toner
A core-shell structured toner with a hydrophobized magnetic material and controlled solubility parameters addresses the issue of uneven releasability and contamination in electrophotographic processes, ensuring high-quality and efficient image formation.
Patent Information
- Application Number
- JP2020199152
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-11-30
AI Technical Summary
Existing toners used in electrophotographic processes face issues with uneven releasability of toner images after fixing, leading to contamination of conveyance members, especially in high-speed image forming processes, which affects image quality and process efficiency.
A toner with a core-shell structure is developed, where the core contains a binder resin and colorant, and the shell is made of a hydrophobized magnetic material with a specific Si spectrum and a crystalline material with a controlled solubility parameter difference, ensuring the crystalline material migrates to the toner surface during fixing, enhancing releasability and reducing contamination.
The toner achieves excellent low-temperature fixability, durability, and reduced contamination of conveyance members, resulting in high-quality electrophotographic images even at high speeds.
Smart Images

Figure 0007562387000013 
Figure 0007562387000014 
Figure 0007562387000015
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE This disclosure relates to toners for use in imaging processes such as electrophotography. [Background technology]
[0002] 2. Description of the Related Art In recent years, image forming apparatuses such as copying machines and printers are being used in increasingly diverse purposes and environments, and there is a demand for them to operate at higher speeds, with higher image quality and greater stability. In the electrophotographic method, a charging step is performed in which an electrostatic latent image carrier (hereinafter referred to as a "photoreceptor") is charged by a charging means, an exposure step is performed in which the charged electrostatic latent image carrier is exposed to light to form an electrostatic latent image, and a development step is performed in which the electrostatic latent image is developed with toner to form a toner image. Then, a transfer step is performed in which the toner image is transferred to a recording material with or without an intermediate transfer material, and a fixing step is performed in which the recording material carrying the toner image is heated, pressurized, and fixed by passing the recording material through a nip portion formed by a pressure member and a rotatable image heating member, and the image is output.
[0003] In order to meet the recent trend of high image quality and energy saving, it is important to optimize each process. Among these, the development process in which a toner image is formed by developing an electrostatic latent image with toner has been important for image quality, while sufficient fixing at low temperatures is important for energy saving. As a means for improving the fixing property, crystalline materials that are quickly compatible with the binder resin of the toner and promote the melting and deformation of the toner particles have been investigated. Patent Document 1 discloses a toner that is excellent in low-temperature fixability and storage stability. Patent Document 2 discloses a toner that is excellent in low-temperature fixability and durability. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6584218 [Patent Document 2] JP 2020-34714 A Summary of the Invention [Problem to be solved by the invention]
[0005] According to the study by the present inventors, it was confirmed that the toner according to Patent Document 1 has excellent low-temperature fixing property and storage stability. However, it was recognized that there is still room for improvement in the speed-up of the image forming process in recent years. Specifically, a phenomenon was observed in which unevenness occurred in the release property of the toner image after the fixing process. This sometimes led to aggravation of the contamination of the member that transports the media.
[0006] According to the study by the present inventors, it was confirmed that the toner according to Patent Document 2 has excellent low-temperature fixing ability and durability. However, it was recognized that there is still room for improvement in the speed-up of the image forming process in recent years. Specifically, a phenomenon was observed in which unevenness occurred in the release property of the toner image after the fixing process. This sometimes led to aggravation of the contamination of the member that transports the media.
[0007] One aspect of the present invention is to provide a toner that is excellent in low-temperature fixability and formation of high-quality electrophotographic images even when applied to a high-speed electrophotographic image forming process. [Means for solving the problem]
[0008] The present invention relates to A toner containing toner particles having a core-shell structure consisting of a core containing a binder resin and a colorant, and a shell, The colorant is a hydrophobic magnetic material whose surface has been hydrophobized with a silane coupling agent, The hydrophobic magnetic material was analyzed by near edge X-ray absorption fine structure (NEXAFS) to determine that the spectrum of Si obtained based on the total electron yield method (TEY) had peak A in the range of 1844.4 eV to 1844.8 eV and peak B in the range of 1846.1 eV to 1846.6 eV, and the area of peak A was calculated as I A , the area of peak B is I B The number of moles of Si derived from the silane compound contained in 1 g of the hydrophobic magnetic material is M Si Then, I A / (I A +I B ) / M Si But it meets the criteria of 40 to 55, the toner contains a crystalline material, and the shell contains an amorphous thermoplastic resin; The SP value of the crystalline material calculated by the Fedors method is SPc (J / cm 3 ) 0.5 The SP value of the amorphous thermoplastic resin calculated by the Fedors method is SPa (J / cm 3 ) 0.5 When SPc and SPa satisfy the following formula (1), The toner is stained with ruthenium by treating the toner in an atmosphere of RuO4 (ruthenium tetroxide) gas at 500 Pa for 15 minutes, and then, when the ratio of the area occupied by the crystalline material per area of the toner surface as observed with a scanning electron microscope (SEM) is defined as S2 (%), the toner is characterized in that S2 (%) satisfies the following formula (2): 2.50≦SPa-SPc≦4.50 Formula (1) 1.0≦S2≦ 20.0 Formula (2) Effect of the Invention
[0009] According to one aspect of the present invention, a toner having excellent low-temperature fixing properties, durability, and prevention of contamination of conveying members can be obtained even when applied to a high-speed electrophotographic image forming process. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 illustrates an example of an electrophotographic image forming apparatus. [Diagram 2] FIG. 1 is a diagram showing an example of a core-shell structure of the present invention. [Diagram 3] FIG. 1 is a diagram showing an example of a core-shell structure of the present invention. [Figure 4] FIG. 1 is a diagram showing an example of a core-shell structure of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Toners with a core-shell structure are suitable for achieving both low-temperature fixability and storage stability and durability. Specifically, toners with a shell are suitable for protecting the core from heat and mechanical shocks by the shell, even if the toner has a core that is softened at low temperatures and has excellent low-temperature fixability. However, during the fixing process, the shell prevents the plasticizer and release agent contained in the core from flowing out to the toner surface, so the surface of the toner image that has undergone the fixing process is likely to have poor releasability. For this reason, a toner image with poor releasability is likely to adhere to a member that conveys a medium that has undergone the fixing process, causing contamination of the member. As a result, the toner image that has adhered to the contaminated member is transferred to the medium, causing vertical streaks. In particular, in a high-speed electrophotographic image forming process, the time required for the fixing process is very short. As a result, the crystalline material is unlikely to migrate to the surface of the toner image, so the releasability of the toner image is unlikely to increase. Therefore, a toner with a core-shell structure has a problem of contamination of the member that conveys the medium.
[0012] Therefore, the present inventors have conducted extensive research to promote the bleeding of the crystalline material from the surface of the toner image during the fixing process, and have found that the above requirements can be met by allowing a crystalline material and a shell, which have a large difference in solubility parameter, to coexist on the surface of the toner.
[0013] That is, the present invention is as follows. A toner containing toner particles having a core-shell structure consisting of a core containing a binder resin and a colorant, and a shell, The colorant is a hydrophobic magnetic material whose surface has been hydrophobized with a silane coupling agent, The hydrophobic magnetic material was analyzed by near edge X-ray absorption fine structure (NEXAFS) to determine that the spectrum of Si obtained based on the total electron yield method (TEY) had peak A in the range of 1844.4 eV to 1844.8 eV and peak B in the range of 1846.1 eV to 1846.6 eV, and the area of peak A was calculated as I A , the area of peak B is I B The number of moles of Si derived from the silane compound contained in 1 g of the hydrophobic magnetic material is M Si Then, I A / (I A +I B ) / M Si But it meets the criteria of 40 to 55, the toner contains a crystalline material, and the shell contains an amorphous thermoplastic resin; The SP value of the crystalline material calculated by the Fedors method is SPc (J / cm 3 ) 0.5 The SP value of the amorphous thermoplastic resin calculated by the Fedors method is SPa (J / cm 3 ) 0.5 When SPc and SPa satisfy the following formula (1), The toner is stained with ruthenium by treating it in an atmosphere of RuO4 (ruthenium tetroxide) gas at 500 Pa for 15 minutes, and then, in the toner observed with a scanning electron microscope (SEM), the ratio of the area occupied by the crystalline material per area of the toner is defined as S2 (%). S2 (%) satisfies the following formula (2). 2.50≦SPa-SPc≦4.50 Formula (1) 1.0≦S2≦20.0 Formula (2)
[0014] As a result of the investigations conducted by the present inventors, it has become possible to provide a toner which is excellent in low-temperature fixing property, durability and storage stability and which is also capable of reducing contamination of conveying members by using the above toner. The above formula (1) means that the difference between the SPc calculated by the Fedors method of the crystalline material and the SPa calculated by the Fedors method of the amorphous thermoplastic resin is relatively large, and the above formula (2) means that the amount of the crystalline material present near the surface of the toner is relatively large.
[0015] As a result of the study by the present inventors, it was found that in the toner having the above-mentioned configuration, when the toner is melted and deformed in the fixing process, the crystalline material having a large SP value difference from the amorphous thermoplastic resin flows out vigorously onto the surface of the toner. This makes it possible to increase the amount of crystalline material present on the surface of the toner image that has been fixed. Therefore, it was found that the toner image has sufficient releasability, and therefore contamination of the conveying member can be reduced. Furthermore, even in conventional evaluation environments expected for testing the storage stability of toner, the difference in SP value between the amorphous thermoplastic resin and the crystalline material is sufficiently large to prevent changes in the performance of the toner. Furthermore, since the difference in SP value between the amorphous thermoplastic resin and the crystalline material is sufficiently large even in a conventional durability test, a high-quality image can be obtained through the durability test.
[0016] After the toner is treated in a ruthenium tetroxide gas atmosphere of 500 Pa for 15 minutes to dye it with ruthenium, the ratio S2 (%) of the area occupied by the crystalline material per area of the toner surface observed by SEM is 1.0% to 20.0%. By dyeing the toner for a long time under a ruthenium tetroxide gas atmosphere of 500 Pa, the area from the toner surface to a depth of about 100 nm is dyed with ruthenium tetroxide gas. At this time, the crystalline material and the amorphous material have different easiness to be dyed by ruthenium tetroxide. By observing the toner that has been treated in advance with SEM or TEM, the state of the crystalline material can be visualized.
[0017] In addition, by comparing the lamellar spacing due to crystallinity confirmed by observation with SEM or TEM after similarly treating the crystalline material alone with the lamellar spacing of the crystalline material detected as S2, it is possible to identify the crystalline material detected as S2. As a method for obtaining the crystalline material alone, a crystalline material used in the production of toner may be used, or a crystalline material obtained by isolating it from a toner may be used. Methods for controlling the proportion S2 of the area occupied by the crystalline material include a method of placing a hydrophobic magnetic material that has an affinity for the crystalline material near the surface, as described below, and an emulsion aggregation method in which emulsified crystalline material is aggregated in multiple stages.
[0018] Schematic diagrams of the toner according to the present invention are shown in FIGS. FIG. 2 shows the shell being thin, with crystalline material in the core. FIG. 3 shows the shell is thick and crystalline material is present in the shell. FIG. 4 shows a shell of intermediate thickness, with crystalline material present in the core and shell. The effects of the present invention can be obtained with any of the configurations shown in FIGS.
[0019] The effect of the present invention will be explained using the schematic diagram of the toner shown in FIG. 2. Reference numeral 301 denotes a shell, reference numeral 302 denotes a crystalline material, reference numeral 303 denotes a core, and reference numeral 304 denotes a region dyed with ruthenium tetroxide. According to the inventors' study, the region dyed with ruthenium tetroxide 304 is about 100 nm from the surface of the toner. When the toner is fixed, the shell 301 and the core 303 are deformed by the heat of the fixing device. At that time, the crystalline material 302 flows out toward the surface of the toner with force. This makes it possible to increase the amount of crystalline material present on the surface of the toner image, thereby greatly reducing the contamination of the conveying member, which is the effect of the present invention. In order to obtain the effect of the present invention, it is important that the shell and the crystalline material are present simultaneously in the region 304.
[0020] In the present invention, the SP value of a crystalline material calculated by the Fedors method is defined as SPc (J / cm 3 ) 0.5 The SP value of the amorphous thermoplastic resin calculated by the Fedors method is SPa (J / cm 3 ) 0.5 In this case, it is preferable that SPc and SPa satisfy the following formula (1). 2.50≦SPa-SPc≦4.50 Formula (1) If the SPa-SPc ratio is less than 2.50, the toner image may not have sufficient releasability, and contamination of the transport member may not be improved. If the SPa-SPc ratio is more than 4.50, the amorphous thermoplastic resin may not easily form a shell, and durability and storage stability may be poor.
[0021] In the present invention, when the toner is stained with ruthenium by treating it in an atmosphere of RuO4 (ruthenium tetroxide) gas at 500 Pa for 15 minutes, and then the ratio of the area occupied by the crystalline material to the area of the toner surface as observed by a scanning electron microscope (SEM) is defined as S2 (%), it is preferable that S2 (%) satisfies the following formula (2): 1.0≦S2≦20.0 Formula (2) If S2 is less than 1.0, the release properties of the toner image may be insufficient, and contamination of the transport member may not be improved. Also, if S2 exceeds 20.0, the amorphous thermoplastic resin may have difficulty in forming a shell, and durability and storage stability may be poor.
[0022] In the present invention, the viscosity of the toner at 100° C. measured by a flow tester temperature rise method is 0.5×10 4 Pa·s or more 9.0×10 5 It is preferable that the viscosity is less than Pa·s. When the viscosity at 100°C is within the above range, a toner with excellent low-temperature fixing property can be provided. Furthermore, in the fixing process, melting and deformation of the toner easily occurs, so that the crystalline material easily seeps out onto the surface of the toner image. This makes it easier to improve the contamination of the conveying member.
[0023] In the present invention, SPa is 11.60 (J / cm 3 ) 0.5 More than 12.40(J / cm 3 ) 0.5 When SPa satisfies the above-mentioned range, it becomes easy to control the formulas (1) and (2) in the present invention within suitable ranges, regardless of which crystalline material is used, and the effects of the present invention are easily exhibited.
[0024] In the present invention, the amorphous thermoplastic resin is preferably an amorphous polyester. The amorphous polyester has excellent chargeability and thermoplasticity, and therefore has excellent low-temperature fixing ability and durability of the toner. Furthermore, by selecting the monomer unit of the amorphous polyester resin, it becomes easy to control SPa and formula (1) within the range suitable for the present invention.
[0025] In the present invention, the amorphous polyester preferably has an isosorbide unit represented by the formula (3). [ka] The isosorbide unit has high phase separation with the crystalline material, which makes it easier to provide excellent storage stability and durability. Furthermore, it makes it easier to promote the exudation of the crystalline material to the toner surface during the fixing process, which makes it easier to reduce contamination of the transport member.
[0026] In the present invention, the amorphous polyester is a condensate of at least one alcohol component selected from the group consisting of dihydric and trihydric or higher alcohols, and at least one carboxylic acid component selected from the group consisting of aromatic polycarboxylic acids, aliphatic polycarboxylic acids, and their anhydrides, the alcohol component contains at least isosorbide, the alcohol component and the carboxylic acid component do not have an ester group, and the amorphous polyester preferably contains isosorbide units represented by the formula (3) derived from the isosorbide in an amount of 0.10 mol% to 30.00 mol% based on all of the monomer units derived from the alcohol component and the monomer units derived from the carboxylic acid component. By satisfying the above-mentioned range of the content of the isosorbide unit, it is easy to provide excellent storage stability and durability. Furthermore, it is easy to promote the exudation of the crystalline material to the toner surface in the fixing process, which makes it easy to reduce the contamination of the conveying member.
[0027] In the present invention, the colorant is preferably a colorant whose surface has been hydrophobized with a silane coupling agent. By being hydrophobized with a silane coupling agent, the above-mentioned S2 can be easily controlled within a range suitable for the present invention in the suspension polymerization method, which is a production method suitable for the present invention.
[0028] In the present invention, the hydrophobized colorant is preferably a hydrophobized magnetic material. By being a hydrophobized magnetic material, the hydrophobized magnetic material is likely to be present near the toner surface in the suspension polymerization method, which is a manufacturing method suitable for the present invention. Therefore, in the suspension polymerization method, the amount of crystalline material present near the toner surface can be easily controlled.
[0029] In the present invention, the hydrophobic magnetic material is measured by using near edge X-ray absorption fine structure (NEXAFS) and the spectrum of Si obtained based on the total electron yield method (TEY) has peak A in the range of 1844.4 eV to 1844.8 eV and peak B in the range of 1846.1 eV to 1846.6 eV, and the area of peak A is I A , the area of peak B is I B The number of moles of Si derived from the silane compound contained in 1 g of the hydrophobic magnetic material is M Si Then, I A / (I A +I B ) / M Si It is preferable that the ratio is 40 or more and 55 or less.
[0030] NEXAFS can provide information about the state of silane compounds bonded to Fe atoms in magnetic materials. The larger the peak A in the Si absorption spectrum, the less silane compounds are bonded to the surface of the magnetic material. Conversely, the larger the peak B, the more silane compounds are bonded to the surface of the magnetic material.
[0031] By measuring the Si absorption spectrum using the above-mentioned NEXAFS, the bonding state between the magnetic material and the silane coupling agent can be evaluated with good reproducibility. It has been found that in order for the silane compound to exert the desired function, it is important that the following formula (5) is satisfied. I A / (I A +I B ) / M Si =40~55 (5) In the formula, I A represents the area of peak A, and I Brepresents the area of peak B, and MSi represents the number of moles of Si derived from the silane compound contained per gram of the hydrophobic magnetic material. A / (I A +I B ) value of M Si The reason for dividing by the value of is for standardization purposes.
[0032] A high value of formula (5) indicates that the amount of hydrophobic treatment agent condensed with itself is relatively greater than the amount of treatment agent bonded to the magnetic material. Compounds formed by polycondensation of hydrophobic treatment agents become very hydrophobic, and therefore tend to have improved affinity with crystalline materials. This makes it easier for a large amount of crystalline material to exist near the magnetic material. This makes it easier for the hydrophobic magnetic material to exist near the surface of the toner in the suspension polymerization method, which is a manufacturing method suitable for the present invention. This makes it easier to control the amount of crystalline material present near the surface of the toner in the suspension polymerization method.
[0033] The toner of the present invention is characterized in that it contains toner particles having a core-shell structure consisting of a core containing a binder resin and a colorant, and a shell. The core-shell structure is a structure in which a core is covered with a shell. The present invention contains a crystalline material, but the effects of the present invention can be obtained whether the crystalline material is contained in the core or the shell. In addition, the effects of the present invention can be obtained whether the crystalline material is contained in both the core and the shell.
[0034] (shell) In the present invention, the shell contains an amorphous thermoplastic resin. The thermoplastic resin refers to a resin that melts and deforms when subjected to heat. In the present invention, the thermoplastic resin is preferably an amorphous polyester. As the amorphous polyester in the present invention, a saturated polyester resin, an unsaturated polyester resin, or both of them can be appropriately selected and used.
[0035] The amorphous polyester used in the present invention may be a known polyester produced from an alcohol component and an acid component, both of which are exemplified below.
[0036] Examples of the alcohol component include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, cyclohexanedimethanol, butenediol, octenediol, cyclohexenedimethanol, hydrogenated bisphenol A, bisphenols represented by the following formula (A) and derivatives thereof; and diols represented by the following formula (B). [ka] (In formula (A), R is an ethylene or propylene group. x and y are each an integer of 0 or more, provided that the average value of x+y is 0 to 10. The propylene group is a functional group derived from 2-propanediol.) [ka] (In the formula (B), R' is any one of the above (B1) to (B3). x' and y' are integers of 0 or more. However, the average value of x'+y' is 0 to 10.)
[0037] In the present invention, the amorphous polyester is preferably a bisphenol of formula (A) or a derivative thereof from the viewpoint of reactivity, and more preferably a compound of bisphenol of formula (A) or a derivative thereof in which the average value of x+y is 1 to 4.
[0038] Examples of trihydric or higher alcohols that can be used in the preparation of the amorphous polyester include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.
[0039] Examples of divalent carboxylic acids that can be used in the preparation of amorphous polyesters include dicarboxylic acids and derivatives thereof, such as phthalic acid, terephthalic acid, isophthalic acid, and phthalic anhydride, benzenedicarboxylic acids, and anhydrides thereof, and lower alkyl esters; alkyldicarboxylic acids, and anhydrides thereof, and lower alkyl esters, such as succinic acid, adipic acid, sebacic acid, and azelaic acid; alkenylsuccinic acids, and alkylsuccinic acids, and anhydrides thereof, and lower alkyl esters, such as n-dodecenylsuccinic acid and n-dodecylsuccinic acid; unsaturated dicarboxylic acids, and anhydrides thereof, and lower alkyl esters, such as fumaric acid, maleic acid, citraconic acid, and itaconic acid; and the like. In the present invention, benzenedicarboxylic acids, such as terephthalic acid and isophthalic acid, are preferably used from the viewpoint of handling and reactivity.
[0040] Examples of trivalent or higher polyvalent carboxylic acid components that can be used in the preparation of the amorphous polyester include trimellitic acid, pyromellitic acid, 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, empol trimer acid, and anhydrides and lower alkyl esters thereof; [ka] (In formula (C), X represents an alkylene group or an alkenylene group. However, X is a substituent having 5 to 30 carbon atoms and having one or more side chains having 3 or more carbon atoms.) and polyvalent carboxylic acids and derivatives thereof, such as their anhydrides and lower alkyl esters, are examples of such tetracarboxylic acids. In the present invention, trimellitic acid is preferably used from the viewpoint of reactivity and ease of adjusting the resin acid value.
[0041] Further, examples of the alcohol component include polyhydric alcohols such as glycerin, pentaerythritol, sorbitol, sorbitan, and oxyalkylene ethers of novolac-type phenolic resins, and examples of the acid component include polyvalent carboxylic acids such as trimellitic acid, pyromellitic acid, 1,2,3,4-butanetetracarboxylic acid, benzophenonetetracarboxylic acid, and anhydrides thereof.
[0042] The amorphous polyester preferably contains 0.10 mol % or more and 30.00 mol % or less, and more preferably 1.00 mol % or more and 15.00 mol % or less, of the isosorbide unit represented by the formula (3) based on the total monomer units constituting the amorphous polyester. Note that the "monomer unit" refers to the reacted form of the monomer substance in the polymer. [ka]
[0043] The amorphous polyester resin having the isosorbide unit of the above formula (3) has a strong phase separation property with the crystalline material. Therefore, in the toner of the present invention, the crystalline material is easily transferred to the surface of the toner image during the fixing process, which is preferable. It is more preferable that the amorphous polyester contains 0.1 mol % or more and 30.0 mol % or less of the unit of formula (3), since the effect of the present invention is easily obtained.
[0044] In the present invention, the amorphous polyester containing the isosorbide unit of formula (3) as a constituent component is prepared by condensing a divalent carboxylic acid or anhydride thereof with isosorbide and a divalent alcohol represented by the following formula (4). Specifically, it can be prepared by a method of dehydration condensation at a reaction temperature of 180 to 260°C in a nitrogen atmosphere in a composition ratio in which a carboxyl group remains. In addition, a monovalent or divalent or higher alcohol other than isosorbide of the following formula (4) may be used in combination as necessary. As the divalent alcohol, the above-mentioned materials can be used. In addition, a monovalent or trivalent or higher carboxylic acid component or anhydride thereof may be used. As the above-mentioned monovalent, divalent, and trivalent carboxylic acids, the above-mentioned materials can be used. [ka] The SP value of amorphous polyester is 11.60 (J / cm 3 ) 0.5 More than 12.40(J / cm 3 ) 0.5 It is preferable that:
[0045] (Coloring agent) The colorants used in the present invention include the following organic pigments, organic dyes, and inorganic pigments. Cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Examples of magenta colorants include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinones, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Examples of black colorants include carbon black, and the above-mentioned yellow colorants, magenta colorants, cyan colorants, and colorants toned black using magnetic powder. These colorants can be used alone or in a mixture or in the form of a solid solution. The colorant used in the present invention is selected in terms of hue angle, chroma, brightness, light resistance, OHP transparency, and dispersibility in toner particles. In the present invention, the content of the colorant is from 1 part by mass to 10 parts by mass with respect to 100 parts by mass of the binder resin. When used in the suspension polymerization method, which is the preferred production method in the present invention, it is highly preferred that the colorant be subjected to a hydrophobic treatment before use.
[0046] When a magnetic powder is used as a colorant in the toner of the present invention, the magnetic powder is composed mainly of magnetic iron oxide such as iron oxide trioxide or γ-iron oxide, and may contain elements such as phosphorus, cobalt, nickel, copper, magnesium, manganese, aluminum, silicon, etc. These magnetic powders have a BET specific surface area of 2 to 30 m2 as measured by a nitrogen adsorption method. 2 / g, preferably 3 to 28m 2 / g. Also, it is preferable that the Mohs hardness is 5 to 7. The shape of the magnetic powder may be polyhedral, octahedral, hexahedral, spherical, needle-like, scale-like, etc., but those with less anisotropy such as polyhedral, octahedral, hexahedral, and spherical shapes are preferable in terms of increasing image density.
[0047] The amount of colorant added is preferably 1 part by mass or more and 20 parts by mass or less relative to 100 parts by mass of the binder resin or the polymerizable monomer constituting the binder resin. When a magnetic powder is used, the amount is preferably 20 parts by mass or more and 200 parts by mass or less, more preferably 40 parts by mass or more and 150 parts by mass or less, relative to 100 parts by mass of the binder resin or the polymerizable monomer constituting the binder resin.
[0048] The magnetic powder preferably has a number-average particle size of 0.10 μm or more and 0.40 μm or less. In general, the smaller the particle size of the magnetic powder, the higher the coloring power, but the magnetic powder is more likely to aggregate, which is undesirable because the magnetic powder is less uniformly dispersed in the toner. If the number-average particle size is less than 0.10 μm, the magnetic powder itself will be black with a reddish tinge, and the image will be particularly reddish in halftone images, which is undesirable because it cannot be said to be a high-quality image. On the other hand, if the number-average particle size exceeds 0.40 μm, the coloring power of the toner will be insufficient, and it will be difficult to achieve uniform dispersion in the suspension polymerization method (described later), which is a suitable method for producing the toner of the present invention, which is undesirable.
[0049] The number-average particle size of the magnetic powder can be measured using a transmission electron microscope. Specifically, the toner particles to be observed are thoroughly dispersed in an epoxy resin, and then the resin is cured for two days in an atmosphere at a temperature of 40°C to obtain a cured product. The cured product is cut into a thin-section sample using a microtome, and the particle sizes of 100 magnetic powder particles in the field of view are measured using a transmission electron microscope (TEM) at a magnification of 10,000 to 40,000. The number-average particle size is calculated based on the equivalent diameter of a circle that is equal to the projected area of the magnetic powder. It is also possible to measure the particle size using an image analyzer.
[0050] The magnetic powder used in the toner of the present invention can be produced, for example, by the following method. An alkali such as sodium hydroxide is added to an aqueous solution of a ferrous salt in an amount equivalent or greater to the iron component to prepare an aqueous solution containing ferrous hydroxide. Air is blown into the aqueous solution while maintaining the pH of the prepared aqueous solution at pH 7 or higher, and the aqueous solution is heated to 70°C or higher to carry out an oxidation reaction of the ferrous hydroxide, thereby first producing seed crystals that will become the cores of the magnetic iron oxide powder.
[0051] Next, an aqueous solution containing ferrous sulfate in an amount of about 1 equivalent based on the amount of alkali added previously is added to the slurry liquid containing the seed crystals. The reaction of ferrous hydroxide is allowed to proceed while air is blown in while maintaining the pH of the liquid at 5 to 10, and magnetic iron oxide powder is grown around the seed crystals as a core. At this time, the shape and magnetic properties of the magnetic powder can be controlled by selecting the desired pH, reaction temperature, and stirring conditions. As the oxidation reaction progresses, the pH of the liquid shifts to the acidic side, but it is preferable not to make the pH of the liquid less than 5. The magnetic material thus obtained can be filtered, washed, and dried in the usual manner to obtain magnetic powder.
[0052] In the present invention, when the toner is produced in an aqueous medium, it is highly preferable to subject the magnetic powder surface to a hydrophobic treatment. When performing the surface treatment in a dry manner, the washed, filtered and dried magnetic powder is treated with a coupling agent. When performing the surface treatment in a wet manner, the dried powder is redispersed after the oxidation reaction is completed, or the iron oxide obtained by washing and filtering after the oxidation reaction is redispersed in another aqueous medium without drying, and then the coupling treatment is performed. In the present invention, either the dry method or the wet method can be appropriately selected.
[0053] Coupling agents that can be used in the surface treatment of the magnetic powder in the present invention include, for example, silane coupling agents, titanium coupling agents, etc. More preferably used are silane coupling agents, which are represented by the general formula (I). R m SiY n (I) [In the formula, R represents an alkoxy group, m represents an integer of 1 to 3, Y represents a functional group such as an alkyl group, a phenyl group, a vinyl group, an epoxy group, or a (meth)acrylic group, and n represents an integer of 1 to 3, provided that m+n=4.]
[0054] Examples of the silane coupling agent represented by the general formula (I) include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltriacetoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, Examples of the silane include diphenyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, n-propyltrimethoxysilane, isopropyltrimethoxysilane, n-butyltrimethoxysilane, isobutyltrimethoxysilane, trimethylmethoxysilane, n-hexyltrimethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, hydroxypropyltrimethoxysilane, n-hexadecyltrimethoxysilane, and n-octadecyltrimethoxysilane. In the present invention, those in which Y in the general formula (I) is an alkyl group can be preferably used. Among them, alkyl groups having 3 to 6 carbon atoms are preferred, and those having 3 or 4 carbon atoms are particularly preferred. When the above-mentioned silane coupling agents are used, they can be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the treatment can be performed with each coupling agent individually or simultaneously. The total amount of coupling agent used is preferably 0.9 to 3.0 parts by mass per 100 parts by mass of magnetic powder, and it is important to adjust the amount of treatment agent depending on the surface area of the magnetic powder, the reactivity of the coupling agent, etc.
[0055] In order to produce the toner of the present invention, it is preferable to improve the affinity between the colorant and the crystalline material. When a silane coupling agent is used as a hydrophobic treatment agent, the conditions for treating the colorant with the silane coupling agent are appropriately adjusted in order to improve the affinity with the crystalline material.
[0056] Specifically, A / (I A +I B ) / M Si A method for adjusting (equation (5)) is described below. When a silane coupling agent is used as a hydrophobic treatment agent, the silane compound obtained by hydrolyzing the silane coupling agent under acidic conditions is generally subjected to a condensation reaction with a colorant under alkaline conditions. The above-mentioned colorant is then washed and dried to obtain a hydrophobically treated colorant. When hydrophobic treatment is performed using this procedure, most of the hydrophobic treatment agent is bonded to the colorant, and there are few components that are condensed between the treatment agents themselves, so I A / (I A +I B ) / M Si becomes smaller. I A / (I A +I B ) / M Si In order to increase the I, the colorant is hydrophobized using a silane compound that has been pretreated with a silane coupling agent under conditions that facilitate simultaneous hydrolysis and condensation reactions. By simultaneously hydrolyzing and condensing the silane coupling agent, a silane compound containing a large amount of oligomers in which silane coupling agents are condensed together can be obtained. By hydrophobizing the colorant using this silane compound, the silane compound can be divided into two types: one that directly bonds to the colorant and one that is condensed and bonds to the colorant at its end. Thus, the greater the amount of condensed silane compound, the greater the I. A / (I A +I B ) / M Si The magnetic material thus obtained exhibits high hydrophobicity and can improve its affinity with crystalline materials that also have high hydrophobicity. The preferred pH range for producing the silane compound is 7.0 to 10.0, more preferably 8.0 to 9.5. The preferred pH range for hydrophobizing a colorant with the silane compound is 7.0 to 11.0, more preferably 8.0 to 9.5.
[0057] (crystalline material) The crystalline material will now be described. There are no particular limitations on the crystalline material, and any known material can be used. A crystalline material is one that exhibits a clear melting point when measured using a differential scanning calorimeter (DSC). In the present invention, from the viewpoints of low-temperature fixability and releasability, it is preferable to use ester wax, hydrocarbon wax, or crystalline polyester resin. The ester wax is a wax whose main component is a fatty acid ester.
[0058] Preferred ester waxes are described below. The functionality described below indicates the number of ester groups contained in one molecule. For example, behenyl behenate is called a monofunctional ester wax, and dipentaerythritol hexabehenate is called a hexafunctional ester wax. The monofunctional ester wax is preferably a condensate of an aliphatic alcohol and an aliphatic carboxylic acid, in which the aliphatic carbon number is preferably 6 to 26.
[0059] Examples of aliphatic alcohols include 1-hexanol, 1-heptanol, 1-octanol, 1-nonanol, 1-decanol, undecyl alcohol, and lauryl alcohol, and examples of aliphatic carboxylic acids include pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, and decanoic acid.
[0060] As the bifunctional ester wax, a combination of a dicarboxylic acid and a monoalcohol, or a diol and a monocarboxylic acid can be used.
[0061] Dicarboxylic acids include adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid.
[0062] Examples of diols include 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol.
[0063] The monoalcohol to be condensed with the dicarboxylic acid is preferably an aliphatic alcohol.Specific examples thereof include tetradecanol, pentadecanol, hexadecanol, heptadecanol, octadecanol, nonadecanol, eicosanol, docosanol, tricosanol, tetracosanol, pentacosanol, hexacosanol, and octacosanol.Of these, docosanol is preferred from the viewpoint of fixing property and developing property.
[0064] The monocarboxylic acid to be condensed with the diol is preferably an aliphatic carboxylic acid.Specific examples of the fatty acid include lauric acid, myristic acid, palmitic acid, margaric acid, stearic acid, tuberculostearic acid, arachidic acid, behenic acid, lignoceric acid, and cerotic acid.Of these, behenic acid is preferred from the viewpoint of fixing property and developing property.
[0065] Although linear fatty acids and linear alcohols are exemplified here, they may have a branched structure.
[0066] The crystalline polyester resin is not particularly limited and any known crystalline polyester resin can be used, but it is preferably a saturated polyester. Furthermore, the crystalline polyester resin is preferably a condensate of an aliphatic dicarboxylic acid and an aliphatic diol, and an aliphatic monocarboxylic acid and / or an aliphatic monoalcohol. More preferably, it is a condensate of an aliphatic dicarboxylic acid and an aliphatic diol, and an aliphatic monocarboxylic acid. By including an aliphatic monocarboxylic acid and / or an aliphatic monoalcohol as a component of the crystalline polyester resin, it becomes easier to adjust the molecular weight and hydroxyl value of the crystalline polyester resin.
[0067] Examples of monomers that can be used are given below. Examples of the aliphatic dicarboxylic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexadecanedicarboxylic acid, and octadecanedicarboxylic acid.
[0068] Examples of aliphatic diols include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, trimethylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,16-hexadecanediol, and 1,18-octadecanediol.
[0069] Examples of aliphatic monocarboxylic acids include decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), eicosanoic acid (arachidic acid), docosanoic acid (behenic acid), and tetracosanoic acid (lignoceric acid).
[0070] Examples of the aliphatic monoalcohols include lauryl alcohol, stearyl alcohol, and behenyl alcohol.
[0071] By using such a monocarboxylic acid and monoalcohol, a crystalline polyester resin having an alkyl group (preferably having 2 to 24 carbon atoms) at the terminal can be obtained. Here, since the monocarboxylic acid has one carboxylic acid, the structure derived from the monocarboxylic acid is located at the end of the molecular chain of the crystalline polyester resin. The weight average molecular weight Mw of the crystalline polyester resin is preferably 5,000 or more and 60,000 or less.
[0072] The crystalline polyester resin can be produced by a conventional polyester synthesis method, for example, by subjecting a dicarboxylic acid component and a diol component to an esterification reaction or an ester exchange reaction, followed by a conventional polycondensation reaction under reduced pressure or by introducing nitrogen gas.
[0073] The hydrocarbon wax is an aliphatic hydrocarbon wax, such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, Fischer-Tropsch wax, paraffin wax, polyolefin wax, and the like.
[0074] In the present invention, a plurality of crystalline materials can be used in combination. In this case, the SP value of the crystalline material detected as S2 is defined as the SPc of the present invention.
[0075] (Binding resin) Examples of the binder resin used in the toner of the present invention include homopolymers of styrene and its substitutes, such as polystyrene and polyvinyltoluene; styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-dimethylaminoethyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-dimethylaminoethyl methacrylate copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl ethyl ether copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; and styrene-based copolymers, such as polymethyl methacrylate, polybutyl methacrylate, polyvinyl acetate, polyethylene, polypropylene, polyvinyl butyral, silicone resins, polyester resins, polyamide resins, epoxy resins, and polyacrylic acid resins, which may be used alone or in combination of two or more. Among these, styrene-acrylic resins, such as styrene-butyl acrylate, are particularly preferred in terms of developing properties, fixing properties, and the like.
[0076] Examples of the polymerizable monomer that forms the styrene-acrylic resin include the following. Examples of the styrene-based polymerizable monomer include styrene; α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, and p-methoxystyrene. Examples of the acrylic polymerizable monomer include acrylic polymerizable monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, iso-propyl acrylate, n-butyl acrylate, iso-butyl acrylate, tert-butyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, and cyclohexyl acrylate. Examples of the methacrylic polymerizable monomer include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, and n-octyl methacrylate.
[0077] The method for producing the styrene-acrylic resin is not particularly limited, and any known method can be used. The binder resin can also be used in combination with other known resins.
[0078] The toner of the present invention may contain a charge control agent in order to keep the chargeability of the toner stable regardless of the environment. Examples of negatively charged charge control agents include monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic and dicarboxylic acid-based metal compounds, aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides, esters, phenol derivatives such as bisphenol, urea derivatives, metal-containing salicylic acid compounds, metal-containing naphthoic acid compounds, boron compounds, quaternary ammonium salts, calixarene, and resin-based charge control agents. Examples of positively charged charge control agents include the following: nigrosine and nigrosine modified with fatty acid metal salts, guanidine compounds, imidazole compounds, quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate and tetrabutylammonium tetrafluoroborate, and onium salts such as phosphonium salts analogous thereto, and lake pigments thereof, triphenylmethane dyes and lake pigments thereof (lake agents include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide, etc.), metal salts of higher fatty acids, diorganotin oxides such as dibutyltin oxide, dioctyltin oxide, and dicyclohexyltin oxide, diorganotin borates such as dibutyltin borate, dioctyltin borate, and dicyclohexyltin borate, and resin-based charge control agents. These can be used alone or in combination of two or more. Among them, as the charge control agent other than the resin-based charge control agent, a metal-containing salicylic acid compound is preferable, and particularly, the metal is aluminum or zirconium. The most preferable control agent is an aluminum salicylic acid compound. As the resin-based charge control agent, it is preferable to use a polymer or copolymer having a sulfonic acid group, a sulfonate group or a sulfonate ester group, a salicylic acid moiety, or a benzoic acid moiety. The amount of the charge control agent to be added is preferably 0.01 to 20 parts by weight, and more preferably 0.05 to 10 parts by weight, per 10.0 parts by weight of the polymerizable monomer.
[0079] The weight average particle diameter (D4) of the toner produced by the present invention is preferably 4.0 μm to 11.0 μm, more preferably 5.0 μm to 10.0 μm. When the weight average particle diameter (D4) is 4.0 μm to 11.0 μm, particularly good fluidity is obtained, and the latent image can be developed faithfully.
[0080] (Toner manufacturing method) The toner of the present invention can be produced by any known method. First, when produced by a pulverization method, for example, necessary components for a toner such as a binder resin, a colorant, a wax, and optionally a charge control agent, and other additives are thoroughly mixed in a mixer such as a Henschel mixer or a ball mill. Then, the toner materials are melt-kneaded using a thermal kneader such as a heating roll, a kneader, or an extruder to disperse or dissolve them, cooled and solidified, pulverized, classified, and if necessary, surface-treated to obtain toner particles. The order of classification and surface treatment does not matter. In the classification step, it is preferable to use a multi-division classifier in terms of production efficiency.
[0081] The pulverization step can be carried out by a method using a known pulverizing device such as a mechanical impact type or a jet type. It is also preferable to pulverize the toner by applying heat or to perform a treatment of applying a mechanical impact as an auxiliary. In addition, a water bath method in which the finely pulverized (classified as necessary) toner particles are dispersed in hot water, or a method in which the toner particles are passed through a hot air current may also be used. Examples of the means for applying mechanical impact force include a method using a mechanical impact grinder such as the Kryptron System manufactured by Kawasaki Heavy Industries, Ltd. or the Turbo Mill manufactured by Turbo Kogyo Co., Ltd. Also usable are devices such as the Mechanofusion System manufactured by Hosokawa Micron Corporation or the Hybridization System manufactured by Nara Machinery Manufacturing Co., Ltd. These devices use centrifugal force to press the toner against the inside of a casing with a blade rotating at high speed, and apply mechanical impact force to the toner by forces such as compression force and friction force.
[0082] When the toner of the present invention is produced by a pulverization method, a step of forming a shell is required in order to obtain a toner having a desired core-shell structure. The toner of the present invention can be produced by the pulverization method as described above. However, since the toner of the present invention needs to have a certain amount of crystalline material on the toner surface and to have a shell formed of an amorphous resin with a large SP value difference, it is preferable to produce the toner in an aqueous medium.
[0083] When producing a toner by emulsion aggregation, if a crystalline material is aggregated so as to be exposed on the surface of the toner, and then an amorphous resin having a large SP value difference from the crystalline material is used, there is a problem that the formation of the shell is easily hindered. To solve this problem, a small amount of an amorphous resin having a relatively small SP value difference from the crystalline material is aggregated on the surface of the toner, and then a shell is formed using another amorphous resin having a relatively large SP value difference, thereby obtaining the toner of the present invention.
[0084] The suspension polymerization method will be described below. In the suspension polymerization method, a polymerizable monomer and a colorant (and, if necessary, a polymerization initiator, a crosslinking agent, a charge control agent, and other additives) are uniformly dissolved or dispersed to obtain a polymerizable monomer composition. This polymerizable monomer composition is then dispersed in a continuous layer (e.g., an aqueous phase) containing a dispersant using an appropriate stirrer, and a polymerization reaction is simultaneously carried out to obtain a toner having a desired particle size. The toner obtained by this suspension polymerization method (hereinafter also referred to as "polymerized toner") has an almost uniform spherical shape for each toner particle, and therefore the distribution of the charge amount is relatively uniform, and therefore improvement in image quality can be expected.
[0085] In the production of the polymerized toner according to the present invention, examples of the polymerizable monomer constituting the polymerizable monomer composition include the following. Examples of the polymerizable monomer include styrene-based monomers such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, and p-ethylstyrene; acrylic acid esters such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, n-propyl acrylate, n-octyl acrylate, dodecyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, 2-chloroethyl acrylate, and phenyl acrylate; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-octyl methacrylate, dodecyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, phenyl methacrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate; and other monomers such as acrylonitrile, methacrylonitrile, and acrylamide. These monomers may be used alone or in combination. Among the above-mentioned monomers, it is preferable to use styrene alone or in combination with other monomers from the viewpoint of the developing characteristics and durability of the toner.
[0086] The polymerization initiator used in the production of the toner of the present invention by polymerization preferably has a half-life of 0.5 to 30 hours during the polymerization reaction. When the polymerization reaction is carried out using an initiator in an amount of 0.5 to 20 parts by mass per 100 parts by mass of the polymerizable monomer, a polymer having a molecular weight maximum between 5,000 and 50,000 can be obtained, which can provide the toner with desirable strength and suitable melting properties. Specific examples of the polymerization initiator include azo or diazo polymerization initiators such as 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile; and peroxide polymerization initiators such as benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, t-butyl peroxy 2-ethylhexanoate, and t-butyl peroxypivalate.
[0087] When the toner of the present invention is produced by a polymerization method, a crosslinking agent may be added. By increasing the amount of the crosslinking agent, the viscosity at 120° C. in the present invention can be increased. The preferred amount of the crosslinking agent is 0.001 to 15 parts by mass per 100 parts by mass of the polymerizable monomer. As the crosslinking agent, a compound having two or more polymerizable double bonds is mainly used, and examples of the crosslinking agent include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; carboxylic acid esters having two double bonds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, and 1,3-butanediol dimethacrylate; divinyl compounds such as divinylaniline, divinyl ether, divinyl sulfide, and divinyl sulfone; and compounds having three or more vinyl groups. These may be used alone or in the form of a mixture of two or more kinds.
[0088] In the method of producing the toner of the present invention by polymerization, the above-mentioned toner composition and the like are generally appropriately added, and the polymerizable monomer composition is uniformly dissolved or dispersed by a dispersing machine such as a homogenizer, a ball mill, or an ultrasonic dispersing machine, and then suspended in an aqueous medium containing a dispersing agent. At this time, the particle size of the obtained toner particles is sharper if a high-speed dispersing machine such as a high-speed stirrer or an ultrasonic dispersing machine is used to obtain the desired toner particle size at once. The timing of adding the polymerization initiator may be the same as when other additives are added to the polymerizable monomer, or it may be mixed just before suspending in the aqueous medium. Also, the polymerization initiator dissolved in the polymerizable monomer or solvent may be added just after granulation and before starting the polymerization reaction. After granulation, stirring may be carried out using a conventional stirrer to such an extent that the particle state is maintained and the floating and settling of the particles is prevented.
[0089] When producing the toner of the present invention, known surfactants, organic dispersants, and inorganic dispersants can be used as dispersants. Among them, inorganic dispersants are preferably used because they are unlikely to produce harmful ultrafine powder, and because they obtain dispersion stability due to their steric hindrance, their stability is unlikely to be lost even when the reaction temperature is changed, and they are easy to wash and do not adversely affect the toner. Examples of such inorganic dispersants include polyvalent metal phosphates such as tricalcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, and hydroxyapatite, carbonates such as calcium carbonate and magnesium carbonate, inorganic salts such as calcium metasilicate, calcium sulfate, and barium sulfate, and inorganic compounds such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide.
[0090] The inorganic dispersant is preferably used in an amount of 0.2 to 20 parts by mass per 100 parts by mass of the polymerizable monomer. The dispersant may be used alone or in combination with a plurality of kinds. Furthermore, a surfactant may be used in an amount of 0.001 to 0.1 parts by mass. When using these inorganic dispersants, they may be used as they are, but in order to obtain finer particles, the inorganic dispersant particles may be formed in an aqueous medium and used. For example, in the case of tricalcium phosphate, a sodium phosphate aqueous solution and a calcium chloride aqueous solution are mixed under high speed stirring to form water-insoluble calcium phosphate, which allows for more uniform and fine dispersion. At the same time, a water-soluble sodium chloride salt is by-produced, but if a water-soluble salt is present in the aqueous medium, the dissolution of the polymerizable monomer in water is suppressed, making it difficult to generate ultrafine toner particles by emulsion polymerization, which is more convenient.
[0091] Examples of the surfactant include sodium dodecylbenzene sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, sodium oleate, sodium laurate, sodium stearate, and potassium stearate. In the step of polymerizing the polymerizable monomer, the polymerization temperature is set to 40°C or higher, generally 50°C to 90°C.
[0092] When producing the toner having a core-shell structure of the present invention, the crystalline material is easily encapsulated inside the toner by using an amorphous thermoplastic resin having a large difference in SP value from the crystalline material. This causes a problem that S2 is likely to be less than 1%. In order to solve this problem, a material that has a high affinity with the crystalline material and that is likely to be unevenly distributed near the surface of the toner is simultaneously used, which makes it easier to achieve formulas (1) and (2) of the present invention. Specifically, in order to produce the toner of the present invention by the suspension polymerization method, it is preferable to use a hydrophobized magnetic material and a hydrophobized pigment. It is particularly preferable to use a hydrophobized magnetic material and a hydrophobized pigment in order to improve the affinity with the crystalline material. A / (I A +I B ) / M Si It is preferable to use a hydrophobic magnetic material having a high value of I. Even if the magnetic material is hydrophobized, it still has some hydrophilicity. Therefore, when the toner is produced by the suspension polymerization method, the magnetic material is unevenly distributed near the surface of the toner. A / (I A +I B) / M Si By using a treated magnetic material with a high SP value, the crystalline material is likely to be present near the magnetic material. As a result, the crystalline material is also likely to be present near the surface. Therefore, even if an amorphous thermoplastic resin with a large SP value difference from the crystalline material is used, the S2 can be controlled within the range of the present invention, and a toner having a core-shell structure of the present invention can be obtained.
[0093] The obtained polymer particles are filtered, washed, and dried by a known method to obtain toner particles. The toner particles are mixed with inorganic fine powder as described below as necessary and attached to the surface of the toner particles to obtain the toner of the present invention. It is also possible to insert a classification process into the manufacturing process (before mixing with inorganic fine powder) to remove coarse powder and fine powder contained in the toner particles.
[0094] The toner of the present invention is prepared by mixing additives such as a fluidizing agent, if necessary, with the toner particles obtained by the above-mentioned production method. As a mixing method, a known method can be used, and for example, a Henschel mixer is a suitable device.
[0095] The toner of the present invention is preferably in a form in which an inorganic fine powder having a number average primary particle diameter of 4 to 80 nm, more preferably 6 to 40 nm, is added to the toner particles as a fluidizing agent. The inorganic fine powder is added to improve the fluidity of the toner and to make the charge of the toner particles uniform, but it is also preferable to give the inorganic fine powder a function of adjusting the charge amount of the toner and improving environmental stability by treating the inorganic fine powder, for example, to make it hydrophobic. The number average primary particle diameter of the inorganic fine powder is measured using a photograph of the toner taken enlarged by a scanning electron microscope.
[0096] As the inorganic fine powder used in the present invention, silica, titanium oxide, alumina, etc. can be used. As the silica fine powder, for example, both dry silica, called dry method or fumed silica, produced by vapor phase oxidation of silicon halide, and wet silica produced from water glass, etc. can be used. However, there are few silanol groups on the surface and inside of the silica fine powder, and Na2O, SO3 2- Dry silica, which produces less production residue such as fluorine, is preferred. In the case of dry silica, it is also possible to obtain a composite fine powder of silica and other metal oxides by using other metal halide compounds such as aluminum chloride and titanium chloride together with the silicon halide compound in the production process, and these are also included.
[0097] The amount of inorganic fine powder having a number-average primary particle size of 4 to 80 nm is preferably 0.1 to 3.0% by mass relative to the toner particles, and if the amount is less than 0.1% by mass, the effect is insufficient, and if it is 3.0% by mass or more, the fixing property becomes poor. The content of inorganic fine powder can be quantified using a calibration curve created from a standard sample by using fluorescent X-ray analysis.
[0098] In the present invention, it is preferable that the inorganic fine powder is hydrophobized, since it can improve the environmental stability of the toner. When the inorganic fine powder added to the toner absorbs moisture, the charge amount of the toner particles is significantly reduced, the charge amount is easily non-uniform, and the toner is easily scattered. As the treatment agent used for the hydrophobization treatment of the inorganic fine powder, silicone varnish, various modified silicone varnishes, silicone oil, various modified silicone oils, silane compounds, silane coupling agents, other organic silicon compounds, organic titanium compounds, etc., may be used alone or in combination of two or more kinds.
[0099] The toner of the present invention may further contain other additives, for example, lubricant powders such as fluororesin powder, zinc stearate powder, and polyvinylidene fluoride powder; abrasives such as cerium oxide powder, silicon carbide powder, and strontium titanate powder; flowability imparting agents such as titanium oxide powder and aluminum oxide powder; caking inhibitors; and organic and inorganic fine particles of opposite polarity as developing property improvers, in a small amount within a range that does not substantially adversely affect the toner. The surfaces of these additives may also be hydrophobized before use.
[0100] Next, an example of an electrophotographic image forming apparatus in which the toner of the present invention can be suitably used will be specifically described with reference to FIG. 1. In FIG. 1, 100 denotes a photosensitive drum, and around it are provided a primary charging roller 117, a developing device 140 equipped with a stirring member 141 having a developing sleeve 102 and a developing blade 103, a transfer charging roller 114, a cleaner 116, a register roller 124, and the like. The photosensitive drum 100 is charged to, for example, -600 V by the primary charging roller 117 (applied voltage is, for example, AC voltage 1.85 kVpp, DC voltage -620 Vdc). Then, exposure is performed by irradiating the photosensitive drum 100 with a laser beam 123 by a laser generator 121, and an electrostatic latent image corresponding to a target image is formed. The electrostatic latent image on the photosensitive drum 100 is developed with one-component toner by the developing device 140 to obtain a toner image, and the toner image is transferred onto a transfer material by a transfer roller 114 abutted against the photosensitive drum 100 via the transfer material. The transfer material carrying the toner image is transported by a transport belt 125 or the like to a fixing device 126, where the toner image is fixed onto the transfer material. Also, the toner remaining on the photoconductor is partially removed by a cleaner 116. Although an image forming apparatus using magnetic one-component jumping development has been shown here, the image forming apparatus may be used for either jumping development or contact development.
[0101] Next, methods for measuring various physical properties related to the toner of the present invention will be described. (Melt point measurement of crystalline materials) The melting point of the crystalline material can be determined as the peak top temperature of the endothermic peak when measured by DSC. If necessary, it is isolated from the toner by the above-mentioned method. The measurement is performed in accordance with ASTM D 3417-99. For these measurements, for example, PerkinElmer's DSC-7, TA Instruments' DSC2920, and TA Instruments' Q1000 can be used. The melting points of indium and zinc are used to correct the temperature of the device's detector, and the heat of fusion of indium is used to correct the amount of heat. An aluminum pan is used as the measurement sample, and an empty pan is set as a control for the measurement.
[0102] (Measurement of weight average particle diameter (D4) and number average particle diameter (D1) of toner (particles)) The weight-average particle size (D4) and number-average particle size (D1) of the toner (particles) are measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube, and the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), for setting measurement conditions and analyzing measurement data, and are calculated by analyzing the measurement data. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0103] Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.
[0104] The specific measurement method is as follows. (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube. (2) Approximately 30 ml of the above-mentioned aqueous electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and approximately 0.3 ml of a solution prepared by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, with a pH of 7, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water is added as a dispersant. (3) A predetermined amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 ml of the Conaminon N is added to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner (particles) is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, add the electrolytic solution (5) in which the toner (particles) is dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to graph / volume %, the "average diameter" on the "analysis / volume statistics (arithmetic mean)" screen is the weight-average particle size (D4), and when the dedicated software is set to graph / number %, the "average diameter" on the "analysis / number statistics (arithmetic mean)" screen is the number-average particle size (D1).
[0105] (Method of measuring molecular weight of crystalline materials) The molecular weights of the crystalline material and the amorphous thermoplastic resin are measured by gel permeation chromatography (GPC) as follows. First, a specimen is dissolved in tetrahydrofuran (THF) at room temperature. The obtained solution is then filtered through a solvent-resistant membrane filter "Maeshori Disk" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: High-speed GPC equipment "HLC-8220GPC" [Tosoh Corporation] Column: LF-604 in two columns Eluent:THF Flow rate: 0.6ml / min Oven temperature: 40℃ Sample injection volume: 0.020ml In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using a standard polystyrene resin (for example, trade names “TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500”), manufactured by Tosoh Corporation) is used.
[0106] (Measurement of the glass transition temperature of the resin and toner) The glass transition temperature (Tg) of the amorphous thermoplastic resin and toner is measured in accordance with ASTM D3418-82 using a differential scanning calorimeter “Q1000” (manufactured by TA Instruments). For temperature correction of the apparatus detection part, the melting points of indium and zinc are used, and for heat quantity correction, the heat of fusion of indium is used. Precisely weigh 3.0 mg of the amorphous saturated polyester resin or toner as the measurement sample. Place this in an aluminum pan, use an empty aluminum pan as a reference, and perform the measurement at a temperature rising rate of 10 ° C / min in the temperature range of 30 to 200 ° C under normal temperature and humidity. In this temperature rising process, a specific heat change can be obtained in the temperature range of 40 ° C to 100 ° C. The intersection of the line at the midpoint between the baseline before and after the specific heat change appears and the differential thermal curve is defined as the glass transition temperature (Tg).
[0107] <Method for measuring SP value> The SP value used in the present invention is calculated from the types and ratios of the monomers constituting the resin by the commonly used Fedors method [Poly.Eng.Sci., 14(2)147 (1974)]. The SP value can be controlled by the types and amounts of the monomers. To increase the SP value, for example, a monomer with a large SP value may be used. On the other hand, to decrease the SP value, for example, a monomer with a small SP value may be used. The unit of the SP value in the present invention is (cal / cm 3 ) 0.5 is.
[0108] <Calculation method for S2, the ratio of area occupied by crystalline material> To calculate the ratio S2 (%) of the area occupied by crystalline material per area of the toner, the toner was dyed for 15 minutes in a RuO4 gas atmosphere of 500 Pa using a vacuum electron dyeing device (Filgen, VSC4R1H), and the image obtained by backscattered electron image observation using a field emission scanning electron microscope S-4800 (Hitachi High-Technologies) was used. Pour liquid nitrogen into the anti-contamination trap attached to the S-4800 housing until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2, and execute it. Check that the emission current due to flushing is 20 to 40 μA. Insert the sample holder into the sample chamber of the S-4800 housing. Press [Origin] on the control panel to move the sample holder to the observation position. Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [5.0 kV] and the emission current to [20 μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Upper (U)] and [+BSE], and select [LA100] in the selection box to the right of [+BSE] to set the observation mode to backscattered electron images. In the [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [3.0 mm]. Press the [ON] button in the accelerating voltage display of the control panel to apply the accelerating voltage. Adjust the focus to the domain of crystalline material that appears black under the above observation conditions, and save the SEM image. The image obtained is processed using the image processing software "Image-Pro Plus (Media Cybernetics)" to calculate the percentage of the area occupied by crystalline material. The area percentage occupied by the crystalline material is measured for 100 toner particles. The area percentage occupied by the crystalline material is the ratio of the area of the crystalline material to the area of the toner.
[0109] <Method of measuring toner viscosity> The melt viscosity of the toner at a temperature of 120° C. was determined from the viscosity value of the toner using a flow tester temperature rise method. The measurement was performed using a flow tester CFT-500D (manufactured by Shimadzu Corporation) under the following conditions. Sample: Approximately 1.1 g of toner is weighed out and molded in a pressure molding machine to create a sample. Die hole diameter: 0.5mm Die length: 1.0mm Cylinder pressure: 9.807×10 5 (Pa) Measurement mode: Temperature ramp method Heating rate: 4.0℃ / min By the above method, the viscosity of the toner is measured at temperatures of 50° C. to 200° C., and the viscosity at a temperature of 120° C. is obtained.
[0110] In addition, by using the toner of the present invention, it is possible to obtain a process cartridge that contributes to the formation of electrophotographic images that are excellent in low-temperature fixing property, durability, and prevention of contamination of transport members.In addition, by using the toner of the present invention, it is possible to obtain an electrophotographic image forming apparatus that can form electrophotographic images that are excellent in low-temperature fixing property, durability, and prevention of contamination of transport members. EXAMPLES
[0111] The present invention will be described in more detail below with reference to Production Examples and Examples, which are not to be construed as limiting the present invention in any way. Note that the numbers of parts in the following formulations all refer to parts by mass.
[0112] <Manufacturing example of magnetic body 1> (Production of magnetic iron oxide) An aqueous solution containing ferrous hydroxide was prepared by mixing 1.00 to 1.10 equivalents of caustic soda solution relative to iron element, P2O5 in an amount equivalent to 0.15 mass% of iron element in terms of phosphorus element, and SiO2 in an amount equivalent to 0.50 mass% of iron element in terms of silicon element into an aqueous solution of ferrous sulfate. The pH of the aqueous solution was adjusted to 8.0, and an oxidation reaction was carried out at 85°C while blowing in air, to prepare a slurry liquid containing seed crystals. Next, an aqueous solution of ferrous sulfate was added to this slurry in an amount of 0.90 to 1.20 equivalents relative to the initial amount of alkali (the sodium component of the caustic soda). The pH of the slurry was then maintained at 7.6, and the oxidation reaction was allowed to proceed while blowing in air, yielding a slurry containing iron oxide.
[0113] (Production of silane compounds) 30 parts by mass of iso-butyltrimethoxysilane was dropped into 70 parts by mass of ion-exchanged water while stirring. Then, this aqueous solution was kept at pH 9.0 and temperature 45°C, and dispersed for 120 minutes at a peripheral speed of 0.46 m / s using a dispersing blade to advance the hydrolysis and condensation reaction. After that, the pH was adjusted to 9.0, and the solution was immediately cooled to 10°C to stop the hydrolysis and condensation reaction. Thus, a liquid containing a silane compound was obtained. Here, the pH (pH1) at which the hydrolysis and condensation reaction of the silane coupling agent was advanced was 9.0.
[0114] (Manufacture of magnetic body 1) The above-mentioned iron oxide-containing slurry was dispersed with a pin mill, while 4.7 parts by mass of the above-mentioned silane compound-containing liquid was added to 100 parts by mass of magnetic iron oxide. At this time, the pH was kept at 9.0 and the temperature was kept at 55°C, and the dispersion was carried out for 60 minutes to proceed with hydrophobization treatment of the magnetic material. Thereafter, the above-mentioned dispersion was filtered using a filter press and washed with a large amount of water. Further, it was dried at 120°C for 2 hours, and the obtained particles were crushed and passed through a sieve with an opening of 100 μm to obtain magnetic material 1 having a number-average particle size of 230 nm. Here, the pH (pH2) at which the reaction of the silane compound with the magnetic material proceeded was 9.0.
[0115] <Production Examples of Magnetic Materials 2 to 5> Magnetic materials 2 to 5 were obtained using the same apparatus and under the same conditions as for producing magnetic material 1, except that the hydrophobizing agent and treatment conditions (hydrophobizing agent, pH 1, and pH 2) were changed to those shown in Table 1.
[0116] [Table 1]
[0117] <Production Example of Amorphous Thermoplastic Resin 1> 100 parts by mass of a mixture of raw material monomers other than trimellitic anhydride in the amounts shown in Table 2 below, and 0.52 parts by mass of tin di(2-ethylhexanoate) catalyst were placed in a polymerization tank equipped with a nitrogen introduction line, a dehydration line, and an agitator. Next, after the polymerization tank was filled with nitrogen, a polycondensation reaction was carried out for 6 hours while heating at 200°C. After further increasing the temperature to 210°C, trimellitic anhydride was added, and the pressure in the polymerization tank was reduced to 40 kPa, after which a further condensation reaction was carried out. The acid value, hydroxyl value, and molecular weight of the obtained resin were as shown in Table 2. This resin is called amorphous thermoplastic resin 1. In addition, isosorbide in the table is a compound having the structure of the above formula (4).
[0118] (Production Examples of Amorphous Thermoplastic Resins 2 to 9) Amorphous thermoplastic resins 2 to 9 were produced by the same operation as for amorphous thermoplastic resin 1, using the raw material monomer charging amounts shown in Table 2 below. At that time, sequential sampling and measurement were performed, and when the desired molecular weight was reached, the polymerization reaction was stopped and the resin was taken out of the polymerization tank. The physical properties of the obtained resin are shown in Table 2 below. In addition, in the production of amorphous thermoplastic resin 8, BPA was used in a molar ratio of 45.0 to 44.2, consisting of bisphenol A propylene oxide 3-mol adduct and bisphenol A ethylene oxide 2-mol adduct. In the production of amorphous thermoplastic resin 9, BPA was used in a molar ratio of 29.8 to 33.0, consisting of bisphenol A propylene oxide 3-mol adduct and bisphenol A ethylene oxide 2-mol adduct. When BPA was not specified, bisphenol A propylene oxide 3-mol adduct was used.
[0119] [Table 2] *The monomer composition is expressed as a molar ratio when the total moles of the alcohol component is taken as 100. The abbreviations in the above table are: TPA: Terephthalic acid IPA: Isophthalic acid TMA: Trimellitic acid BPA: Bisphenol A EG: Ethylene glycol Shows.
[0120] <Toner 1 Manufacturing Example> 850 parts by mass of 0.1 mol / L-Na3PO4 aqueous solution was added to a vessel equipped with a high-speed stirring device Clearmix (manufactured by M Technique Co., Ltd.), and heated to 60°C while stirring at a rotation speed of 33 m / s. 68 parts by mass of 1.0 mol / L-CaCl2 aqueous solution was added to the vessel, preparing an aqueous medium containing a trace amount of poorly water-soluble dispersant Ca3(PO4)2. A solution was prepared by mixing and dissolving the following materials using a propeller-type stirrer. When mixing the following materials, the rotation speed of the stirrer was set to 100 r / min. Styrene 75.0 parts by weight n-Butyl acrylate 25.0 parts by weight Amorphous polyester-1 3.0 parts by weight Hydrophobic magnetic material 1 90.0 mass Department ·Mo Iron complex of noazo dye (T-77: manufactured by Hodogaya Chemical Co., Ltd.) 1.0 parts by mass 1,6-Hexanediol diacrylate 0.5 parts by weight ·Crystalline material 1 20.0 parts by mass The mixture was then heated to 60°C and stirred in a TK homomixer (manufactured by Primix Corporation (formerly Tokushu Kika Kogyo Co., Ltd.)) with the agitator rotation speed set to 9000 r / min to dissolve and disperse the solids. 10.0 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) as a polymerization initiator was added to the mixture and dissolved in the mixture to prepare a polymerizable monomer composition. Next, the polymerizable monomer composition was added to the aqueous medium and heated to a temperature of 60°C, and then granulated for 15 minutes while rotating the Clearmix at a peripheral speed of 33 m / s. The mixture was then transferred to a propeller-type agitator and stirred at 100 rpm while reacting at 70°C for 5 hours, then heated to 85°C and reacted for another 4 hours to produce magnetic toner particles. After the polymerization reaction was completed, the suspension was cooled to room temperature. After cooling, hydrochloric acid was added to lower the pH to 2.0 or less to dissolve the inorganic fine particles. After washing with water several times, the mixture was dried at 40°C for 72 hours using a dryer, and then classified using a multi-division classifier utilizing the Coanda effect to obtain toner particles 1. For the obtained toner particles 1 (100 parts by mass), 2 By externally adding 1.0 part of hydrophobic silica having a particle size of 1.0 μm / g using a Henschel mixer (Nippon Coke Engineering Co., Ltd. (formerly Mitsui Miike Chemical Engineering Co., Ltd.)), toner 1 having a weight average particle size (D4) of 7.1 μm was obtained. The physical properties of toner 1 are shown in Table 3 below.
[0121] <Production Examples of Toners 2 to 12 and Comparative Toners 1 to 4> Toners 2 to 12 and comparative toners 1 to 4 were produced in the same manner as toner 1, except for the magnetic material, crystalline material, amorphous thermoplastic resin, and 1,6-hexanediol diacrylate described in Tables 1 to 4. The physical properties of toners 2 to 12 and comparative toners 1 to 4 are shown in Table 3 below. For the production of toner 2, 20.0 parts by mass of crystalline material 1 and 5.0 parts by mass of crystalline material 6 were used. When toner 2 was analyzed, S2 was 2.5%. When the crystalline material detected as S2 was investigated, it was confirmed to be stearate behenate.
[0122] <Production Example of Toner 13> (Preparation of Resin Particle Dispersion) [Preparation of Resin Particle Dispersion (1)] Terephthalic acid: 30 parts by mole Fumaric acid: 70 parts by mole Bisphenol A ethylene oxide adduct: 5 mole parts Bisphenol A propylene oxide adduct: 95 moles The above materials were charged into a 5-liter flask equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 210°C over 1 hour, and 1 part of titanium tetraethoxide was added for 100 parts of the above materials. The temperature was raised to 230°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at that temperature for 1 hour, and then the reactant was cooled. In this way, polyester resin (1) with a weight average molecular weight of 18,500, an acid value of 14 mgKOH / g, and a glass transition temperature of 59°C was synthesized. Into a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of polyester resin (1) were gradually added and dissolved therein, and a 10% by mass aqueous ammonia solution (equivalent to 3 times the amount by molar ratio relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the container was replaced with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was dropped at a rate of 2 parts / min while stirring the mixture, to perform emulsification. After the dropwise addition was completed, the emulsion was returned to room temperature (20°C to 25°C), and dry nitrogen was bubbled for 48 hours while stirring to reduce ethyl acetate and 2-butanol to 1,000 ppm or less, and a resin particle dispersion in which resin particles having a volume average particle size of 200 nm were dispersed was obtained. Ion-exchanged water was added to the resin particle dispersion to adjust the solid content to 20 mass%, to obtain resin particle dispersion (1).
[0123] (Preparation of Resin Particle Dispersion (2)) Resin particle dispersion (2) was obtained in the same manner as in preparation of the above-mentioned resin particle dispersion 1, except that the amorphous thermoplastic resin 1 was used instead of the polyester resin.
[0124] (Preparation of Resin Particle Dispersion (3)) Resin particle dispersion (3) was obtained in the same manner as in preparation of the above-mentioned resin particle dispersion 1, except that the amorphous thermoplastic resin 6 was used instead of the polyester resin.
[0125] (Preparation of Colorant Particle Dispersion) [Preparation of Colorant Particle Dispersion (1)] Cyan pigment CI Pigment Blue 15:3 (copper phthalocyanine, manufactured by DIC Corporation, product name: FASTOGEN BLUE LA5380): 70 parts Anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 5 parts - Ion-exchanged water: 200 parts The above materials were mixed and dispersed for 10 minutes using a homogenizer (Ultra Turrax T50 manufactured by IKA Corporation). Ion-exchanged water was added so that the solid content in the dispersion was 20% by mass, and a colorant particle dispersion (1) in which colorant particles having a volume average particle size of 190 nm were dispersed was obtained.
[0126] (Preparation of Release Agent Particle Dispersion) [Preparation of Release Agent Particle Dispersion (1)] ·Crystalline material 1 100 parts Anionic surfactant (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 1 part 350 parts of ion-exchanged water The above materials were mixed and heated to 100°C, dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA), and then dispersed using a Manton-Gaulin high pressure homogenizer (manufactured by Gaulin) to obtain a release agent particle dispersion (solid content 20% by mass) (1) in which release agent particles having a volume average particle size of 200 nm were dispersed.
[0127] (Preparation of toner particles) [Preparation of toner particles (13)] An apparatus was prepared in which a round stainless steel flask and a container A were connected by a tube pump A, and the liquid contained in the container A was sent to the flask by driving the tube pump A, and the container A and a container B were connected by a tube pump B, and the liquid contained in the container B was sent to the container A by driving the tube pump B. Then, the following operations were carried out using this apparatus. ·Resin particle dispersion (1): 500 parts Colorant particle dispersion (1): 40 parts Anionic surfactant (TaycaPower): 2 parts The above materials were placed in a round stainless steel flask, and 0.1N nitric acid was added to adjust the pH to 3.5, after which 30 parts of an aqueous nitric acid solution with a polyaluminum chloride concentration of 10% by mass was added. The materials were then dispersed at 30°C using a homogenizer (IKA Ultra Turrax T50), and the particle size of the aggregated particles was allowed to grow while increasing the temperature in a heating oil bath at a rate of 1°C / 30 minutes. Meanwhile, 50 parts of the resin particle dispersion (3) was placed in the container A of a polyester bottle, and 25 parts of the release agent particle dispersion (1) was placed in the container B. Next, the liquid delivery speed of the tube pump A was set to 0.70 parts / min, and the liquid delivery speed of the tube pump B was set to 0.14 parts / min, and the tube pumps A and B were driven when the temperature in the round stainless steel flask during the formation of aggregated particles reached 37.0°C, and the delivery of each dispersion liquid was started. As a result, the mixed dispersion in which the resin particles and the release agent particles were dispersed was delivered from the container A to the round stainless steel flask during the formation of aggregated particles, while gradually increasing the concentration of the release agent particles. After the transfer of each dispersion liquid to the flask was completed and the temperature inside the flask reached 48° C., the flask was maintained at this temperature for 30 minutes to form secondary aggregated particles. Then, 50 parts of the resin particle dispersion (2) was slowly added and held for 1 hour, and a 0.1 N aqueous sodium hydroxide solution was added to adjust the pH to 8.5, and the mixture was heated to 85° C. with continued stirring and held for 5 hours. Then, the mixture was cooled to 20° C. at a rate of 20° C. / min. The dispersion liquid was filtered, thoroughly washed with ion-exchanged water, and dried to obtain toner particles 13 having a volume average particle size of 7.0 μm. The physical properties of the obtained toner particles 13 are shown in Table 3.
[0128] <Production Example of Comparative Toner 5> (Method of manufacturing untreated magnetic material) In the ferrous sulfate aqueous solution, 1.1 molar equivalents of caustic soda solution relative to iron element, SiO2 in an amount equivalent to 0.60 mass% of silicon element relative to iron element, and sodium phosphate in an amount equivalent to 0.15 mass% of phosphorus element relative to iron element were mixed. In this way, an aqueous solution containing ferrous hydroxide was prepared. Next, the pH of the aqueous solution was adjusted to 8.0, and an oxidation reaction was carried out at 85°C while blowing in air, to prepare a slurry liquid containing seed crystals. Next, an aqueous solution of ferrous sulfate was added to this slurry to obtain 1.0 molar equivalent to the initial amount of alkali (sodium component of caustic soda), and the pH of the slurry was maintained at 7.5, and the oxidation reaction was allowed to proceed while blowing in air, to obtain a slurry containing magnetic iron oxide. This slurry was filtered, washed, dried, and crushed to obtain untreated magnetic material with a number-average primary particle size (D1) of 0.21 μm.
[0129] [Preparation of silane compound] An aqueous solution was prepared by dropping 20 parts by mass of isobutyltrimethoxysilane into 80 parts by mass of ion-exchanged water while stirring. The pH of the aqueous solution was then adjusted to 5.5, and the solution was dispersed at 0.46 m / s for 2 hours using a dispersing blade while maintaining the temperature at 40° C., to carry out hydrolysis, thereby obtaining a silane compound that is an aqueous solution containing a hydrolyzate.
[0130] (Production of Hydrophobized Magnetic Material 6) The untreated magnetic material was placed in a Henschel mixer (manufactured by Nippon Coke Engineering Co., Ltd. (formerly Mitsui Miike Chemical Engineering Co., Ltd.)), and the untreated magnetic material was dispersed at a rotation speed of 34.5 m / s. The silane compound (3.8 parts by mass) was then added while being sprayed. The magnetic material was then left to disperse for 10 minutes, after which the magnetic material to which the silane compound had been adsorbed was taken out and left to stand quietly at 160°C for 2 hours to dry the treated magnetic material and to allow the condensation reaction of the silane compound to proceed. The magnetic material was then passed through a sieve with a mesh size of 100 μm to obtain hydrophobic magnetic material 6. The physical properties of the obtained hydrophobic magnetic material 6 are shown in Table 1.
[0131] (Production of Comparative Toner 5) 850 parts by mass of 0.1 mol / L-Na3PO4 aqueous solution was added to a vessel equipped with a high-speed stirring device Clearmix (manufactured by M Technique Co., Ltd.), and heated to 60°C while stirring at a rotation speed of 33 m / s. 68 parts by mass of 1.0 mol / L-CaCl2 aqueous solution was added to the vessel, preparing an aqueous medium containing a trace amount of poorly water-soluble dispersant Ca3(PO4)2. A solution was prepared by mixing and dissolving the following materials using a propeller-type stirrer. When mixing the following materials, the rotation speed of the stirrer was set to 100 r / min. Styrene 75.0 parts by weight n-Butyl acrylate 25.0 parts by weight Amorphous polyester-1 3.0 parts by weight Hydrophobic magnetic material 6 90.0 parts by weight Crystalline material 4 (crystalline polyester, condensation product of 1-9 nonanediol and sebacic acid, acid value 2.0 mg / KOH, weight average molecular weight Mw20400, melting point 74.0°, SP value 9.62) 8.0 parts by mass Monoazo dye iron complex (T-77: manufactured by Hodogaya Chemical Co., Ltd.) 1.0 part by weight ·Crystalline material 6 15.0 parts by mass The mixture was then heated to 60°C and stirred in a TK homomixer (manufactured by Primix Corporation (formerly Tokushu Kika Kogyo Co., Ltd.)) with the agitator rotation speed set to 9000 r / min to dissolve and disperse the solids. 10.0 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) as a polymerization initiator was added to the mixture and dissolved in the mixture to prepare a polymerizable monomer composition. Next, the polymerizable monomer composition was added to the aqueous medium and heated to a temperature of 60°C, and then granulated for 15 minutes while rotating the Clearmix at a peripheral speed of 33 m / s. After that, the mixture was transferred to a propeller-type agitator and stirred at 100 rpm while reacting at 70°C for 5 hours, then heated to 85°C and reacted for another 4 hours to produce magnetic toner particles. After the polymerization reaction was completed, the suspension was heated to 100°C and held for 2 hours, and the residual monomer was removed under reduced pressure. Next, as a cooling step, ice was added to the suspension, and the suspension was cooled from 100°C to 20°C in 2 minutes. After cooling, hydrochloric acid was added to reduce the pH to 2.0 or less to dissolve the inorganic fine particles. After repeated washing with water, the mixture was dried at 40°C for 72 hours using a dryer, and then classified using a multi-division classifier utilizing the Coanda effect to obtain comparative toner particles 5.
[0132] The obtained comparative toner particles 5 (100 parts by mass) were subjected to a test to determine whether the specific surface area by the BET method was 200 m 2 Comparative toner 5 having a weight average particle size (D4) of 8.1 μm was obtained by externally adding 1.0 part of hydrophobic silica having a molecular weight of 1.0 μm / g using a Henschel mixer (manufactured by Nippon Coke Engineering Co., Ltd. (formerly Mitsui Miike Chemical Engineering Co., Ltd.)). The physical properties of comparative toner 5 are shown in Table 3 below. The S2 of the obtained toner was 0.2%. The crystalline material detected in S2 was confirmed to be dibehenyl sebacate.
[0133] <Production Example of Comparative Toner 6> (Preparation of aqueous medium) Ion-exchanged water: 400.0 parts Trisodium phosphate: 7.0 parts The mixture was stirred at 15,000 rpm with a high-speed stirring device Clearmix (manufactured by M Technique Co., Ltd.) and maintained at 60° C. Next, 4.1 parts of calcium chloride was added to prepare an aqueous medium containing an inorganic dispersion stabilizer.
[0134] (Preparation of Polymerizable Monomer Composition 1) Styrene: 40.0 parts Copper phthalocyanine pigment (Pigment Blue 15:3): 6.5 parts Charge control agent LR-147 (manufactured by Nippon Carlit Co., Ltd.): 0.3 parts The above materials were mixed and stirred with zirconia beads (3 / 16 inch) in an attritor (Mitsui Mining Co., Ltd.) at 200 rpm for 4 hours, and the beads were separated to prepare a pigment dispersion (pigment dispersion step).
[0135] (Preparation of Polymerizable Monomer Composition 2) Styrene: 35.0 parts n-Butyl acrylate: 25.0 parts Amorphous resin 8:4.0 parts The above materials were mixed and stirred for 2 hours to dissolve the amorphous resin 8, thereby obtaining a polymerizable monomer composition 2.
[0136] (Preparation of Polymerizable Monomer Composition 3: Dissolution Step) After the polymerizable monomer compositions 1 and 2 were mixed, the following materials were added. Fischer-Tropsch wax: 10.0 parts (Melting point 78℃) Divinylbenzene: 0.02 parts After the addition, the mixture was heated to 60° C. and stirred for 10 minutes to obtain a polymerizable monomer composition 3.
[0137] (granulation / polymerization process) The obtained polymerizable monomer composition 3 was put into the above aqueous medium. Then, 10.0 parts of t-butyl peroxypivalate (25% toluene solution) was added, and the stirring speed was maintained at 15,000 rpm while granulating for 10 minutes. After that, the stirring speed was changed from the high-speed stirring speed to a propeller stirring blade, the internal temperature was raised to 70°C, and the reaction was carried out for 5 hours while slowly stirring. Next, the temperature inside the vessel was raised to 85°C, and the polymerization reaction was carried out for another 4 hours.
[0138] (Distillation / Washing / Drying / Classification / External Addition Process) After the polymerization reaction was completed, toluene and residual monomers were removed by distillation under reduced pressure with heating, and then the mixture was cooled and hydrochloric acid was added to lower the pH to 2.0 or less to dissolve the inorganic dispersion stabilizer. The mixture was then filtered and washed with water, and then dried at 40°C for 72 hours using a dryer. The resulting dried product was simultaneously classified and removed to remove fine and coarse powders using an elbow jet classifier (manufactured by Nittetsu Mining Co., Ltd.) to obtain comparative cyan toner particles 6. For 100.0 parts of comparative toner particles 6, a BET specific surface area of 200 m 2 1.0 part of hydrophobic silica having a BET specific surface area of 100 m 2 0.3 parts of titanium oxide having a molecular weight of 1.01g / g was added for 300 seconds in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.) to obtain Comparative Toner 6. The physical properties of Comparative Toner 6 obtained are shown in Table 3. The S2 of the obtained toner was 0.2%. The crystalline material detected in S2 was confirmed to be Fischer-Tropsch wax.
[0139] <Production Example of Comparative Toner 7> Comparative toner 7 was produced in the same manner as comparative toner 6, except that the amorphous thermoplastic resin was changed as shown in Table 3. The physical properties of the obtained comparative toner 7 are shown in Table 3. The S2 of the obtained toner was 0.2%. The crystalline material detected in S2 was confirmed to be Fischer-Tropsch wax.
[0140] <Production Example of Comparative Toner 8> (Production of magnetic iron oxide) Fe 2+ 50 L of an aqueous solution of ferrous sulfate containing 2.0 mol / L was mixed with 55 L of an aqueous solution of sodium hydroxide containing 4.0 mol / L, and stirred to obtain an aqueous solution of ferrous salt containing ferrous hydroxide colloid. This aqueous solution was kept at 85°C and an oxidation reaction was carried out while blowing in air at 20 L / min, to obtain a slurry containing core particles. The obtained slurry was filtered and washed with a filter press, and the core particles were dispersed again in water to reslurry. Sodium silicate was added to this reslurry liquid in an amount equivalent to 0.20% by mass of silicon per 100 parts by mass of core particles, the pH of the slurry liquid was adjusted to 6.0, and the mixture was stirred to obtain magnetic iron oxide particles with a silicon-rich surface. The obtained slurry was filtered and washed with a filter press, and further reslurried with ion-exchanged water. 500g (10% by mass relative to the magnetic iron oxide) of ion-exchange resin SK110 (manufactured by Mitsubishi Chemical) was added to this reslurry liquid (solid content 50g / L) and stirred for 2 hours to perform ion exchange. Thereafter, the ion-exchange resin was removed by filtration with a mesh, filtered and washed with a filter press, dried and crushed to obtain magnetic iron oxide with a number average diameter of 0.23 μm.
[0141] (Production of silane compounds) 30 parts by mass of iso-butyltrimethoxysilane was dropped into 70 parts by mass of ion-exchanged water while stirring. Then, this aqueous solution was kept at pH 5.5 and temperature 55°C, and dispersed for 120 minutes at a peripheral speed of 0.46 m / s using a dispersing blade to perform hydrolysis. Then, the pH of the aqueous solution was adjusted to 7.0, and the solution was cooled to 10°C to stop the hydrolysis reaction. Thus, an aqueous solution containing a silane compound was obtained.
[0142] (Manufacture of magnetic body 7) 100 parts by mass of magnetic iron oxide was placed in a high-speed mixer (LFS-2 model manufactured by Fukae Powtec Co., Ltd.), and while stirring at a rotation speed of 2000 rpm, 8.0 parts by mass of an aqueous solution containing a silane compound was added dropwise over a period of 2 minutes. The mixture was then mixed and stirred for 5 minutes. Next, in order to increase the adhesion of the silane compound, it was dried at 40°C for 1 hour to reduce the moisture, and then the mixture was dried at 110°C for 3 hours to allow the condensation reaction of the silane compound to proceed. The mixture was then crushed and passed through a sieve with 100 μm openings to obtain magnetic material 7.
[0143] (Production of amorphous polyester resin) In a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, 40 mol% terephthalic acid, 10 mol% trimellitic acid and 50 mol% bisphenol A-PO 2 mol adduct were put, and then 1.5 parts by mass of dibutyltin was added as a catalyst to 100 parts by mass of the total amount of monomers. Next, the temperature was quickly raised to 180°C under normal pressure in a nitrogen atmosphere, and then water was distilled off while heating from 180°C to 210°C at a rate of 10°C / hour to carry out polycondensation. After reaching 210°C, the pressure in the reaction vessel was reduced to 5 kPa or less, and polycondensation was carried out under conditions of 210°C and 5 kPa or less to obtain an amorphous polyester resin. At that time, the polymerization time was adjusted so that the softening point of the obtained polyester resin was 120°C.
[0144] (Production of crystalline polyester) In a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, 49 mol% of 1,9-nonanediol, 49 mol% of 1,10-decanedioic acid and 2 mol% of n-octadecanoic acid were added, and 1 part by mass of tin dioctylate was added as a catalyst for 100 parts by mass of the total amount of monomers. The mixture was heated to 140°C under a nitrogen atmosphere and reacted for 6 hours while distilling off water under normal pressure. The mixture was then reacted while increasing the temperature to 200°C at a rate of 10°C / hour, and reacted for 2 hours after reaching 200°C. The pressure in the reaction vessel was reduced to 5 kPa or less, and the mixture was reacted at 200°C for 3 hours to obtain a crystalline polyester. The acid value of the crystalline polyester was 2.2, the molecular weight (Mw) was 34200, and the SP value SPa was 11.47.
[0145] <Production Example of Comparative Toner 8> (Preparation of First Aqueous Medium) 2.9 parts by mass of sodium phosphate 12-hydrate was added to 353.8 parts by mass of ion-exchanged water and heated to 60°C while stirring using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.). After that, an aqueous calcium chloride solution prepared by adding 1.7 parts by mass of calcium chloride dihydrate to 11.7 parts by mass of ion-exchanged water and an aqueous magnesium chloride solution prepared by adding 0.5 parts by mass of magnesium chloride to 15.0 parts by mass of ion-exchanged water were added and stirring was continued to obtain a first aqueous medium containing dispersion stabilizer A.
[0146] (Preparation of Polymerizable Monomer Composition) Styrene 75.0 parts by weight n-Butyl acrylate 25.0 parts by weight 1,6-Hexanediol diacrylate 0.5 parts by weight ·Magnetic material 95.0 parts by mass Amorphous polyester resin 5.0 parts by weight The above materials were uniformly dispersed and mixed using an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then heated to 60°C. 15.0 parts by mass of stearate behenate (behenyl stearate wax (melting point 68°C)) as an ester wax and 8.0 parts by mass of paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd.) as a hydrocarbon wax were added, mixed, and dissolved to obtain a polymerizable monomer composition.
[0147] (Preparation of second aqueous medium) 0.6 parts by mass of sodium phosphate 12-hydrate was added to 166.8 parts by mass of ion-exchanged water and heated to 60°C while stirring using a paddle stirring blade. After that, an aqueous calcium chloride solution prepared by adding 0.3 parts by mass of calcium chloride dihydrate to 2.3 parts by mass of ion-exchanged water was added and stirring was continued to obtain a second aqueous medium containing dispersion stabilizer B.
[0148] (granulation) The above polymerizable monomer composition was added to the first aqueous medium, and the granulation liquid was treated with a Cavitron (manufactured by Eurotech) at a rotor speed of 29 m / s for 1 hour to uniformly disperse and mix. Further, 7.0 parts by mass of t-butyl peroxypivalate was added as a polymerization initiator, and the mixture was granulated at 60°C under a N2 atmosphere with a Clearmix (manufactured by M Technique) at a peripheral speed of 22 m / s for 10 minutes, to obtain a granulation liquid containing droplets of the polymerizable monomer composition.
[0149] (Polymerization / Distillation / Drying / External Addition) The granulation liquid was added to the second aqueous medium, and the mixture was reacted at 74°C for 3 hours while stirring with a paddle impeller. After the reaction was completed, the mixture was heated to 98°C and distilled for 3 hours to obtain a reaction slurry. Thereafter, in a cooling step, 0°C water was added to the reaction slurry, and the reaction slurry was cooled from 98°C to 45°C at a rate of 100°C / min, and then further heated and held at 50°C for 3 hours. The mixture was then allowed to cool to 25°C at room temperature. The cooled reaction slurry was washed with hydrochloric acid, filtered, and dried to obtain comparative toner particles 8 having a weight average particle size of 7.4 μm.
[0150] The following materials were mixed with 100 parts by mass of the obtained comparative toner particles 8 in a Henschel mixer (FM-10 model, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain comparative toner 8. The physical properties of the obtained comparative toner 8 are shown in Table 3. The S2 of the obtained toner was confirmed to be 0.2%. The crystalline material detected in S2 was confirmed to be paraffin wax.
[0151] [Table 3]
[0152] [Table 4]
[0153] <Example 1> (Evaluation of low temperature fixability) Toner 1 was used to carry out the following evaluations. The evaluation was carried out in an environment of 23°C and 50% RH. The fixing media was FOX RIVER BOND paper (110 g / m 2) was used. By using thick media with a relatively large surface irregularity, the white spots described below are more likely to occur, allowing for a strict evaluation of low-temperature fixability. The image forming device used was a commercially available LBP-3100 (Canon), modified to increase the print speed from 16 pages per minute to 40 pages per minute. In addition, the size of the fixer was reduced so that the time the media was in contact with the fixer as it passed through it was reduced from 150 ms to 50 ms. While these conditions allow for both high-speed printing and a more compact fixer, they result in a very strict evaluation of the fixability of the toner. With the fixing unit cooled to room temperature (25°C), 100 sheets of solid black were printed continuously, and the average number of blanks in the solid black images from 95 to 100 sheets was measured. By continuously printing solid black, the heat of the fixing unit is taken by the media, resulting in a state in which sufficient heat is not retained, which results in a strict evaluation of the low-temperature fixing ability of the toner. If the fixing ability of the toner is insufficient, a so-called blank image in which the unfixed toner is blanked out is output. The evaluation result is judged based on the number of blanks. In this case, the average number of blanks that occurred is visually observed using a microscope that can be magnified 10 times or more. The smaller the number, the better the low-temperature fixing ability of the toner. In this evaluation, the fixing performance was evaluated based on the temperature of the fixing unit at which the number of blanks was less than 10. The lower this temperature, the better the low-temperature fixing ability of the toner.
[0154] (Evaluation of contamination of transport components) Toner 1 was used to carry out the following evaluations. The evaluation was carried out in an environment of 23°C and 50% RH. The fixing media was Canon A4 size Oce Red Label paper (grammage 80 g / m 2 ) was used. A commercially available LBP-3100 (Canon) was used as the image forming device, and the printing speed was modified from 16 pages per minute to 40 pages per minute. In addition, the size of the fixing unit was reduced so that the time that the media was in contact with the fixing unit as it passed through it was reduced from 150 ms to 50 ms. The temperature of the fixing unit was set to the temperature obtained in the evaluation of low-temperature fixing properties, and 2,000 halftone images with a print rate of 10% were printed continuously. If toner adheres to the conveying member, vertical stripes will appear in the printed solid white image. The solid white image was observed under a microscope and the width of the vertical stripes was measured. The narrower the width of the vertical stripes, the better the soiling of the conveying member.
[0155] (Durability rating) Toner 1 was used to carry out the following evaluations. The evaluation was carried out in an environment of 23°C and 50% RH. The fixing media was Canon A4 size Oce Red Label paper (grammage 80 g / m 2 ) was used. A commercially available LBP-3100 (Canon) was used as the image forming device, and the printing speed was modified from 16 pages per minute to 40 pages per minute. In addition, the size of the fixing unit was reduced so that the time that the media was in contact with the fixing unit as it passed through it was reduced from 150 ms to 50 ms. The temperature of the fixing unit was set to the temperature obtained in the evaluation of low-temperature fixing property, and 2000 sheets of horizontal line images with a printing rate of 5% were printed in intermittent mode. The density of the solid image before and after durability was measured using a Macbeth densitometer (manufactured by Macbeth Co., Ltd.). The higher the density, the better the durability.
[0156] <Examples 2 to 13 and Comparative Examples 1 to 8> Image output tests were performed in the same manner as in Example 1, except that toner 1 in Example 1 was changed to toners 2 to 13 and comparative toners 1 to 8. In Example 13, Comparative Example 6, and Comparative Example 7, the image forming apparatus was modified so that it could output non-magnetic toners, and then evaluation was performed. The results of these evaluations are shown in Table 5.
[0157] [Table 5] [Explanation of symbols]
[0158] 100: Electrostatic latent image carrier (photoconductor) 102: Toner carrier 103: Development blade 114: Transfer member (transfer charging roller) 116: Cleaner container 117: Charging member (charging roller) 121: Laser generating device (latent image forming means, exposure device) 123: Laser 124: Pickup roller 125: Conveyor belt 126: Fixing unit 140: Developer 141: Stirring member 301:Shell 302: Crystalline material 303: Core 304: Area detected as S2
Claims
1. A toner containing toner particles having a core-shell structure consisting of a core containing a binder resin and a colorant, and a shell, The colorant is a hydrophobic magnetic material whose surface has been hydrophobized with a silane coupling agent, the hydrophobized magnetic material has a spectrum of Si obtained by using near edge X-ray absorption fine structure (NEXAFS) and based on a total electron yield method (TEY), the spectrum having a peak A in the range of 1844.4 eV to 1844.8 eV and a peak B in the range of 1846.1 eV to 1846.6 eV, the area of peak A being I A , the area of peak B being I B , and the number of moles of Si derived from the silane compound contained per gram of the hydrophobized magnetic material being M Si , the ratio I A / (I A +I B ) / M Si satisfies 40 to 55, The toner comprises a crystalline material, the shell contains an amorphous thermoplastic resin, The SP value of the crystalline material calculated by the Fedors method is SPc (J / cm 3 ) 0.5 The SP value of the amorphous thermoplastic resin calculated by the Fedors method is SPa (J / cm 3 ) 0.5 When SPc and SPa satisfy the following formula (1), The toner was mixed with RuO 4 A toner characterized in that, when the ratio of an area occupied by the crystalline material per area of a toner observed with a scanning electron microscope (SEM) is defined as S2 (%), the ratio satisfies the following formula (2): 2.50≦SPa-SPc≦4.50 Formula (1) 1.0≦S2≦20.0 Formula (2)
2. The viscosity of the toner at 100° C. measured by a flow tester temperature rise method is 0.5×10 4 Pa・s or more 9.0×10 5 2. The toner according to claim 1, having a viscosity of not more than Pa·s.
3. The SPa is 11.60 (J / cm 3 ) 0.5 12.40 (J / cm 3 ) 0.5 3. The toner according to claim 1, wherein:
4. 4. The toner according to claim 1, wherein the amorphous thermoplastic resin is an amorphous polyester.
5. The toner according to claim 4, wherein the amorphous polyester has an isosorbide unit represented by formula (3). 【Chemistry 1】
6. 6. The toner according to claim 5, wherein the amorphous polyester is a condensate of at least one alcohol component selected from the group consisting of dihydric and trihydric or higher alcohols, and at least one carboxylic acid component selected from the group consisting of aromatic polycarboxylic acids, aliphatic polycarboxylic acids, and anhydrides thereof, the alcohol component contains at least isosorbide, the alcohol component and the carboxylic acid component do not have an ester group, and the amorphous polyester contains isosorbide units represented by formula (3) derived from the isosorbide in an amount of 0.10 mol % to 30.00 mol % based on all of the monomer units derived from the alcohol component and the monomer units derived from the carboxylic acid component.
Citation Information
Patent Citations
Toner, image forming method, image forming apparatus and developing device
JP2009063969A
Toner, manufacturing method of toner, developer using toner, and process cartridge
JP2015059949A
Magnetic toner and method of manufacturing magnetic toner
JP2017040845A
Toner and method for producing toner
JP2017044952A
Magnetic toner
JP2020034714A