Lithium secondary battery
A non-aqueous organic solvent electrolyte with a lithium salt and additive, paired with a Si-carbon composite negative electrode, addresses the capacity and cycle life challenges of lithium secondary batteries, particularly at high temperatures, by enhancing oxidation resistance and stability.
Patent Information
- Application Number
- JP2023513217
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-06
- Filing Date
- 2021-10-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-10-07
AI Technical Summary
Lithium secondary batteries face challenges in achieving high capacity and improved cycle life characteristics, particularly in high-temperature environments.
The use of a non-aqueous organic solvent electrolyte containing a lithium salt and an additive represented by a specific chemical formula, combined with a negative electrode using a Si-carbon composite and a positive electrode, enhances the battery's performance by improving oxidation resistance and stability, thereby reducing resistance and increasing capacity.
The electrolyte system with the Si-carbon composite and additive improves high voltage characteristics, leading to enhanced cycle life and reduced resistance, especially under high-temperature conditions.
Smart Images

Figure 0007564337000009 
Figure 0007564337000010 
Figure 0007564337000011
Abstract
Description
Technical Field
[0001] Relates to a lithium secondary battery.
Background Art
[0002] Lithium secondary batteries have attracted attention as power sources for various electronic devices because of their high discharge voltage and high energy density.
[0003] As the positive electrode active material of the lithium secondary battery, oxides composed of lithium and transition metals having a structure capable of intercalation of lithium ions, such as LiCoO2, LiMn2O4, LiNi 1-x Co x O2 (0 < x < 1), etc., are mainly used.
[0004] As the negative electrode active material, carbon-based materials in the form including artificial and natural graphite and hard carbon capable of insertion / desorption of lithium are mainly used. As the electrolyte of the lithium secondary battery, an organic solvent in which a lithium salt is dissolved is used.
Summary of the Invention
Problems to be Solved by the Invention
[0005] One embodiment is to provide a lithium secondary battery exhibiting improved high capacity and improved cycle life characteristics.
Means for Solving the Problems
[0006] According to one embodiment, there is provided a lithium secondary battery including an electrolyte containing a non-aqueous organic solvent, a lithium salt, and an additive represented by the following Chemical Formula 1, a negative electrode including a negative electrode active material containing a Si-carbon composite, and a positive electrode including a positive electrode active material.
[0007]
Chemical Formula
[0008] In the above Chemical Formula 1, R 1 ~R 8 may each independently be a hydrogen atom, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C2 to C10 alkenyl group, a substituted or unsubstituted C2 to C10 alkynyl group, a substituted or unsubstituted C3 to C10 cycloalkyl group, a substituted or unsubstituted C3 to C10 cycloalkenyl group, a substituted or unsubstituted C3 to C10 cycloalkynyl group, or a substituted or unsubstituted C6 to C10 aryl group.
[0009] In one embodiment, the additive represented by Formula 1 may be sulfolane, methyl sulfolane, dimethyl sulfolane, or a combination thereof.
[0010] The content of the additive represented by Chemical Formula 1 may be 0.1% by weight to 10% by weight, based on the content of the non-aqueous organic solvent and the lithium salt being 100% by weight.
[0011] The content of the Si-C carbon composite may be 0.1 wt % to 5 wt % based on the total weight of the negative active material. Also, the negative active material may further include crystalline carbon.
[0012] The non-aqueous organic solvent may include a propionate-based solvent. The propionate-based solvent may be methyl propionate, ethyl propionate, propyl propionate, or a combination thereof. The content of the propionate-based solvent may be 5% by volume to 80% by volume based on the total volume of the non-aqueous organic solvent.
[0013] The Si-carbon composite may include Si nanoparticles and amorphous carbon. According to one embodiment, the Si-carbon composite may include a core and a coating layer surrounding the core, the core may include amorphous carbon or crystalline carbon and Si nanoparticles, and the coating layer may include amorphous carbon.
[0014] In one embodiment, the coating layer may have a thickness of 1 nm to 100 nm. In one embodiment, the content of the Si nanoparticles may be 1 wt % to 60 wt % based on 100 wt % of the total weight of the Si-carbon composite. Other specific details of the embodiments are included in the following detailed description. Effect of the Invention
[0015] Since the lithium secondary battery according to the embodiment of the present invention uses an electrolyte having excellent oxidation stability, it is possible to improve high voltage characteristics and reduce resistance, thereby exhibiting high capacity and excellent cycle life characteristics. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a diagram illustrating a lithium secondary battery according to an embodiment. [Diagram 2] 4 is a graph showing the initial DC resistance, high-temperature storage DC resistance, and resistance increase rate of the lithium secondary batteries produced in Examples 2 and 5 and Comparative Example 3. [Diagram 3] 1 is a graph showing the initial DC resistance, high-temperature storage DC resistance, and resistance increase rate of the lithium secondary batteries produced in Examples 1 to 6, Reference Examples 1 and 2, and Comparative Examples 1 to 7. [Figure 4]1 is a graph showing the initial DC resistance, high-temperature storage DC resistance, and resistance increase rate of the lithium secondary batteries produced in Examples 1 to 3, Reference Example 1, and Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail, but they are given by way of example only and are not intended to limit the present invention, which is defined only by the scope of the claims set forth below.
[0018] Unless otherwise defined in this specification, "substituted" means that a hydrogen atom in the compound is substituted with a substituent selected from a halogen atom (F, Br, Cl or I), a hydroxy group, an alkoxy group, a nitro group, a cyano group, an amino group, an azido group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid or a salt thereof, a C1-C20 alkyl group, a C2-C20 alkenyl group, a C2-C20 alkynyl group, a C6-C30 aryl group, a C7-C30 arylalkyl group, a C1-C4 alkoxy group, a C1-C20 heteroalkyl group, a C3-C20 heteroarylalkyl group, a C3-C30 cycloalkyl group, a C3-C15 cycloalkenyl group, a C6-C15 cycloalkynyl group, a C2-C20 heterocycloalkyl group, and combinations thereof.
[0019] One embodiment provides a lithium secondary battery including an electrolyte including a non-aqueous organic solvent, a lithium salt, and an additive represented by the following Chemical Formula 1, an anode including an anode active material including a Si-carbon composite, and a cathode including a cathode active material:
[0020] [ka]
[0021] In the above Chemical Formula 1, R 1 ~R 8are each independently a hydrogen atom, a substituted or unsubstituted C1 to C30 alkyl group, a substituted or unsubstituted C2 to C30 alkenyl group, a substituted or unsubstituted C2 to C30 alkynyl group, a substituted or unsubstituted C3 to C30 cycloalkyl group, a substituted or unsubstituted C3 to C30 cycloalkenyl group, a substituted or unsubstituted C3 to C30 cycloalkynyl group, or a substituted or unsubstituted C6 to C30 aryl group.
[0022] In one embodiment, the R 1 ~R 8 may each independently be a hydrogen atom, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C2 to C10 alkenyl group, a substituted or unsubstituted C2 to C10 alkynyl group, a substituted or unsubstituted C3 to C10 cycloalkyl group, a substituted or unsubstituted C3 to C10 cycloalkenyl group, a substituted or unsubstituted C3 to C10 cycloalkynyl group, or a substituted or unsubstituted C6 to C10 aryl group.
[0023] For example, the additive represented by Formula 1 can be sulfolane, methyl sulfolane, such as 3-methyl sulfolane, dimethyl sulfolane, such as 2,4-dimethyl sulfolane, or a combination thereof.
[0024] In this case, the content of the additive represented by the formula 1 may be 0.1 wt% to 10 wt% based on the weight of the non-aqueous organic solvent and the lithium salt, i.e., when the content of the non-aqueous organic solvent and the lithium salt is 100 wt% (based on the total content of the non-aqueous organic solvent and the lithium salt being 100 wt%), and according to one embodiment, it may be 0.5 wt% to 7.5 wt%, and according to another embodiment, it may be 2.5 wt% to 7.5 wt%. When the content of the additive represented by the formula 1 is within the above range, it is appropriate because it can exhibit high temperature reliability characteristics, for example, the effect of reducing the high temperature resistance increase rate.
[0025] The negative active material may further include crystalline carbon other than the Si-C composite, and the content of the Si-C composite may be 0.1 wt % to 5 wt % based on the total weight of the negative active material, i.e., 100 wt %.
[0026] When a negative electrode active material containing a Si-C composite is used in a battery using an electrolyte containing the additive of Chemical Formula 1, it is appropriate because it can effectively suppress an increase in high temperature resistance, and such an effect can be further increased when the negative electrode active material contains 0.1 wt% to 5 wt%, in one embodiment, 1 wt% to 5 wt%, and in another embodiment, 2.5 wt% to 5 wt%. When the negative electrode active material contains 0.1 wt% to 5 wt% of the Si-C composite, the desired high capacity and volume expansion suppression effect can be best obtained.
[0027] The Si-carbon composite can include Si nanoparticles and amorphous carbon. According to one embodiment, the Si-carbon composite can include a core and a coating layer surrounding the core, the core can include amorphous carbon or crystalline carbon and Si nanoparticles, and the coating layer can include amorphous carbon.
[0028] The amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbon, calcined coke, or a combination thereof. The crystalline carbon may be natural graphite, artificial graphite, or a combination thereof.
[0029] When the Si-carbon composite includes Si nanoparticles and amorphous carbon, the mixing ratio of the Si nanoparticles and amorphous carbon may be 2:1 to 1.5:1 by weight. When the Si-carbon composite includes a core and a coating layer, the content of the coating layer may be 0.08:1 to 0.2:1 by weight with respect to 100% by weight of the entire composite, and the content of the Si nanoparticles may be 1% to 60% by weight with respect to 100% by weight of the entire Si-carbon composite, and according to one embodiment, 3% to 60% by weight. The content of amorphous carbon or crystalline carbon included in the core may be 20% to 60% by weight with respect to 100% by weight of the entire composite.
[0030] Furthermore, the thickness of the coating layer can be from 1 nm to 100 nm, for example, from 5 nm to 100 nm.
[0031] In addition, regardless of the form of the Si-carbon composite, the particle size of the Si nanoparticles may be 5 nm to 150 nm. For example, it may be 10 nm to 150 nm, specifically 30 nm to 150 nm, more specifically 50 nm to 150 nm, and narrowly 60 nm to 100 nm, more specifically 80 nm to 100 nm. In this specification, the size may be a particle size, or an average particle size of the particle size. In this case, the average particle size means a particle size (D50) measured by a cumulative volume. Unless otherwise defined in this specification, such a particle size (D50) means an average particle size (D50) which means a diameter of a particle having a cumulative volume of 50% by volume in a particle size distribution. D50 may be measured by a method widely known to those skilled in the art, for example, it may be measured by a particle size analyzer, or it may be measured from a TEM (Transmission electron microscopy) or SEM photograph. After measurement using another method, for example, a measuring device using dynamic light-scattering, data analysis is performed to count the number of particles for each size range, and the average particle size can be easily calculated based on this.
[0032] In the electrolyte according to an embodiment, the non-aqueous organic solvent may include a carbonate-based solvent, and may also include a propionate-based solvent.
[0033] The content of the propionate-based solvent in the non-aqueous organic solvent may be 5% by volume to 80% by volume based on the total volume of the non-aqueous organic solvent. When the non-aqueous organic solvent contains a propionate-based solvent, particularly in the above content, the problem of gas generation during high temperature storage or use, particularly in a pouch-type battery, can be more effectively suppressed.
[0034] The propionate solvent may be methyl propionate, ethyl propionate, propyl propionate, or a combination thereof. When one or more propionate solvents are used, the mixing ratio may be appropriately adjusted. For example, ethyl propionate and propyl propionate may be mixed and used as the propionate solvent. In this case, the non-aqueous organic solvent may contain 5% to 40% by volume of ethyl propionate and 55% to 75% by volume of propyl propionate, and the remaining amount may contain a carbonate solvent. The mixing ratio of ethyl propionate and propyl propionate may be 25:75 to 30:70 by volume. When ethyl propionate and propyl propionate are used as the propionate solvent, particularly when used at the above content, gas generation can be more effectively suppressed and low-temperature cycle life characteristics can also be further improved.
[0035] The carbonate-based solvent may be dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), or a combination thereof. When one or more of the carbonate-based solvents are used, the mixing ratio may be appropriately adjusted. In addition, in the case of the carbonate-based solvent, it is preferable to mix a cyclic carbonate and a chain carbonate. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of 1:1 to 1:9, excellent electrolyte performance can be obtained.
[0036] In one embodiment, the non-aqueous organic solvent may further comprise an ester, an ether, a ketone, an alcohol, or an aprotic solvent.
[0037] Examples of the ester solvent include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, and caprolactone.
[0038] The ether solvent may be dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or the like, and the ketone solvent may be cyclohexanone, or the like.
[0039] Examples of the alcohol solvent that can be used include ethyl alcohol and isopropyl alcohol, and examples of the aprotic solvent that can be used include nitriles such as T-CN (T is a hydrocarbon group having a linear, branched, or cyclic structure with 2 to 20 carbon atoms and can contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, and dioxolanes such as 1,3-dioxolane.
[0040] In addition, the non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent. As the aromatic hydrocarbon-based organic solvent, an aromatic hydrocarbon-based compound represented by the following formula 2 may be used.
[0041] [ka]
[0042] (In the above Chemical Formula 2, R 10 ~R 15 are the same or different and are selected from the group consisting of hydrogen, halogen, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group, and combinations thereof.
[0043] Specific examples of the aromatic hydrocarbon organic solvent include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, It is selected from the group consisting of fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0044] The lithium secondary battery electrolyte may further include vinyl ethylene carbonate, vinylene carbonate, an ethylene carbonate-based compound represented by the following Formula 3, or a combination thereof, as a life-improving additive in order to improve the battery life.
[0045] [ka]
[0046] (In the above Chemical Formula 3, R 16 and R 17 are each independently selected from the group consisting of hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, R 16 and R17 At least one of is selected from the group consisting of a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, R 16 and R 17 are not all hydrogen.)
[0047] Representative examples of the ethylene carbonate-based compound include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, etc. When such a life-improving additive is further used, the amount used can be appropriately adjusted.
[0048] The lithium salt dissolves in an organic solvent and acts as a lithium ion source in the battery, enabling basic lithium secondary battery operation and promoting lithium ion movement between the positive and negative electrodes. Representative examples of such lithium salts include LiPF6, LiSbF6, LiAsF6, LiPO2F2, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide: LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiN(C x F 2x+1 SO2)(C y F 2y+1The electrolyte contains one or more supporting electrolyte salts selected from the group consisting of lithium difluoro(bisoxalato) phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato) borate: LiBOB), and lithium difluoro(oxolato)borate (LiDFOB). The lithium salt concentration is preferably within the range of 0.1M to 2.0M. When the lithium salt concentration is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore excellent electrolyte performance can be exhibited, and lithium ions can be effectively transferred.
[0049] In one embodiment, a negative electrode including the negative electrode active material includes a negative electrode active material layer including the negative electrode active material, and a current collector supporting the negative electrode active material layer.
[0050] The negative electrode active material layer includes a negative electrode active material and a binder, and may optionally further include a conductive material.
[0051] The content of the negative active material in the negative active material layer may be 95% by weight to 99% by weight based on the total weight of the negative active material layer. The content of the binder in the negative active material layer may be 1% by weight to 5% by weight based on the total weight of the negative active material layer. When a conductive material is further included, the negative active material may be 90% by weight to 98% by weight, the binder may be 1% by weight to 5% by weight, and the conductive material may be 1% by weight to 5% by weight.
[0052] The binder serves to adhere the negative active material particles to each other and to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.
[0053] The non-water-soluble binder may be an ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0054] Examples of the water-soluble binder include styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polymers containing ethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, ethylene propylene diene copolymers, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resins, acrylic resins, phenolic resins, epoxy resins, polyvinyl alcohol, and combinations thereof.
[0055] When a water-soluble binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity may be further included as a thickener. The cellulose-based compound may be a mixture of one or more of carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof. The alkali metal may be Na, K, or Li. The content of such a thickener may be 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.
[0056] The conductive material is used to impart electrical conductivity to the electrodes, and any material that does not cause chemical changes in the battery and is electronically conductive can be used. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, denka black, and carbon fibers; metal-based materials such as metal powders or metal fibers of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures thereof.
[0057] The current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0058] In one embodiment, a positive electrode comprising the positive electrode active material includes a positive electrode active material layer comprising the positive electrode active material and a current collector supporting the positive electrode active material layer.
[0059] The positive electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium (lithiated intercalation compound), and more specifically, one or more of cobalt, manganese, nickel, and a composite oxide of a metal and lithium obtained from a combination thereof may be used. More specifically, a compound represented by any one of the following chemical formulas may be used. Li a A 1-b X b D2(0.90≦a≦1.8,0≦b≦0.5);Li a A 1-b X b O2- c D c (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.05);Li a E 1-b X b O2- c D c (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.05);Li a E 2-b X b O 4-c D c (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.05);Li a Ni 1-b-c Co b X c D α (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.5,0<α≦2);Li a Ni 1-b-c Cob X c O 2-α T α (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.5,0<α<2);Li a Ni 1-b-c Co b X c O 2-α T2(0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.5,0<α<2);Li a Ni 1-b-c Mr b X c D α (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.5,0<α≦2);Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.5,0<α<2);Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.5,0<α<2);Li a Ni b HAVE BEEN c G d O2(0.90≦a≦1.8,0≦b≦0.9,0≦c≦0.5,0.001≦d≦0.1);Li a Ni b Co c Mr d G e O2(0.90≦a≦1.8,0≦b≦0.9,0≦c≦0.5,0≦d≦0.5,0.001≦e≦0.1);Li a NiG b O2(0.90≦a≦1.8,0.001≦b≦0.1) Li a CoG b O2(0.90≦a≦1.8,0.001≦b≦0.1);Li a Mr 1-b G b O2(0.90≦a≦1.8,0.001≦b≦0.1);Li a Mn2G bO4(0.90≦a≦1.8,0.001≦b≦0.1);Li a Mn 1-g G g PO4(0.90≦a≦1.8,0≦g≦0.5);QO2;QS2;LiQS2;V2O5;LiV2O5;LiZO2;LiNiVO4;Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) Fe2(PO4)3(0≦f≦2);Li a FePO4(0.90≦a≦1.8)
[0060] In the above formula, A is selected from the group consisting of Ni, Co, Mn, and combinations thereof; X is selected from the group consisting of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, and combinations thereof; D is selected from the group consisting of O, F, S, P, and combinations thereof; E is selected from the group consisting of Co, Mn, and combinations thereof; T is selected from the group consisting of F, S, P, and combinations thereof; G is selected from the group consisting of Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, and combinations thereof; Q is selected from the group consisting of Ti, Mo, Mn, and combinations thereof; Z is selected from the group consisting of Cr, V, Fe, Sc, Y, and combinations thereof; and J is obtained from the group consisting of V, Cr, Mn, Co, Ni, Cu, and combinations thereof.
[0061] Of course, the compound may have a coating layer on its surface, or the compound may be mixed with a compound having a coating layer. The coating layer may contain at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming the coating layer may be amorphous or crystalline. The coating elements contained in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming process may use any coating method as long as the compound is coated with such elements in a manner that does not adversely affect the properties of the positive electrode active material (e.g., spray coating, immersion, etc.), and this is well understood by those skilled in the art, so a detailed explanation will be omitted.
[0062] In one embodiment, the positive electrode active material is Li a Co 1-b X b D2(0.90≦a≦1.8,0≦b≦0.5), Li a Co 1-b X b O2- c D c (0.90≦a≦1.8,0≦b≦0.5,0≦c≦0.05);Li a Co 1-b X b O2- c D c (0≦b≦0.5, 0≦c≦0.05), or a combination of these is appropriate.
[0063] In the positive electrode, the content of the positive electrode active material may be 90 wt % to 98 wt % based on the total weight of the positive electrode active material layer.
[0064] In an embodiment, the positive electrode active material layer may further include a binder and a conductive material, the content of the binder and the conductive material being 1 wt % to 5 wt %, respectively, based on the total weight of the positive electrode active material layer.
[0065] The binder serves to adhere the positive electrode active material particles to each other and to the current collector. Representative examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, and nylon.
[0066] The conductive material is used to impart electrical conductivity to the electrodes, and any material that does not cause chemical changes in the battery and is electronically conductive can be used. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures thereof.
[0067] The current collector may be, but is not limited to, aluminum foil, nickel foil, or a combination thereof.
[0068] The positive and negative active material layers are formed by mixing an active material, a binder, and optionally a conductive material in a solvent to prepare an active material composition, and then coating the active material composition on a current collector. Since the method of forming the active material layer is widely known in the art, a detailed description thereof will be omitted in this specification. The solvent may be, but is not limited to, N-methylpyrrolidone. In addition, when a water-soluble binder is used in the negative active material layer, water may be used as the solvent used in preparing the negative active material composition.
[0069] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As the separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multi-layer film of two or more layers of these may be used, and of course, a mixed multi-layer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.
[0070] According to another embodiment, the separator may be a composite porous separator including a porous substrate and a functional layer located on the porous substrate. The functional layer may be capable of adding additional functions, and may be, for example, at least one of a heat-resistant layer and an adhesive layer. The heat-resistant layer may include a heat-resistant resin and, optionally, a filler. The adhesive layer may include an adhesive resin and, optionally, a filler. The filler may be an organic filler, an inorganic filler, or a combination thereof. The heat-resistant resin, adhesive resin, and filler may be any that can be used in separators in the art.
[0071] An exploded perspective view of a lithium secondary battery according to an embodiment of the present invention is shown in Fig. 1. Although the lithium secondary battery according to an embodiment has been described using a pouch-type battery as an example, the present invention is not limited thereto and may be applied to batteries of various shapes such as a cylindrical type and a square type.
[0072] 1, a lithium secondary pouch battery 100 according to an embodiment includes an electrode assembly 110 wound between a positive electrode 10 and a negative electrode 20 with a separator 30 interposed therebetween, a case 120 in which the electrode assembly 110 is housed, and an electrode tab 130 serving as an electrical path for directing a current generated in the electrode assembly 110 to the outside. Two surfaces of the case 120 are overlapped and sealed. An electrolyte is injected into the case 120 housing the electrode assembly 110, and the positive electrode 10, the negative electrode 20, and the separator 30 are immersed in the electrolyte (not shown). EXAMPLES
[0073] Examples and comparative examples of the present invention will be described below. However, the following examples are merely examples of the present invention, and the present invention is not limited to the following examples.
[0074] Example 1 An electrolyte for a lithium secondary battery was prepared by dissolving 1.3M LiPF6 in a non-aqueous organic solvent in which ethylene carbonate, propylene carbonate, ethyl propionate, and propyl propionate were mixed in a ratio of 10:15:30:45 by volume, and adding sulfolane of the following formula 1a. At this time, the content of sulfolane of the following formula 1a was 2.5 wt% based on the total content of the non-aqueous organic solvent and lithium salt (100 wt%).
[0075] [ka]
[0076] A negative electrode active material slurry was prepared by mixing 96% by weight of a negative electrode active material, which was a mixture of natural graphite and Si-carbon composite in a weight ratio of 95:5, 2% by weight of styrene-butadiene rubber binder, and 2% by weight of carboxymethyl cellulose in an aqueous solvent. The negative electrode active material slurry was coated on a copper foil, dried, and rolled to prepare a negative electrode. The Si-carbon composite had a core containing artificial graphite and silicon particles, and the surface of the core was coated with soft carbon, and the content of the artificial graphite was 40% by weight, the content of the silicon particles was 40% by weight, and the content of the amorphous carbon was 20% by weight, based on the total weight of the Si-carbon composite. The thickness of the soft carbon coating layer was 20 nm, and the average particle size (D50) of the silicon particles was 100 nm.
[0077] A positive electrode active material slurry was prepared by mixing 96 wt% LiCoO2 positive electrode active material, 2 wt% Ketjen black conductive material, and 2 wt% polyvinylidene fluoride in N-methylpyrrolidone solvent. The positive electrode active material slurry was coated on an aluminum foil, dried, and rolled to prepare a positive electrode. A 4.4V pouch-type lithium secondary battery was manufactured by a conventional method using the electrolyte, the positive electrode and the negative electrode.
[0078] Example 2 An electrolyte was prepared in the same manner as in Example 1, except that the content of the additive of Formula 1a was changed to 5 wt % based on the total content of the non-aqueous organic solvent and lithium salt (100 wt %). A pouch-type lithium secondary battery was prepared in the same manner as in Example 1 using the electrolyte and the anode and cathode of Example 1.
[0079] Example 3 An electrolyte was prepared in the same manner as in Example 1, except that the content of the additive of Formula 1a was changed to 10 wt % based on the total content of the non-aqueous organic solvent and lithium salt (100 wt %). A pouch-type lithium secondary battery was prepared in the same manner as in Example 1 using the electrolyte and the anode and cathode of Example 1.
[0080] (Reference example 1) An anode was prepared in the same manner as in Example 1, except that the mixing ratio of the natural graphite and the Si-carbon composite was changed to 95:5 by weight. An electrolyte was prepared in the same manner as in Example 1, except that the content of the additive of Chemical Formula 1a was changed to 12.5 wt % based on the total content of the non-aqueous organic solvent and the lithium salt (100 wt %). A pouch-type lithium secondary battery was prepared in the same manner as in Example 1, using the anode, the electrolyte, and the cathode of Example 1.
[0081] Example 4 A negative electrode was manufactured in the same manner as in Example 1, except that the mixing ratio of the natural graphite and the Si-carbon composite was changed to 97.5:2.5 by weight. A pouch-type lithium secondary battery was manufactured in the same manner as in Example 4, using the electrolyte of Example 1 and the positive electrode of Example 1.
[0082] Example 5 A pouch-type lithium secondary battery was manufactured in the same manner as in Example 4 using the negative electrode of Example 4, the electrolyte of Example 2, and the positive electrode of Example 1.
[0083] Example 6 A pouch-type lithium secondary battery was manufactured in the same manner as in Example 4 using the negative electrode of Example 4, the electrolyte of Example 3, and the positive electrode of Example 1.
[0084] (Reference example 2) A pouch-type lithium secondary battery was manufactured in the same manner as in Example 4 using the negative electrode of Example 4, the electrolyte of Reference Example 1, and the positive electrode of Example 1.
[0085] Comparative Example 1 An electrolyte for a lithium secondary battery was prepared by dissolving 1.3M LiPF6 in a non-aqueous organic solvent in which ethylene carbonate, propylene carbonate, ethyl propionate, and propyl propionate were mixed in a ratio of 10:15:30:45 by volume. A negative electrode active material slurry was prepared by mixing 96 wt% natural graphite negative electrode active material, 2 wt% styrene-butadiene rubber binder, and 2 wt% carboxymethyl cellulose in an aqueous solvent. The negative electrode active material slurry was coated on a copper foil, dried, and rolled to prepare a negative electrode. A pouch-type lithium secondary battery was manufactured in the same manner as in Example 1, except that the electrolyte, the negative electrode, and the positive electrode of Example 1 were used.
[0086] Comparative Example 2 A pouch-type lithium secondary battery was manufactured in the same manner as in Comparative Example 1 using the electrolyte of Example 1, the anode of Comparative Example 1, and the cathode of Comparative Example 1.
[0087] Comparative Example 3 A pouch-type lithium secondary battery was manufactured in the same manner as in Comparative Example 2, except that an electrolyte prepared by changing the content of sulfolane of Formula 1a to 5 wt % based on the total content of the non-aqueous organic solvent and lithium salt (100 wt %) was used.
[0088] Comparative Example 4 A pouch-type lithium secondary battery was manufactured in the same manner as in Comparative Example 2, except that an electrolyte prepared by changing the content of sulfolane of Formula 1a to 10 wt % based on the total content of the non-aqueous organic solvent and lithium salt (100 wt %) was used.
[0089] Comparative Example 5 A pouch-type lithium secondary battery was manufactured in the same manner as in Comparative Example 1, except that the electrolyte of Comparative Example 1, the anode of Example 1, and the cathode of Example 1 were used.
[0090] Comparative Example 6 A pouch-type lithium secondary battery was manufactured in the same manner as in Comparative Example 1, except that the electrolyte of Comparative Example 1, the anode of Example 5, and the cathode of Comparative Example 1 were used.
[0091] Comparative Example 7 A negative electrode was prepared in the same manner as in Example 1, except that the mixing ratio of the natural graphite and the Si-carbon composite was changed to 92.5:7.5 by weight. A pouch-type lithium secondary battery was prepared in the same manner as in Comparative Example 1, except that the negative electrode, the electrolyte of Comparative Example 3, and the positive electrode of Comparative Example 1 were used.
[0092] The mixing ratios of the graphite and the Si-carbon composite and the sulfolane content of Chemical Formula 1a in Examples 1 to 6, Reference Examples 1 and 2, and Comparative Examples 1 to 7 are summarized in Table 1 below.
[0093] [Table 1]
[0094] *Evaluation of direct current internal resistance (DC-IR)
[0095] The lithium secondary batteries produced in Examples 1 to 6, Reference Examples 1 and 2, and Comparative Examples 1 to 7 were discharged at a constant current of 10 A for 10 seconds at SOC100 (state of charge, fully charged state, a state in which the battery is charged to 100% charge capacity when the total battery charge capacity is 100%) at 60° C., discharged at a constant current of 1 A for 10 seconds, and then discharged at a constant current of 10 A for 4 seconds, and the voltage and current values immediately before storage were measured, and the batteries were also stored at 60° C. for 30 days, and the voltage and current values were measured.
[0096] The DC resistance was calculated from the data at 18 seconds and 23 seconds using the formula ΔR=ΔV / ΔI, i.e., (measured voltage values after 10 sec discharge at 10 A, 10 sec discharge at 1 A, and 4 sec discharge at 10 A - measured voltage values after 10 sec discharge at 10 A and 8 sec discharge at 1 A) / current value after 10 sec discharge at 10 A and 8 sec discharge.
[0097] The DC resistance value immediately before storage and the DC resistance value measured after 30 days were used to calculate the resistance increase rate according to the following formula 1.
[0098] The result, early DC-IR, 60 In °C The DC-IR and the rate of increase in resistance after three days of storage are shown in Table 1 below. In order to more clearly examine the effect according to the content of the Si-carbon composite, the results of Examples 2 and 5 and Comparative Example 3 are shown in Figure 2, and the results of Examples 1 to 6, Reference Examples 1 and 2, and Comparative Examples 1 to 7 are shown in Figure 3. In order to more clearly examine the effect according to the content of sulfolane in Chemical Formula 1a, the results of Examples 1 to 3, Reference Example 1, and Comparative Example 5 are shown in Figure 4. [Formula 1] DCIR increase rate = [DCIR(30d.)] / DCIR(0d.)×100% In formula 1, DCIR(30d.) indicates the DCIR after 30 days, and DCIR(0d.) indicates the DCIR immediately before storage.
[0099] [Table 2]
[0100] As shown in Table 2 and FIG. 3, the lithium secondary batteries of Examples 1 to 6 using artificial graphite and Si-carbon composite as negative electrode active materials and electrolytes containing sulfolane of Chemical Formula 1a, particularly 0.1 wt % to 10 wt %, maintained appropriate initial resistance and exhibited low resistance increase rates after high-temperature storage.
[0101] It can be seen that, in the case of Reference Examples 1 and 2 in which artificial graphite and a Si-carbon composite were used as negative electrode active materials and sulfolane of Chemical Formula 1a was included, and an excessive amount of sulfolane was included at 12.5 wt %, the resistance increase rate after high-temperature storage was very high.
[0102] As can be seen from the results of Comparative Examples 1 to 7 in Table 2 and Figure 3, when no Si-carbon composite is used as the negative electrode active material, the high temperature resistance increase rate is high even when sulfolane of Chemical Formula 1a is included. From the results shown in Figure 2, it can be clearly seen that the effect of reducing the DC-IR and high temperature storage increase rate after storage at 60°C for 30 days by including sulfolane of Chemical Formula 1a can be obtained when the Si-carbon composite is included as the negative electrode active material.
[0103] Furthermore, it can be clearly seen from the results of FIG. 4 that the DC-IR and high-temperature storage increase rate after storage at 60° C. for 30 days are reduced by using an electrolyte containing 2.5 wt %, 5 wt %, and 10 wt % of sulfolane of chemical formula 1a.
[0104] The present invention is not limited to the above embodiment, and can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention pertains can understand that the present invention can be embodied in other specific forms without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the above embodiment is illustrative in all respects and not limiting.
Claims
1. An electrolyte comprising a non-aqueous organic solvent, a lithium salt, and an additive represented by the following Chemical Formula 1: A negative electrode comprising a negative electrode active material comprising a Si-carbon composite; and A positive electrode containing a positive electrode active material A lithium secondary battery comprising: 【Chemistry 1】 (In the above Chemical Formula 1, R 1 ~R 8 are each independently a hydrogen atom, a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C2-C30 alkenyl group, a substituted or unsubstituted C2-C30 alkynyl group, a substituted or unsubstituted C3-C30 cycloalkyl group, a substituted or unsubstituted C3-C30 cycloalkenyl group, a substituted or unsubstituted C3-C30 cycloalkynyl group, or a substituted or unsubstituted C6-C30 aryl group. The content of the additive represented by the formula 1 is 0.1 wt % to 10 wt % based on the content of the non-aqueous organic solvent and the lithium salt being 100 wt %; The content of the Si-carbon composite is 0.1 wt % to 5 wt % based on the total weight of the negative electrode active material.
2. The R 1 ~R 8 are each independently a hydrogen atom, a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C2 to C10 alkenyl group, a substituted or unsubstituted C2 to C10 alkynyl group, a substituted or unsubstituted C3 to C10 cycloalkyl group, a substituted or unsubstituted C3 to C10 cycloalkenyl group, a substituted or unsubstituted C3 to C10 cycloalkynyl group, or a substituted or unsubstituted C6 to C10 aryl group. The lithium secondary battery according to claim 1,
3. 2. The lithium secondary battery of claim 1, wherein the additive represented by Chemical Formula 1 is sulfolane, methylsulfolane, dimethylsulfolane, or a combination thereof.
4. The lithium secondary battery according to claim 1 , wherein the negative electrode active material further comprises crystalline carbon.
5. 2. The lithium secondary battery according to claim 1, wherein the non-aqueous organic solvent comprises a propionate-based solvent.
6. 6. The lithium secondary battery according to claim 5, wherein the propionate-based solvent is methyl propionate, ethyl propionate, propyl propionate, or a combination thereof.
7. The lithium secondary battery according to claim 5, wherein the content of the propionate-based solvent is 5% by volume to 80% by volume based on the total volume of the non-aqueous organic solvent.
8. 2. The lithium secondary battery of claim 1, wherein the Si-carbon composite comprises Si nanoparticles and amorphous carbon.
9. The Si-carbon composite includes a core and a coating layer surrounding the core, the core comprises amorphous or crystalline carbon and Si nanoparticles; The lithium secondary battery according to claim 1 , wherein the coating layer comprises amorphous carbon.
10. 10. The lithium secondary battery according to claim 9, wherein the coating layer has a thickness of 1 nm to 100 nm.
11. 10. The lithium secondary battery according to claim 9, wherein the content of the Si nanoparticles is 1% by weight to 60% by weight based on 100% by weight of the entire Si-carbon composite.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery, and battery pack
JP2012094353A
Non-aqueous electrolyte secondary cell
WO2013069793A1
Electrolyte solution and electrochemical device
WO2014038343A1
Lithium ion secondary battery
WO2014080871A1
Secondary cell electrolyte and secondary cell
WO2014181877A1