Organic film forming material, substrate for manufacturing semiconductor device, organic film forming method, pattern forming method
The organic film-forming material with a specific compound and solvent combination addresses the challenges of pattern collapse and etching resistance in semiconductor manufacturing by providing high heat resistance and planarization, ensuring precise pattern transfer and improved yield in semiconductor devices.
Patent Information
- Application Number
- JP2021191479
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2041-11-25
AI Technical Summary
The challenge in semiconductor manufacturing lies in forming fine patterns with thinner photoresist films that have weak etching resistance, leading to pattern collapse and inadequate transfer of resist patterns to substrates due to insufficient dry etching selectivity, especially with the miniaturization of LSIs and the need for materials and processes that can withstand high temperatures during CVD hard mask intermediate film formation.
An organic film-forming material containing a specific organic compound represented by general formula (1A) and an organic solvent, which provides high heat resistance and advanced embedding/planarization properties, allowing for the formation of organic films that can withstand high temperatures and maintain film integrity during CVD processes, even on substrates with complex structures like wide trenches.
The organic film-forming material enables the formation of films with excellent embedding and planarization properties, ensuring precise pattern transfer and maintaining film thickness stability during high-temperature processing, thereby improving the yield and quality of semiconductor devices.
Smart Images

Figure 00000055_0000 
Figure 00000056_0000 
Figure 00000056_0001
Abstract
Description
[Technical field]
[0001] The present invention relates to an organic film-forming material used in a semiconductor device manufacturing process, a substrate for manufacturing a semiconductor device using said material, a method for forming an organic film, and a pattern formation method using a multilayer resist method. [Background technology]
[0002] As LSIs become more highly integrated and faster, pattern dimensions are becoming finer. Lithography technology has achieved the formation of finer patterns by shortening the wavelength of light sources and selecting appropriate resist compositions to match them, in line with this trend. The core of this technology is a positive photoresist composition used in a single layer. This single-layer positive photoresist composition has a skeleton in the resist resin that is resistant to dry etching using chlorine- or fluorine-based gas plasma, and also has a switching mechanism that dissolves the exposed areas, forming a pattern by dissolving the exposed areas, and then dry etching the substrate using the remaining resist pattern as an etching mask.
[0003] However, when the thickness of the photoresist film used is made finer, that is, when the pattern width is made smaller, the resolution performance of the photoresist film is reduced, and when an attempt is made to develop the photoresist film into a pattern using a developer, the so-called aspect ratio becomes too large, resulting in problems such as pattern collapse. For this reason, photoresist films have been made thinner as patterns become finer.
[0004] On the other hand, in processing a substrate to be processed, a method is usually used in which a photoresist film on which a pattern is formed is used as an etching mask to process the substrate by dry etching, but in reality, there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the substrate to be processed. Therefore, there is a problem that the photoresist film is also damaged and collapsed during processing of the substrate, and the resist pattern cannot be accurately transferred to the substrate to be processed. Therefore, with the miniaturization of patterns, higher dry etching resistance has been required for resist compositions. However, on the other hand, in order to improve resolution, resins used in photoresist compositions have been required to have low light absorption at the exposure wavelength. Therefore, as the exposure light has become shorter in wavelength from i-line to KrF and ArF, resins have also changed to novolac resins, polyhydroxystyrene, and resins with aliphatic polycyclic skeletons, but in reality, the etching speed under dry etching conditions during substrate processing has become faster, and recent photoresist compositions with high resolution tend to have weaker etching resistance.
[0005] For this reason, the substrate to be processed must be dry etched using a thinner photoresist film with a weaker etching resistance, and it is important to ensure the availability of materials and processes for this processing step.
[0006] One method for solving such problems is the multi-layer resist method, in which a resist intermediate film having a different etching selectivity from the photoresist film (i.e., resist upper film) is interposed between the resist upper film and the substrate to be processed, and after a pattern is obtained in the resist upper film, the pattern is transferred to the resist intermediate film by dry etching using the resist upper film pattern as a dry etching mask, and the pattern is further transferred to the substrate to be processed by dry etching using the resist intermediate film as a dry etching mask.
[0007] One of the multilayer resist methods is a three-layer resist method that can be performed using a general resist composition used in a single-layer resist method. In this three-layer resist method, for example, an organic film made of novolac resin or the like is formed on a substrate to be processed as a resist underlayer film, a silicon-containing resist intermediate film is formed on the organic film as a resist intermediate film, and a normal organic photoresist film is formed on the organic film as a resist upper layer film. When dry etching is performed using fluorine-based gas plasma, the organic resist upper layer film has a good etching selectivity to the silicon-containing resist intermediate film, so that the resist upper layer film pattern can be transferred to the silicon-containing resist intermediate film by dry etching using fluorine-based gas plasma. According to this method, even if a resist composition that is difficult to form a pattern with a sufficient film thickness for directly processing a substrate to be processed or a resist composition that does not have sufficient dry etching resistance for processing a substrate is used, a pattern can be transferred to the silicon-containing resist intermediate film (resist intermediate film), and then, by performing pattern transfer by dry etching using oxygen-based or hydrogen-based gas plasma, a pattern of an organic film (resist underlayer film) made of novolac resin or the like that has sufficient dry etching resistance for processing a substrate can be obtained. As the above-mentioned resist underlayer film, many films are already known, for example, the one described in Patent Document 1.
[0008] On the other hand, in recent years, the manufacturing of semiconductor devices having new structures such as a multi-gate structure has been actively studied, and in response to this, there is an increasing demand for resist underlayer films with better planarization and filling properties than before. For example, when the underlying substrate to be processed has a micropattern structure such as a hole, a trench, or a fin, the resist underlayer film needs to have the property of filling the pattern with a film without gaps (gap-filling). In addition, when the underlying substrate to be processed has a step or when a pattern-dense area and a pattern-free area exist on the same wafer, the resist underlayer film needs to planarize the film surface. By planarizing the surface of the resist underlayer film, it is possible to suppress the film thickness fluctuation of the resist intermediate film and resist top layer film formed thereon, and to suppress the focus margin of lithography and the margin reduction in the subsequent processing process of the substrate to be processed.
[0009] In addition, organic film materials with excellent filling / planarization properties are not limited to underlayer films for multilayer resists, but can also be widely used as planarization materials in semiconductor device manufacturing, for example, for substrate planarization prior to patterning by nanoimprinting. Furthermore, while the CMP process is currently commonly used for global planarization in the semiconductor device manufacturing process, CMP is a high-cost process, and these materials are expected to be used as an alternative global planarization method.
[0010] In order to form a planarizing film for planarizing uneven semiconductor substrates, an organic film material containing a compound of a specific structure containing an aromatic part having a terminal triple bond and a chain ether part has been proposed (Patent Document 2). Furthermore, organic film materials using triple bonds as intermolecular cross-linking groups of curable resins are known in Patent Documents 3 to 14. However, the planarizing performance of such materials in wide trench regions in substrates is insufficient to meet the requirements of cutting-edge devices, and there is a demand for organic film materials that are excellent in planarization on a wider range of substrate structures.
[0011] Also, a process is being considered in which an organic film is formed by spin coating, and an inorganic hard mask intermediate film is formed on the organic hard mask intermediate film as a resist intermediate film by CVD. When forming an inorganic hard mask intermediate film by CVD, it is necessary to heat the substrate to at least 300°C, usually 400°C, especially in the formation of nitride-based films. Therefore, when forming an organic film by spin coating, heat resistance to 400°C is required, but even ordinary cresol novolac, naphthol novolac, and fluorene bisphenol, which has high heat resistance, cannot withstand heating at 400°C, and a large film loss occurs after heating. Thus, there is a demand for an organic film that can withstand high temperatures when forming an inorganic hard mask intermediate film by CVD. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2004-205685 A [Patent Document 2] JP 2017-119670 A [Patent Document 3] Special Publication No. 11-512430 [Patent Document 4] JP 2005-041938 A [Patent Document 5] JP 2009-206447 A [Patent Document 6] JP 2010-181605 A [Patent Document 7] JP 2012-215842 A [Patent Document 8] International Publication No. 2014 / 208324 [Patent Document 9] JP 2016-044272 A [Patent Document 10] JP 2016-060886 A [Patent Document 11] JP 2017-014193 A [Patent Document 12] JP 2017-119671 A [Patent Document 13] JP 2018-092170 A [Patent Document 14] International Publication No. 2019 / 098109 Summary of the Invention [Problem to be solved by the invention]
[0013] The present invention has been made in consideration of the above circumstances, and aims to provide an organic film-forming material that not only enables an organic film with excellent flatness and film-forming properties to be formed even on a substrate to be processed having a portion that is particularly difficult to flatten, such as a wide trench structure, in a fine patterning process using a multilayer resist method in a semiconductor device manufacturing process, but also can withstand high-temperature heating when forming an inorganic hard mask intermediate film by a CVD method.Furthermore, the present invention also provides a substrate for manufacturing a semiconductor device, a method for forming an organic film, and a method for forming a pattern using the material. [Means for solving the problem]
[0014] In order to solve the above problems, the present invention provides an organic film-forming material, which contains (A) an organic film-forming compound represented by the following general formula (1A) and (B) an organic solvent. [ka] (In general formula (1A), Ar1 is an optionally substituted benzene ring or naphthalene ring, W1 is a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom, W2 is -O- or -NR3-, R1 is each independently a group represented by the following formula (1B), R2 is each independently a halogen atom, a cyano group, or a nitro group, R3 is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, a=2 to 4, b=1 to 4, and c=1 to 4, with the proviso that b+c≦5.) [ka] (In formula (1B), the dashed lines represent bonds.)
[0015] An organic film-forming material containing a compound having W1, a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom, as represented by the above general formula (1A), a diaryl ether structure or a diarylamine structure, and a structure in which an electron-withdrawing group is bonded to the benzene ring of a triple bond-containing terminal group, is an organic film-forming material capable of forming an organic film having high heat resistance and advanced filling / planarization properties, even on a processed substrate having a wide trench structure.
[0016] Furthermore, it is preferable that R2 in the component (A) is a fluorine atom.
[0017] By introducing a fluorine atom into R2 of the organic film-forming compound as described above, the intermolecular interactions are alleviated, thereby enabling the curing temperature to be increased, and by improving the thermal flow, it becomes possible to achieve both the conflicting properties of heat resistance and filling / planarization characteristics, even on a processed substrate having a wide trench structure.
[0018] Furthermore, it is particularly preferable that W1 of the component (A) is represented by the following formula (1C). [ka] (In formula (1C), the dashed lines represent bonds.)
[0019] By having the above-described central structure in the organic film-forming compound, it is possible to achieve both the conflicting properties of heat resistance and filling / planarization characteristics, even on a substrate to be processed that has a wide trench structure.
[0020] In addition, the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn in terms of polystyrene as determined by gel permeation chromatography of the organic film-forming compound of the component (A) is preferably 1.00≦Mw / Mn≦1.35.
[0021] By controlling the Mw / Mn of the organic film-forming compound within such a range, an organic film having excellent filling properties and flatness can be formed.
[0022] Moreover, the component (B) is preferably a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
[0023] In the case of such an organic film-forming material, the addition of a high boiling point solvent to the organic film-forming compound gives it thermal fluidity, so that the organic film-forming material has both higher levels of filling and planarizing properties.
[0024] It is also preferable that the organic film-forming material further contains one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, and (F) a plasticizer.
[0025] The organic film-forming material of the present invention may contain one or more of the above components (C) to (F) depending on the purpose.
[0026] Furthermore, the present invention provides a substrate for manufacturing a semiconductor device, which comprises a substrate on which an organic film is formed by curing the organic film-forming material described above.
[0027] The organic film-forming material of the present invention has both high filling / planarization properties, and thus an organic film is formed without microvoids due to insufficient filling or unevenness on the organic film surface due to insufficient planarization. Substrates for manufacturing semiconductor devices that are planarized with the organic film-forming material of the present invention have a wide process margin during patterning, making it possible to manufacture semiconductor devices with a high yield.
[0028] The present invention also provides a method for forming an organic film that is applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material described above onto a substrate to be processed, and heat-treating the substrate to which the organic film-forming material has been applied in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0029] The present invention also provides a method for forming an organic film applied in a manufacturing process of a semiconductor device, which comprises spin-coating the organic film-forming material described above onto a substrate to be processed, heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0030] The organic film formed by the organic film forming method of the present invention and applied in the manufacturing process of a semiconductor device has high heat resistance and advanced filling / planarization properties, and when used in the manufacturing process of a semiconductor device, the yield of the semiconductor device is improved.
[0031] In addition, it is preferable that the oxygen concentration in the inert gas atmosphere is 1% or less.
[0032] This method is useful because, even if the substrate to be processed contains a material that is unstable when heated in an oxygen atmosphere, it promotes the crosslinking reaction during the formation of the organic film without causing deterioration of the substrate to be processed, sufficiently hardens without generating sublimates, and more highly suppresses mixing with the resist overcoat film.
[0033] The present invention also provides a method for forming an organic film that is applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material described above onto a substrate to be processed, and heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0034] The organic film formed by the organic film forming method of the present invention and applied in the manufacturing process of a semiconductor device has high heat resistance and advanced filling / planarization properties, and when used in the manufacturing process of a semiconductor device, the yield of the semiconductor device is improved.
[0035] It is also preferable that the oxygen concentration in the air is 1% or more and 21% or less.
[0036] By using such a method, the crosslinking reaction during the formation of the organic film can be promoted, and mixing with the resist upper layer film can be suppressed to a greater extent. In addition, by appropriately adjusting the heat treatment temperature, time, and oxygen concentration within the above ranges, the filling / planarization characteristics and hardening characteristics of the organic film suitable for the application can be obtained.
[0037] In addition, it is preferable to use a substrate having a structure or step having a height of 30 nm or more as the substrate to be processed.
[0038] The method for forming an organic film of the present invention is particularly useful for forming a flat organic film on such a substrate.
[0039] The present invention also provides a pattern forming method for forming a pattern on a workpiece substrate, comprising the steps of forming an organic film on the workpiece substrate using the organic film-forming material described above, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece substrate by etching using the organic film to which the pattern has been transferred as a mask.
[0040] Furthermore, the present invention provides a method for forming a pattern on a substrate to be processed, comprising the steps of forming an organic film on the substrate to be processed using the organic film-forming material described above, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming an organic antireflective film on the silicon-containing resist intermediate film, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
[0041] In addition, the present invention provides a pattern forming method for forming a pattern on a substrate to be processed, comprising the steps of forming an organic film on the substrate to be processed using the organic film forming material described above, forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
[0042] The present invention also provides a pattern forming method for forming a pattern on a substrate to be processed, comprising the steps of forming an organic film on the substrate to be processed using the organic film forming material described above, forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming an organic antireflective film on the inorganic hard mask intermediate film, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
[0043] The organic film-forming material of the present invention can be suitably used in various pattern forming methods, such as a three-layer resist process using a silicon-containing resist intermediate film or an inorganic hard mask intermediate film, and a four-layer resist process using an organic anti-reflective film in addition to these. In the manufacturing process of a semiconductor device, if a circuit pattern is formed by such a pattern forming method of the present invention, the semiconductor device can be manufactured with a high yield.
[0044] The inorganic hard mask intermediate film is preferably formed by a CVD method or an ALD method.
[0045] In the pattern formation method of the present invention, for example, an inorganic hard mask intermediate film can be formed in this manner.
[0046] Furthermore, in forming the circuit pattern, it is preferable to form the circuit pattern by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.
[0047] In addition, in forming the circuit pattern, it is preferable to develop the circuit pattern using an alkali developer or an organic solvent.
[0048] In the pattern forming method of the present invention, such a circuit pattern forming means and developing means can be suitably used.
[0049] In addition, it is preferable to use, as the substrate to be processed, a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
[0050] Furthermore, it is preferable to use a metal for the substrate to be processed that contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0051] According to the pattern forming method of the present invention, a pattern can be formed by processing the above-mentioned substrate to be processed. Effect of the Invention
[0052] As described above, the organic film-forming compound contained in the organic film-forming material of the present invention is a useful compound for forming an organic film having high embedding and planarization properties, heat resistance, etching resistance, and film-forming properties even on a substrate to be processed having a part that is particularly difficult to planarize, such as a wide trench structure, in a fine patterning process by a multilayer resist method in a semiconductor device manufacturing process. In addition, the organic film-forming material of the present invention containing this compound is a material for forming an organic film having excellent embedding / planarization properties and various properties such as heat resistance, etching resistance, and film-forming properties. Therefore, it is extremely useful as an organic film material in a multilayer resist method such as a two-layer resist method, a three-layer resist method using a silicon-containing resist intermediate film, and a four-layer resist method using a silicon-containing resist intermediate film and an organic anti-reflective film, or as a planarization material for semiconductor device manufacturing. In addition, the organic film formed from the organic film-forming material of the present invention has excellent heat resistance, so that even when a CVD hard mask intermediate film is formed on the organic film, there is no film thickness fluctuation due to thermal decomposition, making it suitable for pattern formation. [Brief description of the drawings]
[0053] [Figure 1] FIG. 4 is an explanatory diagram of flattening characteristics in the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of an example of a pattern forming method using a three-layer resist method according to the present invention. [Diagram 3] FIG. 2 is an explanatory diagram of a method for evaluating embedding characteristics in an embodiment. [Figure 4] FIG. 4 is an explanatory diagram of a method for evaluating flattening characteristics in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] As described above, in a fine patterning process using a multilayer resist method in a semiconductor device manufacturing process, there has been a demand for the development of an organic film-forming material that not only has excellent filling and planarization characteristics for a pattern formed on a substrate, but also has good resistance to dry etching during substrate processing, even on a substrate to be processed that has a portion that is particularly difficult to planarize, such as a wide trench structure, and that does not cause a change in the thickness of the organic film due to thermal decomposition, even when a CVD hard mask intermediate film is formed on the organic film, and an organic film-forming compound that is useful for a pattern formation method using the material.
[0055] Usually, when forming an organic film, an organic film forming compound is dissolved in an organic solvent to form an organic film forming material, which is applied to a substrate on which the structure and wiring of a semiconductor device are formed, and baked to form an organic film. Immediately after application of the organic film forming material, a coating film is formed that conforms to the shape of the step structure on the substrate, but when the coating film is baked, most of the organic solvent evaporates before it hardens, and the organic film is formed by the organic film forming compound remaining on the substrate. The present inventors have conceived that if the organic film forming compound remaining on the substrate at this time has sufficient thermal fluidity, it is possible to flatten the step shape immediately after application by thermal fluidity and form a flat film.
[0056] As a result of further intensive research, the present inventors have found that an organic film-forming compound represented by the above general formula (1A) has thermosetting properties equivalent to conventional organic film materials not only in air but also in an inert gas atmosphere due to the action of the substituent represented by R1, and also has W1 which is a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom, a diaryl ether structure or a diarylamine structure, and a structure in which an electron-withdrawing group is bonded to the benzene ring of the triple bond-containing terminal group, thereby imparting thermal fluidity and advanced embedding / planarization properties, thereby providing an organic film-forming material having heat resistance without variation in coating film thickness due to thermal decomposition even when forming a CVD hard mask intermediate film, and have completed the present invention.
[0057] That is, the present invention is an organic film-forming material that contains (A) an organic film-forming compound represented by the following general formula (1A) and (B) an organic solvent. [ka] (In general formula (1A), Ar1 is an optionally substituted benzene ring or naphthalene ring, W1 is a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom, W2 is -O- or -NR3-, R1 is each independently a group represented by the following formula (1B), R2 is each independently a halogen atom, a cyano group, or a nitro group, R3 is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, a=2 to 4, b=1 to 4, and c=1 to 4, with the proviso that b+c≦5.) [ka] (In formula (1B), the dashed lines represent bonds.)
[0058] The present invention will be described in detail below, but the present invention is not limited thereto.
[0059] <Compounds for organic film formation> The organic film-forming compound contained in the organic film-forming material of the present invention is a compound for forming an organic film represented by the following general formula (1A). [ka] (In general formula (1A), Ar1 is an optionally substituted benzene ring or naphthalene ring, W1 is a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom, W2 is -O- or -NR3-, R1 is each independently a group represented by the following formula (1B), R2 is each independently a halogen atom, a cyano group, or a nitro group, R3 is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, a=2 to 4, b=1 to 4, and c=1 to 4, with the proviso that b+c≦5.) [ka] (In formula (1B), the dashed lines represent bonds.)
[0060] In the above general formula (1A), W1 is a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom. Ar1 is a benzene ring or a naphthalene ring which may be substituted, and W2 is -O- or -NR3-, and has a diaryl ether structure or a diarylamine structure. Each R2 is independently a halogen atom, a cyano group, or a nitro group, and has an electron-withdrawing group on the benzene ring to which the substituent represented by R1, which is a bridging group, is bonded.
[0061] Compounds having W1, a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with fluorine atoms as in the above general formula (1A), a diaryl ether structure or diarylamine structure, and a structure in which an electron-withdrawing group is bonded to the benzene ring of a triple bond-containing terminal group, are excellent in planarization characteristics and heat resistance even on a substrate to be processed having a wide trench structure, and can be hardened in air and in an inert gas atmosphere by the action of the substituent represented by R1.Therefore, the organic film formed using the organic film-forming compound contained in the organic film-forming material of the present invention can prevent film peeling caused by defects caused by insufficient heat resistance of the organic film when an inorganic hard mask intermediate film is formed on the organic film by CVD or ALD.
[0062] Examples of W1 in the above general formula (1A) include, but are not limited to, the following: Among these, those having an aromatic ring may have a substituent on the aromatic ring, and examples of the substituent include an alkyl group having 1 to 10 carbon atoms, an alkynyl group and an alkenyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a nitro group, a halogen atom, a nitrile group, an alkoxycarbonyl group having 1 to 10 carbon atoms, and an alkanoyloxy group having 1 to 10 carbon atoms.
[0063] [ka]
[0064] In the organic film forming compound contained in the organic film forming material of the present invention, the R2 in the component (A) is preferably a fluorine atom.
[0065] Since R2 of component (A) is a fluorine atom, the intermolecular interactions are alleviated, allowing the curing temperature to be increased, and thereby improving the thermal flow, making it possible to achieve both the conflicting properties of heat resistance and filling / planarization properties, even on a substrate to be processed having a wide trench structure.
[0066] In the organic film-forming compound contained in the organic film-forming material of the present invention, it is particularly preferable that W1 of the component (A) is represented by the following formula (1C). [ka]
[0067] By having the above-described central structure in the organic film-forming compound, it is possible to achieve both the conflicting properties of heat resistance and filling / planarization characteristics, even on a substrate to be processed that has a wide trench structure.
[0068] The organic film-forming compound contained in the organic film-forming material of the present invention preferably has a ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn in terms of polystyrene as measured by gel permeation chromatography of the organic film-forming compound of the component (A) of 1.00≦Mw / Mn≦1.35. By definition, if it is a monomolecular compound, Mw / Mn is 1.00, but due to the convenience of GPC separation, the measured value may exceed 1.00. In general, it is extremely difficult for a polymer having a repeating unit to approach Mw / Mn=1.00 unless a special polymerization method is used, and the Mw / Mn value exceeds 1 due to the Mw distribution. In the present invention, 1.00≦Mw / Mn≦1.35 is defined as an index indicating monomolecularity in order to distinguish between monomolecular compounds and polymers.
[0069] By controlling the Mw / Mn of the organic film-forming compound within such a range, an organic film having excellent filling properties and flatness can be formed.
[0070] If the Mw / Mn is within the above range, the thermal fluidity of the organic film-forming compound will be even better, so that when it is blended into an organic film-forming material, not only will it be possible to satisfactorily embed the microstructure formed on the substrate, but it will also be possible to form an organic film that flattens the entire substrate.
[0071] [Method of manufacturing organic film-forming compound] (1) If W2 is -O- The organic film-forming compound contained in the organic film-forming material of the present invention can be obtained by synthesis by a substitution reaction between a-valent phenols or naphthols and fluorobenzenes having substituents R1 and R2 using a base catalyst as shown below. The a-valent phenols or naphthols and fluorobenzenes having substituents R1 and R2 used in the synthesis can be used alone or in combination of two or more. These can be appropriately selected and combined depending on the required properties. In the following formula, Ar1, W1, R1, R2, a, b, and c are the same as above.
[0072] [ka]
[0073] Examples of the base catalyst used in this case include inorganic base compounds such as sodium hydrogen carbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, and potassium phosphate, and organic amine compounds such as triethylamine, pyridine, and N-methylmorpholine, which may be used alone or in combination of two or more. The amount of these catalysts used is preferably in the range of 0.1 to 20 mol, more preferably 0.2 to 10 mol, per mol of hydroxyl group of the a-valent phenols or naphthols used as the raw material.
[0074] The solvent used in this case is not particularly limited as long as it is a solvent inert to the above reaction, but for example, ether solvents such as diethyl ether, tetrahydrofuran, dioxane, etc., aromatic solvents such as benzene, toluene, xylene, etc., acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., can be used alone or in combination. These solvents can be used in the range of 0 to 2000 parts by mass per 100 parts by mass of the reaction raw materials, and the reaction temperature is preferably from -50°C to the boiling point of the solvent, more preferably from room temperature to 150°C. The reaction time is appropriately selected from 0.1 to 100 hours.
[0075] The reaction method includes a method of charging phenols or naphthols and fluorobenzenes in a solvent all at once, a method of dropping phenols or naphthols and fluorobenzenes separately or mixed and dispersed or dissolved, and a method of dispersing or dissolving either one of phenols or naphthols and fluorobenzenes in a solvent and then dropping the other one dispersed or dissolved in the solvent. When a plurality of phenols or naphthols and fluorobenzenes are charged, they may be mixed and reacted in advance, or reacted individually and sequentially. When a base catalyst is used, the method includes a method of charging phenols or naphthols and fluorobenzenes all at once, and a method of dropping the base catalyst after dispersing or dissolving it in advance.
[0076] (2) When W2 is -NR3- The organic film-forming compound contained in the organic film-forming material of the present invention can be obtained by synthesis by a substitution reaction between a-valent anilines or naphthylamines and fluorobenzenes having substituents R1 and R2 using a base catalyst as shown below. The a-valent anilines or naphthylamines and fluorobenzenes having substituents R1 and R2 used in the synthesis can be used alone or in combination of two or more. These can be appropriately selected and combined depending on the required properties. In the following formula, Ar1, W1, R1, R2, R3, a, b, and c are the same as above. [ka]
[0077] Examples of the base catalyst used in this case include inorganic base compounds such as sodium hydrogen carbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, and potassium phosphate, and organic amine compounds such as triethylamine, pyridine, and N-methylmorpholine, which may be used alone or in combination of two or more. The amount of these catalysts used is preferably in the range of 0.1 to 20 mol, more preferably 0.2 to 10 mol, per mol of amino group of the a-valent anilines or naphthylamines of the raw material.
[0078] The solvent used in this case is not particularly limited as long as it is a solvent inert to the above reaction, but for example, ether solvents such as diethyl ether, tetrahydrofuran, dioxane, etc., aromatic solvents such as benzene, toluene, xylene, etc., acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., can be used alone or in combination. These solvents can be used in the range of 0 to 2000 parts by mass per 100 parts by mass of the reaction raw materials, and the reaction temperature is preferably from -50°C to the boiling point of the solvent, more preferably from room temperature to 150°C. The reaction time is appropriately selected from 0.1 to 100 hours.
[0079] The reaction method includes a method of charging anilines or naphthylamines and fluorobenzenes in a solvent all at once, a method of dropping anilines or naphthylamines and fluorobenzenes separately or mixed and dispersed or dissolved, and a method of dispersing or dissolving either one of anilines or naphthylamines and fluorobenzenes in a solvent and then dropping the other one dispersed or dissolved in the solvent. In addition, when a plurality of anilines or naphthylamines and fluorobenzenes are charged, they may be mixed and reacted in advance, or reacted individually and sequentially. In the case of using a base catalyst, a method of charging anilines or naphthylamines and fluorobenzenes in a lump, a method of dispersing or dissolving a base catalyst in advance and then dropping it, and the like can be mentioned.
[0080] In either case where W2 is --O-- or --NR3--, the resulting reaction solution can be diluted with an organic solvent to remove unreacted raw materials, catalysts, etc. present in the system, and then recovered by separation and washing.
[0081] The organic solvent used for the separation washing is not particularly limited as long as it can dissolve the compound and separate into two layers when mixed with water, but examples thereof include hydrocarbons such as hexane, heptane, benzene, toluene, and xylene, esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate, ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone, ethers such as diethyl ether, diisopropyl ether, methyl-tert-butyl ether, and ethylcyclopentyl methyl ether, chlorine-based solvents such as methylene chloride, chloroform, dichloroethane, and trichloroethylene, and mixtures thereof. The washing water used in this case is usually what is called deionized water or ultrapure water. The number of washings may be one or more times, but since washing ten or more times does not necessarily provide the effect of washing alone, it is preferably about 1 to 5 times.
[0082] In order to remove unreacted raw materials or acidic components from the system during separation washing, washing may be performed with a basic aqueous solution. Specific examples of the base include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.
[0083] Furthermore, in order to remove unreacted raw materials, metal impurities, or basic components from the system during separation and washing, washing may be performed with an acidic aqueous solution. Specific examples of the acid include inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropolyacids, and organic acids such as oxalic acid, fumaric acid, maleic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid.
[0084] The above-mentioned separation washing with a basic aqueous solution and an acidic aqueous solution may be performed either alone or in combination. From the viewpoint of removing metal impurities, the separation washing is preferably performed in the order of a basic aqueous solution and an acidic aqueous solution.
[0085] After the above-mentioned separation washing with the basic aqueous solution or acidic aqueous solution, washing with neutral water may be performed. As the neutral water, the above-mentioned deionized water or ultrapure water may be used. The number of washings may be one or more, but if the number of washings is too few, the basic components and acidic components may not be removed. Even if washing is performed 10 or more times, the effect of washing alone may not be obtained, so the number of washings is preferably about 1 to 5 times.
[0086] Furthermore, the reaction product after the liquid separation operation can be recovered as a powder by concentrating the solvent to dryness or crystallizing it under reduced pressure or normal pressure, but it can also be left in a solution state of a moderate concentration in order to improve operability when preparing an organic film-forming material. The concentration at this time is preferably 0.1 to 50 mass%, more preferably 0.5 to 30 mass%. If the concentration is such, the viscosity is unlikely to increase, so that the operability is prevented from being impaired, and the amount of the solvent is not excessive, so that it is economical.
[0087] The solvent used in this case is not particularly limited as long as it can dissolve the compound, and specific examples include ketones such as cyclohexanone and methyl-2-amyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono tert-butyl ether acetate. These can be used alone or in combination of two or more.
[0088] In the above reaction, it is possible to combine phenols, naphthols, anilines or naphthylamines with fluorobenzenes according to the required performance. Specifically, it is possible to use those that are introduced according to the desired required performance, such as solvent solubility, adhesion, curability, filling / planarization characteristics, etching resistance, and substituents that contribute to film formation. Organic film forming materials using these compounds can achieve both filling / planarization characteristics and heat resistance at a high level.
[0089] As described above, the organic film-forming compound contained in the organic film-forming material of the present invention provides an organic film-forming material that has heat resistance of 400°C or more and high-level filling / planarization properties, even on a substrate to be processed that has a wide trench structure.
[0090] In the present invention, the planarization property refers to the ability to planarize the surface of a substrate. For example, as shown in FIG. 1, the organic film-forming material of the present invention containing an organic film-forming compound can reduce a 100 nm step in the substrate 1 to 30 nm or less by applying an organic film-forming material 3' onto the substrate 1 and heating it to form an organic film 3. The step shape shown in FIG. 1 shows a typical example of the step shape in a substrate for manufacturing a semiconductor device, and the step shape of the substrate that can be planarized by the organic film-forming material of the present invention containing an organic film-forming compound is not limited to this.
[0091] <Organic film forming material> The present invention also provides an organic film-forming material (organic film-forming composition) that contains (A) an organic film-forming compound represented by the above general formula (1A) and (B) an organic solvent. In the organic film-forming material of the present invention, the above-mentioned organic film-forming compounds can be used alone or in combination of two or more.
[0092] [(B) Organic solvent] The organic solvent usable in the organic film-forming material of the present invention is not particularly limited as long as it dissolves the above-mentioned compounds and the components contained in the materials such as other additives. Specifically, solvents having a boiling point of less than 180°C, such as those described in paragraphs
[0091] to
[0092] of JP-A-2007-199653, can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and mixtures of two or more of these are preferably used. The amount of the organic solvent is preferably 200 to 10,000 parts, more preferably 300 to 5,000 parts, based on 100 parts of the above-mentioned compound (A).
[0093] Such an organic film-forming material can be applied by spin coating, and since it contains the organic film-forming compound described above, it is an organic film-forming material that has heat resistance of 400°C or more and high-level filling / planarization properties, even on a substrate to be processed that has a wide trench structure.
[0094] Furthermore, in the organic film-forming material of the present invention, it is also possible to add a high-boiling point solvent having a boiling point of 180°C or more to the above-mentioned solvent having a boiling point of less than 180°C as the organic solvent. That is, the component (B) can be a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or more. The high-boiling point solvent is not particularly limited as long as it can dissolve the organic film-forming compound, and may be any of hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc., but specific examples include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butylene glycol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, 2-ethyl-1,3-Hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerin, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol monomethyl ether, triethylene glycol-n-butyl ether, triethylene glycol butyl methyl ether, triethylene Glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, 1,Examples of the monomer include 6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, and dibutyl adipate, and these may be used alone or in combination.
[0095] The boiling point of the high-boiling solvent may be appropriately selected according to the temperature at which the organic film-forming material is heat-treated, and the boiling point of the high-boiling solvent to be added is preferably 180°C to 300°C, and more preferably 200°C to 300°C. If the boiling point is in this range, there is no risk of the solvent volatilizing too quickly during baking (heat treatment), and sufficient thermal fluidity can be obtained. In addition, if the boiling point is in this range, the solvent will not remain in the film after baking without volatilizing, and there is no risk of adversely affecting the film properties such as etching resistance.
[0096] Furthermore, when the high boiling point solvent is used, the blending amount of the high boiling point solvent is preferably 1 to 30 parts by mass per 100 parts by mass of the solvent having a boiling point of less than 180° C. Such a blending amount can impart sufficient thermal fluidity during baking, and does not remain in the film, which may lead to deterioration of the film properties such as etching resistance.
[0097] In the case of such an organic film-forming material, by imparting thermal fluidity to the above-mentioned organic film-forming compound by adding a high-boiling point solvent, the organic film-forming material becomes one having both high-level filling and planarizing properties.
[0098] [(C) Acid generator] The organic film-forming material of the present invention may contain an acid generator (C) in order to further accelerate the curing reaction. The acid generator may be one that generates an acid by thermal decomposition or one that generates an acid by light irradiation, and either one may be contained. Specifically, the organic film-forming material may contain an acid generator described in paragraphs
[0061] to
[0085] of JP-A-2007-199653, but is not limited thereto.
[0099] The acid generators can be used alone or in combination of two or more. When an acid generator is added, the amount of the acid generator added is preferably 0.05 to 50 parts, more preferably 0.1 to 10 parts, based on 100 parts of the compound.
[0100] [(D) Surfactant] The organic film-forming material of the present invention may contain a surfactant (D) in order to improve the coating property in spin coating. For example, the surfactants described in paragraphs
[0142] to
[0147] of JP-A-2009-269953 can be used. When the surfactant is contained, the content is preferably 0.01 to 10 parts, more preferably 0.05 to 5 parts, based on 100 parts of the compound.
[0101] [(E) Crosslinking agent] In addition, the organic film-forming material of the present invention may contain a crosslinking agent (E) in order to enhance the curability and further suppress intermixing with the resist upper layer film. The crosslinking agent is not particularly limited, and various known crosslinking agents can be widely used. Examples include melamine-based crosslinking agents, glycoluril-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, and epoxy-based crosslinking agents.
[0102] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy- and / or hydroxy-substituted products thereof, and partial self-condensates thereof. Specific examples of glycoluril crosslinking agents include tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, alkoxy and / or hydroxy substituted products thereof, and partial self-condensates thereof. Specific examples of benzoguanamine-based crosslinking agents include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, alkoxy- and / or hydroxy-substituted products thereof, and partial self-condensates thereof. Specific examples of the urea-based crosslinking agent include dimethoxymethylated dimethoxyethyleneurea, its alkoxy and / or hydroxyl substituted derivatives, and partial self-condensates thereof. A specific example of the β-hydroxyalkylamide crosslinking agent is N,N,N',N'-tetra(2-hydroxyethyl)adipamide. Specific examples of the isocyanurate crosslinking agent include triglycidyl isocyanurate and triallyl isocyanurate. Specific examples of the aziridine crosslinking agent include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of the oxazoline-based crosslinking agent include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tertbutyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymer. Specific examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether. When a crosslinking agent is contained, the content is preferably 1 to 100 parts, more preferably 5 to 50 parts, based on 100 parts of the above compound.
[0103] [(F) Plasticizer] In addition, the organic film-forming material of the present invention may contain a plasticizer (F) in order to further improve the flattening / filling properties. The plasticizer is not particularly limited, and various known plasticizers can be widely used. Examples include low molecular weight compounds such as phthalates, adipic esters, phosphates, trimellitates, and citrates, polyethers, polyesters, and polymers such as the polyacetal polymers described in JP-A-2013-253227. When a plasticizer is contained, the content is preferably 1 to 100 parts, more preferably 5 to 30 parts, based on 100 parts of the above compound.
[0104] [Additives] In addition, in the organic film-forming material of the present invention, as an additive for imparting filling / flattening properties in the same manner as a plasticizer, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a thermally decomposable polymer having a weight loss rate of 40% by mass or more between 30°C and 250°C and a weight average molecular weight of 300 to 200,000 is preferably used. This thermally decomposable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a). When these additives are contained, the content is preferably 1 to 100 parts, more preferably 5 to 50 parts, based on 100 parts of the above compound.
[0105] [ka] (In general formula (DP1), X1 is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. Y1 is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.)
[0106] [ka] (In general formula (DP1a), X a is an alkyl group having 1 to 4 carbon atoms. a is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, which may have an ether bond; l represents the average number of repeating units and is an integer of 3 to 500.
[0107] As described above, the organic film-forming material of the present invention is an organic film-forming material that has heat resistance of 400°C or more and high embedding / flattening properties even on a substrate to be processed having a wide trench structure.Therefore, the organic film-forming material of the present invention is extremely useful as an organic film-forming material for multi-layer resist methods such as a two-layer resist method, a three-layer resist method using a silicon-containing resist intermediate film or an inorganic hard mask intermediate film, and a four-layer resist method using a silicon-containing resist intermediate film or an inorganic hard mask intermediate film and an organic anti-reflective film.In addition, the organic film-forming material of the present invention does not generate by-products even when formed in an inert gas atmosphere, and has excellent embedding / flattening properties, so it can be suitably used as a flattening material in semiconductor device manufacturing processes other than the multi-layer resist method.
[0108] <Substrates for manufacturing semiconductor devices> The present invention also provides a substrate for manufacturing a semiconductor device, which comprises a substrate on which an organic film is formed by curing the organic film-forming material described above.
[0109] An organic film formed from the organic film-forming material of the present invention has both high filling / planarization properties, and is therefore an organic film that is free of microvoids due to insufficient filling or unevenness on the organic film surface due to insufficient planarization. A substrate for manufacturing semiconductor device that is planarized with such an organic film has a wide process tolerance during patterning, making it possible to manufacture semiconductor devices with a high yield.
[0110] <Method of forming organic film> The present invention provides a method for forming an organic film that is applied in the manufacturing process of a semiconductor device, which comprises spin-coating the organic film-forming material described above onto a substrate to be processed, and heat-treating the substrate to which the organic film-forming material has been applied in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a hardened film (one-stage bake).
[0111] The present invention also provides a method for forming an organic film applied in a manufacturing process of a semiconductor device, which comprises spin-coating the organic film-forming material described above onto a substrate to be processed, heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower, preferably at a temperature of 250°C or higher, for a period of 10 to 7200 seconds to obtain a cured film (two-stage bake).
[0112] In this method for forming an organic film, first, the organic film forming material of the present invention described above is spin-coated (spin-coated) onto a substrate to be processed. By using the spin-coating method, good embedding properties can be obtained. After spin-coating, baking (heat treatment) is performed to promote flattening by thermal flow and cross-linking reaction. This baking can evaporate the organic solvent in the organic film forming material, so that mixing can be prevented even when a resist top layer film or a silicon-containing resist intermediate film is formed on the organic film.
[0113] The heating film-forming step for forming an organic film (organic underlayer film) can employ one-stage baking, two-stage baking, or three or more stage baking, but one-stage baking or two-stage baking is economically preferred.
[0114] The film formation by one-stage baking is preferably carried out in an inert gas atmosphere at a temperature of 50° C. to 600° C. for 10 to 7200 seconds, preferably at a temperature of 150° C. to 500° C. for 10 to 3600 seconds. By carrying out the heat treatment under such conditions, flattening due to thermal flow and crosslinking reaction can be promoted.
[0115] In the multi-layer resist method, a coating type silicon-containing resist intermediate film or a CVD hard mask intermediate film may be formed on the obtained film. When a coating type silicon-containing resist intermediate film is applied, it is preferable to form the film at a temperature higher than the temperature at which the silicon-containing resist intermediate film is formed. Usually, the silicon-containing resist intermediate film is formed at 100°C or more and 400°C or less, preferably 150°C or more and 350°C or less. When the organic film is formed at a temperature higher than this temperature, it is possible to prevent the organic film from being dissolved by the composition for forming the silicon-containing resist intermediate film, and to form an organic film that does not mix with the composition. When the CVD hard mask intermediate film is applied in a single-stage bake, it is preferable to form the organic film at a temperature higher than the temperature at which the CVD hard mask intermediate film is formed. The temperature at which the CVD hard mask intermediate film is formed can be exemplified by a temperature of 150°C or more and 500°C or less.
[0116] On the other hand, in the case of film formation by two-stage baking, the first stage of baking is performed in air at a temperature of 50° C. to 300° C., preferably 250° C. or less, for 5 to 600 seconds, taking into consideration the influence of corrosion of the substrate caused by oxygen in the air. The second stage of baking is performed in an inert gas atmosphere, and the baking temperature is higher than the first stage baking temperature, 200° C. to 600° C., preferably 250° C. to 500° C., for 10 to 7200 seconds.
[0117] In the multilayer resist method, a coating type silicon-containing resist intermediate film or a CVD hard mask intermediate film may be formed on the obtained film. When a coating type silicon-containing resist intermediate film is applied, it is preferable to form the film at a temperature higher than the temperature at which the silicon-containing resist intermediate film is formed. Usually, the silicon-containing resist intermediate film is formed at 100°C or more and 400°C or less, preferably 150°C or more and 350°C or less. When the organic film is formed at a temperature higher than this temperature, it is possible to prevent the organic film from being dissolved by the composition for forming the silicon-containing resist intermediate film, and to form an organic film that does not mix with the composition. When the CVD hard mask intermediate film is applied by two-stage baking, it is preferable to form the organic film at a temperature higher than the temperature at which the CVD hard mask intermediate film is formed. The temperature at which the CVD hard mask intermediate film is formed can be exemplified by a temperature of 150°C or more and 500°C or less.
[0118] The present invention also provides a method for forming an organic film that functions as an organic underlayer film used in the manufacturing process of a semiconductor device, in which a hardened film is formed by heat-treating a substrate to be processed in an atmosphere with an oxygen concentration of 1% or less in order to prevent corrosion of the substrate to be processed, that is, the method for forming an organic film in which the oxygen concentration in the inert gas atmosphere is 1% or less is provided.
[0119] In this method for forming an organic film, first, the organic film forming material of the present invention is spin-coated on a substrate to be processed. After spin-coating, in a two-stage bake, the first stage is baked in air at 300° C. or less, and then the second stage is baked in an atmosphere with an oxygen concentration of 1% or less. In the case of a one-stage bake, the first stage bake in air may be skipped. In addition, examples of the atmosphere during baking include inert gases such as nitrogen, argon, and helium. With the organic film forming material of the present invention, even if it is baked in such an inert gas atmosphere, it is possible to form a sufficiently hardened organic film without generating sublimates.
[0120] The present invention also provides a method for forming an organic film that is applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material described above onto a substrate to be processed, and heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0121] At this time, it is preferable that the oxygen concentration in the air is 1% or more and 21% or less.
[0122] In this method for forming an organic film, first, the organic film forming material of the present invention is spin-coated onto a substrate to be processed. After spin-coating, in a two-stage bake, the first stage is baked in air at 300° C. or less, and then the second stage is baked in air with an oxygen concentration of 1% to 21%. In the case of a one-stage bake, the first stage bake in air may be skipped. With the organic film forming material of the present invention, even if it is baked in air with an oxygen concentration of 1% to 21%, a sufficiently cured organic film can be formed without generating sublimates.
[0123] In addition, the organic film forming method of the present invention can use a substrate to be processed having a structure or step having a height of 30 nm or more. As described above, the organic film forming material of the present invention has excellent embedding / flattening properties, so that even if the substrate to be processed has a structure or step (unevenness) having a height of 30 nm or more, a flat cured film can be formed. In other words, the organic film forming method of the present invention is particularly useful when forming a flat organic film on such a substrate to be processed.
[0124] The thickness of the organic film to be formed may be appropriately selected, but is preferably 30 to 20,000 nm, and more preferably 50 to 15,000 nm.
[0125] The above-mentioned method for forming an organic film can be applied to both the case of forming an organic film for an organic underlayer film using the organic film-forming material of the present invention and the case of forming an organic film for a planarizing film.
[0126] <Pattern formation method> [Three-layer resist method using silicon-containing resist intermediate film] The present invention provides a pattern forming method for forming a pattern on a workpiece substrate, comprising the steps of forming an organic film on the workpiece substrate using the organic film forming material described above, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece substrate by etching using the organic film to which the pattern has been transferred as a mask.
[0127] As the substrate to be processed, it is preferable to use a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon. More specifically, although not limited to, a substrate such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, or the like, or a substrate having the above-mentioned metal film formed thereon as a layer to be processed, etc., may be used.
[0128] As the processed layer, various low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, and their stopper films are used, and can be formed to a thickness of usually 50 to 10,000 nm, particularly 100 to 5,000 nm. When forming the processed layer, the substrate and the processed layer are made of different materials.
[0129] It is preferable to use a metal for the substrate to be processed that contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0130] In addition, it is preferable to use a substrate to be processed that has a structure or step having a height of 30 nm or more.
[0131] When forming an organic film on a substrate to be processed using the organic film forming material of the present invention, the above-mentioned organic film forming method of the present invention may be applied.
[0132] Next, a resist intermediate film (silicon-containing resist intermediate film) is formed on the organic film using a silicon atom-containing resist intermediate film material. As the silicon-containing resist intermediate film material, a polysiloxane-based resist intermediate film material is preferable. By imparting an anti-reflection effect to the silicon-containing resist intermediate film, reflection can be suppressed. In particular, for 193 nm exposure, if a material containing many aromatic groups and having high etching selectivity with the substrate is used as the organic film forming material, the k value becomes high and the substrate reflection becomes high, but by imparting absorption to the silicon-containing resist intermediate film so that the k value becomes appropriate, it becomes possible to suppress reflection, and the substrate reflection can be reduced to 0.5% or less. As a silicon-containing resist intermediate film having an anti-reflection effect, anthracene is preferably used for 248 nm and 157 nm exposure, and polysiloxane having a phenyl group or a light-absorbing group having a silicon-silicon bond in a pendant structure or polysiloxane structure for 193 nm exposure, and crosslinking with acid or heat is preferably used.
[0133] Next, a resist upper layer film is formed on the silicon-containing resist intermediate film using a resist upper layer film material consisting of a photoresist composition. The resist upper layer film material may be either positive or negative, and the same as a commonly used photoresist composition can be used. After spin-coating the resist upper layer film material, it is preferable to perform pre-baking at 60 to 180°C for 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, and further post-exposure baking (PEB) and development are performed to obtain a resist upper layer film pattern. The thickness of the resist upper layer film is not particularly limited, but is preferably 30 to 500 nm, and particularly preferably 50 to 400 nm.
[0134] Next, a circuit pattern (resist upper layer film pattern) is formed on the resist upper layer film. In forming the circuit pattern, it is preferable to form the circuit pattern by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination thereof.
[0135] Examples of the exposure light include high-energy rays with a wavelength of 300 nm or less, specifically far ultraviolet rays, KrF excimer laser light (248 nm), ArF excimer laser light (193 nm), F2 laser light (157 nm), Kr2 laser light (146 nm), Ar2 laser light (126 nm), soft X-rays (EUV) of 3 to 20 nm, electron beams (EB), ion beams, X-rays, and the like.
[0136] In forming the circuit pattern, it is preferable to develop the circuit pattern using an alkali developer or an organic solvent.
[0137] Next, the circuit pattern is formed on the resist upper layer film as a mask, and the pattern is transferred to the silicon-containing resist intermediate film by etching. The etching of the silicon-containing resist intermediate film using the resist upper layer film pattern as a mask is preferably performed using a fluorocarbon gas. Thus, a silicon-containing resist intermediate film pattern is formed.
[0138] Next, the pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask. The silicon-containing resist intermediate film exhibits higher etching resistance to oxygen gas or hydrogen gas than organic matter, so the etching of the organic film using the silicon-containing resist intermediate film pattern as a mask is preferably performed using an etching gas mainly composed of oxygen gas or hydrogen gas. This allows the organic film pattern to be formed.
[0139] Next, the pattern is transferred to the substrate by etching using the organic film with the transferred pattern as a mask. The substrate (layer) to be processed can be etched by a conventional method. For example, if the substrate is made of SiO2, SiN, or a silica-based low dielectric constant insulating film, etching is performed mainly with fluorocarbon gas, and if it is made of p-Si, Al, or W, etching is performed mainly with chlorine or bromine gas. When the substrate is processed by etching with fluorocarbon gas, the silicon-containing resist intermediate film pattern is peeled off at the same time as the substrate is processed. On the other hand, when the substrate is processed by etching with chlorine or bromine gas, it is necessary to separately perform dry etching stripping with fluorocarbon gas after the substrate is processed in order to strip the silicon-containing resist intermediate film pattern.
[0140] An organic film obtained by using the organic film-forming material of the present invention can have excellent etching resistance when etching the substrate to be processed as described above.
[0141] [Four-layer resist method using silicon-containing resist intermediate film and organic anti-reflective film] The present invention also provides a pattern forming method for forming a pattern on a workpiece substrate, comprising the steps of forming an organic film on the workpiece substrate using the organic film-forming material described above, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming an organic antireflective film on the silicon-containing resist intermediate film, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece substrate by etching using the organic film to which the pattern has been transferred as a mask.
[0142] This method can be carried out in the same manner as the three-layer resist method using the silicon-containing resist intermediate film described above, except that an organic antireflective coating (BARC) is formed between the silicon-containing resist intermediate film and the resist top layer film.
[0143] The organic anti-reflection film can be formed by spin coating using a known organic anti-reflection film material.
[0144] [Three-layer resist method using inorganic hard mask intermediate film] The present invention also provides a pattern forming method for forming a pattern on a substrate to be processed, comprising the steps of forming an organic film on the substrate to be processed using the organic film forming material described above, forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
[0145] This method can be carried out in the same manner as the three-layer resist method using the silicon-containing resist intermediate film described above, except that an inorganic hard mask intermediate film is formed on the organic film instead of the silicon-containing resist intermediate film.
[0146] The inorganic hard mask intermediate film selected from silicon oxide film, silicon nitride film, silicon oxide nitride film (SiON film), titanium oxide film and titanium nitride film can be formed by CVD method, ALD method, etc. In particular, it is preferable to form the inorganic hard mask intermediate film by CVD method or ALD method. Methods for forming silicon nitride film are described in, for example, JP-A-2002-334869 and WO-A-2004 / 066377. The thickness of the inorganic hard mask intermediate film is preferably 5 to 200 nm, more preferably 10 to 100 nm. As the inorganic hard mask intermediate film, a SiON film, which has a high effect as an anti-reflection film, is most preferably used. Since the substrate temperature when forming the SiON film is 300 to 500°C, the organic film needs to withstand temperatures of 300 to 500°C. The organic film formed using the organic film-forming material of the present invention has high heat resistance and can withstand high temperatures of 300°C to 500°C, so it is possible to combine an inorganic hard mask intermediate film formed by a CVD method or an ALD method with an organic film formed by a spin coating method.
[0147] [Four-layer resist method using inorganic hard mask intermediate film and organic anti-reflective film] The present invention also provides a pattern forming method for forming a pattern on a substrate to be processed, comprising the steps of forming an organic film on the substrate to be processed using the organic film forming material described above, forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming an organic antireflective film on the inorganic hard mask intermediate film, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
[0148] This method can be performed in the same manner as the three-layer resist method using the inorganic hard mask intermediate film described above, except that an organic antireflective coating (BARC) is formed between the inorganic hard mask intermediate film and the resist top layer film.
[0149] In particular, when a SiON film is used as the inorganic hard mask intermediate film, the two-layer anti-reflection film of the SiON film and the BARC makes it possible to suppress reflections even in immersion lithography with a high NA exceeding 1.0. Another advantage of forming the BARC is that it has the effect of reducing the tailing of the resist top layer film pattern directly above the SiON film.
[0150] Here, an example of a pattern forming method by the three-layer resist method of the present invention is shown in Figures 2(A) to (F). In the case of the three-layer resist method, as shown in Figure 2(A), an organic film 3 is formed on a workpiece layer 2 formed on a substrate 1 using the organic film forming material of the present invention, and then a silicon-containing resist intermediate film 4 is formed thereon, and a resist upper layer film 5 is formed thereon. Then, as shown in Figure 2(B), an exposed portion 6 of the resist upper layer film 5 is exposed to light, and PEB (post exposure bake) is performed. Then, as shown in Figure 2(C), development is performed to form a resist upper layer film pattern 5a. Then, as shown in Figure 2(D), the silicon-containing resist intermediate film 4 is dry-etched using a fluorocarbon gas with the resist upper layer film pattern 5a as a mask, to form a silicon-containing resist intermediate film pattern 4a. Then, as shown in Figure 2(E), after removing the resist upper layer film pattern 5a, the organic film 3 is oxygen plasma etched with the silicon-containing resist intermediate film pattern 4a as a mask, to form an organic film pattern 3a. Furthermore, as shown in FIG. 2(F), after removing the silicon-containing resist intermediate film pattern 4a, the process layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a.
[0151] When forming an inorganic hard mask intermediate film, the silicon-containing resist intermediate film 4 may be changed to an inorganic hard mask intermediate film, and when forming a BARC, the BARC may be formed between the silicon-containing resist intermediate film 4 and the resist upper layer film 5. Etching of the BARC may be performed consecutively prior to etching of the silicon-containing resist intermediate film 4, or etching of only the BARC may be performed, and then etching of the silicon-containing resist intermediate film 4 may be performed by changing the etching device, for example.
[0152] As described above, the pattern forming method of the present invention makes it possible to form a fine pattern on a substrate to be processed with high precision by a multi-layer resist method. EXAMPLES
[0153] The present invention will be described in more detail below with reference to Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited thereto. Note that, as for the molecular weight and dispersity, the weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene were determined by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent, and the dispersity (Mw / Mn) was determined.
[0154] Synthesis example: Synthesis of compounds for forming organic films The following phenols or anilines (B1) to (B9) and fluorobenzenes (C1) to (C7) were used to synthesize the organic film-forming compounds (A1) to (A21). Comparative compounds (R1) to (R5) were synthesized using comparative synthesis raw materials (D1) to (D8).
[0155] Phenols or anilines: [ka]
[0156] Fluorobenzene: [ka]
[0157] Synthetic raw materials for comparative examples: [ka]
[0158] [Synthesis Example 1] Synthesis of organic film-forming compound (A1) 40 g of N-methylpyrrolidone was added to 3.4 g of phenols (B1), 4.1 g of fluorobenzene (C1), and 4.1 g of potassium carbonate, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100 ml of methyl isobutyl ketone and 100 ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 10 g of THF was added to the residue to make a homogenous solution, and then crystallized with 50 g of methanol. The precipitated crystals were separated by filtration, washed twice with 20 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A1). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A1): Mw = 680, Mw / Mn = 1.30 [ka]
[0159] [Synthesis Example 2] Synthesis of organic film-forming compound (A2) 5.0 g of phenols (B2), 4.1 g of fluorobenzene (C1), and 4.1 g of potassium carbonate were added to 40 g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100 ml of methyl isobutyl ketone and 100 ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 10 g of THF was added to the residue to make a homogenous solution, and then crystallized with 50 g of methanol. The precipitated crystals were separated by filtration, washed twice with 20 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A2). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A2): Mw = 690, Mw / Mn = 1.30 [ka]
[0160] [Synthesis Example 3] Synthesis of organic film-forming compound (A3) 5.0 g of aniline (B3), 4.1 g of fluorobenzene (C1), and 4.1 g of potassium carbonate were added with 40 g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100 ml of methyl isobutyl ketone and 100 ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 10 g of THF was added to the residue to make a homogenous solution, and then crystallized with 50 g of methanol. The precipitated crystals were separated by filtration, washed twice with 20 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A3). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A3): Mw=680, Mw / Mn=1.28 [ka]
[0161] [Synthesis Example 4] Synthesis of organic film-forming compound (A4) 5.2g of phenols (B4), 4.1g of fluorobenzene (C1), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A4). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A4): Mw=780, Mw / Mn=1.32 [ka]
[0162] [Synthesis Example 5] Synthesis of organic film-forming compound (A5) 6.8g of phenols (B5), 4.1g of fluorobenzene (C1), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A5). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A5): Mw=910, Mw / Mn=1.33 [ka]
[0163] [Synthesis Example 6] Synthesis of organic film-forming compound (A6) 2.9g of phenols (B6), 4.1g of fluorobenzene (C1), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A6). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A6): Mw=1420, Mw / Mn=1.35 [ka]
[0164] [Synthesis Example 7] Synthesis of organic film-forming compound (A7) 3.1g of phenols (B7), 4.1g of fluorobenzene (C1), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A7). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A7): Mw=1260, Mw / Mn=1.34 [ka]
[0165] [Synthesis Example 8] Synthesis of organic film-forming compound (A8) 3.1g of phenols (B7), 4.6g of fluorobenzene (C2), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A8). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A8): Mw=1310, Mw / Mn=1.35 [ka]
[0166] [Synthesis Example 9] Synthesis of organic film-forming compound (A9) 3.1g of phenols (B7), 4.7g of fluorobenzene (C3), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A9). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A9): Mw=1370, Mw / Mn=1.35 [ka]
[0167] [Synthesis Example 10] Synthesis of organic film-forming compound (A10) 40 g of N-methylpyrrolidone was added to 4.2 g of phenols (B8), 4.1 g of fluorobenzene (C1), and 4.1 g of potassium carbonate, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100 ml of methyl isobutyl ketone and 100 ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 10 g of THF was added to the residue to make a homogenous solution, and then crystallized with 50 g of methanol. The precipitated crystals were separated by filtration, washed twice with 20 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A10). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A10): Mw = 1350, Mw / Mn = 1.27 [ka]
[0168] [Synthesis Example 11] Synthesis of organic film-forming compound (A11) 3.8g of phenols (B9), 5.5g of fluorobenzene (C1), and 5.5g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A11). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A11): Mw = 1550, Mw / Mn = 1.30 [ka]
[0169] [Synthesis Example 12] Synthesis of organic film-forming compound (A12) 3.4g of phenols (B1), 5.2g of fluorobenzene (C4), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A12). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A12): Mw = 1100, Mw / Mn = 1.35 [ka]
[0170] [Synthesis Example 13] Synthesis of organic film-forming compound (A13) 5.2g of phenols (B4), 5.2g of fluorobenzene (C4), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A13). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A13): Mw = 840, Mw / Mn = 1.11 [ka]
[0171] [Synthesis Example 14] Synthesis of organic film-forming compound (A14) 6.8g of phenols (B5), 5.2g of fluorobenzene (C4), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A14). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A14): Mw = 940, Mw / Mn = 1.13 [ka]
[0172] [Synthesis Example 15] Synthesis of organic film-forming compound (A15) 3.1g of phenols (B7), 5.2g of fluorobenzene (C4), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A15). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A15): Mw = 1040, Mw / Mn = 1.03 [ka]
[0173] [Synthesis Example 16] Synthesis of organic film-forming compound (A16) 3.1g of phenols (B7), 5.8g of fluorobenzene (C5), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A16). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A16): Mw = 870, Mw / Mn = 1.00 [ka]
[0174] [Synthesis Example 17] Synthesis of organic film-forming compound (A17) 3.1g of phenols (B7), 5.0g of fluorobenzene (C6), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A17). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A17): Mw=1350, Mw / Mn=1.34 [ka]
[0175] [Synthesis Example 18] Synthesis of organic film-forming compound (A18) 3.1g of phenols (B7), 5.5g of fluorobenzene (C7), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A18). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A18): Mw=1390, Mw / Mn=1.32 [ka]
[0176] [Synthesis Example 19] Synthesis of organic film-forming compound (A19) 2.9g of phenols (B6), 5.0g of fluorobenzene (C6), and 4.1g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A19). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A19): Mw=1410, Mw / Mn=1.35 [ka]
[0177] [Synthesis Example 20] Synthesis of organic film-forming compound (A20) 40 g of N-methylpyrrolidone was added to 4.2 g of phenols (B8), 5.0 g of fluorobenzene (C6), and 4.1 g of potassium carbonate, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100 ml of methyl isobutyl ketone and 100 ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 10 g of THF was added to the residue to make a homogenous solution, and then crystallized with 50 g of methanol. The precipitated crystals were separated by filtration, washed twice with 20 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A20). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A20): Mw=1430, Mw / Mn=1.33 [ka]
[0178] [Synthesis Example 21] Synthesis of organic film-forming compound (A21) 3.8g of phenols (B9), 6.7g of fluorobenzene (C6), and 5.5g of potassium carbonate were added with 40g of N-methylpyrrolidone, and the mixture was reacted for 24 hours at an internal temperature of 140°C under a nitrogen atmosphere. After cooling at room temperature, 100ml of methyl isobutyl ketone and 100ml of pure water were added to the reaction solution to homogenize it, and the separated aqueous layer was removed. The organic layer was further washed twice with 100ml of 3% aqueous nitric acid solution and five times with 100ml of pure water, and then the organic layer was dried under reduced pressure. 10g of THF was added to the residue to make a homogenous solution, and then crystallized with 50g of methanol. The precipitated crystals were separated by filtration, washed twice with 20g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (A21). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (A21): Mw = 1580, Mw / Mn = 1.34 [ka]
[0179] [Synthesis Example 22] Synthesis of Comparative Compound (R1) In a 500mL four-neck flask, 6.1g of the synthetic raw material for comparative example (D1), 15.2g of the synthetic raw material for comparative example (D2), 13.8g of potassium carbonate, 100g of toluene, and 200g of DMSO were charged and stirred at 120°C for 5hr under a nitrogen stream. Toluene, acetic acid, and water were added and separated, and the oil layer was distilled off under reduced pressure to obtain a hexabromo compound. The hexabromo compound obtained above, 200 g of triethylamine, and 0.8 g of CuI(I) were charged into a 500 mL four-neck flask, and stirred for 30 minutes at room temperature under an Ar stream. After charging 42.7 g of Pd(0)(TPP) and 11.8 g of trimethylsilylacetylene, the temperature was raised to 80°C and the mixture was stirred for 5 hours while maintaining the temperature. The reaction mass was filtered, and the filtrate was concentrated, then subjected to column treatment with toluene and concentrated to obtain a hexa(trimethylsilylethynyl) compound. The hexa(trimethylsilylethynyl) compound obtained above was directly charged into a 300 mL four-neck flask, and 50 g of toluene, 50 g of methanol, and 16.5 g of potassium carbonate were added and stirred at room temperature for 18 hours. The reaction mass was neutralized directly with acetic acid, toluene was added and washed with water, and the toluene was distilled off under reduced pressure to obtain (R1). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (R1): Mw=970, Mw / Mn=1.03 [ka]
[0180] [Synthesis Example 23] Synthesis of Comparative Compound (R2) 20.0 g of synthetic raw material for comparative example (D3), 16.4 g of synthetic raw material for comparative example (D4), and 23.3 g of potassium carbonate were added with 200 g of N-methylpyrrolidone, and the reaction was carried out for 24 hours at an internal temperature of 140 ° C. under a nitrogen atmosphere. After cooling at room temperature, 300 ml of methyl isobutyl ketone and 300 ml of pure water were added to the reaction solution to homogenize it, and then the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to make a homogenous solution, and then crystallized with 350 g of methanol. The precipitated crystals were separated by filtration, washed twice with 200 g of methanol, and collected. The collected crystals were vacuum dried at 70 ° C. to obtain (R2). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (R2): Mw=580, Mw / Mn=1.03 [ka]
[0181] [Synthesis Example 24] Synthesis of Comparative Compound (R3) 10.0 g of synthetic raw material for comparative example (D3), 8.5 g of synthetic raw material for comparative example (D5), and 7.9 g of potassium carbonate were added with 40 g of N-methylpyrrolidone, and the reaction was carried out for 24 hours at an internal temperature of 140 ° C. under a nitrogen atmosphere. After cooling at room temperature, 100 ml of methyl isobutyl ketone and 100 ml of pure water were added to the reaction solution to homogenize it, and then the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 10 g of THF was added to the residue to make a homogenous solution, and then crystallized with 50 g of methanol. The precipitated crystals were separated by filtration, washed twice with 20 g of methanol, and collected. The collected crystals were vacuum dried at 70 ° C. to obtain (R3). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (R3): Mw=1550, Mw / Mn=1.85 [ka]
[0182] [Synthesis Example 25] Synthesis of Comparative Compound (R4) 20.0 g of synthetic raw material for comparative example (D6), 16.2 g of synthetic raw material for comparative example (D7), and 25.4 g of potassium carbonate were added with 200 g of N-methylpyrrolidone, and the reaction was carried out for 8 hours at an internal temperature of 120 ° C. under a nitrogen atmosphere. After cooling at room temperature, 300 ml of methyl isobutyl ketone and 300 ml of pure water were added to the reaction solution to homogenize it, and then the separated aqueous layer was removed. The organic layer was further washed twice with 100 ml of 3% aqueous nitric acid solution and five times with 100 ml of pure water, and then the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to make a homogenous solution, and then crystallized with 400 g of methanol. The precipitated crystals were separated by filtration, washed twice with 300 g of methanol, and collected. The collected crystals were dried in a vacuum at 70 ° C. to obtain (R4) as the mixture shown below. The isomer ratio measured by LC is also shown. In addition, the weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows. (R4): Mw=760, Mw / Mn=1.04 [ka]
[0183] [Synthesis Example 26] Synthesis of Comparative Compound (R5) Under a nitrogen atmosphere, 80 g of the synthetic raw material for comparative example (D8), 22 g of 37% formalin solution, and 250 g of 1,2-dichloroethane were made into a homogeneous solution at a liquid temperature of 70 ° C., and then 5 g of methanesulfonic acid was slowly added and reacted at a liquid temperature of 80 ° C. for 12 hours. After cooling to room temperature, 500 ml of MIBK was added, and the organic layer was washed five times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 300 g of THF was added to the residue to make a homogeneous solution, and the polymer was reprecipitated with 2000 g of hexane. The precipitated polymer was separated by filtration and dried under reduced pressure to obtain compound (R5). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the following results were obtained. (R5): Mw=3000, Mw / Mn=1.58 [ka]
[0184] Preparation of organic film-forming materials (UDL-1 to 23, comparative UDL-1 to 5) The organic film-forming compounds (A1) to (A21) and the comparative compounds (R1) to (R5) were dissolved in an organic solvent containing propylene glycol monomethyl ether acetate (PGMEA) and 0.1 mass % of FC-4430 (manufactured by Sumitomo 3M Limited) in the proportions shown in Table 1, as high boiling point solvents (S1) 1,6-diacetoxyhexane: boiling point 260°C and (S2) tripropylene glycol monomethyl ether: boiling point 242°C, and filtered through a 0.1 μm fluororesin filter to prepare organic film-forming materials (UDL-1 to 23, comparative UDL-1 to 5).
[0185] [Table 1]
[0186] Example 1 Solvent Resistance Measurement (Examples 1-1 to 1-23, Comparative Examples 1-1 to 1-5) The organic film-forming materials (UDL-1 to 23, comparative UDL-1 to 5) prepared above were applied onto a silicon substrate, baked in air at 400°C for 60 seconds, the film thickness was measured, PGMEA solvent was dispensed onto the substrate, left for 30 seconds, spin-dried, and baked at 100°C for 60 seconds to evaporate the PGMEA solvent. The film thickness was measured again, and the difference in film thickness before and after PGMEA treatment was calculated to evaluate the solvent resistance. The results are shown in Table 2.
[0187] [Table 2]
[0188] As shown in Table 2, the organic film-forming materials of the present invention (Examples 1-1 to 1-23) were found to produce films with excellent solvent resistance with almost no film loss due to solvent treatment. It was found that sufficient solvent resistance was exhibited even when an electron-withdrawing group was bonded to the benzene ring of the triple bond-containing terminal group.
[0189] Example 2 Evaluation of heat resistance characteristics (Examples 2-1 to 2-23, Comparative Examples 2-1 to 2-5) The above organic film-forming materials (UDL-1 to 23, Comparative UDL-1 to 5) were each applied onto a silicon substrate and baked in air at 180°C to form a 200 nm coating film, and the film thickness was measured. This substrate was further baked at 400°C for 10 minutes in a nitrogen stream with an oxygen concentration controlled to 0.2% or less, and the film thickness was measured. The results are shown in Table 3.
[0190] [Table 3]
[0191] As shown in Table 3, the organic film-forming material of the present invention (Examples 2-1 to 2-23) shows a film thickness reduction of 3% or less even after baking at 400°C for 10 minutes, and the organic film-forming material of the present invention can form an organic film having high heat resistance even under high temperature conditions of 400°C. It was found that the heat resistance is excellent even if the material has a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom, a diaryl ether structure or a diarylamine structure, and a structure in which an electron-withdrawing group is bonded to the benzene ring of a triple bond-containing terminal group. In contrast, a large film thickness reduction of more than 10% occurred in Comparative Examples 2-3 and 2-5, and it was shown that a compound having a structure in which one propargyl group is bonded to a nitrogen atom and a novolac structure do not have high heat resistance under high temperature conditions of 400°C. From the above, it is found that R1 in the general formula (1A) in the present invention has an ethynyl structure or a propargyl ether structure as shown in formula (1B) has high heat resistance.
[0192] Example 3: Evaluation of filling characteristics (Examples 3-1 to 3-23, Comparative Examples 3-1 to 3-5) As shown in FIG. 3, the above organic film forming materials (UDL-1 to 23, comparative UDL-1 to 5) were applied onto a SiO2 wafer substrate having a dense hole pattern (hole diameter 0.16 μm, hole depth 0.50 μm, distance between the centers of two adjacent holes 0.32 μm), and baked in air at 400° C. for 60 seconds to form an organic film 8. The substrate used was a base substrate 7 (SiO2 wafer substrate) having a dense hole pattern as shown in FIG. 3(G) (overhead view) and (H) (cross-sectional view). The cross-sectional shape of each of the obtained wafer substrates was observed using a scanning electron microscope (SEM) to confirm whether the holes were filled with the organic film 8 without any voids (air gaps). The results are shown in Table 4. When an organic film forming material with poor filling properties was used, voids were generated inside the holes in this evaluation. When an organic film forming material with good filling properties is used, in this evaluation, the organic film 8 fills the inside of the hole without leaving any voids, as shown in FIG. 3(I).
[0193] [Table 4]
[0194] As shown in Table 4, it was confirmed that the organic film-forming materials of the present invention (Examples 3-1 to 3-23) were capable of filling hole patterns without generating voids and had good filling properties. On the other hand, in Comparative Examples 3-3 and 3-5, voids were generated due to insufficient heat resistance, as in the results of Example 2. From these results, it was confirmed that the organic film-forming materials of the present invention have good filling properties.
[0195] Example 4: Evaluation of planarization characteristics (Examples 4-1 to 4-23, Comparative Examples 4-1 to 4-5) Each of the organic film forming materials (UDL-1 to 23, comparative UDL-1 to 5) was applied onto a base substrate 9 (SiO2 wafer substrate) having a giant isolated trench pattern (FIG. 4(J), trench width 25 μm, trench depth 0.10 μm), and baked in air at 400°C for 60 seconds to form an organic film 10. The step delta10 between the trench portion and the non-trench portion of the organic film was observed using a KLA-Tencor D-600 (stylus profiler). The results are shown in Table 5. In this evaluation, the smaller the step, the better the planarization characteristics. In this evaluation, a trench pattern with a depth of 0.10 μm was planarized using an organic film material with a normal film thickness of about 0.2 μm, which is a strict evaluation condition for evaluating the superiority or inferiority of the planarization characteristics.
[0196] [Table 5]
[0197] As shown in Table 5, the organic film-forming material of the present invention (Examples 4-1 to 4-23) had a smaller step between the organic film in the trench portion and the non-trench portion than Comparative Examples 4-1 to 4-5, and was confirmed to have excellent flattening properties. In Comparative Examples 4-1, 4-2, and 4-3, since an electron-withdrawing group was not bonded to the benzene ring of the triple bond-containing terminal group, the interaction between molecules was not relaxed, the crosslinking temperature was low, and the flatness due to thermal flow could not be ensured, resulting in deterioration of the flatness. In Comparative Example 4-4, although a fluorine atom was present on the benzene ring of the triple bond-containing terminal group, the material had a dioxane ring structure and did not have a diaryl ether structure, so that the fluidity was insufficient in the wide trench portion, resulting in poor flatness. In Comparative Examples 4-3 and 4-5, the heat resistance was insufficient as shown in the results of the heat resistance property evaluation in Comparative Example 2, so the film was greatly shrunk by baking at 400°C, resulting in deterioration of the flatness. In addition, when Examples 4-22 and 4-23 in which a high-boiling point solvent was added were compared with Example 4-7 in which no high-boiling point solvent was added, it was found that the flatness was improved by the addition of a high-boiling point solvent. From these results, it was found that the organic film-forming material of the present invention has excellent heat resistance, and therefore film shrink during high-temperature baking is suppressed, thereby exhibiting excellent flattening properties.
[0198] Example 5 Pattern formation test (Examples 5-1 to 5-23, Comparative Examples 5-1 to 5-3) The above organic film forming materials (UDL-1 to 23, comparative UDL-1 to 2, 4) were each applied onto a base substrate 9 (SiO2 wafer substrate) having a giant isolated trench pattern (FIG. 4(J), trench width 25 μm, trench depth 0.10 μm), and baked in air at 400 ° C for 60 seconds to form an organic film (resist underlayer film). A CVD-SiON hard mask intermediate film was formed thereon at 400 ° C, and an organic anti-reflective film material (ARC-29A: manufactured by Nissan Chemical Co., Ltd.) was further applied and baked at 210 ° C for 60 seconds to form an organic anti-reflective film with a film thickness of 80 nm, and a single layer resist for ArF of the resist upper layer film material was applied thereon and baked at 105 ° C for 60 seconds to form a photoresist film with a film thickness of 100 nm. An immersion protective film material (TC-1) was applied onto the photoresist film and baked at 90 ° C for 60 seconds to form a protective film with a film thickness of 50 nm. As for Comparative UDL-3 and Comparative UDL-5, since the heat resistance was poor as in the result of Comparative Example 2, it was not possible to form a CVD-SiON hard mask intermediate film, and therefore it was not possible to proceed to the subsequent pattern formation test.
[0199] The resist top layer film material (ArF single layer resist) was prepared by dissolving a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass% FC-430 (Sumitomo 3M Limited) in the proportions shown in Table 6, and filtering the solution through a 0.1 μm fluororesin filter.
[0200] [Table 6]
[0201] The polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used are shown below. [ka]
[0202] The immersion protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent in the ratio shown in Table 7, and filtering the solution through a 0.1 μm fluorine resin filter.
[0203] [Table 7]
[0204] The protective film polymer (PP1) used is shown below. [ka]
[0205] Next, the resist was exposed using an ArF immersion exposure tool (Nikon Corporation; NSR-S610C, NA 1.30, σ 0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% halftone phase shift mask), baked at 100°C for 60 seconds (PEB), and developed in a 2.38 mass% tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a 55 nm 1:1 positive line and space pattern (resist pattern).
[0206] Next, the organic anti-reflective film and the CVD-SiON hard mask were etched by dry etching using the resist pattern as a mask using a Tokyo Electron etching device, Telius, to form a hard mask pattern, the organic film was etched using the obtained hard mask pattern as a mask to form an organic film pattern, and the SiO2 film was etched using the obtained organic film pattern as a mask. The etching conditions are as follows:
[0207] Transfer conditions of resist pattern onto SiON hard mask. Chamber pressure 10.0Pa RF power: 1,500W CF4 gas flow rate: 75sccm O2 gas flow rate: 15sccm Time 15sec
[0208] Conditions for transferring hard mask patterns to organic films. Chamber pressure 2.0Pa RF power 500W Ar gas flow rate: 75sccm O2 gas flow rate: 45sccm Time 120sec
[0209] Transfer conditions of organic film pattern onto SiO2 film. Chamber pressure 2.0Pa RF power: 2,200W C5F 12 Gas flow rate: 20sccm C2F6 gas flow rate: 10sccm Ar gas flow rate: 300sccm O2 gas flow rate: 60sccm Time 90sec
[0210] The pattern cross sections of the non-trench portion and the trench portion were observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd. The results are shown in Table 8.
[0211] [Table 8]
[0212] As shown in Table 8, the results of the organic film-forming material of the present invention (Examples 5-1 to 5-23) confirmed that in all cases, the resist upper layer film pattern was finally transferred to the substrate well, and the organic film-forming material of the present invention is suitable for use in microfabrication using a multilayer resist method. In Comparative Examples 5-1, 5-2, and 5-3, as in the results of the planarization characteristic evaluation of Comparative Example 4, the planarity was insufficient, so a large step was generated between the trench portion and the non-trench portion, and even after forming a CVD-SiON hard mask, an organic anti-reflective film material, and a resist upper layer film thereon, a large film thickness difference was generated between the trench portion and the non-trench portion, so that the focus shift during exposure was significant in the trench portion, and a pattern could not be formed.
[0213] From the above, it has become clear that the organic film-forming material of the present invention containing the organic film-forming compound has heat resistance at 400°C or higher and high-level filling / planarization properties, even on a substrate to be processed having a wide trench structure, and is therefore extremely useful as an organic film material for use in a multilayer resist method, and that the pattern formation method of the present invention using this material makes it possible to form fine patterns with high precision, even on a substrate to be processed having steps.
[0214] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0215] 1...substrate, 2...processed layer, 2a...pattern (pattern formed on the processed layer), 3... organic film, 3'... organic film forming material, 3a... organic film pattern, 4...silicon-containing resist intermediate film, 4a...silicon-containing resist intermediate film pattern, 5...resist upper layer film, 5a...resist upper layer film pattern, 6...exposed portion, 7 ... base substrate having a dense hole pattern, 8 ... organic film, 9...Base substrate having a giant isolated trench pattern; 10...Organic film; Delta 10: Difference in height between the organic film in the trench and non-trench areas.
Claims
1. An organic film-forming material, comprising: (A) an organic film-forming compound represented by the following general formula (1A); and (B) an organic solvent: 【Chemistry 1】 (In general formula (1A), Ar 1 is an optionally substituted benzene ring or naphthalene ring; W 1 is a hydrocarbon group having 1 to 15 carbon atoms which may be substituted with a fluorine atom; W 2 is -O- or -NR 3 - and R 1 are each independently a group represented by the following formula (1B), 2 are each independently a halogen atom, a cyano group, or a nitro group; R 3 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, a=2 to 4, b=1 to 4, and c=1 to 4, provided that b+c≦5. 【Chemistry 2】 (In formula (1B), the dashed lines represent bonds.)
2. The R of the component (A) 2 2. The organic film-forming material according to claim 1, wherein is a fluorine atom.
3. The W of the component (A) 1 The organic film-forming material according to claim 1 or 2, characterized in that: 【Chemistry 3】 (In formula (1C), the dashed lines represent bonds.)
4. The organic film-forming material according to any one of claims 1 to 3, characterized in that the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn in terms of polystyrene as determined by a gel permeation chromatography method of the organic film-forming compound of the component (A) is 1.00≦Mw / Mn≦1.
35.
5. The organic film-forming material according to any one of claims 1 to 4, characterized in that the component (B) is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
6. The organic film-forming material according to any one of claims 1 to 5, characterized in that the organic film-forming material further contains one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, and (F) a plasticizer.
7. 7. A substrate for manufacturing a semiconductor device, comprising a substrate on which an organic film is formed by curing the organic film-forming material according to claim 1.
8. A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material according to any one of claims 1 to 6 onto a substrate to be processed, and heat-treating the substrate to which the organic film-forming material has been applied in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
9. A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material according to any one of claims 1 to 6 onto a substrate to be processed, heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds in an inert gas atmosphere to obtain a cured film.
10. 10. The method for forming an organic film according to claim 8, wherein the oxygen concentration in the inert gas atmosphere is set to 1% or less.
11. A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material according to any one of claims 1 to 6 onto a substrate to be processed, and heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
12. 12. The method for forming an organic film according to claim 11, wherein the oxygen concentration in the air is 1% or more and 21% or less.
13. 13. The method for forming an organic film according to claim 8, wherein the substrate to be processed has a structure or step having a height of 30 nm or more.
14. 7. A method for forming a pattern on a workpiece substrate, comprising the steps of: forming an organic film on the workpiece substrate using the organic film-forming material according to claim 1; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece substrate by etching using the organic film on which the pattern has been transferred as a mask.
15. A method for forming a pattern on a substrate to be processed, comprising the steps of: forming an organic film on the substrate to be processed using the organic film-forming material according to any one of claims 1 to 6; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective film on the silicon-containing resist intermediate film; forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
16. 7. A method for forming a pattern on a substrate to be processed, comprising the steps of: forming an organic film on the substrate to be processed using the organic film-forming material according to claim 1; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask intermediate film on which the pattern has been transferred as a mask; and further transferring the pattern to the substrate to be processed by etching using the organic film on which the pattern has been transferred as a mask.
17. 7. A method for forming a pattern on a substrate to be processed, comprising the steps of: forming an organic film on the substrate to be processed using the organic film-forming material according to claim 1; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming an organic antireflective film on the inorganic hard mask intermediate film; forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film and the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; and further transferring the pattern to the substrate to be processed by etching using the organic film to which the pattern has been transferred as a mask.
18. 18. The pattern formation method according to claim 16, wherein the inorganic hard mask intermediate film is formed by a CVD method or an ALD method.
19. 19. The method for forming a pattern according to claim 14, wherein the circuit pattern is formed by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct writing with an electron beam, nanoimprinting, or a combination thereof.
20. 20. The method for forming a pattern according to claim 14, wherein in forming the circuit pattern, the circuit pattern is developed with an alkali developer or an organic solvent.
21. 21. The pattern forming method according to claim 14, wherein the workpiece substrate is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
22. 22. The pattern formation method according to claim 21, wherein the metal of the substrate to be processed is selected from the group consisting of silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, and alloys thereof.
Citation Information
Patent Citations
Ethynyl-substituted aromatic compounds, their synthesis, polymers and uses
JP1999512430A
Pattern forming method, and material for forming underlayer film
JP2004205685A
Organic insulating film-forming composition
JP2005041938A
New acetylene compound, composition, cured product and method for making cured product
JP2009191109A
Film-forming composition, insulating film, and electronic device
JP2009206447A