toner

The toner formulation addresses low-temperature fixability and uniform image density issues by controlling storage modulus and area ratios, ensuring effective adhesion and spreading, thus enhancing performance in high-speed image forming.

JP7562342B2Active Publication Date: 2024-10-07CANON KK
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020150549
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-13
Filing Date
2020-09-08
Publication Date
2024-10-07
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

Existing toners face challenges in achieving low-temperature fixability while maintaining uniform solid image density, especially in high-speed image forming apparatuses, due to issues with viscosity and external stress, leading to uneven density and durability problems.

Method used

A toner formulation with specific storage modulus and area ratio parameters, controlled through the composition of binder resin, crystalline polyester, and wax, ensuring rapid melting and uniform spreading on paper surfaces.

Benefits of technology

The toner achieves good low-temperature fixability and suppresses unevenness in solid image density, even in high-speed machines, by optimizing the toner's viscosity and adhesion properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562342000001
    Figure 0007562342000001
  • Figure 0007562342000002
    Figure 0007562342000002
  • Figure 0007562342000003
    Figure 0007562342000003
Patent Text Reader

Abstract

To provide a toner excellent in low-temperature fixability even in a high-speed machine and capable of suppressing the unevenness of solid image density.SOLUTION: The toner includes toner particles containing binder resin. In a temperature T-storage modulus G' curve obtained by measuring the toner by a rheometer, a storage modulus G'(80°C) at 80°C is 2.0×103 Pa or more and 2.0×105 Pa or less, and the local minimum of a variation (dG' / dT) of a storage-modulus G' in a range of 60-80°C to a temperature T is -1.0x106 or less. When the toner is heated, when setting the projected area of the toner at 80°C to S1 (μm2), the radius of the projected area of the toner at 80°C to R1 (μm) and the projected area of the toner at 120°C to S2 (μm2), S1, R1 and S2 satisfy the following formula (1), (1) S2 / S1×1 / R1≤0.22.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in an image forming method for visualizing electrostatic images, such as electrophotography. [Background technology]

[0002] Image forming apparatuses using electrophotography are in high demand for energy saving, and there is a demand for improved low-temperature fixing properties of toner. Generally, low-temperature fixing properties are related to the viscosity of toner, and toner whose viscosity is quickly reduced by heat during fixing is required. However, toners that satisfy such low-temperature fixing properties are vulnerable to external stresses such as stirring in the developing device and temperature rise of the main body, and are prone to problems such as reduced durability and reduced storage stability due to the inclusion of external additives. In recent years, in addition to energy saving, there is also a strong demand for faster equipment. When a full-page solid image is output with a high-speed image forming device, there is a problem of uneven density caused by differences in the melting degree of the toner due to the unevenness of the paper surface. This phenomenon is likely to occur with toner with low viscosity, and it is very difficult to achieve both energy saving and high speed due to the high technical hurdles. Patent Document 1 describes a toner in which the storage modulus G' at 80° C. to 140° C. is controlled in order to improve low-temperature fixing properties and offset resistance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-167602 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, it has been found that the toner with the storage modulus G' controlled as described in the above document has a certain effect on low-temperature fixing property, but generates uneven density of solid images in a high-speed image forming apparatus. Therefore, there is room for improvement in the uneven density of solid images. The present invention provides a toner which overcomes the above problems. That is, the present invention provides a toner that has good low-temperature fixing properties even in high-speed machines and can suppress uneven density of solid images. [Means for solving the problem]

[0005] As a result of extensive investigations, the inventors have found that the above requirements can be satisfied by adopting the following configuration, and have arrived at the present invention. That is, the present invention provides a toner having toner particles containing a binder resin, In the measurement of the toner using a rotating plate type rheometer, the temperature T (°C) vs. storage modulus G' (Pa) curve obtained when the temperature is increased at a rate of 2.0°C / min is as follows: (i) The storage modulus G'(80°C) at 80°C is 2.0×10 3 Pa or more 2.0×10 5 Pa or less, (ii) The minimum value of the change in storage modulus G' with respect to temperature T (dG' / dT) in the range from 60°C to 80°C is -1.0×10 6 is as follows: When the toner is heated from 25°C to 120°C at a heating rate of 10°C / min, the projected area of ​​the toner at 80°C is S1 (μm 2 ), the radius of the projected area of ​​the toner at 80° C. is R1 (μm), and the projected area of ​​the toner at 120° C. is S2 (μm 2 ), The toner, wherein S1, R1 and S2 satisfy the following formula (1): (1) S2 / S1×1 / R1≦0.22 Effect of the Invention

[0006] According to the present invention, it is possible to provide a toner that has good low-temperature fixing properties even in high-speed machines and can suppress density unevenness in solid images. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The expressions "XX or more and YY or less" or "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. When numerical ranges are stated in stages, the upper and lower limits of each numerical range can be combined in any way. To achieve good low-temperature fixing properties, it is necessary to melt the toner quickly in the short time it takes to pass through the fixing nip. A commonly known method for melting the toner quickly is to control the melting properties of the resin components in the toner. In recent years, various methods have been investigated that use fixing aids (additives such as low-melting wax and crystalline resins) to control the melting properties of the resin components through their plasticizing effect. Therefore, from the viewpoint of improving low-temperature fixing ability, we evaluated toners to which crystalline polyester was added, and found that although there was a certain effect on low-temperature fixing ability, it caused uneven density of solid images under high-speed printing conditions assumed for the next generation. Therefore, to meet the future demands for energy saving and high speed, it is necessary to study toners that can suppress uneven density of solid images by preventing the toner from spreading too much on the convex parts of the paper even if the viscosity of the toner is reduced when passing through the fixing nip.

[0008] As a result of the inventors' investigations into solving the trade-off between improving low-temperature fixing ability and suppressing density unevenness in solid images, they came to the conclusion that the above problem can be solved by using a toner having the characteristics described below. That is, the present invention is A toner having toner particles containing a binder resin, In the measurement of the toner using a rotating plate type rheometer, the temperature T (°C) vs. storage modulus G' (Pa) curve obtained when the temperature is increased at a rate of 2.0°C / min is as follows: (i) The storage modulus G'(80°C) at 80°C is 2.0×10 3 Pa or more 2.0×105 Pa or less, (ii) The minimum value of the change in storage modulus G' with respect to temperature T (dG' / dT) in the range from 60°C to 80°C is -1.0×10 6 is as follows: When the toner is heated from 25°C to 120°C at a heating rate of 10°C / min, the projected area of ​​the toner at 80°C is S1 (μm 2 ), the radius of the projected area of ​​the toner at 80° C. is R1 (μm), and the projected area of ​​the toner at 120° C. is S2 (μm 2 ), The S1, R1 and S2 are characterized in that they satisfy the following formula (1). (1) S2 / S1×1 / R1≦0.22

[0009] The toner will be specifically described below. In the measurement of the toner using a rotating plate type rheometer, the temperature T (℃)-storage modulus G' (Pa) curve obtained when the temperature was increased at 2.0℃ / min showed that the storage modulus G' (80℃) at 80℃ was 2.0×10 3 Pa or more 2.0×10 5 It is necessary that the pressure is less than or equal to Pa. In addition, the storage modulus G' (80°C) is set to 2.0×10 3 Pa or more 1.5×10 5 Pa or less is preferable, and 2.0×10 3 Pa or more 1.0×10 5 Pa or less is more preferable.

[0010] Usually, there are countless concaves and convexes on the surface of paper, and the concaves tend to receive less heat and pressure than the convex parts when passing through the fixing nip. Therefore, the toner on the concaves does not melt as easily as the toner on the convex parts. As a result of extensive research by the present inventors, it was found that the storage modulus G'(80° C.) of the toner at 80° C. corresponds to the degree of melting of the toner in the recesses on the paper. The storage modulus G' is an index that represents the elasticity of a polymer, that is, the reversible property against stress. The storage modulus G' of a toner represents the force with which the toner returns to its original state when it is deformed by heat and pressure in the fixing nip. In other words, it indicates whether the molecules that make up the toner have spring-like properties, and the smaller the value, the softer the toner is, indicating that it has good low-temperature fixing properties.

[0011] The storage modulus G' (80°C) of the toner is 2.0×10 5 If the pressure is greater than Pa, the toner does not become sufficiently low-viscosity due to the heat it receives in the fixing nip and the residual heat it receives after passing through the fixing nip, resulting in poor fixing, in which the toner peels off from the media surface when the fixed image is rubbed.

[0012] In addition, when images are output under high-speed printing conditions, there are also cases where the printed area is chipped or missing when the media passes through the fixing nip, resulting in poor fixing performance. This is thought to be due to the fact that the time for the toner on the media to pass through the fixing nip decreases as the machine speed increases. Toner that is not melted sufficiently while passing through the fixing nip adheres strongly to the fixing member, which is the heat source, causing the printed portion to be offset. Since this missing or chipped portion of the printed portion occurs the moment the toner passes through the fixing nip, whether or not it occurs is determined solely by the amount of heat the toner receives in the fixing nip. In other words, the melting of the toner due to residual heat after passing through the fixing nip has no effect. As a result of extensive research by the present inventors into how to suppress missing and chipped portions of printed material, they came to the idea that this problem could be solved by adopting the following configuration.

[0013] When the toner was measured using a rotating plate rheometer, the minimum value of the change in storage modulus G' with respect to temperature T (dG' / dT) in the temperature T [℃]-storage modulus G' [Pa] curve obtained when the temperature was raised at 2.0℃ / min was -1.0×10 6 The following is the result. The minimum value of the change (dG' / dT) is −5.0×10 6 The lower limit is not particularly limited, but is preferably −1.0×10 8 More preferably, it is −5.0×10 7 That's all.

[0014] The amount of change (dG' / dT) indicates the slope of the storage modulus G' versus temperature T. In other words, the smaller the value, the more rapidly the toner's viscosity changes, and the toner is more likely to suppress missing or chipped portions in the printed area. The minimum value of the change in the storage modulus G' of the toner with respect to the temperature T (dG' / dT) is -1.0×10 6 If it is larger than 100%, the viscosity of the toner cannot be sufficiently reduced within the short time that the toner passes through the fixing nip, resulting in voids and chipping in the printed portion.

[0015] The storage modulus G' (80°C) of the toner and the minimum value of the change in the storage modulus G' with respect to temperature T (dG' / dT) can be controlled, for example, by changing the composition of the resin component in the toner, the composition of the fixing aid, and further the dispersibility of the materials (fixing aid, colorant, etc.). In addition, they can also be controlled by adjusting the content of inorganic particles contained in the toner.

[0016] In addition, in the temperature T (°C)-storage modulus G' (Pa) curve, the storage modulus G' (120) at 120°C is 2.0 x 10 3 Pa or more 2.0×10 4 Pa or less, and 4.0×10 3 Pa or more 1.0×10 4 It is more preferable that the pressure is 0.1 Pa or less.

[0017] As described above, the convex parts of the paper surface receive more heat than the concave parts when passing through the fixing nip. Therefore, the toner on the convex parts is likely to melt excessively compared to the toner on the concave parts, which tends to cause uneven density in a solid image. As a result of extensive research by the present inventors, it was found that the storage modulus G'(120) of the toner at 120°C corresponds to the degree of melting on the convex parts on paper. By setting the storage modulus G'(120°C) of the toner in the above range, it is possible to suppress unevenness in density of solid images and obtain a toner with good hot offset resistance. The storage modulus G'(120°C) can be controlled, for example, by changing the composition of the resin component in the toner, the composition of the fixing aid, and further the dispersibility of the materials (fixing aid, colorant, etc.). In addition, it can be controlled by adjusting the content of inorganic particles contained in the toner.

[0018] When the toner is heated from 25°C to 120°C at a heating rate of 10°C / min, the projected area of ​​the toner at 80°C is S1 [μm 2 ], the radius of the projected area of ​​the toner at 80°C is R1 [μm], and the projected area of ​​the toner at 120°C is S2 [μm 2 ], S1, R1 and S2 satisfy the following formula (1). (1) S2 / S1×1 / R1≦0.22

[0019] By setting the relationship between S1, S2, and R1 within the above range, it is possible to suppress uneven density of a solid image even during high-speed printing. The reason for this is considered as follows. As mentioned above, the main cause of uneven density in solid images is thought to be uneven toner melting caused by the unevenness of the media. In particular, in the case of commonly used paper, there is a variation of about 30 μm between the concave and convex parts of the paper surface. Normally, the temperature of the fixing unit is set so that the toner on the concave parts, which receives less heat in the fixing nip, can be fixed, so the toner on the convex parts receives an excessive amount of heat in the fixing nip. In machines that support high speeds, the difference in the amount of heat received by the toner on the concave parts and the toner on the convex parts becomes larger, and it was found that there is a difference of about 40°C in the temperature that the toner reaches. Therefore, even in a high-speed machine, in order to suppress uneven density of a solid image, it is required that there is little difference in the area where the toner spreads on the paper even under different temperature conditions. As a result of extensive research by the inventors to achieve such an effect, it was found that it is important to set the wetting spread parameter calculated from formula (1) in the above range.

[0020] The ease with which toner spreads on media can be controlled by the combination of toner materials and toner particle size. However, toner particle size is often limited by the configuration of the main body or cartridge CRG, and cannot be freely selected in many cases. Therefore, we focused on controlling the ease with which toner spreads on media by the combination of toner materials. Specifically, in order to eliminate the factor of toner particle size from the ease with which the toner spreads on the media, we decided to take the product 1 / R1. The reason for this is as follows.

[0021] If we assume that the toner is spherical, the volume of the toner before fixing is proportional to the cube of the radius. On the other hand, the projected area of ​​the toner on the media is proportional to the square of the radius. If we assume that the toner spreads on the media by wetting to a certain thickness, we must take into account the difference between the exponents of volume and area. Therefore, it is believed that the factor of toner particle size can be eliminated by taking the product of 1 / R1 for the rate of change S2 / S1 of the toner's projected area at 80° C. and the projected area at 120° C.

[0022] If S2 / S1×1 / R1 is greater than 0.22, the change in toner area between the convex portion and the concave portion of the paper surface becomes large, resulting in uneven density of the solid image. S2 / S1×1 / R1 is preferably 0.20 or less. On the other hand, the lower limit is not particularly limited, but is preferably 0.12 or more, and more preferably 0.15 or more. The value of S2 / S1×1 / R1 can be controlled by using a binder resin, for example, as described below. It can also be controlled by adjusting the dispersion diameter, melting point, and compatibility with the binder resin of the crystalline material (crystalline resin, wax, etc.).

[0023] In Soxhlet extraction of a toner using ethyl acetate, when the content of ethyl acetate insoluble matter in the toner after extraction for 18 hours is defined as α% by mass, α is preferably 25.0% by mass or more and 55.0% by mass or less, and more preferably 30.0% by mass or more and 50.0% by mass or less.

[0024] Ethyl acetate has an ester group and is highly polar, so it can extract linear components that also have an ester group and are highly polar. On the other hand, even if the components are highly polar, extraction of non-polar components hardly proceeds when the molecules are strongly entangled with each other. That is, the crosslinked structure between the vinyl polymer portion and the amorphous polyester portion, which will be described later, and the crosslinked structure in the amorphous polyester portion, etc. become insoluble in ethyl acetate. Since the linear component soluble in ethyl acetate plasticizes the resin in a high-temperature, high-humidity environment, when the content of the ethyl acetate insoluble matter in the binder resin satisfies the above range, plasticization of the toner is suppressed when used for a long period of time in a high-temperature, high-humidity environment, and durability is improved. The content of the ethyl acetate insoluble matter can be adjusted by changing the monomer composition and production conditions of the binder resin, and the production conditions of the toner.

[0025] Furthermore, in a Soxhlet extraction of a toner using tetrahydrofuran (THF), when the content of tetrahydrofuran insoluble matter in the toner after extraction for 18 hours is defined as β (mass %), β preferably satisfies the following formula (2), more preferably satisfies the following formula (2'), and further preferably satisfies the following formula (2''). (2) 5.0 ≦ β ≦ 30.0 (2') 5.0 ≦ β ≦ 20.0 (2'') 8.0 ≦ β ≦ 20.0

[0026] THF has a furan ring and can elute not only polar linear components, but also strongly entangled polar components and non-polar linear components, making it possible to elute most of the components of the binder resin. That is, the crosslinked structure in the amorphous polyester portion described later becomes the insoluble portion in THF. The insoluble portion in THF is less likely to deform in the temperature range during fixing, and can suppress the toner from deforming excessively when melted, thereby suppressing unevenness in the density of a solid image. In addition, the toner has good durability because it can suppress the embedding of external additives in the toner. The content of the THF insoluble matter can be adjusted by changing the monomer composition and production conditions of the binder resin, and the production conditions of the toner.

[0027] Furthermore, the content α (mass%) of the ethyl acetate insoluble matter and the content β (mass%) of the tetrahydrofuran insoluble matter preferably satisfy the following formula (3), more preferably satisfy the following formula (3'), and further preferably satisfy the following formula (3''). (3) 10.0≦(α-β)≦40.0 (3') 15.0≦(α-β)≦33.0 (3'') 17.0≦(α-β)≦25.0

[0028] As described above, the amount of ethyl acetate insoluble matter may be affected by, for example, the crosslinked structure between the vinyl polymer portion and the amorphous polyester portion, and the crosslinked structure in the amorphous polyester portion. Also, the amount of THF insoluble matter may be affected by the crosslinked structure in the amorphous polyester portion. In other words, (α-β) in formula (3) may be affected by the crosslinked structure between the vinyl polymer portion and the amorphous polyester portion. As will be described later, the crosslinked structure between the vinyl polymer portion and the amorphous polyester portion is Since the distance is short and the mesh is dense, it can be entangled with other raw materials and improve the material dispersion in the toner. As a result, a toner having (α-β) satisfying the above range can suppress density unevenness of a solid image and also suppress fogging.

[0029] It is preferable that the toner contains tetrahydrofuran insoluble matter when the toner is subjected to Soxhlet extraction using tetrahydrofuran for 18 hours. The storage modulus G'(120) at 120°C measured at a temperature rise rate of 2.0°C / min by measurement using a rotating plate type rheometer is 1.0×10 5 Pa or more 1.0×10 7 Pa or less, and 2.0×10 5 Pa or more 5.0×10 6 It is more preferable that the pressure is 0.1 Pa or less. When the storage modulus G'(120) of the THF insoluble matter satisfies the above range, it is possible to suppress unevenness in density of a solid image and to obtain a toner having good durability.

[0030] (Binding resin) The binder resin is not particularly limited and may be a known resin. The binder resin preferably contains a hybrid resin having a vinyl polymer portion and an amorphous polyester portion. The binder resin contains a hybrid resin having an amorphous polyester portion with excellent melting properties and a vinyl polymer portion with excellent charging properties and a high softening point, so that the binder resin has excellent charging stability and low-temperature fixing property while increasing the softening point. As a result, the low-temperature fixing property and the stability of the image density in a high-humidity environment are further improved. The content of the hybrid resin in the binder resin is preferably 50% by mass or more and 100% by mass or less, more preferably 80% by mass or more and 100% by mass or less, and even more preferably 90% by mass or more and 100% by mass or less.

[0031] In the hybrid resin, the vinyl polymer portion and the amorphous polyester portion are preferably hybridized by an ester exchange reaction, which forms a crosslinked structure between the vinyl polymer portion and the amorphous polyester portion, making it easier to control the ethyl acetate insoluble content α% by mass and the THF insoluble content β% by mass. The crosslinked structure has a short distance between crosslinking points and can easily form a relatively small network, so that the storage modulus G' of the crosslinked site can be increased, thereby suppressing uneven density of a solid image.

[0032] In the hybrid resin, the mass ratio of the amorphous polyester segment to the vinyl polymer segment (amorphous polyester segment:vinyl polymer segment) is preferably 50:50 to 98:2, more preferably 70:30 to 97:3, and further preferably 90:10 to 97:3. That is, the content of the amorphous polyester portion in the hybrid resin is preferably 50% by mass or more and 98% by mass or less, more preferably 70% by mass or more and 97% by mass or less, and even more preferably 90% by mass or more and 97% by mass or less. By setting the content in the above range, the hybrid resin can obtain the advantages thereof while exhibiting stable low-temperature fixability regardless of the environment. In addition, the content α% by mass of the ethyl acetate insoluble matter and the content β% by mass of the THF insoluble matter can be easily controlled, and density unevenness of a solid image can be suppressed.

[0033] Examples of monomers constituting the polyester resin or polyester moiety include the following compounds. Examples of the alcohol component include dihydric alcohols such as ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, bisphenols and derivatives thereof represented by the following formula (I), and diols represented by the following formula (II).

[0034] [ka] (In the formula, R represents an ethylene group or a propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 or more and 10 or less.)

[0035] [ka]

[0036] Examples of the acid component include the following divalent carboxylic acids. Benzenedicarboxylic acids or their anhydrides, such as phthalic acid, terephthalic acid, isophthalic acid, and phthalic anhydride; alkyldicarboxylic acids or their anhydrides, such as succinic acid, adipic acid, sebacic acid, and azelaic acid; succinic acid or its anhydride substituted with an alkyl group having 6 to 18 carbon atoms or an alkenyl group having 6 to 18 carbon atoms; unsaturated dicarboxylic acids or their anhydrides, such as fumaric acid, maleic acid, citraconic acid, and itaconic acid.

[0037] The polyester resin or polyester moiety preferably contains a monomer unit derived from a polyhydric alcohol or a monomer unit derived from a polycarboxylic acid. That is, the amorphous polyester moiety preferably has a structure crosslinked with at least one selected from the group consisting of a polyhydric alcohol having a valence of three or more and a polycarboxylic acid having a valence of three or more. This allows a crosslinked structure to be formed in the amorphous polyester moiety, making it easier to control the THF content (β% by mass). The crosslinked structure has a long distance between crosslinking points and is easy to form a relatively large network, so that a three-dimensional network structure can be constructed throughout the binder resin, thereby improving the density unevenness of solid images and the durability and stability of the toner.

[0038] Examples of trivalent or higher polyvalent carboxylic acids include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 1,2,4-cyclohexanetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, pyromellitic acid, and their acid anhydrides or lower alkyl esters. Among the above, aromatic compounds that are highly stable against environmental changes are preferred, such as 1,2,4-benzenetricarboxylic acid and its anhydride. Examples of trihydric or higher polyhydric alcohols include 1,2,3-propanetriol, trimethylolpropane, hexanetriol, and pentaerythritol.

[0039] The binder resin preferably includes a resin composition containing a hybrid resin having a vinyl polymer portion and an amorphous polyester portion, and more preferably a resin composition containing a hybrid resin having a vinyl polymer portion and an amorphous polyester portion. The resin composition comprises: i) at least one of a structure in which a long-chain alkyl monoalcohol having an average carbon number of 27 to 50 is condensed at an end of an amorphous polyester moiety and a structure in which a long-chain alkyl monocarboxylic acid having an average carbon number of 27 to 50 is condensed at an end of an amorphous polyester moiety, and ii) aliphatic hydrocarbons having an average carbon number of 27 to 50; It is preferred that the compound contains By including the resin composition in the binder resin, when a crystalline polyester is added, the crystallization speed of the crystalline polyester is improved, and a toner having good heat-resistant storage stability can be obtained. The content of the resin composition in the binder resin is preferably 50% by mass or more and 100% by mass or less, more preferably 80% by mass or more and 100% by mass or less, and even more preferably 90% by mass or more and 100% by mass or less. The condensed structure of a long-chain alkyl monoalcohol is hereinafter also referred to as an alcohol residue. The condensed structure of a long-chain alkyl monocarboxylic acid is hereinafter also referred to as a carboxylic acid residue. These residues are also referred to as long-chain alkyl components.

[0040] Here, a polyester resin having at least one of the alcohol residues of a long-chain alkyl monoalcohol and the carboxylic acid residue of a long-chain alkyl monocarboxylic acid at its terminal refers to a resin in which these long-chain alkyl components have reacted and been incorporated into the polyester resin, which is the main binder component. On the other hand, the resin composition containing aliphatic hydrocarbons having the above average carbon number means that, for example, the resin composition also contains unmodified components when the long-chain alkyl component is modified with alcohol or acid. The resin composition is meant to have a polyester resin having a long-chain alkyl component incorporated therein, and an aliphatic hydrocarbon component (eg, an unmodified version of the long-chain alkyl component).

[0041] The average carbon number of the long-chain alkyl components is determined by the following method. The carbon number distribution of long-chain alkyl components is measured by gas chromatography (GC) as follows: 10 mg of sample is precisely weighed and placed in a sample bottle. 10 g of precisely weighed hexane is added to the sample bottle, which is then capped and heated to 150°C on a hot plate for mixing. The sample is then quickly injected into the gas chromatograph inlet so as not to precipitate long-chain alkyl components, and analyzed using the following measuring device and conditions: A chart is obtained with the carbon number on the horizontal axis and the signal intensity on the vertical axis. Next, in the obtained chart, the ratio of the peak area of ​​each carbon number component to the total area of ​​all detected peaks is calculated, and this is taken as the abundance ratio (area %) of each hydrocarbon compound. Then, a carbon number distribution chart is created with the carbon number on the horizontal axis and the abundance ratio (area %) of the hydrocarbon compound on the vertical axis. The carbon number at the peak top of the carbon number distribution chart is taken as the average carbon number.

[0042] The measuring device and measuring conditions are as follows. GC: HP 6890GC Column: ULTRA ALLOY-1 P / N: UA1-30m-0.5F (manufactured by Frontier Labs) Carrier gas: He Oven: (1) Hold at 100°C for 5 minutes, (2) Raise temperature to 360°C at 30°C / min, (3) Hold at 360°C for 60 minutes Inlet: Temperature 300℃ Initial pressure: 10.523 psi Split ratio: 50:1 Column flow rate: 1mL / min

[0043] In addition, the total content of aliphatic hydrocarbons having an average carbon number of 27 to 50, structures (alcohol residues) obtained by condensation of long-chain alkyl monoalcohols having an average carbon number of 27 to 50, and structures (carboxylic acid residues) obtained by condensation of long-chain alkyl monocarboxylic acids having an average carbon number of 27 to 50 is preferably 2.5% by mass or more and 10.0% by mass or less, and more preferably 3.5% by mass or more and 7.5% by mass or less. By setting the ratio of the component derived from the long-chain alkyl group within the above range, the crystallization speed of the crystalline polyester becomes easy to control, and a toner having good storage stability can be obtained.

[0044] Moreover, the resin composition preferably has an endothermic peak top temperature of 60.0° C. or higher and 90.0° C. or lower in a temperature-endothermic curve obtained by differential scanning calorimetry (DSC). The endothermic amount (ΔH) of the endothermic peak is preferably 0.10 J / g or more and 1.90 J / g or less, and more preferably 0.20 J / g or more and 1.00 J / g or less.

[0045] In order to achieve both low-temperature fixability of the toner and suppression of uneven density of solid images, it is preferable to uniformly disperse the crystalline polyester in the toner. For this purpose, it is preferable that the component derived from the long-chain alkyl is uniformly dispersed in the binder resin, and it is preferable to optimize the amount of the component that is not bonded to the polyester resin component and is free, that is, the unmodified aliphatic hydrocarbon.

[0046] This unmodified aliphatic hydrocarbon exhibits an endothermic peak in the temperature-endothermic curve obtained by differential scanning calorimetry (DSC). The endothermic heat ΔH observed by DSC being within the above range indicates that there is little free long-chain alkyl component, i.e., it is incorporated into the polyester resin (main binder). Therefore, the present inventors believe that by optimizing the endothermic amount (ΔH) of this endothermic peak, the components derived from the long-chain alkyl group can be more easily dispersed uniformly in the resin composition.

[0047] The peak top temperature and endothermic amount (ΔH) of the endothermic peak are measured by the following method. The peak top temperature and endothermic amount of the endothermic peak in differential scanning calorimetry (DSC) are measured in accordance with ASTM D3418-82 using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the detector of the device, and the heat of fusion of indium is used for heat correction. Specifically, approximately 5 mg of the measurement sample is precisely weighed and placed in an aluminum pan. Using an empty aluminum pan as a reference, measurements are performed at room temperature and humidity with a temperature rise rate of 10°C / min in the measurement temperature range of 30 to 200°C. In the measurement, the temperature is raised to 200°C once, then lowered to 30°C, and then raised again. In the DSC curve (temperature-endothermic amount curve) obtained during this heating process, the peak top temperature of the maximum endothermic peak in the temperature range of 30°C to 200°C is obtained. The endothermic amount ΔH of the endothermic peak is the integral value of the endothermic peak.

[0048] Methods for controlling the amount of liberated long-chain alkyl components, that is, the amount of endothermic peaks in DSC, include a method for increasing the alcohol modification rate or acid modification rate of aliphatic hydrocarbons. That is, when alcohol- or acid-modified long-chain alkyl components react with polyester resins in a polymerization reaction and are incorporated into the polyester resins, no endothermic peak appears in DSC measurements. On the other hand, unmodified aliphatic hydrocarbons do not have reaction sites with polyester resins, so they exist in a free state in the polyester resins, increasing the amount of heat absorbed by DSC.

[0049] Long-chain alkyl monoalcohols with an average carbon number of 27 to 50, and Long-chain alkyl monocarboxylic acids with a value of 27 to 50 can be obtained industrially by modifying aliphatic hydrocarbons as raw materials with alcohol or acid. Aliphatic hydrocarbons include saturated and unsaturated hydrocarbons, and examples thereof include alkanes, alkenes, alkynes, and cyclic hydrocarbons such as cyclohexane, with saturated hydrocarbons (alkanes) being preferred.

[0050] For example, it is known that, with regard to alcohol-denatured products, aliphatic hydrocarbons having a carbon number of 27 to 50 can be converted to alcohols by liquid-phase oxidation with a molecular oxygen-containing gas in the presence of a catalyst such as boric acid, boric anhydride, or metaboric acid. The amount of catalyst used is preferably 0.01 mol to 0.5 mol per mol of the raw aliphatic hydrocarbon. The molecular oxygen-containing gas to be blown into the reaction system can be oxygen, air, or a wide range of gases obtained by diluting these gases with an inert gas, but the oxygen concentration is preferably 3% to 20%. The reaction temperature is preferably 100°C or higher and 200°C or lower. The endothermic heat quantity of DSC can be controlled by optimizing the reaction conditions or by performing a purification operation after the modification reaction to remove unmodified aliphatic hydrocarbon components. The modification rate of the aliphatic hydrocarbon components is preferably 85% or more, more preferably 90% or more. On the other hand, the upper limit is preferably 99% or less.

[0051] The resin composition preferably contains a structure in which a long-chain alkyl monoalcohol having an average carbon number of 27 to 50 is condensed at the terminal, and an aliphatic hydrocarbon having an average carbon number of 27 to 50. The long-chain alkyl monoalcohol preferably contains a secondary alcohol, and more preferably contains a secondary alcohol as the main component. Incidentally, "containing a secondary alcohol as the main component" means that 50% by mass or more of the long-chain alkyl monoalcohol is a secondary alcohol. By using a secondary alcohol as the main component of the long-chain alkyl monoalcohol, the long-chain alkyl component can easily take a folded structure, which suppresses steric hindrance and the like, making it easier for the long-chain alkyl component to exist more uniformly in the resin composition, and improving storage stability.

[0052] The vinyl polymer moiety contained in the hybrid resin contains a monomer unit derived from styrene and a monomer unit derived from an acrylic acid ester and / or a methacrylic acid ester, and the total content of the monomer units derived from an acrylic acid ester and a methacrylic acid ester is preferably 50 mol% or more and 98 mol% or less, more preferably 70 mol% or more and 97 mol% or less, and even more preferably 85 mol% or more and 97 mol% or less, of all the monomer units forming the vinyl polymer moiety. This makes it possible to adjust the density of the cross-linked structure between the vinyl polymer portion and the amorphous polyester portion, making it easier to control the ethyl acetate insoluble content α% by mass and the THF insoluble content β% by mass, thereby suppressing uneven density of solid images.

[0053] Examples of the vinyl monomer constituting the vinyl polymer moiety include the following compounds. Styrene; styrene derivatives such as o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, 3,4-dichlorostyrene, p-ethylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene; unsaturated monoolefins such as ethylene, propylene, butylene, isobutylene; unsaturated polyenes such as butadiene, isoprene; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl bromide, vinyl fluoride; vinyl esters such as vinyl acetate, vinyl propionate, vinyl benzoate; methyl methacrylate, ethyl methacrylate, methacrylate esters such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, n-octyl methacrylate, dodecyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, phenyl methacrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate; methacrylic acid esters such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, propyl acrylate, n-octyl acrylate, dodecyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, vinyl ethers such as vinyl methyl ether, vinyl ethyl ether, vinyl isobutyl ether; vinyl ketones such as vinyl methyl ketone, vinyl hexyl ketone, methyl isopropenyl ketone; N-vinyl compounds such as N-vinylpyrrole, N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone; vinyl naphthalenes; acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile, acrylamide.

[0054] Further examples include the following: unsaturated dibasic acids such as maleic acid, citraconic acid, itaconic acid, alkenylsuccinic acid, fumaric acid, and mesaconic acid; unsaturated dibasic acid anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, and alkenylsuccinic anhydride; methyl maleate half ester, ethyl maleate half ester, butyl maleate half ester, methyl citraconic acid half ester, ethyl citraconic acid half ester, butyl citraconic acid half ester, methyl itaconic acid half ester, methyl alkenylsuccinic acid half ester, fumaric acid, and mesaconic acid. unsaturated dibasic acid esters such as dimethyl maleic acid and dimethyl fumaric acid; α,β-unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid and cinnamic acid; α,β-unsaturated acid anhydrides such as crotonic acid anhydride and cinnamic acid anhydride, anhydrides of the above α,β-unsaturated acids and lower fatty acids; and monomers having a carboxy group such as alkenyl malonic acid, alkenyl glutaric acid, alkenyl adipic acid, acid anhydrides thereof, and monoesters thereof.

[0055] Further examples include acrylic acid or methacrylic acid esters such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate; and monomers having a hydroxy group such as 4-(1-hydroxy-1-methylbutyl)styrene and 4-(1-hydroxy-1-methylhexyl)styrene.

[0056] The vinyl polymer portion preferably has a structure in which at least one selected from the group consisting of an acrylic acid ester and a methacrylic acid ester is polymerized. The vinyl polymer portion preferably has a structure in which at least one selected from the group consisting of an acrylic acid ester and a methacrylic acid ester is polymerized, and a structure in which styrene is polymerized. The total content of structures in which at least one selected from the group consisting of acrylic acid esters and methacrylic acid esters is polymerized in the vinyl polymer portion is preferably 50% by mass or more and 98% by mass or less, and more preferably 70% by mass or more and 98% by mass or less. The binder resin preferably has both a crosslinked structure between the vinyl polymer portion and the amorphous polyester portion and a crosslinked structure in the amorphous polyester portion, which makes it easier to control the storage modulus G' and the wetting and spreading index of the toner within the above ranges.

[0057] (Crystalline polyester resin) The toner particles preferably contain a crystalline polyester resin. Here, the crystalline polyester is defined as a polyester resin that has a clear endothermic peak when measured by a differential scanning calorimeter (DSC). The crystalline polyester resin will now be described.

[0058] The crystalline polyester resin may be a known one, for example, a condensation polymer of an aliphatic dicarboxylic acid and an aliphatic diol. The crystalline polyester resin is preferably a condensation polymer of at least one selected from the group consisting of an aliphatic dicarboxylic acid, an aliphatic diol, an aliphatic monocarboxylic acid, and an aliphatic monoalcohol, and more preferably a condensation polymer of an aliphatic dicarboxylic acid, an aliphatic diol, and an aliphatic monocarboxylic acid.

[0059] The aliphatic dicarboxylic acid may be an aliphatic dicarboxylic acid having 2 to 20 carbon atoms, such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedicarboxylic acid, and octadecanedicarboxylic acid.

[0060] The aliphatic diol may be an aliphatic diol having 2 to 20 carbon atoms, such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, trimethylene glycol, neopentyl glycol, 1,4-butanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,16-hexadecanediol, and 1,18-octadecanediol.

[0061] Examples of the aliphatic monocarboxylic acid include aliphatic monocarboxylic acids having 6 to 20 carbon atoms, such as hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), eicosanoic acid (arachidic acid), docosanoic acid (behenic acid), and tetracosanoic acid (lignoceric acid). The aliphatic monoalcohol may be an aliphatic monoalcohol having a carbon number of 6 to 20. For example, capryl alcohol, undecanol, lauryl alcohol, tridecanol, myristyl alcohol, pentadecanol, palmityl alcohol, margaryl alcohol, stearyl alcohol, nonadecanol, and arachidyl alcohol may be mentioned.

[0062] The crystalline polyester resin is preferably a condensation polymer of an alcohol component containing an aliphatic diol and an acid component containing an aliphatic dicarboxylic acid. When the carbon number of the aliphatic diol is C1 and the carbon number of the aliphatic dicarboxylic acid is C2, the sum of C1 and C2 is preferably 10 to 16, more preferably 12 to 16. When a plurality of aliphatic diols and / or aliphatic dicarboxylic acids are used, the carbon number of each is used as an average value based on mass fraction.

[0063] The sum of C1 and C2 being 10 or more and 16 or less means that the total number of carbon atoms in the aliphatic diol and aliphatic dicarboxylic acid constituting the crystalline polyester resin is relatively small. By reducing the sum of C1 and C2 to the above range, the number of ester groups contained in the crystalline polyester resin increases. The increase in the number of ester groups increases the polarity of the crystalline polyester resin. As a result, the speed at which the binder resin is plasticized becomes very fast, making it easier to achieve the effects of the present invention.

[0064] In addition, it is preferable that the crystalline polyester resin is a condensation polymer of an alcohol component containing an aliphatic diol and an acid component containing an aliphatic dicarboxylic acid, and has at least one of a structure in which an aliphatic monocarboxylic acid is condensed at an end and a structure in which an aliphatic monoalcohol is condensed at an end. And a structure in which an aliphatic monocarboxylic acid is condensed and a structure in which an aliphatic monoalcohol is condensed It is preferable that the carbon number C3 of at least one of the above is 6 or more and 14 or less.

[0065] The melting point of the crystalline polyester resin is preferably from 65° C. to 100° C. The melting point is determined by the combination of the carboxylic acid component and the alcohol component used, and may be appropriately selected so as to be within the above range. The content of the crystalline polyester resin is preferably 5 parts by mass or more and 30 parts by mass or less, more preferably 8 parts by mass or more and 30 parts by mass or less, even more preferably 10 parts by mass or more and 25 parts by mass or less, and still more preferably 10 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0066] The crystalline polyester resin can be produced by a conventional polyester synthesis method, for example, by subjecting an acid component and an alcohol component to an esterification reaction or an ester exchange reaction, followed by a conventional polycondensation reaction under reduced pressure or by introducing nitrogen gas. In the esterification or transesterification reaction, a conventional esterification catalyst or transesterification catalyst such as sulfuric acid, tertiary butyl titanium butoxide, dibutyltin oxide, manganese acetate, magnesium acetate, etc. can be used as necessary. In addition, in the polymerization, a conventional polymerization catalyst such as a known one, for example, tertiary butyl titanium butoxide, dibutyltin oxide, tin acetate, zinc acetate, tin disulfide, antimony trioxide, germanium dioxide, etc. can be used. The polymerization temperature and the amount of catalyst are not particularly limited and may be selected as necessary. The catalyst used is preferably a titanium catalyst, and more preferably a chelate-type titanium catalyst, because the reactivity of the titanium catalyst is appropriate and a polyester having a desired molecular weight distribution can be obtained in the present invention.

[0067] (Coloring agent) The toner may contain a colorant, which may include the following organic pigments, organic dyes, and inorganic pigments. Cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Examples of magenta colorants include the following: condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Examples of black colorants include carbon black, and the above-mentioned yellow colorants, magenta colorants, cyan colorants, and colorants toned black using magnetic powder. These colorants can be used alone or in a mixture or in the form of a solid solution. The colorant used in the present invention is selected in terms of hue angle, chroma, brightness, light resistance, OHP transparency, and dispersibility in toner particles. The content of the colorant is preferably 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0068] (magnetic particles) Magnetic particles may be used as a black colorant. When magnetic particles are used, it is preferable that the magnetic particles have a core particle containing a magnetic iron oxide particle and a coating layer provided on the surface of the core particle. Core particles containing magnetic iron oxide particles include magnetic iron oxides such as magnetite, maghemite, ferrite, and other metal oxides; metal oxides such as Fe, Co, and Ni; Examples of suitable metals include alloys of these metals with metals such as Al, Co, Cu, Pb, Mg, Ni, Sn, Zn, Sb, Be, Bi, Cd, Ca, Mn, Ti, W, and V, and mixtures thereof.

[0069] The coating layer may uniformly cover the entire surface of the core particle, or may cover the surface of the core particle with a part exposed. In either coating mode, the coating layer is preferably the outermost layer, and preferably thinly covers the surface of the core particle. The elements forming the coating layer preferably contain Si and Al. The method for forming the coating layer is not particularly limited, and a known method may be used. For example, after producing core particles containing magnetite, a silicon source or an aluminum source such as sodium silicate or aluminum sulfate is added to an aqueous solution of ferrous sulfate. Then, the pH and temperature of the mixture are adjusted while air is blown in to form a coating layer containing a specific oxide on the surface of the core particles. The thickness of the coating layer can be controlled by adjusting the amounts of the aqueous ferrous sulfate solution, sodium silicate, aluminum sulfate, and the like added.

[0070] From the viewpoints of facilitating the formation of the coating layer described above and improving the magnetic properties and coloring power, the magnetic particles are preferably octahedral. The shape of the magnetic particles can be controlled by a conventional method. One method for forming magnetic particles into an octahedral shape is to set the pH to 9 or higher during the wet oxidation reaction in the production of core particles. From the viewpoint of low-temperature fixability, the content of the magnetic particles is preferably 25 parts by mass or more and 100 parts by mass or less, and more preferably 30 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0071] (Other constituent materials of toner) In order to impart releasability to the toner, the toner particles preferably contain a release agent (wax). Specific examples of waxes include the following: Oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax, or block copolymers thereof; waxes mainly composed of fatty acid esters such as carnauba wax, sazol wax, and montan acid ester wax; partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax; saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; long-chain alkyl alcohols; polyhydric alcohols such as sorbitol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene saturated fatty acid bisamides such as ethylene bislauric acid amide and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipic acid amide and N,N-dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N-distearyl isophthalic acid amide; fatty acid metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxy groups obtained by hydrogenating vegetable oils and fats.

[0072] More specifically, the following may be mentioned: Viscol (registered trademark) 330-P, 550-P, 660-P, TS-200 (Sanyo Chemical Industries, Ltd.); Hiwax 400P, 200P, 100P, 410P, 420P, 320P, 220P, 210P, 110P (Mitsui Chemicals, Inc.); Sasol H1, H2, C80, C105, C77 (Sasol); HNP-1, HNP-3, HNP-9, HNP-10, HNP-11, HNP-12 (Nippon Seiro Co., Ltd.); Unilin (registered trademark) 350, 425, 550, 700, Unicid (registered trademark) 350, 425, 550, 700 (Toyo Petrolite Co., Ltd.); wood wax, beeswax, rice wax, candelilla wax, carnauba wax (Cerarica NODA Co., Ltd.).

[0073] From the viewpoint of low-temperature fixability, the melting point of the wax is preferably 65.0° C. or more and 120.0° C. or less. Furthermore, the difference between the melting point of the wax and the melting point of the crystalline polyester resin is preferably 0° C. or more and 25° C. or less, and more preferably 0° C. or more and 35° C. or less. Compared with the crystalline polyester resin, the wax is more likely to crystallize in the toner particles at room temperature. By making the difference between their melting points closer, the crystallization of the crystalline polyester resin is also promoted along with the crystallization of the wax, making it easier to control the Tg1 below within a specific range.

[0074] In order to stabilize the triboelectric charging property of the toner, the toner may contain a charge control agent. The content of the charge control agent varies depending on the type and the physical properties of other toner constituent materials, but in general, it is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 0.1 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0075] There are known charge control agents that control the toner to be negatively charged and those that control the toner to be positively charged. Depending on the type and application of the toner, one or more of various charge control agents can be used. Examples of the toner that can be controlled to have a negative charge include the following. Organometallic complexes (monoazo metal complexes; acetylacetone metal complexes); metal complexes or metal salts of aromatic hydroxycarboxylic acids or aromatic dicarboxylic acids; aromatic mono- and polycarboxylic acids and their metal salts and anhydrides; esters and phenol derivatives such as bisphenol.

[0076] Examples of the toner that can be controlled to have a positive charge include the following. Nigrosine and modifications with metal salts of fatty acids; quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate, tetrabutylammonium tetrafluoroborate, and their analogues; onium salts such as phosphonium salts and their lake pigments; triphenylmethane dyes and their lake pigments (lake forming agents include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide compounds, etc.); metal salts of higher fatty acids. Among these, nigrosine compounds, quaternary ammonium salts, etc. are preferred.

[0077] A charge control resin can also be used, and can be used in combination with the charge control agent described above. Specific examples of the charge control agent include the following. Spilon Black TRH, T-77, T-95, TN-105 (Hodogaya Chemical Industry Co., Ltd.); BONTRON (registered trademark) S-34, S-44, E-84, E-88 (Orient Chemical Industry Co., Ltd.); TP-302, TP-415 (Hodogaya Chemical Industry Co., Ltd.); BONTRON (registered trademark) N-01, N-04, N-07, P-51 (Orient Chemical Industry Co., Ltd.); Copy Blue PR (Clariant).

[0078] The toner may contain silica fine particles or the like as an external additive in order to improve charging stability, durable developing property, fluidity, and durability. The silica particles have a specific surface area of ​​30m2 as determined by the BET method using nitrogen adsorption. 2 / g or more Preferably, 50m2 / g or more 400m 2 The content of the silica fine particles is preferably from 0.01 to 8.00 parts by mass, and more preferably from 0.10 to 5.00 parts by mass, relative to 100 parts by mass of the toner particles.

[0079] The BET specific surface area of ​​silica microparticles can be calculated, for example, by adsorbing nitrogen gas onto the surface of the silica microparticles using a specific surface area measuring device such as Autosorb 1 (manufactured by Yuasa Ionics), GEMINI 2360 / 2375 (manufactured by Micrometilix), or Tristar 3000 (manufactured by Micrometilix), and using the BET multi-point method. It is also preferred that the silica fine particles are treated, as necessary, with a treating agent such as unmodified silicone varnish, various modified silicone varnishes, unmodified silicone oil, various modified silicone oils, a silane coupling agent, a silane compound having a functional group, or other organosilicon compounds, or with a combination of various treating agents, for the purpose of controlling triboelectric charging.

[0080] Furthermore, other external additives may be added to the toner as necessary. Examples of such external additives include resin fine particles and inorganic fine particles that act as a charge assistant, a conductivity imparting agent, a fluidity imparting agent, a caking inhibitor, a release agent during heat roller fixing, a lubricant, an abrasive, etc. Examples of the lubricant include polyethylene fluoride powder, zinc stearate powder, and polyvinylidene fluoride powder. Examples of the abrasive include cerium oxide powder, silicon carbide powder, and strontium titanate powder, and among these, strontium titanate powder is preferred.

[0081] The toner may be mixed with a carrier to be used as a two-component developer. As the carrier, a carrier such as a normal ferrite or magnetite or a resin-coated carrier can be used. A binder-type carrier in which a magnetic material is dispersed in a resin can also be used.

[0082] Resin-coated carriers are composed of carrier core particles and a coating material, which is a resin that coats the surfaces of the carrier core particles. Examples of resins used in the coating material include styrene-acrylic resins such as styrene-acrylic acid ester copolymers and styrene-methacrylic acid ester copolymers; acrylic resins such as acrylic acid ester copolymers and methacrylic acid ester copolymers; fluorine-containing resins such as polytetrafluoroethylene, monochlorotrifluoroethylene polymers, and polyvinylidene fluoride; silicone resins; polyester resins; polyamide resins; polyvinyl butyral; and aminoacrylate resins. Other examples include ionomer resins and polyphenylene sulfide resins. These resins can be used alone or in combination.

[0083] In the differential scanning calorimeter (DSC) measurement of the toner, (i) The number of cold crystallization peaks in the range of 40° C. to 120° C. during cooling is defined as X, (ii) When the number of endothermic peaks in the range of 40°C to 120°C during the second heating is Y It is preferable that X and Y satisfy the following formulae (7) and (8), more preferably the following formulae (7') and (8'), and further preferably X=1 and Y=2. (7) X ≧ 1 (8) Y ≧ X+1 (7') 2 ≧ X ≧ 1 (8') Y = X + 1

[0084] The above-mentioned constitution improves the crystallization rate of the crystalline polyester resin and improves the heat-resistant storage stability. The reason for this is considered as follows. As described above, it takes a long time for the crystalline polyester resin to crystallize. Generally, the crystalline polyester resin that is not completely crystallized causes a decrease in the glass transition temperature (Tg) of the toner, which tends to deteriorate the heat-resistant storage stability. It is preferable that the toner particles contain a wax that is easily oriented with the crystalline polyester resin. It is believed that the wax can accelerate the crystallization speed of the crystalline polyester resin. It is believed that the fact that X and Y satisfy the above relational formula indicates that the crystalline polyester resin and the wax are oriented.

[0085] The toner particles preferably contain a crystalline polyester resin. In the differential scanning calorimetry of the toner, The temperature is increased from 25°C to 120°C at a rate of 1000°C / sec (first heating step), The temperature is held at 120°C for 100 ms (0.100 s) (high temperature holding process), then cooled to 25°C at a rate of 1000°C / s (cooling process), The temperature is increased to 120°C at a rate of 1000°C / s (second heating process), When the glass transition temperature in the first heating is Tg1 (℃) and the glass transition temperature in the second heating is Tg2 (℃), It is preferable that the following formulas (9) and (10) are satisfied. (9) 65℃≦Tg1≦85℃ (10) 7℃≦Tg1-Tg2≦30℃

[0086] These DSC measurement conditions are equivalent to the heat that the toner receives from the fixing device. Specifically, the temperature and time of the high-temperature holding process were adjusted so that the toner was heated at 120°C for 100 ms. The degree of plasticization of the crystalline polyester resin into the toner when exposed to that heat is indicated by the glass transition temperature Tg2 obtained by measuring the second temperature rise process. That is, a large Tg1-Tg2 indicates that the crystalline polyester resin can sufficiently plasticize the toner even if the heating time is very short.

[0087] Here, in order to reduce heat other than during the high-temperature holding process, the heating rate was set to a very fast 1000°C / sec so that the toner would not be overheated other than during the high-temperature holding process. Furthermore, the cooling rate was also set to a very fast 1000°C / sec so that the plasticization of the crystalline polyester resin into the toner would be close to the state it was in when it passed through the fixing device. This is because the crystalline polyester plasticizes the toner when it is held at 120°C for 100 ms, but if the cooling rate is slow, the crystalline polyester crystallizes during the cooling process. Therefore, the Tg2 obtained in the second heating process is affected by two factors, the plasticization during the high-temperature holding process and the crystallization during the cooling process, and there is a high possibility that the state that is originally intended to be measured cannot be measured.

[0088] The measurement conditions commonly used for conventional measurements, compared to the DSC measurement conditions, are shown below. The temperature is increased from 25°C to 120°C at a rate of 10°C / min (first heating step), Hold the temperature at 120°C for 5 minutes (high temperature holding process), After cooling to 25°C at a rate of 10°C / min (cooling process), The temperature is increased to 120° C. at a rate of 10° C. / min (second temperature increase step). In this measurement, the high-temperature retention process is longer than the conditions in the present invention, so that even if the toner has a composition that does not plasticize the toner quickly enough, the crystalline polyester resin is likely to plasticize the toner sufficiently. On the other hand, in the present invention, it is shown that the crystalline polyester can plasticize the toner even during a very short high temperature holding process.

[0089] Formula (9) indicates that the glass transition temperature Tg1 (°C) of the toner in the first temperature rise process is 65°C or more and 85°C or less. Tg1 is higher than the result obtained for Tg measured at a temperature rise rate of 10°C / min, which is the conventional measurement condition. When Tg1 is 65° C. or more, a toner having good storage stability is obtained. When Tg1 is 85° C. or less, a toner having good low-temperature fixing property is obtained. Tg1 is preferably 70° C. or more and 80° C. or less.

[0090] Formula (10) indicates that the difference between the glass transition temperature Tg2 of the toner in the second temperature increase process and the glass transition temperature Tg1 of the toner in the first temperature increase process is 7° C. or more and 30° C. or less. When formula (10) is satisfied, it indicates that the crystalline polyester resin can plasticize the toner even with a very short high-temperature retention time. This allows the toner to be sufficiently plasticized within the very short time it takes for the media to pass through the fixing device. This results in a toner that can achieve both good low-temperature fixing properties and suppression of uneven density in solid images. Tg1-Tg2 is preferably 10°C or higher and 30°C or lower. Tg1-Tg2 can be controlled, for example, by changing the composition of the resin component in the toner or the composition of the fixing aid. Tg2 is preferably 40°C or higher and 75°C or lower, and more preferably 45°C or higher and 70°C or lower.

[0091] A preferred configuration of the toner is described below. In order to satisfy the formulas (9) and (10), it is preferable that the crystalline polyester resin plasticizes the toner even when the toner is held at a high temperature for a very short period of time. As a means for achieving this, a method of making the crystalline polyester resin compatible with the binder resin of the toner when it is exposed to heat can be mentioned. Specific means include selection of a compound constituting the crystalline polyester resin, selection of a compound constituting the binder resin, bringing the solubility parameter SP value of the crystalline polyester resin and the binder resin closer to each other, improving the dispersibility of the crystalline polyester resin in the toner particles, and improving the crystallinity of the crystalline polyester, etc. By combining these, the formulas (9) and (10) can be satisfied.

[0092] When the toner was measured using a rotating plate rheometer, the temperature T (℃)-storage modulus G' (Pa) curve obtained when the temperature was increased at a rate of 2.0℃ / min showed that the storage modulus was 1.0×10 3 The temperature at which the temperature becomes Pa is T1 (℃), In a DSC curve obtained by differential scanning calorimetry of the toner, when the DSC curve has an endothermic peak in the range of 30°C to 120°C and the peak temperature of the peak on the lowest temperature side of the endothermic peak is T2 (°C), it is preferable that the following formula (11) is satisfied. (11) T1-T2≧40

[0093] Generally, a binder resin (e.g., an amorphous resin) has a glass transition point (Tg). The viscosity of a binder resin that exceeds the Tg gradually decreases, but the rate of decrease in viscosity is slow. On the other hand, a crystalline material (crystalline polyester resin, wax, etc.) has a melting point specific to the material, and when the crystalline material reaches or exceeds the melting point, the viscosity decreases abruptly. This behavior is the same when the toner contains a crystalline material, and if the difference in viscosity between the crystalline material and the binder resin is too large, the crystalline material may separate from the binder resin, causing uneven density in a solid image. In other words, it is preferable for the difference between the melting point of the crystalline material and the temperature at which the toner reaches a certain viscosity to be small. If T1-T2 satisfies the relationship of formula (11), uneven density in a solid image can be suppressed. It is more preferable that T1-T2 is 0 or more and 35 or less.

[0094] (Toner manufacturing method) The method for producing the toner is not particularly limited, and any known production method can be used. Hereinafter, a specific example of a method for producing a toner through a melt-kneading step and a pulverization step will be described, but the method is not limited thereto.

[0095] For example, a binder resin and, if necessary, a crystalline polyester resin, a colorant, a release agent, a charge control agent, and other additives are thoroughly mixed using a mixer such as a Henschel mixer or a ball mill (mixing step), and the resulting mixture is melt-kneaded using a thermal kneader such as a twin-screw kneading extruder, a heating roll, a kneader, or an extruder (melt-kneading step). The resulting molten mixture is cooled and solidified, then pulverized using a pulverizer (pulverization step), and classified using a classifier (classification step) to obtain toner particles. If necessary, the toner particles and an external additive are mixed in a mixer such as a Henschel mixer to obtain a toner.

[0096] Examples of mixers include the following: FM Mixer (Nippon Coke & Engineering Co., Ltd.); Super Mixer (Kawata Corporation); Rebocone (Okawahara Manufacturing Co., Ltd.); Nauta Mixer, Turbulizer, Cyclomix (Hosokawa Micron Corporation); Spiral Pin Mixer (Taiheiyo Kiko Co., Ltd.); and Lödige Mixer (Matsubo Corporation).

[0097] Examples of the thermal kneading machine include the following: KRC kneader (manufactured by Kurimoto Iron Works); Buss-Co kneader (manufactured by Buss); TEM type extruder (manufactured by Toshiba Machine); TEX twin-shaft Kneader (manufactured by Japan Steel Works); PCM kneader (manufactured by Ikegai Iron Works); three-roll mill, mixing roll mill, kneader (manufactured by Inoue Seisakusho); Kneadex (manufactured by Mitsui Mining Co., Ltd.); M-second pressure kneader, Niderruder (manufactured by Moriyama Seisakusho); Banbury mixer (manufactured by Kobe Steel, Ltd.).

[0098] Examples of pulverizers include the following: Counter Jet Mill, Micron Jet, Innomizer (manufactured by Hosokawa Micron Corporation); IDS type mill, PJM jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.); Urmax (manufactured by Nisso Engineering Co., Ltd.); SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.); Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.); Turbo Mill (manufactured by Turbo Kogyo Co., Ltd.); and Super Rotor (manufactured by Nisshin Engineering Co., Ltd.).

[0099] Examples of classifiers include the following: Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turboplex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).

[0100] In addition, the following sieving device may be used to sieve out coarse particles. Ultrasonic (manufactured by Kouei Sangyo Co., Ltd.); Resonaseave, Gyroshifter (Tokuju Kogyo Co., Ltd.); Vibrasonic System (manufactured by Dalton); Soniclean (manufactured by Shinto Kogyo Co., Ltd.); Turbo Screener (manufactured by Turbo Kogyo Co., Ltd.); Microshifter (manufactured by Makino Sangyo Co., Ltd.); circular vibrating sieve.

[0101] An annealing process may be performed to facilitate control of the minimum value of the change in storage modulus G' with respect to temperature T (dG' / dT). The annealing process is a process for crystallizing a crystalline material such as a crystalline polyester resin in the toner particles. In particular, when a crystalline polyester resin that easily plasticizes the binder resin is used, it is preferable to carry out crystallization by an annealing step in order to sufficiently advance the crystallization of the crystalline polyester resin at room temperature.

[0102] Next, the measurement methods for each physical property will be described. <Method for measuring storage modulus G'(80℃) and storage modulus G'(120℃)> (1) Preparation of measurement samples The measurement sample is prepared by compressing approximately 0.15 g (varies depending on the specific gravity of the sample) of the toner or the THF insoluble portion of the toner at 20 MPa for 60 seconds in a 25°C environment using a tablet compression machine to prepare a cylindrical sample with a diameter of 8 mm and a height of 2.0±0.3 mm.

[0103] (2) Mounting the sample The measurement device used is a rotating plate type rheometer "ARES" (manufactured by TA INSTRUMENTS). The sample is attached to the parallel plate, and the axial force is adjusted to 250-300 and held. Next, the temperature is raised from room temperature (25°C) to 65°C (adjusted appropriately within the range of toner Tg+5-10°C), and the temperature is maintained for 10 minutes. After that, the sample is reshaped and cooled to 30°C.

[0104] (3) Measurement The measurement is carried out under the following conditions: · Uses parallel plates with a diameter of 8 mm. The frequency is 6.28rad / sec (1.0Hz). Set the initial applied strain (Strain) to 0.1%. Measurements are performed at a temperature ramp rate of 2.0°C / min between 50°C and 120°C, and at a temperature ramp rate of 2.0°C / min between 120°C and 50°C. Measurements are performed under the following auto adjustment mode settings. Measurements are performed in auto strain adjustment mode. Set Max Applied Strain to 20.0%. Set the maximum torque (Max Allowed Torque) to 200.0g·cm and the minimum torque (Min Allowed Torque) to 0.2g·cm. Set the strain adjustment to 20.0% of current strain. Use the auto tension adjustment mode for the measurement. Set Auto Tension Direction to Compression. Set the Initial Static Force to 10.0g and the Auto Tension Sensitivity to 40.0g. · The operating conditions of Auto Tension are such that the Sample Modulus is 1.0×10 2 (Pa) or more. From the temperature T (°C) - storage modulus G’ (Pa) curve obtained by the above method, the storage modulus G’ (80°C) and the storage modulus G’ (120°C) are determined. Also, dG’ / dT is calculated for every two consecutive plots, and the minimum value of the change amount (dG’ / dT) of the storage modulus G’ with respect to the temperature T in the range from 60°C to 80°C is determined. Also, from the obtained temperature T (°C) - storage modulus G’ (Pa) curve, the temperature T1 (°C) at which the storage modulus becomes 1.0×10 3 Pa is read.

[0105] <Measurement method of S2 / S1×1 / R1> The projected area S1 of the toner at 80°C, the radius R1 of the toner at 80°C, and the projected area S2 of the toner at 120°C were measured as follows. (1) Preparation of measurement sample Premium Presentation 120g Laser Paper (HP) was cut into 10 mm squares, and toner was adhered onto the Premium Presentation 120 g Laser Paper (HP). A cotton swab was used for adhering the toner, and the toner was adhered so that it was scattered one particle by one particle on the Premium Presentation 120g Laser Paper (HP). (2) Measurement The Premium Presentation 120g Laser with the adhered toner Paper (HP) is set on a heating plate (TH-600PM cooling and heating stage for Linkam microscope). The heating plate is then heated at 10°C / min, and still images are taken at 80°C and 120°C while observing with an optical microscope. Next, the projected area S1 of the toner at 80°C, the radius R1 of the toner at 80°C, and the projected area S2 of the toner at 120°C are calculated from the still images using image analysis software (Image J). S1, R 1、 The calculation of S2 is the arithmetic mean value of 100 particles. If the toner is not spherical, the average value of the major and minor axes of the toner particle is regarded as the diameter of the toner to calculate the toner radius.

[0106] <Measurement of glass transition temperatures Tg1 and Tg2> The glass transition temperature Tg1 (° C.) and the glass transition temperature Tg2 (° C.) are measured using a differential scanning calorimeter "Flash DSC1 STARe System" (manufactured by METTLER TOLEDO).

[0107] Measurement procedure The toner is placed on a dedicated chip sensor that has been temperature-corrected in advance. The temperature control of the chip sensor is as follows: After maintaining at 25°C for 10 seconds, the temperature is increased to 120°C at a rate of 1000°C / s (first heating process). After maintaining at 120°C for 100 ms (high temperature holding process), the temperature is cooled to 25°C at a rate of 1000°C / s (cooling process). After maintaining at 25°C for 100 ms, the temperature is increased to 120°C at a rate of 1000°C / s (second heating process). Of the above temperature controls, the glass transition temperature Tg1 (° C.) is calculated from the temperature rise curve showing the amount of heat absorption obtained in the first temperature rise process. Also, the glass transition temperature Tg2 (° C.) is calculated from the temperature rise curve showing the amount of heat absorption obtained in the second temperature rise process.

[0108] <Method for measuring ethyl acetate insoluble matter content> Weigh out approximately 1.5 g of toner (W1 [g]), place it in a pre-weighed cylindrical filter paper (product name: No. 86R, size 28 x 100 mm, manufactured by Advantec Toyo Co., Ltd.), and set it in a Soxhlet extractor. Extract for 18 hours using 200 mL of ethyl acetate as the solvent. At that time, extraction is performed at a reflux speed such that the solvent extraction cycle occurs approximately once every 5 minutes. After the extraction is complete, the thimble is removed and air-dried, and then vacuum-dried at 50°C for 24 hours. The mass of the thimble containing the extraction residue is weighed, and the mass of the extraction residue (W2 [g]) is calculated by subtracting the mass of the thimble.

[0109] Next, the content (W3 [g]) of components other than the binder resin is determined by the following procedure. Approximately 2 g of toner is precisely weighed (Wa [g]) into a pre-weighed 30 mL magnetic crucible. The magnetic crucible is placed in an electric furnace and heated to approximately 900°C for approximately 3 hours. It is then allowed to cool in the electric furnace and then allowed to cool at room temperature in a desiccator for at least 1 hour. The mass of the crucible including the incineration ash is weighed and the mass of the crucible is subtracted to calculate the incineration ash content (Wb [g]). Then, the mass (W3 [g]) of the incineration ash in the sample W1 [g] is calculated using the following formula (A). W3 = W1 × (Wb / Wa) (A) In this case, the content of the ethyl acetate insoluble matter in the binder resin can be calculated by the following formula (B). Ethyl acetate insoluble matter (mass%) = {(W2-W3) / (W1-W3)} x 100 (B)

[0110] <Method for measuring the content of tetrahydrofuran (THF) insoluble matter> The content of the resin-derived THF insoluble matter is determined in the same manner as in the above "Method for measuring ethyl acetate insoluble matter" except that the solvent is changed to THF. In the process of obtaining the THF-insoluble fraction, the storage modulus G' (120°C) of the THF-insoluble fraction can be measured by the method using the rotating plate rheometer described above, using a sample that has been subjected to Soxhlet extraction and then vacuum dried at 50°C for 24 hours.

[0111] <Measurement of peak temperature T2> In the DSC curve obtained by differential scanning calorimetry of toner, the peak temperature T2 (°C) of the peak existing on the lowest temperature side among the endothermic peaks in the range of 30°C to 120°C is measured as follows. Using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments), measure in accordance with ASTM D3418-82. For the temperature correction of the device detection part, use the melting points of indium and zinc, and for the heat quantity correction, use the heat of fusion of indium. Specifically, accurately weigh about 5 mg of the measurement sample, put this into an aluminum pan, and use an empty aluminum pan as a reference to perform the measurement at a temperature rising rate of 10°C / min under normal temperature and humidity in the measurement temperature range of 30°C or higher and 120°C or lower. In the DSC curve obtained in this temperature rising process, the temperature of the peak top existing on the lowest temperature side among the endothermic peaks in the range of 30°C or higher and 120°C or lower is defined as T2 (°C).

[0112] <Measurement of the number X of cold crystallization peaks and the number Y of endothermic peaks during the second temperature rise in DSC measurement> The measurement of the number X of cold crystallization peaks and the number Y of endothermic peaks during the second temperature rise is performed as follows. Using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments), measure in accordance with ASTM D3418-82. For the temperature correction of the device detection part, use the melting points of indium and zinc, and for the heat quantity correction, use the heat of fusion of indium. Specifically, accurately weigh about 5 mg of the measurement sample, put this into an aluminum pan, and use an empty aluminum pan as a reference to perform the measurement at a temperature rising rate of 10°C / min under normal temperature and humidity in the measurement temperature range of 30°C or higher and 180°C or lower. In the measurement, first raise the temperature to 180°C, then cool down to 30°C at a rate of 10°C / min, and then raise the temperature again. In the DSC curve obtained during this cooling process, the number of exothermic peaks in the temperature range of 40° C. to 120° C. is defined as the number of cold crystallization peaks X. In addition, in the DSC curve obtained during the second heating process, the number of endothermic peaks in the temperature range of 40° C. to 120° C. is defined as the number of endothermic peaks during the second heating process Y.

[0113] <Measurement of C1 and C2 from toner> The molecular structure of the crystalline polyester resin can be confirmed by known analytical methods such as NMR measurement of a solution or solid, X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. Also, known methods can be used for isolating the crystalline polyester resin from the toner. Specifically, the isolation process is carried out as follows. First, the toner is dispersed in ethanol, which is a poor solvent for the toner, and the temperature is raised to a temperature exceeding the melting point of the crystalline polyester resin. At this time, pressure may be applied if necessary. At this point, the crystalline polyester resin, which has exceeded its melting point, is molten. After that, the crystalline polyester resin can be extracted from the toner by performing solid-liquid separation.

[0114] <The acrylic acid ester and the vinyl polymer portion of the hybrid resin contained in the toner Measurement of the content of a structure in which at least one selected from the group consisting of methacrylic acid esters is polymerized> In addition to solid-state NMR measurement, this can be confirmed by known analytical methods such as X-ray diffraction, GC / MS, LC / MS, and IR measurement.

[0115] <Measurement of the content of amorphous polyester moiety in hybrid resin contained in toner> In addition to solid-state NMR measurement, this can be confirmed by known analytical methods such as X-ray diffraction, GC / MS, LC / MS, and IR measurement. EXAMPLES

[0116] The present invention will be specifically described below based on examples. However, the present invention is not limited to these examples. In the following formulations, parts and percentages are by weight unless otherwise specified. Hereinafter, Examples 3 and 7 to 18 will be referred to as Reference Examples 3 and 7 to 18, respectively.

[0117] <Production Example of Long Chain Alkyl Monomer (W-1)> 1200 parts of linear saturated hydrocarbons with an average carbon number of 35 were placed in a cylindrical glass reaction vessel, and 38.5 parts of boric acid were added at a temperature of 140°C. Immediately after that, a mixed gas of 50% by volume of air and 50% by volume of nitrogen with an oxygen concentration of about 10% by volume was blown in at a rate of 20 L per minute, and the reaction was carried out at 200°C for 3.0 hours. After the reaction, hot water was added to the reaction liquid, and hydrolysis was carried out at 95°C for 2 hours, and after standing, the upper layer reaction product (modified product) was obtained. 20 parts of the resulting modified product was added to 100 parts of n-hexane, and purified to dissolve and remove a portion of the unmodified components to obtain a long-chain alkyl monomer (W-1). The long-chain alkyl monomer (W-1) had a modification rate of 93.6% by mass, i.e., contained 6.4% by mass of aliphatic hydrocarbons. Various physical properties are shown in Table 1.

[0118] [Table 1] In Table 1, W-2 (※) is Unilin 700 (manufactured by Toyo Petrolite Co., Ltd.).

[0119] <Production Example of Resin Composition (A-1)> Bisphenol A ethylene oxide adduct (2.0 mol adduct) 20.0 mol parts Bisphenol A propylene oxide adduct (2.3 mol adduct) 80.0 mol parts Terephthalic acid 67.0 mol parts Dodecanedioic acid 7.0 mol parts In addition to 96 parts of the polyester monomer, a long-chain alkyl monomer (W-1) was added so as to be 5.0% by mass based on the entire polyester resin composition. The resulting mixture was placed in a four-neck flask, and stirred at 160°C under a nitrogen atmosphere, equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device and a stirrer. A vinyl-based polymerization monomer (styrene: 10.0 molybdenum) that constitutes the vinyl polymer moiety is added to the mixture. A mixture of 1.1 parts of butyl acrylate (90.0 mol parts) and 0.7 parts of benzoyl peroxide as a polymerization initiator was added dropwise from the dropping funnel over a period of 4 hours. After that, after reacting at 160 ° C for 5 hours, the temperature was raised to 200 ° C, 0.15 parts of titanium diisopropylate bistriethanol aminate and 0.01 parts of gallic acid were added, and then polycondensation reaction was carried out at 230 ° C for 6 hours, and further reaction was carried out at 230 ° C and 8.0 kPa for 1 hour. After cooling to 180 ° C, 0.01 parts of tert-butylcatechol and 15.0 mol parts of trimellitic anhydride relative to the above polyester monomer were added, and the reaction time was adjusted to obtain the desired viscosity. After the reaction was completed, the mixture was removed from the container, cooled, and pulverized to obtain a resin composition (A-1). Various physical properties are shown in Table 2.

[0120] <Production Examples of Resin Compositions (A-2) to (A-12)> Resin compositions (A-2) to (A-12) were obtained in the same manner as in the production example of resin composition (A-1), except that the monomer formulation was changed to that shown in Table 3. Various physical properties are shown in Table 2.

[0121] <Production Example of Resin Composition (A-13)> A total of 6,550 g of the alcohol components and carboxylic acid components other than trimellitic anhydride listed in Table 3, 45 g of tin(II) 2-ethylhexanoate, and 5 g of gallic acid were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water at 100°C was passed, a stirrer, and a thermocouple, and the mixture was kept at 180°C for 1 hour under a nitrogen atmosphere, and then the temperature was increased from 180°C to 230°C at a rate of 10°C / h, and then a polycondensation reaction was carried out at 230°C for 6 hours. After reacting at 230°C and 8.0 kPa for 1 hour, trimellitic anhydride was further reacted at 210°C, and the reaction time was adjusted to obtain the desired viscosity. After the reaction was completed, the mixture was taken out of the vessel, cooled, and pulverized to obtain a resin composition (A-13). The various physical properties are shown in Table 2.

[0122] <Production Example of Resin Composition (A-14)> Of the monomers shown in Table 3, the raw material monomers for the polyester resin other than fumaric acid and trimellitic anhydride were placed in a 10-liter four-neck flask equipped with a dehydration tube equipped with a nitrogen inlet tube, a stirrer, and a thermocouple, and heated to 160°C in a mantle heater under a nitrogen atmosphere. Then, a mixture of the raw material monomers of the vinyl resin and the polymerization initiator was dropped over 1 hour using a dropping funnel. After dropping, the addition polymerization reaction was matured for 1 hour while maintaining the temperature at 160°C, and then the temperature was raised to 200°C, and 0.15 parts of titanium diisopropylate bistriethanolamine and 0.015 parts of gallic acid were added per 100 parts of the monomers listed in Table 3. Then, a polycondensation reaction was carried out at 235°C for 6 hours, and a reaction was further carried out at 235°C and 8.0 kPa for 1 hour. After cooling to 180°C, 0.015 parts of tert-butylcatechol per 100 parts of fumaric acid and trimellitic anhydride shown in Table 3 and monomers shown in Table 3 were added, and the temperature was raised from 180°C to 210°C at 10°C / h, and the reaction time was adjusted to obtain the desired viscosity. After the reaction was completed, the mixture was removed from the vessel, cooled, and pulverized to obtain a resin composition (A-14). Various physical properties are shown in Table 2.

[0123] [Table 2]

[0124] [Table 3] In Table 3, the abbreviations are as follows. BPA-PO: Bisphenol A propylene oxide adduct (2.3 mol adduct) BPA-EO: Bisphenol A ethylene oxide adduct (2.0 mol adduct) TPA: Terephthalic acid IPA: Isophthalic acid TMA: Trimellitic anhydride St: styrene BA: Butyl acrylate In the table, the values ​​for monomers other than long-chain alkyl monomers represent mol parts. *1: The mol part of monomer indicates the ratio when the total monomer amount of alcohol components (excluding long-chain alkyl monomers) is 100 mol parts. *2: The mol part of monomer indicates the ratio when the total amount of monomer in the vinyl polymer portion is 100 mol parts. *3: PES / StAc ratio is polyester portion (excluding long-chain alkyl monomers) / vinyl polymer portion (mass basis).

[0125] <Production Example of Polyester Resin Composition (B-1)> In a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, the raw material monomers shown in Table 4 were charged in the amounts (parts by mole) shown in Table 4, and then 1.0 part of dibutyltin oxide was added as a catalyst per 100 parts of the total amount of raw material monomers. At this time, W-2 (Unilin 700, manufactured by Toyo Petrolite Co., Ltd.) was used as the long-chain alkyl monomer. The temperature inside the tank was then raised to 150° C. under a nitrogen atmosphere while stirring, and the temperature was then increased from 150° C. to 200° C. at a rate of 10° C. / hour while distilling off water to carry out polymerization. After the temperature reached 200°C, the pressure inside the reaction vessel was reduced to 5 kPa or less, and polycondensation was carried out for 3 hours under the conditions of 200°C and 5 kPa or less. After the reaction was completed, the mixture was removed from the vessel, cooled, and pulverized to obtain a polyester resin composition (B-1). The physical properties are shown in Table 5.

[0126] <Production Example of Polyester Resin Composition (B-2)> In addition to the alcohol components shown in Table 4, and the carboxylic acid components other than adipic acid and trimellitic anhydride, 0.02 parts of tin(II) 2-ethylhexanoate and 0.025 parts of gallic acid per 100 parts of the monomers shown in Table 4 were placed in a 10-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water at 100°C was passed, a stirrer, and a thermocouple. After keeping at 180°C for 1 hour under a nitrogen atmosphere, the temperature was increased from 180°C to 230°C at a rate of 10°C / h, and then polycondensation reaction was carried out at 230°C for 6 hours. After reacting at 230°C and 8.0 kPa for 1 hour, adipic acid and trimellitic anhydride were further reacted at 210°C, and the reaction time was adjusted to obtain the desired viscosity. After the reaction was completed, the mixture was taken out of the vessel, cooled, and pulverized to obtain a resin composition (B-2). The physical properties are shown in Table 5.

[0127] [Table 4] In Table 4, the abbreviations are as follows. BPA-PO: Bisphenol A propylene oxide adduct (2.0 mol adduct) BPA-EO: Bisphenol A ethylene oxide adduct (2.0 mol adduct) EG: Ethylene glycol TPA: Terephthalic acid IPA: Isophthalic acid TMA: Trimellitic anhydride In the table, the values ​​for monomers other than long-chain alkyl monomers represent mol parts. *1: The mol part of monomer indicates the ratio when the total monomer amount of alcohol components (excluding long-chain alkyl monomers) is 100 mol parts.

[0128] [Table 5]

[0129] <Production Example of Crystalline Polyester (C-1)> Ethylene glycol 100.0 mol parts Tetradecanedioic acid 90.0 mol parts Lauric acid 20.0 mol parts The above monomers and 0.2% by mass of dibutyltin oxide based on the total amount of the monomers were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and reacted at 180°C for 4 hours. The temperature was then increased to 210°C at a rate of 10°C / hour, and the mixture was kept at 210°C for 8 hours, and then reacted at 8.3kPa for 1 hour to obtain crystalline polyester (C-1). The physical properties are shown in Table 6.

[0130] <Production Examples of Crystalline Polyesters (C-2) to (C-11)> Resin compositions (C-2) to (C-11) were obtained in the same manner as in the production example of crystalline polyester (C-1), except that the monomer formulation was changed to that shown in Table 6. Various physical properties are shown in Table 6.

[0131] [Table 6]

[0132] <Production Example of Magnetic Particle 1> (1) Production of core particles Fe 2+ 92 L of ferrous sulfate aqueous solution with a concentration of 1.60 mol / L and 88 L of sodium hydroxide aqueous solution with a concentration of 3.50 mol / L were added and mixed and stirred. The pH of this solution was 6.5. While maintaining the temperature of this solution at 89°C and the pH at 9 to 12, air was blown in at 20 L / min to cause an oxidation reaction and generate core particles. When the ferrous hydroxide was completely consumed, the blowing of air was stopped and the oxidation reaction was terminated. The obtained core particles made of magnetite had an octahedral shape. (2) Formation of the coating layer 2.50 L of 0.7 mol / L sodium silicate aqueous solution and 2.00 L of 0.90 mol / L ferrous sulfate aqueous solution were mixed, and then 1.00 L of water was added to make a 5.00 L aqueous solution. The solution was added to the above-mentioned reaction-result slurry containing 13,500 g of core particles while maintaining the pH at 7 to 9. The Fe in the slurry was then 2+ Air was blown in at 10 L / min until no more remained. Next, 0.70 L of 1.50 mol / L aluminum sulfate aqueous solution and 2.00 L of 0.90 mol / L ferrous sulfate aqueous solution were mixed, and then 1.00 L of water was added to make a 5.00 L aqueous solution, which was added to the above-mentioned reacted slurry containing core particles while maintaining the pH at 7 to 9. Then, the Fe in the slurry was 2+ Air was blown in at 10 L / min until no more air remained. The temperature of the slurry was maintained at 89° C. After mixing and stirring for 30 minutes, the slurry was filtered, washed, and dried to obtain magnetic particles 1. The shape of magnetic particles 1 was octahedral, and the number average particle size (D1) of the primary particles of magnetic particles 1 was 110 nm. Table 7 shows the physical properties of the obtained magnetic particles 1.

[0133] [Table 7]

[0134] <Release agents 1 to 4> The release agents listed in Table 8 were used.

[0135] [Table 8]

[0136] <Example 1> Polyester resin composition (A-1) 100.0 parts Crystalline polyester (C-1) 12.0 parts ·Magnetic particles 1 50.0 parts Release agent-1 2.0 parts Charge control agent (T-77, manufactured by Hodogaya Chemical Co., Ltd.) 1.0 part The above materials were premixed in a Henschel mixer, and then melt-kneaded at a set temperature of 120° C. using a twin-screw kneading extruder (PCM-30 model, manufactured by Ikegai Iron Works, Ltd.). The obtained kneaded product was cooled and coarsely pulverized with a hammer mill, and then annealed for one day in an environment with a temperature of 50° C. and a relative humidity of 95%. The coarsely pulverized material was then pulverized using a mechanical pulverizer (T-250 manufactured by Turbo Kogyo Co., Ltd.), and the resulting finely pulverized powder was classified using a multi-division classifier utilizing the Coanda effect to obtain negatively charged toner particles having a weight average particle size (D4) of 7.0 μm. For 100 parts of toner particles, 1 part of hydrophobic silica fine particles [BET specific surface area 150 m 2 / g, 100 parts of silica fine particles, 30 parts of hexamethyldisilazane (HMDS) and 10 parts of dimethyl silicone oil were used to hydrophobize the silica fine particles, 1.0 parts were added and mixed in a Henschel mixer (FM-75 type manufactured by Nippon Coke & Engineering Co., Ltd.), and the mixture was sieved through a 150 μm mesh to obtain toner (T-1). The physical properties of the obtained toner (T-1) are shown in Table 9.

[0137] The obtained toner was subjected to the following evaluations. <Test> Considering the possibility of further increasing the printer speed in the future, we used an HP LaserJet Enterprise M609dn, which was modified to have a process speed of 450 mm / sec. The evaluation results are shown in Table 10.

[0138] <Low temperature fixability 1; Rubbing density loss rate> The rate of decrease in rubbing density was measured by removing the fixing device of the above-mentioned evaluation machine from the outside, modifying the fixing device so that the temperature could be arbitrarily set, and using an external fixing device with a process speed of 450 mm / sec. Using the above device, in a low temperature and low humidity environment (temperature 15°C, humidity 10% RH), the toner loading amount per unit area was 0.5 mg / cm 2 The unfixed image, set at 100° C., was passed through the fixing device set at 200° C. The evaluation paper was “PB PAPER” (Canon Marketing Japan, basis weight 66 g / cm 2 The resulting fixed image was subjected to a pressure of 4.9 kPa (50 g / cm 2 The image was rubbed with Silbon paper under a load of 1000 g (1.0 kg) and evaluated based on the decrease in image density (%) before and after rubbing. Image density was measured using a Macbeth densitometer (manufactured by Macbeth) which is a reflection densitometer, and an SPI filter. Ranks A and B were considered to be acceptable. A: The decrease in image density is less than 10.0%. B: The decrease rate of image density is 10.0% or more and less than 15.0%. C: The decrease rate of image density is 15.0% or more and less than 20.0%. D: The decrease in image density is 20.0% or more.

[0139] <Low temperature fixability 2: Missing fixation spots> For fixing popping, the fixing unit of the above evaluation machine was taken outside, and an external fixing unit was used which was modified so that the temperature of the fixing unit could be set arbitrarily and the process speed was set to 480 mm / sec. Using the above device, in a low temperature and low humidity environment (temperature 15°C, humidity 10% RH), the toner loading amount per unit area was 1.0 mg / cm 2 The entire solid unfixed image, set at 100° C., was passed through a fixing unit set at 200° C. The evaluation paper was “PB PAPER” (Canon Marketing Japan, basis weight 66 g / cm 2 , Letter) was used. The obtained image was visually inspected, and the number of spots where the toner was not fixed sufficiently and the toner was missing was counted, and the fixing spots were evaluated according to the following criteria. Ranks A and B were considered to be acceptable. A: The number of missing pieces is less than 3. B: The number of missing pieces is 3 or more and less than 6. C: The number of missing pieces is 6 or more and less than 9. D: The number of missing pieces is 9 or more.

[0140] <Uneven density of solid images> For the solid image density unevenness, the fixing device of the above evaluation machine was taken outside, and an external fixing device was modified so that the fixing device temperature could be set arbitrarily and the process speed was set to 480 mm / sec. In a high temperature and high humidity environment (temperature 32.5°C, humidity 85% RH), the toner loading amount per unit area was 1.0 mg / cm 2 The entire solid unfixed image set at 0.05 was passed through a fixing unit whose temperature was adjusted to 200°C. The evaluation paper was Vitality (Xerox, basis weight 75 g / cm 2, Letter), evaluation was performed on recording media having a surface roughness measurement (described later) of 3.00 μm or more Sa (arithmetic mean height). The density of the obtained image was measured at 20 random points, and the difference between the maximum and minimum measured density was used for evaluation. The image density was evaluated according to the following criteria, using a SPI filter and changing the measurement spot diameter of a Macbeth densitometer (manufactured by Macbeth Co., Ltd.), which is a reflection densitometer. A and B ranks were considered to be acceptable. A: The concentration difference is less than 0.10. B: The concentration difference is 0.10 or more and less than 0.20. C: The concentration difference is 0.20 or more and less than 0.30. D: The concentration difference is 0.30 or more.

[0141] <Evaluation of fogging> In a high temperature and high humidity environment (temperature 32°C, relative humidity 80%), the operation of outputting an image with a printing ratio of 1% was repeated, and each time the number of output sheets reached 500, it was left overnight. After that, the process of outputting 500 sheets and leaving it overnight was repeated as described above, and finally 5,000 images were output, and evaluation was performed using the following method. The evaluation paper was "PB PAPER" (Canon Marketing Japan, basis weight 66 g / cm 2 , Letter) was used. In the image output test, one image having a white background was output each time. After that, for all images having a white background, the fog density (%) (=Dr(%)-Ds(%)) was calculated from the difference between the whiteness (reflectance Ds(%)) of the white background of the image having a white background and the whiteness (average reflectance Dr(%)) of the transfer paper. The whiteness was measured using a "REFLECTMETER MODEL TC-6DS" (manufactured by Tokyo Denshoku Co., Ltd.). The filter used was an amber light filter. The images with the worst fog density were ranked as follows. Ranks A to C were considered to be acceptable. A: The fog density is less than 2.5%. B: The fog density is 2.5% or more and less than 4.5%. C: The fog density is 4.5% or more and less than 6.5%. D: The fog density is 6.5% or more.

[0142] <Image density after durability test> Evaluation was carried out using the modified machine. After emptying the toner from the cartridge, 700 g of toner (T-1) was filled into the cartridge. A 25,000-sheet image output test was conducted in a mode where a horizontal line pattern with a print rate of 1.5% was printed on two sheets per job, and the machine was set to pause between jobs before the next job began. The evaluation was conducted in a high-temperature, high-humidity environment (temperature 32.5°C, humidity 85% RH). The evaluation paper was PB PAPER (Canon Marketing Japan, basis weight 66g / cm 2 , Letter) was used. On the 25,001st sheet, a checkerboard image was printed with a 5 mm leading margin, 5 mm left and right margins, in three places on the left, right and centre, and three more places 30 mm apart in the longitudinal direction, for a total of nine 5 mm x 5 mm solid black patch images. The image density of the nine solid black patch image portions of this check image was measured, and the average value was calculated. The image density was measured using a Macbeth densitometer (manufactured by Macbeth Co., Ltd.), which is a reflection densitometer, using an SPI filter. The measurements were performed using the following criteria: A and B ranks were considered passing. A. Image density is 1.30 or higher. B. Image density is 1.10 or more and less than 1.30. C. Image density is 0.90 or more and less than 1.10. D. Image density is less than 0.90.

[0143] <Severe storage stability> After emptying the toner from the cartridge, 700 g of toner (T-1) was filled in. First, the cartridge was tapped 300 times with the drive side facing down to pack the toner tightly. Then, the cartridge was left in a harsh environment (temperature 40°C, humidity 95% RH) for 90 days with the drive side facing down to evaluate the harsh storage stability under harsh conditions. After removing the cartridge, an image output test was carried out in a high temperature and high humidity environment (temperature 32.5° C., humidity 85% RH) using the modified machine, and the severe storage stability was evaluated. The image output test started with 20,000 images of a horizontal line pattern with a print rate of 2.0% printed on 2 sheets per job, in a mode where the machine stopped between jobs before starting the next job. After that, a check image was output in the same environment. A 200mm x 280mm halftone image (dot printing rate 23%) was printed as the check image, and the check image was visually inspected for the presence of vertical streaks and rated according to the following criteria. Ranks A and B were deemed acceptable. A: No streaks were observed. B: 1 to 5 streaks less than 1 mm occurred, and no streaks of 1 mm or more occurred. C: 6 or more streaks less than 1 mm occurred, and no streaks of 1 mm or more occurred. D: Streaks of 1 mm or more have occurred.

[0144] <Examples 2 to 18> Toners (T-2) to (T-18) were obtained in the same manner as in Example 1, except that the formulations were as shown in Table 10. Various physical properties are shown in Table 9. The results of evaluation performed in the same manner as in Example 1 are shown in Table 11.

[0145] <Comparative Examples 1 to 2> Toners (T-19) to (T-20) were obtained in the same manner as in Example 1, except that the formulations were as shown in Table 10. The physical properties of the toners are shown in Table 9. The results of evaluation performed in the same manner as in Example 1 are shown in Table 11.

[0146] <Comparative Example 3 and Comparative Example 6> Except for changing the formulation to that shown in Table 10 and not carrying out the annealing treatment, the same procedure as in Example 1 was carried out to obtain toners (T-21) and (T-24). The results of evaluation performed in the same manner as in Example 1 are shown in Table 11.

[0147] <Comparative Example 4> (Preparation of crystalline polyester resin dispersion) 100 g of crystalline polyester (C-9) and 400 g of ethyl acetate were placed in a 2 L metal container, and the mixture was dissolved by heating at 75° C., then quenched in an ice-water bath at a rate of 27° C. / min. 500 ml of glass beads (3 mm diameter) were added, and the mixture was ground for 10 hours using a batch-type sand mill (Kanpe Hapio Co., Ltd.) to obtain [Crystalline polyester dispersion 1].

[0148] (Synthesis of amorphous polyester (low molecular weight amorphous polyester) resin) In a 5-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 229 parts of bisphenol A ethylene oxide 2 mol adduct, 529 parts of bisphenol A propylene oxide 3 mol adduct, 100 parts of isophthalic acid, 108 parts of terephthalic acid, 46 parts of adipic acid, and 2 parts of dibutyltin oxide were added to the reaction vessel, and the mixture was reacted at normal pressure and 230°C for 10 hours, and then at a reduced pressure of 10 to 15 mmHg for 5 hours. After that, 30 parts of trimellitic anhydride was added to the reaction vessel, and the mixture was reacted at 180°C and normal pressure for 3 hours to obtain [amorphous polyester 1]. [Amorphous polyester 1] had a number average molecular weight of 1,800, a weight average molecular weight of 5,500, a Tg of 50° C., and an acid value of 20 mg KOH / g.

[0149] (Synthesis of polyester prepolymer (binder resin precursor)) Into a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube, 682 parts of bisphenol A ethylene oxide 2-mol adduct, 81 parts of bisphenol A propylene oxide 2-mol adduct, 283 parts of terephthalic acid, 22 parts of trimellitic anhydride, and 2 parts of dibutyltin oxide were placed. This was reacted at normal pressure and 230°C for 8 hours, and further reacted at a reduced pressure of 10 to 15 mmHg for 5 hours to obtain [intermediate polyester 1]. [Intermediate polyester 1] had a number average molecular weight of 2,100, a weight average molecular weight of 9,500, a Tg of 55° C., an acid value of 0.5 mg KOH / g, and a hydroxyl value of 51 mg KOH / g. Next, 410 parts of [Intermediate polyester 1], 89 parts of isophorone diisocyanate, and 500 parts of ethyl acetate were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 100° C. for 5 hours to obtain [Prepolymer 1]. The amount of free isocyanate in [Prepolymer 1] was 1.53% by mass.

[0150] (Ketimine synthesis) In a reaction vessel equipped with a stirring bar and a thermometer, 170 parts of isophoronediamine and 75 parts of methyl ethyl ketone were charged and reacted at 50° C. for 5 hours to obtain [Ketimine Compound 1]. The amine value of [ketimine compound 1] was 418 mg KOH / g.

[0151] (Masterbatch (MB) synthesis) 1,200 parts of water, 1:1,200 parts of magnetic particles, and 1:1,200 parts of amorphous polyester resin were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). The mixture was kneaded using two rolls at 150°C for 30 minutes, then rolled and cooled, and pulverized in a pulverizer to obtain [Master Batch 1].

[0152] (Preparation of oil phase) In a vessel equipped with a stirring rod and a thermometer, 378 parts of [amorphous polyester 1], 110 parts of carnauba wax, 22 parts of CCA (salicylic acid metal complex E-84: Orient Chemical Industry), and 947 parts of ethyl acetate were charged, and the mixture was heated to 80°C while stirring, and then kept at 80°C for 5 hours, and then cooled to 30°C in 1 hour. Next, 690 parts of [master batch 1] and 500 parts of ethyl acetate were charged in the vessel, and mixed for 1 hour to obtain [raw material solution 1]. 1,324 parts of [Raw material solution 1] were transferred to a container, and magnetic particles 1 and wax were dispersed using a bead mill (Ultraviscomill, manufactured by Imex) under the following conditions: liquid delivery speed 1 kg / hr, disk peripheral speed 6 m / sec, 80% volume loading of 0.5 mm zirconia beads, and 3 passes. Next, 1,042.3 parts of a 65% ethyl acetate solution of [Amorphous polyester 1] was added, and the bead mill was passed once under the above conditions to obtain [Pigment-wax dispersion 1]. The solids concentration of [Pigment-wax dispersion 1] (130°C, 30 minutes) was 50%.

[0153] (Synthesis of organic fine particle emulsion) In a reaction vessel equipped with a stirring rod and a thermometer, 683 parts of water, 11 parts of sodium salt of methacrylic acid ethylene oxide adduct sulfate (Eleminol RS-30: manufactured by Sanyo Chemical Industries), 138 parts of styrene, 138 parts of methacrylic acid, and 1 part of ammonium persulfate were charged, and the mixture was stirred for 4 hours. After stirring at 100 rpm for 15 minutes, a white emulsion was obtained. The system was heated to 75° C. and reacted for 5 hours. Further, 30 parts of 1% ammonium persulfate aqueous solution was added and aged at 75°C for 5 hours to obtain an aqueous dispersion of vinyl resin (a copolymer of styrene-methacrylic acid-methacrylic acid ethylene oxide adduct sulfate ester sodium salt) [Fine Particle Dispersion 1]. The volume average particle diameter of [Fine Particle Dispersion 1] measured with LA-920 was 0.14μm. A part of [Fine Particle Dispersion 1] was dried to isolate the resin content.

[0154] (Preparation of aqueous phase) 990 parts of water, 83 parts of [fine particle dispersion 1], 37 parts of a 48.5% aqueous solution of sodium dodecyldiphenyletherdisulfonate (Eleminol MON-7: manufactured by Sanyo Chemical Industries), and 90 parts of ethyl acetate were mixed and stirred to obtain a milky white liquid. This was designated as [aqueous phase 1].

[0155] (Emulsification / solvent removal) 664 parts of [Pigment / WAX Dispersion 1], 109.4 parts of [Prepolymer 1], 73.9 parts of [Crystalline Polyester Dispersion 1], and 4.6 parts of [Ketimine Compound 1] were placed in a container and mixed at 5,000 rpm for 1 minute with a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.). Then, 1,200 parts of [Aqueous Phase 1] was added to the container and mixed at 13,000 rpm for 20 minutes with a TK Homomixer to obtain [Emulsified Slurry 1]. [Emulsified slurry 1] was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed at 30°C for 8 hours, and then aged at 45°C for 4 hours to obtain [Dispersed slurry 1].

[0156] (Washing and drying) [Dispersion Slurry 1] 100 parts was filtered under reduced pressure, (1): Add 100 parts of ion-exchanged water to the filter cake, mix with a TK homomixer (at 12,000 rpm for 10 minutes), and then filter. (2): Add 100 parts of 10% aqueous sodium hydroxide solution to the filter cake of (1), mix with a TK homomixer (at 12,000 rpm for 30 minutes), and then filter under reduced pressure. (3): Add 100 parts of 10% hydrochloric acid to the filter cake of (2), mix with a TK homomixer (at 12,000 rpm for 10 minutes), and then filter. (4) Add 300 parts of ion-exchanged water to the filter cake of (3), mix with a TK homomixer (at 12,000 rpm for 10 minutes), and then filter. The steps (1) to (4) were repeated twice to obtain [Filter Cake 1]. [Filter cake 1] was dried in a circulating air dryer at 45° C. for 48 hours, and sieved through a 75 μm mesh to obtain toner particles. For 100 parts of toner particles, 1 part of hydrophobic silica fine particles [BET specific surface area 150 m 2 / g, 100 parts of silica fine particles, 30 parts of hexamethyldisilazane (HMDS) and 10 parts of dimethyl silicone oil were used to hydrophobize the silica fine particles, 1.0 parts were added and mixed in a Henschel mixer (FM-75 type manufactured by Nippon Coke & Co., Ltd.), and the mixture was sieved through a 150 μm mesh to obtain a toner (T-22). The various physical properties are shown in Table 9.

[0157] <Comparative Example 5> (Synthesis of non-linear amorphous polyester) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, adipic acid, and trimethylolpropane were placed so that the molar ratio of hydroxyl groups to carboxyl groups [OH] / [COOH] was 1.1. At this time, trimethylolpropane was added at 1.5 mol% relative to the total monomers, and titanium tetraisopropoxide was added at 1000 ppm relative to the total monomers. Next, the temperature was raised to 200°C in about 4 hours, and then to 230°C in 2 hours, and the reaction was continued until no more water was discharged. The reaction was then continued for 5 hours under reduced pressure of 10 to 15 mmHg, and the water was removed. A non-linear amorphous polyester having an acid group was obtained.

[0158] (Synthesis of linear amorphous polyester) A reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was charged with 2 moles of ethylene oxide adduct of bisphenol A, 2 moles of propylene oxide adduct of bisphenol A, isophthalic acid, and adipic acid so that the molar ratio of hydroxyl groups to carboxyl groups [OH] / [COOH] was 1.2. In this case, the diol consisted of 80 mol % of an ethylene oxide side 2-mol adduct of bisphenol A and 20 mol % of a propylene oxide 2-mol adduct of bisphenol A, the dicarboxylic acid consisted of 80 mol % of isophthalic acid and 20 mol % of adipic acid, and 500 ppm of titanium tetraisopropoxide was added based on the total monomers. Next, the mixture was reacted at 230°C for 8 hours, and then reacted under reduced pressure of 10 to 15 mmHg for 4 hours. Trimellitic anhydride was added to the mixture at 1 mol% relative to the total monomers, and the mixture was reacted at 180°C for 3 hours to obtain a linear amorphous polyester. The weight average molecular weight was 5500, and the glass transition point was 50°C.

[0159] (Masterbatch Production) 1200 parts of water, 500 parts of carbon black Printex35 (manufactured by Dexa) with DBP oil absorption of 42 mL / 100 mg and pH of 9.5, and 500 parts of linear amorphous polyester were mixed using a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), and then kneaded using a two-roll mill at 150° C. for 30 minutes. Next, the mixture was rolled and cooled, and then pulverized using a pulverizer to obtain a master batch.

[0160] (Preparation of release agent dispersion) In a container equipped with a stirring rod and a thermometer, 50 parts of paraffin wax HNP-9 (manufactured by Nippon Seiro Co., Ltd.) with a melting point of 75°C and 450 parts of ethyl acetate were placed, and the mixture was heated to 80°C while stirring and maintained for 5 hours. Next, after cooling to 30°C in 1 hour, a bead mill, Ultraviscomill (manufactured by Imex Co., Ltd.), was used to fill the mixture with 80% by volume of zirconia beads with a diameter of 0.5 mm, and dispersed under the conditions of 3 passes at a liquid delivery rate of 1 kg / h and a disk peripheral speed of 6 m / s to obtain a release agent dispersion.

[0161] (Preparation of Crystalline Polyester Dispersion) In a container equipped with a stirring rod and a thermometer, 50 parts of crystalline polyester (C-10) and 450 parts of ethyl acetate were placed, and the mixture was heated to 80°C while stirring and maintained for 5 hours. Next, the mixture was cooled to 30°C in 1 hour, and then dispersed using a bead mill, Ultraviscomill (manufactured by Imex), with a liquid delivery rate of 1 kg / h, a disk peripheral speed of 6 m / s, and 80% by volume of zirconia beads with a diameter of 0.5 mm, under three-pass conditions to obtain a crystalline polyester dispersion.

[0162] (Preparation of oil phase) 50 parts of the release agent dispersion, 200 parts of the non-linear amorphous polyester, 500 parts of the crystalline polyester dispersion, 700 parts of the linear amorphous polyester, 50 parts of the master batch, and 1:2 parts of the ketimine compound were placed in a container, and then mixed at 5,000 rpm for 60 minutes using a TK homomixer (manufactured by Tokushu Kika Co., Ltd.) to obtain an oil phase.

[0163] (Preparation of aqueous dispersion of vinyl resin) In a reaction vessel equipped with a stirring rod and a thermometer, 683 parts of water, 11 parts of the sodium salt of sulfate of ethylene oxide adduct of methacrylic acid (Eleminol RS-30 (manufactured by Sanyo Chemical Industries)), 138 parts of styrene, 138 parts of methacrylic acid, and 1 part of ammonium persulfate were placed, and the mixture was stirred at 400 rpm for 15 minutes. The temperature was then raised to 75°C, and the mixture was allowed to react for 5 hours. Thereafter, 30 parts of a 1% by mass aqueous solution of ammonium persulfate was added, and the mixture was aged at 75° C. for 5 hours to obtain an aqueous dispersion of a vinyl resin. The volume average particle size of the aqueous dispersion of the vinyl resin was measured using a laser diffraction / scattering type particle size distribution analyzer LA-920 (manufactured by HORIBA Corporation) and found to be 0.14 μm.

[0164] (Preparation of aqueous phase) 990 parts of water, 83 parts of an aqueous dispersion of a vinyl resin, 37 parts of a 48.5% by mass aqueous solution of sodium dodecyldiphenyletherdisulfonate Eleminol MON-7 (manufactured by Sanyo Chemical Industries), and 90 parts of ethyl acetate were mixed and stirred to obtain an aqueous phase.

[0165] (Emulsification / solvent removal) To a vessel containing 1,052 parts of the oil phase, 1,200 parts of the water phase were added, and then mixed at 13,000 rpm for 20 minutes using a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.) to obtain an emulsified slurry. The emulsified slurry was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 8 hours, and then the mixture was aged at 45° C. for 4 hours to obtain a dispersed slurry.

[0166] (Washing and drying) 100 parts of the dispersed slurry was filtered under reduced pressure. The following operations (1) to (4) were repeated twice for the obtained filter cake. (1): 100 parts of ion-exchanged water is added to the filter cake, and the mixture is mixed at 12,000 rpm for 10 minutes using a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.), and then filtered. (2): 100 parts of a 10% by weight aqueous sodium hydroxide solution is added to the filter cake of (1), and mixed at 12,000 rpm for 30 minutes using a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.), and then filtered under reduced pressure. (3): 100 parts of 10% by weight hydrochloric acid is added to the filter cake of (2), and the mixture is mixed at 12,000 rpm for 10 minutes using a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.), and then filtered. (4): 300 parts of ion-exchanged water is added to the filter cake of (3), and the mixture is mixed at 12,000 rpm for 10 minutes using a TK Homomixer (manufactured by Tokushu Kika Co., Ltd.), and then filtered. The obtained filter cake was dried at 45° C. for 48 hours using a circulating air dryer, and then sieved through a 75 μm mesh to obtain base particles. 100 parts of the base particles and 1.0 part of hydrophobic silica HDK-2000 (manufactured by Wacker Chemie) were mixed for 30 seconds at a peripheral speed of 30 m / s using a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), and then the process of stopping for 1 minute was repeated five times, and the mixture was sieved through a 35 μm mesh to obtain toner (T-23). ​​The physical properties are shown in Table 9.

[0167] [Table 9]

[0168] [Table 10]

[0169] [Table 11]

Claims

1. A toner having toner particles containing a binder resin and a crystalline polyester, the binder resin contains a hybrid resin having a vinyl polymer portion and an amorphous polyester portion, the crystalline polyester is a condensation polymer of an alcohol component containing an aliphatic diol and an acid component containing an aliphatic dicarboxylic acid, and has at least one of a structure in which an aliphatic monocarboxylic acid is condensed at an end and a structure in which an aliphatic monoalcohol is condensed at an end, wherein the number of carbon atoms of the aliphatic diol is C1 and the number of carbon atoms of the aliphatic dicarboxylic acid is C2, the sum of C1 and C2 is 10 or more and 16 or less, In the measurement of the toner using a rotary plate rheometer, the toner has a temperature T (°C) vs. storage modulus G' (Pa) curve obtained when the toner is heated at a rate of 2.0°C / min. (i) Storage modulus G'(80°C) at 80°C is 2.0 x 10 3 Pa or more 2.0×10 5 Pa or less, (ii) The minimum value of the change in storage modulus G' with respect to temperature T (dG' / dT) in the range of 60°C to 80°C is -1.0 x 10 6 is as follows: When the toner is heated from 25° C. to 120° C. at a temperature increase rate of 10° C. / min, the projected area of ​​the toner at 80° C. is S 1 (μm 2 ) and the radius of the projected area of ​​the toner at 80° C. is R 1 (μm), and the projected area of ​​the toner at 120° C. is S 2 (μm 2 ) and The S 1 , R 1 and S 2 The toner is characterized in that the following formula (1) is satisfied: (1) S 2 / S 1 ×1 / R 1 ≦0.22

2. In the temperature T (° C.)-storage modulus G′ (Pa) curve, The storage modulus G' (120°C) at 120°C is 2.0 x 10 3 Pa or more 2.0×10 4 2. The toner according to claim 1, wherein the viscosity is 0.1 Pa or less.

3. When the toner is subjected to Soxhlet extraction using tetrahydrofuran for 18 hours, the toner contains a tetrahydrofuran insoluble matter, The storage modulus G'(120°C) of the tetrahydrofuran insoluble portion at 120°C measured with a rotating plate rheometer when the temperature was increased at a rate of 2.0°C / min was 1.0 x 10 5 Pa or more 1.0×10 7 3. The toner according to claim 1, wherein the viscosity is 0.1 Pa or less.

4. In a Soxhlet extraction of the toner using ethyl acetate, the content of ethyl acetate insoluble matter in the toner after extraction for 18 hours is defined as α% by mass, In the Soxhlet extraction of the toner using tetrahydrofuran, when the content of the tetrahydrofuran insoluble matter of the toner after extraction for 18 hours is defined as β% by mass, The toner according to any one of claims 1 to 3, wherein the α and the β satisfy the following formulas (2) and (3): (2) 5.0 ≦ β ≦ 30.0 (3) 10.0≦(α-β)≦40.0

5. the vinyl polymer portion has a structure in which at least one selected from the group consisting of an acrylic acid ester and a methacrylic acid ester is polymerized, The toner according to any one of claims 1 to 4, wherein the total content of the structure in which at least one selected from the group consisting of acrylic acid esters and methacrylic acid esters is polymerized in the vinyl polymer segment is 50% by mass or more and 98% by mass or less.

6. 6. The toner according to claim 1, wherein the content of the amorphous polyester moiety in the hybrid resin is 50% by mass or more and 98% by mass or less.

7. The toner according to any one of claims 1 to 6, wherein the amorphous polyester moiety has a structure crosslinked with at least one selected from the group consisting of trivalent or higher polyhydric alcohols and trivalent or higher polyvalent carboxylic acids.

8. In a differential scanning calorimeter (DSC) measurement of the toner, (i) the number of cold crystallization peaks in the range of 40° C. or more and 120° C. or less during cooling is defined as X; (ii) When the number of endothermic peaks in the range of 40° C. or more and 120° C. or less during the second temperature increase is Y X and Y satisfy the following formulas (7) and (8). The toner according to any one of claims 1 to 7. (7) X≧1 (8) Y≧X+1

9. the toner particles contain a crystalline polyester resin, In the differential scanning calorimetry of the toner, The temperature is increased from 25°C to 120°C at a rate of 1000°C / sec. The temperature was held at 120° C. for 100 ms, and then cooled to 25° C. at a rate of 1000° C. / s. The temperature is increased to 120°C at a rate of 1000°C / sec. When the glass transition temperature in the first heating is Tg1 (°C) and the glass transition temperature in the second heating is Tg2 (°C), The toner according to any one of claims 1 to 8, which satisfies the following formulas (9) and (10): (9) 65° C.≦Tg1≦85° C. (10) 7°C≦Tg1-Tg2≦30°C

10. In the temperature T (° C.)-storage modulus G′ (Pa) curve, the storage modulus is 1.0×10 3 The temperature at which the temperature becomes Pa is T1 (°C), The toner has an endothermic peak in the range of 30° C. to 120° C. in a DSC curve obtained by differential scanning calorimetry, When the peak temperature of the peak present on the lowest temperature side of the endothermic peak is T2 (°C), The toner according to any one of claims 1 to 9, which satisfies the following formula (11): (11) T1-T2≧40

Citation Information

Patent Citations

  • Electrostatic charge image developing toner

    JP1993297629A

  • Reusable transfer material and image forming method

    JP2004170606A

  • Electrophotographic toner, two-component developer including the toner, and image forming apparatus

    JP2014167602A

  • toner

    JP2016071377A

  • Toner and method for producing toner

    JP2017173545A