Toner manufacturing method
The described toner production method addresses excessive shell layer formation by controlling temperature and pH in the aqueous medium process, enhancing fixing properties and storage stability.
Patent Information
- Application Number
- JP2020099455
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-08
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-06-08
Smart Images

Figure 0007562300000001 
Figure 0007562300000002 
Figure 0007562300000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a toner for developing electrostatic images used in electrophotographic imaging. [Background technology]
[0002] In recent years, the quality requirements for image forming apparatuses such as copiers and printers are strict, and the performance required for toners is also becoming more advanced. In particular, in full-color copiers and full-color printers, there is a strong demand for miniaturization, energy saving, and environmental friendliness, and further improvement in storage stability and low-temperature fixability is required. Toners are also required to have better storage stability and low-temperature fixability. To address the above-mentioned problem, for example, Patent Document 1 discloses a method of forming recesses on the surface of a toner core while controlling the location where a shell is formed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-116712 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, it was found that the method of controlling the shell portion by forming recesses in the toner core does not allow sufficient control of the formation of the shell layer in the recesses, and results in more shell layer than necessary being formed in the recesses, resulting in issues with fixability. The present disclosure provides a method for producing a toner having excellent fixability and storage stability by forming a shell that does not impair fixability. [Means for solving the problem]
[0005] A method for producing a toner having toner particles containing a core particle and a shell layer covering a surface of the core particle, comprising the steps of: The core particles are made of a polyester resin. and wax Contains The production method comprises the steps of: a step of melt-kneading a mixture containing the polyester resin and the wax to obtain a molten kneaded product; pulverizing the molten mixture to obtain the core particles; A step of covering the surfaces of the core particles with the shell layer in an aqueous medium. and, having the coating step includes a temperature increasing step of increasing the temperature of the aqueous medium containing the core particles and the material for forming the shell layer to 58.0° C. or higher, The pH of the aqueous medium at the end of the temperature increasing step is 6.60 or more; The coating step includes a cooling step of cooling the aqueous medium to 42.0°C or less using a heat exchanger after the heating step. fruit, In the cooling step, the cooling rate when cooling the aqueous medium is 2.00° C. / sec or more. A method for producing a toner comprising the steps of: Effect of the Invention
[0006] According to the present disclosure, a method for producing a toner having excellent fixability and storage stability can be provided by forming a shell that does not impair fixability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The expressions "XX to YY" or "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified.
[0008] The present disclosure relates to a method for producing a toner having toner particles containing a core particle and a shell layer covering a surface of the core particle, the method comprising the steps of: The core particles contain a polyester resin, The production method includes a coating step of covering the surfaces of the core particles with the shell layer in an aqueous medium, the coating step includes a temperature increasing step of increasing the temperature of the aqueous medium containing the core particles and the material for forming the shell layer to 58.0° C. or higher, The pH of the aqueous medium at the end of the temperature increasing step is 6.60 or more; The coating step relates to a method for producing a toner, which includes a cooling step of cooling the aqueous medium to 42.0° C. or lower using a heat exchanger after the temperature increasing step.
[0009] The present inventors consider the reason why the above-mentioned effects are exhibited as follows. In the production of toner particles having a core particle and a shell layer covering the surface of the core particle, the core particle contains a polyester resin, and hydrolysis of the polyester resin occurs under specific conditions. As the hydrolysis proceeds, recesses are formed on the surface of the core particle. Furthermore, the hydrolyzate generated by the hydrolysis remains in the recesses formed on the surface of the core particle. When the coating process for coating the surface of the core particles with a shell layer is carried out in an aqueous medium, the presence of the hydrolyzate of the polyester resin on the surface of the core particles makes it difficult for a shell layer to be formed at the location where the hydrolyzate is present. As the core particles are not coated with an excessive shell layer, a toner having both improved storage stability and fixability can be obtained.
[0010] The coating step includes a temperature increasing step in which the temperature of the aqueous medium containing the core particles and the material for forming the shell layer is increased to 58.0° C. or higher. When the temperature of the aqueous medium reaches 58.0° C. or higher in the temperature increasing step, hydrolysis of the polyester resin progresses, and a hydrolyzate that enables good shell layer formation is generated. The pH of the aqueous medium at the end of the temperature increasing step is set to 6.60 or more. By controlling the pH in this way, the hydrolysis of the polyester resin progresses, and a hydrolysate capable of forming a good shell layer is generated.
[0011] After the temperature raising step, the aqueous medium is cooled to 42.0°C or less using a heat exchanger. By cooling the aqueous medium using a heat exchanger, the concentration of the aqueous medium does not decrease, and the hydrolysate remains in the recesses on the surface of the core particles. When cold water mixing or the like is used as a cooling method, the concentration of the aqueous medium decreases, and the hydrolysate that inhibits the formation of a shell layer is removed from the recesses on the surface of the core particles, so that an excessive shell layer is formed in the recesses on the surface of the core particles. In addition, although the reason is not clear, by cooling the temperature of the aqueous medium to 42.0° C. or lower, the hydrolyzate is more likely to remain in the recesses on the surface of the core particles.
[0012] The polyester resin preferably contains a crystalline polyester resin, which is more easily hydrolyzed than an amorphous polyester resin and therefore more likely to exhibit the above-mentioned effects. A crystalline resin is a resin that has a clear endothermic peak in differential scanning calorimetry (DSC). The content of the crystalline polyester resin in the core particles is preferably 1.50% by mass or more and 21.00% by mass or less, and more preferably 2.00% by mass or more and 20.00% by mass or less. When the content is in the above range, the fixing property and storage stability are good.
[0013] In the cooling step, the cooling rate of the aqueous medium is preferably 1.50° C. / sec or more, more preferably 2.00° C. / sec or more. When the cooling rate is 1.50° C. / sec or more, the hydrolyzate is more likely to remain on the core particle surface. There is no particular upper limit, but it is preferably 30.00° C. / sec or less, more preferably 15.00° C. / sec or less.
[0014] The core particles contain a polyester resin. The polyester resin preferably contains a crystalline polyester resin, and more preferably contains a crystalline polyester resin and an amorphous polyester resin. The content of the amorphous polyester resin in the core particles is preferably from 50.00% by mass to 90.00% by mass, and more preferably from 60.00% by mass to 85.00% by mass. In addition to the polyester resin, the core particles may contain other resins to the extent that the above-mentioned effects are not impaired. For example, known resins used as binder resins for toners can be used. Specific examples include resins such as styrene-based resins, acrylic-based resins, styrene-acrylic-based resins, polyethylene-based resins, polypropylene-based resins, vinyl chloride-based resins, polyamide-based resins, polyurethane-based resins, polyvinyl alcohol-based resins, vinyl ether-based resins, N-vinyl-based resins, and styrene-butadiene-based resins. Among these resins, styrene-acrylic resins are preferred from the standpoint of dispersibility of the colorant in the toner, the chargeability of the toner, and fixability to paper. The styrene-acrylic resin and polyester resin will be described below.
[0015] Styrene-acrylic resins are copolymers of styrene-based monomers and acrylic-based monomers. Specific examples of styrene-based monomers include styrene, α-methylstyrene, p-hydroxystyrene, m-hydroxystyrene, vinyltoluene, α-chlorostyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, and p-ethylstyrene. Specific examples of acrylic monomers include (meth)acrylic acid; (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; and (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxypropyl (meth)acrylate.
[0016] The polyester resin can be obtained by polycondensation or copolycondensation of a divalent or trivalent or higher alcohol and a divalent or trivalent or higher carboxylic acid. The following alcohols and carboxylic acids can be used as materials for synthesizing the polyester resin. Specific examples of alcohols used in synthesizing the polyester resin include diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; bisphenol A, hydrogenated bisphenol A, polyoxyethylene bisphenols such as polyoxypropylene-substituted bisphenol A, or polyoxypropylene-substituted bisphenol A; and trihydric or higher alcohols such as sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, diglycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, or 1,3,5-trihydroxymethylbenzene.
[0017] Specific examples of carboxylic acids used in synthesizing polyester resins include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, cyclohexanedicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, alkyl succinic acid (more specifically, n-butyl succinic acid, isobutyl dibasic carboxylic acids such as succinic acid, n-octyl succinic acid, n-dodecyl succinic acid, or isododecyl succinic acid, or alkenyl succinic acid (more specifically, n-butenyl succinic acid, isobutenyl succinic acid, n-octenyl succinic acid, n-dodecenyl succinic acid, or isododecenyl succinic acid); 1,2,4-benzenetricarboxylic acid (trimellitic acid), 1,2,5-benzenetricarboxylic acid, 2,5,7-naphthalene tricarboxylic acid Examples of such carboxylic acids include tricarboxylic acids having a valence of 3 or more, such as carboxylic acid, 1,2,4-naphthalene tricarboxylic acid, 1,2,4-butane tricarboxylic acid, 1,2,5-hexane tricarboxylic acid, 1,3-dicarboxy-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexane tricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octane tetracarboxylic acid, pyromellitic acid, and empol trimer acid. These di- or tri- or higher carboxylic acids may be used in the form of ester-forming derivatives such as acid halides, acid anhydrides, or lower alkyl esters, where "lower alkyl" means an alkyl group having 1 to 6 carbon atoms.
[0018] When producing a crystalline polyester resin or an amorphous polyester resin, the resin may be synthesized by appropriately selecting monomers from the above-mentioned known alcohols and carboxylic acids. In the case of a crystalline polyester resin, it is preferable to select an alcohol and a carboxylic acid from aliphatic dicarboxylic acids having 2 to 20 carbon atoms (preferably 4 to 16) and aliphatic diols having 2 to 20 carbon atoms (preferably 4 to 16).
[0019] [Coloring agent] The toner particles preferably contain a colorant. Examples of black colorants include carbon black, and a mixture of a yellow colorant, a magenta colorant, and a cyan colorant toned to black. As the colorant, a pigment may be used alone, but it is more preferable to use a dye and a pigment in combination to improve the clarity of the colorant from the viewpoint of the image quality of a full-color image. Magenta colored pigments include: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35. Magenta coloring dyes include: CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1, and other solvent dyes; CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28, and other basic dyes.
[0020] Cyan coloring pigments include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45, copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton. Cyan coloring dyes include CI Solvent Blue 70. Yellow coloring pigments include the following: CI Pigment Yellow 1 , 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185;CI Bat Yellow 1, 3, 20. Yellow coloring dyes include CI Solvent Yellow 162. The content of the colorant in the core particles is preferably from 0.1% by mass to 30.0% by mass, and more preferably from 0.5% by mass to 10.0% by mass.
[0021] [wax] The toner particles preferably contain a wax. The wax is not particularly limited, but examples thereof include the following. Hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes whose main component is fatty acid esters such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax. Further examples include the following: saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, hexamethylene biphenyl amide, ethylene bisstearic acid amide, ethylene bisstearic acid amide, ethylene bisstearic acid amide, hexamethylene biphenyl ... Saturated fatty acid bisamides such as stearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N' dioleyl adipic acid amide, and N,N' dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearyl isophthalic acid amide; fatty acid metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols, such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.
[0022] Among these waxes, from the viewpoint of improving low-temperature fixing property and anti-wrapping property after fixing, hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax, and ester wax are preferred. The ester wax is preferably a saturated fatty acid monoester such as stearyl stearate or behenyl behenate. The content of the wax in the core particles is preferably from 0.5% by mass to 25.0% by mass, and more preferably from 2.0% by mass to 15.0% by mass. From the viewpoint of achieving both storage stability and high-temperature offset resistance of the toner, it is preferable that the peak temperature of the maximum endothermic peak of the wax existing in the temperature range of 30°C or more and 200°C or less in the endothermic curve during temperature rise measured by a differential scanning calorimeter (DSC) is 50°C or more and 110°C or less.
[0023] [Charge control agent] The toner may contain a charge control agent as required. A known charge control agent can be used. The charge control agent may be added internally or externally to the toner particles. The amount of the charge control agent added is preferably 0.2 parts by mass or more and 10.0 parts by mass or less with respect to 100.0 parts by mass of the resin component of the core particles.
[0024] The toner may be used as a one-component developer. In order to obtain stable images over a long period of time, the toner may be mixed with a magnetic carrier and used as a two-component developer. [Carrier] As the magnetic carrier, the following known magnetic carriers can be used: For example, surface-oxidized iron powder, unoxidized iron powder, metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, and rare earth elements, alloy particles thereof, oxide particles, magnetic materials such as ferrite, and magnetic material-dispersed resin carriers (so-called resin carriers) containing magnetic materials and a binder resin that holds the magnetic materials in a dispersed state.
[0025] [Preparation of toner core particles] The core particles can be produced by a conventional method such as a pulverization method, an emulsion aggregation method, a dissolution suspension method, or a suspension polymerization method. The production method using the pulverization method will be described below. After mixing the polyester resin and, if necessary, optional components such as other resins, colorants, waxes, and charge control agents, the resulting mixture is melt-kneaded, and the resulting melt-kneaded product is then pulverized and classified to obtain core particles having a desired particle size.
[0026] [Shell layer formation method] The formation of the shell layer covering the core particles is carried out in an aqueous medium, for example, by adding a material for forming the shell layer to the aqueous medium containing the core particles. When the core particles are produced in an aqueous medium by a suspension polymerization method or the like, the aqueous medium containing the obtained core particles may be used as it is as a dispersion liquid for forming the shell layer. In the case of a pulverization method, the obtained core particles may be added to an aqueous medium. Methods for dispersing the core particles well in the aqueous medium include a method for mechanically dispersing the core particles in the aqueous medium using a device capable of vigorously stirring the dispersion, and a method for dispersing the core particles in an aqueous medium containing a dispersant. In the method using a dispersant, the core particles are uniformly dispersed in the aqueous medium, making it easy to form a shell layer. As an apparatus capable of vigorously stirring the dispersion, an apparatus such as Hivismix (manufactured by Primix Co., Ltd.) is preferable.
[0027] In the coating step, the surface of the core particles is covered with a shell layer in an aqueous medium. The coating step of forming a shell layer includes a temperature increasing step of increasing the temperature of the aqueous medium containing the core particles and the material for forming the shell layer to 58.0°C or higher. The material for forming the shell layer may be added before, during, or after the temperature increase. It is sufficient that the temperature of the aqueous medium containing the material for forming the shell layer and the core particles can be set to the above temperature. It is preferable to add the material for forming the shell layer to the aqueous medium containing the core particles, and then increase the temperature to the above temperature. By forming the shell layer at a temperature within this range, the formation of the shell layer can be smoothly promoted while coalescence of the formed toner particles can be suppressed. Furthermore, by forming the shell layer at a temperature within this range, hydrolysis of the polyester resin contained in the core particles, which is necessary for controlling the formation of the shell layer, occurs. The temperature in the temperature increasing step is preferably 58.0°C or higher and 85.0°C or lower, and more preferably 60.0°C or higher and 75.0°C or lower. After the temperature is raised to the above temperature in the temperature-raising step (before the cooling step), a holding step may be provided in which the temperature is held for 0.5 to 5 hours (preferably 1 to 3 hours).
[0028] The coating process for forming the shell layer is carried out by setting the pH of the aqueous medium to 6.60 or higher. The pH of the aqueous medium at the end of the process is 6.60 or more. Preferably, the pH in the subsequent holding step is also 6.60 or more. By making the pH of the aqueous medium 6.60 or more, hydrolysis of the polyester resin contained in the core particles occurs, which is necessary for controlling the formation of the shell layer. The pH at the end of the temperature-raising step and / or during the holding step is preferably 6.60 to 9.00, more preferably 6.80 to 8.50, and even more preferably 7.00 to 8.00.
[0029] After the shell layer is formed as described above, i.e., after the temperature increasing step (after the holding step if a holding step is performed), the aqueous medium is cooled to 42.0° C. or lower using a heat exchanger. There are no particular limitations on the heat exchanger, and any known heat exchanger can be used as long as it does not reduce the concentration of the aqueous medium. The heat exchanger is used to cool the aqueous medium without decreasing its concentration. For example, a plate heat exchanger, a fin tube heat exchanger, etc. can be used. The temperature after cooling by the heat exchanger is preferably 20.0°C or more and 42.0°C or less, more preferably 25.0°C or more and 40.0°C or less.
[0030] The material for forming the shell layer is not particularly limited. For example, resin particles or monomers can be used. The material for forming the shell layer is preferably a resin for forming a shell layer, for example, a dispersion of resin particles can be used. In the aqueous medium, the resin particles or monomers are attached to the surfaces of the core particles. Then, at the above-mentioned temperature in the temperature increasing step, the resin particles are fused or the monomers are polymerized and cured to form a shell layer on the surfaces of the core particles. If necessary, a polymerization initiator may be added to the aqueous medium. The material for forming the shell layer may be any of the resins described above for the core particles or monomers thereof.
[0031] The resin forming the shell layer is preferably a styrene-acrylic resin, more preferably a styrene-(meth)acrylic acid alkyl ester copolymer (the number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 2 to 6). These resins forming the shell layer may be crosslinked with a crosslinking agent. The amount of the material forming the shell layer added is preferably 0.1 to 5.0 parts by mass, and more preferably 0.5 to 2.0 parts by mass, relative to 100 parts by mass of the core particles.
[0032] The dispersion liquid containing the core particles covered with the shell layer is cooled to room temperature to obtain a dispersion liquid of toner particles. Thereafter, if necessary, a washing step for washing the toner particles and a drying step for drying the toner particles are performed to obtain toner particles.
[0033] The toner particles may be used as they are as a toner, or may be used as a toner after an external additive is attached to the surface of the toner particles, if necessary. A preferred method is to mix the toner particles and the external additives using a mixer such as an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) while adjusting the conditions so that the external additives are not embedded in the surfaces of the toner particles.
[0034] The methods for measuring various physical properties will be described below. <Method of measuring the volume-based median diameter (Dv50) and number-based median diameter (Dn50) of toner particles (or core particles)> The volume-based median diameter (Dv50) and number-based median diameter (Dn50) of the toner particles (or core particles) are calculated as follows. The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000. The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1 mass %, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm.
[0035] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) About 30 mL of the electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees and an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add approximately 2 mL of Contaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner particles are added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolyte solution (5) in which the toner particles are dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software provided with the device, and the volume-based median diameter (Dv50) and number-based median diameter (Dn50) are calculated. The closer the ratio of Dv50 to Dn50 (Dv50 / Dn50) is to 1.00, the sharper the particle size distribution. EXAMPLES
[0036] The present invention will now be described in more detail with reference to the following examples. The number of parts in the examples and comparative examples is by weight unless otherwise specified.
[0037] <Production of amorphous polyester resin> Into a reaction vessel equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dehydration tube, and a pressure reducing device, 80.0 parts of terephthalic acid, 16.4 parts of trimellitic anhydride, 123.3 parts of bisphenol A, and 14.1 parts of ethylene glycol were added and heated to a temperature of 130°C with stirring. After adding 0.5 parts of titanium (IV) isopropoxide as an esterification catalyst, the temperature was raised to 160° C. and polycondensation was carried out over 5 hours. Thereafter, the temperature was raised to 180° C. and the reaction was carried out under reduced pressure to obtain an amorphous polyester resin.
[0038] <Production of Crystalline Polyester Resin> 34.5 parts of 1,6-hexanediol, 65.5 parts of dodecanedioic acid, and 0.5 parts of tin 2-ethylhexanoate were added to a reaction tank equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple, and the atmosphere in the flask was replaced with nitrogen gas. The temperature was then gradually increased with stirring, and the mixture was reacted for 3 hours with stirring at a temperature of 140°C. Next, the pressure in the reaction vessel was reduced to 8.3 kPa, and the reaction was carried out for 4 hours while maintaining the temperature at 200° C. Thereafter, the pressure in the reaction vessel was reduced again to 5 kPa or less, and the reaction was carried out at 200° C. for 3 hours, thereby obtaining a crystalline polyester resin.
[0039] <Production of styrene-acrylic resin> Into a reaction vessel equipped with a stirrer, a thermometer, and a nitrogen inlet tube, 80.0 parts of styrene, 20.0 parts of n-butyl acrylate, and 0.3 parts of hexanediol diacrylate were added and heated to a temperature of 80° C. with stirring. Subsequently, 2.0 parts of Perbutyl O (10-hour half-life temperature 72.1° C. (manufactured by Nippon Oil & Fats)) was added as a polymerization initiator, and polymerization was continued for 5 hours to obtain a styrene-acrylic resin as a resin for core particles.
[0040] <Production of shell resin> 79.6 parts of styrene, 19.5 parts of n-butyl acrylate, and 0.9 parts of ethylene glycol dimethacrylate were added to an aqueous solution of 3.0 parts of a surfactant, Neogen RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), dissolved in 50 parts of ion-exchanged water, and dispersed. An aqueous solution of 0.3 parts of potassium persulfate dissolved in 10 parts of ion-exchanged water was added while slowly stirring for 10 minutes. After nitrogen replacement, emulsion polymerization was carried out at 70°C for 6 hours. After the polymerization was completed, the reaction liquid was cooled to room temperature, and ion-exchanged water was added to obtain an aqueous dispersion of the shell resin with a solid content concentration of 50.0% by mass.
[0041] (Production of Core Particle 1) Amorphous polyester resin: 72.30 parts Crystalline polyester resin: 10.00 parts CI Pigment Blue 15:3 (copper phthalocyanine): 4.00 parts Ester wax (behenyl behenate: melting point 72°C) 12.10 parts Fischer-Tropsch wax (Sasol C105, melting point: 105°C): 1.60 copies The above materials were premixed in a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then melt-kneaded using a twin-screw extruder (product name: PCM-30, manufactured by Ikegai Iron Works Co., Ltd.) with the temperature set so that the molten temperature at the discharge outlet was 140°C. The kneaded product thus obtained was cooled, coarsely pulverized with a hammer mill, and then finely pulverized with a pulverizer (product name: Turbo Mill T250, manufactured by Turbo Kogyo Co., Ltd.). The finely pulverized powder thus obtained was classified with a multi-division classifier utilizing the Coanda effect to obtain a volume-based median diameter (Dv50) of 6.8. Core particles 1 of 1 μm were obtained.
[0042] (Production of Core Particles 2 to 8) Core particles 2 to 8 were obtained by the same production method as for core particle 1, except that the conditions were changed as shown in Table 1.
[0043] [Table 1]
[0044] Example 1 1.8 parts of calcium phosphate was added to 250.0 parts of ion-exchanged water heated to 40° C., and the mixture was stirred at a stirring speed of 15,000 rpm using a Hibismix (manufactured by Primix Corporation) to prepare an aqueous medium. 100.0 parts of core particles 1 were added to the aqueous medium to prepare a slurry of core particles 1. Then, 2.0 parts of an aqueous dispersion of a shell resin with a solid content concentration of 50.0% by mass was added to add 1.0 part of shell resin to 100.0 parts of core particles 1. The pH of the aqueous medium was then adjusted to 7.50, and the temperature was raised to 70.0°C and maintained for 2 hours to form a shell layer on the surface of the core particles. The pH after the temperature rise was also 7.50. The aqueous medium was then passed through a plate-type heat exchanger and cooled to 30.0°C at a rate of 10.00°C / sec. After cooling, hydrochloric acid was added to dissolve the calcium phosphate dispersant, and the mixture was filtered, washed with water, and dried to obtain toner particles 1 having a core-shell structure and a volume-based median diameter (Dv50) of 6.8 μm. 100.0 parts of toner particles 1 and 1.5 parts of dry silica particles ("AEROSIL (registered trademark) REA90" manufactured by Nippon Aerosil Co., Ltd.: positively charged hydrophobically treated silica particles) were mixed for 3 minutes using an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) to adhere the silica particles to the toner particles 1. Thereafter, the mixture was sieved through a 300 mesh (mesh opening: 48 μm) to obtain toner 1.
[0045] <Examples 2 to 12 and Comparative Examples 1, 3 to 5> Toners 2 to 13 and 15 to 17 were obtained in the same production method as for Toner 1, except that the conditions were changed as shown in Table 2. Incidentally, Example 3 was evaluated as a reference example.
[0046] [Table 2] In the table, the aqueous medium pH indicates the pH after the temperature was raised.
[0047] Comparative Example 2 1.8 parts of calcium phosphate was added to 250.0 parts of ion-exchanged water heated to 40° C., and the mixture was stirred at a stirring speed of 15,000 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare an aqueous medium. 100.0 parts of core particles 1 were added to an aqueous medium to prepare a slurry of core particles 1. Next, 2.0 parts of an aqueous dispersion of a shell resin with a solid content concentration of 50.0% by mass was added to add 1.0 part of shell resin to 100.0 parts of core particles 1. The pH of the aqueous medium was then adjusted to 7.50, and the temperature was raised to 70.0°C and maintained for 2 hours to form a shell layer on the surface of the core particles. Thereafter, cold water was mixed into the aqueous medium and cooled to 30.0° C. at a rate of 10.00° C. / sec. After cooling, hydrochloric acid was added to dissolve the calcium phosphate dispersant, and the mixture was filtered, washed with water, and dried to obtain toner particles 14 having a core-shell structure and a volume-based median diameter (Dv50) of 6.8 μm. 100.0 parts of toner particles 14 and 1.5 parts of dry silica particles ("AEROSIL (registered trademark) REA90" manufactured by Nippon Aerosil Co., Ltd.: positively charged hydrophobically treated silica particles) were mixed for 3 minutes using an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) to adhere the silica particles to the toner particles 14. Thereafter, the mixture was sieved through a 300 mesh (mesh opening: 48 μm) to obtain toner 14.
[0048] <Image evaluation> The image evaluation was performed on a commercially available color laser printer ("FS-C5250DN" manufactured by Kyocera Document Solutions Inc.) that was partially modified so that it could operate with only one color process cartridge installed. In addition, the printer was modified so that the fixing unit temperature could be changed to any desired value. The two-component developer prepared according to the following method was placed in the developing section of the evaluation machine, and the toner was The toner was then placed in a toner container and the following image evaluation was performed.
[0049] [Preparation of Two-Component Developer] A two-component developer was prepared by mixing 100 parts of the developer carrier (carrier for FS-C5250DN) and 10 parts of each toner to be evaluated for 30 minutes using a ball mill. The specific image evaluation items are as follows:
[0050] [Fixability Rank] Solid image on transfer material (toner load: 0.9 mg / cm 2 ) were printed at different fixing temperatures and evaluated according to the following criteria. The fixing temperature was measured on the surface of the fixing roller using a non-contact thermometer. The transfer material was LETTER size plain paper (XEROX 4200, manufactured by XEROX, 75 g / m 2 ) was used. (Evaluation Criteria) A: No offset at 140℃ B: Offset occurred at 140℃ but not at 150℃ C: Offset occurs at 150℃
[0051] [Blocking (storage rank)] 5 g of each toner was placed in a 50 ml resin cup, and left to stand for 3 days at a temperature of 60° C. and a humidity of 10% RH. The presence or absence of aggregates was examined and evaluated according to the following criteria. (Evaluation Criteria) A: No clumps formed B: Slight clumps formed, crumbles when lightly pressed with fingers C: Agglomerates form, but do not crumble when lightly pressed with fingers
[0052] [Table 3] The fixing temperature indicates the lowest temperature at which offset does not occur.
Claims
1. A method for producing a toner having toner particles containing a core particle and a shell layer covering a surface of the core particle, comprising the steps of: The core particles contain a polyester resin and a wax, The production method comprises the steps of: a step of melt-kneading a mixture containing the polyester resin and the wax to obtain a molten kneaded product; pulverizing the molten mixture to obtain the core particles; a coating step of covering the surfaces of the core particles with the shell layer in an aqueous medium; having The coating step includes a temperature increasing step of increasing the temperature of the aqueous medium containing the core particles and the material for forming the shell layer to 58.0° C. or higher, The pH of the aqueous medium at the end of the temperature increasing step is 6.60 or more; The coating step includes a cooling step of cooling the aqueous medium to 42.0° C. or less using a heat exchanger after the heating step, The method for producing a toner, wherein in the cooling step, the aqueous medium is cooled at a cooling rate of 2.00° C. / second or more.
2. The method for producing a toner according to claim 1 , wherein the polyester resin comprises a crystalline polyester resin.
3. The method for producing a toner according to claim 2 , wherein the content of the crystalline polyester resin in the core particles is from 1.50% by mass to 21.00% by mass.
4. 4. The method for producing a toner according to claim 1, further comprising a holding step of holding the toner at the temperature raised in the temperature raising step for 0.5 hour to 5 hours.
5. 5. The method for producing a toner according to claim 1, wherein the polyester resin comprises a crystalline polyester resin and an amorphous polyester resin.
6. The content of the amorphous polyester resin in the core particles is 50.00% by mass or more and 90.00% by mass or more. The method for producing a toner according to claim 5, wherein the content of the toner is 0.00% by mass or less.
Citation Information
Patent Citations
Toner for electrostatic latent image development and manufacturing method of the same
JP2017116712A
Toner
JP2017201395A
Toner for electrostatic latent image development
JP2019138934A