Method for manufacturing liquid crystal layer
The method of using a photoalignment film with an azobenzene compound to align liquid crystal layers without a peeling layer addresses alignment issues, ensuring high-quality orientation and increasing productivity by allowing repeated use of the alignment film.
Patent Information
- Application Number
- JP2022506856
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-13
- Filing Date
- 2021-03-12
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Existing methods for manufacturing liquid crystal layers face issues with insufficient alignment of liquid crystal compounds due to the presence of a peeling layer between the liquid crystal alignment layer and the liquid crystal layer, particularly when smaller periodic patterns are used, leading to reduced orientation and alignment quality.
A method involving the use of a photoalignment film containing an azobenzene compound, where the liquid crystal alignment layer is peeled off from the alignment film, and a second liquid crystal composition is aligned on the peeled surface to form a liquid crystal layer, allowing for repeated use of the alignment film without a peeling layer, ensuring high alignment quality.
This approach enables sufficient alignment of liquid crystal compounds in the liquid crystal layer, improving orientation and allowing for higher productivity by reusing the alignment film, reducing alignment defects and maintaining alignment quality across multiple productions.
Smart Images

Figure 0007561828000007 
Figure 0007561828000008 
Figure 0007561828000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a liquid crystal layer. [Background technology]
[0002] A liquid crystal layer formed by using a liquid crystal composition containing a liquid crystal compound is used as various liquid crystal layers such as a diffraction element, an optically anisotropic layer, a wavelength selective reflection layer, etc. The liquid crystal layer exhibits various functions such as diffraction, imparting a phase difference, and reflecting a selected wavelength by aligning the contained liquid crystal compound in a predetermined orientation state.
[0003] In order to align the liquid crystal compound in the liquid crystal layer, an alignment film is used. For example, a liquid crystal composition that will become the liquid crystal layer is applied onto an alignment film formed on a support, an alignment treatment is performed, and the liquid crystal compound in the liquid crystal composition is brought into a predetermined alignment state, and the aligned liquid crystal composition is cured to form the liquid crystal layer.
[0004] Incidentally, in order to manufacture the liquid crystal layer with higher productivity, it has been considered to separate the liquid crystal layer from the alignment film after the liquid crystal layer is manufactured and reuse the alignment film.
[0005] For example, Patent Document 1 describes a process for patterning a liquid crystal polymer layer, which includes contacting the liquid crystal polymer layer with a reusable alignment template having a surface alignment pattern so that the liquid crystal molecules of the liquid crystal polymer layer are aligned to the surface alignment pattern of the reusable alignment template primarily through chemical, steric, or other intermolecular interactions, polymerizing the liquid crystal polymer layer, and separating the patterned polymerized liquid crystal polymer layer and the reusable alignment template, wherein the reusable alignment template has an optical alignment layer having a surface alignment pattern.
[0006] This Patent Document 1 describes a configuration in which a liquid crystal polymer layer is provided on a light alignment layer (alignment film), and the orientation of the liquid crystal compound in this liquid crystal polymer layer (liquid crystal alignment layer) is utilized to align the polymerized liquid crystal polymer layer. It describes that the configuration in which the liquid crystal polymer layer is provided on the alignment film improves light and heat stability. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2020-502565 Summary of the Invention [Problem to be solved by the invention]
[0008] In Patent Document 1, in the case of a configuration in which a liquid crystal alignment layer is formed on an alignment film and the liquid crystal layer is aligned by the liquid crystal alignment layer, a peeling layer is provided between the liquid crystal alignment layer and the liquid crystal layer to allow peeling between the liquid crystal alignment layer and the liquid crystal layer. However, when a peeling layer is present between the liquid crystal alignment layer and the liquid crystal layer, there is a problem that the alignment of the liquid crystal layer formed is insufficient due to the interposition of the peeling layer. In addition, since the alignment of the liquid crystal compound is low on the surface of the liquid crystal alignment layer opposite the alignment film, there is a problem that the alignment of the liquid crystal layer is insufficient when the liquid crystal layer is formed on the surface of the liquid crystal alignment layer opposite the alignment film. In particular, there is a problem that the liquid crystal compound in the liquid crystal layer cannot be sufficiently aligned when the liquid crystal compound in the liquid crystal layer is aligned in a smaller periodic pattern.
[0009] The object of the present invention is to solve such problems of the conventional technology, and to provide a method for manufacturing a liquid crystal layer that can satisfactorily align the liquid crystal compound in the liquid crystal layer in a method for manufacturing a liquid crystal layer that repeatedly uses an alignment film. [Means for solving the problem]
[0010] In order to solve this problem, the present invention has the following configuration. [1] An alignment film forming step of forming an alignment film on a support; a liquid crystal alignment layer alignment step of laminating a first liquid crystal composition containing a polymerizable liquid crystal compound on the alignment film and aligning the first liquid crystal composition; a liquid crystal alignment layer forming step of polymerizing the aligned first liquid crystal composition to form a liquid crystal alignment layer; a peeling step of laminating and fixing the surface of the liquid crystal alignment layer opposite to the alignment film to an adherend, and peeling off the liquid crystal alignment layer at the interface between the alignment film and the liquid crystal alignment layer; a liquid crystal layer alignment step of laminating a second liquid crystal composition containing a polymerizable liquid crystal compound on the surface of the liquid crystal alignment layer from which the alignment film has been peeled off, and aligning the second liquid crystal composition; a liquid crystal layer forming step of polymerizing the aligned second liquid crystal composition to form a liquid crystal layer; and a liquid crystal layer separation step of separating the formed liquid crystal layer from the liquid crystal alignment layer; The method for producing a liquid crystal layer includes repeating a liquid crystal layer alignment step to a liquid crystal layer separation step to repeatedly produce a liquid crystal layer. [2] A method for manufacturing a liquid crystal layer according to [1], in which, in a liquid crystal layer alignment step, the liquid crystal alignment layer creates an alignment state in which the direction of the optical axis derived from the liquid crystal compound in the liquid crystal layer changes while continuously rotating along at least one direction in the plane. [3] The method for producing a liquid crystal layer according to [1] or [2], wherein the alignment film formed in the alignment film formation step is formed from a photoalignment composition containing an azobenzene-based compound. [4] The method for producing a liquid crystal layer according to any one of [1] to [3], wherein in the alignment film forming step, the alignment film is exposed to laser interference exposure. [5] The method for producing a liquid crystal layer according to any one of [1] to [4], wherein the first liquid crystal composition contains a polyfunctional polymerizable compound. [6] The method for producing a liquid crystal layer according to [5], wherein the polymerizable liquid crystal compound contained in the first liquid crystal composition is a polyfunctional polymerizable liquid crystal compound. Effect of the Invention
[0011] According to the present invention, it is possible to provide a method for manufacturing a liquid crystal layer which uses an alignment film repeatedly and which is capable of sufficiently aligning liquid crystal compounds in the liquid crystal layer. [Brief description of the drawings]
[0012] [Figure 1] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Diagram 2] FIG. 1 is a conceptual diagram of an example of an exposure apparatus for exposing an alignment film. [Diagram 3] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Figure 4] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Diagram 5] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Figure 6] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Figure 7] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Figure 8] 1 is a conceptual diagram for explaining an example of a method for producing a liquid crystal layer according to the present invention. [Figure 9] FIG. 2 is a diagram conceptually illustrating an example of a liquid crystal layer. [Figure 10] 10 is a plan view conceptually showing the liquid crystal layer shown in FIG. [Figure 11] 10 is a diagram conceptually showing a cross-sectional SEM (scanning electron microscope) image of the liquid crystal layer shown in FIG. [Figure 12] 10 is a conceptual diagram for explaining the function of the liquid crystal layer shown in FIG. [Figure 13] FIG. 13 is a diagram conceptually illustrating another example of a liquid crystal layer. [Figure 14] FIG. 13 is a diagram conceptually illustrating another example of a liquid crystal layer. [Figure 15] FIG. 13 is a diagram conceptually illustrating another example of a liquid crystal layer. [Figure 16] FIG. 16 is a diagram conceptually showing a plan view of the liquid crystal layer shown in FIG. [Figure 17] 16 is a diagram for explaining the function of the liquid crystal layer shown in FIG. 15. [Figure 18] 16 is a diagram for explaining the function of the liquid crystal layer shown in FIG. 15. [Figure 19] FIG. 13 is a diagram conceptually illustrating another example of a liquid crystal layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the method for producing a liquid crystal layer of the present invention will be described in detail with reference to preferred embodiments shown in the accompanying drawings.
[0014] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, "(meth)acrylate" is used to mean "either one or both of acrylate and methacrylate." In this specification, the terms "same" and "identical" include a generally acceptable margin of error in the technical field.
[0015] [Method of manufacturing liquid crystal layer] The method for producing a liquid crystal layer of the present invention comprises the steps of: An alignment film forming step of forming an alignment film on a support; a liquid crystal alignment layer alignment step of laminating a first liquid crystal composition containing a polymerizable liquid crystal compound on the alignment film and aligning the first liquid crystal composition; a liquid crystal alignment film forming step of polymerizing the aligned first liquid crystal composition to form a liquid crystal alignment layer; a peeling step of laminating and fixing the surface of the liquid crystal alignment layer opposite to the alignment film to an adherend, and peeling off the liquid crystal alignment layer at the interface between the alignment film and the liquid crystal alignment layer; a liquid crystal layer alignment step of laminating a second liquid crystal composition containing a polymerizable liquid crystal compound on the surface of the liquid crystal alignment layer from which the alignment film has been peeled off, and aligning the second liquid crystal composition; a liquid crystal layer forming step of polymerizing the aligned second liquid crystal composition to form a liquid crystal layer; and a liquid crystal layer separation step of separating the formed liquid crystal layer from the liquid crystal alignment layer; The method for producing a liquid crystal layer includes the steps of: orienting a liquid crystal layer; separating a liquid crystal layer; and repeating the steps to produce a liquid crystal layer.
[0016] An example of a method for producing a liquid crystal layer according to the present invention will be described with reference to FIGS.
[0017] [Alignment film forming process] As shown in FIG. 1, the alignment film forming step is a step of forming an alignment film 32 on a support 30. As a method for forming the alignment film, a conventionally known method for forming an alignment film used in forming a liquid crystal layer can be used depending on the material for forming the alignment film.
[0018] The alignment film 32 may be of any of various known types. Examples include rubbed films made of organic compounds such as polymers, obliquely evaporated films of inorganic compounds, films with microgrooves, and films formed by stacking LB (Langmuir-Blodgett) films made of organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate using the Langmuir-Blodgett method.
[0019] The alignment film 32 formed by rubbing treatment can be formed by rubbing the surface of the polymer layer several times in a certain direction with paper or cloth. Preferred materials for use in forming the alignment film 32 by rubbing treatment include polyimide, polyvinyl alcohol, polymers having polymerizable groups as described in JP-A-9-152509, and materials used in forming the alignment films 32 described in JP-A-2005-97377, JP-A-2005-99228, and JP-A-2005-128503.
[0020] In the present invention, a so-called photo-alignment film obtained by irradiating a photo-alignable material with polarized or non-polarized light to form the alignment film 32 is preferably used as the alignment film 32. That is, in the present invention, a photo-alignment film formed by applying a photo-alignment material onto the support 30 is preferably used as the alignment film 32. The photo-alignment film can be irradiated with polarized light from a vertical direction or an oblique direction, while the photo-alignment film can be irradiated with unpolarized light from an oblique direction.
[0021] Examples of photo-alignment materials used in the alignment film that can be used in the present invention include those described in JP-A-2006-285197, JP-A-2007-76839, JP-A-2007-138138, JP-A-2007-94071, JP-A-2007-121721, JP-A-2007-140465, JP-A-2007-156439, and JP-A-2007 azo compounds described in JP-A-133184, JP-A-2009-109831, JP-A-3883848 and JP-A-4151746; aromatic ester compounds described in JP-A-2002-229039; maleimides having photo-orientable units described in JP-A-2002-265541 and JP-A-2002-317013; / or alkenyl-substituted nadimide compounds, photocrosslinkable silane derivatives described in Japanese Patent No. 4205195 and Japanese Patent No. 4205198, photocrosslinkable polyimides, photocrosslinkable polyamides and photocrosslinkable polyesters described in JP-T-2003-520878, JP-T-2004-529220 and Japanese Patent No. 4162850, and photodimerizable compounds described in JP-A-9-118717, JP-T-10-506420, JP-T-2003-505561, WO 2010 / 150748, JP-A-2013-177561 and JP-A-2014-12823, particularly cinnamate compounds, chalcone compounds and coumarin compounds, etc. are exemplified as preferred examples. Among these, azo compounds, photocrosslinkable polyimides, photocrosslinkable polyamides, photocrosslinkable polyesters, cinnamate compounds, and chalcone compounds are preferably used.
[0022] In the present invention, it is further preferable that the alignment film formed in the alignment film forming step is formed from a photoalignment composition containing an azobenzene-based compound. The azobenzene compound is a compound having an azobenzene group which is a photoreactive group. The azobenzene compound is not particularly limited, but is preferably a compound represented by the general formula (I).
[0023] General formula (I)
[0024] [ka]
[0025] R 21 ~R 24 each independently represents a hydrogen atom or a substituent, provided that R 21 ~R 24 At least one of the groups represented by the formula (I) represents a carboxyl group or a salt thereof, or a sulfo group or a salt thereof, m represents an integer of 1 to 4, n represents an integer of 1 to 4, o represents an integer of 1 to 5, and p represents an integer of 1 to 5. When m, n, o, and p each represent an integer of 2 or more, R 21 ~R 24 may be the same or different.
[0026] In general formula (I), R 21 ~R 24 Examples of the substituents represented by each of the formulas below include a carboxyl group or a salt thereof (note that examples of salts of a carboxyl group include salts with alkali metals, and sodium salts are preferred), a sulfo group or a salt thereof (note that examples of salts of a sulfo group include salts with alkali metals, and sodium salts are preferred), an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a substituted or unsubstituted amino group, an alkoxy group, an alkoxycarbonyl group, an acyloxy group, an acylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfonylamino group, a sulfamoyl group, a carbamoyl group, an alkylthio group, an arylthio group, a sulfonyl group, a sulfinyl group, a ureido group, a phosphoric acid amide group, a hydroxy group, a mercapto group, a halogen atom, a cyano group, a nitro group, a hydroxamic acid group, a sulfino group, a hydrazino group, an imino group, a heterocyclic group, and a silyl group. These substituents may be further substituted with other substituents. When two or more substituents are present, they may be the same or different. If possible, they may be bonded to each other to form a ring.
[0027] In general formula (I), R 21 ~R24 The group represented by the formula (I) is preferably a hydrogen atom, a carboxyl group or a salt thereof, a sulfo group or a salt thereof, a halogen atom, an alkyl group, an alkoxy group, a cyano group, a nitro group, an alkoxycarbonyl group, or a carbamoyl group, more preferably a hydrogen atom, a carboxyl group or a salt thereof, a sulfo group or a salt thereof, a halogen atom, a halogenated methyl group, a halogenated methoxy group, a cyano group, a nitro group, or a methoxycarbonyl group, and even more preferably a hydrogen atom, a carboxyl group or a salt thereof, a sulfo group or a salt thereof, a halogen atom, a cyano group, or a nitro group.
[0028] R 21 ~R 24 At least one of the groups represented by the formula (I) is a carboxyl group or a salt thereof, or a sulfo group or a salt thereof. There are no particular limitations on the substitution position of the carboxyl group or a salt thereof, or the sulfo group or a salt thereof, but in terms of photoactivity, at least one of the groups represented by the formula (I) is preferably a carboxyl group or a salt thereof, or a sulfo group or a salt thereof. 21 and / or at least one R 22 is preferably a sulfo group or a salt thereof, and at least one R 21 and at least one R 22 It is more preferable that at least one R 23 and / or at least one R 24 is preferably a carboxyl group or a salt thereof, and at least one R 23 and at least one R 24 More preferably, R is a carboxyl group or a salt thereof. The carboxyl group or a salt thereof is R substituted at the meta position relative to the azo group. 23 and R 24 It is even more preferable that:
[0029] In general formula (I), m represents an integer of 1 to 4, n represents an integer of 1 to 4, o represents an integer of 1 to 5, and p represents an integer of 1 to 5. Preferably, m is an integer of 1 to 2, n is an integer of 1 to 2, o is an integer of 1 to 2, and p is an integer of 1 to 2.
[0030] Specific examples of the compound represented by formula (I) are given below, but the compound is not limited to these specific examples.
[0031] [ka]
[0032] There is no limitation on the thickness of the alignment film 32, and the thickness may be appropriately set so as to obtain the necessary alignment function depending on the material from which the alignment film 32 is formed. The thickness of the alignment film 32 is preferably 0.01 to 5 μm, and more preferably 0.05 to 2 μm.
[0033] There is no limitation on the method for forming the photo-alignment film, and various known methods can be used according to the material for forming the photo-alignment film. As an example, there is a method in which the photo-alignment film 32 is applied to the surface of the support 30 and dried, and then the photo-alignment film 32 is exposed to laser light to form an alignment pattern.
[0034] FIG. 2 conceptually shows an example of an exposure apparatus for exposing the alignment film 32 to light to form an alignment pattern. The exposure device 60 shown in FIG. 2 includes a light source 64 having a laser 62, a λ / 2 plate 65 that changes the polarization direction of laser light M emitted by the laser 62, a polarizing beam splitter 68 that splits the laser light M emitted by the laser 62 into two light beams MA and MB, mirrors 70A and 70B that are respectively arranged on the optical paths of the two split light beams MA and MB, and λ / 4 plates 72A and 72B. The light source 64 emits linearly polarized light P0. The λ / 4 plate 72A converts the linearly polarized light P0 (light beam MA) into right-handed circularly polarized light P R The λ / 4 plate 72B converts the linearly polarized light P0 (light beam MB) into left-handed circularly polarized light P L , respectively.
[0035] A support 30 having an alignment film 32 before an alignment pattern is formed is placed in an exposure section, and two light beams MA and MB are caused to intersect and interfere on the alignment film 32, and the alignment film 32 is exposed by being irradiated with the interference light. Due to the interference at this time, the polarization state of the light irradiated to the alignment film 32 changes periodically in the form of interference fringes, thereby obtaining an alignment film having an alignment pattern in which the alignment state changes periodically (hereinafter also referred to as a pattern alignment film).
[0036] In the exposure device 60, the period of the alignment pattern can be adjusted by changing the crossing angle α of the two light beams MA and MB. That is, in the exposure device 60, in an alignment pattern in which the optical axis 40A originating from the liquid crystal compound 40 in the liquid crystal layer 34 rotates continuously along one direction, the length of one period in which the optical axis 40A rotates by 180° in one direction in which the optical axis 40A rotates can be adjusted by adjusting the crossing angle α.
[0037] By forming a liquid crystal layer on the alignment film 32 having an alignment pattern in which the alignment state changes periodically, it is possible to form a liquid crystal layer 34 having a liquid crystal alignment pattern in which the optical axis 40A derived from the liquid crystal compound 40 rotates continuously along one direction, as described below. Moreover, by rotating the optical axes of the λ / 4 plates 72A and 72B by 90°, respectively, the rotation direction of the optical axis 40A can be reversed.
[0038] As described above, the patterned alignment film has an alignment pattern that aligns the liquid crystal compound so that the direction of the optical axis of the liquid crystal compound in the liquid crystal layer formed on the patterned alignment film changes while continuously rotating along at least one direction in the plane. If the axis along which the patterned alignment film aligns the liquid crystal compound is defined as the alignment axis, the patterned alignment film can be said to have an alignment pattern in which the direction of the alignment axis changes while continuously rotating along at least one direction in the plane. The alignment axis of the patterned alignment film can be detected by measuring the absorption anisotropy. For example, when the patterned alignment film is irradiated with linearly polarized light while rotating and the amount of light transmitted through the patterned alignment film is measured, the direction in which the amount of light is maximum or minimum is observed to change gradually along one direction in the plane.
[0039] In the present invention, the alignment film 32 is provided as a preferred embodiment, but is not an essential component. For example, by forming an alignment pattern on the support 30 by a method of subjecting the support 30 to a rubbing treatment, a method of processing the support 30 with laser light, or the like, it is possible to configure the liquid crystal layer to have a liquid crystal alignment pattern in which the direction of the optical axis 40A derived from the liquid crystal compound 40 changes while continuously rotating along at least one direction in the plane. That is, in the present invention, the support 30 may act as an alignment film.
[0040] <Support> The support 30 supports an alignment film 32 and a liquid crystal layer 34 . The support 30 may be any type of sheet-like material (film, plate-like material) that can support the alignment film 32 and the liquid crystal layer . The support 30 preferably has a transmittance to the corresponding light of 50% or more, more preferably 70% or more, and even more preferably 85% or more.
[0041] There is no limitation on the thickness of the support 30, and the thickness may be appropriately set depending on the material from which the support 30 is formed, so long as the thickness is sufficient to support the alignment film 32 and the liquid crystal layer . The thickness of the support 30 is preferably from 1 to 2000 μm, more preferably from 3 to 500 μm, and further preferably from 5 to 250 μm.
[0042] The support 30 may be a single layer or multiple layers. Examples of the support 30 in the case of a single layer include support 30 made of glass, triacetyl cellulose (TAC), polyethylene terephthalate (PET), polycarbonate, polyvinyl chloride, acrylic, polyolefin, etc. Examples of the support 30 in the case of a multilayer include a support that includes any of the above-mentioned single-layer supports as a substrate, and another layer is provided on the surface of this substrate.
[0043] [Liquid crystal alignment layer alignment process] The liquid crystal alignment layer alignment step is a step of laminating a first liquid crystal composition containing a polymerizable liquid crystal compound on an alignment film and aligning the first liquid crystal composition. In the liquid crystal alignment layer alignment step, the first liquid crystal composition is applied onto the alignment film 32, and the liquid crystal compound is aligned in a desired liquid crystal phase state.
[0044] The first liquid crystal composition can be applied by any known method capable of uniformly applying a liquid to a sheet-like material, such as a printing method, such as inkjet printing or scroll printing, or a method, such as spin coating, bar coating or spray coating.
[0045] The applied first liquid crystal composition is dried and / or heated as necessary, so that the liquid crystal compounds in the first liquid crystal composition are aligned in a predetermined alignment state according to the alignment pattern of the alignment film 32. When heating is performed, the heating temperature is preferably 200° C. or less, and more preferably 130° C. or less.
[0046] [Liquid crystal alignment layer forming process] The liquid crystal alignment layer forming step is a step of polymerizing the aligned first liquid crystal composition to form a liquid crystal alignment layer.
[0047] The polymerization may be either thermal polymerization or photopolymerization by light irradiation, but photopolymerization is preferred. The light irradiation is preferably performed using ultraviolet light. The irradiation energy is 20 mJ / cm. 2 ~50J / cm 2 is preferred, and 50 mJ / cm 2 ~1500mJ / cm 2 In order to promote the photopolymerization reaction, the light irradiation may be performed under heating conditions or in a nitrogen atmosphere. The wavelength of the ultraviolet light to be irradiated is preferably 250 to 430 nm. Through the liquid crystal alignment layer alignment step and the liquid crystal alignment layer formation step, a liquid crystal alignment layer 33 is formed as shown in FIG.
[0048] Here, in the present invention, the liquid crystal alignment layer 33 may be in any alignment state in the thickness direction as long as the liquid crystal compound is aligned according to the alignment pattern of the alignment film 32 at least in the region on the surface side of the alignment film 32. For example, the liquid crystal alignment layer 33 may be in a homogeneous alignment state or a cholesteric alignment state. Alternatively, the liquid crystal alignment layer 33 may be in a non-aligned state in the thickness direction.
[0049] <First Liquid Crystal Composition> The first liquid crystal composition contains a polymerizable liquid crystal compound, and may further contain a surfactant, a chiral agent, a polymerization initiator, a crosslinking agent, other additives, and a solvent. The first liquid crystal composition preferably contains a multifunctional polymerizable compound. The polymerizable liquid crystal compound is preferably a multifunctional polymerizable liquid crystal compound.
[0050] --Polymerizable liquid crystal compound-- The polymerizable liquid crystal compound may be a rod-shaped liquid crystal compound or a discotic liquid crystal compound. Examples of rod-shaped polymerizable liquid crystal compounds include rod-shaped nematic liquid crystal compounds.As rod-shaped nematic liquid crystal compounds, azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexane carboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles are preferably used.Not only low molecular weight liquid crystal compounds but also high molecular weight liquid crystal compounds can be used.
[0051] The polymerizable liquid crystal compound is obtained by introducing a polymerizable group into a liquid crystal compound. Examples of the polymerizable group include an unsaturated polymerizable group, an epoxy group, and an aziridinyl group, and an unsaturated polymerizable group is preferable, and an ethylenically unsaturated polymerizable group is more preferable. The polymerizable group can be introduced into the molecule of the liquid crystal compound by various methods. The number of polymerizable groups that the polymerizable liquid crystal compound has is preferably 1 to 6, more preferably 1 to 3. Examples of the polymerizable liquid crystal compound include compounds described in Makromol.Chem., Vol. 190, p. 2255 (1989), Advanced Materials, Vol. 5, p. 107 (1993), U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, International Publication No. 95 / 22586, International Publication No. 95 / 24455, International Publication No. 97 / 00600, International Publication No. 98 / 23580, International Publication No. 98 / 52905, JP-A-1-272551, JP-A-6-16616, JP-A-7-110469, JP-A-11-80081, and JP-A-2001-328973. Two or more polymerizable liquid crystal compounds may be used in combination. The alignment temperature can be lowered by using two or more kinds of polymerizable liquid crystal compounds in combination.
[0052] As other polymerizable liquid crystal compounds, a cyclic organopolysiloxane compound having a cholesteric phase as disclosed in JP-A-57-165480 can be used. As the above-mentioned polymer liquid crystal compounds, a polymer having a mesogen group exhibiting liquid crystal property introduced into the main chain, the side chain, or both the main chain and the side chain, a polymer cholesteric liquid crystal having a cholesteryl group introduced into the side chain, a liquid crystal polymer as disclosed in JP-A-9-133810, and a liquid crystal polymer as disclosed in JP-A-11-293252 can be used.
[0053] Furthermore, the liquid crystal compound is preferably a polyfunctional polymerizable liquid crystal compound. The polyfunctional polymerizable liquid crystal compound is a liquid crystal compound having a plurality of polymerizable groups. The types of the polymerizable groups are as described above. The number of polymerizable groups in the polyfunctional polymerizable liquid crystal compound is 2 or more, and preferably 2 to 6. The polyfunctional polymerizable liquid crystal compound may be a discotic liquid crystal compound or a rod-shaped liquid crystal compound, so long as it has a plurality of polymerizable groups.
[0054] Furthermore, the amount of the polymerizable liquid crystal compound added in the first liquid crystal composition is preferably 75 to 99.9 mass %, more preferably 80 to 99 mass %, and even more preferably 85 to 90 mass %, relative to the solid content mass of the liquid crystal composition (mass excluding the solvent).
[0055] --Surfactant-- The first liquid crystal composition may contain a surfactant. The surfactant is preferably a compound that can function as an alignment control agent that contributes to the alignment of the liquid crystal phase stably or quickly. Examples of the surfactant include silicone surfactants and fluorine surfactants, and fluorine surfactants are preferred.
[0056] Specific examples of surfactants include the compounds described in paragraphs
[0082] to
[0090] of JP-A-2014-119605, the compounds described in paragraphs
[0031] to
[0034] of JP-A-2012-203237, the compounds exemplified in paragraphs
[0092] and
[0093] of JP-A-2005-99248, the compounds exemplified in paragraphs
[0076] to
[0078] and paragraphs
[0082] to
[0085] of JP-A-2002-129162, and the fluorine (meth)acrylate polymers described in paragraphs
[0018] to
[0043] of JP-A-2007-272185, etc. The surfactant may be used alone or in combination of two or more kinds. As the fluorine-based surfactant, the compounds described in paragraphs
[0082] to
[0090] of JP2014-119605A are preferred.
[0057] The amount of the surfactant added in the first liquid crystal composition is preferably 0.01 to 10 mass %, more preferably 0.01 to 5 mass %, and further preferably 0.02 to 1 mass %, based on the total mass of the liquid crystal compound.
[0058] --Chiral agents (optically active compounds)-- Chiral agents have the function of inducing a helical structure in the cholesteric liquid crystal phase. Chiral agents can be selected according to the purpose, since the twist direction or helical pitch of the helix induced varies depending on the compound. The chiral agent is not particularly limited, and known compounds (for example, those described in Liquid Crystal Device Handbook, Chapter 3, Section 4-3, Chiral Agents for TN (twisted nematic) and STN (Super Twisted Nematic), p. 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989), isosorbide, and isomannide derivatives can be used. Although the chiral agent generally contains an asymmetric carbon atom, an axially asymmetric compound or a planarly asymmetric compound that does not contain an asymmetric carbon atom can also be used as the chiral agent. Examples of the axially asymmetric compound or the planarly asymmetric compound include binaphthyl, helicene, paracyclophane, and derivatives thereof. The chiral agent may have a polymerizable group. When both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by a polymerization reaction between the polymerizable chiral agent and the polymerizable liquid crystal compound. In this embodiment, the polymerizable group of the polymerizable chiral agent is preferably the same type of group as the polymerizable group of the polymerizable liquid crystal compound. Therefore, the polymerizable group of the chiral agent is also preferably an unsaturated polymerizable group, an epoxy group, or an aziridinyl group, more preferably an unsaturated polymerizable group, and even more preferably an ethylenically unsaturated polymerizable group. The chiral agent may also be a liquid crystal compound.
[0059] The chiral agent may have a photoisomerizable group, which is preferably an isomerizable moiety of a compound exhibiting photochromic properties, an azo group, an azoxy group, or a cinnamoyl group. Specific compounds that can be used include those described in JP-A-2002-80478, JP-A-2002-80851, JP-A-2002-179668, JP-A-2002-179669, JP-A-2002-179670, JP-A-2002-179681, JP-A-2002-179682, JP-A-2002-338575, JP-A-2002-338668, JP-A-2003-313189, and JP-A-2003-313292.
[0060] The content of the chiral dopant in the first liquid crystal composition is preferably 0.01 to 200 mol %, more preferably 1 to 30 mol %, based on the molar amount of the liquid crystal compound contained.
[0061] --Polymerization initiator-- When the first liquid crystal composition contains a polymerizable compound, it preferably contains a polymerization initiator. In an embodiment in which the polymerization reaction is caused to proceed by ultraviolet irradiation, the polymerization initiator used is preferably a photopolymerization initiator capable of initiating the polymerization reaction by ultraviolet irradiation. Examples of the photopolymerization initiator include α-carbonyl compounds (described in U.S. Pat. Nos. 2,367,661 and 2,367,670), acyloin ethers (described in U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (described in U.S. Pat. No. 2,722,512), polynuclear quinone compounds (described in U.S. Pat. Nos. 3,046,127 and 2,951,758), combinations of triarylimidazole dimers and p-aminophenyl ketones (described in U.S. Pat. No. 3,549,367), acridine and phenazine compounds (described in JP-A-60-105,667 and U.S. Pat. No. 4,239,850), and oxadiazole compounds (described in U.S. Pat. No. 4,212,970). The content of the photopolymerization initiator in the first liquid crystal composition is preferably 0.1 to 20% by mass, and more preferably 0.5 to 12% by mass, based on the content of the liquid crystal compound.
[0062] --Crosslinking agent-- The first liquid crystal composition may contain a crosslinking agent to improve the film strength and durability after curing. As the crosslinking agent, those that are cured by ultraviolet light, heat, moisture, etc. can be suitably used. The crosslinking agent is not particularly limited and can be appropriately selected according to the purpose. For example, polyfunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate; epoxy compounds such as glycidyl (meth)acrylate and ethylene glycol diglycidyl ether; aziridine compounds such as 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate] and 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane; isocyanate compounds such as hexamethylene diisocyanate and biuret type isocyanate; polyoxazoline compounds having an oxazoline group in the side chain; and alkoxysilane compounds such as vinyltrimethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane. In addition, a known catalyst can be used according to the reactivity of the crosslinking agent, which can improve productivity in addition to improving film strength and durability. These may be used alone or in combination of two or more. The content of the crosslinking agent is preferably 3 to 20 mass %, more preferably 5 to 15 mass %, based on the solid content mass of the first liquid crystal composition. When the content of the crosslinking agent is within the above range, the effect of improving the crosslinking density is easily obtained, and the stability of the liquid crystal phase is further improved.
[0063] --Other additives-- If necessary, a polymerization inhibitor, an antioxidant, an ultraviolet absorber, a light stabilizer, a colorant, metal oxide fine particles, etc. may be added to the first liquid crystal composition within a range that does not impair optical performance, etc.
[0064] --solvent-- The first liquid crystal composition is preferably used in the form of a liquid when forming a liquid crystal layer. The first liquid crystal composition may contain a solvent. There is no limitation on the solvent and it can be appropriately selected depending on the purpose, but an organic solvent is preferable. The organic solvent is not limited and can be appropriately selected according to the purpose, and examples thereof include ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers. These may be used alone or in combination of two or more. Among these, ketones are preferred when considering the burden on the environment.
[0065] [Peeling process] The peeling process is a process in which an adherend 35 is laminated and fixed to the surface of the liquid crystal alignment layer 33 opposite the alignment film 32, as shown in Figure 4, and the liquid crystal alignment layer 33 is peeled off at the interface with the alignment film 32, as shown in Figure 5.
[0066] As the adherend 35, various known materials can be used, such as a film in which an adhesive layer with weak adhesive strength is formed on a resin film.
[0067] Examples include so-called laminate films (protective films) used to protect various materials and products, such as protecting the display screen of a display device, protecting the surfaces of various film products, and protecting the surfaces of home appliances, and transfer films used to attach a film (layer) formed on a support with weak adhesive strength, peel it off from the support, and attach it to another support with strong adhesive strength (peeling transfer).
[0068] Moreover, it is preferable that the adherend 35 is a flexible film-like material. By using a flexible film-like adherend 35, the workability of peeling can be improved.
[0069] Furthermore, when the adherend 35 does not have an adhesive layer, the adherend 35 may be laminated and fixed to the liquid crystal alignment layer 33 using an adhesive, a bonding agent, an adhesive tape, or the like.
[0070] The adhesive and pressure-sensitive adhesive may be any adhesive capable of bonding the adherend 35 and the liquid crystal alignment layer 33, and any adhesive and pressure-sensitive adhesive used in various known optical films may be used as appropriate.
[0071] The adhesive may be formed by combining one or more of water-based adhesives, active energy ray curing adhesives, pressure sensitive adhesives, etc. Examples of water-based adhesives include polyvinyl alcohol resin aqueous solutions and water-based two-liquid urethane emulsion adhesives. Examples of active energy ray curing adhesives are adhesives that are cured by irradiation with active energy rays such as ultraviolet rays, and include those containing a polymerizable compound and a photopolymerization initiator, those containing a photoreactive resin, and those containing a binder resin and a photoreactive crosslinking agent. Examples of the polymerizable compound include photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, and photocurable urethane monomers, and oligomers derived from these monomers. Examples of the photopolymerization initiator include those containing a substance that generates active species such as neutral radicals, anion radicals, and cation radicals when irradiated with active energy rays such as ultraviolet rays.
[0072] Examples of the adhesive include compositions containing a base polymer such as a (meth)acrylic resin, a styrene resin, or a silicone resin, to which a crosslinking agent such as an isocyanate compound, an epoxy compound, or an aziridine compound is added.
[0073] There is no limitation on the method for peeling off the liquid crystal alignment layer 33 and the alignment film 32 at the interface therebetween, and various known methods can be used.
[0074] Photo-alignment films using photo-alignment materials, particularly photo-alignment films using azo-based photo-alignment materials as the photo-alignment materials, have low adhesion to liquid crystal layers mainly composed of liquid crystal compounds. Therefore, by attaching adherend 35 to liquid crystal alignment layer 33 and peeling adherend 35, liquid crystal alignment layer 33 can be easily peeled off from alignment film 32.
[0075] 6, the surface 33a of the peeled liquid crystal alignment layer 33, which is the side from which the alignment film 32 has been peeled off, is used to perform the following alignment of the liquid crystal layer 34. On the surface 33a, the liquid crystal compound is aligned according to the alignment pattern of the alignment film 32.
[0076] [Liquid Crystal Layer Alignment Process] The liquid crystal layer alignment step is a step of laminating a second liquid crystal composition containing a polymerizable liquid crystal compound on the surface of the liquid crystal alignment layer from which the alignment film has been peeled off, and aligning the second liquid crystal composition. In the liquid crystal layer alignment step, the second liquid crystal composition is applied onto surface 33a of liquid crystal alignment layer 33, and the liquid crystal compound is aligned in a desired liquid crystal phase state.
[0077] The second liquid crystal composition can be applied by any known method capable of uniformly applying a liquid to a sheet-like material, such as a printing method including ink-jet printing and scroll printing, as well as spin coating, bar coating and spray coating.
[0078] The applied second liquid crystal composition is dried and / or heated as necessary, so that the liquid crystal compounds in the second liquid crystal composition are aligned in a predetermined alignment state according to the alignment pattern formed on the surface 33a of the liquid crystal alignment layer 33. When heating is performed, the heating temperature is preferably 200° C. or lower, more preferably 130° C. or lower.
[0079] [Liquid crystal layer formation process] The liquid crystal layer forming step is a step of polymerizing the aligned second liquid crystal composition to form a liquid crystal layer.
[0080] The polymerization may be either thermal polymerization or photopolymerization by light irradiation, but photopolymerization is preferred. The light irradiation is preferably performed using ultraviolet light. The irradiation energy is 20 mJ / cm. 2 ~50J / cm 2 is preferred, and 50 mJ / cm 2 ~1500mJ / cm 2In order to promote the photopolymerization reaction, the light irradiation may be performed under heating conditions or in a nitrogen atmosphere. The wavelength of the ultraviolet light to be irradiated is preferably 250 to 430 nm. Through the liquid crystal layer alignment step and the liquid crystal layer formation step, a liquid crystal layer 34 is formed as shown in FIG.
[0081] The second liquid crystal composition may be the same as the first liquid crystal composition described above. The first and second liquid crystal compositions may be the same or different.
[0082] [Liquid crystal layer separation process] 8, the liquid crystal layer separation process is a process of separating the formed liquid crystal layer 34 from the liquid crystal alignment layer 33. There is no limitation on the method of separating the liquid crystal layer 34 from the liquid crystal alignment layer 33, and various known methods can be used.
[0083] As an example, a transfer film or the like may be attached to the liquid crystal layer 34, and the liquid crystal layer 34 may be separated together with the transfer film from the liquid crystal alignment layer 33, similarly to the above-described peeling step. In this case, it is preferable that the adhesive strength between the liquid crystal alignment layer 33 and the adherend 35 and the adhesive strength between the liquid crystal layer 34 and the transfer film are greater than the adhesive strength between the liquid crystal alignment layer 33 and the liquid crystal layer 34. The adhesive strength between the liquid crystal alignment layer 33 and the liquid crystal layer 34 can be reduced, for example, by selecting and treating a system (material) that is unable or difficult to form a covalent bond at the interface between the liquid crystal alignment layer 33 and the liquid crystal layer 34. For example, the polymerization systems of the liquid crystal alignment layer 33 and the liquid crystal layer 34 can be changed. Specifically, an acrylate-based material can be used as one material and an epoxy-based material can be used as the other material. Furthermore, even if the polymerization system is the same (for example, an acrylate-based material), the surface of the liquid crystal alignment layer 33 may be treated, such as by halogenation, so that no acrylate remains.
[0084] Through the above steps, the liquid crystal layer 34 can be manufactured.
[0085] Here, in the method for producing a liquid crystal layer of the present invention, the liquid crystal layer 34 can be repeatedly produced by repeating the liquid crystal layer alignment step to the liquid crystal layer separation step. This eliminates the need to form an alignment film for each liquid crystal layer, and can increase productivity. In particular, when forming an alignment pattern by performing laser interference exposure on the alignment film, an exposure time of about 5 minutes is required for an area of about 5 cm square, which is very low productivity. However, by forming a liquid crystal layer using a liquid crystal alignment layer as in the present invention, it is not necessary to expose the alignment film every time a liquid crystal layer is produced, and therefore productivity can be increased.
[0086] As described above, when reusing the alignment film, in the case of a configuration having a release layer between the liquid crystal alignment layer and the liquid crystal layer to separate the liquid crystal alignment layer and the liquid crystal layer, if a release layer is present between the liquid crystal alignment layer and the liquid crystal layer, there is a problem that the alignment of the liquid crystal layer formed is insufficient due to the presence of the release layer. In addition, since the alignment of the liquid crystal compound is low on the surface of the liquid crystal alignment layer opposite the alignment film, there is a problem that the alignment of the liquid crystal layer is insufficient when the liquid crystal layer is formed on the surface of the liquid crystal alignment layer opposite the alignment film. In particular, when the liquid crystal compound in the liquid crystal layer is aligned in a smaller periodic pattern, there is a problem that the liquid crystal compound in the liquid crystal layer cannot be aligned sufficiently.
[0087] In contrast, in the method for manufacturing a liquid crystal layer of the present invention, a liquid crystal layer 34 is formed on surface 33a of liquid crystal alignment layer 33 from which alignment film 32 has been peeled off. Since surface 33a of liquid crystal alignment layer 33 from which alignment film 32 has been peeled off has a high degree of alignment of the liquid crystal compound, by forming liquid crystal layer 34 on this surface 33a, liquid crystal layer 34 can be sufficiently aligned. Furthermore, since no peeling layer is provided between liquid crystal alignment layer 33 and liquid crystal layer 34, it is possible to prevent the alignment of liquid crystal layer 34 from being reduced by the peeling layer.
[0088] Here, in the present invention, the alignment film formed in the alignment film forming step is preferably formed from a photoalignment composition containing an azobenzene-based compound. An alignment film using an azobenzene-based compound can have higher alignment. Therefore, the alignment of the liquid crystal alignment layer can be made higher, and the alignment of the liquid crystal layer to be produced can be made higher. In addition, when the liquid crystal layer is produced repeatedly multiple times, the alignment of the liquid crystal alignment layer gradually deteriorates, but since the alignment of the original liquid crystal alignment layer is high, more liquid crystal layers having a certain level of alignment or higher can be produced.
[0089] In the present invention, the first liquid crystal composition preferably contains a polyfunctional polymerizable liquid crystal compound. That is, the polymerizable liquid crystal compound contained in the first liquid crystal composition is preferably polyfunctionally polymerizable. By containing a polyfunctional polymerizable liquid crystal compound in the first liquid crystal composition that becomes the liquid crystal alignment layer, the strength of the liquid crystal alignment layer can be increased. As a result, when the liquid crystal layer is repeatedly produced, the liquid crystal alignment layer is less likely to deteriorate, and more liquid crystal layers can be produced.
[0090] The liquid crystal layer of the present invention produced by the production method of the present invention will be described below.
[0091] <Liquid crystal layer> An example of the liquid crystal layer will be described with reference to FIGS. Fig. 9 is a conceptual diagram of the cholesteric liquid crystal layer 34. Fig. 10 is a schematic diagram showing the alignment state of liquid crystal compounds in the plane of the main surface of the cholesteric liquid crystal layer 34 shown in Fig. 9. In the following description, the principal surface of the cholesteric liquid crystal layer 34 is defined as the XY plane, and the cross section perpendicular to the XY plane is defined as the XZ plane. That is, Fig. 9 corresponds to a schematic diagram of the XZ plane of the cholesteric liquid crystal layer 34, and Fig. 10 corresponds to a schematic diagram of the XY plane of the cholesteric liquid crystal layer 34.
[0092] As shown in Figures 9 and 10, the cholesteric liquid crystal layer 34 is a layer in which a liquid crystal compound is cholesterically oriented. Figures 9 and 10 show an example in which the liquid crystal compound constituting the cholesteric liquid crystal layer is a rod-shaped liquid crystal compound. In the following description, the cholesteric liquid crystal layer is also simply referred to as a liquid crystal layer.
[0093] The liquid crystal layer 34 is a cholesteric liquid crystal layer having a fixed cholesteric liquid crystal phase, and has a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound changes while continuously rotating along at least one direction in the plane.
[0094] As conceptually shown in Figure 9, the liquid crystal layer 34 has a helical structure in which liquid crystal compounds 40 are spirally stacked, similar to a cholesteric liquid crystal layer formed by fixing a normal cholesteric liquid crystal phase, and has a structure in which liquid crystal compounds 40 spirally spirally spirally spirally stacked at multiple pitches, with one helical pitch (pitch P) being one rotation (360° rotation) of the liquid crystal compounds 40 stacked in a helical shape.
[0095] As is well known, cholesteric liquid crystal phases exhibit selective reflection for either left-handed or right-handed circularly polarized light at a specific wavelength. Whether the reflected light is right-handed or left-handed circularly polarized light depends on the twist direction (sense) of the helix of the cholesteric liquid crystal phase. When the helix of the cholesteric liquid crystal phase is twisted to the right, right-handed circularly polarized light is reflected, and when the helix is twisted to the left, left-handed circularly polarized light is reflected. The direction of rotation of the cholesteric liquid crystal phase can be adjusted by the type of liquid crystal compound forming the cholesteric liquid crystal layer and / or the type of chiral agent added.
[0096] Furthermore, the half-width Δλ (nm) of the selective reflection band (circularly polarized light reflection band) exhibiting selective reflection depends on the Δn of the cholesteric liquid crystal phase and the helical pitch P, and follows the relationship Δλ = Δn × P. Therefore, the width of the selective reflection band can be controlled by adjusting Δn. Δn can be adjusted by the type and mixing ratio of the liquid crystal compounds forming the cholesteric liquid crystal layer, as well as the temperature at which the orientation is fixed. Therefore, the wavelength of light reflected (diffracted) by the liquid crystal layer can be appropriately set by adjusting, for example, the helical pitch P of the liquid crystal layer to set the selective reflection wavelength range of the liquid crystal layer. The half width of the reflection wavelength range is adjusted depending on the application of the liquid crystal layer and may be, for example, 10 to 500 nm, preferably 20 to 300 nm, and more preferably 30 to 100 nm.
[0097] 10, in the XY plane of the liquid crystal layer 34, the liquid crystal compounds 40 are aligned along a plurality of alignment axes D parallel to each other in the XY plane, and on each alignment axis D, the direction of the optical axis 40A of the liquid crystal compounds 40 changes while continuously rotating in one direction in the plane along the alignment axis D. For the sake of explanation, it is assumed that the alignment axis D is oriented in the X direction. In addition, in the Y direction, the liquid crystal compounds 40 having the same direction of the optical axis 40A are aligned at equal intervals. Here, "the orientation of the optical axis 40A of the liquid crystal compound 40 changes while continuously rotating in one direction in the plane along the arrangement axis D" means that the angle between the optical axis 40A of the liquid crystal compound 40 and the arrangement axis D varies depending on the position along the arrangement axis D, and the angle between the optical axis 40A and the arrangement axis D gradually changes from θ to θ+180° or θ-180° along the arrangement axis D. In other words, the optical axes 40A of the multiple liquid crystal compounds 40 aligned along the arrangement axis D change while rotating at a constant angle along the arrangement axis D, as shown in FIG. The difference in angle between the optical axes 40A of the liquid crystal compounds 40 adjacent to each other in the direction of the alignment axis D is preferably 45° or less, more preferably 15° or less, and even more preferably a smaller angle. In addition, in this specification, when the liquid crystal compound 40 is a rod-shaped liquid crystal compound, the optical axis 40A of the liquid crystal compound 40 refers to the molecular long axis of the rod-shaped liquid crystal compound. On the other hand, when the liquid crystal compound 40 is a discotic liquid crystal compound, the optical axis 40A of the liquid crystal compound 40 refers to the axis parallel to the normal direction to the disc surface of the discotic liquid crystal compound.
[0098] In the liquid crystal layer 34, in the liquid crystal orientation pattern of such liquid crystal compound 40, the length (distance) over which the optical axis 40A of the liquid crystal compound 40 rotates 180° in the direction of the alignment axis D along which the optical axis 40A continuously rotates and changes in the plane is defined as the length Λ of one period of the liquid crystal orientation pattern. That is, the length Λ of one period is defined as the distance between the centers in the direction of the arrangement axis D of two liquid crystal compounds 40 that are at the same angle with respect to the direction of the arrangement axis D. Specifically, as shown in Fig. 10, the length Λ of one period is defined as the distance between the centers in the direction of the arrangement axis D of two liquid crystal compounds 40 whose directions of the arrangement axis D and the optical axis 40A coincide with each other. In the following description, this length Λ of one period is also referred to as "one period Λ". The liquid crystal orientation pattern of the liquid crystal layer 34 repeats this one period Λ in one direction along the direction of the arrangement axis D, that is, the direction of the optical axis 40A, which continuously rotates and changes. In the liquid crystal diffraction element, this one period Λ becomes the period of the diffraction structure.
[0099] On the other hand, the liquid crystal compound 40 forming the liquid crystal layer 34 has the same orientation of the optical axis 40A in a direction perpendicular to the direction of the alignment axis D (Y direction in Figure 10), i.e., in the Y direction perpendicular to the direction in which the optical axis 40A continuously rotates. In other words, in the liquid crystal compound 40 forming the liquid crystal layer 34, the angle between the optical axis 40A of the liquid crystal compound 40 and the direction of the alignment axis D is equal in the Y direction.
[0100] When the XZ plane of the liquid crystal layer 34 shown in FIG. 9 is observed with a SEM (scanning electron microscope), a striped pattern is observed in which the arrangement direction of the alternating bright and dark portions 42 and 44 as shown in FIG. 11 is inclined at a predetermined angle with respect to the main surface (XY plane). In such an SEM cross section, the interval in the normal direction of the lines formed by the bright and dark portions 42 and 44 from adjacent bright and dark portions 42 and 44 is approximately equal to 1 / 2 pitch. That is, as shown by P in FIG. 11, two bright portions 42 and two dark portions 44 are approximately equal to one pitch of the spiral (one winding of the spiral), that is, the pitch P. When the inclination of the liquid crystal compound is equal to the inclination of the bright and dark portions as shown in FIG. 13, the spiral pitch is approximately equal to the pitch P of the bright and dark lines shown in FIG. 11. Furthermore, when the inclination of the liquid crystal compound does not match the inclination of the light and dark areas as in Figure 9, the helical pitch deviates slightly from the pitch P of the light and dark lines shown in Figure 11, but in the following explanation, no distinction is made between the helical pitch and the pitch of the light and dark lines.
[0101] The effect of diffraction by the liquid crystal layer will now be described. In a conventional cholesteric liquid crystal layer, the helical axis derived from the cholesteric liquid crystal phase is perpendicular to the main surface (XY plane), and the reflection surface is parallel to the main surface (XY plane). In addition, the optical axis of the liquid crystal compound is not tilted with respect to the main surface (XY plane). In other words, the optical axis is parallel to the main surface (XY plane). Therefore, when the XZ plane of a conventional cholesteric liquid crystal layer is observed with an SEM, the alignment direction in which light and dark areas are alternately arranged is perpendicular to the main surface (XY plane). Since the cholesteric liquid crystal phase has specular reflectivity, for example, when light is incident on a cholesteric liquid crystal layer from the normal direction, the light is reflected in the normal direction.
[0102] In contrast, the liquid crystal layer 34 reflects the incident light with an inclination toward the direction of the arrangement axis D with respect to the specular reflection. The liquid crystal layer 34 has a liquid crystal orientation pattern in which the optical axis 40A changes while continuously rotating in the plane along the direction of the arrangement axis D (a predetermined direction). The following will be described with reference to FIG. 12.
[0103] As an example, the liquid crystal layer 34 is configured to polarize right-handed circularly polarized red light R R Therefore, when light is incident on the liquid crystal layer 34, the liquid crystal layer 34 selectively reflects right-handed circularly polarized red light R R It reflects only light and transmits all other light.
[0104] In the liquid crystal layer 34, the optical axis 40A of the liquid crystal compound 40 changes while rotating along the direction of the arrangement axis D (one direction). The liquid crystal alignment pattern formed in the liquid crystal layer 34 is a periodic pattern in the direction of the alignment axis D. Therefore, the right-handed circularly polarized light R R As conceptually shown in Figure 12, the right-handed circularly polarized light R of the reflected red light is reflected (diffracted) in a direction according to the period of the liquid crystal orientation pattern. R is reflected (diffracted) in a direction inclined toward the alignment axis D direction with respect to the XY plane (the main surface of the cholesteric liquid crystal layer).
[0105] That is, the liquid crystal layer 34 can be used as a diffraction element that reflects (diffracts) incident light in a direction different from the direction of specular reflection.
[0106] In the liquid crystal layer 34, the direction of the arrangement axis D, which is one direction in which the optical axis 40A rotates, can be appropriately set to adjust the reflection direction (diffraction angle) of light.
[0107] When circularly polarized light of the same wavelength and rotation direction is reflected, the reflection direction of the circularly polarized light can be reversed by reversing the rotation direction of the optical axis 40A of the liquid crystal compound 40 facing the alignment axis D. For example, in Figures 9 and 10, the rotation direction of the optical axis 40A toward the array axis D is clockwise, and some circularly polarized light is reflected with an inclination toward the array axis D, but by changing this to counterclockwise, some circularly polarized light is reflected with an inclination in the opposite direction to the array axis D.
[0108] Furthermore, in liquid crystal layers having the same liquid crystal orientation pattern, the reflection direction is reversed depending on the helical rotation direction of the liquid crystal compound 40, that is, the rotation direction of the reflected circularly polarized light. For example, when the direction of rotation of the helix is right-twisted, right-handed circularly polarized light is selectively reflected, and by having a liquid crystal orientation pattern in which the optical axis 40A rotates clockwise along the direction of the array axis D, right-handed circularly polarized light is reflected at an inclination toward the direction of the array axis D. Furthermore, for example, when the direction of rotation of the helix is left twisted, left-handed circularly polarized light is selectively reflected, and a liquid crystal layer having a liquid crystal orientation pattern in which the optical axis 40A rotates clockwise along the direction of the arrangement axis D reflects left-handed circularly polarized light tilted in the direction opposite to the direction of the arrangement axis D.
[0109] In the liquid crystal orientation pattern of the liquid crystal compound in the liquid crystal layer, one period Λ, which is the length for the optical axis of the liquid crystal compound to rotate 180°, is the period (one period) of the diffraction structure. In addition, in the liquid crystal layer, one direction (direction of the alignment axis D) in which the optical axis of the liquid crystal compound changes while rotating is the periodic direction of the diffraction structure. In the present invention, there is no limitation on the length of one period Λ of the diffraction element, and it may be set appropriately depending on the desired diffraction angle and the like. The length of one period Λ is preferably from 0.1 to 10 μm, more preferably from 0.15 to 2 μm, and even more preferably from 0.2 to 1 μm.
[0110] In a liquid crystal layer having a liquid crystal alignment pattern, the shorter the period Λ, the larger the angle of the reflected light with respect to the incident light. In other words, the shorter the period Λ, the greater the angle at which the reflected light can be reflected with respect to the incident light. In addition, in a liquid crystal layer having this liquid crystal orientation pattern, the reflection angle (diffraction angle) of light varies depending on the wavelength of the reflected light. Specifically, the longer the wavelength of light, the larger the angle of the reflected light with respect to the incident light.
[0111] The example shown in FIG. 9 is configured such that in the XZ plane of the liquid crystal layer 34, the liquid crystal compound 40 has its optical axis 40A aligned parallel to the principal plane (XY plane). However, the present invention is not limited thereto. For example, as conceptually shown in Fig. 13, in the XZ plane of the liquid crystal layer 34, the liquid crystal compound 40 may be configured such that its optical axis 40A is inclined with respect to the main plane (XY plane).
[0112] 13, the inclination angle (tilt angle) of the liquid crystal compound 40 with respect to the principal surface (XY plane) in the XZ plane of the liquid crystal layer 34 is uniform in the thickness direction (Z direction), but the present invention is not limited thereto. The liquid crystal layer 34 may have a region in which the tilt angle of the liquid crystal compound 40 varies in the thickness direction. For example, in the example shown in FIG. 14, the optical axis 40A of the liquid crystal compound 40 is parallel to the main surface (pretilt angle is 0) at the interface on the alignment film 32 side of the liquid crystal layer, and the tilt angle of the liquid crystal compound 40 increases with increasing distance in the thickness direction from the interface on the alignment film 32 side, and thereafter, the liquid crystal compound is oriented at a constant tilt angle up to the other interface (air interface).
[0113] In this way, in the liquid crystal layer 34, the optical axis of the liquid crystal compound may have a pretilt angle at one of the upper and lower interfaces, or may have pretilt angles at both interfaces. Also, the pretilt angles may be different at both interfaces. When the liquid crystal compound has a tilt angle (is inclined) in this way, the effective birefringence of the liquid crystal compound increases when light is diffracted, and the diffraction efficiency can be improved.
[0114] The average angle (average tilt angle) between the optical axis 40A of the liquid crystal compound 40 and the principal surface (XY plane) is preferably 5 to 45°, more preferably 12 to 22°. The average tilt angle can be measured by observing the XZ plane of the liquid crystal layer 34 with a polarizing microscope. In particular, in the XZ plane of the liquid crystal layer 34, the optical axis 40A of the liquid crystal compound 40 is preferably tilted in the same direction with respect to the principal surface (XY plane). The tilt angle is an arithmetic average of angles between the optical axis 40A of the liquid crystal compound 40 and the principal surface measured at any five or more points in a cross section of the cholesteric liquid crystal layer observed under a polarizing microscope.
[0115] Light that is perpendicularly incident on the liquid crystal layer 34 travels obliquely within the liquid crystal layer due to the bending force acting on it. As the light travels within the liquid crystal layer, a deviation occurs from conditions such as the diffraction period that are set to obtain a desired diffraction angle for perpendicular incidence, resulting in diffraction loss. When a liquid crystal compound is tilted, there exists a direction in which a higher birefringence occurs with respect to the direction in which light is diffracted, compared to when it is not tilted. In this direction, the effective extraordinary refractive index becomes larger, and therefore the birefringence, which is the difference between the extraordinary refractive index and the ordinary refractive index, becomes higher. By setting the tilt angle direction in accordance with the desired diffraction direction, it is possible to suppress deviation from the original diffraction conditions at that direction. As a result, it is believed that a higher diffraction efficiency can be obtained when using a liquid crystal compound with a tilt angle.
[0116] Moreover, the tilt angle is preferably controlled by treatment of the interface of the liquid crystal layer 34 . At the interface on the support side, the tilt angle of the liquid crystal compound can be controlled by performing a pretilt treatment on the photo-alignment film. For example, when forming the photo-alignment film, the photo-alignment film is exposed to ultraviolet light from the front and then from an oblique angle, so that a pretilt angle can be generated in the liquid crystal compound in the liquid crystal layer formed on the photo-alignment film. In this case, the liquid crystal compound is pretilted in the direction in which the single axis side is visible with respect to the second irradiation direction. However, since the liquid crystal compound in the direction perpendicular to the second irradiation direction does not pretilt, there are regions in the plane that are pretilted and regions that are not pretilted. This contributes to increasing the birefringence in the desired direction when diffracting light in that direction, and is therefore suitable for increasing diffraction efficiency. Furthermore, an additive that promotes the pretilt angle can be added to the liquid crystal layer or the photo-alignment film, in which case the additive can be used as a factor for further increasing the diffraction efficiency. This additive can also be used to control the pretilt angle of the air-side interface.
[0117] Here, in the cross section of the liquid crystal layer 34 observed by SEM, the bright and dark areas derived from the cholesteric liquid crystal phase are inclined with respect to the main surface. When the in-plane retardation Re of the liquid crystal layer is measured from the normal direction and the direction inclined with respect to the normal, it is preferable that the direction in which the in-plane retardation Re is minimum is inclined with respect to the normal direction in either the slow axis plane or the fast axis plane. Specifically, it is preferable that the absolute value of the measurement angle between the normal line and the direction in which the in-plane retardation Re is minimum is 5° or more. In other words, it is preferable that the liquid crystal compound of the liquid crystal layer is inclined with respect to the main surface, and the inclination direction approximately coincides with the bright and dark areas of the liquid crystal layer. The normal direction is a direction perpendicular to the main surface. The liquid crystal layer having such a configuration can diffract circularly polarized light with higher diffraction efficiency than a liquid crystal layer in which the liquid crystal compound is parallel to the main surface.
[0118] In a configuration in which the liquid crystal compound of the liquid crystal layer is tilted with respect to the main surface and the tilt direction is approximately the same as the light and dark areas, the light and dark areas corresponding to the reflecting surface are aligned with the optical axis of the liquid crystal compound. Therefore, the effect of the liquid crystal compound on the reflection (diffraction) of light is increased, and the diffraction efficiency can be improved. As a result, the amount of reflected light relative to the incident light can be further improved.
[0119] In the fast axis plane or slow axis plane of the liquid crystal layer, the absolute value of the optical axis tilt angle of the liquid crystal layer is preferably 5° or more, more preferably 15° or more, and even more preferably 20° or more. By setting the absolute value of the optical axis tilt angle to 15° or more, it is possible to more suitably match the directions of the liquid crystal compounds with the light and dark areas, which is preferable in terms of improving the diffraction efficiency.
[0120] The liquid crystal layer shown in FIG. 9 is a cholesteric liquid crystal layer, but the liquid crystal layer produced by the production method of the present invention is not limited to this.
[0121] 15 and 16 show another example of a liquid crystal layer produced by the production method of the present invention. 16, the liquid crystal layer 36, like the cholesteric liquid crystal layer 34, has a liquid crystal alignment pattern in which the optical axis 40A of the liquid crystal compound 40 continuously rotates along the direction of the alignment axis D. Note that, like the above-mentioned FIG. 10, FIG. 16 also shows only the liquid crystal compound on the surface of the alignment film 32. As shown in Fig. 15, the liquid crystal compound 40 forming the liquid crystal layer 36 is not twisted in a helical manner in the thickness direction, and the optical axis 40A is located at the same position in the plane direction. Such a liquid crystal layer can be formed by not adding a chiral agent to the liquid crystal composition in the formation of the above-mentioned cholesteric liquid crystal layer. Note that such a liquid crystal layer may have a configuration in which the liquid crystal compound is twisted in the thickness direction to such an extent that it does not become a cholesteric liquid crystal phase.
[0122] As described above, the liquid crystal layer 36 has a liquid crystal alignment pattern in which the direction of the optical axis 40A derived from the liquid crystal compound 40 changes while continuously rotating along the alignment axis D in the plane. On the other hand, the liquid crystal compounds 40 forming the liquid crystal layer 36 are arranged at equal intervals in the Y direction perpendicular to the direction of the arrangement axis D, i.e., in the Y direction perpendicular to the one direction in which the optical axis 40A continuously rotates, with the liquid crystal compounds 40 having the same orientation of the optical axis 40A being aligned. In other words, in the liquid crystal compounds 40 forming the liquid crystal layer 36, the angles between the optical axes 40A and the alignment axis D direction are equal to each other among the liquid crystal compounds 40 aligned in the Y direction.
[0123] In the liquid crystal layer 36, the liquid crystal compounds aligned in the Y direction have the same angle between their optical axes 40A and the direction of the alignment axis D (one direction in which the orientation of the optical axes of the liquid crystal compounds 40 rotates). A region in which the liquid crystal compounds 40, in which the optical axes 40A and the direction of the alignment axis D form the same angle, are arranged in the Y direction is referred to as a region R. In this case, the value of the in-plane retardation (Re) in each region R is preferably half the wavelength, i.e., λ / 2. These in-plane retardations are calculated by the product of the refractive index difference Δn associated with the refractive index anisotropy of the region R and the thickness of the optically anisotropic layer. Here, the refractive index difference associated with the refractive index anisotropy of the region R in the optically anisotropic layer is a refractive index difference defined by the difference between the refractive index in the direction of the slow axis in the plane of the region R and the refractive index in the direction perpendicular to the direction of the slow axis. That is, the refractive index difference Δn associated with the refractive index anisotropy of the region R is equal to the difference between the refractive index of the liquid crystal compound 40 in the direction of the optical axis 40A and the refractive index of the liquid crystal compound 40 in the direction perpendicular to the optical axis 40A in the plane of the region R. That is, the refractive index difference Δn is equal to the refractive index difference of the liquid crystal compound 40.
[0124] When circularly polarized light enters such a liquid crystal layer 36, the light is refracted and the direction of the circular polarization is changed. This action is conceptually shown in Figures 17 and 18. In the liquid crystal layer 36, the product of the refractive index difference of the liquid crystal compound and the thickness of the optically anisotropic layer is assumed to be λ / 2. As shown in Figure 17, when the product of the refractive index difference of the liquid crystal compound in the liquid crystal layer 36 and the thickness of the optically anisotropic layer is λ / 2, when incident light L1 that is left-handed circularly polarized light is incident on the liquid crystal layer 36, the incident light L1 is given a phase difference of 180° as it passes through the liquid crystal layer 36, and the transmitted light L2 is converted into right-handed circularly polarized light. In addition, since the liquid crystal orientation pattern formed in the liquid crystal layer 36 is a periodic pattern in the direction of the array axis D, the transmitted light L2 travels in a direction different from that of the incident light L1. In this way, the left-handed circularly polarized incident light L1 is converted into right-handed circularly polarized transmitted light L2 that is tilted at a certain angle in the direction of the array axis D with respect to the incident direction.
[0125] On the other hand, as shown in Figure 18, when the product of the refractive index difference of the liquid crystal compound in the liquid crystal layer 36 and the thickness of the optically anisotropic layer is λ / 2, when right-handed circularly polarized incident light L4 is incident on the liquid crystal layer 36, the incident light L4 is given a phase difference of 180° by passing through the liquid crystal layer 36 and is converted into left-handed circularly polarized transmitted light L5. Furthermore, since the liquid crystal orientation pattern formed in the liquid crystal layer 36 is a periodic pattern in the direction of the array axis D, the transmitted light L5 travels in a direction different from that of the incident light L4. At this time, the transmitted light L5 travels in a direction different from that of the transmitted light L2, that is, in the opposite direction to the direction of the arrow X with respect to the incident direction. In this way, the incident light L4 is converted into the transmitted light L5 of left-handed circular polarization tilted at a certain angle in the opposite direction to the array axis D with respect to the incident direction.
[0126] Like the cholesteric liquid crystal layer 34, the liquid crystal layer 36 can adjust the angles of refraction of the transmitted light L2 and L5 by changing one period Λ of the formed liquid crystal orientation pattern. Specifically, the shorter the period Λ of the liquid crystal orientation pattern of the liquid crystal layer 36, the stronger the interference between the lights that have passed through adjacent liquid crystal compounds 40, and therefore the greater the refraction of the transmitted light L2 and L5. Furthermore, the direction of refraction of transmitted light can be reversed by reversing the direction of rotation of the optical axis 40A of the liquid crystal compound 40, which rotates along the direction of the arrangement axis D. That is, in the example shown in Figures 15 and 16, the direction of rotation of the optical axis 40A facing the direction of the arrangement axis D is clockwise, but by changing this rotation direction to counterclockwise, the direction of refraction of transmitted light can be reversed.
[0127] From the viewpoint of diffraction efficiency, it is preferable that such a liquid crystal layer that transmits and diffracts incident light has a region in which the liquid crystal compound is twisted and rotated (the twist angle is less than 360°).
[0128] Furthermore, such a liquid crystal layer having a region in which the liquid crystal compound is not cholesterically oriented but is twisted and rotated (the twist angle is less than 360°) can also be used as a reflective diffraction element. In such a diffraction element, diffracted light is reflected at the interface of the diffraction element and emitted from the light incident side, and the light is diffracted while being reflected, so that the diffraction element can also function as a reflective diffraction element.
[0129] In addition, the liquid crystal layer 36 shown in FIG. 15 has a configuration in which the optical axis of the liquid crystal compound is parallel to the main surface of the liquid crystal layer, but this is not limited to this. For example, the optical axis of the liquid crystal compound in the above-mentioned liquid crystal layer 36 may be inclined to the main surface of the liquid crystal layer, as in the liquid crystal layer 36b shown in Fig. 19. Note that the liquid crystal layer 36b is similar to the above-mentioned liquid crystal layer 36 in that it has a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound changes while continuously rotating along one direction in the plane. That is, the plan view of the liquid crystal layer 36b is similar to that of Fig. 16.
[0130] The method for manufacturing a liquid crystal layer according to the present invention has been described in detail above. However, the present invention is not limited to the above-mentioned examples, and various improvements and modifications may be made without departing from the gist of the present invention. EXAMPLES
[0131] The features of the present invention will be described in more detail below with reference to examples. The materials, reagents, amounts used, amounts of substances, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0132] [Example 1] (Formation of photo-alignment film) A glass substrate was prepared as a support (first support). The following coating solution for forming a photo-alignment film was applied onto the support at 2500 rpm for 30 seconds using a spin coater. The support on which the coating solution for forming a photo-alignment film was formed was dried on a hot plate at 60° C. for 60 seconds to form a photo-alignment film.
[0133] Coating liquid for photo alignment film formation ---------------------------------------------------------------------------------- 1.00 parts by weight of the following photoalignment material Water 16.00 parts by mass Butoxyethanol 42.00 parts by weight Propylene glycol monomethyl ether 42.00 parts by mass ----------------------------------------------------------------------------------
[0134] -Material for photo alignment- [ka]
[0135] (Exposure of photo-alignment film) The photo-alignment film was exposed to light using the exposure device shown in FIG. 2 in an environment of a temperature of 25° C. and a relative humidity of 10%, to form a photo-alignment film P-1 having an alignment pattern. The exposure device used was a laser that emitted a laser beam with a wavelength of 325 nm. The exposure dose by the interference light was 3000 mJ / cm 2 The crossing angle (crossing angle α) of the two laser beams was set to 61.0°.
[0136] (Formation of liquid crystal alignment layer) The following liquid crystal composition LCMA-1 was prepared as a liquid crystal composition for forming a liquid crystal alignment layer. The solid content of this liquid crystal composition LCMA-1 was 15 wt %.
[0137] Liquid crystal composition LCMA-1 ---------------------------------------------------------------------------------- The following liquid crystal compound L-1: 100.00 parts by mass 3.00 parts by mass of the following polymerization initiator I-1 6.20 parts by mass of the following chiral agent Ch-1 Methyl ethyl ketone 619.00 parts by mass ----------------------------------------------------------------------------------
[0138] Liquid crystal compound L-1 [ka]
[0139] Polymerization initiator I-1 [ka]
[0140] Chiral Agent Ch-1 [ka]
[0141] Hereinafter, the environmental temperature from before the exposure step of the alignment film to the application of the liquid crystal layer was set to 25° C. and the relative humidity was set to 10%. A liquid crystal alignment layer was formed as follows.
[0142] The liquid crystal composition LCMA-1 was applied onto the photo-alignment film P-1, and the film was rotated at 1000 rpm for 10 seconds using a spin coater. The coating of the liquid crystal composition LCMA-1 was heated on a hot plate at 80°C for 3 minutes (180 sec). Thereafter, ultraviolet light having a wavelength of 365 nm was applied at 500 mJ / cm using a high-pressure mercury lamp in a nitrogen atmosphere at 80°C. 2 The coating film was irradiated with an irradiation amount of 1000 nm to cure the liquid crystal composition LCMA-1 and fix the alignment of the liquid crystal compound, thereby forming a liquid crystal alignment layer MA-1.
[0143] A glass substrate with a separately prepared adhesive was attached onto the obtained liquid crystal alignment layer MA-1, and the liquid crystal alignment layer MA-1 was peeled off from the interface with the photo-alignment film. After peeling, the air interface of the liquid crystal alignment layer MA-1 was the interface that had been in contact with the photo-alignment film.
[0144] (Formation of cholesteric liquid crystal layer) The following liquid crystal composition LC-1 was prepared as a liquid crystal composition for forming a cholesteric liquid crystal layer, and the solid content of this liquid crystal composition LC-1 was 35 wt %.
[0145] Liquid crystal composition LC-1 ------------------------------------------------------------------ The liquid crystal compound L-1 100.00 parts by mass The polymerization initiator I-1: 3.00 parts by mass The above chiral agent Ch-1 6.20 parts by mass Methyl ethyl ketone 202.99 parts by mass ------------------------------------------------------------------
[0146] A cholesteric liquid crystal layer was formed as follows: As described above, the temperature of the environment was 25° C. and the relative humidity was 10% until the liquid crystal composition that would become the liquid crystal layer was applied onto the liquid crystal alignment layer.
[0147] The liquid crystal composition LC-1 was applied onto the liquid crystal alignment layer MA-1, and the layer was rotated at 1000 rpm for 10 seconds using a spin coater. The coating of the liquid crystal composition LC-1 was heated on a hot plate at 80°C for 3 minutes (180 seconds). Thereafter, ultraviolet light having a wavelength of 365 nm was applied at 500 mJ / cm2 using a high-pressure mercury lamp in a nitrogen atmosphere at 80°C. 2 The coating film was irradiated with an irradiation dose of 100 nm to cure the liquid crystal composition LC-1 and fix the alignment of the liquid crystal compound, thereby forming a cholesteric liquid crystal layer.
[0148] The obtained cholesteric liquid crystal layer was transferred onto another glass substrate and separated at the interface with the liquid crystal alignment layer MA-1, and at the same time, the liquid crystal alignment layer MA-1 was reproduced.
[0149] The fabricated cholesteric liquid crystal layer was cut in the direction along the rotation direction of the optical axis, and the cross section was observed by SEM. By analyzing the SEM image, one period Λ in the liquid crystal alignment pattern was measured. One period Λ was 0.32 μm.
[0150] The number of times that cholesteric liquid crystal layers can be fabricated from one liquid crystal alignment layer was evaluated, and it was found to be five times.
[0151] [Example 2] A liquid crystal alignment layer MA-2 was prepared in the same manner as in Example 1, except that the liquid crystal composition LCMA-2 described below was used as the liquid crystal composition forming the liquid crystal alignment layer. The solid content of the liquid crystal composition LCMA-2 was 20 wt %.
[0152] Liquid crystal composition LCMA-2 ------------------------------------------------------------------ The liquid crystal compound L-1 100.00 parts by mass The polymerization initiator I-1: 3.00 parts by mass Methyl ethyl ketone 437.00 parts by mass ------------------------------------------------------------------
[0153] Using the liquid crystal alignment layer MA-2, the preparation and separation of a cholesteric liquid crystal layer was repeated in the same manner as in Example 1. One period Λ in the liquid crystal alignment pattern of the obtained optical element was 0.32 μm, the same as in Example 1.
[0154] The number of times that cholesteric liquid crystal layers can be fabricated from one liquid crystal alignment layer was evaluated, and it was found to be five times.
[0155] [Comparative Example 1] The photo-alignment film P-1 was subjected to interference exposure with laser light at a crossing angle (crossing angle α) of 61.0° in the same manner as in Example 1. The liquid crystal composition LCMA-2 was applied onto the exposed photo-alignment film P-1 in the same manner as in Example 2, and the liquid crystal composition LCMA-2 was cured by heating and irradiating with ultraviolet light in the same manner as in Example 1.
[0156] On the cured liquid crystal composition LCMA-2 (liquid crystal alignment layer), a UV-curable PDMS (X-34-4184A, X-34-4184B; manufactured by Shin-Etsu Chemical Co., Ltd.) diluted 10 times with decamethylcyclopentasiloxane was applied as a release layer, and the mixture was rotated at 3000 rpm for 10 seconds using a spin coater. Then, in a nitrogen atmosphere, a high-pressure mercury lamp was used to irradiate ultraviolet light with a wavelength of 365 nm at 500 mJ / cm 2 The release layer was fixed by irradiating the coating with a dose of 1000 nm.
[0157] Except for forming a cholesteric liquid crystal layer on a release layer, the preparation of a cholesteric liquid crystal layer and the separation of the cholesteric liquid crystal layer were repeated in the same manner as in Example 1. As a result, the prepared cholesteric liquid crystal layer had alignment defects, and a proper cholesteric liquid crystal layer could not be prepared. Therefore, the number of times that a cholesteric liquid crystal layer could be prepared from one liquid crystal alignment layer was zero. From the above results, the effects of the present invention are clear. [Industrial Applicability]
[0158] The present invention can be suitably used for producing liquid crystal layers used in various applications for refracting light in optical devices, such as diffraction elements that cause light to enter and exit the light guide plates of AR glasses. [Explanation of symbols]
[0159] 30 Support 32 Alignment film 33 Liquid crystal alignment layer 34, 36, 36b liquid crystal layer 35 Adherent 40 Liquid crystal compounds 40A optical axis 42 Akabe 44 Dark part 60 Exposure Equipment 62 Laser 64 Light source 65 λ / 2 plate 68 Polarizing Beam Splitter 70A, 70B Mirror 72A,72B λ / 4 board R R Red right-handed circularly polarized light M Laser light MA,MB rays P O Linearly polarized P R Right circular polarization P L Left circular polarization L1,L4 incident light L2,L5 transmitted light D Array axis Λ 1 period Pitch
Claims
1. An alignment film forming step of forming an alignment film on a support; a liquid crystal alignment layer alignment step of laminating a first liquid crystal composition containing a polymerizable liquid crystal compound on the alignment film and aligning the first liquid crystal composition; a liquid crystal alignment layer forming step of polymerizing the aligned first liquid crystal composition to form a liquid crystal alignment layer; a peeling step of laminating and fixing the surface of the liquid crystal alignment layer opposite to the alignment film to an adherend, and peeling the liquid crystal alignment layer and the alignment film at an interface between the liquid crystal alignment layer and the alignment film; a liquid crystal layer alignment step of directly laminating a second liquid crystal composition containing a polymerizable liquid crystal compound on the surface of the liquid crystal alignment layer from which the alignment film has been peeled off, and aligning the second liquid crystal composition; a liquid crystal layer forming step of polymerizing the aligned second liquid crystal composition to form a liquid crystal layer; and a liquid crystal layer separation step of separating the formed liquid crystal layer from the liquid crystal alignment layer; The liquid crystal layer is repeatedly produced by repeating the liquid crystal layer alignment step to the liquid crystal layer separation step, In the liquid crystal layer orienting step, the liquid crystal orientation layer causes the orientation of the optical axis derived from the liquid crystal compound in the liquid crystal layer to change while continuously rotating along at least one direction in the plane, A method for manufacturing a liquid crystal layer, wherein one of the materials of the liquid crystal alignment layer and the liquid crystal layer is an acrylate-based material, and the other of the materials of the liquid crystal alignment layer and the liquid crystal layer is an epoxy-based material.
2. The method for producing a liquid crystal layer according to claim 1 , wherein the alignment film formed in the alignment film forming step is formed from a photoalignment composition containing an azobenzene compound.
3. 3. The method for manufacturing a liquid crystal layer according to claim 1, wherein in the alignment film forming step, the alignment film is exposed to laser interference.
4. 4. The method for producing a liquid crystal layer according to claim 1, wherein the first liquid crystal composition contains a polyfunctional polymerizable compound.
5. The method for producing a liquid crystal layer according to claim 4 , wherein the polymerizable liquid crystal compound contained in the first liquid crystal composition is a polyfunctional polymerizable liquid crystal compound.
6. The method for manufacturing a liquid crystal layer according to any one of claims 1 to 5, wherein the liquid crystal alignment layer and the liquid crystal layer have different polymerization systems.
7. 7. The method for producing a liquid crystal layer according to claim 1, wherein the liquid crystal layer formed in the liquid crystal layer forming step does not have a release layer between the liquid crystal layer and the liquid crystal alignment layer.
Citation Information
Patent Citations
Optical film, image display device and method of manufacturing optical film
JP2013246302A
Counterfeit prevention device and production method thereof
JP2015089638A
Patterning liquid crystals using soft imprint replication of surface-matched patterns
JP2020502565A
Optical laminate manufacturing method, optical laminate, and image display device
WO2019131943A1
Method for producing optical element, and optical element
WO2020022513A1