High-capacity, compact lithium thin-film battery

By embedding the cathode layer within a substrate trench and optimizing layer deposition, the method addresses capacity limitations and manufacturing inefficiencies in conventional thin film lithium batteries, resulting in compact, high-capacity batteries with reduced seal area and cost-effective production.

JP7563854B2Active Publication Date: 2024-10-08INTERNATIONAL BUSINESS MACHINE CORPORATION

Patent Information

Application Number
JP2022517351
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-23
Filing Date
2020-08-19
Publication Date
2024-10-08
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

Conventional thin film lithium batteries are limited by the thickness and structure of the cathode layer, leading to capacity constraints, and the manufacturing process is time-consuming and expensive, especially for larger batteries, requiring large seals to protect against contamination.

Method used

A method involving the use of a stencil and pressure head to embed the cathode layer within a substrate trench, reducing its thickness and eliminating the need for a thick seal, combined with additional layer deposition techniques to enhance battery capacity and efficiency.

Benefits of technology

This approach reduces processing time and cost while increasing battery capacity and minimizing the seal area, making it suitable for compact, high-capacity lithium thin film batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563854000001
    Figure 0007563854000001
  • Figure 0007563854000002
    Figure 0007563854000002
  • Figure 0007563854000003
    Figure 0007563854000003
Patent Text Reader

Abstract

A method for forming a thin-film battery includes forming a trench in a substrate, depositing a stencil on a top surface of the substrate, where the stencil is aligned with the trench, depositing a cathode in the trench, where the cathode layer is in direct contact with the stencil, and pressing the cathode layer into the trench to reduce a thickness of the cathode layer. Pressing the cathode layer into the trench includes applying isotropic pressure to the cathode layer using a pressure head. The method also includes depositing an electrolyte layer on top of the cathode layer, depositing an anode layer on top of the electrolyte layer, and depositing an anode-collector layer on top of the anode layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to thin film batteries, and more particularly to methods and structures for forming high capacity, compact lithium thin film batteries. [Background technology]

[0002] A typical thin-film lithium battery contains different layers of materials, including, but not limited to, a cathode, a separator, and an anode. The capacity of such batteries is generally limited by the thickness and structure of the cathode layer. Thus, a thick cathode layer can be interpreted as a battery with a high capacity, whereas a thin cathode layer can be interpreted as a battery with a low capacity. Furthermore, the layers are deposited using thin-film vacuum deposition techniques such as sputtering or plasma enhanced chemical vapor deposition. Summary of the Invention

[0003] According to one embodiment of the present invention, a method for forming a thin film battery is provided. The method can include forming a trench in a substrate, depositing a stencil on a top surface of the substrate, where the stencil is aligned with the trench, depositing a cathode in the trench, where the cathode layer is in direct contact with the stencil, and pressing the cathode layer into the trench to reduce a thickness of the cathode layer. Pressing the cathode layer into the trench includes applying isotropic pressure to the cathode layer using a pressure head. The stencil can be made from a high temperature polymer or a low temperature polymer. The method can include depositing a cathode collector layer along the sidewalls and bottom of the trench, depositing the cathode layer inside the trench, and pressing the cathode layer into the trench to reduce a thickness of the cathode layer. The method can also include depositing an electrolyte layer on top of the cathode layer, depositing an anode layer on top of the electrolyte layer, and depositing an anode collector layer on top of the anode layer.

[0004] According to another embodiment of the present invention, there is provided a method of forming a plurality of thin film batteries, the method including forming a plurality of trenches in a substrate, forming a plurality of dice channels in the substrate, where each of the plurality of dice channels is formed between each of the plurality of trenches, depositing a stencil on a top surface of the substrate, where the stencil is aligned with the trenches, depositing a cathode layer in the plurality of trenches, where the cathode layer directly contacts the stencil, and pressing the cathode layer into the plurality of trenches to reduce a thickness of the cathode layer.

[0005] According to another embodiment of the present invention, a structure is provided. The structure may include a cathode collector layer disposed along a substrate and a cathode layer embedded within the substrate, where a top surface of the cathode layer is substantially flush with the cathode collector layer. The structure may include an anode layer disposed on top of an electrolysis layer, where the electrolysis layer separates the cathode layer from the anode layer, an anode collector disposed on top of the anode layer, and an insulating layer disposed on top of the anode collector layer.

[0006] The following detailed description of the present invention is provided for purposes of example and is not intended to limit the present invention thereto, and is best understood in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a cross-sectional view illustrating a trench formed in a substrate in accordance with an example embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a cathode deposited according to an exemplary embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing a pressure head aligned on top of a cathode according to an exemplary embodiment. [Figure 4] FIG. 4 is a cross-sectional view of a polished cathode according to an exemplary embodiment. [Diagram 5] FIG. 5 is a cross-sectional view illustrating the deposition of an additional layer on top of a polished cathode layer according to an example embodiment. [Figure 6] FIG. 6 is a cross-sectional view illustrating a cover over the top of a deposited layer according to an exemplary embodiment. [Figure 7] FIG. 7 is a cross-sectional view illustrating multiple batteries according to an exemplary embodiment. [Figure 8A] FIG. 8A is a cross-sectional view illustrating multiple batteries according to an exemplary embodiment. [Figure 8B] FIG. 8B is a cross-sectional view illustrating multiple batteries according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The drawings are not necessarily to scale. The drawings are merely exemplary overviews and are not intended to illustrate specific parameters of the invention. The drawings are intended only to illustrate typical embodiments of the invention. In the drawings, like numbers represent like elements.

[0009] Although detailed embodiments of the claimed structures and methods are disclosed herein, it can be understood that the disclosed embodiments are merely exemplary of the claimed structures and methods, which can be embodied in various forms. The present invention, however, can be embodied in many different forms and should not be considered as being limited to the exemplary embodiments described herein. Rather, these exemplary embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. In this specification, details of well-known features and techniques may be omitted to avoid unnecessarily obscuring the present embodiments.

[0010] For purposes of the following description, the terms "upper", "lower", "right", "left", "vertical", "horizontal", "top", "bottom", and derivatives thereof, refer to the disclosed structures and methods as arranged in the illustrated drawings. The terms "overlying", "atop", "on top", "disposed on" or "disposed on" mean that a first element, such as a first structure, is above a second element, such as a second structure, where an intervening element, such as an interfacial structure, may be between the first element and the second element. The term "direct contact" means that a first element, such as a first structure, and a second element, such as a second structure, are joined at an interface between the two elements without any intermediate conductive, insulating, or semiconducting layers.

[0011] In the detailed description that follows, some process steps or operations known in the art may be combined with each other for presentation and illustration purposes, and in some instances may not be described in detail, so as not to obscure the presentation of the embodiments of the present invention. In other instances, some process steps or operations known in the art may not be described at all. Rather, it should be understood that the following description focuses on the distinctive features or elements of various embodiments of the present invention.

[0012] FIELD OF THE DISCLOSURE

[0002] Embodiments of the present invention relate generally to high capacity, compact lithium thin film batteries, and more particularly to structures and methods for forming high capacity lithium thin film batteries having small sealing surface areas.

[0013] Typically, thin-film lithium batteries are fabricated from different materials, where each material is stacked on top of one another. Such layers can include, but are not limited to, a cathode collector layer, a cathode layer, an electrolyte layer, an anode layer, an anode collector layer, and a shielding layer. Furthermore, the capacity of conventional thin-film lithium batteries is generally limited by the thickness and structure of the cathode layer. Thus, a thicker cathode layer can be interpreted as a larger capacity, while a thinner cathode can be interpreted as a lower capacity.

[0014] Generally, these layers are deposited using different vacuum deposition techniques such as sputtering. However, these vacuum deposition techniques are limited by their deposition rates. Therefore, using sputtering deposition techniques to manufacture thin-film lithium batteries is time-consuming and expensive. Moreover, it is more time-consuming and expensive to manufacture large-capacity batteries because such batteries require thicker cathodes, which translates into longer sputtering times to deposit the thicker cathodes. In addition, since lithium is highly reactive, such batteries require large seals to protect the lithium layers from contaminants such as water or oxygen. As a result, the batteries manufactured are also larger than 10 mm. 2 ~1000mm 2 and the seal itself has a surface area of ​​at least 1 mm 2 It is.

[0015] With the advancement of technology, the new emergence of Internet of Things sensors and smart devices requires 10mm 2 Therefore, a battery with a large capacity and a total surface area including the seal of less than 10 mm2 may be required. 2 , preferably 1 mm 2There is a need to develop thin film lithium batteries with total surface areas smaller than 10 mm. In addition, there is a need to reduce processing costs to levels well below those that can be achieved using current thin film technology. To this end, embodiments of the present invention provide a method for fabricating thin film lithium batteries with total surface areas smaller than 10 mm while reducing processing times and costs. 2 BRIEF SUMMARY OF THE DISCLOSURE The present invention provides a structure and method for producing a high capacity battery having a total surface area of ​​less than 100 nm.

[0016] 1, a structure 100 is shown according to an embodiment. The structure 100 may include a substrate 102, a cathode collector layer 104, a stencil 106, and a trench 108. The substrate 102 may include a silicon-based material. Exemplary silicon-based materials suitable for the substrate 102 may include, but are not limited to, silicon, silicon, silicon-germanium, silicon-germanium-carbon, silicon-carbon, and multilayers thereof. In an embodiment, the substrate 102 may be multi-doped silicon to allow for back electrode connection.

[0017] The substrate 102 may be patterned using known lithography techniques to form trenches 108. The substrate 102 may also be etched to form trenches 108. For example, reactive ion etching may be used to etch the trenches 108 into the substrate 102. Once the trenches 108 are formed, the cathode collector layer 104 is conformally deposited on the top surface of the substrate 102 and along the sidewalls and bottom of the trenches 108. The cathode collector layer 104 may be deposited using different deposition processes, such as, for example, evaporation, chemical vapor deposition, atomic layer deposition, sputtering, or other suitable deposition processes.

[0018] The cathode collector layer 104 can be formed from a non-reactive material, such as, for example, copper, silver, gold, platinum, or any other non-reactive material. The cathode collector layer 104 is electrically conductive and acts as a barrier. In addition to providing a current path to the cathode (110), the cathode collector layer 104 can block impurities found in the substrate 102 and the environment that collect in other layers that may be deposited on top of the top surface of the cathode collector layer 104.

[0019] The stencil 106 may be deposited on the top surface of the cathode collector layer 104 using any suitable known deposition technique as described herein above. In an embodiment, the stencil 106 is deposited on the top surface of the cathode collector layer 104 and on the sidewalls and bottom of the trench 108. Once the stencil 106 is deposited, it may be patterned using known techniques to remove the stencil 106 previously deposited in the trench 108. As a result, the trench 108 is surrounded by the cathode collector layer 104 and does not have any stencil 106 therein. The stencil 106 only remains on the top surface of the cathode collector layer 104 on top of the top surface of the substrate 102.

[0020] The stencil 106 further defines a patterned trench 108 in the substrate 102. Because the stencil 106 only remains on the top surface of the cathode collector layer 104, the stencil 106 extends to the top surface of the cathode collector layer 104 and to the sidewalls of the trench 108 above the substrate 102. As a result, the sidewall of the stencil 106 closest to the trench 108 is substantially aligned with the sidewall of the trench 108. The stencil 106 also protects the cathode collector layer 104 from subsequent processing steps in battery fabrication.

[0021] The stencil 106 can also be removable and fabricated from a different polymer. For example, if a low temperature pressurized processing step is subsequently used to form the cathode layer, the stencil 106 is fabricated from a high temperature pressurizable polymer. However, if a high temperature pressurized processing step is subsequently used to form the cathode layer, the stencil 106 is formed from a low temperature polymer.

[0022] 2, after the stencil 106 is deposited on the top surface of the cathode-collector layer 104, a cathode layer 110 is deposited in the trenches 108. The cathode layer 110 may be, for example, LiCO 2 , LiMn 2 O 4 , LiFePO 4 or other suitable cathode materials (e.g., metal oxides). Once deposited, the cathode layer 110 extends over the top surface of the cathode collector layer 104 but below the top surface of the stencil 106. As such, the cathode layer 110 is contained within the trench 108 inside the sidewalls created by the stencil 106 and in direct contact with portions of the sidewalls of the stencil 106. In an embodiment, the cathode layer 110 extends over the top surface of the cathode collector layer 104 such that after further processing, as described with reference to Figures 3-4 herein, the cathode layer 110 can be substantially flush with the top surface of the cathode collector layer 104 that extends along the top surface of the substrate 102, describing the initial and final desired density of the cathode layer 110.

[0023] 3, a pressure head 112 is positioned directly above the cathode layer 110. The pressure head 112 may be formed of the same material as the substrate 102, for example, silicon, or any other suitable material. Positioning of the pressure head 112 is aided by the sidewalls of the stencil 106, which extend above the top surface of the cathode layer 110. As a result, the pressure head 112 fits directly above the cathode layer 110 between the areas formed by the stencil 106.

[0024] Once the pressure head 112 is positioned, it is used to isotropically press the cathode layer 110 into the trenches patterned in the substrate 102. The cathode layer 110 is first deposited into the trenches 108 such that the cathode layer 110 fits into the trenches 108 and extends above the top surface of the cathode collector layer 104 but below the top surface of the stencil 106. This results in more cathode layer 110 being deposited than is necessary to just fill the trenches 108. This is accomplished by reducing the thickness of the cathode layer 110 as it is pressed into the trenches patterned in the substrate 102.

[0025] Isostatic pressing of the cathode layer 110 can be done at either low or high temperatures. In embodiments, the cathode layer 110 can be isostatically pressed or compressed at a low temperature that the stencil 106 can accommodate. Once the cathode layer 110 is compressed, the stencil 106 is removed and the cathode layer 110 is further pressed and heated. During isostatic pressing, the pressure head 112 applies equal pressure in all directions and presses down on the cathode layer 110 to densify it.

[0026] Typically, when a deposition technique such as sputtering is used to deposit the cathode, a polishing step is required before subsequently depositing additional layers on top of the cathode. The sputtering deposition step can introduce impurities to the cathode. Using a pressure head 112 to compress the cathode layer 110 produces a dense cathode layer 110 that is free of impurities. After compressing it using the pressure head 112, the cathode layer 110 has a clean interface that can be subsequently patterned and sealed.

[0027] Additionally, compressing the cathode layer 110 using the pressure head 112, rather than as in a conventional sputtering deposition process, allows for control of the porosity of the cathode layer 110. The porosity of the cathode layer 110 can be controlled by controlling the properties of the deposited cathode layer 110, for example, the properties of the cathode layer 110 referring to the shape of the particles that form the cathode layer 110.

[0028] The porosity of the cathode layer 110 can also be controlled by the amount of pressure applied by the pressure head 112 to the cathode layer 110. For example, the same thickness of the cathode layer 110 is deposited in both scenarios. In the first scenario, if more pressure is applied by the pressure head 112 to the cathode layer 110, the cathode layer 110 can be more densely packed. However, in the second scenario, if less pressure is applied by the pressure head 112, the cathode layer 110 is packed but it is less dense and more porous.

[0029] The porosity of the cathode layer 110 can be controlled by the duration of compression of the cathode layer 110. For example, the duration of compression of the cathode layer 110 by the pressure head 112 results in different densities of the cathode layer 110. For example, the same thickness of the cathode layer 110 is deposited. If the duration of compression is short, the cathode layer 110 is less dense compared to if the duration of compression is longer.

[0030] The porosity of the cathode layer 110 can also be controlled by the temperature at which the cathode layer 110 is compressed. Under the sintering process, the cathode layer 110 can be compressed, which causes the particles that form the cathode layer 110 to adhere and bond to one another, forming a cathode layer 110 that is less porous than the cathode layer 110 that was originally deposited in the trench (108).

[0031] Additionally, the cathode layer 110 is combined with additives that increase the efficiency of the battery. In an embodiment, the cathode layer 110 can be combined with a low vapor pressure ionic liquid electrolyte to increase the performance of the cathode layer 110. In another embodiment, the cathode layer 110 can be combined with conductive carbon, which also increases the performance of the cathode layer 110 by increasing its electrical conductivity. In an embodiment, if a hot press is used to compress the cathode layer 110, then the ionic liquid electrolyte can be added to the cathode layer 110 by flowing the ionic liquid electrolyte into the compressed cathode layer 110 via capillary forces. In an alternative embodiment, if a cold press is used to compress the cathode layer 110, then the ionic liquid electrolyte can be added to the cathode layer 110 before the cathode layer is compressed with the press head 112.

[0032] 4, the cathode layer 110 is compressed so that the top surface of the cathode layer 110 is substantially flush with the top surface of the cathode collector layer 104 that extends along the top surface of the substrate 102. To fully ensure this, the cathode layer 110 is deposited such that when compressed by the pressing head 112, the cathode layer 110 is substantially flush with the cathode collector layer 104. Generally, when manufacturing lithium batteries, the cathode layer is deposited on top of the cathode collector layer 104 using a deposition process, such as sputtering. As described herein above, the thicker the cathode layer 110, the greater the capacity of the battery. This is therefore useful for manufacturing batteries with thick cathode layers 110. However, conventional deposition processes are time consuming and expensive. The use of a pressure head 112 to hot or cold press the cathode layer 110 into the trench 108 (FIG. 1) produces a cathode layer 110 of a desired thickness and density than would be achieved if deposited using conventional techniques, further increasing the capacity of the battery.

[0033] Embedding the cathode layer 110 in the substrate 102 also reduces the seal area of ​​the battery. As described herein above, when making a conventional battery, the cathode layer is deposited on top of the cathode collector layer, and the cathode collector layer is deposited on top of the substrate. As a result, a conventional battery has stacked layers that need to be sealed. The seal needs to be made thicker to fit the shape of the cathode. This in turn requires a larger seal area. Furthermore, to make a high efficiency battery, the thickness of the cathode layer is increased. This accounts for a larger seal area since the additional stack of layers is higher. With a higher layer stack, the seal area is increased to protect the layers from environmental sources of contamination.

[0034] In the embodiment, the cathode layer 110 no longer sits on the top surface of the substrate 102. Instead, the cathode layer 110 is embedded within the substrate 102, and the top surface of the cathode layer 110 is substantially flush with the top surface of the cathode collector layer 104. Because the cathode layer 110 is no longer deposited on top of the substrate 102, there is not as much stacking of layers as there is when fabricating a conventional battery in which the cathode layer is deposited on top of the substrate. The lower stacking of layers accounts for the smaller seal area. Additionally, fabrication of a battery with a thicker cathode layer 110 does not increase the stacking height because the cathode layer 110 is embedded further within the substrate 102 and the cathode layer 110 does not extend above the top surface of the cathode collector layer 104.

[0035] In embodiments, once the cathode layer 110 is isotropically compressed, a surface planarization process can be used to smooth the top surface of the cathode layer 110 and prepare it for further processing.

[0036] 5, once the cathode layer 110 is compressed, additional layers are deposited on the top surfaces of the cathode layer 110 and the cathode collector layer 104. Deposition of the additional layers can be accomplished using standard techniques. The additional layers include, but are not limited to, an electrolyte layer 114, an anode layer 116, an anode collector layer 118, and a shield layer 120.

[0037] The electrolyte layer 114 includes a solid electrolyte that provides in-situ processing without breaking the hermetic seal. In an embodiment, the electrolyte layer 114 can include a thin solid film, such as LiPON, or a spin-on sol-gel, although other materials can be used. The electrolyte layer can be deposited by evaporation, chemical vapor deposition, sputtering, or other suitable deposition process. The electrolyte layer 114 can be deposited on the top surface of the cathode layer 110 between the cathode layer 110 and the anode layer 116, separating the layers 110, 116. The electrolyte layer 114 can provide ionic conductivity between the cathode layer 110 and the anode layer 116.

[0038] An anode layer 116 may be deposited on the top surface of the electrolyte layer 114. The anode layer 116 may be formed of lithium, a lithium alloy, or any other suitable material. The anode layer 116 may be deposited by evaporation, chemical vapor deposition, sputtering, or other suitable deposition process.

[0039] The anode collector layer 118 may be deposited on the top surface of the anode layer 116. The anode collector layer 118 provides a current path for the anode layer 116. The anode collector layer 118 may be formed from a non-reactive material, such as, for example, copper, silver, gold, platinum, or any other suitable material. The anode collector layer 118 may be deposited by evaporation, chemical vapor deposition, sputtering, or other suitable deposition process. In an embodiment, the anode collector layer 118 may be in direct contact with the substrate 102 to form a seal. In an embodiment, the anode collector layer 118 and the cathode collector layer 104 are both exposed from the seal but are not in direct contact with each other.

[0040] A shielding layer 120 may be deposited on the top surface of the anode-collector layer 118. The shielding layer 120 may be made of a conductive material, such as aluminum, or any other suitable material. The shielding layer 120 may maintain electrical insulation of the structure from the external environment.

[0041] 6, a cap layer 122 is deposited on the top surface of the shielding layer 120. The cap layer 122 can be formed from the same silicon-based materials that form the substrate 102, such as silicon, silicon, silicon-germanium, silicon-germanium-carbon, silicon-carbon, and multilayers thereof. The cap layer 122 can also be formed from any combination of materials that exhibit low permeability to oxygen, water, and other species that degrade batteries. Exemplary examples of such materials can include, but are not limited to, metal films, multilayer metal films, insulator films, multilayer insulator films, or multilayer metal and insulator films. The cap layer 122 can be formed by chemical vapor deposition, sputtering, evaporation, or any other suitable deposition process.

[0042] The cap layer 122 covers the cathode-collector layer 104, the cathode layer 110, the electrolyte layer 114, the anode layer 116, the anode-collector layer 118, and the shielding layer 120. The cap layer 122 protects these layers from exposure to environmental elements, corrosion, or damage. In an embodiment, the cap layer 122 is deposited on top of the shielding layer 120. In an alternative embodiment, the cap layer 122 is not deposited on top of the shielding layer 120. Instead, the shielding layer 120 is the top layer of the structure 100. However, it is more beneficial to cover the other layers, including the shielding layer 120, with the cap layer 122, since the cap layer 122 shields from environmental elements better than the shielding layer 120, increasing the shelf life of the structure 100.

[0043] Conventional batteries are typically patterned with isolation vias through either the insulating or separator layers to access the cathode or anode. In addition, contacts are typically formed on the anode side of the battery. In an embodiment, for example, the anode contact can be formed by patterning an isolation via through the shielding layer 120. However, the cathode contact can be formed using a conductive cathode substrate, for example, multiply doped silicon. If a conductive cathode substrate is used, the cathode collector layer 104 can be in ohmic contact with the substrate 102, allowing for the patterning of a backside ohmic metal contact. The backside contact occupies less area compared to conventional anode side (or front side) connection schemes, allowing for the use of more area for electrochemical materials.

[0044] 7, there is illustrated a structure 200. The structure 200 represents multiple structures 100, or a battery, fabricated side-by-side on a single wafer. Although only two structures 100 are illustrated, embodiments of the present invention contemplate multiple structures 100 fabricated on a single substrate 102, as described herein with reference to FIGS. 1-6.

[0045] 8A and 8B, both of which illustrate a structure 200 having two or more batteries (100). FIG. 8A shows a structure 200 fabricated using conventional sputtering processing, and FIG. 8B shows a structure 200 fabricated according to the present invention. The structure 200 can include multiple batteries, each of which includes a cathode layer 110. It should be noted that other components of the battery (100) have been omitted from FIGS. 8A and 8B for clarity and understanding. After forming the battery (100), the structure 200 is cut or diced along lines 124 to produce multiple individual batteries. As discussed herein above, the fabrication of batteries using conventional sputtering processing produces batteries with a larger seal area relative to the area of ​​their cathode layer 110 due to the stack of layers that need to be sealed and protected from environmental contaminants. In addition, the larger seal area is also necessary to protect the integrity of the layers during cutting of the structure 200 when separating into individual batteries. Therefore, compared to batteries produced according to the present invention, conventional processing results in batteries having smaller cathode layers 110 and larger seal areas.

[0046] As described herein above with reference to Figures 1-6 and shown in Figure 8B, by embedding the cathode layer 110 within the substrate 102, the size of the cathode layer 110 can be increased and the seal area can be reduced / decreased while maintaining the same dicing footprint. Because the cathode layer 110 no longer extends above the substrate 102, less layer stacking is possible, thereby reducing the seal while maintaining the function and physical integrity of the individual battery structure (100). As a result of the reduced size of the seal area / width, the cathode layer 110 can be increased (width / length), thus increasing the capacity of the battery.

[0047] Additionally, while etching trenches in the substrate 102 (FIG. 1), dicing channels 126 can also be simultaneously etched in the substrate 102. The dicing channels 126 can be disposed between and define the edges of each structure 100 (FIG. 7). The dicing channels 126 are small channels in the substrate 102 that aid in cutting the substrate to form single structures 100.

[0048] In an embodiment of the present invention, dicing channels 126 are added to reduce stresses applied when the structure 200 is cut into individual batteries (structure 100). The dicing channels 126 allow each battery to maintain its seal integrity. In addition, each cathode layer 110 can be made larger because a larger seal area is no longer necessary. Thus, by including dicing channels 126 and embedding the cathode layer 110 within the substrate 102, an embodiment of the present invention provides a battery whose seal-to-cathode layer 110 ratio is reduced compared to the seal-to-cathode layer 110 ratio of a conventional battery. As such, the total surface area of ​​the battery is also reduced from that of a conventional battery.

[0049] The description of various embodiments of the present disclosure has been presented for illustrative purposes, but is not intended to be exclusive or limited to the disclosed embodiments. Many modifications or variations will be obvious to those skilled in the art without departing from the scope and spirit of the present disclosure. The terms used in this specification are selected to best explain the principles of the present embodiments, practical applications, or technical improvements beyond the technology found in the market, or to allow others skilled in the art to understand the embodiments disclosed herein.

Claims

1. 1. A method for forming a thin film battery, the method comprising: forming a trench in a substrate; depositing a stencil on a top surface of the substrate having sidewalls aligned with sidewalls of the trench; depositing a cathode layer in the trench in direct contact with the stencil; and pressing the cathode layer into the trench to reduce a thickness of the cathode layer; A method comprising:

2. moreover, depositing a cathode collector layer along the sidewalls and bottom of the trench; depositing the cathode layer in the trench; and forcing the cathode layer into the trench to reduce a thickness of the cathode layer; The method of claim 1 , comprising:

3. The method of claim 1 or 2, wherein depositing the cathode layer in the trench includes depositing the cathode layer along portions of a sidewall of the stencil.

4. The method of any one of claims 1 to 3, wherein pressing the cathode layer into the trench comprises applying isotropic pressure to the cathode layer using a pressure head.

5. moreover, depositing an electrolyte layer on top of the cathode layer; depositing an anode layer on top of the electrolyte layer; and depositing an anode collector layer on top of said anode layer; The method according to any one of claims 1 to 4, comprising:

6. The method of any one of claims 1 to 5, further comprising adding an ionic liquid electrolyte to the cathode layer.

7. The method of any one of claims 1 to 6, wherein the substrate is multiply doped silicon and, as a result of the substrate being multiply doped silicon, a rear cathode contact is patterned on the substrate.

8. 1. A method for forming a thin film battery, the method comprising: forming a plurality of trenches in the substrate, each trench corresponding to a different one of the batteries; forming a plurality of dicing channels in the substrate between each of the plurality of trenches; and Forming each of said batteries by the method according to any one of claims 1 to 7. The method includes:

9. each said dicing channel is formed in said substrate using reactive ion etching; The method according to claim 8.

Citation Information

Patent Citations

  • Biomedical energization elements with polymer electrolytes and cavity structures

    JP2017103222A

  • Solid electrolyte cell and production method thereof

    WO2002065573A1

Cited By

  • High capacity compact lithium thin film battery

    US12506137B2