Unit and image forming apparatus
The use of surfactants and a modified intermediate transfer belt with reduced adhesion force addresses the issue of flat toner transfer failures, enhancing transfer efficiency and image quality in image forming devices.
Patent Information
- Application Number
- JP2021015150
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-02
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-02-02
AI Technical Summary
The use of flat glitter toners in image forming devices can lead to transfer failures due to increased adhesion to the intermediate transfer belt, resulting in defective toner images when high blowing pressures are applied.
A developing device using flat toners with specific surfactants and a modified intermediate transfer belt surface with reduced non-electrostatic adhesion force, allowing toner separation at lower pressures, and incorporating a surfactant with a perfluoroalkyl or silicone structure to enhance transferability.
The solution effectively suppresses defective toner image transfer by ensuring complete separation of flat toners from the belt surface at lower pressures, improving transfer performance even on textured papers.
Smart Images

Figure 0007563206000003 
Figure 0007563206000004 
Figure 0007563206000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a unit and an image forming apparatus. [Background technology]
[0002] In an image forming apparatus (such as a copier, a facsimile, or a printer) using an electrophotographic method, a toner image formed on the surface of an image carrier is transferred to the surface of a recording medium and fixed on the recording medium to form an image.
[0003] In recent years, the use of glittering toners containing glittering pigments has been investigated for the purpose of forming images having a metallic luster.
[0004] For example, Patent Document 1 discloses a "glossy toner comprising a glittering pigment, an organic pigment, a binder resin, a release agent and an external additive, in which the toluene-insoluble matter other than the glittering pigment and the external additives is 8% by mass or more and 40% by mass or less." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-062413 A Summary of the Invention [Problem to be solved by the invention]
[0006] Since the glitter pigment is a flat pigment, the toner also has a flat shape. In a transfer device using an intermediate transfer belt, when a toner image made of a flat toner containing a flat pigment is transferred onto a recording medium by the intermediate transfer belt, transfer defects may occur.
[0007] Therefore, the object of the present invention is to provide a unit that contains resin and conductive carbon particles, and when flat toner is adhered to the outer peripheral surface and then air is blown onto the outer peripheral surface from above while increasing the blowing pressure, in which case poor transfer of the toner image caused by flat toner is suppressed compared to a case in which an intermediate transfer belt is provided in which all of the flat toner adhered to the outer peripheral surface remains on the outer peripheral surface even when the blowing pressure exceeds 25 kPa. [Means for solving the problem]
[0008] Means for solving the above problems include the following aspects. <1> a developing device that contains a developer having a flat toner containing a flat pigment and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the developer; a transfer device which comprises an intermediate transfer belt onto which a toner image formed on the surface of said image carrier is primarily transferred, a primary transfer device which performs primary transfer of the toner image formed on the surface of said image carrier onto the surface of said intermediate transfer belt, and a secondary transfer device which performs secondary transfer of the toner image on the surface of said intermediate transfer belt onto a surface of a recording medium, said intermediate transfer belt containing resin and conductive carbon particles, and a transfer device which, after the flat toner is adhered to the outer peripheral surface of said intermediate transfer belt, blows air onto said outer peripheral surface from above said outer peripheral surface while increasing the blowing pressure, and all of said flat toner adhered to said outer peripheral surface is separated from said outer peripheral surface within said blowing pressure of 25 kPa or less; A unit equipped with. <2> After the flat toner is adhered to the outer peripheral surface of the intermediate transfer belt, when air is blown onto the outer peripheral surface from above the outer peripheral surface while increasing the blowing pressure, all of the flat toner adhered to the outer peripheral surface is separated from the outer peripheral surface when the blowing pressure is 2 kPa or more. <1> The unit described in. <3> The intermediate transfer belt further contains a surfactant. <1> or <2> The unit described in. <4> The surfactant is at least one of an oligomer having a substituent with 6 or less carbon atoms and a fluorine atom, and an oligomer having a silicone structure with a methyl group. <3> The unit described in. <5> The oligomer having a carbon number of 6 or less and a substituent having a fluorine atom is an oligomer having a perfluoroalkyl structure having a carbon number of 6 or less. <4> The unit described in. <6> The number of repeating units of the monomer in the oligomer is 4 or more. <4> or <5> The unit described in. <7> The surface free energy of the outer peripheral surface of the intermediate transfer belt is 47 mN / m or less. <1> ~ <6> 13. A unit according to any one of claims 1 to 12. <8> The water contact angle of the outer peripheral surface of the intermediate transfer belt is 85° or more. <7> The unit described in. <9> An image carrier; <1> ~~ <8> a toner image forming device having the developing device among the units described in any one of claims 1 to 5 and forming a toner image on a surface of the image carrier; A transfer device that transfers the toner image formed on the surface of the image carrier to a surface of a recording medium, <1> ~~ <8> The transfer device of the unit according to any one of claims 1 to 5, An image forming apparatus comprising: Effect of the Invention
[0009] <1> According to the invention, a unit is provided which contains a resin and conductive carbon particles, and when flat toner is adhered to the outer peripheral surface and then air is blown onto the outer peripheral surface from above while increasing the blowing pressure, even when the blowing pressure exceeds 25 kPa, poor transfer of the toner image caused by flat toner is suppressed compared to a case in which an intermediate transfer belt is provided in which all of the flat toner adhered to the outer peripheral surface remains on the outer peripheral surface. <2> According to the invention, a unit is provided in which, when flat toner is adhered to the outer peripheral surface of an intermediate transfer belt and then air is blown onto the outer peripheral surface from above the outer peripheral surface while increasing the blowing pressure, poor transfer of the toner image caused by flat toner is suppressed compared to a case in which the blowing pressure is less than 2 kPa and all of the flat toner adhered to the outer peripheral surface is separated from the outer peripheral surface.
[0010] <3> According to the present invention, a unit is provided in which transfer defects of a toner image caused by flat toner are suppressed, as compared with a case in which the intermediate transfer belt does not contain a surfactant.
[0011] <4> , <5> or <6> According to the invention, an endless belt is provided which is excellent in transferability to textured paper, as compared with a case in which the surfactant has a monomer structure.
[0012] <7> According to the present invention, an endless belt is provided which is superior in transferability to textured paper, as compared with an intermediate transfer belt having a surface free energy of more than 47 mN / m on the outer peripheral surface. <8> According to the invention, an endless belt is provided which is superior in transferability to textured paper, as compared with an intermediate transfer belt having a water contact angle of more than 85° on its outer peripheral surface.
[0013] <9> According to the invention, an image forming device is provided in which when flat toner is adhered to the outer peripheral surface and then air is blown onto the outer peripheral surface from above while increasing the blowing pressure, even when the blowing pressure exceeds 25 kPa, poor transfer of the toner image caused by flat toner is suppressed compared to when a unit is applied that includes an intermediate transfer belt in which all of the flat toner adhered to the outer peripheral surface remains on the outer peripheral surface. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating an example of a flat toner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the present embodiment, which is an example of the present invention, will be described. These descriptions and examples are merely illustrative of the embodiment, and do not limit the scope of the present invention.
[0016] In the numerical ranges described in the present embodiment, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in the present embodiment. In addition, in the numerical ranges described in the present embodiment, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In this embodiment, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. When the embodiment is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this. In this embodiment, each component may contain multiple types of corresponding substances. When referring to the amount of each component in the composition in this embodiment, if multiple types of substances corresponding to each component are present in the composition, the amount refers to the total amount of the multiple types of substances present in the composition, unless otherwise specified.
[0017] [unit] The unit according to this embodiment includes a developing device that contains a developer having a flat toner including a flat pigment and develops an electrostatic charge image formed on the surface of an image holder into a toner image using the image developer, an intermediate transfer belt onto which the toner image formed on the surface of the image holder is primarily transferred, a primary transfer device that primarily transfers the toner image formed on the surface of the image holder onto the surface of the intermediate transfer belt, and a transfer device having a secondary transfer device that secondarily transfers the toner image on the surface of the intermediate transfer belt onto the surface of a recording medium. The intermediate transfer belt used includes a resin and conductive carbon particles, and after flat toner is adhered to its outer peripheral surface, when air is blown onto the outer peripheral surface from above the outer peripheral surface while increasing the blowing pressure, all of the flat toner adhered to the outer peripheral surface separates from the outer peripheral surface when the blowing pressure is within 25 kPa.
[0018] Hereinafter, the "property that flat toner adhering to the outer peripheral surface of the endless belt separates from the outer peripheral surface when the spray pressure is within 25 kPa" is also referred to as the "adhesion force property".
[0019] The unit according to the present embodiment has the above-described configuration, which suppresses transfer defects of a toner image caused by flat toner particles. Although the reason for this is not clear, it is presumed to be as follows.
[0020] In an image forming apparatus using an intermediate transfer belt, when flat toner is used as the toner, transfer failure of the toner image may occur when the toner image is transferred from the intermediate transfer belt to a recording medium. This is because flat toner has a larger contact area with the outer circumferential surface of the intermediate transfer belt than normal spherical toner, and the adhesive force is increased.
[0021] In contrast, in the unit according to the present embodiment, an endless belt with satisfactory adhesive properties is used as the intermediate transfer belt. In other words, an endless belt with reduced non-electrostatic adhesive force on the outer circumferential surface itself is used as the intermediate transfer belt. This reduces the non-electrostatic adhesive force generated between the outer circumferential surface of the intermediate transfer belt and the flat toner. Therefore, the transferability is improved even for toner images made of flat toner.
[0022] As described above, in the unit according to this embodiment, transfer defects of a toner image caused by flat toner are suppressed.
[0023] [Image forming device] An image forming apparatus including a unit according to this embodiment will be described below.
[0024] The image forming apparatus according to this embodiment includes a toner image forming device having an image carrier and a developing device among the units according to this embodiment, which forms a toner image on the surface of the image carrier, and a transfer device which transfers the toner image formed on the surface of the image carrier to the surface of a recording medium, which is also a transfer device among the units according to this embodiment.
[0025] An example of a toner image forming device is a device that includes an image carrier, a charging device that charges the surface of the image carrier, an electrostatic image forming device that forms an electrostatic image on the surface of the charged image carrier, and a developing device that develops the electrostatic image formed on the surface of the image carrier using a developer containing flat toner to form a toner image.
[0026] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as an apparatus equipped with a fixing device that fixes a toner image transferred onto the surface of a recording medium; an apparatus equipped with a cleaning device that cleans the surface of an image holder before charging after the toner image is transferred; an apparatus equipped with a static elimination device that irradiates the surface of an image holder with static elimination light before charging after the toner image is transferred; and an apparatus equipped with an image holder heating member that increases the temperature of the image holder and reduces the relative temperature.
[0027] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted. In the following description, the flat toner will be referred to as "silver toner."
[0028] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted. In the following description, the glitter toner will be referred to as "silver toner."
[0029] FIG. 1 is a schematic diagram showing an example of an image forming apparatus according to the present embodiment, and shows a five-unit tandem type and intermediate transfer type image forming apparatus. Figure 1 The image forming apparatus shown in FIG. 1 includes first to fifth electrophotographic image forming units 150Y, 150M, 150C, 150K, and 150B (an example of a toner image forming apparatus) that output images of each color, yellow (Y), magenta (M), cyan (C), black (K), and silver (B), based on color-separated image data. These image forming units 150Y, 150M, 150C, 150K, and 150B are arranged in parallel at a predetermined distance from each other in the horizontal direction. These image forming units 150Y, 150M, 150C, 150K, and 150B may be process cartridges that are detachably attached to the image forming apparatus.
[0030] An intermediate transfer belt 133 is provided below each of the image forming units 150Y, 150M, 150C, 150K, and 150B, and extends through each unit. The intermediate transfer belt 133 is provided by being wound around a driving roll 113, a support roll 112, and an opposing roll 114, which are in contact with the inner surface of the intermediate transfer belt 133, and runs in a direction from the first image forming unit 150Y to the fifth image forming unit 150B (in the direction of the arrow B in FIG. 1). An intermediate transfer belt cleaning device 116 is provided on the image carrying surface side of the intermediate transfer belt 133, facing the driving roll 113. In addition, a voltage application device 160 is provided on the upstream side of the intermediate transfer belt cleaning device 116 in the rotation direction of the intermediate transfer belt 133, which generates an electric field between the intermediate transfer belt 133 and the support roll 113 by generating a potential difference between the intermediate transfer belt 133 and the intermediate transfer belt cleaning device 116. The developing devices (examples of developing devices) 120Y, 120M, 120C, 120K, and 120B of each image forming unit 150Y, 150M, 150C, 150K, and 150B are supplied with yellow, magenta, cyan, black, and silver toner contained in toner cartridges 140Y, 140M, 140C, 140K, and 140B, respectively.
[0031] Since the first to fifth image forming units 150Y, 150M, 150C, 150K, and 150B have the same configuration, operation, and function, the first image forming unit 150Y that forms a yellow image and is arranged upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example.
[0032] The first image forming unit 150Y has a photoconductor 111Y that acts as an image carrier. Around the photoconductor 111Y, a charging roll (an example of a charging device) 118Y that charges the surface of the photoconductor 111Y to a predetermined potential, an exposure device (an example of an electrostatic image forming device) 119Y that exposes the charged surface to a laser beam based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing device) 120Y that supplies toner to the electrostatic image to develop it, a primary transfer roll (an example of a primary transfer device) 117Y that transfers the developed toner image onto the intermediate transfer belt 133, and a photoconductor cleaning device (an example of a cleaning device) 115Y that removes toner remaining on the surface of the photoconductor 111Y after the primary transfer are arranged in this order. The primary transfer roll 117Y is disposed inside the intermediate transfer belt 133, and is provided at a position facing the photoconductor 111Y. A bias power supply (not shown) that applies a primary transfer bias is connected to the primary transfer rolls 117Y, 117M, 117C, 117K, and 117B of each image forming unit. Each bias power supply changes the value of the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).
[0033] Hereinafter, the operation of forming a yellow image in first image forming unit 150Y will be described. First, prior to operation, the surface of the photoconductor 111Y is charged to a potential of −600V to −800V by the charging roll 118Y. The photoconductor 111Y has a conductivity (for example, a volume resistivity of 1×10 at 20° C. -6The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam, the resistivity of the portion irradiated with the laser beam changes. Therefore, a laser beam is irradiated from an exposure device 119Y onto the charged surface of the photosensitive member 111Y in accordance with image data for yellow sent from a control unit (not shown). As a result, an electrostatic charge image of a yellow image pattern is formed on the surface of the photosensitive member 111Y.
[0034] An electrostatic image is an image formed on the surface of the photoconductor 111Y by electrostatic charging. The laser beam from the exposure device 119Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 111Y to flow, while the charges remain in the parts not irradiated by the laser beam. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 111Y rotates to a predetermined developing position as the photoconductor 111Y travels. At this developing position, the electrostatic image on the photoconductor 111Y is developed into a toner image by the developing device 120Y and made visible.
[0035] The developing device 120Y contains a developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 120Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 111Y. As the surface of the photoconductor 111Y passes through the developing device 120Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 111Y, and the latent image is developed with the yellow toner. The photoconductor 111Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 111Y is transported to a predetermined primary transfer position.
[0036] When the yellow toner image on the photoconductor 111Y is transported to the primary transfer position, a primary transfer bias is applied to the primary transfer roll 117Y, and an electrostatic force from the photoconductor 111Y toward the primary transfer roll 117Y acts on the toner image, and the toner image on the photoconductor 111Y is transferred onto the intermediate transfer belt 133. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and is controlled to, for example, +10 μA by a control unit (not shown) in the first image forming unit 150Y. On the other hand, the toner remaining on the photoconductor 111Y is removed and collected by the photoconductor cleaning device 115Y.
[0037] The primary transfer bias applied to the primary transfer rolls 117M, 117C, 117K, and 117B subsequent to the second image forming unit 150M is also controlled in accordance with the first image forming unit 150Y. In this manner, the intermediate transfer belt 133 onto which the yellow toner image has been transferred by the first image forming unit 150Y is transported successively through the second to fifth image forming units 150M, 150C, 150K, and 150B, where the toner images of each color are superimposed and multi-transferred.
[0038] The intermediate transfer belt 133 onto which the five color toner images are transferred in multiple layers through the first to fifth image forming units reaches a secondary transfer section that is composed of the intermediate transfer belt 133, the opposing roll 114 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer device) 134 arranged on the image carrying surface side of the intermediate transfer belt 133. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 134 and the intermediate transfer belt 133 via a supply mechanism, and a secondary transfer bias is applied to the opposing roll 114. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 133 toward the recording paper P acts on the toner image, and the toner image on the intermediate transfer belt 133 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection device (not shown) that detects the resistance of the secondary transfer section, and is voltage controlled.
[0039] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing device) 135, where the toner image is fixed onto the recording paper P, forming a fixed image.
[0040] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets and the like. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with a resin or the like, art paper for printing, etc. are preferably used.
[0041] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.
[0042] Here, the developing device 120B of the image forming unit 150B corresponds to an example of the developing device in the unit according to the present embodiment. The device including the intermediate transfer belt 133, the primary transfer roll 117B, and the secondary transfer roll 134 corresponds to an example of the transfer device in the unit according to the present embodiment. An apparatus including the developing device 120B and the transfer device having the intermediate transfer belt 133, the primary transfer roll 117B, and the secondary transfer roll 134 corresponds to an example of the unit according to the above-described embodiment.
[0043] 1 is an image forming apparatus having a configuration in which toner cartridges 140Y, 140M, 140C, 140K, and 140B are detachably attached, and developing devices 120Y, 120M, 120C, 120K, and 120B are connected to toner cartridges corresponding to the respective developing devices (colors) by toner supply pipes (not shown). When the toner contained in a toner cartridge becomes low, the toner cartridge is replaced.
[0044] The main parts (developing device and transfer device) of the unit and image forming apparatus according to the present embodiment will be described in more detail below. Note that the reference numerals will be omitted in the following description.
[0045] [Developing device] The developing device will now be described. The developing device is provided, for example, downstream in the rotation direction of the image carrier from the position where light is irradiated by the electrostatic image forming device. A container for containing the developer is provided within the developing device. The container contains the developer having flat toner containing flat pigments. The flat toner is contained, for example, in a charged state within the developing device. Details of the flat toner will be described later.
[0046] The developing device 18 includes a developing member that develops the electrostatic image formed on the surface of the image carrier with a developer containing flat toner, and a power source that applies a developing voltage to the developing member. The developing member is electrically connected to the power source, for example.
[0047] The developing member of the developing device is selected depending on the type of developer, and may be, for example, a developing roll having a developing sleeve with a built-in magnet.
[0048] In the developing device (including the power source), for example, a developing voltage is applied to the developing member. The developing member to which the developing voltage is applied is charged to a developing potential corresponding to the developing voltage. Then, the developing member charged to the developing potential holds the developer contained in the developing device on its surface, for example, and supplies the flat toner contained in the developer from inside the developing device to the surface of the image carrier.
[0049] The toner supplied onto the image carrier adheres to the electrostatic image on the image carrier by electrostatic force, for example. In detail, the flat toner contained in the developer is supplied to the area on the image carrier where the electrostatic image is formed by the potential difference in the area where the image carrier faces the developing member, that is, the potential difference between the potential of the surface of the image carrier in the area and the development potential of the developing member. If the developer contains a carrier, the carrier returns to the developing device while being held by the developing member.
[0050] For example, an electrostatic image on the image carrier is developed with flat toner supplied from a developing member, and a toner image corresponding to the electrostatic image is formed on the image carrier.
[0051] [Flat toner] The flat toner will now be described. The flat toner contains a flat pigment. Specifically, the flat toner has flat toner particles containing a flat pigment. The flat toner may also contain an external additive.
[0052] (Flat toner particles) The flat toner particles contain, for example, a binder resin and a flat pigment. The flat toner particles may contain a colorant, a release agent, and other components other than the flat pigment.
[0053] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.
[0054] In particular, it is preferable to use a combination of an amorphous resin and a crystalline resin as the binder resin. However, the mass ratio of the amorphous resin to the crystalline resin (crystalline resin / amorphous resin) is preferably from 3 / 97 to 50 / 50, and more preferably from 7 / 93 to 30 / 70.
[0055] Here, the term "amorphous resin" refers to a resin that, in a thermal analysis measurement using differential scanning calorimetry (DSC), has only a stepwise endothermic change rather than a clear endothermic peak, is a solid at room temperature, and is thermoplasticized at a temperature equal to or higher than the glass transition temperature. On the other hand, a crystalline resin refers to a resin that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC). Specifically, for example, a crystalline resin means a resin whose half-width of an endothermic peak is within 10°C when measured at a heating rate of 10°C / min, and an amorphous resin means a resin whose half-width exceeds 10°C or a resin in which no clear endothermic peak is observed.
[0056] The amorphous resin will now be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene-acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, amorphous polyester resin and amorphous vinyl resin (particularly styrene-acrylic resin) are preferred, and amorphous polyester resin is more preferred. In addition, it is also a preferred embodiment to use an amorphous polyester resin and a styrene-acrylic resin in combination as the amorphous resin. It is also a preferred embodiment to use an amorphous resin having an amorphous polyester resin segment and a styrene-acrylic resin segment as the amorphous resin.
[0057] Examples of the crystalline resin include known crystalline resins such as crystalline polyester resins and crystalline vinyl resins (e.g., polyalkylene resins, long-chain alkyl (meth)acrylate resins, etc.). Among these, crystalline polyester resins are preferred from the viewpoints of mechanical strength and low-temperature fixability of the flat toner.
[0058] The content of the binder resin is preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total amount of the flat toner particles.
[0059] -Flat pigment- The flat pigment is preferably a glittering pigment. Examples of the luster pigment include pigments (luster pigments) that can impart a sense of luster such as metallic luster.Specific examples of the luster pigment include metal powders such as aluminum (metal of aluminum alone), brass, bronze, nickel, stainless steel, and zinc; mica coated with titanium oxide, yellow iron oxide, and the like; coated flaky inorganic crystal substrates such as barium sulfate, layered silicate, and layered aluminum silicate; single crystal plate-like titanium oxide; basic carbonate; acid oxychloride bismuth; natural guanine; flaky glass powder; and metal-deposited flaky glass powder, and there is no particular limit to the luster pigments. Among these, metal powders are preferred as the bright pigment, particularly from the viewpoint of specular reflection intensity, and among these, aluminum is most preferred.
[0060] The average length in the major axis direction of the flat pigment is preferably from 1 μm to 30 μm, more preferably from 3 μm to 20 μm, and even more preferably from 5 μm to 15 μm. The ratio (aspect ratio) of the average length in the major axis direction to the average length in the thickness direction of the flat pigment is preferably 5 or more and 200 or less, more preferably 10 or more and 100 or less, and even more preferably 30 or more and 70 or less.
[0061] The average length and aspect ratio of each flat pigment are measured by the following method: Using a scanning electron microscope (S-4800, manufactured by Hitachi High-Technologies Corporation), a photograph of the flat pigment is taken at a measurable magnification (300 to 100,000 times), and the image of the flat pigment obtained is two-dimensionalized, and the length in the major axis direction and the length in the thickness direction of each particle are measured, and the average length in the major axis direction and the aspect ratio of the flat pigment are calculated. Here, the length in the major axis direction of the flat pigment refers to the longest part when the flat pigment is observed from the thickness direction of the flat pigment, and the length in the thickness direction of the flat pigment refers to the longest part when the flat pigment is observed from the direction perpendicular to the thickness direction of the flat pigment.
[0062] The volume average particle size of the flat pigment is preferably from 1.0 μm to 20.0 μm, and more preferably from 2.0 μm to 15.0 μm.
[0063] The volume average particle size of the flat pigment is measured as follows. Based on the particle size distribution measured with a measuring device such as Multisizer II (manufactured by Coulter), a cumulative distribution is drawn for each volume of divided particle size ranges (channels) from the smallest diameter side, and the particle size at which the cumulative 50% is reached is the volume average particle size. The method for measuring the volume average particle size of the flat pigment in the flat toner particles after production is to mix and stir the flat toner with a solvent that can dissolve only the resin but not the flat pigment, and after the resin has been sufficiently dissolved in the solvent, the flat pigment is subjected to solid-liquid separation and the volume average particle size is measured using a particle size distribution measuring device similar to that described above.
[0064] The content of the flat pigment is preferably from 1% by mass to 70% by mass, more preferably from 5% by mass to 50% by mass, and even more preferably from 5% by mass to 40% by mass, based on the total mass of the flat toner particles.
[0065] -Colorants other than flat pigments- Examples of colorants other than flat pigments include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, etc. pigments such as blue, ultramarine blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate; and dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based. The colorants other than the flat pigment may be used alone or in combination of two or more kinds.
[0066] The colorant other than the flat pigment may be a colorant that has been surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of colorants may be used in combination.
[0067] The content of colorants other than the flat pigment is adjusted according to the color tone of the flat toner.
[0068] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.
[0069] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature of the release agent is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."
[0070] The content of the release agent is preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the flat toner particles.
[0071] -Other additives- Examples of other additives include known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the flat toner particles as internal additives.
[0072] -Characteristics of flat toner particles- The flat toner particles are flat and have an average equivalent circle diameter D longer than the average maximum thickness C thereof. If the flat toner particles are flat with a circular equivalent diameter longer than their thickness (see Figure 2), then in the fixing process of image formation, the pressure applied during fixing causes the flat toner particles to line up so that their flat surfaces face the recording medium surface. In Figure 2, 2 indicates the flat toner particles, 4 indicates the flat pigment, and L indicates the thickness of the flat toner particles.
[0073] The ratio (C / D) of the average maximum thickness C to the average equivalent circular diameter D is preferably in the range of 0.001 or more and 0.700 or less, more preferably in the range of 0.001 or more and 0.500 or less, even more preferably in the range of 0.100 or more and 0.600 or less, and particularly preferably in the range of 0.300 or more and 0.450 or less. By making the ratio (C / D) 0.001 or more, the strength of the toner particles is ensured, breakage due to stress during image formation is suppressed, and the decrease in charge caused by the exposure of the flat pigment, which results in the occurrence of fog, is suppressed. On the other hand, when the flat pigment is a glitter pigment, by making the ratio (C / D) 0.700 or less, excellent glitter is obtained.
[0074] The average maximum thickness C and the average equivalent circle diameter D are measured by the following method. The flat toner particles are placed on a smooth surface and then vibrated to disperse them evenly. For 1,000 toner particles, the maximum thickness C of the toner particles and the equivalent circle diameter D of the surface as viewed from above are measured at 1,000 times magnification using a color laser microscope "VK-9700" (manufactured by Keyence Corporation), and the arithmetic average value is calculated.
[0075] When a cross section of a flat toner particle in the thickness direction is observed, the proportion (by number) of flat pigments in which the angle between the long axis direction of the toner particle in the cross section and the long axis direction of the flat pigment is in the range of -30° to +30° is preferably 60% or more of all observed flat pigments.Moreover, the above proportion is more preferably 70% to 95%, and particularly preferably 80% to 90%. When the flat pigment is a glittering pigment, excellent glittering properties can be obtained by setting the above ratio to 60% or more.
[0076] Here, a method for observing the cross section of a flat toner particle will be described. The toner particles are embedded in a bisphenol A liquid epoxy resin and a curing agent, and then a cutting sample is prepared. The cutting sample is then cut at -100°C using a cutting machine with a diamond knife, for example, an ultramicrotome (UltracutUCT, manufactured by Leica), to prepare a sample for observation. The observation sample is observed, for example, with an ultra-high resolution field emission scanning electron microscope (S-4800, manufactured by Hitachi High-Technologies Corporation) at a magnification where one to ten flat pigment toner particles are visible in one field of view. Specifically, the cross-section of a flat toner particle (cross-section along the thickness direction of the flat toner particle) is observed, and for 100 observed flat toner particles, the number of flat pigments in which the angle between the long axis direction in the cross-section of the flat toner particle and the long axis direction of the flat pigment is in the range of -30° to +30° is counted using image analysis software such as image analysis software (Win ROOF) manufactured by Mitani Shoji Co., Ltd., or an output sample of the observed image and a protractor, and the percentage is calculated.
[0077] The volume average particle diameter of the flat toner particles is preferably 3 μm or more and 30 μm or less, and more preferably 5 μm or more and 20 μm or less.
[0078] The various average particle sizes and various particle size distribution indices of the flat toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:
[0079] (External additives) Examples of the external additive include inorganic particles, such as SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4.
[0080] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.
[0081] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles).
[0082] The amount of the external additive added is, for example, preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.
[0083] (Method of manufacturing flat toner) The flat toner can be obtained, for example, by producing flat toner particles and then externally adding an external additive to the flat toner particles.
[0084] The flat toner particles may be produced by any of a dry production method (e.g., a kneading and grinding method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution and suspension method, etc.). There is no particular limitation on these production methods, and any known production method may be used. Among these, it is preferable to obtain the flat toner particles by the aggregation and coalescence method.
[0085] [Developer] The developer may be a one-component developer containing only flat toner, or a two-component developer containing a mixture of flat toner and a carrier.
[0086] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.
[0087] In the two-component developer, the mixture ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.
[0088] [Transfer device] The transfer device includes an intermediate transfer belt having an outer peripheral surface onto which a toner image is transferred, a primary transfer device having a primary transfer member which primarily transfers the toner image formed on the surface of an image carrier onto the outer peripheral surface of the intermediate transfer belt, and a secondary transfer device which is disposed in contact with the outer peripheral surface of the intermediate transfer belt and has a secondary transfer member which secondarily transfers the toner image transferred onto the outer peripheral surface of the intermediate transfer belt onto the surface of a recording medium. The intermediate transfer belt will be described in detail later.
[0089] In the primary transfer device, a primary transfer member is disposed opposite to an image carrier with an intermediate transfer belt interposed therebetween. In the primary transfer device, a voltage of a polarity opposite to the charge polarity of the toner is applied to the intermediate transfer belt by the primary transfer member, whereby the toner image is primarily transferred onto the outer peripheral surface of the intermediate transfer belt.
[0090] In the secondary transfer device, the secondary transfer member is disposed on the toner image carrying side of the intermediate transfer belt. The secondary transfer device includes, for example, a backing member disposed on the opposite side of the intermediate transfer belt from the toner image carrying side together with the secondary transfer member. In the secondary transfer device, the intermediate transfer belt and the recording medium are sandwiched between the secondary transfer member and the backing member to form a transfer electric field, whereby the toner image on the intermediate transfer belt is secondarily transferred to the recording medium. The secondary transfer member may be a secondary transfer roll or a secondary transfer belt. The backing member may be, for example, a backing roll.
[0091] The transfer device according to the present embodiment may be a transfer device that transfers a toner image onto a surface of a recording medium via multiple intermediate transfer bodies. In other words, the transfer device may be, for example, a transfer device that performs primary transfer of a toner image from an image carrier to a first intermediate transfer belt, secondary transfer of the toner image from the first intermediate transfer body to a second intermediate transfer body, and then tertiary transfer of the toner image from the second intermediate transfer body to a recording medium. When the transfer device includes a plurality of intermediate transfer bodies, at least a transfer belt, which will be described later, is used as an intermediate transfer belt that transfers a toner image onto a recording medium.
[0092] [Intermediate transfer belt] The intermediate transfer belt has the following adhesion characteristics:
[0093] (Adhesive properties) The intermediate transfer belt has a characteristic that when flat toner is adhered to the outer peripheral surface and then air is blown onto the outer peripheral surface from above the outer peripheral surface while increasing the blowing pressure, all of the flat toner adhered to the outer peripheral surface separates from the outer peripheral surface at a blowing pressure of 25 kPa or less (preferably 20 kPa or less, and more preferably 10 kPa or less, from the viewpoint of suppressing poor transfer of the toner image due to the flat toner). By satisfying this adhesive force characteristic, the non-electrostatic adhesive force generated between the outer peripheral surface of the intermediate transfer belt and the toner is reduced, and even when a flat toner is used, the transferability is improved and transfer defects are suppressed.
[0094] However, from the viewpoint of preventing poor transfer of the toner image due to flat toner, it is preferable that the intermediate transfer belt has the property that when flat toner is adhered to the outer peripheral surface and then air is blown onto the outer peripheral surface from above while increasing the blowing pressure, all of the flat toner adhered to the outer peripheral surface is separated from the outer peripheral surface at a blowing pressure of 2 kPa or more. When the flat toner has a certain degree of adhesion to the intermediate transfer belt, the flat toner is fixed on the outer circumferential surface of the intermediate transfer belt, making it easier to suppress transfer defects.
[0095] Here, the determination as to whether or not the adhesive force characteristics are satisfied is made as follows. First, a sample piece measuring 3 cm x 4 cm is taken from the target intermediate transfer belt. Next, in an environment of 22°C and 15%, a voltage of 10 kV was applied from above a height of 15 cm to the surface of the sample corresponding to the outer peripheral surface of the intermediate transfer belt, horizontally to the surface corresponding to the outer peripheral surface of the intermediate transfer belt. In this state, the target flat toner was scattered and measured at a concentration of 3 g / cm.2 The adhesive is applied with a loading amount of .
[0096] Next, air is blown onto the center of the flat toner-adhering surface of the sample piece from an air outlet with a diameter of 0.7 mm located 3 cm above the center at a pressure of 0.1 kPa, and the blowing pressure is increased at a rate of 0.5 kPa / sec. When the spray pressure reaches 25 kPa, if all the flat toner particles are separated from the sample piece, it is determined that the adhesive force characteristics are satisfied. On the other hand, if flat toner remains on the sample piece even when the spray pressure exceeds 25 kPa, it is determined that the adhesive force characteristics are not satisfied.
[0097] (Surface Free Energy) The surface free energy of the outer peripheral surface of the intermediate transfer belt is preferably 47 mN / m or less, more preferably 40 mN / m or less, and even more preferably 35 mN / m or less, from the viewpoint of suppressing transfer failure of the toner image due to flat toner. The lower limit of the surface free energy is, for example, 10 mN / m or more, from the viewpoint of cleaning property of the belt.
[0098] The surface free energy is measured using a contact angle meter CAM-200 (KSV) and is calculated using the Zisman method with a built-in program.
[0099] (water contact angle) The water contact angle of the outer peripheral surface of the intermediate transfer belt is preferably 80° or more, more preferably 85° or more, even more preferably 90° or more, and particularly preferably 95° or more, from the viewpoint of suppressing poor transfer of the toner image due to the flat toner. The lower limit of the water contact angle is, for example, 110° or less, from the viewpoint of the cleaning property of the belt.
[0100] The water contact angle is an index showing water repellency, and is measured as follows. In an environment of 25°C temperature and 50% humidity, 3 μl of pure water is dropped onto the surface of the measurement object using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd., model number: CA-X-FACE), and the droplet is photographed 3 seconds after dropping using an optical microscope. Then, the water contact angle θ is calculated from the photograph obtained based on the θ / 2 method.
[0101] (Layer composition) The intermediate transfer belt contains a resin and conductive carbon particles. From the viewpoint of satisfying the above-mentioned adhesive force characteristics, surface free energy, and water contact angle, the intermediate transfer belt preferably further contains a surfactant. Specifically, the intermediate transfer belt may be a single layer including a layer containing a resin, conductive carbon particles, and a surfactant, or a laminate having a layer including a resin, conductive carbon particles, and a surfactant as the outermost layer. The laminate may be a laminate of two or more layers having a base layer containing resin and conductive carbon particles, and a surface-outer layer provided on the outer peripheral surface side of the base layer and containing resin, conductive carbon particles, and a surfactant. Each layer may contain other components.
[0102] -resin- Examples of the resin include polyimide resin (PI resin), polyamideimide resin (PAI resin), aromatic polyether ketone resin (e.g., aromatic polyether ether ketone resin, etc.), polyphenylene sulfide resin (PPS resin), polyetherimide resin (PEI resin), polyester resin, polyamide resin, polycarbonate resin, etc. From the viewpoint of mechanical strength and dispersibility of conductive carbon particles, the resin preferably contains at least one selected from the group consisting of polyimide resin, polyamideimide resin, aromatic polyether ether ketone resin, polyetherimide resin, and polyphenylene sulfide resin, and more preferably contains at least one selected from the group consisting of polyimide resin and polyamideimide resin. Among them, polyimide resin is more preferable from the viewpoint of mechanical strength. The resin may be one type of resin or a mixture of two or more types of resins.
[0103] Examples of polyimide resins include imidized products of polyamic acids (precursors of polyimide resins), which are polymers of tetracarboxylic dianhydrides and diamine compounds. An example of the polyimide resin is a resin having a structural unit represented by the following general formula (I).
[0104] [ka]
[0105] In general formula (I), R 1 represents a tetravalent organic group, R 2 represents a divalent organic group. R 1 Examples of the tetravalent organic group represented by the formula (1) include an aromatic group, an aliphatic group, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, and groups in which these groups are substituted. Specific examples of the tetravalent organic group include residues of tetracarboxylic dianhydrides, which will be described later. R 2 Examples of the divalent organic group represented by the formula (1) include an aromatic group, an aliphatic group, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, and groups in which these groups are substituted. Specific examples of the divalent organic group include residues of diamine compounds described below.
[0106] Specific examples of tetracarboxylic dianhydrides used as raw materials for polyimide resins include pyromellitic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4-biphenyltetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenyl)sulfonic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, and ethylenetetracarboxylic dianhydride.
[0107] Specific examples of diamine compounds used as raw materials for polyimide resins include 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 1,5-diaminonaphthalene, m-phenylenediamine, p-phenylenediamine, 3,3'-dimethyl 4,4'-biphenyldiamine, benzidine, and 3,3'-dimethyl Benzidine, 3,3'-dimethoxybenzidine, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenylpropane, 2,4-bis(β-amino tert-butyl)toluene, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminophenyl)benzene, bis-p-(1,1-dimethyl-5-amino-pentyl)benzene, 1-isopropyl-2,4-m-phenylenediamine, m-xylylenediamine, p-xylylenediamine, di(p -aminocyclohexyl)methane, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, diaminopropyltetramethylene, 3-methylheptamethylenediamine, 4,4-dimethylheptamethylenediamine, 2,11-diaminododecane, 1,2-bis-3-aminopropoxyethane, 2,2-dimethylpropylenediamine, 3-methoxyhexamethylenediamine, 2,5-dimethylheptamethylenediamine, Examples include 3-methylheptamethylenediamine, 5-methylnonamethylenediamine, 2,17-diaminoeicosadecane, 1,4-diaminocyclohexane, 1,10-diamino-1,10-dimethyldecane, 12-diaminooctadecane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, piperazine, H2N(CH2)3O(CH2)2O(CH2)NH2, H2N(CH2)3S(CH2)3NH2, and H2N(CH2)3N(CH3)2(CH2)3NH2.
[0108] -Polyamide-imide resin- The polyamide-imide resin includes a resin having an imide bond and an amide bond in the repeating unit. More specifically, the polyamide-imide resin may be a polymer of a trivalent carboxylic acid compound (also called tricarboxylic acid) having an acid anhydride group, and a diisocyanate compound or a diamine compound.
[0109] As the tricarboxylic acid, trimellitic anhydride and its derivatives are preferable. In addition to the tricarboxylic acid, tetracarboxylic dianhydride, aliphatic dicarboxylic acid, aromatic dicarboxylic acid, etc. may be used in combination.
[0110] Examples of the diisocyanate compound include 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 2,2'-dimethylbiphenyl-4,4'-diisocyanate, biphenyl-4,4'-diisocyanate, biphenyl-3,3'-diisocyanate, biphenyl-3,4'-diisocyanate, 3,3'-diethylbiphenyl-4,4'-diisocyanate, 2,2'-diethylbiphenyl-4,4'-diisocyanate, 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, 2,2'-dimethoxybiphenyl-4,4'-diisocyanate, naphthalene-1,5-diisocyanate, and naphthalene-2,6-diisocyanate. The diamine compound may be a compound having a structure similar to that of the above-mentioned isocyanate, but having an amino group instead of the isocyanato group.
[0111] -Aromatic polyether ketone resin- Examples of aromatic polyether ketone resins include resins in which aromatic rings such as benzene rings are linearly bonded via ether bonds and ketone bonds. Examples of aromatic polyetherketone resins include polyetherketone (PEK) in which ether bonds and ketone bonds are arranged alternately, polyetheretherketone (PEEK) in which ether bonds, ether bonds, and ketone bonds are arranged in this order, polyetherketoneketone (PEKK) in which ether bonds, ketone bonds, and ketone bonds are arranged in this order, polyetheretherketoneketone (PEEKK) in which ether bonds, ether bonds, ketone bonds, and ketone bonds are arranged in this order, and polyetherketoneester containing ester bonds.
[0112] From the viewpoints of mechanical strength and volume resistivity adjustment, the resin content is preferably 60% by mass or more and 95% by mass or less, more preferably 70% by mass or more and 95% by mass or less, and even more preferably 75% by mass or more and 90% by mass or less.
[0113] (Conductive carbon particles) An example of the conductive carbon particles is carbon black. Examples of carbon black include ketjen black, oil furnace black, channel black, acetylene black, etc. As the carbon black, surface-treated carbon black (hereinafter also referred to as "surface-treated carbon black") may be used. Surface-treated carbon black can be obtained by imparting, for example, a carboxy group, a quinone group, a lactone group, a hydroxy group, etc. to its surface. Examples of the surface treatment method include an air oxidation method in which the carbon black is reacted by contacting with air in a high-temperature atmosphere, a method in which the carbon black is reacted with nitrogen oxides or ozone at room temperature (e.g., 22°C), and a method in which the carbon black is oxidized with air in a high-temperature atmosphere and then oxidized with ozone at a low temperature.
[0114] Among these, the carbon black is preferably channel black, and surface-treated channel black is more preferable.
[0115] The pH of the conductive carbon particles is, for example, in the range of 1.0 to 5.5, and preferably in the range of 1.0 to 3.0.
[0116] The number average primary particle size of the conductive carbon particles is preferably 40 nm or less, 20 nm or less, 18 nm or less, 15 nm or less, or 13 nm or less, from the viewpoints of dispersibility, mechanical strength, volume resistivity, film-forming properties, and the like. On the other hand, the number average primary particle size of the conductive carbon particles is preferably 2 nm or more, 5 nm or more, or 10 nm or more.
[0117] The number average primary particle size of the conductive carbon particles is measured by the following method. First, a measurement sample having a thickness of 100 nm is taken from the obtained belt using a microtome, and this measurement sample is observed using a TEM (transmission electron microscope).Then, the diameter of a circle equal to the projected area of each of 50 conductive carbon particles (i.e., the equivalent circle diameter) is taken as the particle diameter, and the average value of these is taken as the number-average primary particle diameter.
[0118] From the viewpoint of ensuring strength, the content of the conductive carbon particles is preferably 10% by mass or more and 50% by mass or less, more preferably 13% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less, based on the entire layer.
[0119] -Surfactants- The surfactant is preferably a surfactant having at least one of a perfluoroalkyl structure, an alkylene oxide structure, and a silicone structure. When a surfactant having such a structure is used, the adhesive properties, surface free energy, water contact angle, and diiodomethane contact angle are satisfied, and the transferability to the textured paper is easily improved.
[0120] Suitable surfactants having a perfluoroalkyl structure include perfluoroalkyl sulfonic acids (e.g., perfluorobutanesulfonic acid, perfluorooctane sulfonic acid, etc.), perfluoroalkyl carboxylic acids (e.g., perfluorobutane carboxylic acid, perfluorooctane carboxylic acid, etc.), and perfluoroalkyl group-containing phosphates. The perfluoroalkyl sulfonic acids and perfluoroalkyl carboxylic acids may be salts thereof or amide-modified products thereof.
[0121] Commercially available surfactants having a perfluoroalkyl structure include, for example, the Megafac series (manufactured by DIC), the F-Top series (manufactured by JEMCO), the F-tergent series (manufactured by Neos), the Surflon series (manufactured by AGC Seimi Chemical Co., Ltd.), the PF series (manufactured by Kitamura Chemical Co., Ltd.), and the FC series (manufactured by 3M).
[0122] Examples of surfactants having an alkylene oxide structure include polyethylene glycol, polyether antifoaming agents, and polyether modified silicone oils. The polyethylene glycol preferably has a number average molecular weight of 2000 or less. Examples of polyethylene glycols having a number average molecular weight of 2000 or less include polyethylene glycol 2000 (number average molecular weight 2000), polyethylene glycol 600 (number average molecular weight 600), polyethylene glycol 400 (number average molecular weight 400), polyethylene glycol 200 (number average molecular weight 200), etc. Examples of polyether defoamers include the PE series (manufactured by Wako Pure Chemical Industries, Ltd.) and the defoamer series (manufactured by Kao Corporation). The polyether-modified silicone oil may be a silicone oil in which at least one of the side chains and the terminals of the polysiloxane chain is modified with a polyalkylene oxide.
[0123] Examples of surfactants having a silicone structure include common silicone oils such as dimethyl silicone, methylphenyl silicone, diphenyl silicone, and derivatives thereof. Examples of surfactants having a silicone structure include KF Series 351(A), KF352(A), KF353(A), KF354(A), KF355(A), KF615(A), KF618, KF945(A), KF6004, KP126, KP109 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF Series (manufactured by GE Toshiba Silicon), BYK Series-UV Series, etc. (manufactured by BYK Japan KK), and Ogsol Series (manufactured by Osaka Gas Chemicals Co., Ltd.).
[0124] Among these, the surfactant is preferably at least one of an oligomer having a perfluoroalkyl structure with 6 or less carbon atoms and an oligomer having a silicone structure with a methyl group. By using these surfactants, the adhesive properties, surface free energy, and water contact angle are satisfied, and it becomes easier to suppress poor transfer of a toner image caused by flat toner.
[0125] Here, the oligomer having a perfluoroalkyl structure with 6 or less carbon atoms may be an oligomer having 6 or less carbon atoms (preferably 2 to 6 carbon atoms) and a substituent having a fluorine atom. However, from the viewpoint of satisfying the adhesive force characteristics, surface free energy, and water contact angle and suppressing transfer failure of a toner image due to a flat toner, an oligomer having a perfluoroalkyl structure with 6 or less carbon atoms (preferably 2 to 6 carbon atoms) is preferred.
[0126] In addition, from the viewpoint of satisfying the adhesive properties, surface free energy, and water contact angle and suppressing poor transfer of toner images due to flat toner, preferred examples of oligomers having a silicone structure with a methyl group include oligomers having at least one of the following silicone structures: a "-SiH(CH3)-O-" structure, a "-Si(CH3)2-O-" structure, and a "-Si(CH3)(Ph)-O-" structure (in the structural formula, Ph represents a phenyl group). The surfactant may be an oligomer having a silane structure with a methyl group. Specifically, the oligomer having a silane structure with a methyl group is -[SiH(CH)] n-Structure, -[Si(CH3)2] n - Structure, and -[Si(CH3)(Ph)] n Preferred examples of the oligomer include oligomers having at least one of the following structures: -structure (in the structural formula, Ph is a phenyl group, and n is an integer of 2 or more).
[0127] From the viewpoint of satisfying the adhesive property, surface free energy, and water contact angle and suppressing the transfer failure of the toner image by the flat toner, these oligomers are preferably polymers in which 4 or more monomers are bonded, that is, the number of repeating units of the monomer in the oligomer is preferably 4 or more. The oligomer is preferably a polymer in which 4 to 1000 (or 4 to 300) monomers are bonded together. In other words, the number of repeating units of the monomer in the oligomer is preferably 4 to 1000 (or 4 to 300). In addition, the monomer in the oligomer is a monomer having a perfluoroalkyl structure (e.g., (meth)acrylic acid ester, etc.) in the case of an oligomer having a perfluoroalkyl structure with 6 or less carbon atoms, and is a siloxane having a methyl group in the case of an oligomer having a silicone structure with a methyl group.
[0128] The content of the surfactant is adjusted within a range that satisfies the adhesive properties, surface free energy, and water contact angle. The content of the surfactant is preferably from 0.5 to 10% by mass, more preferably from 0.7 to 7% by mass, and even more preferably from 1.0 to 5% by mass, based on the layer containing the surfactant.
[0129] -Other ingredients- Examples of other components include conductive agents other than conductive carbon particles, fillers for improving the strength of the belt, antioxidants for preventing thermal deterioration of the belt, surfactants for improving fluidity, and heat-resistant anti-aging agents.
[0130] (Volume resistivity of intermediate transfer belt) From the viewpoint of suppressing poor transfer of toner images caused by flat toner, the common logarithm of the volume resistivity when a voltage of 500 V is applied to the intermediate transfer belt for 10 seconds is preferably 9.0 (log Ω·cm) or more and 13.5 (log Ω·cm) or less, more preferably 9.5 (log Ω·cm) or more and 13.2 (log Ω·cm) or less, and particularly preferably 10.0 (log Ω·cm) or more and 12.5 (log Ω·cm) or less. The volume resistivity of the endless belt when a voltage of 500 V is applied for 10 seconds is measured by the following method. A microammeter (Advantest R8430A) is used as the resistance measuring device, and a UR probe (Mitsubishi Chemical Analytech Co., Ltd.) is used as the probe to measure the volume resistivity (log Ω cm) at 6 equally spaced points in the circumferential direction of the endless belt, and 3 points in the center and both ends in the width direction, for a total of 18 points, at a voltage of 500 V, application time of 10 seconds, and pressure of 1 kgf, and the average value is calculated. The measurements are also performed in an environment with a temperature of 22°C and a humidity of 55% RH.
[0131] (Surface resistivity of intermediate transfer belt) From the viewpoint of suppressing poor transfer of a toner image due to flat toner, the common logarithm of the surface resistivity when a voltage of 500 V is applied for 10 seconds to the outer peripheral surface of the intermediate transfer belt is preferably 10.0 (log Ω / suq.) or more and 15.0 (log Ω / suq.) or less, more preferably 10.5 (log Ω / suq.) or more and 14.0 (log Ω / suq.) or less, and particularly preferably 11.0 (log Ω / suq.) or more and 13.5 (log Ω / suq.) or less, The unit of surface resistivity, logΩ / suq., is the logarithmic value of the resistance per unit area, and is also expressed as log(Ω / suq.), logΩ / suquare, logΩ / □, etc. The surface resistivity when a voltage of 500 V is applied to the outer peripheral surface of the intermediate transfer belt for 10 seconds is measured by the following method. A microammeter (R8430A manufactured by Advantest) is used as the resistance measuring device, and a UR probe (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) is used as the probe to measure the surface resistivity (logΩ / suq.) of the outer peripheral surface of the endless belt at 6 equally spaced points in the circumferential direction, and 3 points at the center and both ends in the width direction, for a total of 18 points, at a voltage of 500V, application time of 10 seconds, and pressure of 1kgf, and the average value is calculated. The measurements are also performed in an environment with a temperature of 22°C and a humidity of 55%RH.
[0132] (Manufacturing method of intermediate transfer belt) The method for producing the intermediate transfer belt is not particularly limited. An example of a method for manufacturing an intermediate transfer belt includes a method in which a coating liquid containing a resin or a precursor thereof, conductive carbon particles, and a solvent is applied onto the outer periphery of a substrate to form a coating film, and the coating film is then dried. In the method for producing the intermediate transfer belt, when a resin precursor is used, the coating film dried by drying may be baked. Another example of a method for producing an intermediate transfer belt may be a method in which pellets containing a resin and conductive carbon particles are prepared, and the pellets are melt-extruded to form a belt.
[0133] Although the present embodiment has been described above, the present invention is not limited to the above embodiment, and various modifications, changes, and improvements are possible. EXAMPLES
[0134] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the following examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0135] <Developer> [Developer (1)] (Synthesis of binder resin) Dimethyl adipate: 74 parts Dimethyl terephthalate: 192 parts Bisphenol A ethylene oxide adduct: 216 parts Ethylene glycol: 38 parts Tetrabutoxytitanate (catalyst): 0.037 parts,
[0136] The above components were placed in a heated and dried two-necked flask, nitrogen gas was introduced into the vessel to maintain an inert atmosphere, and the temperature was raised while stirring, after which a polycondensation reaction was carried out at 160°C for 7 hours, after which the pressure was gradually reduced to 10 Torr while the temperature was raised to 220°C and maintained for 4 hours. The pressure was once returned to normal, 9 parts of trimellitic anhydride was added, the pressure was gradually reduced again to 10 Torr, and the mixture was maintained at 220°C for 1 hour to synthesize a binder resin.
[0137] The glass transition temperature (Tg) of the binder resin was determined in accordance with ASTM D3418-8 by using a differential scanning calorimeter (Shimadzu: DSC-50) under conditions of a temperature rise rate of 10°C / min from room temperature (25°C) to 150°C. The glass transition temperature was the temperature at the intersection of the baseline in the endothermic part and the extension of the rising line. The glass transition temperature of the binder resin was 63.5°C.
[0138] (Preparation of Resin Particle Dispersion) Binder resin: 160 parts Ethyl acetate: 233 parts Sodium hydroxide solution (0.3N): 0.1 part
[0139] The above components were placed in a 1000 ml separable flask, heated to 70°C, and stirred with a Three-One Motor (Shinto Scientific Co., Ltd.) to prepare a resin mixture. While stirring this resin mixture at 90 rpm, 373 parts of ion-exchanged water was gradually added to cause phase inversion emulsification and desolvation to obtain a resin particle dispersion (solid concentration: 30%). The volume average particle diameter of the resin particle dispersion was 162 nm.
[0140] (Preparation of release agent dispersion) Carnauba wax (Toa Kasei Co., Ltd., RC-160): 50 parts Anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1.0 part -Ion-exchanged water: 200 parts
[0141] The above ingredients were mixed and heated to 95°C, and dispersed using a homogenizer (Ultra Turrax T50, manufactured by IKA Corporation). After that, a dispersion treatment was carried out for 360 minutes using a Manton-Gaulin high pressure homogenizer (Gaulin Corporation) to prepare a release agent dispersion liquid (solid content concentration: 20%) in which release agent particles having a volume average particle diameter of 0.23 μm were dispersed.
[0142] (Preparation of Metal Pigment Particle Dispersion) Aluminum pigment (Showa Aluminum Powder Co., Ltd., 2173EA): 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen R): 1.5 parts Ion-exchanged water: 900 parts
[0143] After removing the solvent from the aluminum pigment paste, the above was mixed, dissolved, and dispersed for about 1 hour using an emulsifying disperser Cavitron (manufactured by Pacific Machinery Co., Ltd., CR1010) to prepare a metal pigment particle dispersion (solids concentration: 10%) in which metal pigment particles (aluminum pigment) were dispersed. The average length in the major axis direction of the aluminum pigment (flat pigment) was 8 μm, and the average length in the thickness direction was 0.1 μm.
[0144] (Preparation of External Additive (1)) An external additive (1) having a surface treatment amount of 5 mass % with dimethyl silicone oil and an average primary particle size of 100 nm was prepared by a sol-gel method.
[0145] (Preparation of Flat Toner (1)) ·Resin particle dispersion: 380 parts Release agent dispersion: 72 parts Metal pigment particle dispersion: 140 parts
[0146] The above-mentioned metal pigment particle dispersion, resin particle dispersion, and release agent dispersion were placed in a 2 L cylindrical stainless steel container, and dispersed and mixed for 10 minutes while applying shear force at 4000 rpm using a homogenizer (IKA Ultra Turrax T50). Next, 1.75 parts of a 10% aqueous nitric acid solution of polyaluminum chloride as a flocculant was gradually added dropwise, and the homogenizer was rotated at 5000 rpm to disperse and mix for 15 minutes to obtain a raw material dispersion.
[0147] Thereafter, the raw material dispersion was transferred to a polymerization kettle equipped with a stirrer using two paddle stirring blades and a thermometer, the stirring speed was set to 810 rpm, heating was started with a mantle heater, and aggregated particles were grown at 54° C. At this time, the pH of the raw material dispersion was controlled in the range of 2.2 to 3.5 with 0.3 N nitric acid or 1 N sodium hydroxide aqueous solution. The pH was maintained in the above range for about 2 hours to form aggregated particles.
[0148] Next, the resin particle dispersion liquid was added, and the resin particles of the binder resin were attached to the surface of the aggregated particles. The temperature was further increased to 56°C, and the aggregated particles were adjusted while checking the particle size and shape with an optical microscope and a Multisizer II. Thereafter, the pH was increased to 8.0 to fuse the aggregated particles, and the temperature was increased to 67.5°C. After confirming that the aggregated particles were fused with an optical microscope, the pH was lowered to 6.0 while maintaining the temperature at 67.5°C, and heating was stopped after 1 hour, and the mixture was cooled and flattened at a temperature drop rate of 0.1°C / min. The mixture was then sieved through a 20 μm mesh, washed repeatedly with water, and dried in a vacuum dryer to obtain flat toner particles.
[0149] Furthermore, the flat toner particles were heat-treated in a hot air dryer at 45° C. for 1 hour. 1.2 parts of external additive (1), 1.5 parts of hydrophobic silica (manufactured by Nippon Aerosil Co., Ltd., RY50), and 1.0 part of hydrophobic titanium oxide (manufactured by Nippon Aerosil Co., Ltd., T805) were mixed with a sample mill at 10,000 rpm for 30 seconds per 100 parts of the flat toner particles after the heat treatment. The mixture was then sieved with a vibrating sieve with an opening of 45 μm to produce flat toner (1).
[0150] The volume average particle diameter of the flat toner particles was 12.2 μm, and the ratio (C / D) of the average maximum thickness C of the flat toner particles to the average equivalent circle diameter D of the flat toner particles was 0.31.
[0151] (Creating the carrier) Ferrite particles (volume average particle size: 35 μm): 100 parts Toluene: 14 parts Perfluorooctylethyl acrylate / methyl methacrylate copolymer: 1.6 parts Carbon black (product name: VXC-72, manufactured by Cabot Corporation): 0.12 parts Crosslinked melamine resin particles (average particle size: 0.3 μm, insoluble in toluene): 0.3 parts
[0152] First, carbon black was diluted with toluene and added to perfluorooctylethyl acrylate / methyl methacrylate copolymer, and dispersed with a sand mill. Next, the above-mentioned components other than ferrite particles were dispersed in the mixture with a stirrer for 10 minutes to prepare a coating layer forming solution. Next, the coating layer forming solution and ferrite particles were placed in a vacuum degassing kneader, stirred at a temperature of 60°C for 30 minutes, and then the pressure was reduced to remove toluene, forming a resin coating layer and obtaining a carrier.
[0153] (Preparation of developer) 36 parts of the flat toner and 414 parts of the carrier were placed in a 2-liter V blender and stirred for 20 minutes, and then sieved through a 212 μm sieve to prepare developer (1).
[0154] [Developer (2)] Flat toner (2) was obtained in the same manner as flat toner (1), except that the amount of external additive (1) was changed to 1.7 parts in the preparation of flat toner (1). A developer (2) was obtained in the same manner as the developer (1), except that the obtained flat toner (2) was used.
[0155] [Developer (3)] Flat toner (3) was obtained in the same manner as flat toner (1), except that flat toner (3) was produced without adding external additive (1). A developer (3) was obtained in the same manner as the developer (1), except that the obtained flat toner (3) was used.
[0156] <Intermediate transfer belt> [Intermediate transfer belt (1)] Polyamic acid solution DA-A1 (solid content: 45% by weight) 70 parts by weight Polyamic acid solution DC-A1 (solid content: 15% by weight) 30 parts by weight Acidic carbon black (dry; conductive carbon particles) [Color Black FW200, manufactured by Orion Engineered Carbons, gas black (i.e., channel black), number-average primary particle size: 13 nm, pH: 3.0 (hereinafter abbreviated as "FW200")] 18 parts by mass Surfactant (Surflon S-651): The amount shown in Table 1 (content relative to the layer containing the surfactant (hereinafter the same)) The polyamic acid solutions DA-A1 and DC-A1 having the above compositions were mixed, and a surfactant was added together with FW200, and the mixture was dispersed in the polyamic acid solution by dispersing for 12 hours at 30° C. in a ball mill. The mixture in which FW200 was dispersed was then filtered through a #800 stainless steel mesh to obtain a coating solution.
[0157] A cylindrical mold made of stainless steel with an outer diameter of 366 mm and a length of 400 mm was prepared as the material to be coated. A silicone-based mold release agent (Shin-Etsu Chemical Co., Ltd., product name: Sepacoat SP) was applied to the outer surface of the mold release agent, and a drying process (mold release agent treatment) was performed.
[0158] While rotating a cylindrical mold treated with a mold release agent in the circumferential direction at a speed of 10 rpm, the above coating liquid was discharged from a dispenser with a diameter of 1.0 mm from the end of the cylindrical mold, and applied by pressing with a uniform pressure using a metal blade installed on the mold. The dispenser unit was moved in the axial direction of the cylindrical mold at a speed of 100 mm / min, whereby Coating Liquid A1 was applied in a spiral shape onto the cylindrical mold to form a coating film. Next, the coating film was dried in a drying oven for 15 minutes at 140° C. in an air atmosphere while rotating at 10 rpm. The integrated average heating rate A / B in the drying process of the coating film was 6.00° C. / min.
[0159] Next, the endless belt was obtained by placing the endless belt in an oven for 4 hours at a temperature of 320° C. The total thickness of the endless belt (i.e., the thickness of a single layer) was 80 μm. The endless belt was removed from the mold, stretched around a holder, and cut with a cutter whose insertion angle was adjusted to obtain an intermediate transfer belt (1) having a diameter of 366 mm and a width of 369 mm. When the volume resistivity and the surface resistivity of the outer peripheral surface of the intermediate transfer belt (1) were measured by the above-mentioned method, the common logarithm value of the volume resistivity was 11.4 (log Ω cm), and the common logarithm value of the surface resistivity was 11.2 (log Ω / suq.).
[0160] [Intermediate transfer belt (2)~(14)] Intermediate transfer belts (2) to (14) were obtained in the same manner as intermediate transfer belt (1), except that the type and content of the surfactant were changed according to Table 1.
[0161] The types of surfactants used in the intermediate transfer belts (1) to (14) are as follows: Surflon S-431: AGC Seimi Chemical Co., Ltd., oligomer with a perfluoroalkyl structure with 5 carbon atoms (oligomer with 30 repeating units of a monomer with a perfluoroalkyl structure with 5 carbon atoms) Futergent 601ADH: Manufactured by Neos Corporation, an oligomer with a perfluoroalkyl structure with 5 carbon atoms (an oligomer with 200 repeating units of a monomer with a perfluoroalkyl structure with 5 carbon atoms). KP109: Manufactured by Shin-Etsu Chemical Co., Ltd., an oligomer with a silicone structure containing methyl groups (siloxane repeat number 500) KP126: Shin-Etsu Chemical Co., Ltd., an oligomer with a silicone structure containing methyl groups (siloxane repeat number: 500) OGSOL SI 10-10: Manufactured by Osaka Gas Chemicals Co., Ltd., an oligomer with a silane structure having methyl and phenyl groups (silane repeat number: 10) FC4430: 3M, oligomer with a perfluoroalkyl structure with 4 carbon atoms (10 repeating units of monomer with a perfluoroalkyl structure with 4 carbon atoms) FC4432: 3M, oligomer with a perfluoroalkyl structure having 4 carbon atoms (10 repeating units of monomer having a perfluoroalkyl structure having 4 carbon atoms) In Table 1, the column for the number of carbon atoms in the surfactant indicates the number of carbon atoms in the "perfluoroalkyl structure" of the surfactant, the siloxane substituent (methyl group), and the silane substituent (phenyl group).
[0162] [Evaluation of intermediate transfer belt characteristics] The intermediate transfer belt was measured for the following properties according to the methods described above, and the results are shown in Table 1. Adhesion amount characteristics (when flat toner is adhered to the outer peripheral surface of the intermediate transfer belt, and then air is blown onto the outer peripheral surface from above while increasing the blowing pressure, all of the polyester resin particles adhered to the outer peripheral surface are separated from the outer peripheral surface when the blowing pressure is within 25 kPa). The numerical value in the adhesion amount characteristics column in the table indicates the air blowing pressure when all of the flat toner adhered to the outer peripheral surface of the intermediate transfer belt is separated from the outer peripheral surface. Surface free energy of the outer surface of the endless belt (mN / m) ·Water contact angle of the outer surface of the endless belt (°)
[0163] <Examples 1 to 13, Comparative Example 1> The developer was filled into the developing device for forming glossy images of the image forming apparatus "Fuji Xerox Co., Ltd. DocuColor-7171P" in the combination shown in Table 1, and the intermediate transfer belt was installed in the transfer device. Then, the following evaluations were carried out using this image forming apparatus.
[0164] (Transfer failure evaluation) A solid blue image was formed on OS coated paper under conditions of a temperature of 22°C and a humidity of 55% RH, and the recording medium transport speed in the secondary transfer area was 366 mm / s, and the image was visually evaluated for uneven density. The evaluation criteria were as follows, and the results are shown in Table 1. -Evaluation criteria- A: No uneven density B: Slight unevenness in density C: Clear density unevenness occurs
[0165] [Table 1]
[0166] From the above results, it is understood that in this embodiment, transfer defects of a toner image caused by flat toner are suppressed compared to the comparative example. [Explanation of symbols]
[0167] 2. Flat toner particles 4. Flat pigments L Thickness of flat toner particles 111Y, 111M, 111C, 111K, 111B photoconductor 113 Driving Roll 112 Support roll 114 Opposing Roll 115Y, 115M, 115C, 115K, 115B Cleaning device 116 Intermediate transfer belt cleaning device 117Y, 117M, 117C, 117K, 117B Primary transfer roll 118Y, 118M, 118C, 118K, 118B Charging Roll 119Y, 119M, 119C, 119K, 119B Exposure equipment 120Y, 120M, 120C, 120K, 120B developing device 133 Intermediate transfer belt 134 Secondary transfer roll 135 Fixing device 140Y, 140M, 140C, 140K, 140B toner cartridges 150Y, 150M, 150C, 150K, 150B Image forming unit
Claims
1. a developing device that contains a developer having a flat toner containing a flat pigment and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the developer; a transfer device including an intermediate transfer belt onto which a toner image formed on the surface of said image carrier is primarily transferred, a primary transfer device which performs primary transfer of the toner image formed on the surface of said image carrier onto the surface of said intermediate transfer belt, and a secondary transfer device which performs secondary transfer of the toner image on the surface of said intermediate transfer belt onto a surface of a recording medium, said intermediate transfer belt including a resin and conductive carbon particles, and a transfer device in which, after said flat toner is adhered to an outer peripheral surface of said intermediate transfer belt, when air is blown onto said outer peripheral surface from above said outer peripheral surface while increasing the blowing pressure, all of said flat toner adhered to said outer peripheral surface is separated from said outer peripheral surface within said blowing pressure of 25 kPa or less; A unit equipped with.
2. A unit as described in claim 1, wherein after the flat toner is adhered to the outer peripheral surface of the intermediate transfer belt, when air is blown onto the outer peripheral surface from above the outer peripheral surface while increasing the blowing pressure, when the blowing pressure is 2 kPa or more, all of the flat toner adhered to the outer peripheral surface separates from the outer peripheral surface.
3. 3. The unit according to claim 1 or 2, wherein the intermediate transfer belt further comprises a surfactant.
4. The unit according to claim 3 , wherein the surfactant is at least one of an oligomer having a carbon number of 6 or less and a substituent having a fluorine atom, and an oligomer having a silicone structure having a methyl group.
5. The unit according to claim 4 , wherein the oligomer having a carbon atom or less and a substituent having a fluorine atom is an oligomer having a perfluoroalkyl structure having a carbon atom or less.
6. The unit according to claim 4 or 5, wherein the number of repeating units of the monomer in the oligomer is 4 or more.
7. 7. The unit according to claim 1, wherein the surface free energy of the outer peripheral surface of the intermediate transfer belt is 47 mN / m or less.
8. 8. The unit according to claim 7, wherein the water contact angle of the outer peripheral surface of the intermediate transfer belt is 85[deg.] or more.
9. a toner image forming device including an image carrier and the developing device of the unit according to any one of claims 1 to 8, the toner image being formed on a surface of the image carrier; A transfer device that transfers the toner image formed on the surface of the image carrier to a surface of a recording medium, the transfer device being one of the units according to any one of claims 1 to 8; An image forming apparatus comprising:
Citation Information
Patent Citations
Endless belt and endless belt unit
JP2010231023A
Endless flexible members for image forming devices
JP2012159838A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2015055841A
Photoluminescent toner, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2015184364A
Photoluminescent toner, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2017062413A