toner

The toner particles with organic-inorganic composite particles address the challenges of high developability, low-temperature fixability, and storage stability by using inorganic fine particles with a hydrophobicity of 50% or more, exposed on the surface, forming convex portions, and a crystalline resin core and amorphous thermoplastic resin shell, enhancing adhesion and stability in harsh environments.

JP7562350B2Active Publication Date: 2024-10-07CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020156569
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-17
Publication Date
2024-10-07
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Existing toners face challenges in achieving high developability, low-temperature fixability, and storage stability under high temperature and high humidity conditions, particularly in regions like Southeast Asia and the Middle East.

Method used

The development of toner particles with a binder resin and an external additive comprising organic-inorganic composite particles, where inorganic fine particles with a hydrophobicity of 50% or more are exposed on the surface, forming convex portions, and having a median diameter of 80 nm to 500 nm, combined with a crystalline resin core and amorphous thermoplastic resin shell.

Benefits of technology

The toner exhibits improved low-temperature fixability and storage stability under high temperature and high humidity conditions, maintaining adhesion to paper and preventing fusion with other toner particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562350000001
    Figure 0007562350000001
  • Figure 0007562350000002
    Figure 0007562350000002
Patent Text Reader

Abstract

To provide a toner excellent in low temperature fixability and storage stability.SOLUTION: A toner has toner particles having a binder resin and a colorant, and an external additive. The external additive is organic-inorganic complex particles including inorganic fine particles, a crystalline resin, and an amorphous thermoplastic resin. The organic-inorganic complex particles each have a core that contains the crystalline resin and a shell that contains the amorphous thermoplastic resin. The degree of hydrophobization of the inorganic fine particles is 50% or more. At least part of the inorganic fine particles are exposed on the surface of the organic-inorganic complex particle to form convex parts. The median diameter of the organic-inorganic complex particles is 80 nm-500 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in an image forming method such as an electrophotographic method. To Regarding. [Background technology]

[0002] Electrophotographic image forming apparatuses are required to operate at high speed, have a long life, and save energy, and in order to meet these demands, toners are also required to have further improved performance in various aspects. In particular, for a long life, it is important that the toner's developability is maintained even after long-term use. In addition, from the viewpoints of speed and energy saving, toners are required to have further improved low-temperature fixability.

[0003] Furthermore, as the market expands, the frequency of use of electrophotographic image forming apparatuses is also increasing in hot and humid regions such as Southeast Asia and the Middle East. Therefore, the storage stability of toner when left under high temperature and high humidity conditions assumed in such regions is also becoming important.

[0004] Therefore, various toners have been proposed in order to satisfy the requirements for stable developing performance over a long period of time, further improvement in low-temperature fixing performance, and storage stability under high-temperature and high-humidity conditions.

[0005] For example, Patent Document 1 proposes reducing the environmental dependency of toner by externally adding composite particles in which inorganic fine particles are embedded in the surfaces of resin fine particles to toner particles.Furthermore, Patent Document 2 proposes that the low-temperature fixability of toner can be improved by using an external additive for toner made of composite particles in which inorganic fine particles are embedded in crystalline resin particles. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-15868 A [Patent Document 2] JP 2015-45859 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors have conducted extensive research into the toners described in the above-mentioned Patent Documents 1 and 2. As a result, the external additive and the toner using the same according to Patent Document 1 have a coating layer of the external additive formed using a thermosetting resin, so there is still room for improvement in the low-temperature fixability of the toner using this external additive. Also, the toner according to Patent Document 2 has still room for improvement in storage stability under high temperature and high humidity conditions.

[0008] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a toner which is excellent in low-temperature fixing property and also excellent in storage stability under high-temperature and high-humidity conditions. [Means for solving the problem]

[0009] The present invention relates to toner particles having a binder resin and a colorant, and a toner having an external additive, the external additive being organic-inorganic composite particles containing inorganic fine particles, a crystalline resin, and an amorphous thermoplastic resin, the organic-inorganic composite particles having a core containing the crystalline resin and a shell containing the amorphous thermoplastic resin, the inorganic fine particles having a hydrophobicity of 50% or more, at least a part of the inorganic fine particles being exposed on the surface of the organic-inorganic composite particles to form convex portions, and the organic-inorganic composite particles having a median diameter of 80 nm to 500 nm. The thermoplastic resin is a styrene-(meth)acrylic acid copolymer. The present invention relates to a toner characterized by: Effect of the Invention

[0010] By using the toner of the present invention, good low-temperature fixability can be obtained, and excellent storage stability can be obtained even under high-temperature and high-humidity conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. As described above, there is a demand for toners that satisfy a higher level of excellent developability, low-temperature fixability, and storage stability under high-temperature and high-humidity conditions.

[0012] When the viscosity of toner particles (meaning the toner base) is reduced in order to improve low-temperature fixability, the developability and storage stability under high temperature and high humidity may be reduced. In addition, a large amount of inorganic fine particles may be externally added in order to maintain the developability of the toner as the electrophotographic image forming process is accelerated. Although such a toner has good developability and storage stability under high temperature and high humidity, it may have poor low-temperature fixability. Thus, it has not been easy to obtain a toner that satisfies high levels of developability, low-temperature fixability, and storage stability under high temperature and high humidity.

[0013] In order to improve the low-temperature fixing property, it is effective to externally add a low-melting material to the toner particles. If a material that melts at a low temperature is externally added to the surface of the toner particles, the surface of the toner can be melted and the toner particles and the toner can be bonded to each other or to paper even in a short heating time. However, the presence of the low-melting material on the toner surface alone may lead to a decrease in charging property and adhesion of the low-melting material to the developer carrier of the developing device, which may lead to a decrease in developability. The adhesion of the low-melting material to the developer carrier reduces the developer carrier's ability to impart charge to the toner, which leads to a decrease in developability. Furthermore, a toner to which a low-melting material is externally added may also have a decrease in storage stability under high temperature and high humidity.

[0014] Therefore, the present inventors have devised a method for suppressing the exposure of external additives having low melting points to make them less susceptible to the effects of humidity and temperature, and have found that this method makes it possible to maintain storage stability under high temperature and high humidity conditions while maintaining low temperature fixability.

[0015] Specifically, the present inventors have found that a toner that simultaneously satisfies high levels of low-temperature fixability and storage stability can be obtained by having organic-inorganic composite particles on the surface of a toner particle, the organic-inorganic composite particles comprising inorganic fine particles, a crystalline resin, and an amorphous thermoplastic resin, having a core containing the crystalline resin and a shell containing the amorphous thermoplastic resin, the inorganic fine particles having a hydrophobicity of 50% or more, at least a portion of the inorganic fine particles being exposed on the surface to form convex portions, and having a median diameter of 80 nm to 500 nm.

[0016] When such organic-inorganic composite particles are used as an external additive, the external additive melts in an extremely short time due to heat received from a fixing device, and the external additive present on the toner surface melts in a short time, so that the toner particles can be quickly bonded to each other and to paper, improving low-temperature fixability.

[0017] In addition, such organic-inorganic composite particles can prevent the organic-inorganic composite particles on the toner particles from fusing with other toner particles or with the organic-inorganic composite particles on the toner particles, thereby preventing the resin from adhering to the surface of the developer carrier of the developing device and further improving storage stability under high temperature and high humidity conditions. Furthermore, by exposing at least a portion of the inorganic fine particles on the surface of the organic-inorganic composite particles to form protrusions, the contact area of ​​the external additive (organic-inorganic composite particles) with the toner particles and paper can be increased in the fixing step, thereby increasing the adhesive force of unfixed toner to paper and suppressing detachment of unfixed toner from the paper.

[0018] <Organic-inorganic composite particles> The organic-inorganic composite particles according to the present invention will now be described. The organic-inorganic composite particles according to the present invention have a structure in which inorganic fine particles having a hydrophobicity of 50% or more are dispersed in a resin portion composed of a core containing a crystalline resin and a shell containing an amorphous thermoplastic resin, and at least a part of the inorganic fine particles are exposed on the surface of the organic-inorganic composite particles to form a convex portion, and the median diameter of the organic-inorganic composite particles is 80 nm to 500 nm. When the resin particles and the inorganic fine particles are simultaneously added to the toner particles, or when the resin particles and the inorganic fine particles are added to the toner particles in order, the resin particles and the inorganic fine particles may aggregate on the toner particles, and appear to be an integrated organic-inorganic composite particle. However, in this method, the uniformity of the resin particles and the inorganic fine particles is often insufficient, or the inorganic fine particles are not sufficiently combined with the resin particles, making it difficult to obtain the effects of the present invention.

[0019] The median diameter of the organic-inorganic composite particles according to the present invention is 80 nm to 500 nm. When the median diameter of the organic-inorganic composite particles is in this range, the organic-inorganic composite particles are easily melted when they are subjected to heat from a fixing device, so that the toner particles can be firmly bonded to each other and to the toner and paper. This is also effective in maintaining the developability.

[0020] The content of inorganic fine particles in the organic-inorganic composite particles according to the present invention is preferably 50% by mass or more and 80% by mass or less, and more preferably 60% by mass or more and 80% by mass or less, based on the mass of the organic-inorganic composite particles. When the organic-inorganic composite particles having the content of inorganic fine particles in this range are used as an external additive for a toner, the external additive is easily melted instantly by heat received from a fixing device, and the low-temperature fixing property of the toner can be further improved.

[0021] In the organic-inorganic composite particles according to the present invention, the exposed area of ​​the shell containing the amorphous thermoplastic resin is preferably 30% to 70% of the surface area of ​​the organic-inorganic composite particles. When the organic-inorganic composite particles having an exposed shell area of ​​30% or more are used as an external additive for toner, the external additive has high conductivity of heat received from a fixing device, and the low-temperature fixing property of the toner can be further improved. In addition, when the organic-inorganic composite particles having an exposed shell area of ​​70% or less are used as an external additive for toner, the particles are less susceptible to the effects of humidity and temperature, and the storage stability under high temperature and high humidity can be further improved.

[0022] <Inorganic fine particles> The organic-inorganic composite particles according to the present invention contain inorganic fine particles. The inorganic fine particles used in the organic-inorganic composite particles according to the present invention have a hydrophobicity of 50% or more. If the hydrophobicity of the inorganic fine particles is lower than 50%, the adhesiveness to the resin forming the organic-inorganic composite particles, particularly the crystalline resin forming the core of the organic-inorganic composite particles, decreases. If such organic-inorganic composite particles are used as a toner external additive, the organic-inorganic composite particles will deform during toner storage, and storage stability will decrease.

[0023] The inorganic fine particles used in the organic-inorganic composite particles according to the present invention can be any known fine particles as long as they have a hydrophobicity of 50% or more. Examples of such inorganic fine particles include silica fine particles, alumina fine particles, titania fine particles, zinc oxide fine particles, strontium titanate fine particles, cerium oxide fine particles, and calcium carbonate fine particles. Two or more kinds selected from these fine particle groups in any combination can also be used.

[0024] In particular, the toner according to the present invention, which is externally added with organic-inorganic composite particles using silica fine particles as inorganic fine particles having a hydrophobicity of 50% or more, is preferable because it has particularly excellent charging properties. The silica fine particles may be those obtained by a dry method such as fumed silica, or those obtained by a wet method such as a sol-gel method. Examples of such silica fine particles include AEROSIL NX90G (manufactured by Nippon Aerosil Co., Ltd.) and organosilica sol TOL-ST (manufactured by Nissan Chemical Industries, Ltd.).

[0025] The inorganic fine particles used in the organic-inorganic composite particles can be made hydrophobic by chemically treating them with an organosilicon compound that reacts with or physically adsorbs to the inorganic fine particles.

[0026] A preferred method for hydrophobizing the silica particles is to treat the silica particles produced by vapor phase oxidation of a silicon halide compound with an organosilicon compound. Examples of the organosilicon compound include the following:

[0027] Hexamethyldisilazane, methyltrimethoxysilane, octyltrimethoxysilane, isobutyltrimethoxysilane, trimethylsilane, trimethylchlorosilane, trimethylethoxysilane, dimethyldichlorosilane, methyltrichlorosilane, allyldimethylchlorosilane, allylphenyldichlorosilane, benzyldimethylchlorosilane, bromomethyldimethylchlorosilane, α-chloroethyltrichlorosilane, β-chloroethyltrichlorosilane, chloromethyldimethylchlorosilane, triorganosilylmercaptan, trimethylsilylmercaptan, triorganosilylacrylate, vinyldimethylacetoxysilane, dimethylethoxysilane, dimethyldimethoxysilane, diphenyldiethoxysilane, 1-hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane, 1,3-diphenyltetramethyldisiloxane and dimethylpolysiloxane. These may be used alone or in combination of two or more.

[0028] The inorganic fine particles used in the organic-inorganic composite particles may be treated with silicone oil, and may be treated in addition to the above-mentioned hydrophobization treatment.

[0029] The preferred silicone oil has a viscosity of 30 mm at 25°C. 2 / s or more 1000mm 2 Specific examples of such silicone oils include dimethyl silicone oil, methylphenyl silicone oil, α-methylstyrene modified silicone oil, chlorophenyl silicone oil, and fluorine modified silicone oil.

[0030] The silicone oil treatment method can be the following: Directly mix the silica fine particles treated with a silane coupling agent with silicone oil using a mixer such as a Henschel mixer. Spray silicone oil onto the silica fine particles as the base. Alternatively, more preferably, dissolve or disperse silicone oil in a suitable organic solvent, add silica fine particles, mix, and then remove the organic solvent.

[0031] The inorganic fine particles preferably have a median diameter of 5 nm to 100 nm, more preferably 10 nm to 30 nm. When the inorganic fine particles have a median diameter of 5 nm to 100 nm, the inorganic fine particles tend to cover the surfaces of the organic-inorganic composite particles, which is effective in preventing contamination of the developer carrier and improving storage stability at high temperatures.

[0032] <Crystalline resin> The organic-inorganic composite particles according to the present invention have a core containing a crystalline resin. Any known crystalline resin can be used as the crystalline resin. The crystalline resin is not limited to the following, but examples thereof include polyester, polyethylene, polypropylene, ethylene-ethyl (meth)acrylate copolymer, and ethylene-vinyl acetate copolymer. Among these, crystalline polyester is preferred.

[0033] When a crystalline polyester is used as the crystalline resin, the acid value of the crystalline polyester is preferably 5 mgKOH / g or less. Although the reason for this is unclear, it is believed that when the acid value of the crystalline polyester is more than 5 mgKOH / g, the crystalline polyester bleeds onto the surface of the organic-inorganic composite particles over time, reducing the elastic modulus of the surface of the organic-inorganic composite particles and reducing storage stability under high temperature and high humidity.

[0034] When a polyester is used as the crystalline resin, examples of aliphatic diols that can be used to synthesize the crystalline polyester include the following: 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, etc. These can be used alone or in combination. The aliphatic diols according to the present invention are not limited to these.

[0035] In addition, as the aliphatic diol, an aliphatic diol having a double bond can also be used. Examples of the aliphatic diol having a double bond include the following: 2-butene-1,4-diol, 3-hexene-1,6-diol, 4-octene-1,8-diol, etc.

[0036] Next, the acid component that can be used in the synthesis of the crystalline polyester will be described. The acid component that can be used in the synthesis of the crystalline polyester is preferably a polycarboxylic acid.

[0037] Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Or lower alkyl esters or acid anhydrides thereof. Among these, sebacic acid, adipic acid, and 1,10-decanedicarboxylic acid or lower alkyl esters or acid anhydrides thereof. These can be used alone or in combination. In addition, the present invention is not limited to these.

[0038] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, etc. Among these, terephthalic acid is preferred in terms of availability and ease of forming a polymer with a low melting point.

[0039] Furthermore, as the acid component, a dicarboxylic acid having a double bond can also be used. Examples of such dicarboxylic acids include fumaric acid, maleic acid, 3-hexenedioic acid, and 3-octenedioic acid. Lower alkyl esters and acid anhydrides of these can also be used. Among them, fumaric acid and maleic acid are preferred from the viewpoint of cost.

[0040] The method for producing the crystalline polyester is not particularly limited, and the crystalline polyester can be produced by a general polyester polymerization method in which an acid component and an alcohol component are reacted. For example, the crystalline polyester can be produced by appropriately using a direct polycondensation method or an ester exchange method depending on the type of monomer.

[0041] The production of the crystalline polyester is preferably carried out at a polymerization temperature of 180° C. or higher and 230° C. or lower, and it is preferable to reduce the pressure in the reaction system as necessary and to carry out the reaction while removing water and alcohol generated during condensation.

[0042] If the monomer is not soluble or compatible at the reaction temperature, it is advisable to add a high boiling organic solvent as a solubilizing agent to dissolve the monomer. The polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present in the copolymerization reaction, it is preferable to condense the monomer with the acid or alcohol to be polycondensed in advance and then polycondense it with the main component.

[0043] Examples of the catalyst that can be used in the production of the crystalline polyester include titanium catalysts and tin catalysts. Examples of titanium catalysts include titanium tetraethoxide, titanium tetrapropoxide, titanium tetraisopropoxide, titanium tetrabutoxide, etc. Examples of tin catalysts include dibutyltin dichloride, dibutyltin oxide, diphenyltin oxide, etc.

[0044] The melting point of the crystalline resin according to the present invention is preferably 70°C or higher and 150°C or lower. In the organic-inorganic composite particles according to the present invention, the core containing a crystalline resin preferably contains inorganic fine particles having the specific hydrophobicity and median diameter described above. When the core of the organic-inorganic composite particles contains inorganic fine particles having the specific hydrophobicity and median diameter described above, the mechanical strength of the particles is increased, and therefore the storage stability of the toner under high temperature and high humidity conditions is improved when the particles are externally added to the toner particles.

[0045] <Amorphous thermoplastic resin> The organic-inorganic composite particles according to the present invention have a shell containing an amorphous thermoplastic resin. Any known amorphous thermoplastic resin can be used as the amorphous thermoplastic resin. Examples of the amorphous thermoplastic resin include vinyl resin, polyester resin, and epoxy resin, and among them, vinyl resin is preferred.

[0046] The amorphous vinyl resin may be a known one. For example, polystyrene, polymethyl methacrylate, polybutyl methacrylate, poly(meth)acrylic acid, or a copolymer thereof may be used. In particular, a styrene-(meth)acrylic acid copolymer is preferred.

[0047] When a styrene-(meth)acrylic acid copolymer is used as the amorphous thermoplastic resin, its acid value is preferably 10 mgKOH / g or more and 25 mgKOH / g or less. When the acid value of the styrene-(meth)acrylic acid copolymer is less than 10 mgKOH / g, the compatibility with the crystalline resin forming the core is high, so that the crystalline resin bleeds over time, and the storage stability under high temperature and high humidity is reduced. When the acid value of the styrene-(meth)acrylic acid copolymer exceeds 25 mgKOH / g, the hydrophobicity of the surface of the organic-inorganic composite particle according to the present invention is reduced, so that the amount of moisture adsorbed in the air increases, and the liquid bridging adhesion force between the organic-inorganic composite particles increases, resulting in fusion.

[0048] <Method of Manufacturing Organic-Inorganic Composite Particles> The organic-inorganic composite particles according to the present invention can be obtained by any known method. For example, organic-inorganic composite particles can be prepared by preparing thermoplastic resin particles by emulsion polymerization in the presence of inorganic fine particles and emulsified crystalline polyester.Also, organic-inorganic composite particles having a structure in which inorganic fine particles are embedded in resin particles can be prepared by dissolving crystalline polyester and thermoplastic resin in an organic solvent, adding inorganic fine particles to the solution, and carrying out phase inversion emulsification or forced emulsification in this state.

[0049] The method for producing organic-inorganic composite particles of the present invention is characterized by the steps of preparing a dispersion containing inorganic fine particles, a crystalline resin, an amorphous thermoplastic resin, and an organic solvent, mixing the dispersion with a neutralizer and water and stirring to prepare an emulsion, and distilling off the organic solvent from the emulsion to form organic-inorganic composite particles. The median diameter of the organic-inorganic composite particles produced by this method is likely to be 100 nm to 150 nm, which is suitable for use as an external additive.

[0050] The organic solvent used when producing the organic-inorganic composite particles according to the present invention by phase inversion emulsification or forced emulsification is not particularly limited as long as it dissolves the resin, and examples of the organic solvent that can be used include tetrahydrofuran, toluene, methyl ethyl ketone, hexane, ethyl acetate, and acetone.

[0051] The organic-inorganic composite particles according to the present invention are preferably surface-treated with an organosilicon compound or silicone oil. By treating with an organosilicon compound or silicone oil, the hydrophobicity of the external additive can be increased, and a toner having stable developability even in a high-temperature and high-humidity environment can be obtained.

[0052] Examples of methods for producing external additives that have been surface-treated with an organosilicon compound or silicone oil include a method of subjecting organic-inorganic composite particles to a surface treatment, and a method of compounding inorganic fine particles that have been previously surface-treated with an organosilicon compound or silicone oil with a resin.

[0053] The organic-inorganic composite particles can be made hydrophobic by chemically treating them with an organosilicon compound that reacts with or physically adsorbs to the organic-inorganic composite particles, in the same manner as the inorganic fine particles used in the organic-inorganic composite particles.

[0054] The organic-inorganic composite particles may be treated with silicone oil in the same manner as the inorganic fine particles used in the organic-inorganic composite particles, and may be treated in addition to the above-mentioned hydrophobization treatment.

[0055] <Toner> The toner according to the present invention has toner particles having a binder resin and a colorant, and an external additive. The content of the external additive (organic-inorganic composite particles) according to the present invention in the toner according to the present invention is preferably 0.1 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of the toner particles. The toner according to the present invention may contain other external additives in addition to the organic-inorganic composite particles. In particular, in order to improve the fluidity and chargeability of the toner, it is preferable to add a fluidity improver as another external additive.

[0056] <Flow improver> As the flow improver, the following can be used. For example, fluororesin powders such as vinylidene fluoride fine powder and polytetrafluoroethylene fine powder; fine powdered silica such as wet-processed silica and dry-processed silica, fine powdered titanium oxide, fine powdered alumina, treated silica obtained by surface-treating these with a silane compound, a titanium coupling agent, or silicone oil; oxides such as zinc oxide and tin oxide; double oxides such as strontium titanate, barium titanate, calcium titanate, strontium zirconate, and calcium zirconate; carbonate compounds such as calcium carbonate and magnesium carbonate, etc.

[0057] A preferred flow improver is a fine powder produced by the vapor phase oxidation of a silicon halide compound, which is called dry process silica or fumed silica. For example, it utilizes the thermal decomposition oxidation reaction of silicon tetrachloride gas in an oxyhydrogen flame, and the basic reaction formula is as follows: SiCl4+2H2+O2→SiO2+4HCl

[0058] In this manufacturing process, it is also possible to obtain a composite fine powder of silica and another metal oxide by using other metal halide compounds such as aluminum chloride or titanium chloride together with the silicon halide compound, and these are also included in the silica.

[0059] It is preferable that the average primary particle size in the particle size distribution on a number basis is 5 nm or more and 30 nm or less, since this allows the toner to have high electrostatic chargeability and flowability.

[0060] Furthermore, as the flowability improver used in the present invention, a treated silica fine powder obtained by subjecting the silica fine powder produced by the gas phase oxidation of the silicon halogen compound to a hydrophobic treatment is more preferable. The hydrophobic treatment can be performed by using a method similar to the surface treatment of the organic-inorganic composite particles or the inorganic fine particles used in the organic-inorganic composite particles.

[0061] The flow improver has a specific surface area of ​​30 m2 as measured by nitrogen adsorption using the BET method. 2 / g or more 300m 2 It is preferable to use the flowability improver in a total amount of 0.01 parts by mass or more and 3 parts by mass or less per 100 parts by mass of the toner.

[0062] The toner according to the present invention can be used as a one-component developer by mixing it with the flowability improver and, if necessary, with other external additives (such as a charge control agent, etc.), or can be used as a two-component developer by mixing it with a carrier.

[0063] As the carrier for use in the two-component development method, any of the conventionally known carriers can be used. Specifically, metals such as iron, nickel, cobalt, manganese, chromium, and rare earth elements, and alloys or oxides thereof, which are surface oxidized or unoxidized, are preferably used.

[0064] Furthermore, the surfaces of the carrier particles are preferably coated or adhered with a material selected from the group consisting of styrene resin, acrylic resin, silicone resin, fluorine resin, and polyester resin.

[0065] <Toner particles> Next, the toner particles according to the present invention will be described. First, the binder resin used in the toner particles according to the present invention will be described. Examples of the binder resin include polyester resins, vinyl resins, epoxy resins, and polyurethane resins. From the viewpoint of storage stability, the binder resin preferably has a glass transition point (Tg) of 45° C. or more and 70° C. or less.

[0066] The toner according to the present invention may further contain magnetic iron oxide particles and be used as a magnetic toner. In this case, the magnetic iron oxide particles may also function as a colorant. In the present invention, examples of the magnetic iron oxide particles contained in the magnetic toner include iron oxides such as magnetite, hematite, and ferrite, metals such as iron, cobalt, and nickel, and alloys and mixtures of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, bismuth, calcium, manganese, titanium, tungsten, and vanadium.

[0067] The magnetic iron oxide particles preferably have an average particle size of 2 μm or less, more preferably 0.05 μm or more and 0.5 μm or less. The amount of the magnetic iron oxide particles contained in the toner is preferably 20 parts by mass or more and 200 parts by mass or less, and more preferably 40 parts by mass or more and 150 parts by mass or less, per 100 parts by mass of the resin component.

[0068] Examples of colorants that can be used in the present invention are given below. As the black colorant, for example, carbon black, grafted carbon, or a colorant toned to black using the yellow / magenta / cyan colorants shown below can be used. As the yellow colorant, compounds such as condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds can be mentioned. As the magenta colorant, compounds such as condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinones, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds can be mentioned. As the cyan colorant, copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds can be mentioned. These colorants can be used alone or in a mixture, or in the form of a solid solution.

[0069] The colorant according to the present invention is selected from the viewpoints of hue angle, chroma, brightness, weather resistance, OHP transparency, and dispersibility in the toner. The colorant is added in an amount of 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the binder resin.

[0070] The toner according to the present invention may further contain a known wax. Specific examples of the wax include low molecular weight polyethylene, low molecular weight polypropylene, polyolefin copolymers, polyolefin wax, microcrystalline wax, paraffin wax, aliphatic hydrocarbon waxes such as Fischer-Tropsch wax, oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax, block copolymers of aliphatic hydrocarbon waxes, and oxides thereof.

[0071] Specific examples of waxes include Viscol 330-P, 550-P, 660-P, TS-200 (Sanyo Chemical Industries), Hiwax 400P, 200P, 100P, 410P, 420P, 320P, 220P, 210P, 110P (Mitsui Chemicals), Sasol H1, H2, C80, C105, C77 (Schumann Sasol), HNP-1, HNP-3, HNP-9, HNP-10, HNP-11, HNP-12 (Nippon Seiro), Unilin 350, 425, 550, 700, Unisid, Unisid 350, 425, 550, 700 (Toyo Petrolite), wood wax, beeswax, rice wax, candelilla wax, and carnauba wax (Cerarica NODA).

[0072] It is preferable to use a charge control agent in the toner according to the present invention in order to stabilize the chargeability. As such a charge control agent, an organic metal complex or a chelate compound, which easily interacts with the central metal and the acid group or hydroxyl group present at the terminal of the binder resin used in the present invention, is effective. Examples of such a charge control agent include monoazo metal complexes, acetylacetone metal complexes, and metal complexes or metal salts of aromatic hydroxycarboxylic acids or aromatic dicarboxylic acids. Specific examples of charge control agents that can be used include Spilon Black TRH, T-77, and T-95 (Hodogaya Chemical Co., Ltd.), and BONTRON (registered trademark) S-34, S-44, S-54, E-84, E-88, and E-89 (Orient Chemical Co., Ltd.). Charge control resins can also be used in combination with the above-mentioned charge control agents.

[0073] <Method of manufacturing toner particles> The method for producing the toner particles according to the present invention is not particularly limited, and for example, a pulverization method or a so-called polymerization method such as an emulsion polymerization method, a suspension polymerization method, or a solution suspension method can be used. In the pulverization method, first, the binder resin, colorant, wax, charge control agent, etc. that constitute the toner particles are thoroughly mixed using a mixer such as a Henschel mixer or a ball mill. Next, the resulting mixture is melt-kneaded using a thermal kneader such as a twin-screw kneading extruder, a heating roll, a kneader, or an extruder, and then cooled and solidified, followed by pulverization and classification. This gives the toner particles according to the present invention. Furthermore, if necessary, desired external additives may be thoroughly mixed with a mixer such as a Henschel mixer to obtain the toner according to the present invention.

[0074] Examples of mixers include the following: Henschel Mixer (manufactured by Mitsui Mining Co., Ltd.), Super Mixer (manufactured by Kawata Co., Ltd.), Ribocone (manufactured by Okawara Manufacturing Co., Ltd.), Nauta Mixer, Turbulizer, Cyclomix (manufactured by Hosokawa Micron Corporation), Spiral Pin Mixer (manufactured by Pacific Machinery Co., Ltd.), and Loedige Mixer (manufactured by Matsubo Co., Ltd.).

[0075] Examples of kneading machines include the following: KRC kneader (Kurimoto Iron Works); Buss-Co kneader (Buss); TEM type extruder (Toshiba Machine); TEX twin-screw kneader (Japan Steel Works); PCM kneader (Ikegai Iron Works); three-roll mill, mixing roll mill, kneader (Inoue Seisakusho); Kneadex (Mitsui Mining); MS-type pressure kneader, Niderruder (Moriyama Seisakusho); Banbury mixer (Kobe Steel, Ltd.).

[0076] Examples of pulverizers include the following: Counter Jet Mill, Micron Jet, Innomizer (manufactured by Hosokawa Micron Corporation); IDS type mill, PJM jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.); Urmax (manufactured by Nisso Engineering Co., Ltd.); SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.); Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.); Turbo Mill (manufactured by Turbo Industrial Co., Ltd.); Super Rotor (manufactured by Nisshin Engineering Co., Ltd.).

[0077] Examples of classifiers include the following: Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turboplex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Industry Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).

[0078] In the polymerization method, first, a polymerizable monomer capable of producing a binder resin and various additives as necessary are mixed, and the materials are dissolved or dispersed using a disperser to prepare a polymerizable monomer composition. Examples of the various additives include colorants, waxes, charge control agents, polymerization initiators, and chain transfer agents. Examples of the disperser include a homogenizer, a ball mill, a colloid mill, and an ultrasonic disperser. Next, the polymerizable monomer composition is put into an aqueous medium containing poorly water-soluble inorganic fine particles, and droplets of the polymerizable monomer composition are prepared using a high-speed disperser such as a high-speed stirrer or an ultrasonic disperser (granulation process). After that, the polymerizable monomer in the droplets is polymerized to obtain toner mother particles (polymerization process). The polymerization initiator may be mixed when preparing the polymerizable monomer composition, or may be mixed into the polymerizable monomer composition immediately before forming droplets in the aqueous medium. Also, during or after the granulation of the droplets, i.e., immediately before the start of the polymerization reaction, the toner may be added in a dissolved state in a polymerizable monomer or another solvent, as required. After the polymerizable monomer is polymerized to obtain a binder resin, a solvent removal process may be performed as required to obtain a dispersion of toner base particles. EXAMPLES

[0079] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass", respectively.

[0080] <Measurement methods for various physical properties> The measurement methods used in the examples are described below.

[0081] <Method of measuring toner cohesion> The degree of cohesion of the toner was measured as follows. The measuring device used was a "Powder Tester" (trade name; manufactured by Hosokawa Micron Corporation) with a digital display vibration meter "DigiVibro MODEL 1332A" (trade name; manufactured by Showa Sokki Co., Ltd.) connected to the side of the vibration table. A sieve with a mesh size of 38 μm (400 mesh), a sieve with a mesh size of 75 μm (200 mesh), and a sieve with a mesh size of 150 μm (100 mesh) were stacked on top of each other on the vibration table of the powder tester from the bottom up. The measurements were carried out in an environment of 23°C and 60% RH as follows. (1) The vibration amplitude of the vibration table was adjusted in advance so that the displacement value on the digital display vibrometer was 0.60 mm (peak-to-peak). (2) 5 g of the toner that had been left to stand for 24 hours in an environment of 23° C. and 60% RH was precisely weighed and gently placed on the top sieve with 150 μm openings. (3) After the sieves were vibrated for 15 seconds, the mass of the toner remaining on each sieve was measured and the degree of cohesion was calculated according to the following formula. Cohesion degree (%) = {(Sample mass (g) on ​​a sieve with 150 μm openings) / 5(g)}×100 + {(Sample mass (g) on ​​75 μm mesh sieve) / 5(g)} x 100 x 0.6 + {(Sample mass (g) on ​​38 μm mesh sieve) / 5(g)} x 100 x 0.2

[0082] <Method for measuring the hydrophobicity of inorganic fine particles> The hydrophobicity of inorganic fine particles was measured by methanol titration. The hydrophobicity by methanol titration was measured by the following procedure. That is, in a mixed solution in which 0.2 g of inorganic fine particles were added to 50 ml of water, methanol was dropped from a burette while stirring the mixed solution until the entire amount of inorganic fine particles was wetted. Whether the entire amount was wetted was judged by whether the inorganic fine particles floating on the water surface were all submerged in the liquid and suspended in the liquid. At this time, the percentage value of methanol to the total amount of the mixed solution and the dropped methanol at the end of the drop is taken as the hydrophobicity. The higher the value of the hydrophobicity, the higher the hydrophobicity.

[0083] <Method for evaluating the presence or absence of exposed inorganic fine particles> The presence or absence of exposed inorganic fine particles in the organic-inorganic composite particles can be evaluated by X-ray photoelectron spectroscopy (XPS). Specifically, in XPS, the total of the concentration of carbon atoms dC, the concentration of oxygen atoms dO, and the concentration of metal and silicon atoms dM derived from the inorganic fine particles on the surface of the organic-inorganic composite particles is taken as 100.0 atomic %. In this case, the content of the metal and silicon atoms derived from the inorganic fine particles calculated by the following formula (i) is expressed as Za [mass %]. Za [mass%] = {dM × (atomic weight of metal and silicon atoms)} / [{dC × (atomic weight of carbon)} + {dO × (atomic weight of oxygen)} + {dM × (atomic weight of metal and silicon atoms)}] × 100 (i)

[0084] When Za is less than 1 mass%, it means that the inorganic fine particles are not exposed on the surface layer of the organic-inorganic composite particles. When Za is 1 mass% or more, it means that the inorganic fine particles are exposed on the surface layer of the organic-inorganic composite particles. Za can be controlled by the hydrophobicity of the inorganic fine particles, the content of the inorganic fine particles relative to the organic-inorganic composite particles, and the temperature, pH, etc. when preparing the organic-inorganic composite particles. The XPS device and measurement conditions are as follows. Equipment used: ULVAC-PHI Quantum 2000 Analysis method: Narrow analysis ·X-ray source: Al-Kα ·X-ray conditions: 100μm, 25W, 15kV Photoelectron capture angle: 45° PassEnergy: 58.70eV Measurement range: φ100μm

[0085] <Method for measuring the amount of shell surface exposure> The amount of exposed shell on the surface of the organic-inorganic composite particle was measured as follows. The cross section of the organic-inorganic composite particle was observed using a scanning electron microscope (SEM) (S-4800, Hitachi High-Technologies Corporation) to obtain an SEM image. From the obtained SEM image, the shell surface was connected with a line to obtain a circle as the outline, and the proportion of the outline that was occupied by the shell excluding the inorganic fine particle portion was measured for the SEM images of the cross sections of 10 external additive particles. The average value of these values ​​was then calculated.

[0086] <Method for measuring the acid value of resin> The acid value of the resin was determined by the following method. Basic operations are based on JIS K-0070. 1) Accurately weigh 0.5 to 2.0 g of a sample. The mass at this point is M1 (g). 2) Place the sample in a 50 ml beaker and add 25 ml of a mixture of tetrahydrofuran / ethanol (2 / 1) to dissolve. 3) Using a 0.1 mol / l ethanol solution of potassium hydroxide, titration is performed using a potentiometric titration measuring device (for example, an automatic titration measuring device "COM-2500" manufactured by Hiranuma Sangyo Co., Ltd. can be used). 4) The amount of potassium hydroxide solution used at this time is A (ml). At the same time, measure the blank and the amount of potassium hydroxide used at this time is B (ml). 5) Calculate the acid value using the following formula (ii), where f is the factor of the potassium hydroxide solution. Formula (ii) Acid value [mgKOH / g]=[(AB)×f×5.61] / M1···(ii)

[0087] <Method for measuring the median diameter of organic-inorganic composite particles> After diluting the organic-inorganic composite particles with purified water, measurements were performed using Nanotrac 150 (manufactured by Nikkiso Co., Ltd.) with the range set to 0.001 μm to 10 μm, and the median diameter of the organic-inorganic composite particles was evaluated by measuring the number-average particle diameter.

[0088] <Method for measuring the content of inorganic fine particles in organic-inorganic composite particles> The content of inorganic fine particles in the organic-inorganic composite particles was evaluated by measuring the weight change using a STA7200RV (a simultaneous thermogravimetry and differential thermal analyzer, manufactured by Hitachi High-Tech Science Corporation).

[0089] <Method of manufacturing crystalline resin> [Production method of crystalline polyester 1] In a reaction vessel equipped with a stirrer, a thermometer, and a nitrogen inlet tube, 159 g of decanedicarboxylic acid as an acid component and 90 g of 1,6-hexanediol as an alcohol component were placed. Next, 0.1% by mass of tetraisobutyl titanate was placed in the reaction vessel relative to the total amount of raw materials, and the mixture was reacted at 180°C for 4 hours, then the temperature was raised to 210°C at a rate of 10°C / hour and maintained at 210°C for 8 hours. The mixture was then reacted at 8.3 kPa for 1 hour to obtain crystalline polyester 1. The melting point of crystalline polyester 1 was 72°C.

[0090] [Production method of crystalline polyester 2] Crystalline polyester 2 was obtained in the same manner as in the production of crystalline polyester 1, except that the raw materials were 159 g of sebacic acid as the acid component and 90 g of 1,9-nonanediol as the alcohol component.

[0091] [Production method of crystalline polyester 3] Crystalline polyester 3 was obtained in the same manner as in the production of crystalline polyester 1, except that the raw materials were 159 g of sebacic acid as the acid component and 90 g of 1,6-hexanediol as the alcohol component.

[0092] <Method for producing amorphous thermoplastic resin> [Method of producing amorphous polyester 1] In a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, 100 parts of terephthalic acid, 125 parts by mass of isophthalic acid, 285 parts of ethylene oxide 2 moles of bisphenol A, 60 parts by mass of ethylene glycol, 20 parts by mass of neopentyl glycol, 0.1 parts by mass of n-tetrabutyl titanate as a catalyst, 2 parts by mass of Irganox 1330 as an antioxidant, and 0.3 parts by mass of sodium acetate as a polymerization stabilizer were added, and an ester exchange reaction was carried out at 220 ° C. for 2 hours. Thereafter, the reaction system was heated from 220 ° C. to 270 ° C. while reducing the pressure inside the system, and then a polycondensation reaction was carried out at 1 Torr or less for 5 hours. After the reaction was completed, the system was returned from vacuum to normal pressure using nitrogen. Furthermore, 2.88 parts by mass of trimellitic anhydride was added as an acid value-imparting polycarboxylic acid, and reacted at 220 ° C. for 30 minutes to obtain a polyester. 100 parts by mass of the obtained polyester was dissolved in 200 parts by mass of chloroform, and the solution was placed in a separatory funnel together with 300 parts by mass of ion-exchanged water, stirred, allowed to stand, and the upper layer was discarded. The lower layer was further washed twice with water, and the chloroform was removed by an evaporator to obtain amorphous polyester 1.

[0093] <Production Example of Organic-Inorganic Composite Particle 1> 5 g of crystalline polyester 1 (acid value: 2 mg KOH / g), 5 g of styrene-acrylic copolymer 1 (copolymerization ratio: styrene / acrylic acid=24 / 1, acid value: 22.3 mg KOH / g), and 65 g of methyl ethyl ketone were charged into a glass container and dissolved by heating to 65°C. Next, while stirring at 60°C, 58.3 g of organosilica sol (trade name: organosilica sol TOL-ST, manufactured by Nissan Chemical Industries, Ltd., average particle size 15 nm, solid weight ratio 40%, hydrophobicity 70 wt%) was added as inorganic fine particles. Then, 200 g of 0.01 mol / l aqueous sodium hydroxide solution at 60°C was added, and forced emulsification was performed by high-speed stirring (rotation speed 15,000 rpm) using a homogenizer (manufactured by IKA: Ultra Turrax T50). Next, methyl ethyl ketone and toluene were volatilized at a temperature of 50°C using a rotary evaporator to obtain a dispersion of organic-inorganic composite particles 1. After that, the mixture was filtered and dried to obtain organic-inorganic composite particles 1. Organic-inorganic composite particle 1 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a surface exposure rate of 57% of the shell, and has a median diameter of 115 nm.

[0094] <Production Example of Organic-Inorganic Composite Particle 2> Organic-inorganic composite particles 2 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that crystalline polyester 2 (acid value: 5 mgKOH / g) was used instead of crystalline polyester 1. Organic-inorganic composite particle 2 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a shell surface exposure rate of 42%, and has a median diameter of 123 nm.

[0095] <Production Example of Organic-Inorganic Composite Particle 3> Organic-inorganic composite particles 3 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that styrene-acrylic copolymer 2 (copolymerization ratio: styrene / acrylic acid=24 / 1, acid value: 21.5 mg KOH / g) was used instead of styrene-acrylic copolymer 1. Organic-inorganic composite particle 3 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a surface exposure rate of 64% of the shell, and has a median diameter of 119 nm.

[0096] <Production Example of Organic-Inorganic Composite Particle 4> Organic-inorganic composite particles 4 were obtained in the same manner as in the production example of organic-inorganic composite particles 3, except that crystalline polyester 2 was used instead of crystalline polyester 1. Organic-inorganic composite particle 4 has a structure in which inorganic fine particles are embedded in resin particles, and a portion of the inorganic fine particles is exposed on the surface of the organic-inorganic composite particle. The inorganic fine particles are contained in the core, the surface exposure rate of the shell is 32%, and the median diameter is 122 nm.

[0097] <Production Example of Organic-Inorganic Composite Particle 5> Organic-inorganic composite particles 5 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that 23.3 g of vapor-phase silica (product name: AEROSIL NX90G, manufactured by Nippon Aerosil Co., Ltd., average particle diameter 20 nm, hydrophobicity degree 70 wt%) was used instead of organosilica sol TOL-ST. Organic-inorganic composite particle 5 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a shell surface exposure rate of 43%, and has a median diameter of 134 nm.

[0098] <Production Example of Organic-Inorganic Composite Particle 6> Organic-inorganic composite particles 6 were obtained in the same manner as in the production example of organic-inorganic composite particles 5, except that crystalline polyester 2 was used instead of crystalline polyester 1. Organic-inorganic composite particle 6 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a surface exposure rate of 47% of the shell, and has a median diameter of 131 nm.

[0099] <Production Example of Organic-Inorganic Composite Particle 7> Organic-inorganic composite particles 7 were obtained in the same manner as in the production example of organic-inorganic composite particles 5, except that styrene-acrylic copolymer 2 was used instead of styrene-acrylic copolymer 1. Organic-inorganic composite particle 7 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a surface exposure rate of 58% of the shell, and has a median diameter of 128 nm.

[0100] <Production Example of Organic-Inorganic Composite Particle 8> Organic-inorganic composite particles 8 were obtained in the same manner as in the production example of organic-inorganic composite particles 7, except that crystalline polyester 2 was used instead of crystalline polyester 1. Organic-inorganic composite particle 8 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a shell surface exposure rate of 54%, and has a median diameter of 135 nm.

[0101] <Production Example of Organic-Inorganic Composite Particle 9> Organic-inorganic composite particle 9 was obtained in the same manner as in the production example of organic-inorganic composite particle 1, except that organosilica sol MEK-ST-40 (product name: organosilica sol MEK-ST-40, manufactured by Nissan Chemical Industries, Ltd., average particle size 15 nm, solid weight ratio 40%, hydrophobicity degree 60 wt%) was used instead of organosilica sol TOL-ST. Organic-inorganic composite particle 9 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 50% of the shell, and has a median diameter of 105 nm.

[0102] <Production Example of Organic-Inorganic Composite Particle 10> Organic-inorganic composite particle 10 was obtained in the same manner as in the production example of organic-inorganic composite particle 1, except that 77.7 g of organosilica sol EAC-ST (product name: Organosilica sol EAC-ST, manufactured by Nissan Chemical Industries, Ltd., average particle diameter 15 nm, solid weight ratio 30%, hydrophobicity degree 50 wt%) was used instead of organosilica sol TOL-ST. The organic-inorganic composite particle 10 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 38% of the shell, and has a median diameter of 116 nm.

[0103] <Production Example of Organic-Inorganic Composite Particle 11> Organic-inorganic composite particles 11 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that 200 g of a 0.02 mol / l aqueous sodium hydroxide solution was used instead of 200 g of a 0.01 mol / l aqueous sodium hydroxide solution. Organic-inorganic composite particle 11 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a shell surface exposure rate of 62%, and has a median diameter of 85 nm.

[0104] <Production Example of Organic-Inorganic Composite Particle 12> In a glass vessel, 5 g of crystalline polyester 1 and 35 g of methyl ethyl ketone were charged and heated to 65° C. to dissolve them. Next, 200 g of 0.01 mol / l aqueous sodium hydroxide solution at 60° C. was added, and forced emulsification was performed by high-speed stirring (rotation speed: 15,000 rpm) using a homogenizer. Next, 240 g of the emulsion prepared by forced emulsification, 46 g of water, 23.1 g of organosilica sol TOL-ST as inorganic microparticles, 0.14 g of acrylic acid, and 4.86 g of styrene were added to a separable flask equipped with a stirrer, a condenser, a thermometer, and a nitrogen inlet tube, and the mixture was heated to 60°C with stirring to prepare an emulsion particle dispersion. Subsequently, 0.27 g of a 50% by mass toluene solution of 2,2'-azobis(2,4-dimethylvaleronitrile) was added as a polymerization initiator to the emulsion particle dispersion, and the mixture was kept at 60°C for 4 hours to carry out a polymerization reaction under a nitrogen atmosphere. Next, methyl ethyl ketone and toluene were evaporated at a temperature of 50° C. using a rotary evaporator to obtain a dispersion liquid of organic-inorganic composite particles 12. After that, the mixture was filtered and dried to obtain organic-inorganic composite particles 12. Organic-inorganic composite particle 12 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 57% of the shell, and has a median diameter of 450 nm.

[0105] <Production Example of Organic-Inorganic Composite Particle 13> Organic-inorganic composite particles 13 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that crystalline polyester 3 (acid value: 6 mgKOH / g) was used instead of crystalline polyester 1. Organic-inorganic composite particle 13 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 65% of the shell, and has a median diameter of 125 nm.

[0106] <Production Example of Organic-Inorganic Composite Particle 14> Organic-inorganic composite particles 14 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that EV150 (ethylene-vinyl acetate copolymer, manufactured by Mitsui-Dow Polychemicals) was used instead of crystalline polyester 1. Organic-inorganic composite particle 14 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a surface exposure rate of 45% of the shell, and has a median diameter of 132 nm.

[0107] <Production Example of Organic-Inorganic Composite Particle 15> Organic-inorganic composite particles 15 were obtained in the same manner as in the production example of organic-inorganic composite particles 14, except that the amount of organosilica sol TOL-ST added was 30.56 g. Organic-inorganic composite particle 15 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a shell surface exposure rate of 43%, and has a median diameter of 129 nm.

[0108] <Production Example of Organic-Inorganic Composite Particle 16> Organic-inorganic composite particles 16 were obtained in the same manner as in the production example of organic-inorganic composite particles 14, except that the amount of organosilica sol TOL-ST added was 141.67 g. Organic-inorganic composite particle 16 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 56% of the shell, and has a median diameter of 128 nm.

[0109] <Production Example of Organic-Inorganic Composite Particle 17> Organic-inorganic composite particles 17 were obtained in the same manner as in the production example of organic-inorganic composite particles 14, except that the amount of organosilica sol TOL-ST added was 23.1 g. Organic-inorganic composite particle 18 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a shell surface exposure rate of 51%, and has a median diameter of 133 nm.

[0110] <Production Example of Organic-Inorganic Composite Particle 18> 5 g of EV150 and 35 g of methyl ethyl ketone were placed in a glass container and heated to 65° C. to dissolve. Next, 200 g of 0.01 mol / l aqueous sodium hydroxide solution at 60° C. was added, and forced emulsification was performed by high-speed stirring (rotation speed: 15,000 rpm) using a homogenizer. Next, 5 g of styrene-acrylic copolymer 1 was dissolved in 30 g of methyl ethyl ketone at 65°C by heating, and the mixture was added with 23.1 g of organosilica sol TOL-ST. The mixture was added to the emulsion prepared by forced emulsification, and stirred at high speed (15,000 rpm) using a homogenizer. Next, methyl ethyl ketone and toluene were evaporated at a temperature of 50°C using a rotary evaporator, and a dispersion of organic-inorganic composite particles 18 was obtained. After that, the mixture was filtered and dried to obtain organic-inorganic composite particles 18. Organic-inorganic composite particle 18 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles are contained in the core, the surface exposure rate of the shell is 60%, and the median diameter is 111 nm.

[0111] <Production Example of Organic-Inorganic Composite Particle 19> Organic-inorganic composite particles 19 were obtained in the same manner as in the production example of organic-inorganic composite particles 18, except that the volatilization operation of methyl ethyl ketone and toluene with the rotary evaporator was carried out at a temperature of 60°C. Organic-inorganic composite particle 19 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles are contained in the core, the shell exposure rate is 24%, and the median diameter is 125 nm.

[0112] <Production Example of Organic-Inorganic Composite Particles 20> Organic-inorganic composite particles 20 were obtained in the same manner as in the production example of organic-inorganic composite particles 18, except that the volatilization operation of methyl ethyl ketone and toluene with the rotary evaporator was carried out at a temperature of 40°C. The organic-inorganic composite particle 20 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles are contained in the core, the shell exposure rate is 72%, and the median diameter is 132 nm.

[0113] <Production Example of Organic-Inorganic Composite Particle 21> Organic-inorganic composite particles 21 were obtained in the same manner as in the production example of organic-inorganic composite particles 19, except that styrene-acrylic copolymer 3 (copolymerization ratio: styrene / acrylic acid=15 / 1, acid value: 27.1 mg KOH / g) was used instead of styrene-acrylic copolymer 1. Organic-inorganic composite particle 21 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles are contained in the core, the shell surface exposure rate is 21%, and the median diameter is 117 nm.

[0114] <Production Example of Organic-Inorganic Composite Particle 22> Organic-inorganic composite particles 22 were obtained in the same manner as in the production example of organic-inorganic composite particles 19, except that styrene-acrylic copolymer 4 (copolymerization ratio: styrene / acrylic acid=50 / 1, acid value: 9.2 mg KOH / g) was used instead of styrene-acrylic copolymer 1. The organic-inorganic composite particle 22 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles being encapsulated in the core, the surface exposure rate of the shell being 27%, and the median diameter being 134 nm.

[0115] <Production Example of Organic-Inorganic Composite Particle 23> Organic-inorganic composite particles 23 were obtained in the same manner as in the production example of organic-inorganic composite particles 19, except that HF77 (polystyrene, manufactured by PS Japan) was used instead of the styrene-acrylic copolymer 1. Organic-inorganic composite particle 23 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles are contained in the core, the surface exposure rate of the shell is 24%, and the median diameter is 106 nm.

[0116] <Production Example of Organic-Inorganic Composite Particle 24> Organic-inorganic composite particles 24 were obtained in the same manner as in the production example of organic-inorganic composite particles 19, except that amorphous polyester 1 (acid value: 12.6 mg KOH / g) was used instead of styrene-acrylic copolymer 1. Organic-inorganic composite particle 24 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, no inorganic fine particles are contained in the core, the surface exposure rate of the shell is 25%, and the median diameter is 117 nm.

[0117] <Production Example of Organic-Inorganic Composite Particle 25> Organic-inorganic composite particles 25 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that styrene-acrylic copolymer 2 was used instead of crystalline polyester 1. Organic-inorganic composite particle 25 has a structure in which inorganic fine particles are embedded in resin particles, and a portion of the inorganic fine particles is exposed on the surface of the organic-inorganic composite particle. It has inorganic fine particles contained in the core, the surface exposure rate of the shell is 52%, and the median diameter is 121 nm.

[0118] <Production Example of Organic-Inorganic Composite Particle 26> Into a glass vessel were charged 5 g of crystalline polyester 1, 58.3 g of organosilica sol TOL-ST, and 35 g of methyl ethyl ketone, and the mixture was heated to 65° C. to dissolve. Next, 200 g of 0.01 mol / l aqueous sodium hydroxide solution at 60° C. was added, and forced emulsification was performed by high-speed stirring (rotation speed: 15,000 rpm) using a homogenizer. Subsequently, methyl ethyl ketone and toluene were evaporated in a rotary evaporator at a temperature of 50° C. to obtain a dispersion liquid. The solid content concentration of the dispersion liquid was adjusted to 60%. The glass container was placed in a water bath set at 30°C, and 313 g of water was added. Hydrochloric acid was added to the water in the container to adjust the pH of the aqueous solution to 4. 6.25 g of an aqueous solution of hexamethylolmelamine prepolymer (Milben Resin SM-607, manufactured by Showa Denko K.K., solid content concentration 80% by mass) was added and dissolved in the aqueous solution. 47.2 g of the dispersion was added to the solution and stirred, and then 625 g of water was added to prepare a mixed solution. While stirring the mixture, the temperature of the mixture was raised to 70° C. at a rate of 1° C. / min, and the mixture was further stirred for 2 hours. The pH of the mixture was then adjusted to 7. The contents of the vessel were filtered, and the obtained solid was washed and dried to obtain organic-inorganic composite particles 26. Organic-inorganic composite particle 26 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 47% of the shell, and has a median diameter of 123 nm.

[0119] <Production Example of Organic-Inorganic Composite Particle 27> Organic-inorganic composite particles 27 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that crystalline polyester 1 was not used and the weight of styrene-acrylic copolymer 1 used was 10 g. Organic-inorganic composite particle 27 has a structure in which inorganic fine particles are embedded in resin particles, and some of the inorganic fine particles are exposed on the surface of the organic-inorganic composite particle. It has inorganic fine particles contained in the core, the surface exposure rate of the shell is 59%, and the median diameter is 114 nm.

[0120] <Production Example of Organic-Inorganic Composite Particle 28> 10 g of crystalline polyester 1 and 58.3 g of organosilica sol TOL-ST were placed in a separable flask and heated to 130°C in an oil bath over 1 hour while stirring at 200 rpm with a three-one motor. After holding at 130°C for 1 hour, the mixture was slowly cooled at a rate of -15°C per hour to produce an organic-inorganic composite particle precursor. The obtained organic-inorganic composite particle precursor was in a paste form. The organic-inorganic composite particle precursor was packed in a Classic Line P-6 (planetary bead mill, Fritsch) together with zirconia grinding balls (Tosoh) with a diameter of 0.5 mm, and ground at room temperature at 200 rpm for 4 hours to obtain an organic-inorganic composite particle dispersion (solid content 50% by mass). The mixture was then filtered and dried to obtain organic-inorganic composite particles 28. Organic-inorganic composite particle 28 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 40% of the shell, and has a median diameter of 135 nm.

[0121] <Production Example of Organic-Inorganic Composite Particle 29> Organic-inorganic composite particles 29 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that 77.7 g of organosilica sol IPA-ST (product name: Organosilica sol IPA-ST, manufactured by Nissan Chemical Industries, Ltd., average particle diameter 12 nm, solid weight ratio 30%, hydrophobicity degree 48 wt%) was used instead of organosilica sol TOL-ST. Organic-inorganic composite particle 29 has a structure in which inorganic fine particles are embedded in resin particles, and some of the inorganic fine particles are exposed on the surface of the organic-inorganic composite particle. It has inorganic fine particles contained in the core, the surface exposure rate of the shell is 47%, and the median diameter is 122 nm.

[0122] <Production Example of Organic-Inorganic Composite Particles 30> In a glass vessel, 5 g of crystalline polyester 1, 58.3 g of organosilica sol TOL-ST, and 30 g of methyl ethyl ketone were charged and heated to 65° C. to dissolve. Next, 200 g of 0.01 mol / l aqueous sodium hydroxide solution at 60° C. was added, and forced emulsification was performed by high-speed stirring (rotation speed: 15,000 rpm) using a homogenizer. Next, 5 g of styrene-acrylic copolymer 1 was dissolved in 35 g of methyl ethyl ketone at 65° C., and the solution was added to the emulsion prepared by forced emulsification, and the mixture was stirred at high speed (15,000 rpm) using a homogenizer. Then, methyl ethyl ketone and toluene were evaporated at 50° C. using a rotary evaporator to obtain a dispersion of organic-inorganic composite particles 30. Subsequently, the methyl ethyl ketone and toluene were evaporated at a temperature of 50° C. using a rotary evaporator to obtain a dispersion liquid of the organic-inorganic composite particles 30. Thereafter, the mixture was filtered and dried to obtain the organic-inorganic composite particles 30. Organic-inorganic composite particle 30 has a structure in which inorganic fine particles are embedded in resin particles, the inorganic fine particles are not exposed on the surface of the organic-inorganic composite particle but are completely covered with resin, the inorganic fine particles are contained in the core, the surface exposure rate of the shell is 100%, and the median diameter is 137 nm.

[0123] <Production Example of Organic-Inorganic Composite Particle 31> Organic-inorganic composite particles 31 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that 200 g of a 0.05 mol / l aqueous sodium hydroxide solution was used instead of 200 g of a 0.01 mol / l aqueous sodium hydroxide solution. Organic-inorganic composite particle 31 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles encapsulated in the core, has a shell surface exposure rate of 63%, and has a median diameter of 75 nm.

[0124] <Production Example of Organic-Inorganic Composite Particle 32> Organic-inorganic composite particles 32 were obtained in the same manner as in the production example of organic-inorganic composite particles 1, except that 200 g of 0.001 mol / l aqueous sodium hydroxide solution was used instead of 200 g of 0.01 mol / l aqueous sodium hydroxide solution. Organic-inorganic composite particle 32 has a structure in which inorganic fine particles are embedded in resin particles, with some of the inorganic fine particles exposed on the surface of the organic-inorganic composite particle, has inorganic fine particles contained in the core, has a surface exposure rate of 58% of the shell, and has a median diameter of 550 nm. The configurations and characteristics of the above-mentioned organic-inorganic composite particles 1 to 32 are shown in Table 1-1.

[0125] <Production Example of Toner Particle 1> 100 parts by mass of amorphous polyester resin 1, 75 parts by mass of magnetic iron oxide particles, 2 parts by mass of Fischer-Tropsch wax (C105 manufactured by Sasol, melting point: 105°C), and 2 parts by mass of charge control agent (T-77 manufactured by Hodogaya Chemical Co., Ltd.) were premixed in a Henschel mixer, and then melt-kneaded using a twin-screw extruder (product name: PCM-30, manufactured by Ikegai Iron Works) with the temperature set so that the molten temperature at the discharge outlet was 150°C. The obtained kneaded product was cooled, coarsely pulverized with a hammer mill, and then finely pulverized with a pulverizer (product name: Turbo Mill T250, manufactured by Turbo Kogyo Co., Ltd.) The obtained finely pulverized powder was classified with a multi-division classifier utilizing the Coanda effect to obtain toner particles 1 having a weight average particle size of 7.2 μm.

[0126] <Toner 1 Manufacturing Example> The organic-inorganic composite particles were externally added to the toner particles 1 by a dry method. 100 parts by mass of the toner particles 1, 3 parts by mass of the organic-inorganic composite particles 1, and 1.5 parts by mass of fumed silica (BET specific surface area: 200 m2 / g) were added to a Henschel mixer and externally mixed. After that, the mixture was sieved through a mesh with an opening of 150 μm to obtain a toner 1 in which the organic-inorganic composite particles 1 were externally added to the toner particles 1.

[0127] <Production Examples of Toners 2 to 24> Toners 2 to 24 were obtained in the same manner as in the production example of toner 1, except that organic-inorganic composite particles 2 to 24 were used instead of organic-inorganic composite particles 1.

[0128] <Production Example of Comparative Toner 1> Comparative toner 1 was obtained in the same manner as in the production example of toner 1, except that organic-inorganic composite particles 25 were used instead of organic-inorganic composite particles 1.

[0129] <Production Examples of Comparative Toners 2 to 8> Comparative toners 2 to 8 were obtained in the same manner as in the production example of comparative toner 1, except that organic-inorganic composite particles 26 to 32 were used instead of organic-inorganic composite particles 25.

[0130] <Example 1> The following evaluations were carried out using Toner 1. <Evaluation of low-temperature fixing ability of toner> A commercially available magnetic single-component printer, HP LaserJet Enterprise600 M603dn (Hewlett-Packard: process speed 350 mm / s), was used. This evaluation machine was modified so that the fixing temperature of the fixing device could be set arbitrarily. Using this device, the temperature of the fixing unit was adjusted in 5°C increments within the range of 180°C to 220°C, and a bond paper (75 g / m 2 A halftone image is output so that the image density is 0.60 to 0.65 on the paper. The image obtained is rubbed back and forth five times with Silbon paper under a load of 4.9 kPa, and the lowest temperature at which the image density before and after rubbing decreased by 10% or less is measured and ranked as follows. The lower this temperature, the better the low-temperature fixability. Rank 10: Less than 180℃ Rank 9: 180℃ or higher but less than 185℃ Rank 8: 185℃ or higher but less than 190℃ Rank 7: 190℃ or higher but less than 195℃ Rank 6: 195℃ or higher but less than 200℃ Rank 5: 200℃ or higher but less than 205℃ Rank 4: 205℃ or higher but less than 210℃ Rank 3: 210℃ or higher but less than 215℃ Rank 2: 215℃ or higher but less than 220℃ Rank 1: 220℃ or higher In the above ranking, if the toner to which the organic-inorganic composite particles are externally added is rated as being rank 6 or higher, it is determined that the toner has good low-temperature fixing property. The evaluation results are shown in Table 1-2.

[0131] <Evaluation of Storage Stability of Toner> 10 g of Toner 1 was placed in a 100 ml plastic cup and left to stand at 50° C. for 3 days, after which the degree of cohesion was measured and ranked as follows: A smaller value indicates better fluidity. Rank 10: Less than 10% Rank 9: 10% to 15% Rank 8: 15% to 20% Rank 7: 20% to 25% Rank 6: 25% to 30% Rank 5: 30% to 35% Rank 4: 35% to less than 40% Rank 3: 40% to less than 45% Rank 2: 45% to less than 50% Rank 1: 50% or higher In the above ranking, it was determined that the storage stability of the toner to which the organic-inorganic composite particles were externally added was good if the ranking was 5 or higher. The evaluation results are shown in Table 1-2.

[0132] <Evaluation of storage stability of organic-inorganic composite particles> 10 g of organic / inorganic composite particles 1 were placed in a 100 ml plastic cup and left to stand at 50° C. for 3 days, after which the degree of aggregation was measured and categorized into the following ranks. A smaller value indicates better fluidity. Rank 10: Less than 10% Rank 9: 10% to 15% Rank 8: 15% to 20% Rank 7: 20% to 25% Rank 6: 25% to 30% Rank 5: 30% to 35% Rank 4: 35% to less than 40% Rank 3: 40% to less than 45% Rank 2: 45% to less than 50% Rank 1: 50% or higher In the above ranking, the storage stability of the organic-inorganic composite particles was judged to be good if the ranking was 5 or higher. The evaluation results are shown in Table 1-2. In regard to Example 1, good results were obtained in all cases.

[0133] <Examples 2 to 24 and Comparative Examples 1 to 8> Using toners 2 to 24 and comparative toners 1 to 8, the low temperature fixability of the toners, the storage stability of the toners, and the storage stability of the organic-inorganic composite particles were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1-2.

[0134] [Table 1-1]

[0135] [Table 1-2]

[0136] From the results in Table 1, it can be seen that the toner having organic-inorganic composite particles added thereto has poor low-temperature fixing property in Comparative Example 2, which is the conventional technology, and that the storage stability of the organic-inorganic composite particles and the toner having them added thereto is poor in Comparative Example 4, which is the conventional technology. In contrast, it can be seen that Examples 1 to 12 of the present invention provide good low-temperature fixing property for the toner having organic-inorganic composite particles added thereto, and good storage stability for the organic-inorganic composite particles and the toner having them added thereto.

[0137] In addition, a comparison between Example 1 and Example 12 shows that by preparing the organic-inorganic composite particles by the forced emulsification method rather than the polymerization method, a toner to which the organic-inorganic composite particles are externally added can have better low-temperature fixing properties.

[0138] Furthermore, a comparison between Example 1 and Example 13 shows that even better storage stability can be obtained by using a crystalline polyester having an acid value of 5 mgKOH / g or less.

[0139] Furthermore, a comparison between Example 13 and Example 14 shows that by using a crystalline polyester as the crystalline resin contained in the organic-inorganic composite particles, even better low-temperature fixability can be obtained.

[0140] Furthermore, a comparison of Example 14 with Examples 15 to 17 shows that good storage stability and low-temperature fixability can be obtained by adjusting the content of inorganic fine particles in the organic-inorganic composite particles to 50% by mass or more and 80% by mass or less, and even better storage stability and low-temperature fixability can be obtained by adjusting the content of inorganic fine particles to 60% by mass or more and 80% by mass or less.

[0141] Furthermore, a comparison between Example 17 and Example 18 shows that the organic-inorganic composite particles have better storage stability when they contain inorganic fine particles contained in their cores.

[0142] Furthermore, a comparison of Example 18 with Examples 19 and 20 shows that good storage stability and low-temperature fixability can be obtained by setting the exposed area of ​​the shell to 30% or more and 70% or less of the surface area of ​​the organic-inorganic composite particles.

[0143] Furthermore, a comparison of Example 19 with Examples 21 and 22 shows that good storage stability and low-temperature fixability can be obtained by adjusting the acid value of the styrene-(meth)acrylic acid copolymer contained in the shell to 10 mgKOH / g or more and 25 mgKOH / g or less.

[0144] Furthermore, a comparison of Examples 19, 21, and 22 with Example 23 shows that good storage stability and low-temperature fixability can be obtained by using a styrene-(meth)acrylic acid copolymer as the vinyl resin contained in the shell.

[0145] Furthermore, a comparison of Examples 19, 21, 22, and 23 with Example 24 shows that good storage stability and low-temperature fixability can be obtained by using a vinyl resin as the thermoplastic resin contained in the shell. [Industrial Applicability]

[0146] According to the present invention, a toner having excellent low-temperature fixing property and storage stability can be provided.

Claims

1. A toner having toner particles including a binder resin and a colorant, and an external additive, The external additive is an organic-inorganic composite particle containing inorganic fine particles, a crystalline resin, and an amorphous thermoplastic resin, The organic-inorganic composite particles have a core containing the crystalline resin and a shell containing the amorphous thermoplastic resin, the inorganic fine particles have a hydrophobicity of 50% or more, and at least a portion of the inorganic fine particles is exposed on the surface of the organic-inorganic composite particle to form a convex portion; The organic-inorganic composite particles have a median diameter of 80 nm to 500 nm; The toner is characterized in that the thermoplastic resin is a styrene-(meth)acrylic acid copolymer.

2. 2. The toner according to claim 1, wherein the acid value of the styrene-(meth)acrylic acid copolymer is from 10 mgKOH / g to 25 mgKOH / g.

3. 3. The toner according to claim 1, wherein an exposed area of ​​the shell containing the thermoplastic resin is 30% or more and 70% or less of a surface area of ​​the organic-inorganic composite particle.

4. A toner having toner particles including a binder resin and a colorant, and an external additive, The external additive is an organic-inorganic composite particle containing inorganic fine particles, a crystalline resin, and an amorphous thermoplastic resin, The organic-inorganic composite particles have a core containing the crystalline resin and a shell containing the amorphous thermoplastic resin, the inorganic fine particles have a hydrophobicity of 50% or more, and at least a portion of the inorganic fine particles is exposed on the surface of the organic-inorganic composite particle to form a convex portion; The organic-inorganic composite particles have a median diameter of 80 nm to 500 nm; The toner is characterized in that the organic-inorganic composite particles contain inorganic fine particles enclosed in the core.

5. A toner having toner particles including a binder resin and a colorant, and an external additive, The external additive is an organic-inorganic composite particle containing inorganic fine particles, a crystalline resin, and an amorphous thermoplastic resin, The organic-inorganic composite particles have a core containing the crystalline resin and a shell containing the amorphous thermoplastic resin, the inorganic fine particles have a hydrophobicity of 50% or more, and at least a portion of the inorganic fine particles is exposed on the surface of the organic-inorganic composite particle to form a convex portion; The organic-inorganic composite particles have a median diameter of 80 nm to 500 nm; The toner is characterized in that the content of the inorganic fine particles in the organic-inorganic composite particles is 50% by mass or more and 80% by mass or less based on the mass of the organic-inorganic composite particles.

6. 6. The toner according to claim 5, wherein the content of the inorganic fine particles in the organic-inorganic composite particles is 60% by mass or more and 80% by mass or less based on the mass of the organic-inorganic composite particles.

7. 7. The toner according to claim 1, wherein the crystalline resin is a crystalline polyester.

8. 8. The toner according to claim 7, wherein the crystalline polyester has an acid value of 5 mgKOH / g or less.

Citation Information

Patent Citations

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2012163694A

  • Toner

    JP2015045859A

  • Toner for electrostatic latent image development and external additive

    JP2017015868A

  • Toner and external additive for toner

    JP2017134398A

  • Toner

    JP2018189895A