Method for producing ceramic powder, method for producing ceramic powder and dense ceramic body
The method enhances ceramic particle densification by forming flaky particles through spray pyrolysis with dehydrating organic compounds and acids, addressing impurity issues and improving sinterability for dense ceramic bodies.
Patent Information
- Application Number
- JP2019050090
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-03-18
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2039-03-18
AI Technical Summary
Existing spray pyrolysis methods produce spherical ceramic particles with low densification efficiency and can introduce impurities or inhibit the function of dense ceramic bodies due to the use of sintering aids.
A method involving the use of a dehydrating organic compound with alcoholic hydroxyl groups and an acid catalyst in the spray pyrolysis process to promote the formation of flaky ceramic particles with a large specific surface area, avoiding impurities and enhancing sinterability.
The method produces high-purity, flaky ceramic particles with excellent sinterability, suitable for dense ceramic bodies, particularly in solid oxide fuel cells, without the need for additional sintering aids.
Smart Images

Figure 00000012_0000 
Figure 00000012_0001 
Figure 00000012_0002
Abstract
Description
[Technical field]
[0001] The present specification relates to a method for producing a ceramic powder, a method for producing a ceramic powder and a dense ceramic body, etc. [Background technology]
[0002] When attempting to obtain a dense ceramic body by firing, it is common to form a compact, in which ceramic powder, the raw material for the dense body, is molded into a desired three-dimensional shape, and then densify the compact through a sintering process. Since the sintering process is a thermal activation process, the higher the firing temperature and the longer the firing time, the more densified the compact will be. On the other hand, under the same firing conditions, the smaller the particle size of the ceramic particles that make up the ceramic powder, the more densified the compact will be. This is because the smaller the particle size of the ceramic particles, the larger their specific surface area.
[0003] One method for synthesizing ceramic powder is the spray pyrolysis method, which involves supplying a ceramic raw material solution or the like in the form of fine droplets to a heating furnace accompanied by a gas flow, and synthesizing ceramics from the ceramic raw material in the droplets in the heating furnace to synthesize ceramic particles (Patent Document 1, etc.).
[0004] In order to accelerate sintering, it is also effective to add a sintering aid that accelerates the diffusion of the ceramic compound to the ceramic powder. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-18466 A Summary of the Invention [Problem to be solved by the invention]
[0006] The spray pyrolysis method can synthesize ceramic particles with small particle sizes. However, the ceramic particles synthesized by the spray pyrolysis method are generally spherical with a diameter of about 1 μm. Spherical bodies have the smallest surface area relative to their particle size and volume. Therefore, when considering the particle size and volume, the spherical particles obtained by the spray pyrolysis method cannot be said to have a high efficiency in promoting densification, and the spray pyrolysis method has not necessarily been an effective method for manufacturing ceramic raw materials for dense bodies.
[0007] It is also possible to pulverize spherical or other ceramic particles using, for example, a ball mill. However, impurities may be mixed in during the pulverization process, and these impurities may cause problems in the formation of a dense ceramic body.
[0008] Furthermore, in the method using a sintering aid, the aid may remain as an impurity after sintering, impairing the function of the dense ceramic body.
[0009] The present specification provides a method for synthesizing a ceramic powder suitable for producing a dense ceramic body, a method for producing the ceramic powder and the dense ceramic body, and the like. [Means for solving the problem]
[0010] The present inventors have found that in the spray pyrolysis method, by adding a compound such as glycol to the raw material liquid containing the ceramic raw material so that a dehydration reaction occurs, the synthesis of spherical particles is hindered by the water vapor, gas, and pyrolysis of the compound after dehydration generated in the pyrolysis process, and flake-shaped particles with a large specific surface area can be synthesized. Based on this finding, the disclosure of this specification provides the following means.
[0011] [1] A method for producing a ceramic powder, comprising the steps of: a pyrolysis step of synthesizing ceramic powder by pyrolyzing a raw material liquid containing a metal atomic compound serving as a raw material for ceramic powder by a spray pyrolysis method; Equipped with The raw material liquid further contains a dehydrating organic compound having at least one alcoholic hydroxyl group and undergoing an intramolecular or intermolecular dehydration reaction in the presence of an acid, and an acid capable of catalyzing the dehydration reaction. [2] The method according to [1], further comprising a step of firing the ceramic powder after the pyrolysis step. [3] The method according to [1] or [2], wherein the dehydratable organic compound comprises one or more compounds selected from the group consisting of polyhydric aliphatic alcohols, polyalkylene glycols and hydroxy acids. [4] The method according to any one of [1] to [3], wherein the acid comprises nitric acid. [5] The method according to any one of [1] to [4], wherein the raw material liquid, the dehydratable organic compound and / or the acid are prepared so that the generated ceramic powder contains flaky ceramic particles. [6] The method according to any one of [1] to [5], wherein the ceramic powder is an ion-conductive material for a solid oxide fuel cell. [7] The method according to any one of [1] to [6], wherein the ceramic powder contains a rare earth element-added ceria-based oxide. [8] A ceramic powder produced by the method according to any one of [1] to [7]. [9] A ceramic powder obtained by spray pyrolysis, The ceramic powder has a specific surface area of 10 m as-is after spray pyrolysis and subsequent sintering. 2 A ceramic powder comprising flake particles having a particle size of 1 / g or more.
[10] A step of preparing a ceramic molded body using the ceramic powder according to [8] or [9]; sintering the ceramic molded body; A method for producing a ceramic dense body comprising:
[11] A dense ceramic body obtained by sintering the ceramic powder according to [8] or [9]. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 is a diagram showing an overview of the spray pyrolysis method. [Diagram 2] FIG. 2 is a diagram showing the results of SEM observation of gadolinium-added ceria powder (Examples and Comparative Examples) obtained by spray pyrolysis before firing. [Diagram 3] FIG. 2 is a diagram showing the results of SEM observation of gadolinium-added ceria powder (Examples and Comparative Examples) obtained by spray pyrolysis after firing. [Figure 4] FIG. 1 is a diagram showing the relative density of a dense body using the gadolinium-added ceria powder obtained by the spray pyrolysis method of the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The disclosure of this specification relates to a method for producing a ceramic powder and a ceramic powder utilizing spray pyrolysis, and a method for producing a ceramic dense body and a ceramic dense body.
[0014] According to the method for producing a ceramic powder disclosed in this specification (hereinafter also referred to as the present production method), it is possible to obtain flake-like ceramic particles, which is a form that could not be obtained by the conventional spray pyrolysis method.
[0015] According to this manufacturing method, since the ceramic powder contains ceramic particles having a flake shape even without pulverization, the specific surface area is easily increased, and the ceramic powder has excellent sinterability. Furthermore, it is possible to obtain a ceramic powder with high purity and no functional impairment without the risk of introducing impurities, even after the pyrolysis process. It is also possible to simultaneously synthesize spherical ceramic particles according to this manufacturing method. According to this manufacturing method, it is possible to obtain ceramic particles with a large surface area even without pulverization. According to this manufacturing method, it is suitable for manufacturing an ion-conductive material to be used, for example, as a solid electrolyte for a solid oxide fuel cell.
[0016] The ceramic powder disclosed in this specification (hereinafter also referred to as the present ceramic powder) can be produced, for example, by the present production method. The present ceramic powder is in an unpulverized state and can contain, for example, flake-like particles having a maximum diameter of 1 μm or less. The present ceramic powder can also contain, for example, the above-mentioned flake-like particles as a main component. Here, the flake-like particles refer to particles having the form of thin pieces or fragments. The flake-like particles do not include spherical particles.
[0017] For example, the ceramic powder may contain flake particles having a maximum diameter of 1 μm or less and flake particles having a maximum diameter of 100 nm or less. For example, the ceramic powder may contain these flake particles as the main component. The ceramic powder has a large specific surface area and is therefore excellent in sinterability, and since it is not pulverized, the inclusion of impurities from the container or balls used in the pulverization process is avoided or suppressed. For this reason, it is suitable for producing high-performance ceramic molded bodies such as ion-conductive materials and structural materials for solid oxide fuel cells.
[0018] According to the method for producing a dense ceramic body disclosed in this specification (also referred to as the present method for producing a dense ceramic body), a dense ceramic body having excellent density can be produced. For example, a dense ceramic body having excellent density can be produced without using an auxiliary agent. In addition, a dense ceramic body having excellent purity can be produced.
[0019] The ceramic dense body disclosed in this specification (hereinafter also referred to as the present ceramic dense body) has excellent density and purity, and is suitable, for example, as a solid electrolyte or structural material for solid oxide fuel cells.
[0020] The disclosure of this specification will be described in detail below with reference to the drawings as appropriate.
[0021] (Method of manufacturing ceramic powder) This manufacturing method includes a pyrolysis step in which a raw material liquid containing (a) a metal atomic compound, which serves as a raw material for the ceramic powder, is pyrolyzed by a spray pyrolysis method to synthesize ceramic powder, and the raw material liquid may further contain (b) a dehydrating organic compound having at least one alcoholic hydroxyl group and which undergoes an intramolecular or intermolecular dehydration reaction in the presence of an acid, and (c) an acid capable of catalyzing the dehydration reaction.
[0022] (pyrolysis process) In this manufacturing method, a ceramic powder is manufactured by carrying out a pyrolysis step by spray pyrolysis, which is a well-known technique in the technical field of ceramic powder synthesis, in which a solution or dispersion containing the raw materials of the powder to be obtained is made into droplets by an appropriate means, and the droplets are heated to evaporate the liquid, thereby at least partially pyrolyzing the raw materials and granulating them.
[0023] (a) Metal atom compound The raw material liquid to be subjected to the pyrolysis step contains a metal atom compound which is the raw material of the ceramic powder to be produced. The metal atom compound is a compound containing the constituent metal atoms of the ceramic of the ceramic powder, and one or more types are used as necessary. Examples of the metal atom compound include salts of metal atoms with various acids such as nitric acid and acetic acid, hydroxides of metal atoms, oxides of metal atoms, and various alkoxides of metal atoms. For example, when it is intended to obtain ceria to which a rare earth element is added, the molar ratio of Ce:rare earth element is adjusted so that the content of Ce and the rare earth element to be obtained is the content of the rare earth element to be obtained. The metal atom compound may be a hydrate or the like.
[0024] For example, rare earth element-added ceria-based oxides that serve as ion-conductive materials for solid electrolytes and air electrode materials in solid oxide fuel cells can be synthesized. Here, the rare earth elements are rare earths other than cerium (Ce), such as samarium (Sm), gadolinium (Gd), lanthanum (La), zirconia (Zr), yttrium (Y), and neodymium (Nd). In addition, ceria-based oxides that are added with Group 2 metal elements such as Ca are also useful as ion-conductive materials in solid oxide fuel cells.
[0025] (b) Dehydrating organic compounds The raw material liquid also contains a dehydrating organic compound that has at least one alcoholic hydroxyl group and undergoes an intramolecular or intermolecular dehydration reaction in the presence of an acid. It is considered that the dehydrating reaction of the dehydrating organic compound causes intramolecular and / or intermolecular dehydration condensation, which generates a condensation compound along with the generation and evaporation of water, and further, the condensation compound is thermally decomposed by heating to generate flake-shaped particles. As the raw material liquid, cerium nitrate (which may be hexahydrate), a nitric acid solution of gadolinium oxide, samarium nitrate (which may be hexahydrate), lanthanum nitrate (which may be hexahydrate), gadolinium nitrate (which may be hexahydrate), etc. can be appropriately used.
[0026] The dehydratable organic compound is not particularly limited, but examples thereof include polyhydric alcohols having two or more alcoholic hydroxyl groups, polyalkylene glycols, hydroxy acids, etc. The dehydratable organic compound may be used alone or in combination of two or more.
[0027] The polyhydric alcohol is not particularly limited, but includes polyhydric alcohols such as glycols and triols, which have a linear or branched alkyl group having 1 to 10 carbon atoms. The number of carbon atoms in the alkyl group is, for example, 2 to 6, for example, 2 to 5, for example, 2 to 4, for example, 2 to 3. The polyhydric alcohol is, for example, dihydric or trihydric. Typical examples of such polyhydric alcohols include ethylene glycol, glycerin, and the like.
[0028] The polyalkylene glycol is not particularly limited, but examples thereof include polyalkylene glycols having a repeating number of 2 to 5 and an alkylene chain length of about 2 to 4. Typical examples thereof include polyethylene glycols such as diethylene glycol and triethylene glycol.
[0029] Hydroxy acids include, but are not limited to, lactic acid, malic acid, tartaric acid, citric acid, and the like.
[0030] The content of the dehydratable organic compound in the raw material liquid is not particularly limited, but for example, the total number of moles of metal atoms intended for the ceramic powder in the raw material liquid is 1 time or more, for example, 2 times or more, for example, 3 times or more, or for example, 4 times or more. Also, it is 10 times or less, 8 times or less, 6 times or less, or 5 times or less. The range of the content of the dehydratable organic compound relative to the total number of moles of metal atoms is not particularly limited, but for example, these lower and upper limits can be appropriately combined. For example, the range is 1 time or more and 10 times or less, 2 times or more and 8 times or less, 3 times or more and 7 times or less, or 4 times or more and 6 times or less.
[0031] (c) acid The acid is not particularly limited as long as it can catalyze the dehydration reaction of the dehydratable organic compound, and examples of the acid include acid catalysts such as nitric acid, sulfuric acid, etc. The acid concentration in the raw material liquid is not particularly limited, but it is sufficient if it results in flaking of the generated ceramic particles, and can be, for example, 0.1 mass% to 10 mass%, or, for example, 0.2 mass% to 5 mass%, or, for example, 0.3 mass% to 3 mass%, etc.
[0032] The medium of the raw material liquid is not particularly limited, but may be water, an organic solvent, or a mixture thereof. From the viewpoint of purity, solubility of acid, etc., examples include water or a mixture of water, water, and an organic solvent (compatible with water). In addition, the medium of the raw material liquid is preferably composed mainly of water. That is, it is preferable that the medium contains 50% by volume or more of water, and it is preferable that the medium contains more water.
[0033] In the pyrolysis step, the raw material liquid is turned into droplets by an appropriate droplet forming means, and the droplets of the raw material liquid are heated to continuously dry and at least partially pyrolyze to synthesize ceramic particles. An example of a spray pyrolysis device used in the pyrolysis step is outlined in Figure 1.
[0034] In the thermal decomposition process, the evaporation of the medium in the raw material liquid, the thermal decomposition of the metal atom compound, the intramolecular and / or intermolecular dehydration reaction of the dehydrated organic compound, the formation of dehydrated compounds, thermal decomposition, and gas generation proceed, and the spheroidization of the particles is suppressed or the spherical particles are decomposed. As a result, flake-shaped particles are generated.
[0035] The liquid droplet generating means 2 used in the pyrolysis step is not particularly limited, and any means that is applied to a known spray pyrolysis method can be used. Therefore, there is no particular limitation, and a spray nozzle, ultrasonic atomizing means, electrostatic atomizing means, etc. can be appropriately selected and used. In FIG. 1, an ultrasonic atomizing means is provided as the liquid droplet generating means 2.
[0036] In the pyrolysis step, a heating furnace 4 utilizing various heat sources 6 can be used. The heating furnace 4 is not particularly limited, and various heating furnaces such as an infrared heating furnace, a microwave heating furnace, and a resistance heating furnace that are applied to known spray pyrolysis methods can be appropriately used. In FIG. 1, a resistance heating furnace is provided as the heating furnace 4.
[0037] The heating temperature in the pyrolysis step is not particularly limited, and may be, for example, a constant temperature, but may be gradually increased from the inlet to the outlet of the heating furnace. Typically, the temperature can be set to suit the drying and pyrolysis of the droplets. For drying the droplets, a temperature of approximately 200°C to 600°C can be set. For pyrolysis, a temperature of approximately 600°C to 1600°C can be set.
[0038] For example, it is preferable to heat the entire heating furnace at a temperature range of 200°C to 800°C, or, for example, 200°C to 1000°C, by arranging heat sources controlled to two or more, more preferably three or more, and even more preferably four or more different temperatures (for example, 200°C, 400°C, 800°C, and 1000°C) within these temperature ranges.
[0039] The gas is not particularly limited, but from the viewpoint of oxide ceramic production, for example, an oxidizing gas containing oxygen, typically air, can be used. The flow rate can be set according to the known spray pyrolysis method, for example, in the range of 1 L / min to 10 L / min, or, for example, 2 L / min to 8 L / min.
[0040] The properties of the resulting particles can be appropriately controlled by adjusting the temperature conditions and gas flow conditions in the pyrolysis step, i.e., the degree of pyrolysis of the metal atom compound in the particles, the crystallinity of the ceramics (monoclinic, tetragonal, cubic), the degree of sintering and thermal contraction of the ceramics, the degree of crystal grain growth, the degree of generation of flake-like particles, etc. can be controlled.
[0041] The particles obtained in the pyrolysis step are appropriately captured by a known capturing means 8. Capturing means generally used in spray pyrolysis methods can be appropriately adopted for such capturing means 8. In the spray pyrolysis apparatus of FIG. 1, a filter is used as the capturing means 8.
[0042] (Firing process) The method may further include a step of firing the ceramic powder produced in the pyrolysis step after the pyrolysis step. By carrying out the firing step, it is possible to adjust the crystallinity and crystal type of the ceramic, particle size (diameter and distribution), particle characteristics such as specific surface area, and even the shrinkage rate of the ceramic itself.
[0043] The firing step may be carried out, for example, as a crystallization step in which the ceramic particles obtained in the pyrolysis step are heated to promote the crystallization of the ceramic, or as a step in which the dehydratable organic compound is completely pyrolyzed or burned off and / or grain growth is caused. The firing step may also be carried out as a step in which even smaller flake-like particles are produced. According to this manufacturing method, flake-like particles can be obtained by spray pyrolysis, and when grain growth occurs within the flake-like particles in the firing step, there is a tendency for even smaller particles to be separated from the flake-like particles due to the grain growth. Furthermore, it is possible to make adjustments such as leaving a certain amount of the dehydratable organic compound or suppressing the crystallinity and sintering degree of the ceramic to ensure the shrinkage rate when the sintered body is obtained.
[0044] For example, when carrying out a crystallization step, the firing temperature can be set according to the crystal form of the ceramic to be obtained. For example, when cubic ceria with a fluorite structure is the main crystal form, the firing temperature can be set to about 400°C or more and 1000°C or less. For example, the firing temperature can be set to about 600°C or more and 1000°C or less, or for example, 700°C or more and 900°C or less. The firing time can also be set appropriately, for example, from about 1 hour to 3 or 4 hours or less, typically within 2 or 3 hours.
[0045] According to this manufacturing method, flake-shaped ceramic particles are produced in the presence of an acid through the dehydration reaction of a dehydrated organic compound, the evaporation of water, the pyrolysis of the dehydrated compound, the generation of gas, etc. That is, a ceramic powder containing flake-shaped particles with an average diameter of 2 μm or less is produced in an unpulverized state after spray pyrolysis. In addition to flake-shaped particles, conventional spherical particles may also be produced.
[0046] The thickness (average value) of the flake particles in the present ceramic powder is, for example, 10 nm to 50 nm, or, for example, 20 nm to 40 nm. The thickness can be obtained by, for example, measuring the thickness of the flake particles in the present ceramic powder at 5 to 10 points in a scanning electron microscope (SEM) observation (at a magnification of 50,000 to 100,000 times) from the portion where the thickness of the flake particles can be observed, and taking the average value of the thicknesses measured for the five flake particles as a whole.
[0047] The ceramic powder of the present invention has a large specific surface area and can exhibit excellent sinterability when sintered. In addition, since the specific surface area is large even without a pulverization step, the inclusion of impurities such as zirconia due to pulverization can be suppressed or avoided, and the total content of impurities other than the ceramic powder of the present invention, such as zirconia, or the zirconia content is, for example, 2000 ppm or less, for example, 1500 ppm or less, or for example, 1000 ppm or less, as measured by SEM / EDX.
[0048] The ceramic powder has a specific surface area of, for example, 10 m 2 / g or more, e.g., 12m 2 / g or more, e.g., 14m 2 / g or more, e.g., 15m 2 / g or more, e.g., 16m 2 / g or more, e.g., 17m 2 / g or more, e.g., 18m 2 / g or more of ceramic powder can be obtained. The ceramic powder can have such a specific surface area in an unpulverized state after pyrolysis. The specific surface area of the ceramic powder can be calculated from the BET equation by a gas adsorption method (3 points). In particular, the ceramic powder can have a specific surface area of 10 m 2 / g or more, e.g., 12m 2 / g or more, e.g., 14m 2 / g or more, e.g., 15m 2 The ceramic powder of the present invention can have such a specific surface area even without being pulverized, and is also extremely advantageous in terms of purity.
[0049] In the present production method, a particle crushing step may be carried out at any stage after the pyrolysis step to break up the aggregated state of the ceramic particles obtained. Such a crushing step may be an ultrasonic crushing step in a liquid phase in addition to a normal grinding step.
[0050] (ceramic powder) The present ceramic powder can be produced by the present manufacturing method. As described above, the present ceramic powder is characterized by its particle shape, etc. The present ceramic powder contains particles of a shape that could not be obtained by conventional spray pyrolysis methods. The present ceramic powder was obtained for the first time by the present manufacturing method, and contains a novel particle shape, making it a new ceramic powder in itself.
[0051] The ceramic powder is used, for example, as an ion-conductive material for solid oxide fuel cells. The solid electrolyte of solid oxide fuel cells requires high density, but the ceramic powder of the present invention can ensure high density by sintering, as well as high purity. When used as an ion-conductive material, the ceramic powder of the present invention is a ceria-based oxide to which rare earth elements such as gadolinium, samarium, and zirconium are added.
[0052] (Method of manufacturing dense ceramic body and said dense ceramic body) The method for producing a dense ceramic body includes the steps of preparing a ceramic molded body using the ceramic powder and firing the ceramic molded body. According to the method, a dense ceramic body having excellent density can be obtained. When the ceramic powder is used as an ion-conductive material for a solid electrolyte of a solid oxide fuel cell, the method for producing a dense ceramic body can be implemented as a method for producing a solid electrolyte of a solid oxide fuel cell, for example, or as a method for producing a solid oxide fuel cell including the method for producing a solid electrolyte of a solid oxide fuel cell as a part of the overall process.
[0053] The process for preparing a ceramic molded body using the present ceramic powder is a process for preparing a ceramic molded body for firing by a known method using only the present ceramic powder or the present ceramic powder together with other ceramic powders, and if necessary, known binders and dispersion media. For example, in the case of a ceramic molded body for a solid electrolyte of a solid oxide fuel cell, a ceramic powder that is an air electrode material can be mixed as the other ceramic powder.
[0054] In the firing process of the ceramic molded body, the ceramic molded body is fired to sinter the ceramic powder. The temperature conditions in the firing process are appropriately determined depending on the type of the ceramic powder. In the case of a rare earth element-added ceria-based acid compound, the temperature can be, for example, 1200°C to 1600°C, or, for example, 1300°C to 1500°C. In addition, the atmospheric gas can be appropriately selected depending on the type of ceramic powder, and when the ceramic powder is an oxide, it can be fired in an oxidizing atmosphere such as air.
[0055] The present ceramic dense body obtained by the present method for producing a dense ceramic body, for example, when it is a dense body containing rare earth-added ceria-based metal oxide ceramics, can obtain a high relative density at a relatively low firing temperature, such as a relative density of 75% or more when held at 1300° C. for 2 hours and fired, a relative density of 80% or more when held and fired at 1350° C. for 2 hours, a relative density of 85% or more when held and fired at 1400° C. for 2 hours, and a relative density of 90% or more when held and fired at 1500° C. for 2 hours. The relative density of the present ceramic dense body can be measured by the Archimedes method. EXAMPLES
[0056] In the following, examples are given as specific examples to more specifically explain the disclosure of the present specification. The following examples are intended to explain the disclosure of the present specification, but are not intended to limit the scope thereof. EXAMPLES
[0057] In this example, gadolinium-doped ceria ((Ce) 0.9 Gd 0.1 )O 2-x , GDC) and lanthanum doped ceria ((Ce 0.8 La 0.2 )O 2-x , LDC) was synthesized by spray pyrolysis and calcined to obtain the product.
[0058] [1] Raw material liquid for GDC Gadolinium oxide was dissolved in 50cc of nitric acid, and then cerium nitrate hexahydrate was dissolved in ion-exchanged water so that the composition ratio of Ce:Gd was 9:1, and ethylene glycol was added in an amount of N times the molar number of all cations (N=0.5, 1, 3, 5) to prepare 500mL of raw solution. The concentration of the raw solution was 0.4mol / L in terms of the molar number of all cations (Example Samples 1 to 9).
[0059] [2] Raw material liquid for LDC Cerium nitrate hexahydrate and lanthanum nitrate hexahydrate were dissolved in ion-exchanged water so that the composition ratio of Ce:La was 8:2, and ethylene glycol was added in an amount of 5 times the molar number of the total cations to prepare 500 mL of raw solution (Example samples 10 and 11, Comparative example samples 6 and 7). The concentration of the raw solution was 0.4 mol / L in terms of the molar number of the total cations. Some of the solutions (Example samples 10 and 11) contained 50 cc of nitric acid in the raw solution.
[0060] Furthermore, as the raw material solutions of the comparative examples, raw material solutions for GDC (Comparative Samples 1 and 2; containing nitric acid) having the same composition as the Examples except that they do not contain ethylene glycol, raw material solutions for LDC (Comparative Samples 4 and 5) having the same composition as the Examples except that they do not contain ethylene glycol and excess nitric acid, and raw material solutions for LDC (Comparative Samples 6 and 7; containing 5 times the molar amount of ethylene glycol) having the same composition as the Examples except that they do not contain excess nitric acid were prepared.
[0061] In addition, a commercially available GDC (by the solid phase method) was used as Comparative Example Sample 3.
[0062] [3] Spray pyrolysis conditions A spray pyrolysis device (manufactured by ON General Electric Co., Ltd.) was used for spray pyrolysis. This device is composed of a polyvinyl chloride resin atomizer, an alumina reaction tube (inner diameter 20 mmφ, outer diameter 25 mmφ, length 1500 mm), and a glass collector. The reaction tube is also equipped with four independent heating furnaces (Kanthal heaters). A membrane filter (142 mmφ, pore size: 0.45 μm, Omnipore JHWP14225) is set inside the collector to collect the synthesized particles.
[0063] The spray pyrolysis synthesis conditions were as follows: the reaction tube temperatures were 200°C, 400°C, 800°C, and 1000°C from the side closest to the atomizer, and the collector was kept at 100°C using a mantle heater to prevent condensation. The ultrasonic atomizer water bath temperature was 30°C, and the solution container temperature was 27°C. The carrier gas flow rate during synthesis was 3.0 L / min. Air was used as the carrier gas.
[0064] [4] Firing conditions The various powders obtained by spray pyrolysis were calcined at 800° C. for 2 or 4 hours (Example samples 2, 4, 6, 8, 9, 11, Comparative samples 2, 5, 7). Example samples 1, 3, 5, 7, and 10 and Comparative samples 1, 3, 4, and 6 were not calcined.
[0065] The results of measuring the specific surface area by the BET method (three points) for the example samples and the comparative sample are shown in the following table. The specific surface area was measured according to JIS R1626 "Method of measuring the specific surface area of fine ceramic powders by the gas adsorption BET method." In the table, GDC-0.5EG-N means that it contains 0.5 times the moles of ethylene glycol relative to GDC, and contains an excess of nitric acid.
[0066] [Table 1]
[0067] As shown in Table 1, from the results of Example Samples 1-9 and Comparative Samples 1-3, it was found that as the amount of ethylene glycol added increases, the specific surface area after pyrolysis and after pyrolysis and calcination increases, and the decrease in the specific surface area after calcination is suppressed, resulting in a high specific surface area even after calcination. It was also found that when the amount of ethylene glycol added is in the range of 0.5 to 5 times the number of moles of the metal elements in GDC, an excellent specific surface area is obtained both after pyrolysis and after pyrolysis and calcination. In contrast, in the case of the conventional spray pyrolysis method, although the specific surface area is higher than that of the commercially available GDC (Comparative Example 3) after pyrolysis, the non-surface area tends to decrease rapidly due to grain growth caused by calcination.
[0068] Moreover, from the results of Example Samples 10 to 11 and Comparative Examples 4 to 7, it was found that the inclusion of ethylene glycol and nitric acid is useful for ensuring an excellent specific surface area after pyrolysis and firing.
[0069] FIG. 2 shows the SEM observation results of Example Sample 7, Comparative Sample 1, and Comparative Sample 3 before firing after spray pyrolysis, and FIG. 3 shows the SEM observation results of Example Sample 9, Comparative Sample 2, and Comparative Sample 3 (commercially available GDC) after the same firing (800° C., 4 hours).
[0070] As shown in Figure 2, it was found that flake-shaped ceramic particles were generated in Example Sample 7. In contrast, in Comparative Example Sample 1, nearly spherical particles were generated, similar to the conventional spray pyrolysis method. Moreover, in the case of the commercial product GDC produced by the solid phase method, particles with a shape obtained by pulverization were observed.
[0071] In addition, as shown in Figure 3, in the example sample 9 after firing, the particles tended to become smaller than those before firing, but the flake shape was maintained. It was found that the flake particles before firing were separated into even finer flake particles as the particles grew during firing. EXAMPLES
[0072] The GDC powders of Example Sample 3 and Comparative Samples 2 and 3 obtained in Example 1 were uniaxially pressed (29.4 MPa) using a mold, and then fired at various temperatures for 2 hours and sintered at normal pressure. The relative density of the sintered bodies was measured by Archimedes' method. The results are shown in Figure 4. As shown in Figure 4, the relative density increases with increasing firing temperature, but the GDC powder synthesized by this technology exhibits a higher relative density than GDC produced by the conventional method and commercially available GDC, indicating that it is a powder with improved sinterability.
Claims
1. A method for producing a ceramic powder, comprising: a pyrolysis step of pyrolyzing a raw material liquid containing raw materials for the ceramic powder by a spray pyrolysis method to synthesize the ceramic powder containing flake-shaped ceramic particles; Equipped with the ceramic powder is gadolinium-doped ceria or lanthanum-doped ceria; The raw material liquid is As the raw material, when the ceramic powder is gadolinium-added ceria, a salt or oxide of cerium (Ce) or a hydrate thereof, and a salt or oxide of gadolinium (Gd) or a hydrate thereof, and when the ceramic powder is lanthanum-added ceria, a salt or oxide of cerium (Ce) or a hydrate thereof, and a salt or oxide of lanthanum (La) or a hydrate thereof, a dehydrating organic compound selected from polyhydric alcohols having two or more alcoholic hydroxyl groups and having a linear or branched alkyl group having 1 to 10 carbon atoms, and which undergoes an intramolecular or intermolecular dehydration reaction in the presence of an acid catalyst, an acid, which is nitric acid or sulfuric acid; The method comprising:
2. The method of claim 1 , wherein the acid is nitric acid.
3. The method according to claim 1 or 2, further comprising the step of firing the ceramic powder after the pyrolysis step.
4. The method according to any one of claims 1 to 3, wherein the ceramic powder is an ionically conductive material for a solid oxide fuel cell.
5. A ceramic powder obtained by spray pyrolysis, The ceramic powder is gadolinium-doped ceria or lanthanum-doped ceria in which gadolinium (Gd) or lanthanum (La) is added to cerium (Ce), After spray pyrolysis and subsequent calcination, the specific surface area is 10 m 2 / g or more.
6. A step of preparing a ceramic molded body using the ceramic powder according to claim 5; sintering the ceramic molded body; A method for producing a dense ceramic body comprising the steps of:
7. A dense ceramic body obtained by sintering the ceramic powder according to claim 5.
Citation Information
Patent Citations
Synthesis of starting material comprising fine oxide particle
JP1989172221A
Method of activating hydrogen storage alloy for ni / Mh secondary battery
JP2001196056A
Method for manufacturing highly-crystallized double oxide powder
JP2004043216A
Manufacturing method of complex particulate for fuel cell electrode, fuel electrode for fuel cell, and fuel cell
JP2008226531A
Reaction chamber for spray thermal decomposition apparatus, and spray thermal decomposition apparatus
JP2010018466A