regulating force that aligns the polymerizable liquid crystal compound in a desired direction. Among these, an alignment film having an alignment regulating force that aligns the polymerizable liquid crystal compound in the horizontal direction is sometimes called a horizontal alignment film, and an alignment film having an alignment regulating force that aligns the polymerizable liquid crystal compound in the vertical direction is sometimes called a vertical alignment film. The alignment regulating force can be arbitrarily adjusted by the type of alignment film, the surface state, the rubbing conditions, etc., and when the alignment film is formed from a photoalignable polymer, it can be arbitrarily adjusted by the polarized light irradiation conditions, etc.

[0143] The alignment film is preferably one that has solvent resistance such that the polymerizable liquid crystal composition does not dissolve when applied, and also has heat resistance in the heat treatment for removing the solvent and for orienting the polymerizable liquid crystal compound described later. Examples of the alignment film include an alignment film containing an alignment polymer, a photo-alignment film, a groove alignment film having a concave-convex pattern or a plurality of grooves on the surface, and a stretched film stretched in the alignment direction, and the like, and a photo-alignment film is preferred from the viewpoint of the accuracy of the alignment angle and the quality.

[0144] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among them, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.

[0145] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an "alignment polymer composition") to a substrate and removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing (rubbing method). Examples of the solvent include the same solvents as those exemplified above as solvents that can be used in the polymerizable liquid crystal composition.

[0146] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably about 0.1 to 10%.

[0147] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).

[0148] The method for applying the alignable polymer composition to the substrate may be the same as the method exemplified for applying the polymerizable liquid crystal composition to the substrate.

[0149] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0150] In order to impart an orientation control force to the orientation film, a rubbing treatment can be performed as necessary (rubbing method). A method for imparting an orientation control force by the rubbing method includes a method in which an orientation polymer composition is applied to a substrate and annealed to bring an orientation polymer film formed on the substrate surface into contact with a rotating rubbing roll wrapped with a rubbing cloth. If masking is performed during the rubbing treatment, multiple regions (patterns) with different orientation directions can also be formed on the orientation film.

[0151] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film forming composition") to a substrate, removing the solvent, and then irradiating the substrate with polarized light (preferably polarized UV). Photo-alignment films are also advantageous in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.

[0152] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that induce molecular alignment or are the origin of liquid crystal alignment ability, such as isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, caused by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.

[0153] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.

[0154] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.

[0155] A photo-alignment layer can be formed on a substrate by applying the composition for forming a photo-alignment film on the substrate. The solvent contained in the composition can be the same as the solvents exemplified above as the solvents usable for the polymerizable liquid crystal composition, and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.

[0156] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the desired photo-alignment film, but is preferably at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, based on the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.

[0157] The method of applying the composition for forming a photo-alignment film to a substrate may be the same as the method of applying the oriented polymer composition to a substrate. Examples of the method of removing the solvent from the applied composition for forming a photo-alignment film include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0158] The polarized light may be irradiated by directly irradiating the polarized UV light onto the composition for forming a photo-aligned film coated on the substrate after removing the solvent, or by irradiating the polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The light from the light source can be irradiated by passing through an appropriate polarizer to irradiate the polarized UV light. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.

[0159] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.

[0160] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film with multiple equally spaced linear grooves, the liquid crystal molecules are aligned in the direction along the grooves.

[0161] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form an uneven pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to a substrate and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on a substrate to form unevenness, followed by curing.

[0162] As a material that exhibits an alignment control force that aligns the polymerizable liquid crystal compound in a direction perpendicular to the coating film plane, in addition to the above-mentioned alignment polymers, fluorine-based polymers such as perfluoroalkyl, silane compounds, and polysiloxane compounds obtained by condensation reactions thereof may be used.

[0163] When a silane compound is used as a material for forming the alignment film, a compound containing Si and C elements as constituent elements is preferable from the viewpoint of easily reducing surface tension and easily increasing adhesion with a layer adjacent to the alignment film, and a silane compound can be suitably used. As the silane compound, a nonionic silane compound described later or a silane-containing ionic compound as exemplified in the section on ionic compounds can be used, and the vertical alignment regulating force can be increased by using these silane compounds. These silane compounds may be used alone or in combination of two or more kinds, or may be used in combination with other materials. When the silane compound is a nonionic silane compound, a silane compound having an alkyl group at the molecular end is preferable from the viewpoint of easily increasing the vertical alignment regulating force, and a silane compound having an alkyl group having 3 to 30 carbon atoms is more preferable.

[0164] The thickness of the alignment film (alignment film containing an alignment polymer or photoalignment film) is usually in the range of 10 to 10,000 nm, preferably in the range of 10 to 1000 nm, more preferably 10 to 500 nm or less, even more preferably 10 to 300 nm, and particularly preferably 50 to 250 nm.

[0165] <Orientation promoter> In another embodiment of the vertically aligned liquid crystal cured film of the present invention, the coating film of the polymerizable liquid crystal composition does not require an alignment film and can be formed directly on a substrate. In this embodiment, the polymerizable liquid crystal composition for forming the vertically aligned liquid crystal cured film usually contains an alignment promoter. In the present invention, the alignment promoter means a material that promotes the liquid crystal alignment of the polymerizable liquid crystal compound in a desired direction. Examples of the alignment promoter that promotes the alignment of the polymerizable liquid crystal compound in the vertical direction include an ionic compound consisting of nonmetallic atoms and a nonionic silane compound. It is preferable that the polymerizable liquid crystal composition that forms the vertically aligned liquid crystal cured film contains at least one of an ionic compound consisting of nonmetallic atoms and a nonionic silane compound, and it is more preferable that it contains both an ionic compound consisting of nonmetallic atoms and a nonionic silane compound.

[0166] When the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film contains an ionic compound consisting of a nonmetallic atom, in a dried coating film formed on a substrate from the composition for forming a vertically aligned liquid crystal cured film, a vertical alignment regulating force for the polymerizable liquid crystal compound is exerted by electrostatic interaction, and the polymerizable liquid crystal compound tends to be aligned in a vertical direction to the substrate surface in the dried coating film. This allows the polymerizable liquid crystal compound to maintain a vertically aligned state and form a liquid crystal cured film.

[0167] Examples of ionic compounds consisting of nonmetallic atoms include onium salts (more specifically, quaternary ammonium salts in which the nitrogen atom has a positive charge, tertiary sulfonium salts, and quaternary phosphonium salts in which the phosphorus atom has a positive charge). Among these onium salts, quaternary onium salts are preferred from the viewpoint of further improving the vertical alignment property of the polymerizable liquid crystal compound, and quaternary phosphonium salts or quaternary ammonium salts are more preferred from the viewpoint of improving availability and mass productivity. The onium salt may have two or more quaternary onium salt sites in the molecule, and may be an oligomer or polymer.

[0168] The molecular weight of the ionic compound is preferably 100 or more and 10,000 or less. When the molecular weight is within the above range, it is easy to improve the vertical alignment property of the polymerizable liquid crystal compound while ensuring the coatability of the polymerizable composition. The molecular weight of the ionic compound is more preferably 5000 or less, and further preferably 3000 or less.

[0169] The cationic component of the ionic compound may be, for example, an inorganic cation or an organic cation. Among them, the organic cation is preferred because it is less likely to cause alignment defects of the polymerizable liquid crystal compound. The organic cation may be, for example, an imidazolium cation, a pyridinium cation, an ammonium cation, a sulfonium cation, and a phosphonium cation.

[0170] Ionic compounds generally have a counter anion. Examples of the anion component that is the counter ion of the cationic component include inorganic anions and organic anions. Among them, organic anions are preferred because they are less likely to cause alignment defects of the polymerizable liquid crystal compound. It is not necessary that the cation and the anion correspond one-to-one.

[0171] Specific examples of the anion component include the following: Chloride anion [Cl - 〕, Bromide anion [Br - 〕, Iodide anion [I - 〕, Tetrachloroaluminate anion [AlCl 4 - 〕, Heptachlorodialuminate anion [Al 2 Cl 7 - 〕, Tetrafluoroborate anion [BF 4 - 〕, Hexafluorophosphate anion (PF 6 - 〕, Perchlorate anion [ClO 4 - 〕, Nitrate anion (NO 3 - 〕, Acetate anion [CH 3 COO - 〕, Trifluoroacetate anion [CF 3 COO - 〕, Fluorosulfonate anion (FSO 3 - 〕, Methanesulfonate anion [CH 3 SO 3 - 〕, Trifluoromethanesulfonate anion [CF 3 SO 3 - 〕, p-Toluenesulfonate anion [p-CH 3 C 6 H 4 SO 3 - 〕, Bis(fluorosulfonyl)imide anion [(FSO 2 ) 2 N - 〕, Bis(trifluoromethanesulfonyl)imide anion [(CF 3 SO 2 ) 2 N - 〕, Tris(trifluoromethanesulfonyl)methanide anion [(CF 3 SO 2 ) 3 C - 〕, Hexafluoroarsenate anion [AsF 6 - 〕, Hexafluoroantimonate anion [SbF 6 - 〕, Hexafluoroniobate anion [NbF 6 - 〕, Hexafluorotantalate anion [TaF 6 - 〕, Dimethylphosphinate anion [(CH 3 ) 2 POO - 〕, (Poly)hydrofluorofluoride anion [F(HF) n - (for example, n is an integer from 1 to 3), Dicyanamide anion (CN) 2 N - 〕, Thiocyanine anion (SCN - 〕, Perfluorobutanesulfonate anion [C4 F 9 SO 3 - 〕, Bis(pentafluoroethanesulfonyl)imide anion [(C 2 F 5 SO 2 ) 2 N - 〕, Perfluorobutanoate anion [C 3 F 7 COO - ], and (Trifluoromethanesulfonyl)(trifluoromethanecarbonyl)imide anion 〔(CF 3 SO 2 )(CF 3 CO)N - 〕.

[0172] Specific examples of the ionic compound can be appropriately selected from the above-mentioned combinations of cationic and anionic components. Specific examples of the compound that is a combination of a cationic component and an anionic component include the following.

[0173] (Pyridinium salts) N-Hexylpyridinium hexafluorophosphate, N-octylpyridinium hexafluorophosphate, N-methyl-4-hexylpyridinium hexafluorophosphate, N-butyl-4-methylpyridinium hexafluorophosphate, N-octyl-4-methylpyridinium hexafluorophosphate, N-Hexylpyridinium bis(fluorosulfonyl)imide, N-Octylpyridinium bis(fluorosulfonyl)imide, N-methyl-4-hexylpyridinium bis(fluorosulfonyl)imide, N-butyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-octyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-Octylpyridinium bis(trifluoromethanesulfonyl)imide, N-methyl-4-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-butyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-octyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-Hexylpyridinium p-toluenesulfonate, N-Octylpyridinium p-toluenesulfonate, N-methyl-4-hexylpyridinium p-toluenesulfonate, N-Butyl-4-methylpyridinium p-toluenesulfonate, and N-Octyl-4-methylpyridinium p-toluenesulfonate.

[0174] (Imidazolium salt) 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium p-toluenesulfonate, 1-Butyl-3-methylimidazolium methanesulfonate, etc.

[0175] (Pyrrolidinium salts) N-butyl-N-methylpyrrolidinium hexafluorophosphate, N-butyl-N-methylpyrrolidinium bis(fluorosulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-Butyl-N-methylpyrrolidinium p-toluenesulfonate, etc.

[0176] (Ammonium salt) tetrabutylammonium hexafluorophosphate, Tetrabutylammonium bis(fluorosulfonyl)imide, Tetrahexylammonium bis(fluorosulfonyl)imide, trioctylmethylammonium bis(fluorosulfonyl)imide, (2-hydroxyethyl)trimethylammonium bis(fluorosulfonyl)imide, tetrabutylammonium bis(trifluoromethanesulfonyl)imide, tetrahexylammonium bis(trifluoromethanesulfonyl)imide, trioctylmethylammonium bis(trifluoromethanesulfonyl)imide, (2-hydroxyethyl)trimethylammonium bis(trifluoromethanesulfonyl)imide, tetrabutylammonium p-toluenesulfonate, Tetrahexylammonium p-toluenesulfonate, Trioctylmethylammonium p-toluenesulfonate, (2-hydroxyethyl)trimethylammonium p-toluenesulfonate, (2-Hydroxyethyl)trimethylammonium dimethylphosphinate 1-(3-trimethoxysilylpropyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylpropyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylbutyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylbutyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide, N-{(3-triethoxysilylpropyl)carbamoyloxyethyl)}-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide, and N-[2-{3-(3-trimethoxysilylpropylamino)-1-oxopropoxy}ethyl]-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide.

[0177] (phosphonium salts) tributyl(2-methoxyethyl)phosphonium bis(trifluoromethanesulfonyl)imide, tributylmethylphosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[4-(trimethoxysilyl)butyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-tributyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-tributyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, and 1,1,1-Tributyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide. These ionic compounds may be used alone or in combination of two or more.

[0178] From the viewpoint of further improving the vertical alignment of the polymerizable liquid crystal compound, the ionic compound preferably has a Si element and / or an F element in the molecular structure of the cationic moiety. When the ionic compound has a Si element and / or an F element in the molecular structure of the cationic moiety, the ionic compound is easily segregated on the surface of the vertically aligned liquid crystal cured film. Among them, the following ionic compounds (i) to (iii) are preferred as ionic compounds whose constituent elements are all nonmetallic elements.

[0179] (Ionic compound (i)) [ka] (Ionic compound (ii)) [ka] (Ionic compound (iii)) [ka]

[0180] As a method for improving the vertical alignment of polymerizable liquid crystal compounds, for example, a method of treating the substrate surface with a surfactant having an alkyl group with a relatively long chain length is known (see, for example, Chapter 2, Liquid Crystal Orientation and Physical Properties, of the Liquid Crystal Handbook (published by Maruzen Co., Ltd.)). Such a method for improving the vertical alignment of liquid crystal compounds with a surfactant can also be applied to ionic compounds. That is, by treating the substrate surface with an ionic compound having an alkyl group with a relatively long chain length, the vertical alignment of polymerizable liquid crystal compounds can be effectively improved.

[0181] Specifically, it is preferable that the ionic compound satisfies the following formula (8). 5 <M<16 (8) In formula (8), M is expressed by the following formula (9). M = (number of covalent bonds from the positively charged atom to the end of the molecular chain of the substituent with the most covalent bonds to the end of the molecular chain among the substituents directly bonded to the positively charged atom) ÷ (number of positively charged atoms) (9) When the ionic compound satisfies the above condition (8), the vertical alignment property of the polymerizable liquid crystal compound can be effectively improved.

[0182] In addition, when there are two or more positively charged atoms in the molecule of an ionic compound, for a substituent having two or more positively charged atoms, the number of covalent bonds from the positively charged atom considered as the base point to the nearest other positively charged atom is defined as the "number of covalent bonds from the positively charged atom to the molecular chain end" as defined in the above definition of M. In addition, when the ionic compound is an oligomer or polymer having two or more repeating units, the constituent unit is considered as one molecule and the above M is calculated. When a positively charged atom is incorporated in a ring structure, the number of covalent bonds from the ring structure to the positively charged atom or the number of covalent bonds to the end of the substituent bonded to the ring structure, whichever is larger, is defined as the "number of covalent bonds from the positively charged atom to the molecular chain end" as defined in the above definition of M.

[0183] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains an ionic compound, the content thereof is usually preferably 0.01 to 5 mass %, more preferably 0.05 to 4 mass %, and further preferably 0.1 to 3 mass % based on the solid content of the polymerizable liquid crystal composition. When the content of the ionic compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining good coatability of the polymerizable liquid crystal composition.

[0184] When the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film contains a nonionic silane compound, the nonionic silane compound reduces the surface tension of the polymerizable liquid crystal composition, and in a dried coating film formed on a substrate from the composition for forming a vertically aligned liquid crystal cured film, the nonionic silane compound is present on the surface of the dried coating film opposite to the substrate, increasing the vertical alignment control force for the polymerizable liquid crystal compound, and the polymerizable liquid crystal compound tends to be aligned in a vertical direction to the substrate surface in the dried coating film. This allows the polymerizable liquid crystal compound to maintain a vertically aligned state and form a liquid crystal cured film.

[0185] Nonionic silane compound is a compound that is nonionic and contains Si element.For example, nonionic silane compound includes silicon polymer such as polysilane, silicone resin such as silicone oil and silicone resin, silicone oligomer, organic inorganic silane compound such as silsesquioxane and alkoxysilane (more specifically, silane coupling agent, etc.), silane-containing compound described in the leveling agent section, etc.

[0186] The nonionic silane compound may be of the silicone monomer type or of the silicone oligomer (polymer) type. When the silicone oligomer is expressed in the form of a (monomer)-(monomer) copolymer, it may be a copolymer containing a mercaptopropyl group, such as 3-mercaptopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-mercaptopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-mercaptopropyltriethoxysilane-tetramethoxysilane copolymer, and 3-mercaptopropyltriethoxysilane-tetraethoxysilane copolymer; a copolymer containing a mercaptomethyl group, such as mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltriethoxysilane-tetramethoxysilane copolymer, mercaptomethyltriethoxysilane-tetramethoxysilane copolymer, and mercaptomethyltriethoxysilane-tetraethoxysilane copolymer; Methacryloyloxypropyl group-containing copolymers such as methacryloyloxypropyl trimethoxysilane-tetramethoxysilane copolymer, 3-methacryloyloxypropyl trimethoxysilane-tetraethoxysilane copolymer, 3-methacryloyloxypropyl triethoxysilane-tetramethoxysilane copolymer, 3-methacryloyloxypropyl triethoxysilane-tetraethoxysilane copolymer, 3-methacryloyloxypropyl methyldimethoxysilane-tetramethoxysilane copolymer, 3-methacryloyloxypropyl methyldimethoxysilane-tetraethoxysilane copolymer, 3-methacryloyloxypropyl methyldiethoxysilane-tetramethoxysilane copolymer and 3-methacryloyloxypropyl methyldiethoxysilane-tetraethoxysilane copolymer;3-Acryloyloxypropyltrimethoxysilane-tetramethoxysilane copolymer, 3-Acryloyloxypropyltrimethoxysilane-tetraethoxysilane copolymer, 3-Acryloyloxypropyltriethoxysilane-tetramethoxysilane copolymer, 3-Acryloyloxypropyltriethoxysilane-tetraethoxysilane copolymer, 3-Acryloyloxypropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-Acryloyloxypropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-Acryloyloxypropylmethyldiethoxysilane-tetramethoxysilane copolymer and 3-Acryloyloxypropylmethyldimethoxysilane-tetramethoxysilane copolymer. copolymers containing acryloyloxypropyl groups, such as ethyldiethoxysilane-tetraethoxysilane copolymer; copolymers containing vinyl groups, such as vinyltrimethoxysilane-tetramethoxysilane copolymer, vinyltrimethoxysilane-tetraethoxysilane copolymer, vinyltriethoxysilane-tetramethoxysilane copolymer, vinyltriethoxysilane-tetraethoxysilane copolymer, vinylmethyldimethoxysilane-tetramethoxysilane copolymer, vinylmethyldimethoxysilane-tetraethoxysilane copolymer, vinylmethyldiethoxysilane-tetramethoxysilane copolymer, and vinylmethyldiethoxysilane-tetraethoxysilane copolymer;Examples of the copolymer include amino group-containing copolymers such as 3-aminopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer, and 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymer. These nonionic silane compounds may be used alone or in combination of two or more. Among them, silane coupling agents are preferred from the viewpoint of further improving adhesion to adjacent layers.;

[0187] The silane coupling agent is a compound containing an Si element having at least one functional group selected from the group consisting of vinyl group, epoxy group, styryl group, methacryl group, acrylic group, amino group, isocyanurate group, ureido group, mercapto group, isocyanate group, carboxy group, and hydroxy group at the end, and at least one alkoxysilyl group or silanol group. By appropriately selecting these functional groups, it is possible to impart unique effects such as improving the mechanical strength of the vertically aligned liquid crystal cured film, modifying the surface of the vertically aligned liquid crystal cured film, and improving the adhesion between the vertically aligned liquid crystal cured film and an adjacent layer (for example, a substrate). From the viewpoint of adhesion, it is preferable that the silane coupling agent is a silane coupling agent having an alkoxysilyl group and another different reactive group (for example, the above-mentioned functional group). Furthermore, it is preferable that the silane coupling agent is a silane coupling agent having an alkoxysilyl group and a polar group. When the silane coupling agent has at least one alkoxysilyl group and at least one polar group in its molecule, the vertical alignment of the polymerizable liquid crystal compound is more easily improved, and the vertical alignment promotion effect tends to be significantly obtained.The polar group can be, for example, an epoxy group, an amino group, an isocyanurate group, a mercapto group, a carboxy group, and a hydroxy group.The polar group may have a suitable substituent or a protective group in order to control the reactivity of the silane coupling agent.

[0188] Specific examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldi ... Examples of suitable silanes include ethyl dimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyldimethoxymethylsilane, and 3-glycidoxypropylethoxydimethylsilane.

[0189] In addition, examples of commercially available silane coupling agents include KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KB Examples of silane coupling agents available from Shin-Etsu Chemical Co., Ltd. include silane coupling agents such as E-502, KBE-503, KBM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBM-9659, KBE-585, KBM-802, KBM-803, KBE-846, and KBE-9007.

[0190] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains a nonionic silane compound, the content thereof is usually preferably 0.01% by mass to 5% by mass, more preferably 0.05% by mass to 4% by mass, and even more preferably 0.1% by mass to 3% by mass, based on the solid content of the polymerizable liquid crystal composition. When the content of the nonionic silane compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining good coatability of the polymerizable liquid crystal composition.

[0191] By containing both an ionic compound and a nonionic silane compound in the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film, the vertical alignment of the polymerizable liquid crystal compound is more easily promoted in the dried coating film formed on the substrate from the composition for forming a vertically aligned liquid crystal cured film due to the electrostatic interaction derived from the ionic compound and the surface tension reducing effect derived from the nonionic silane compound. This makes it possible to form a liquid crystal cured film while maintaining the polymerizable liquid crystal compound in a more precisely vertically aligned state.

[0192] <Horizontal alignment liquid crystal cured film> The horizontally aligned liquid crystal cured film in the present invention refers to a liquid crystal cured film obtained by applying the above-mentioned polymerizable liquid crystal composition onto a substrate or an alignment film, and curing the substrate in a state in which the polymerizable liquid crystal compound in the polymerizable liquid crystal composition is aligned in the in-plane direction of the alignment film.

[0193] In the present invention, it is preferable that the uniformity of the horizontally aligned liquid crystal cured film satisfies the following formula (S2). ReA(450) / ReA(550)<1.00 (S2) [In formula (S2), ReA(λ) represents an in-plane retardation value of the horizontally aligned retardation film at a wavelength of λ nm, and ReA(λ)=(nxA(λ)-nyA(λ))×dA (in the formula, nxA(λ) represents the principal refractive index at a wavelength of λ nm in the plane of the horizontally aligned retardation film, nyA(λ) represents the refractive index at a wavelength of λ nm in the same plane as nxA and in a direction perpendicular to the direction of nxA, and dA represents the film thickness of the horizontally aligned retardation film)]

[0194] When the horizontally aligned liquid crystal cured film satisfies the formula (S2), the horizontally aligned liquid crystal cured film exhibits a so-called reverse wavelength dispersion, in which the in-plane retardation value at a short wavelength is smaller than the in-plane retardation value at a long wavelength. When such a horizontally aligned liquid crystal cured film is incorporated into an organic EL display device, the front reflection hue during black display can be improved. In order to further enhance the effect of improving the reflection hue in the front direction, ReA(450) / ReA(550) is preferably 0.70 or more, more preferably 0.78 or more, and also preferably 0.95 or less, more preferably 0.92 or less.

[0195] The in-plane retardation value can be adjusted by the thickness dA of the horizontally aligned liquid crystal cured film. Since the in-plane retardation value is determined by the above formula ReA(λ)=(nxA(λ)-nyA(λ))×dA, the three-dimensional refractive index and the film thickness dA can be adjusted to obtain a desired in-plane retardation value (ReA(λ): in-plane retardation value of the horizontally aligned liquid crystal cured film at a wavelength λ(nm)).

[0196] In addition, it is preferable that the horizontally aligned liquid crystal cured film satisfies the following formula (S1). 100nm≦ReA(550)≦180nm (S1) [In formula (S1), ReA(λ) has the same meaning as above] When the in-plane retardation ReA(550) of the horizontally aligned liquid crystal cured film is within the range of formula (S1), the effect of improving the front reflection hue during black display (the effect of suppressing coloration) becomes significant when applied to an organic EL display device. A more preferable range of the in-plane retardation value is 120 nm≦ReA≦170 nm, and an even more preferable range is 130 nm≦ReA(550)≦150 nm.

[0197] A polymerizable liquid crystal compound that is conventionally known in the field of horizontally aligned liquid crystal cured films can be used. Among them, a polymerizable liquid crystal compound that exhibits so-called reverse wavelength dispersion is preferable, and as such a polymerizable liquid crystal compound, for example, a polymerizable liquid crystal compound represented by the above formula (X) can be preferably used. The polymerizable liquid crystal compound can be used alone or in combination of two or more kinds.

[0198] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition used for forming the horizontally aligned liquid crystal cured film is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and further preferably 90 to 95 parts by mass, relative to 100 parts by mass of the solid content of the polymerizable liquid crystal composition. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous from the viewpoint of the alignment of the obtained liquid crystal cured film.

[0199] The polymerizable liquid crystal composition used for forming the horizontally aligned liquid crystal cured film may further contain additives such as a solvent, a photopolymerization initiator, a leveling agent, an antioxidant, a photosensitizer, etc., in addition to the polymerizable liquid crystal compound. Examples of these components include the same ones as those exemplified above as components that can be used in the vertically aligned liquid crystal cured film, and each of them may be used alone or in combination of two or more.

[0200] The polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film can be obtained by stirring the polymerizable liquid crystal compound and components other than the polymerizable liquid crystal compound, such as a solvent and a photopolymerization initiator, at a predetermined temperature.

[0201] The horizontally aligned liquid crystal cured film is, for example, A step of applying a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film onto a substrate or an alignment film to obtain a coating film; drying the coating to form a dry coating; and A process of irradiating the dried coating with active energy rays to form a horizontally aligned liquid crystal cured film. The composition can be produced by a method comprising the steps of:

[0202] The formation of a coating film of the polymerizable liquid crystal composition can be carried out, for example, by applying the polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film onto a substrate, an alignment film, etc. As the substrate that can be used here, the same substrates as those exemplified above as substrates that can be used for producing a vertically aligned liquid crystal cured film can be used.

[0203] The alignment film can be appropriately selected from materials having a horizontal alignment regulating force that aligns the polymerizable liquid crystal compound in the horizontal direction relative to the coating film plane. The alignment regulating force can be arbitrarily adjusted by the type of alignment layer, the surface state, the rubbing conditions, etc., and when it is formed from a photo-alignable polymer, it can be arbitrarily adjusted by the polarized light irradiation conditions, etc. Examples of such materials include the above-mentioned alignment polymers as the alignment film that can be used in the manufacture of the vertically aligned liquid crystal cured film. The horizontal alignment film can be obtained by applying a composition containing such a material and a solvent, for example, the solvent exemplified in the vertically aligned liquid crystal cured film, to a substrate, removing the solvent, and then heating the applied film. It is preferable to use a photo-alignment film as the horizontal alignment film from the viewpoint of quality.

[0204] Next, the solvent is removed by drying or the like to form a dried coating film. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying. Heat drying is preferred from the viewpoint of productivity, and the heating temperature in this case is preferably such that the solvent can be removed and is equal to or higher than the phase transition temperature of the polymerizable liquid crystal compound. The procedure and conditions in this step may be the same as those that can be adopted in the manufacturing method of the vertically aligned liquid crystal cured film.

[0205] The obtained dried coating film is irradiated with active energy rays (more specifically, ultraviolet rays, etc.) to polymerize the polymerizable liquid crystal compound while maintaining the state in which the polymerizable liquid crystal compound is aligned in the horizontal direction relative to the coating film plane, thereby forming a horizontally aligned liquid crystal cured film. As the polymerization method, a method similar to the method that can be adopted in the manufacturing method of the vertically aligned liquid crystal cured film can be used.

[0206] <Horizontal alignment liquid crystal cured film containing dichroic dye> In the present invention, among the horizontally aligned liquid crystal cured films containing a dichroic dye, a film having a polarizing function may be called a polarizing film. In particular, in the case of a horizontally aligned liquid crystal cured film containing a dichroic dye, the higher the degree of alignment order of the liquid crystal, the more the absorption selectivity derived from the dichroic dye is improved, so it is preferable to use a polymerizable liquid crystal compound exhibiting the above-mentioned smectic phase, particularly a high-order smectic phase, and it is preferable to polymerize while maintaining the liquid crystal state of the smectic phase, preferably a high-order smectic phase, to form a polarizing film. A polarizing film obtained by polymerizing a polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase has an advantage of having high polarization performance, due to the action of the dichroic dye, compared to a conventional host-guest type polarizing film, that is, a polarizing film consisting of a liquid crystal state of a nematic phase. Furthermore, it also has an advantage of having excellent strength compared to a film coated with only a dichroic dye or a lyotropic liquid crystal.

[0207] A polarizing film having a high degree of orientation order shows a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase in X-ray diffraction measurement. The Bragg peak means a peak derived from a planar periodic structure of molecular orientation. Therefore, in a polarizing film formed from the polymerizable liquid crystal composition of the present invention, it is preferable that the polymerizable liquid crystal compound or its polymer is oriented so that the polarizing film shows a Bragg peak in X-ray diffraction measurement, and more preferably, the polymerizable liquid crystal compound is oriented in a "horizontal orientation" in which the molecules of the polymerizable liquid crystal compound are oriented in the direction in which light is absorbed. In the present invention, a polarizing film having a planar periodicity interval of the molecular orientation of 3.0 to 6.0 Å is preferable. A high degree of orientation order that shows a Bragg peak can be realized by controlling the type of polymerizable liquid crystal compound used, the type and amount of antioxidant, the type and amount of dichroic dye, etc.

[0208] The thickness of the horizontally aligned liquid crystal cured film can be appropriately selected, and is preferably 0.1 to 5 μm, more preferably 0.3 to 4 μm, and further preferably 0.4 to 3 μm.

[0209] <Elliptical polarizing plate> The present invention includes an elliptically polarizing plate comprising the cured liquid crystal film of the present invention. The elliptically polarizing plate is a laminate comprising at least a retardation film and a polarizing film.

[0210] The polarizing film is a film having a polarizing function, and examples thereof include the above-mentioned polarizing film, a stretched film having a dye having absorption anisotropy adsorbed thereon, a film having a polarizer coated with a dye having absorption anisotropy, etc. Examples of the dye having absorption anisotropy include a dichroic dye.

[0211] A film including, as a polarizer, a stretched film having adsorbed thereon a dye having absorption anisotropy is usually produced by uniaxially stretching a polyvinyl alcohol-based resin film, dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, treating the polyvinyl alcohol-based resin film having the adsorbed dichroic dye with an aqueous boric acid solution, and washing the film with water after the treatment with the aqueous boric acid solution, and then sandwiching the film between a transparent protective film via an adhesive on at least one surface of the polarizer produced through these steps.

[0212] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. As polyvinyl acetate resins, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith are used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.

[0213] The degree of saponification of the polyvinyl alcohol resin is usually about 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can also be used. The degree of polymerization of the polyvinyl alcohol resin is usually about 1,000 to 10,000, preferably in the range of 1,500 to 5,000.

[0214] Such a polyvinyl alcohol-based resin is used as a raw film for a polarizing film. The method for forming a film of the polyvinyl alcohol-based resin is not particularly limited, and the film can be formed by a known method. The thickness of the polyvinyl alcohol-based raw film can be, for example, about 10 to 150 μm.

[0215] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. It is also possible to perform the uniaxial stretching at these multiple stages. In the uniaxial stretching, the film may be uniaxially stretched between rolls having different peripheral speeds, or may be uniaxially stretched using a heated roll. The uniaxial stretching may be dry stretching in which the film is stretched in the air, or wet stretching in which the polyvinyl alcohol-based resin film is stretched in a swollen state using a solvent. The stretching ratio is usually about 3 to 8 times.

[0216] Dyeing of a polyvinyl alcohol-based resin film with a dichroic dye is carried out, for example, by a method of immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye.

[0217] Specifically, iodine or a dichroic organic dye is used as the dichroic pigment. Examples of the dichroic organic dye include a dichroic direct dye made of a disazo compound such as CIDIRECT RED 39, and a dichroic direct dye made of a compound such as trisazo or tetrakisazo. It is preferable that the polyvinyl alcohol resin film is immersed in water before the dyeing process.

[0218] When iodine is used as the dichroic dye, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing iodine and potassium iodide is usually adopted. The content of iodine in this aqueous solution is usually about 0.01 to 1 part by mass per 100 parts by mass of water. The content of potassium iodide is usually about 0.5 to 20 parts by mass per 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is usually about 20 to 40°C. The immersion time in this aqueous solution (dyeing time) is usually about 20 to 1,800 seconds.

[0219] On the other hand, when a dichroic organic dye is used as the dichroic pigment, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing a water-soluble dichroic dye is usually adopted. The content of the dichroic organic dye in this aqueous solution is usually 1×10 -4 ~10 parts by mass, preferably 1 × 10 -3 ~1 part by mass, more preferably 1 × 10 -3 ~1×10 -2 The amount of the dye in the aqueous solution is expressed by parts by mass. This aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing assistant. The temperature of the aqueous dichroic dye solution used for dyeing is usually about 20 to 80° C. The immersion time in the aqueous solution (dyeing time) is usually about 10 to 1,800 seconds.

[0220] The boric acid treatment after dyeing with a dichroic dye can usually be carried out by immersing the dyed polyvinyl alcohol resin film in an aqueous boric acid solution. The content of boric acid in this aqueous boric acid solution is usually about 2 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. When iodine is used as the dichroic dye, this aqueous boric acid solution preferably contains potassium iodide, and in this case, the content of potassium iodide is usually about 0.1 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. The immersion time in the aqueous boric acid solution is usually about 60 to 1,200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the boric acid treatment is usually 50°C or higher, preferably 50 to 85°C, and more preferably 60 to 80°C.

[0221] The polyvinyl alcohol-based resin film after the boric acid treatment is usually washed with water. The washing can be performed, for example, by immersing the boric acid-treated polyvinyl alcohol-based resin film in water. The temperature of the water used in the washing is usually about 5 to 40° C. The immersion time is usually about 1 to 120 seconds.

[0222] After washing with water, a drying treatment is carried out to obtain a polarizer. The drying treatment can be carried out, for example, using a hot air dryer or a far-infrared heater. The temperature of the drying treatment is usually about 30 to 100°C, and preferably 50 to 80°C. The time of the drying treatment is usually about 60 to 600 seconds, and preferably 120 to 600 seconds. The moisture content of the polarizer is reduced to a practical level by the drying treatment. The moisture content is usually about 5 to 20 mass%, and preferably 8 to 15 mass%. If the moisture content is less than 5 mass%, the polarizer loses its flexibility, and the polarizer may be damaged or broken after drying. If the moisture content exceeds 20 mass%, the thermal stability of the polarizer may be deteriorated.

[0223] The polyvinyl alcohol-based resin film is then uniaxially stretched, dyed with a dichroic dye, treated with boric acid, washed with water and dried to obtain a polarizer having a thickness of preferably 5 to 40 μm.

[0224] Examples of the film coated with a dye having absorption anisotropy include a film obtained by coating a composition containing a dichroic dye having liquid crystal properties or a composition containing a dichroic dye and a polymerizable liquid crystal. The film preferably has a protective film on one or both sides. Examples of the protective film include the same resin film as the above-mentioned example of a substrate that can be used for producing a horizontally aligned liquid crystal cured film.

[0225] The film coated with the dye having absorption anisotropy is preferably thin, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the film is usually 20 μm or less, preferably 5 μm or less, and more preferably 0.5 to 3 μm.

[0226] Specific examples of the film coated with a dye having absorption anisotropy include the films described in JP-A-2012-33249 and the like.

[0227] A polarizing film can be obtained by laminating a transparent protective film on at least one surface of the polarizer thus obtained via an adhesive. As the transparent protective film, a transparent film similar to the resin film exemplified above as a substrate usable for producing a horizontally aligned liquid crystal cured film can be preferably used.

[0228] The elliptical polarizing plate of the present invention is configured to include the liquid crystal cured film of the present invention. For example, the elliptical polarizing plate of the present invention can be obtained by laminating the liquid crystal cured film of the present invention to a polarizing film or the like via an adhesive layer or the like.

[0229] In one embodiment of the present invention, when the laminate of the present invention and a polarizing film are laminated, it is preferable to laminate them so that the angle between the slow axis (optical axis) of the horizontally aligned retardation film constituting the laminate and the absorption axis of the polarizing film is 45±5°.

[0230] The elliptical polarizing plate of the present invention may have a structure similar to that of a conventional general elliptical polarizing plate, or a polarizing film and a retardation film. Examples of such structures include an adhesive layer (sheet) for attaching the elliptical polarizing plate to a display element such as an organic EL display, and a protective film used for protecting the surface of the polarizing film or retardation film from scratches and dirt.

[0231] The laminate and the elliptically polarizing plate of the present invention can be used in various display devices. A display device is a device having a display element, and includes a light-emitting element or a light-emitting device as a light source. Examples of display devices include liquid crystal display devices, organic electroluminescence (EL) display devices, inorganic electroluminescence (EL) display devices, touch panel display devices, electron emission display devices (e.g., field emission display devices (FEDs) and surface field emission displays (SEDs)), electronic paper (display devices using electronic ink or electrophoretic elements, plasma display devices, projection display devices (e.g., grating light valve (GLV) display devices and display devices having a digital micromirror device (DMD)), and piezoelectric ceramic displays. Examples of liquid crystal display devices include transmissive liquid crystal display devices, semi-transmissive liquid crystal display devices, and reflective liquid crystal display devices. The elliptically polarizing plate of the present invention includes any of a direct-view type liquid crystal display device and a projection type liquid crystal display device. These displays may be displays that display two-dimensional images or stereoscopic displays that display three-dimensional images. In particular, the elliptically polarizing plate of the present invention can be suitably used in organic electroluminescence (EL) displays because the effects thereof are easily exhibited remarkably, and the laminate of the present invention can be suitably used in liquid crystal displays and touch panel displays. These displays are excellent in front reflection hue and oblique reflection hue during black display, and are also excellent in front hue and oblique hue during white display, and can exhibit good image display characteristics. EXAMPLES

[0232] The present invention will now be described in more detail with reference to the following examples. In the examples, "%" and "parts" mean "% by mass" and "parts by mass", respectively, unless otherwise specified.

[0233] <Example 1> [Preparation of Liquid Crystal Compounds] Liquid crystal compound A was produced according to the method described in JP 2010-31223 A. Liquid crystal compound B was produced according to the method described in JP 2009-173893 A. The molecular structures of liquid crystal compound A and liquid crystal compound B are shown below.

[0234] (Liquid crystal compound A) [ka]

[0235] (Liquid crystal compound B) [ka]

[0236] [Preparation of composition for forming vertically aligned liquid crystal cured film] Liquid crystal compound A and liquid crystal compound B were mixed in a mass ratio of 90:10 to obtain a mixture. 0.10 parts by mass of leveling agent "BYK-361N" (manufactured by BYK-Chemie), 0.25 parts by mass of leveling agent "F-556" (manufactured by DIC), 2.0 parts by mass of ionic compound A prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of KBE-9103 manufactured by Shin-Etsu Chemical Co., Ltd., and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. The mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a vertically aligned liquid crystal cured film.

[0237] Ionic compound A: [ka] The molecular weight of the acrylic leveling agent "BYK-361N" was measured by GPC (Tosoh Corporation, HLC-8220GPC, solvent: tetrahydrofuran, detector: RI) and found to be 4,800 in number average molecular weight.

[0238] [Method for producing a vertically aligned liquid crystal cured film] A corona treatment was performed on a cycloolefin film (ZF-14-50) manufactured by Zeon Corporation, a composition for forming a cured film of vertically aligned liquid crystals was applied using a bar coater, and the composition was heated at 120°C for 60 seconds. After that, ultraviolet light was irradiated from the surface on which the composition for forming a cured film of horizontally aligned liquid crystals was applied using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (accumulated light amount at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm2). 2 ) to form a vertically aligned liquid crystal cured film. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and was found to be 1.2 μm.

[0239] [Rth measurement of vertically aligned liquid crystal cured film] When using KOBRA-WPR manufactured by Oji Scientific Instruments, the phase difference of a film having anisotropic absorption in visible light cannot be measured. Therefore, a composition for forming a vertically aligned liquid crystal cured film was prepared by removing only the dichroic dye A from the composition for forming a vertically aligned liquid crystal cured film, and then the composition was used to form a vertically aligned liquid crystal cured film in the same manner. After confirming that the cycloolefin film had no phase difference, the angle of incidence of light on the sample for measuring optical properties was changed to measure the front phase difference value (in-plane phase difference value) of the vertically aligned liquid crystal cured film and the phase difference value when tilted 40° from the center of the fast axis using "KOBRA-WPR" manufactured by Oji Scientific Instruments. The average refractive index at each wavelength was measured using an ellipsometer M-220 manufactured by JASCO Corporation. The film thickness was also measured using an Optical NanoGauge film thickness meter C12562-01 manufactured by Hamamatsu Photonics K.K. The three-dimensional refractive index was calculated from the aforementioned front retardation value (in-plane retardation value), retardation value when tilted 40° from the fast axis center, average refractive index, and film thickness, with reference to Oji Scientific Instruments' technical documentation (http: / / www.oji-keisoku.co.jp / products / kobra / reference.html). The optical properties of each vertically aligned liquid crystal cured film were calculated from the obtained three-dimensional refractive index according to the following formula, and the results are shown in Table 1. RthC(λ)=((nxC(λ)+nyC(λ)) / 2-nzC(λ))×dC αthC = RthC(450) / RthC(550)

[0240] [Production of polarizing film] A polyvinyl alcohol film having an average degree of polymerization of about 2,400, a degree of saponification of 99.9 mol% or more, and a thickness of 75 μm was immersed in pure water at 30° C., and then immersed in an aqueous solution having a weight ratio of iodine / potassium iodide / water of 0.02 / 2 / 100 at 30° C. to perform iodine dyeing (iodine dyeing step). The polyvinyl alcohol film that had undergone the iodine dyeing step was immersed in an aqueous solution having a weight ratio of potassium iodide / boric acid / water of 12 / 5 / 100 at 56.5° C. to perform boric acid treatment (boric acid treatment step). The polyvinyl alcohol film that had undergone the boric acid treatment step was washed with pure water at 8° C., and then dried at 65° C. to obtain a polarizer (thickness 27 μm after stretching) in which iodine was adsorbed and aligned in the polyvinyl alcohol. At this time, stretching was performed in the iodine dyeing step and the boric acid treatment step. The total stretching ratio in such stretching was 5.3 times. The obtained polarizer and a saponified triacetyl cellulose film (KC4UYTAC 40μm, manufactured by Konica Minolta) were bonded together by nip rolls via a water-based adhesive. The resulting laminate was dried at 60°C for 2 minutes while maintaining a tension of 430N / m to obtain a polarizing film having a triacetyl cellulose film as a protective film on one side. The water-based adhesive was prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (Kuraray Poval KL318, manufactured by Kuraray) and 1.5 parts of water-soluble polyamide epoxy resin (Sumirez Resin 650, manufactured by Sumika Chemtex, aqueous solution with a solid content of 30%) to 100 parts of water.

[0241] The obtained polarizing film was checked for unevenness and evaluated for orientation. Measurements were performed using a spectrophotometer (V7100, manufactured by JASCO) with the polarizer surface of the polarizing plate obtained above as the incident surface. The obtained luminous efficiency-corrected single transmittance was 42.1%, luminous efficiency-corrected polarization degree was 99.996%, single hue a was -1.1, and single hue b was 3.7.

[0242] [Check for unevenness] In a darkroom, the brightness of a Tritec A4-500 backlight was set to 4700 lux, and two polarizing films manufactured by the above method were placed on the backlight in a crossed Nicol configuration. Next, the vertically aligned liquid crystal cured film manufactured by the above method was placed between the two polarizing films, and the vertically aligned liquid crystal cured film was rotated while tilted so that the angle between the film and the backlight surface was 60°, so that the light leakage due to the phase difference of the vertically aligned liquid crystal cured film was maximized when viewed from the polarizing film surface side. In the above state, the unevenness of the vertically aligned liquid crystal cured film was confirmed according to the following criteria. .circle-solid.: No visible unevenness. ○: Some unevenness is visible. △: Unevenness is visible. ×: Strong unevenness is visible.

[0243] [Orientation Evaluation] First, the vertically aligned liquid crystal cured film was attached to a glass of 5×5 cm×0.7 mm thickness via a pressure-sensitive adhesive (25 μm) manufactured by Lintec Corporation. The obtained sample was observed at a magnification of 200 times using a polarizing microscope (Olympus Corporation's "BX-51"), and the number of alignment defects in a field of view of 480 μm×320 μm was counted. Here, only the number of alignment defects caused by the measurement sample was counted, and the number of defects caused by environmental foreign matter other than the sample was excluded and not counted. From the observation results using the polarizing microscope, the alignment of the vertically aligned liquid crystal cured film was evaluated based on the following evaluation criteria. In addition, ◯ and △ were judged to have excellent alignment. Evaluation criteria: ◯ (Very good): The number of orientation defects is 5 or less. △ (good): The number of orientation defects is 6 or more and 20 or less. × (bad): The number of orientation defects is 21 or more, or there is no orientation at all.

[0244] <Examples 2 to 5> When preparing the composition for forming a vertically aligned liquid crystal cured film, the leveling agent added was changed to "BYK-361N" (acrylic leveling agent), "BYK-UV3500" (silicon leveling agent), and "F-556" (fluorine leveling agent) manufactured by DIC Corporation as shown in Table 1, and the amount of the leveling agent added was changed. A vertically aligned liquid crystal cured film was produced in the same manner as in Example 1, and its Rth was measured, and unevenness and alignment were confirmed. The results are shown in Table 1.

[0245] <Example 6> [Preparation of composition for forming horizontal alignment film] Five parts of a photoalignment material (weight average molecular weight: 30,000) having the following structure and 95 parts of cyclopentanone (solvent) were mixed as components, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a horizontal alignment film. [ka]

[0246] [Preparation of composition for forming horizontally aligned liquid crystal cured film] Liquid crystal compound A and liquid crystal compound B were mixed in a mass ratio of 90:10 to obtain a mixture. 0.1 mass parts of a leveling agent "BYK-361N" (manufactured by BYK-Chemie), 0.25 mass parts of a leveling agent "F-556" (manufactured by DIC), and 6 mass parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 mass parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. A composition for forming a horizontally aligned liquid crystal cured film was obtained by stirring at 80 ° C. for 1 hour.

[0247] A 1 mg / 50 mL tetrahydrofuran solution of liquid crystal compound A was prepared, and the measurement sample was placed in a measurement cell with an optical path length of 1 cm. The measurement sample was then set in an ultraviolet-visible spectrophotometer (Shimadzu Corporation, "UV-2450") to measure the absorption spectrum. The wavelength at which the maximum absorbance was obtained was read from the obtained absorption spectrum. The maximum absorption wavelength λ in the wavelength range of 300 to 400 nm was max was 350 nm.

[0248] [Method for producing horizontally aligned liquid crystal cured film] The composition for forming a horizontal alignment film was applied onto a cycloolefin film (ZF-14-50) manufactured by Zeon Corporation using a bar coater, dried at 80°C for 1 minute, and then irradiated with a polarized UV irradiation device (SPOT CURE SP-9; manufactured by Ushio Inc.) with an integrated light amount of 100 mJ / cm at a wavelength of 313 nm. 2 The film thickness of the obtained horizontal alignment film was measured by an ellipsometer and found to be 200 nm.

[0249] Next, a composition for forming a horizontally aligned liquid crystal cured film was applied onto the horizontal alignment film using a bar coater, and heated at 120°C for 60 seconds. After that, ultraviolet light was irradiated from the surface onto which the composition for forming a horizontally aligned liquid crystal cured film was applied using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, cumulative light amount at a wavelength of 365 nm: 500 mJ / cm 2 ) to form a horizontally aligned liquid crystal cured film. After confirming that the COP film had no retardation, Re(450) and Re(550) were measured using KOBRA-WPR manufactured by Oji Scientific Instruments. The results are shown in Table 1.

[0250] [Check for unevenness] In a darkroom, with the brightness of a Tritec A4-500 backlight set to 4700 lux, two polarizing films manufactured by the above method were placed on the backlight in a crossed Nicol configuration. Next, the horizontally aligned liquid crystal cured film was placed between the two polarizing films so that the angle between the slow axis of the horizontally aligned liquid crystal cured film manufactured by the above method and the absorption axis of the polarizing film was 45°, and the unevenness of the horizontally aligned liquid crystal cured film was confirmed by visual inspection from the side opposite to the backlight according to the following criteria. .circle-solid.: No visible unevenness. ○: Some unevenness is visible. △: Unevenness is visible. ×: Strong unevenness is visible.

[0251] [Orientation Evaluation] First, the horizontally aligned liquid crystal cured film was attached to a glass of 5×5 cm×0.7 mm thickness via a pressure-sensitive adhesive (25 μm) manufactured by Lintec Corporation. The obtained sample was observed at a magnification of 200 times using a polarizing microscope (Olympus Corporation's "BX-51"), and the number of alignment defects in a field of view of 480 μm×320 μm was counted. Here, only the number of alignment defects caused by the measurement sample was counted, and the number of defects caused by environmental foreign matter other than the sample was excluded and not counted. From the observation results using the polarizing microscope, the alignment of the vertically aligned liquid crystal cured film was evaluated based on the following evaluation criteria. In addition, ◯ and △ were judged to have excellent alignment. Evaluation criteria: ◯ (Very good): The number of orientation defects is 5 or less. △ (good): The number of orientation defects is 6 or more and 20 or less. × (bad): The number of orientation defects is 21 or more, or there is no orientation at all.

[0252] <Example 7> [Preparation of composition for forming horizontal alignment film] Five parts of a photoalignment material (weight average molecular weight: 30,000) having the following structure and 95 parts of cyclopentanone (solvent) were mixed as components, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a horizontal alignment film. [ka]

[0253] [Preparation of horizontally aligned liquid crystal cured film composition] The following components were mixed and stirred at 80°C for 1 hour to obtain a horizontally aligned liquid crystal cured film composition (polarizing layer forming composition). The dichroic dye used was an azo dye described in the examples of JP2013-101328A. The polymerizable liquid crystal compounds represented by formulae (1-6) and (1-7) were produced according to the method described in lub et al., Recl.Trav.Chim.Pays-Bas, 115, 321-328(1996).

[0254] Polymerizable liquid crystal compound: [ka] 75 copies [ka] 25 copies Dichroic dye 1: polyazo dye; compound (1-8) 2.5 parts [ka] Compound (1-5) 2.5 parts [ka] Compound (1-16) 2.5 parts [ka] Polymerization initiator; 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals) 6 parts Leveling agent; "BYK-361N" (BYK-Chemie) 0.1 parts by mass (acrylic leveling agent) "F-556" (DIC Corporation) 0.25 parts by mass (fluorine-based leveling agent) Solvent: o-xylene 250 parts

[0255] [Production of horizontally aligned liquid crystal cured film] A triacetyl cellulose film (KC4UY) manufactured by Konica Minolta, Inc. was treated once using a corona treatment device (AGF-B10 manufactured by Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. A composition for forming a horizontal alignment film (composition for forming a polarizing layer) was applied to the corona-treated surface with a bar coater, dried at 80°C for 1 minute, and then irradiated with 100 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7 manufactured by Ushio Inc.). 2 The film was exposed to polarized UV light at an axial angle of 90° with an integrated light amount of 10 ... Next, a composition for forming a horizontally aligned liquid crystal cured film (composition for forming a polarizing layer) was applied using a bar coater, and then dried for 1 minute in a drying oven set at 120°C to obtain a dried coating film in which the polymerizable liquid crystal compound and the dichroic dye were aligned. After this dried coating film was naturally cooled to room temperature, it was irradiated with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm2) using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.). 2 ) to polymerize the polymerizable liquid crystal compound, thereby producing a horizontally aligned liquid crystal cured film (polarizing film).

[0256] [Measurement of polarization degree and single transmittance] The polarization degree and single transmittance of the obtained horizontally aligned liquid crystal cured film (polarizing film) were measured as follows. 1 ) and transmittance along the absorption axis (T 2) was measured in the wavelength range of 380 to 680 nm in 2 nm steps using a spectrophotometer (Shimadzu Corporation UV-3150) equipped with a polarizer folder by the double beam method. The unit transmittance and degree of polarization at each wavelength were calculated using the following formulas (p) and (q), and luminosity correction was performed using the 2-degree visual field (C light source) of JIS Z 8701 to calculate the luminosity-corrected unit transmittance (Ty) and luminosity-corrected degree of polarization (Py). The unit transmittance was 42% and the degree of polarization was 97%, confirming that these values ​​are useful for a polarizing film. Single unit transmittance (%) = (T 1 +T 2 ) / 2(p) Degree of polarization (%) = {(T 1 -T 2 ) / (T 1 +T 2 )}×100 (q)

[0257] [Check for unevenness] In a darkroom, with the brightness of a Tritec A4-500 backlight set to 4700 lux, one sheet of polarizing film manufactured by the above method was placed on the backlight, and a horizontally aligned liquid crystal cured film was placed so that the angle between the absorption axis of the horizontally aligned liquid crystal cured film and the absorption axis of the polarizing film was 90° (cross Nicol state). The placed sample was visually observed from the side opposite the backlight, and unevenness of the horizontally aligned liquid crystal cured film was confirmed according to the following criteria. .circle-solid.: No visible unevenness. ○: Some unevenness is visible. △: Unevenness is visible. ×: Strong unevenness is visible.

[0258] [Orientation Evaluation] First, the horizontally aligned liquid crystal cured film was attached to a glass of 5×5 cm×0.7 mm thickness via a pressure-sensitive adhesive (25 μm) manufactured by Lintec Corporation. The obtained sample was observed at a magnification of 200 times using a polarizing microscope (Olympus Corporation's "BX-51"), and the number of alignment defects in a field of view of 480 μm×320 μm was counted. Here, only the number of alignment defects caused by the measurement sample was counted, and the number of defects caused by environmental foreign matter other than the sample was excluded and not counted. From the observation results using the polarizing microscope, the alignment of the vertically aligned liquid crystal cured film was evaluated based on the following evaluation criteria. In addition, ◯ and △ were judged to have excellent alignment. Evaluation criteria: ◯ (Very good): The number of orientation defects is 5 or less. △ (good): The number of orientation defects is 6 or more and 20 or less. × (bad): The number of orientation defects is 21 or more, or there is no orientation at all.

[0259] <Example 8> A vertically aligned liquid crystal cured film was produced in the same manner as in Example 1, except that the preparation method of the composition for forming a vertically aligned liquid crystal cured film was changed as shown below, and unevenness and alignment were confirmed. The results are shown in Table 1. Incidentally, the retardation value of the vertically aligned liquid crystal cured film was not measured because it includes a dichroic formula. In addition, when the absorbance of the vertically aligned liquid crystal cured film was measured by the method described below, λmax=600 nm, AxC=0.024, and AxC(z=60)=0.175.

[0260] [Preparation of polymerizable liquid crystal composition for forming vertically aligned liquid crystal cured film] The liquid crystal compound (A) and the liquid crystal compound (B) were mixed in a mass ratio of 90:10 to obtain a mixture. 0.1 parts by mass of a leveling agent "BYK-361N" (manufactured by BYK-Chemie), 0.25 parts by mass of a leveling agent "F-556" (manufactured by DIC), 1.5 parts by mass of the dichroic dye A shown below described in JP-A-2013-101328, 2.0 parts by mass of an ionic compound A (molecular weight: 645) prepared with reference to JP-A-2016-514802, 0.5 parts by mass of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") were added to 100 parts by mass of the obtained mixture. Further, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration became 13%. The mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film.

[0261] Dichroic compound A: [ka]

[0262] [Measurement of absorbance of cured film of vertically aligned liquid crystal] The coated surface of the vertically aligned liquid crystal cured film prepared by the above method was attached to a 4 × 4 cm × 0.7 mm thick glass plate via a 25 μm pressure-sensitive adhesive (manufactured by Lintec Corporation). The plate was then set in a UV-visible spectrophotometer (Shimadzu Corporation, “UV-2450”) to measure the absorbance, and the maximum absorption wavelength (λmax) at wavelengths of 400 to 750 nm, AxC, and AxC(z=60) were calculated. Here, the x-axis means any direction in the plane of the vertically aligned liquid crystal cured film, the y-axis means a direction perpendicular to the x-axis in the film plane, and the z-axis means the thickness direction of the vertically aligned liquid crystal cured film. AxC and AxC(z=60) are both absorbances at the maximum absorption wavelength of 400 to 750 nm of the vertically aligned liquid crystal cured film, where AxC represents the absorbance of linearly polarized light vibrating in the x-axis direction, and AxC(z=60) represents the absorbance of linearly polarized light vibrating in the x-axis direction when the film is rotated 60° around the y-axis as the rotation axis.

[0263] When measuring absorbance, the sample was set in an ultraviolet-visible spectrophotometer (Shimadzu Corporation, "UV-2450") and AxC was measured after correcting the absorbance at 800 nm to zero. For AxC (z=60), the sample was set and tilted in the same manner, and the absorbance at 800 nm was corrected to zero, after which AxC (z=60) was measured.

[0264] <Comparative Examples 1 to 4> A vertically aligned liquid crystal cured film was produced in the same manner as in Example 1, except that the leveling agent added during preparation of the composition for forming the vertically aligned liquid crystal cured film was changed to "BYK-361N" and "BYK-392" manufactured by BYK-chemie, and "F-556" manufactured by DIC, and the amount of the leveling agent added was changed, as shown in Table 1. The unevenness and alignment of the film were confirmed. The results are shown in Table 1.

[0265] The molecular weight of the acrylic leveling agent "BYK-392" was measured by GPC (Tosoh Corporation, HLC-8220GPC, solvent: tetrahydrofuran, detector: RI) and found to be 13,100 in number average molecular weight.

[0266] [Table 1] In Table 1, Re represents either the in-plane retardation value of the horizontal alignment film or the in-plane retardation value of the vertical alignment film.

[0267] According to the present invention, by using a predetermined leveling agent, it is possible to improve unevenness without impairing the alignment of the liquid crystal cured film.

Claims

1. At least one silicone-based leveling agent, at least one acrylic-based leveling agent, and at least one polymerizable liquid crystal compound represented by the following formula (X): A liquid crystal cured film-forming composition, wherein the total amount of a leveling agent is 3.0% by mass or less based on the total amount of a polymerizable liquid crystal compound. 【Chemistry 1】 In formula (X), Ar represents a divalent group having an aromatic group which may have a substituent. G 1 and G 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. L 1 , L 2 , B 1 and B 2 each independently represents a single bond or a divalent linking group. k and l each independently represent an integer of 0 to 3, and satisfy the relationship of 1≦k+l. Here, when 2≦k+l, B 1 and B 2 , G 1 and G 2 may be the same as or different from each other. E 1 and E 2 each independently represents an alkanediyl group having 1 to 17 carbon atoms. Herein, a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and —CH 2 - is -O-, -S-, -SiH 2 It may be substituted with -- or --C(.dbd.O)--. P 1 and P 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.

2. The composition for forming a liquid crystal cured film according to claim 1 , further comprising a dichroic dye.

3. 3. The composition for forming a liquid crystal cured film according to claim 1, wherein the polymerizable liquid crystal compound is a polymerizable liquid crystal compound exhibiting a smectic phase.

4. 4. The composition for forming a liquid crystal cured film according to claim 1, wherein the polymerizable liquid crystal compound is a liquid crystal compound having a T-shaped structure.

5. 5. A liquid crystal cured film obtained by curing a polymerizable liquid crystal compound contained in the composition for forming a liquid crystal cured film according to claim 1 in an aligned state.

6. The liquid crystal cured film according to claim 5 , wherein the thickness of the liquid crystal cured film is 0.3 μm or more and 5.0 μm or less.

7. The liquid crystal cured film according to claim 5 or 6, which is a horizontally aligned liquid crystal cured film obtained by curing a polymerizable liquid crystal compound in a state where the polymerizable liquid crystal compound is aligned in a direction parallel to an in-plane direction.

8. The liquid crystal cured film according to any one of claims 5 to 7, further satisfying the following formula (S1): 100nm≦ReA(550)≦180nm...(S1) (In the formula, ReA(550) represents an in-plane retardation value at a wavelength of 550 nm.)

9. The liquid crystal cured film according to any one of claims 5 to 8, further satisfying the following formula (S2): ReA(450) / ReA(550)<1.0...(S2) (In the formula, ReA(450) represents an in-plane retardation value at a wavelength of 450 nm.)

10. The horizontally aligned liquid crystal cured film according to any one of claims 5 to 9, which is a horizontally aligned liquid crystal cured film and shows a Bragg peak in X-ray diffraction measurement.

11. The liquid crystal cured film according to claim 5 or 6, which is a vertically aligned liquid crystal cured film in which the polymerizable liquid crystal compound is cured in a state where it is aligned in a direction perpendicular to the in-plane direction.

12. The liquid crystal cured film according to claim 11, further satisfying the following relational formula (S3): -150≦RthC(550)≦-30...(S3) [In the relational formula (S3), RthC(550) represents a retardation value in the thickness direction of the liquid crystal cured film at a wavelength of 550 nm]

13. The liquid crystal cured film according to claim 11 or 12, further satisfying the following relational formula (S4): RthC(450) / RthC(550)≦1.0...(S4) [In the relational formula (S4), RthC(450) represents a retardation value in the thickness direction of the liquid crystal cured film at a wavelength of 450 nm, and RthC(550) represents a retardation value in the thickness direction of the liquid crystal cured film at a wavelength of 550 nm]

14. An elliptical polarizing plate including a horizontally aligned retardation film and a polarizing film, An elliptically polarizing plate, wherein at least one of a horizontally aligned retardation film and a polarizing film is the liquid crystal cured film according to any one of claims 5 to 10.

15. An elliptical polarizing plate including a horizontally aligned retardation film, a vertically aligned liquid crystal cured film, and a polarizing film, An elliptically polarizing plate, wherein at least one of a horizontally aligned retardation film, a vertically aligned liquid crystal cured film, and a polarizing film is the liquid crystal cured film according to any one of claims 5 to 13.

16. 16. The elliptically polarizing plate according to claim 14, wherein an angle between a slow axis of the horizontally aligned retardation film and an absorption axis of the polarizing plate is 45±5°.

17. An organic EL display device comprising the elliptically polarizing plate according to any one of claims 14 to 16.

Citation Information

Patent Citations

  • Optical film

    JP2015163935A

  • Phase difference film

    JP2017120431A

  • Elliptically polarizing plate

    JP2017167517A

  • Composite polarizing plate

    US20160291224A1

  • Elliptical polarizing plate

    WO2018016360A1