Manufacturing method for individual pieces of phosphor glass thin plate
The described method addresses the breakage issue in thin phosphor glass plate manufacturing by polishing both surfaces and cutting along grooves, resulting in reliable production of thin plates with improved luminous efficiency and brightness contrast.
Patent Information
- Application Number
- JP2018102191
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-02-05
- Filing Date
- 2018-05-29
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2038-05-29
AI Technical Summary
Thin phosphor glass plates are prone to breakage during manufacturing, leading to lower yield and making it difficult to produce thinner plates reliably.
A method involving polishing both main surfaces of a phosphor glass base material using a polishing member with an abrasive layer, rotating the member and stage in opposite directions, and fixing the glass on a stage for reliable thin plate production, followed by cutting along dividing grooves to create individual pieces with precise thickness and surface roughness.
The method enables the reliable production of thin phosphor glass plates and individual pieces with reduced breakage, enhancing luminous efficiency and brightness contrast in light-emitting devices.
Smart Images

Figure 0007561481000001 
Figure 0007561481000002 
Figure 0007561481000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a phosphor glass thin plate and individual pieces thereof, and to a phosphor glass thin plate and individual pieces thereof. [Background technology]
[0002] In recent years, light-emitting devices using LEDs and LDs have been attracting attention as next-generation light sources to replace fluorescent lamps and incandescent lamps. As an example of such a next-generation light source, a light-emitting device has been disclosed that combines an LED that emits blue light with a wavelength conversion member that includes a phosphor layer that absorbs part of the light from the LED and converts it to yellow light. This light-emitting device emits white light that is a composite light of the blue light emitted from the LED and the yellow light emitted from the wavelength conversion member. Patent Document 1 proposes a wavelength conversion member as a phosphor glass plate in which phosphor powder is dispersed in a glass matrix. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-122067 A Summary of the Invention [Problem to be solved by the invention]
[0004] The thinner the phosphor glass plate, the higher the luminous flux value can be and the easier it is to reduce the size. However, the thinner the phosphor glass plate, the more likely it is to break during production, which reduces the yield.
[0005] An object of the present invention is to provide a method for producing a phosphor glass thin plate, which can produce a phosphor glass thin plate more reliably.
[0006] Another object of the present invention is to provide a phosphor glass sheet more reliably. [Means for solving the problem]
[0007] The method for manufacturing a phosphor glass thin plate of the present invention is characterized by comprising the steps of: preparing a phosphor glass base material having opposing first and second main surfaces; placing the phosphor glass base material on a stage and fixing the second main surface to the stage; and polishing the first main surface of the phosphor glass base material with a polishing member having an abrasive layer.
[0008] It is preferable that the method further comprises the steps of fixing the first main surface of the phosphor glass base material on a stage, and polishing the second main surface of the phosphor glass base material with a polishing member.
[0009] In the step of polishing the phosphor glass base material, it is preferable that the polishing member is rotated about a rotation axis extending in the thickness direction of the phosphor glass base material.
[0010] In the step of polishing the phosphor glass base material, it is preferable that the stage is rotated about a rotation axis extending in the thickness direction of the phosphor glass base material.
[0011] In the step of polishing the phosphor glass base material, it is more preferable that the polishing member and the stage are rotated in opposite directions about a rotation axis extending in the thickness direction of the phosphor glass base material.
[0012] In the step of polishing the phosphor glass base material, it is preferable to polish it so that the thickness becomes 0.15 mm or less.
[0013] In the step of polishing the phosphor glass base material, it is preferable to polish the phosphor glass base material so that the arithmetic mean roughness (Ra) of the surface to be polished out of the first main surface and the second main surface is less than 0.1 μm.
[0014] The phosphor glass base material is preferably fixed onto the stage by suction.
[0015] After the step of polishing the phosphor glass base material, it is preferable to separate the phosphor glass base material from the stage by injecting a liquid onto the phosphor glass base material from the stage side.
[0016] The method for manufacturing individual pieces of a thin phosphor glass plate of the present invention is characterized by comprising the steps of: forming a dividing groove on a main surface of the thin phosphor glass plate manufactured by the above-described manufacturing method; and breaking the thin phosphor glass plate along the dividing groove.
[0017] The phosphor glass thin plate of the present invention has first and second main surfaces opposed to each other, the first main surface having an arithmetic mean roughness (Ra) of less than 0.1 μm, and a thickness of 0.15 mm or less.
[0018] The individual pieces of the phosphor glass thin plate of the present invention are individual pieces of the phosphor glass thin plate formed by dividing the above-mentioned phosphor glass thin plate, and are characterized in that the thickness of a portion located at the outer peripheral edge in a planar view is thinner than the thickness of a portion located at the center in a planar view. Effect of the Invention
[0019] According to the present invention, it is possible to provide a method for producing a phosphor glass thin plate, which can more reliably produce a phosphor glass thin plate and an individual piece thereof. Also, according to the present invention, it is possible to more reliably provide a phosphor glass thin plate and an individual piece thereof. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic cross-sectional view showing a phosphor glass thin plate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic enlarged cross-sectional view showing a phosphor glass thin plate according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing an individual piece of a phosphor glass thin plate according to one embodiment of the present invention. [Figure 4] FIG. 2 is a schematic plan view for explaining a method for producing a phosphor glass thin plate according to an embodiment of the present invention. [Diagram 5]5(a) and 5(b) are schematic cross-sectional views for explaining a method for producing a phosphor glass thin plate according to one embodiment of the present invention. [Figure 6] 1 is a diagram showing a polishing member used in a manufacturing method of a phosphor glass thin plate according to an embodiment of the present invention, viewed from the side where a phosphor glass base material is polished. FIG. [Figure 7] FIG. 2 is a schematic perspective view for explaining a method for producing a phosphor glass thin plate according to an embodiment of the present invention. [Figure 8] 8(a) and 8(b) are schematic cross-sectional views for explaining a method for producing a phosphor glass thin plate according to one embodiment of the present invention. [Figure 9] 9(a) and 9(b) are schematic cross-sectional views illustrating a method for producing a phosphor glass thin plate according to one embodiment of the present invention. [Figure 10] 1 is a schematic cross-sectional view showing an example of a light-emitting device using an individual piece of a phosphor glass thin plate according to an embodiment of the present invention. [Figure 11] FIG. 1 is a schematic plan view showing an example of a light-emitting device using an individual piece of a phosphor glass thin plate according to an embodiment of the present invention. [Figure 12] FIG. 2 is a schematic cross-sectional view of a light-emitting device of a comparative example. [Figure 13] FIG. 2 is a schematic plan view of a light-emitting device of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in each drawing, components having substantially the same functions may be referred to by the same reference numerals.
[0022] (Phosphor glass thin plate and individual pieces) Fig. 1 is a schematic cross-sectional view showing a phosphor glass thin plate according to one embodiment of the present invention. Fig. 2 is a schematic enlarged cross-sectional view showing a phosphor glass thin plate according to one embodiment of the present invention. The phosphor glass thin plate 1 shown in Fig. 1 is used, for example, as a wavelength conversion member. As shown in Fig. 2, in this embodiment, the phosphor glass thin plate 1 has a phosphor 2 and a glass matrix 3 in which the phosphor 2 is dispersed.
[0023] For example, excitation light is emitted from a light source such as an LED, and the excitation light is incident on the phosphor glass thin plate 1. A part of the excitation light is wavelength-converted by the phosphor 2, and fluorescence is emitted. The combined light of the fluorescence and the excitation light is emitted from the phosphor glass thin plate 1.
[0024] The phosphor 2 is not particularly limited as long as it emits fluorescence when excitation light is incident on it. Specific examples of the phosphor 2 include at least one selected from oxide phosphors, nitride phosphors, oxynitride phosphors, chloride phosphors, oxychloride phosphors, sulfide phosphors, oxysulfide phosphors, halide phosphors, chalcogenide phosphors, aluminate phosphors, halophosphate chloride phosphors, and garnet compound phosphors. When blue light is used as the excitation light, for example, a phosphor that emits green light, yellow light, or red light as fluorescence can be used.
[0025] The glass matrix 3 is not particularly limited as long as it can be used as a dispersion medium for the phosphor 2. For example, borosilicate glass, phosphate glass, tin phosphate glass, bismuthate glass, etc. can be used. Examples of borosilicate glass include those containing, by mass%, 30% to 85% SiO2, 30% to 30% Al2O, 30% to 50% B2O, 0% to 10% Li2O+Na2O+K2O, and 0% to 50% MgO+CaO+SrO+BaO. Examples of tin phosphate glass include those containing, by molar%, 30% to 90% SnO and 51% to 70% P2O.
[0026] As shown in FIG. 1, the phosphor glass thin plate 1 has a first main surface 1a and a second main surface 1b facing each other. The arithmetic mean roughness (Ra) of the first main surface 1a and the second main surface 1b is less than 0.1 μm. This makes it difficult for light to be scattered when excitation light is incident on the phosphor glass thin plate 1. Similarly, when a composite light of the excitation light and the fluorescence is emitted from the phosphor glass thin plate 1, light scattering is difficult to occur. This makes it possible to improve the luminous efficiency. Note that it is sufficient that at least the arithmetic mean roughness (Ra) of the first main surface 1a is less than 0.1 μm. Here, the arithmetic mean roughness (Ra) in this specification is the arithmetic mean roughness (Ra) specified in JIS B 0601:2013.
[0027] The arithmetic mean roughness (Ra) of the first principal surface 1a and the second principal surface 1b is preferably 0.05 μm or less, thereby enabling the luminous efficiency to be further increased.
[0028] The thickness of the phosphor glass thin plate 1 is preferably 0.03 mm to less than 0.3 mm, 0.05 mm to 0.15 mm, and particularly preferably 0.08 mm to 0.12 mm. This makes it possible to effectively increase the luminous flux value. In addition, it is possible to obtain the effect of improving the luminance contrast, as described later.
[0029] The phosphor glass thin plate 1 of this embodiment has a rectangular shape in plan view. However, the shape of the phosphor glass thin plate 1 in plan view is not limited to the above, and may be, for example, a substantially circular shape or a polygon other than a rectangle.
[0030] FIG. 3 is a schematic cross-sectional view showing an individual piece of a phosphor glass thin plate according to an embodiment of the present invention. As shown in FIG. 3, an individual piece 11 of the phosphor glass thin plate has a first main surface 11a and a second main surface 11b facing each other. The individual piece 11 of the phosphor glass thin plate is formed by dividing a phosphor glass thin plate 1. More specifically, the phosphor glass thin plate 1 is broken along a division groove formed by scribing the first main surface 1a or the like. Therefore, when the thickness of a portion located at the outer peripheral edge 11c of the phosphor glass thin plate individual piece 11 in a plan view is T1 and the thickness of a portion located at the center of the phosphor glass thin plate individual piece 11 in a plan view is T2, the thickness T1 is thinner than the thickness T2.
[0031] By using the phosphor glass thin plate piece 11 in a light emitting device, it is possible to effectively increase the luminance contrast between the light emitting portion and the non-light emitting portion. The details of this will be described with reference to an example of the light emitting device.
[0032] Fig. 10 is a schematic cross-sectional view showing an example of a light-emitting device using an individual piece of a phosphor glass thin plate according to one embodiment of the present invention. Fig. 11 is a schematic plan view showing an example of a light-emitting device using an individual piece of a phosphor glass thin plate according to one embodiment of the present invention.
[0033] As shown in Fig. 10, light-emitting device 30 includes phosphor glass thin plate piece 11, a light source 34 that causes excitation light to be incident on phosphor glass thin plate piece 11, and a reflecting member 35 provided to surround phosphor glass thin plate piece 11 and light source 34. As shown in Fig. 11, the light-emitting portion of light-emitting device 30 is the portion where phosphor glass thin plate piece 11 is arranged in plan view. The non-light-emitting portion is the portion where reflecting member 35 is arranged in plan view.
[0034] For example, an LED chip or the like can be used as the light source 34. For example, a resin containing a filler having high reflectance can be used as the material for the reflective member 35.
[0035] Fig. 12 is a schematic cross-sectional view of a light emitting device of a comparative example, and Fig. 13 is a schematic plan view of the light emitting device of the comparative example.
[0036] In the light-emitting device 100 of the comparative example shown in FIG. 12, a thick phosphor glass piece 101 is used. Here, the reflecting member 35 does not reflect all of the excitation light and the fluorescence. The excitation light and the fluorescence may pass through the contact portion where the phosphor glass piece 101 and the reflecting member 35 are in contact, and may leak from the non-light-emitting portion around the light-emitting portion, as shown by the dashed arrow. The leakage is particularly likely to occur in areas with high energy. In the comparative example, since the phosphor glass piece 101 is thick, the contact portion is also thick, and the leakage of light from the non-light-emitting portion cannot be sufficiently suppressed. Therefore, the contrast near the boundary between the light-emitting portion and the non-light-emitting portion is low. As shown in FIG. 13, the leakage may cause the area E where the luminance is relatively high in the non-light-emitting area to become wider.
[0037] In contrast, in the light-emitting device 30 shown in Fig. 10, the phosphor glass thin plate piece 11 is thin, so that the contact portion with the reflective member 35 can be effectively thinned. Therefore, the leakage of excitation light and fluorescence from the non-light-emitting portion can be effectively suppressed, and the contrast near the boundary between the light-emitting portion and the non-light-emitting portion can be effectively increased. As shown in Fig. 11, the above leakage can be suppressed from widening the area E where the luminance is relatively high in the non-light-emitting region. Therefore, when designing an optical system that combines optical components such as lenses and mirrors, stray light is less likely to occur in the light-emitting device 30, and light distribution characteristics that conform to the optical design can be easily obtained.
[0038] The light-emitting device 30 incorporating the individual pieces 11 of the phosphor glass thin plate can be suitably used, for example, in ADB (adaptable beam) headlights, which require high directionality and high contrast near the boundary between the illuminated and non-illuminated areas.
[0039] An anti-reflection film may be provided on the first main surface 11a (light exit surface) of the phosphor glass thin plate piece 11. In this way, when the fluorescence or excitation light is emitted from the first main surface 11a, it is possible to suppress a decrease in the light extraction efficiency caused by the refractive index difference between the phosphor glass thin plate piece 11 and air. Examples of the anti-reflection film include single-layer or multi-layer dielectric films made of SiO2, Al2O3, TiO2, Nb2O5, Ta2O5, etc. In addition, an anti-reflection film may be provided on the second main surface 11b (light entrance surface) of the phosphor glass thin plate piece 11. In this way, it is possible to suppress a decrease in the excitation light incidence efficiency caused by the refractive index difference between the phosphor glass thin plate piece 11 and an adhesive layer (not shown) (adhesive layer provided between the phosphor glass thin plate piece 11 and the light source 34) when the excitation light is incident on the phosphor glass thin plate piece 11.
[0040] Incidentally, the anti-reflection film is usually designed taking into consideration the refractive index of the glass matrix 3 in the phosphor glass thin plate piece 11. Here, if the phosphor is exposed on the first main surface 11a of the phosphor glass thin plate piece 11, the phosphor has a relatively high refractive index, so that the anti-reflection film formed on the phosphor portion is not appropriately designed, and there is a risk that sufficient anti-reflection function cannot be obtained. Therefore, it is preferable to provide a glass layer (a glass layer not containing phosphor) on the first main surface 11a of the phosphor glass thin plate piece 11 so that the exposed phosphor is covered. In this way, the refractive index of the first main surface 11a of the phosphor glass thin plate piece 11 becomes uniform, and the effect of the anti-reflection film can be enhanced. It is also preferable to provide a glass layer on the second main surface 11b of the phosphor glass thin plate piece 11 in order to enhance the anti-reflection effect as described above.
[0041] The glass constituting the glass layer is preferably the same as the glass constituting the glass matrix 3 in the phosphor glass thin plate piece 11. In this way, the difference in refractive index between the glass matrix 3 in the phosphor glass thin plate piece 11 and the glass layer becomes extremely small, and light reflection loss at both interfaces can be suppressed. The thickness of the glass layer is preferably 0.003 mm to 0.1 mm, 0.005 mm to 0.03 mm, and particularly 0.01 mm to 0.02 mm. If the glass layer is too thin, it may not be possible to sufficiently cover the exposed phosphor. On the other hand, if the glass layer is too thick, excitation light and fluorescence may be absorbed, resulting in a decrease in luminous efficiency.
[0042] Generally, the thinner the phosphor glass sheet to be obtained, the more likely it is that the phosphor glass sheet will crack during production. In particular, when a phosphor glass sheet with a thickness of less than 0.3 mm is to be obtained, the phosphor glass sheet will be more likely to crack during the production process. In contrast, the phosphor glass sheet 1 and phosphor glass sheet pieces 11 according to the present invention can be produced more reliably by the production method described below. However, the production method described below is only one example of the method for producing the phosphor glass sheet according to the present invention.
[0043] (Manufacturing method) FIG. 4 is a schematic plan view for explaining a method for producing a phosphor glass thin plate according to one embodiment of the present invention. FIGS. 5(a) and 5(b) are schematic cross-sectional views for explaining a method for producing a phosphor glass thin plate according to one embodiment of the present invention. FIG. 6 is a view of a polishing member used in a method for producing a phosphor glass thin plate according to one embodiment of the present invention, seen from the side where a phosphor glass base material is polished. FIG. 7 is a schematic perspective view for explaining a method for producing a phosphor glass thin plate according to one embodiment of the present invention. FIGS. 8(a) and 8(b) are schematic cross-sectional views for explaining a method for producing a phosphor glass thin plate according to one embodiment of the present invention. Note that FIGS. 5(a) and 5(b) and FIGS. 8(a) and 8(b) show a cross section corresponding to a portion along line II in FIG. 7.
[0044] As shown in Fig. 4, a plurality of phosphor glass base materials 21 are prepared. The phosphor glass base material 21 is a base material having the phosphor 2 shown in Fig. 2 and the glass matrix 3 in which the phosphor 2 is dispersed. The phosphor glass base material 21 has a first main surface 21a and a second main surface 21b facing each other. It is sufficient to prepare at least one phosphor glass base material 21.
[0045] Next, the phosphor glass base material 21 is placed on the stage 22, and the second main surface 21b is fixed on the stage 22. Here, as shown in FIG. 5(a), the stage 22 has a plurality of first holes 22a and a plurality of second holes 22b. In this embodiment, the phosphor glass base material 21 is fixed on the stage 22 by sucking it through the plurality of first holes 22a as shown by arrow A. Note that the method of fixing the phosphor glass base material 21 is not limited to the above. Also, the first holes 22a and the second holes 22b may be connected to each other.
[0046] Next, as shown in FIG. 5(b), the first main surface 21a of the phosphor glass base material 21 is polished by the polishing member 23. Here, as shown in FIG. 6, the polishing member 23 has an abrasive layer 24. The abrasive layer 24 has a circular ring shape. The abrasive layer 24 may be composed of a plurality of abrasive layer pieces arranged in a circular ring shape. In this case, it is preferable that a gap is provided between each adjacent abrasive layer piece at an interval of, for example, 5° or more and 15° or less in a plan view. In this way, the polishing sludge generated in the process of polishing the phosphor glass base material 21 can be efficiently discharged to the outside through the gap between each abrasive layer piece. In this embodiment, the abrasive layer 24 is a glass sintered body containing diamond particles. The polishing member 23 has a substantially cylindrical shape and has an opening 23a. However, the shape and material of the abrasive layer 24 and the shape of the polishing member 23 are not limited to the above.
[0047] As shown in FIG. 7, in the step of polishing the phosphor glass base material 21, the polishing member 23 and the stage 22 are arranged so that the center of the polishing member 23 and the center of the stage 22 are at different positions in a plan view. In this embodiment, the polishing member 23 is arranged so that the outer periphery of the abrasive layer 24 reaches the center of the stage 22 in a plan view. Next, as shown by the arrow B in FIG. 7, the polishing member 23 is rotated counterclockwise around a rotation axis extending in the thickness direction of the phosphor glass base material 21. Furthermore, as shown by the arrow C, the stage 22 is rotated clockwise around the rotation axis extending in the thickness direction. That is, the polishing member 23 and the stage 22 are rotated in opposite directions to each other around the rotation axis extending in the thickness direction. This allows the phosphor glass base material 21 to be polished efficiently. However, the phosphor glass base material 21 may be rotated clockwise and the stage 22 may be rotated counterclockwise.
[0048] Although the positional relationship between the polishing member 23 and the stage 22 in a plan view is not particularly limited, it is preferable that, as in this embodiment, the outer periphery of the abrasive layer 24 reaches the center of the stage 22. This makes it possible to reliably and efficiently polish all of the phosphor glass base materials 21 on the stage 22 by rotating the polishing member 23 and the stage 22 in the opposite directions as described above.
[0049] It should be noted that the method of polishing the phosphor glass base material 21 is not limited to the above. For example, the phosphor glass base material 21 may be polished by rotating only one of the polishing member 23 and the stage 22. Alternatively, the phosphor glass base material 21 may be polished by translating at least one of the polishing member 23 and the stage 22.
[0050] Conventionally, when manufacturing a phosphor glass thin plate, the phosphor glass base material is fixed by fitting it into an opening of a plate-shaped jig (carrier) having an opening placed on a stage. Therefore, in order to polish the main surface of the phosphor glass base material, it is necessary to make the thickness of the jig thinner than the thickness of the phosphor glass base material. The thinner the phosphor glass thin plate is, the thinner the jig is required, and the strength of the jig is reduced. Therefore, the phosphor glass base material may be damaged by the jig being damaged during polishing of the phosphor glass base material. In particular, when manufacturing a phosphor glass thin plate having a thickness of less than 0.3 mm, the phosphor glass base material is more likely to be damaged.
[0051] In this embodiment, the second main surface 21b of the phosphor glass base material 21 is directly fixed onto the stage 22. Therefore, the phosphor glass base material 21 can be polished without using a jig as described above. Therefore, the phosphor glass base material 21 is less likely to be damaged, and the phosphor glass thin plate 1 can be manufactured more reliably.
[0052] In the process of polishing the phosphor glass base material 21, it is preferable to spray a liquid such as water onto the phosphor glass base material 21. For example, the liquid may be sprayed onto the phosphor glass base material 21 from the opening 23a of the polishing member 23, or the liquid may be sprayed onto the phosphor glass base material 21 from the outside of the polishing member 23 and the stage 22. This allows the phosphor glass base material 21 to be effectively cooled when polishing the phosphor glass base material 21. This prevents the temperature of the phosphor glass base material 21 from unduly increasing during polishing and softening and deformation, and as a result, the softened and deformed glass from being burned onto the abrasive layer 24, or the polishing rate from changing due to an increase in temperature. In addition, by spraying a liquid such as water onto the phosphor glass base material 21, polishing sludge can be efficiently discharged to the outside, so that it is possible to prevent unduly scratching the surface of the phosphor glass base material 21 due to excess polishing sludge.
[0053] At least one groove extending from the opening 23a to the outer peripheral edge may be provided on the surface of the abrasive layer 24 on the side where the phosphor glass base material 21 is polished. In this case, when the phosphor glass base material 21 is polished while a liquid is sprayed from the opening 23a, polishing sludge can be suitably discharged from the groove. Thus, the phosphor glass base material 21 can be polished more efficiently.
[0054] Next, as shown in FIG. 8(a), the suction from the first hole 22a is released, and the phosphor glass base material 21 is peeled off from the stage 22. At this time, as shown by the arrow D, a liquid such as water is sprayed from the second hole 22b of the stage 22 onto the second main surface 21b of the phosphor glass base material 21, and the phosphor glass base material 21 is peeled off from the stage 22. This makes it possible to peel off the phosphor glass base material 21 from the stage 22 more reliably. In this embodiment, suction is performed from the first hole 22a, and liquid is sprayed from the second hole 22b, but the stage 22 may have holes that perform both suction and liquid spray. For example, the stage 22 may be made of a porous body, and suction and liquid spray may be performed through each fine hole formed in the porous body. Note that liquid spraying during the above peeling is not necessarily performed. Also, instead of liquid, gas may be sprayed from the second hole 22b to peel off the phosphor glass base material 21 from the stage 22.
[0055] Next, as shown in Fig. 8(b), the phosphor glass base material 21 is turned over and the polished first main surface 21a is fixed on the stage 22. Next, the second main surface 21b of the phosphor glass base material 21 is polished by a polishing member 23. At this time, fixing and polishing are performed in the same manner as in the steps shown in Figs. 5(a), 5(b) and 7. In this way, the phosphor glass thin plate 1 shown in Fig. 1 can be obtained.
[0056] Here, in the step of polishing the first main surface 21a and the step of polishing the second main surface 21b, it is preferable to polish the surfaces so that their arithmetic mean roughness (Ra) is less than 0.1 μm, particularly 0.05 μm or less. This makes it difficult for light to be scattered when the excitation light enters and when the composite light of the excitation light and the fluorescence is emitted, thereby improving the luminous efficiency.
[0057] In the step of polishing the first main surface 21a and the step of polishing the second main surface 21b, it is preferable to polish the plate so that the thickness is 0.03 mm to 0.3 mm (excluding 0.3 mm), 0.05 mm to 0.15 mm, and particularly 0.08 mm to 0.12 mm. This effectively increases the luminous flux value, provides a phosphor glass sheet without breakage, and makes it easier to mount individual pieces of the phosphor glass sheet on LEDs, etc.
[0058] 8(a), the phosphor glass thin plate 1 is peeled off from the stage 22. It is not necessary to polish the second main surface 21b of the phosphor glass base material 21, and the phosphor glass thin plate 1 may be obtained by polishing only the first main surface 21a. In this case, it is preferable to polish the first main surface 21a to within the above thickness range in the step of polishing the first main surface 21a.
[0059] An example of a method for manufacturing the phosphor glass thin plate piece 11 shown in FIG. 3 will be described below.
[0060] 9(a) and 9(b) are schematic cross-sectional views for explaining a method for producing individual pieces of a phosphor glass thin plate according to one embodiment of the present invention.
[0061] A phosphor glass sheet 1 is prepared by the above-mentioned manufacturing method or the like. Next, as shown in Fig. 9(a), the second main surface 1b of the phosphor glass sheet 1 is attached onto a support sheet 25. In this embodiment, the support sheet 25 is a UV-curable resin such as an acrylic resin or an epoxy resin applied onto a sheet made of a polyethylene resin, a polyolefin resin, a PVC resin, or the like, and the UV-curable resin side is attached to the second main surface 1b of the phosphor glass sheet 1. Note that the material of the support sheet 25 is not limited to the above.
[0062] Next, division grooves 1c are formed on the first main surface 1a of the phosphor glass thin plate 1. In this embodiment, the division grooves 1c are formed in a lattice pattern. The division grooves 1c are not particularly limited, but can be formed, for example, by scribing the first main surface 1a of the phosphor glass thin plate 1. The division grooves 1c may be formed before the phosphor glass thin plate 1 is attached to the support sheet 25. The surface of the phosphor glass thin plate 1 that is attached to the support sheet 25 may be the first main surface 1a. The division grooves 1c may be formed on the second main surface 1b.
[0063] 9(b), a film 26 is attached to the first main surface 1a on which the dividing grooves 1c are formed. In this embodiment, the film 26 is made of polyethylene resin, polyolefin resin, PVC resin, or the like. Note that the material of the film 26 is not limited to the above.
[0064] On the other hand, a plurality of receiving blades 27 are prepared for placing the thin phosphor glass plate 1 on. Next, the thin phosphor glass plate 1 is turned over and placed on the plurality of receiving blades 27 so that the film 26 is in contact with the plurality of receiving blades 27. In this embodiment, the thin phosphor glass plate 1 is supported by the receiving blades 27 via the film 26. Therefore, scratches are unlikely to occur on the thin phosphor glass plate 1. Note that the film 26 does not necessarily have to be used in the method for manufacturing individual pieces of the thin phosphor glass plate.
[0065] Next, a pressing member 28 is placed at a position facing the dividing groove 1c. The pressing member 28 has a blade 29. The blade 29 presses the area where the dividing groove 1c is formed from the support sheet 25 side. As a result, the phosphor glass thin plate 1 is cut in the thickness direction along the dividing groove 1c while still attached to the support sheet 25, and is divided into a plurality of parts. The same cutting is performed in the other areas where the dividing grooves 1c are formed. Next, the film 26 is peeled off from the assembly of phosphor glass thin plate pieces 11 into which the phosphor glass thin plate 1 is divided. Next, UV is irradiated from the support sheet 25 side to harden the UV-curable resin in the support sheet 25. Next, the phosphor glass thin plate pieces 11 are peeled off from the support sheet 25. By dividing the phosphor glass thin plate 1 as described above, a plurality of phosphor glass thin plate pieces 11 can be obtained.
[0066] In this embodiment, the thickness of the phosphor glass thin plate 1 before division is thinned by polishing. Therefore, since it can be divided with smaller stress, the phosphor glass thin plate 1 is less likely to break during the division, and the phosphor glass thin plate pieces 11 can be manufactured more reliably. In addition, since the phosphor glass thin plate 1 is thin and can be easily divided even when the pitch of the division grooves 1c is narrow, small phosphor glass thin plate pieces 11 can be manufactured more easily and more reliably. Therefore, it is possible to easily manufacture even smaller light-emitting devices.
[0067] The phosphor glass thin plate 1 may be divided by dicing. However, it is preferable to divide the phosphor glass thin plate 1 by the above-mentioned breaking. This makes it even more difficult for the thin phosphor glass plate 1 to crack during division because of its thinness. [Explanation of symbols]
[0068] 1...Thin phosphor glass plate 1a...First main surface 1b…Second main surface 1c…Dividing groove 2. Phosphor 3…Glass matrix 11...Individual pieces of phosphor glass thin plate 11a...first main surface 11b...Second main surface 11c...Outer edge 21...Phosphor glass base material 21a...first main surface 21b...Second main surface 22...Stage 22a…First hole 22b…Second hole 23...Abrasive material 23a...Opening 24...abrasive layer 25…Support sheet 26...Film 27…Cutting edge 28...Pressing member 29…Blade 30...Light emitting device 34…Light source 35...Reflective material 100...Light emitting device 101...Individual piece of phosphor glass plate
Claims
1. providing a phosphor glass base material having a first main surface and a second main surface opposed to each other; placing the phosphor glass base material on a stage and fixing the second main surface on the stage; a step of polishing the first main surface of the phosphor glass base material having a thickness of 0.3 mm or more with a polishing member having an abrasive layer to obtain a phosphor glass thin plate having a thickness of less than 0.3 mm; forming a dividing groove on a main surface of the phosphor glass thin plate; and breaking the phosphor glass thin plate along the division grooves. The phosphor glass base material is fixed on the stage by suction.
2. fixing the first main surface of the phosphor glass base material on the stage; 2. The method for manufacturing an individual phosphor glass thin plate according to claim 1, further comprising the step of polishing the second main surface of the phosphor glass base material with the polishing member.
3. 3. The method for producing individual phosphor glass thin plate pieces according to claim 1, wherein in the step of polishing the phosphor glass base material, the polishing member is rotated around a rotation axis extending in a thickness direction of the phosphor glass base material.
4. 4. The method for manufacturing individual pieces of phosphor glass thin plate according to claim 1, wherein in the step of polishing the phosphor glass base material, the stage is rotated around a rotation axis extending in a thickness direction of the phosphor glass base material.
5. 5. The method for producing individual phosphor glass thin plate pieces according to claim 3, wherein in the step of polishing the phosphor glass base material, the polishing member and the stage are rotated in opposite directions to each other around a rotation axis extending in a thickness direction of the phosphor glass base material.
6. The method for producing individual phosphor glass thin plate pieces according to any one of claims 1 to 5, wherein in the step of polishing the phosphor glass base material, the phosphor glass base material is polished to a thickness of 0.15 mm or less.
7. 7. The method for producing an individual piece of a phosphor glass thin plate according to claim 1, wherein in the step of polishing the phosphor glass base material, the first main surface and the second main surface are polished so that the arithmetic mean roughness (Ra) of the surface to be polished is less than 0.1 μm.
8. 8. The method for manufacturing individual pieces of phosphor glass thin plate according to claim 1, wherein after the step of polishing the phosphor glass base material, the phosphor glass base material is peeled off from the stage by spraying a liquid onto the phosphor glass base material from the stage side.
9. 9. The method for manufacturing individual pieces of a phosphor glass thin plate according to claim 1, wherein in the step of breaking the phosphor glass thin plate, a pressing member is used to press the phosphor glass thin plate at a position facing the division groove, thereby breaking the phosphor glass thin plate.
10. The method for producing individual phosphor glass sheet pieces according to claim 9 , further comprising the step of: cleaving the phosphor glass sheet in a state in which a film is attached to a main surface of the phosphor glass sheet on which the division grooves are formed.
11. The method for producing individual phosphor glass thin plate pieces according to claim 10, wherein the film is made of a polyethylene resin, a polyolefin resin or a vinyl chloride resin.
Citation Information
Patent Citations
Device for preventing adhesion of product in lapping / polishing machine
JP1986203269A
Method of manufacturing small-sized glassware
JP2006131468A
Grinding method of substrate
JP2007290078A
Apparatus for manufacturing glass substrate for information recording medium
JP2010082700A
Near infrared ray cutting filter glass, and method for manufacturing the same
JP2010197595A