Starter two-component developer, refill two-component developer, and method for producing two-component developer

The two-component developer system addresses non-uniform charge distribution issues by using silica fine particles with controlled properties, enhancing charging uniformity and transferability for stable high-quality image output.

JP7560996B2Active Publication Date: 2024-10-03CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020179909
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-10-03
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

Existing two-component developers in electrophotography face challenges in achieving high image quality and stable transferability due to non-uniform charge distribution on toner particles, leading to issues like increased electrostatic adhesion and transferability problems.

Method used

A starter and replenishment two-component developer system is developed, utilizing magnetic carriers with silica fine particles having specific particle size, charge decay constants, and coverage rates to enhance charging uniformity and reduce electrostatic adhesion, ensuring stable high-quality image output over time.

Benefits of technology

The system achieves improved transferability and reduced electrostatic adhesion, maintaining high image quality and stability over a long period by optimizing silica fine particle properties on magnetic carriers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560996000007
    Figure 0007560996000007
  • Figure 0007560996000008
    Figure 0007560996000008
  • Figure 0007560996000001
    Figure 0007560996000001
Patent Text Reader

Abstract

To provide a two-component developer that has satisfactory transfer properties and can stably output high image quality for a long period from the initial stage of its use.SOLUTION: A starter two-component developer includes toner and magnetic carrier. The magnetic carrier is a magnetic carrier having a magnetic carrier particle, and silica fine particles A present on the surface of the magnetic carrier particle. The number average particle diameter of primary particles of the silica fine particles A is 10 nm or more and 200 nm or less. After 1800 seconds from when the silica fine particles A are electrified in an environment of a temperature of 23°C and a relative humidity of 50%, the silica fine particles A have a charge attenuation constant α of 0.0005 or more and 0.0100 or less. The coverage of the surface of the magnetic carrier particle by the silica fine particles A is 1.0 area% or more and 15.0 area% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a starter two-component developer, a replenishment two-component developer, and a method for producing the two-component developer, which are used in an image forming method for visualizing an electrostatic image by electrophotography. [Background technology]

[0002] Conventionally, in the electrophotographic image forming method, a method is generally used in which an electrostatic latent image is formed on an electrostatic latent image carrier by using various means, and a toner is attached to the electrostatic latent image to develop it. In this development, a two-component development method is widely adopted in which a magnetic carrier is mixed with a toner, and the toner is triboelectrically charged to give an appropriate amount of positive or negative charge to the toner, and the charge is used as a driving force for development.

[0003] In the two-component development method, the magnetic carrier can be given functions such as stirring, transporting, and charging the developer, so the division of functions between the magnetic carrier and the toner is clear, which has the advantage of good controllability of developer performance.

[0004] On the other hand, in recent years, with the advancement of technology in the field of electrophotography, there is an increasingly strict demand for higher speed and longer life of the device as well as higher definition and stable image quality. In order to meet such demands, there is a demand for higher performance of two-component developers.

[0005] For example, in order to obtain a developer that can stably maintain the charge amount from the initial use, a manufacturing method has been proposed in which inorganic fine particles are attached to the carrier surface, and then toner is electrostatically mixed and attached to the carrier surface (Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 5-303235 Summary of the Invention [Problem to be solved by the invention]

[0007] Patent Document 1 has improved the stability of charging over a long period of time. However, in terms of high image quality to meet the print-on-demand market, there is still room for improvement in terms of transferability. In order to improve transferability, it is necessary to further improve the developability of the toner, and for this purpose, the uniformity of charge on the surface of each toner particle is important. For example, when silica fine particles are externally added to magnetic carrier particles, the distribution of the silica fine particles on the surface of each magnetic carrier particle may inevitably become uneven. Since silica fine particles have high electrical resistance, the charge distribution of each magnetic carrier particle may become uneven, and the charge distribution may also become uneven on the surface of each toner particle after frictional charging with the toner. As a result, the electrostatic adhesion force between the toner and the electrostatic latent image carrier may become high, which may affect transferability and cause problems.

[0008] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to solve the above-mentioned problems and to provide a two-component developer capable of stably outputting high image quality with good transferability from the initial stage of use over a long period of time. [Means for solving the problem]

[0009] The present inventors have found that by using a starter two-component developer and a replenishment two-component developer as described below, the charging uniformity of the surface of each toner particle is improved, and high image quality with good transferability can be stably output from the initial stage of use over a long period of time.

[0010] That is, the present invention is A starter two-component developer containing a toner and a magnetic carrier, The magnetic carrier has magnetic carrier particles and silica fine particles A present on the surfaces of the magnetic carrier particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more 150 nm or less, The silica fine particles A have a charge decay constant α of 0.00 after 1800 seconds from being charged in an environment of a temperature of 23° C. and a relative humidity of 50%. 20 is equal to or greater than 0.0100 and is equal to or less than 0.0100, The coverage of the surfaces of the magnetic carrier particles with the silica fine particles A is 1.0% by area or more. 5.2 % or less by area.

[0011] Another aspect of the present invention is A replenishing two-component developer containing a toner and a magnetic carrier, The magnetic carrier has magnetic carrier particles and silica fine particles A present on the surfaces of the magnetic carrier particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more 150 nm or less, The silica fine particles A have a charge decay constant α of 0.00 after 1800 seconds from being charged in an environment of a temperature of 23° C. and a relative humidity of 50%. 20 is equal to or greater than 0.0100 and is equal to or less than 0.0100, The coverage of the surfaces of the magnetic carrier particles with the silica fine particles A is 1.0% by area or more. 5.2 % or less by area. Effect of the Invention

[0012] According to the present invention, it is possible to provide a starter two-component developer capable of stably outputting high image quality with good transferability from the initial stage of use over a long period of time. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram of an image forming apparatus. [Diagram 2] FIG. 1 is a schematic diagram of an image forming apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In the present invention, the description "XX to XX" representing a numerical range means a numerical range including the lower and upper limits which are the endpoints, unless otherwise specified.

[0015] The starter two-component developer and replenishment two-component developer containing a magnetic carrier and a toner according to the present invention are magnetic carriers in which silica fine particles A are present on the surface of the magnetic carrier particles, and the silica fine particles A satisfy the following requirements. The silica fine particles A have a number average particle size of primary particles of 10 nm or more and 200 nm or less. The silica fine particles A have a charge decay constant α of 0.0005 or more and 0.0100 or less 1800 seconds after being charged in an environment having a temperature of 23° C. and a relative humidity of 50%. Moreover, the coverage of the surfaces of the magnetic carrier particles with the silica fine particles A is 1.0 area % or more and 15.0 area % or less.

[0016] By satisfying this requirement, the effect of improving the transferability of electrophotographic properties can be obtained. The improvement in the transferability is believed to be due to the following reasons. When conventional silica fine particles are attached to the surface of magnetic carrier particles, the distribution of silica fine particles on the surface of each magnetic carrier particle becomes non-uniform, and the charge distribution on the surface of each magnetic carrier particle also becomes non-uniform. As a result, the uniformity of the charge distribution on the surface of each toner particle charged by frictional charging with the magnetic carrier also deteriorates. In particular, since the movement of charges is slow with conventional silica fine particles, it is difficult to obtain the effect of uniform charge distribution, and it is difficult to obtain the effect of leveling the charge distribution on the surface of each toner particle.

[0017] However, in the present invention, the magnetic carrier particles have silica fine particles A on their surfaces, the silica fine particles A having a charge decay constant α of 0.0005 or more and 0.0100 or less in an environment of 23° C. and 50% RH. By setting the charge decay constant α of silica fine particles A within the above range, the effect of accelerating the movement of charge in silica fine particles A present on the surface of the magnetic carrier particles can be obtained. Therefore, when the magnetic carrier and toner are frictionally charged, charge is quickly exchanged between each magnetic carrier particle and each toner particle, and the effect of leveling the charge distribution on the surface of each toner particle can be obtained. As a result, it is believed that the charge uniformity of the surface layer of each toner particle is improved, the electrostatic adhesion force between the toner and the electrostatic latent image carrier is reduced, and transferability is improved.

[0018] When the charge decay constant α of the silica fine particles A in an environment of 23°C and 50% RH is 0.0005 or more, it promotes charge transfer in the silica fine particles A. This promotes rapid charge transfer between the magnetic carrier particles and the toner particles, thereby achieving a reduction in electrostatic adhesion force. Furthermore, when the charge decay constant α of the silica microparticles A in an environment of 23°C and 50% RH is 0.0100 or less, the leakage of excess charge from the magnetic carrier surface is suppressed, thereby suppressing localized charging of the toner and preventing problems such as fogging.

[0019] The number average particle size of the primary particles of the silica fine particles A is 10 nm or more and 200 nm or less. When the number-average particle diameter of the primary particles of the silica fine particles A on the surface of the magnetic carrier particles is 10 nm or more, the two-component developer is not embedded in the magnetic carrier particles even when used for a long period of time, and can exhibit a high spacer effect and maintain the charge for a long period of time. Furthermore, when the number-average particle diameter of the primary particles of the silica fine particles A is 200 nm or less, even when the two-component developer is used for a long period of time, the silica fine particles A, which have a large particle diameter, do not migrate from the magnetic carrier particles to the toner or the internal components of the developer due to the influence of mechanical loads in the developer. Therefore, even when the toner is used for a long period of time, the toner can exhibit a high spacer effect and maintain the charge for a long period of time.

[0020] Furthermore, the number average particle size of the primary particles of the silica fine particles A is preferably 80 nm or more and 150 nm or less, from the viewpoint of a higher spacer effect and maintaining the charge for a longer period of time.

[0021] In addition, the coverage of the surface of the magnetic carrier particles with the silica fine particles A is 1.0% by area or more and 15.0% by area or less. When the coverage of the surface of the magnetic carrier particles with the silica fine particles A is 1.0% by area or more, the charging uniformity of each toner particle can be improved. When the coverage of the surface of the magnetic carrier particles with the silica fine particles A is 15.0% by area or less, there is no excessive charge leakage from the surface of the magnetic carrier particles due to the silica fine particles A, and the charge retention of the toner particles can be obtained. In order to obtain a desired coverage of the silica fine particles A, it is preferable to mix the magnetic carrier particles with the silica fine particles A, adjust the coverage of the surface of the magnetic carrier particles with the silica fine particles A to 1.0% by area or more and 16.5% by area or less, and then mix the mixture with the toner. In addition, the desired coverage of the silica fine particles A can be obtained by adjusting the number average particle size, the amount added, and the mixing conditions of the silica fine particles A used.

[0022] Next, preferred embodiments will be described. <Silica fine particles A> The silica fine particles A used in the present invention are particles mainly composed of silica (SiO2) and can be produced by known production methods such as a combustion method, a melting method, hydrothermal synthesis, etc. Among them, silica fine particles A produced by a combustion method or a melting method are preferred in order to further enhance the effect of suppressing charge relaxation in a high-temperature and high-humidity environment and from the viewpoint of having high resistance and being less susceptible to the effects of humidity.

[0023] The combustion method is a method in which the siloxane gas generated by vaporizing a siloxane compound is introduced into a burner together with a carrier gas such as nitrogen, and the siloxane gas is diffused and mixed with a combustion-supporting gas such as oxygen to generate silica fine particles.Another embodiment of the combustion method is a method in which silicon tetrachloride is burned at high temperature together with a mixed gas of oxygen, hydrogen, and a dilution gas such as nitrogen to generate silica fine particles (fumed silica).

[0024] The melting method is a method in which a slurry of metal silicone fine particles is sprayed into a flame and spheroidized while undergoing an oxidation reaction to obtain silica particles.

[0025] In the present invention, from the viewpoint of controllability of the number average particle diameter of the primary particles of the silica microparticles A and controllability of the charge decay constant α in an environment of 23°C and 50% RH, a combustion method in which siloxane gas is combusted to generate silica microparticles is cited as a preferred example. Examples of the siloxane compound include hexamethylcyclotrisiloxane and octamethylcyclotetrasiloxane.

[0026] In the present invention, the charge decay constant α of silica fine particles A in a 23°C, 50% RH environment can be controlled by the content of iron atoms contained in silica fine particles A. In order to control the charge decay constant α, it is preferable that silica fine particles A further contain aluminum atoms. The content of iron atoms contained in silica fine particles A is preferably 20 ppm or more and 2000 ppm or less. The content of aluminum atoms contained in silica fine particles A is preferably 200 ppm or more and 2000 ppm or less.

[0027] As a method for incorporating these metal atoms into the silica fine particles A, it is possible to incorporate them by adjusting the purity of the siloxane compound.

[0028] Furthermore, the silica fine particles A are preferably surface-treated with a silane coupling agent, silicone oil or the like to be made hydrophobic. The silane coupling agent is preferably hexamethyldisilazane (HMDS). As the silicone oil, dimethyl silicone oil is preferred.

[0029] The method of surface treatment with silane coupling agent is not particularly limited, and known methods can be used. For example, a method of stirring silica fine particles A to make it cloud-like, and then spraying vaporized silane coupling agent, or a method of contacting the vapor of silane coupling agent with the cloud-like silica fine particles A is common.

[0030] In the above-mentioned surface treatment with a silane coupling agent, it is preferable to use the silane coupling agent in an amount within the range of 1 to 80 parts by weight per 100 parts by weight of the silica fine particles A.

[0031] In the present invention, the silica fine particles A may be used alone in the magnetic carrier, or a plurality of types of silica fine particles A may be used in combination with other external additives.

[0032] <Magnetic carrier> As the magnetic carrier particles, there can be used ordinary magnetic carrier particles such as ferrite, magnetite, etc., or resin-coated carrier particles. In addition, there can also be used binder-type magnetic carrier core particles in which magnetic powder is dispersed in a resin.

[0033] Resin-coated carrier particles are composed of a magnetic carrier core and a resin coating layer that coats the surface of the magnetic carrier core. Examples of resins used in the resin coating layer include styrene-acrylic resins such as styrene-acrylic acid ester copolymers and styrene-methacrylic acid ester copolymers; acrylic resins such as acrylic acid ester copolymers and methacrylic acid ester copolymers; fluorine-containing resins such as polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymers, monochlorotrifluoroethylene polymers, and polyvinylidene fluoride; silicone resins; polyester resins; polyamide resins; polyvinyl butyral; and aminoacrylate resins. Other examples include ionomer resins and polyphenylene sulfide resins. These resins can be used alone or in combination.

[0034] The magnetic carrier contains silica fine particles A attached to the surface of the magnetic carrier particles. By adding silica fine particles A to the magnetic carrier particles and mixing them using a mixing device such as a V-type mixer, a Henschel mixer, or a Turbula mixer, a magnetic carrier having silica fine particles A attached to the surface of the magnetic carrier particles is obtained.

[0035] <Other external additives for magnetic carriers> To the magnetic carrier particles of the present invention, external additives other than the silica fine particles A may be added in order to improve the flowability of the magnetic carrier particles and adjust the triboelectric charging properties. As the external additive other than the silica fine particles A, inorganic fine particles such as silicon oxide (silica), aluminum oxide (alumina), strontium titanate, titanium oxide (titania), and calcium carbonate are preferable.

[0036] <Developer> The starter two-component developer and the refill two-component developer of the present invention are two-component developers in which a magnetic carrier and a toner are mixed. The mixing ratio of the magnetic carrier and the toner of the starter two-component developer that is initially installed in the developing machine is preferably such that the toner concentration of the starter two-component developer is 2% by mass or more and 15% by mass or less, more preferably 4% by mass or more and 13% by mass or less. In addition, as for the refill two-component developer that is replenished due to long-term use, the mixing ratio of the magnetic carrier and the toner is preferably such that the toner concentration of the refill two-component developer is 85% by mass or more and 98% by mass or less, more preferably 88% by mass or more and 95% by mass or less.

[0037] [Toner particles] <Binding resin> In the toner particles of the present invention, the following polymers can be used as the binder resin. Examples of suitable resins include homopolymers of styrene and its substituted derivatives, such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-based copolymers, such as styrene-p-chlorostyrene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-acrylic acid ester copolymer, and styrene-methacrylic acid ester copolymer; styrene-based copolymer resins, polyester resins, and hybrid resins in which polyester resins and vinyl resins are mixed or in which both are partially reacted; polyvinyl chloride, phenolic resins, naturally modified phenolic resins, naturally modified maleic acid resins, acrylic resins, methacrylic resins, polyvinyl acetate, silicone resins, polyester resins, polyurethanes, polyamide resins, furan resins, epoxy resins, xylene resins, polyethylene resins, and polypropylene resins. Among these, it is preferable to use polyester resin from the viewpoint of low-temperature fixability and chargeability of the toner.

[0038] <Coloring agent> The toner particles in the present invention may contain a colorant, such as a known yellow colorant, magenta colorant, cyan colorant, or black colorant.

[0039] Examples of black colorants include carbon black, and black colorants prepared by using a yellow colorant, a magenta colorant, and a cyan colorant.

[0040] Examples of color pigments for magenta toner include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinones, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds.Specific examples include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, and 81:1. , 83, 87, 88, 89, 9, 112, 114, 122, 123, 144, 146, 150, 163, 166, 169, 177, 184, 185, 202, 206, 207, 209, 220, 221, 238, 254, 269; CI Pigment Violet 19, CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0041] As the colorant, a pigment may be used alone, but a dye and a pigment may be used in combination to improve the color clarity.

[0042] Dyes for magenta toner include the following: oil-soluble dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121, CI Disperse Red 9, CI Solvent Violet 8, 13, 14, 21, 27, and CI Disperse Violet 1; basic dyes such as CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40, and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, and 28.

[0043] Examples of color pigments for cyan toners include: CI Pigment Blue 1, 2, 3, 7, 15:2, 15:3, 15:4, 16, 17, 60, 62, 66; CI Bat Blue 6, CI Acid Blue 45, copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton, and the like.

[0044] Examples of yellow coloring pigments include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal compounds, methine compounds, and allylamide compounds. Specific examples include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 155, 168, 174, 180, 181, 185, 191; CI Bat Yellow 1, 3, and 20. In addition, dyes such as CI Direct Green 6, CI Basic Green 4, CI Basic Green 6, and Solvent Yellow 162 can also be used.

[0045] The amount of the colorant used is 0.1 to 30 parts by mass, preferably 0.5 to 20 parts by mass, and more preferably 3 to 15 parts by mass, relative to 100 parts by mass of the binder resin.

[0046] In addition, it is preferable to use a toner particle in which a colorant is mixed in advance with a binder resin to form a master batch, and the colorant can be well dispersed in the toner particle by melting and kneading the colorant master batch and other raw materials (binder resin, wax, etc.).

[0047] <Release agent> If necessary, one or more kinds of releasing agents may be contained in the toner particles. Examples of the releasing agents include the following. Aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, and paraffin wax are preferably used. Other examples include oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax, or block copolymers thereof; waxes mainly composed of fatty acid esters such as carnauba wax, sazol wax, and montan acid ester wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax.

[0048] The amount of the release agent is preferably 0.1 to 20 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the binder resin.

[0049] The melting point of the release agent, which is determined by the maximum endothermic peak temperature during temperature rise measured by a differential scanning calorimeter (DSC), is preferably 65°C to 130°C. More preferably, it is 80°C to 125°C. If the melting point is 65°C or higher, the viscosity of the toner falls within an appropriate range, and toner adhesion to the photoreceptor is unlikely to occur. If the melting point is 130°C or lower, low-temperature fixability is good.

[0050] <Other external additives> To the toner of the present invention, silica fine particles A or other external additives may be added in order to improve the fluidity of the toner and adjust the triboelectric charging property. As the external additive other than the silica fine particles A, inorganic fine particles such as silicon oxide (silica), aluminum oxide (alumina), strontium titanate, titanium oxide (titania), calcium carbonate, etc. are preferable.

[0051] Next, an image forming apparatus equipped with a developing device using a two-component developer will be described as an example, but the present invention is not limited to this.

[0052] <Image forming method> (Image forming device) An image forming method will be described using an example of an image forming apparatus shown in FIG. 1. An electrostatic latent image carrier 1 rotates in the direction of the arrow in the figure. The electrostatic latent image carrier 1 is charged by a charger 2, which is a charging means. An electrostatic latent image is formed by exposing the surface of the charged electrostatic latent image carrier 1 to light by an exposure device 3, which is an electrostatic latent image forming means. The developing device 4 has a developing container 5 that contains a starter two-component developer, and the developer carrier 6 is arranged in a rotatable state, and the developer carrier 6 contains a magnet 7 as a magnetic field generating means. At least one of the magnets 7 is arranged so as to face the electrostatic latent image carrier 1.

[0053] The starter two-component developer is held on the developer carrier 6 by the magnetic field of a magnet 7, and the amount of the two-component developer is regulated by a regulating member 8, and the developer is transported to a development section facing the electrostatic latent image carrier 1. In the developing section, a magnetic field generated by a magnet 7 forms a magnetic brush. Then, a developing bias consisting of an alternating electric field superimposed on a direct current electric field is applied, so that the electrostatic latent image is visualized as a toner image on the electrostatic latent image carrier 1. The toner image formed on the electrostatic latent image carrier 1 is electrostatically transferred to a recording medium 12 by a transfer charger 11. When the amount of starter two-component developer in the developing container 5 decreases due to long-term use, the image forming method is such that refill two-component developer is replenished from the hopper 17 as needed.

[0054] 2, the electrostatic latent image may be transferred from the electrostatic latent image carrier 1 to an intermediate transfer body 9, and then electrostatically transferred to a transfer material (recording medium) 12. The recording medium 12 is then transported to a fixing device 13, where the toner is fixed onto the recording medium 12 by applying heat and pressure. The recording medium 12 is then discharged outside the apparatus as an output image. After the transfer process, the toner remaining on the electrostatic latent image carrier 1 is removed by a cleaner 15. Thereafter, the electrostatic latent image carrier 1 cleaned by the cleaner 15 is electrically initialized by light irradiation from the pre-exposure 16, and the above image forming operation is repeated.

[0055] FIG. 2 shows an example of a full-color image forming apparatus. The arrangement of image forming units such as K, Y, C, and M in the figure, and the arrows indicating the rotation directions are not limited to those shown here. Incidentally, K stands for black, Y for yellow, C for cyan, and M for magenta. In Fig. 2, electrostatic latent image carriers 1K, 1Y, 1C, and 1M rotate in the direction of the arrows. Each electrostatic latent image carrier 1 is charged by chargers 2K, 2Y, 2C, and 2M, which are charging means, and the surface of each charged electrostatic latent image carrier 1 is exposed by exposure devices 3K, 3Y, 3C, and 3M, which are electrostatic latent image forming means, to form an electrostatic latent image.

[0056] Thereafter, the electrostatic latent image is visualized as a toner image by starter two-component developer carried on developer carriers 6K, 6Y, 6C, and 6M provided in developing devices 4K, 4Y, 4C, and 4M, which are developing means. The toner image is then transferred to intermediate transfer body 9 by intermediate transfer chargers 10K, 10Y, 10C, and 10M, which are transferring means. The toner image is then transferred to recording medium 12 by transfer charger 11, which is also transferring means, and recording medium 12 is fixed by heat and pressure by fixing device 13, which is fixing means, and output as an image. An intermediate transfer body cleaner 14, which is a cleaning member for intermediate transfer body 9, collects the toner remaining after transfer, etc.

[0057] Specifically, the development method is preferably such that an AC voltage is applied to the developer carrier 6 to form an alternating electric field in the development area while the magnetic brush is in contact with the electrostatic latent image carrier 1. The distance (SD distance) between the developer carrier (developing sleeve) 6 and the drum of the electrostatic latent image carrier 1 is preferably 100 μm or more and 1000 μm or less in order to prevent carrier adhesion and improve dot reproducibility in image formation. When the SD distance is 100 μm or more, the supply of developer is sufficient and the image density is good. When the SD distance is 1000 μm or less, the magnetic field lines from the magnet 7 are less likely to spread, the density of the magnetic brush is good, and the dot reproducibility is improved. In addition, the force binding the carrier is increased, and carrier adhesion can be suppressed.

[0058] The peak-to-peak voltage (Vpp) of the alternating electric field is preferably 300 V or more and 3000 V or less, more preferably 500 V or more and 1800 V or less. The frequency of the alternating electric field is preferably 500 Hz or more and 10000 Hz or less, more preferably 1000 Hz or more and 7000 Hz or less, and can be appropriately selected depending on the process.

[0059] In this case, the waveform of the AC bias for forming the AC electric field may be a triangular wave, a square wave, a sine wave, or a waveform with a changed duty ratio. In order to respond to changes in the toner image formation speed, it is preferable to apply a development bias voltage having a discontinuous AC bias voltage (intermittent AC superimposed voltage) to the developer carrier for development. If the applied voltage is 300V or more, sufficient image density is easily obtained, and fogging toner in non-image areas is easily collected. Also, if it is 3000V or less, disturbance of the latent image through the magnetic brush is unlikely to occur, and good image quality is obtained.

[0060] Next, the methods for measuring the various physical properties related to the present invention will be described. <Method for measuring the number-average particle size of primary particles of silica fine particles A> The number average particle size of the primary particles of silica fine particles A is calculated from an image of the silica fine particles A on the surface of the magnetic carrier particles taken with a field emission scanning electron microscope (product name: S-4800, manufactured by Hitachi High-Technologies Corporation) (hereinafter also referred to as "S-4800") The image taking conditions are as follows.

[0061] (1) Sample preparation Apply a thin layer of conductive paste to a sample stage (aluminum sample stage 15 mm x 6 mm), then spray magnetic carrier particles onto the paste. Then, use air to remove excess magnetic carrier particles from the sample stage and allow to dry thoroughly. Set the sample stage in the sample holder and adjust the sample stage height to 36 mm using the sample height gauge.

[0062] (2) S-4800 observation condition setting The number average diameter is calculated using an image obtained by observing the backscattered electron image of the S-4800. Pour liquid nitrogen into the anti-contamination trap attached to the S-4800 body until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2 and execute it. Check that the emission current due to flushing is 20 to 40 μA. Insert the specimen holder into the specimen chamber of the S-4800 body. Press [Origin] on the control panel to move the specimen holder to the observation position. Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [1.1kV] and the emission current to [20μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Upper (U)] and [+BSE], and select [LA100] in the selection box to the right of [+BSE] to set the mode to observation with backscattered electron images. In the same [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [4.5mm]. Press the [ON] button in the accelerating voltage display of the control panel to apply the accelerating voltage.

[0063] (3) Focus adjustment Rotate the focus knob [COARSE] on the operation panel, and adjust the aperture alignment once the image is in focus to a certain extent. Click [Align] on the control panel to display the alignment dialog, and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles. Next, select [Aperture], and rotate the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or to minimize its movement. Close the aperture dialog, and adjust the focus using autofocus. After that, set the magnification to 80,000 (80k), and adjust the focus using the focus knob and STIGMA / ALIGNMENT knob in the same way as above, and then adjust the focus using autofocus again. Repeat this operation to adjust the focus. Here, if the inclination angle of the observation surface is large, the measurement accuracy of the coverage rate is likely to be low, so when adjusting the focus, select an observation surface with as little surface inclination as possible for analysis by selecting one that can simultaneously bring the entire observation surface into focus.

[0064] (4) Image storage Adjust the brightness in ABC mode, take a photo with a size of 640 x 480 pixels, and save it. Use this image file to perform the following analysis. Take one photo for each magnetic carrier particle, and obtain images of at least 25 particles for each magnetic carrier particle.

[0065] (5) Image analysis The particle diameters of at least 300 silica fine particles A on the surface of the magnetic carrier particle are measured to determine the number-average particle diameter. In the present invention, the number-average diameter of the silica fine particles A is calculated by binarizing the image obtained by the above-mentioned method using image analysis software Image-Pro Plus ver.5.0.

[0066] <Method for measuring the charge decay constant α of silica fine particles A> The charge decay constant α of the external additive used in each of the magnetic carrier and toner is calculated using an attachment of an electrostatic diffusion rate measuring device (product name: NS-D100, manufactured by Nano Seeds Corporation) according to a method in accordance with JIS C 61340-2-1. Setting the sample Put the external additive into an aluminum sample pan (with an inner diameter of 10 mm and a recess of 1 mm depth). Then, use a flat plate to push the external additive in from above until it is leveled and filled. ·Environmental neglect The sample pan filled with the external additive is placed on an aluminum sample cell and left to stand for 12 hours or more in an environment with a temperature of 23°C and a relative humidity of 50%. Electrostatic charge The grounded sample cell is placed in the measuring instrument, and the sample is charged by corona discharge for 0.1 seconds. Potential measurement The surface potential is measured for 1800 seconds immediately after the corona discharge ends. The surface potential at the start of the measurement is set as the initial surface potential V0, and the charge decay constant α is calculated from the change in surface potential up to 1800 seconds according to the following formula. ln(Vt / V0)=-αt(1 / 2) (In the above formula, V represents the surface potential (V), Vt represents the surface potential (V) after t seconds, V0 represents the initial surface potential (V), α represents the charge decay constant (1 / s(1 / 2)), and t represents the decay time (seconds).)

[0067] <Method for measuring the coverage of the surface of magnetic carrier particles with silica fine particles A> The coverage rate of the silica fine particles A on the surface of the magnetic carrier particles is measured by calculation from an image of the silica fine particles A on the surface of the magnetic carrier particles taken with a field emission scanning electron microscope (product name: S-4800, manufactured by Hitachi High-Technologies Corporation). First, 20 magnetic carrier surface images taken with the S-4800 are randomly sampled. The image information is binarized using image analysis software (product name: Image-Pro Plus ver.5.0, manufactured by Nippon Roper Co., Ltd.) by utilizing the difference in brightness between the surface of the magnetic carrier particle and the silica fine particle A. This binarization separates the area of ​​the silica fine particle A, SSiO2, from the area of ​​the magnetic carrier particle (including the area of ​​the silica fine particle A portion), SCarrier. The coverage (area %) of the magnetic carrier particles by the silica fine particles A, σSiO2, is calculated by the following formula. σSiO2(area%)=SSiO2 / SCarrier×100

[0068] <Separation of silica fine particles A from magnetic carrier> As a method for separating the silica fine particles A from the magnetic carrier, for example, the following method can be used. Put 30 mL of ion-exchanged water into a 100 mL flat-bottom glass beaker. Add 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made from nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries) diluted 3 times with ion-exchanged water as a dispersant to prepare the Contaminon N solution. Prepare an ultrasonic disperser (product name: Ultrasonic Dispension System Tetra150, manufactured by Nikkaki Bios Co., Ltd.) with an electrical output of 120 W and equipped with two oscillators with an oscillation frequency of 50 kHz, with the phase shift of 180 degrees. Place 3.3 L of ion-exchanged water in the water tank of the ultrasonic disperser, and add 2 mL of Contaminon N to this water tank. Place the beaker containing the Contaminon N solution in the beaker fixing hole of the ultrasonic disperser and operate the ultrasonic disperser. Then, adjust the height of the beaker so that the resonance state of the electrolyte solution surface in the beaker is maximized. In a beaker containing the Contaminon N solution, 1.0 g of magnetic carrier is added and dispersed while ultrasonic waves are irradiated into the electrolyte solution. The ultrasonic dispersion process is continued for 30 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be between 10℃ and 40℃. After that, a magnet is brought close to the beaker containing the magnetic carrier, and the carrier is attracted through the beaker. In this state, the supernatant liquid (Contaminon N solution) in the beaker is collected. The collected supernatant liquid is filtered, and the solid content is washed with 5 g of ion-exchanged water to obtain silica fine particles A. EXAMPLES

[0069] The present invention will be specifically described below based on examples. However, the present invention is not limited to these examples. In addition, all parts are by weight unless otherwise specified.

[0070] <Production Example of Silica Fine Particle A1> Silica fine particles A1 were produced by a diffusion combustion method as follows. In producing silica microparticles A1, a double-tube hydrocarbon-oxygen mixed burner in which an inner flame and an outer flame are formed was used as the combustion furnace. This burner is configured so that a two-fluid nozzle for injecting slurry is grounded in the center of the burner, and the raw material silicon compound is introduced. In addition, a flammable hydrocarbon-oxygen gas is injected from the periphery of the two-fluid nozzle, forming an inner flame and an outer flame, which are a reducing atmosphere. The atmosphere, temperature, and flame length can be adjusted by controlling the amount and flow rate of the flammable gas and oxygen. In the flame, silica fine particles are generated from the raw silicon compound, and the silica fine particles can be fused until they reach a desired particle size. After that, they are cooled and the generated silica fine particles are collected by a bag filter or the like to obtain silica fine particles A having a desired particle size.

[0071] As the silicon compound raw material, hexamethylcyclotrisiloxane containing 180 ppm of iron atoms and 600 ppm of aluminum atoms was used to produce silica fine particles. Next, 100 parts by mass of the obtained silica fine particles were subjected to a surface treatment using 3.9 parts by mass of hexamethyldisilazane to obtain silica fine particles A1.

[0072] The number average particle size of the primary particles of the obtained silica fine particles A1 is shown in Table 1. Table 1 also shows the iron content, aluminum content, and charge decay constant α of the silica fine particles A1 in an environment of 23° C. and 50% RH.

[0073] <Production Examples of Silica Particles A2 to A14> In the production example of silica fine particles A1, the number average particle diameter of the primary particles and the iron content and aluminum content of hexamethylcyclotrisiloxane were changed to obtain silica fine particles A2 to 14. The number average particle diameter of the primary particles, the iron content, the aluminum content, and the charge decay constant α of each silica fine particle A are shown in Table 1.

[0074] [Table 1]

[0075] <Production Example of Magnetic Carrier Particles 1> ·Fe2O363.2 parts ·MnCO329.0 parts ·Mg(OH)26.6 parts ·SrCO31.2 parts The ferrite raw materials were weighed so that the above materials had the above composition ratio. The mixture was then ground and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch. The ground material was then made into pellets of approximately 1 mm square in a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse particles, and then through a vibrating sieve with 0.5 mm openings to remove fine particles, and then fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the resulting calcined ferrite was as follows: (MnO)a(MgO)b(SrO)c(Fe2O3)d In the above formula, a = 0.257, b = 0.117, c = 0.007, d = 0.393

[0076] The obtained calcined ferrite was crushed to about 0.3 mm using a crusher, and then 30 parts of water was added to 100 parts of the calcined ferrite and crushed in a wet ball mill using zirconia beads with a diameter of 1 / 8 inch for 1 hour. The obtained slurry was further crushed in a wet ball mill using alumina beads with a diameter of 1 / 16 inch for 4 hours to obtain a ferrite slurry (finely crushed calcined ferrite). To the obtained ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 2.0 parts of polyvinyl alcohol as a binder were added per 100 parts of calcined ferrite, and the mixture was granulated into spherical particles using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.). After adjusting the particle size of the obtained spherical particles, the mixture was heated at 650°C for 2 hours using a rotary kiln to remove the organic components of the dispersant and binder.

[0077] In order to control the firing atmosphere, the material was heated from room temperature to 1300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at 1150°C for 4 hours. The material was then cooled to 60°C over a period of 4 hours, returned from the nitrogen atmosphere to the air, and removed at a temperature of 40°C or less. After crushing the agglomerated particles, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic carrier cores 1 having a volume distribution standard 50% particle size (D50) of 36.0 μm.

[0078] <Preparation of Coating Resin 1> Cyclohexyl methacrylate monomer 26.8% by mass Methyl methacrylate monomer 0.2% by mass Methyl methacrylate macromonomer 8.4% by mass (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene 31.3% by mass Methyl ethyl ketone 31.3% by mass Azobisisobutyronitrile 2.0% by mass Among the above materials, cyclohexyl methacrylate monomer, methyl methacrylate monomer, methyl methacrylate macromonomer, toluene, and methyl ethyl ketone were mixed in a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer. After introducing nitrogen gas into the separable flask to create a sufficient nitrogen atmosphere, the flask was heated to 80°C, and azobisisobutyronitrile was added and refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction mixture to precipitate the copolymer. The precipitate was separated by filtration and then dried in vacuum to obtain a resin. Next, 30 parts of the obtained resin was dissolved in a mixed solvent of 40 parts of toluene and 30 parts of methyl ethyl ketone to obtain a resin solution 1 (resin solid content concentration: 30% by mass).

[0079] <Preparation of coating resin solution 1> ·Resin solution 1 (resin solid content concentration 30%) 33.3% by mass Toluene 66.4% by mass Carbon black (Regal 330; Cabot Corporation) 0.3% by mass (Number average particle size of primary particles: 25 nm, Nitrogen adsorption specific surface area: 94 m 2 / g, DBP oil absorption: 75mL / 100g) The above materials were placed in a paint shaker and dispersed for 1 hour using zirconia beads having a diameter of 0.5 mm. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.

[0080] <Production Example of Resin-Coated Carrier Particles 1> The coating resin solution 1 and the magnetic carrier particles 1 were charged into a vacuum degassing kneader maintained at room temperature. At this time, the coating resin solution 1 was charged so that the resin component was 2.5 parts per 100 parts of the magnetic carrier particles 1. After adding the coating resin solution 1 and the magnetic carrier particles 1, the mixture was stirred for 15 minutes at a rotation speed of 30 rpm. After a certain amount of the solvent (80% by mass) had evaporated, the mixture was heated to 80°C while mixing under reduced pressure, and the solvent was distilled off over 2 hours before being cooled. The obtained magnetic carrier was subjected to magnetic separation to separate out low magnetic particles, which were then passed through a sieve with openings of 70 μm and classified with an air classifier to obtain resin-coated carrier particles 1 having a volume distribution-based 50% particle size (D50) of 38.4 μm.

[0081] <Production Example of Magnetic Carrier 1-1> 100 parts of resin-coated carrier particles 1 and 0.05 parts of silica fine particles A1 were placed in a Turbula shaker and stirred for 10 minutes to obtain magnetic carrier 1-1. Table 2 shows the coverage of the surfaces of the resin-coated carrier particles 1 of the obtained magnetic carrier 1-1 with the silica fine particles A1.

[0082] <Production Examples of Magnetic Carriers 1-2 to 1-14> As shown in Table 2, magnetic carriers 1-2 to 1-14 were obtained in the same manner as in the production example of magnetic carrier 1-1, except that the amounts of silica fine particles A1 to A14 added were changed. Table 2 shows the coverage of the silica fine particles A2 to A14 on the surface of the resin-coated carrier particles 1 of the obtained magnetic carriers 1-2 to 1-14.

[0083] [Table 2]

[0084] <Production Example of Polyester Resin L> 76.9 parts (0.167 mol) of polyoxypropylene (2.2)-2,2-bis (4-hydroxyphenyl) propane, 25 parts (0.145 mol) of terephthalic acid, 8.0 parts (0.054 mol) of adipic acid, and 0.5 parts of titanium tetrabutoxide were placed in a 4-liter 4-neck glass flask, and a thermometer, a stirring rod, a condenser, and a nitrogen inlet tube were attached and placed in a mantle heater. Next, the flask was substituted with nitrogen gas, and the temperature was gradually raised while stirring, and the mixture was reacted for 4 hours while stirring at a temperature of 200 ° C. Then, 1.2 parts (0.006 mol) of trimellitic anhydride was added and reacted at 180 ° C. for 1 hour to obtain polyester resin L. The acid value of this polyester resin L was 5 mgKOH / g, the hydroxyl value was 65 mgKOH / g, and the molecular weight by GPC was weight average molecular weight (Mw) 8,000, number average molecular weight (Mn) 3,500, peak molecular weight (Mp) 5,700, and softening point 90°C.

[0085] <Production Example of Polyester Resin H> 71.3 parts (0.155 mol) of polyoxypropylene (2.2)-2,2-bis (4-hydroxyphenyl) propane, 24.1 parts (0.145 mol) of terephthalic acid, and 0.6 parts of titanium tetrabutoxide were placed in a 4-liter glass four-neck flask, and a thermometer, a stirring rod, a condenser, and a nitrogen inlet tube were attached and placed in a mantle heater. Next, the flask was purged with nitrogen gas, and the temperature was gradually raised while stirring, and the mixture was reacted for 2 hours while stirring at a temperature of 200°C. Then, 5.8 parts (0.030 mol%) of trimellitic anhydride was added, and the mixture was reacted at 180°C for 10 hours to obtain an amorphous polyester resin H. The molecular weight of this polyester resin H measured by GPC was a weight average molecular weight (Mw) of 200,000, a number average molecular weight (Mn) of 5,500, a peak molecular weight (Mp) of 13,500, and a softening point of 150°C.

[0086] <Toner 1 Manufacturing Example> Polyester resin L 75.00 parts Polyester resin H 25.00 parts CI Pigment Blue 15:3 5.7 parts 0.1 parts of 3,5-di-t-butylsalicylic acid aluminum compound Normal paraffin wax (melting point: 90°C) 5 parts The above materials were premixed in a Henschel mixer (product name: FM-75, manufactured by Mitsui Mining Co., Ltd.), and then melt-kneaded at 160° C. using a twin-screw kneading extruder (product name: PCM-30, manufactured by Ikegai Co., Ltd.). The obtained kneaded product was cooled, coarsely pulverized to 1 mm or less using a hammer mill, and then finely pulverized using a mechanical pulverizer (product name: T-250, manufactured by Turbo Kogyo Co., Ltd.). The resulting finely pulverized product was classified using a Faculty (product name: F-300, manufactured by Hosokawa Micron Corp.) The operating conditions were a classification rotor rotation speed of 11,000 rpm and a dispersion rotor rotation speed of 7,200 rpm. In this way, negatively triboelectrically charged toner particles 1 having a weight average particle size (D4) of 6.2 μm were obtained. Next, 100 parts of toner particles Silica fine particles A1 2.5 parts The raw materials shown in the above recipe were mixed using a Henschel mixer (product name: FM-10C, manufactured by Nippon Coke Co., Ltd.) at a rotation speed of 67 s-1 (4000 rpm) for a rotation time of 2 min, and then sieved through a mesh with 150 μm openings to obtain toner 1. The obtained toner 1 is shown in Table 3.

[0087] <Production Examples of Toners 2 to 14> Toners 2 to 14 were obtained in the same manner as in the production example of toner 1, except that the silica fine particles A1 were changed to silica fine particles A2 to A14 as shown in Table 3.

[0088] [Table 3]

[0089] <Production Examples of Developers 1 to 14> Magnetic carriers 1-1 to 1-14 and toners 1 to 14 shown in Table 4 were combined so that the toner concentration was 8%, and shaken in a shaker (product name: YS-8D type, manufactured by Yayoi Co., Ltd.) to prepare starter two-component developers 1 to 14 shown in Table 4. The vibration conditions of the shaker were 200 rpm and 2 minutes. In addition, in the combinations shown in Table 5, 90 parts of toner 1 to 14 were added to 10 parts of magnetic carrier 1-1 to 1-14, and mixed for 5 minutes in a V-type mixer in an environment of normal temperature and humidity of 23°C / 50% RH to obtain refill two-component developers 1 to 14 shown in Table 5.

[0090] [Table 4]

[0091] [Table 5]

[0092] <Example 1> The starter two-component developer 1 and the replenishment two-component developer 1 were used in combination to carry out the following evaluations.

[0093] [Image evaluation] The following evaluations were carried out using a color copier (product name: imagePRESS C850, manufactured by Canon Inc.) or a modified version thereof. Starter two-component developer 1 was charged into the developing device of the cyan color station of the image forming apparatus, and refill two-component developer 1 was set in the hopper, and transferability and fogging were evaluated before and after a paper feed durability test.

[0094] The transferability was evaluated by a paper feed durability test in a printing environment of 23°C temperature / 5% relative humidity (hereinafter referred to as "N / L" environment) using a test chart with an image ratio of 5% and printing 10,000 sheets. conditions: Paper: High whiteness paper (product name: GF-C081, manufactured by Canon Marketing Japan Inc.: A4 size, 81.4 g / m 2 ) Image formation speed: 85 sheets / min in full color Development conditions: The development contrast can be adjusted to any value and the automatic correction by the main unit has been prevented from operating.

[0095] For the fogging, a paper feed durability test was performed in a printing environment of 30°C temperature / 80% relative humidity (hereinafter referred to as "H / H" environment) using a test chart with an image ratio of 5%, and evaluating the image after printing 10,000 sheets. conditions: Paper Bleached paper (product name: CS-068, manufactured by Canon Marketing Japan Inc.: A4 size, 68.0 g / m 2 ) Image formation speed: 85 sheets / min in full color Development conditions: The development contrast can be adjusted to any value and the automatic correction by the main unit has been prevented from operating.

[0096] The evaluation items are shown below. <Evaluation of transferability before and after paper feed durability test> The following transferability evaluation was performed before (initial stage) the paper feed durability test, and immediately after the 10,000-sheet paper feed durability test, the following transferability evaluation was performed. A solid (FFh) image was formed and evaluated based on the following criteria. The toner remaining on the photoconductor after the primary transfer and the toner on the photoconductor before the primary transfer were taped and peeled off with transparent polyester adhesive tape. The peeled adhesive tape was applied to a piece of paper, and the density was measured with a spectrodensitometer (product name: 500 series, manufactured by X-Rite Corporation). The rate of change between the toner density on the photoconductor before the primary transfer and the toner density remaining on the photoconductor after the transfer was taken as the transfer efficiency, and was evaluated based on the following evaluation criteria. A rating of C or higher was determined to be indicative of the effects of the present invention. (Evaluation Criteria) A: Transfer efficiency: 90% or more B: Transfer efficiency: 85% or more but less than 90% C: Transfer efficiency: 80% or more but less than 85% D: Transfer efficiency: less than 80%

[0097] <Evaluation of fogging after paper feed durability test> A solid white (00h) image was formed and evaluated based on the following criteria. The measurement was performed using a reflectometer (product name: Model TC-6DS, manufactured by Tokyo Denshoku Co., Ltd.), and the worst reflection density of the white background after image formation was defined as Ds, the average reflection density of the recording medium before image formation was defined as Dr, and the fogging evaluation was performed using Dr-Ds as the fogging amount. Therefore, the smaller the value, the less fogging there is. (Evaluation Criteria) A: Fog amount is less than 1.00 B: Fog amount is 1.00 or more and less than 3.00 C: Fog amount is 3.00 or more

[0098] The above results are shown in Table 6. [Table 6]

[0099] <Example 2> 4 and 7, Reference Examples 5, 6, 8, 9 and Comparative Examples 1 to 5> The evaluation was carried out in the same manner as in Example 1, except that the starter two-component developer and the replenishment two-component developer were used in combination as shown in Table 6. The results are shown in Table 6. When all of the above evaluations were rated B or higher, it was determined that the effects of the present invention were achieved. [Explanation of symbols]

[0100] 1 Electrostatic latent image carrier 2 Charger 3 Exposure device 4. Developing Machine 5 Developing container 6 Developer carrier 7. Magnet 8 Regulatory Members 9 Intermediate transfer body 10 Intermediate transfer charger 11 Transfer charger 12 Transfer material (recording medium) 13 Fixing unit 14 Intermediate transfer body cleaner 15. Cleaner 16 Pre-exposure, 17 Hopper

Claims

1. A starter two-component developer containing a toner and a magnetic carrier, The magnetic carrier has magnetic carrier particles and silica fine particles A present on the surfaces of the magnetic carrier particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 150 nm or less, The silica fine particles A have a charge decay constant α of 0.0020 or more and 0.0100 or less 1800 seconds after being charged in an environment having a temperature of 23° C. and a relative humidity of 50%, a coverage of the surfaces of the magnetic carrier particles with the fine silica particles A of 1.0 area % or more and 5.2 area % or less;

2. 2. The starter two-component developer according to claim 1, wherein the toner comprises toner particles containing a binder resin and the silica fine particles A on the surfaces of the toner particles.

3. 3. The method for producing a starter two-component developer according to claim 1, wherein the magnetic carrier particles and the silica fine particles A are mixed together to cause the silica fine particles A to adhere to the surfaces of the magnetic carrier particles, and then the toner is electrostatically mixed and adhered to the surfaces of the magnetic carrier particles.

4. A replenishing two-component developer containing a toner and a magnetic carrier, The magnetic carrier has magnetic carrier particles and silica fine particles A present on the surfaces of the magnetic carrier particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 150 nm or less, The silica fine particles A have a charge decay constant α of 0.0020 or more and 0.0100 or less 1800 seconds after being charged in an environment having a temperature of 23° C. and a relative humidity of 50%, a coverage of the surfaces of the magnetic carrier particles with the fine silica particles A of 1.0 area % or more and 5.2 area % or less;

Citation Information

Patent Citations

  • Production of developer

    JP1993303235A

  • Multi-color toner, image formation device, and image formation method

    JP2017003659A

  • Two-component developer and image forming method using the same

    JP2019056771A

  • Toner external additive, toner, and toner core-shell fine particles

    JP2019148726A