Method for manufacturing multi-junction devices
The use of a low-boiling point aprotic solvent system with organic amines allows for all-solution processed multijunction perovskite solar cells, addressing the inefficiencies of complex processing techniques and enabling cost-effective, reproducible production.
Patent Information
- Application Number
- JP2021521523
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-22
- Filing Date
- 2019-10-18
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2039-10-18
AI Technical Summary
Existing methods for manufacturing multijunction perovskite solar cells face challenges due to the use of high-boiling, toxic solvents like DMF and DMSO, which require complex processing techniques such as sputter coating and lamination, leading to inefficiencies and high costs, and result in irreproducible device performance.
A method using a high volatility, low boiling point, aprotic solvent system with organic amines allows for the stacking of perovskite junctions without complex techniques, enabling all-solution processed multijunction solar cells through inkjet printing, spray coating, or similar methods, with a charge recombination layer deposited using solution-based technology.
This approach enables the fabrication of multijunction solar cells efficiently and cost-effectively, improving reproducibility and reducing internal reflectance losses, suitable for large-scale production on rigid and flexible substrates.
Smart Images

Figure 0007561121000012 
Figure 0007561121000013 
Figure 0007561121000014
Abstract
Description
[Technical field]
[0001] The present invention provides a method for producing a multijunction device comprising a layer of a crystalline A / M / X material. Also provided are multijunction devices obtainable or obtainable by the method of the present invention, comprising at least two photoactive regions, at least one photoactive region comprising a layer of a crystalline A / M / X material, and at least three photoactive regions, each photoactive region comprising a layer of a crystalline A / M / X material. [Background technology]
[0002] When perovskite solar cells were first reported in 2009, they had a solar-to-electrical conversion efficiency of 3%. By 2012, perovskite photovoltaic devices achieving 9.2% and 10.9% had been realized. Since then, research has rapidly expanded into the field of perovskite photovoltaic and photovoltaic devices based on other A / M / X materials that promise to completely change the energy landscape. Perovskite-based photovoltaic devices have since been realized with guaranteed efficiencies of over 23%.
[0003] Apart from the obvious attraction of high power conversion efficiency, one of the most attractive features of A / M / X materials is the relative ease with which films of this material can be produced in high quality. Perovskite films can be fabricated by a wide variety of methods, including one-step spin-coating, evaporation and dip-coating, as well as various combinations of these three routes. However, one-step spin-coating remains the simplest and fastest method, with the added advantage of not requiring the use of particularly expensive equipment. Many variations of this method have been developed, including, for example, an additional step in the form of anti-solvent quenching. It is speculated that solution-processing fabrication methods, such as inkjet printing, spray coating, slot-die coating, blade coating and gravure printing, could be carried out with minor modifications to the spin-coating method developed in the laboratory.
[0004] Perovskite solar cells are of great importance in photovoltaic research, but several concerns remain regarding the commercial potential of this material. One is the stability of the material and the anomalous hysteresis, frequently observed in the JV characteristics of these devices. The origin of this hysteresis has been shown to be ionic motion, and many attempts have been made to mitigate this effect. While so-called inverted positive intrinsic negative (pin) structures have been shown to exhibit negligibly small hysteresis, in regular negative intrinsic positive (nip) structures, the replacement of TiO2, often used as n-type charge collection layer, by organic electron acceptors, such as C60 or phenyl-C61-butyric acid methyl ester (PCBM), or the addition of a thin layer of such material on top of the TiO2 layer, has been quite successful in reducing the hysteresis, which in turn significantly increases the steady-state power output of the devices.
[0005] To date, most reports of solution-processed perovskite films use high-boiling, polar, aprotic solvents (see, for example, Eperon et al., Morphological Control for High Performance, Solution-Processed Planar Heterojunction Perovskite Solar Cells, Adv. Funct. Mater. 2013). The most frequently used solvent is dimethylformamide (DMF), but other solvents include dimethylsulfoxide (DMSO), γ-butyrolactone, and dimethylacetamide (DMA). The choice of solvent is limited in this case by the lead halide salts, which tend to be either poorly soluble or completely insoluble in most solvents commonly used in the processing of organic semiconductor and dye-sensitized solar cell materials. One of the drawbacks of using solvents such as these is the need to heat the perovskite or A / M / X material films to fairly high temperatures (above 100°C) to induce crystallization of the film. This can be circumvented to some extent by using the so-called anti-solvent quenching method, in which the film is immersed in an anti-solvent at a defined point during spin-coating to instantly crystallize the perovskite material, however, this can complicate the process by requiring an additional anti-solvent quenching step.
[0006] As discussed in WO2017 / 153752, there are several problems associated with existing solution-based methods of forming films of A / M / X materials. Currently, the solvents used (e.g., DMF, DMSO, γ-butyrolactone, and DMA) were selected because they can dissolve the precursor compounds of A / M / X materials, particularly metal halide precursors. However, these solvents have high boiling points, which increases the energy requirements or the complexity of solution processing. These solvents also tend to remove existing organic layers during device fabrication. These solvents are known to be toxic and accordingly can be difficult to handle and in some cases prohibitive for mass production due to toxicity concerns. Finally, these solvents are difficult to use in manufacturing because they cause problems for air purification equipment.
[0007] An additional concern is the solubility of other components of multijunction devices (e.g., organic electron-accepting layers in photovoltaic devices) in high boiling solvents, such as DMF, which is the most commonly used solvent for perovskites. Both C60 and PCBM are poorly soluble in DMF. This can lead to two problems when depositing perovskite layers: (i) in the worst case, almost complete washing away of the electron-selective contacts, or (ii) in the best case, shunting due to the formation of pinholes. Even if partial washing away of the electron-selective contacts occurs only on a very small scale, it leads to other problems such as irreproducible device performance, since there is always a change in both the thickness and uniformity of the n-type acceptor.
[0008] Multi-junction device architectures can increase the power conversion efficiency of photovoltaic cells beyond the single-junction thermodynamic limit where most of the current commercially available cells operate. Monolithic tandem solar cells with solution-processed perovskite layers have traditionally required remaining a combination of a silicon PV cell and a single perovskite solar cell junction.
[0009] Metal halide perovskite semiconductors exhibit high performance when integrated into optoelectronic devices such as light emitting diodes (LEDs), photodetectors, lasers and solar cells. These perovskites typically have the general chemical formula ABX3, with band gaps tuned by substituting their chemical substituents, i.e. A-site cations (methylammonium, formamidinium, cesium), B-site metal cations (lead or tin) or X-site anions (iodide, bromide, chloride). This allows halide perovskite semiconductors to be tailored to absorb specific regions of the solar spectrum and used in multi-junction applications with the ability to exceed the Shockley-Queisser and Tiedje-Yablonovitch thermodynamic efficiency limits. By reducing the difference between photon energy and electronic band gaps, the thermal loss of charge carriers can be minimized, thereby increasing the maximum obtainable power conversion efficiency (PCE). To reduce the conversion rate of photon energy to heat, multiple absorber materials with wide band gaps are required. Recently, efficient solar cells based on wide bandgap perovskites have been fabricated by partial substitution of organic A-site cations with cesium (Cs) to improve the structure, thermal and photostability. In addition, narrow bandgap materials have also been explored through modification of the B-site cation, with partial substitution of lead (Pb) with tin (Sn) resulting in unusual bandgap bowing behavior, leading to a bandgap approaching 1.2 eV.
[0010] Because of the potential advantages offered by the perovskite semiconductors described above, particularly the ability to modify their chemical composition to tune the bandgap as needed, it would be highly desirable to be able to construct all-perovskite multijunction solar cells.
[0011] The recent interest in all-perovskite multijunction solar cells has demonstrated the difficulties of fabricating these devices, especially by solution-based methods. This is due in part to the inability to easily build multijunction solar cells one on top of the other using solvents such as DMF and DMSO. Both DMF and DMSO are highly coordinating solvents used to dissolve perovskite salts. These solvents are used to process uniform and high-quality perovskite films and easily penetrate the layers as they are processed, which results in washing away or chemical decomposition of any perovskite layers already processed underneath.
[0012] Perovskite solar cells exhibiting record efficiencies have been processed by solution-based fabrication methods, reaching 23% in single-junction devices. The ability to fabricate high-quality absorber materials from solution-based methods, combined with exceptional optoelectronic properties, has led to a proliferation of perovskite solar cells. In recent years, breakthroughs have been made in four-terminal (4T) and two-terminal (2T) silicon-supported perovskite, Cu(In,Ga)Se2 (CIGS)-supported perovskite, Cu2ZnSn(S,Se)4 (CZTSSe)-supported perovskite, and even perovskite-supported perovskite tandem cells. Tandem solar cells require semi-transparent electrodes and / or recombination layers between each subcell, which can be fabricated using a wide variety of materials and processing methods. These highly conductive transparent layers have been fabricated using silver nanowires (Ag-NWs), 2,2'-(perfluoronaphthalene-2,6-diylidene) dimalononitrile doped with N4,N4,N4",N4"-tetra([1,1'-biphenyl]-4-yl)-[1,1':4',1"-terphenyl]-4,4"-diamine (TaTm:F6-TCNNQ), poly(3,4-ethylenedioxythiophene) polystyrenesulfonate (PEDOT:PSS), aluminum doped zinc oxide (AZO) and most notably indium tin oxide (ITO). These materials may be processed using different deposition techniques such as spray coating, film transfer lamination, vacuum evaporation and sputter coating. Sputtered ITO has gained great attraction due to its high optical transparency across the visible and near infrared (NIR) ranges combined with low resistivity. Due to its dense and compact nature, sputtered ITO can act as a physical barrier to solvents used in processing subsequent material layers, which will rapidly redissolve any underlying perovskite layers unless protected by a dense, pinhole-free layer, such as indium oxide tin oxide (ITO).
[0013] As recently shown, monolithic all-perovskite tandem cells with power conversion efficiencies (PCEs) of over 17% can be fabricated using dense sputtered ITO layers. These sputter-coated TCOs require high vacuum deposition systems and dense buffer layers, including nanoparticle (NP) or atomic layer deposition (ALD) layers, to prevent sputter damage of the organic and perovskite layers. Furthermore, the low refractive index of ITO compared to the perovskite absorber layer introduces significant internal reflectance losses, thus limiting the maximum achievable power conversion efficiency. Thus, the redissolution problem has largely hindered the experimental realization of all-solution-processed multijunction perovskite solar cells without sputter-coated ITO or other more complex processing techniques.
[0014] To date, it has not been possible to construct multijunction all-perovskite solar cells entirely via solution processing. A number of strategies have been used to try to protect the first perovskite layer and enable the fabrication of all-perovskite solar cells, as described below.
[0015] In Eperon et al. (Perovskite-perovskite tandem photovoltaics with optimized bandgaps, Science, 2016), the recombination layer used comprises a layer of tin oxide that is sputter-coated with indium tin oxide to protect the lower first perovskite layer from damage from the solvent used to deposit the second perovskite layer. This recombination layer provides a physical barrier between the perovskite layers that solvents such as DMF / DNSO cannot pass through. However, this requires more complex formulation techniques, e.g. sputter coating, which leads to a more complicated, time-consuming and costly manufacturing process.
[0016] In Heo et al. (CH3NH3PbBr3-CH3NH3PbI3Perovskite-Perovskite Tandem Solar Cells with Exceeding 2.2V Open Circuit Voltage, Adv. Mater. 2016, 28, 5121-5125), the problem of solvent damage to the lower perovskite layer is avoided by fabricating the top and bottom solar cells separately and then laminating them together. A thick hole transport layer is required to maintain adhesion between the front and back cells. The PCE obtained for these solar cells is about 10.8%. This method requires a more complicated sequence of fabrication steps (including lamination) and is therefore not fully solvent-based.
[0017] Sheng et al., Monolithic Wide Band Gap Perovskite / Perovskite Tandem Solar Cells with Organic Recombination Layers, J. Phys. Chem. C 2017, 121, 27256-27262, use a sequential vapor-solution processing method to avoid solution processing of the second perovskite layer with DMF. The resulting tandem solar cell has a PCE of 5.9%. Such a method requires thermal evaporation of the precursors, making it less amenable to large-scale printing techniques.
[0018] Jiang et al., A two-terminal perovskite / perovskite tandem solar cell J. Mater. Chem 2016, 4, 1208-1213, uses anti-solvent quenching technique to deposit the perovskite layer, and uses film transfer lamination technique to place the recombination layer on top of the lower cell. Due to these more complicated techniques, the method cannot be used on a large scale.
[0019] None of these strategies provide a facile, all-solution method for fabricating multijunction devices. [Prior art documents] [Patent documents]
[0020] [Patent Document 1] WO2017 / 153752 [Non-patent literature]
[0021] [Non-Patent Document 1] Eperon et al., Morphological Control for High Performance, Solution-Processed Planar Heterojunction Perovskite Solar Cells, Adv. Funct. Mater. 2013 [Non-Patent Document 2] Eperon et al., Perovskite-perovskite tandem photovoltaics with optimized bandgaps, Science, 2016 [Non-Patent Document 3] Heo et al., CH3NH3PbBr3-CH3NH3PbI3 Perovskite-Perovskite Tandem Solar Cells with Exceeding 2.2V Open Circuit Voltage, Adv. Mater. 2016, 28, 5121-5125 [Non-Patent Document 4] Sheng et al., Monolithic Wide Band Gap Perovskite / Perovskite Tandem Solar Cells with Organic Recombination Layers, J. Phys. Chem. C 2017, 121, 27256-27262 [Non-Patent Document 5] Jiang et al., A two-terminal perovskite / perovskite tandem solar cell J. Mater. Chem 2016, 4, 1208-1213 Summary of the Invention [Problem to be solved by the invention]
[0022] The present invention allows for the construction of A / M / X multijunction devices without the need to use complex processing techniques such as sputter coating, lamination or deposition, thereby allowing an all-solution approach to multijunction devices, allowing cheap and easy fabrication of such devices using conventional printing techniques, such as solution processing fabrication methods such as inkjet printing, spray coating, slot-die coating, blade coating and gravure printing, as well as spin coating. In particular, the present invention provides both a solution-processed perovskite layer and a solution-processed charge recombination layer comprising a tunnel junction.
[0023] It is shown that by using a highly volatile, low boiling point, aprotic solvent / organic amine based solvent system, perovskite junctions can be stacked on top of each other to create fully solution processed all-perovskite multi-junction solar cells. The solvation strength of such a solvent system can be adjusted by varying the amount of organic amine present. This means that the solvent used has the necessary solvation strength to dissolve the A / M / X precursor materials, but with a minimal excess of organic amine, thereby eliminating the risk of damaging underlying layers in the device. It is therefore discovered that the solvent used does not wash away the existing organic layers or the underlying perovskite layers during the fabrication of the multi-junction device. This improves the reproducibility and efficiency of the fabricated devices.
[0024] The inventors have developed a recombination layer that can be placed between various photoactive layers using solution-based techniques. The charge recombination layer described herein can be deposited using solution-based methods. This means that multi-junction devices can be manufactured more easily without the need for complex techniques such as sputter coating, lamination or vacuum deposition. In addition, it also means that thin (less than 100 nm) charge recombination layers can be manufactured, which reduces internal reflectance losses and leads to increased power conversion efficiency.
[0025] This all-solution-processed architecture has the potential to be applied to fabricate large-area films on both rigid and flexible substrates using deposition techniques such as roll-to-roll (R2R) processing, blade coating, slot-die coating, gravure printing or inkjet printing. Thus, the present invention provides a means to deliver fully solution-processed multijunction solar cells. These findings lead to new possibilities for large-scale, low-cost printable perovskite multijunction solar cells. [Means for solving the problem]
[0026] Accordingly, the present invention provides a method for producing a multijunction device comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c wherein [A] comprises one or more A cations, [M] comprises one or more M cations which are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18, said method comprising forming a layer of crystalline A / M / X material by disposing a membrane-forming solution on a substrate, wherein the membrane-forming solution comprises (a) one or more M cations, and (b) Solvent and the solvent is (i) an aprotic solvent, and (ii) Organic amines wherein the substrate includes a photoactive region including a photoactive material, and a charge recombination layer disposed on the photoactive region by a solution deposition process.
[0027] The present invention also provides a multijunction device obtainable or obtained by the method of the invention as defined above.
[0028] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) Charge recombination layer containing transparent conductive oxide nanoparticles Also provided is a multijunction device comprising:
[0029] In contrast to densely sputtered ITO layers, which introduce significant internal reflectance losses due to the lower refractive index of ITO compared to the A / M / X absorbing layers, the nanoparticles result in a non-continuous layer that is not only solution processable but can also scatter light through any subsequent light absorbing layers, thereby increasing the absorbance of the device.
[0030] The present invention also provides (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) A charge recombination layer comprising a conductive polymer Also provided is a multijunction device comprising:
[0031] The present invention also provides (a) at least three photoactive regions, each photoactive region comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X]c at least three photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) at least one charge recombination layer disposed between the photoactive regions; Also provided is a multijunction device comprising:
[0032] The present invention may also be advantageously used to fabricate multi-junction light emitting devices in which multiple junctions of light emitting diodes of different bandgaps provide concentrated white light emission. [Brief description of the drawings]
[0033] [Figure 1A] Results for two-terminal (2T) FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 (MA = methylammonium, CH3NH3+) tandem perovskite solar cells. Figure 1A shows scanning electron microscope (SEM) images of the top view of MAPbI3 thin films deposited on top of the top cell (TC) and intermediate layer, ranging from a 6% relative molar excess of PbI2 to a 6% relative molar excess of MAI for a 100:100 stoichiometric molar ratio of MAI:PbI2, prepared using an acetonitrile (CH3CN) / methylamine (CH3NH2) (ACN / MA) solvent system. [Figure 1B] Figure 1B shows results for a two-terminal (2T) FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 (MA = methylammonium, CH3NH3+) tandem perovskite solar cell. Figure 1B is a schematic diagram showing an all-solution processed perovskite / perovskite two-terminal (2T) tandem perovskite solar cell. Incident light is incident from below the device. [Figure 1C]Figure 1 shows results for a two-terminal (2T) FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 (MA = methylammonium, CH3NH3+) tandem perovskite solar cell. Figure 1C shows an SEM cross-section of a 2T perovskite / perovskite tandem cell. [Figure 1D] Results for two-terminal (2T) FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 (MA = methylammonium, CH3NH3+) tandem perovskite solar cells. Figure 1D shows the JV characteristics of Champion FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem heterojunction solar cell with an added mismatch factor of 1.004 measured at a scan rate of 0.25 V / s. [Figure 1E] Figure 1 shows results for a two-terminal (2T) FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 (MA = methylammonium, CH3NH3+) tandem perovskite solar cell. Figure 1E shows the external quantum efficiency (EQE) spectra of each sub-cell and the integrated current density of the tandem perovskite solar cell. [Figure 2A] Figure 2 shows the effect of changing the composition of A to B site cations in ACN-treated MAPb0.75Sn0.25I3 perovskite materials. Figure 2A) shows Kelvin probe measurements of varying A to B site stoichiometry. [Figure 2B] Figure 2B shows the effect of varying the composition of A to B site cations in ACN-processed MAPb0.75Sn0.25I3 perovskite materials. Normalized time-resolved photoluminescence (PL) measurements taken at the peak emission wavelength for varying A to B site stoichiometry. [Figure 2C] Figure 2C) Effect of varying the composition of A to B site cations in ACN-treated MAPb0.75Sn0.25I3 perovskite materials. Figure 2D) Effect of A to B site stoichiometry on the transient photocurrent. [Figure 2D]Figure 2D shows the effect of changing the composition of A to B site cations in ACN-processed MAPb0.75Sn0.25I3 perovskite materials and the JV characteristics of optimized MAPb0.75Sn0.25I3 single-junction heterojunction solar cells with 15% excess metal ions measured at a scan rate of 0.25 V / s. [Figure 3A] 3A shows a schematic diagram of an FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction perovskite solar cell. Figure 3A is a schematic diagram of an all-solution processed triple junction two-terminal (2T) perovskite solar cell. Incident light is incident from below the device. [Figure 3B] 3A and 3B are SEM cross-sectional views of a triple junction 2T all-perovskite tandem FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction perovskite solar cell. [Figure 3C] 3A and 3B are diagrams showing the JV characteristics of a Champion FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction perovskite solar cell and the fabricated Champion FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction heterojunction solar cell with an added mismatch factor of 1.323, measured at a scan rate of 0.25 V / s. [Figure 3D] 3D shows the open circuit voltage (Voc) of a FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction perovskite solar cell. FIG. 3E shows the open circuit voltage (Voc) of the triple junction heterojunction perovskite solar cell measured over a period of 60 s. [Figure 4A]Optical and electrical modeling of multi-junction perovskite solar cells. Figure 4A shows the calculated JV characteristics of a fully solution-processed FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell with single-junction experimental data and best-in-class ACN / MA MAPbI3 single-junction cell. [Figure 4B] Figure 4A shows optical and electrical modeling of multi-junction perovskite solar cells. Figure 4B shows the EQE spectrum of a fully solution-processed FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell with single-junction experimental data and a best-in-class ACN / MA MAPbI3 single-junction cell. [Figure 4C] Optical and electrical modeling of multi-junction perovskite solar cells. Figure 4C shows the calculated JV characteristics of a FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell assuming optimized layer thicknesses, a <50 nm interlayer, a MgF2 anti-reflective coating, and enhanced top cell performance. [Figure 4D] Optical and electrical modeling of multi-junction perovskite solar cells. Fig. 4D shows the simulated EQE spectrum of a FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell assuming optimized layer thicknesses, a <50 nm interlayer, MgF2 anti-reflective coating, and enhanced top cell performance. [Figure 4E] Optical and electrical modeling of multi-junction perovskite solar cells. Figure 4E shows the JV characteristics of a FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / FA0.6MA0.4Pb0.4Sn0.6I3 triple junction architecture assuming optimized layer thicknesses, sub-50 nm interlayer, MgF2 anti-reflective coating, and enhanced top cell performance. [Figure 4F]Optical and electrical modeling of multi-junction perovskite solar cells. Figure 4F shows simulated EQE spectra of a FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / FA0.6MA0.4Pb0.4Sn0.6I3 triple junction architecture assuming optimized layer thicknesses, sub-50 nm interlayer, MgF2 anti-reflective coating, and enhanced top cell performance. [Figure 5A] 5A shows the optical properties of FA0.83Cs0.17Pb(Br0.7I0.3)3 perovskite material with 2% potassium additive. Figure 5A shows the absorption spectrum of FA0.83Cs0.17Pb(Br0.7I0.3)3 measured with an integrating sphere. [Figure 5B] 5A and 5B show the optical properties of FA0.83Cs0.17Pb(Br0.7I0.3)3 perovskite material with 2% potassium additive, and FIG. 5B shows the Tauc plot of FA0.83Cs0.17Pb(Br0.7I0.3)3 perovskite with assumed optical band gap fitting from direct band gap material and intercept. [Figure 6] FIG. 1 shows an SEM image of the top view of a FA0.83Cs0.17Pb(Br0.7I0.3)3 perovskite film. [Figure 7A] Current-voltage characteristics of SnO2 / PCBM / FA0.83Cs0.17Pb(Br0.7I0.3)3 / spiro-OMeTAD perovskite solar cell with 2% mol potassium (K+) additive. Figure 7A shows the forward bias to short circuit current-voltage curve measured under simulated air mass (AM) 1.5 100 mW cm-2 sunlight using a scan rate of 0.25 V / s. The inset shows the photocurrent density and power conversion efficiency measured at the maximum power point for a period of 60 s. [Figure 7B]Figure 7B shows the current-voltage characteristics of SnO2 / PCBM / FA0.83Cs0.17Pb(Br0.7I0.3)3 / spiro-OMeTAD perovskite solar cells with 2% mol potassium (K+) additive. Figure 7B shows the stabilized open circuit voltage (Voc) of the FA0.83Cs0.17Pb(Br0.7I0.3)3 heterojunction perovskite solar cell. [Figure 8A] Figure 14. Effect of changing the composition of cations from A to B site of ACN / MA solvent-processed MAPbI3 perovskite absorber layer on A) power conversion efficiency incorporated in an all-perovskite tandem solar cell with a FA0.83Cs0.17Pb(Br0.7I0.3)3 front cell and a MAPbI3 back cell. [Figure 8B] Figure 14. Effect of changing the composition of cations from A to B sites on B) fill factor of ACN / MA solvent-processed MAPbI3 perovskite absorber layer incorporated in an all-perovskite tandem solar cell with a FA0.83Cs0.17Pb(Br0.7I0.3)3 front cell and a MAPbI3 back cell. [Figure 8C] Figure 14. Effect of changing the composition of cations from A to B sites of ACN / MA solvent-processed MAPbI3 perovskite absorber layer on C) short circuit current density incorporated in an all-perovskite tandem solar cell with FA0.83Cs0.17Pb(Br0.7I0.3)3 front cell and MAPbI3 back cell. [Figure 8D] Figure 14. Effect of changing the composition of cations from A to B sites of ACN / MA solvent-processed MAPbI3 perovskite absorber layer on D) open circuit voltage incorporated in an all-perovskite tandem solar cell with FA0.83Cs0.17Pb(Br0.7I0.3)3 front cell and MAPbI3 back cell. [Figure 9] Figure 1 shows the photocurrent density and power conversion efficiency of Champion FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual-junction solar cell measured at the maximum power point for a period of 90 s. A mismatch factor of 1.004 was applied to the PCE. [Figure 10]1 shows a table showing the calculated mismatch ratios for tandem and triple junction perovskite solar cells. The mismatch ratios were calculated for the following perovskite materials FA0.83Cs0.17Pb(Br0.7I0.3)3, MAPbI3 and FA0.83Cs0.17Pb0.5Sn0.5I3. The spectra and calibrations are different for both measurements due to the use of KG2 and KG5 filters to mitigate and account for large intensity spikes in the infrared radiation of the solar simulator with a xenon arc lamp. [Figure 11A] 11A and 11B show the measured solar simulator spectrum compared to the AM1.5G spectrum, and the xenon lamp spectrum set intensity with a KG5 filtered silicon reference cell used to measure the FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell. [Figure 11B] 11A and 11B show the measured solar simulator spectrum compared to the AM1.5G spectrum, and the xenon lamp spectrum set intensity with the KG2 filtered control cell used to measure the FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction solar cell. [Figure 12A] Figure 12 shows the device performance of the FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell with maximum open circuit voltage. Figure 12A shows the current-voltage characteristics measured under simulated air mass (AM) 1.5 100 mW cm-2 sunlight using a scan rate of 0.25 V / s. [Figure 12B] Figure 12B shows the device performance of the FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem solar cell with maximum open circuit voltage. Figure 12B shows the photocurrent density and power conversion efficiency measured at the maximum power point for a period of 60 s. A mismatch factor of 1.004 was applied to the PCE. [Figure 13A]13A shows the properties of MAPb0.75Sn0.25I3 perovskite material. Figure 13A shows the EQE spectrum of FTO / SnO2 / PC61BM / MAPb0.75Sn0.75I3 / spiro(TFSI)2 solar cell architecture measured with a 50 Ω resistive load. [Figure 13B] 13A and 13B show the properties of the MAPb0.75Sn0.25I3 perovskite material, which is assumed to be a direct bandgap material, and the Tauc plot of the MAPb0.75Sn0.25I3 perovskite material. [Figure 14A] Figure 1 shows the effect of changing the composition of cations from the A to B site of ACN / MA MAPb0.75Sn0.25I3 perovskite single junction solar cells on A) power conversion efficiency. [Figure 14B] FIG. 14 shows the effect of changing the composition of cations from A to B site on B) fill factor of ACN / MA MAPb0.75Sn0.25I3 perovskite single junction solar cells. [Figure 14C] Figure 1 shows the effect of changing the composition of cations from the A to B sites of ACN / MA MAPb0.75Sn0.25I3 perovskite single junction solar cells on C) short circuit current density. [Figure 14D] Figure 1 shows the effect of changing the composition of cations from the A to B sites on D) the open circuit voltage of ACN / MA MAPb0.75Sn0.25I3 perovskite single junction solar cells. [Figure 15A] Figure 15 shows the device performance of FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction solar cell with maximum open circuit voltage. Figure 15A shows the current-voltage characteristics measured under simulated air mass (AM) 1.5 100 mW cm-2 sunlight using a scan rate of 0.25 V / s. [Figure 15B]Figure 15 shows the device performance of the FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 / MAPb0.75Sn0.25I3 triple junction solar cell with maximum open circuit voltage. Figure 15B shows the photocurrent density and power conversion efficiency measured at the maximum power point for a period of 60 s. A mismatch factor of 1.323 was applied to the PCE. [Figure 16A] 16A shows the optical properties of the recombination intermediate layer and the hole and electron accepting layer. FIG. 16A shows the measured absorption from glass, indium tin oxide nanoparticles (ITO NPs), phenyl-C61-butyric acid methyl ester (PC61BM), phenyl-C61-butyric acid methyl ester (PC61BM), poly(3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS), (2,2',7,7'-tetrakis(N,N'-di-p-methoxyphenylamine)-9,9'-spirobifluorene) (spiro-OMeTAD) from 250 nm to 1050 nm. [Figure 16B] Figure 16B shows the optical properties of the recombination interlayer and the hole and electron accepting layers. Figure 16B shows transmission measurements. [Figure 16C] Fig. 16C shows the optical properties of the recombination interlayer and the hole and electron accepting layers. [Figure 17A] Figure 17 shows the architecture and device characteristics of FA0.83Cs0.17Pb0.5Sn0.5I3 filtered FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual junction solar cell. Figure 17A is a schematic diagram showing filtering of FA0.83Cs0.17Pb0.5Sn0.5I3 perovskite with an all-solution processed perovskite / perovskite two-terminal (2T) FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem perovskite solar cell. [Figure 17B]FIG. 17B shows the architecture and device characteristics of FA0.83Cs0.17Pb0.5Sn0.5I3 filtered by FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual junction solar cell. FIG. 17B shows the EQE spectrum of FA0.83Cs0.17Pb0.5Sn0.5I3 (solid line) filtered by FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual junction solar cell and the integrated current density of the tandem perovskite solar cell. Also shown are the EQE spectra of each subcell of the FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 tandem perovskite solar cell with opaque electrodes and the integrated current density of the tandem perovskite solar cell. [Figure 17C] Figure 17C shows the architecture and device characteristics of FA0.83Cs0.17Pb0.5Sn0.5I3 filtered FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual junction solar cell. Figure 17C shows the JV characteristics of unfiltered and fabricated FA0.83Cs0.17Pb0.5Sn0.5I3 filtered champion FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual junction solar cell measured at a scan rate of 0.25 V / s. [Figure 17D] Figure 17 shows the architecture and device characteristics of FA0.83Cs0.17Pb0.5Sn0.5I3 filtered FA0.83Cs0.17Pb(Br0.7I0.3)3 / MAPbI3 dual junction solar cells. Figure 17D shows the photocurrent density and power conversion efficiency measured at the maximum power point for a period of 60 s for unfiltered and filtered FA0.83Cs0.17Pb0.5Sn0.5I3 solar cells. A mismatch factor of 1.323 was applied to the PCE. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] definition The term "crystalline" as used herein refers to a crystalline compound, which is a compound having an extended 3D crystalline structure. A crystalline compound is typically in the form of crystals or, in the case of polycrystalline compounds, crystallites (i.e., multiple crystals with a particle size of 1 μm or less). Crystals often combine to form layers. The crystals of a crystalline material can be of any size. A crystal can be described as a nanocrystal if it has one or more dimensions ranging from 1 nm up to 1000 nm.
[0035] The terms "organic compound" and "organic solvent" as used herein have their typical meaning in the art and are believed to be readily understood by one of ordinary skill in the art.
[0036] As used herein, the term "crystalline A / M / X material" refers to a material having a crystalline structure that includes one or more A ions, one or more M ions, and one or more X ions. The A and M ions are cations. The X ions are anions. A / M / X materials typically do not include any further types of ions.
[0037] The term "perovskite" as used herein refers to a material having a three-dimensional crystal structure related to that of CaTiO3 or a material that includes a layer of a material having a structure related to that of CaTiO3. The structure of CaTiO3 can be represented by the formula ABX3, where A and B are cations of different sizes and X is an anion. In the unit cell, the A cation is at (0,0,0), the B cation is at (1 / 2,1 / 2,1 / 2), and the X anion is at (1 / 2,1 / 2,0). The A cation is usually larger than the B cation. Those skilled in the art will understand that when A, B, and X are changed, the different ion sizes can distort the structure of the perovskite material from that adopted by CaTiO3 to a structure that is less symmetric. The material also has less symmetry when it includes a layer with a structure related to that of CaTiO3. Materials that include layers of perovskite materials are well known. For example, the structure of the material with K2NiF4 type structure includes layers of perovskite material. Those skilled in the art will understand that perovskite materials can be represented by the formula [A][B][X]3, where [A] is at least one cation, [B] is at least one cation, and [X] is at least one anion. When the perovskite contains more than one A cation, different A cations can be distributed regularly or irregularly across the A sites. When the perovskite contains more than one B cation, different B cations can be distributed regularly or irregularly across the B sites. When the perovskite contains more than one X anion, different X anions can be distributed regularly or irregularly across the X sites. The symmetry of perovskites containing more than one A cation, more than one B cation, or more than one X cation is less than that of CaTiO3. In the case of layered perovskites, the stoichiometry can vary between A, B, and X ions. As an example, if the A cation has an ionic radius that is too large to fit within the 3D perovskite structure, it may adopt the [A]2[B][X]4 structure. The term "perovskite" also encompasses A / M / X materials that adopt the Rdolzden-Popper phase. The Rdolzden-Popper phase refers to perovskites that have a mixture of layered and 3D components.Such perovskites have crystal structure A. n-1 A'2M n X 3n+1 where A and A' are different cations and n is an integer from 1 to 8 or from 2 to 6. The term "mixed 2D and 3D" perovskites refers to AMX3 and A n-1 A'2M n X 3n+ It is used to refer to perovskite films in which regions or domains of both perovskite phases are present.
[0038] As used herein, the term "metal halide perovskite" refers to a perovskite whose formula contains at least one metal cation and at least one halide anion.
[0039] As used herein, the term "mixed-halide perovskite" refers to a perovskite or mixed perovskite that contains at least two types of halide anions.
[0040] As used herein, the term "mixed cation perovskite" refers to a perovskite of mixed perovskite containing at least two types of A cations.
[0041] As used herein, the term "mixed metal perovskite" refers to a perovskite that is a mixed perovskite containing at least two types of metal M cations.
[0042] As used herein, the term "organic-inorganic metal halide perovskite" refers to a metal halide perovskite whose formula contains at least one organic cation.
[0043] As used herein, the term "monocation" refers to any cation having a single positive charge, i.e., a cation of formula A + where A is any moiety, such as a metal atom or an organic moiety. The term "dication" as used herein refers to any cation having a double positive charge, i.e., a cation of formula A 2+where A is any moiety, such as a metal atom or an organic moiety. The term "trication" as used herein refers to any cation having a triple positive charge, i.e., a cation of formula A 3+ where A is any moiety, such as a metal atom or an organic moiety. The term "tetracation" as used herein refers to any cation having a quadruple positive charge, i.e., a cation of formula A 4+ where A is any moiety, for example a metal atom, refers to the cation of.
[0044] The term "alkyl" as used herein refers to a straight or branched chain saturated hydrocarbon group. An alkyl group is a C 1~20 Alkyl group, C 1~14 Alkyl group, C 1~10 Alkyl group, C 1~6 Alkyl group or C 1~4 It may be an alkyl group. 1~10 Examples of alkyl groups include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl or decyl. 1~6 Examples of alkyl groups are methyl, ethyl, propyl, butyl, pentyl or hexyl. 1~4 Examples of alkyl groups include methyl, ethyl, i-propyl, n-propyl, t-butyl, s-butyl, or n-butyl. When the term "alkyl" is used herein without a prefix to specify the number of carbon atoms, it has 1 to 6 carbons (this also applies to any other organic group mentioned herein).
[0045] The term "cycloalkyl" as used herein refers to a saturated or partially unsaturated cyclic hydrocarbon group. A cycloalkyl group is a C 3~10 Cycloalkyl groups, C 3~8 Cycloalkyl group or C 3~6 It may be a cycloalkyl group. 3~8 Examples of cycloalkyl groups include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclohexenyl, cyclohexa-1,3-dienyl, cycloheptyl, and cyclooctyl. 3~6Examples of cycloalkyl groups include cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl.
[0046] The term "alkenyl" as used herein refers to a straight or branched chain hydrocarbon group containing one or more double bonds. An alkenyl group is a C 2~20 Alkenyl group, C 2~14 Alkenyl group, C 2~10 Alkenyl group, C 2~6 Alkenyl group or C 2~4 It may be an alkenyl group. 2~10 Examples of alkenyl groups are ethenyl (vinyl), propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl or decenyl. 2~6 Examples of alkenyl groups are ethenyl, propenyl, butenyl, pentenyl or hexenyl. 2~4 Examples of alkenyl groups are ethenyl, i-propenyl, n-propenyl, s-butenyl or n-butenyl. Alkenyl groups typically contain one or two double bonds.
[0047] The term "alkynyl" as used herein refers to a straight or branched chain hydrocarbon group containing one or more triple bonds. An alkynyl group is a C 2~20 Alkynyl group, C 2~14 Alkynyl group, C 2~10 Alkynyl group, C 2~6 Alkynyl group or C 2~4 It may be an alkynyl group. 2~10 Examples of alkynyl groups are ethynyl, propynyl, butynyl, pentynyl, hexynyl, heptynyl, octynyl, nonynyl or decynyl. 1~6 Examples of alkynyl groups are ethynyl, propynyl, butynyl, pentynyl or hexynyl. Alkynyl groups typically contain one or two triple bonds.
[0048] The term "aryl" as used herein refers to a monocyclic, bicyclic or polycyclic aromatic ring containing 6 to 14 carbon atoms, typically 6 to 10 carbon atoms, in the ring portion. Examples include phenyl, naphthyl, indenyl, indanyl, anthracenyl and pyrenyl groups. The term "aryl group" as used herein includes heteroaryl groups.
[0049] The term "heteroaryl" as used herein typically refers to a monocyclic or bicyclic aromatic heterocycle containing 6 to 10 atoms, including one or more heteroatoms, in the ring portion. Heteroaryl groups are generally 5- or 6-membered rings containing at least one heteroatom selected from O, S, N, P, Se, and Si. For example, they may contain 1, 2, or 3 heteroatoms. Examples of heteroaryl groups include pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, furanyl, thienyl, pyrazolidinyl, pyrrolyl, oxazolyl, oxadiazolyl, isoxazolyl, thiadiazolyl, thiazolyl, isothiazolyl, imidazolyl, pyrazolyl, quinolyl, and isoquinolyl.
[0050] As used herein in the context of substituted organic groups, the term "substituted" refers to any group including, but not limited to, C 1~10 Alkyl, aryl (as defined herein), cyano, amino, nitro, C 1~10 Alkylamino, di(C 1~10 ) Alkylamino, arylamino, diarylamino, aryl(C 1~10 ) Alkylamino, Amido, Acyl Amido, Hydroxy, Oxo, Halo, Carboxy, Ester, Acyl, Acyloxy, C 1~10 Alkoxy, aryloxy, halo(C 1~10 ) Alkyl, Sulfonic Acid, Thiol, C 1~10It refers to an organic group having one or more substituents selected from alkylthio, arylthio, sulfonyl, phosphoric acid, phosphoric acid ester, phosphonic acid and phosphonic acid ester. Examples of substituted alkyl groups include haloalkyl, perhaloalkyl, hydroxyalkyl, aminoalkyl, alkoxyalkyl and alkaryl groups. When a group is substituted, it can have one, two or three substituents. For example, a substituted group can have one or two substituents.
[0051] The term "halide" as used herein refers to a monovalent anion of an element in Group VIII of the periodic table. "Halide" includes fluoride, chloride, bromide, and iodide.
[0052] The term "halo" as used herein refers to a halogen atom. Exemplary halo species include fluoro, chloro, bromo and iodo species.
[0053] As used herein, an amino group is a group of formula -NR2, where each R is a substituent. R is typically selected from hydrogen, alkyl, alkenyl, cycloalkyl, or aryl, each of which is as defined herein. Typically, each R is selected from hydrogen, C 1~10 Alkyl, C 2~10 Alkenyl and C 3~10 Preferably, each R is selected from hydrogen, C 1~6 Alkyl, C 2~6 Alkenyl and C 3~6 More preferably, each R is selected from hydrogen and C 1~6 is selected from alkyl.
[0054] Exemplary amino groups are alkylamino groups of the formula -NR2, where at least one R is an alkyl group as defined herein. 1~6 An alkylamino group is one in which at least one R is C. 1~6 It is an alkylamino group which is an alkyl group.
[0055] As used herein, an imino group is a group of formula RC=N- or -C(R)=NR, where each R is a substituent. That is, an imino group is a group that contains a C=N moiety with a radical moiety either at the N atom or attached to the C atom of said C=N bond. R is as defined herein, that is, R is typically selected from hydrogen, alkyl, alkenyl, cycloalkyl, or aryl, each of which alkyl, alkenyl, cycloalkyl, and aryl are as defined herein. Typically, each R is selected from hydrogen, C 1~10 Alkyl, C 2~10 Alkenyl and C 3~10 Preferably, each R is selected from hydrogen, C 1~6 Alkyl, C 2~6 Alkenyl and C 3~6 More preferably, each R is selected from hydrogen and C 1~6 is selected from alkyl.
[0056] Exemplary imino groups are alkylimino groups, which are groups of formula RC=N- or -C(R)=NR, where at least one R is an alkyl group as defined herein. 1~6 An alkylimino group is one in which the R substituent contains from 1 to 6 carbon atoms.
[0057] The term "ester" as used herein refers to an organic compound of the formula alkyl-C(=O)-O-alkyl, where the alkyl groups are the same or different and are as defined herein. The alkyl groups may be optionally substituted.
[0058] The term "ether" as used herein refers to an oxygen atom substituted with two alkyl groups, as defined herein, which may be optionally substituted and may be the same or different.
[0059] As used herein, the term "ammonium" refers to an organic cation that contains a quaternary nitrogen. The ammonium cation has the formula R 1 R 2 R 3 R 4 N + R is a cation of 1 , R 2 , R 3 and R 4 is a substituent. 1 , R 2 , R 3 and R 4 Each of R is typically independently selected from hydrogen, or optionally substituted alkyl, alkenyl, aryl, cycloalkyl, cycloalkenyl, and amino, where the optional substituents are preferably amino or imino substituents. 1 , R 2 , R 3 and R 4 each independently represents hydrogen, and optionally substituted C 1~10 Alkyl, C 2~10 Alkenyl, C 3~10 Cycloalkyl, C 3~10 Cycloalkenyl, C 6~12 Aryl and C 1~6 The optional substituents, if present, are preferably selected from amino groups, particularly preferably C 1~6 Preferably, R 1 , R 2 , R 3 and R 4 Each of is independently hydrogen, and unsubstituted C 1~10 Alkyl, C 2~10 Alkenyl, C 3~10 Cycloalkyl, C 3~10 Cycloalkenyl, C 6~12 Aryl and C 1~6 In a particularly preferred embodiment, R 1 , R 2 , R 3 and R 4 are independently hydrogen, C 1~10 Alkyl, C 2~10 Alkenyl and C 1~6More preferably, R 1 , R 2 , R 3 and R 4 are independently hydrogen, C 1~6 Alkyl, C 2~6 Alkenyl and C 1~6 Amino.
[0060] As used herein, the term “iminium” refers to a compound of the formula (R 1 R 2 C=NR 3 R 4 ) + (In the formula, R 1 , R 2 , R 3 and R 4 denotes an organic cation of the formula (I) as defined in relation to the ammonium cation. Thus, in a particularly preferred embodiment of the iminium cation, R 1 , R 2 , R 3 and R 4 are independently hydrogen, C 1~10 Alkyl, C 2~10 Alkenyl and C 1~6 In a further preferred embodiment of the iminium cation, R 1 , R 2 , R 3 and R 4 are independently hydrogen, C 1~6 Alkyl, C 2~6 Alkenyl and C 1~6 Amino. In many cases, the iminium cation is selected from formamidinium, i.e., R 1 is NH2 and R 2 , R 3 and R 4 are all H.
[0061] The term "multi-junction device" as used herein refers to a single device that includes two or more optoelectronic devices that are electronically connected to each other in series and arranged successively on top of each other. The optoelectronic device may include a perovskite absorption layer sandwiched between hole and electron accepting layers. A charge recombination layer, which may be tunnel-junctioned, separates each of the optoelectronic devices in the multi-junction device that are stacked on top of each other in the multi-junction device. Typically, the bandgaps of the optoelectronic semiconductors in the multi-junction device are different from each other.
[0062] Examples of multijunction devices include photovoltaic devices, solar cells, photovoltaic diodes, photodetectors, photodiodes, photosensors, color-emitting devices, light-emitting transistors, photosensitive transistors, phototransistors, solid-state triodes, light-emitting devices (light-emitting elements), lasers, or light-emitting diodes. The terms "solar cells" and "photovoltaic diodes" are used interchangeably herein. The term "optoelectronic device," as used herein, refers to a device that sources, controls, or detects light. Light is understood to include any electromagnetic radiation. Examples of optoelectronic devices include photovoltaic devices, photodiodes (including solar cells), phototransistors, photomultipliers, photoresistors, and light-emitting diodes.
[0063] The term "consisting essentially of" refers to a composition that includes the component that essentially constitutes the composition and other components, provided that the other components do not materially affect the essential properties of the composition. Typically, a composition that consists essentially of a particular component contains 95 wt% or more of that component, or 99 wt% or more of that component.
[0064] The term "disposed on" or "disposed on" as used herein refers to making one component available on another component or placing one component on another component. A first component can be made available or placed directly on a second component, or there can be a third component intervening between the first and second components. For example, if a first layer is placed on a second layer, this includes the case where there is a third layer intervening between the first and second layers. Typically, "disposed on" refers to placing one component directly on another component.
[0065] The term "layer" as used herein refers to any structure of substantially laminar morphology (e.g., extending substantially in two perpendicular directions, but with limited extension in a third perpendicular direction). A layer may have a thickness that varies with the extent of the layer. Typically, a layer has a substantially constant thickness. The "thickness" of a layer, as used herein, refers to the average thickness of the layer. The thickness of a layer can be readily measured, for example, by microscopy, for example, electron microscopy of a cross-section of a film, or by surface profilometry, for example, using a stylus profilometer.
[0066] The term "band gap" as used herein refers to the energy difference between the top of the valence band and the bottom of the conduction band in a material. Of course, one skilled in the art can easily measure the band gap of a semiconductor (including that of a perovskite) using well-known procedures that do not require undue experimentation. For example, the band gap of a semiconductor can be evaluated by constructing a photovoltaic diode or solar cell from the semiconductor and determining the photovoltaic action spectrum. Alternatively, the band gap can be evaluated by measuring the optical absorption spectrum by either transmission spectrophotometry or photothermal deflection spectroscopy. The band gap can be determined by constructing a Tauc plot as described in Tauc, J., Grigorovici, R. & Vancu, a. Optical Properties and Electronic Structure of Amorphous Germanium. Phys. Status Solidi 15, 627-637 (1966), in which the square of the product of the absorption coefficient and the photon energy is plotted on the y-axis against the photon energy on the x-axis, and the linear intersection of the absorption edge with the x-axis gives the optical band gap of the semiconductor. Alternatively, the optical band gap can be evaluated by recording the onset of the incident photon-to-electron conversion efficiency as described in [Barkhouse DAR, Gunawan O, Gokmen T, Todorov TK, Mitzi DB. Device characteristics of a 10.1% hydrazineprocessed Cu2ZnSn(Se,S)4 solar cell. Progress in Photovoltaics: Research and Applications 2012; published online DOI: 10.1002 / pip.1160.].
[0067] As used herein, the term "semiconductor" or "semiconductor material" refers to a material having an electrical conductivity intermediate between that of an electrical conductor and a dielectric. A semiconductor may be a negatively charged (n) type semiconductor, a positively charged (p) type semiconductor, or an intrinsic (i) semiconductor. A semiconductor may have a band gap of 0.5 to 3.5 eV, e.g., 0.5 to 2.5 eV or 1.0 to 2.0 eV (measured at 300K).
[0068] As used herein, the term "n-type region" refers to a region of one or more electron-transporting (i.e., n-type) materials. Similarly, the term "n-type layer" refers to a layer of an electron-transporting (i.e., n-type) material. An electron-transporting (i.e., n-type) material can be a single transporting compound or elemental material, or a mixture of two or more electron-transporting compounds or elemental materials. An electron-transporting compound or elemental material can be undoped or doped with one or more dopant elements.
[0069] As used herein, the term "p-type region" refers to a region of one or more hole-transporting (i.e., p-type) materials. Similarly, the term "p-type layer" refers to a layer of hole-transporting (i.e., p-type) materials. A hole-transporting (i.e., p-type) material can be a single hole-transporting compound or elemental material, or a mixture of two or more hole-transporting compounds or elemental materials. A hole-transporting compound or elemental material can be undoped or doped with one or more dopant elements.
[0070] As used herein, the term "electrode material" refers to any material suitable for use in an electrode. The electrode material has high electrical conductivity. As used herein, the term "electrode" refers to a region or layer that consists of or consists essentially of an electrode material.
[0071] The term "nanoparticle" as used herein means a fine particle whose size is typically measured in nanometers (nm). Nanoparticles typically have a particle size of 0.1 nm to 500 nm, such as 0.5 nm to 500 nm. Nanoparticles may be particles having a size of, for example, 0.1 nm to 300 nm, or for example, 0.5 nm to 300 nm. In many cases, nanoparticles have a particle size of 0.1 nm to 100 nm, such as 0.5 nm to 100 nm. Nanoparticles may have a high sphericity, i.e., may be substantially spherical or spherical. Nanoparticles having a high sphericity may have a sphericity of, for example, 0.8 to 1.0. Sphericity is defined as:
[0072]
number
[0073] method The present invention relates to a method for producing a multijunction device comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18, said method comprising forming a layer of crystalline A / M / X material by disposing a membrane-forming solution on a substrate, wherein the membrane-forming solution comprises (a) one or more M cations, and (b) Solvent and the solvent comprises (i) an aprotic solvent, and (ii) Organic amines wherein the substrate includes a photoactive region including a photoactive material and a charge recombination layer disposed on the photoactive region by solution deposition.
[0074] Typically, the method involves disposing a film-forming solution onto the charge recombination layer. Thus, typically, the substrate comprises the following layers in the following order: ·Charge recombination layer, ·Photoactive region.
[0075] Thus, typically, a multijunction device made in accordance with the present invention will include the following layers in the following order: Layers of crystalline A / M / X materials, ·Charge recombination layer, ·Photoactive region.
[0076] The photoactive material in the substrate may be dissolved in dimethylformamide (DMF). In many cases, at least one component of the charge recombination layer in the substrate is dissolved in dimethylformamide (DMF). For example, both the photoactive material in the substrate and at least one component of the charge recombination layer in the substrate may be dissolved in dimethylformamide (DMF). Typically, the photoactive material in the substrate is dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof. In many cases, at least one component of the charge recombination layer in the substrate is dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof. For example, both the photoactive material in the substrate and at least one component of the charge recombination layer in the substrate may be dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof.
[0077] Both the photoactive material in the substrate and the charge recombination layer in the substrate can be dissolved in dimethylformamide (DMF). Typically, both the photoactive material in the substrate and the charge recombination layer in the substrate are dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof.
[0078] Aprotic Solvents Typically, the aprotic solvent does not include dimethylformamide (DMF). Preferably, the aprotic solvent does not include dimethylformamide, dimethylsulfoxide (DMSO), or a mixture thereof.
[0079] The aprotic solvent may be a polar aprotic solvent. Such solvents are known to those skilled in the art. For example, the aprotic solvent may include a compound selected from the group consisting of chlorobenzene, acetone, butanone, methyl ethyl ketone, acetonitrile, propionitrile, or a mixture thereof.
[0080] The aprotic solvent may be a non-polar aprotic solvent. Such solvents are known to those skilled in the art. For example, the aprotic solvent may include toluene.
[0081] Typically, the aprotic solvent comprises a compound selected from the group consisting of chlorobenzene, acetone, butanone, methyl ethyl ketone, acetonitrile, propionitrile, toluene, or a mixture thereof. Preferably, the aprotic solvent comprises acetonitrile. For example, 80 vol% or more of the aprotic solvent may be acetonitrile.
[0082] Organic amines Typically, the organic amine is an unsubstituted or substituted alkylamine or an unsubstituted or substituted arylamine.
[0083] An alkylamine is an organic compound that contains an alkyl group and an amine group, which may be a primary, secondary or tertiary amine group. The alkylamine compound may be a primary amine R A NH2 (in the formula, each R A is an alkyl group which may be substituted or unsubstituted), or a secondary amine R A 2NH (in the formula, each R Ais an alkyl group which may be substituted or unsubstituted), or a tertiary amine R A 3N (in the formula, each R A is an alkyl group which may be substituted or unsubstituted. Typically, the alkyl amine is a primary alkyl amine.
[0084] Typically, the organic amines are unsubstituted or substituted (C 1~10 For example, the alkylamine compound is a primary amine R A NH2 (in the formula, R A is unsubstituted or substituted C 1~10 Alkyl or unsubstituted or substituted C 1~8 Alkyl, e.g., unsubstituted or substituted C 1~6 For example, R A may be methyl, ethyl, propyl, isopropyl, butyl (i.e., n-butyl), pentyl (n-pentyl) or hexyl (n-hexyl).
[0085] Preferably, the organic amine is unsubstituted (C 1~10 alkyl)amine or phenyl group substituted (C 1~10 For example, the organic amine is an unsubstituted (C alkyl) amine. 1~8 alkyl)amines, such as unsubstituted (C 1~6 The organic amine may be a phenyl-substituted (C alkyl)amine, such as methylamine, ethylamine, propylamine, butylamine, or pentylamine or hexylamine. 1~8 alkyl)amines, e.g. phenyl-substituted (C 1~6 It may also be a) amine such as benzylamine or phenylethylamine.
[0086] Thus, the organic amine may be methylamine, ethylamine, propylamine, butylamine or pentylamine, hexylamine, benzylamine or phenylethylamine, or a mixture thereof. For example, the organic amine may be methylamine, propylamine or butylamine. Preferably, the organic amine is methylamine.
[0087] The solvent may comprise two or more organic amine compounds as defined herein. For example, the solvent may comprise methylamine, butylamine, phenylethylamine, hexylamine, octylamine, octadecylamine, alkylamine, naphthylamine, and benzylamine, methoxypolyethyleneglycolamine.
[0088] Arylamines are organic compounds that contain an aryl group and an amine group. Typically, arylamines are derived from ammonia by replacing one or more hydrogen atoms with an aryl group.
[0089] The arylamine may comprise an amine group which may be a primary, secondary or tertiary amine group. The arylamine compound may comprise a primary amine R B NH2 (in the formula, R B is an aryl group, which may be substituted or unsubstituted. For example, R B may be selected from phenyl, naphthyl, indenyl, indanyl, anthracenyl and pyrenyl groups. Typically, R B is a phenyl group, and therefore the arylamine may be a phenylamine (aniline).
[0090] Arylamines are secondary amines, such as those of formula R B R A NH (in the formula, R A is an alkyl group as described herein; R B wherein R is an aryl group as described herein. Arylamines may be tertiary amines, for example, secondary amines of the formula R B R A 2N (in the formula, each RA is the alkyl group as above, and R B is an aryl group as defined above).
[0091] Typically, the solvent in the process of the present invention is generated by adding an organic amine, either as a gaseous organic amine, a liquid organic amine, or an organic amine solution, to an aprotic solvent. Thus, the process may further comprise the step of generating the solvent by adding an organic amine to an aprotic solvent. The gaseous organic amine can be added to the solvent by bubbling the organic amine through the solvent.
[0092] The amount of organic amine in the solvent can vary depending on the requirements. Typically, the amount of organic amine present in the solvent is sufficient to completely solvate the M cation. If A cations and X anions are also present in the membrane-forming solution, the amount of organic amine present in the solvent may be sufficient to completely solvate the M cations, A cations and X anions. Thus, typically, the solvent contains an amount of organic amine sufficient to maintain the membrane-forming solution at its critical solution point. Preferably, only a small excess of organic amine is present, i.e., usually, there should be enough amine in the solvent to dissolve the components. Typically, the volume percentage of amine in the solvent is 50% or less, more typically less than 25%, for example less than 10%.
[0093] It is desirable to have a film-forming solution that uses a minimal amount of organic amine to solvate the M cations and, optionally, any A cations and X anions that may be present. Such a solution is capable of uniformly depositing the M cations and, optionally, any A cations and X anions onto a substrate without dissolving the underlying layers, such as the charge recombination layer, the photoactive region, or any charge transport layer (if present).
[0094] Typically, the membrane-forming solution is prepared by the following steps: preparing a solution in which the M cation, and optionally any A cations and X anions that may be present, are fully solvated in an aprotic solvent by an excess of an organic amine, preparing a dispersion of a compound comprising an M cation and, optionally, a compound(s) comprising an A cation and an X anion in an aprotic solvent that does not contain an organic amine; preparing the membrane-forming solution used in the method of the present invention by adding a solution to the dispersion until the undissolved compounds in the dispersion are completely dissolved; It is prepared by a method comprising:
[0095] As one skilled in the art will appreciate, the solubility of the M cation and, optionally, any A cations and X anions present will vary depending on the concentration and nature of the ions. The above method allows the amount of organic amine to be tailored so that an appropriate amount is used to fully solvate all ions with a minimal excess.
[0096] Typically, a solution in which the M cations, and optionally any A cations and X anions that may be present, are fully solvated with an excess of an organic amine is subjected to the following steps: preparing a dispersion of a compound comprising an M cation and, optionally, a compound(s) comprising an A cation and an X anion, said compound(s) being free of organic amines; adding an organic amine to the dispersion, typically by bubbling the gaseous organic amine through the dispersion, until the compound comprising the M cation and, optionally, the compound(s) comprising the A cation and the X anion are dissolved; The compound is prepared by a method comprising the steps of:
[0097] Typically, the film-forming solution is disposed on the substrate by a solution-phase deposition method, such as gravure coating, slot-die coating, screen printing, inkjet printing, doctor blade coating, spray coating, roll-to-roll (R2R) processing, or spin coating. Typically, disposing the film-forming composition on the substrate comprises spin-coating the film-forming solution on the substrate.
[0098] Typically, spin coating is carried out at a speed of at least 1000 RPM, such as at least 2000 RPM, at least 3000 RPM or at least 4000 RPM, for example between 1000 and 10000 RPM, between 2000 and 8000 RPM, between 2500 and 7500 RPM, preferably about 5000 RPM. Typically, spin coating is carried out for a time of at least 1 second, at least 5 seconds or at least 10 seconds, for example between 1 second and 1 minute, between 10 seconds and 30 seconds, preferably about 20 seconds.
[0099] Typically, the method further comprises removing the solvent to form a layer comprising the crystalline A / M / X material. Removing the solvent may comprise heating the solvent or evaporating the solvent.
[0100] The solvent is usually removed by heating the substrate treated with the membrane-forming solution. For example, the substrate treated with the membrane-forming solution may be heated to a temperature of 30° C. to 400° C., for example, 50° C. to 200° C. Preferably, the treated membrane-forming solution is heated to a temperature of 50° C. to 200° C. for a period of 5 to 200 minutes, preferably 10 to 100 minutes.
[0101] Post-processing The method of the invention may comprise the further step of disposing a composition comprising one or more A cations and optionally one or more X anions on the substrate. The film-forming solution used in the method of the invention may not comprise any A cations and / or X anions. In this case, the A cations and / or X anions may be added to the substrate in a separate step such that a crystalline A / M / X material is formed on the substrate. Alternatively, the film-forming solution used in the method of the invention may comprise A cations and / or X anions, and the further step of disposing a composition comprising one or more A cations and optionally one or more X anions on the substrate is carried out as a post-treatment step on top of the layer of crystalline A / M / X material.
[0102] Typically, the composition comprising one or more A cations and optionally one or more X anions is a solution. Thus, the method of the present invention may further comprise disposing a solution comprising one or more A cations and optionally one or more X anions on a substrate. The method of the present invention may further comprise disposing a composition comprising one or more A cations and one or more X anions, for example a solution comprising one or more A cations and one or more X anions, on a substrate.
[0103] A solution containing one or more A cations and one or more X anions can be formed by dissolving one or more compounds of formula AX, where A and X are as defined herein, in a solvent. The solvent can be different or the same as the solvent in the membrane-forming solution. Typically, the solvent is different from the solvent in the membrane-forming solution. Thus, the solvent can be orthogonal to the solvent in the membrane-forming solution. Importantly, the solvent must not dissolve the underlying perovskite film. For example, the solvent can be isopropanol (2-propanol), ethanol (EtOH), methanol (MeOH), and butanol. The solvent can be toluene. The solvent can also be a mixture of solvents, such as the above alcohols and aprotic solvents, such as toluene, anisole, chlorobenzene.
[0104] Typically, a solution containing one or more cations and one or more X anions is spin-coated onto a substrate. Typically, spin-coating is carried out at a speed of at least 1000 RPM, such as at least 2000 RPM, at least 3000 RPM or at least 4000 RPM, for example between 1000 and 10000 RPM, between 4000 and 8000 RPM, preferably about 6000 RPM. Typically, spin-coating is carried out for a time of at least 1 second, at least 5 seconds or at least 10 seconds, for example between 1 second and 1 minute, between 10 seconds and 30 seconds, preferably about 20 seconds.
[0105] The solvent is usually removed by heating the substrate treated with the membrane-forming solution. For example, the substrate treated with the membrane-forming solution may be heated to a temperature of 30° C. to 400° C., for example, 50° C. to 200° C. Preferably, the treated membrane-forming solution is heated to a temperature of 50° C. to 200° C. for a period of 5 to 200 minutes, preferably 10 to 100 minutes.
[0106] Formula [A] a [M] b [X] c Compound The method of the present invention provides a multijunction device comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c A multijunction device is fabricated comprising a compound of the formula: where [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18. a is often a number from 1 to 4, b is often a number from 1 to 3, and c is often a number from 1 to 8.
[0107] Each of a, b, and c may or may not be an integer. For example, if the compound adopts a structure with vacancies such that the crystal lattice is not fully occupied, a, b, or c may not be an integer. The method of the present invention provides excellent control over the stoichiometry of the product and is therefore well suited to the formation of structures where a, b, or c are not integers (e.g., structures with vacancies at one or more of the A, M, or X sites). Thus, in some embodiments, one or more of a, b, and c are non-integer values. For example, one of a, b, and c may be a non-integer value. In one embodiment, a is a non-integer value. In another embodiment, b is a non-integer value. In yet another embodiment, c is a non-integer value.
[0108] In other embodiments, each of a, b, and c is an integer value. Thus, in some embodiments, a is an integer from 1 to 6, b is an integer from 1 to 6, and c is an integer from 1 to 18. Often a is an integer from 1 to 4, often b is an integer from 1 to 3, and often c is an integer from 1 to 8.
[0109] Formula [A] a [M] b [X] c In general, in compounds of the formula: [A] comprises one or more A cations, where the A cations may be selected, for example, from alkali metal cations or organic monocations; [M] comprises one or more M cations, where the M cations are Pd 4+ , W 4+ , Re 4+ , Os 4+ , Ir 4+ , Pt 4+ , Sn 4+ , Pb 4+ , Ge 4+ , Te 4+ , Bi 3+ , Sb 3+ , Ca 2+ , Sr 2+ , Cd 2+ , Cu 2+ , Ni 2+ , Mn 2+, Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ and Eu 2+ , preferably Sn 2+ , Pb 2+ , Cu 2+ , Ge 2+ and Ni 2+ , particularly preferably Pb 2+ and Sn 2+ is a metal or metalloid cation selected from [X] is a halide anion (e.g., Cl - , Br - and I - ), O 2- , S 2- , Se 2- and Te 2- and one or more X anions selected from a is a number from 1 to 4, b is a number from 1 to 3; c is a number from 1 to 8.
[0110] Preferably, the formula [A] a [M] b [X] c Compounds of the formula [A] include perovskites. a [M] b [X] c Compounds of often include metal halide perovskites.
[0111] [M] Cation [M] includes one or more M cations that are metal or metalloid cations. [M] may include two or more different M cations. [M] may include one or more monocations, one or more dications, one or more trications, or one or more tetracations.
[0112] Typically, one or more of the M cations is Ca 2+ , Sr 2+ , Cd 2+ , Cu2+ , Ni 2+ , Mn 2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ ,EU 2+ , Bi 3+ , Sb 3+ , Pd 4+ , W 4+ , Re 4+ , Os 4+ , Ir 4+ , Pt 4+ , Sn 4+ , Pb 4+ , Ge 4+ and Te 4+ Preferably, one or more M cations are selected from Cu 2+ , Pb 2+ , Ge 2+ Or Sn 2+ is selected from.
[0113] Typically, the [M] cations include one or more metal or metalloid dications. For example, each M cation can be Ca 2+ , Sr 2+ , Cd 2+ , Cu 2+ , Ni 2+ , Mn 2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ and Eu 2+ , preferably Sn 2+ , Pb 2+ , Cu 2+ , Ge 2+ and Ni 2+ , preferably Sn 2+ and Pb 2+ In some embodiments, [M] comprises two different M cations, typically Sn 2+ and Pb 2+ It is.
[0114] The membrane-forming solution used in the method of the invention comprises (a) one or more M cations as described herein, and (b) a solvent as described herein. The method of the invention may comprise forming the membrane-forming solution by dissolving at least one M precursor in a solvent. As described in more detail below, an M precursor is a compound that comprises one or more M cations present in [M]. [M] (i.e., a compound of formula [A] a [M] b [X] c When [M] in the compound of formula (I) contains only one type of M cation, only one type of M precursor is required in the method of the invention.
[0115] M precursor typically comprises one or more counter anions.Thus, membrane-forming solution typically comprises one or more counter anions.Many such counter anions are known to those skilled in the art.One or more M cations and one or more counter anions can both be derived from a first precursor compound, which is dissolved in a solvent as described herein to form a membrane-forming solution.
[0116] The counter anions are halide anions and thiocyanate anions (SCN - ), tetrafluoroborate anion (BF4 - ) or an organic anion. Preferably, the counter anion described herein is a halide anion or an organic anion. The membrane-forming solution may contain more than one counter anion, for example more than one halide anion.
[0117] Typically, the counter anion has the formula RCOO - , ROCOO - , RSO3 - , ROP(O)(OH)O - or RO - (Wherein, R is H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 2~10 Alkenyl, substituted or unsubstituted C 2~10 Alkynyl, substituted or unsubstituted C 3~10Cycloalkyl, substituted or unsubstituted C 3~10 For example, R is H, substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 3~10 R may be cycloalkyl or substituted or unsubstituted aryl. Typically, R is H, substituted or unsubstituted C 1~6 R is an alkyl or substituted or unsubstituted aryl. For example, R is H, unsubstituted C 1~6 R may be alkyl or unsubstituted aryl. Thus, R may be selected from H, methyl, ethyl, propyl, butyl, pentyl, hexyl, cyclopentyl, cyclohexyl, and phenyl. In many cases, the counter anion(s) is a halide anion (e.g., F - , Cl - , Br - and I - ) and formula RCOO - where R is H or methyl.
[0118] Typically, the counter anion is F - , Cl - , Br - , I - , formate or acetate. Preferably, the counter anion is Cl - , Br - , I - or F - More preferably, the counter anion is Cl - , Br - or I - It is.
[0119] Typically, the M precursor is a compound of formula MY2, MY3 or MY4, where M is a metal or metalloid cation as described herein and Y is the counteranion.
[0120] Thus, the M precursor has the formula MY2, where M is Ca 2+ , Sr 2+ , Cd 2+ , Cu 2+ , Ni2+ , Mn 2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ or EU 2+ and Y is F - , Cl - , Br - , I - , formate or acetate. Preferably, M is Cu 2+ , Pb 2+ , Ge 2+ Or Sn 2+ and Y is Cl - , Br - , I - , formate or acetate, preferably Cl - , Br - or I - It is.
[0121] Typically, the M precursor is lead(II) acetate, lead(II) formate, lead(II) fluoride, lead(II) chloride, lead(II) bromide, lead(II) iodide, tin(II) acetate, tin(II) formate, tin(II) fluoride, tin(II) chloride, tin(II) bromide, tin(II) iodide, germanium(II) acetate, germanium(II) formate, germanium(II) fluoride, germanium(II) chloride, germanium(II) bromide, or germanium(II) iodide. In some cases, the first precursor compound comprises lead(II) acetate. In some cases, the first precursor compound comprises lead(II) iodide.
[0122] The M precursor is typically a compound of formula MY2. Preferably, the M precursor is a compound of formula SnI2, SnBr2, SnCl2, PbI2, PbBr2 or PbCl2.
[0123] The M precursor is a compound of the formula MY3, where M is Bi 3+ Or Sb 3+ and Y is F - , Cl - , Br- , I - , SCN - , BF4 - , formate or acetate. Preferably, M is Bi 3+ and Y is Cl - , Br - or I - In this case, the A / M / X material typically comprises a bismuth or antimony halogenometalate.
[0124] The M precursor has the formula MY4, where M is Pd 4+ , W 4+ , Re 4+ , Os 4+ , Ir 4+ , Pt 4+ , Sn 4+ , Pb 4+ , Ge 4+ or Te 4+ and Y is F - , Cl - , Br - , I - , SCN - , BF4 - , formate or acetate. Preferably, M is Sn 4+ , Pb 4+ or Ge 4+ and Cl - , Br - or I - In this case, the A / M / X material typically comprises a hexahalometalate.
[0125] Typically, the total concentration of [M] cations in the membrane-forming solution is between 0.01 and 10M, for example between 0.1 and 5M, between 0.25 and 2.5M, between 0.5 and 1.5M, preferably between 0.75 and 1.25M.
[0126] [A] cation and [X] anion Generally, the one or more A cations are monocations. [A] typically includes one or more A cations, which may be organic and / or inorganic monocations. For example, [A] may include at least two A cations, which may be organic and / or inorganic monocations. Thus, the formula [A] a [M] b [X] c The compound may be a mixed cation perovskite. [A] may include at least one A cation that is an organic cation and at least one A cation that is an inorganic cation. [A] may include at least two A cations that are both organic cations. [A] may include at least two A cations that are both inorganic cations.
[0127] When the A species is an inorganic monocation, A is typically an alkali metal monocation (i.e., a monocation of a metal in Group 1 of the periodic table), such as Li + , Na + , K + , Rb + , Cs + , e.g. Cs + or Rb + Typically, [A] comprises at least one organic monocation. When the A species is an organic monocation, A is typically an ammonium cation, such as methylammonium, or an iminium cation, such as formamidinium.
[0128] Each A cation is an alkali metal cation, e.g., Li + , Na + , K + , Rb + , Cs + , formula [R1R2R3R4N] + (wherein R1, R2, R3, and R4 are each independently hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl, wherein at least one of R1, R2, R3 and R4 is not hydrogen; a cation of the formula [R5R6N=CH-NR7R8] +wherein R5, R6, R7 and R8 are each independently hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl), each of which is unsubstituted or amino, C 1~6 Alkylamino, imino, C 1~6 Alkylimino, C 1~6 Alkyl, C 2~6 Alkenyl, C 3~6 Cycloalkyl and C 6~12 C substituted with one or more substituents selected from aryl 1~10 Alkylammonium, C 2~10 Alkenylammonium, C 1~10 Alkyliminium, C 3~10 Cycloalkylammonium and C 3~10 It may be selected from cycloalkyliminium.
[0129] Preferably, each A cation is Cs + , Rb + , methylammonium [(CH3NH3) + ], ethylammonium [(CH3CH2NH3) + ], propylammonium [(CH3CH2CH2NH3) + ], butylammonium [(CH3CH2CH2CH2NH3) + ], pentylammonium [(CH3CH2CH2CH2CH2NH3) + ], hexylammonium [(CH3CH2CH2CH2CH2CH2NH3) + ], heptylammonium [(CH3CH2CH2CH2CH2CH2CH2NH3) + ], Octylammonium [(CH3CH2CH2CH2CH2CH2CH2CH2NH3) + ], tetramethylammonium [(N(CH3)4) + ], formamidinium [(H2N-C(H)=NH2) + ], 1-aminoethane-1-iminium [(H2N-C(CH3)=NH2) + ] and guanidinium [(H2N-C(NH2)=NH2)+ ] is selected.
[0130] [A] usually contains one, two or three A monocations. [A] is methylammonium [(CH3NH3) + ], ethylammonium [(CH3CH2NH3) + ], propylammonium [(CH3CH2CH2NH3) + ], dimethylammonium [(CH3)2NH + ], tetramethylammonium [(N(CH3)4) + ], formamidinium [(H2N-C(H)=NH2) + ], 1-aminoethane-1-iminium [(H2N-C(CH3)=NH2) + ], guanidinium [(H2N-C(NH2)=NH2) + ], Cs + and Rb + For example, [A] may contain a single cation selected from methylammonium [(CH3NH3) + ].
[0131] Alternatively, [A] is a mixture of two cations selected from this group, such as Cs + and formamidinium [(H2N-C(H)=NH2) + ], e.g. Cs + and Rb + , or for example methylammonium [(CH3NH3) + ] and formamidinium [(H2N-C(H)=NH2) + ] may also be included.
[0132] Typically, in the method of the present invention, [A] is a compound of the formula [R1NH3] + (Wherein R1 is an unsubstituted C 1~10 alkyl) cation, and the organic amine is unsubstituted (C 1~10 The identity of the organic amine in the solvent can be matched to the alkyl amine that corresponds to the cation A when protonated. Thus, the formula [R1NH3] + C on A cation1~10 Alkyl groups and unsubstituted (C 1~10 C on alkyl amines 1~10 The alkyl group can be the same. For example, the A cation can be methylammonium, and the organic amine can contain methylamine, or the A cation can be ethylammonium, and the organic amine can contain ethylamine, or the A cation can be propylammonium, and the organic amine can contain propylamine, or the A cation can be butylammonium, and the organic amine can contain butylamine, or the A cation can be pentylammonium, and the organic amine can contain pentylamine, or the A cation can be hexylammonium, and the organic amine can contain hexylamine, or the A cation can be heptylammonium, and the organic amine can contain heptylamine, or the A cation can be octylammonium, and the organic amine can contain octylamine. In a preferred embodiment, [A] contains methylammonium, and the organic amine contains methylamine.
[0133] [X] comprises one or more X anions. Typically, [X] comprises one or more halide anions, i.e., F - , Br - , Cl - and I - Typically, each X anion is a halide. [X] typically contains one, two or three X anions, which are generally selected from Br - , Cl - and I - Typically, [X] comprises two or more different halide anions. [X] may, for example, consist of two X anions, such as Cl and Br, or Br and I, or Cl and I. Thus, the formula [A] a [M] b [X] c Compounds of formula [A] often include mixed halide perovskites. When [A] contains one or more organic cations, the formula [A] a [M]b [X] c The compound may be an organic-inorganic metal halide perovskite.
[0134] The membrane-forming solution may further comprise one or more A cations as described herein. Thus, it may be preferred that the membrane-forming solution comprises each of one or more A cations present in [A]. The method of the present invention may comprise forming the membrane-forming solution by dissolving at least one A precursor in a solvent. As described in more detail below, the A precursor is a compound that comprises one or more A cations present in [A]. [A] (i.e., a compound of the formula [A] a [M] b [X] c When [A] in the compound of formula (I) contains only one type of A cation, only one type of A precursor is required in the method of the present invention.
[0135] The membrane-forming solution may further comprise one or more X anions as described herein. With regard to the source of X anions in the method of the present invention, it may not be necessary to provide a separate X precursor in the method of the present invention. This is because, in some embodiments, the A precursor (or at least one of them, if the method involves multiple A precursors) and / or the M precursor (or at least one of them, if the method involves multiple M precursors) are salts, such as halide salts, that comprise one or more X anions. In a preferred embodiment, the A precursor (or multiple A precursors, if present) and the M precursor (or multiple M precursors, if present) both comprise the respective X cations present in [X].
[0136] Further X anions, such as fluoride (F - ) or chloride (Cl - ) may be added to the film-forming solution as a "dopant", for example by adding SnF2 or SnCl2, respectively, as an additive to the film-forming solution. In particular, Pb:Sn perovskites may benefit from the addition of additional SnF2 to the solution.
[0137] The membrane-forming solution typically further comprises one or more A cations as described herein and one or more X anions as described herein. In this embodiment, the membrane-forming solution comprises one or more A cations, one or more M cations and one or more X anions. Thus, in one embodiment, the membrane-forming solution comprises a cation represented by the formula [A] a [M] b [X] c The compound may contain all the ions necessary to form the compound.
[0138] Both the A cation and the X anion may be derived from the same precursor compound(s), which are dissolved in a solvent as described herein to form the membrane-forming solution. Preferably, the A / X precursor compound is a compound of the formula [A][X], where [A] comprises one or more A cations as described herein and [X] comprises one or more X anions as described herein. The A / X precursor compound is typically a compound of the formula AX, where X is a halide anion and the A cation is as defined herein. More than one A cation or more than one X anion may be of the formula [A] a [M] b [X] c When present in a compound of formula AX, more than one compound of formula AX may be dissolved in the membrane-forming solution.
[0139] The A / X precursor compound(s) may be, for example, CH3NH3Cl, CH3NH3Br, CH3NH3I, CH3CH2NH3Cl, CH3CH2NH3Br, CH3CH2NH3I, CH3CH2CH2NH3Cl, CH3CH2CH2NH3Br, CH3CH2CH2NH3I, N(CH3)4Cl, N(CH3)4Br, N(CH3)4I, (H2N-C(H)=NH2)Cl, (H2N-C( H)=NH2)Br, (H2N-C(H)=NH2)I, (H2N-C(CH3)=NH2)Cl, (H2N-C(CH3)=NH2)Br, (H2N-C(CH3)=NH2)I, (H2N-C( It can be selected from NH2)=NH2)Cl, (H2N-C(NH2)=NH2)Br, (H2N-C(NH2)=NH2)I, CsCl, CsBr, CsI, RbCl, RbBr and RbI.
[0140] In one embodiment, the membrane-forming solution contains an excess of A cations relative to M cations. In this context, the term "excess" refers to a molar ratio of one ion to another that is greater than or equal to the molar ratio of the formula [A] a [M] b [X] c This means that the ratio of A cations to M cations in the membrane-forming solution is greater than that required by the stoichiometry of the target compound. Typically, the ratio of A cations to M cations in the membrane-forming solution is 1:1 to 5:1, for example 1:1 to 4:1, 1:1 to 3:1, 1:1 to 2:1, 1:1 to 1.5:1, 1:1 to 1.25:1 or 1:1 to 1.1:1.
[0141] In one embodiment, the membrane-forming solution contains an excess of M cations relative to A cations. Typically, the ratio of M cations to A cations in the membrane-forming solution is 1:1 to 5:1, for example, 1:1 to 4:1, 1:1 to 3:1, 1:1 to 2:1, 1:1 to 1.5:1, 1:1 to 1.25:1, or 1:1 to 1.2:1. This is the formula [A] a [M] b [X] c The compound of formula (I) contains two M cations (preferably, [M] is Pb 2+ and Sn 2+ It is preferable when
[0142] Thus, typically, the total concentration of the [A] cation in the membrane-forming solution is between 0.01 and 10M, for example, between 0.1 and 5M, between 0.25 and 2.5M, between 0.5 and 1.5M, and preferably between 0.6 and 1.4M.
[0143] Typically, the total concentration of X anions will depend on the total concentration of A and / or M cations. For example, when using A / X precursor compounds and / or M precursor compounds that contain one or more X anions, the total concentration of X anions will depend on the total amount of A / X and / or M precursor compounds present.
[0144] Formula [A] a [M] b [X] cFurther detailed description of the compound Typically, a=1, b=1 and c=3. Therefore, in the formula [A] a [M] b [X] c The compound may be of the formula [A][M][X]3, where [A], [M] and [X] are as described herein. Typically, the crystalline A / M / X material has the formula (I): [A][M][X]3(I) (wherein [A] includes one or more A cations that are monocations, [M] includes one or more M cations that are dications of a metal or metalloid, and [X] includes one or more anions that are halide anions). Contains perovskites.
[0145] In some embodiments, the perovskite of formula (I) comprises a single A cation, a single M cation and a single X cation, i.e. the perovskite has the formula (IA): AMX3(IA) (wherein A, M and X are as defined above). In a preferred embodiment, A is a perovskite of (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + and M is selected from Pb 2+ Or Sn 2+ and X is Br - , Cl - and I - is selected from.
[0146] For example, the crystalline A / M / X material may comprise, or consist essentially of, a perovskite compound of formula (IA) selected from APbI3, APbBr3, APbCl3, ASnI3, ASnBr3 and ASnCl3, where A is a cation as described herein.
[0147] For example, crystalline A / M / X materials are CH3NH3PbI3, CH3NH3PbBr3, CH3NH3PbCl3, CH3NH3SnI3, CH3NH3SnBr3, CH3NH3SnCl3, CsPbI3, CsPbBr3, CsPbCl3, CsSnI3, CsSnBr3, CsSnCl3, (H2N-C(H)=NH2)PbI3, (H2N-C(H)=NH2)PbBr3 , (H2N-C(H)=NH2)PbCl3, (H2N-C(H)=NH2)SnI3, (H2N-C(H)=NH2)SnBr3 and (H2N-C(H)=NH2)SnCl3, in particular CH3NH3PbI3 or CH3NH3PbBr3, preferably CH3NH3PbI3.
[0148] In one embodiment, the perovskite has formula (IB): [A I x A II 1-x ]MX3(IB) (In the formula, A I and A II is as defined above for A, M and X are as defined above, and x is greater than 0 and less than 1. In a preferred embodiment, the perovskite I and A II are (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) +, Cs + and Rb + and M is selected from Pb 2+ Or Sn 2+ and X is Br - , Cl - and I - Selected from: A I and A II For example, (H2N-C(H)=NH2) + and Cs + or (CH3NH3), respectively. + and (H2N-C(H)=NH2) + Alternatively, Cs + and Rb + may be also possible.
[0149] For example, crystalline A / M / X materials are (Cs x Rb 1-x )PbBr3, (Cs x Rb 1-x )PbCl3, (Cs x Rb 1-x )PbI3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]PbCl3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]PbBr3,[(CH3NH3) x (H2N-C(H)=NH2) 1-x ]PbI3,[(CH3NH3) x Cs 1-x ]PbCl3, [(CH3NH3) x Cs 1-x ]PbBr3,[(CH3NH3) x Cs 1-x ]PbI3, [(H2N-C(H)=NH2) x Cs 1-x ]PbCl3, [(H2N-C(H)=NH2) x Cs 1-x ]PbBr3, [(H2N-C(H)=NH2) x Cs 1-x ]PbI3,[(CH3NH3) x (H2N-C(H)=NH2)1-x ]SnCl3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]SnBr3,[(CH3NH3) x (H2N-C(H)=NH2) 1-x ]SnI3,[(CH3NH3) x Cs 1-x ]SnCl3, [(CH3NH3) x Cs 1-x ]SnBr3,[(CH3NH3) x Cs 1-x ]SnI3, [(H2N-C(H)=NH2) x Cs 1-x ]SnCl3, [(H2N-C(H)=NH2) x Cs 1-x ]SnBr3, and [(H2N-C(H)=NH2) x Cs 1-x ]SnI3, where x is greater than 0 and less than 1, for example x may be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9.
[0150] In one embodiment, the perovskite has formula (IC): AM[X I y X II 1-y ]3(IC) (wherein A and M are as defined above; X I and X II is as defined above for X and y is greater than 0 and less than 1. In a preferred embodiment, A is a perovskite compound represented by the formula (CH3NH3). + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs +and Rb + and M is selected from Pb 2+ Or Sn 2+ and X I and X II are respectively, Br - , Cl - and I - is selected from.
[0151] For example, crystalline A / M / X materials are APb[Br y I 1-y ]3, APb[Br y Cl 1-y ]3, APb[I y Cl 1-y ]3, ASn[Br y I 1-y ]3, ASn[Br y Cl 1-y ]3, ASn[I y Cl 1-y ]3, where y is greater than 0 and less than 1, and A is a cation as described herein. y may be from 0.01 to 0.99. For example, y may be from 0.05 to 0.95 or from 0.1 to 0.9.
[0152] For example, crystalline A / M / X materials are CH3NH3Pb[Br y I 1-y ]3, CH3NH3Pb[Br y Cl 1-y ]3, CH3NH3Pb[I y Cl 1-y ]3, CH3NH3Sn[Br y I 1-y ]3, CH3NH3Sn[Br y Cl 1-y ]3, CH3NH3Sn[I y Cl 1-y ]3, CsPb[Br y I 1-y ]3, CsPb[Br y Cl 1-y ]3, CsPb[I y Cl 1-y ]3, CsSn[Br y I1-y ]3, CsSn[Br y Cl 1-y ]3, CsSn[I y Cl 1-y ]3, (H2N-C(H)=NH2)Pb[Br y I 1-y ]3, (H2N-C(H)=NH2)Pb[Br y Cl 1-y ]3, (H2N-C(H)=NH2)Pb[I y Cl 1-y ]3, (H2N-C(H)=NH2)Sn[Br y I 1-y ]3, (H2N-C(H)=NH2)Sn[Br y Cl 1-y ]3, and (H2N-C(H)=NH2)Sn[I y Cl 1-y ]3 (wherein y is greater than 0 and less than 1, for example y may be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9),
[0153] In a preferred embodiment, the perovskite has the formula (ID): [A I x A II 1-x ]M[X I y X II 1-y ]3(ID) (In the formula, A I and A II is as defined above for A, M is as defined above, and X I and X II is as defined above for X, and both x and y are greater than 0 and less than 1. In a preferred embodiment, the perovskite I and A II are (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) +, (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + and M is selected from Pb 2+ Or Sn 2+ and X I and X II are respectively, Br - , Cl - and I - is selected from.
[0154] For example, crystalline A / M / X materials are (Cs x Rb 1-x )Pb(Br y Cl 1-y )3, (Cs x Rb 1-x )Pb(Br y I 1-y )3, and (Cs x Rb 1-x )Pb(Cl y I 1-y )3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[Br y I 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[Br y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[I y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[Br y I 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[Br y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[I y Cl1-y 3、[(H2N - C(H)=NH2) x Cs 1-x Pb[Br y I 1-y 3、[(H2N - C(H)=NH2) x Cs 1-x Pb[Br y Cl 1-y 3、[(H2N - C(H)=NH2) x Cs 1-x Pb[I y Cl 1-y 3、[(CH3NH3) x (H2N - C(H)=NH2) 1-x Sn[Br y I 1-y 3、[(CH3NH3) x (H2N - C(H)=NH2) 1-x Sn[Br y Cl 1-y 3、[(CH3NH3) x (H2N - C(H)=NH2) 1-x Sn[I y Cl 1-y 3、[(CH3NH3) x Cs 1-x Sn[Br y I 1-y 3、[(CH3NH3) x Cs 1-x Sn[Br y Cl 1-y 3、[(CH3NH3) x Cs 1-x Sn[I y Cl 1-y 3、[(H2N - C(H)=NH2) x Cs 1-x Sn[Br y I 1-y 3、[(H2N - C(H)=NH2) x Cs 1-x Sn[Br y Cl 1-y 3、and [(H2N - C(H)=NH2) x Cs 1-x Sn[I y Cl 1-y]3, wherein x and y are both greater than 0 and less than 1, for example x and y may both be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9.
[0155] In one embodiment, the perovskite has the formula (IE): A[M I z M II 1-z ]X3(IE) (In the formula, M I and M II is as defined above for M, A and X are as defined above, and z is greater than 0 and less than 1. In a preferred embodiment, A is a perovskite of (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + Selected from M I is Pb 2+ And M II is Sn 2+ and X is Br - , Cl - and I - is selected from.
[0156] For example, crystalline A / M / X materials are CH3NH3[Pb z Sn 1-z ]Cl3, CH3NH3[Pb z Sn 1-z ]Br3, CH3NH3[Pb z Sn 1-z ]I3, Cs[Pb z Sn 1-z ]Cl3, Cs[Pb z Sn 1-z]Br3, Cs[Pb z Sn 1-z ]I3, (H2N-C(H)=NH2)[Pb z Sn 1-z ]Cl3, (H2N-C(H)=NH2)[Pb z Sn 1-z ]Br3 and (H2N-C(H)=NH2)[Pb z Sn 1-z ]I3 (wherein z is greater than 0 and less than 1, for example z may be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9).
[0157] In one embodiment, the perovskite has formula (IF): [A I x A II 1-x ][M I z M II 1-z ]X3(IF) (In the formula, A I and A II is as defined above for A, and M I and M II is as defined above for M, X is as defined above, and x and z are both greater than 0 and less than 1. In a preferred embodiment, the perovskite I and A II are (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + Selected from M I is Pb 2+ And M II is Sn2+ and X is Br - , Cl - and I - Selected from: A I and A II For example, (H2N-C(H)=NH2) + and Cs + or (CH3NH3), respectively. + and (H2N-C(H)=NH2) + Alternatively, Cs + and Rb + may be also possible.
[0158] For example, crystalline A / M / X materials are [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]Cl3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]Br3,[(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]I3, [(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ]Cl3, [(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ]Br3,[(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ]I3, [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ]Cl3, [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ]Br3, [(H2N-C(H)=NH2) x Cs1-x ][Pb z Sn 1-z ]I3 (wherein x and z are both greater than 0 and less than 1, for example x and z may each be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9).
[0159] In one embodiment, the perovskite has formula (IG): A[M I z M II 1-z ][X I y X II 1-y ]3(IG) (wherein A is as defined above, M I and M II is as defined above for M, and X I and X II is as defined above for X, and y and z are both greater than 0 and less than 1. In a preferred embodiment, A is a perovskite compound represented by the formula (CH3NH3). + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + Selected from M I is Pb 2+ And M II is Sn 2+ and X I and X II are respectively, Br - , Cl - and I - is selected from.
[0160] For example, a crystalline A / M / X material is A[Pbz Sn 1-z ][Br y I 1-y ]3, A[Pb z Sn 1-z ][Br y Cl 1-y ]3, A[Pb z Sn 1-z ][I y Cl 1-y
[0033] 3, where y and z are both greater than 0 and less than 1, and A is a cation as described herein. Each of y and z may be from 0.01 to 0.99. For example, each of y and z may be from 0.05 to 0.95 or from 0.1 to 0.9.
[0161] For example, crystalline A / M / X materials are CH3NH3[Pb z Sn 1-z ][Br y I 1-y ]3, CH3NH3[Pb z Sn 1-z ][Br y Cl 1-y ]3, CH3NH3[Pb z Sn 1-z ][I y Cl 1-y ]3, Cs[Pb z Sn 1-z ][Br y I 1-y ]3, Cs[Pb z Sn 1-z ][Br y Cl 1-y ]3, Cs[Pb z Sn 1-z ][I y Cl 1-y ]3, (H2N-C(H)=NH2)[Pb z Sn 1-z ][Br y I 1-y ]3, (H2N-C(H)=NH2)[Pb z Sn 1-z ][Br y Cl 1-y ]3, and (H2N-C(H)=NH2)[Pbz Sn 1-z ][I y Cl 1-y ]3, wherein y and z are both greater than 0 and less than 1, for example y and z may each be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9.
[0162] In a preferred embodiment, the perovskite has the formula (IH): [A I x A II 1-x ][M I z M II 1-z ][X I y X II 1-y ]3(IH) (In the formula, A I and A II is as defined above for A, and M I and M II is as defined above for M, and X I and X II is as defined above for X, and x, y, and z are each greater than 0 and less than 1. In a preferred embodiment, the perovskite I and A II are (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + Selected from M I is Pb 2+ And M II is Sn 2+ and XI and X II are respectively, Br - , Cl - and I - is selected from.
[0163] For example, crystalline A / M / X materials are [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ][Br y I 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ][Br y Cl 1-y ]3, (CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ][I y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ][Br y I 1-y ]3, [(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ][Br y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ][I y Cl 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ][Br y I 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ][Br y Cl1-y ]3, and [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ][I y Cl 1-y ]3, wherein x, y and z are each greater than 0 and less than 1, for example x, y and z may each be from 0.01 to 0.99 or from 0.05 to 0.95 or from 0.1 to 0.9.
[0164] In one embodiment, a = 2, b = 1 and c = 4. In this embodiment, the crystalline A / M / X material has the formula (II): [A]2[M][X]4(II) (wherein [A] includes one or more A cations which are monocations; [M] includes one or more M cations which are dications of a metal or metalloid; and [X] includes one or more X anions which are halide anions). ("2D layered perovskite"), in which the A and M cations and X anion are as defined above.
[0165] In another embodiment, a = 2, b = 1 and c = 6. In this embodiment, the crystalline A / M / X material is then represented by formula (III): [A]2[M][X]6(III) (wherein [A] includes one or more A cations which are monocations; [M] includes one or more M cations which are metal or metalloid tetracations; and [X] includes one or more X anions which are halide anions). The hexahalometallate may include:
[0166] The hexahalometalates of formula (III) may, in preferred embodiments, be mixed monocation hexahalometalates. In mixed monocation hexahalometalates, [A] comprises at least two A cations that are monocations, [M] comprises at least one M cation that is a metal or metalloid tetracation (and typically, [M] comprises a single M cation that is a metal or metalloid tetracation), and [X] comprises at least one X anion that is a halide anion (and typically, [X] comprises a single halide anion or two types of halide anions). In mixed metal hexahalometalates, [A] comprises at least one monocation (and typically, [A] is a single monocation or two types of monocations), and [M] comprises at least two metal or metalloid tetracations (e.g., Ge). 4+ and Sn 4+ ), and [X] comprises at least one halide anion (and typically, [X] is a single halide anion or two types of halide anions). In mixed halide hexahalometalates, [A] comprises at least one monocation (and typically, [A] is a single monocation or two types of monocations), [M] comprises at least one metal or metalloid tetracation (and typically, [M] is a single metal tetracation), and [X] comprises at least two halide anions, e.g., Br - and Cl - Or Br - and I - Includes.
[0167] [A] may comprise any suitable monocation, for example at least one A monocation selected from those described above for perovskites. In the case of hexahalometalates, each A cation is typically Li + , Na + , K + , Rb + , Cs + , NH4 +and a monovalent organic cation. The monovalent organic cation is an organic cation with a single positive charge, which may have a molecular weight of, for example, 500 g / mol or less. For example, [A] is Li + , Na + , K + , Rb + , Cs + , NH4 + and a monovalent organic cation. [A] is preferably Rb + , Cs + , NH4 + and at least one A cation which is a monocation selected from a monovalent organic cation. For example, [A] is Li + , Na + , K + , Rb + , Cs + and NH4 + In another embodiment, [A] may be at least one monovalent organic A cation. For example, [A] may be a single monovalent organic A cation. In one embodiment, [A] is (CHNH) + In another embodiment, [A] is (H2N-C(H)=NH2) + It is.
[0168] Preferably, [A] contains two or more types of A cations. [A] may be a single A monocation or in fact two monocations, each of which may be independently selected from K + , Rb + , Cs + , NH4 + , (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (N(CH2CH3)4) + , (N(CH2CH2CH3)4) + , (H2N-C(H)=NH2) + and (H2N-C(CH3)=NH2) + is selected from.
[0169] [M] may include one or more M cations selected from suitable metal or metalloid tetracations. Metals include elements in groups 3-12 of the periodic table as well as Ga, In, Tl, Sn, Pb, Bi, and Po. Metalloids include Si, Ge, As, Sb, and Te. For example, [M] may be Ti 4+ , V 4+ , Mn 4+ , Fe 4+ , Co 4+ , Zr 4+ , Nb 4+ , Mo 4+ , Ru 4+ , Rh 4+ , Pd 4+ , Hf 4+ , Ta 4+ , W 4+ , Re 4+ , Os 4+ , Ir 4+ , Pt 4+ , Sn 4+ , Pb 4+ , Po 4+ , Si 4+ , Ge 4+ and Te 4+ Typically, [M] is selected from the group consisting of Pd 4+ , W 4+ , Re 4+ , Os 4+ , Ir 4+ , Pt 4+ , Sn 4+ , Pb 4+ , Ge 4+ and Te 4+ For example, [M] is selected from the group consisting of Pd 4+ , W 4+ , Re 4+ , Os 4+ , Ir 4+ , Pt 4+ , Sn 4+ , Pb 4+ , Ge 4+ and Te 4+ It may also be a tetracation of a single metal or metalloid selected from:
[0170] Typically, [M] is Sn 4+ , Te 4+ , Ge 4+ and Re 4+ In one embodiment, [M] is selected from the group consisting of Pb 4+ , Sn 4+ , Te 4+ , Ge 4+ and Re 4+ At least one M cation is a tetracation of a metal or metalloid selected from the group consisting of Pb 4+ , Sn 4+ , Te 4+ and Ge 4+ Preferably, [M] is at least one metal or metalloid tetracation selected from Sn 4+ , Te 4+ and Ge 4+ As discussed above, the hexahalometallate compound may be a mixed metal or single metal hexahalometallate. Preferably, the hexahalometallate compound is a single metal hexahalometallate compound. More preferably, [M] is selected from the group consisting of Sn 4+ , Te 4+ and Ge 4+ For example, [M] is Te 4+ For example, [M] may be a single metal or metalloid tetracation, 4+ Most preferably, [M] is a single metal or metalloid tetracation, 4+ is a single metal or metalloid tetracation where
[0171] [X] may include at least one X anion that is a halide anion. Thus, [X] may include F - , Cl - , Br - and I -Typically, [X] is selected from Cl - , Br - and I - The hexahalometallate compound may be a mixed halide hexahalometallate or a single halide hexahalometallate. When the hexahalometallate is mixed, [X] is selected from F - , Cl - , Br - and I - Typically, in the mixed halide compounds, [X] is selected from F - , Cl - , Br - and I - The compound includes two halide anions selected from:
[0172] In some embodiments, [A] is a single monocation and [M] is a single metal or metalloid tetracation. Thus, a crystalline A / M / X material can have, for example, the formula (IIIA): A2M[X]6(IIIA) (wherein A is a monocation, M is a metal or metalloid tetracation, and [X] is at least one halide anion). [X] may include a hexahalometallate compound of the formula: - , Cl - , Br - and I - Preferably selected from Cl - , Br - and I - In formula (IIIA), [X] is preferably one, two or three halide anions selected from the group consisting of Cl - , Br - and I - wherein the anion is one or two halide anions selected from:
[0173] The crystalline A / M / X material can be, for example, a compound represented by formula (IIIB): A2MX6-y X' y (IIIB) (wherein A is a monocation (i.e., a second cation), M is a metal or metalloid tetracation (i.e., a first cation), X and X' are each independently a (different) halide anion (i.e., two second anions), and y is 0 to 6. When y is 0 or 6, the hexahalometallate compound is a single halide compound. When y is between 0.01 and 5.99, the compound is a mixed halide hexahalometallate compound. When the compound is a mixed halide compound, y may be between 0.05 and 5.95. For example, y may be between 1.00 and 5.00.
[0174] The hexahalometalate compound is, for example, A2SnF 6-y Cl y , A2SnF 6-y Br y , A2SnF 6-y I y , A2SnCl 6-y Br y , A2SnCl 6-y I y , A2SnBr 6-y I y , A2TeF 6-y Cl y , A2TeF 6-y Br y , A2TeF 6-y I y , A2TeCl 6-y Br y , A2TeCl 6-y I y , A2TeBr 6-y I y , A2GeF 6-y Cl y , A2GeF 6-y Br y , A2GeF 6-y I y , A2GeCl 6-y Br y , A2GeCl 6-y Iy , A2GeBr 6-y I y , A2ReF 6-y Cl y , A2ReF 6-y Br y , A2ReF 6-y I y , A2ReCl 6-y Br y , A2ReCl 6-y I y or A2ReBr 6-y I y (Wherein, A is K + , Rb + , Cs + , (R 1 NH3) + , (NR 2 4) + or (H2N-C(R 1 )=NH2) + and R 1 is H, substituted or unsubstituted C 1~20 is an alkyl group or a substituted or unsubstituted aryl group, R 2 is a substituted or unsubstituted C 1~10 Optionally, y is from 0.01 to 5.99. When the hexahalometallate compound is a mixed halide compound, y is typically from 1.00 to 5.00. A may be as defined above. For example, A can be Cs + , NH4 + , (CH3NH3) + , (CH3CH2NH3) + , (N(CH3)4) + , (N(CH2CH3)4) + , (H2N-C(H)=NH2) + or (H2N-C(CH3)=NH2) + , e.g. Cs + , NH4 + or (CH3NH3) + may be also possible.
[0175] The hexahalometalate compound is typically A2SnF 6-y Cl y , A2SnF6-y Br y , A2SnF 6-y I y , A2SnCl 6-y Br y , A2SnCl 6-y I y or A2SnBr 6-y I y (Wherein, A is K + , Rb + , Cs + , (R 1 NH3) + , (NR 2 4) + or (H2N-C(R 1 )=NH2) + or A is as defined herein, and R 1 is H, substituted or unsubstituted C 1~20 an alkyl group or a substituted or unsubstituted aryl group, or R 2 is a substituted or unsubstituted C 1~10 and y is an alkyl group, and y is 0 to 6.
[0176] In another embodiment, the hexahalometalate compound is A2GeF 6-y Cl y , A2GeF 6-y Br y , A2GeF 6-y I y , A2GeCl 6-y Br y , A2GeCl 6-y I y or A2GeBr 6-y I y (Wherein, A is K + , Rb + , Cs + , (R 1 NH3) + , (NR 2 4) + or (H2N-C(R 1 )=NH2) + or A is as defined herein, and R 1 is H, substituted or unsubstituted C 1~20is an alkyl group or a substituted or unsubstituted aryl group, R 2 is a substituted or unsubstituted C 1~10 an alkyl group, and y is 0 to 6.
[0177] The hexahalometalate compound is, for example, A2TeF 6-y Cl y , A2TeF 6-y Br y , A2TeF 6-y I y , A2TeCl 6-y Br y , A2TeCl 6-y I y or A2TeBr 6-y I y (Wherein, A is K + , Rb + , Cs + , (R 1 NH3) + , (NR 2 4) + or (H2N-C(R 1 )=NH2) + or A is as defined herein, and R 1 is H, substituted or unsubstituted C 1~20 is an alkyl group or a substituted or unsubstituted aryl group, R 2 is a substituted or unsubstituted C 1~10 an alkyl group, where y is 0 to 6, or y is as defined herein.
[0178] In many cases, y is between 1.50 and 2.50. For example, y may be between 1.80 and 2.20. This may occur when the compound is produced using 2 equivalents of AX' and 1 equivalent of MX4, as described below.
[0179] In some embodiments, all ions are a single anion or cation. Thus, the crystalline A / M / X material has the formula (IIIC): A2MX6(IIIC) where A is a monocation, M is a metal or metalloid tetracation, and X is a halide anion. A, M and X may be as defined herein.
[0180] The hexahalometalate compound may be A2SnF6, A2SnCl6, A2SnBr6, A2SnI6, A2TeF6, A2TeCl6, A2TeBr6, A2TeI6, A2GeF6, A2GeCl6, A2GeBr6, A2GeI6, A2ReF6, A2ReCl6, A2ReBr6, or A2ReI6 (wherein A is K). + , Rb + , Cs + , (R 1 NH3) + , (NR 2 4) + or (H2N-C(R 1 )=NH2) + and R 1 is H, substituted or unsubstituted C 1~20 is an alkyl group or a substituted or unsubstituted aryl group, R 2 is substituted or unsubstituted C 1~10 A may be as defined herein. Preferably, the hexahalometalate compound is Cs2SnI6, Cs2SnBr6, Cs2SnBr 6-y I y , Cs2SnCl 6-y I y , Cs2SnCl 6-y Br y , (CH3NH3)2SnI6, (CH3NH3)2SnBr6, (CH3NH3)2SnBr 6-y I y , (CH3NH3)2SnCl 6-y I y , (CH3NH3)2SnCl 6-y Br y , (H2N-C(H)=NH2)2SnI6, (H2N-C(H)=NH2)2SnBr6, (H2N-C(H)=NH2)2SnBr 6-y I y, (H2N-C(H)=NH2)2SnCl 6-y I y or (H2N-C(H)=NH2)2SnCl 6-y Br y In the formula, y is 0.01 to 5.99. For example, the hexahalometalate compound may be (CH3NH3)2SnI6, (CH3NH3)2SnBr6, (CH3NH3)2SnCl6, (H2N-C(H)=NH2)2SnI6, (H2N-C(H)=NH2)2SnBr6, or (H2N-C(H)=NH2)2SnCl6. The hexahalometalate compound may be Cs2SnI6, Cs2SnBr6, Cs2SnCl 6-y Br y , (CH3NH3)2SnI6, (CH3NH3)2SnBr6 or (H2N-C(H)=NH2)2SnI6.
[0181] The crystalline A / M / X material may comprise a bismuth or antimony halogenometallate. For example, the crystalline A / M / X material may comprise a halogenometallate compound comprising (i) one or more monocations ([A]) or one or more dications ([B]), (ii) one or more metal or metalloid trications ([M]), and (iii) one or more halide anions ([X]). The compound may have the formula BBiX5, B2BiX7, or B3BiX9, where B is (H3NCH2NH3). 2+ , (H3N(CH2)2NH3) 2+ , (H3N(CH2)3NH3) 2+ , (H3N(CH2)4NH3) 2+ , (H3N(CH2)5NH3) 2+ , (H3N(CH2)6NH3) 2+ , (H3N(CH2)7NH3) 2+ , (H3N(CH2)8NH3) 2+ or (H3N-C6H4-NH3) 2+ and X is I - , Br - Or Cl - and preferably I - The compound may be a compound represented by the formula:
[0182] In a further embodiment, the crystalline A / M / X material may be a double perovskite. Such compounds are defined in WO2017 / 037448, the entire contents of which are incorporated herein by reference. Typically, the compound has the formula (IV): [A]2[B + ][B 3+ ][X]6(IV) (wherein [A] comprises one or more A cations, which are monocations as defined herein, and [B + ] and [B 3+ ] is equal to [M], where M includes one or more M cations that are monocations and one or more M cations that are tricationic, and [X] includes one or more X anions that are halide anions. It is a double perovskite compound.
[0183] [B + The one or more M cations which are monocations in the formula (I) are typically selected from metal and semimetal monocations. Preferably, the one or more M cations which are monocations are Li + , Na + , K + , Rb + , Cs + , Cu + , Ag + , Au + and Hg + More preferably, the one or more M cations that are monocations are selected from Cu + , Ag + and Au + Most preferably, the one or more M cations that are monocations are selected from Ag + and Au + For example, [B + ] is Ag + or [B + ] is Au + It may also be one monocation in which
[0184] [B 3+The one or more M cations in the trication are typically selected from metal and metalloid trications. Preferably, the one or more M cations in the trication are selected from Bi 3+ , Sb 3+ , Cr 3+ , Fe 3+ , Co 3+ , Ga 3+ , As 3+ , Ru 3+ , Rh 3+ , In 3+ , Ir 3+ and Au 3+ More preferably, the one or more M cations that are trications are selected from Bi 3+ and Sb 3+ For example, [B 3+ ] is Bi 3+ or [B 3+ ] is Sb 3+ Bismuth has relatively low toxicity compared to heavy metals, such as lead. In some embodiments, the monocation ([B + ]) is one or more M cations, Cu + , Ag + and Au + and a trication ([B 3+ ]) is Bi 3+ and Sb 3+ is selected from.
[0185] An exemplary double perovskite is Cs2BiAgBr6.
[0186] Typically, when the compound is a double perovskite, it has the formula (IVa): A2B + B 3+ [X]6(IVa) (wherein A cation is as defined herein; B + is a monocation, M, as defined herein, and B 3+is the M cation, which is a trication as defined herein, and [X] is one or more X anions, which are halide anions, e.g., two or more halide anions, preferably a single halide anion. It is a compound of the formula:
[0187] In yet another embodiment, the compound has the formula (V): [A]4[B + ][B 3+ ][X]8(V) (In the formula, [A], [B + ], [B 3+ ] and [X] are as defined above. In some embodiments, the layered double perovskite compound may be a layered double perovskite compound of formula (Va): A4B + B 3+ [X]8(Va) (wherein A cation is as defined herein; B + is a monocation, M, as defined herein, and B 3+ is an M cation which is a trication as defined herein, and [X] is one or more X anions which are halide anions, e.g., two or more halide anions, preferably a single halide anion or two halide anions. It is a double perovskite compound.
[0188] In yet another embodiment, the compound has formula (VI): [A]4[M][X]6(VI) (wherein [A], [M] and [X] are as defined above (e.g., for compounds of formula (I) or (II)). However, preferably the compound is not a compound of formula (VI). When the compound is a compound of formula (VI), it is preferably a compound of formula (VIA) [A I A II ]4[M][X]6(VIA) In another preferred embodiment, the compound of formula (VI) may be a compound of formula (VIB): [A]4[M][X I X II ]6(VIB) In yet another preferred embodiment, the compound of formula (VI) may be a compound of formula (VIC): [A I A II ]4[M][X I X II ]6(VIC) i.e., a compound of formula (VI) where [A] comprises two A monocations and [X] comprises two X anions. In formulas (VIa), (VIb) and (VIc), [A], [M] and [X] are each as defined above (e.g., for compounds of formula (I) or (II)).
[0189] In another embodiment, a = 1, b = 1 and c = 4. In this embodiment, the crystalline A / M / X material is then represented by formula (VII): [A][M][X]4(VII) (wherein [A] includes one or more A cations that are monocations; [M] includes one or more M cations that are metal or metalloid trications; and [X] includes one or more X anions that are halide anions). The A monocation and M trication are as defined herein. An exemplary compound of formula (VII) is AgBiI4.
[0190] It should be understood that the present invention also encompasses methods of making variations of the above structures (I), (II), (III), (IV), (V), (VI) and (VII) where one or more of the associated a, b and c values are non-integer values.
[0191] Preferably, the formula [A] a [M]b [X] c The compound of formula [A][M][X]3, the compound of formula [A]4[M][X]6 or the compound of formula [A]2[M][X]6. For example, in a preferred embodiment, a [M] b [X] c The compound of formula (I) is, for example, a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), or a compound of formula (IIIB), (IIIC), (VIA), (VIB) or (VIC). a [M] b [X] c is a compound of formula (I), for example a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH).
[0192] In some embodiments, the formula [A] a [M] b [X] c Compounds of formula [A] are compounds in which [A] contains two or more different A cations. For example, [A] may contain two types of cations. In some embodiments, the compound of formula [A] a [M] b [X] c Compounds of formula [A] are compounds in which [X] comprises two or more different X anions. For example, [X] may contain two types of anions, such as halide anions. In some embodiments, compounds of formula [A] a [M] b [X] c Compounds of formula (I) are compounds in which [M] contains two or more different M cations. For example, [X] contains two types of anions, e.g., Sn 2+ and Pb 2+ may also contain
[0193] In one aspect of each of these embodiments, a compound of formula [A] a [M] b [X] cis a compound in which [A] contains two or more different A cations and [X] contains two or more different X anions. For example, [A] may contain two types of A cations and [X] may contain two types of X anions (e.g., two types of halide anions).
[0194] In one aspect of each of these embodiments, a compound of formula [A] a [M] b [X] c A compound is a compound in which [A] contains two or more different A cations and [M] contains two or more different M cations. For example, [A] may contain two types of A cations and [M] may contain two types of M cations (e.g., Sn 2+ and Pb 2+ ) may also be contained.
[0195] In one aspect of each of these embodiments, a compound of formula [A] a [M] b [X] c Compounds of formula (I) are compounds in which [X] contains two or more different X anions and [M] contains two or more different M cations. For example, [X] may contain two types of X anions (e.g., two types of halide anions) and [M] may contain two types of M cations (e.g., Sn 2+ and Pb 2+ ) may also be contained.
[0196] In one aspect of each of these embodiments, a compound of formula [A] a [M] b [X] c is a compound in which [A] contains two or more different A cations, [X] contains two or more different X anions, and [M] contains two or more different M cations. For example, [A] may contain two types of A cations, [X] may contain two types of X anions (e.g., two types of halide anions), and [M] may contain two types of M cations (e.g., Sn 2+ and Pb 2+ ) may also be contained.
[0197] charge transport layer The substrate may include one or more additional layers. For example, the substrate may further include a layer of a charge transport material. Preferably, the layer of charge transport material is disposed on the charge recombination layer. Typically, the layer of charge transport material is disposed directly on the charge recombination layer. Alternatively, there may be an intervening layer between the layer of charge transport material and the charge recombination layer. Thus, the substrate may include the following layers in the following order: a layer of charge transport material (typically an n-type material as described herein, but which may alternatively be a p-type material); ·Charge recombination layer, ·Photoactive region.
[0198] Typically, the layer of crystalline A / M / X material is disposed directly on the layer of charge transport material. Alternatively, there may be an intervening layer between the layer of charge transport material and the layer of crystalline A / M / X material. Typically, the layer of charge transport material is disposed directly on the charge recombination layer and the layer of crystalline A / M / X material is disposed directly on the layer of charge transport material. Thus, a multijunction device made in accordance with the present invention may include the following layers in the following order: Layers of crystalline A / M / X materials, a layer of charge transport material (typically an n-type material as described herein, but which may alternatively be a p-type material); ·Charge recombination layer, ·Photoactive region.
[0199] In one embodiment, the layer of charge transport material is a layer of electron transporting (n-type) material. In another embodiment, the layer of charge transport material is a layer of hole transporting (p-type) material. Typically, the layer of charge transport material is a layer of electron transporting (n-type) material.
[0200] Typically, the charge transport material is soluble in dimethylformamide. Thus, the charge transport material may be dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof.
[0201] Typically, the layer of the charge transport material has a thickness of less than 1000 nm, or less than 500 nm, or less than 250 nm, preferably less than 100 nm. For example, the layer of the charge transport material may have a thickness of 1 to 500 nm, for example 5 to 250 nm, or 10 to 75 nm.
[0202] Examples of electron transporting (n-type) materials are known to those skilled in the art. Suitable n-type materials may be organic or inorganic. Suitable inorganic n-type materials may be selected from metal oxides, metal sulfides, metal selenides, metal tellurides, perovskites, amorphous Si, n-type Group IV semiconductors, n-type Group III-V semiconductors, n-type Group II-VI semiconductors, n-type Group I-VII semiconductors, n-type Group IV-VI semiconductors, n-type Group V-VI semiconductors, and n-type Group II-V semiconductors, any of which may be doped or undoped. More typically, n-type materials are selected from metal oxides, metal sulfides, metal selenides, and metal tellurides.
[0203] Thus, the n-type layer may comprise an inorganic material selected from oxides of titanium, tin, zinc, niobium, tantalum, tungsten, indium, gallium, neodymium, palladium or cadmium, or oxides of a mixture of two or more of said metals. For example, the n-type layer may comprise TiO2, SnO2, ZnO, Nb2O5, Ta2O5, WO3, W2O5, In2O3, Ga2O3, Nd2O3, PbO or CdO. Other suitable n-type materials that may be used include sulfides of cadmium, tin, copper or zinc (including sulfides of a mixture of two or more of said metals). For example, the sulfides may be FeS2, CdS, ZnS, SnS, BiS, SbS or Cu2ZnSnS4.
[0204] The n-type layer may, for example, comprise a selenide of cadmium, zinc, indium or gallium, or a selenide of a mixture of two or more of said metals, or a telluride of cadmium, zinc, cadmium or tin, or a telluride of a mixture of two or more of said metals. For example, the selenide may be Cu(In,Ga)Se2. Typically, the telluride is a telluride of cadmium, zinc, cadmium or tin. For example, the telluride may be CdTe.
[0205] The n-type layer may comprise an inorganic material selected from, for example, an oxide of titanium (e.g., TiO2), an oxide of tin (e.g., SnO2), an oxide of zinc (e.g., ZnO), an oxide of niobium, tantalum, tungsten, indium, gallium, neodymium, palladium, cadmium, or an oxide of a mixture of two or more of the aforementioned metals, a sulfide of cadmium, tin, copper, zinc, or a sulfide of a mixture of two or more of the aforementioned metals, a selenide of cadmium, zinc, indium, gallium, or a selenide of a mixture of two or more of the aforementioned metals, or a telluride of cadmium, zinc, cadmium, or tin, or a telluride of a mixture of two or more of the aforementioned metals.
[0206] Examples of other semiconductors that may be suitable n-type materials, for example when n-doped, include Group IV element or compound semiconductors, amorphous Si, Group III-V semiconductors (e.g., gallium arsenide), Group II-VI semiconductors (e.g., cadmium selenide), Group I-VII semiconductors (e.g., cuprous chloride), Group IV-VI semiconductors (e.g., lead selenide), Group V-VI semiconductors (e.g., bismuth telluride), and Group II-V semiconductors (e.g., cadmium arsenide).
[0207] Other n-type materials may also be used, including organic and polymeric electron transport materials and electrolytes. Suitable examples include fullerenes or fullerene derivatives (e.g., C 60 , C 70 , Phenyl-C 61 -Butyric acid methyl ester (PCBM), PC 71 BM (i.e., phenyl C 71 butyric acid methyl ester), bis[C60 ]BM (i.e., bis-C 60 butyric acid methyl ester) and 1',1",4',4"-tetrahydro-di[1,4]methanonaphthaleno[1,2:2',3',56,60:2",3"][5,6]fullerene-C 60 (ICBA)), organic electron transporting materials including perylene or its derivatives, or poly{[N,N0-bis(2-octyldodecyl)-naphthalene-1,4,5,8-bis(dicarboximide)-2,6-diyl]-alt-5,50-(2,20-bithiophene)} (P(NDI2OD-T2)).
[0208] Preferably, the n-type material is phenyl-C61-butyric acid methyl ester (PCBM).
[0209] Examples of hole-transporting (p-type) materials are known to those skilled in the art. A p-type material may be a single p-type compound or elemental material, or a mixture of two or more p-type compounds or elemental materials, which may be undoped or doped with one or more dopant elements.
[0210] The p-type material may comprise an inorganic or an organic p-type material. Typically, the p-type material is an organic p-type material.
[0211] Suitable p-type materials can be selected from polymeric or molecular hole transporters, such as spiro-OMeTAD (2,2',7,7'-tetrakis-(N,N-di-p-methoxyphenylamine)9,9'-spirobifluorene), P3HT (poly(3-hexylthiophene)), PCPDTBT (poly[2,1,3-benzothiadiazole-4,7-diyl[4,4-bis(2-ethylhexyl)-4H-cyclopenta[2,1-b:3,4-b']dithiophene-2,6-diyl]]), PVK (poly(N-vinylcarbazole)), HTM-TFSI (1-hexyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide), Li-TFSI (lithium bis(trifluoromethanesulfonyl)imide), spiro-OMETAD +-Bis(trifluoromethanesulfonyl)imide - (spiro(TFSI)2), tBP (tert-butylpyridine), m-MTDATA (4,4',4"-tris(methylphenylphenylamino)triphenylamine), MeOTPD (N,N,N',N'-tetrakis(4-methoxyphenyl)-benzidine), BP2T (5,5'-di(biphenyl-4-yl)-2,2'-bithiophene), di-NPB (N,N'-di-[(1-naphthyl)-N,N'-diphenyl]-1,1'-biphenyl)-4,4'-diamine), α-NPB (N,N'-di(naphthalen-1-yl)-N,N'-diphenyl-benzidine), TNATA (4,4',4"-tris-(N-(naphthyl)-N-phenylamine)triphenylamine), The p-type material may include carbon nanotubes. Typically, the p-type material is selected from spiro-OMeTAD, P3HT, PCPDTBT, spiro(TFSI)2 and PVK. Preferably, the p-type material is spiro-OMeTAD or spiro(TFSI)2.
[0212] Suitable p-type materials also include molecular hole transporters, polymeric hole transporters and copolymeric hole transporters. A p-type material may be, for example, a molecular hole transport material, a polymer or copolymer that includes one or more of the following moieties: thiophenyl, phenelenyl, dithiazolyl, benzothiazolyl, diketopyrrolopyrrolyl, ethoxydithiophenyl, amino, triphenylamino, carbazolyl, ethylenedioxythiophenyl, dioxythiophenyl, or fluorenyl.
[0213] The p-type material may be doped, for example, with tert-butylpyridine and LiTFSI. The p-type material may be doped to increase the hole density. The p-type material may be doped, for example, with NOBF4 (nitrosonium tetrafluoroborate) to increase the hole density.
[0214] In other embodiments, the p-type layer may include an inorganic hole transporter. For example, the p-type layer may include inorganic hole transporters including oxides of nickel (e.g., NiO), oxides of vanadium, copper or molybdenum, CuI, CuBr, CuSCN, Cu2O, CuO or CIS, perovskite, amorphous Si, p-type Group IV semiconductors, p-type Group III-V semiconductors, p-type Group II-VI semiconductors, p-type Group I-VII semiconductors, p-type Group IV-VI semiconductors, p-type Group V-VI semiconductors, and p-type Group II-V semiconductors (wherein the inorganic material may be doped or undoped). The p-type layer may be a dense layer of the inorganic hole transporter.
[0215] The p-type material may be an inorganic p-type material, such as an oxide of nickel, vanadium, copper or molybdenum, CuI, CuBr, CuSCN, CuO, CuO or CIS, amorphous Si, a p-type Group IV semiconductor, a p-type Group III-V semiconductor, a p-type Group II-VI semiconductor, a p-type Group I-VII semiconductor, a p-type Group IV-VI semiconductor, a p-type Group V-VI semiconductor, and a p-type Group II-V semiconductor (wherein the inorganic material may be doped or undoped). The p-type material may comprise an inorganic hole transporter, for example selected from CuI, CuBr, CuSCN, CuO, CuO and CIS.
[0216] In one embodiment, the present invention includes forming a substrate by disposing a layer of a charge transport material described herein on a charge recombination layer. Typically, a composition comprising a charge transport material, preferably a solution comprising a charge transport material, is disposed on the charge recombination layer. The solution comprising a charge transport material is typically disposed on the charge recombination layer by a solution-phase deposition method, such as gravure coating, slot die coating, screen printing, inkjet printing, doctor blade coating, spray coating, roll-to-roll (R2R) processing, or spin coating, preferably by spin coating.
[0217] Typically, the solvent in the solution containing the charge transport material is selected from chlorobenzene, chloroform, anisole, toluene, tetrahydrofuran, xylene, or mixtures thereof. For example, the process of forming a substrate by disposing a layer of a charge transport material over a charge recombination layer may include: preparing a solution of a charge transport material, preferably a solution of an electron transport (n-type) material in chlorobenzene, chloroform or a mixture thereof, more preferably the electron transport (n-type) material is PCBM, A charge transport material is deposited on the charge recombination layer by spin coating. may include:
[0218] charge recombination layer The method of the present invention may further include the step of preparing a substrate by disposing a charge recombination layer on the photoactive region by solution deposition.
[0219] Typically, the charge recombination layer comprises nanoparticles of a transparent conductive oxide. The nanoparticles create an ohmic contact between both the electron and hole transport layers, thereby allowing efficient charge transfer to the recombination layer. Moreover, such nanoparticles are easily processed using solution-based methods to form the substrate.
[0220] The transparent conductive oxide nanoparticles may include indium zinc oxide (IZO), indium tin oxide (ITO), aluminum zinc oxide (AZO), indium cadmium oxide, fluorine doped tin oxide (FTO), antimony doped tin oxide, antimony doped titanium dioxide, niobium doped tin oxide, niobium doped titanium dioxide, barium stannate, strontium vanadate, and calcium vanadate. Preferably, the transparent conductive oxide nanoparticles include indium tin oxide (ITO). Thus, the transparent conductive oxide nanoparticles may be indium tin oxide nanoparticles. Preferably, the transparent conductive oxide nanoparticles are indium tin oxide nanoparticles having a size of less than 500 nm, preferably less than 250 nm, more preferably less than 100 nm. Typically, the size of the nanoparticles can be determined by dynamic light scattering in solution or transmission electron microscopy of dried films.
[0221] The transparent conductive oxide nanoparticles may be disposed in a matrix material. The matrix material may be an inorganic or organic matrix material. It is often a dielectric matrix material, e.g. an inorganic or organic dielectric matrix material. Alternatively, it may be an electron transport matrix material. Usually, the matrix material is an organic matrix material. Typically, the organic matrix material is an electron transport organic matrix material. Suitable examples include, but are not limited to, fullerenes or fullerene derivatives (e.g., C 60 or phenyl-C61-butyric acid methyl ester (PCBM), organic electron transport materials including perylene or its derivatives, or poly{[N,N0-bis(2-octyldodecyl)-naphthalene-1,4,5,8-bis(dicarboximide)-2,6-diyl]-alt-5,50-(2,20-bithiophene)} (P(NDI2OD-T2)). Preferably, the organic matrix material includes [6,6]-phenyl-C61-butyric acid methyl ester (PCBM).
[0222] Typically, the charge recombination layer further comprises a conductive polymer. For example, the charge recombination layer may comprise p-doped polyTPD, polytriarylamine (PTAA), polythiophene. Typically, the conductive polymer comprises poly(3,4-ethylenedioxythiophene) (PEDOT) or its derivatives. For example, the conductive polymer may comprise poly(3,4-ethylenedioxythiophene) and polystyrenesulfonate (PEDOT:PSS) or poly(3,4-ethylenedioxythiophene)-tetramethacrylate (PEDOT:TMA). Preferably, the conductive polymer comprises poly(3,4-ethylenedioxythiophene) and polystyrenesulfonate (PEDOT:PSS).
[0223] The charge recombination layer may include transparent conductive oxide nanoparticles and a conductive polymer. For example, the charge recombination layer may include indium tin oxide (ITO) nanoparticles and poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate (PEDOT:PSS). The transparent conductive oxide nanoparticles may be uniformly distributed in the conductive polymer of the charge recombination layer. Alternatively, the transparent conductive oxide nanoparticles and the conductive polymer may form two separate sublayers in the charge recombination layer.
[0224] Typically, the charge recombination layer has a thickness of less than 1000 nm, for example less than 750 nm, less than 250 nm, preferably less than 100 nm. For example, the charge recombination layer may have a thickness of 5 to 500 nm, 10 to 250 nm, 20 to 150 nm, preferably 25 to 125 nm. In some embodiments, for example when the charge recombination layer is a tunnel junction, the charge recombination layer has a thickness of less than 50 nm, for example less than 30 nm, for example 20 nm or less, or for example 10 nm or less.
[0225] The charge recombination layer may be a tunnel junction. A tunnel junction is generally a very thin film, for example having a thickness of 20 nm or less, for example 10 nm or less. The film typically comprises a very thin film of highly doped n-type material interfaced with a very thin film of highly doped p-type material. This allows charge to tunnel through the junction.
[0226] Thus, in one embodiment, the charge recombination layer is a tunnel junction. Typically, the tunnel junction has a thickness of less than 30 nm, for example 20 nm or less, or 10 nm or less. The tunnel junction typically includes, more typically consists of, a first sublayer disposed on a second sublayer, one of the first and second sublayers being an n-type material and the other of the first and second sublayers being a p-type material. The n-type material may include any of the n-type materials described herein. The n-type material is generally doped with a dopant. The p-type material may include any of the p-type materials described herein. Generally, the p-type material is doped with a dopant. Dopants for doping the n- and p-type materials in the tunnel junction are known in the art.
[0227] Typically, disposing the charge recombination layer over the photoactive region includes disposing a solvent dispersion of nanoparticles of a transparent conductive oxide over the photoactive region.
[0228] Typically, the solvent is selected to be orthogonal to that used in the underlayer, e.g., the photoactive region and / or charge transport layer (if present). A solvent is orthogonal to another solvent if it does not dissolve the layer of material deposited from the other solvent. For example, the solvent may be a polar solvent, e.g., a polar protic solvent, e.g., an alcohol. For example, it may be isopropanol (2-propanol), methanol, or ethanol. It may also be a polar aprotic solvent, e.g., acetone, acetonitrile, methyl ethyl ketone.
[0229] Typically, the solvent dispersion of transparent conductive oxide nanoparticles is a dispersion of indium tin oxide nanoparticles in isopropanol.
[0230] Typically, the indium tin oxide nanoparticles comprise less than 75% by weight of the solvent dispersion (total weight of solvent plus nanoparticles), such as less than 50% by weight of the solvent dispersion. For example, the indium tin oxide nanoparticles may comprise between 0.001 and 50% by weight of the solvent dispersion, between 0.1 and 10% by weight of the solvent dispersion, between 0.5 and 5% by weight of the solvent dispersion, and preferably about 1% by weight of the solvent dispersion.
[0231] The solvent dispersion of transparent conductive oxide nanoparticles may be disposed on the photoactive area by roll-to-roll (R2R) processing, blade coating, inkjet printing or spin coating. Typically, the solvent dispersion of transparent conductive oxide nanoparticles is disposed on the photoactive area by spin coating. In one embodiment, the solvent dispersion of transparent conductive oxide nanoparticles is spin coated directly on the photoactive area. Typically, the spin coating is performed at a speed of at least 1000 RPM, such as at least 2000 RPM, at least 3000 RPM, at least 4000 RPM or at least 5000 RPM, such as between 2000 and 10000 RPM, between 4000 and 8000 RPM, preferably about 6000 RPM. Typically, the spin coating is performed for a time of at least 1 second, at least 5 seconds or at least 10 seconds, such as between 1 second and 1 minute, between 10 seconds and 30 seconds, preferably about 20 seconds.
[0232] Thus, preparing a substrate by disposing a charge recombination layer on a photoactive region by solution deposition may include spin-coating a solvent dispersion of indium tin oxide nanoparticles in isopropanol onto the substrate (photoactive region) at a speed of about 6000 RPM for about 20 seconds.
[0233] The charge recombination layer may further comprise a matrix material. The matrix material may be an inorganic or organic matrix material. It may be a dielectric matrix material, for example an inorganic or organic dielectric matrix material. However, it is often an electron transport matrix material. Typically, the matrix material is an organic matrix material as described herein. Thus, the solvent dispersion of nanoparticles may further comprise a matrix material, for example an organic matrix material as described herein. The matrix material may be, for example, a dielectric matrix material or an electron transport matrix material. The matrix material may be organic or inorganic, but is typically organic, for example an organic electron transport matrix material. The step of disposing the charge recombination layer on the photoactive region may include disposing a solvent dispersion of nanoparticles of transparent conductive oxide and a matrix material, for example an organic matrix material, on the photoactive region.
[0234] The matrix material and the nanoparticles may be disposed together (e.g., as described above) or separately in the method of the present invention. When they are disposed separately, one option is to first dispose the nanoparticles, e.g., as a solvent dispersion of the nanoparticles, followed by disposing the matrix material, e.g., as a solution or dispersion of the matrix material in a solvent. The matrix material may then be impregnated into the disposed nanoparticles such that the nanoparticles are dispersed in the matrix material.
[0235] When a conductive polymer is present in the charge recombination layer, disposing the charge recombination layer on the photoactive region may include disposing the conductive polymer on the photoactive region and disposing a solvent dispersion of nanoparticles of a transparent conductive oxide on the photoactive region. Preferably, the conductive polymer comprises poly(3,4-ethylenedioxythiophene) and polystyrenesulfonate (PEDOT:PSS). Typically, the conductive polymer is dispersed in a solvent. For example, the conductive polymer may be dispersed in alcohol, water, a mixture of one or more alcohols and water, or a mixture of alcohols, such as isopropanol (2-propanol), ethanol (EtOH), methanol (MeOH), or water, or a mixture thereof. Thus, disposing the charge recombination layer on the photoactive region may include disposing a dispersion of poly(3,4-ethylenedioxythiophene) and polystyrenesulfonate (PEDOT:PSS) in isopropanol (2-propanol), ethanol (EtOH), methanol (MeOH), water, or a mixture thereof, on the photoactive region.
[0236] The conductive polymer may be disposed on the photoactive region by roll-to-roll (R2R) processing, blade coating, inkjet printing or spin coating. Typically, the conductive polymer is disposed on the photoactive region by spin coating. In one embodiment, the conductive polymer is spin coated directly on the photoactive region. Typically, the spin coating is performed at a speed of at least 1000 RPM, such as at least 2000 RPM, at least 3000 RPM, at least 4000 RPM or at least 5000 RPM, such as between 2000 and 10000 RPM, between 4000 and 8000 RPM, preferably about 6000 RPM. Typically, the spin coating is performed for a time of at least 1 second, at least 5 seconds or at least 10 seconds, such as between 1 second and 1 minute, between 10 seconds and 30 seconds, preferably about 20 seconds.
[0237] Typically, the process of disposing the charge recombination layer on the photoactive region involves two steps: 1) disposing a conductive polymer onto a photoactive region; 2) placing a solvent dispersion of transparent conductive oxide nanoparticles onto the photoactive area; Includes.
[0238] Typically, both the solvent dispersion of nanoparticles and the conductive polymer are disposed on the photoactive area by spin coating. The step of spin coating the solvent dispersion of nanoparticles and the conductive polymer (if present) on the photoactive area may be combined with one or more annealing steps. Typically, the annealing is carried out at a temperature of at least 20°C, for example at a temperature in the range of 20-150°C, for example at 30-120°C, 40-110°C, 60-100°C, 70-90°C, preferably at about 80°C. Typically, the annealing is carried out for a period of 1-120 minutes, for example at 2-60 minutes, 3-45 minutes, 4-30 minutes, 5-15 minutes or about 10 minutes. Thus, the annealing may be carried out at a temperature of 20-150°C for a period of 1-120 minutes, for example at a temperature of 60-100°C for a period of 4-30 minutes, preferably at about 80°C for about 10 minutes.
[0239] In one embodiment, the step of disposing the charge recombination layer over the photoactive region comprises the steps of: 1. disposing a conductive polymer (optionally by spin coating) by disposing a solvent dispersion of the conductive polymer onto the photoactive area (preferably the conductive polymer comprises poly(3,4-ethylenedioxythiophene) and polystyrenesulfonate (PEDOT:PSS)); 2. Optionally, annealing the conductive polymer disposed on the photoactive region, preferably at about 80° C. for about 10 minutes; 3. Disposing (optionally by spin coating) a solvent dispersion of nanoparticles of a transparent conductive oxide onto the photoactive area (preferably the nanoparticles are indium tin oxide (ITO) nanoparticles); 4. Optionally, annealing the transparent conductive oxide nanoparticles on the photoactive region, preferably at about 80° C. for about 10 minutes. Includes.
[0240] Disposing the charge recombination layer on the photoactive region may include simultaneously disposing a conductive polymer and a solvent dispersion of transparent conductive oxide nanoparticles on the photoactive region. For example, the conductive polymer and the transparent conductive oxide nanoparticles may be present in the same solvent dispersion. The dispersion containing the conductive polymer and the transparent conductive oxide nanoparticles may be disposed on the photoactive region by spin coating as described above.
[0241] photoactive region The photoactive material in the photoactive region of the substrate may include any suitable photoactive material known to one of skill in the art. For example, the photoactive material in the photoactive region may be silicon, Cu(In,Ga)Se2 (CIGS), Cu2ZnSn(S,Se)4 (CZTSSe), CuInS (CIS) metal chalcogenide nanocrystals, such as PbS, PbSe, or PbS 1-x Se x , chalcogenide thin films, such as CdTe or CdTe 1-x Se x or CdTe 1-x S x Typically, the photoactive material in the photoactive region of the substrate comprises a crystalline A / M / X material, which has the formula [A] a [M] b [X] c This includes compounds of the formula:
[0242] For example, the photoactive material in the photoactive region may have the formula [A] a [M] b [X] c The photoactive material in the photoactive region may comprise a compound of formula [A], which is a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein. Typically, the photoactive material in the photoactive region may comprise a compound of formula [A] a [M] b [X] cwherein the compound is a compound of formula (I), such as a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH).
[0243] For example, the photoactive material in the photoactive region can have the formula (IA): AMX3(IA) (wherein A, M and X are as defined above). In a preferred embodiment, A is a compound of the formula: + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + and M is selected from Pb 2+ Or Sn 2+ and X is Br - , Cl - and I - is selected from.
[0244] For example, the photoactive material in the photoactive region may comprise, or consist essentially of, a perovskite compound of formula (IA) selected from APbI3, APbBr3, APbCl3, ASnI3, ASnBr3 and ASnCl3, where A is a cation as described herein.
[0245] For example, the photoactive materials in the photoactive region can be CH3NH3PbI3, CH3NH3PbBr3, CH3NH3PbCl3, CH3NH3SnI3, CH3NH3SnBr3, CH3NH3SnCl3, CsPbI3, CsPbBr3, CsPbCl3, CsSnI3, CsSnBr3, CsSnCl3, (H2N-C(H)=NH2)PbI3, (H2N-C(H)=NH2)PbBr3 , (H2N-C(H)=NH2)PbCl3, (H2N-C(H)=NH2)SnI3, (H2N-C(H)=NH2)SnBr3 and (H2N-C(H)=NH2)SnCl3, in particular CH3NH3PbI3 or CH3NH3PbBr3, preferably CH3NH3PbI3.
[0246] For example, the photoactive material in the photoactive region may have the formula (ID): [A I x A II 1-x ]M[X I y X II 1-y ]3(ID) (In the formula, A I and A II is as defined above for A, M is as defined above, and X I and X II is as defined above for X, and both x and y are greater than 0 and less than 1. In a preferred embodiment, the compound A I and A II are (CH3NH3) + , (CH3CH2NH3) + , (CH3CH2CH2NH3) + , (N(CH3)4) + , (H2N-C(H)=NH2) + , (H2N-C(CH3)=NH2) + , (H2N-C(NH2)=NH2) + , Cs + and Rb + and M is selected from Pb2+ Or Sn 2+ and X I and X II are respectively, Br - , Cl - and I - is selected from.
[0247] For example, the photoactive material in the photoactive region may be [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[Br y I 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[Br y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[I y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[Br y I 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[Br y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[I y Cl 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Pb[Br y I 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Pb[Br y Cl 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Pb[I y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Sn[Br y I 1-y ]3, [(CH3NH3) x(H2N-C(H)=NH2) 1-x ]Sn[Br y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Sn[I y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Sn[Br y I 1-y ]3, [(CH3NH3) x Cs 1-x ]Sn[Br y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Sn[I y Cl 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Sn[Br y I 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Sn[Br y Cl 1-y ]3, and [(H2N-C(H)=NH2) x Cs 1-x ]Sn[I y Cl 1-y ]3, where x and y are both greater than 0 and less than 1, for example x and y may both be 0.01 to 0.99 or 0.05 to 0.95 or 0.1 to 0.9. Preferably, the photoactive material in the photoactive region comprises or consists essentially of a perovskite compound of formula (ID) selected from the formula [(H2N-C(H)=NH2) x Cs 1-x ]Pb[Br y I 1-y ]3 (wherein x and y are both 0.1 to 0.9).
[0248] The crystalline A / M / X material deposited on the substrate and the crystalline A / M / X material in the photoactive region may be different or the same. Typically, the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X material in the photoactive region are different. For example, the crystalline A / M / X material in the photoactive region may comprise or essentially consist of a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein, preferably a compound of formula (I), such as a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH) as described herein; The crystalline A / M / X material deposited on the substrate may comprise or essentially consist of a compound of different formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein, preferably a compound of formula (I), such as a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH) as described herein.
[0249] For example, the crystalline A / M / X material in the photoactive region may comprise or consist essentially of a compound of formula (IA), and the crystalline A / M / X material deposited on the substrate may comprise or consist essentially of a compound of formula (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein, such as a compound of formula (IB), (IC), (ID), (IE), (IF), (IG) or (IH) as described herein, preferably a compound of formula (ID), (IE) or (IF) as described herein.
[0250] For example, the crystalline A / M / X material in the photoactive region may comprise or consist essentially of a compound of formula APbI3, APbBr3, APbCl3, ASnI3, ASnBr3 or ASnCl3 (wherein A is a cation as described herein), preferably APbI3, more preferably CH3NH3PbI3, and the crystalline A / M / X material deposited on the substrate may comprise or consist essentially of a compound of formula CH3NH3[Pb z Sn 1-z ]Cl3, CH3NH3[Pb z Sn 1-z ]Br3, CH3NH3[Pb z Sn 1-z ]I3, Cs[Pb z Sn 1-z ]Cl3, Cs[Pb z Sn 1-z ]Br3, Cs[Pb z Sn 1-z ]I3, (H2N-C(H)=NH2)[Pb z Sn 1-z ]Cl3, (H2N-C(H)=NH2)[Pb z Sn 1-z ]Br3 or (H2N-C(H)=NH2)[Pb z Sn 1-z ]I3 (wherein z is greater than 0 and less than 1, for example z may be 0.01 to 0.99, or 0.05 to 0.95, or 0.1 to 0.9), or a compound of the formula [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]Cl3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]Br3,[(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]I3, [(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ]Cl3, [(CH3NH3) x Cs 1-x ][Pbz Sn 1-z ]Br3,[(CH3NH3) x Cs 1-x ][Pb z Sn 1-z ]I3, [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ]Cl3, [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ]Br3 or [(H2N-C(H)=NH2) x Cs 1-x ][Pb z Sn 1-z ]I3 (wherein x and z are both greater than 0 and less than 1, for example, x and z may each be 0.01 to 0.99 or 0.05 to 0.95 or 0.1 to 0.9), preferably a compound of the formula CH3NH3[Pb z Sn 1-z ]I3 or [(CH3NH3) x (H2N-C(H)=NH2) 1-x ][Pb z Sn 1-z ]I3, where x, y and z are each between 0.05 and 0.95 or between 0.1 and 0.9.
[0251] The photoactive material in the photoactive region has the formula: Cs z (H2N-C(H)=NH2) (1-z) [M][X]3 (wherein [M] is as defined above and may, for example, include Pb, Sn or a mixture of Pb and Sn, [X] is one or more different halide anions, for example two or more different halide anions, and z is 0.01 to 0.99). For example, the perovskite may include a perovskite compound of the formula Cs z (H2N-C(H)=NH2) (1-z) [Pb x Sn 1-x ]I3, Csz (H2N-C(H)=NH2) (1-z) [Pb x Sn 1-x ]Br3 or Cs z (H2N-C(H)=NH2) (1-z) [Pb x Sn 1-x ]I y Br 3(1-y) (wherein z is as defined above, x is 0 to 1 (for example, it may be 0.5), and y is 0.01 to 0.99).
[0252] The photoactive material in the photoactive region has the formula: Cs z (H2N-C(H)=NH2) (1-z) [M]X 3y X' 3(1-y) where [M] is as defined above and may, for example, include Pb, Sn, or a mixture of Pb and Sn, and X is I - , Br - , Cl - and F - X′ is a first halide anion selected from the group consisting of: - , Br - , Cl - and F - wherein z is 0.01 to 0.99 and y is 0.01 to 0.99. For example, perovskites may include compounds of the formula Cs z (H2N-C(H)=NH2) (1-z) PbBr 3y I 3(1-y) It may also be a compound of the formula:
[0253] The crystalline A / M / X material in the photoactive region may comprise or consist essentially of a compound of formula (ID), and the crystalline A / M / X material deposited on the substrate may comprise or consist essentially of a compound of formula (IA), (IB), (IC), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein, such as a compound of formula (IA), (IB), (IC), (IE), (IF), (IG) or (IH) as described herein, preferably a compound of formula (IA), (IE) or (IF) as described herein.
[0254] For example, the crystalline A / M / X material in the photoactive region may have the formula [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[Br y I 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[Br y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Pb[I y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[Br y I 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[Br y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Pb[I y Cl 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Pb[Br y I 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Pb[Br y Cl 1-y ]3, [(H2N-C(H)=NH2) xCs 1-x ]Pb[I y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Sn[Br y I 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Sn[Br y Cl 1-y ]3, [(CH3NH3) x (H2N-C(H)=NH2) 1-x ]Sn[I y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Sn[Br y I 1-y ]3, [(CH3NH3) x Cs 1-x ]Sn[Br y Cl 1-y ]3, [(CH3NH3) x Cs 1-x ]Sn[I y Cl 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Sn[Br y I 1-y ]3, [(H2N-C(H)=NH2) x Cs 1-x ]Sn[Br y Cl 1-y ]3, or [(H2N-C(H)=NH2) x Cs 1-x ]Sn[I y Cl 1-y ]3 (wherein x and y are both greater than 0 and less than 1, for example, x and y may both be 0.01 to 0.99 or 0.05 to 0.95 or 0.1 to 0.9), preferably a compound of the formula [(CH3NH3) x Cs 1-x ]Pb[Br y I 1-y]3, where x and y are from 0.05 to 0.95 or from 0.1 to 0.9, and the crystalline A / M / X material deposited on the substrate may comprise or consist essentially of a compound of formula APbI3, APbBr3, APbCl3, ASnI3, ASnBr3 or ASnCl3, where A is a cation as described herein, preferably APbI3, more preferably CH3NH3PbI3; or CH3NH3[Pb z Sn 1-z ]Cl3, CH3NH3[Pb z Sn 1-z ]Br3, CH3NH3[Pb z Sn 1-z ]I3, Cs[Pb z Sn 1-z ]Cl3, Cs[Pb z Sn 1-z ]Br3, Cs[Pb z Sn 1-z ]I3, (H2N-C(H)=NH2)[Pb z Sn 1-z ]Cl3, (H2N-C(H)=NH2)[Pb z Sn 1-z ]Br3 and (H2N-C(H)=NH2)[Pb z Sn 1-z ]I3 (wherein z is greater than 0 and less than 1, for example z may be 0.01 to 0.99, 0.05 to 0.95, or 0.1 to 0.9), preferably CH3NH3[Pb z Sn 1-z ]I3, where z is 0.05 to 0.95 or 0.1 to 0.9.
[0255] Alternatively, the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X material in the photoactive region may both be compounds of the same formula ((IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein) but may have different chemical compositions (e.g., one may be CH3NH3PbI3 and the other may be CH3NH3PbBr3, or one may be CH3NH3PbI3 and the other may be CH3NH3SnI3).
[0256] Typically, the photoactive region includes one or more charge transport layers, for example two charge transport layers. The charge transport layer may be a layer of an electron transporting (n-type) material as described herein, or a layer of a hole transporting (p-type) material as described herein. Typically, the photoactive region includes two charge transport layers, one of the charge transport layers being a layer of an electron transporting (n-type) material as described herein, and the other charge transport layer being a layer of a hole transporting (p-type) material as described herein.
[0257] Preferably, the photoactive region comprises a layer of an electron transporting (n-type) material, said electron transporting material comprising PCBM, and the other charge transporting layer is a layer of a hole transporting (p-type) material, said hole transporting material comprising spiro-OMeTAD or spiro(TFSI)2.
[0258] Thus, the photoactive region may comprise the following layers in the following order: a layer of a charge transporting material, preferably a layer of a hole transporting (p-type) material (more preferably, said hole transporting material comprises spiro-OMeTAD), a layer of a photoactive material as described herein, A layer of a charge transporting material, preferably an electron transporting (n-type) material (more preferably, said electron transporting material comprises PCBM).
[0259] The layer of electron transport (n-type) material may, for example, include a layer of organic n-type material and a layer of inorganic n-type material. Often, a layer of organic n-type material (which may be as further defined herein, for example PCBM) is disposed on a layer of inorganic n-type material (which may also be as further defined herein, for example SnO2). The layer of electron transport (n-type) material typically has this structure when in contact with an electrode, for example a first electrode comprising a transparent conductive oxide (for example fluorine doped tin oxide (FTO) or indium doped tin oxide (ITO) etc.). Typically, the inorganic n-type layer of the layer of electron transport material (often SnO2) is in contact with a transparent conductive oxide, for example FTO. Indeed, the inventors have found that such an inorganic n-type layer improves the electronic contact between the organic n-type layer and the transparent conductive oxide. Similarly, the inventors have found that an organic n-type layer (e.g., PCBM) provides a more stable electronic contact with the photoactive material compared to an inorganic n-type layer, particularly when the photoactive material is a crystalline A / M / X material as defined herein. The inventors have also found that having a double n-layer helps inhibit pinholes in the n-layer. Thus, the present invention typically uses two n-type layers between the electrode comprising a transparent conductive oxide and the photoactive material. The inventors have found that a double SnO2 / PCBM n-type layer is improved compared to SnO2 alone, in particular because SnO2 improves the electronic contact of PCBM with FTO, and PCBM provides a more stable electronic contact with the perovskite photoactive material.
[0260] Typically, the photoactive region including the layer of photoactive material and, optionally, the layer of charge transport material, has a total thickness of from 10 to 5000 nm, e.g., from 50 to 3000 nm, from 100 to 2000 nm, from 200 to 1500 nm, preferably from 250 to 1250 nm. Typically, the layers of optional charge transport material, if present, have individual thicknesses of less than 200 nm, e.g., less than 150 nm or less than 100 nm, from 1 to 100 nm, typically from 10 to 75 nm, typically from 30 to 60 nm.
[0261] The layer of photoactive material in the photoactive region can also be prepared using the aprotic solvent / organic amine solvent system used in the method of the invention. For example, the method of the invention can further include preparing a substrate by disposing a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] as described herein. a [M] b [X] c and the method includes forming a layer of crystalline A / M / X material by disposing a film-forming solution on a substrate layer, such as an n-type or p-type layer in the substrate, the film-forming solution comprising (a) one or more M cations, and (b) Solvent wherein the solvent comprises (i) an aprotic solvent, and (ii) Organic amines Includes.
[0262] Alternatively, the layer of photoactive material in the photoactive region may be prepared according to other methods known to those skilled in the art. For example, the method of the present invention may further comprise preparing a substrate by disposing a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] as described herein. a [M] b [X] c and the method includes forming a layer of crystalline A / M / X material by conventional high boiling point solvent deposition, for example by disposing (e.g., by spin coating) a solution of the A / M / X precursor compound in DMF, DMSO, or mixtures thereof, onto a substrate precursor.
[0263] Triple Junction Device In one embodiment, the substrate comprises two separate photoactive regions as described herein, each photoactive region comprising a photoactive material. By two separate photoactive regions, it is meant a substrate comprising two photoactive regions that are not in direct physical contact with each other. When the substrate comprises two separate photoactive regions, the layer of crystalline A / M / X material formed on the substrate forms part of a third photoactive region. Thus, a multijunction device produced according to the method of the present invention may comprise three photoactive regions. Thus, a multijunction device produced according to the method of the present invention may be a triple junction device. Typically, at least two of the photoactive regions in the multijunction device are formed using a film-forming solution as defined herein with reference to the method of the present invention.
[0264] In this embodiment, the additional charge recombination layer described herein may be disposed between two photoactive regions in the substrate. Thus, the substrate may include two photoactive regions separated by an additional charge recombination layer. For example, the substrate may include the following layers in the following order: an optional charge transport layer, preferably a layer of an electron transporting (n-type) material; ·Charge recombination layer, ·Photoactive region, ·Charge recombination layer, ·Photoactive region.
[0265] Each photoactive region may be as described above. For example, each photoactive region may include one or more charge transport layers, such as two charge transport layers, as described herein. The charge transport layer may be a layer of an electron transporting (n-type) material as described herein, or a layer of a hole transporting (p-type) material as described herein. Typically, each photoactive region includes two charge transport layers, one of which is a layer of an electron transporting (n-type) material as described herein, and the other charge transport layer is a layer of a hole transporting (p-type) material as described herein. These layers are generally disposed on either side (respectively above and below) of a layer of a photoactive material as described herein.
[0266] Preferably, each photoactive region comprises a layer of an electron transporting (n-type) material, said electron transporting material comprising PCBM, and the other charge transporting layer is a layer of a hole transporting (p-type) material, said hole transporting material comprising spiro-OMeTAD.
[0267] The layer of electron transport material in one of the photoactive regions may include a layer of an organic n-type material and a layer of an inorganic n-type material. Often, a layer of organic n-type material (e.g., PCBM) is disposed on a layer of inorganic n-type material (e.g., SnO2). The layer of electron transport (n-type) material typically has this structure when in contact with an electrode, for example, a first electrode comprising a transparent conductive oxide (e.g., fluorine-doped tin oxide (FTO) or the like).
[0268] Thus, each photoactive region may include the following layers in the following order: a layer of a charge transporting material, preferably a layer of a hole transporting (p-type) material (more preferably, said hole transporting material comprises spiro-OMeTAD), a layer of a photoactive material as described herein, A layer of a charge transporting material, preferably an electron transporting (n-type) material (more preferably, said electron transporting material comprises PCBM or comprises PCBM and SnO2).
[0269] Each photoactive material in each photoactive region may comprise a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c For example, each photoactive material in the photoactive region comprises a compound of the formula [A] a [M] b [X] c The compound may comprise a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein. Typically, each photoactive material in the photoactive region is a compound of formula [A] a [M] b [X] cwherein the compound is a compound of formula (I), such as a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH).
[0270] The crystalline A / M / X materials in the two photoactive regions may be the same crystalline A / M / X material as described herein, or may be different crystalline A / M / X materials. Preferably, at least two of the crystalline A / M / X materials selected from the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X materials in the two photoactive regions are different. In one embodiment, all three crystalline A / M / X materials selected from the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X materials in the two photoactive regions are different.
[0271] For example, a layer of photoactive material in one photoactive region may comprise a compound of formula ID, a layer of photoactive material in the other photoactive region may comprise a compound of formula IA, and the crystalline A / M / X material deposited on the substrate may comprise a compound of formula IE.
[0272] Preferably, at least one of the layers of crystalline A / M / X material in one of the photoactive regions is deposited using an aprotic solvent / organic amine solvent system as used in the method of the present invention. In one embodiment, each layer of photoactive material in each photoactive region may be deposited using an aprotic solvent / organic amine solvent system as used in the method of the present invention.
[0273] Alternatively, one of the layers of photoactive material in one of the photoactive regions is fabricated according to other methods known to those skilled in the art, for example, the layer of photoactive material may be deposited by conventional high boiling point solvent deposition techniques, such as by spin coating a solution of the A / M / X precursor compound in DMF, DMSO, or mixtures thereof.
[0274] electrode The substrate typically includes a first electrode. The first electrode may include a metal (e.g., silver, gold, aluminum, or tungsten) or a transparent conductive oxide (e.g., fluorine-doped tin oxide (FTO) or indium-doped tin oxide (ITO)). Typically, the first electrode includes a transparent conductive oxide. The thickness of the layer of the first electrode is typically 5 nm to 100 nm.
[0275] The substrate is typically i) a first electrode (preferably the first electrode comprises a transparent conductive oxide); ii) a photoactive region, said photoactive region preferably comprising a crystalline A / M / X material, said crystalline A / M / X material having the formula [A] a [M] b [X] c (including compounds of iii) a charge recombination layer, as described herein, disposed over the photoactive region; and iv) optionally, a layer of a charge transport material as described herein disposed over the charge recombination layer. Includes.
[0276] To fabricate a triple junction device, the substrate is typically i) a first electrode (preferably the first electrode comprises a transparent conductive oxide); ii) a photoactive region, said photoactive region preferably comprising a crystalline A / M / X material, said crystalline A / M / X material having the formula [A] a [M] b [X] c (including compounds of iii) a charge recombination layer, as described herein, disposed over the photoactive region; iv) a photoactive region, said photoactive region preferably comprising a crystalline A / M / X material, said crystalline A / M / X material having the formula [A] a [M] b [X] c (including compounds of v) a charge recombination layer, as described herein, disposed over the photoactive region; and vi) optionally, a layer of a charge transport material as described herein disposed over the charge recombination layer. Includes.
[0277] The first electrode may be deposited on a layer of transparent material, such as a layer of glass. The layer of transparent material may be treated with an anti-reflective coating. Typically, the anti-reflective coating comprises magnesium fluoride (MgF2).
[0278] The method may further include depositing a second electrode onto the layer of crystalline A / M / X material deposited on the substrate.
[0279] The second electrode may be as defined above for the first electrode. Typically, the second electrode comprises or consists essentially of a metal, such as an elemental metal. Examples of metals that the second electrode material may comprise or consist essentially of include silver, gold, copper, aluminum, platinum, palladium or tungsten. The second electrode may be deposited by vacuum evaporation. The layer of the second electrode material typically has a thickness of 1 to 250 nm, preferably 5 nm to 100 nm.
[0280] Preferably, the method comprises disposing a layer of a charge transport material as described herein on a layer of a crystalline A / M / X material deposited on a substrate, and disposing a second electrode on the charge transport material. The layer of charge transport material may be a layer of an electron transporting (n-type) material as described herein, or a layer of a hole transporting (p-type) material as described herein. Typically, the layer of charge transport material disposed on the layer of crystalline A / M / X material is a layer of a hole transporting (p-type) material as described herein, preferably the hole transport material comprises spiro-OMeTAD.
[0281] Thus, a multijunction device produced by the method of the present invention may comprise the following layers in the following order: A first electrode, ·Photoactive region, ·Charge recombination layer, an optional layer of a charge transporting material, preferably a layer of an electron transporting (n-type) material (preferably said electron transporting material comprises PCBM); a layer of a crystalline A / M / X material as described herein; an optional layer of a charge transport material, preferably a layer of a hole transport (p-type) material (preferably, said hole transport material comprises spiro-OMeTAD); · Second electrode.
[0282] In the case of a triple junction device made by the method of the present invention, the triple junction device may comprise the following layers in the following order: A first electrode, ·Photoactive region, ·Charge recombination layer, ·Photoactive region, ·Charge recombination layer, an optional layer of a charge transporting material, preferably a layer of an electron transporting (n-type) material (preferably, said electron transporting material comprises PCBM); a layer of a crystalline A / M / X material as described herein; an optional layer of a charge transport material, preferably a layer of a hole transport (p-type) material (preferably, said hole transport material comprises spiro-OMeTAD); · Second electrode.
[0283] In one embodiment, at least two of the photoactive regions in a multijunction device are formed using a film-forming solution described herein. In this embodiment, the method of the invention includes the steps of forming a layer of crystalline A / M / X material by disposing the film-forming solution on a substrate, where the substrate includes one photoactive region comprising a photoactive material and a charge recombination layer disposed on the photoactive region by a solution deposition method, followed by the further steps of: optionally forming a layer of a charge transport material as described herein on the layer of crystalline A / M / X material deposited on a substrate (preferably the charge transport material comprises a hole transport (p-type) material); forming a further charge recombination layer as described herein, forming a further photoactive region by depositing a layer of a crystalline A / M / X material using a film-forming solution as described herein, and optionally forming one or more charge transport layers as described herein; A process for forming a second electrode may include:
[0284] Thus, such a device may comprise the following layers in the following order: A first electrode, ·Photoactive region, ·Charge recombination layer, an optional layer of a charge transporting material, preferably a layer of an electron transporting (n-type) material (preferably, said electron transporting material comprises PCBM); a layer of a crystalline A / M / X material as described herein; an optional layer of a charge transport material, preferably a layer of a hole transport (p-type) material (preferably, said hole transport material comprises spiro-OMeTAD); ·Charge recombination layer, an optional layer of a charge transporting material, preferably a layer of an electron transporting (n-type) material (preferably, said electron transporting material comprises PCBM); a layer of a crystalline A / M / X material as described herein; an optional layer of a charge transport material, preferably a layer of a hole transport (p-type) material (preferably, said hole transport material comprises spiro-OMeTAD); · Second electrode.
[0285] Multijunction Devices The present invention also relates to a multijunction device obtainable or obtained by the method of the present invention. The multijunction device may include any of the features described above in relation to the method of making a multijunction device. For example, the multijunction device may include any of the layer orders and material combinations described above. Also, each of the crystalline A / M / X material(s) may be as further defined anywhere herein.
[0286] In one embodiment, the present invention provides (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) Charge recombination layer containing transparent conductive oxide nanoparticles The present invention also relates to a multijunction device comprising:
[0287] The transparent conductive oxide nanoparticles may be any of the transparent conductive oxide nanoparticles described herein. For example, the transparent conductive oxide nanoparticles may be indium tin oxide (ITO) nanoparticles, preferably ITO nanoparticles having a size of less than 100 nm.
[0288] The present invention also provides (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) A charge recombination layer comprising a conductive polymer The present invention also relates to a multijunction device comprising:
[0289] In the above multijunction devices, [A], [M] and [X] may all be as described herein. Each A / M / X material may be as further defined herein. Each photoactive region may also be as further defined herein, for example, each may further comprise a layer of n-type material and a layer of p-type material, where the n-type and p-type materials may be as further defined herein.
[0290] The conductive polymer may be any conductive polymer described herein. For example, the conductive polymer may include poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate (PEDOT:PSS).
[0291] In the above multijunction devices, the charge recombination layer typically comprises transparent conductive oxide nanoparticles and a conductive polymer, both of which may be as further defined elsewhere herein. Thus, the charge recombination layer may comprise (i) indium tin oxide (ITO) nanoparticles and (ii) a polymer comprising poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate.
[0292] In the multijunction device, two of the photoactive regions may comprise a layer of a crystalline A / M / X material as described herein. In one embodiment, the multijunction device comprises at least three photoactive regions. Preferably, each photoactive region comprises a layer of a crystalline A / M / X material as described herein. Each crystalline A / M / X material may comprise or consist essentially of a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein, preferably a compound of formula (I), such as a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH) as described herein. Each photoactive region may further comprise n-type and p-type layers as further defined herein.
[0293] The present invention also provides (a) at least three photoactive regions, each photoactive region comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least three photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) at least one charge recombination layer disposed between the photoactive regions; The present invention also relates to a multijunction device comprising:
[0294] In a multijunction device containing three photoactive regions, [A], [M] and [X] may all be as described herein.
[0295] Typically, at least two charge recombination layers are disposed between the photoactive regions. For example, a multijunction device may include the following layers in the following order: ·Photoactive region, ·Charge recombination layer, ·Photoactive region, ·Charge recombination layer, ·Photoactive region.
[0296] Typically, at least one of the charge recombination layers comprises nanoparticles of a conductive polymer or a transparent conductive oxide, for example, each charge recombination layer comprises nanoparticles of a conductive polymer or a transparent conductive oxide.
[0297] Typically, at least one of the charge recombination layers comprises transparent conductive oxide nanoparticles and a conductive polymer. For example, each charge recombination layer may comprise transparent conductive oxide nanoparticles and a conductive polymer. The transparent conductive oxide nanoparticles and the conductive polymer may be as described herein, for example, the transparent conductive oxide nanoparticles may be indium tin oxide (ITO) nanoparticles, preferably ITO nanoparticles having a size of less than 100 nm, and the conductive polymer may comprise poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate (PEDOT:PSS). Thus, each of the charge recombination layer(s) may comprise (i) indium tin oxide (ITO) nanoparticles and (ii) a polymer comprising poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate.
[0298] In the multijunction devices described above, at least two of the crystalline A / M / X materials may be different from each other. In one embodiment, three or more crystalline A / M / X materials are different from each other. For example, in a multijunction device in which there are three crystalline A / M / X materials, all three crystalline A / M / X materials may be different from each other. The crystalline A / M / X materials in each photoactive region may comprise or consist essentially of a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG), (IH), (IIIA), (IIIB), (IIIC), (VIA), (VIB) or (VIC) as described herein, preferably a compound of formula (I), such as a compound of formula (IA), (IB), (IC), (ID), (IE), (IF), (IG) or (IH) as described herein. Each photoactive region may further comprise at least one, preferably two, charge transport layers, such as an n-type layer and a p-type layer as further defined herein.
[0299] The multijunction device may further comprise a first electrode and a second electrode as described herein, with the photoactive region and the charge recombination layer(s) disposed between the first electrode and the second electrode. Preferably, the first electrode comprises a transparent conductive oxide and the second electrode comprises an elemental metal.
[0300] Typically, the multijunction device described herein is selected from the group consisting of optoelectronic devices, photovoltaic devices, solar cells, photodetectors, photodiodes, photosensors, color-emitting devices, transistors, photosensitive transistors, phototransistors, solid-state triodes, batteries, battery electrodes, capacitors, supercapacitors, light-emitting devices, light-emitting diodes, and lasers. For example, the multijunction device may be an optoelectronic device. Examples of optoelectronic devices include photovoltaic devices, photodiodes (including solar cells), phototransistors, photomultipliers, photoresistors, and light-emitting devices. Preferably, the multijunction device is a photovoltaic device or a light-emitting device. Some embodiments are given below. Item 1 A method for manufacturing a multijunction device comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c (In the formula, [A] contains one or more A cations, [M] comprises one or more M cations which are metal or metalloid cations; [X] comprises one or more X anions; a is a number from 1 to 6, b is a number from 1 to 6, (c is a number between 1 and 18) and the method includes forming a layer of the crystalline A / M / X material by disposing a film-forming solution on a substrate, wherein the film-forming solution comprises a compound of (a) one or more M cations, and (b) Solvent wherein the solvent comprises (i) an aprotic solvent, and (ii) Organic amines The substrate comprises: a photoactive region comprising a photoactive material; and a charge recombination layer disposed over the photoactive region by solution deposition; A method comprising: Section 2 Item 3. The method according to item 1, wherein the aprotic solvent is a polar aprotic solvent. Section 3 3. The method of claim 1 or 2, wherein the substrate further comprises a layer of a charge transport material disposed on the charge recombination layer. Section 4 disposing the charge recombination layer over the photoactive region by solution deposition; and Optionally, disposing a layer of a charge transport material over the charge recombination layer. The method according to any one of items 1 to 3, comprising the step of producing the substrate by the method according to any one of items 1 to 3. Section 5 the photoactive material in the substrate is dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof, or at least one component of the charge recombination layer in the substrate is dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof; Preferably, both the photoactive material in the substrate and at least one component of the charge recombination layer in the substrate are dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof; More preferably, the photoactive material in the substrate and the charge recombination layer in the substrate are both dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO) or a mixture thereof. Section 6 Item 6. The method of any one of items 1 to 5, wherein the charge recombination layer comprises nanoparticles of a transparent conductive oxide, and optionally, the transparent conductive oxide comprises indium tin oxide (ITO). Section 7 Item 7. The method of item 6, wherein the transparent conductive oxide nanoparticles are disposed in a matrix material, such as an organic matrix material, optionally an electron transporting organic matrix material, and optionally the organic matrix material comprises [6,6]-phenyl-C61-butyric acid methyl ester (PCBM). Section 8 Item 8. The method of item 6 or 7, wherein the charge recombination layer further comprises a conductive polymer, preferably the conductive polymer comprises poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate (PEDOT:PSS). Section 9 Item 9. The method according to any one of items 4 to 8, wherein the step of disposing the charge recombination layer on the photoactive region comprises disposing a solvent dispersion of nanoparticles of a transparent conductive oxide on the photoactive region, preferably the step of disposing the charge recombination layer on the photoactive region comprises disposing a conductive polymer on the photoactive region and disposing a solvent dispersion of nanoparticles of a transparent conductive oxide on the photoactive region, optionally the solvent dispersion of nanoparticles further comprises a matrix material, e.g. an organic matrix material, and optionally the solvent dispersion of nanoparticles and / or the conductive polymer are disposed on the photoactive region by spin coating. Section 10 Item 10. The method according to any one of Items 1 to 9, wherein the aprotic solvent does not contain dimethylformamide, and preferably the aprotic solvent does not contain dimethylformamide, dimethylsulfoxide, or a mixture thereof. Section 11 The method according to any one of items 1 to 10, wherein the aprotic solvent comprises a compound selected from the group consisting of chlorobenzene, acetone, butanone, methyl ethyl ketone, acetonitrile, propionitrile, toluene, or a mixture thereof, and preferably, the aprotic solvent comprises acetonitrile. Section 12 Item 12. The method according to any one of items 1 to 11, wherein the organic amine is an unsubstituted or substituted alkylamine or an unsubstituted or substituted arylamine. Item 13 The organic amine may be unsubstituted or substituted (C 1~10 alkyl)amine, preferably the organic amine is an unsubstituted (C 1~10 alkyl)amine or phenyl group substituted (C 1~10 Item 13. The method according to item 12, wherein the organic amine is a methylamine, an ethylamine, a propylamine, a butylamine, a pentylamine, a hexylamine, a benzylamine or a phenylethylamine, more preferably the organic amine is a methylamine. Section 14 The above formula [A] a [M] b [X] c The compound of formula [A][M][X] 3 (wherein [A], [M] and [X] are as defined in item 1) Item 15 Item 15. The method according to any one of items 1 to 14, wherein [A] contains at least one organic cation. Section 16 Each A cation is an alkali metal cation, a compound of the formula [R 1 R2 R 3 R 4 N] + (In the formula, R 1 、R 2 、R 3 、R 4 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl; R 1 、R 2 、R 3 and R 4 at least one of which is not hydrogen; 5 R 6 N=CH-NR 7 R 8 ] + (In the formula, R 5 、R 6 、R 7 and R 8 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl), and C 1~10 Alkylammonium, C 2~10 Alkenylammonium, C 1~10 Alkyliminium, C 3~10 Cycloalkylammonium and C 3~10 Cycloalkyliminium (which may be unsubstituted or amino, C 1~6 Alkylamino, imino, C 1~6 Alkylimino, C 1~6 Alkyl, C 2~6 Alkenyl, C 3~6 Cycloalkyl and C 6~12 aryl), and preferably each A cation is selected from Cs + , Rb + ammonium, methylammonium, dimethylammonium, trimethylammonium, ethylammonium, propylammonium, butylammonium, pentylammonium, hexylammonium, heptylammonium, octylammonium, tetramethylammonium, formamidinium, 1-aminoethane-1-iminium and guanidinium. Section 17 Item 17. The method according to any one of items 1 to 16, wherein [M] comprises two or more different M cations. Section 18 Each M cation is Ca 2+ 、Sr 2+ , Cd 2+ , Cu 2+ , Ni 2+ , Mn2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ and Eu 2+ , preferably Sn 2+ , Pb 2+ , Cu 2+ , Ge 2+ and Ni 2+ , preferably Sn 2+ and Pb 2+ Item 18. The method according to any one of items 1 to 17, wherein the method is selected from the following: Section 19 19. The method of any one of paragraphs 1 to 18, wherein each X anion is a halide, and optionally, [X] comprises two or more different halide anions. Section 20 [A] is a compound represented by the formula [R 1 NH 3 ] + (In the formula, R 1 is unsubstituted C 1~10 alkyl), and the organic amine is unsubstituted (C 1~10 alkyl)amines, preferably of the formula [R 1 NH 3 ] + C on A cation 1~10 Alkyl groups and unsubstituted (C 1~10 C on alkyl amines 1~10 20. The method according to any one of items 1 to 19, wherein the alkyl groups are the same, more preferably [A] comprises methylammonium and the organic amine comprises methylamine. Section 21 The photoactive material in the photoactive region of the substrate comprises a crystalline A / M / X material, and the crystalline A / M / X material has the formula [A] defined in any one of items 1 and 14 to 20. a [M] b [X] c 21. The method according to any one of items 1 to 20, comprising the compound of formula (1). Section 22 22. The method of claim 21, wherein the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X material in the photoactive region are different. Section 23 The substrate comprises two separate photoactive regions, each photoactive region comprising a photoactive material, preferably each photoactive material in each photoactive region comprises a crystalline A / M / X material, the crystalline A / M / X material being represented by formula [A] as defined in any one of items 1 and 14 to 20. a [M] b [X] c and optionally at least two of the crystalline A / M / X materials selected from the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X materials in the two photoactive regions are different, and optionally all three of the crystalline A / M / X materials selected from the crystalline A / M / X material deposited on the substrate and the crystalline A / M / X materials in the two photoactive regions are different. Section 24 24. The method according to any one of items 1 to 23, wherein the membrane-forming solution further comprises one or more A cations and one or more X anions. Section 25 24. The method according to any one of items 1 to 23, further comprising disposing a composition comprising one or more A cations and optionally one or more X anions on the substrate. Section 26 26. The method according to any one of items 1 to 25, wherein the step of disposing the film-forming solution on a substrate comprises a step of spin-coating the film-forming solution on the substrate. Section 27 27. The method according to any one of items 1 to 26, wherein the method further comprises removing the solvent to form the layer comprising the crystalline A / M / X material, and optionally the solvent is removed by heating the substrate treated with the film-forming solution, optionally by heating the substrate treated with the film-forming solution at a temperature between 50° C. and 200° C., optionally for a time between 10 and 100 minutes. Section 28 The substrate is i) a first electrode, wherein preferably said first electrode comprises a transparent conductive oxide; ii) a photoactive region, wherein the photoactive region preferably comprises a crystalline A / M / X material, the crystalline A / M / X material being represented by formula [A] as defined in any one of items 1 and 14 to 20. a [M] b [X] c Compounds of the formula: iii) a charge recombination layer disposed on the photoactive region, where optionally the charge recombination layer is as defined in any one of paragraphs 6 to 8; and iv) optionally, a layer of charge transport material disposed over the charge recombination layer. The method according to any one of items 1 to 28, comprising: Section 29 The method further comprising: disposing a second electrode on the layer of crystalline A / M / X material disposed on the substrate; or Preferably, disposing a charge transport material over the layer of crystalline A / M / X material disposed on the substrate, and disposing a second electrode over the charge transport material. Further comprising: Preferably said second electrode comprises an elemental metal; The method according to any one of items 1 to 28. Item 30 30. A multijunction device obtainable by the method defined in any one of items 1 to 29. Item 31 Item 31. The method of any one of items 1 to 29, or the multijunction device of item 30, wherein the multijunction device is an optoelectronic device, and optionally the optoelectronic device is a photovoltaic device or a light-emitting device. Section 32 (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) Charge recombination layer containing transparent conductive oxide nanoparticles A multijunction device comprising: Item 33 (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) A charge recombination layer comprising a conductive polymer A multijunction device comprising: Section 34 Item 34. The multijunction device of item 32 or 33, wherein the charge recombination layer comprises nanoparticles of a transparent conductive oxide and a conductive polymer, and optionally the charge recombination layer is as further defined in any one of items 6 to 8. Item 35 35. The multijunction device of any one of claims 32-34, wherein two of the photoactive regions comprise a layer of a crystalline A / M / X material as defined in claim 32 or 33, and optionally the A / M / X material is as further defined in any one of claims 14-20. Section 36 35. The multijunction device of any one of claims 32 to 34, comprising at least three photoactive regions, preferably each photoactive region comprising a layer of a crystalline A / M / X material as defined in claim 32 or 33, optionally the A / M / X material being as further defined in any one of claims 14 to 20. Section 37 (a) at least three photoactive regions, each photoactive region comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least three photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) at least one charge recombination layer disposed between said photoactive regions. A multijunction device comprising: Section 38 38. The multijunction device of claim 37, comprising at least two charge recombination layers disposed between the photoactive regions. Item 39 Item 39. The multijunction device of item 37 or 38, wherein at least one of the charge recombination layers comprises nanoparticles of a conductive polymer or a transparent conductive oxide. Section 40 40. The multijunction device of claim 39, wherein at least one of the charge recombination layers comprises nanoparticles of a transparent conductive oxide and a conductive polymer, and optionally at least one of the charge recombination layers is as further defined in any one of claims 6 to 8. Section 41 41. The multijunction device of any one of claims 32 to 40, wherein each photoactive region comprises a layer of a crystalline A / M / X material as further defined in any one of claims 14 to 20. Section 42 Item 32-41, wherein at least one of the charge recombination layers comprises (i) nanoparticles of indium tin oxide (ITO) and (ii) a polymer comprising poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate. Section 43 Item 43. The multi-junction device according to any one of items 32 to 42, wherein at least two of the crystalline A / M / X materials are different from each other, and optionally, three or more of the crystalline A / M / X materials are different from each other. Section 44 Item 44. The multijunction device according to any one of items 32 to 43, further comprising a first electrode and a second electrode, wherein at least one of the photoactive region and the charge recombination layer is disposed between the first electrode and the second electrode, preferably wherein the first electrode comprises a transparent conductive oxide and the second electrode comprises an elemental metal. Section 45 Item 45. The multijunction device according to any one of items 32 to 44, which is a photovoltaic device or a light-emitting device. EXAMPLES
[0301] The advantages of the present invention are described below with reference to some specific examples.
[0302] Herein, we present a method to enable sequential processing of a perovskite absorber layer on a bottom perovskite device using an acetonitrile / methylamine (ACN / MA) composite solvent previously introduced by Noel et al. (NK Noel, SN Habisreutinger, B. Wenger, MT Klug, MT Horantner, MB Johnson, RJ Nicholas, DT Moore, HJ Snaith, Energy Environ. Sci. 2017, 10, 145). This all-solution processed architecture may be applied to fabricate large area films on both rigid and flexible substrates using deposition techniques such as roll-to-roll (R2R) processing, blade coating or inkjet printing. An all-solution processed tandem architecture is provided that achieves a stabilized power conversion efficiency (PCE) of over 15% and delivers an open circuit voltage (Voc) of 2.18 V. Furthermore, we demonstrate the fabrication of a mixed metal Sn / Pb perovskite MAPb 0.75 Sn 0.25 We show that I3 can also be processed via an ACN / MA solvent system, and the reducing nature of MA allows one to achieve comparable efficiencies, eliminating the need to use SnF2, and obtain scanning PCEs of over 11% (stabilized at 10.5%) using the nip architecture. Mixed-metal MAPb was used to extend the optical absorption of the multijunction to 925 nm. 0.75 Sn 0.25Using I3 perovskite material, the first monolithic triple junction perovskite solar cell with an open circuit voltage (Voc) of 2.83V is realized. Optical and electronic models are utilized to validate the experimental results and account for the optical losses present in this particular architecture. The triple junction perovskite solar cell is then modeled using the electronic properties of currently feasible 1.94 / 1.57 / 1.24 eV perovskite materials, showing the possibility of achieving triple junction devices with a PCE of 24.3% and a corresponding Voc of 3.15V.
[0303] Results and Discussion All-perovskite monolithic 2T tandem and multijunction solar cells require tunnel junctions (TJs) or recombination layers to provide a means of creating an electronic series connection between the different subcells. In turn, the photovoltages resulting from each subcell are summed, resulting in a high voltage device. However, due to the conservation of charge, the current density flowing out of each subcell must be matched, and thus the current is limited to the lowest current density resulting from any subjunction. Therefore, to maximize the photocurrent density in a 2T monolithic tandem, both subcells should produce equal current densities, which can be achieved by carefully tailoring the band gap and thickness of each junction. The recombination layers between the subcells must meet stringent requirements. First, they must enable ohmic contact to the charge extraction layer and facilitate the recombination of collected electrons and holes without introducing resistive losses. Second, they must be as optically transparent as possible to avoid parasitic absorption of light. Third, it is necessary that the deposition of the recombination layer does not damage any layers below, which is typically achieved by introducing a "buffer layer" during sputtering or by using orthogonal solvents for solution processing. Finally, this intermediate layer must be a sufficient barrier to solvent penetration to prevent any redissolution of the underlying perovskite layer or other electronic layers during subsequent processing of another perovskite layer.
[0304] Here, recombination layers and nip perovskite solar cell architectures are developed that meet these constraints. For the recombination layer, the combination of a PEDOT:PSS layer followed by an ITO nanoparticle layer is found to be very suitable. In a first example, a "wide bandgap" for a purely lead-based perovskite tandem cell is developed by processing the top cell at about 1.94 eV (determined by the Tauc plot shown in Figure 5) above the top of the bottom cell at 1.57 eV. The wide bandgap junction is processed first, so that the issue of solvent orthogonality does not have to be considered too much. Thus, following the traditional solution processing route, 2% (molar concentration with respect to Pb) potassium (K + ) FA with additives 0.83 Cs 0.17 Pb(Br 0.7 I 0.3)3 also (Z. Tang, T. Bessho, F. Awai, T. Kinoshita, MM Maitani, R. Jono, TN Murakami, H. Wang, T. Kubo, S. Uchida, H. Segawa, Sci. Rep. 2017, 7. 12183; JK Nam, SU Chai, 2017). https: / / doi.org / 10.1016 / S0022-5376(02)00011-0 , Google Scholar Crossref , CAS 52. W. Cha, YJ Choi, J. Kim, JH Park, Nano Lett., 17, 2028; http: / / dx.doi.org / 10.1037 / 0021-843X.107.2.202 , Google Scholar Crossref , CAS 57. T. Bu, Y. Zhou, X. Huang, J. Xiao, F. Huang, Y. Zhong, Energy Environ. Stavrakas C, Philippe B, Richter JM, Alsari M, Booker EP, Hutter EM, Pearson AJ, Lilliu S, Savenije TJ, Rensmo H, Divitini G, Ducati C, Friend RH, Stranks SD, Nature, 2018, 555, 497-501.As described previously, deposition techniques using hydrohalic acid additives have been used to fabricate highly ordered perovskite materials with grains reaching micron size in diameter (Figure 6) (DP McMeekin, Z. Wang, W. Rehman, F. Pulvirenti, JB Patel, NK Noel, MB Johnston, SR Marder, LM Herz, HJ Snaith, Adv. Mater. 2017, 1607039). Highly crystalline perovskite materials with low energy disorder have been shown to prevent halide segregation (W. Rehman, RL Milot, GE Eperon, C. Wehrenfennig, JL Boland, HJ Snaith, MB Johnston, LM Herz, Adv. Mater. 2015, n / a). Additionally, potassium is utilized as an additive to block ion migration and reduce the anomalous hysteretic behavior inherently present in perovskite solar cells, as suggested by the recent report referenced above (HJ Snaith, A. Abate, JM Ball, GE Eperon, T. Leijtens, NK Noel, SD Stranks, JT-W. Wang, K. Wojciechowski, W. Zhang, J. Phys. Chem. Lett. 2014, 5, 1511). With this absorber material, open circuit voltages up to 1.27 V and stabilized power conversion efficiencies of 10.9% are obtained in single-junction perovskite solar cells, as shown in Figure 7.
[0305] In the bottom cell processed on top of the wide gap cell, the issue of dissolution of the bottom perovskite film must be considered. When using one of the standard DMF / DMSO solvent based approaches, the bottom perovskite film can be fully solvated and discolored, evidence that the recombination layer is not impermeable to DMF or DMSO. These high boiling point solvents remain on the surface long enough to slowly penetrate the solution processed interlayer and redissolve the bottom perovskite layer, thus limiting their usefulness in all-solution processed tandem solar cells. ACN / MA based composite solvent system for processing perovskite films has been developed previously (DP McMeekin, Z. Wang, W. Rehman, F. Pulvirenti, JB Patel, NK Noel, MB Johnston, SR Marder, LM Herz, HJ Snaith, Adv. Mater. 2017, 1607039) that has several distinct advantages. First, the solvent is much more volatile than DMF, allowing for very rapid drying. Second, the strength of solvation can be adjusted by varying the amount of methylamine incorporated. The correct amount of MA is selected to completely dissolve the salt, but with a minimum excess. It has been discovered that having an excess amount of MA in solution can have a detrimental effect on the device. Unwanted pinholes in the interlayer can result in methylamine penetration and re-dissolution of the perovskite underlayer. Therefore, the MA content in the solution is carefully adjusted to obtain a solution at its critical dissolution point, minimizing the possibility of re-dissolving the underlayer. This dissolution point is determined by slowly adding the ACN / MA perovskite solution to the neat ACN perovskite dispersion until the mixture is a complete perovskite solution. Through this means, a robust and reliable protocol for fabricating all-perovskite multijunction solar cells has been obtained.
[0306] To achieve optimal results, MAPbI3 and MAPbI4 were processed via ACN / MA solvent route. 0.75 Sn 0.25For both I3 perovskite materials, careful tuning of the B-site metal ion content was required. 61 -Butyric acid methyl ester (PC 61 FA on the BM layer 0.83 Cs 0.17 Pb(Br 0.7 I 0.33) A series of scanning electron microscope (SEM) top-view images of MAPbI3 perovskite films processed with the ACN / MA solvent system at various non-stoichiometric compositions fabricated on top of the top cell (TC).The effect of non-stoichiometric perovskite precursor solutions has been previously discussed (C. Roldan-Carmona, P. Gratia, I. Zimmermann, G. Grancini, P. Gao, M. Graetzel, MK Nazeeruddin, Energy Environ. Sci. 2015, 8, 3550; M. Yang, Z. Li, MO Reese, OG Reid, DH Kim, S. Siol, TR Klein, Y. Yan, JJ Berry, MFAM van Hest, K. Zhu, Nat. Energy 2017, 2, 17038; D. Bi, W. Tress, MI Dar, P. Gao, J. Luo, C. Renevier, K. Schenk, A. Abate, F. Giordano, J. -P. Correa Baena, J.-D. Decoppet, SM Zakeeruddin, MK Nazeeruddin, M. Gra tzel, A. Hagfeldt, Sci. Adv. 2016, 2, e1501170; Q. Chen, H. Zhou, T.-B. Song, S. Luo, Z. Hong, H.-S. Duan, L. Dou, Y. Liu, Y. Yang, Nano Lett. 2014, 14, 4158; TJ Jacobsson, J.-P. Correa-Baena, E. Halvani Anaraki, B. Philippe, SD Stranks, MEF Bouduban, W. Tress, K. Schenk, J. Teuscher, J.-E. Moser, H. Rensmo, A. Hagfeldt, J. Am. Chem. Soc. 2016, 138, 10331), however, the research community still has to unanimously agree that strict non-stoichiometry is theoretical. Some studies have shown that an excess of organoammonium leads to improved performance, while others have shown the benefits of having an excess of PbI2 in the precursor solution.However, it is clear that these small changes in stoichiometry affect perovskites in a variety of ways, ranging from effects on morphology, luminescence, trap passivation and stability.
[0307] In Figure 1A, we show a series of top-view SEM images of various A-site to B-site compositions of ACN-MA precursor solutions ranging from 6% excess MAI to 6% excess PbI2 when processed on top of an existing solar cell. The effect on the morphology and surface coverage of precursor solutions with different compositions was observed.
[0308] In all solution-processed tandem architectures, it is essential to eliminate the presence of pinholes to prevent dissolution of the underlying layers. In Figure 8, we show the tandem solar cell performance of devices processed with a range of different compositions. The ideal composition to maximize single-junction cell efficiency contains 3% excess MAI, and the full tandem solar cell was fabricated with this composition.
[0309] 1B and 1C show a schematic diagram of the 2T tandem and the corresponding cross-sectional scanning electron microscope (SEM) images. The solar cell was fabricated with a conventional nip architecture, with a 2,2′,7,7′-tetrakis(N,N′-di-p-methoxyphenylamine)-9,9′-spirobifluorene (spiro-OMeTAD) p-type charge extraction layer and an n-doped PC 61 A recombination layer consisting of PEDOT:PSS sandwiched between the BM electron transporter and followed by indium tin oxide (ITO) nanoparticles was found to work very well.
[0310] In Figure 1D, the power density is 100 mW cm -2 The forward and reverse current density voltage (JV) characteristics of one of the best performing two-terminal tandem solar cells measured under simulated air mass (AM) 1.5 solar radiation with a . A detailed explanation of the calculation method of the mismatch factor can be found below.
[0311] In this work, the recombination layer comprises sublayers of PEDOT:PSS and indium tin oxide (ITO) nanoparticles (NPs). A highly conductive PEDOT:PSS (Heraus H1000) solution is diluted in isopropanol (IPA) and spin-coated directly onto the spiro-OMeTAD layer, which serves as both the recombination layer and the solvent barrier. The ITO layer is then spin-coated from a solvent dispersion of ITO nanoparticles (>100 nm). The fabricated ITO nanoparticle layer can be porous and discontinuous. However, these nanoparticles have a high carrier density that allows the holes from the PEDOT:PSS and the PC 61 It recombines electrons from the BM to improve the recombination process. The ITO NP layer creates an ohmic contact between both the electron and hole accepting layers, allowing efficient charge transfer to the recombination layer.
[0312] This tandem device delivers 11.5mA cm -2 Short circuit current density (J SC ), Fill Factor (FF) of 0.63, Open Circuit Voltage (V oc ), and a power conversion efficiency (stabilized) of 15.2% (Figure 9). Perovskite solar cells tend to exhibit hysteretic behavior. Therefore, a stabilized efficiency measurement was performed by holding the device at a fixed maximum power point voltage of 1.72 V, reaching a stabilized efficiency of 15.2%, as shown in the inset of Figure 3A. In Figure 3B, the integrated current density was 10.0 mA cm in the front cell. -2 and 9.3mA cm in the back cell -2 The external quantum efficiency (EQE) of both junctions of the optically biased subcell during the EQE measurement is shown in Fig. 1. oc A voltage bias was applied to the solar cell equal to J scThe current density was measured close to the AM1.5G spectrum. Note the slight current density mismatch between the two subcells. In FIG. 10, we show the calculated mismatch factor for each material used in the multijunction solar cell. Due to the high intensity spike in the infrared part of the spectrum, the xenon arc lamp spectrum can be significantly mismatched with the AM1.5G spectrum (shown in FIG. 11). As a result, certain subcells of a multijunction solar cell can be overestimated or underestimated, especially in the case of multijunction solar cells. Here, in this particular case, the tandem cell is the rear cell confined under the AM1.5G spectrum, and the top cell confined under the solar simulator lamp. To counter these differences, a mismatch factor correction was applied, which reduced our estimated efficiency by about 0.4% relative. However, in the triple junction case, the spike in xenon intensity causes a significant mismatch factor, which requires a correction of a relative efficiency drop of 32.3% to counter the spectral mismatch. Both correction factors were applied to the reported efficiencies. The estimation of the voltage loss is an important metric to obtain the quality of the recombination interlayer. As shown in Figure 12, a 2T tandem V equivalent to 2.22 V was obtained using a PEDOT:PSS / ITO NP interlayer as the recombination layer. oc and both subcells had a maximum measured single-junction V of 1.27V for the front cell and 1.11V for the rear cell. oc Assuming that a voltage drop of about 180 mV occurred, this resulted in a loss of voltage in the middle layer.
[0313] Although neat lead-based devices result in stable perovskite materials, narrowing the band gap using unstable tin-based perovskites is still highly desirable for tandem applications. By tuning the ratio of A-sites to B-sites, MAPb 0.75 Sn 0.25 The effect of non-stoichiometric precursor solutions on the material properties of I3 (which has a band gap of 1.34 eV as determined from the Tauc plot in FIG. 13) was also examined. 0.75 Sn 0.25To maintain the I3 perovskite composition, excess PbI2 and SnI2 were added in a ratio of 75:25. Figure 2A shows a Kelvin probe force microscopy (KPFM) image of the excess metal ions in the MAPb 0.75 Sn 0.25 Upon incorporation into the I3 perovskite precursor solution, a sharp increase in the work function is observed. Note also the slower time-resolved photoluminescence (PL) decay shown in FIG. 2B. FIG. 2C shows the transient photoconductivity of the corresponding samples at various excitation densities, measuring the maximum perturbation of the electrical conductivity (conductivity, conductance) decay after photoexcitation with a laser pulse. Similarly, an increase in the photoconductivity of the film with excess metal ions is observed, implying a higher effective mobility. These longer carrier lifetimes and higher photoconductivities are found to correlate with a substantial improvement in device performance (FIG. 14), which is shown in FIG. 2D with an optimized MAPb of over 11%. 0.75 Sn 0.25 Brings PCE of I3.
[0314] Surprisingly, substantial differences were found in the optimal A-site to B-site ratios of tin-lead based perovskite materials compared to neat lead-based perovskite. In the case of Sn / Pb-based perovskites, the research community appears to have consistently observed improved performance when using excess tin halides, most notably in the form of tin fluoride (SnF2) or tin chloride (SnCl2) (D. Zhao, Y. Yu, C. Wang, W. Liao, N. Shrestha, CR Grice, AJ Cimaroli, L. Guan, RJ Ellingson, K. Zhu, X. Zhao, R.-G. Xiong, Y. Yan, Nat. Energy 2017, 2, 17018; KP Marshall, M. Walker, RI Walton, RA Hatton, Nat. Energy 2016, 1, 16178; SJ Lee, SS Shin, YC Kim, D. Kim, TK Ahn, JH Noh, J. Seo, S. I1 Seok, J. Am. Chem. Soc. 2016, 138, 3974; MH Kumar, S. Dharani, WL Leong, PP Boix, RR Prabhakar, T. Baikie, C. Shi, H. Ding, R. Ramesh, M. Asta, M. Graetzel, SG Mhaisalkar, N. Mathews, Adv. Mater. 2014, 26, 7122; AG Kontos, A. Kaltzoglou, E. Siranidi, D. Palles, GK Angeli, MK Arfanis, V. Psycharis, YS Raptis, EI Kamitsos, PN Trikalitis, CC Stoumpos, MG Kanatzidis, P. Falaras, Inorg. Chem. 2017, 56, 84). Tin fluoride as an additive is Sn 2+ From Sn4+ It has been readily used as a reducing agent to inhibit the oxidation of tin to Sn 2+ Vacancies are limited, which causes the unwanted p-type behavior seen in Sn-based perovskites. In this study, MA is relied upon to act as a reducing agent instead of SnF2, since SnF2 is poorly soluble in the ACN / MA solvent system. Amines are known to act as reducing agents, a phenomenon most often exploited during the synthesis of metal nanoparticles (see JDSN and GJ Blanchard*, 2006, DOI 10.1021 / LA060045Z). Here, the reducing properties of amines are exploited to allow SnF2 to effectively replace MA. Figure 14 shows plots of unoptimized devices with various ratios of A-site and B-site cations. Devices with excess MAI result in near-zero PCE and slight to no short circuit density (Jsc), while devices with excess amounts of metal ions clearly show an increase in single-junction device efficiency, with the optimal composition being achieved at 15% excess metal ions. Thus, tin-based perovskites can be fabricated using a combination of Sn 2+ From Sn 4+ Not only do they require a reducing agent to prevent oxidation to Sn, but they also require excess metal ions for optimal performance. This is consistent with the findings by Song et al., who observed that a nonstoichiometric CsSnI3 perovskite composition of 0.4:1 CsI:SnI2 was required for optimal performance when treated under a reducing hydrazine atmosphere (see T.-B. Song, T. Yokoyama, S. Aramaki, M. G. Kanatzidis, ACS Energy Lett. 2017, 2, 897). Excess SnI2 can be converted to Sn by exposure to moisture or oxygen. 2+ loses two electrons to Sn 4+ Any Sn resulting in 2+ It was confirmed that the salt functions as a “compensation factor” to replace the vacancies. In Figure 2A, MAPb 0.75 Sn 0.25Note the deeper Fermi level in I3 perovskite, which is due to the high concentration of Sn 2+ This is consistent with vacancies and is predicted to lead to p-doping of the perovskite. In contrast, the shallower Fermi level observed in metal-ion enriched perovskite films is consistent with Sn 2+ This could correspond to a more intrinsic perovskite material exhibiting fewer vacancies. The increased carrier lifetime in the perovskite absorber observed in FIG. 2A was interpreted as consistent with and indicative of a transition from a highly p-type material to a more intrinsic semiconductor. Furthermore, this Fermi level change could be due to the presence of a dielectric constant between the perovskite and the electron or hole accepting layer, in this case PC, respectively. 61 BM and Spiro-OMETAD + Bis(trifluoromethanesulfonyl)imide - This could potentially induce an energy barrier between the doped spiro-OMeTAD and (spiro(TFSI)2).
[0315] FIG. 3 shows the structure and performance characteristics of the first all-perovskite monolithic triple junction solar cell prepared via solution processing route. 0.75 Sn 0.25 The I3 perovskite solar cell was processed on top of the dual-junction tandem solar cell architecture described in Figure 1 to fabricate a triple-junction solar cell that absorbs light up to 925 nm. Figure 3A shows the FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3 perovskite serves as the front cell, MAPbI3 perovskite is the middle cell, and MAPb 0.75 Sn 0.25 I3, Perovskite is the rear cell, FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3 / MAPbI3 / MAPb 0.75 Sn 0.25 Figure 3B shows a schematic of a 2T triple-junction cell constructed with I3. Figure 3B shows the corresponding cross-sectional SEM image. Figure 3C shows a 100 mW cm -2Figure 3D shows the forward and reverse current density voltage (JV) characteristics of one of the "best performing" two-terminal triple junction solar cells measured under simulated air mass (AM) 1.5 and solar radiation. A PCE of 7.5% (7.1% stabilized) was measured, with the maximum V oc is measured on a separate device (shown in FIG. 15) and shows a stabilized open circuit voltage of 2.83 V after 60 seconds.
[0316] FIG. 17 shows the FA without the Ag electrode treated with DMF / DMSO solvent. 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 High-performance FA in pin architecture filtered ZnO3 / MAPbI3 tandem solar cells 0.83 Cs 0.17 Pb 0.5 Sn 0.5 Figure 17C shows the I3 perovskite. Although this is not a four-terminal (4T) tandem measurement since no semi-transparent electrode was used on the front tandem stack, this measurement allows a rough estimation of the efficiency gains that can be expected if high performance and low band gap are obtained by ACN / MA solvent-based means. Figure 17C shows the I3 perovskite with an absorption onset of 1.22 eV and PCE (stabilized) of 15.5% without filtering. 0.83 Cs 0.17 Pb 0.5 Sn 0.5 I3-based junctions can be obtained, and FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 We show that when filtered by the tandem MAPbI3 / MAPbI3, a PCE (stabilized) of 2.6% can be obtained. Thus, narrow band gap materials have the potential to be 0.83 Cs 0.17 Pb(Br 0.7 I 0.3)3 / MAPbI3 can be boosted by over 2.6% to reach a PCE of 17.7%. Note also that this measurement includes the air gap between the tandem and narrow bandgap single junction solar cells, as well as the additional PEDOT:PSS layer that would not otherwise be present in a standard monolithic triple junction solar cell. For these reasons, we measure a lower integrated current density from the EQE shown in FIG. 17B.
[0317] As reported by Hoerantner et al., all-perovskite triple junction solar cells using perovskite absorbers with bandgaps similar to those used by the inventors in this work should be capable of better performing single and dual junction efficiencies. Hoerantner et al.'s modeling indicates that an optimized 1.22 eV bandgap material could current match two wide bandgap subcells, 2.04 eV and 1.58 eV, to achieve 12 mA cm. -2 Theoretical maximum J SC , V of 3.54V oc and should deliver a PCE of 36.6% (see MT Horantner, T. Leijtens, ME Ziffer, GE Eperon, MG Christoforo, MD McGehee, HJ Snaith, ACS Energy Lett. 2017, 2, 2506). However, this performance can only be obtained with an optically transparent interlayer that reduces parasitic absorption and reflection losses. Figure 16 shows the optical properties of each interlayer used in the multi-junction stack. A PCE of about 100 nm thick was used in the interlayer structure. 61 The BM layer is responsible for most of the parasitic absorption and reflection losses.
[0318] To assess the true potential of this fully solution-processed all-perovskite multijunction solar cell architecture, we simulate this semiconductor stack using optical and electrical models similar to those used by Hoerantner et al. and show that it can be improved to further enhance the performance of multijunction devices. Using experimental thicknesses, combined with the extracted electrical properties of state-of-the-art single-junction perovskite cells, Figures 4A-B show the estimated performance of the tandem stack, and the corresponding modeled external quantum efficiency spectra. The current champion FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 It was estimated that by combining the electrical properties of ACN / MA MAPbI3 with the best-in-class ACN / MA MAPbI3, the PCE of a tandem solar cell (subcells with band gaps of 1.94 eV and 1.57 eV) can be increased by almost 19%. A stack with the same absorber and interlayer material but with state-of-the-art MAPbI3, processed via DMF / DMSO means, with optimized perovskite thickness, interlayer with thickness reduced to 50 nm, and MgF2 anti-reflection coating was modeled (shown in Figure 4C-D). These improvements allow the tandem cell to reach a PCE of 21.8%. In this figure, an optimized stack with an enhanced front cell with improved electrical properties was also modeled, with the FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3, electroluminescence efficiency (EQE) of 1% EL ), 4·10 -2 Ωcm 2 A series resistor (R S ) and 10MΩcm 2 The shunt resistance (R SH ) was envisaged, increasing the achievable PCE to 26.8%. Figure 4E–F shows the optimized perovskite thickness for current matching, the state-of-the-art MAPbI3 and FA 0.6 MA 0.4 Pb 0.4 Sn 0.6They reveal the performance of a triple-junction architecture envisioned with an I3 perovskite sub-cell and an anti-reflective coating added on top. With optimized thicknesses, a PCE of 26.7% can be achieved, with the V oc Triple junction efficiencies of >30% PCE are within reach by improving . The specific layer thicknesses for each simulation are listed below along with a detailed description of these.
[0319] conclusion The provided all-solution-processed all-perovskite multijunction solar cells pave the way for the large-scale fabrication of highly efficient multijunction architectures. These tandem architectures could be realized using a highly volatile ACN / MA-based solvent system, which enabled the sequential deposition of perovskite absorbers of various energy gaps. The first all-solution-processed monolithic FA was fabricated using a highly transparent and efficient PEDOT:PSS / ITO NP recombination layer. 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 A narrow bandgap MAPbI3 / MAPbI3 tandem solar cell was fabricated and achieved a stabilized power conversion efficiency of 15.2%. 0.75 Sn 0.25 By adding an I3 perovskite junction, the optical absorption of the multi-junction is extended to 925 nm, producing the first triple-junction perovskite solar cell, achieving a record-high V of 2.83 V. oc Achieve this.
[0320] Experimental details Fabrication of upper cell (TC): Glass / FTO / SnO2 / PC 61 BM / FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3 / Spiro-OMeTAD Substrate preparation: Fluorine-doped tin oxide (FTO) coated glass (Pilkington, 15 Ω -1Devices were fabricated on a SiO2-based GaN-based GaN-GaN-GaN ...
[0321] Fabrication of tin oxide (SnO2) layer: Just before spin-coating, we used 17.5 mg ml tin oxide dissolved in anhydrous 2-propanol (IPA). -1 A SnO2 precursor solution consisting of tin(IV) chloride pentahydrate (SnCl4·5H2O) (Sigma-Aldrich) was prepared. The solution was spin-coated at 3000 rpm for 30 s with a ramp of 200 rpm / s in nitrogen. The substrate was then dried at 100 °C for 10 min in nitrogen. A subsequent annealing step was performed in air at 180 °C for 90 min.
[0322] PC 61 Preparation of BM layer: 7.5 mg ml in anhydrous chlorobenzene (CB) (Sigma) -1 PC 61 Phenyl-C61-butyric acid methyl ester (PC) was prepared by dissolving BM (99%, solenne). 61 We prepared a PCBM precursor solution using dihydro-1H-benzimidazol-2-yl (N-DBI) derivatives, specifically 3-dimethyl-2-phenyl-2,3-dihydro-1H-benzimidazole (N-DMBI). 61Doped BM (S. Rossbauer, C. Muller, TD Anthopoulos, Adv. Funct. Mater. 2014, 24, n / a; Z. Wang, DP McMeekin, N. Sakai, S. van Reenen, K. Wojciechowski, JB Patel, MB Johnston, HJ Snaith, Adv. Mater. 2017, 29, 1604186; SS Kim, S. Bae, WH Jo, Chem. Commun. 2015, 51, 17413; P. Wei, T. Menke, BD Naab, K. Leo, M. Riede, Z. Bao, J. Am. Chem. Soc. 2012, 134, 3999; BD Naab, S. Guo, S. Olthof, EGB Evans, P. Wei, (See GL Millhauser, A. Kahn, S. Barlow, SR Marder, Z. Bao, J. Am. Chem. Soc. 2013, 135, 15018; P. Wei, JH Oh, G. Dong, Z. Bao, J. Am. Chem. Soc. 2010, 132, 8852). 61 The BM precursor solution was doped with 0.25% wt% N-DMBI. The solution was then filtered using a 0.45 μm PTFE filter. We spin-coated the solution at 2000 rpm for 20 seconds with a ramp rate of 1000 rpm / s in a nitrogen-filled glove box, and annealed the substrate at 80° C. for 10 minutes.
[0323] FAI synthesis: Formamidinium iodide (FAI) was synthesized by dissolving formamidine acetate (99%, Sigma-Aldrich) in a 1.5× molar excess of hydroiodic acid (HI) (57 wt% in H2O, distilled and stabilized, 99.95% (Sigma-Aldrich)). After the acid was added, the solution was left stirring at 50°C for 10 min. After drying at 100°C for 2 h in a large glass dish, a yellow-white powder was formed. This was then washed three times with diethyl ether. The powder was later dissolved in absolute ethanol (99.5%, Sigma-Aldrich) and heated under a N2-enriched atmosphere at 120°C to obtain a supersaturated solution. Once completely dissolved, the solution was then slowly cooled to room temperature under a N2-enriched atmosphere until recrystallization occurred. The recrystallization process resulted in the formation of white flaky crystals. The solution was then placed in a refrigerator at 4°C and then transferred to a freezer for further crystallization. The powder was then washed three times with diethyl ether. Finally, the powder was dried overnight in a vacuum oven at 50°C.
[0324] FA with 2% K additive 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 3) Preparation of perovskite precursor solution: Precursor salts were dissolved in anhydrous N,N-dimethylformamide (DMF) to obtain the desired FA with a molar ratio of KI to KBr of 30% to 70%. 0.83 Cs 0.17 Pb(Br 0.7 I 0.3Formamidinium / Cs (FA / Cs) perovskite solutions with 2% K additive were prepared by obtaining a stoichiometric solution with the 3-composition and 2% K additive. The precursor solution was prepared using the following precursor salts: formamidinium iodide (FAI), cesium iodide (CsI) (99.9%, Alfa Aesar), lead iodide (PbI2) (99%, Sigma-Aldrich), lead bromide (PbBr2) (98%, Alfa Aesar), potassium iodide (KI) (99%, Sigma-Aldrich), potassium bromide (99%, KBr) (Sigma-Aldrich). Hydroiodic acid (HI) (57 wt% in HO, distilled and stabilized, 99.95%, Sigma-Aldrich) 27.2 μl / ml and hydrobromic acid (HBr) (48 wt% in HO) 54.8 μl / ml were added to 1 mL of the 0.75 M precursor solution. After the addition of the acids, the perovskite precursor solution was aged under nitrogen atmosphere for 2 days.
[0325] FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3 Preparation of perovskite layer: The aged precursor perovskite solution was spin-coated at 1200 rpm for 45 seconds with a ramp rate of 500 rpm / s in a nitrogen-filled glove box. The film was dried on a hot plate at a temperature of 70° C. in a N2 glove box for 1 minute. The film was then annealed in an oven under air atmosphere at 185° C. for 90 minutes. During this annealing process, the sample was covered with a large glass container to prevent dust contamination.
[0326] Fabrication of spiro-OMeTAD hole transport layer: The electron blocking layer was deposited with 72.5 mg / mL of 2,2',7,7'-tetrakis-(N,N-di-p-methoxyphenylamine) 9,9'-spirobifluorene (spiro-OMeTAD) (Lumtec) solution in chlorobenzene. 38 μl of lithium bis(trifluoromethanesulfonyl)imide (170 mg / mL in 1-butanol solution) was added per mL of spiro-OMeTAD solution and 21 μl of 4-tert-butylpyridine (TBP) per mL of spiro-OMeTAD solution. The sample was left in a desiccator for 24 h to oxidize. Spin coating was performed in a nitrogen-filled glove box at 2000 rpm for 20 s with a ramp rate of 1000 rpm / s.
[0327] Fabrication of recombination interlayer (for both TC / MC and MC / BC): PEDOT:PSS / ITO NP The intermediate layer is fabricated using both PEDOT:PSS (PH1000) in water (Heraeus Clevios) and a 30 wt% indium tin oxide, (ITO) >100 nm nanoparticle (NP) dispersion (Sigma) in isopropanol (IPA) as precursor solutions. First, we deposit a thin layer of PEDOT:PSS directly on top of the existing spiro-OMeTAD layer. The PEDOT:PSS precursor solution was prepared immediately before spin-coating by diluting PEDOT:PSS (PH1000) in anhydrous 2-propanol (IPA) at a 1:1.5 volume ratio (PEDOT:PSS to IPA) and then filtering through a 2.7 μm GF / D membrane filter (Whatman). The substrate was preheated at 80°C, then we dynamically spin-coated the diluted PEDOT:PSS solution at a speed of 6000 rpm for 20 seconds under a dry air atmosphere with a relative humidity (RHM) of more than 10%, and then annealed at 80°C for 10 minutes. Then we deposited the ITO NP layer. We prepared the ITO NP precursor solution by diluting 30 wt% in IPA down to 1 wt% in IPA. Before deposition, the diluted solution was sonicated in an ultrasonic bath for 15 minutes. We dynamically spin-coated the diluted ITO NP solution at a speed of 6000 rpm for 20 seconds under a dry air atmosphere with a relative humidity (RHM) of more than 10%, and then annealed at 80°C for 10 minutes.
[0328] Production of middle cell (MC): PC 61 BM / MAPbI3 / spiro-OMeTAD PC 61 Preparation of BM layer: 30 mg ml in a mixture of anhydrous chlorobenzene (CB) (sigma) and anhydrous chloroform (CF) solvents. -1 PC 61 Phenyl-C61-butyric acid methyl ester (PC) was prepared by dissolving BM (99%, Solenne). 61A PCBM precursor solution was prepared. The solvents were mixed with CB and CF in a volume ratio of 2 to 1. We used dihydro-1H-benzimidazol-2-yl (N-DBI) derivatives, specifically 3-dimethyl-2-phenyl-2,3-dihydro-1H-benzimidazole (N-DMBI), to synthesize PC 61 The inventors doped PCBM. 61 The BM precursor solution was doped with 0.25 wt% N-DMBI. The solution was then filtered using a 0.45 μm PTFE filter. The substrate was preheated at 80° C., and then we dynamically spin-coated the solution at 4000 rpm for 20 seconds under a dry air atmosphere with a relative humidity (RHM) of >10%, and annealed the substrate at 80° C. for 10 minutes.
[0329] Preparation of ACN / MA MAPbI3 perovskite precursor solution: In this procedure, we found that controlling the MA content in the acetonitrile (CH3CN) / methylamine (CH3NH2) (ACN / MA) MAPbI3 solution resulted in better tandem performance with higher reproducibility. Excess MA in the ACN / MA MAPbI3 solution could potentially seep through pinholes in the thin and incomplete interlayer, and thus dissolve the lower junction partially or entirely. Therefore, a solution containing the minimum amount of MA required to dissolve the perovskite was used. Control of the MA content in the solution could potentially be achieved by controlling the MA flow rate and the stirring speed, but these parameters were sometimes difficult to precisely control. Instead, we prepared two ACN MAPbI3 dispersions, one complete ACN / MA MAPbI3 solution with excess MA, and the other ACN MAPbI3 dispersion without MA. Just before spin-coating, ACN / MA MAPbI3 with excess MA was slowly added to the ACN MAPbI3 dispersion until the dispersion was completely dissolved and a complete solution was obtained. The resulting solution is the ACN / MA MAPbI3 solution at the critical solution point. The preparation of the ACN / MA MAPbI3 solution and the ACN MAPbI3 dispersion is described below. The MA-free ACN MAPbI3 perovskite precursor solution was prepared under nitrogen using the precursor salts methylammonium iodide (MAI) (Dyesol) and lead iodide (PbI2) (TCI) at concentrations of 1.03 M for MAI and 1 M for PbI2 in anhydrous acetonitrile (ACN) (Sigma Aldrich) to obtain a non-stoichiometric solution (1.03:1 = MAI:PbI2). The solution is then sonicated in an ultrasonic bath for 1 h to completely react MAI and PbI2, precipitating a black perovskite dispersion at the bottom of a vial filled with ACN.
[0330] ACN / MA MAPbI3 perovskite precursor solution was prepared using an adapted method described by Noel et al. (see NK Noel, SN Habisreutinger, B. Wenger, MT Klug, MT Horantner, MB Johnston, RJ Nicholas, DT Moore, HJ Snaith, Energy Environ. Sci. 2017, 10, 145). We first prepare the ACN / MA MAPbI3 perovskite precursor solution using the same preparation method as above. To dissolve the perovskite in ACN, a solution of methylamine (MA) in ethanol (Sigma Aldrich, 33 wt%) was placed in an aerator that was placed in an ice bath. Nitrogen was then bubbled into the solution to degas the MA solution. The generated MA gas was then passed through a drying tube filled with desiccants (Drietire and CaO). The ACN / MA MAPbI3 dispersion was vigorously stirred using a large magnetic stir bar at a speed of about 700 rpm while gas was bubbled through the black dispersion. The dispersion was bubbled for 15 minutes to completely dissolve the black perovskite particles and yield a clear, pale yellow solution. We noted that this solution had an "excess" amount of MA in the ACN / MA MAPbI3 solution.
[0331] Preparation of ACN / MA MAPbI3 perovskite layer: ACN / MA MAPbI3 precursor perovskite solution (at its critical dissolution point) is immediately dynamically spin-coated at 5000 rpm for 20 seconds under a dry air atmosphere with a relative humidity (RHM) of more than 10%. Then, a methylammonium chloride (MACl) post-treatment is performed by dynamically spin-coating 50 μl of MACl (Alfa Aesar, 2 mg / ml in isopropanol) at 6000 rpm for 20 seconds. The film is then annealed in an oven for 90 minutes under an air atmosphere at 80°C. During this annealing process, the sample is covered with a large glass container to prevent dust contamination.
[0332] Fabrication of spiro-OMeTAD hole transport layer: An electron blocking layer was deposited by dynamic spin coating of 85 mg / ml of 2,2',7,7'-tetrakis-(N,N-di-p-methoxyphenylamine)9,9'-spirobifluorene (spiro-OMeTAD) (Lumtec) solution in chlorobenzene. 20 μl of lithium bis(trifluoromethanesulfonyl)imide (520 mg / mL in acetonitrile solution) was added per ml of spiro-OMeTAD solution and 33 μl of 4-tert-butylpyridine (tBP) per ml of spiro-OMeTAD solution. Spin coating was performed dynamically at 2000 rpm for 30 s under a dry air atmosphere with a relative humidity (RHM) of >10%. The sample was left to oxidize in a desiccator for 24 h.
[0333] Fabrication of the lower cell (BC): PC 61 BM / ACN / MA MA-MAPb 0.75 Sn 0.25 I3 / Spiro(TFSI)2PC 61 Preparation of BM layer: 30 mg / ml -1 PC 61 Phenyl-C61-butyric acid methyl ester (PC) was prepared by dissolving BM (99%, solenne) in a mixture of anhydrous chlorobenzene (CB) (sigma) and anhydrous chloroform (CF) solvents. 61 A precursor solution of PCBM was prepared. The solvent was mixed with CB and CF in a volume ratio of 2:1. 61 The BM was doped using dihydro-1H-benzimidazol-2-yl (N-DBI) derivatives, specifically 3-dimethyl-2-phenyl-2,3-dihydro-1H-benzimidazole (N-DMBI). 61 The BM precursor solution was doped with 0.25% wt% N-DMBI. The solution was then filtered using a 0.45 μm PTFE filter. The substrate was preheated at 80° C., and then we dynamically spin-coated the solution at 4000 rpm for 20 seconds under a dry air atmosphere with a relative humidity (RHM) of >10%, and annealed the substrate at 80° C. for 10 minutes.
[0334] ACN / MA-MA Pb 0.75 Sn 0.25 Preparation of I3 perovskite precursor solution: mixed metal ACN / MA MAPb 0.75 Sn 0.25 To obtain the I3 perovskite precursor solution, we prepared ACN / MA MAPbI3 and ACN / MA MAPb 0.5 Sn 0.5 I3 (without MA) was mixed in a 1:1 volume ratio to obtain ACN / MA MAPb 0.75 Sn 0.25 I3 was obtained. ACN / MA MAPb without MA 0.5 Sn 0.5 A perovskite precursor solution was prepared under nitrogen using the precursor salts methylammonium iodide (MAI) (Dyesol), lead iodide (PbI2) (TCI), and anhydrous tin iodide (SnI2) beads (TCI) at concentrations of 0.8 M for MAI, 0.46 M for PbI2, and 0.46 M for SnI2 in anhydrous acetonitrile (Sigma Aldrich) to give a non-stoichiometric solution with a 15% excess of metal salts (1:1.15 = MAI:PbI2 + SnI2). The solution was then stirred under nitrogen at 70 °C for 1 hour to fully react the MAI with the mixed metals, and then the black perovskite dispersion was precipitated at the bottom of a vial filled with ACN.
[0335] ACN / MA MAPbI3 perovskite precursor solution was prepared using an adapted method described by Noel et al. We first prepared ACN / MA MAPbI3 perovskite precursor solution at 0.8 M in MAI and 0.46 M in PbI2, resulting in a non-stoichiometric solution with 15% excess of metal salts (1:1.15 = MAI:PbI2). To dissolve the perovskite in ACN, a solution of methylamine (MA) in ethanol H2O (Sigma Aldrich, 40 wt%) was placed in an aerator that was placed in an ice bath. Nitrogen was then bubbled into the solution to degas the MA solution. The generated MA gas was then passed through a drying tube filled with desiccants (Drietire and CaO). The gas was bubbled through the black dispersion while vigorously stirring the ACN / MA MAPbI3 dispersion using a large magnetic stir bar at a speed of about 700 rpm. The dispersion was bubbled for 15 min to completely dissolve the black perovskite particles, resulting in a clear, pale yellow solution. We noted that this solution had an "excess" amount of MA in the ACN / MA MAPbI3 solution. The solution was then stored in nitrogen with activated 3 Å molecular sieves for approximately 3 h to remove any H2O introduced during the MA bubbling process.
[0336] ACN / MA MAPb 0.75 Sn 0.25 I3 perovskite layer: This precursor perovskite solution is immediately dynamically spin-coated in a nitrogen glove box at 5000 rpm for 20 seconds. A second subsequent spin-coating step was used to deposit methylammonium chloride (MACl) as a post-treatment. 2 mg ml in IPA -1 A solution of MACl was dynamically spin-coated at 6000 rpm for 20 s, and the film was then annealed at 80 °C for 90 min in nitrogen.
[0337] Spiro(TFSI)2 synthesis: MAPb 0.75 Sn 0.25Spiro(TFSI)2 hole transport layers for use in I3 perovskites were prepared using an adapted method described by Nguyen et al. (See WH Nguyen, CD Bailie, EL Unger, MD McGehee, J. Am. Chem. Soc. 2014, 136, 10996). We first prepared a solution of 2,2',7,7'-tetrakis-(N,N-di-p-methoxyphenylamine) 9,9'-spirobifluorene (spiro-OMeTAD) (Lumtec) in chlorobenzene (CB) at 2 mg ml -1 Separately, the inventors dissolved silver(I) bis(trifluoromethanesulfonyl)imide (Ag-TFSI) in methanol at a concentration of 100 mg ml -1 We mixed both solutions in equal amounts slowly with stirring. The final molar ratio is 1 to 0.95 (spiro-OMeTAD to Ag-TFSI). We then left the mixture with stirring overnight. We filtered the solution through a 2 μm PTFE filter to remove the Ag colloids. We removed the CB using a rotary evaporator until about 5% of the original volume remained. We then added toluene to the remaining flask at a volume of 50% of the initial CB volume. We kept the solution in the refrigerator for 24 hours to precipitate a fine black powder. Once the black powder was completely precipitated, we removed the excess toluene using a glass frit filter. We washed the powder with cold toluene at 4 °C. Once the powder was dry, we dissolved it in a 20 mg ml -1 was prepared. This black powder should not have low solubility in methanol, which would initiate the precipitation process. We refrigerated the solution at 4°C overnight. The black powder was collected from the bottom of the vial. We removed the excess toluene using a glass frit filter and washed with 4°C methanol. Once dry, we collected and weighed the spiro(TFSI)2 powder.
[0338] Fabrication of spiro-OMeTAD hole transport layer doped with 10 wt% spiro(TFSI)2: The electron blocking layer was deposited by dynamic spin coating of spiro-OMeTAD doped with spiro(TFSI)2 at 2000 rpm for 30 s in a nitrogen glove box. The precursor solution was 7.25 mg ml -1 of spiro(TFSI)2 and 65.25 mg ml -1 72.5 mg ml of 2,2',7,7'-tetrakis-(N,N-di-p-methoxyphenylamine) 9,9'-spirobifluorene (spiro-OMeTAD) (Lumtec) solution -1 The spiro-OMeTAD solution was prepared using a 100% by weight solution. No additives were added to the spiro-OMeTAD solution.
[0339] Fabrication of the lower cell (BC): PEDOT:PSS / FA 0.83 Cs 0.17 Pb 0.5 Sn 0.5 I3 / PC 61 BM / BCP FA 0.83 Cs 0.17 Pb 0.5 Sn 0.5 Preparation of I3 perovskite precursor: 1.2 M of FAI was prepared by dissolving FAI (Dyesol), CsI (99.9%, Alfa Aesar), PbI2 (99.999%, Alfa Aesar), and SnI2 (99.999%, Alfa Aesar) in a 4:1 volumetric ratio of DMF:DMSO mixture under nitrogen atmosphere. 0.83 Cs 0.17 Pb 0.5 Sn 0.5 A stoichiometric solution of I3 was prepared, and 60 mM tin(II) fluoride (SnF2, 99%, Sigma Aldrich) and 36 mM lead(II) thiocyanate (99.5%, Sigma Aldrich) were also dissolved in the solution.
[0340] Device preparation: Patterned indium tin oxide (ITO) substrates were cleaned by sequential rinsing in acetone and IPA. Once dry, the substrates were cleaned with O2 plasma for 10 min. Immediately after plasma treatment, a PEDOT:PSS solution (PVP AI4083, Heraeus, 1:2 volume ratio with methanol) was spin-coated at ambient conditions at 4 krpm for 30 s and subsequently annealed at 150 °C for 10 min. The devices were immediately transferred to a N2 glove box. Just before fabricating the perovskite films, the PEDOT:PSS-coated ITO substrates were again annealed at 120 °C for 10 min. Perovskite films were fabricated by spin-coating the solution at 3.6 krpm for 14 s with a 6 s rotational ramp. 13 s after starting the spin-coating program, 200 μL of anisole was dispensed onto the spinning substrate. Once spin-coating was completed, a N2 flow was applied to the film for 15 seconds and then immediately annealed at 120 °C for 10 minutes. 61 PC was prepared by dynamic spin-coating of 50 uL of a hot solution (90 °C) of BM (20 mg / mL dissolved in a 3:1 volumetric ratio of chlorobenzene:1,2-dichlorobenzene) at 2 krpm for 30 s, followed by annealing at 90 °C for 2 min. 61 The BM layer was prepared by cooling to room temperature and dynamically spin-coating 70 μL of a 0.5 mg / mL solution of bathocuproine (BCP, 98%, Alfa Aesar) at 4 krpm for 20 s.
[0341] Electrodes: 100 nm silver or gold electrodes, approximately 10 -6 Under a vacuum of Torr, approximately 0.2 nm s -1 The mixture was then thermally evaporated at a rate of 1000 .mu.m.
[0342] Characterization of solar cells: 100mWcm irradiance generated by the Abet Class AAB Solar 2000 simulator -2Current density-voltage (JV) curves were measured (2400 Series SourceMeter, Keithley Instruments) under simulated AM1.5 sunlight and intensity calibrated with an NREL calibrated KG5 filtered Si reference cell. The mismatch was calculated to be less than 1%. The active area of the solar cell is 0.0919 cm. -2 The forward JV scan was measured from forward bias (FB) to short circuit (SC), and the reverse scan was measured from short circuit to forward bias, both at a scan rate of 0.25 V s -1 A 1 sun illumination, 5 second settling time and a forward bias of 0.3 V above the expected VOC were performed before the scan.
[0343] EQE characterization: The multijunction EQE was measured by optically biasing the unmeasured subcell with a 3W 470-475nm LED and a 3W 730-740nm LED at TC and BC, respectively. During the measurement, a negative bias equal to the Voc of the optically biased subjunction was applied to the tandem. This allows the response of the tandem under short circuit conditions to be measured.
[0344] Transient photoconductivity: A Nd:YAG laser excitation source tuned to 470 nm, pulsed at 7 ns, excited at 10 Hz is used at a range of fluences to have the various charge carrier densities described in the text. This pulsed light is irradiated over the entire sample surface, uniformly exciting the film. A bias of 24 V is applied across the in-plane (lateral) electrodes. Here, we use a two-electrode conductivity measurement, since the constant resistance between the perovskite film and the Au electrodes is rather small compared to the resistance of the sample. The variable resistor is in series with the sample in the circuit, and is always less than 1% of the sample resistance. We monitored the voltage drop across the variable series resistor through a parallel oscilloscope (1 MΩ) to determine the potential drop across the two in-plane Au electrodes (channel-to-channel distance of 4 mm) at the sample. The perovskite film is scribed to have a channel width of 5 mm and coated with 200 nm of inert PMMA. Transient photoconductivity (σ Ph ) into the formula
[0345]
number
[0346] modeling: Overview: We modelled the optical properties of the stack using the general transfer matrix method (TMM) (see E. Centurioni, Appl. Opt. 2005, 44, 7532). All calculations were done in Python making extensive use of the NumPy and SciPy libraries. The wavelength-dependent complex refractive index, layer thicknesses and angle of incidence were taken as inputs. The TMM model outputs the electric field distribution in the stack. This was used to calculate the transmission T(E), reflectance R(E) and absorptance A(E) of each layer. The short-circuit current of each subcell was then determined by assuming the internal quantum efficiency to be unity.
[0347]
number
[0348] The J-V curves from each subcell are modeled using this SC and the electrical characteristics of a state-of-the-art single-junction cell. To do this, we parameterized the JV curve of the state-of-the-art single-junction according to a single-diode equivalent model:
[0349]
number
[0350] Optical and electrical model inputs: ITO, FTO, PEDOT:PSS, PCBM, Spiro-OMeTAD, Ag, MA 0.4 FA 0.6 Sn 0.6 Pb 0.4The refractive indices of I3 and MAPbI3 are from the literature (T. A. F. Konig, P. A. Ledin, J. Kerszulis, M. A. Mahmoud, M. A. El-Sayed, J. R. Reynolds, V. V. Tsukruk, ACS Nano 2014, 8, 6182; J. M. Ball, S. D. Stranks, M. T. Horantner, S. Huttner, W. Zhang, E. J. W. Crossland, I. Ramirez, M. Riede, M. B. Johnston, R. H. Friend, H. J. Snaith, Energy Environ. Sci. 2015, 8, 602; D. Shi, V. Adinolfi, R. Comin, M. Yuan, E. Alarousu, A. Buin, Y. Chen, S. Hoogland, A. Rothenberger, K. Katsiev, Y. Losovyj, X. Zhang, P. A. Dowben, O. F. Mohammed, E. H. Sargent, O. M. Bakr, Science 2015, 347, 519; V. S. Gevaerts, L. J. A. Koster, M. M. Wienk, R. A. J. Janssen, ACS Appl. Mater. Interfaces 2011, 3, 3252; M. Filipic, P. Loper, B. Niesen, S. De Wolf, J. Krc, C. Ballif, M. Topic, Opt. Express 2015, 23, A263; P. B. Johnson, R. W. Christy, Phys. Rev. B 1972, 6, 4370; M. T. Horantner, T. Leijtens, M. E. Ziffer, G. E. Eperon, M. G. Christoforo, M. D. McGehee, H. J. Snaith, ACS Energy Lett. 2017, 2, 2506; P. Loper, M. Stuckelberger, B. Niesen, J.Werner, M. Filipic, S.-J. Moon, J.-H. Yum, M. Topic, S. De Wolf, C. Ballif, J. Phys. Chem. Lett. 2015, 6, 66). F.A. 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 The extinction coefficient k of 3 was calculated by measuring the transmittance T and reflectance R of a thin film of thickness t on glass and using the following relationship:
[0351]
number
[0352]
number
[0353]
number
[0354] Tandem Simulation FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3 / MAPbI3 simulation - Figure 4A, B: The thicknesses used in the optical model are taken from SEM cross sections of the tandem. 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 The electrical properties of ACN-treated MAPbI3 and MAPbI3 are extracted from our own single-junction devices (Figure 7). The dotted JV line models the performance that MAPbI3 is expected to perform similarly to the best ACN-treated MAPbI3 cells in the literature.
[0355] [Table 1]
[0356] FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3)3 / MAPbI3 (optimized) - Fig. 4C,D: We limit the thickness of the non-perovskite layer to 50 nm. We add a MgF2 anti-reflection coating. We optimize the thickness of the perovskite layer and the anti-reflection coating using a differential evolution algorithm to maximize the limiting current. FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 The electrical properties of MAPbI3 are from our own device (Fig. 7). The properties of MAPbI3 are from the best MAPbI3 cell in the literature (see SS Shin, EJ Yeom, WS Yang, S. Hur, MG Kim, J. Im, J. Seo, JH Noh, S. Il Seok, Science 2017, 356, 167). The dotted JV curve models the performance of the tandem where the top cell is assumed to perform electrically similar to current state-of-the-art perovskites. We followed the approach of Hoerantner et al. for this (see MT Hoerantner, T. Leijtens, ME Ziffer, GE Eperon, MG Christoforo, MD McGehee, HJ Snaith, ACS Energy Lett. 2017, 2, 2506) and used the EQE EL = 0.01, R S =4 10 -2 Ωcm 2 and R SH =10MΩcm 2 It is assumed that:
[0357] [Table 2]
[0358] FA 0.83 Cs 0.17 Pb(Br 0.7 I 0.3 )3 / MAPbI3 / MA 0.4 FA 0.6 Pb 0.4 Sn 0.6I3 (Optimization) Simulation - Fig. 4E, F: The calculations in Fig. 4E, F are carried out similarly to Fig. C, D. In the dotted triple junction JV curves, both the bottom and top cells are modeled as current state-of-the-art perovskite cells.
[0359] [Table 3]
Claims
1. 1. A method of manufacturing a multijunction device including a layer of crystalline A / M / X material, comprising: A crystalline A / M / X material has the formula [A] a [M] b [X] c (In the formula, [A] contains one or more A cations, [M] comprises one or more M cations which are metal or metalloid cations; [X] comprises one or more X anions; a is a number from 1 to 6, b is a number from 1 to 6, (c is a number between 1 and 18) The compound includes the method includes forming a layer of the crystalline A / M / X material by disposing a film-forming solution on a substrate; Here, the membrane-forming solution is (a) one or more M cations, and (b) Solvent Including, The solvent is (i) an aprotic solvent, and (ii) Organic amines Including, The substrate is a photoactive region comprising a photoactive material; and a charge recombination layer disposed over the photoactive region by solution deposition; wherein the charge recombination layer comprises nanoparticles of a transparent conductive oxide disposed in an electron transporting organic matrix material, and the charge recombination layer further comprises a conductive polymer.
2. The method of claim 1 , wherein the aprotic solvent is a polar aprotic solvent and / or the substrate further comprises a layer of a charge transport material disposed on the charge recombination layer.
3. disposing said charge recombination layer over said photoactive region by solution deposition. The method according to claim 1 or 2, comprising the step of producing the substrate by
4. The method of claim 3 , further comprising disposing a layer of a charge transport material over the charge recombination layer.
5. 5. The method of any one of claims 1 to 4, wherein the photoactive material in the substrate is soluble in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof, or at least one component of the charge recombination layer in the substrate is soluble in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof.
6. 6. The method of claim 5, wherein both the photoactive material in the substrate and at least one component of the charge recombination layer in the substrate are dissolved in dimethylformamide (DMF), dimethylsulfoxide (DMSO), or a mixture thereof.
7. The method of any one of claims 1 to 6, wherein the transparent conductive oxide comprises indium tin oxide (ITO).
8. The method of any one of claims 1 to 7, wherein the organic matrix material comprises [6,6]-phenyl-C61-butyric acid methyl ester (PCBM).
9. The method of any one of claims 1 to 8, wherein the conductive polymer comprises poly(3,4-ethylenedioxythiophene) and polystyrenesulfonate (PEDOT:PSS).
10. 10. The method of any one of claims 1 to 9, wherein disposing the charge recombination layer over the photoactive region comprises disposing a solvent dispersion of nanoparticles of a transparent conductive oxide over the photoactive region.
11. 11. The method of claim 10, wherein disposing the charge recombination layer over the photoactive region comprises disposing a conductive polymer over the photoactive region and disposing a solvent dispersion of nanoparticles of a transparent conductive oxide over the photoactive region.
12. 12. The method according to claim 10 or claim 11, wherein the solvent dispersion of nanoparticles and / or the conductive polymer are disposed on the photoactive area by spin coating.
13. the aprotic solvent does not comprise dimethylformamide or dimethylsulfoxide or a mixture thereof; and / or the aprotic solvent comprises a compound selected from the group consisting of chlorobenzene, acetone, butanone, methyl ethyl ketone, acetonitrile, propionitrile, toluene or mixtures thereof; and / or The organic amine is an unsubstituted or substituted alkylamine or an unsubstituted or substituted arylamine; 13. The method according to any one of claims 1 to 12.
14. 14. The method of claim 13, wherein the aprotic solvent comprises acetonitrile.
15. The organic amine may be unsubstituted or substituted (C 1~10 15. The method according to claim 13 or 14, wherein the amine is a (alkyl)amine.
16. 16. The method of claim 15, wherein the organic amine is methylamine, ethylamine, propylamine, butylamine or pentylamine or hexylamine, benzylamine or phenylethylamine.
17. 17. The method of claim 16, wherein the organic amine is methylamine.
18. The above formula [A] a [M] b [X] c The compound of formula [A][M][X] 3 and / or a compound of the formula: [A] contains at least one organic cation, and / or Each A cation is an alkali metal cation, a compound of the formula [R 1 R 2 R 3 R 4 N] + (In the formula, R 1 , R 2 , R 3 , R 4 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl; R 1 , R 2 , R 3 and R 4 at least one of which is not hydrogen; 5 R 6 N=CH-NR 7 R 8 ] + (In the formula, R 5 , R 6 , R 7 and R 8 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl), and C 1~10 Alkylammonium, C 2~10 Alkenylammonium, C 1~10 Alkyliminium, C 3~10 Cycloalkylammonium and C 3~10 Cycloalkyliminium (which may be unsubstituted or amino, C 1~6 Alkylamino, imino, C 1~6 Alkylimino, C 1~6 Alkyl, C 2~6 Alkenyl, C 3~6 Cycloalkyl and C 6~12 aryl), and / or [M] comprises two or more different M cations, and / or Each M cation is Ca 2+ , Sr 2+ , Cd 2+ , Cu 2+ , Ni 2+ , Mn 2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ and Eu 2+ and / or each X anion is a halide; and / or [A] is a compound represented by the formula [R 1 NH 3 ] + (In the formula, R 1 is unsubstituted C 1~10 alkyl), and the organic amine is unsubstituted (C 1~10 18. The method of claim 1, comprising the step of:
19. Each A cation is Cs + , Rb + 19. The method of claim 18, wherein the ammonium salt is selected from the group consisting of methylammonium, dimethylammonium, trimethylammonium, ethylammonium, propylammonium, butylammonium, pentylammonium, hexylammonium, heptylammonium, octylammonium, tetramethylammonium, formamidinium, 1-aminoethane-1-iminium and guanidinium.
20. Each M cation is Sn 2+ and Pb 2+ 20. The method of claim 18 or 19, wherein the method is selected from the group consisting of:
21. 21. The method of any one of claims 18 to 20, wherein [X] comprises two or more different halide anions.
22. Formula [R 1 NH 3 ] + C on A cation 1~10 Alkyl groups and unsubstituted (C 1~10 C on alkyl amines 1~10 The method according to any one of claims 18 to 21, wherein the alkyl groups are the same.
23. The photoactive material in the photoactive region in the substrate comprises a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] as defined in any one of claims 1 or 18 to 22. a [M] b [X] c and / or the substrate comprises two separate photoactive regions, each photoactive region comprising a photoactive material; and / or the membrane-forming solution further comprises one or more A cations and one or more X anions; and / or the method further comprises disposing a composition comprising one or more A cations onto the substrate; and / or and / or the step of disposing the film-forming solution on the substrate comprises spin-coating the film-forming solution on the substrate; 23. The method of any one of claims 1 to 22, wherein the method further comprises removing the solvent to form the layer comprising the crystalline A / M / X material.
24. The substrate comprises two separate photoactive regions, each photoactive region comprising a photoactive material comprising a crystalline A / M / X material, the crystalline A / M / X material having formula [A] as defined in any one of claims 1 or 18 to 22. a [M] b [X] c 24. The method of claim 23, comprising the compound of formula:
25. 25. The method of claim 23 or claim 24, wherein the method further comprises disposing a composition comprising one or more A cations and one or more X anions onto the substrate.
26. 26. The method of any one of claims 23 to 25, wherein the method further comprises removing the solvent to form the layer comprising the crystalline A / M / X material, and wherein the solvent is removed by heating a substrate treated with a film-forming solution.
27. the substrate further comprises a first electrode; The method further comprising: disposing a second electrode on the layer of crystalline A / M / X material disposed on the substrate; or disposing a charge transport material over the layer of crystalline A / M / X material disposed on the substrate and disposing a second electrode over the charge transport material. Further comprising:
27. The method according to any one of claims 1 to 26.
28. 28. The method of claim 27, wherein the substrate comprises a layer of a charge transport material disposed on the charge recombination layer.
29. 28. The method of claim 27, wherein the second electrode comprises an elemental metal.
30. (a) at least two photoactive regions, at least one of the photoactive regions comprising a layer of a crystalline A / M / X material, the crystalline A / M / X material having the formula [A] a [M] b [X] c at least two photoactive regions comprising a compound of the formula: wherein [A] comprises one or more A cations, [M] comprises one or more M cations that are metal or metalloid cations, [X] comprises one or more X anions, a is a number from 1 to 6, b is a number from 1 to 6, and c is a number from 1 to 18; and (b) at least one charge recombination layer, the charge recombination layer comprising nanoparticles of a transparent conductive oxide disposed in an electron transporting organic matrix material, the charge recombination layer further comprising a conductive polymer; A multijunction device comprising:
31. the charge recombination layer comprises indium tin oxide; and / or two of the photoactive regions comprise a layer of the crystalline A / M / X material; and / or The multijunction device of claim 30 , wherein the multijunction device comprises at least three photoactive regions.
32. 32. The multijunction device of claim 31 , wherein each photoactive region comprises a layer of the crystalline A / M / X material.
33. [A] contains at least one organic cation, and / or Each A cation is an alkali metal cation, a compound of the formula [R 1 R 2 R 3 R 4 N] + (In the formula, R 1 , R 2 , R 3 , R 4 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl; R 1 , R 2 , R 3 and R 4 at least one of which is not hydrogen; 5 R 6 N=CH-NR 7 R 8 ] + (In the formula, R 5 , R 6 , R 7 and R 8 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl), and C 1~10 Alkylammonium, C 2~10 Alkenylammonium, C 1~10 Alkyliminium, C 3~10 Cycloalkylammonium and C 3~10 Cycloalkyliminium (which may be unsubstituted or amino, C 1~6 Alkylamino, imino, C 1~6 Alkylimino, C 1~6 Alkyl, C 2~6 Alkenyl, C 3~6 Cycloalkyl and C 6~12 aryl), and / or [M] comprises two or more different M cations, and / or Each M cation is Ca 2+ , Sr 2+ , Cd 2+ , Cu 2+ , Ni 2+ , Mn 2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ and Eu 2+ and / or each X anion is a halide; The multijunction device of any one of claims 30 to 32.
34. the multijunction device comprises at least two charge recombination layers disposed between the photoactive regions; and / or the multijunction device comprises at least two charge recombination layers, at least one of the second or further charge recombination layers comprising nanoparticles of a conductive polymer or a transparent conductive oxide; and / or 34. The multijunction device of claim 33, wherein the multijunction device comprises at least two charge recombination layers, and at least one of the second or further charge recombination layers comprises nanoparticles of a transparent conductive oxide and a conductive polymer.
35. each photoactive region includes a layer of crystalline A / M / X material; [A] contains at least one organic cation, and / or Each A cation is an alkali metal cation, a compound of the formula [R 1 R 2 R 3 R 4 N] + (In the formula, R 1 , R 2 , R 3 , R 4 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl; R 1 , R 2 , R 3 and R 4 at least one of which is not hydrogen; 5 R 6 N=CH-NR 7 R 8 ] + (In the formula, R 5 , R 6 , R 7 and R 8 each independently represents hydrogen, unsubstituted or substituted C 1~20 Alkyl, and unsubstituted or substituted C 6~12 aryl), and C 1~10 Alkylammonium, C 2~10 Alkenylammonium, C 1~10 Alkyliminium, C 3~10 Cycloalkylammonium and C 3~10 Cycloalkyliminium (which may be unsubstituted or amino, C 1~6 Alkylamino, imino, C 1~6 Alkylimino, C 1~6 Alkyl, C 2~6 Alkenyl, C 3~6 Cycloalkyl and C 6~12 aryl), and / or [M] comprises two or more different M cations, and / or Each M cation is Ca 2+ , Sr 2+ , Cd 2+ , Cu 2+ , Ni 2+ , Mn 2+ , Fe 2+ , Co 2+ , Pd 2+ , Ge 2+ , Sn 2+ , Pb 2+ , Yb 2+ and Eu 2+ and / or each X anion is a halide; and / or At least one of the charge recombination layers comprises (i) nanoparticles of indium tin oxide (ITO) and (ii) a polymer comprising poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate; and / or At least two of the crystalline A / M / X materials are different from each other; and / or 35. The multijunction device of any one of claims 30 to 34, wherein the multijunction device further comprises a first electrode and a second electrode, and at least one of the photoactive region and the charge recombination layer is disposed between the first electrode and the second electrode.
Citation Information
Patent Citations
photocell
JP2017503348A
photovoltaic device
JP2018517303A
Organic tandem photovoltaic device and methods
US20160005795A1
A / m / x material production process with alkylamine
WO2017153752A1