Toner and image forming method

The toner composition with silica fine particles and iron atoms addresses the issue of decreased electrostatic binding force and fogging by maintaining toner fluidity and preventing contamination, effectively reducing white background fogging.

JP7560997B2Active Publication Date: 2024-10-03CANON KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020180037
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-10-03
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

Existing toner formulations, despite reducing white background image fogging, suffer from decreased electrostatic binding force leading to contamination and increased fine powder scattering, especially in high-temperature, high-humidity environments.

Method used

A toner composition with silica fine particles on the surface, containing iron atoms, having a specific particle size and charge decay constant, maintains electrostatic binding force and prevents aggregation, thereby reducing fogging.

Benefits of technology

The toner composition ensures toner fluidity, prevents contamination, and reduces fogging in white background areas by enhancing electrostatic binding force and scattering of fine powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560997000001
    Figure 0007560997000001
  • Figure 0007560997000002
    Figure 0007560997000002
Patent Text Reader

Abstract

To solve the problem in which: a reduction in particle diameter of toner causes scattering of fine powder from carrier on a developing roller and deterioration of contamination in a fuser and fogging on a white background of an image.SOLUTION: A toner has toner particles containing a binder resin and silica fine particles on the surface of each of the toner particles. The silica fine particles contain silica fine particles A containing iron atoms. Primary particles of the silica fine particles A have a number average particle diameter of 80 nm or more and 200 nm or less. After 1800 seconds from when the silica fine particles A are electrified in an environment of a temperature of 23°C and a relative humidity of 50%, the silica fine particles A have a charge attenuation constant α of 0.0005 or more and 0.0100 or less. The toner particles have a weight average particle diameter (D4) of 3.0 μm or more and 5.7 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, and a toner jet system, and also to an image forming method for the electrophotographic system. [Background technology]

[0002] As copiers and printers become more widespread, the performance required of toner is becoming more advanced. In recent years, a digital printing technology called print on demand (POD), which prints directly without going through a plate-making process, has been attracting attention. This print on demand (POD) has advantages over conventional offset printing because it can handle short-run printing, printing with different contents for each sheet (variable printing), and distributed printing. When considering the application of image formation methods using toner to the POD market, it is required to stably obtain print products with high image quality even when outputting a large amount at high speed over a long period of time in various environments. One of the factors that degrades the quality of print products is white background image fog. This is a phenomenon in which toner adheres to areas that should be white, resulting in a decrease in image quality. A method for suppressing this white background image fog is proposed in the following patent documents.

[0003] In Patent Document 1, angular alumina particles with particle diameters of 5 to 60 nm are used as a toner external additive, thereby reducing the amount of the external additive migrating to the carrier, maintaining charging properties, and suppressing fogging in the white areas of the image. In addition, in Patent Document 2, strontium titanate having a primary particle size of 30 nm or more and 100 nm or less, an average circularity of the primary particles of 0.82 or more and 0.94 or less, and a circularity of more than 0.92 which accounts for 84% of the cumulative primary particles, is used as an external toner additive, thereby achieving excellent dispersibility, maintaining electrostatic properties, and suppressing fogging in the white areas of the image. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-138990 A [Patent Document 2] JP 2019-28428 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, while the configurations of Patent Documents 1 and 2 have a certain effect in suppressing fogging in the white parts of an image, when the amount of toner and fine particles smaller than the average particle size of the toner increases due to the reduction in the particle size of the toner, the electrostatic binding force with the carrier decreases, which may result in contamination inside the developing unit and worsening fogging in the white parts of an image. [Means for solving the problem]

[0006] The above problems can be solved by using the following toner. A toner having toner particles containing a binder resin and silica fine particles on the surface of the toner particles, the silica fine particles having iron atoms 200ppm or more and 2000ppm or less The silica fine particles A contain silica fine particles A, the number average particle diameter of the primary particles being 80 nm or more and 200 nm or less, and the charge decay constant α after 1800 seconds from a charged state in an environment of a temperature of 23° C. and a relative humidity of 50% is 0.0005 or more and 0.0100 or less, The toner is characterized in that the weight average particle diameter (D4) of the toner particles is 3.0 μm or more and 5.7 μm or less. Effect of the Invention

[0007] According to the present invention, toner fluidity is maintained, toner aggregation is prevented, the electrostatic binding force between the fine powder and the carrier on the developing roller is improved, scattering of the fine powder is reduced, and fogging of the white background of the image can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the present invention will be described in detail. One embodiment of the present invention is a toner having toner particles containing a binder resin and silica fine particles on the surfaces of the toner particles, The silica fine particles contain iron atoms. 200ppm or more and 2000ppm or less Contains silica fine particles A, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 200 nm or less, and The charge decay constant α after 1800 seconds from the charged state in an environment with a temperature of 23°C and a relative humidity of 50% is 0.0005 or more and 0.0100 or less, The toner is characterized in that the weight average particle diameter (D4) of the toner particles is 3.0 μm or more and 5.7 μm or less.

[0009] In still another embodiment of the present invention, the weight average particle diameter (D4) of the toner is 3.0 μm or more and 5.3 μm or less. ,before The toner is characterized in that the fine silica particles A contain aluminum atoms in an amount of 200 ppm or more and 2000 ppm or less, and the fine silica particles A are silica particles that have been subjected to a hydrophobic treatment.

[0010] By using such a toner of the present invention, the above-mentioned problem of fogging in the white background of an image can be suppressed.

[0011] The present inventors presume as follows the mechanism by which the toner of the present invention functions to suppress fogging in the white background of an image.

[0012] The reason why contamination inside the developing device and fogging of the white background of an image occur is that the electrostatic binding force between the toner and the carrier is easily weakened.

[0013] In the present invention, it is considered that the following actions and effects are achieved by externally adding silica, which causes moderate charge decay, to toner particles. The toner to which silica, which causes moderate charge decay, is externally added has a fast charge rise and rapid charge exchange, so that the electrostatic binding force to the carrier increases, the toner and fine powder scatter, and the adhesion to the photoreceptor is eliminated, thereby suppressing contamination in the developing device and fogging of the white background of the image. In particular, when a small-particle toner is used in a high-temperature and high-humidity environment, the fine powder particle size tends to be small in many cases, the amount of fine powder tends to increase, and there is a concern of a decrease in charge, so the effect of using the toner of the present invention is more remarkable. As described above, by externally adding silica, which has a relatively large particle size and causes moderate charge decay, to toner fluidity can be ensured, and toner aggregation, contamination in the developing device, and fogging of the white background of the image can be prevented. Each component for achieving the object of the present invention will be described in detail below.

[0014] [Silica microparticles A] For the toner of the present invention, silica fine particles A having silicon oxide (silica) fine particles on the toner particle surface and having a number average particle size of primary particles of 80 nm to 200 nm can be preferably used. When the particle size of silica fine particles A is within the above range, the toner surface can maintain convex portions even when subjected to mechanical load in the developing device, the toner charge amount is less likely to decrease, and this contributes to reducing variations in reflection density and fogging in non-image areas.

[0015] The silica fine particles A used in the present invention are particles mainly composed of silica (i.e., SiO2), and can be produced by known production methods such as a combustion method, a melting method, hydrothermal synthesis, etc. Among them, in order to further enhance the effect of suppressing the charge relaxation in a high-temperature and high-humidity environment, and from the viewpoint of having high resistance and being less susceptible to the influence of humidity, silica fine particles A produced by the combustion method or the melting method are more preferable.

[0016] The combustion method is a method in which siloxane gas is produced by vaporizing siloxane compound, and introduced into a burner together with a carrier gas such as nitrogen, and the siloxane gas is diffused and mixed with a combustion-supporting gas such as oxygen, and then combusted to produce silica fine particles.Another combustion method is a method in which silicon tetrachloride is combusted at high temperature together with a mixed gas of oxygen, hydrogen, and a dilution gas such as nitrogen, to produce silica fine particles (fumed silica). The melting method is a method in which a slurry of metal silicon particles is sprayed into a flame to cause an oxidation reaction and to form the particles into spheroids, thereby obtaining silica particles.

[0017] In the present invention, from the viewpoint of controlling the number average particle size of the primary particles of the silica fine particles A to 80 nm or more and 200 nm or less and of incorporating iron atoms, a preferred example is the combustion method in which siloxane gas is combusted to produce silica fine particles. Examples of the siloxane compound include hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, etc. As a method for incorporating metal atoms into the silica fine particles A, it is possible to incorporate the metal atoms by adjusting the purity of the siloxane compound.

[0018] In the present invention, the silica fine particles A used in the present invention can be obtained by incorporating iron atoms, and preferably further aluminum atoms, into the silica fine particles A. There is a method for incorporating these metal atoms into the silica fine particles A while adjusting the purity of the siloxane compound. From the viewpoint of ensuring toner fluidity and preventing toner aggregation, contamination inside the developing device, and fogging of white areas of an image, it is preferable that the silica fine particles A contain iron atoms in an amount of 20 ppm or more and 2000 ppm or less, and aluminum atoms in an amount of 200 ppm or more and 2000 ppm or less. Furthermore, from the viewpoint of ensuring toner fluidity and preventing toner aggregation, contamination inside the developing device, and fogging of white areas of images, it is preferable that the charge decay constant α of the silica microparticles A after 1800 seconds from being charged in an environment of a temperature of 23°C and a relative humidity of 50% is 0.0005 or more and 0.0100 or less.

[0019] The silica fine particles may be surface-treated with a fatty acid or a metal salt thereof, a disilylamine compound, a halogenated silane compound, silicone oil, a silane coupling agent, a titanium coupling agent, or the like. These hydrophobic treatments are preferred in that they can improve the charge stability of the toner, particularly in high-temperature and high-humidity environments. Among these, n-octylethoxysilane treatment, 3,3,3-trifluoropropyltrimethoxysilane treatment, and hexamethyldisilazane treatment are preferred in that they further enhance the effect of charge stability.

[0020] The silica fine particles can be mixed with the toner particles using a known mixer such as a Henschel mixer, Mechano Hybrid (manufactured by Nippon Coke Corporation), a Super Mixer, or Nobilta (manufactured by Hosokawa Micron Corporation), and the device is not particularly limited. The amount of the silica fine particles added in the present invention is 0.5% by mass or more and 15% by mass or less based on the toner particles.

[0021] [Other external additives] In addition to the silica fine particles described above, the toner of the present invention may contain other inorganic fine powders as necessary to adjust the charge amount and fluidity. The inorganic fine powders may be added internally to the toner particles or may be mixed with the toner particles as an external additive. As the external additive, inorganic fine powders such as silica, titanium oxide, strontium titanate, aluminum oxide, magnesium oxide, and calcium carbonate are preferred. The inorganic fine powders may be hydrophobized with a hydrophobizing agent such as a stearic acid compound, a silane compound, silicone oil, or a mixture thereof.

[0022] The external additive is preferably used in an amount of 0.1 parts by mass to 10.0 parts by mass based on 100 parts by mass of toner particles. The toner particles and the external additive can be mixed using a known mixer such as a Henschel mixer.

[0023] [Binding resin] The binder resin used in the toner of the present invention is not particularly limited, and the following polymers or resins can be used.

[0024] For example, homopolymers of styrene and its substitutes such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-p-chlorostyrene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-acrylic acid ester copolymers, styrene-methacrylic acid ester copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl ethyl ether copolymers, styrene-vinyl methyl ketone copolymers, and styrene-acrylonitrile-indene copolymers; polyvinyl chloride, phenolic resins, naturally modified phenolic resins, naturally modified maleic acid resins, acrylic resins, methacrylic resins, polyvinyl acetate, silicone resins, polyester resins, polyurethanes, polyamide resins, furan resins, epoxy resins, xylene resins, polyvinyl butyral, terpene resins, coumarone-indene resins, and petroleum-based resins can be used.

[0025] Of these, it is preferable to use polyester resins from the viewpoints of low-temperature fixability and charge control.

[0026] The polyester resin preferably used in the present invention is a resin having a "polyester unit" in the binder resin chain. Specific examples of components constituting the polyester unit include divalent or higher alcohol monomer components and acid monomer components such as divalent or higher carboxylic acids, divalent or higher carboxylic acid anhydrides, and divalent or higher carboxylic acid esters.

[0027] Examples of the divalent or higher alcohol monomer component include the following: alkylene oxide adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(3.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(2.0)-polyoxyethylene(2.0)-2,2-bis(4-hydroxyphenyl)propane, and polyoxypropylene(6)-2,2-bis(4-hydroxyphenyl)propane, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, and 1,4-butanediol. , neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5-trihydroxymethylbenzene, etc.

[0028] Among these, the alcohol monomer component that is preferably used is an aromatic diol, and the alcohol monomer component that constitutes the polyester resin preferably contains the aromatic diol in a proportion of 80 mol % or more.

[0029] On the other hand, examples of the acid monomer components such as divalent or higher carboxylic acids, divalent or higher carboxylic acid anhydrides, and divalent or higher carboxylic acid esters include the following: aromatic dicarboxylic acids or anhydrides thereof, such as phthalic acid, isophthalic acid, and terephthalic acid; alkyl dicarboxylic acids or anhydrides thereof, such as succinic acid, adipic acid, sebacic acid, and azelaic acid; succinic acid or anhydrides thereof substituted with an alkyl or alkenyl group having 6 to 18 carbon atoms; and unsaturated dicarboxylic acids or anhydrides thereof, such as fumaric acid, maleic acid, and citraconic acid.

[0030] Among these, preferred acid monomer components are polyvalent carboxylic acids such as terephthalic acid, succinic acid, adipic acid, fumaric acid, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and anhydrides thereof.

[0031] The acid value of the polyester resin is preferably 20 mgKOH / g or less from the viewpoints of pigment dispersibility and triboelectric charge stability.

[0032] The acid value can be adjusted to the above range by adjusting the type and amount of monomers used in the resin. Specifically, the acid value can be controlled by adjusting the alcohol monomer component ratio / acid monomer component ratio and molecular weight during resin production. In addition, the acid value can be controlled by reacting the terminal alcohol with a polyacid monomer (e.g., trimellitic acid) after ester condensation polymerization.

[0033] [Coloring agent] When a full-color image is formed by developing with the toner of the present invention, a colorant is added to prepare color toners of black toner, magenta toner, cyan toner, and yellow toner for use. Examples of colorants that can be contained in the toner of the present invention include the following.

[0034] As the black colorant, carbon black is mainly used, and dyes and pigments may be added as necessary. In addition, a yellow colorant, a magenta colorant, and a cyan colorant may be used to tone the color black. As the colorant, a pigment may be used alone, but it is more preferable to use a dye and a pigment in combination to improve the clarity of the color image from the viewpoint of image quality of a full-color image.

[0035] Magenta colored pigments include: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 5.7:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0036] Magenta coloring dyes include: CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1, and other solvent dyes; CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28, and other basic dyes.

[0037] Cyan coloring pigments include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45; copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton. Cyan coloring dyes include CI Solvent Blue 70.

[0038] Yellow coloring pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65.73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20. Yellow coloring dyes include CI Solvent Yellow 162.

[0039] The colorant is preferably used in an amount of 0.1 parts by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0040] [Release agent: wax] Examples of the release agent used in the toner of the present invention include the following waxes. Hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes whose main component is fatty acid esters such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax.

[0041] Further examples include the following: saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, hexamethylene bis Saturated fatty acid bisamides such as stearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipic acid amide, and N,N'-dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'-distearyl isophthalic acid amide; fatty metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols, such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.

[0042] Among these waxes, from the viewpoint of improving low-temperature fixability and high-temperature offset resistance, preferred are hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax, and fatty acid ester waxes such as carnauba wax.

[0043] The content of the wax is preferably 1.0 part by mass or more and 15 parts by mass or less relative to 100 parts by mass of the binder resin. When the content of the wax is in this range, offset resistance at high temperatures can be efficiently exhibited.

[0044] From the viewpoint of achieving both storage stability and high-temperature offset resistance of the toner, it is preferable that the peak temperature of the maximum endothermic peak present in the temperature range of 30°C or more and 200°C or less in the endothermic curve upon temperature rise measured by a differential scanning calorimeter (DSC) is 50°C or more and 110°C or less.

[0045] [Wax dispersant] In order to improve the dispersibility of the wax in the binder resin, a resin having both a polarity site similar to that of the wax component and a polarity site similar to that of the resin may be added as a wax dispersant. Specifically, a styrene-acrylic resin graft-modified with a hydrocarbon compound is preferable.

[0046] The wax dispersant improves the charge retention of the toner by introducing a cyclic hydrocarbon group or an aromatic ring into the resin portion thereof, which is preferable because it suppresses the toner particles from reducing the charge assisting properties of the strontium titanate particles of the present invention.

[0047] [Charge control agent] The toner may contain a charge control agent as necessary. Any known charge control agent may be used as the charge control agent contained in the toner, but a metal compound of an aromatic carboxylic acid is particularly preferred, as it is colorless, the toner can be charged quickly, and a constant charge amount can be stably maintained.

[0048] Examples of negative charge control agents include the following: metal salicylate compounds, metal naphthoate compounds, metal dicarboxylate compounds, polymeric compounds having sulfonic acid or carboxylic acid on the side chain, polymeric compounds having sulfonate or sulfonate ester on the side chain, polymeric compounds having carboxylate or carboxylate ester on the side chain, boron compounds, urea compounds, silicon compounds, and calixarene. Examples of positive charge control agents include quaternary ammonium salts, polymeric compounds having the quaternary ammonium salt on the side chain, guanidine compounds, and imidazole compounds. The charge control agent may be added internally or externally to the toner particles. The amount of the charge control agent added is preferably 0.2 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the binder resin.

[0049] [Developer] The toner of the present invention can be used as a one-component developer, but in order to further improve dot reproducibility, it is preferable to mix it with a magnetic carrier and use it as a two-component developer. It is also preferable to use it as a two-component developer in order to obtain stable images over a long period of time.

[0050] As the magnetic carrier, the following known magnetic carriers can be used: surface-oxidized iron powder or unoxidized iron powder, metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, and rare earth elements, alloy particles thereof, oxide particles, magnetic materials such as ferrite, and magnetic material-dispersed resin carriers (so-called resin carriers) that contain a magnetic material and a binder resin that holds the magnetic material in a dispersed state.

[0051] When the toner of the present invention is mixed with a magnetic carrier to be used as a two-component developer, good results can be obtained by mixing the toner with the magnetic carrier in a ratio of 2% by mass to 15% by mass, preferably 4% by mass to 13% by mass, in terms of the toner concentration in the two-component developer.

[0052] [Manufacturing method] The method for producing the toner of the present invention is not particularly limited as long as it is a conventionally known toner production method such as an emulsion aggregation method, a melt kneading method, or a dissolution suspension method. From the viewpoint of improving the dispersibility of the raw materials, the melt kneading method is preferred.

[0053] The melt-kneading method is characterized in that a toner composition, which is a raw material for toner particles, is melt-kneaded and the resulting kneaded product is pulverized. An example of the production method will be described below.

[0054] In the raw material mixing process, the materials constituting the toner particles, such as polyester resin, release agent, colorant, and other components such as charge control agent as necessary, are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, and a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.).

[0055] Next, the mixed materials are melt-kneaded to disperse other raw materials in the binder resin. In the melt-kneading process, a batch-type kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of being capable of continuous production. For example, a KTK type twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM type twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. Furthermore, the resin composition obtained by melt-kneading may be rolled with a two-roller or the like, and cooled with water or the like in a cooling process.

[0056] The cooled resin composition is then pulverized to a desired particle size in a pulverization process. In the pulverization process, the resin composition is coarsely pulverized using a pulverizer such as a crusher, hammer mill, or feather mill, and then further pulverized using a fine pulverizer. Examples of fine pulverizers include the Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), Super Rotor (manufactured by Nisshin Engineering, Inc.), Turbo Mill (manufactured by Freund Turbo Corp.), and fine pulverizers using an air jet system.

[0057] Thereafter, as necessary, the mixture is classified using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nippon Steel Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), or a Faculty (manufactured by Hosokawa Micron Corporation) to obtain toner particles.

[0058] The weight average particle diameter of the toner particles is preferably 3.0 μm or more and 5.7 μm or less, since the effect of the external additive of the present invention can be fully obtained. Furthermore, the circularity of the toner particles may be increased by applying a mechanical impact force to the particles and performing a heat treatment using hot air or the like. In order to increase the opportunity for charge transfer between toner particles and the frictional sliding force between the toner particles and to increase the charge rise speed, the average circularity of the toner particles is preferably 0.962 or more and 0.972 or less.

[0059] The toner particles produced by the above-mentioned production method are mixed with selected external additives as required (external addition). Examples of mixing devices include a double cone mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, and a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.).

[0060] [Image forming method] The toner set having a color toner obtained by adding a colorant to the toner of the present invention and a black toner can be applied to a known image forming method. Specifically, the toner set can be suitably used in an image forming method including a step of charging an electrostatic image carrier, a step of forming an electrostatic image on the charged electrostatic image carrier, a step of developing the formed electrostatic image with a toner to form a toner image, a step of transferring the formed toner image to a transfer material, and a step of fixing the transferred toner image to the transfer material to form a fixed image.

[0061] The process of developing the electrostatic image formed with toner to form a toner image may include a process of forming a black toner image using a black toner of the toner set, and a process of forming a color toner image using a color toner of the toner set. If the color toners are three types, that is, a magenta toner, a cyan toner, and a yellow toner, the process for the color toners is three. In the embodiment described later, the cyan toner is used as a representative color toner, and an example of a toner set of a black toner and a cyan toner is shown.

[0062] [Method for measuring weight-average particle size (D4) of toner particles] The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube, and the accompanying dedicated software, "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), for setting measurement conditions and analyzing measurement data. The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels, and the measurement data is analyzed and calculated.

[0063] The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1 mass %, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.).

[0064] Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) Screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter, Inc.). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1,600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement.

[0065] In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0066] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube. (2) Approximately 30 mL of the aqueous electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and approximately 0.3 mL of the diluent described below is added as a dispersant. Dilution solution: "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water. (3) A specified amount of ion-exchanged water is placed in the water tank of the ultrasonic disperser described below, which has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 mL of the Conaminon N is added to this water tank. Ultrasonic disperser: "UltrAsonic Dispension System TetorA150" (manufactured by Nikkaki Bios Co., Ltd.) (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 15°C or higher and 40°C or lower. (6) Using a pipette, add the electrolytic solution (5) in which the toner has been dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4). EXAMPLES

[0067] The present invention will be described below with reference to Production Examples and Examples. <Manufacturing example of silica fine particles> For the production of silica, a combustion furnace was used with a hydrocarbon-oxygen mixed burner with a double-tube structure capable of forming an inner flame and an outer flame. A two-fluid nozzle for injecting slurry was grounded in the center of the burner, and the raw material silicon compound was introduced. A flammable hydrocarbon-oxygen gas was injected from around the two-fluid nozzle, forming an inner flame and an outer flame, which are reducing atmospheres. The atmosphere, temperature, flame length, etc. were adjusted by controlling the amount and flow rate of the flammable gas and oxygen. In the flame, silica fine particles were formed from the silicon compound, and were then fused until they reached the desired particle size. After cooling, the silica was collected using a bag filter or the like to obtain the product.

[0068] Silica is produced using hexamethylcyclotrisiloxane as a silicon compound raw material, and 100 parts by mass of the obtained inorganic fine particles are surface-treated using a surface treatment agent to obtain silica fine particles. As the surface treatment agent, fatty acid or its metal salt, disilylamine compound, halogenated silane compound, silicone oil, silane coupling agent, titanium coupling agent, etc. are preferable in terms of improving the charging stability of the toner. Among them, n-octylethoxysilane treatment, 3,3,3-trifluoropropyltrimethoxysilane treatment, and hexamethyldisilazane treatment are preferable in terms of improving the effect of charging stability.

[0069] <Examples of binder resin production> (Production example of polyester resin) Polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 80.0 mol% based on the total number of moles of polyhydric alcohol Polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 20.0 mol% based on the total number of moles of polyhydric alcohol Terephthalic acid: 80.0 mol% based on the total number of moles of polycarboxylic acids Trimellitic anhydride: 20.0 mol% based on the total number of moles of polycarboxylic acids The above materials were put into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Then, 1.5 parts by mass of tin 2-ethylhexanoate (esterification catalyst) was added as a catalyst to 100 parts by mass of the total amount of monomers. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised while stirring, and the reaction was carried out for 2.5 hours while stirring at a temperature of 200°C.

[0070] The pressure in the reaction vessel was then lowered to 8.3 kPA and maintained for 1 hour, after which the vessel was cooled to 180°C and reacted as is. After confirming that the softening point measured according to ASTM D36-86 reached 110°C, the temperature was lowered to stop the reaction. The softening point (Tm) of the resulting polyester resin 1 was 115°C.

[0071] <Production example of wax dispersant> In an autoclave reaction tank equipped with a thermometer and a stirrer, 300.0 parts by mass of xylene and 10.0 parts by mass of polypropylene (melting point 75°C) were placed and thoroughly dissolved, and after nitrogen replacement, a mixed solution of 73.0 parts by mass of styrene, 5.0 parts by mass of cyclohexyl methacrylate, 12.0 parts by mass of butyl acrylate, and 250.0 parts by mass of xylene was dropped at 180°C for 3 hours to polymerize. The mixture was further held at this temperature for 30 minutes to remove the solvent, and a wax dispersant was obtained.

[0072] <Toner manufacturing example> As a typical example of color toner, a production example of a cyan toner will be described below.

[0073] Polyester resin 100.0 parts by weight 0.1 parts by weight of 3,5-di-t-butylsalicylic acid aluminum compound Fischer-Tropsch wax (maximum endothermic peak temperature 90°C) 5.0 parts by mass Wax dispersant 6.5 parts by weight CI Pigment Blue 15:3 5.0 parts by weight The raw materials shown in the above recipe were mixed in a Henschel mixer (FM75J type, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Corporation) set at a temperature of 130°C and a barrel rotation speed of 200 rpm. The kneaded mixture was cooled and coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed using a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). Classification was then performed using a rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) to obtain toner particles. The operating conditions of the rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) were a classification rotor rotation speed of 50.0 s -1 The resulting toner particles had a weight average particle size (D4) of 4.9 μm.

[0074] To the obtained toner particles, 5.0% by mass of silica fine particles and 0.2% by mass of hydrophobic small-diameter silica fine particles with a primary average particle size of 10 nm that had been surface-treated with 10.0% by mass of hexamethyldisilazane were added, and the mixture was mixed in a Henschel mixer (FM75J type, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 15 s. -1 Mixing was performed with a rotation time of 10 minutes and a jacket temperature of 45°C.

[0075] After that, 3.0 mass% of strontium titanate and 0.8 mass% of hydrophobic small-diameter silica particles with a primary average particle size of 10 nm that had been surface-treated with 10.0 mass% of hexamethyldisilazane were added, and the mixture was rotated at a speed of 30 s. -1 After mixing at a rotation time of 4 minutes and a jacket temperature of 20° C., the mixture was passed through an ultrasonic vibration sieve with an opening of 54 μm to obtain Toner 1 having an average circularity of 0.967.

[0076] [Production of toners 2 to 22] In the manufacturing examples described above, the weight average particle size of the toner particles, the number average particle size of the toner external additive (silica), the charge decay constant, and the presence or absence of surface hydrophobic treatment were adjusted to be as shown in Table 1, and toners 2 to 22 were obtained in the same manner as in the manufacturing example of toner 1.

[0077] [Table 1]

[0078] <Manufacturing example of magnetic core particles> (Step 1: Weighing and mixing step) ·Fe2O362.7 parts by mass ·MnCO329.5 parts by mass ·Mg(OH)26.8 parts by mass ·SrCO31.0 parts by mass The ferrite raw materials were weighed so as to obtain the above composition ratio, and then crushed and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch.

[0079] Step 2 (Pre-firing): The obtained pulverized material was made into pellets of about 1 mm square using a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then passed through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then fired in a burner-type firing furnace at 1,000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the resulting calcined ferrite was as follows: (MnO) A (MgO) b (SrO) c (Fe2O3) d In the above formula, A = 0.25.7, b = 0.117, c = 0.007, and d = 0.393.

[0080] (Step 3: Crushing step) The obtained calcined ferrite was crushed to about 0.3 mm using a crusher, and then 30 parts by mass of water was added to 100 parts by mass of the calcined ferrite using zirconia beads with a diameter of 1 / 8 inch, and the mixture was crushed in a wet ball mill for 1 hour. The slurry was crushed for 4 hours in a wet ball mill using alumina beads with a diameter of 1 / 16 inch to obtain a ferrite slurry (finely crushed calcined ferrite).

[0081] (Process 4: Granulation process) To the ferrite slurry, 1.0 parts by mass of ammonium polycarboxylate as a dispersant and 2.0 parts by mass of polyvinyl alcohol as a binder were added per 100 parts by mass of the calcined ferrite. Then, the mixture was granulated into spherical particles using a spray dryer (manufacturer: Okawara Kakoki Co., Ltd.). After adjusting the particle size of the obtained particles, the mixture was heated in a rotary kiln at a temperature of 650°C for 2 hours to remove the organic components of the dispersant and binder.

[0082] (Step 5: Firing step) In order to control the firing atmosphere, the material was heated from room temperature to 1,300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at 1,150°C for 4 hours. The temperature was then lowered to 60°C over a period of 4 hours, and the material was returned from the nitrogen atmosphere to the air, and the fired material was removed at a temperature of 40°C or less.

[0083] (Step 6: Sorting step) After crushing the agglomerated particles of the fired material, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic core particles 1 with a volume distribution-based median diameter of 37.0 μm.

[0084] <Preparation of Coating Resin> Cyclohexyl methacrylate monomer 26.8% by mass Methyl methacrylate monomer 0.2% by mass Methyl methacrylate macromonomer 8.4% by mass (A macromonomer with a weight-average molecular weight of 5,000 and a methacryloyl group at one end) Toluene 31.3% by mass Methyl ethyl ketone 31.3% by mass Azobisisobutyronitrile 2.0% by mass Among the above materials, cyclohexyl methacrylate, methyl methacrylate, methyl methacrylate macromonomer, toluene, and methyl ethyl ketone were placed in a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer, and nitrogen gas was introduced to replace the inside of the system with nitrogen gas. After that, the temperature was raised to 80°C, azobisisobutyronitrile was added, and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction product to precipitate a copolymer, and the precipitate was filtered and then vacuum dried to obtain coating resin 1. The obtained coating resin 1 was dissolved in 30 parts by mass, 40 parts by mass of toluene, and 30 parts by mass of methyl ethyl ketone to obtain polymer solution 1 (solid content 30% by mass).

[0085] <Preparation of coating resin solution> ·Polymer solution 1 (resin solid content concentration 30%) 33.3% by mass Toluene 66.4% by mass Carbon black 0.3% by mass (Primary particle size 25 nm, nitrogen adsorption specific surface area 94 m 2 / g, DBP oil absorption 75mL / 100g) The above materials were dispersed for 1 hour using zirconia beads having a diameter of 0.5 mm in a paint shaker. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.

[0086] [Magnetic carrier manufacturing] (Resin coating process) Coating resin solution 1 was added to a vacuum degassing kneader maintained at room temperature so that the resin component was 2.5 parts by mass per 100 parts by mass of magnetic core particles 1. After addition, the mixture was stirred at a rotation speed of 30 rpm for 15 minutes, and after a certain amount of the solvent (80% by mass) had evaporated, the mixture was heated to 80°C while mixing under reduced pressure, and toluene was distilled off over 2 hours, after which it was cooled. The magnetic carrier obtained was separated into low magnetic products by magnetic separation, passed through a sieve with an opening of 70 μm, and then classified with a wind classifier to obtain a magnetic carrier having a median diameter of 38.2 μm based on the volume distribution.

[0087] [Example 1~ 6 and 8, Reference Examples 7 and 9 17, Comparative Examples 1 to 5] Mix toner 1 and magnetic carrier in a V-type mixer (V-10 type: Tokuju Manufacturing Co., Ltd.) for 0.5 s so that the toner concentration becomes 10% by mass. -1 The mixture was mixed for a rotation time of 5 minutes to obtain two-component developer 1. Similarly, toners 2 to 22 and a magnetic carrier shown in Table 1 were mixed to obtain two-component developers 2 to 22.

[0088] The two-component developers 1 to 17 are used in Examples 1 to 6 and 8, Reference Examples 7 and 9 As No. 17, two-component developers 18 to 22 were used as comparative examples 1 to 5, and the following print durability test was carried out, after which the toner performance was evaluated according to (1) to (3).

[0089] <Print durability test> The image forming apparatus used was a modified Canon digital commercial printer imAgeRUNNER ADVANCE C5560, and two-component developer 1 was placed in the developing device in the black position. The modifications to the apparatus included the fixing temperature, process speed, and DC voltage V of the developer carrier. DC , the charging voltage of the electrostatic latent image carrier V D The laser power and the laser power can be freely set. The image output evaluation is performed by outputting a FFh image (solid image) with the desired image ratio, and adjusting the V DC , V D and laser power were adjusted and the evaluation described below was performed.

[0090] FFh is a hexadecimal value representing 256 gradations, with 00h being the first gradation (white background) of the 256 gradations, and FFh being the 256th gradation (solid area) of the 256 gradations.

[0091] A print durability test was conducted in a high temperature and high humidity environment (temperature 30°C, relative humidity 80%) with 15,000 sheets of 10% image duty images, and the developer was sampled from inside the device to evaluate the toner performance.

[0092] Toner Performance Evaluation (1) Cover measurement Paper: CS-680 (680g / m 2 ) (Canon Marketing Japan Inc.) Evaluation image: 00h image on the entire surface of the above A4 paper VbAck: 150V (The DC voltage of the developer carrier V DC , the charging voltage of the electrostatic latent image carrier V D , and adjusted by laser power) Test environment: High temperature and humidity environment (temperature 30℃ / humidity 80%RH) Fixing temperature: 170℃ Process speed: 377mm / sec The evaluation image was output and the fog was evaluated. The fog value was used as an evaluation index for fog. Using a reflectometer (REFLECTOMETER MODEL TC-6DS: manufactured by Tokyo Denshoku), the average reflectance Ds (%) of the evaluation paper before paper passing was measured. Next, the average reflectance Dr (%) of the evaluation paper after paper passing was measured. Then, the fog value was calculated using the following formula. The obtained fog value was evaluated according to the following evaluation criteria. Fog = Dr(%)-Ds(%) (Evaluation Criteria) Rank A: Less than 1.0% fogging Rank B: Fog 1.0% or more, less than 1.5% Rank C: Fog 1.5% or more, less than 2.0% Rank D: Fog 2.0% or more, less than 2.5% Rank E: Fog 2.5% or more, less than 3.0% Rank F: Fog 3.0% or more

[0093] (2)Agglomeration degree measurement: The degree of cohesion was measured using a powder rheometer (FT4, Freeman Technology). 10 g of toner was weighed into a specified container, stirred, compacted with a certain pressure, and stored in a high temperature and high humidity environment (room temperature 30°C, humidity 80%) for 72 hours. After storage, the force used to pierce the toner with a special needle-shaped tool was measured. The magnitude of this value was used to evaluate the degree of cohesion, and the following judgments were made based on the obtained value. The unit of the value of the degree of cohesion is [mJ / mm]. Rank A: Less than 20 Rank B: 20 ​​or more, less than 22 Rank C: 22 or more, less than 24 Rank D: 24 or more, less than 26 Rank E: 26 or more, less than 30 Rank F: 30 or above

[0094] (3) Fluidity measurement: 100g of toner that had been stored for 72 hours in a high temperature and humidity environment (room temperature 30°C, humidity 80%) was placed in a cylindrical container (bottom diameter 15 cm, height 30 cm), and the container was subjected to vibrations that changed its orientation at 90 degrees per second for 30 seconds. Immediately after this, the container was stood upright and the lid covering the 5 cm x 5 cm hole in the bottom of the container was removed. The amount of toner discharged from the container was measured, and the size of the percentage of this discharged toner was used to evaluate fluidity, and judged as follows. Rank A: 72% or more Rank B: 68% or more, less than 72% Rank C: 64% or more, less than 68% Rank D: 60% or more, less than 64% Rank E: 50% or more, less than 59% Rank F: Less than 50% The results of the performance evaluation of the obtained toner are shown in Table 2.

[0095] [Table 2]

[0096] As shown by the above results, according to the present invention, it is possible to prevent toner aggregation while maintaining toner fluidity, and to suppress fogging of white images.

Claims

1. A toner having toner particles containing a binder resin and silica fine particles on the surfaces of the toner particles, The silica fine particles contain silica fine particles A containing 200 ppm or more and 2000 ppm or less of iron atoms, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 200 nm or less, and The charge decay constant α after 1800 seconds from the charged state in an environment of a temperature of 23° C. and a relative humidity of 50% is 0.0005 or more and 0.0100 or less, The toner is characterized in that the weight average particle diameter (D4) of the toner particles is 3.0 μm or more and 5.7 μm or less.

2. 2. The toner according to claim 1, wherein the weight average particle diameter (D4) of the toner is 3.0 μm or more and 5.3 μm or less.

3. 2. The toner according to claim 1, wherein the silica fine particles A contain aluminum atoms in an amount of 200 ppm or more and 2000 ppm or less.

4. 4. The toner according to claim 1, wherein the silica fine particles A are silica particles which have been subjected to a hydrophobic treatment.

Citation Information

Patent Citations

  • silica

    JP2005536611A

  • Toner

    JP2009134073A

  • silanized fumed silica

    JP2009520667A

  • Hydrophobic fumed silica and silicone rubber materials containing the fumed silica

    JP2010527882A

  • Toner and two-component-based developer

    JP2015084095A