Toner for developing electrostatic images

A toner formulation with a specific aromatic vinyl thermoplastic elastomer and controlled crystalline domains addresses the trade-off between low-temperature fixability and storage stability, enhancing both properties for improved energy efficiency and printing performance.

JP7563542B2Active Publication Date: 2024-10-08ZEON CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023136565
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-27
Filing Date
2023-08-24
Publication Date
2024-10-08
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

Existing toners face a trade-off between low-temperature fixability and storage stability, with improvements in low-temperature fixing properties often compromising storage stability, and vice versa, leading to energy inefficiencies and performance issues.

Method used

A toner formulation containing a binder resin, colorant, charge control agent, and a specific aromatic vinyl thermoplastic elastomer with a diblock copolymer structure, along with a mold release agent, is developed to enhance both low-temperature fixability and storage stability by controlling the number and aspect ratio of crystalline domains within the toner particles.

Benefits of technology

The toner achieves excellent storage stability and low-temperature fixability, reducing energy consumption and improving printing efficiency by effectively preventing toner particle aggregation and fusion, thus meeting the demands for reduced energy use and faster printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563542000007
    Figure 0007563542000007
  • Figure 0007563542000001
    Figure 0007563542000001
  • Figure 0007563542000002
    Figure 0007563542000002
Patent Text Reader

Abstract

To provide an electrostatic charge image development toner excellent in storage stability and low temperature fixability.SOLUTION: An electrostatic charge image development toner includes: coloring resin particles including a binder resin, a colorant, a release agent and an aromatic vinyl based thermoplastic elastomer; and an external additive. The aromatic vinyl based thermoplastic elastomer includes a diblock copolymer consisting of the block of an aromatic vinyl polymer and the block of a polymer copolymerizable with the aromatic vinyl polymer at a ratio of 40 wt.% or more; and the content of the aromatic vinyl based thermoplastic elastomer to the binder resin of 100 pts.mass is 1-10 pts.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing electrostatic images, which is used for developing electrostatic latent images in electrophotography, electrostatic recording, electrostatic printing and the like. [Background technology]

[0002] 2. Description of the Related Art Image forming apparatuses such as electrophotographic apparatuses, electrostatic recording apparatuses, and electrostatic printing apparatuses widely employ a method of forming a desired image by developing an electrostatic latent image formed on a photoconductor with a toner for developing an electrostatic image, and this method is applied to copiers, printers, facsimiles, and multifunction machines thereof.

[0003] For example, in an electrophotographic device using electrophotography, the surface of a photoconductor made of a photoconductive material is generally uniformly charged by various means, an electrostatic latent image is then formed on the photoconductor, the electrostatic latent image is then developed using toner (developing process), and if necessary, the toner image is transferred to a recording material such as paper (transfer process), and the toner is then fixed to the recording material by heating or the like (fixing process) to obtain a printed matter.

[0004] Among the image forming processes, in the fixing process, it is usually necessary to heat the fixing roll to 150° C. or higher during fixing, and a large amount of electricity is consumed as an energy source. In response to this, in recent years, with the increasing demand for reducing energy consumption and increasing printing speed for the image forming apparatus, there is a demand for the design of a toner that can maintain a high fixing rate even at a low fixing temperature (a toner with excellent low-temperature fixing ability).

[0005] In response to the above demands, proposals have been made to lower the glass transition temperature (Tg) of the toner, to incorporate a low melting point resin and / or a low molecular weight resin into the toner, and to incorporate a low softening point substance (releasing agent) having releasability (peelability) such as wax into the toner.

[0006] However, while improving low-temperature fixability allows the temperature of the fixing roll to be set lower during fixing, when the toner is used at high temperatures or when the toner is left (stored) for a long period of time, fusion (blocking (aggregation)) between toner particles may occur more easily, and the storage stability of the toner may decrease. For this reason, when designing a toner, it is necessary to take into consideration storage stability, which is a property that is opposed to low-temperature fixability, and to develop a toner that can improve low-temperature fixability without impairing storage stability and reduce power consumption.

[0007] For example, Patent Document 1 discloses a black toner having toner particles containing a binder resin, a crystalline material, and a black colorant, characterized in that, in a cross section of the toner particle observed with a transmission electron microscope, when the major axis of the toner particle cross section is R (μm) and the major axis of a domain of the crystalline material is r (μm), for the toner particle cross section where R (μm) satisfies 4≦R≦12, a domain of the crystalline material that satisfies the following formula (i) is defined as domain A, and the number of domains A per toner particle cross section is 20 to 300. (i) 5.0×10 -4 ≦r / R≦7.0×10 -2

[0008] According to the technology of Patent Document 1, during thermal fixing, domain A melts, plasticizing the entire resin, and further, the crystalline material constituting domain A seeps out onto the surface of the toner particles, improving the fixing property and providing releasability from a fixing member such as a fixing film.

[0009] In addition, Patent Document 2 discloses a toner having toner particles containing a binder resin and a colorant, the toner having a storage modulus (G'60) at a temperature of 60°C in viscoelastic properties measured using a rotating plate rheometer at a frequency of 6.28 rad / sec is 1.0×10 7 ~1.0×10 9 (Pa), and the maximum value of the storage modulus (G'p) exists between 110°C and 140°C, and G'p is 5.0×10 4 ~5.0×106 (Pa). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2019-12188 A [Patent Document 2] JP 2012-177914 A Summary of the Invention [Problem to be solved by the invention]

[0011] On the other hand, although the technique of Patent Document 1 improves fixability such as low-temperature fixability, storage stability is insufficient, and therefore further improvement is required. Furthermore, the technique of Patent Document 2 uses a polyester resin as a binder resin, and the technique of Patent Document 2 has a problem in that low-temperature fixability is insufficient. An object of the present invention is to provide a toner for developing electrostatic images which is excellent in storage stability and low-temperature fixing ability. [Means for solving the problem]

[0012] According to the present invention, there is provided a toner for developing electrostatic images, comprising a binder resin, a colorant, a release agent, colored resin particles containing an aromatic vinyl thermoplastic elastomer, and an external additive, the aromatic vinyl thermoplastic elastomer contains a diblock copolymer consisting of an aromatic vinyl polymer block and a polymer block copolymerizable with the aromatic vinyl polymer in a proportion of 40% by weight or more; The toner for developing electrostatic images is provided, in which the content of the aromatic vinyl thermoplastic elastomer is 1 to 10 parts by mass relative to 100 parts by mass of the binder resin. In the electrostatic image developing toner of the present invention, the content of the aromatic vinyl monomer units in the aromatic vinyl thermoplastic elastomer is preferably 10 to 30% by mass based on the total monomer units. In the electrostatic image developing toner of the present invention, the release agent is preferably a fatty acid ester compound having a number average molecular weight (Mn) of 500 to 1,500.

[0013] Furthermore, the present inventors have conducted studies to achieve the above object, and have found that the above problem can also be solved by incorporating an additive having a polydiene structure and a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g in a toner for developing electrostatic images, which contains colored resin particles including a binder resin, a colorant, a charge control agent, and a release agent, into the colored resin particles, and by controlling the number of crystal domains of the release agent, which have an aspect ratio in the range of 2 to 10, in the colored resin particles to be within a specific range, thereby completing the present invention. Further, the present inventors have conducted further studies and have found that, in a toner for developing electrostatic images containing colored resin particles including a binder resin, a colorant, a charge control agent, and a release agent, an additive having a polydiene structure and a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g is contained in the colored resin particles as an additive, and the storage modulus G'(60) of the colored resin particles at 60° C., as determined by dynamic viscoelasticity measurement, is 1.6×10 8 ~5.0×10 8 It has been found that the above problem can be solved by controlling the pressure within the Pa range. That is, according to the present invention, there is provided a toner for developing electrostatic images according to a first aspect, which comprises a binder resin, a colorant, a charge control agent, a release agent, and colored resin particles containing an additive having a polydiene structure, the additive having a polydiene structure has a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g; The toner for developing electrostatic images is provided, in which, when a cross section of the colored resin particle is observed with a transmission electron microscope (TEM), the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 within a field of view of 2 μm × 2 μm on the cross section of the colored resin particle is 2 to 30.

[0014] Alternatively, according to the present invention, there is provided a toner for developing electrostatic images according to a second aspect, which comprises a binder resin, a colorant, a charge control agent, a release agent, and colored resin particles containing an additive having a polydiene structure, the additive having a polydiene structure has a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g; The storage modulus G'(60) of the colored resin particles at 60°C determined by dynamic viscoelasticity measurement is 1.6 x 10 8 ~5.0×10 8 A toner for developing electrostatic images having a viscosity of 10 Pa is provided.

[0015] In the toner for developing electrostatic images according to the second aspect of the present invention, the storage modulus G'(100) of the colored resin particles at 100°C determined by dynamic viscoelasticity measurement is 1.0 x 10 5 ~3.0×10 5 It is preferred that the value is Pa. In the toner for developing electrostatic images according to the second aspect of the present invention, the ratio G'(60) / G'(100) of the storage modulus G'(60) at 60° C. to the storage modulus G'(100) at 100° C. of the colored resin particles, which is determined by dynamic viscoelasticity measurement, is 1.0×10 3 ~5.0×10 3 It is preferable that:

[0016] In the toner for developing electrostatic images of the present invention, the additive having a polydiene structure is preferably an aromatic vinyl thermoplastic elastomer. Alternatively, in the toner for developing electrostatic images of the present invention, the conjugated diene-aromatic vinyl thermoplastic elastomer is preferably a conjugated diene-aromatic vinyl thermoplastic elastomer containing 40 mass % or more of a diblock copolymer consisting of an aromatic vinyl polymer block and a block of a polymer copolymerizable with the aromatic vinyl polymer. In the electrostatic image developing toner of the present invention, the content of aromatic vinyl monomer units in the conjugated diene-aromatic vinyl thermoplastic elastomer is preferably 10 to 30% by mass based on the total monomer units. In the toner for developing electrostatic images of the present invention, the content of the additive having a polydiene structure is preferably 1 to 10 parts by mass with respect to 100 parts by mass of the binder resin. Furthermore, in the electrostatic image developing toner of the present invention, the release agent is preferably a fatty acid ester compound having a number average molecular weight (Mn) of 500 to 1,500. Effect of the Invention

[0017] According to the present invention, it is possible to provide a toner for developing electrostatic images, which has excellent storage stability and low-temperature fixing ability. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1(A) is a transmission electron microscope (TEM) photograph of a cross section of a colored resin particle in Example 1-1, and FIG. 1(B) is a transmission electron microscope (TEM) photograph of a cross section of a colored resin particle in Comparative Example 1-1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] <Toner for Developing Electrostatic Charge Images According to a First Aspect> The toner for developing electrostatic images according to a first aspect of the present invention (hereinafter, may be simply referred to as "toner") is a toner for developing electrostatic images, which contains a binder resin, a colorant, a charge control agent, a release agent, and colored resin particles containing an additive having a polydiene structure, the additive having a polydiene structure has a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g; When the cross section of the colored resin particle is observed with a transmission electron microscope (TEM), the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 in a field of view of 2 μm × 2 μm square on the cross section of the colored resin particle is in the range of 2 to 30.

[0020] First, a method for producing the colored resin particles constituting the toner according to the first aspect of the present invention will be described.

[0021] The manufacturing methods of the colored resin particles constituting the toner according to the first aspect of the present invention are roughly divided into dry methods such as pulverization methods and wet methods such as emulsion polymerization aggregation methods, dispersion polymerization methods, suspension polymerization methods and dissolution suspension methods, with the wet methods being preferred since they are more likely to produce toners with excellent printing characteristics such as image reproducibility. Among the wet methods, polymerization methods such as emulsion polymerization aggregation methods, dispersion polymerization methods and suspension polymerization methods are more preferred since they are more likely to produce toners with a relatively small particle size distribution on the order of microns, with the suspension polymerization method being more preferred among these.

[0022] The emulsion polymerization aggregation method is a method for producing colored resin particles by polymerizing an emulsified polymerizable monomer to obtain resin fine particles, and aggregating the resin fine particles with a colorant, etc. The dissolution suspension method is a method for producing colored resin particles by dropping a solution in which toner components such as a binder resin and a colorant are dissolved or dispersed in an organic solvent into an aqueous medium to form droplets, and then removing the organic solvent, and each of these methods can be known.

[0023] The colored resin particles constituting the toner according to the first aspect of the present invention can be produced by either a wet method or a dry method, but when the colored resin particles are produced by adopting the (A) suspension polymerization method, which is preferable among the wet methods, or the (B) pulverization method, which is representative among the dry methods, the process is as follows. First, the (A) suspension polymerization method will be described.

[0024] (A) Suspension polymerization method (A-1) Preparation of polymerizable monomer composition In the suspension polymerization method, first, a polymerizable monomer, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure, as well as other additives used as necessary, are mixed and dissolved to prepare a polymerizable monomer composition. The mixing for preparing the polymerizable monomer composition is carried out, for example, using a media type disperser.

[0025] In the present invention, the polymerizable monomer refers to a compound that can be polymerized, and the polymerizable monomer becomes a binder resin by polymerization. As the polymerizable monomer, it is preferable to use a monovinyl monomer as a main component constituting the polymerizable monomer. Examples of the monovinyl monomer include styrene-based monomers such as styrene, vinyl toluene, α-methylstyrene, and ethylstyrene; (meth)acrylate-based monomers such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, dimethylaminoethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and dimethylaminoethyl methacrylate; acrylic acid and methacrylic acid; nitrile compounds such as acrylonitrile and methacrylonitrile; amide compounds such as acrylamide and methacrylamide; and olefins such as ethylene, propylene, and butylene. These monovinyl monomers can be used alone or in combination of two or more. Among these, styrene-based monomers and (meth)acrylate-based monomers are preferred, and styrene and butyl acrylate are more preferred. In addition, it is preferred to use at least a styrene-based monomer and a (meth)acrylate-based monomer as the monovinyl monomer, since the low-temperature fixing property of the resulting toner can be further improved.

[0026] The content of the styrene monomer unit in the binder resin used in the present invention is preferably 60% by mass or more, more preferably 65% ​​by mass or more, even more preferably 68% by mass or more, and particularly preferably 70% by mass or more, and the upper limit is preferably 85% by mass or less, more preferably 80% by mass or less, even more preferably 77% by mass or less, and particularly preferably 74% by mass or less. The content of the (meth)acrylate monomer unit is preferably 20% by mass or more, more preferably 21% by mass or more, even more preferably 21.5% by mass or more, even more preferably 22% by mass or more, and particularly preferably 24% by mass or more, and the upper limit is preferably 40% by mass or less, more preferably 35% by mass or less, even more preferably 32% by mass or less, even more preferably 30% by mass or less, particularly preferably 28% by mass or less, and most preferably 26% by mass or less. By setting the content of the styrene monomer unit and the (meth)acrylate monomer unit in the above range, the obtained toner can be improved in low-temperature fixability while having excellent storage stability.

[0027] In the present invention, in order to improve hot offset and storage stability, it is preferable to use any crosslinkable polymerizable monomer together with the monovinyl monomer. The crosslinkable polymerizable monomer refers to a monomer having two or more polymerizable functional groups. Examples of the crosslinkable polymerizable monomer include aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof; ester compounds in which two or more carboxylic acids are ester-bonded to an alcohol having two or more hydroxyl groups, such as ethylene glycol dimethacrylate and diethylene glycol dimethacrylate; other divinyl compounds such as N,N-divinylaniline and divinyl ether; and compounds having three or more vinyl groups. These crosslinkable polymerizable monomers can be used alone or in combination of two or more. The amount of the crosslinkable polymerizable monomer used is preferably 0.1 to 5 parts by mass, more preferably 0.15 to 2 parts by mass, and even more preferably 0.2 to 0.7 parts by mass, relative to 100 parts by mass of the monovinyl monomer, and the content of the crosslinkable polymerizable monomer unit in the binder resin used in the present invention is preferably 0.1 to 5% by mass, more preferably 0.15 to 2% by mass, and even more preferably 0.2 to 0.7% by mass. By setting the amount and content of the crosslinkable polymerizable monomer within the above ranges, the storage stability and low-temperature fixability of the obtained toner can be further improved.

[0028] In addition, when a macromonomer is used as a part of the polymerizable monomer, the storage stability and low-temperature fixability of the obtained toner can be further improved, so it is preferable to use any macromonomer. A macromonomer is a reactive oligomer or polymer having a polymerizable carbon-carbon unsaturated bond at the end of the molecular chain, and usually has a number average molecular weight (Mn) of 1,000 to 30,000. It is preferable that the macromonomer gives a polymer having a higher Tg (glass transition temperature) than the Tg of a polymer obtained without polymerizing the macromonomer. The amount of the macromonomer used is preferably 0.03 to 5 parts by mass, more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the monovinyl monomer.

[0029] In the present invention, a colorant is used, and when producing a color toner (usually, four types of toner are used: black toner, cyan toner, yellow toner, and magenta toner), a black colorant, a cyan colorant, a yellow colorant, and a magenta colorant can be used, respectively.

[0030] As the black colorant, for example, pigments and dyes such as carbon black, titanium black, and magnetic powders such as zinc iron oxide and nickel iron oxide can be used.

[0031] Examples of cyan colorants include copper phthalocyanine pigments, their derivatives, and anthraquinone pigments and dyes. Specific examples include CI Pigment Blue 2, 3, 6, 15, 15:1, 15:2, 15:3, 15:4, 16, 17:1, 60, etc.

[0032] Examples of the yellow colorant include azo pigments such as monoazo pigments and disazo pigments, condensed polycyclic pigments, dyes, and other compounds. Specific examples include CI Pigment Yellow 3, 12, 13, 14, 15, 17, 62, 65, 73, 74, 83, 93, 97, 120, 138, 151, 155, 180, 181, 185, 186, 214, 219, CI Solvent Yellow 98, 162, and the like.

[0033] Examples of magenta colorants include monoazo pigments, azo pigments such as disazo pigments, condensed polycyclic pigments, dyes, and other compounds. Specific examples include CI Pigment Red 31, 48, 57:1, 58, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 144, 146, 149, 150, 163, 170, 184, 185, 187, 202, 206, 207, 209, 251, CI Solvent Violet 31, 47, 59, and CI Pigment Violet 19.

[0034] In the present invention, each colorant may be used alone or in combination of two or more kinds, and the amount of the colorant used is preferably 1 to 10 parts by mass based on 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0035] The charge control agent is not particularly limited as long as it is one that is generally used as a charge control agent for toners. Among the charge control agents, positively or negatively charged charge control resins are preferred from the viewpoint of having high compatibility with polymerizable monomers and being able to impart stable chargeability (charge stability) to toner particles, thereby improving the dispersibility of the colorant. Furthermore, from the viewpoint of obtaining a negatively charged toner, negatively charged charge control resins are more preferably used.

[0036] Positively charged charge control agents include nigrosine dyes, quaternary ammonium salts, triaminotriphenylmethane compounds, and imidazole compounds, as well as polyamine resins, quaternary ammonium group-containing copolymers, and quaternary ammonium base-containing copolymers, which are preferably used as charge control resins.

[0037] Examples of negatively chargeable charge control agents include azo dyes containing metals such as Cr, Co, Al, and Fe, metal salicylate compounds, and metal alkylsalicylate compounds, as well as sulfonic acid group-containing copolymers, sulfonate salt group-containing copolymers, carboxylate group-containing copolymers, and carboxylate salt group-containing copolymers, which are preferably used as charge control resins.

[0038] The weight average molecular weight (Mw) of the charge control resin is in the range of 5,000 to 30,000, preferably in the range of 8,000 to 25,000, and more preferably in the range of 10,000 to 20,000, in terms of polystyrene, measured by gel permeation chromatography (GPC) using tetrahydrofuran.

[0039] Furthermore, the copolymerization ratio of the monomer having a functional group such as a quaternary ammonium group or a sulfonate group in the charge control resin is preferably within the range of 0.5 to 12 mass%, more preferably within the range of 1.0 to 6 mass%, and even more preferably within the range of 1.5 to 3 mass%.

[0040] The content of the charge control agent is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 8 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the amount of the charge control agent added within the above range, it is possible to effectively suppress the occurrence of fog and print stains while appropriately increasing the dispersibility of the colorant.

[0041] The release agent can be any one that is generally used as a toner release agent without any particular limitations, but from the viewpoint of appropriately increasing the low-temperature fixing property of the resulting toner, it is preferable that the number average molecular weight (Mn) is 500 to 1500, and more preferably a fatty acid ester compound having a number average molecular weight (Mn) of 500 to 1500. The term "fatty acid ester compound" refers to a product of an ester reaction between a monohydric alcohol and / or a polyhydric alcohol and a saturated fatty acid and / or an unsaturated fatty acid.

[0042] Specific examples of monohydric alcohols include monohydric saturated aliphatic alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 1-pentanol, 1-hexanol, octanol, 2-ethyl-1-hexanol, nonyl alcohol, lauryl alcohol, cetyl alcohol, stearyl alcohol, and behenyl alcohol; monohydric unsaturated aliphatic alcohols such as allyl alcohol, methallyl alcohol, crotyl alcohol, and oleyl alcohol; monohydric alicyclic alcohols such as cyclohexanol; and monohydric aromatic alcohols such as phenol, phenylmethanol (benzyl alcohol), methylphenol (cresol), p-ethylphenol, dimethylphenol (xylenol), nonylphenol, dodecylphenol, phenylphenol, and naphthol.

[0043] Specific examples of polyhydric alcohols include dihydric saturated aliphatic alcohols such as ethylene glycol and propylene glycol; dihydric aromatic alcohols such as catechol and hydroquinone; and trihydric or higher saturated aliphatic alcohols such as glycerin, pentaerythritol, dipentaerythritol, and polyglycerin.

[0044] Among these monohydric alcohols and polyhydric alcohols, monohydric to tetrahydric saturated aliphatic alcohols are preferred, stearyl alcohol, behenyl alcohol and pentaerythritol are more preferred, stearyl alcohol and behenyl alcohol are more preferred, and behenyl alcohol is particularly preferred.

[0045] The fatty acid used as the raw material for the fatty acid ester compound is preferably a saturated fatty acid and / or an unsaturated fatty acid having a carbon number of 12 to 22, more preferably a carbon number of 14 to 18. Among them, the saturated fatty acid having the above carbon numbers is particularly preferred because it is easy to obtain a fatty acid ester compound having a number average molecular weight (Mn) of 500 to 1500.

[0046] Specific examples of saturated fatty acids having the above carbon numbers include, but are not limited to, lauric acid (carbon number 12), myristic acid (carbon number 14), pentadecylic acid (carbon number 15), palmitic acid (carbon number 16), margaric acid (carbon number 17), stearic acid (carbon number 18), arachidic acid (carbon number 20), and behenic acid (carbon number 22). Among these saturated fatty acids, stearic acid (carbon number 18), arachidic acid (carbon number 20), and behenic acid (carbon number 22) are preferred, and stearic acid (carbon number 18) is more preferred.

[0047] Specific examples of unsaturated fatty acids include, but are not limited to, the following compounds: Palmitoleic acid (CH3(CH2)5CH=CH(CH2)7COOH) Oleic acid (CH3(CH2)7CH=CH(CH2)7COOH) Vaccenic acid (CH3(CH2)5CH=CH(CH2)9COOH) Linoleic acid (CH3(CH2)3(CH2CH=CH)2(CH2)7COOH) (9,12,15)-Linolenic Acid (CH3(CH2CH=CH)3(CH2)7CO OH) (6,9,12)-Linolenic acid (CH3(CH2)3(CH2CH=CH)3(CH2)4COOH) Eleostearic acid (CH3(CH2)3(CH=CH)3(CH2)7COOH) Arachidonic acid (CH3(CH2)3(CH2CH=CH)4(CH2)3COOH)

[0048] The above-mentioned saturated fatty acids and / or unsaturated fatty acids may be used alone or in combination of two or more. Among the saturated fatty acids and unsaturated fatty acids, saturated fatty acids are preferred, stearic acid, arachidic acid and behenic acid are more preferred, stearic acid and behenic acid are even more preferred, and behenic acid is particularly preferred.

[0049] The fatty acid ester compounds as described above can be produced according to a conventional method. For example, a method of producing such fatty acid ester compounds includes a method of carrying out an ester reaction using a monohydric alcohol and / or a polyhydric alcohol and a saturated fatty acid and / or an unsaturated fatty acid. In addition, a commercially available fatty acid ester compound can be used as the fatty acid ester compound, and examples of the commercially available fatty acid ester compound include "WEP2", "WEP3", "WEP4", "WEP5", "WE6", and "WE11" (all of which are product names) manufactured by NOF Corporation.

[0050] In the present invention, instead of the above-mentioned fatty acid ester compound, or together with the fatty acid ester compound, a release agent other than a fatty acid ester compound may be used as the release agent, and examples thereof include low molecular weight polyolefin wax and modified wax thereof, natural plant wax such as jojoba, petroleum wax such as paraffin, mineral wax such as ozokerite, synthetic wax such as Fischer-Tropsch wax, polyhydric alcohol ester such as dipentaerythritol ester, etc. These may be used alone or in combination of two or more.

[0051] The number average molecular weight (Mn) of the release agent is preferably 500 to 1500, more preferably 550 to 1200, and further preferably 550 to 1100. The number average molecular weight (Mn) of the release agent can be measured, for example, in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran.

[0052] The content of the release agent is preferably 1 to 30 parts by mass, more preferably 8 to 28 parts by mass, and further preferably 12 to 25 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the content of the release agent within the above range, it is possible to further improve the low-temperature fixability while making the particle size distribution of the obtained toner relatively uniform.

[0053] In the present invention, the colored resin particles further contain an additive having a polydiene structure, the solubility of which in styrene at a temperature of 40° C. is 3 to 40 g / 100 g or more. In the present invention, by using such an additive having a polydiene structure, the release agent can be finely dispersed in the colored resin particles in a state in which it has a specific crystal domain structure due to the compatibility of the additive having a polydiene structure with the release agent. In the present invention, the release agent is finely dispersed in a state in which it has a specific crystal domain structure, and the effect of improving low-temperature fixability by adding the release agent can be sufficiently achieved while effectively suppressing blocking of the toner obtained, and as a result, the toner obtained can have excellent storage stability and low-temperature fixability.

[0054] The additive having a polydiene structure used in the present invention is not particularly limited as long as it has a polydiene structure (i.e., a structure derived from a diene compound) and has a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g. The solubility of the additive having a polydiene structure in styrene at a temperature of 40° C. is preferably 5 to 30 g / 100 g, more preferably 10 to 25 g / 100 g. If the solubility in styrene at a temperature of 40° C. is too low, the dispersibility in the colored resin particles decreases, which reduces the compatibility with the release agent, resulting in insufficient dispersion of the release agent. As a result, the low-temperature fixability and storage stability of the toner obtained decrease. On the other hand, if the solubility in styrene is too high, the release agent becomes compatible with the binder resin in the colored resin particles, making it impossible to form a crystal domain, and the low-temperature fixability and storage stability of the toner deteriorate.

[0055] The additive having a polydiene structure used in the present invention is not particularly limited, and examples thereof include conjugated diene-aromatic vinyl thermoplastic elastomers, which are polymers having structural units derived from a conjugated diene compound and structural units derived from an aromatic vinyl compound; conjugated diene elastomers such as polybutadiene rubber and polyisoprene rubber; and the like. Of these, conjugated diene-aromatic vinyl thermoplastic elastomers are preferred, and among the conjugated diene-aromatic vinyl thermoplastic elastomers, unhydrogenated conjugated diene-aromatic vinyl thermoplastic elastomers are particularly preferred.

[0056] The conjugated diene-aromatic vinyl thermoplastic elastomer used in the present invention as an additive having a polydiene structure has a polymerization-reactive unsaturated bond in its structure, and by having such a polymerization-reactive unsaturated bond, the polymerization-reactive unsaturated bond reacts with the binder resin, and the conjugated diene-aromatic vinyl thermoplastic elastomer interacts with the release agent while being fixed to the binder resin. This allows the release agent to be well finely dispersed in the binder resin constituting the colored resin particles, and as a result, the effect of improving low-temperature fixability by adding the release agent can be sufficiently achieved while effectively suppressing blocking of the toner obtained, and as a result, the toner obtained can have better storage stability and low-temperature fixability. In the present invention, the "polymerization-reactive unsaturated bond" means an unsaturated bond having polymerization activity, and preferably includes an olefinic carbon-carbon double bond having polymerization activity.

[0057] The conjugated diene-aromatic vinyl thermoplastic elastomer used in the present invention includes random, block, graft and other copolymers of a conjugated diene monomer, an aromatic vinyl monomer, and, if necessary, other monomers copolymerizable therewith, and hydrogenated products of such copolymers.

[0058] Such a conjugated diene-aromatic vinyl thermoplastic elastomer is not particularly limited, but from the viewpoint of further improving the storage stability and low-temperature fixing property of the toner, a block copolymer containing at least one aromatic vinyl polymer block and at least one conjugated diene polymer block can be preferably used.

[0059] Hereinafter, a block copolymer containing at least one aromatic vinyl polymer block and at least one conjugated diene polymer block (hereinafter, sometimes simply referred to as "block copolymer"), which is a representative example of a conjugated diene-aromatic vinyl thermoplastic elastomer, will be described. The block copolymer used in the present invention contains at least one aromatic vinyl polymer block obtained by polymerizing an aromatic vinyl monomer and at least one conjugated diene polymer block obtained by polymerizing a conjugated diene monomer.

[0060] The aromatic vinyl monomer is not particularly limited as long as it is an aromatic vinyl compound, and examples thereof include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, and vinylnaphthalene. Among these, it is preferable to use styrene. These aromatic vinyl monomers can be used alone or in combination of two or more in each aromatic vinyl polymer block. In addition, when the block copolymer has a plurality of aromatic vinyl polymer blocks, each aromatic vinyl polymer block may be composed of the same aromatic vinyl monomer unit or may be composed of different aromatic vinyl monomer units.

[0061] The aromatic vinyl polymer block may contain other monomer units as long as the aromatic vinyl monomer unit is the main repeating unit. Examples of other monomers that can be used in the aromatic vinyl polymer block include conjugated diene monomers such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene), α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or acid anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. The content of monomer units other than aromatic vinyl monomer units in the aromatic vinyl polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.

[0062] The conjugated diene monomer is not particularly limited as long as it is a conjugated diene compound, and examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. Among these, from the viewpoint of high effect of improving storage stability and low-temperature fixability, it is preferable to use 1,3-butadiene and / or isoprene, and it is particularly preferable to use isoprene. These conjugated diene monomers can be used alone or in combination of two or more in each conjugated diene polymer block. In addition, when the block copolymer has a plurality of conjugated diene polymer blocks, each conjugated diene polymer block may be composed of the same conjugated diene monomer unit or may be composed of different conjugated diene monomer units. Furthermore, a hydrogenation reaction may be performed on a part of the unsaturated bonds of each conjugated diene polymer block.

[0063] The conjugated diene polymer block may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. Examples of other monomers that can be used in the conjugated diene polymer block include aromatic vinyl monomers such as styrene and α-methylstyrene, α,β-unsaturated nitrile monomers, unsaturated carboxylic acid monomers, unsaturated carboxylic anhydride monomers, unsaturated carboxylic ester monomers, and non-conjugated diene monomers. The content of monomer units other than the conjugated diene monomer units in the conjugated diene polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.

[0064] The vinyl bond content of the conjugated diene polymer block (the ratio of 1,2-vinyl bond units and 3,4-vinyl bond units to all conjugated diene monomer units in the conjugated diene polymer block) is not particularly limited, but is preferably 1 to 20 mol%, more preferably 2 to 15 mol%, and particularly preferably 3 to 10 mol%.

[0065] The block copolymer is not particularly limited in the number of each polymer block and the bonding form thereof, so long as it contains at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. Specific examples of the block copolymer used in the present invention include the following. In the following specific examples, Ar represents an aromatic vinyl polymer block, D represents a conjugated diene polymer block, X represents a residue of a coupling agent, and n represents an integer of 2 or more. (a) Aromatic vinyl-conjugated diene block copolymer represented as Ar-D (b) Aromatic vinyl-conjugated diene-aromatic vinyl block copolymers represented as Ar-D-Ar and / or (Ar-D)nX (c) conjugated diene-vinyl aromatic-conjugated diene block copolymers represented as D-Ar-D and / or (D-Ar)nX (d) an aromatic vinyl-conjugated diene-aromatic vinyl-conjugated diene block copolymer represented as Ar-D-Ar-D; (e) A block copolymer composition comprising any combination of two or more of the above (a) to (d).

[0066] In the present invention, it is preferable to use a block copolymer containing at least the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D, and it is more preferable to use a block copolymer containing at least the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D and the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)nX. The content of the aromatic vinyl-conjugated diene block copolymer represented by Ar-D (i.e., a diblock copolymer consisting of an aromatic vinyl polymer block and a block of a polymer copolymerizable with the aromatic vinyl polymer) in the conjugated diene-aromatic vinyl thermoplastic elastomer used in the present invention is preferably 40% by mass (weight %) or more, preferably 50% by mass or more, and more preferably 55% by mass or more. The upper limit is not particularly limited, but is preferably 98% by mass or less, and more preferably 95% by mass or less. By controlling the content of the aromatic vinyl-conjugated diene block copolymer represented by Ar-D (i.e., a diblock copolymer consisting of an aromatic vinyl polymer block and a block of a polymer copolymerizable with the aromatic vinyl polymer) in the conjugated diene-aromatic vinyl thermoplastic elastomer used in the present invention to 40 mass % or more, the toner obtained has high chargeability, is suppressed in bleeding out of the release agent, and is effectively suppressed from jetting out and sticking to the blade under high temperature and high humidity conditions.

[0067] In the aromatic vinyl-conjugated diene block copolymer represented by Ar-D, the weight average molecular weight (Mw(Ar)) of the aromatic vinyl polymer block Ar is not particularly limited, but is preferably 10,000 to 50,000, more preferably 15,000 to 30,000, and the weight average molecular weight (Mw(D)) of the conjugated diene polymer block D is not particularly limited, but is preferably 50,000 to 200,000, more preferably 60,000 to 150,000.

[0068] In the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by Ar-D-Ar and / or (Ar-D)nX, the weight average molecular weight (Mw(Ar)) of the aromatic vinyl polymer block Ar is not particularly limited, but is preferably 20,000 to 70,000, more preferably 25,000 to 50,000, and the weight average molecular weight (Mw(D)) of the conjugated diene polymer block D is not particularly limited, but is preferably 100,000 to 300,000, more preferably 120,000 to 250,000. The weight average molecular weights are all values ​​calculated as polystyrene equivalents measured by gel permeation chromatography (GPC) using tetrahydrofuran.

[0069] In the block copolymer used in the present invention, the content ratio of aromatic vinyl monomer units to all monomer units is preferably 10 to 30 mass%, more preferably 12 to 25 mass%, and even more preferably 15 to 25 mass%. By setting the content ratio of aromatic vinyl monomer units within the above range, the affinity of the block copolymer to the release agent and the affinity of the block copolymer to the binder resin can be highly balanced, and the resulting toner can have excellent storage stability and low-temperature fixability.

[0070] In the case where all polymer components constituting the block copolymer are composed only of aromatic vinyl monomer units and conjugated diene monomer units, the content of aromatic vinyl monomer units in the block copolymer can be easily measured by subjecting the block copolymer to ozonolysis and then reduction with lithium aluminum hydride according to the method described in Rubber Chem. Technol., 45, 1295 (1972), whereby the conjugated diene monomer unit portion is decomposed and only the aromatic vinyl monomer unit portion can be isolated, so that the total aromatic vinyl monomer unit content can be easily measured.

[0071] The weight average molecular weight (Mw) of the aromatic vinyl monomer unit in the block copolymer is not particularly limited, but is preferably 10,000 to 50,000, more preferably 20,000 to 40,000, in terms of polystyrene measured by gel permeation chromatography (GPC) using tetrahydrofuran. The weight average molecular weight (Mw) of the conjugated diene monomer unit in the block copolymer is not particularly limited, but is preferably 50,000 to 200,000, more preferably 60,000 to 180,000.

[0072] The melt index (MI) of the block copolymer is not particularly limited, but is selected, for example, from the range of 1 to 1000 g / 10 min, and preferably from 5 to 30 g / 10 min, as a value measured in accordance with ASTM D-1238 (G condition, 200° C., 5 kg).

[0073] The block copolymer used in the present invention can be produced by a conventional method. For example, a method of producing such a block copolymer includes a method of sequentially polymerizing an aromatic vinyl monomer and a conjugated diene monomer by an anionic living polymerization method to form a polymer block, and then reacting a coupling agent to perform coupling, if necessary.

[0074] In addition, when the block copolymer used in the present invention contains at least the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D and the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)X, the following method can be adopted.

[0075] That is, first, an aromatic vinyl monomer is polymerized by an anionic living polymerization method, and then a conjugated diene monomer is added and polymerized to obtain a diblock copolymer having an active end. Next, a coupling agent less than 1 molar equivalent is added to the active end of the diblock copolymer having an active end, and a part of the diblock copolymer having an active end is subjected to a coupling reaction to obtain an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented as (Ar-D)nX, and then a polymerization terminator is added to inactivate the remaining diblock copolymer having an active end to obtain a diblock copolymer represented as Ar-D. In this case, a bifunctional coupling agent such as dichlorosilane, monomethyldichlorosilane, dimethyldichlorosilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dichloroethane, dibromoethane, methylene chloride, and dibromomethane can be used as the coupling agent to obtain an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented as Ar-D-Ar (D includes a residue of the coupling agent).

[0076] In the present invention, the content ratio of the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D and the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)nX is not particularly limited, but the content ratio of the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D is preferably 10 to 90 mass%, more preferably 20 to 80 mass%. Also, the content ratio of the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)nX is preferably 10 to 90 mass%, more preferably 20 to 80 mass%.

[0077] In addition, as the conjugated diene-aromatic vinyl thermoplastic elastomer, a random copolymer of an aromatic vinyl monomer and a conjugated diene monomer can be used instead of the above-mentioned block copolymer. The random copolymer of an aromatic vinyl monomer and a conjugated diene monomer can be produced by living anionic polymerization using, for example, an organic alkali metal compound as a polymerization initiator. Examples of the organic alkali metal compound include organic lithium compounds, organic sodium compounds, and organic potassium compounds. Specifically, organic monolithium compounds such as n-butyl lithium, sec-butyl lithium, t-butyl lithium, hexyl lithium, phenyl lithium, and stilbene lithium; organic polyvalent lithium compounds such as dilithiomethane, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, 1,3,5-trilithiobenzene, and 1,3,5-tris(lithiomethyl)benzene; organic sodium compounds such as sodium naphthalene; and organic potassium compounds such as potassium naphthalene. Among these organic metal compounds, n-butyl lithium is preferably used.

[0078] In the random copolymer of aromatic vinyl monomer and conjugated diene monomer used in the present invention, the content ratio of aromatic vinyl monomer units to all monomer units is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. By setting the content ratio of aromatic vinyl monomer units within the above range, the affinity of the random copolymer to the release agent and the affinity of the block copolymer to the binder resin can be highly balanced, and the resulting toner can have excellent storage stability and low-temperature fixability.

[0079] Furthermore, in the present invention, conjugated diene elastomers such as polybutadiene rubber and polyisoprene rubber can also be suitably used as additives having a polydiene structure. Conjugated diene elastomers such as polybutadiene rubber and polyisoprene rubber can be produced, for example, by living anionic polymerization using an organic alkali metal compound as a polymerization initiator. As the organic alkali metal compound, for example, the above-mentioned compounds can be used.

[0080] The weight average molecular weight (Mw) of the additive having a polydiene structure used in the present invention is not particularly limited, but is preferably 60,000 to 350,000, more preferably 80,000 to 250,000, in terms of polystyrene measured by gel permeation chromatography (GPC) using tetrahydrofuran. By setting the weight average molecular weight (Mw) within the above range, the storage stability and low-temperature fixability of the obtained toner can be further improved.

[0081] The content of the additive having a polydiene structure is preferably 1 to 10 parts by mass, more preferably 1.5 to 8 parts by mass, and even more preferably 2 to 5 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the content of the additive having a polydiene structure within the above range, the effect of adding the additive, i.e., the effect of improving the storage stability and low-temperature fixability of the toner obtained, can be further enhanced.

[0082] In the present invention, an acrylic resin can be used as another additive in order to further suppress bleeding out of the release agent. The acrylic resin is a copolymer (acrylate copolymer) mainly composed of at least one of an acrylic acid ester and a methacrylic acid ester and at least one of an acrylic acid and a methacrylic acid. The acid monomer is preferably acrylic acid.

[0083] Examples of the acrylic resin include copolymers of an acrylic acid ester and acrylic acid, copolymers of an acrylic acid ester and methacrylic acid, copolymers of a methacrylic acid ester and acrylic acid, copolymers of a methacrylic acid ester and methacrylic acid, copolymers of an acrylic acid ester, a methacrylic acid ester and acrylic acid, copolymers of an acrylic acid ester, a methacrylic acid ester and methacrylic acid, and copolymers of an acrylic acid ester, a methacrylic acid ester, an acrylic acid and a methacrylic acid. Of these, it is preferable to use a copolymer of an acrylic acid ester, a methacrylic acid ester and acrylic acid.

[0084] The acid value of the acrylic resin is usually 0.5 to 7 mgKOH / g, preferably 1 to 6 mgKOH / g, and more preferably 1.5 to 4 mgKOH / g. By setting the acid value of the acrylic resin within the above range, it is possible to satisfactorily prepare desired colored resin particles, while improving heat-resistant storage stability, low-temperature fixability, and print durability under temperature and humidity environments ranging from low-temperature and low-humidity environments to high-temperature and high-humidity environments. The acid value of the acrylic resin is a value measured in accordance with JIS K 0070, a standard method for analyzing fats and oils established by the Japanese Industrial Standards Committee (JICS).

[0085] The weight average molecular weight (Mw) of the acrylic resin is usually from 6,000 to 50,000, preferably from 8,000 to 25,000, and more preferably from 10,000 to 20,000. When the weight average molecular weight (Mw) of the acrylic resin is within the above range, the heat-resistant storage stability, durability, and low-temperature fixability can be improved.

[0086] The glass transition temperature Tg of the acrylic resin is usually 60 to 85° C., preferably 65 to 80° C., and more preferably 70 to 77° C. When the glass transition temperature is in the above range, the heat-resistant storage stability and low-temperature fixability can be improved. The glass transition temperature Tg of the acrylic resin can be determined, for example, in accordance with ASTM D3418-82.

[0087] The ratio of the acrylic acid ester monomer units, the methacrylic acid ester monomer units, the acrylic acid monomer units, and the methacrylic acid monomer units in the acrylic resin is not particularly limited as long as the above-mentioned acid value, weight average molecular weight Mw, and glass transition temperature are satisfied.

[0088] The ratio of the above four types of monomer units can be adjusted by the mass ratio of the amounts of acrylic acid ester, methacrylic acid ester, acrylic acid, and methacrylic acid added during copolymer synthesis. The mass ratio of the amounts added may be, for example, (acrylic acid ester and / or methacrylic acid ester):(acrylic acid and / or methacrylic acid)=(99-99.95):(0.05-1), preferably (acrylic acid ester and / or methacrylic acid ester):(acrylic acid and / or methacrylic acid)=(99.4-99.9):(0.1-0.6), and more preferably (acrylic acid ester and / or methacrylic acid ester):(acrylic acid and / or methacrylic acid)=(99.5-99.7):(0.3-0.5). Among these polymerizable monomers, the acrylic acid esters and / or methacrylic acid esters may be substituted with other monomers such as styrene derivatives, nitrile compounds, and amide compounds exemplified as the monovinyl monomers constituting the binder resin, within the scope of not impairing the effects of the present invention. The proportion of such monomers is 10% by mass or less, preferably 2% by mass or less, of the total amount of the acrylic acid esters and / or methacrylic acid esters added, and it is preferable that they are not substituted.

[0089] Examples of acrylic esters used in the acrylic resin include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-pentyl acrylate, sec-pentyl acrylate, isopentyl acrylate, neopentyl acrylate, n-hexyl acrylate, isohexyl acrylate, neohexyl acrylate, sec-hexyl acrylate, and tert-hexyl acrylate, and among these, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and n-butyl acrylate are preferred, and n-butyl acrylate is more preferred.

[0090] Examples of methacrylic acid esters used in acrylic resins include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, sec-pentyl methacrylate, isopentyl methacrylate, neopentyl methacrylate, n-hexyl methacrylate, isohexyl methacrylate, neohexyl methacrylate, sec-hexyl methacrylate, and tert-hexyl methacrylate, and among these, methyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, and n-butyl methacrylate are preferred, and methyl methacrylate is more preferred.

[0091] The amount of the acrylic resin added is preferably 0.3 to 4 parts by mass, more preferably 0.5 to 3.0 parts by mass, and even more preferably 0.7 to 2.0 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the amount of the acrylic resin added within the above range, it is possible to obtain a sufficient effect of adding the acrylic resin while improving the environmental stability.

[0092] Although commercially available acrylic resins can be used, the acrylic resins can be produced by known methods such as solution polymerization, aqueous solution polymerization, ionic polymerization, high-temperature high-pressure polymerization, and suspension polymerization.

[0093] Furthermore, a molecular weight regulator may be used as another additive. The molecular weight regulator is not particularly limited as long as it is generally used as a molecular weight regulator for toners, and examples thereof include mercaptans such as t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, and 2,2,4,6,6-pentamethylheptane-4-thiol; and thiuram disulfides such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, N,N'-dimethyl-N,N'-diphenylthiuram disulfide, and N,N'-dioctadecyl-N,N'-diisopropylthiuram disulfide. These molecular weight regulators may be used alone or in combination of two or more kinds. The amount of the molecular weight regulator used is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0094] (A-2) Suspension step for obtaining a suspension (droplet formation step) Next, the polymerizable monomer composition containing the polymerizable monomer, colorant, charge control agent, release agent, and additive having a polydiene structure obtained by the above-mentioned (A-1) polymerizable monomer composition preparation step is dispersed in an aqueous dispersion medium, a polymerization initiator is added, and then droplets of the polymerizable monomer composition are formed. Here, suspension means that droplets of the polymerizable monomer composition are formed in an aqueous dispersion medium. The dispersion process for forming droplets can be performed using a device capable of strong stirring, such as an in-line type emulsifying and dispersing machine (manufactured by Pacific Machinery Works, product name: Milder) or a high-speed emulsifying and dispersing machine (manufactured by Primix Corporation, product name: TK Homomixer MARK II type).

[0095] Examples of the polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; azo compounds such as 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide), 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobisisobutyronitrile; and organic peroxides such as di-t-butyl peroxide, benzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylbutanoate, diisopropylperoxydicarbonate, di-t-butylperoxyisophthalate, and t-butylperoxyisobutyrate. These can be used alone or in combination of two or more. Among these, organic peroxides are preferred because they can reduce the amount of residual polymerizable monomers and have excellent print durability. Among organic peroxides, peroxyesters are preferred because they have good initiator efficiency and can reduce the amount of residual polymerizable monomers, and non-aromatic peroxyesters, i.e., peroxyesters without an aromatic ring, are more preferred.

[0096] As described above, the polymerization initiator may be added after the polymerizable monomer composition is dispersed in an aqueous medium and before droplets are formed, or may be added to the polymerizable monomer composition before it is dispersed in an aqueous medium (a medium mainly composed of water).

[0097] The amount of the polymerization initiator used for polymerization of the polymerizable monomer composition is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and particularly preferably 1 to 10 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0098] In the present invention, it is preferable to add a dispersion stabilizer to the aqueous medium. Examples of the dispersion stabilizer include inorganic compounds such as sulfates such as barium sulfate and calcium sulfate; carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates such as calcium phosphate; metal oxides such as aluminum oxide and titanium oxide; metal hydroxides such as aluminum hydroxide, magnesium hydroxide, and ferric hydroxide; and organic compounds such as water-soluble polymers such as polyvinyl alcohol, methyl cellulose, and gelatin; anionic surfactants; nonionic surfactants; and amphoteric surfactants. The dispersion stabilizers can be used alone or in combination of two or more. The amount of the dispersion stabilizer added is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 10 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0099] Among the above dispersion stabilizers, inorganic compounds, particularly colloids of poorly water-soluble metal hydroxides, are preferred. By using an inorganic compound, particularly colloids of poorly water-soluble metal hydroxides, the particle size distribution of the colored resin particles can be narrowed and the amount of the dispersion stabilizer remaining after washing can be reduced, so that the environmental stability is not deteriorated and the reproduction of images by the obtained toner can be made clearer.

[0100] (A-3) Polymerization process The desired suspension (aqueous dispersion medium containing droplets of the polymerizable monomer composition) obtained in the above (A-2) step of obtaining a suspension (droplet forming step) is heated to initiate polymerization, thereby obtaining an aqueous dispersion of colored resin particles containing a binder resin, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure.

[0101] The polymerization temperature in the present invention is preferably 50° C. or higher, and more preferably from 60 to 95° C. The polymerization time in the present invention is preferably from 1 to 20 hours, and more preferably from 2 to 15 hours.

[0102] From the viewpoint of carrying out polymerization in a state in which droplets of the polymerizable monomer composition are stably dispersed, in the polymerization step, following the step of obtaining the suspension (A-2) (droplet formation step), the polymerization reaction may be allowed to proceed while carrying out a dispersion treatment by stirring.

[0103] In the present invention, the thus obtained colored resin particles may be used as a toner by adding an external additive as it is, but the colored resin particles obtained by the polymerization process may be used as a core layer, and a shell layer different from the core layer may be formed on the outside of the core layer to obtain so-called core-shell type (also called "capsule type") colored resin particles. The core-shell type colored resin particles can further improve the storage stability and low-temperature fixability of the obtained toner by covering the core layer made of a material with a low softening point with a material with a higher softening point.

[0104] The method for producing the core-shell type colored resin particles is not particularly limited and may be any conventionally known method, but in situ polymerization method or phase separation method is preferred from the viewpoint of production efficiency.

[0105] A method for producing core-shell type colored resin particles by in situ polymerization will be described below. In the in situ polymerization method, a polymerizable monomer for forming a shell layer (polymerizable monomer for shell) and a polymerization initiator for the shell are added to an aqueous dispersion medium in which colored resin particles are dispersed, and polymerization is carried out to obtain core-shell type colored resin particles.

[0106] As the polymerizable monomer for the shell, the same polymerizable monomers as those mentioned above can be used. Among them, it is preferable to use a monomer that can give a polymer with a Tg of more than 80° C., such as styrene or methyl methacrylate, either alone or in combination of two or more kinds.

[0107] Examples of the polymerization initiator for the shell used in the polymerization of the polymerizable monomer for the shell include metal persulfates such as potassium persulfate and ammonium persulfate; and water-soluble azo compounds such as 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide) and 2,2'-azobis-(2-methyl-N-(1,1-bis(hydroxymethyl)2-hydroxyethyl)propionamide). The amount of the polymerization initiator for the shell used is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the polymerizable monomer for the shell.

[0108] The polymerization temperature for the shell layer is preferably 50° C. or higher, more preferably 60 to 95° C. The polymerization time for the shell layer is preferably 1 to 20 hours, more preferably 2 to 15 hours.

[0109] (A-4) Washing, filtering, dehydrating, and drying steps After the polymerization is completed, the aqueous dispersion of colored resin particles obtained in the above polymerization step (A-3) is preferably subjected to a series of operations of washing, filtering, dehydrating, and drying in a conventional manner, and if necessary, repeated several times.

[0110] First, in order to remove the dispersion stabilizer remaining in the aqueous dispersion of the colored resin particles, it is preferable to add an acid or an alkali to the aqueous dispersion of the colored resin particles and wash it. When the dispersion stabilizer used is an inorganic compound soluble in acid, it is preferable to add an acid to the aqueous dispersion of the colored resin particles and wash it, while when the dispersion stabilizer used is an inorganic compound soluble in alkali, it is preferable to add an alkali to the aqueous dispersion of the colored resin particles and wash it.

[0111] Furthermore, when an acid-soluble inorganic compound is used as the dispersion stabilizer, it is preferable to add an acid to the aqueous dispersion of the colored resin particles to adjust the pH to preferably 6.5 or less, more preferably 6 or less. The acid to be added may be an inorganic acid such as sulfuric acid, hydrochloric acid, or nitric acid, or an organic acid such as formic acid or acetic acid, but sulfuric acid is particularly preferable because it has a high efficiency of removing the dispersion stabilizer and places a small burden on the production equipment.

[0112] The dehydration and filtration methods can be any of various known methods, and are not particularly limited. For example, centrifugal filtration, vacuum filtration, pressure filtration, etc. The drying method is also not particularly limited, and various methods can be used.

[0113] (B) Crushing method When the colored resin particles are produced by the pulverization method, the process is as follows. First, the binder resin, the colorant, the charge control agent, the release agent, and the additive having a polydiene structure, as well as other additives added as necessary, are mixed using a mixer, such as a ball mill, a V-type mixer, a Henschel mixer (trade name), a high-speed dissolver, an internal mixer, a Forberg, etc. Next, the mixture obtained above is kneaded while being heated using a pressure kneader, a twin-screw extrusion kneader, a roller, etc. The kneaded product obtained is coarsely pulverized using a pulverizer such as a hammer mill, a cutter mill, or a roller mill. Furthermore, after finely pulverizing using a pulverizer such as a jet mill or a high-speed rotary pulverizer, the particles are classified into the desired particle size using a classifier such as an air classifier or an airflow classifier, and colored resin particles can be obtained by a pulverization method.

[0114] The binder resin, colorant, charge control agent, release agent, and additive having a polydiene structure used in the pulverization method, as well as other additives added as necessary, may be the same as those listed in the suspension polymerization method (A) above. The colored resin particles obtained by the pulverization method may also be made into core-shell type colored resin particles by a method such as in situ polymerization, like the colored resin particles obtained by the suspension polymerization method (A) above.

[0115] In addition to the above-mentioned binder resins, resins that have been widely used in toners can be used as the binder resin. Specific examples of the binder resin used in the pulverization method include polystyrene, styrene-butyl acrylate copolymer, polyester resin, and epoxy resin.

[0116] (Colored resin particles) The colored resin particles can be obtained by the above-mentioned (A) suspension polymerization method or (B) pulverization method. The colored resin particles constituting the toner will be described below. The colored resin particles described below include both core-shell type and non-core-shell type particles.

[0117] The colored resin particles used in the first aspect of the present invention are those containing a specific number of crystal domains of a release agent contained in the colored resin particles, each having a specific shape. That is, when the cross section of the colored resin particles is observed with a transmission electron microscope (TEM), the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 in a 2 μm×2 μm square field of view of the cross section of the colored resin particles is in the range of 2 to 30. In the first aspect of the present invention, the release agent contained in the colored resin particles is finely dispersed in a state having a crystal domain structure with an aspect ratio of 2 to 10, and the number of domains is in the range of 2 to 30 in a 2 μm×2 μm square field of view, thereby effectively suppressing blocking of the toner obtained, and sufficiently improving the low-temperature fixability by adding the release agent. As a result, the toner obtained can be excellent in storage stability and low-temperature fixability.

[0118] The number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 in a 2 μm × 2 μm square field of view is 2 to 30, preferably 3 to 27, and more preferably 5 to 25. In the first aspect of the present invention, the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 may be within the above range, but from the viewpoint of further enhancing the effects of the present invention, it is preferable that the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8 in a 2 μm × 2 μm square field of view is also within the above range.

[0119] The number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 and the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8 in a 2 μm×2 μm square field of view can be measured, for example, by the following method. That is, first, colored resin particles are dispersed in an epoxy resin and cured, cooled to a temperature of -80°C, and then cut with a microtome to prepare a thin slice. Then, the thin slice is stained with a vapor of an aqueous solution of ruthenium tetroxide and observed with a transmission electron microscope (TEM), and the number of crystal domains of the release agent and the aspect ratio of the crystal domains of the release agent present in a 2 μm×2 μm square field of view of the cross section of the colored resin particle are calculated by image analysis. Then, the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 and the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8 can be obtained. In these measurements, a visual field that is sufficiently wider than 2 μm × 2 μm square (for example, a visual field in which the cross sections of 5 or more colored resin particles can be observed) is observed, and within that visual field, the number of crystalline domains of the release agent having an aspect ratio in the range of 2 to 10 and the number of crystalline domains of the release agent having an aspect ratio in the range of 3 to 8 in the observed colored resin particles are calculated, and the calculation results are converted into the number within a visual field of 2 μm × 2 μm square, which can be used as the measured value.

[0120] The method for controlling the number of crystal domains of the release agent having an aspect ratio of 2 to 10 within the above range is not particularly limited, but includes a method of incorporating an additive having a polydiene structure in the colored resin particles. Specifically, by incorporating an additive having a polydiene structure, the release agent can be appropriately dispersed in the colored resin particles due to the compatibility of the additive having a polydiene structure with the release agent, and thus the number of crystal domains of the release agent having an aspect ratio of 2 to 10 can be controlled within the above range. In addition, in the first aspect of the present invention, the method for controlling the number of crystal domains of the release agent having an aspect ratio of 2 to 10 within the above range is not particularly limited, but includes a method of adjusting the type of additive having a polydiene structure used, the type of release agent used, the amount of additive having a polydiene structure used, and the amount of release agent used, and these may be combined.

[0121] The average aspect ratio of the crystal domains of the release agent contained in the colored resin particles is not particularly limited, but is preferably 2 to 10, more preferably 3 to 9, and even more preferably 3.5 to 8.5. The average major axis (average major axis) of the crystal domains of the release agent is preferably 0.20 to 1.0 μm, more preferably 0.25 to 0.90 μm, and the average minor axis (average minor axis) of the crystal domains of the release agent is preferably 0.03 to 0.15 μm, more preferably 0.04 to 0.10 μm. By setting the average aspect ratio, average major axis, and average minor axis of the crystal domains of the release agent within the above ranges, the effect of improving storage stability and low-temperature fixability can be further enhanced. The average aspect ratio, average major axis, and average minor axis of the crystal domains of the release agent can be determined by measuring the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 and the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8, measuring the aspect ratio, major axis, and minor axis of each of the crystal domains of the release agent measured, and calculating the average values ​​of all the crystal domains of the release agent measured.

[0122] From the viewpoint of image reproducibility, the volume average particle diameter Dv of the colored resin particles is preferably 3 to 15 μm, more preferably 4 to 12 μm, and further preferably 5 to 8 μm. If the volume average particle diameter Dv of the colored resin particles is less than the above range, the toner fluidity may decrease, and deterioration of image quality due to fogging or the like may easily occur. On the other hand, if the volume average particle diameter Dv of the colored resin particles exceeds the above range, the resolution of the obtained image may decrease.

[0123] In addition, the particle size distribution (Dv / Dn), which is the ratio of the volume average particle size (Dv) to the number average particle size (Dn) of the colored resin particles, is preferably 1.00 to 1.30, more preferably 1.00 to 1.20, from the viewpoint of image reproducibility. If the particle size distribution (Dv / Dn) of the colored resin particles exceeds the above range, the fluidity of the toner may decrease, and image quality may be easily deteriorated due to fogging or the like. The volume average particle size Dv and number average particle size Dn of the colored resin particles can be measured, for example, using a particle size analyzer (manufactured by Beckman Coulter, product name: Multisizer) or the like.

[0124] Moreover, the average circularity of the above-mentioned colored resin particles is preferably from 0.960 to 1.000, more preferably from 0.970 to 1.000, and even more preferably from 0.980 to 1.000, from the viewpoint of image reproducibility.

[0125] In addition, from the viewpoint of improving hot offset resistance and low-temperature fixability, the gel content (amount insoluble in tetrahydrofuran) of the above-mentioned colored resin particles is preferably 1 to 50% by weight, more preferably 5 to 47% by weight, even more preferably 10 to 45% by weight, and particularly preferably 15 to 40% by weight.

[0126] The weight average molecular weight (Mw) of the above-mentioned colored resin particles is preferably 20,000 to 200,000, more preferably 30,000 to 180,000, further preferably 35,000 to 150,000, and particularly preferably 40,000 to 90,000.

[0127] The above-mentioned colored resin particles may be used as a toner as is or by mixing the colored resin particles with carrier particles (ferrite, iron powder, etc.). In order to adjust the chargeability, fluidity, storage stability, etc. of the toner, an external additive may be added and mixed into the colored resin particles using a high-speed mixer (for example, FM Mixer (product name, manufactured by Nippon Coke & Engineering Co., Ltd.)) to form a one-component toner, or the colored resin particles, an external additive, and carrier particles may be mixed to form a two-component toner.

[0128] The agitator used for the external addition treatment is not particularly limited as long as it is a stirring device that can adhere an external additive to the surface of the colored resin particles, and the external addition treatment can be performed using an agitator capable of mixing and stirring, such as FM Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.), Super Mixer (product name, manufactured by Kawada Manufacturing Co., Ltd.), Q Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.), Mechanofusion System (product name, manufactured by Hosokawa Micron Corporation), or Mechano Mill (product name, manufactured by Okada Seiko Co., Ltd.).

[0129] Examples of the external additive include inorganic fine particles made of silica, titanium oxide, aluminum oxide, zinc oxide, tin oxide, calcium carbonate, calcium phosphate, and cerium oxide; and organic fine particles made of polymethyl methacrylate resin, silicone resin, and melamine resin. Among these, inorganic fine particles are preferred, silica and titanium oxide are more preferred, and silica is particularly preferred. In addition, it is preferred to use two or more types of fine particles in combination as the external additive. Although each of these external additives can be used alone, it is preferred to use two or more types in combination.

[0130] The external additive is preferably used in an amount of 0.3 to 6 parts by mass, and more preferably 1.2 to 3 parts by mass, based on 100 parts by mass of the colored resin particles.

[0131] The toner according to the first aspect of the present invention uses colored resin particles that contain a binder resin, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure whose solubility in styrene at a temperature of 40°C is 3 to 40 g / 100 g, and in a 2 μm × 2 μm square field of view of a cross section of the colored resin particles observed with a transmission electron microscope (TEM), the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 is 2 to 30. Such a toner according to the first aspect of the present invention has excellent storage stability and low-temperature fixing property and is therefore able to fully meet the recent demands for reduced energy consumption and faster printing.

[0132] <Toner for developing electrostatic images according to a second aspect> Further, a toner for developing electrostatic images according to a second aspect of the present invention is a toner for developing electrostatic images, which contains a binder resin, a colorant, a charge control agent, a release agent, and colored resin particles containing an additive having a polydiene structure, the additive having a polydiene structure has a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g; The storage modulus G'(60) of the colored resin particles at 60°C determined by dynamic viscoelasticity measurement is 1.6 x 10 8 ~5.0×10 8 It is Pa.

[0133] The colored resin particles constituting the toner according to the second aspect of the present invention can be produced by any of dry methods such as pulverization, or wet methods such as emulsion polymerization aggregation, dispersion polymerization, suspension polymerization, and dissolution suspension, as in the case of the toner according to the first aspect described above, but those produced by wet methods are preferred because toners excellent in printing characteristics such as image reproducibility can be easily obtained. Also, when the colored resin particles constituting the toner according to the second aspect of the present invention are produced by adopting (A) suspension polymerization, which is preferred among wet methods, or (B) pulverization, which is typical among dry methods, the colored resin particles are produced by the same process as in the case of the toner according to the first aspect described above.

[0134] When the colored resin particles constituting the toner according to the second aspect of the present invention are obtained by (A) suspension polymerization, they can be produced through (A-1) a polymerizable monomer composition preparation step, (A-2) a suspension step (droplet formation step) for obtaining a suspension, (A-3) a polymerization step, and (A-4) washing, filtration, dehydration, and drying steps, in the same manner as in the case of the toner according to the first aspect described above. In this case, the raw materials used for producing the colored resin particles, such as the polymerizable monomer, colorant, charge control agent, release agent, and additive having a polydiene structure, and other additives used as necessary, can be the same as those in the case of the toner according to the first aspect described above, and the production conditions can be the same.

[0135] Furthermore, when the colored resin particles constituting the toner according to the second aspect of the present invention are obtained by the (B) pulverization method, they can be produced by the same method as in the case of the toner according to the first aspect described above, and the raw materials used in producing the colored resin particles can be the same as those in the case of the toner according to the first aspect described above, and the production conditions can be the same as well.

[0136] The colored resin particles constituting the toner according to the second aspect of the present invention can be produced, for example, by the above-mentioned (A) suspension polymerization method or (B) pulverization method. In the second aspect of the present invention, the colored resin particles are preferably a toner having a storage modulus G'(60) at 60°C, determined by dynamic viscoelasticity measurement, of 1.6 x 10 8 ~5.0×10 8 The colored resin particles are used in such a manner that the storage modulus G'(60) at 60°C, determined by dynamic viscoelasticity measurement, is controlled within the above range. By controlling the storage modulus G'(60) at 60°C, determined by dynamic viscoelasticity measurement, within the above range, it is possible to effectively suppress blocking of the resulting toner while ensuring a sufficient effect of improving low-temperature fixability by adding a release agent. As a result, the resulting toner has excellent storage stability and low-temperature fixability.

[0137] The storage modulus G'(60) of the colored resin particles at 60°C, as determined by dynamic viscoelasticity measurement, is 1.6×10 8 ~5.0×10 8 The range may be 1.8×10 Pa, but preferably 1.8×10 8 ~4.5×10 8 Pa range, more preferably 2.0×10 8 ~4.0×10 8 The range is Pa.

[0138] In the second aspect of the present invention, the storage modulus G'(60) of the colored resin particles at 60° C., as determined by dynamic viscoelasticity measurement, may be within the above range. However, from the viewpoint of making the resulting toner more excellent in storage stability and low-temperature fixability, it is preferable that the storage modulus G'(100) of the colored resin particles at 100° C., as determined by dynamic viscoelasticity measurement, is within the above range. 5 ~3.0×10 5 It is preferable that the pressure is controlled within the range of 1.1×10 Pa. 5 ~2.9×10 5 It is more preferable that the pressure is controlled within the range of 1.2×10 Pa. 5 ~2.8×10 5 It is more preferable that the pressure is controlled within the Pa range.

[0139] The ratio G'(60) / G'(100) of the storage modulus G'(60) at 60° C. to the storage modulus G'(100) at 100° C., which is determined by dynamic viscoelasticity measurement, is not particularly limited. However, from the viewpoint of making the resulting toner superior in storage stability and low-temperature fixability, it is preferably 1.0×10 3 ~5.0×10 3 It is preferable that the range of the concentration is controlled to be within 1.0×10 3 ~4.0×10 3 More preferably, the range is 1.0×10 3 ~3.0×10 3 It is more preferable that the amount of the fluorine-containing compound is controlled within the range of 1 to 5.

[0140] The method for measuring the storage modulus G'(60) at 60°C and the storage modulus G'(100) at 100°C of the colored resin particles is not particularly limited, but the colored resin particles are sandwiched between a pair of 8 mmφ plates under a load of 20 g (the colored resin particles are uniformly distributed over an area of ​​8 mmφ and sandwiched between a pair of plates under a load of 20 g) as a measurement sample, and dynamic viscoelasticity measurement is performed in the range of 45 to 150°C using a dynamic viscoelasticity measuring device using a rotational plane rheometer at a measurement frequency of 24 Hz and a heating rate of 5°C / min.

[0141] In the second aspect of the present invention, the method for adjusting the storage modulus G'(60) of the colored resin particles at 60°C and further the storage modulus G'(100) of the colored resin particles at 100°C to the above range is not particularly limited, but may be a method of incorporating an additive having a polydiene structure in the colored resin particles. Specifically, by incorporating an additive having a polydiene structure, the release agent can be appropriately dispersed in the colored resin particles due to the compatibility of the additive having a polydiene structure with the release agent, and this makes it possible to adjust the storage modulus G'(60) of the colored resin particles at 60°C and the storage modulus G'(100) of the colored resin particles at 100°C to the above range. In the first aspect of the present invention, the storage modulus G'(60) of the colored resin particles at 60°C is 1.6×10 8 ~5.0×10 8 Methods for further controlling the elastic modulus within the range of Pa are not particularly limited, but include a method of adjusting the type of additive having a polydiene structure used, the type of release agent used, the amount of additive having a polydiene structure used, and the amount of release agent used, and these may be combined. Similarly, when the storage modulus G'(100) at 100°C of the colored resin particles is adjusted to 1.0×10 5 ~3.0×10 5The method for further control within the Pa range is not particularly limited, but includes a method of adjusting the type of additive having a polydiene structure used, the type of release agent used, the amount of additive having a polydiene structure used, and the amount of release agent used, and these may be combined.

[0142] The volume average particle size (Dv), number average particle size (Dn), particle size distribution (Dv / Dn), and average circularity of the colored resin particles are preferably in the same ranges as those of the colored resin particles according to the first aspect described above, for the same reasons.

[0143] Moreover, the gel content (amount insoluble in tetrahydrofuran) and weight average molecular weight (Mw) of the above-mentioned colored resin particles are preferably in the same ranges as those of the colored resin particles according to the first aspect, for the same reasons as those of the above-mentioned colored resin particles according to the first aspect.

[0144] The above-mentioned colored resin particles may be used as a toner as is or by mixing the colored resin particles with carrier particles (ferrite, iron powder, etc.); however, in order to adjust the chargeability, fluidity, storage stability, etc. of the toner, an external additive may be added and mixed with the colored resin particles using a high-speed mixer (for example, FM Mixer (product name, manufactured by Nippon Coke & Engineering Co., Ltd.)) to form a one-component toner, or the colored resin particles, the external additive, and the carrier particles may be mixed to form a two-component toner. The mixer for carrying out the external addition process may be the same as that in the first aspect described above, and the external additive may be the same as that in the first aspect described above in the same ratio.

[0145] The toner according to a second aspect of the present invention comprises, as colored resin particles, a binder resin, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure and a solubility in styrene at a temperature of 40° C. of 3 to 40 g / 100 g, and the storage modulus G'(60) of the colored resin particles at 60° C., as determined by dynamic viscoelasticity measurement, is 1.6×10 8 ~5.0×10 8The toner according to the second aspect of the present invention is excellent in storage stability and low-temperature fixing property, and therefore can fully meet the recent demands for reducing energy consumption and increasing printing speed. EXAMPLES

[0146] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Note that "parts" and "%" are by weight unless otherwise specified. The test methods used in the present examples and comparative examples are as follows.

[0147] (1) Weight average molecular weight of conjugated diene-aromatic vinyl thermoplastic elastomer The molecular weight was calculated as polystyrene equivalent molecular weight by high performance liquid chromatography using tetrahydrofuran as a carrier at a flow rate of 0.35 ml / min. The apparatus used was a Tosoh HLC8220, the column used was a combination of three Showa Denko Shodex (registered trademark) KF-404HQ columns (column temperature 40°C), and the detectors used were a differential refractometer and an ultraviolet detector. The molecular weight was calibrated at 12 points using standard polystyrene (5 to 3 million) from Polymer Laboratory.

[0148] (2) Content of each block copolymer in the conjugated diene-aromatic vinyl thermoplastic elastomer The ratio was determined from the area ratio of the peaks corresponding to each block copolymer in the chart obtained by the above-mentioned high performance liquid chromatography.

[0149] (3) Weight average molecular weight of the styrene polymer block of the block copolymer constituting the conjugated diene-aromatic vinyl thermoplastic elastomer According to the method described in Rubber Chem. Technol., 45, 1295 (1972), the block copolymer was reacted with ozone and reduced with lithium aluminum hydride to decompose the isoprene polymer block of the block copolymer. Specifically, the following procedure was followed. That is, 300 mg of the sample was dissolved in a reaction vessel containing 100 ml of dichloromethane treated with molecular sieves. After placing this reaction vessel in a cooling bath and lowering the temperature to -25°C, ozone generated by an ozone generator was introduced into the reaction vessel while oxygen was flowing at a flow rate of 170 ml / min. After 30 minutes had passed since the start of the reaction, the completion of the reaction was confirmed by introducing the gas flowing out of the reaction vessel into the potassium iodide aqueous solution. Next, 50 ml of diethyl ether and 470 mg of lithium aluminum hydride were charged into another reaction vessel substituted with nitrogen, and the solution reacted with ozone was slowly dropped into the reaction vessel while cooling the reaction vessel with ice water. The reaction vessel was then placed in a water bath, gradually heated, and refluxed at 40°C for 30 minutes. After that, while stirring the solution, dilute hydrochloric acid was dripped into the reaction vessel in small amounts until hydrogen generation was almost no longer observed. After this reaction, the solid product generated in the solution was filtered, and the solid product was extracted with 100 ml of diethyl ether for 10 minutes. This extract was combined with the filtrate obtained by filtration, and the solvent was distilled off to obtain a solid sample. The weight average molecular weight of the sample thus obtained was measured according to the above-mentioned method for measuring weight average molecular weight, and the value was taken as the weight average molecular weight of the styrene polymer block.

[0150] (4) Weight average molecular weight of the isoprene polymer block of the block copolymer constituting the conjugated diene-aromatic vinyl thermoplastic elastomer The weight average molecular weight of the corresponding styrene polymer block was subtracted from the weight average molecular weight of the block copolymer thus determined, and the weight average molecular weight of the isoprene polymer block was calculated based on the calculated value.

[0151] (5) Styrene unit content of the block copolymer constituting the conjugated diene-aromatic vinyl thermoplastic elastomer The value was determined based on the ratio of the detection intensities of the differential refractometer and the ultraviolet detector in the measurement by high performance liquid chromatography. Note that copolymers having different styrene unit contents were prepared in advance, and a calibration curve was prepared using them.

[0152] (6) Vinyl bond content of the isoprene polymer block of the block copolymer constituting the conjugated diene-aromatic vinyl thermoplastic elastomer It was determined based on proton NMR measurement.

[0153] (7) Styrene unit content of conjugated diene-aromatic vinyl thermoplastic elastomer It was determined based on proton NMR measurement.

[0154] (8) Melt index of conjugated diene-aromatic vinyl thermoplastic elastomer Measurements were performed in accordance with ASTM D1238 (G condition, 200°C, 5 kg load).

[0155] (9) Volume average particle size of colored resin particles (Dv) Approximately 0.1 g of colored resin particles were weighed out and placed in a beaker, and 0.1 mL of a surfactant solution (manufactured by Fujifilm, product name: Drywell) was added as a dispersant. 10 to 30 mL of Isoton II was further added to the beaker, and the particles were dispersed for 3 minutes using a 20 W ultrasonic disperser. The volume average particle size (Dv) of the colored resin particles was then measured using a particle size measuring device (manufactured by Beckman Coulter, product name: Multisizer) under the following conditions: aperture diameter: 100 μm, medium: Isoton II, number of particles measured: 100,000.

[0156] (10) Gel content of colored resin particles 1.0 g of colored resin particles was weighed out and placed in a Soxhlet extractor containing a cylindrical filter paper (Toyo Filter Paper Co., Ltd.: No. 86R, size 28 x 100 mm), and the extract was refluxed for 5 hours using 100 ml of tetrahydrofuran (THF) as a solvent to obtain an extract. The THF was evaporated from the extract to obtain non-volatile components, which were then vacuum-dried at 50°C for 1 hour, precisely weighed, and calculated using the following formula. THF insoluble matter (%) = [(TS) / (T)] x 100 T: Amount of colored resin particles sample (g) S: Amount of extracted non-volatile components (g)

[0157] (11) Weight average molecular weight (Mw) of colored resin particles 0.1 g of precisely weighed colored resin particles was placed in a 100 mL glass sample bottle, and then 49.9 g of tetrahydrofuran (THF) was added to each bottle. Next, a stirrer tip was added, and the mixture was stirred at room temperature for 1 hour using a magnetic stirrer, and then filtered through a 0.2 μm PTFE filter to obtain a THF solution of colored resin particles. Finally, 100 μL of each THF solution was injected into a GPC measurement device and subjected to GPC measurement. The weight average molecular weight (Mw) was calculated from the calibration curve of commercially available monodisperse standard polystyrene based on the obtained GPC elution curve. (GPC measurement conditions) GPC: HLC-8220 (Tosoh Corporation) Column: TSK-GEL MULTIPORE HXL-M, 2 columns connected together (Tosoh Corporation) Eluent:THF Flow rate: 1.0mL / min Temperature: 40℃

[0158] (12) Melting temperature of colored resin particles (T1 / 2) The melting temperature (T1 / 2) of the colored resin particles in the 1 / 2 method was calculated from the melt viscosity measured using a flow tester. Specifically, the melt viscosity was measured using a flow tester (manufactured by Shimadzu Corporation, product name: CFT-500C) under the conditions of a given starting temperature, heating rate, preheating time, and shear stress. Then, the melting temperature (T1 / 2) in the 1 / 2 method was calculated from the obtained melt viscosity. Measurement start temperature: 40℃, heating rate: 3℃ / min, preheating time: 5 min, cylinder pressure: 10kgf / cm 2 , Die diameter: 0.5mm, Die length: 1.0mm

[0159] (13) The average aspect ratio, average major axis, average minor axis, number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10, and number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8. Colored resin particles were dispersed in an epoxy resin, cured, cooled to a temperature of -80°C, and cut with a microtome to prepare a thin section. The prepared thin section was then stained with 0.5% aqueous ruthenium tetroxide vapor for about 5 minutes, and the stained thin section was observed with a transmission electron microscope (TEM). When preparing the thin section as a measurement sample, the concentration of colored resin particles in the thin section was adjusted to a concentration such that 5 to 10 cross sections could be observed within a range of 28 μm x 35 μm (magnification 5,000 to 6,000 times). Then, a measurement image was obtained in a field of view of 28 μm x 35 μm, and colored resin particles that did not show the entire image of the colored resin particle cross section and colored resin particles that were outside the range of 0.6 to 1.2 times the volume average particle size (Dv) were excluded from the evaluation, and 5 or more colored resin particles to be evaluated were identified. Then, for the specified colored resin particles, the number of crystal domains of the release agent, the aspect ratio, the long diameter and the short diameter of the crystal domains of the release agent were calculated by image analysis, and the average aspect ratio, average long diameter and average short diameter of the crystal domains of the release agent, as well as the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 and the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8 in a field of view of 2 μm × 2 μm square were calculated using the calculated results. The number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 and the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8 were calculated by converting the above calculation results into the number in a field of view of 2 μm × 2 μm square.

[0160] (14) Storage modulus G'(60) at 60°C and storage modulus G'(100) at 100°C of colored resin particles The colored resin particles were sandwiched between a pair of 8 mmφ plates (parallel plates or crosshatch plates) with a load of 20 g (the colored resin particles were uniformly arranged over an area of ​​8 mmφ and sandwiched between the pair of plates with a load of 20 g) as the measurement sample, and dynamic viscoelasticity measurements were performed in the range of 45 to 150°C at a measurement frequency of 24 Hz, a load of 20 g, and a heating rate of 5°C / min using a dynamic viscoelasticity measuring device (product name "ARES-G2", manufactured by TA Instruments) using a rotational planar rheometer to determine the dynamic viscoelasticity.

[0161] (15) Evaluation of toner storage stability 10 g of toner was placed in a 100 mL polyethylene container and sealed, and then the container was submerged in a thermostatic water bath set at a predetermined temperature, and after 8 hours, it was taken out. The toner was transferred from the container onto a 42 mesh sieve with as little vibration as possible, and set in a powder measuring instrument (manufactured by Hosokawa Micron Corporation, product name: Powder Tester PT-R). The sieve amplitude was set to 1.0 mm, and the sieve was vibrated for 30 seconds, after which the mass of the toner remaining on the sieve was measured, and this was taken as the mass of the aggregated toner. The maximum temperature (°C) at which the mass of the aggregated toner became 0.5 g or less was taken as the storage stability temperature, and was used as an index of storage stability.

[0162] (16) Minimum fixing temperature of toner A fixing test was conducted using a commercially available non-magnetic single-component development printer (printing speed 20 ppm) modified to change the temperature of the fixing roll. The fixing test was conducted by printing a solid black image (100% print density) and changing the temperature of the fixing roll of the modified printer by 5°C increments, measuring the toner fixing rate at each temperature, and determining the relationship between temperature and fixing rate. The fixing rate was calculated from the ratio of image density before and after tape peeling by peeling tape in the printed area of ​​the solid black image (100% print density). In other words, if the image density before tape peeling is ID (before) and the image density after tape peeling is ID (after), the fixing rate can be calculated by the following formula. Retention rate (%) = (ID (later) / ID (previous)) x 100 Here, the tape peeling operation refers to a series of operations in which an adhesive tape (manufactured by Sumitomo 3M, product name: Scotch Mending Tape 810-3-18) is applied to the measurement portion of the test paper, pressed with a constant pressure to adhere, and then the adhesive tape is peeled off in the direction along the paper at a constant speed. The image density was measured using a reflection type image densitometer (manufactured by Macbeth, product name: RD914). In this fixing test, the lowest fixing roll temperature at which the fixing rate exceeded 80% was determined as the minimum fixing temperature of the toner.

[0163] (17) Toner hot offset occurrence temperature A hot offset test was conducted using a commercially available non-magnetic single-component development printer (printing speed 20 ppm) modified to change the temperature of the fixing roll. The hot offset test was conducted by changing the temperature of the fixing roll from 150°C to 220°C in 5°C increments, printing a 5cm square solid image on paper (Xerox, product name: Vitarity), and visually observing whether the toner had melted onto the fixing roll or whether the hot offset phenomenon had occurred. In this hot offset test, the lowest set temperature at which the toner started to melt and adhere to the fixing roll was taken as the hot offset occurrence temperature.

[0164] (18) Toner charge The charge amount (μC / g) of the toner was evaluated in a normal humidity environment (23°C, 50%RH) by mounting a cartridge filled with toner that had been left in a normal humidity environment (23°C, 50%RH) for one day on a commercially available printer (print speed 20 ppm) using a non-magnetic one-component development method. First, two solid white prints were made, and then the charge amount (μC / g) of the toner adhering to the developing roll was measured using a suction type charge amount measuring device (manufactured by Trek Japan, product name: 210HS-2A). The charge amount of the toner was evaluated for Examples 4-1 to 4-4 and Comparative Examples 4-1 to 4-3.

[0165] (19) Bleed rate The toner was stored for 30 days in an environment at a temperature of 40° C., and the bleeding rate of the toner after storage was measured. Specifically, the toner after storage for 30 days was observed by SEM, and the presence or absence of bleeding of the release agent was evaluated for approximately 100 toner particles, and the ratio of toner particles that had bleed was taken as the bleeding rate (unit: %). The bleeding rate evaluation was performed for Examples 4-1 to 4-4 and Comparative Examples 4-1 to 4-3.

[0166] (20) Ejection evaluation A commercially available non-magnetic one-component development printer (printing speed 20 ppm) was used, and the toner cartridge of the development device was filled with toner, and the toner cartridge filled with toner was left for 30 days under conditions of 40°C, and then the cartridge was removed and set in the printer, and continuous printing was performed under conditions of temperature: 32.5°C and humidity: 80%. Printing was performed with a halftone image density of 30%. Then, after the start of continuous printing, the presence or absence of toner ejection from the toner cartridge onto the printing paper (presence or absence of spots of 0.3 x 0.3 mm or more due to toner on the halftone) was confirmed every hour. The longer the time when toner ejection from the toner cartridge onto the printing paper was not confirmed, the higher the effect of suppressing ejection is recognized. The ejection evaluation was performed for Examples 4-1 to 4-4 and Comparative Examples 4-1 to 4-3.

[0167] (21) Blade adhesion A commercially available non-magnetic one-component development printer (printing speed 20 ppm) was used, and the toner cartridge of the development device was filled with toner, and the toner cartridge filled with toner was left for 30 days at 40° C., and then the presence or absence of adhered matter on the blade (the blade that defines the toner layer) was confirmed. The evaluation of the adhered matter on the blade was performed for Examples 4-1 to 4-4 and Comparative Examples 4-1 to 4-3.

[0168] [Production Example 1] In a pressure-resistant reactor, 23.2 kg of cyclohexane, 1.5 mmol of N,N,N',N'-tetramethylethylenediamine (hereinafter referred to as TMEDA), and 1.70 kg of styrene were added, and while stirring at 40°C, 99.1 mmol of n-butyllithium was added, and polymerization was carried out for 1 hour while raising the temperature to 50°C. The polymerization conversion rate of styrene was 100% by mass. Subsequently, 6.03 kg of isoprene was continuously added to the reactor over 1 hour while controlling the temperature to maintain 50-60°C. After the addition of isoprene was completed, polymerization was carried out for another 1 hour to form a styrene-isoprene diblock copolymer B (copolymer B represented by Ar-D). The polymerization conversion rate of isoprene was 100%. Next, 15.0 mmol of dimethyldichlorosilane was added as a coupling agent to carry out a coupling reaction for 2 hours, and a styrene-isoprene-styrene triblock copolymer (copolymer A represented by Ar-D-Ar) was formed. Thereafter, 198 mmol of methanol was added as a polymerization terminator and mixed thoroughly to terminate the reaction, thereby obtaining a reaction liquid containing a block copolymer composition (α1). A portion of the obtained reaction liquid was taken out, and the weight average molecular weight, content ratio, and vinyl bond content of each block copolymer and the entire block copolymer composition were determined. The obtained results are shown in Table 1. Then, 0.3 parts of 2,6-di-tert-butyl-p-cresol was added as an antioxidant to 100 parts of the reaction liquid obtained in this way (containing 30 parts of polymer component) and mixed, and the mixed solution was dropped into hot water heated to 85 to 95 ° C. in small amounts to volatilize the solvent and obtain a precipitate, which was crushed and dried with hot air at 85 ° C. to recover the block copolymer composition (α1). The melt index of the obtained block copolymer composition (α1) was measured, and the obtained results are shown in Table 2. In addition, the solubility of the obtained block copolymer composition (α1) in styrene at a temperature of 40 ° C. was measured, and it was 20 g / 100 g.

[0169] [Production Example 2] A block copolymer composition (α2) of Production Example 2 was obtained in the same manner as in Production Example 1, except that the amounts of styrene, n-butyllithium, TMEDA, isoprene, dimethyldichlorosilane, and methanol were changed as shown in Table 1, and measurements were performed in the same manner. The measurement results are shown in Table 2. In addition, the solubility of the obtained block copolymer composition (α2) in styrene at a temperature of 40° C. was measured and found to be 20 g / 100 g.

[0170] [Production Example 3] A block copolymer composition (α3) of Production Example 3 was obtained in the same manner as in Production Example 1, except that the amounts of styrene, n-butyllithium, TMEDA, isoprene, dimethyldichlorosilane, and methanol were changed as shown in Table 1, and measurements were performed in the same manner. The measurement results are shown in Table 2. In addition, the solubility of the obtained block copolymer composition (α3) in styrene at a temperature of 40° C. was measured and found to be 20 g / 100 g.

[0171] [Production Example 4] A block copolymer composition (α4) of Production Example 4 was obtained in the same manner as in Production Example 1, except that the amounts of styrene, n-butyllithium, TMEDA, isoprene, dimethyldichlorosilane, and methanol were changed as shown in Table 1, and measurements were performed in the same manner. The measurement results are shown in Table 2. In addition, the solubility of the obtained block copolymer composition (α4) in styrene at a temperature of 40° C. was measured and found to be 4 g / 100 g.

[0172] [Production Example 5] The amounts of styrene, n-butyllithium, TMEDA, isoprene, and methanol were changed as shown in Table 1, and tetramethoxysilane was used in place of dimethyldichlorosilane in the amount shown in Table 1. The block copolymer composition (α5) of Production Example 5 was obtained in the same manner as in Production Example 1, and measurements were performed in the same manner. The measurement results are shown in Table 2. The block copolymer composition (α5) obtained in Production Example 5 contained styrene-isoprene diblock copolymer B (copolymer B represented by Ar-D), 3-branched styrene-isoprene block copolymer C (copolymer C represented by (Ar-D)3X), and 4-branched styrene-isoprene block copolymer D (copolymer D represented by (Ar-D)4X). The solubility of the obtained block copolymer composition (α5) in styrene at a temperature of 40° C. was measured and found to be 2 g / 100 g.

[0173] [Production Example 6, Production Example of Acrylic Resin] 200 parts of toluene were added to the reaction vessel, and the inside of the reaction vessel was thoroughly replaced with nitrogen while stirring the toluene, and then the temperature was raised to 90°C. Then, a mixed solution of 95 parts of methyl methacrylate, 4.6 parts of n-butyl acrylate, 0.4 parts of acrylic acid, and 2.8 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name: Perbutyl O) was dropped into the reaction vessel over 2 hours. The mixture was further kept under toluene reflux for 10 hours to complete polymerization, and then the solvent was distilled off under reduced pressure. In this way, an acrylic resin (Tg 70°C, acid value 2.5, weight average molecular weight (Mw) 11000) was obtained.

[0174] [Table 1]

[0175] [Table 2]

[0176] [Example 1-1] 77 parts of styrene and 23 parts of n-butyl acrylate as monovinyl monomers, 7 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name: #25B) as a colorant, 0.6 parts of divinylbenzene as a crosslinkable polymerizable monomer, 1.2 parts of t-dodecyl mercaptan as a molecular weight modifier, 0.3 parts of polymethacrylic acid ester macromonomer (manufactured by Toa Gosei Chemical Industry Co., Ltd., product name: AA6, Tg = 94 ° C) as a macromonomer, and 1 part of the acrylic resin obtained in Production Example 2 were wet-pulverized using a media-type wet pulverizer, and then 1 part of the charge control resin (styrene / acrylic resin containing quaternary ammonium salt as a functional group, copolymerization ratio of monomer containing quaternary ammonium salt functional group: 2%) as a charge control agent, 20 parts of behenyl stearate (number average molecular weight (Mn): 592) as a mold release agent, and 5 parts of the block copolymer composition (α1) obtained in Production Example 1 as an additive having a polydiene structure were added and mixed to obtain a polymerizable monomer composition.

[0177] Separately, in a stirring tank at room temperature, an aqueous solution of 4.1 parts of sodium hydroxide (alkali metal hydroxide) in 50 parts of ion-exchanged water was gradually added to an aqueous solution of 7.4 parts of magnesium chloride (water-soluble polyvalent metal salt) in 250 parts of ion-exchanged water while stirring, to prepare a magnesium hydroxide colloid (poorly water-soluble metal hydroxide colloid) dispersion.

[0178] On the other hand, 2 parts of methyl methacrylate as a polymerizable monomer for the shell and 65 parts of ion-exchanged water were subjected to a fine dispersion treatment by an ultrasonic emulsifier to obtain an aqueous dispersion of the polymerizable monomer for the shell.

[0179] The polymerizable monomer composition was added to the magnesium hydroxide colloidal dispersion obtained above and stirred until the droplets became stable. 6 parts of t-butyl peroxyisobutyrate (manufactured by NOF Corp., product name: Perbutyl IB) was added as a polymerization initiator. Then, using an in-line emulsifying disperser (manufactured by Pacific Machinery Works, product name: Milder), the mixture was stirred with high shear at a rotation speed of 15,000 rpm, and dispersed while circulating, to form droplets of the polymerizable monomer composition.

[0180] Next, 1 part of sodium tetraborate decahydrate was added to the aqueous dispersion of the polymerizable monomer composition that had formed droplets, and the mixture was placed in a reactor equipped with an agitator and heated to 85°C to carry out a polymerization reaction. After the polymerization conversion rate reached nearly 100%, the aqueous dispersion of the shell polymerizable monomer prepared above and 0.3 parts of 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)-propionamide) (manufactured by Wako Pure Chemical Industries, Ltd., trade name: VA-086, water-soluble) as a polymerization initiator for the shell were added to the reactor. After further continuing the polymerization for 4 hours, the reaction was stopped by cooling with water to obtain an aqueous dispersion of colored resin particles having a core-shell structure.

[0181] The aqueous dispersion of the colored resin particles was washed with dilute sulfuric acid (25°C, 10 minutes) to adjust the pH to 4.5 or less. Next, after separating the water by filtration, 200 parts of fresh ion-exchanged water was added to re-slurry the mixture, and the water washing treatment (washing, filtration, dehydration) was repeated several times at room temperature (25°C). The solid matter obtained was separated by filtration, and then vacuum dried to obtain dried colored resin particles. The obtained colored resin particles were subjected to various measurements according to the above-mentioned method, including the average aspect ratio of the crystal domains of the release agent, the average major axis, the average minor axis, the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10, the number of crystal domains of the release agent having an aspect ratio in the range of 3 to 8, the storage modulus G'(60) at 60°C, and the storage modulus G'(100) at 100°C. These results are shown in Table 3.

[0182] In addition, 0.5 parts of silica fine particles having a number average primary particle diameter of 7 nm and hydrophobized with cyclic silazane, and 1 part of silica fine particles having a number average primary particle diameter of 35 nm and hydrophobized with amino-modified silicone oil were added to 100 parts of the colored resin particles obtained above as external additives, and the mixture was mixed and stirred using a high-speed mixer (manufactured by Nippon Coke & Engineering Co., Ltd., product name: FM Mixer) to perform external addition treatment, thereby preparing a toner for developing electrostatic images. The above-mentioned measurements were performed using the obtained toner for developing electrostatic images. The results are shown in Table 2.

[0183] [Example 1-2] As a release agent, 20 parts of stearyl stearate (number average molecular weight (Mn): 536) was used instead of 20 parts of behenyl stearate, and the same procedure as in Example 1-1 was used to obtain colored resin particles and a toner for developing electrostatic images of Example 1-2, and the evaluation was performed in the same manner. The results are shown in Table 3.

[0184] [Examples 1-3] As a release agent, 20 parts of behenyl behenate (number average molecular weight (Mn): 648) was used instead of 20 parts of behenyl stearate, and the same procedure as in Example 1-1 was used to obtain colored resin particles and a toner for developing electrostatic images of Example 1-3, and the evaluation was performed in the same manner. The results are shown in Table 3.

[0185] [Reference example 1] The colored resin particles and electrostatic image developing toner of Reference Example 1 were obtained in the same manner as in Example 1-1, except that 1.7 parts of solution polymerization polyisoprene rubber 1 (trade name "Kuraray LIR-30", manufactured by Kuraray Co., Ltd., weight average molecular weight (Mw): 28,000, solubility in styrene at a temperature of 40°C: 16 g / 100 g) were used instead of 5 parts of the block copolymer composition (α1) obtained in Production Example 1 as an additive having a polydiene structure, and evaluations were performed in the same manner. The results are shown in Table 3.

[0186] [Examples 1-5] Except for changing the amount of block copolymer composition (α1) used as an additive having a polydiene structure from 5 parts to 2 parts, the same procedure as in Example 1-1 was followed to obtain colored resin particles and electrostatic image developing toner of Example 1-5, and the evaluation was performed in the same manner. The results are shown in Table 3.

[0187] [Examples 1-6] The colored resin particles and the toner for developing electrostatic images of Example 1-6 were obtained in the same manner as in Example 1-1, except that the amount of the block copolymer composition (α1) used as the additive having a polydiene structure was changed from 5 parts to 10 parts, and the evaluation was performed in the same manner. The results are shown in Table 3.

[0188] [Comparative Example 1-1] Except for not adding the block copolymer composition (α1) as an additive having a polydiene structure, the colored resin particles and the toner for developing electrostatic images of Comparative Example 1-1 were obtained in the same manner as in Example 1-1, and were evaluated in the same manner. The results are shown in Table 3.

[0189] [Comparative Example 1-2] As a release agent, 20 parts of behenyl behenate (number average molecular weight (Mn): 648) were used instead of 20 parts of behenyl stearate, and the same procedure as in Comparative Example 1-1 was used to obtain colored resin particles and a toner for developing electrostatic images in Comparative Example 1-2, which were then evaluated in the same manner. The results are shown in Table 3.

[0190] [Comparative Example 1-3] The colored resin particles and the toner for developing electrostatic images of Comparative Example 1-3 were obtained in the same manner as in Example 1-1, except that 1.7 parts of solution-polymerized polyisoprene rubber 2 (product name "IR2200", manufactured by Zeon Corporation, weight average molecular weight (Mw): 1,100,000, solubility in styrene at a temperature of 40°C: 2.4 g / 100 g) were used instead of 5 parts of the block copolymer composition (α1) obtained in Production Example 1 as an additive having a polydiene structure, and were evaluated in the same manner. The results are shown in Table 3.

[0191] [Table 3]

[0192] [Evaluation of Examples 1-1 to 1-6 and Comparative Examples 1-1 to 1-3] As shown in Table 3, the colored resin particles include a binder resin, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure whose solubility in styrene at a temperature of 40° C. is 3 to 40 g / 100 g. In addition, the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 in a 2 μm × 2 μm square field of view of the cross section observed with a transmission electron microscope (TEM) is 2 to 30, and further, the storage modulus G'(60) at 60° C. is 1.6 × 10 8 ~5.0×10 8The toners of Examples 1-1 to 1-6 obtained using the colored resin particles having a Pa had a high storage temperature, excellent storage stability, a low minimum fixing temperature, and excellent low-temperature fixing property. Moreover, the toners of Examples 1-1 to 1-6 also had a high hot offset occurrence temperature and excellent hot offset resistance.

[0193] On the other hand, the toners of Comparative Examples 1-1 to 1-3 obtained using colored resin particles that did not contain an additive having a polydiene structure, had a solubility in styrene at a temperature of 40°C of 3 to 40 g / 100 g, and contained less than two crystal domains of a release agent having an aspect ratio in the range of 2 to 10, had a low storage temperature and poor storage stability.

[0194] Fig. 1(A) is a cross-sectional photograph of the colored resin particles of Example 1-1 taken by a transmission electron microscope (TEM), and Fig. 1(B) is a cross-sectional photograph of the colored resin particles of Comparative Example 1-1 taken by a transmission electron microscope (TEM). As shown in Fig. 1(A), in Examples 1-1 to 1-6, crystal domains of the release agent having an aspect ratio in the range of 2 to 10 were finely dispersed in the colored resin particles (the same applies to Examples 2-1 to 2-2, 3-1 to 3-7, and 4-1 to 4-4 described later), whereas in Comparative Examples 1-1 to 1-3, as shown in Fig. 1(B), the release agent was localized near the center of the colored resin particles (slightly to the lower left of the center) to form a large domain structure.

[0195] [Example 2-1] The colored resin particles and the toner for developing electrostatic images of Example 2-1 were obtained in the same manner as in Example 1-1, except that the amount of divinylbenzene used was changed from 0.6 parts to 0.3 parts, and the evaluation was performed in the same manner. The results are shown in Table 4.

[0196] [Example 2-2] The colored resin particles and the toner for developing electrostatic images of Example 2-2 were obtained in the same manner as in Example 2-1, except that the amount of divinylbenzene used was changed from 0.3 parts to 0.33 parts, and the evaluation was performed in the same manner. The results are shown in Table 4.

[0197] [Comparative Example 2-1] The amount of divinylbenzene used was changed from 0.3 parts to 0.51 parts, and the block copolymer composition (α1) was not added as an additive having a polydiene structure, so that the same procedure as in Example 2-1 was followed to obtain the colored resin particles and the toner for developing electrostatic images of Comparative Example 2-1, and the evaluation was carried out in the same manner. The results are shown in Table 4.

[0198] [Comparative Example 2-2] The amount of divinylbenzene used was changed from 0.3 parts to 0.54 parts, and the block copolymer composition (α1) was not added as an additive having a polydiene structure, so that the same procedure as in Example 2-1 was followed to obtain colored resin particles and a toner for developing electrostatic images of Comparative Example 2-2, and the evaluation was carried out in the same manner. The results are shown in Table 4.

[0199] [Comparative Example 2-3] The amount of divinylbenzene used was changed from 0.3 parts to 0.6 parts, and 5 parts of a styrene-ethylene propylene-styrene block copolymer (manufactured by Kuraray Co., Ltd., product name: Septon 2104, styrene unit content: 65% by mass, weight average molecular weight (Mw): 64,000, solubility in styrene at a temperature of 40°C: 15 g / 100 g) was used instead of 5 parts of the block copolymer composition (α1) as an additive having a polydiene structure. The colored resin particles and the toner for developing electrostatic images of Comparative Example 2-3 were obtained in the same manner as in Example 2-1, and were evaluated in the same manner. The results are shown in Table 4.

[0200] [Comparative Example 2-4] The amount of divinylbenzene used was changed from 0.3 parts to 0.6 parts, and 5 parts of a styrene-ethylene propylene-styrene block copolymer (manufactured by Kuraray Co., Ltd., product name: Septon 4033, styrene unit content: 30 mass%, weight average molecular weight (Mw): 81,000, solubility in styrene at a temperature of 40°C: 15 g / 100 g) was used instead of 5 parts of the block copolymer composition (α1) as an additive having a polydiene structure. The colored resin particles and the toner for developing electrostatic images of Comparative Example 2-4 were obtained in the same manner as in Example 2-1, and were evaluated in the same manner. The results are shown in Table 4.

[0201] [Table 4]

[0202] [Evaluation of Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-4] As shown in Table 4, the colored resin particles include a binder resin, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure whose solubility in styrene at a temperature of 40°C is 3 to 40 g / 100 g. In addition, the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 in a 2 μm × 2 μm square field of view of the cross section observed with a transmission electron microscope (TEM) is 2 to 30, and further, the storage modulus G'(60) at 60°C is 1.6 × 10 8 ~5.0×10 8 The toners of Examples 2-1 and 2-2 obtained using colored resin particles with a Pa had a high storage temperature, excellent storage stability, a low minimum fixing temperature, and excellent low-temperature fixing properties.

[0203] On the other hand, the storage modulus G'(60) at 60°C is 1.6×10 8 The toners of Comparative Examples 2-1 to 2-4 obtained using colored resin particles with a surface tension less than 1 Pa had a low storage temperature and were poor in storage stability.

[0204] [Example 3-1] The colored resin particles and the toner for developing electrostatic images of Example 3-1 were obtained in the same manner as in Example 1-1, except that the amount of divinylbenzene used was changed from 0.6 parts to 0.45 parts, and the evaluation was performed in the same manner. The results are shown in Table 5.

[0205] [Example 3-2] The colored resin particles and the toner for developing electrostatic images of Example 3-2 were obtained in the same manner as in Example 3-1, except that the amount of divinylbenzene used was changed from 0.6 parts to 0.3 parts, and the evaluation was performed in the same manner. The results are shown in Table 5.

[0206] [Example 3-3] The colored resin particles and the toner for developing electrostatic images of Example 3-3 were obtained in the same manner as in Example 3-1, except that the amount of divinylbenzene used was changed from 0.45 parts to 0.6 parts, and the amount of the block copolymer composition (α1) obtained in Production Example 1 was changed from 5 parts to 2 parts, and the evaluation was performed in the same manner. The results are shown in Table 5.

[0207] [Example 3-4] The colored resin particles and the toner for developing electrostatic images of Example 3-4 were obtained in the same manner as in Example 3-3, except that the amount of divinylbenzene used was changed from 0.6 parts to 0.5 parts, and the evaluation was performed in the same manner. The results are shown in Table 5.

[0208] [Examples 3-5] The colored resin particles and the toner for developing electrostatic images of Example 3-5 were obtained in the same manner as in Example 3-3, except that the amount of divinylbenzene used was changed from 0.6 parts to 0.4 parts, and the evaluation was performed in the same manner. The results are shown in Table 5.

[0209] [Examples 3-6] The colored resin particles and the toner for developing electrostatic images of Example 3-6 were obtained in the same manner as in Example 3-1, except that the amount of styrene used was changed from 77 parts to 83 parts, the amount of n-butyl acrylate used was changed from 23 parts to 17 parts, and the amount of divinylbenzene used was changed from 0.45 parts to 0.6 parts, and the evaluation was performed in the same manner. The results are shown in Table 5.

[0210] [Examples 3-7] The colored resin particles and the toner for developing electrostatic images of Example 3-7 were obtained in the same manner as in Example 3-3, except that the acrylic resin obtained in Production Example 2 was not added, and the evaluations were performed in the same manner. The results are shown in Table 5.

[0211] [Comparative Example 3-1] The colored resin particles and the toner for developing electrostatic images of Comparative Example 3-1 were obtained in the same manner as in Example 3-3, except that the block copolymer composition (α1) obtained in Production Example 1 was not used, and the evaluations were performed in the same manner. The results are shown in Table 5.

[0212] [Comparative Example 3-2] Colored resin particles and a toner for developing electrostatic images of Comparative Example 3-2 were obtained in the same manner as in Example 3-3, except that 2 parts of a styrene-ethylene-propylene block copolymer (manufactured by Kuraray Co., Ltd., product name: Septon 2063, styrene unit content: 13 mass%, weight average molecular weight (Mw): 91000, solubility in styrene at a temperature of 40°C: 15 g / 100 g) were used instead of 5 parts of the block copolymer composition (α1) obtained in Production Example 1, and evaluations were similarly performed. The results are shown in Table 5.

[0213] [Comparative Example 3-3] Colored resin particles and a toner for developing electrostatic images of Comparative Example 3-3 were obtained and evaluated in the same manner as in Example 3-3, except that 5 parts of a styrene-ethylene-propylene block copolymer (manufactured by Kuraray Co., Ltd., product name: Septon 2063) was used instead of 5 parts of the block copolymer composition (α1) obtained in Production Example 1. The results are shown in Table 5.

[0214] [Comparative Example 3-4] The colored resin particles and the toner for developing electrostatic images of Comparative Example 3-4 were obtained in the same manner as in Example 3-3, except that 2 parts of a styrene-ethylene-propylene-styrene block copolymer (manufactured by Kuraray Co., Ltd., product name: Septon 2104) were used instead of 5 parts of the block copolymer composition (α1) obtained in Production Example 1, and were evaluated in the same manner. The results are shown in Table 5.

[0215] [Comparative Example 3-5] The colored resin particles and the toner for developing electrostatic images of Comparative Example 3-5 were obtained in the same manner as in Example 3-3, except that 2 parts of a styrene-ethylene-propylene-styrene block copolymer (manufactured by Kuraray Co., Ltd., product name: Septon 4033) were used instead of 5 parts of the block copolymer composition (α1) obtained in Production Example 1, and were evaluated in the same manner. The results are shown in Table 5.

[0216] [Table 5]

[0217] [Evaluation of Examples 3-1 to 3-7 and Comparative Examples 3-1 to 3-5] As shown in Table 5, the colored resin particles include a binder resin, a colorant, a charge control agent, a release agent, and an additive having a polydiene structure whose solubility in styrene at a temperature of 40° C. is 3 to 40 g / 100 g. In addition, the number of crystal domains of the release agent having an aspect ratio in the range of 2 to 10 in a 2 μm × 2 μm square field of view of the cross section observed with a transmission electron microscope (TEM) is 2 to 30, and further, the storage modulus G'(60) at 60° C. is 1.6 × 10 8 ~5.0×10 8 The toners of Examples 3-1 to 3-7 obtained using colored resin particles with a Pa had a high storage temperature, excellent storage stability, a low minimum fixing temperature, and excellent low-temperature fixing properties.

[0218] On the other hand, the toners of Comparative Examples 3-1 to 3-5, which did not contain an additive having a polydiene structure or instead used an aromatic vinyl thermoplastic elastomer that did not have a polydiene structure and therefore did not have a polymerization-reactive unsaturated bond, had low storage temperatures and poor storage stability. In addition, when the state of behenyl stearate as a release agent in the toners of Comparative Examples 3-1 to 3-5 was confirmed by cross-sectional SEM and TEM, it was confirmed that behenyl stearate was localized near the center of the toner particle and formed a large domain structure.

[0219] [Example 4-1] 70.5 parts of styrene and 29.5 parts of n-butyl acrylate as monovinyl monomers, 7 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name: #25B) as a colorant, 0.6 parts of divinylbenzene as a crosslinkable polymerizable monomer, 1.2 parts of t-dodecyl mercaptan as a molecular weight modifier, 0.3 parts of polymethacrylic acid ester macromonomer (manufactured by Toa Gosei Chemical Industry Co., Ltd., product name: AA6, Tg = 94 ° C) as a macromonomer, and 1 part of the acrylic resin obtained in Production Example 6 were wet-ground using a media-type wet grinder, and then 1 part of the charge control resin (styrene / acrylic resin containing quaternary ammonium salt as a functional group, copolymerization ratio of monomer containing quaternary ammonium salt functional group: 2%) as a charge control agent, 20 parts of behenyl stearate (number average molecular weight (Mn): 592) as a mold release agent, and 5 parts of the block copolymer composition (α2) obtained in Production Example 2 as an aromatic vinyl thermoplastic elastomer were added and mixed to obtain a polymerizable monomer composition.

[0220] Then, except for using the polymerizable monomer composition obtained above, the same procedure as in Example 1-1 was followed to obtain colored resin particles and a toner for developing electrostatic images of Example 4-1, and the evaluations were performed in the same manner. The results are shown in Table 6.

[0221] [Example 4-2] The colored resin particles and the toner for developing electrostatic images of Example 4-2 were obtained in the same manner as in Example 4-1, except that 5 parts of the block copolymer composition (α1) obtained in Production Example 1 was used instead of 5 parts of the block copolymer composition (α2) obtained in Production Example 2, and were evaluated in the same manner. The results are shown in Table 6.

[0222] [Example 4-3] The colored resin particles and the toner for developing electrostatic images of Example 4-3 were obtained in the same manner as in Example 4-1, except that 5 parts of the block copolymer composition (α3) obtained in Production Example 3 was used instead of 5 parts of the block copolymer composition (α2) obtained in Production Example 2, and were evaluated in the same manner. The results are shown in Table 6.

[0223] [Example 4-4] The colored resin particles and the toner for developing electrostatic images of Example 4-4 were obtained in the same manner as in Example 4-1, except that 5 parts of the block copolymer composition (α2) obtained in Production Example 2 was replaced with 5 parts of the block copolymer composition (α1) obtained in Production Example 1, and the low molecular weight acrylic resin obtained in Production Example 6 was not used, and the evaluation was performed in the same manner. The results are shown in Table 6.

[0224] [Comparative Example 4-1] Except for not using the block copolymer composition (α2) obtained in Production Example 2, the same procedures as in Example 1 and Example 4-1 were carried out to obtain colored resin particles and a toner for developing electrostatic images of Comparative Example 4-1, and the evaluations were carried out in the same manner. The results are shown in Table 6.

[0225] [Comparative Example 4-2] Colored resin particles and a toner for developing electrostatic images of Comparative Example 4-2 were obtained in the same manner as in Example 4-1, except that 5 parts of the block copolymer composition (α4) obtained in Production Example 4 was used instead of 5 parts of the block copolymer composition (α2) obtained in Production Example 2, and were evaluated in the same manner. The results are shown in Table 6.

[0226] [Comparative Example 4-3] Colored resin particles and a toner for developing electrostatic images of Comparative Example 4-3 were obtained and evaluated in the same manner as in Example 4-1, except that 5 parts of the block copolymer composition (α5) obtained in Production Example 5 was used instead of 5 parts of the block copolymer composition (α2) obtained in Production Example 2. The results are shown in Table 6.

[0227] [Table 6]

[0228] As shown in Table 6, the toners of Examples 4-1 to 4-4 obtained by further containing an aromatic vinyl thermoplastic elastomer containing 40% by weight or more of a diblock copolymer consisting of an aromatic vinyl polymer block and a block of a polymer copolymerizable with the aromatic vinyl polymer as an additive having a polydiene structure, in addition to the characteristics of a high storage temperature, excellent storage stability, a low minimum fixing temperature, and excellent low-temperature fixing property, were confirmed to have high charging properties, suppressed bleeding out of the release agent, and effectively suppressed the occurrence of spraying and adhesion to the blade under high temperature and high humidity conditions.

[0229] On the other hand, the toners of Comparative Examples 4-1 to 4-3, which did not contain a diblock copolymer consisting of an aromatic vinyl polymer block and a block of a polymer copolymerizable with the aromatic vinyl polymer, or which used an aromatic vinyl thermoplastic elastomer with a diblock copolymer content of less than 40% by weight, resulted in ejection and adhesion to the blade under high temperature and high humidity conditions.

Claims

1. A toner for developing electrostatic images, comprising colored resin particles containing a binder resin, a colorant, a release agent, and an aromatic vinyl thermoplastic elastomer, and an external additive, the aromatic vinyl thermoplastic elastomer contains an aromatic vinyl-conjugated diene diblock copolymer and an aromatic vinyl-conjugated diene-aromatic vinyl triblock copolymer; the aromatic vinyl thermoplastic elastomer contains the aromatic vinyl-conjugated diene diblock copolymer in an amount of 40% by weight or more and 95% by mass or less; the content of the aromatic vinyl thermoplastic elastomer is 1 to 10 parts by mass relative to 100 parts by mass of the binder resin, The toner for developing electrostatic images, wherein when a cross section of the colored resin particle is observed with a transmission electron microscope (TEM), the number of crystal domains of the release agent present within a 2 μm×2 μm square field of view of the cross section of the colored resin particle, the crystal domains having an aspect ratio in the range of 2 to 10, is 2 to 30.

2. 2. The toner for developing electrostatic images according to claim 1, wherein the content of the aromatic vinyl monomer units in the aromatic vinyl thermoplastic elastomer is 10 to 30% by mass based on the total monomer units.

3. 3. The toner for developing electrostatic images according to claim 1, wherein the releasing agent is a fatty acid ester compound having a number average molecular weight (Mn) of 500 to 1,500.

Citation Information

Patent Citations

  • Electrostatic charge image developing toner and its production

    JP1995181740A

  • Binder resin for toner, and toner

    JP2004062168A

  • Electrostatic charge image developing toner

    JP2011128413A

  • Toner and method for producing toner

    JP2011150229A

  • toner

    JP2012177914A