toner
A balanced toner formulation with irregular silica and controlled metal oxide adhesion addresses the trade-off between sleeve ghost resistance and cleaning performance, enhancing transferability and stability in electrophotographic systems.
Patent Information
- Application Number
- JP2020150937
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-09
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-09-09
AI Technical Summary
Existing electrophotographic toners face a trade-off between sleeve ghost resistance and cleaning performance, with increased fine particles for improved transferability leading to more noticeable density differences and cleaning defects.
The toner formulation includes irregularly shaped silica particles and a metal oxide with controlled adhesion rates, ensuring balanced supply to the electrostatic latent image carrier, reducing sleeve ghosts and cleaning performance issues.
The toner achieves excellent transfer properties, sleeve ghost resistance, and cleaning performance by maintaining consistent supply rates of additives, minimizing chatter and defects during long-term use.
Smart Images

Figure 0007562343000007 
Figure 0007562343000008 
Figure 0007562343000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner and a developing method used in electrophotography, electrostatic recording, electrostatic printing, and the like. [Background technology]
[0002] In recent years, as full-color electrophotographic copying machines have come into widespread use, there has been a demand for higher image quality as well as stability during long-term use. When used for a long time, especially when a large amount of images of the same pattern are printed, the amount of fine particles such as external additives supplied from the toner present on the electrostatic latent image carrier differs between the printed and non-printed areas on the developing sleeve. In this case, the electric field strength applied to the toner differs due to the influence of the electric field lines formed by the charge of the fine particles, and the history of the previous image may be printed as a difference in image density (hereinafter referred to as sleeve ghosting). Regarding sleeve ghosting, for example, Patent Document 1 discloses a technology that can suppress sleeve ghosting in low-temperature, low-humidity environments by adding silica having a number-average particle size of 5 nm or more and 20 nm or less and silica having a number-average particle size of 80 nm or more and 200 nm or less to the toner, thereby controlling the electrostatic charge and fluidity of the toner. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-110095 A [Patent Document 2] JP 2017-138482 A [Patent Document 3] Japanese Patent Application Publication No. 63-96664 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in order to improve the transferability, it is necessary to further increase the amount of fine particles such as silica, as described in Patent Document 1, to improve the coverage and reduce the non-electrostatic adhesion, but as the amount of fine particles added increases, the proportion of fine particles supplied to the electrostatic latent image carrier increases, which increases the shading difference of the previous image and makes the sleeve ghost more noticeable. As a result, it has been difficult to achieve both sleeve ghost and transferability. Therefore, the present inventors have found that sleeve ghosts can be suppressed by using an irregularly shaped additive as described in Patent Document 2. This is believed to be because the irregularly shaped additive has a high effect of scraping off the additive on the electrostatic latent image carrier, so that even when the same image is output, the image density difference is less likely to occur. However, when such irregularly shaped silica is supplied between the electrostatic latent image carrier and the cleaning blade, the number of contact points with each increases, and the static friction coefficient μ between the cleaning blade and the electrostatic latent image carrier increases. As a result, the cleaning blade is locally and momentarily deformed as if dragged by the electrostatic latent image carrier, and then momentarily returns to its original shape, causing so-called chatter (stick-slip), which can result in poor cleaning. In addition, as described in Patent Document 3, a method has been proposed in which a metal oxide having lubricity, such as zinc stearate, is added to reduce the static friction coefficient and suppress poor cleaning. However, when the amount of the metal oxide supplied to the cleaning blade decreases during a period of durability, such as that reached during long-term use, it has been difficult to improve the cleaning performance due to the above mechanism. For the above reasons, there is a trade-off between the sleeve ghost resistance and the cleaning ability, and it is urgent to develop a toner for electrophotography that can break away from this trade-off and achieve high image quality. That is, an object of the present invention is to provide a toner that satisfies all of the requirements for excellent transferability, sleeve ghost resistance, and cleaning ability. [Means for solving the problem]
[0005] As a result of extensive research, the inventors have found that by equating the adhesion rate with the metal oxide, as well as equating the charging series of the irregular additive and the metal oxide, it is possible to equate the supply rate of the irregular additive and the metal oxide supplied by the development bias, and this makes it possible to reduce sleeve ghosts even during durability testing, while also improving cleaning performance. By using the toner of the present invention, the supply rates of the irregularly shaped additive and the metal oxide supplied onto the cleaning blade are equivalent even during long-term use, which is believed to make it possible to reduce the aforementioned issues of chatter caused by excessive supply of the irregularly shaped additive and chatter caused by insufficient supply of the metal oxide during long-term use. That is, the present invention is directed to a toner particle containing silica particles A, and when the surface of the toner is observed using a scanning electron microscope, 1) The area of each silica particle A is 0.005 μm 2 More than 0.100μm 2 is as follows: 2) In a toner having a shape index of silica particles A calculated by the following formula (I), the density is 0.4 or more and 0.8 or less, the toner contains a fatty acid metal salt B, The silica in the toner particle the content Ca of A is 1.0 parts by mass or more and 3.0 parts by mass or less with respect to 100 parts by mass of the toner particles, The silica in the toner particle The adhesion rate Ka of A is 50% or more and 90% or less, a content Cb of the fatty acid metal salt B in the toner is 0.10 parts by mass or more and 0.60 parts by mass or less with respect to 100 parts by mass of the toner particles, the fatty acid metal salt B in the toner has a fixing rate Kb of 20% or more and 50% or less; The relationship between Ca, Ka, Cb, and Kb satisfies the following formula (II), The silica particleThe toner is characterized in that a surface potential difference C when a rubbing test is carried out using A and a fatty acid metal salt B is -70 V or more and +70 V or less. Formula (I) Density = (area of silica particle A) / (area of silica particle A surrounded by a convex hull) Formula (II) 2.00≦Ca×(100-Ka) / Cb×(100-Kb)≦20.00 Surface potential difference C = (surface potential D measured after rubbing a pellet prepared using the fatty acid metal salt B with the silica particles A and then the silica particles A are attached to the fatty acid metal salt B) - (surface potential E measured using a pellet obtained by rubbing a pellet prepared using the fatty acid metal salt B with the silica particles A and then removing the silica particles A with an air blower) Effect of the Invention
[0006] According to the present invention, it is possible to provide a toner having excellent transferability, resistance to sleeve ghosting, and cleanability. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is an explanatory diagram of an apparatus suitable for performing surface treatment on toner using hot air. [Diagram 2] FIG. 13 is an explanatory diagram of sleeve ghost evaluation on a halftone image. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In the present invention, the expressions "xx or more and xx or less" and "xx to xx" expressing a numerical range mean a numerical range including the lower and upper limit endpoints, unless otherwise specified.
[0009] The toner of the present invention contains toner particles and silica particles A, and when the surface of the toner is observed using a scanning electron microscope, the silica particles A have the following characteristics: 1) The area of each silica particle A is 0.005 μm 2 More than 0.100μm 2 is as follows: 2) In a toner having a shape index of silica particles A calculated by the following formula (I), the density is 0.4 or more and 0.8 or less, the toner contains a fatty acid metal salt B, the content Ca of the silica A in the toner is 1.0 parts by mass or more and 3.0 parts by mass or less; the adhesion rate Ka of the silica A in the toner is 50% or more and 90% or less; a content Cb of the fatty acid metal salt B in the toner is 0.10 parts by mass or more and 0.60 parts by mass or less with respect to 100 parts by mass of the toner particles, the fatty acid metal salt B in the toner has a fixing rate Kb of 20% or more and 50% or less; The relationship between Ca, Ka, Cb, and Kb satisfies the following formula (II), The toner is characterized in that a surface potential difference C when a rubbing test is carried out using the silica A and the fatty acid metal salt B is -70 V or more and +70 V or less. Formula (I) Density = (area of silica particle A) / (area of silica particle A surrounded by a convex hull) Formula (II) 2.00≦Ca×(100-Ka) / Cb×(100-Kb)≦20.00 Surface potential difference C = (surface potential D measured after rubbing a pellet prepared using the fatty acid metal salt B with the silica particles A and then the silica particles A are attached to the fatty acid metal salt B) - (surface potential E measured using a pellet obtained by rubbing a pellet prepared using the fatty acid metal salt B with the silica particles A and then removing the silica particles A with an air blower) It is.
[0010] As described above, in the toner described in Patent Document 1, it is difficult to achieve both transferability and resistance to sleeve ghosting simply by controlling the amount of silica particles added. Therefore, the silica particles used in the toner of the present invention have the following characteristics when the toner surface is observed using a scanning electron microscope: 1) The area of each silica particle A is 0.005 μm 2 More than 0.100μm 2The shape index, which is calculated by the following formula (I), is 0.4 or more and 0.8 or less. Formula (I) Density = (area of silica particle A) / (area of silica particle A surrounded by a convex hull)
[0011] The density is determined by observation and image analysis using a scanning electron microscope S-4800. In the same manner as above, an image of the toner surface is obtained using the S-4800.
[0012] The area of silica particle A is the value extracted by defining particles with an aspect ratio exceeding 1.2 among the high-brightness silica particles in the observation field using image analysis software, Image J.
[0013] Specifically, the area is measured as follows. Using particle analysis, the external additive particles (silica particles in this case) and toner particles in the image are color-coded through binarization. From the external additive particles, particles equivalent to external additive b (aspect ratio of 1.2 or less) are removed. For the remaining particles derived from external additive a, the area is displayed on the selection screen in the measurement settings. This operation is performed multiple times to find the average value of 100 particles, thereby calculating the area per particle of external additive a.
[0014] The solidity is a value calculated by the area of the external additive and the area of the external additive surrounded by the envelope, and is expressed by the following formula. In the image analysis software Image J (developed by Wayne Rasband), the solidity can be specified as a numerical range under the name Solidity. Density = (area of additive particle) / area of additive particle surrounded by envelope
[0015] The density is a quantity that takes a value between 0 and 1, and the smaller the value, the more recesses there are and the more intricate the shape. The specific measurement method is as follows.
[0016] 100 toner particles are selected that have a major axis R (μm) that satisfies the relationship 0.9≦R / D4≦1.1, where D4 (μm) is the weight-based circular equivalent weight average diameter of the toner measured using a particle size distribution measuring device "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.) described below, and a relatively flat portion of the toner surface (a field of view where the entire observation surface is in focus) is selected, and one field of view is observed for each toner particle, obtaining 100 images.
[0017] Image Analysis: From the obtained SEM observation images, the average density is calculated using the image processing software ImageJ (developed by Wayne Rashand). The calculation procedure is shown below. 1) Set the scale by selecting [Analyze]-[Set Scale]. 2) Set the threshold in [Image]-[Adjust]-[Threshold]. (Set to a value that eliminates noise and leaves behind the silica particles A to be measured.) 3) Use [Image]-[Crop] to select the image portion of silica particle A that was measured. 4) Overlapping silica particles are removed by image editing. 5) Invert the black and white image by selecting [Edit]-[Invert]. 6) In [Analyze]-[Set Measurements], check [Area], [Shape Descriptors], [Perimeter], [Fit Ellipse], and [Ferets Diameter]. Also, set [Redirect to] to [None] and [Decimal Place(0-9)] to 3. 7) [Analyze] - [Analyze Particle], set the particle area to 0.005μm 2 Specify the above and execute. 8) Obtain the solidity value of each particle specified in 7) above. 9) Measurements are made for 100 observed images, and the arithmetic mean value of the obtained solidity is calculated to be the density.
[0018] In the toner of the present invention, the content Ca of the silica particles A is 1.0 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the toner particles, and the adhesion rate Ka of the silica particles A is 50% or more and 90% or less.
[0019] If the content of the silica particles A is less than 1.0 part by mass, the anti-electrostatic adhesion is reduced, resulting in poor transferability, whereas if the content is more than 3.0 parts by mass, the amount of the silica particles A in the electrostatic latent image carrier becomes excessive, resulting in poor sleeve ghosting.
[0020] If the adhesion rate of the silica particles A is less than 50%, the amount of the silica particles A supplied to the electrostatic latent image carrier is too large, resulting in worsening of sleeve ghosting.If the adhesion rate is more than 90%, the amount of the silica particles A supplied to the cleaning blade is insufficient, resulting in a decrease in cleaning scraping performance, resulting in worsening of sleeve ghosting.
[0021] The adhesion rate Ka of the silica particles A is measured and calculated by the following method.
[0022] The glass bottle containing the sample is shaken in a Yayoi shaker at 200 rpm for 5 minutes. After shaking, the solution is transferred to a glass tube for a swing rotor (50 mL) and separated in a centrifuge at 3,500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. Visually check that the toner and aqueous solution are sufficiently separated, and collect the toner that has separated into the top layer with a spatula or similar. The collected toner is filtered with a vacuum filter and then dried in a dryer for at least 1 hour to obtain toner particles from which the external additives have been separated.
[0023] The adhesion rate is measured as follows. First, the amount of silica particles contained in the toner before the above separation process is quantified. This is done by measuring the Si element intensity: Si-B in the toner particles using a wavelength dispersive X-ray fluorescence analyzer Axios advanced (manufactured by PANalytical). Next, the Si element intensity: Si-A of the toner after the above separation process is measured in the same way. The adhesion rate is calculated as (Si-A / Si-B) x 100 (%).
[0024] The toner of the present invention contains a fatty acid metal salt B, the content Cb of the fatty acid metal salt B is 0.10 parts by mass or more and 0.60 parts by mass or less per 100 parts by mass of the toner particles, and the adhesion rate Kb of the fatty acid metal salt B is 20% or more and 50% or less.
[0025] If the content Cb of the fatty acid metal salt B is less than 0.10 parts by mass, the amount of the fatty acid metal salt B supplied to the cleaning blade is reduced, resulting in an increase in sleeve ghosting.If the content Cb is more than 0.60 parts by mass, the toner resistance is too low, resulting in a decrease in the amount of charge and a decrease in image density stability.
[0026] When the fixing rate Kb of the fatty acid metal salt B is lower than 20%, the supply rate of the fatty acid metal salt B supplied to the electrostatic latent image bearing member is high, so that the supply of the long-chain fatty acid B is insufficient during endurance testing, and chattering worsens during endurance testing.When the fixing rate Kb is higher than 50%, the cleaning performance worsens due to the shortage of fatty acid metal salt B supplied to the cleaning blade.
[0027] Moreover, the Ca, Ka, Cb, and Kb satisfy the following formula (II). Formula (II) 2.00≦Ca×(100-Ka) / Cb×(100-Kb)≦20.00
[0028] In this formula, the term Ca×(100-Ka) / Cb×(100-Kb) indicates the weight ratio of the silica particles A and the fatty acid metal salt B supplied onto the cleaning blade. When the value of this ratio is 2.00 or more and 20.00 or less, sleeve ghosting and cleaning performance are improved. When it is less than 2.00, the amount of fatty acid metal salt B supplied is large relative to the silica particles A, and when an image with a low image density is continuously output, the amount of fatty acid metal salt B supplied decreases, and cleaning performance is likely to deteriorate. When it is more than 20.00, the amount of fatty acid metal salt B supplied is insufficient relative to the amount of silica particles supplied, and cleaning performance is likely to deteriorate. In addition, the following formula (III) Formula (III) 5.00≦Ca×(100-Ka) / Cb×(100-Kb)≦10.00 If the above condition is satisfied, sleeve ghost during durability and cleaning properties are improved, which is preferable.
[0029] The toner of the present invention has a surface potential difference C of −70 V or more and +70 V or less when a rubbing test is carried out using the silica particles A and the fatty acid metal salt B. The rubbing test is carried out by the following method.
[0030] First, pellets are made using fatty acid metal salt B. For example, pellets can be made as follows. The fatty acid metal salt B is sandwiched between 40 μm thick PTFE sheets on a hot plate heated to a temperature higher than the melting point of the fatty acid metal salt (preferably 20°C above the melting point of the fatty acid metal salt, e.g. 150°C for zinc stearate), and pressure is applied with a hammer or other flat object to make the pellets. The dimensions of the pellets are approximately 2 cm long x 2 cm wide x 1 mm high.
[0031] Next, the surface of the produced pellet is neutralized by a static eliminator, which irradiates the pellet with weak X-rays (tube voltage 15 kV, irradiation angle 130°) from an X-ray generator (Photoionizer, manufactured by Hamamatsu Photonics KK) for 30 seconds to remove static electricity.
[0032] It is confirmed that no potential remains on the pellet by checking with a surface potential meter (Trek Japan Model 347) that the potential is between -70 V and +70 V. Here, the distance between the surface potential meter and the pellet is 1 cm.
[0033] Next, silica particles A are placed on the pellet, and the silica particles A are sandwiched between another similarly prepared pellet and the pellet, and rubbed back and forth 30 times.
[0034] Here, the surface potential of the pellet measured when the silica particles A are attached to the pellet is taken as surface potential D.
[0035] The silica particles A are removed by air blowing so as not to generate frictional electrification, and the surface potential measured using the pellets is taken as surface potential E.
[0036] By calculating the difference between the surface potential D and the surface potential E, it is possible to calculate the amount of potential possessed by the silica particle A.
[0037] That is, the triboelectric series of the fatty acid metal salt B and the silica particles A can be calculated by the following formula. Surface potential difference C = (surface potential D of a pellet measured after rubbing a pellet of fatty acid metal salt B with silica particles A and then removing silica particles A from the pellet) - (surface potential E measured using a pellet obtained by rubbing a pellet of fatty acid metal salt B with silica particles A and then removing silica particles A with an air blower)
[0038] By setting the surface potential difference C to -70 V to +70 V, the amounts of the silica particles A and the fatty acid metal salt B supplied to the electrostatic latent image bearing member are maintained at a constant ratio, so that it is possible to achieve both sleeve ghost prevention and cleaning performance.
[0039] The silica particles A of the present invention may be surface-treated, and the triboelectric series with the fatty acid metal salt B can be adjusted by adjusting the surface treatment agent, the amount of surface treatment, and the like.
[0040] Examples of the fatty acid metal salt B of the present invention include (higher) fatty acid metal salts such as zinc, lead, aluminum, copper, magnesium, calcium, etc. stearic acid salts, zinc, manganese, iron, copper, magnesium, etc. oleic acid salts, zinc, copper, magnesium, etc. palmitic acid salts, zinc, calcium, etc. linoleic acid salts, zinc, calcium, etc. ricinoleic acid salts, etc. Zinc stearate, which is easy to spread and has the highest degree of hydrophobicity, is preferred from the viewpoints of performance as a lubricant and electrostatic toner retention.
[0041] <Binding resin> The toner particles in the present invention may use the following polymers as the binder resin. Homopolymers of styrene and its substitutes, such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-based copolymers, such as styrene-p-chlorostyrene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-acrylic acid ester copolymer, and styrene-methacrylic acid ester copolymer; styrene-based copolymer resin, polyester resin, a mixture of polyester resin and vinyl resin, or a hybrid resin in which both are partially reacted; polyvinyl chloride, phenol resin, naturally modified phenol resin, naturally modified maleic acid resin, acrylic resin, methacrylic resin, polyvinyl acetate, silicone resin, polyester resin, polyurethane, polyamide resin, furan resin, epoxy resin, xylene resin, polyethylene resin, and polypropylene resin. Among these, polyester resin is preferably used as the main component from the viewpoint of low-temperature fixability.
[0042] As the monomers used in the polyester unit of the polyester resin, polyhydric alcohols (divalent or trivalent or higher alcohols), polyvalent carboxylic acids (divalent or trivalent or higher carboxylic acids), their acid anhydrides or their lower alkyl esters are used. Here, in order to create a branched polymer in order to express "strain hardening", it is effective to partially crosslink the amorphous resin molecule, and for this purpose, it is preferable to use a polyfunctional compound having a valence of three or more. Therefore, it is preferable to include a trivalent or higher carboxylic acid, its acid anhydride or its lower alkyl ester, and / or a trivalent or higher alcohol as the raw material monomer of the polyester unit.
[0043] As the polyhydric alcohol monomer used in the polyester unit of the polyester resin, the following polyhydric alcohol monomers can be used.
[0044] Examples of the dihydric alcohol component include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, and bisphenol represented by formula (A) and its derivatives;
[0045] [ka] (In the formula, R is an ethylene or propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 or more and 10 or less.)
[0046] Diols represented by formula (B);
[0047] [ka]
[0048] Examples of trihydric or higher alcohol components include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene. Among these, glycerol, trimethylolpropane, and pentaerythritol are preferably used. These dihydric alcohols and trihydric or higher alcohols can be used alone or in combination.
[0049] As the polybasic carboxylic acid monomer used in the polyester unit of the polyester resin, the following polybasic carboxylic acid monomers can be used.
[0050] Examples of divalent carboxylic acid components include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, n-octenylsuccinic acid, n-octylsuccinic acid, isooctylsuccinic acid, isooctylsuccinic acid, anhydrides of these acids, and lower alkyl esters thereof. Of these, maleic acid, fumaric acid, terephthalic acid, and n-dodecenylsuccinic acid are preferably used.
[0051] Examples of trivalent or higher carboxylic acids, their anhydrides or their lower alkyl esters include 1,2,4-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, their anhydrides or their lower alkyl esters. Among these, 1,2,4-benzenetricarboxylic acid, i.e., trimellitic acid or its derivatives, is particularly preferred because it is inexpensive and easy to control the reaction. These divalent carboxylic acids and trivalent or higher carboxylic acids can be used alone or in combination.
[0052] The method for producing the polyester unit of the present invention is not particularly limited, and a known method can be used. For example, the above-mentioned alcohol monomer and carboxylic acid monomer are simultaneously charged, and polymerized through an esterification reaction or an ester exchange reaction and a condensation reaction to produce a polyester resin. The polymerization temperature is not particularly limited, but is preferably in the range of 180°C to 290°C. For the polymerization of the polyester unit, for example, a polymerization catalyst such as a titanium-based catalyst, a tin-based catalyst, zinc acetate, antimony trioxide, or germanium dioxide can be used. In particular, the binder resin of the present invention is more preferably a polyester unit polymerized using a tin-based catalyst.
[0053] In addition, it is preferable from the viewpoint of suppressing fogging that the acid value of the polyester resin is 5 mgKOH / g or more and 20 mgKOH / g or less, and the hydroxyl value is 20 mgKOH / g or more and 70 mgKOH / g or less, since this can suppress the amount of moisture adsorption in a high temperature and high humidity environment and can keep the non-electrostatic adhesion low.
[0054] The binder resin may be a mixture of a low molecular weight resin and a high molecular weight resin. The content ratio of the high molecular weight resin to the low molecular weight resin is preferably 40 / 60 or more and 85 / 15 or less on a mass basis from the viewpoint of low temperature fixability and hot offset resistance.
[0055] <Release agent> Examples of waxes that can be used in the toner of the present invention include the following: hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes containing fatty acid esters as the main component such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax. Further examples include the following. Saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and valinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, hexamethylene Saturated fatty acid bisamides such as bisstearamide; unsaturated fatty acid amides such as ethylene bisoleamide, hexamethylene bisoleamide, N,N' dioleyl adipamide, and N,N' dioleyl sebacamide; aromatic bisamides such as m-xylene bisstearamide and N,N' distearyl isophthalamide; fatty metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.
[0056] Among these waxes, from the viewpoint of improving low-temperature fixing property and fixing separation property, preferred are hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax, and fatty acid ester waxes such as carnauba wax. In the present invention, the hydrocarbon waxes are more preferred from the viewpoint of further improving hot offset resistance.
[0057] In the present invention, the wax is preferably used in an amount of 3 parts by mass or more and 8 parts by mass or less per 100 parts by mass of the binder resin.
[0058] In addition, in an endothermic curve during temperature rise measured by a differential scanning calorimetry (DSC) device, the peak temperature of the maximum endothermic peak of the wax is preferably 45° C. or more and 140° C. or less. If the peak temperature of the maximum endothermic peak of the wax is within the above range, it is preferable because it is possible to achieve both storage stability and hot offset resistance of the toner.
[0059] <Coloring agent> The toner particles in the present invention may contain a colorant. Examples of the colorant include the following.
[0060] Examples of black colorants include carbon black, yellow colorants, magenta colorants, and cyan colorants used to tone the color to black. Although a pigment may be used alone as the colorant, it is more preferable to use a dye and a pigment in combination to improve the clarity of the colorant from the viewpoint of image quality of a full-color image.
[0061] Magenta toner pigments include the following: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.
[0062] Dyes for magenta toners include solvent dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1; basic dyes such as CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28.
[0063] Pigments for cyan toners include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45; copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton.
[0064] Dyes for cyan toners include CI Solvent Blue 70.
[0065] Yellow toner pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20.
[0066] Yellow toner dyes include CI Solvent Yellow 162.
[0067] These colorants can be used alone or in combination, or in the form of a solid solution. The colorant is selected in consideration of hue angle, chroma, brightness, light resistance, transparency on an OHP sheet, and dispersibility in a toner.
[0068] The content of the colorant is preferably 0.1 parts by mass or more and 30.0 parts by mass or less based on the total amount of the resin components.
[0069] <Inorganic fine particles> The toner in the present invention contains the above-mentioned silica particles A. If necessary, the toner may contain two or more types of fine particles corresponding to the silica particles A or other silica particles.
[0070] The inorganic fine particles may be added internally to the toner particles or may be mixed with the toner particles as an external additive, but it is necessary to design the silica particles A so that their adhesion rate is 50% or more and 90% or less.
[0071] As the external additive, in addition to silica particles, inorganic fine particles such as strontium titanate, titanium oxide, and aluminum oxide are preferred, and in particular, external additives with low resistance such as strontium titanate and titanium oxide are preferred from the viewpoint of preventing fogging and transferring efficiency, since they can suppress the change in the charge amount due to the temperature and humidity environment, suppress the localization of the charge of the toner, and reduce the electrostatic adhesion force. The inorganic fine particles are preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof.
[0072] The toner particles and the external additives can be mixed using a known mixer such as a Henschel mixer.
[0073] <Developer> The toner of the present invention can be used as a one-component developer, but in order to suppress localization of charge on the toner surface, it can also be mixed with a magnetic carrier and used as a two-component developer.
[0074] As the magnetic carrier, generally known carriers can be used, such as iron oxide; metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, and rare earth elements, alloy particles thereof, and oxide particles thereof; magnetic materials such as ferrite; and magnetic material-dispersed resin carriers (so-called resin carriers) that contain a magnetic material and a binder resin that holds the magnetic material in a dispersed state.
[0075] When the toner is mixed with a magnetic carrier to be used as a two-component developer, the mixing ratio of the magnetic carrier in this case is preferably 2% by mass or more and 15% by mass or less, and more preferably 4% by mass or more and 13% by mass or less, in terms of the toner concentration in the two-component developer.
[0076] <Toner manufacturing method> The method for producing toner particles is not particularly limited, but a pulverization method is preferred from the viewpoint of dispersing the release agent and the polymer in which a styrene-acrylic polymer is graft-polymerized onto a polyolefin. The reason is that when toner particles are produced in an aqueous medium, the release agent, which is highly hydrophobic, and the polymer in which a styrene-acrylic polymer is graft-polymerized onto a polyolefin tend to be localized inside the toner particles. Therefore, it becomes difficult to form a core-shell structure by the above-mentioned heat treatment device.
[0077] The procedure for producing the toner by the pulverization method will be described below.
[0078] In the raw material mixing process, materials constituting the toner particles, such as binder resin, release agent, colorant, crystalline polyester, and other components such as charge control agent as necessary, are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include double con mixers, V-type mixers, drum mixers, super mixers, Henschel mixers, Nauta mixers, and Mechano Hybrids (manufactured by Nippon Coke & Engineering Co., Ltd.).
[0079] Next, the mixed materials are melt-kneaded to disperse the wax in the binder resin. In the melt-kneading process, a batch-type kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of continuous production. For example, a KTK twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Iron Works Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. Furthermore, the resin composition obtained by melt-kneading may be rolled with a two-roller or the like, and cooled with water or the like in a cooling process.
[0080] The cooled resin composition is then pulverized to a desired particle size in a pulverization process, which involves coarse pulverization using a pulverizer such as a crusher, hammer mill, or feather mill, followed by further pulverization using a pulverizer such as a Cryptron System (Kawasaki Heavy Industries), a Super Rotor (Nisshin Engineering), a Turbo Mill (Turbo Kogyo), or an air jet type pulverizer.
[0081] Thereafter, as necessary, the mixture is classified using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), or a Faculty (manufactured by Hosokawa Micron Corporation).
[0082] Thereafter, the toner particles are surface-treated by heating to control the adhesion rate of the silica particles A and the fatty acid metal salt B and to increase the circularity of the toner. For example, the surface treatment can be performed by hot air using a surface treatment device shown in FIG.
[0083] The mixture supplied by the material supply means 1 is introduced into an introduction pipe 3, which is installed vertically to the material supply means, by compressed gas adjusted by a compressed gas adjustment means 2. The mixture passing through the introduction pipe is uniformly dispersed by a conical protruding member 4 installed in the center of the material supply means, and is introduced into eight supply pipes 5 that radiate outward, and then into a treatment chamber 6 where heat treatment is carried out.
[0084] At this time, the flow of the mixture supplied to the treatment chamber is regulated by a regulating means 9 for regulating the flow of the mixture provided in the treatment chamber. Therefore, the mixture supplied to the treatment chamber is heat-treated while swirling in the treatment chamber, and then cooled.
[0085] Hot air for heat-treating the supplied mixture is supplied from hot air supplying means 7, and is introduced into the treatment chamber by spirally swirling the hot air using a swirling member 13 for swirling the hot air. In terms of the configuration, the swirling member 13 for swirling the hot air has a plurality of blades, and the swirling of the hot air can be controlled by the number and angle of the blades. The hot air supplied into the treatment chamber preferably has a temperature of 100°C to 300°C at the outlet of the hot air supplying means 7. If the temperature at the outlet of the hot air supplying means is within the above range, it is possible to uniformly spheronize the toner particles while preventing the toner particles from fusing or coalescing due to excessive heating of the mixture.
[0086] The heat-treated toner particles are then cooled by cold air supplied from cold air supply means 8, and the temperature of the cold air supplied from cold air supply means 8 is preferably -20°C to 30°C. If the temperature of the cold air is within the above range, the heat-treated toner particles can be efficiently cooled, and the fusion and coalescence of the heat-treated toner particles can be prevented without impeding the uniform spheroidization of the mixture. The absolute moisture content of the cold air is 0.5 g / m3 More than 15.0g / m 3 It is preferable that:
[0087] Next, the cooled heat-treated toner particles are collected by the collecting means 10 at the bottom end of the processing chamber. A blower (not shown) is provided ahead of the collecting means, so that the toner particles are sucked and transported by the blower.
[0088] The powder particle supply port 14 is provided so that the swirling direction of the supplied mixture and the swirling direction of the hot air are the same, and the recovery means 10 of the surface treatment device is provided on the outer periphery of the treatment chamber so as to maintain the swirling direction of the swirled powder particles. Furthermore, the cold air supplied from the cold air supply means 8 is configured to be supplied from the outer periphery of the device to the circumferential surface inside the treatment chamber in a horizontal and tangential direction. The swirling directions of the toner supplied from the powder supply port, the swirling direction of the cold air supplied from the cold air supply means, and the swirling direction of the hot air supplied from the hot air supply means are all the same. Therefore, no turbulence occurs in the treatment chamber, the swirling flow in the device is strengthened, a strong centrifugal force is applied to the toner, and the dispersibility of the toner is further improved, so that a toner with a uniform shape and few coalesced particles can be obtained.
[0089] When the average circularity of the toner is 0.960 or more and 0.980 or less, the non-electrostatic adhesion can be kept low, which is preferable from the viewpoint of suppressing fogging.
[0090] Then, the fine powder side is divided into two parts, one for fine powder and the other for coarse powder. For example, the two parts are divided into two parts using an inertial classification system, Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.). A desired amount of silica fine particles A is externally added to the surface of each of the two heat-treated toner particles. Examples of the method of externally adding the toner particles include a method of stirring and mixing using a mixing device such as a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.), or a Nobilta (manufactured by Hosokawa Micron Corporation) as an external adder. In this case, an external additive other than silica fine particles, such as a fluidizing agent, may be externally added, if necessary.
[0091] The measurement methods for various physical properties of toner and raw materials will be described below.
[0092] <Measurement of peak molecular weight and weight average molecular weight of polymer in which styrene-acrylic polymer is graft-polymerized to binder resin and polyolefin by GPC> The molecular weight distribution of the THF-soluble component of the resin is measured by gel permeation chromatography (GPC) as follows.
[0093] First, dissolve the toner in tetrahydrofuran (THF) over 24 hours at room temperature. Then, filter the resulting solution through a solvent-resistant membrane filter "MAESORIDISC" with a pore size of 0.2 μm (manufactured by Tosoh Corporation) to obtain a sample solution. Incidentally, the sample solution is adjusted so that the concentration of the components soluble in THF is about 0.8 mass%. Using this sample solution, measurement is performed under the following conditions. Apparatus: HLC8120 GPC (Detector: RI) (manufactured by Tosoh Corporation) Column: 7-series of Shodex KF-801, 802, 803, 804, 805, 806, 807 (manufactured by Showa Denko KK) Eluent: Tetrahydrofuran (THF) Flow rate: 1.0 ml / min Oven temperature: 40.0 °C Sample injection volume: 0.10 ml
[0094] When calculating the molecular weight of the sample, a molecular weight calibration curve prepared using a standard polystyrene resin (for example, trade names "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.
[0095] <Measurement method for softening point of binder resin> The softening point is measured using a constant load extrusion type capillary rheometer "Flow property evaluation device Flow Tester CFT-500D" (Shimadzu Corporation) according to the manual that comes with the device. With this device, a constant load is applied from above the measurement sample by a piston while the measurement sample filled in a cylinder is heated and melted, and the molten measurement sample is extruded from a die at the bottom of the cylinder, and a flow curve showing the relationship between the piston descent amount and temperature can be obtained.
[0096] In the present invention, the "melting temperature in the 1 / 2 method" described in the manual attached to the "Flow characteristic evaluation device Flow Tester CFT-500D" is used as the softening point. The melting temperature in the 1 / 2 method is calculated as follows. First, 1 / 2 of the difference between the amount of piston descent Smax at the time when the outflow ends and the amount of piston descent Smin at the time when the outflow starts is calculated (this is designated as X; X=(Smax-Smin) / 2). Then, the temperature of the flow curve when the amount of piston descent on the flow curve is X is the melting temperature in the 1 / 2 method.
[0097] The measurement sample is prepared by compressing approximately 1.0 g of resin at approximately 10 MPa for approximately 60 seconds using a tablet molding machine (e.g., NT-100H, manufactured by NPA Systems) in an environment of 25°C to form a cylindrical shape with a diameter of approximately 8 mm.
[0098] The measurement conditions for the CFT-500D are as follows. Test mode: Temperature rise method Starting temperature: 50℃ Achieved temperature: 200℃ Measurement interval: 1.0℃ Heating rate: 4.0℃ / min Piston cross-sectional area: 1.000cm 2 Test load (piston load): 10.0kgf (0.9807MPa) Preheat time: 300 seconds Die hole diameter: 1.0mm Die length: 1.0mm
[0099] <Measurement of glass transition temperature (Tg) of binder resin> The glass transition temperature and the melting peak temperature are measured using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments) in accordance with ASTM D3418-82.
[0100] The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction.
[0101] Specifically, about 3 mg of resin or toner is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and measurement is performed under the following conditions. Heating rate: 10℃ / min Measurement start temperature: 30℃ End of measurement temperature: 180℃
[0102] Measurements are performed at a heating rate of 10°C / min in the measurement range of 30 to 180°C. The temperature is raised to 180°C once and held for 10 minutes, then cooled to 30°C, and then raised again. During this second heating process, the specific heat change is obtained in the temperature range of 30 to 100°C. The point at which the line midway between the baselines before and after the specific heat change appears and the differential thermal curve intersects is taken as the glass transition temperature (Tg) of the resin.
[0103] <Method for measuring number-average particle size (D1) of primary particles of inorganic fine particles> The number average particle size of the primary particles of the external additive is measured using a transmission electron microscope (TEM) "JEM2800" (manufactured by JEOL Ltd.).
[0104] First, a measurement sample is prepared. 1 mL of isopropanol is added to approximately 5 mg of external additive, and the mixture is dispersed for 5 minutes using an ultrasonic disperser (ultrasonic cleaner). Next, a drop of the above dispersion liquid is placed on a microgrid (150 mesh) with a support film for TEM, and the mixture is dried to prepare a measurement sample.
[0105] Next, images are taken using a transmission electron microscope (TEM) at an accelerating voltage of 200 kV and a magnification (e.g., 200k to 1M) that allows sufficient measurement of the external additive in the field of view, and the particle size of 100 randomly selected primary particles of the external additive is measured to determine the number average particle size. The particle size of the primary particles may be measured manually or using a measuring tool.
[0106] <Method of measuring weight average particle size (D4) of toner particles> The weight average particle diameter (D4) of the toner particles is calculated as follows. The measuring device used is a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). Measurements were performed with an effective measurement channel count of 25,000 channels, and the measurement data was analyzed and calculated.
[0107] The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1 mass %, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.).
[0108] Before carrying out the measurements and analyses, the dedicated software was set up as follows.
[0109] In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, the total count number in the control mode was set to 50,000 particles, the number of measurements was set to 1, and the Kd value was set to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter, Inc.). The threshold and noise level were automatically set by pressing the threshold / noise level measurement button. In addition, the current was set to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and the aperture tube flush after measurement was checked.
[0110] In the "Pulse to particle size conversion setting screen" of the dedicated software, the bin interval was set to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.
[0111] The specific measurement method is as follows. (1) Approximately 200 mL of the electrolyte solution was placed in a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, which was then set on the sample stand. The stirrer rod was stirred counterclockwise at 24 revolutions per second. Dirt and air bubbles in the aperture tube were then removed in advance using the "aperture flush" function of the analysis software. (2) About 30 mL of the aqueous electrolyte solution was placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of a dilution obtained by diluting the below-mentioned "Contaminon N" three times by mass with ion-exchanged water was added thereto as a dispersant. Contaminon N: A 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd. (3) A predetermined amount of ion-exchanged water was placed in the water tank of an ultrasonic disperser "Ultrasonic Dispension System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 mL of the above-mentioned Contaminon N was added to this water tank. (4) The beaker (2) was set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser was operated. Then, the height of the beaker was adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker was maximized. (5) In the state where the electrolyte solution in the beaker in (4) was irradiated with ultrasonic waves, about 10 mg of toner was added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment was continued for another 60 seconds. During the ultrasonic dispersion, the water temperature in the water tank was appropriately adjusted to be 10°C or higher and 40°C or lower. (6) The electrolyte solution (5) in which the toner was dispersed was dropped using a pipette into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration was adjusted to about 5%. Then, the measurement was continued until the number of particles measured reached 50,000. (7) The measurement data was analyzed using the dedicated software that came with the device, and the weight-average particle size (D4) was calculated. Note that the "average diameter" on the analysis / volume statistics (arithmetic mean) screen when the dedicated software was set to graph / volume% was used as the weight-average particle size (D4).
[0112] <Method for measuring average circularity of toner> The average circularity of the toner is measured using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions during the calibration process.
[0113] The measurement principle of the flow-type particle image analyzer "FPIA-3000" (Sysmex Corporation) is to capture still images of flowing particles and perform image analysis. The sample added to the sample chamber is sent to the flat sheath flow cell by the sample suction syringe. The sample sent to the flat sheath flow is sandwiched between the sheath liquid and forms a flat flow. The sample passing through the flat sheath flow cell is irradiated with a strobe light at 1 / 60 second intervals, making it possible to capture still images of the flowing particles. In addition, since the flow is flat, the image is captured in focus. The particle images are captured by a CCD camera, and the captured images are processed with an image processing resolution of 512 x 512 pixels (0.37 x 0.37 μm per pixel), and the contours of each particle image are extracted, and the projected area S and perimeter L of the particle image are measured.
[0114] Next, the equivalent circle diameter and circularity are calculated using the above area S and perimeter L. The equivalent circle diameter is the diameter of a circle having the same area as the projected area of the particle image, and the circularity is defined as the perimeter of the circle calculated from the equivalent circle diameter divided by the perimeter of the projected particle image, and is calculated using the following formula. Circularity = 2 × (π × S) 1 / 2 / L
[0115] When the particle image is circular, the circularity is 1.000, and the greater the degree of unevenness on the outer periphery of the particle image, the smaller the circularity value. After calculating the circularity of each particle, the range of circularity between 0.200 and 1.000 is divided into 800, the arithmetic mean of the resulting circularities is calculated, and this value is the average circularity.
[0116] The specific measurement method is as follows.
[0117] First, about 20 mL of ion-exchanged water from which impurities such as solids have been removed is placed in a glass container, and about 0.2 mL of a solution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made from a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries) diluted about three times by mass with ion-exchanged water is added as a dispersant.
[0118] Furthermore, about 0.02 g of the measurement sample is added, and the dispersion is treated for 2 minutes using an ultrasonic disperser to obtain a dispersion liquid for measurement. At this time, the temperature of the dispersion liquid is appropriately cooled so that it is 10°C or higher and 40°C or lower. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser ("VS-150" (manufactured by Vervoclear Co., Ltd.)) with an oscillation frequency of 50 kHz and an electrical output of 150 W is used, and a predetermined amount of ion-exchanged water is placed in the water tank, and about 2 mL of the Contaminon N is added to the water tank.
[0119] For the measurement, the flow type particle image analyzer equipped with a standard objective lens (10x) is used, and the particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid. The dispersion liquid prepared according to the procedure is introduced into the flow type particle image analyzer, and 3000 toner particles are measured in HPF measurement mode and total count mode.
[0120] The binarization threshold for particle analysis is set to 85%, the analysis particle diameter is set to a circle-equivalent diameter of 1.98 μm to 39.96 μm, and the average circularity of the toner is calculated.
[0121] Before starting the measurement, automatic focus adjustment is performed using standard latex particles (e.g., Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water). After that, it is preferable to perform focus adjustment every 2 hours from the start of the measurement. EXAMPLES
[0122] The present invention will be described in more detail below using examples and comparative examples, but the aspects of the present invention are not limited thereto. Note that the number of parts in the examples and comparative examples is based on mass unless otherwise specified.
[0123] <Production Example of Silica Particle A> In a 3-liter glass reactor equipped with a stirrer, a dropping funnel, and a thermometer, 590.0 g of methanol, 42.0 g of water, and 48.0 g of 28% by mass ammonia water were added and mixed. The obtained solution was adjusted to 35°C, and while stirring, 1100.0 g (7.23 mol) of tetramethoxysilane and 395.0 g of 5.5% by mass ammonia water were added simultaneously. Tetramethoxysilane was added dropwise over 6 hours, and ammonia water was added dropwise over 5 hours. After the dropping was completed, stirring was continued for another 0.5 hours to perform hydrolysis, thereby obtaining a methanol-water dispersion of hydrophilic spherical sol-gel silica particles. Next, an ester adapter and a cooling tube were attached to the glass reactor, and the dispersion was thoroughly dried at 80°C under reduced pressure. The obtained silica particles were heated in a thermostatic bath at 400°C for 10 minutes.
[0124] The above process was repeated several tens of times, and the obtained silica particles were subjected to a pulverizing treatment using a pulverizer (manufactured by Hosokawa Micron Corporation).
[0125] Then, 500 g of silica particles were placed in a 1000 ml polytetrafluoroethylene inner cylinder stainless steel autoclave. After replacing the inside of the autoclave with nitrogen gas, the stirring blade attached to the autoclave was turned on at 6.6 s. -1While rotating at (rpm), 0.5 g of HMDS (hexamethyldisilazane) and 0.1 g of water were sprayed uniformly onto the silica powder in the form of mist using a two-fluid nozzle. After stirring for 30 minutes, the autoclave was sealed and heated at 220°C for 2 hours. Next, the system was depressurized while still heated to perform a deammoniating treatment, and silica particles A (silica particles A-1) were obtained.
[0126] Moreover, the area and density of the silica particles A were controlled by adjusting the amount of tetramethoxysilane added, and silica particles A-2 to A-4 were obtained in the same manner.
[0127] Silica particles A-5 were obtained in the same manner as for silica particles A-1, except that tetramethoxysilane was changed to dimethyldichlorosilane.
[0128] The physical properties of silica particles A are shown in Table 1.
[0129] [Table 1]
[0130] <Production Example of Zinc Stearate Fine Particles> <Production Example of Fatty Acid Metal Salt B-1> A receiving vessel equipped with an agitator was prepared, and the agitator was rotated at 350 rpm. 500 parts of 0.5% by mass sodium stearate aqueous solution was added to the receiving vessel, and the liquid temperature was adjusted to 85°C. Next, 525 parts of 0.2% by mass zinc sulfate aqueous solution was dropped into the receiving vessel over 15 minutes. After the entire amount was added, the mixture was aged for 10 minutes at the reaction temperature to terminate the reaction.
[0131] Next, the fatty acid metal salt slurry thus obtained was filtered and washed. The fatty acid metal salt cake obtained after washing was crushed roughly, and then dried at 105°C using a continuous instantaneous airflow dryer. Then, it was pulverized in a nano grinding mill [NJ-300] (manufactured by Sunrex Co., Ltd.) under conditions of an air volume of 6.0 m3 / min and a processing speed of 80 kg / h, and then reslurried and removed fine particles and coarse particles using a wet centrifugal classifier, and then dried at 80°C using a continuous instantaneous airflow dryer to obtain fatty acid metal salt B-1. The volume-based median diameter (D50) of the obtained fatty acid metal salt B-1 was 0.45 μm, and the number-average particle size (D1) was 0.31 μm.
[0132] <Production Example of Fatty Acid Metal Salt B-2> Fatty acid metal salt B-2 was obtained in the same manner as fatty acid metal salt B-1, except that zinc stearate was replaced with lead stearate. The volume-based median diameter (D50) of the obtained fatty acid metal salt B-2 was 0.67 μm, and the number-average particle diameter (D1) was 0.51 μm.
[0133] <Production Example of Fatty Acid Metal Salt B-3> The fatty acid metal salt B-3 was obtained in the same manner as the fatty acid metal salt B-1, except that zinc stearate was replaced with zinc laurate. The volume-based median diameter (D50) of the obtained fatty acid metal salt B-3 was 0.57 μm, and the number-average particle diameter (D1) was 0.40 μm.
[0134] <Binding resin: Production example of polyester resin> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 73.8 parts (0.19 moles; 100.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 12.5 parts (0.08 moles; 48.0 mol% based on the total number of moles of polycarboxylic acids) Adipic acid: 7.8 parts (0.05 moles; 34.0 mol% based on the total number of moles of polycarboxylic acids) Titanium tetrabutoxide (esterification catalyst): 0.5 parts The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 2 hours at a temperature of 200°C with stirring.
[0135] Furthermore, the pressure inside the reaction vessel was reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 160 and returned to atmospheric pressure (first reaction step). Trimellitic acid: 5.9 parts (0.03 moles; 18.0 mole % based on the total number of moles of polycarboxylic acids) tert-Butylcatechol (polymerization inhibitor): 0.1 parts After that, the above materials were added, the pressure in the reaction vessel was lowered to 8.3 kPa, and the reaction was carried out for 15 hours while maintaining the temperature at 200°C. After confirming that the softening point measured according to ASTM D36-86 reached 120°C, the temperature was lowered to stop the reaction. eye( Second reaction step), binding bond Fat The obtained binding tree Fat The peak molecular weight Mp was 10,000, the softening point Tm was 110°C, and the glass transition temperature Tg was 60°C.
[0136] <Toner 1 Manufacturing Example> Binding resin 100 parts Fischer-Tropsch wax (maximum endothermic peak temperature 90℃) 4 parts 0.3 parts of 3,5-di-t-butylsalicylic acid aluminum compound (Bontron E88, manufactured by Orient Chemical Industry Co., Ltd.) Carbon black 10 parts The above materials were mixed using a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 1500 rpm for a rotation time of 5 min, and then kneaded using a twin-screw kneader (PCM-30, manufactured by Ikegai Co., Ltd.) set at a temperature of 130°C. The kneaded product obtained was cooled and coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The coarsely crushed product obtained was finely crushed using a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). Further, classification was performed using a Faculty (F-300, manufactured by Hosokawa Micron Corporation), and toner base particles 1 were obtained. The operating conditions were a classification rotor rotation speed of 11000 rpm and a dispersion rotor rotation speed of 7200 rpm.
[0137] 100 parts of toner base particles Silica fine particles A-1 2.5 parts Fatty acid metal salt B-1 0.3 parts The raw materials shown in the above recipe were mixed using a Henschel mixer (FM-10C type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 1900 rpm for a rotation time of 3 minutes, and then heat-treated using the surface treatment device shown in Figure 1 to obtain heat-treated toner particles 1. The operating conditions were feed rate = 5 kg / hr, hot air temperature = 160°C, and hot air flow rate = 6 m 3 / min., cold air temperature = -5℃, cold air flow rate = 4m 3 / min., Blower air volume = 20m 3 / min., Injection air flow rate = 1m 3 / min.
[0138] Heat-treated toner particles 1 100 parts Silica fine particles C (number average particle size (D1) is 20 nm) 0.6 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 1900 rpm for a rotation time of 3 minutes to obtain Toner 1.
[0139] <Toner 2 Manufacturing Example> Toner 2 was obtained in the same manner as in the production example of toner 1, except that the surface treatment device was not used and the raw materials were mixed in a Henschel mixer at a rotation speed of 1900 rpm for a rotation time of 10 minutes.
[0140] <Toner 3-18, 20-25 manufacturing examples> Toners 3 to 18 and 20 to 25 were obtained by the same procedure as in the production example of toner 1, except that the amount of strontium titanate added, particle size, surface treatment, and the silica particles, particle size, and amount of added were changed as shown in Tables 1 and 2.
[0141] <Production Example of Toner 19> Toner 19 was obtained in the same manner as in the production example of toner 2, except that the raw materials were mixed using a Henschel mixer at a rotation speed of 1900 rpm for a rotation time of 3 minutes.
[0142] The physical properties of Toners 1 to 25 are shown in Table 2.
[0143] [Table 2]
[0144] <Production Example of Magnetic Core Particle 1> Step 1 (weighing and mixing): Fe 2 O 3 62.7 copies MnCO 3 29.5 copies Mg(OH) 2 6.8 parts SrCO 3 1.0 copies The ferrite raw materials were weighed so as to obtain the above composition ratio, and then pulverized and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch.
[0145] Step 2 (Pre-firing): The obtained pulverized material was made into pellets of about 1 mm square using a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the calcined ferrite obtained was as follows: (MnO) a (MgO) b (SrO) c (Fe 2 O 3 ) d In the above formula, a = 0.257, b = 0.117, c = 0.007, d = 0.393
[0146] Step 3 (Crushing): The obtained calcined ferrite was crushed to about 0.3 mm using a crusher, and then 30 parts of water were added to 100 parts of the calcined ferrite and crushed in a wet ball mill using zirconia beads with a diameter of 1 / 8 inch for 1 hour. The obtained slurry was crushed in a wet ball mill using alumina beads with a diameter of 1 / 16 inch for 4 hours to obtain a ferrite slurry (finely crushed calcined ferrite).
[0147] ·Process 4 (granulation process): To the ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 2.0 parts of polyvinyl alcohol as a binder were added per 100 parts of calcined ferrite, and the mixture was granulated into spherical particles using a spray dryer (manufacturer: Okawara Kakoki). After adjusting the particle size of the resulting particles, the mixture was heated at 650°C for 2 hours in a rotary kiln to remove the organic components of the dispersant and binder.
[0148] Step 5 (firing): In order to control the firing atmosphere, the material was heated from room temperature to 1300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at 1150°C for 4 hours. The material was then cooled to 60°C over a period of 4 hours, returned from the nitrogen atmosphere to the air, and removed at a temperature of 40°C or less.
[0149] Step 6 (sorting step): After crushing the agglomerated particles, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic core particles 1 having a volume distribution standard 50% particle size (D50) of 37.0 μm.
[0150] <Preparation of Coating Resin 1> Cyclohexyl methacrylate monomer 26.8% by mass Methyl methacrylate monomer 0.2% by mass Methyl methacrylate macromonomer 8.4% by mass (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene 31.3% by mass Methyl ethyl ketone 31.3% by mass Azobisisobutyronitrile 2.0% by mass Among the above materials, cyclohexyl methacrylate monomer, methyl methacrylate monomer, methyl methacrylate macromonomer, toluene, and methyl ethyl ketone were placed in a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer, and nitrogen gas was introduced to create a sufficient nitrogen atmosphere. After that, the mixture was heated to 80°C, azobisisobutyronitrile was added, and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction product to precipitate the copolymer, and the precipitate was filtered and then dried in vacuum to obtain coating resin 1.
[0151] Next, 30 parts of coating resin 1 was dissolved in 40 parts of toluene and 30 parts of methyl ethyl ketone to obtain polymer solution 1 (solid content 30% by mass).
[0152] <Preparation of coating resin solution 1> Polymer solution 1 (resin solids concentration 30%) 33.3% by mass Toluene 66.4% by mass Carbon black Regal 330 (Cabot) 0.3% by mass (Primary particle size 25 nm, nitrogen adsorption specific surface area 94 m2 / g, DBP oil absorption 75mL / 100g) The mixture was dispersed for 1 hour using a paint shaker with zirconia beads having a diameter of 0.5 mm. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.
[0153] <Magnetic Carrier 1 Manufacturing Example> (Resin coating process): Magnetic core particles 1 and coating resin solution 1 were put into a vacuum degassing kneader maintained at room temperature (the amount of coating resin solution put in was 2.5 parts as resin component for 100 parts of magnetic core particles 1). After putting in, it was stirred at a rotation speed of 30 rpm for 15 minutes, and after the solvent had evaporated to a certain extent (80 mass%) or more, it was heated to 80°C while mixing under reduced pressure, and toluene was distilled off over 2 hours, and then cooled. The obtained magnetic carrier was separated into low magnetic products by magnetic separation, passed through a sieve with an opening of 70 μm, and then classified with a wind classifier to obtain magnetic carrier 1 with a 50% particle size (D50) of 38.2 μm based on volume distribution.
[0154] <Production example of two-component developer 1> 92.0 parts of magnetic carrier 1 and 8.0 parts of toner 1 were mixed in a V-type mixer (V-20, manufactured by Seishin Enterprise Co., Ltd.) to obtain two-component developer 1.
[0155] <Production examples of two-component developers 2 to 25> In the production example of two-component developer 1, the same operation was carried out except for the changes shown in Table 3, to obtain two-component developers 2 to 25.
[0156] [Table 3]
[0157] Example 1 The above two-component developer 1 was used to carry out the evaluation described below.
[0158] [Transferability] Paper: GF-C081 (81.0g / m 2 ) (Canon Marketing Japan Inc.) Toner load on solid image: 0.35mg / cm 2 Primary transfer current: 30μA Test environment: Normal temperature and humidity (temperature 23°C / humidity 50% RH) Process speed: 377mm / sec
[0159] A commercially available full-color digital copier (CLC1100, manufactured by Canon Inc.) was used, and the two-component developer 1 was placed in a cyan developer container, and the evaluation described below was carried out.
[0160] The toner remaining on the photoconductor after the primary transfer and the toner before the primary transfer were each taped and peeled off with transparent polyester adhesive tape. The peeled adhesive tape was applied to a piece of paper, and the density was measured with a spectrodensitometer 500 series (X-Rite Corporation).
[0161] The rate of change between the image density before the primary transfer and the image density of the residual image obtained as described above was taken as the transfer efficiency, and was evaluated based on the following evaluation criteria. A score of B or higher was determined to be indicative of the effect of the present invention. A: Transfer efficiency: 90% or more B: Transfer efficiency: 80% or more but less than 90% C: Transfer efficiency: less than 80%
[0162] [Sleeve Ghost Review] Sleeve ghosting was evaluated in a low temperature and low humidity environment (15°C, 10% RH) as follows. Ta.
[0163] After 999 sheets of a test chart with a solid black vertical band and solid white except for the vertical band were printed in succession, the 1000th sheet was printed with a full halftone image within the same job.
[0164] On the halftone image, the image density was measured in the area (a) where the solid black vertical band was passed and the area (b) where the solid white was passed in Figure 2, and the sleeve ghost was evaluated based on the difference in density. Note that areas (a) and (b) are within the range of the first revolution of the sleeve.
[0165] The image density was measured using an X-Rite color reflection densitometer (X-rite 500 Series, manufactured by X-rite Corporation). A: The density difference between area (a) and area (b) is less than 0.02. B: The density difference between area (a) and area (b) is 0.02 or more and less than 0.06. C: The density difference between area (a) and area (b) is 0.06 or more.
[0166] [Evaluation of cleaning ability] The cleaning performance was evaluated as follows: The pressure of the cleaning member against the photoreceptor was changed to 0.52 N (0.53 kgf), and 100,000 sheets of A4 character chart with a print rate of 5% were continuously printed in a low temperature and low humidity environment (15°C / 10% RH). The occurrence of vertical streaks due to poor cleaning was checked on the image during paper feed, and the state of contamination of the charging member by toner and external additives was checked after the endurance paper feed was completed, and the evaluation was based on the following criteria. A: No image defects due to poor cleaning were observed throughout the paper feed durability test, and the contamination state of the charging member after the paper feed durability test was also good. B: No image defects due to poor cleaning were observed throughout the paper feed durability test, but slight contamination was observed on the charging member after the paper feed durability test was completed. C: No image defects due to poor cleaning were observed throughout the paper feed durability test, but contamination was observed on the charging member after the paper feed durability test was completed. D: During paper feed durability, image defects were observed due to poor cleaning.
[0167] [Evaluation of image density stability] Using a modified Canon Inc. digital electrophotographic device "image RUNNER ADVANCE C5560" (product name), the development bias was set so that the initial reflection density was 1.4, and a continuous paper feed test was conducted up to 100,000 sheets in a H / H environment with a solid white image with a print ratio of 0%. After 100,000 sheets, an original image with 20mm square solid black patches arranged in five places within the development area was output, and the image density stability was evaluated by comparing the density difference of the image density after the continuous paper feed test with the initial image density of the five-point average density.
[0168] The image density was measured using a Macbeth Reflection Densitometer RD918 (manufactured by Macbeth Co.) as a relative density to the image in the white background portion where the document density was 0.00. A: Density difference less than 0.10 B: Density difference 0.10 or more and less than 0.30 C: Concentration difference 0.30 or more
[0169] [Examples 2 to 15 and Comparative Examples 1 to 10] Except for using two-component developers 2 to 25, evaluation was performed in the same manner as in Example 1. The evaluation results are shown in Table 4.
[0170] [Table 4] [Explanation of symbols]
[0171] 1. raw material fixed quantity supply means, 2. compressed gas flow rate adjustment means, 3. introduction pipe, 4. protruding member, 5. supply pipe, 6. treatment chamber, 7. hot air supply means, 8. cold air supply means, 9. regulating means, 10. recovery means, 11. hot air supply means outlet, 12. distribution member, 13. swirling member, 14. powder particle supply port
Claims
1. The toner contains toner particles and silica particles A, and when the surface of the toner is observed using a scanning electron microscope, the silica particles A have the following characteristics: 1) The area of each silica particle A is 0.005 μm 2 0.100 μm or more 2 is as follows: 2) In a toner having a shape index of silica particles A calculated by the following formula (I), the density is 0.4 or more and 0.8 or less, the toner contains a fatty acid metal salt B, a content Ca of the silica particles A in the toner is 1.0 parts by mass or more and 3.0 parts by mass or less with respect to 100 parts by mass of the toner particles, the adhesion rate Ka of the silica particles A in the toner is 50% or more and 90% or less; the content Cb of the fatty acid metal salt B in the toner is 0.10 parts by mass or more and 0.60 parts by mass or less with respect to 100 parts by mass of the toner particles, the fatty acid metal salt B in the toner has a fixing rate Kb of 20% or more and 50% or less; The relationship between Ca, Ka, Cb, and Kb satisfies the following formula (II), The toner is characterized in that a surface potential difference C when a rubbing test is carried out using the silica particles A and the fatty acid metal salt B is -70 V or more and +70 V or less. Formula (I) Density=(area of silica particle A) / (area of silica particle A surrounded by a convex hull) Formula (II) 2.00≦Ca×(100-Ka) / Cb×(100-Kb)≦20.00 Surface potential difference C=(surface potential D measured after rubbing a pellet prepared using the fatty acid metal salt B with the silica particles A and then the silica particles A are attached to the fatty acid metal salt B)−(surface potential E measured using a pellet obtained by rubbing a pellet prepared using the fatty acid metal salt B with the silica particles A and then removing the silica particles A with an air blower).
2. 2. The toner according to claim 1, wherein said fatty acid metal salt B is zinc stearate.
3. The toner according to claim 1 or 2, which satisfies formula (III). Formula (III) 5.00≦Ca×(100-Ka) / Cb×(100-Kb)≦10.00
Citation Information
Patent Citations
Toner composition
JP1988096664A
Image forming apparatus, and process cartridge
JP2015014650A
Image forming method
JP2015121671A
Toner and method for manufacturing toner
JP2016110095A
Toner and image forming method
JP2016142760A