Light-absorbing composition, light-absorbing film, optical filter, and method for producing optical filter

A light-absorbing composition with phosphonic acid and copper components addresses the inefficiencies of existing filters by effectively blocking ultraviolet and infrared light, aligning spectral sensitivity with human visibility, and improving image quality in imaging devices.

JP7564278B2Active Publication Date: 2024-10-08NIPPON SHEET GLASS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023064681
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-08
Estimated Expiration
2039-07-16

AI Technical Summary

Technical Problem

Existing optical filters, such as those described in Patent Documents 1 and 2, struggle to effectively block light around a wavelength of 400 nm, which is crucial for aligning spectral sensitivity with human visibility and improving image quality in imaging devices.

Method used

A light-absorbing composition containing phosphonic acid and a copper component, formulated to achieve specific transmittance ratios at wavelengths of 400 nm, 550 nm, and 800 nm, ensuring effective blocking of ultraviolet and infrared light while maintaining high transmittance in the visible range, is used to create a light-absorbing film and optical filter.

Benefits of technology

The composition achieves desired optical properties by effectively blocking ultraviolet and infrared light, aligning spectral sensitivity with human visibility, and reducing ghosting and flare occurrences, while allowing high transmittance in the visible range, thus enhancing image quality in imaging devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564278000010
    Figure 0007564278000010
  • Figure 0007564278000011
    Figure 0007564278000011
  • Figure 0007564278000012
    Figure 0007564278000012
Patent Text Reader

Abstract

To provide technique advantageous for providing a light absorption film or an optical filter having desired optical characteristics.SOLUTION: A light-absorbing composition according to the present invention contains a light-absorbing agent formed of phosphonic acid and a copper component. In a light absorption film obtained by curing the light-absorbing composition, the transmissivity T400 at a wavelength of 400 nm, the transmissivity T550 at a wavelength of 550 nm, and the transmissivity T800 at a wavelength 800 nm satisfy the conditions of 4≤T550 / T400 and 8≤T550 / T800.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a light-absorbing composition, a light-absorbing film, and an optical filter. [Background technology]

[0002] CCD (Charge Coupled Device) or CMOS (Complementary Metal Oxide Semiconductor) In imaging devices using solid-state imaging elements such as the IR-1000 and IR-10000 series, various optical filters are arranged in front of the solid-state imaging element in order to obtain images with good color reproducibility. In general, solid-state imaging elements have spectral sensitivity in a wide wavelength range from the ultraviolet region to the infrared region. Meanwhile, human visual sensitivity exists only in the visible light region. For this reason, a technique is known in which an optical filter that blocks part of infrared or ultraviolet light is arranged in front of the solid-state imaging element in order to bring the spectral sensitivity of the solid-state imaging element in the imaging device closer to the human visual sensitivity.

[0003] Conventionally, such optical filters generally use light reflection by a dielectric multilayer film to block infrared or ultraviolet rays. Meanwhile, in recent years, optical filters with a film containing a light absorbent have been attracting attention. The transmittance characteristics of an optical filter with a film containing a light absorbent are not easily affected by the angle of incidence, so that even if light is obliquely incident on the optical filter in an imaging device, a good image with little change in color can be obtained. In addition, a light-absorbing optical filter that does not use a light-reflecting film can suppress the occurrence of ghosts and flares caused by multiple reflections by the light-reflecting film, so that good images can be easily obtained in backlit conditions or when photographing night scenes. In addition, an optical filter with a film containing a light absorbent is also advantageous in terms of miniaturizing and thinning the imaging device.

[0004] As such a light absorbing agent, a light absorbing agent formed by phosphonic acid and copper ions is known. For example, Patent Document 1 describes an optical filter having a light absorbing layer containing a light absorbing agent formed by phosphonic acid having a phenyl group or a halogenated phenyl group and copper ions.

[0005] Patent Document 2 also describes an optical filter having a UV-IR absorbing layer capable of absorbing infrared and ultraviolet rays. The UV-IR absorbing layer contains a UV-IR absorbent formed of phosphonic acid and copper ions. The UV-IR absorbing composition contains, for example, a phenyl-based phosphonic acid and an alkyl-based phosphonic acid so that the optical filter meets certain optical properties. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2018 / 088561 [Patent Document 2] Patent No. 6232161 Summary of the Invention [Problem to be solved by the invention]

[0007] The optical filters described in Patent Documents 1 and 2 have room for improvement in terms of effectively blocking light with a wavelength of about 400 nm. Therefore, the present invention provides a technique that is advantageous for providing a light absorbing film or an optical filter having desired optical characteristics that are difficult to achieve with the techniques described in Patent Documents 1 and 2. [Means for solving the problem]

[0008] The present invention relates to 1. A light absorbing composition comprising: Contains a light absorber formed by a phosphonic acid and a copper component, In the transmittance spectrum at an incident angle of 0 degrees of the light-absorbing film obtained by curing the light-absorbing composition, the transmittance T 400 , transmittance at wavelength 550 nm T 550 , and transmittance T at a wavelength of 800 nm 800 4≦T 550 / T 400 and 8≦T 550 / T 800 Fulfill the conditions of A light absorbing composition is provided.

[0009] The present invention relates to Contains a light absorber formed by a phosphonic acid and a copper component, In the transmittance spectrum at an incident angle of 0 degrees, the transmittance T at a wavelength of 400 nm 400 , transmittance T at wavelength 550 nm 550 , and transmittance T at a wavelength of 800 nm 800 4≦T 550 / T 400 and 8≦T 550 / T 800 Fulfill the conditions of A light absorbing film is provided.

[0010] The present invention also provides an optical filter comprising the above light absorbing film. Effect of the Invention

[0011] The light-absorbing composition is advantageous in providing a light-absorbing film having desired optical properties. The light-absorbing film and the optical filter tend to have desired optical properties. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a light absorbing film according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of an optical filter according to the present invention. [Diagram 3]FIG. 3 shows the transmittance spectrum of the optical filter according to the first embodiment. [Figure 4] FIG. 4 shows the transmittance spectrum of the optical filter according to Example 1 after the baking treatment. [Diagram 5] FIG. 5 shows the transmittance spectrum of the optical filter according to the second embodiment. [Figure 6] FIG. 6 shows the transmittance spectrum of the optical filter according to Example 2 after the baking treatment. [Figure 7] FIG. 7 shows the transmittance spectrum of the optical filter according to the third embodiment. [Figure 8] FIG. 8 shows the transmittance spectrum of the optical filter according to the fourth embodiment. [Figure 9] FIG. 9 shows the transmittance spectrum of the optical filter according to the fifth embodiment. [Figure 10] FIG. 10 shows the transmittance spectrum of the optical filter according to Comparative Example 1. As shown in FIG. [Figure 11] FIG. 11 shows the transmittance spectrum of the optical filter according to Comparative Example 2. As shown in FIG. [Figure 12] FIG. 12 shows the transmittance spectrum of a transparent glass substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In recent years, there has been a demand for optical filters that can effectively block light in a specific wavelength range, including some ultraviolet light. For example, there has been a demand for optical filters that have a high spectral transmittance in the visible light range, a high light blocking ability in the infrared and ultraviolet ranges, and can effectively block light with a wavelength of about 400 nm.

[0014] The optical filter described in Patent Document 1 has a UV cutoff wavelength of less than 400 nm, and its ultraviolet absorbing ability is not sufficient. In this specification, the UV cutoff wavelength is a wavelength at which the transmittance is 50% in the wavelength range of 300 nm to 480 nm.

[0015] In the optical filter described in Patent Document 2, it is considered that the specifications required for an optical filter are easily satisfied by containing phenyl-based phosphonic acid and alkyl-based phosphonic acid. This is because phenyl-based copper phosphonate absorbs light in the range of relatively short wavelengths in the near infrared. This is because alkylphosphonic acid copper is likely to absorb light in the relatively long wavelength range of near infrared rays, and alkylphosphonic acid copper is likely to absorb light in the relatively long wavelength range of near infrared rays. However, in the transmittance spectrum of the optical filter described in Patent Document 2, the transmittance at a wavelength of 400 nm is 20% or more, and it is difficult to say that it can effectively block light with a wavelength of around 400 nm.

[0016] Therefore, the present inventors have conducted extensive research to realize desired optical characteristics in a light absorbing film and an optical filter that are difficult to achieve with the techniques described in Patent Documents 1 and 2, and have completed the present invention.

[0017] Hereinafter, an embodiment of the present invention will be described. Note that the following description is merely an example of the present invention, and the present invention is not limited to the following embodiment.

[0018] The light-absorbing composition according to the present invention contains a light-absorbing agent formed of a phosphonic acid and a copper component. The light-absorbing film obtained by curing this light-absorbing composition has a transmittance T at a wavelength of 400 nm in a transmittance spectrum at an incident angle of 0 degrees. 400 , wavelength 550nm Transmittance T 550 , and transmittance T at a wavelength of 800 nm 800 4≦T 550 / T 400 and 8≦T 550 / T 800 Meet the conditions.

[0019] Transmittance T 400 , transmittance T 550 , and transmittance T 800 Preferably, 8≦T 550 / T 400 and 2 8≦T 550 / T 800and more preferably 16≦T 550 / T 400 and 60≦T 550 / T 800 and more preferably, 20≦T 550 / T 400 and 80≦T 550 / T 800 Meet the conditions.

[0020] The light absorbing agent includes, for example, a first light absorbing agent. The first light absorbing agent is formed of a first phosphonic acid represented by the following formula (A) and a copper component. The light absorbing composition contains the first light absorbing agent, and the light absorbing film obtained by curing the light absorbing composition has a viscosity of 4≦T 550 / T 400 and 8≦T 550 / T 800 This is advantageous in terms of satisfying the above conditions.

[0021] [ka] [In formula (A), R1 is a substituent exhibiting electron donating properties, and a plurality of R1 may be present in formula (A). R2 is an alkylene group having 1 to 3 carbon atoms, and In the above, R2 may be absent.

[0022] The light absorbing agent further includes, for example, a second light absorbing agent. The second light absorbing agent is formed of a second phosphonic acid, which is a phosphonic acid represented by the following formula (B), and a copper component. It is advantageous for the light absorbing composition to contain the second light absorbing agent in terms of realizing good dispersion of the light absorbing agent in the light absorbing composition.

[0023] [ka] [R 21is an alkyl group, a halogenated alkyl group in which at least one hydrogen atom is substituted with a halogen atom, an aryl group, or a halogenated aryl group in which at least one hydrogen atom is substituted with a halogen atom.

[0024] π-π of benzene rings in organic compounds * In the optical absorption based on transitions, the benzene ring When an electron-donating substituent is bonded to the benzene ring, the π-electron band is affected by the electrons donated by the substituent. For example, when an electron-donating substituent is bonded to the benzene ring, a bathochromic effect accompanied by a red shift that moves the absorption spectrum to the long wavelength side is easily exhibited compared to when such a substituent is not bonded to the benzene ring. Since the first light absorber has the substituent R1, the wavelength (λmax) at which the absorption is maximum in the first light absorber is easily lengthened. This makes it easy to appropriately absorb light in a wavelength range that includes part of ultraviolet light and includes a wavelength of 400 nm. However, according to the study by the present inventors, the first light absorber is easily aggregated in the light absorbing composition alone. On the other hand, the present inventors have newly found that the first light absorber is less likely to aggregate in the light absorbing composition when the light absorbing composition contains a second light absorber in addition to the first light absorber. For this reason, it is easy to realize a light absorbing film or optical filter having desired optical properties using the light absorbing composition.

[0025] Conventionally, when a copper complex or the like is used as a light absorbing agent, the transmittance spectrum of the optical filter includes part of ultraviolet light, and does not sufficiently block light in a wavelength range including a wavelength of 400 nm. Therefore, when an optical filter containing such a light absorbing agent is used in an imaging device, there is a possibility that the discrepancy between the characteristics of the optical filter and the visual sensitivity of humans may become a problem. On the other hand, the light absorbing composition contains a first light absorbing agent formed by a phosphonic acid having a substituent R1, Therefore, the use of a light absorbing composition can eliminate such problems.

[0026] Substituent R1 is not limited to a specific group as long as it exhibits electron donating properties. Substituent R1 is, for example, a substituent with a negative Hammett's substituent constant (σp) at the para position, or a halogen group. In this case, it is easier to realize a light absorbing film or optical filter having desired optical properties by using the light absorbing composition.

[0027] Substituents with a negative Hammett substituent constant (σp) at the para position are not limited to specific groups. Substituents that satisfy this condition are groups such as a hydroxy group, an alkoxy group, an alkyl group, and an amino group. Examples of substituents with a negative Hammett substituent constant (σp) at the para position, together with the value of the substituent constant (σp), include a hydroxy group (-OH; σp = -0.37), a methoxy group (-O-CH3; σp = -0.27), an ethoxy group (-O-CH3; σp = -0.27), and an ethoxy group (-O-CH3; σp = -0.27). oxy group (-O-CH2CH3; σp=-0.24), methyl group (-CH3; σp=-0.1 7), ethyl group (-CH2CH3; σp = -0.15), n-propyl group (-CH2CH2CH3; σp = -0.13), isopropyl group (-CH(CH3)2; σp = -0.15), n-Butyl group (-CH2CH2CH2CH3; σp=-0.16), isobutyl group (-CH2 CH(CH3)2;σp=-0.12), s-butyl group (-CH(CH3)CH2CH3;σ p = -0.12), t-butyl group (-C(CH3)3; σp = -0.20), and amino group (-NH2; σp = -0.66).

[0028] When the substituent constant (σp) of a substituent is negative, typically, the larger its absolute value, the more likely it is to be a substituent. The electron donating property of the substituent is high. In formula (A), the substituent constant (σp) of R1 is -0.1 This makes it easier to obtain a light absorbing film or an optical filter having desired optical characteristics.

[0029] In formula (A), the substituent constant (σp) of R1 may be -0.2 or less. In the formula (I), the substituent constant (σp) of R1 is, for example, −0.8 or more, and −0.7 or more. It's fine.

[0030] For the substituent constant (σp) of a given substituent, reference can be made, for example, to the following literature: International Publication No. 2010 / 024441 Yusuke Miyano, "Hammett's Rule", Journal of the Society of Synthetic Organic Chemistry, Society of Synthetic Organic Chemistry, August 1965, Vol. 23, No. 8, pp. 631-642 Miki Akamatsu, "QSAR parameters and their applications", Journal of the Pesticide Science Society of Japan, Pesticide Science Society of Japan, August 2013, Vol. 38, No. 2, pp. 195-203 John A. Dean, “LANGE'S HANDBOOK OF CHEMISTRY fifteenth edition”, McGRAW-HILL, INC., 1998

[0031] In formula (A), the substituent R1 may be a halogen group. The Hammett's substituent constant (σp) in is positive. For example, the substituent constant (σp) of -F is 0.06, the substituent constant (σp) of -Cl is 0.23, the substituent constant (σp) of -Br is 0.23, and the substituent constant (σp) of -I is 0.18. Substituents with positive substituent constants (σp) typically exhibit electron-withdrawing properties. However, halogen groups have an unshared electron pair and can exhibit electron-donating properties at the site corresponding to the benzene ring in the phosphonic acid shown in formula (A). As a result, when the substituent R1 is such a halogen atom, Even if the thickness is small, it is possible to realize a light absorbing film or an optical filter having desired optical characteristics.

[0032] In formula (A), the substituent R1 is, for example, in the para or ortho position. By using the absorbing composition, it is easy to realize a light absorbing film or an optical filter having desired optical properties more reliably. In other words, the substituent R1 is a p (para)-oriented group or an o (ortho)-oriented group. The orientation of the substituent R1 in the phosphonic acid shown in formula (A) may be It is determined based on the group containing the phosphorus atom that is bonded to the Zene ring.

[0033] In formula (A), the phosphorus atom may be directly bonded to the benzene ring. In other words, the phosphonic acid represented by formula (A) may be a phosphonic acid represented by the following formula (A-1). In this case, it is easier to realize a light-absorbing film or optical filter having desired optical properties by using the light-absorbing composition more reliably.

[0034] [ka]

[0035] The phosphonic acid represented by formula (A) is not limited to a specific phosphonic acid. Examples of the phosphonic acid represented by formula (A) include the following phosphonic acids. 4-Hydroxyphenylphosphonic acid, 4-Methoxyphenylphosphonic acid, 4-Ethoxyphenylphosphonic acid, 4-Methylphenylphosphonic acid, 4-Ethylphenylphosphonic acid, 4-Normalpropylphenylphosphonic acid, 4-Isopropylphenylphosphonic acid, 4- n-Butylphenylphosphonic acid, 4-isobutylphenylphosphonic acid, 4-sec-butylphenylphosphonic acid, 4-tert-butylphenylphosphonic acid, 4-aminophenylphosphonic acid, 4-fluorophenylphosphonic acid, 4-chlorophenylphosphonic acid, 4-bromophenylphosphonic acid, 4-iodophenylphosphonic acid, 2-hydroxyphenylphosphonic acid, 2-methoxyphenylphosphonic acid, 2-ethoxyphenylphosphonic acid, 2-methylphenylphosphonic acid, 2-ethylphenylphosphonic acid, 2-n-propylphenylphosphonic acid, 2-isopropylphenylphosphonic acid, isopropylphenylphosphonic acid, 2-n-butylphenylphosphonic acid, 2-isobutylphenylphosphonic acid, 2-sec-butylphenylphosphonic acid, 2-tert-butylphenylphosphonic acid, 2-aminophenylphosphonic acid, 2-fluorophenylphosphonic acid, 2-chlorophenylphosphonic acid, 2-bromophenylphosphonic acid, 2-iodophenylphosphonic acid, 4-hydroxybenzylphosphonic acid, 4-methoxybenzylphosphonic acid, 4-ethoxybenzylphosphonic acid, 4-methylbenzylphosphonic acid, 4-ethylbenzylphosphonic acid, 4-n-butylphenylphosphonic acid, Propylbenzylphosphonic acid, 4-isopropylbenzylphosphonic acid, 4-normalbutylbenzylphosphonic acid, 4-isobutylbenzylphosphonic acid, 4-secbutylbenzylphosphonic acid, 4-tertbutylbenzylphosphonic acid, 4-aminobenzylphosphonic acid, 4-fluorobenzylphosphonic acid, 4-chlorobenzylphosphonic acid, 4-bromobenzylphosphonic acid, 4-iodobenzylphosphonic acid, 2-hydroxybenzylphosphonic acid, 2-methoxybenzylphosphonic acid, 2-ethoxybenzylphosphonic acid, 2-methylbenzylphosphonic acid, 2-ethylbenzylphosphonic acid benzylphosphonic acid, 2-normal propyl benzyl phosphonic acid, 2-isopropyl benzyl phosphonic acid, 2-normal butyl benzyl phosphonic acid, 2-isobutyl benzyl phosphonic acid, 2-sec butyl benzyl phosphonic acid, 2-tert butyl benzyl phosphonic acid, 2-amino benzyl phosphonic acid, 2-fluoro benzyl phosphonic acid, 2-chloro benzyl phosphonic acid, 2-bromo benzyl phosphonic acid, 2-iodo benzyl phosphonic acid, 4-hydroxy phenethyl phosphonic acid, 4-methoxy phenethyl phosphonic acid, 4-ethoxy phenethyl phosphonic acid,4-Methylphenethylphosphonic acid, 4-ethylphenethylphosphonic acid, 4-normal propylphenethylphosphonic acid, 4-isopropylphenethylphosphonic acid, 4-normal butylphenethylphosphonic acid, 4-isobutylphenethylphosphonic acid, 4-secbutylphenethylphosphonic acid, 4-tertbutylphenethylphosphonic acid, 4-aminophenethylphosphonic acid, 4-fluorophenethylphosphonic acid, 4-chlorophenethylphosphonic acid, 4-bromophenethylphosphonic acid, 4-iodophenethylphosphonic acid, 2-hydroxyphenethylphosphonic acid, 2-methoxyphenethyl ethyl phosphonic acid, 2-ethoxyphenethyl phosphonic acid, 2-methylphenethyl phosphonic acid, 2-ethylphenethyl phosphonic acid, 2-normal propyl phenethyl phosphonic acid, 2-isopropyl phenethyl phosphonic acid, 2-normal butyl phenethyl phosphonic acid, 2-isobutyl phenethyl phosphonic acid, 2-sec butyl phenethyl phosphonic acid, 2-tert butyl phenethyl phosphonic acid, 2-amino phenethyl phosphonic acid, 2-fluoro phenethyl phosphonic acid, 2-chloro phenethyl phosphonic acid, 2-bromo phenethyl phosphonic acid, and 2-iodo phenethyl phosphonic acid.

[0036] The phosphonic acid represented by formula (B) is not limited to a specific phosphonic acid. The phosphonic acid represented by formula (B) includes, but is not limited to, methylphosphonic acid, ethylphosphonic acid, normal propylphosphonic acid, isopropylphosphonic acid, normal butylphosphonic acid, isobutylphosphonic acid, secbutylphosphonic acid, tertbutylphosphonic acid, phenylphosphonic acid, and other phosphonic acids, as well as bromomethylphosphonic acid, fluoroethylphosphonic acid, bromophenylphosphonic acid, iodophenylphosphonic acid, and other phosphonic acids in which at least one hydrogen atom is replaced with a halogen atom.

[0037] In the light-absorbing composition, the phosphonic acid represented by formula (B) is typically a different type of phosphonic acid from the phosphonic acid represented by formula (A). By using the phosphonic acid represented by formula (B) together with the phosphonic acid represented by formula (A), the light-absorbing agent, the light-absorbing composition, In the composition or light absorbing film, and in the manufacturing process thereof, aggregation of the light absorbing agent can be suppressed within a range that does not affect the light absorbing performance.

[0038] In the light-absorbing composition, the copper component contains divalent copper ions. The copper component is added in the form of a copper salt when the light-absorbing composition is prepared. Examples of copper salts that supply the copper component include copper acetate, copper benzoate, copper formate, copper stearate, copper pyrophosphate, copper oxide, copper chloride, copper hydroxide, and hydrates thereof.

[0039] In the light-absorbing composition, the ratio of the total content of the phosphonic acid represented by formula (A) and the phosphonic acid represented by formula (B) to the content of the copper component is, on a substance amount basis, for example, 0.4 to 2.0, preferably 0.5 to 1.5, and more preferably 0.6 to 1.2. This makes it easier to realize a light-absorbing film or optical filter having desired optical properties more reliably using the light-absorbing composition.

[0040] In the light-absorbing composition, the ratio of the content of the phosphonic acid represented by formula (A) to the content of the phosphonic acid represented by formula (B) is, for example, 0.1 to 10.0, preferably 0.2 to 5.0, and more preferably 0.3 to 3.0, based on the amount of substance. This makes it easier to realize a light-absorbing film or optical filter having desired optical properties using the light-absorbing composition more reliably. In addition, the first light-absorbing agent and the second light-absorbing agent are less likely to aggregate in the light-absorbing composition.

[0041] The first light absorbent and the second light absorbent are typically dispersed in the light absorbing composition. For example, fine particles containing at least one of the first light absorbent and the second light absorbent are formed in the light absorbing composition. The average particle diameter of the fine particles is, for example, 5 nm to 200 nm. If the average particle diameter of the fine particles is 5 nm or more, no special process is required for finely fining the fine particles, and the structure of the fine particles containing at least the light absorbent is less likely to be broken. In addition, the fine particles are well dispersed in the light absorbing composition. In addition, if the average particle diameter of the fine particles is 200 nm or less, the effect of Mie scattering can be reduced, the transmittance of visible light can be improved in the light absorbing film, and the deterioration of characteristics such as contrast and haze of the image captured by the imaging device can be suppressed. The average particle diameter of the fine particles is preferably 100 nm or less. In this case, the effect of Rayleigh scattering is reduced, so that the transparency to visible light is increased in the light absorbing film formed using the light absorbing composition. In addition, the average particle diameter of the fine particles is more preferably 75 nm or less. In this case, the transparency to visible light of the light absorbing film produced using the light absorbing composition is particularly high. The average particle size of the fine particles can be measured by a dynamic light scattering method.

[0042] The light absorbing composition may further contain a resin. The resin is preferably a transparent resin that exhibits high transmittance at least in the visible light region. For example, but not limited to, acrylic resin, epoxy resin, polycarbonate resin, polyether resin, polyester resin, cyclic olefin resin, silicone resin, etc. are used as the resin.

[0043] The resin is preferably a silicone resin containing an aryl group such as a phenyl group. If the resin contained in the light absorbing film is hard (rigid), as the thickness of the layer containing the resin increases, cracks are likely to occur due to hardening shrinkage during the preparation of the light absorbing film. If the resin is a silicone resin containing an aryl group, the light absorbing film formed by the light absorbing composition is likely to have good crack resistance. In addition, the silicone resin containing an aryl group has high compatibility with the phosphonic acid represented by formula (A) or formula (B), and is unlikely to cause the light absorber to aggregate. Specific examples of silicone resins include KR-255, KR-300, KR-2621-1, KR-211, KR-311, KR-216, KR-212, KR-251, and KR-5230. All of these are silicone resins manufactured by Shin-Etsu Chemical Co., Ltd.

[0044] The light absorbing composition may further contain, for example, a phosphoric acid ester. The action of the phosphoric acid ester makes it easy for the light absorber to be appropriately dispersed in the light absorbing composition or the light absorbing film obtained by curing the light absorbing composition. In addition, the phosphoric acid ester may function as a dispersant, and a part of the phosphoric acid ester may react with a copper component to form a compound. In addition, the phosphoric acid ester may further coordinate or react with a compound formed by a copper component and a phosphonic acid to form a compound. The light absorber may contain these compounds or components of their copper salts.

[0045] The phosphate ester is, for example, a phosphate ester having a polyoxyalkyl group. The phosphate ester having a polyoxyalkyl group is not limited to a specific phosphate ester. The phosphate ester having a polyoxyalkyl group is, for example, Plysurf A208N: polyoxyethylene alkyl (C12, C13) ether phosphate ester, Plysurf A208F: polyoxyethylene alkyl (C8) ether phosphate ester, Plysurf A208B: polyoxyethylene lauryl ether phosphate ester, Plysurf A219B: polyoxyethylene lauryl ether phosphate ester, Plysurf AL: polyoxyethylene styrenated phenyl ether phosphate ester, Plysurf A212C: polyoxyethylene tridecyl ether phosphate ester, or Plysurf A215C: polyoxyethylene tridecyl ether phosphate ester. All of these are products manufactured by Daiichi Kogyo Seiyaku Co., Ltd. The phosphate ester may also be, for example, NIKKOL DDP-2: polyoxyethylene alkyl ether phosphate ester, NIKKOL DDP-4: polyoxyethylene alkyl ether phosphate ester, or NIKKOL DDP-6: polyoxyethylene alkyl ether phosphate ester. These are all products manufactured by Nikko Chemicals Co., Ltd. When the light absorbing composition is produced, the mass ratio of the content of phosphonic acid to the content of phosphoric ester is 0.2 to 10.0, and preferably 0.3 to 8.0.

[0046] The light absorbing composition may further contain alkoxysilane as required. In this case, siloxane bond (-Si-O-Si-) is formed by hydrolysis and polycondensation of alkoxysilane, and the light absorbing film is likely to have a dense structure. The alkoxysilane may be a monomer, or may be in the form of an oligomer or polymer in which hydrolysis and polycondensation have progressed to a certain extent, or may be a mixture thereof.

[0047] Examples of the alkoxysilane monomer include tetraethoxysilane, tetramethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, dimethyldiethoxysilane, diethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane, from the viewpoints of easy availability, easy reaction control, film adhesion, film weather resistance, etc. One or more types of alkoxysilanes can be used within the range that does not affect the effects of the present invention.

[0048] The inclusion of these alkoxysilanes in the light-absorbing composition suppresses the aggregation of the light-absorbing agent consisting of phosphonic acid and a copper component, making it possible to reduce the amount of phosphoric acid ester compound added as a dispersant. In the light-absorbing composition, the ratio of the content of the alkoxysilane converted into a monomer to the content of the copper component is, for example, 2.0 or more, preferably 2.5 or more, based on the amount of substance. In addition, when the light-absorbing composition contains at least one of trialkoxysilane and dialkoxysilane, the ratio of the content of the trialkoxysilane and dialkoxysilane converted into a monomer to the content of the copper component in the light-absorbing composition is, for example, 1.5 or more, based on the amount of substance. With regard to these characteristics, International Publication No. The matters described in Patent Publication No. 2019 / 093076 can be taken into consideration, and the matters described therein are appropriately incorporated into this specification.

[0049] An example of a method for preparing a light-absorbing composition will be described. A copper salt such as copper acetate monohydrate is added to a predetermined solvent such as tetrahydrofuran (THF) and stirred to prepare a solution A of the copper salt. In preparing the solution A, a phosphoric acid ester may be added. Next, phosphonic acids represented by formulas (A) and (B) are added to a predetermined solvent such as THF and stirred to prepare a solution B. Each phosphonic acid may be added to a predetermined solvent such as THF and stirred to prepare a mixture of a plurality of spare solutions prepared for each type of phosphonic acid. While stirring the solution A, the solution B is added to the solution A and stirred for a predetermined time. Next, a predetermined solvent such as toluene is added to this solution and stirred to obtain a solution C. Next, the solution C is heated and subjected to a desolvation treatment for a predetermined time to obtain a solution D. As a result, components generated by dissociation of the copper salt such as the solvent THF and acetic acid (boiling point: about 118°C) are removed, and a first light absorber is generated by the phosphonic acid represented by formula (A) and the copper component, and a second light absorber is generated by the phosphonic acid represented by formula (B) and the copper component. The temperature to which Liquid C is heated is determined based on the boiling point of the component to be removed that has dissociated from the copper salt. In the desolvation process, the solvent used to obtain Liquid C, such as toluene (boiling point: about 110°C), also volatilizes. It is desirable for this solvent to remain to some extent in the light-absorbing composition, so the amount of solvent added and the time of the desolvation process can be determined from this perspective. In addition, o-xylene (boiling point: about 144°C) can also be used instead of toluene to obtain Liquid C. In this case, since the boiling point of o-xylene is higher than that of toluene, the amount added can be reduced to about one-fourth of the amount added of toluene.

[0050] If necessary, the light absorbing composition can be prepared by mixing Liquid D with a resin such as a silicone resin and stirring the mixture for a predetermined period of time.

[0051] The light-absorbing composition can be used to provide, for example, a light-absorbing film 10 as shown in FIG. 1. The light-absorbing film 10 can be obtained, for example, by curing a coating of the light-absorbing composition. The light-absorbing film 10 contains a light absorber formed of phosphonic acid and a copper component. In the transmittance spectrum of the light-absorbing film 10 at an incident angle of 0 degrees, the transmittance T400 , transmittance T at wavelength 550 nm 550 , and transmittance T at a wavelength of 800 nm 800 teeth, 4≦T 550 / T 400 and 8≦T 550 / T 800 Therefore, light in a wavelength range including part of ultraviolet light and including 400 nm is easily absorbed by the light absorbing film 10. Therefore, for example, the spectral characteristics of the light absorbing film 10 regarding the transmittance in the vicinity of wavelengths of 350 nm to 430 nm tend to become close to the visual sensitivity of humans.

[0052] In the light absorbing film 10, the transmittance T 400 , transmittance T 550 , and transmittance T 800 is preferably 8≦T 550 / T 400 and 28≦T 550 / T 800 and more preferably 16≦T 550 / T 400 and 60≦T 550 / T 800 and more preferably, 20≦T 550 / T 400 and 80≦T 550 / T 800 Meet the conditions.

[0053] The light absorbing agent in the light absorbing film 10 contains, for example, a first light absorbing agent formed by phosphonic acid represented by the above formula (A) and a copper component. 550 / T 400 and 8≦T 550 / T 800 This is advantageous in terms of satisfying the above conditions.

[0054] The light absorbing agent in the light absorbing film 10 further contains a second light absorbing agent formed by, for example, phosphonic acid represented by the above formula (B) and a copper component. This is advantageous from the viewpoint of realizing good dispersion of the light absorbing agent in the light absorbing film.

[0055] As shown in FIG. 1, an optical filter 1a having a light absorbing film 10 can be provided. The optical filter 1a is capable of absorbing light in a wavelength range including a part of ultraviolet light and including 400 nm. Therefore, for example, the spectral characteristics of the optical filter 1a relating to the transmittance in the vicinity of wavelengths of 350 nm to 430 nm tend to become close to the visual sensitivity of humans.

[0056] In the transmittance spectrum of the optical filter 1a at an incident angle of 0 degrees, the transmittance T 400 , transmittance T at wavelength 550 nm 550 , and transmittance T at a wavelength of 800 nm 800 4≦T 550 / T 400 and 8≦T 550 / T 800 Meet the conditions.

[0057] In the optical filter 1a, the transmittance T 400 , transmittance T 550 , and transmittance T 800 is desirable <8≦T 550 / T 400 and 28≦T 550 / T 800 and more preferably 16≦T 550 / T 400 and 60≦T 550 / T 800 and more preferably, 20≦T 550 / T 400 and 80≦T 550 / T 800 Meet the conditions.

[0058] The optical filter 1a may be, for example, any one of the following (I), (II), (III), (IV), (V), and Condition (VI) is further satisfied. (I) Maximum transmittance T at wavelengths of 300 nm to 380 nm M 300-380 (II) The transmittance T at a wavelength of 400 nm is 1% or less.400 is less than 20%. (III) UV cutoff wavelengths with a transmittance of 50% in the range of 300 nm to 480 nm Toe-off wavelength λ UV 405 nm ≦ λ UV Meets the condition of ≦480nm. (IV) Average transmittance T at wavelengths of 480 nm to 580 nm A 480-580 is more than 78%. (V) IR cutoff wavelength λ, which is the wavelength at which the transmittance is 50% in the wavelength range of 580 nm to 750 nm IR , 600nm≦λ IR Meets the condition of ≦700nm. (VI) Maximum transmittance T at wavelengths from 800 nm to 1100 nm M 800-1100 is less than 10% be.

[0059] With respect to the above condition (I), the optical filter 1a preferably satisfies the following condition (Ia), and more preferably satisfies condition (Ib). (Ia) Maximum transmittance T at wavelengths from 300 nm to 385 nm M 300-385 (Ib) The maximum transmittance T at wavelengths of 300 nm to 390 nm is 1% or less. M 300-390 is less than 1%.

[0060] Regarding the above condition (II), in the optical filter 1a, the transmittance T 400 is preferably 10 % or less, and more preferably 5% or less.

[0061] Regarding the above condition (III), the optical filter 1a is preferably 405 nm≦λ UV <=47 0 nm, and more preferably 405 nm≦λ UV Meets the condition of ≦460nm.

[0062] Regarding the above condition (IV), in the optical filter 1a, the average transmittance T A 480-580 is preferably 80% or more, and more preferably 82% or more.

[0063] Regarding the above condition (V), the optical filter 1a is preferably 620 nm≦λ IR Meets the condition of ≦680nm.

[0064] Regarding the above condition (VI), the optical filter 1a has a maximum transmittance T M 800-1000 is preferably 3% or less, more preferably 1% The following is the result.

[0065] The optical filter 1a may satisfy, for example, the following conditions (α), (β), and (γ): Range means a value obtained by subtracting the minimum value from the maximum value. (α) A lens having a transmittance of 1% or less continuously in the wavelength range of 300 nm to 450 nm. DiΔλ 1% UV is 85 nm or more. (β) The wavelength range Δλ where the transmittance is continuously 1% or less in the wavelength range from 700 nm to 1200 nm 1% IR is 200 nm or more. (γ) UV cutoff wavelength λ UV and IR cutoff wavelength λ IR Absolute value of the difference between |λ UV -λ IR | is 180 nm or more.

[0066] Regarding the condition (α), the range Δλ of the optical filter 1a 1% UV is preferably 90 nm or more.

[0067] Regarding the condition (β), the range Δλ of the optical filter 1a 1% IR is preferably 220 nm or more.

[0068] Regarding the condition (γ), the absolute value |λ of the optical filter 1a UV -λ IR is preferably 190 nm or more.

[0069] The optical filter 1a is, for example, composed of a single light absorbing film 10. In this case, the optical filter 1a can be used, for example, separately from an imaging element or an optical component. The optical filter 1a may be bonded to the imaging element and the optical component. On the other hand, the optical filter 1a may be constructed by applying the above-mentioned light absorbing composition to the imaging element or the optical component and curing the light absorbing composition.

[0070] The thickness of the light absorbing film 10 is not limited to a specific value. The thickness of the light absorbing film 10 is, for example, 10 μm to 600 μm, may be 20 μm to 400 μm, or may be 30 μm to 300 μm.

[0071] The optical filter 1a can be produced, for example, by peeling off the light absorbing film 10 formed on a substrate from the substrate. In this case, the material of the substrate may be glass, resin, or metal. The surface of the substrate may be subjected to a surface treatment such as coating with a fluorine-containing compound.

[0072] The optical filter 1a may be modified, for example, to the optical filter 1b shown in FIG. 2. The optical filter 1b is configured similarly to the optical filter 1a unless otherwise specified. The components of the optical filter 1b that are the same as or correspond to the components of the optical filter 1a are given the same reference numerals, and detailed description is omitted. The description of the optical filter 1a also applies to the optical filter 1b as long as there is no technical contradiction.

[0073] 2, the optical filter 1b includes a light-absorbing film 10 and a transparent dielectric substrate 20. The light-absorbing film 10 is formed parallel to one of the main surfaces of the transparent dielectric substrate 20. The light-absorbing film 10 may be in contact with one of the main surfaces of the transparent dielectric substrate 20, for example. In this case, the light-absorbing film 10 can be formed, for example, by applying the above-mentioned light-absorbing composition to one of the main surfaces of the transparent dielectric substrate 20 and curing the light-absorbing composition.

[0074] The type of the transparent dielectric substrate 20 is not limited to a specific type. The transparent dielectric substrate 20 may have an absorption ability in the infrared region. The transparent dielectric substrate 20 may have an average spectral transmittance of 90% or more at wavelengths of, for example, 350 nm to 900 nm. The material of the transparent dielectric substrate 20 is not limited to a specific material, and may be, for example, a specific glass or resin. When the material of the transparent dielectric substrate 20 is glass, the transparent dielectric substrate 20 may be, for example, transparent glass made of silicate glass such as soda-lime glass and borosilicate glass, or phosphate glass and fluorophosphate glass containing coloring components such as Cu and Co. Phosphate glass and fluorophosphate glass containing coloring components are, for example, infrared absorbing glass. When the light absorbing film 10 is used together with a transparent dielectric substrate 20 made of infrared absorbing glass, the light absorption and transmittance spectra of both can be adjusted to produce an optical filter having desired optical characteristics, providing a high degree of freedom in designing the optical filter.

[0075] When the material of the transparent dielectric substrate 20 is a resin, the resin is, for example, a cyclic olefin resin such as a norbornene resin, a polyarylate resin, an acrylic resin, a modified acrylic resin, a polyimide resin, a polyetherimide resin, a polysulfone resin, a polyethersulfone resin, a polycarbonate resin, or a silicone resin.

[0076] Each of the optical filters 1a and 1b may be modified to further include other functional films, such as an infrared reflecting film and an anti-reflection film. Such functional films may be formed on the light absorbing film 10 or the transparent dielectric substrate 20. For example, the optical filter may include an anti-reflection film to increase the transmittance in a predetermined wavelength range (e.g., the visible light range). The anti-reflection film may be configured as a layer of a low refractive index material such as MgF2 and SiO2, or may be configured as a laminate of such a layer of a low refractive index material and a layer of a high refractive index material such as TiO2. Such an anti-reflection film may be formed by a method involving a physical reaction, such as a vacuum deposition method or a sputtering method, or by a method involving a chemical reaction, such as a CVD method or a sol-gel method.

[0077] The optical filter may be configured, for example, with the light absorbing film 10 disposed between two sheets of glass in the form of plates. This improves the rigidity and mechanical strength of the optical filter. In addition, the main surface of the optical filter becomes hard, which is advantageous from the viewpoint of preventing scratches, etc. In particular, when a relatively flexible resin is used as the binder or matrix in the light absorbing film 10, such an advantage is important. EXAMPLES

[0078] The present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples.

[0079] <Example 1> 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 4.333g of Plysurf A208N (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain A1 solution. 40g of THF was added to 1.590g of 4-hydroxyphenylphosphonic acid (manufactured by Tokyo Kasei Kogyo Co., Ltd.) and stirred for 30 minutes to obtain B1(a) solution. 40g of THF was added to 1.444g of phenylphosphonic acid (manufactured by Nissan Chemical Industries Co., Ltd.) and stirred for 30 minutes to obtain B1(b) solution. While stirring A1 solution, B1(a) solution and B1(b) solution were added to A1 solution, and stirred at room temperature for 1 minute. Next, 120g of toluene was added to this solution, and then stirred at room temperature for 1 minute to obtain C1 solution. The C1 liquid was placed in a flask and heated in an oil bath (Tokyo Rikakikai Co., Ltd., model: OSB-2100) while being subjected to a solvent removal treatment using a rotary evaporator (Tokyo Rikakikai Co., Ltd., model: N-1110SF). The temperature of the oil bath was adjusted to 105°C. The liquid after the solvent removal treatment was then removed from the flask to obtain D1 liquid, which was a dispersion of a light absorber formed of 4-hydroxyphenylphosphonic acid and copper ions, and a light absorber formed of phenylphosphonic acid and copper ions. The appearance of D1 liquid was transparent, and it was estimated that the dispersion state of the fine particles of the light absorber was good.

[0080] 8.80 g of silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR-300) was added to the D1 liquid and stirred for 30 minutes to obtain a light absorbing composition according to Example 1 containing a light absorbent. The amounts of materials added used in the preparation of the light absorbing composition according to Example 1 are shown in Table 1. The mass ratio of the phosphonic acid content to the phosphoric acid ester content in the light absorbing composition and the copper iridium content in the light absorbing composition are shown in Table 1. The ratio of the phosphonic acid content to the ion content based on the amount of substance is shown in Table 1.

[0081] The light absorbing composition according to Example 1 was applied to a 40 mm×40 mm area in the center of one of the main surfaces of a transparent glass substrate (manufactured by SCHOTT, product name: D263 T eco) made of borosilicate glass having dimensions of 76 mm×76 mm×0.21 mm using a dispenser to form a coating film. The resulting coating film was thoroughly dried at room temperature, and then placed in an oven and heat-treated at 45° C. for 2 hours and at 85° C. for 30 minutes to volatilize the solvent and harden the film. In this way, the light absorbing film according to Example 1 was formed, and the optical filter according to Example 1 was obtained.

[0082] The optical filter according to Example 1 was further subjected to a baking treatment at 125° C. for 3 hours and at 150° C. for 1 hour.

[0083] <Example 2> 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 4.333g of Plysurf A208N (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain A2 solution. 40g of THF was added to 1.590g of 4-hydroxyphenylphosphonic acid (manufactured by Tokyo Kasei Kogyo Co., Ltd.) and stirred for 30 minutes to obtain B2(a) solution. 40g of THF was added to 1.444g of phenylphosphonic acid (manufactured by Nissan Chemical Industries Co., Ltd.) and stirred for 30 minutes to obtain B2(b) solution. While stirring A2 solution, B2(a) solution and B2(b) solution were added to A2 solution, and stirred at room temperature for 1 minute. Next, 120g of toluene was added to this solution, and then stirred at room temperature for 1 minute to obtain C2 solution. This C2 liquid was placed in a flask and heated in an oil bath (Tokyo Rikakikai Co., Ltd., model: OSB-2100) while undergoing a solvent removal treatment using a rotary evaporator (Tokyo Rikakikai Co., Ltd., model: N-1110SF). The temperature of the oil bath was adjusted to 105°C. The liquid after the solvent removal treatment was then removed from the flask to obtain D2 liquid, which was a dispersion of a light absorber formed of 4-hydroxyphenylphosphonic acid and copper ions, and a light absorber formed of phenylphosphonic acid and copper ions. The appearance of D2 liquid was transparent, and it was estimated that the dispersion state of the fine particles of each light absorber was good.

[0084] 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 2.572g of Plysurf A208N (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain A3 solution. Also, 40g of THF was added to 2.886g of n-butylphosphonic acid and stirred for 30 minutes to obtain B3 solution. While stirring A3 solution, B3 solution was added to A3 solution and stirred at room temperature for 1 minute. Next, 100g of toluene was added to this solution and stirred at room temperature for 1 minute to obtain C3 solution. This C3 solution was placed in a flask and heated in an oil bath (manufactured by Tokyo Rikakikai Co., Ltd., model: OSB-2100) while performing a solvent removal treatment using a rotary evaporator (manufactured by Tokyo Rikakikai Co., Ltd., model: N-1110SF). The set temperature of the oil bath was adjusted to 105°C. After that, the liquid after the solvent removal treatment was taken out of the flask, and D3 liquid, which is a dispersion liquid of a light absorber formed by n-butylphosphonic acid and copper ions, was obtained. The appearance of D3 liquid was transparent, and it was estimated that the dispersion state of the light absorber particles was good.

[0085] D3 liquid in an amount equivalent to 40 mass % of the total amount of D3 liquid and 8.80 g of silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR-300) were added to D2 liquid and stirred for 30 minutes to obtain a light absorbing composition according to Example 2, which contains a light absorber formed from 4-hydroxyphenylphosphonic acid and copper ions, a light absorber formed from phenylphosphonic acid and copper ions, and a light absorber formed from n-butylphosphonic acid and copper ions. The amounts of materials added used in the preparation of the light absorbing composition according to Example 2 are shown in Table 1. In addition, the ratio of the phosphonic acid content to the phosphoric acid ester content on a mass basis and the ratio of the phosphonic acid content to the copper ion content on a substance basis in the light absorbing composition according to Example 2 are shown in Table 1. As shown in.

[0086] Except for using the light absorbing composition according to Example 2 instead of the light absorbing composition according to Example 1, the light absorbing film according to Example 2 was formed in the same manner as in Example 1, and the optical filter according to Example 2 was obtained.

[0087] The optical filter according to Example 2 was further subjected to a baking treatment at 125° C. for 3 hours and at 150° C. for 1 hour.

[0088] <Example 3> A light-absorbing composition according to Example 3 was prepared in the same manner as in Example 2. The amounts of materials added used in preparing the light-absorbing composition according to Example 3 are shown in Table 1. In addition, Table 1 shows the ratio of the phosphonic acid content to the phosphoric acid ester content on a mass basis and the ratio of the phosphonic acid content to the copper ion content on a substance amount basis in the light-absorbing composition according to Example 3.

[0089] 0.1 g of a surface antifouling coating agent (manufactured by Daikin Industries, product name: Optool DSX, concentration of active ingredient: 20% by mass) and 19.9 g of a hydrofluoroether-containing liquid (manufactured by 3M, product name: Novec 7100) were mixed and stirred for 5 minutes to prepare a fluorine treatment agent (concentration of active ingredient: 0.1% by mass). This fluorine treatment agent was poured onto a transparent glass substrate (manufactured by SCHOTT, product name: D263 T eco) made of borosilicate glass having dimensions of 76 mm x 76 mm x 0.21 mm. The glass substrate was then left at room temperature for 24 hours to dry the coating of the fluorine treatment agent, and the glass surface was then lightly wiped with a dust-free cloth containing Novec 7100 to remove excess fluorine treatment agent. In this way, a fluorine-treated substrate was produced.

[0090] The light absorbing composition according to Example 3 was applied to a 40 mm x 40 mm area in the center of the fluorine-treated surface of the fluorine-treated substrate using a dispenser to form a coating film. The resulting coating film was thoroughly dried at room temperature, and then placed in an oven and heat-treated at 45°C for 2 hours and at 85°C for 30 minutes to volatilize the solvent and harden it. Then, it was further baked at 125°C for 3 hours and at 150°C for 1 hour. The end of the light absorbing film thus obtained was lifted and peeled off from the substrate to obtain an optical filter according to Example 3.

[0091] <Example 4> 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 2.166g of Plysurf A208N (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain A4 solution. 40g of THF was added to 2.025g of 4-methoxyphenylphosphonic acid (manufactured by Tokyo Kasei Kogyo Co., Ltd.) and stirred for 30 minutes to obtain B4(a) solution. 40g of THF was added to 1.702g of phenylphosphonic acid (manufactured by Nissan Chemical Industries Co., Ltd.) and stirred for 30 minutes to obtain B4(b) solution. While stirring A4 solution, B4(a) solution and B4(b) solution were added to A4 solution, and stirred at room temperature for 1 minute. Next, 120g of toluene was added to this solution, and then stirred at room temperature for 1 minute to obtain C4 solution. The C4 liquid was placed in a flask and heated in an oil bath (Tokyo Rikakikai Co., Ltd., model: OSB-2100) while being subjected to a solvent removal treatment using a rotary evaporator (Tokyo Rikakikai Co., Ltd., model: N-1110SF). The temperature of the oil bath was adjusted to 105°C. The liquid after the solvent removal treatment was then removed from the flask to obtain D4 liquid, which is a dispersion of a light absorber formed of 4-methoxyphenylphosphonic acid and copper ions and a light absorber formed of phenylphosphonic acid and copper ions. The appearance of D4 liquid was transparent, and it was estimated that the dispersion state of the fine particles of each light absorber was good.

[0092] Add 8.80 g of silicone resin (Shin-Etsu Chemical Co., Ltd., product name: KR-300) to D4 liquid. The mixture was added and stirred for 30 minutes to obtain a light-absorbing composition according to Example 4, which contains a light absorber formed by 4-methoxyphenylphosphonic acid and copper ions, and a light absorber formed by phenylphosphonic acid and copper ions. The amounts of materials added used in the preparation of the light-absorbing composition according to Example 4 are shown in Table 1. In addition, Table 1 shows the ratio of the phosphonic acid content to the phosphoric acid ester content on a mass basis, and the ratio of the phosphonic acid content to the copper ion content on a substance basis, in the light-absorbing composition according to Example 4.

[0093] Except for using the light absorbing composition according to Example 4 instead of the light absorbing composition according to Example 1, the light absorbing film according to Example 4 was formed in the same manner as in Example 1, and the optical filter according to Example 4 was obtained.

[0094] <Example 5> 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 2.166g of Plysurf A208N (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain A5 solution. 40g of THF was added to 2.176g of 4-ethoxyphenylphosphonic acid (manufactured by Sigma-Aldrich Co., Ltd.) and stirred for 30 minutes to obtain B5(a) solution. 40g of THF was added to 1.702g of phenylphosphonic acid (manufactured by Nissan Chemical Industries, Ltd.) and stirred for 30 minutes to obtain B5(b) solution. While stirring A5 solution, B5(a) solution and B5(b) solution were added to A5 solution, and stirred at room temperature for 1 minute. Next, 120g of toluene was added to this solution, and then stirred at room temperature for 1 minute to obtain C5 solution. The C5 liquid was placed in a flask and heated in an oil bath (Tokyo Rikakikai Co., Ltd., model: OSB-2100) while being subjected to a solvent removal treatment using a rotary evaporator (Tokyo Rikakikai Co., Ltd., model: N-1110SF). The temperature of the oil bath was adjusted to 105°C. The liquid after the solvent removal treatment was then removed from the flask to obtain D5 liquid, which is a dispersion of a light absorber formed of 4-ethoxyphenylphosphonic acid and copper ions and a light absorber formed of phenylphosphonic acid and copper ions. The D5 liquid had a transparent appearance, and it was estimated that the dispersion state of the fine particles of each light absorber was good.

[0095] 8.80 g of silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR-300) was added to the D5 liquid and stirred for 30 minutes to obtain a light absorbing composition according to Example 5, which contains a light absorber formed by 4-ethoxyphenylphosphonic acid and copper ions, and a light absorber formed by phenylphosphonic acid and copper ions. The amounts of materials added used in the preparation of the light absorbing composition according to Example 5 are shown in Table 1. In addition, Table 1 shows the ratio of the phosphonic acid content to the phosphoric acid ester content on a mass basis, and the ratio of the phosphonic acid content to the copper ion content on a substance basis, in the light absorbing composition according to Example 5.

[0096] Except for using the light absorbing composition according to Example 5 instead of the light absorbing composition according to Example 1, the light absorbing film according to Example 5 was formed in the same manner as in Example 1, and the optical filter according to Example 5 was obtained.

[0097] <Comparative Example 1> 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 7.172g of Plysurf A208F (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain a solution A6. 40g of THF was added to 2.508g of phenylphosphonic acid (manufactured by Nissan Chemical Industries Co., Ltd.) and stirred for 30 minutes to obtain a solution B6. While stirring the solution A6, solution B6 was added to the solution A6 and stirred for 1 minute at room temperature. Next, 180g of toluene was added to this solution, and the solution was stirred for 1 minute at room temperature to obtain a solution C6. This solution C6 was placed in a flask and heated in an oil bath (manufactured by Tokyo Rikakikai Co., Ltd., model: OSB-2100) while performing a solvent removal treatment using a rotary evaporator (manufactured by Tokyo Rikakikai Co., Ltd., model: N-1110SF). The temperature of the oil bath was set at 1 The temperature was adjusted to 20° C. Thereafter, the liquid after the solvent removal treatment was taken out of the flask, and a D6 liquid, which was a dispersion liquid of a light absorber formed of phenylphosphonic acid and copper ions, was obtained.

[0098] 17.60 g of silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR-300) was added to the D6 liquid and stirred for 30 minutes to obtain a light-absorbing composition according to Comparative Example 1, which contains a light absorber formed by phenylphosphonic acid and copper ions. The amounts of materials added used in preparing the light-absorbing composition according to Comparative Example 1 are shown in Table 1. In addition, Table 1 shows the ratio of the phosphonic acid content to the phosphoric acid ester content on a mass basis and the ratio of the phosphonic acid content to the copper ion content on a substance basis in the light-absorbing composition according to Comparative Example 1.

[0099] A light absorbing composition according to Comparative Example 1 was applied to a 40 mm×40 mm area in the center of one main surface of a transparent glass substrate (manufactured by SCHOTT, product name: D263 T eco) made of borosilicate glass having dimensions of 76 mm×76 mm×0.21 mm using a dispenser to form a coating film. The obtained coating film was thoroughly dried at room temperature, and then placed in an oven and heat-treated at 85° C. for 3 hours to volatilize the solvent. The coating film was further baked at 125° C. for 3 hours, 150° C. for 1 hour, and 170° C. for 8 hours to thoroughly harden the coating film. In this way, a light absorbing film according to Comparative Example 1 was formed, and an optical filter according to Comparative Example 1 was obtained.

[0100] <Comparative Example 2> 4.500g of copper acetate monohydrate and 240g of tetrahydrofuran (THF) were mixed and stirred for 3 hours to obtain a copper acetate solution. Next, 4.333g of Plysurf A208F (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), a phosphate ester compound, was added to the obtained copper acetate solution and stirred for 30 minutes to obtain A7 solution. 40g of THF was added to 2.523g of n-butylphosphonic acid (manufactured by Johoku Chemical Industry Co., Ltd.) and stirred for 30 minutes to obtain B7 solution. While stirring A7 solution, B7 solution was added to A7 solution and stirred for 1 minute at room temperature. Next, 120g of toluene was added to this solution, and the solution was stirred for 1 minute at room temperature to obtain C7 solution. This C7 solution was placed in a flask and heated in an oil bath (manufactured by Tokyo Rika Kikai Co., Ltd., model: OSB-2100), and the solvent was removed using a rotary evaporator (manufactured by Tokyo Rika Kikai Co., Ltd., model: N-1110SF). The set temperature of the oil bath was adjusted to 105°C. Thereafter, the liquid after the solvent removal treatment was taken out of the flask, and liquid D7, which was a dispersion liquid of a light absorber formed of n-butylphosphonic acid and copper ions, was obtained.

[0101] 8.80 g of silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR-300) was added to the D7 liquid and stirred for 30 minutes to obtain a light-absorbing composition according to Comparative Example 2, which contains a light absorber formed by n-butylphosphonic acid and copper ions. The amounts of materials added used in preparing the light-absorbing composition according to Comparative Example 2 are shown in Table 1. In addition, Table 1 shows the ratio of the phosphonic acid content to the phosphoric acid ester content on a mass basis and the ratio of the phosphonic acid content to the copper ion content on a substance basis in the light-absorbing composition according to Comparative Example 2.

[0102] The light absorbing composition according to Comparative Example 2 was applied to a 40 mm x 40 mm area in the center of one main surface of a transparent glass substrate (manufactured by SCHOTT, product name: D263 T eco) made of borosilicate glass having dimensions of 76 mm x 76 mm x 0.21 mm using a dispenser to form a coating film. The obtained coating film was thoroughly dried at room temperature, and then placed in an oven and heat-treated at 45°C for 2 hours and at 85°C for 30 minutes to volatilize the solvent. The coating film was then sufficiently cured by baking at 125°C for 3 hours, 150°C for 1 hour, and 170°C for 3 hours. In this manner, the light absorbing film according to Comparative Example 2 was formed, and an optical filter according to Comparative Example 2 was obtained.

[0103] <Transmittance spectrum measurement> Using an ultraviolet-visible-near infrared spectrophotometer (manufactured by JASCO Corporation, product name: V-670), the transmittance spectra at an incident angle of 0° of the optical filters according to Examples 1 and 2 before and after the baking treatment were measured. The transmittance spectrum, the transmittance spectrum according to Example 2 before the baking treatment, and the transmittance spectrum according to Example 2 after the baking treatment are shown in Figs. 3, 4, 5, and 6, respectively. The transmittance spectra of the optical filters according to Examples 3 to 5 and the optical filters according to Comparative Examples 1 and 2 at an incident angle of 0° were also measured in the same manner. The transmittance spectra of the optical filters according to Examples 3 to 5 and the optical filters according to Comparative Examples 1 and 2 at an incident angle of 0° are shown in Figs. 7 to 9, 10, and 11, respectively. The characteristics of the transmittance of each optical filter read from Figs. 3 to 11 are shown in Tables 2 and 3. The transmittance spectrum of the transparent glass substrate used in Example 1 and the like is shown in Fig. 12. It is understood that the transparent glass substrate exhibits high transmittance in the wavelength range of 360 nm to 1200 nm.

[0104] <Thickness measurement> The distance from the surface of each optical filter was measured using a laser displacement meter (Keyence Corporation, product name: LK-H008), and the thickness of the light absorbing film was measured by subtracting the thickness of the transparent glass substrate as necessary. The results are shown in Table 2.

[0105] According to Figs. 3 to 6 and Tables 2 and 3, it was confirmed that the optical filters according to Examples 1 and 2 before the baking treatment had appropriate light absorption performance and good optical properties. In addition, it was confirmed that the optical filters according to Examples 1 and 2 after the baking treatment also had good optical properties, and that the change in optical properties before and after the baking treatment was small in the optical filters according to Examples 1 and 2. Such a small change in optical properties before and after the baking treatment indicates that the optical filters according to Examples 1 and 2 have good heat resistance at 150°C. In addition, it indicates that an optical filter having good optical properties and heat resistance can be produced by curing the coating film of the light absorbing composition at a relatively low temperature of 85°C in a short time of within 1 hour. Note that "the change in optical properties is small" means, for example, that the change in transmittance before and after the baking treatment is within 3 points, and the change in UV cutoff wavelength and IR cutoff wavelength is within 10 nm.

[0106] The optical filters according to Examples 1 and 2 have the advantage of being heat-resistant at 150°C while being fabricated by a curing process at a low temperature. In particular, it is advantageous that the curing process can be performed at a temperature of 100°C or less, and the fact that the curing process can be performed at 85°C is very advantageous in terms of constructing a fabrication process. In addition, in Examples 1 and 2, the curing process time at 85°C is within 1 hour, and more specifically, the curing process time at 85°C is 30 minutes, which is very advantageous in terms of productivity in terms of shortening the takt time of fabricating an optical filter. In addition, it is also advantageous that additional processes such as humidification are not required in Examples 1 and 2. It is understood that these advantages are obtained by using a phosphonic acid having an electron-donating substituent (hydroxy group) on the benzene ring.

[0107] 7 to 9 and Tables 2 and 3, it was confirmed that the optical filters according to Examples 3 to 5 exhibited sufficient ultraviolet absorbing ability and had good optical characteristics.

[0108] 10 and 11 and Tables 2 and 3, it was confirmed that the optical filters according to Comparative Examples 1 and 2 did not have sufficient ultraviolet absorbing ability and did not have sufficient optical properties required of an optical filter.

[0109] [Table 1]

[0110] [Table 2]

[0111] [Table 3] [Explanation of symbols]

[0112] 1a, 1b Optical filters 10 Light absorbing film 20 Transparent dielectric substrate

Claims

1. 1. A light absorbing composition comprising: Contains a light absorbing agent and a resin, The light absorber contains a phosphonic acid represented by the following formula (A) and a copper component: In the transmittance spectrum at an incident angle of 0 degrees of the light-absorbing film obtained by curing the light-absorbing composition, the transmittance T 400 , transmittance T at a wavelength of 550 nm 550 , and transmittance T at a wavelength of 800 nm 800 , 16≦T 550 / T 400 and 8≦T 550 / T 800 Fulfill the conditions of In the transmittance spectrum, the average transmittance in the wavelength range of 480 nm to 580 nm is 78% or more. Light absorbing composition. 【Chemistry 1】 [In formula (A), R 1 is a substituent exhibiting electron donating properties, and a plurality of R 1 may be present in formula (A). R 2 is an alkylene group having 1 to 3 carbon atoms, and R 2 may not be present in formula (A).]

2. A light absorber comprising a phosphonic acid represented by the following formula (A) and a copper component: A resin is included, In the transmittance spectrum at an incident angle of 0 degrees, the transmittance T 400 , transmittance T at a wavelength of 550 nm 550 , and transmittance T at a wavelength of 800 nm 800 , 16≦T 550 / T 400 and 8≦T 550 / T 800 Fulfill the conditions of In the transmittance spectrum, the average transmittance in the wavelength range of 480 nm to 580 nm is 78% or more. Light absorbing film. 【Chemistry 2】 [In formula (A), R 1 is a substituent exhibiting electron donating properties, and a plurality of R 1 may be present in formula (A). R 2 is an alkylene group having 1 to 3 carbon atoms, and R 2 may not be present in formula (A).]

3. The light absorbing film according to claim 2 is provided, At an incident angle of 0°, the transmission spectrum satisfies the following conditions (I), (II), (III), (V), and (VI): Optical filters. (I) The maximum transmittance in the wavelength range of 300 nm to 380 nm is 1% or less. (II) Transmittance T at a wavelength of 400 nm 400 is less than 20%. (III) UV cutoff wavelength λ, which is the wavelength at which the transmittance is 50% at wavelengths of 480 nm or less UV 405 nm≦λ UV The condition of ≦480 nm is satisfied. (V) IR cutoff wavelength λ, which is the wavelength at which the transmittance is 50% in the wavelength range of 580 nm to 750 nm IR 600 nm≦λ IR The condition of ≦700 nm is satisfied. (VI) The maximum transmittance in the wavelength range of 800 nm to 1100 nm is 10% or less.

4. In the transmittance spectrum, the following conditions (α), (β), and (γ) are further satisfied: The optical filter according to claim 3 . (α) The wavelength range in which the transmittance is continuously equal to or less than 1% from 300 nm to 450 nm is equal to or greater than 85 nm. (β) The wavelength range in which the transmittance is continuously 1% or less from 700 nm to 1200 nm is 200 nm or more. (γ) the UV cutoff wavelength λ UV and the IR cutoff wavelength λ IR The absolute value of the difference between the above is 180 nm or more.

5. The light absorbing film has a thickness of 30 μm to 300 μm. The optical filter according to claim 3 .

6. 1. A method for manufacturing an optical filter, comprising the steps of: The method includes the steps of: applying a light-absorbing composition obtained by mixing a light-absorbing agent containing a phosphonic acid represented by the following formula (A) and a copper component, a resin, and a solvent onto a substrate, and solidifying the resulting coating film to prepare a light-absorbing film; In the transmission spectrum of the optical filter at an incident angle of 0°, the transmittance at a wavelength of 400 nm is T 400 , the transmittance at a wavelength of 550 nm is T 550 , the transmittance at a wavelength of 800 nm is T 800 Then, 16≦T 550 / T 400 and 8≦T 550 / T 800 The condition is met, In the transmission spectrum, the average transmittance in the wavelength range of 480 nm to 580 nm is 78% or more. method. 【Chemistry 3】 [In formula (A), R 1 is a substituent exhibiting electron donating properties, and a plurality of R 1 may be present in formula (A). R 2 is an alkylene group having 1 to 3 carbon atoms, and R 2 may not be present in formula (A).]

Citation Information

Patent Citations

  • Ink composition

    JP1987032161A

  • Optical material

    JP2011063814A

  • Optical filter

    JP2019028162A

  • Optical filter

    JP2019028420A

  • Light absorbing composition and optical filter

    JP2019066866A