Polyester resin composition, polyester injection molded article, polyester extrusion molded article, polyester foam, polyester container, polyester bottle, polyester tableware, and polyester baby bottle

A polyester resin composition with a specific diol and dicarboxylic acid blend and polycarbodiimide improves heat resistance and transparency, addressing the limitations of existing resins for high-heat applications.

JP7564998B2Active Publication Date: 2024-10-10MITSUBISHI GAS CHEM CO INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021516152
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-25
Filing Date
2020-04-22
Publication Date
2024-10-10
Estimated Expiration
2040-04-22

AI Technical Summary

Technical Problem

Existing polyester resins, such as PET and modified PET, suffer from issues of high crystallinity leading to loss of transparency and poor heat resistance, making them unsuitable for applications requiring high heat resistance and transparency, such as baby bottles and tableware.

Method used

A polyester resin composition containing a specific blend of polyester resin and polycarbodiimide, with predetermined diol and dicarboxylic acid units, including a cyclic acetal skeleton and alicyclic diols, to enhance heat resistance, transparency, and impact resistance.

Benefits of technology

The composition exhibits excellent heat resistance, transparency, and impact resistance, reducing brittleness after heat treatment, suitable for applications like baby bottles and tableware that require high heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564998000001
    Figure 0007564998000001
  • Figure 0007564998000002
    Figure 0007564998000002
  • Figure 0007564998000003
    Figure 0007564998000003
Patent Text Reader

Abstract

A polyester resin composition including 97.0 mass% to 99.9 mass% of a polyester resin (A) and 0.1 mass % to 3.0 mass% of a polycarbodiimide (B), wherein dicarboxylic acid constituent units in the polyester resin (A) include terephthalic acid units and / or 2,6-napthalene dicarboxylic acid units, 5 mol% to 90 mol% of the diol constituent units in the polyester resin (A) are units derived from a diol having a cyclic acetal skeleton represented by formula (1) or formula (2), 0 mol% to 90 mol% of the diol constituent units being units derived from an alicyclic diol, and the polycarbodiimide (B) having two or more carbodiimide groups in each molecule thereof. (In formula (1), R1 and R2 each independently represent a C1-10 aliphatic group, a C3-10 alicyclic group, or a C6-10 aromatic group.) (In formula (2), R1 is the same as in formula (1), and R3 represents a C1-10 aliphatic group, a C3-10 alicyclic group, or a C6-10 aromatic group.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester resin composition, a polyester injection molded article, a polyester extrusion molded article, a polyester foam, a polyester container, a polyester bottle, a polyester tableware, and a polyester baby bottle. [Background technology]

[0002] Aromatic saturated polyester resins, particularly polyethylene terephthalate (hereinafter sometimes referred to as "PET"), are resins with a good balance of mechanical properties, solvent resistance, aroma retention, weather resistance, recyclability, etc., and are widely used mainly for applications such as bottles and films. However, PET has drawbacks in terms of crystallinity and heat resistance. That is, in terms of crystallinity, PET is highly crystalline, so when attempting to manufacture thick molded bodies or sheets, it will whiten due to crystallization and lose transparency. In terms of heat resistance, PET has a glass transition temperature of about 80°C, so it is unsuitable for applications requiring high heat resistance and transparency, such as products used inside automobiles, packaging materials for import and export, food packaging materials that are retorted or heated in a microwave oven, and baby bottles and tableware that are heat sterilized.

[0003] For this reason, low-crystalline polyester resins such as modified PET partially copolymerized with 1,4-cyclohexanedimethanol and modified PET partially modified with isophthalic acid have been used in applications requiring transparency. However, although modified PET partially copolymerized with 1,4-cyclohexanedimethanol and modified PET partially modified with isophthalic acid have improved transparency compared to PET, the glass transition temperatures of these resins are around 80°C and they have poor heat resistance.

[0004] In addition, in fields where heat resistance is required, polyester resins with high glass transition temperatures, such as polyethylene 2,6-naphthalate (hereinafter sometimes referred to as "PEN") and poly(1,4-cyclohexanedimethylene terephthalate), have been used. However, although PEN and poly(1,4-cyclohexanedimethylene terephthalate) have improved heat resistance, they also have high crystallinity and poor transparency.

[0005] On the other hand, polyester resins containing diols having a cyclic acetal skeleton have been proposed as polyester resins that have high transparency while improving the heat resistance of PET and PEN (see, for example, Patent Document 1). Such polyester resins can be used in applications that require transparency and heat resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-105873 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the polyester resin described in Patent Document 1 has heat resistance sufficient to maintain its shape when heated for a long period of time in an oven or with hot water, but has a problem of embrittlement. Considering applications requiring high impact resistance even after heat treatment, there is still room for improvement. The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and an object of the present invention is to provide a polyester resin composition that is excellent in heat resistance, transparency, and impact resistance and is less likely to become embrittled after heat treatment. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted extensive research and found that a polyester resin composition containing a polyester resin having a specified composition and a specified amount of polycarbodiimide has excellent heat resistance, transparency and impact resistance, and is less likely to become embrittled after heat treatment, thereby completing the present invention.

[0009] That is, the present invention includes the following aspects. [1] A polyester resin composition comprising: 97.0% by mass or more and 99.9% by mass or less of a polyester resin (A); and 0.1% by mass or more and 3.0% by mass or less of a polycarbodiimide (B), the dicarboxylic acid constituent units in the polyester resin (A) contain terephthalic acid units and / or 2,6-naphthalenedicarboxylic acid units, the polyester resin (A) contains diol structural units that are derived from a diol having a cyclic acetal skeleton represented by the following formula (1) or (2), and the diol structural units contain diol structural units that are derived from an alicyclic diol, The polyester resin composition, wherein the polycarbodiimide (B) has two or more carbodiimide groups in the molecule. [ka] (In formula (1), R 1 and R 2 each independently represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms. [ka] (In formula (2), R 1 is the same as above, and R 3 represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms. [2] The polyester resin composition according to [1], wherein the diol having a cyclic acetal skeleton is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane. [3] The polyester resin composition according to [1], wherein the alicyclic diol is 1,4-cyclohexanedimethanol. [4] A polyester-based injection-molded article comprising the polyester resin composition according to any one of [1] to [3]. [5] A polyester-based extrusion molded product comprising the polyester resin composition according to any one of [1] to [3]. [6] A polyester foam comprising the polyester resin composition according to any one of [1] to [3]. [7] A polyester-based container comprising the polyester resin composition according to any one of [1] to [3]. [8] A polyester bottle comprising the polyester resin composition according to any one of [1] to [3]. [9] A polyester-based tableware comprising the polyester resin composition according to any one of [1] to [3].

[10] A polyester-based baby bottle comprising the polyester resin composition according to any one of [1] to [3]. Effect of the Invention

[0010] The polyester resin composition of the present invention is excellent in heat resistance, transparency, and impact resistance, and is less susceptible to embrittlement after heat treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0012] <Polyester resin composition> The polyester resin composition of the present embodiment is a polyester resin composition comprising 97.0 mass % or more and 99.9 mass % or less of a polyester resin (A) and 0.1 mass % or more and 3.0 mass % or less of a polycarbodiimide (B), in which the dicarboxylic acid constituent units in the polyester resin (A) contain terephthalic acid units and / or 2,6-naphthalenedicarboxylic acid units, 5 mol % or more and 90 mol % or less of the diol constituent units in the polyester resin (A) are units derived from a diol having a cyclic acetal skeleton represented by the following formula (1) or formula (2), and 0 mol % or more and 90 mol % or less of the diol constituent units are units derived from an alicyclic diol, and the polycarbodiimide (B) has two or more carbodiimide groups in its molecule. [ka] (In formula (1), R 1 and R 2 each independently represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms. [ka] (In formula (2), R 1 is the same as above, and R 3 represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms.

[0013] Since the polyester resin composition of the present embodiment is constituted as described above, it has excellent heat resistance, transparency, and impact resistance, and is less likely to become brittle after heat treatment. Therefore, it can be suitably used for products used inside automobiles, packaging materials for import and export, food packaging materials that undergo retort treatment or microwave heating, containers such as baby bottles and tableware that undergo heat sterilization treatment, and other applications that require high heat resistance. Hereinafter, each component contained in the polyester resin composition of the present embodiment will be described.

[0014] [Polyester resin (A)] As described above, the polyester resin (A) has the specified dicarboxylic acid constituent units and diol constituent units, and is contained in an amount of 97.0% by mass or more and 99.9% by mass or less relative to 100% by mass of the polyester resin composition.

[0015] (Diol building block) The diol constituent units in the polyester resin (A) contain 5 mol % to 90 mol % of units derived from a diol having a cyclic acetal skeleton represented by the above formula (1) or (2) relative to 100 mol % of the diol constituent units, and contain 0 mol % to 90 mol % of units derived from an alicyclic diol. Thus, the units derived from an alicyclic diol in this embodiment are optional constituent units that do not need to be contained in the polyester resin (A).

[0016] (Units derived from diols having a cyclic acetal skeleton) In the above formulas (1) and (2), R 1 and R 2 R each independently represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms, and is preferably a methylene group, an ethylene group, a propylene group, a butylene group, or a structural isomer thereof, such as an isopropylene group or an isobutylene group. 3is an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms, and is preferably a methyl group, an ethyl group, a propyl group, a butyl group, or a structural isomer thereof, such as an isopropyl group or an isobutyl group. As the diol having a cyclic acetal skeleton represented by the above formula (1), 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane is particularly preferred, and as the diol having a cyclic acetal skeleton represented by the above formula (2), 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane is particularly preferred.

[0017] (Units derived from alicyclic diols) The alicyclic diol unit in the diol constituent unit of the polyester resin (A) is not particularly limited, and examples thereof include units derived from diols such as 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,2-decahydronaphthalenedimethanol, 1,3-decahydronaphthalenedimethanol, 1,4-decahydronaphthalenedimethanol, 1,5-decahydronaphthalenedimethanol, 1,6-decahydronaphthalenedimethanol, 2,7-decahydronaphthalenedimethanol, tetralin dimethanol, norbornene dimethanol, tricyclodecane dimethanol, and pentacyclododecane dimethanol. Of these, units derived from 1,4-cyclohexanedimethanol, norbornene dimethanol, tricyclodecane dimethanol, and 2,6-decahydronaphthalenedimethanol are preferred, and units derived from 1,4-cyclohexanedimethanol are particularly preferred.

[0018] (Other diol building blocks) The diol structural unit of the present embodiment may contain other diol structural units other than the diol unit having a cyclic acetal skeleton and the alicyclic diol unit. The content of the other diol structural units may be 0 mol% or more and 95 mol% or less with respect to 100 mol% of the diol structural units. Examples of other diol constituent units include units derived from diols such as aliphatic diols, such as ethylene glycol, trimethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, propylene glycol, and neopentyl glycol; polyether compounds, such as polyethylene glycol, polypropylene glycol, and polybutylene glycol; bisphenols, such as 4,4'-(1-methylethylidene)bisphenol, methylenebisphenol (bisphenol F), 4,4'-cyclohexylidenebisphenol (bisphenol Z), and 4,4'-sulfonylbisphenol (bisphenol S); alkylene oxide adducts of the above bisphenols; aromatic dihydroxy compounds, such as hydroquinone, resorcinol, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, and 4,4'-dihydroxydiphenylbenzophenone; and alkylene oxide adducts of the above aromatic dihydroxy compounds. In consideration of the mechanical strength, heat resistance, and availability of the polyester resin, when other diol constituent units are contained, it is preferable that the units are derived from ethylene glycol.

[0019] (Dicarboxylic acid structural unit) The dicarboxylic acid unit in the polyester resin (A) contains a terephthalic acid unit and / or a 2,6-naphthalenedicarboxylic acid unit. The terephthalic acid unit means a unit derived from terephthalic acid, and the 2,6-naphthalenedicarboxylic acid unit means a unit derived from 2,6-naphthalenedicarboxylic acid. The dicarboxylic acid unit may contain other dicarboxylic acid units as long as the object of the present embodiment is not impaired. Examples of other dicarboxylic acid constituent units include, but are not limited to, units derived from aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, dodecanedicarboxylic acid, cyclohexanedicarboxylic acid, decalindicarboxylic acid, norbornanedicarboxylic acid, tricyclodecanedicarboxylic acid, pentacyclododecanedicarboxylic acid, 3,9-bis(1,1-dimethyl-2-carboxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, and 5-carboxy-5-ethyl-2-(1,1-dimethyl-2-carboxyethyl)-1,3-dioxane; and units derived from aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 2-methylterephthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, biphenyldicarboxylic acid, and tetralindicarboxylic acid. In this embodiment, from the viewpoint of sufficiently enhancing the balance of physical properties such as transparency, heat resistance, impact resistance, and mechanical strength of the polyester resin (A), the terephthalic acid unit and / or the 2,6-naphthalenedicarboxylic acid unit is preferably contained in an amount of 80 mol% or more and 100 mol% or less, more preferably 90 mol% or more and 100 mol% or less, and particularly preferably 100 mol%, relative to 100 mol% of the dicarboxylic acid constituent units.

[0020] The polyester resin (A) contains 5 mol % or more and 90 mol % or less of the units derived from the diol having a cyclic acetal skeleton relative to 100 mol % of all diol constituent units, so that the crystallinity is reduced and the glass transition temperature is increased, resulting in high transparency and high heat resistance. The polyester resin (A) has a good balance of transparency and heat resistance compared to, for example, polyester resins in which 100 mol % of the diol constituent units are units derived from ethylene glycol and 1,4-cyclohexanedimethanol, and other polyester resins such as PET, polybutylene terephthalate, and polylactic acid. From the same viewpoint, the polyester resin (A) preferably contains 15 mol % or more and 80 mol % or less, more preferably 20 mol % or more and 70 mol % or less of the units derived from the diol having a cyclic acetal skeleton.

[0021] The polyester resin (A) contains the above-mentioned alicyclic diol-derived units in an amount of 0 mol % to 90 mol % based on 100 mol % of all diol constituent units. In the present embodiment, from the viewpoint of further improving the impact resistance of the polyester resin (A), the polyester resin (A) contains the alicyclic diol-derived units in an amount of preferably 10 mol % to 90 mol %, more preferably 15 mol % to 90 mol %.

[0022] In the present embodiment, from the viewpoint of impact resistance, examples of the polyester resin (A) include a polyester resin in which 15 mol % or more and 50 mol % or less of the diol constituent units are units derived from a diol having a cyclic acetal skeleton, and 15 mol % or more and 85 mol % or less of the units are units derived from an alicyclic diol.

[0023] In this embodiment, particularly taking into consideration the balance of transparency, heat resistance, impact resistance, mechanical strength, and the like, it is preferred that 100 mol % of the dicarboxylic acid constituent units in the polyester resin (A) are terephthalic acid units and / or 2,6-naphthalenedicarboxylic acid, and that 5 mol % to 90 mol % of the diol constituent units are units derived from 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, that 0 mol % to 90 mol % of units derived from 1,4-cyclohexanedimethanol, and that 0 mol % to 90 mol % of units derived from ethylene glycol. From a similar viewpoint, it is particularly preferred that 100 mol % of the dicarboxylic acid constituent units in the polyester resin (A) are terephthalic acid units and / or 2,6-naphthalenedicarboxylic acid units, and that 15 mol % to 50 mol % of the diol constituent units are units derived from 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 15 mol % to 85 mol % are units derived from 1,4-cyclohexanedimethanol, and 0 mol % to 70 mol % are units derived from ethylene glycol.

[0024] (Other building blocks) The polyester resin (A) may contain monoalcohol units such as butyl alcohol, hexyl alcohol, and octyl alcohol; trihydric or higher polyhydric alcohol units such as trimethylolpropane, glycerin, 1,3,5-pentanetriol, and pentaerythritol; monocarboxylic acid units such as benzoic acid, propionic acid, and butyric acid; polycarboxylic acid units such as trimellitic acid and pyromellitic acid; and oxyacid units such as glycolic acid, lactic acid, hydroxybutyric acid, 2-hydroxyisobutyric acid, and hydroxybenzoic acid, provided that the object of this embodiment is not impaired.

[0025] The method for producing the polyester resin of the present embodiment is not particularly limited, and a conventionally known method can be applied. For example, a melt polymerization method such as an ester exchange method or a direct esterification method, or a solution polymerization method can be mentioned. Conventionally known ester exchange catalysts, esterification catalysts, etherification inhibitors, various stabilizers such as heat stabilizers and light stabilizers, polymerization regulators, etc. can also be used.

[0026] [Polycarbodiimide (B)] The polycarbodiimide (B) in this embodiment is not particularly limited as long as it has two or more carbodiimide groups in the molecule, and various known polycarbodiimides can be used. For example, aromatic polycarbodiimides and aliphatic polycarbodiimides described later can be mentioned.

[0027] Aromatic polycarbodiimide is a compound in which a carbodiimide group is directly bonded to an aromatic ring, and can be synthesized by decarboxylation condensation reaction of diisocyanate using a carbodiimidization catalyst such as an organic phosphorus compound or an organic metal compound, but is not limited thereto. Specific examples of the diisocyanate include, but are not limited to, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 3,3',5,5'-tetraisopropylbiphenyl-4,4'-diisocyanate, 1,3,5-triisopropylbenzene-2,4-diisocyanate, etc. These may be used alone or in combination of two or more. Among these, 4,4'-diphenylmethane diisocyanate and 1,3,5-triisopropylbenzene-2,4-diisocyanate are preferred from the viewpoint of stability.

[0028] Aliphatic polycarbodiimide is a compound in which a carbodiimide group is bonded to a carbon atom other than an aromatic ring, and can be synthesized by decarboxylation condensation reaction of diisocyanate using a carbodiimidization catalyst such as an organic phosphorus compound or an organic metal compound, without being particularly limited thereto. Specific examples of the diisocyanate include, but are not limited to, hexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, methylcyclohexane diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, xylylene diisocyanate, tetramethylxylylene diisocyanate, etc. These may be used alone or in combination of two or more. Among these, 4,4'-dicyclohexylmethane diisocyanate is preferred from the viewpoint of stability.

[0029] The aromatic polycarbodiimide or aliphatic polycarbodiimide can be capped by reacting with a monofunctional compound that is reactive with the isocyanate group at the end of the diisocyanate used in the synthesis, thereby adjusting the degree of polymerization.Specific examples of such compounds include, but are not limited to, monoisocyanates such as phenylisocyanate, tolylisocyanate, isopropylphenylisocyanate, and cyclohexylisocyanate; alcohols such as methanol, isopropyl alcohol, phenol, and polyethylene glycol monomethyl ether; amines such as butylamine, diethylamine, and cyclohexylamine; and carboxylic acids such as propionic acid and benzoic acid.

[0030] From the viewpoints of improving the impact resistance of the polyester resin composition and suppressing embrittlement after heat treatment, the degree of polymerization of the polycarbodiimide (B) is preferably from 2 to 50, more preferably from 5 to 30. From the viewpoints of further improving the impact resistance of the polyester resin composition and further suppressing embrittlement after heat treatment, it is particularly preferable to use an aliphatic polycarbodiimide made of 4,4'-dicyclohexylmethane diisocyanate having a degree of polymerization of from 5 to 30 as the polycarbodiimide (B).

[0031] The polycarbodiimide (B) may be an aromatic polycarbodiimide or an aliphatic polycarbodiimide, and may be used alone or in combination of two or more of them. In the present embodiment, it is preferable to use an aliphatic polycarbodiimide from the viewpoint of stability and reactivity of the carbodiimide group.

[0032] (Mechanism of action) Here, the mechanism of action of the polyester resin composition of the present embodiment will be described, but this explanation is based on speculation and is not intended to limit the mechanism of action to the following. That is, as described above, the polyester resin (A) exhibits excellent performance in heat resistance, transparency and impact resistance, but in the polyester resin composition of this embodiment, the polycarbodiimide (B) extends or branches the molecular chain of the polyester resin (A), thereby not only obtaining a good balance of physical properties such as heat resistance, transparency and impact resistance, but also making the balance of physical properties particularly good. That is, the action of the polycarbodiimide (B) in combination with the performance of the polyester resin (A) ensures good heat resistance and transparency, and in particular improves impact resistance, and the effect of significantly suppressing embrittlement after heat treatment is achieved. From the above viewpoint, the content of the polyester resin (A) is 97.0 mass% or more and the content of the polycarbodiimide (B) is 3.0 mass% or less with respect to 100 mass% of the polyester resin composition. If the content of the polyester resin (A) is less than 97.0 mass%, it becomes difficult to ensure a balance of heat resistance, transparency and impact resistance. If the content of polycarbodiimide (B) exceeds 3.0% by mass, the impact resistance becomes insufficient due to aggregates, deterioration products, gelation products, etc. caused by polycarbodiimide (B), and embrittlement after heat treatment is extremely likely to progress. Therefore, it is important that the polyester resin composition of this embodiment contains 97.0% by mass or more and 99.9% by mass or less of polyester resin (A) and 0.1% by mass or more and 3.0% by mass or less of polycarbodiimide (B). From the above-mentioned viewpoint, the content of polyester resin (A) in the polyester resin composition is preferably 98.0% by mass or more and 99.9% by mass or less, and more preferably 99.0% by mass or more and 99.9% by mass or less. Similarly, the content of polycarbodiimide (B) in the polyester resin composition is preferably 0.1% by mass or more and 2.0% by mass or less, more preferably 0.1% by mass or more and 1.0% by mass or less, and even more preferably 0.2% by mass or more and 1.0% by mass or less.

[0033] The method of adding the polycarbodiimide (B) and the optional components described later to the polyester resin (A) is not particularly limited, but melt-kneading using an extruder is preferred. In this case, a high-concentration polycarbodiimide may be melt-kneaded to prepare a master batch, which may be diluted to a predetermined concentration during molding.

[0034] [Optional ingredients] The polyester resin composition of the present embodiment may further contain optional components other than the polyester resin (A) and the polycarbodiimide (B). Such optional components are not limited to the following, but may include various additives such as antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, extenders, matting agents, drying regulators, antistatic agents, antisettling agents, surfactants, flow improvers, drying oils, waxes, fillers, colorants, reinforcing agents, surface smoothing agents, leveling agents, and curing reaction accelerators, and molding aids. In addition, the optional components may include resins and oligomers such as polyolefin resins, polyester resins other than the polyester resin (A), polyamide resins, polycarbonate resins, acrylonitrile resins, vinyl chloride resins, vinyl acetate resins, polyacrylic acid resins, polymethacrylic acid resins, polystyrene, ABS resins, polyimide resins, and AS resins. The content of the optional components is not particularly limited, but from the viewpoints of improving impact resistance while ensuring good heat resistance and transparency, and effectively suppressing embrittlement after heat treatment, the content is preferably 2.9 mass% or less, more preferably 1.0 mass% or less, and particularly preferably 0.5 mass% or less, relative to 100 mass% of the polyester resin composition.

[0035] [Physical Properties] The glass transition temperature of the polyester resin (A) is preferably 95°C or higher, more preferably 110°C or higher, and even more preferably 130°C or higher. When the glass transition temperature is within the above range, the polyester resin composition of the present embodiment tends to have better heat resistance. Therefore, it can be used in applications requiring high heat resistance that could not be used with conventional PET or modified PET partially copolymerized with 1,4-cyclohexanedimethanol or isophthalic acid. For example, it can be used in automobiles and holds of ships passing through the equator (said to reach 70 to 80°C), so it can be suitably used for automobile interiors, containers for air fresheners and eye drops used in automobiles, and packaging materials used for import and export, such as blister packs. It can also be suitably used for applications in which high-temperature treatment is performed, such as food packaging materials that are heated in a microwave oven or retorted, and containers such as baby bottles and tableware that are heat sterilized. The glass transition temperature can be measured based on the method described in the examples below. The glass transition temperature can be adjusted to the above-mentioned preferred range, for example, by appropriately selecting the dicarboxylic acid constituent unit and the diol constituent unit in the polyester resin (A) based on the above-mentioned preferred embodiment.

[0036] The calorific value of the crystallization exothermic peak during cooling of the polyester resin (A) is preferably 5 J / g or less, more preferably 3 J / g or less. When the crystallization exothermic peak during cooling is within the above range, the polyester resin composition of the present embodiment tends to have lower crystallinity, and can be suitably used for applications requiring high transparency. The calorific value of the crystallization peak during cooling can be measured based on the method described in the examples below. The calorific value of the crystallization peak during cooling can be adjusted to the above-mentioned preferred range, for example, by appropriately selecting the dicarboxylic acid constituent unit and the diol constituent unit in the polyester resin (A) based on the above-mentioned preferred embodiment.

[0037] The haze of a test piece having a thickness of 3.2 mm obtained by injection molding the polyester resin composition of this embodiment is preferably 4% or less, more preferably 3% or less. When the haze is within the above range, the polyester resin composition of this embodiment tends to exhibit higher transparency. The haze can be measured based on the method described in the examples below. The haze can be adjusted to the above-mentioned preferred range, for example, by appropriately selecting the dicarboxylic acid constituent unit and the diol constituent unit in the polyester resin (A) based on the above-mentioned preferred embodiment.

[0038] Ten test pieces, each having a length of 63.5 mm, a width of 12.7 mm, a thickness of 3.2 mm, and no notch, obtained by injection molding the polyester resin composition of this embodiment are immersed in hot water at 50 to 100°C for 24 hours, and then the number of breaks in the test pieces in an Izod test carried out using a hammer with a capacity of 4 J is preferably 2 or less, more preferably 1 or less. When the number of breaks is within the above range, the polyester resin composition of this embodiment tends to exhibit practically sufficient impact resistance in many applications. The number of breaks can be measured based on the method described in the examples below. The number of breaks can be adjusted to the above-mentioned preferred range, for example, by appropriately selecting the dicarboxylic acid constitutional unit and the diol constitutional unit in the polyester resin (A) based on the above-mentioned preferred embodiment.

[0039] The polyester resin composition of this embodiment can be further provided with UV barrier properties by adjusting the 2,6-naphthalenedicarboxylic acid unit in the dicarboxylic acid constituent unit in the polyester resin (A) to an appropriate ratio. Specifically, when 0.1 mol % or more and 100 mol % or less of the dicarboxylic acid constituent unit is a 2,6-naphthalenedicarboxylic acid unit, the polyester resin composition of this embodiment tends to have good UV barrier properties. From the same viewpoint, it is particularly preferable that 90 mol % or more and 100 mol % or less of the dicarboxylic acid constituent unit in the polyester resin (A) is a 2,6-naphthalenedicarboxylic acid unit.

[0040] The polyester resin composition of the present embodiment may further contain a thermoplastic resin such as polyethylene terephthalate, polybutylene terephthalate, etc., as a polyester resin other than the polyester resin (A) within a range that does not impair the object. In this case, too, the polyester resin composition can be prepared by melt-kneading the polyester resin (A), the polycarbodiimide (B), and the thermoplastic resin.

[0041] <Uses of polyester resin composition> The polyester resin composition of the present embodiment can be used in various applications. For example, it can be used for injection molded articles, extrusion molded articles such as sheets, films, and pipes, bottles, foams, adhesives, adhesives, paints, and the like. More specifically, the injection molded article may be insert molded or two-color molded. The sheet may be single-layered or multi-layered, and the film may be single-layered or multi-layered, and may be unstretched, stretched in one direction or two directions, or laminated on a steel plate or the like. The film may be inflation molded. The bottle may be a direct blow bottle, an injection blow bottle, or an injection molded bottle. The foam may be a bead foam or an extrusion foam. In particular, it can be suitably used for applications requiring high heat resistance, such as products used inside automobiles, packaging materials for import and export, food packaging materials that are subjected to retort processing or microwave heating, and containers such as baby bottles and tableware that are subjected to heat sterilization. It can also be suitably used for packaging materials such as containers that require UV barrier properties. That is, the polyester-based injection molded article, polyester-based extrusion molded article, polyester-based foam, polyester-based container, polyester-based bottle, polyester-based tableware, and polyester-based baby bottle of this embodiment can each be said to contain the polyester resin composition of this embodiment. These are not particularly limited as long as they contain the polyester resin composition of this embodiment, and can be in various known forms according to their respective uses. EXAMPLES

[0042] The present embodiment will be described in more detail below with reference to examples, but the scope of the present embodiment is not limited to these examples.

[0043] [Evaluation method] The polyester resins and polyester resin compositions in the examples were evaluated as follows. (1) Ratio of diol units having a cyclic acetal skeleton and alicyclic diol units The ratio of the units derived from the diol having a cyclic acetal skeleton and the units derived from the alicyclic diol in the polyester resin is 1 Calculation was performed by H-NMR measurement. Measurement was performed using an AscendTM500 measuring device manufactured by Bruker BioSpin KK. Deuterated chloroform was used as the solvent. (2) Glass transition temperature and crystallization exothermic peak when cooling The glass transition temperature (Tgm) of polyester resin was measured by placing about 10 mg of sample in an aluminum non-sealed container and measuring at a heating rate of 20°C / min in a nitrogen gas (30mL / min) flow, and the glass transition temperature was determined as the temperature at which the temperature changed by half the difference in the baseline before and after the transition of the DSC curve. The crystallization exothermic peak during cooling was measured from the area of ​​the exothermic peak that appeared when the temperature was lowered at a rate of 10°C / min after holding at 280°C for 1 minute after measuring the above glass transition temperature. (3) Hayes The haze was measured in accordance with JIS-K-7105 and ASTM D1003. That is, a disk having a diameter of 50 mm and a thickness of 3.2 mm obtained by injection molding of a polyester resin composition was conditioned for 48 hours, and then measured in an atmosphere of 23°C and a relative humidity of 50%. The measurement device used was a haze value measuring device (model: COH-300A) manufactured by Nippon Denshoku Industries Co., Ltd. (4) Impact resistance Impact resistance was evaluated by an Izod test according to JIS K7110. That is, ten test pieces without a notch, each having a length of 63.5 mm, a width of 12.7 mm, and a thickness of 3.2 mm, obtained by injection molding of a polyester resin composition, were immersed in hot water at 50°C, 60°C, or 100°C for 24 hours, and then tested using a 4J hammer in an atmosphere at 23°C and a relative humidity of 50%, and the number of pieces broken was counted. An Izod impact tester manufactured by Ueshima Seisakusho Co., Ltd. was used as the test machine.

[0044] [Production Examples 1 to 3] [Synthesis of polyester resins (PEs-1, PEs-2 and PEs-3)] A 30L polyester production apparatus equipped with a packed column type rectification column, a partial condenser, a total condenser, a cold trap, an agitator, a heating device and a nitrogen inlet tube was charged with the raw material monomers shown in Table 1, and 0.005 mol% of tetra-n-butoxytitanium and 0.02 mol% of potassium acetate were added to the dicarboxylic acid component, and the temperature was raised to 225°C under a nitrogen atmosphere to carry out an ester exchange reaction. After the reaction conversion rate of the dicarboxylic acid component was 90% or more, 0.025 mol% of germanium dioxide and 0.05 mol% of triethyl phosphate were added to the dicarboxylic acid component, and the temperature was gradually raised and the pressure was reduced, and finally polycondensation was carried out at 280°C and 0.1 kPa or less. The reaction was terminated when the appropriate melt viscosity was reached, and polyester resins PEs-1, PEs-2 and PEs-3 were synthesized, respectively.

[0045] [Table 1]

[0046] The meanings of the abbreviations in Table 1 are as follows: DMT: Dimethyl terephthalate NDCM: 2,6-naphthalenedicarboxylate dimethyl EG: Ethylene glycol SPG: 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane CHDM: 1,4-cyclohexanedimethanol

[0047] [Polycarbodiimide] As the polycarbodiimide, Carbodilite HMV-15CA (aliphatic polycarbodiimide made of 4,4'-dicyclohexylmethane diisocyanate, polymerization degree 15) manufactured by Nisshinbo Chemical Inc. was used.

[0048] [Example 1] (Preparation of mixed pellets) Using a twin-screw kneading extruder (Toshiba Machine Co., Ltd., model: TEM26SX, screw diameter: 26 mmφ, L / D: 48), the polyester resin and polycarbodiimide synthesized in Production Example 1 were dry-blended at a ratio of 99.9 / 0.1% by mass and charged from a hopper. Strands were extruded under conditions of a cylinder temperature of 180 to 260°C, a die temperature of 260°C, a screw rotation speed of 75 rpm, and a discharge rate of 15 kg / h, and were pelletized after water cooling to obtain polyester resin / polycarbodiimide kneaded pellets.

[0049] (Injection molding of kneaded pellets) Next, the obtained kneaded pellets were injection molded. For injection molding, a Japan Steel Works, Ltd., model: J85AD injection molding machine was used, and molding was performed under the conditions of a cylinder temperature of 245 to 280°C and a mold temperature of 15 to 50°C. Using the molded test pieces, haze measurement and an Izod test after immersion in hot water at 100°C for 24 hours were performed. The results are shown in Table 2.

[0050] [Examples 2 to 10] Test pieces were produced and evaluated in the same manner as in Example 1, except that the polyester resin, the mixing ratio with polycarbodiimide, and the hot water immersion temperature were changed as shown in Table 2. The results are shown in Table 2.

[0051] [Comparative Examples 1 to 6] Test pieces were produced and evaluated in the same manner as in Example 1, except that the polyester resin, the mixing ratio with polycarbodiimide, and the hot water immersion temperature were changed as shown in Table 3. The results are shown in Table 3.

[0052] [Table 2]

[0053] [Table 3]

[0054] The polyester resin compositions of Examples 1 to 10 were significantly improved in impact resistance after immersion in hot water as compared with the polyester resin compositions of Comparative Examples 1 to 6.

[0055] This application is based on a Japanese patent application (Patent Application No. 2019-084202) filed on April 25, 2019, the contents of which are incorporated herein by reference. [Industrial Applicability]

[0056] INDUSTRIAL APPLICABILITY The polyester resin composition of the present invention is excellent in heat resistance, transparency, and impact resistance retention, and can be suitably used for products to be used inside automobiles, packaging materials for import and export, food packaging materials that undergo retort treatment or microwave heating, containers such as baby bottles and tableware that undergo heat sterilization treatment, and applications requiring high heat resistance, and the like, and therefore the present invention is of great industrial significance.

Claims

1. A polyester resin composition comprising: 97.0% by mass or more and 99.9% by mass or less of a polyester resin (A); and 0.1% by mass or more and 3.0% by mass or less of a polycarbodiimide (B), the dicarboxylic acid constituent unit in the polyester resin (A) contains a terephthalic acid unit and / or a 2,6-naphthalenedicarboxylic acid unit, the polyester resin (A) contains diol structural units that are derived from a diol having a cyclic acetal skeleton represented by the following formula (1) or (2), and the diol structural units contain diol structural units that are derived from an alicyclic diol, The polyester resin composition, wherein the polycarbodiimide (B) has two or more carbodiimide groups in the molecule. 【Chemistry 1】 (In formula (1), R 1 and R 2 each independently represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms. 【Chemistry 2】 (In formula (2), R 1 is the same as above, R 3 represents an aliphatic group having 1 to 10 carbon atoms, an alicyclic group having 3 to 10 carbon atoms, or an aromatic group having 6 to 10 carbon atoms.

2. 2. The polyester resin composition according to claim 1, wherein the diol having a cyclic acetal skeleton is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane.

3. The polyester resin composition according to claim 1, wherein the alicyclic diol is 1,4-cyclohexanedimethanol.

4. A polyester-based injection molded article comprising the polyester resin composition according to any one of claims 1 to 3.

5. A polyester extrusion molding comprising the polyester resin composition according to any one of claims 1 to 3.

6. A polyester foam comprising the polyester resin composition according to any one of claims 1 to 3.

7. A polyester-based container comprising the polyester resin composition according to any one of claims 1 to 3.

8. A polyester bottle comprising the polyester resin composition according to any one of claims 1 to 3.

9. A polyester-based tableware comprising the polyester resin composition according to any one of claims 1 to 3.

10. A polyester-based baby bottle comprising the polyester resin composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Optical fluorine-containing copolyester, optical film and production method thereof

    CN104497290A

  • Polyester block copolymer composition

    JP1995292229A

  • Polyester of 2,6-naphthalenedicarboxylic acid with improved hydrolytic stability

    JP1999506487A

  • Polyethylene naphthalate fiber

    JP2003193330A

  • Polyester resin

    JP2017105873A