Organosiloxane nano / microspheres with adjustable hydrophobicity / hydrophilicity and their manufacturing method

A surfactant-free process for producing organosiloxane nano/microspheres with adjustable hydrophobicity/hydrophilicity addresses contamination issues and improves payload release control, enhancing handling and reducing costs.

JP7565268B2Active Publication Date: 2024-10-10ファーマ イン シリカ ラボラトリーズ インコーポレイティド
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021525786
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-13
Filing Date
2019-11-12
Publication Date
2024-10-10
Estimated Expiration
2039-11-12

AI Technical Summary

Technical Problem

Existing methods for producing organosiloxane nano/microspheres often require surfactants, leading to additional cleaning steps and potential residual contamination, and there is a need for better control over the release of active substances encapsulated within these spheres.

Method used

A surfactant-free process is developed to produce organosiloxane nano/microspheres by hydrolyzing silica precursors, forming a dispersed phase, and emulsifying it in a continuous phase to create a water-in-oil emulsion, followed by adding a condensation catalyst to control the hydrophobicity/hydrophilicity and regulate payload release.

Benefits of technology

This method allows for the production of surfactant-free organosiloxane nano/microspheres with adjustable hydrophobicity/hydrophilicity, enabling controlled release of active substances, reducing contamination risks and manufacturing costs, and enhancing handling and payload control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565268000012
    Figure 0007565268000012
  • Figure 0007565268000013
    Figure 0007565268000013
  • Figure 0007565268000014
    Figure 0007565268000014
Patent Text Reader

Abstract

The present disclosure relates to organosiloxane nano / microspheres with tunable hydrophobicity / hydrophilicity, with or without an active substance / payload, and a surfactant-free, one-pot, versatile process for their preparation. By adjusting the hydrophobicity / hydrophilicity of the organosiloxane nano / microspheres, their release can be controlled. The preparation process includes the steps of: i0) separately hydrolyzing one or more silica precursors in a hydrolysis medium; i1) combining the prehydrolyzed precursors; or i2) removing some or all of the volatile solvent; or i3) preparing a dispersed phase containing a hydrophilic solvent to provide a dispersed phase; i4) emulsifying the dispersed phase of step i1), i2), or i3) in a continuous phase in the absence of a surfactant to provide a water-in-oil emulsion; and i5) adding a condensation catalyst to the emulsion to provide the nano / microspheres.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to tunable hydrophobicity / hydrophilicity organosiloxane nano / microspheres with or without active substances / payloads, and methods for making the same, the release of which can be controlled by adjusting the hydrophobicity / hydrophilicity of the organosiloxane nano / microspheres. [Background technology]

[0002] Active substance / payload sequestration has been widely adapted in the past decades in an increasing number of industrial sectors for different purposes (e.g., pharmaceuticals, cosmetics, food, construction, agriculture, catalysis) due to several concomitant attractive properties of this technology, such as reducing volatility, masking unpleasant odors, protecting labile payloads, preventing premature release of active substances, achieving better handling and better control of payload release, etc.

[0003] Organosiloxane materials are of particular interest due to their inherent advantages, such as chemical inertness, mechanical robustness, controllable morphology, tunable porosity, and diverse functionality. Moreover, organosiloxane materials are considered GRAS (i.e., "Generally Recognized As Safe"). Summary of the Invention

[0004] In one embodiment, there is provided a method for producing organosiloxane nano / microspheres, comprising the steps of: i0) separately hydrolyzing one or more silica precursors in a hydrolysis medium to provide one or more pre-hydrolyzed silica precursors; i1) combining the pre-hydrolyzed silica precursors of step i0) to provide a dispersed phase comprising the combined pre-hydrolyzed silica precursors; or i2) removing some or all of the volatile solvent from the combined pre-hydrolyzed silica precursor to provide a dispersed phase comprising a pre-condensed silica precursor; or i3) preparing a dispersed phase comprising a hydrophilic solvent by adding a hydrophilic solvent to the dispersed phase comprising the combined pre-hydrolyzed silica precursors obtained in step i1) or by adding a hydrophilic solvent to the dispersed phase comprising the pre-condensed silica precursors obtained in step i2); i4) emulsifying the dispersed phase of step i1), i2), or i3) in the absence of a surfactant in a continuous phase to provide a water-in-oil emulsion; i5) adding a condensation catalyst to the emulsion of step i4) to provide said organosiloxane nano / microspheres.

[0005] In a further aspect, there is provided organosiloxane spherical nano / microspheres comprising a network of organosiloxane, which are non-calcined, amorphous, surfactant-free, submicron to micron sized particles, optionally containing an active agent / payload.

[0006] In yet another aspect, there is provided a method for modulating the release of an active agent / payload comprising incorporating said active agent / payload into a nano / microsphere as defined herein or incorporating said active agent / payload into a process as defined herein. [Brief description of the drawings]

[0007] Example figures corresponding to the drawings are listed as follows: [Figure 1] SEM images of example microspheres: A) Example 1-1 (scale bar = 200 μm), B) Example 1-2 (scale bar = 200 μm), C) Example 1-3 (scale bar = 10 μm). [Diagram 2] SEM images of example microspheres: A) Example 2-1 (scale bar = 200 μm), B) Example 2-2 (scale bar = 10 μm). [Diagram 3]SEM images of examples of the obtained microspheres. A) Example 3 (scale bar = 40 μm), B) Example 4 (scale bar = 200 μm), C) Example 5 (scale bar = 100 μm), D) Example 6-1 (scale bar = 5 μm), E) Example 6-2 (scale bar = 10 μm), F) Example 7 (scale bar = 10 μm), G) Example 8 (scale bar = 10 μm), H) Example 9 (scale bar = 100 μm), I) Example 10 (scale bar = 3 μm), J) Example 11 (scale bar = 400 μm), K) Example 12 (scale bar = 3 μm). (Scale bar = 5 μm), L) Example 13 (Scale bar = 100 μm), M) Example 14 (Scale bar = 200 μm), N) Example 15 (Scale bar = 500 μm), O) Example 16 (Scale bar = 100 μm), P) Example 17-1 (Scale bar = 200 μm), Q) Example 17-2 (Scale bar = 100 μm), R) Example 17-3 (Scale bar = 100 μm), S) Example 17-4 (Scale bar = 100 μm), T) Example 18 (Scale bar = 100 μm). [Figure 4] Contact angle photographs: A) Example 15, B) Example 4, C) Example 5. [Diagram 5] SEM images of examples of microspheres containing active agents / payloads: A) Example 20-1 (scale bar = 200 μm), B) Example 20-2 (scale bar = 100 μm), C) Example 20-3 (scale bar = 70 μm). [Figure 6] SEM images of examples of microspheres containing active agents / payloads: A) Example 21-1 (scale bar = 10 μm), B) Example 21-2 (scale bar = 100 μm), C) Example 21-3 (scale bar = 100 μm), D) Example 21-4 (scale bar = 100 μm). [Figure 7] SEM images of examples of microspheres containing active agents / payloads: A) Example 22-1 (scale bar = 100 μm), B) Example 22-2 (scale bar = 10 μm), C) Example 22-3 (scale bar = 10 μm). [Figure 8]SEM images of examples of active agent / payload loaded microspheres: A) Example 23-1 (scale bar = 100 μm), B) Example 23-2 (scale bar = 10 μm). [Figure 9] SEM images of examples of active agent / payload loaded microspheres: A) Example 24-1 (scale bar=10 μm), B) Example 24-2 (scale bar=500 μm), c) Example 24-3 (scale bar=100 μm), D) Example 24-4 (scale bar=10 μm), E) Example 24-5 (scale bar=50 μm), F) Example 24-6 (scale bar=50 μm), G) Example 24-7 (scale bar=50 μm), H) Example 24-8 (scale bar=50 μm), I) Example 24-9 (scale bar=100 μm), J) Example 24-10 (scale bar=100 μm), K) Example 25 (scale bar=120 μm). [Figure 10] Release profiles of uracil from microspheres developed at pH 7 (A, C, and D) and pH 5.5 (B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Detailed Description The present disclosure relates to a versatile process that provides: 1) a one-pot process, 2) distribution of active ingredients throughout organosiloxane spherical materials in solid or liquid state with or without in situ active / payload administration / sequestration, 3) tunable hydrophobicity / hydrophilicity of pre-hydrolyzed / pre-condensed silica precursors compatible with active ingredients, and 4) control of active / payload release parameters by adjusting the hydrophobicity and hydrophilicity of the external and internal surfaces of organosiloxane spherical materials.

[0009] The process herein is carried out without surfactants, which present a series of disadvantages due to the need for additional cleaning steps and potential residual contamination remaining in the organosiloxane nano / microspheres. Thus, the use of surfactants requires additional cost / production time.

[0010] A surfactant is understood to be any agent that does not participate in the bonding of the siloxane network (forming Si-O-Si). Certain silica precursors used herein may have amphiphilic moieties, however, these are not excluded from the process herein since they participate in the creation of the siloxane network.

[0011] The present process and organosiloxane nano / microspheres do not contain any surfactants other than the amphiphilic silane.

[0012] The processes herein are preferably carried out under high shear or dispersive forces.

[0013] As used herein, a "silica precursor" refers to a compound having the formula R 4-x Si(L) x or a compound of the formula (L)3Si-R'-Si(L)3, where: R is a monosilylated residue as an alkyl, alkenyl, alkynyl, cycloaliphatic, aryl, alkylaryl group, which is a halogen atom, -OH, -SH, -N(R a )2, -N + (R a )3, -P(R a ) optionally replaced by 2; R a can be alkyl, alkenyl, alkynyl, alicyclic, aryl, and alkylaryl; L is halogen or acetoxide -OC(O)R a , or alkoxide OR a Is a base; X is an integer from 1 to 4; and R' is a disilyl residue as an alkyl, alkenyl, alkynyl, cycloaliphatic, aryl, alkylaryl group, which is a halogen atom, -OH, -SH, -N(R a )2, -N + (R a )3, -P(R a )2. In one embodiment, the silica precursor R4-x Si(L) x Or (L)3Si-R'-Si(L)3 is a silicon alkoxide, such as a tetraalkoxysilane, a monoalkyl-trialkoxysilane, or a dialkyldialkoxysilane, or a bis-trialkoxy bridged silane. In a further embodiment, the silica precursor is a mixture of silicon alkoxides, such as a tetraalkoxysilane, and / or a monoalkyl-trialkoxysilane, and / or a dialkyl-dialkoxysilane, and / or a bis-trialkoxy bridged silane.

[0014] In one embodiment, the monoalkyltrialkoxysilane RSi(L)3 includes a monoalkyl that is a linear or branched group of 1 to 18 carbon atoms, and the trialkoxy is a triethoxy or trimethoxy group.

[0015] In one embodiment, the dialkyldialkoxysilane R2Si(L)2 includes a dialkyl that is a linear or branched group of 1 to 18 carbon atoms, and the dialkoxy is a diethoxy or dimethoxy group.

[0016] In one embodiment, the trialkylmonoalkoxysilane R3Si(L) comprises a trialkyl which is a linear or branched group of 1 to 18 carbon atoms, and the monoalkoxy is a monoethoxy or monomethoxy group.

[0017] In one embodiment, the trialkoxy bridged silane (L)3Si-R'-Si(L)3 comprises a bridged linear alkyl or alkenyl group of 2 to 18 carbon atoms, where the trialkoxy is a triethoxy or trimethoxy group.

[0018] The hydrolysis medium used in the present disclosure will promote the formation of silanol functional groups Si-OH generated from the hydrolysis of the silica precursor. Examples of such media include aqueous media, for example water, optionally mixed with a water-miscible organic solvent such as ethanol or THF, and inorganic acids such as HCl, H3PO4, H2SO4, HNO3, etc. Preferably, the concentration of the hydrolysis medium is about 0.01 mol / L to 0.05 mol / L, and preferentially the inorganic acid is HCl.

[0019] Condensation catalyst refers to any reagent known in the art to promote polycondensation to form siloxane Si-O-Si bonds, which achieves a final pH of about 9.0-11.5 in suspension. Condensation catalysts can be, but are not limited to, NH4OH, NaOH, KOH, LiOH, Ca(OH)2, NaF, KF, TBAF, TBAOH, TMAOH, triethanolamine, triethylamine, primene, L-lysine, aminopropylsilane.

[0020] In one embodiment, the condensation catalyst is concentrated NH4OH. In one embodiment, the condensation catalyst is NaOH.

[0021] As used herein, "dispersed phase" refers to a mixture of prehydrolyzed and / or precondensed silica precursors with or without an active substance / payload. Prehydrolyzed silica precursors are silica precursors that are formed in the hydrolysis medium at a temperature of R 4-x Si(L) x or (L)3Si-R'-Si(L)3 by hydrolysis of the L group. The pre-condensed silica precursor is obtained by partial condensation of the pre-hydrolyzed silica precursor by evaporating the volatile solvents present in the hydrolysis medium. The dispersed phase may also contain one or more hydrophilic solvents.

[0022] "Continuous phase" as used herein means a solvent known in the art to have opposite polarity compared to the dispersed phase and thus form an inverse emulsion (water in oil).

[0023] The continuous phase may be, for example, but is not limited to, toluene, xylene, benzene, hexane, cyclohexane, pentane, heptane, 2-butanone, trichloroethylene, diethyl ether, diisopropyl ether, ethyl acetate, 1,2-dichloromethane, chloroform, carbon tetrachloride, butyl acetate, n-butanol, n-pentanol. In one embodiment, the continuous phase is preferentially toluene, xylene, hexane, or cyclohexane.

[0024] In one embodiment, the volume ratio of the continuous phase to the dispersed phase comprising the pre-hydrolyzed / pre-condensed silica precursor is 5:500, preferably 10:100.

[0025] As used herein, "emulsion process" refers to a process that involves a piece of laboratory or industrial equipment used to mix two or more normally immiscible liquids to produce a dispersion of droplets (the dispersed phase) in the volume of the continuous phase, preferably rotor-stator homogenizers and sonic disrupters.

[0026] In one embodiment, a rotor-stator homogenizer is used in the emulsion process. Typically, the homogenizer speed is about 4,000 rpm to 20,000 rpm. Preferably, it is about 12,000 rpm or 20,000 rpm.

[0027] In one embodiment, the emulsion process uses a sonic disruption homogenizer. Typically, the homogenizer power potentiometer is about 50%-100%, and the on / off cycle is on for 50%-100% of the time. Preferably, the power potentiometer is about 100%, and is on for 100% of the cycle time.

[0028] The size of the microspheres can be modified by emulsification methods. Rotor-stator homogenizers induce the formation of microspheres with a mean diameter generally between 1 and 200 μm. Sonic disrupters induce the formation of nanospheres with a mean diameter generally between 0.05 and 10 μm. The size of the nano / microspheres can be modified by other parameters, such as the ratio of the continuous phase to the dispersed phase. The higher this ratio, the smaller the nano / microspheres. For the size of the nano / microspheres, it is important to take into account the speed of the rotor-stator homogenizer or the power of the sonic disrupter. The higher the speed or power, the smaller the nano / microspheres.

[0029] As used herein, "active agent / payload" refers to the compound of interest entrapped in the nano / microsphere. The active agent / payload is preferably insoluble in the continuous phase. The active agent / payload may be in solid or liquid form. They may be incorporated by solubilization, dispersion, or emulsification in the dispersed phase.

[0030] In one embodiment, the active agent / payload is a hydrophilic molecule that can be dissolved in aqueous and / or polar solvents.

[0031] In one embodiment, the active agent / payload is a cosmetic, cosmeceutical, or pharmaceutical compound.

[0032] In one embodiment, uracil is used as the active substance / payload. In one embodiment, 5-fluorouracil is used as the active substance / payload. In one embodiment, the active substance / payload is a sugar or derivative, preferably a monosaccharide such as mannose (especially D-mannose) and glucose (especially D-glucose). In one embodiment, the active substance is a vitamin (e.g. vitamin C).

[0033] According to the present disclosure, the general process may or may not include an active agent / payload: A) In one embodiment, no active agent / payload is used in any process step; B) In a further embodiment, at least one active agent / payload is used in at least one process step.

[0034] (Method A) In one embodiment, the method for preparing active agent / payload free silica nano / microspheres comprises the steps of: A0) separately hydrolyzing one or more silica precursors in a hydrolysis medium to provide one or more pre-hydrolyzed silica precursors; A1) combining the pre-hydrolyzed silica precursors of step A0) to provide a dispersed phase comprising combined pre-hydrolyzed silica precursors; or A2) removing some or all of the volatile solvent from the combined pre-hydrolyzed silica precursors obtained in step A1) to provide a dispersed phase comprising pre-condensed silica precursors; or A3) removing the hydrophilic solvent from the combined pre-hydrolyzed silica precursors obtained in step A2) to provide a dispersed phase comprising pre-condensed silica precursors; A4) preparing a dispersed phase comprising a hydrophilic solvent by adding said hydrophilic solvent to said dispersed phase comprising a pre-condensed silica precursor obtained in step A1), A2) or A3) with a continuous phase in the absence of a surfactant to obtain a water-in-oil emulsion; A5) adding a condensation catalyst to the emulsion of step A4) to obtain said organosiloxane nano / microspheres; A6) optionally aging the suspension; A7) optionally isolating, washing and / or drying the nano / microspheres.

[0035] In one embodiment, all silica precursors are independently hydrolyzed and combined in one vessel (A0) with stirring at room temperature and a stirring speed of at least 500 rpm for a minimum of 1 hour.

[0036] In one embodiment, all pre-hydrolyzed silica precursors (A0) are combined in one vessel and used as the dispersed phase (A1) without further processing (eg, solvent removal, pre-condensation).

[0037] In one embodiment, the desired amount of volatile solvent from the hydrolysis medium can be removed by i) evaporation under reduced pressure on a rotary evaporator at room temperature to 70° C., or ii) distillation at a preferred temperature of 90-120° C., applying lower and higher temperatures, if necessary (A2).

[0038] In one embodiment, a water-miscible solvent, such as dimethylsulfoxide (DMSO), is introduced into the dispersed phase (A3).

[0039] In one embodiment, emulsification of the dispersed phase (A1 or A2 or A3) in the continuous phase can be achieved using a rotor-stator homogenizer, which produces stable microdroplets. In one embodiment, emulsification of the dispersed phase (A1 or A2 or A3) in the continuous phase can be achieved using a sonic disrupter, which produces stable nanodroplets (A4).

[0040] In one embodiment, during emulsification, a condensation catalyst is added to the emulsion, and the emulsification process is maintained for 15-60 seconds to obtain a nano / microsphere suspension. A condensation catalyst amount is added until the pH of the suspension reaches 9.0-11.5 (A5).

[0041] In one embodiment, after step (A5), a silica precursor is optionally added with or without pre-hydrolysis for delayed external surface functionalization.

[0042] In one embodiment, the nano / microsphere suspension is aged for 12-24 hours at room temperature with stirring or shaking to maintain a stable suspension and avoid agglomeration (A6).

[0043] In one embodiment, the nano / microspheres are isolated by filtration for microspheres, or by centrifugation for nanospheres, preferably at 5,000-100,000G, e.g., 15,000G, for 10 minutes. In one embodiment, the nano / microspheres are washed alternately with organic solvent and water until the supernatant reaches neutrality (i.e., pH about 7). Finally, the resulting material can be dried at room temperature or up to 70°C, at atmospheric or reduced pressure, e.g., for one or more days (A7).

[0044] (Method B) In one embodiment, the process for preparing silica nano / microspheres with active agent / payload comprises the steps of: B0) separately hydrolyzing one or more silica precursors in a hydrolysis medium to provide one or more pre-hydrolyzed silica precursors; B1) combining the pre-hydrolyzed silica precursors of step B0) to provide a dispersed phase comprising combined pre-hydrolyzed silica precursors; or B2) removing some or all of the volatile solvent from the combined pre-hydrolyzed silica precursors obtained in step B1) to provide a dispersed phase comprising pre-condensed silica precursors; or B3) removing the hydrophilic solvent from the combined pre-hydrolyzed silica precursors obtained in step B2) to provide a dispersed phase comprising pre-condensed silica precursors; B4) preparing a dispersed phase comprising a hydrophilic solvent by adding a hydrophilic solvent to the dispersed phase comprising the pre-condensed silica precursor obtained in step B1), B2) or B3) in a continuous phase in the absence of a surfactant to obtain a water-in-oil emulsion; B5) adding a condensation catalyst to the emulsion of step B4) to obtain the organosiloxane nano / microspheres; B6) optionally aging the suspension; B7) optionally isolating, washing and / or drying the nano / microspheres. Depending on the solubility of the active substances / payloads, they can be introduced in steps (B1), (B2), (B3), (B4) or / and (B5) of the process.

[0045] In one embodiment, all silica precursors are independently hydrolyzed by stirring at room temperature with a stirring speed of at least 500 rpm for a minimum of 1 hour and combined in one vessel. The active agent / payload can be solubilized, dispersed or emulsified in the dispersed phase (B0).

[0046] In one embodiment, all pre-hydrolyzed silica precursors (B0) are combined in one vessel and used as the dispersed phase (B1) without further processing (eg, solvent removal, pre-condensation).

[0047] In one embodiment, the desired amount of volatile solvent can be removed from the hydrolysis medium by i) evaporation under reduced pressure on a rotary evaporator at room temperature to 70° C., or ii) distillation at a preferred temperature of 90-120° C., applying lower and higher temperatures if necessary. The active substance / payload can be solubilized, dispersed or emulsified in the resulting dispersed phase (B2).

[0048] In one embodiment, a water-miscible solvent, such as dimethylsulfoxide, is introduced into the dispersed phase (B1 or B2). The active agent / payload can be solubilized, dispersed, or emulsified in the resulting dispersed phase (B3).

[0049] In one embodiment, emulsification of the dispersed phase (B1 or B2 or B3) optionally containing active substance / payload in the continuous phase can be achieved with a rotor-stator homogenizer, which produces stable microdroplets. In one embodiment, emulsification of the dispersed phase (B1 or B2 or B3) optionally containing active substance / payload in the continuous phase can be achieved with a sonic disrupter, which produces stable nanodroplets. In one embodiment, the active substance / payload can be dispersed in the continuous phase as a solid state. In another embodiment, the active substance / payload solubilized in a water-miscible solvent can be added to the emulsion (B4).

[0050] In one embodiment, the active agent / payload can be solubilized in a condensation catalyst. During emulsification, a condensation catalyst is added to the emulsion and the emulsification process is maintained for 15-60 seconds to obtain a nano / microsphere suspension. An amount of condensation catalyst is added to reach a pH of the suspension of 9.0-11.5 (B5).

[0051] In one embodiment, after step (B5), a silica precursor is optionally added with or without pre-hydrolysis for delayed external surface functionalization.

[0052] In one embodiment, the nano / microsphere suspension is aged for 12-24 hours at room temperature with stirring or shaking to maintain a stable suspension and avoid agglomeration (B6).

[0053] In one embodiment, the nano / microspheres are isolated by filtration for microspheres or by centrifugation for nanospheres, preferably at 5,000-100,000 G, e.g. 15,000 G for 10 min. The nano / microspheres are washed with a solvent that has the lowest solubility for the active substance / payload to avoid leaching. Finally, the obtained material is dried (B7) at room temperature or up to 70° C., at atmospheric or reduced pressure, for example for one or more days, depending on the properties of the active substance / payload.

[0054] The amount of active substance / payload entrapped in the nano / microspheres is determined by analytical methods such as high performance liquid chromatography (HPLC), elemental analysis (EA), and thermogravimetric analysis (TGA).

[0055] The sequestration yield is defined by the following formula (Equation 1). The experimental amount of active substance corresponds to the active substance quantified by analytical methods. The theoretical amount of active substance corresponds to the amount initially introduced. The sequestration yield is between 70 and 100%.

number

[0056] The loading capacity is defined by the following formula (Equation 2): The experimental active substance amount corresponds to the active substance quantified by analytical methods. The total mass corresponds to the mass of the obtained nano / microspheres, excluding the water content. The loading capacity depends on the active substance / payload. In one embodiment, the loading capacity is 0.1% to 80% by weight.

number

[0057] In all embodiments, the porous structure of the nano / microspheres is unorganized. Nitrogen adsorption / desorption isotherms determine the surface area of ​​the nano / microspheres, which is typically up to 1,000 m 2 / g.

[0058] The hydrophobicity / hydrophilicity of the outer surface of the nano / microspheres is the result of the mixing of a silica precursor or a mixture of silica precursors.

[0059] In one embodiment, the hydrophobic / hydrophilic properties of the nano / microspheres can be controlled by the composition of the silica precursor, such as tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), methyltriethoxysilane (C1-TES), butyltriethoxysilane (C4-TES), octyltriethoxysilane (C8-TES), octadecyltriethoxysilane (C18-TES), dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride (DOAPS), and 3-dimethylaminopropyltrimethoxysilane (DMAM).

[0060] In one embodiment, when only TEOS is used as the silica precursor without active substance / payload loading, the contact angle of the corresponding nano / microspheres is 0°-40°, which indicates a completely hydrophilic outer surface property. In another embodiment, when C4-TES and / or C8-TES and / or C18-TES are used, mixed or not with other silica precursors, the resulting nano / microspheres show contact angles in the range of 80°-150°, which confirms the tunable outer surface properties of these matrices from hydrophilic to hydrophobic.

[0061] To confirm the above observations, the outer surface composition of the nano / microspheres, analyzed by X-ray photoelectron spectroscopy (XPS), is compared to the elemental composition of the whole nano / microsphere to confirm the hydrophobic / hydrophilic balance of the outer surface.

[0062] In one embodiment, DOAPS, a positively charged silica precursor with C18 alkyl chains, is used and mixed with other silica precursors. Typically, a positive zeta potential of +10 to +55 eV is observed, proving that the hydrophobic C18 alkyl chains on the outer surface of the nano / microspheres provide access to the positively charged ammonium functional groups.

[0063] Preparation of organosiloxane nano / microspheres without active substances / payloads In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH.

[0064] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA.

[0065] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH.

[0066] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA.

[0067] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably sunflower; and 3) the condensation catalyst is preferably NH4OH.

[0068] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and pre-condensed C18-TES and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 99%-25%; 2) the continuous phase is preferably cyclohexane; and 3) the condensation catalyst is preferably NH4OH.

[0069] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and pre-condensed C8-TES and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 99%-25%; 2) the continuous phase is preferably cyclohexane; and 3) the condensation catalyst is preferably TEA.

[0070] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C8-TES and TEOS silica precursors are used in a molar ratio preferably of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH.

[0071] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C8-TES and TEOS silica precursors are used in a molar ratio preferably of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA.

[0072] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH.

[0073] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C8-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA.

[0074] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferably 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH.

[0075] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferably 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA.

[0076] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferably 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH.

[0077] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferably 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA.

[0078] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C4-TES and TEOS silica precursors are used in a molar ratio preferably of 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH.

[0079] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed C4-TES and TEOS silica precursors are used in a molar ratio preferably of 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA.

[0080] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C4-TES and TEOS silica precursors are used in a molar ratio preferably of 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH.

[0081] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C4-TES and TEOS silica precursors are used in a molar ratio of preferably 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA.

[0082] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0083] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0084] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method A, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0085] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method A, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0086] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV.

[0087] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are used in a molar ratio of preferably 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0088] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV.

[0089] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0090] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C8-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV.

[0091] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C8-TES, DOAPS, and TEOS silica precursors are used in a molar ratio of preferably 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably toluene. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV.

[0092] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and non-precondensed C8-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0093] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method A, where: 1) prehydrolyzed and non-precondensed C8-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV.

[0094] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are used in a molar ratio preferably of 10%-20% / 2.5%-7.5% / 90%-60%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably cyclohexane; and 3) the condensation catalyst is preferably NH4OH.

[0095] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are used in a molar ratio of preferably 0%-75% / 0%-75% / 99%-25%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably cyclohexane; and 3) the condensation catalyst is preferably TEA.

[0096] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are preferably used in a molar ratio of 10%-20% / 2.5%-7.5% / 90%-60%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably cyclohexane; 3) the condensation catalyst is preferably NH4OH; and 4) DOAPS silica precursor is added in a suspension of nano / microspheres in a weight ratio of 0.5-5%, preferably 2% (ratio of weight of DOAPS to weight of precondensed silica precursor). The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV.

[0097] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA; and 4) DOAPS silica precursor is added in a suspension of nano / microspheres in a weight ratio of 0.5-5%, preferably 2% (ratio of weight of DOAPS to weight of precondensed silica precursor). The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV.

[0098] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed SH-TES and TEOS silica precursors are preferably used in a molar ratio of 0%-100% / 100%-0%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH.

[0099] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed SH-TES and TEOS silica precursors are preferably used in a molar ratio of 0%-100% / 100%-0%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA.

[0100] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed SH-TES and TEOS silica precursors are preferably used in a molar ratio of 0%-100% / 100%-0%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH.

[0101] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method A, where: 1) pre-hydrolyzed and non-pre-condensed SH-TES and TEOS silica precursors are preferably used in a molar ratio of 0%-100% / 100%-0%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA.

[0102] Preparation of organosiloxane nano / microspheres with active substances / payloads In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably NH4OH; and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%; or c) solubilization in the condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0103] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA; and 4) where the nano / microspheres contain a hydrophilic active substance / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%.

[0104] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0105] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%.

[0106] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 5% / 95%; 2) the continuous phase is preferably sunflower; 3) the condensation catalyst is preferably NH4OH; and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being 5-FU, preferentially with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0107] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and precondensed C18-TES and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 99%-25%; 2) the continuous phase is preferably cyclohexane; 3) the condensation catalyst is preferably NH4OH; and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the precondensed dispersed phase, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the precondensed dispersed phase with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0108] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and precondensed C18-TES and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 99%-25%; 2) the continuous phase is preferably cyclohexane; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the precondensed dispersed phase, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the precondensed dispersed phase with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0109] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%; or c) solubilization in the condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%

[0110] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%.

[0111] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES and TEOS silica precursors are used in a molar ratio of preferably 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0112] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 10% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%.

[0113] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferably 5% / 5% / 90%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably NH4OH; and 4) where the nano / microspheres contain a hydrophilic active / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0114] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferably 5% / 5% / 90%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA; and 4) where the nano / microspheres contain a hydrophilic active / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0115] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) pre-hydrolyzed and non-pre-condensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres comprise a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or f) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0116] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) pre-hydrolyzed and non-pre-condensed C8-TES, C18-TES, and TEOS silica precursors are used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres comprise a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%.

[0117] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C4-TES and TEOS silica precursors are used in a molar ratio of preferably 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably NH4OH; and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being 5-FU with preferentially 100% isolation yield and maximum loading capacity of 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0118] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C4-TES and TEOS silica precursors are used in a molar ratio of preferably 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%.

[0119] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) pre-hydrolyzed and non-pre-condensed C4-TES and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres comprise a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or f) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0120] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) pre-hydrolyzed and non-pre-condensed C4-TES and TEOS silica precursors are used, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 10%-50% / 90%-50%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres comprise a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%.

[0121] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0122] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0123] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically between +10 and +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or f) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0124] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) DOAPS (prehydrolyzed or not) and prehydrolyzed TEOS silica precursors are used without precondensation, preferably in a molar ratio of 1%-75% / 99%-25%, preferentially 1%-20% / 99%-80%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferably 100% xylene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically +10-+55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%.

[0125] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 1%-75% / 1%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0126] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0127] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferably 100% xylene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%. or e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0128] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C18-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferably 100% xylene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%.

[0129] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) prehydrolyzed and non-precondensed C8-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst, the hydrophilic active substance / payload being preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0130] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in Method B, where: 1) prehydrolyzed and non-precondensed C8-TES, DOAPS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably toluene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0131] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES, DOPAS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably NH4OH. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in the prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or f) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0132] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed C8-TES, DOPAS, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 5% / 5% / 90%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; and 3) the condensation catalyst is preferably TEA. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10 to +55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 50% loading capacity, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum of 10% loading capacity, preferentially 5%.

[0133] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are used in a molar ratio of preferably 10%-20% / 2.5%-7.5% / 90%-60%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably cyclohexane; 3) the condensation catalyst is preferably NH4OH; 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the precondensed dispersed phase, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the precondensed dispersed phase with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0134] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75% / 99%-25%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably cyclohexane; 3) the condensation catalyst is preferably TEA; 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in the precondensed dispersed phase, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the precondensed dispersed phase with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0135] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are preferably used in a molar ratio of 10%-20% / 2.5%-7.5% / 90%-60%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably cyclohexane; 3) the condensation catalyst is preferably NH4OH; and 4) the DOAPS silica precursor is added in a suspension of nano / microspheres in a weight ratio of 0.5-5%, preferably 2% (ratio of weight of DOAPS to weight of precondensed silica precursor). The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are characterized by a positive zeta potential, typically +10-+55 eV; and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in the precondensed dispersed phase, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the precondensed dispersed phase with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) solubilization in the condensation catalyst, the hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0136] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and precondensed C1-TES, C8-TES, and TEOS silica precursors are preferably used in a molar ratio of 0%-75% / 0%-75 / 99%-25%, preferentially 22.5% / 7.5% / 70%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA; and 4) the DOAPS silica precursor is added in a weight ratio (ratio of weight of DOAPS to weight of precondensed silica precursor) of 0.5-5%, preferably 2%, in the suspension of nano / microspheres. The resulting nano / microspheres, when suspended in aqueous solutions (water and phosphate buffered saline), are typically characterized by a positive zeta potential of +10-+55 eV, and 4) where the nano / microspheres contain a hydrophilic active agent / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in the pre-condensed dispersed phase, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in the pre-condensed dispersed phase with the aid of a hydrophilic co-solvent, the hydrophilic co-solvent being preferentially DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%.

[0137] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed SH-TES and TEOS precursors are preferably used in a molar ratio of 0% to 100% / 100% to 0%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres contain a hydrophilic active substance / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; or b) dispersion in a continuous phase prior to the emulsification process, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%; or c) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0138] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed SH-TES and TEOS precursors are preferably used in a molar ratio of 0% to 100% / 100% to 0%; 2) the continuous phase is preferably toluene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload. This hydrophilic active substance / payload can be introduced by: a) solubilization or dispersion in the prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 10%, preferentially 5%; or b) dispersion in the continuous phase before the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a 100% isolation yield and a maximum loading capacity of 50%, preferentially 20%.

[0139] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed SH-TES and TEOS precursors are preferably used in a molar ratio of 0%-100% / 100%-0%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably NH4OH, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in prehydrolyzed silica precursor with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 50%, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 100% and a loading capacity of up to 10%, preferentially 5%; or e) solubilization in a condensation catalyst. The hydrophilic active substance / payload is preferentially 5-FU with an isolation yield of 70-90% and a loading capacity of up to 10%, preferentially 5%.

[0140] In one embodiment, organosiloxane nano / microspheres are synthesized according to the method described in method B, where: 1) prehydrolyzed and non-precondensed SH-TES and TEOS precursors are preferably used in a molar ratio of 0%-100% / 100%-0%; 2) the continuous phase is preferably composed of 50%-100% xylene and 50%-0% cyclohexane, preferentially 100% xylene; 3) the condensation catalyst is preferably TEA, and 4) where the nano / microspheres contain a hydrophilic active substance / payload, which can be introduced by: a) solubilization or dispersion in a prehydrolyzed silica precursor, the hydrophilic active substance / payload being preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%; or b) solubilization in a prehydrolyzed silica precursor with the aid of a hydrophilic cosolvent, and preferentially the hydrophilic cosolvent is DMSO. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or c) dispersion in a continuous phase prior to the emulsification process. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 50%, preferentially 20%; or d) solubilization in a hydrophilic co-solvent, preferentially DMSO, and addition to the emulsion. The hydrophilic active substance / payload is preferentially 5-FU with a sequestration yield of 100% and a loading capacity of up to 10%, preferentially 5%.

[0141] Example of nano / microspheres obtained by method A (i.e. in the absence of active substance / payload): Example 1 Preparation of Microspheres with Fully Hydrolyzed, Non-Precondensed C18-TES and TEOS in Toluene (Method A)

[0142] Examples 1-1 : C18-TES / TEOS molar ratio = 1% / 99% microspheres Typically, 11.02 g (57.7 mmol) of TEOS was prehydrolyzed in 6.18 g of 0.01 N HCl under acidic conditions with stirring for 1 h. Meanwhile, prehydrolysis of 2.45 g of C18-TES was carried out in a mixture of 0.69 g of 0.05 N HCl, 4.99 g of THF and / or without 0.5 mL of EtOH in a separate vial with stirring for 1 h. Then, the prehydrolyzed C18-TES silica precursor was added to the prehydrolyzed TEOS and stirred at room temperature for 15-30 min to form hydrolyzed 1% / 99% C18-TES / TEOS silica precursor. This resulting dispersed phase was added to 200 g of toluene as the continuous phase while mixing with an Ultra-Turrax homogenizer (Ultra-Turrax® T25 combined with S25N-18G) at high speed (7,000-15,000) rpm. The mixture was stirred for 5 minutes to produce a uniform emulsion. Then, 1 g of concentrated NH4OH was added as a condensation catalyst. After 1 minute, the Ultra-Turrax was stopped and the suspension was kept stirring gently for at least overnight. The suspension of microspheres was then filtered, washed with toluene and ethanol, and finally dried at room temperature for 3 days. The morphological and textural characteristics of the obtained spheres are shown in Figure 1 and Table 1.

[0143] Examples 1-2 : Microspheres with C18-TES / TEOS molar ratio = 10% / 90%

[0144] Silica microspheres containing x% C18-TES and y% TEOS were prepared using the same method as described in Example 1-1. The main characteristics of the obtained spheres are summarized in Figure 1 and Table 1.

[0145] Examples 1 to 3 : Microspheres with a molar ratio of C18-TES / TEOS = 75% / 25%

[0146] Silica microspheres containing 75% C18-TES and 25% TEOS were prepared using the same method as described in Example 1-1. The main characteristics of the obtained microspheres are reported in Figure 1 and Table 1. [Table 1]

[0147] Example 2 Preparation of microspheres with fully hydrolyzed, non-precondensed C18-TES and TEOS (molar ratio: 7% / 93%, Method A) in another continuous phase

[0148] Example 2-1 In 75% xylene / 25% cyclohexane

[0149] Silica microspheres containing 7% C18-TES and 93% TEOS were prepared using the same method as described in Example 1.1, except that the mixture of hydrolyzed silanes was emulsified in a mixture of xylene and cyclohexane (75% and 25%, respectively). The main characteristics of the microspheres are summarized in Figure 2 and Table 2.

[0150] Example 2-2 : in sunflower oil

[0151] Silica microspheres containing 7% C18-TES and 93% TEOS were prepared using the same method as described in Example 1.1, where the mixture of hydrolyzed silanes was emulsified in sunflower oil. The main characteristics of the microspheres are summarized in Figure 2 and Table 2. [Table 2]

[0152] Example 3 Preparation of microspheres with fully hydrolyzed and precondensed C18-TES and TEOS (molar ratio: 72% / 28%, Method A) in hexane

[0153] Typically, a 250 mL round-bottom flask was first charged with 0.12 g of 0.01N HCl and 0.55 g of ethanol, followed by the addition of 1.23 g (5.9 mmol) of TEOS. In a 30 ml vial, 0.96 g (2.3 mmol) of C18-TES was mixed with 0.14 g of 0.05N HCl and 1.3 g of THF, respectively. These two mixtures were stirred for about 1.5 hours and then combined into a 250 mL round-bottom flask. The ethanol added and produced during the hydrolysis process was slowly evaporated under reduced pressure at 40° C. to produce a dispersed phase with a viscosity of about 25 cp. Then, 3 g (38.3 mmol) of DMSO was added. To produce a water-in-oil (W / O) emulsion, 150 mL of hexane in a separate vessel was stirred at 18,000 rpm using an Ultra-Turrax homogenizer, and then the dispersed phase was added. After continuous stirring at 18,000 rpm for 5 min, 1.6 ml (11.2 mmol) of NH4OH (7N in methanol) was introduced dropwise into the emulsion under stirring as a condensation catalyst. Mixing was continued for 1 min. The resulting suspension was further aged overnight in a shaker at room temperature at a speed of 200 rpm. The product was filtered off and dried at room temperature for 3 days. The average particle size of the resulting spheres is d50=9 μm with d90 / d10=9 (Figure 3-A).

[0154] Example 4 Preparation of microspheres with fully hydrolyzed and non-precondensed C8-TES and TEOS (molar ratio: 10% / 90%, Method A) in toluene

[0155] Silica microspheres containing 10% C8-TES and 90% TEOS were prepared using the same method as described in Example 1-1. The average diameter of the obtained microspheres was 23 μm (d50), with d90 / d10=9 (FIG. 3-B).

[0156] Example 5 Preparation of microspheres with fully hydrolyzed, non-precondensed C4-TES and TEOS (molar ratio: 10% / 90%, Method A) in toluene

[0157] Silica microspheres containing 10% C4-TES and 90% TEOS were prepared using the same method as described in Example 1-1. The average diameter of the obtained microspheres is d50=70 μm and d90 / d10=8 (FIG. 3-C).

[0158] Example 6: Preparation of microspheres with DOAPS and fully hydrolyzed, non-precondensed TEOS in toluene (molar ratio: 10% / 90%, Method A)

[0159] Example 6.1 : Using fully hydrolyzed, non-precondensed DOAPS. Using the same method as described in Example 1-1, silica microspheres containing 10% DOAPS and 90% TEOS were prepared. Microspheres with an average particle size of 18 μm (d50) were obtained (FIG. 3-D), including the presence of a proportion of nanospheres of about 200 nm (d90 / d10=18). When suspended in water (pH=6), positively charged microspheres were produced with a zeta potential value of +55 mV, indicating the presence of DOAPS molecules on the outer surface of the microspheres.

[0160] Example 6.2 : Using non-hydrolyzed and non-precondensed DOAPS. Using the same method as described in Example 1-1, silica microspheres containing 10% DOAPS and 90% TEOS were prepared. Microspheres with an average particle size of 15 μm (d50) were obtained with the presence of a proportion of nanospheres of about 200 nm (d90 / d10=18) (Figure 3-E). When suspended in water (pH=6), negatively charged microspheres were produced with a zeta potential value of -20 mV. This is in accordance with the CNS results (%C) which confirm the presence of DOAPS in the resulting spheres. (CNSにより得られた) =28.5% vs. %C (理論値) =29%, and %N (CNSにより得られた) =1.3% vs. %C (理論値)= 1.5%) and the value of the hydrophobic contact angle (131°), suggest that the passive charges of DOAPS are not accessible on the outer surface of the microspheres.

[0161] Example 7 Preparation of microspheres with fully hydrolyzed, non-precondensed DMAM and TEOS (molar ratio: 10% / 90%, Method A) in toluene

[0162] Silica microspheres containing 10% DMAM and 90% TEOS were prepared using the same method as described in Example 1-1. The average particle size of the resulting microspheres was 67 μm (d50), with d90 / d10=45 (FIG. 3-F).

[0163] Example 8 Preparation of microspheres with fully hydrolyzed and non-precondensed SH-TES (mercaptopropyltriethoxysilane) and TEOS (molar ratio: 19% / 81%, method A) in toluene

[0164] Silica microspheres containing 19% SH-TES and 81% TEOS were prepared using the same method as described in Example 1-1. The average diameter of the obtained microspheres is d50=34 μm, and d90 / d10=29 (FIG. 3-G).

[0165] Example 9 Preparation of microspheres with fully hydrolyzed, non-precondensed 7-bromoheptyltrimethoxysilane (BrC7-TES) and TEOS (molar ratio: 50% / 50%, Method A) in toluene

[0166] Silica microspheres containing 50% BrC7-TES and 50% TEOS were prepared using the same method as described in Example 1-1. The average particle size of the resulting microspheres was 11 μm (d50), with d90 / d10=5 (FIG. 3-H).

[0167] Example 10 Preparation of microspheres with fully hydrolyzed and precondensed triethoxy(trifluoromethyl)silane (CF3-TES) and TEOS (molar ratio: 60% / 40%, Method A) in hexane

[0168] Silica microspheres containing 60% CF3-TES and 40% TEOS were prepared using the same method as described in Example 3. This resulted in microspheres with an average size of 40 μm (d50) and d90 / d10=4 (Figure 3-I).

[0169] Example 11 Preparation of microspheres with fully hydrolyzed and non-precondensed diPh-DES (2-(diphenylphosphino)ethyltriethoxysilane) and TEOS (molar ratio: 50% / 50%, method A) in toluene

[0170] Silica microspheres containing 50% diPh-DES and 50% TEOS were prepared using the same method as described in Example 1.1, resulting in microspheres with a mean diameter of 68 μm (d50) and d90 / d10=2 (Figure 3-J).

[0171] Example 12 Preparation of microspheres with fully hydrolyzed, non-precondensed C1-TES (100%, Method A) in toluene

[0172] Silica microspheres containing 100% C1-TES were prepared using the same method as described in Example 1-1. The average diameter of the obtained microspheres was d50=3.5 μm and d90 / d10=11 (FIG. 3-K).

[0173] Example 13 Preparation of microspheres with fully hydrolyzed, non-precondensed 100% BTES-ethane in toluene (100%, Method A)

[0174] Silica microspheres containing 100% BTES-ethane were prepared using the same method as described in Example 1-1. The average diameter of the resulting microspheres was 45 μm (d50), with d90 / 10=39 (FIG. 3-L).

[0175] Example 14 Preparation of microspheres with fully hydrolyzed and precondensed 100% BTES-ethylene in hexane (100%, Method A)

[0176] Silica microspheres containing 100% BTES-ethylene were prepared using the same method as described in Example 3. The average size of the resulting microspheres was 37 μm (d50) with d90 / d10=9 (FIG. 3-M).

[0177] Example 15 Preparation of microspheres with fully hydrolyzed, non-precondensed TEOS (100%, Method A) in toluene

[0178] Silica microspheres containing 100% TEOS were prepared using the same method as described in Example 1-1. The average diameter of the resulting microspheres was 104 μm (d50), with d90 / d10=111 (FIG. 3-N).

[0179] Example 16 Preparation of Microspheres with Fully Hydrolyzed and Precondensed TEOS (100%, Method A) in Hexane

[0180] Silica microspheres containing 100% TEOS were prepared using the same method as described in Example 3. The average particle size of the resulting microspheres was 37 μm (d50) with d90 / d10=3 (FIG. 1-O).

[0181] Example 17 Preparation of microspheres with combinations of several ormosils (.GEQ.2)

[0182] Example 17-1 : Using fully hydrolyzed, non-precondensed C8-TES, C18-TES, and TEOS (molar ratio 5% / 5% / 90%, method A) in toluene.

[0183] Silica microspheres containing 5% C8-TES, 5% C18-TES, and 90% TEOS were prepared using the same method as described in Example 1.1. The average particle size of the resulting microspheres was d50=22 μm, with d90 / d10=6 (FIG. 3-P).

[0184] Example 17-2 : Using fully hydrolyzed and precondensed TMS (trimethylsilane), C8-TES, and TEOS (molar ratio 22.5% / 7.5% / 70%, method A) in hexane.

[0185] Silica microspheres containing 22.5% TMS, 7.5% C8-TES, and 70% TEOS were prepared using the same method as described in Example 3. The average particle size of the resulting microspheres was d50=18 μm, with d90 / d10=2 (FIG. 3-Q).

[0186] Example 17-3 : Using fully hydrolyzed and precondensed C1-TES, DOAPS, and TEOS (molar ratio 22.5% / 7.5% / 70%, method A) in hexane.

[0187] Silica microspheres containing 22.5% C1-TES, 7.5% DOAPS, and 70% TEOS were prepared using the same method as described in Example 3. The average particle size of the resulting microspheres was d50=19 μm, with d90 / d10=3 (Figure 3-R).

[0188] Example 17-4 : Using fully hydrolyzed and precondensed BTES-ethylene, C1-TES, and C8-TES (molar ratio 70% / 22.5% / 7.5%, method A) in hexane.

[0189] Silica microspheres containing 22.5% C1-TES, 7.5% DOAPS, and 70% TEOS were prepared using the same method as described in Example 3. The average particle size of the resulting microspheres was d50=19 μm, with d90 / d10=3 (FIG. 3-S).

[0190] Example 18 Preparation of microspheres with fully hydrolyzed and precondensed C1-TES, C8-TES, and TEOS (molar ratio 22.5% / 7.5% / 70%, Method A) in hexane using primene as organic base

[0191] Silica microspheres containing 22.5% C1-TES, 7.5% C8-TES, and 70% TEOS were prepared using the same method as described in Example 3, except that primene was used instead of NH4OH as the condensation catalyst. The average particle size of the resulting microspheres was d50=18 μm, with d90 / d10=2 (Figure 3-T).

[0192] Example 19 Examples of physicochemical characterization of microspheres

[0193] Thermogravimetric analysis (TGA) shows the thermal decomposition of the organic groups at 180-500 °C, which confirms the presence of organic molecules corresponding to the organosilanes used.

[0194] Since XPS detects the presence of elements only at a maximum depth of a few nanometers, the analysis of the Si(2s), C(1s), O(1s), and N(1s) peaks confirms the presence of organosilane functional groups on the outer surface of the nano / microspheres. These data (Table 3) show that the longer the alkyl chain, the higher the percentage of carbon atoms (%C) and the carbon to silicon ratio (C / Si). Interestingly, using DOAPS, XPS shows the appearance of a quantifiable amount of nitrogen element (Table 3, Example 6-1). Furthermore, high-resolution analysis of the C peaks confirmed the presence of only C-C and C-H bonds (band at 285 eV) associated with the C8 alkyl functional groups of the microspheres (with 10% C8-TES) shown in Example 4.

[0195] Furthermore, by comparing the C / Si ratio obtained by XPS (analysis of the outer surface, 5 nm depth) with that obtained by elemental analysis (CNS and XRF, analysis of the whole nano / microsphere), the significantly lower C / Si ratio found by elemental analysis confirms that the alkyl chains of the used organosilanes are mainly located on the outer surface of the nano / microspheres. [Table 3]

[0196] The measured contact angles confirm the tunable hydrophobic / hydrophilic properties of the outer surface of the microspheres. Indeed, 1) a completely hydrophilic outer surface of the microspheres was obtained with 100% TEOS (Example 15) with a contact angle of less than 40° (FIG. 4-A), 2) a completely hydrophobic outer surface was obtained with C8-TES (Example 4) with a contact angle of 120-150° (FIG. 4-B), and 3) a balanced hydrophilic / hydrophobic outer surface was obtained with C4-TES (Example 5) with a contact angle of 80-90° (FIG. 4-C).

[0197] Example of nano / microspheres obtained by method B (i.e. when active substance / payload is present): Example 20 Preparation of active substance / payload containing microspheres by the method of adding active substance / payload to the dispersed phase (B1); active substance / payload entrapped in a solubilized state

[0198] Example 20-1 Preparation of D-glucose-containing microspheres with fully hydrolyzed and non-precondensed C18-TES and TEOS (molar ratio: 5% / 95%, method B)

[0199] Using the method described in Example 1.1, except that D-glucose was solubilized in the dispersed phase (B1), microspheres with a loading capacity of 33 wt. % D-glucose (Table 4) were prepared. The resulting microspheres have an average particle size of 50 μm (FIG. 5-A). After extraction of the active substance (i.e., D-glucose), the porosity data of the resulting microspheres are summarized in Table 4.

[0200] Example 20-2 Preparation of uracil-containing microspheres with fully hydrolyzed and non-precondensed C18-TES, C8-TES, and TEOS (molar ratio: 5% / 5% / 90%, Method B)

[0201] Using the method described in Example 1.1, microspheres with a loading capacity of 5 wt.% uracil (Table 4) were prepared, except that uracil was solubilized in DMSO as a water-miscible solvent and then added to the dispersed phase (B3) before the emulsification step, in which xylene was used as the continuous phase. The resulting microspheres have an average particle size of 28 μm (Figure 5-B). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 4.

[0202] Example 20-3 Preparation of uracil-containing microspheres with fully hydrolyzed and precondensed C1-TES, C8-TES, and TEOS (molar ratio: 22.5% / 7.5% / 70%, method B)

[0203] Using the method described in Example 3, microspheres with a loading capacity of 9 wt.% uracil (Table 4) were prepared, except that uracil was solubilized in the dispersed phase after precondensation and before the emulsification step (B2); here cyclohexane was used as the continuous phase. The resulting microspheres have an average particle size of 9 μm (d50) (FIG. 5-C). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 4. [Table 4]

[0204] Example 21 Preparation of microspheres containing active substances / payloads by methods of adding active substances / payloads to the dispersed phase; active substances / payloads entrapped in the solid state

[0205] Example 21-1 Preparation of 5-FU-containing microspheres with fully hydrolyzed and non-precondensed C18-TES, C8-TES, and TEOS (molar ratio: 5% / 5% / 90%, Method B)

[0206] Using the method described in Example 1.1, microspheres with a loading capacity of 20 wt% uracil (Table 5) were prepared, except that 5-FU powder was suspended in the dispersed phase (B1) and then DMSO was added (B3) before the emulsification step. Here xylene was used as the continuous phase. The resulting spheres have an average particle size of 21 μm (Figure 6-A). After extraction of the active substance (i.e. uracil), the porosity data of the resulting microspheres are summarized in Table 5.

[0207] Example 21-2 Preparation of uracil-containing microspheres with fully hydrolyzed and precondensed C1-TES, C8-TES, and TEOS (molar ratio: 22.5% / 7.5% / 70%, method B)

[0208] Using the method described in Example 3, microspheres with a loading capacity of 20 wt.% uracil (Table 5) were prepared, except that the uracil powder was suspended in dispersed phase B2 before the emulsification step; here cyclohexane was used as the continuous phase. The resulting microspheres have an average particle size of 48 μm (FIG. 6-B). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 5.

[0209] Example 21-3 Preparation of uracil-containing microspheres with fully hydrolyzed and precondensed C1-TES, C8-TES, and TEOS (molar ratio: 22.5% / 7.5% / 70%, method B) and with non-hydrolyzed and non-precondensed TMAPS

[0210] Using the method described in Example 3, microspheres (Table 5) with a loading capacity of 48 wt% uracil were prepared, except that 1) uracil powder was suspended in the dispersed phase (B2) before the emulsification step, 2) cyclohexane was used here as the continuous phase, and 3) after overnight aging of the suspension of microspheres, 10 mL of non-hydrolyzed and non-condensed TMAPS (50% in methanol) was added and the mixture was kept for another night. The average particle size of the resulting microspheres is 40 μm (Figure 6-C). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 5. When suspended in water (pH=6), positively charged microspheres were produced with a zeta potential value of +50 mV. This confirms that the TMAPS molecules are localized on the outer surface of the microspheres.

[0211] Example 21-4 Preparation of uracil-containing microspheres with fully hydrolyzed and precondensed C1-TES, C8-TES, and TEOS (molar ratio: 22.5% / 7.5% / 70%, method B) and with non-hydrolyzed and non-precondensed DOAPS

[0212] Using the method described in Example 3, microspheres (Table 5) with a loading capacity of 46 wt% uracil were prepared, except that 1) uracil powder was suspended in the dispersed phase (B2) before the emulsification step, 2) cyclohexane was used here as the continuous phase, and 3) after overnight aging of the suspension of microspheres, 11 mL of non-hydrolyzed and non-condensed DOAPS (60% in ethanol) was added and the mixture was kept for another night. The average particle size of the resulting microspheres is 35 μm (Figure 6-D). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 5. When suspended in water (pH=6), positively charged microspheres were produced with a zeta potential value of +55 mV. This confirms the presence of DOAPS molecules on the outer surface of the microspheres. [Table 5]

[0213] Example 22 Preparation of active substance / payload loaded microspheres by adding the active substance / payload to the continuous phase; active substance / payload sequestered in the solid state (B4)

[0214] Example 22-1 Preparation of uracil-loaded microspheres with fully hydrolyzed and non-precondensed C18-TES, C8-TES, and TEOS (molar ratio: 5% / 5% / 90%, Method B)

[0215] Using the method described in Example 1.1, microspheres (Table 6) with a loading capacity of 20 wt.% uracil were prepared (B4), except that the uracil powder was suspended in the continuous phase (i.e., toluene). The average size of the resulting microspheres is 23 μm (Figure 7-A). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 6.

[0216] Example 22-2Preparation of 5-FU-loaded microspheres with fully hydrolyzed and non-precondensed C18-TES and TEOS (molar ratio: 5% / 95%, Method B)

[0217] Using the method described in Example 1.1, microspheres with a loading capacity of 13 wt% 5-FU (Table 6) were prepared, except that the 5-FU powder was suspended in the continuous phase (i.e., toluene) (B4). The resulting microspheres have an average size of 14 μm (Figure 7-B). After extraction of the active substance (i.e., 5-FU), the porosity data of the resulting microspheres are summarized in Table 6.

[0218] Example 22-3 Preparation of 5-FU-loaded microspheres with fully hydrolyzed and non-precondensed DOAPS and TEOS (molar ratio: 5% / 95%, Method B)

[0219] Using the method described in Example 1.1, microspheres containing 20 wt. % 5-FU (Table 6) were prepared, except that the 5-FU powder was suspended in the continuous phase (i.e., toluene) (B4). The resulting microspheres have an average size of 14 μm (Figure 7-C). After extraction of the active substance (i.e., 5-FU), the porosity data of the resulting microspheres are summarized in Table 6. [Table 6]

[0220] Example 23 Preparation of active substance / payload loaded microspheres by adding the active substance / payload to an emulsion; the active substance / payload is sequestered in a solubilized state in a water-miscible solvent (B3)

[0221] Example 23-1 Preparation of uracil-loaded microspheres with fully hydrolyzed and non-precondensed C18-TES, C8-TES, and TEOS (molar ratio: 5% / 5% / 90%, Method B)

[0222] Using the method described in Example 1.1, microspheres with a loading capacity of 5 wt.% uracil (Table 7) were prepared, except that uracil was solubilized in DMSO and added to the emulsion after the emulsification step and before the addition of the condensation catalyst (B3); here xylene was used as the continuous phase. The average particle size of the resulting microspheres is 16 μm (Figure 8-A). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 7.

[0223] Example 23-2 Preparation of uracil-loaded microspheres with fully hydrolyzed and non-precondensed DOAPS and TEOS (molar ratio: 3% / 97%, Method B)

[0224] Using the method described in Example 1.1, microspheres with a loading capacity of 5 wt.% uracil (Table 7) were prepared, except that uracil was solubilized in DMSO and added to the emulsion after the emulsification step and before the addition of the condensation catalyst (B3); here xylene was used as the continuous phase. The average particle size of the resulting microspheres is 7 μm (Figure 8-B). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 7. [Table 7]

[0225] Example 24 Preparation of active substance / payload loaded microspheres by adding the active substance / payload to an emulsion; the active substance / payload is sequestered in a solubilized state in the condensation catalyst (B5)

[0226] Example 24-1 Preparation of uracil-loaded microspheres with fully hydrolyzed and precondensed C1-TES, C8-TES, and TEOS (molar ratio: 22.5% / 7.5% / 70%, Method B)

[0227] Microspheres with a loading capacity of 1 wt% uracil were prepared using the method described in Example 3, except that uracil was solubilized in the condensation catalyst used (i.e., NaOH was used here); here cyclohexane was used as the continuous phase (B5). The average particle size of the resulting microspheres is 9 μm (Figure 9-A).

[0228] Example 24-2 Preparation of uracil-loaded microspheres with fully hydrolyzed and non-precondensed C4-TES and TEOS (molar ratio: 35% / 65%, Method B)

[0229] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 4 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 34 μm (Figure 9-B). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8.

[0230] Example 24-3 Preparation of uracil-loaded microspheres with fully hydrolyzed and non-precondensed C8-TES and TEOS (molar ratio: 10% / 90%, Method B)

[0231] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 4 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 14 μm (Figure 9-C). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8.

[0232] Example 24-4 Preparation of uracil-containing microspheres with fully hydrolyzed and non-precondensed C18-TES, C8-TES, and TEOS (molar ratio: 5% / 5% / 90%, Method B)

[0233] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 2 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 21 μm (Figure 9-D). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8.

[0234] Example 24-5 Preparation of uracil-containing microspheres with fully hydrolyzed and non-precondensed C18-TES, C8-TES, and TEOS (molar ratio: 10% / 10% / 90%, Method B)

[0235] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 2 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 21 μm (Figure 9-E). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8.

[0236] Example 24-6 Preparation of uracil-containing microspheres with fully hydrolyzed and non-precondensed DOAPS and TEOS (molar ratio: 3% / 97%, method B)

[0237] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 2 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 5 μm (Figure 9-F). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8. When suspended in water (pH=6), positively charged microspheres were produced with a zeta potential value of +55 mV, indicating the presence of DOAPS molecules on the outer surface of the microspheres.

[0238] Example 24-7 Preparation of uracil-containing microspheres with fully hydrolyzed and non-precondensed DOAPS, C8-TES, and TEOS (molar ratio: 3% / 5% / 93%, Method B)

[0239] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 2 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 12 μm (Figure 9-G). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8. When suspended in water (pH=6), positively charged microspheres were produced with a zeta potential value of +10 mV, indicating the presence of DOAPS molecules on the outer surface of the microspheres.

[0240] Example 24-8 Preparation of uracil-containing microspheres with fully hydrolyzed and non-precondensed DOAPS, C18-TES, and TEOS (molar ratio: 3% / 5% / 93%, Method B)

[0241] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 2 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where NH4OH was added) (B5). The average particle size of the resulting microspheres is 18 μm (Figure 9-H). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8. When suspended in water (pH=6), positively charged microspheres were produced with a zeta potential value of +29 mV, indicating the presence of DOAPS molecules on the outer surface of the microspheres.

[0242] Example 24-9Preparation of 5-FU-containing microspheres with fully hydrolyzed and non-precondensed C18-TES and TEOS (molar ratio: 5% / 95%, method B)

[0243] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 7 wt.% 5-FU were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where hot NH4OH was added) (B5). The average particle size of the resulting microspheres is 15 μm (Figure 9-I). After extraction of the active substance (i.e., 5-FU), the porosity data of the resulting microspheres are summarized in Table 8.

[0244] Example 24-10 : Preparation of uracil-containing microspheres with 100% TEOS that is fully hydrolyzed and not precondensed (Method B)

[0245] Using the method described in Example 1.1, microspheres (Table 8) with a loading capacity of 5 wt.% uracil were prepared, except that uracil was solubilized in the condensation catalyst solution (i.e., where hot NH4OH was added) (B5). The average particle size of the resulting microspheres is 27 μm (Figure 9-J). After extraction of the active substance (i.e., uracil), the porosity data of the resulting microspheres are summarized in Table 8.

[0246] The porosity data of the microspheres initially containing the active substance / payload are always higher than the porosity data of the corresponding microspheres in the absence of the active substance / payload. [Table 8]

[0247] Example 25 Preparation of active / payload loaded microspheres by combining two or more active / payload loading strategies: for example, adding solubilized active / payload to both the dispersed phase and the condensation catalyst solution

[0248] Preparation of uracil-loaded microspheres with fully hydrolyzed and pre-condensed C1-TES, C8-TES, and TEOS (molar ratio: 22.5% / 7.5% / 70%, Method B). Using the method described in Example 3, microspheres with a loading capacity of 10 wt. % uracil were prepared, except that 1) uracil was solubilized in the dispersed phase (B2) and 2) uracil was also solubilized in the condensation catalyst solution (i.e., NH4OH) (B5); here, cyclohexane was used as the continuous phase. The textural and structural properties of the resulting microspheres are summarized in Figure 9-K and Table 9. [Table 9]

[0249] Example 26 Examples of controlled release performance achieved with the resulting microspheres

[0250] Control of active agent / payload release can be achieved in function of the hydrophobicity / hydrophilicity of the matrix and the outer surface, as shown in FIG.

[0251] The interaction of the payload / active substance with the surface has a significant impact on the kinetic release. The external surface of the spheres can act as a diffusion barrier, which has a major impact on the active substance release rate. The barrier can be the result of repulsive action from the outer layer (hydrophilic / hydrophobic repulsion in this case) or / and steric confinement (long-chain organosilanes in this case). The more hydrophobic groups in the matrix, the slower the release. It has been demonstrated that after 1 h, depending on the composition of the matrix, 5-80% of the initial amount of active substance / payload present in the microspheres has been released. Similar results have been obtained for loadings of various active substance contents. The choice of organosilanes for the microsphere matrix is ​​therefore very important to tune the release kinetics of the active substance / payload.

[0252] Sample characterization Specific surface area (BET) and porosity: The surface area and porosity of the silica microspheres are characterized using Micrometrics TriStar™ 3000 V4.01 and Micrometrics TriStar™ 3020 V3.02 at 77 K. The collected data uses standard Brunauer-Emmett-Teller (BET) to obtain the surface area, and the pore size is obtained from the maximum of the pore size distribution curve calculated by the Barrett-Joyner-Halenda (BJH) method using the adsorption branch of the isotherm.

[0253] Particle size distribution: To measure particle size distribution, silica nano / microspheres (~50 mg) were dispersed in ~5 mL of methanol in an ultrasonic bath for 5 min to obtain a well-dispersed solution, which was then added to the sonication bath of a Malvern Mastersizer 2000 (Hydro 2000S, model AWA2001) until the signal interference was ~5-8%.

[0254] Quantification of active substance in silica spheres: The loading of active substance sequestered in silica spheres is measured by suspending a certain amount of sequestered silica spheres containing approximately 100 mg of active substance in 10 mL of 10% aqueous ammonia solution, then sonicating for 30 min in a Branson 8800 ultrasonic bath, followed by shaking for 2 h at 200 mot / min using an IKA HS-501 horizontal shaker to achieve complete release. Filtering the silica spheres through a 0.22 μm filter gives a clear solution for HPLC analysis.

[0255] The HPLC used to measure the concentration of active substances in the above obtained solution is an Agilent 1100 equipped with a quaternary solvent delivery system (G1311A), a vacuum degassing unit (G1322A), a UV photodiode array detector (G1314A), a standard autosampler (G1313A), and a thermostat column compartment (G1316A). A 3 x 150 mm ID, 5 μm, 100 Å SiliaChrom DtC18 column is used to detect the active substances. 0.1% formic acid with water is used as the mobile phase MPA, and 0.1% formic acid with acetonitrile is used as the mobile phase MPB. The injection volume is 2 μL. The starting mobile phase is 95% MPA and 5% MPB, ending with 95% MPB in 4 min and held for another 2 min. The flow rate, column temperature, and detector are set at 0.5 ml / min, 23 °C, and 260 nm, respectively. The uracil retention time is 1.88 min and the 5-FU retention time is 2.39 min. A calibration curve is generated using pure compounds purchased from Sigma Aldrich.

[0256] Scanning Electron Microscopy (SEM): SEM images of the microspheres were recorded on an FEI Quanta-3D-FEG at 3.0 kV without coating or a JEOL 840-A at 15 kV with gold coating.

[0257] Water determination in silica (Karl Fischer): The proportion of water is estimated using a titrator Compact V20s from Mettler Toledo.

[0258] Zeta Potential: To measure the zeta potential of nano / microspheres, a suspension is first prepared by dispersing 10 mg of nano / microspheres in 10 mL of water, followed by sonication for 10 min and vortex mixing for 1 min. The mixture is further diluted 10 times and placed in a Capillary Zeta Cell to measure the zeta potential using a Malvern, Zetasizer Nano ZS.

[0259] Contact angle: A few milligrams of nano / microspheres are deposited on one side of Micro-Tec D12 double-sided non-conductive adhesive and fixed to a microscope slide. The sample layer is smoothed as much as possible. The contact angle is then characterized using a VCA 2500 XE system.

[0260] Elemental Analysis (CNS and ICP-ES): Carbon, nitrogen, and sulfur content are measured using a Perkin Elmer 2400 Series II CHNS / O analyzer. Silicon content is measured using ICP-ES.

[0261] X-ray Photoelectron Spectroscopy (XPS): The chemical composition of the external surface was investigated by X-ray Photoelectron Spectroscopy using an Axis-Ultra de Kratos (UK) to a maximum depth of 5 nm. The main XPS chamber had a resolution of <5.10 -8 A base pressure of 1000 Torr was maintained. A 250 W monochromatic aluminum X-ray source (Al kα = 1486.6 eV) was used to record survey spectra (1400–0 eV) and high-resolution spectra with charge neutralization. The detection angle was set at 45° to the surface normal and the analyzed area was 0.016 cm 2 (Opening 5).

[0262] Thermogravimetry-Differential Scanning Calorimetry (TGA-DSC): Measurements were performed using a Netzsch STA 449C thermogravimetry analyzer at an airflow rate of 20 mL / min and a heating rate of 10 °C / min from 35 to 700 °C. Some embodiments of the present invention are described in the following items [1]-

[18] . [1] A method for producing organosiloxane nano / microspheres, comprising the steps of: i0) separately hydrolyzing one or more silica precursors in a hydrolysis medium to provide one or more pre-hydrolyzed silica precursors; i1) combining the pre-hydrolyzed silica precursors of step i0) to provide a dispersed phase comprising the combined pre-hydrolyzed silica precursors; i2) removing some or all of the volatile solvent from the combined pre-hydrolyzed silica precursor to provide a dispersed phase comprising a pre-condensed silica precursor; i3) preparing a dispersed phase comprising a hydrophilic solvent by adding a hydrophilic solvent to said dispersed phase comprising the combined pre-hydrolyzed silica precursors obtained in step i1) or by adding a hydrophilic solvent to said dispersed phase comprising the pre-condensed silica precursors obtained in step i2); i4) emulsifying the dispersed phase of step i1), i2), or i3) in the absence of a surfactant in a continuous phase to provide a water-in-oil emulsion; i5) adding a condensation catalyst to the emulsion of step i4) to provide said organosiloxane nano / microspheres. [2] The silica precursor has the formula R 4-x Si(L) x Or formula (L) 3 Si-R'-Si(L) 3 2. The method according to claim 1, wherein R is a monosilylated residue as an alkyl, alkenyl, alkynyl, alicyclic, aryl, alkylaryl group, which may be a halogen atom, glycidyloxy-, -OH, -SH, polyethylene glycol (PEG), -N(R a ) 2 、-N + (R a ) 3 optionally replaced by; L is halogen or acetoxide -OC(O)R a , or alkoxide OR a It is a base; R' is a disilyl residue as an alkyl, alkenyl, alkynyl, cycloaliphatic, aryl, alkylaryl group, which is a halogen atom, -OH, -SH, -N(R a ) 2 、-N + (R a ) 3 optionally replaced by; R a can be hydrogen, alkyl, alkenyl, alkynyl, alicyclic, aryl, and alkylaryl; and The above method, wherein X is an integer of 1 to 4, or X is an integer of 1 to 3. [3] 2. The method according to claim 1, wherein an active agent / payload insoluble in the continuous phase is added in step (i1) to the combined pre-hydrolyzed silica precursor. [4] 2. The method according to claim 1, wherein an active substance / payload insoluble in the continuous phase is added to the pre-condensed silica precursor in step (i2). [5] 2. The method according to claim 1, wherein an active substance / payload insoluble in the continuous phase is added to the dispersed phase in step (i3). [6] 2. The method according to claim 1, wherein an active substance / payload that is insoluble in the continuous phase is added to the continuous phase in step (i4). [7] 2. The method according to claim 1, wherein an active substance / payload insoluble in the continuous phase is added to the emulsion in step (i4). [8] 2. The method according to claim 1, wherein an active substance / payload insoluble in the continuous phase is added to the condensation catalyst in step (i5). [9] 9. The method according to any of items 3 to 8, wherein the active substance / payload that is insoluble in the continuous phase is a hydrophilic molecule in a liquid state.

[10] 9. The method according to any of items 3 to 8, wherein the active agent / payload that is insoluble in the continuous phase is a hydrophilic molecule in the solid state.

[11] 11. The method according to any of items 3 to 10, wherein the active substance / payload that is insoluble in the continuous phase is a cosmetic, cosmeceutical, or pharmaceutical compound.

[12] 11. The method according to any of items 3 to 10, wherein the active agent / payload that is insoluble in the continuous phase is 5-fluorouracil.

[13] 11. The method according to any of items 3 to 10, wherein the active substance / payload that is insoluble in the continuous phase is a sugar or derivative.

[14] Organosiloxane spherical nano / microspheres comprising a network of organosiloxane, which are non-calcined, amorphous, surfactant-free, submicron to micron sized particles, optionally containing an active agent / payload.

[15] are submicron to micron sized; N 2 is porous as assessed by pore volume, pore diameter, and specific surface area measured by physical adsorption; 15. The organosiloxane spherical nano / microsphere according to item 14, wherein the external surface hydrophobic / hydrophilic properties evaluated by contact angle measurement are hydrophilic if the contact angle is less than 90°, hydrophobic if the contact angle is greater than 90°, or balanced hydrophobic if the contact angle is between 85° and 95°.

[16] 14. An organosiloxane spherical nano / microsphere prepared by the method according to any one of items 1 to 13.

[17] 17. A method for in situ sequestration of an active agent / payload throughout the nano / microspheres according to items 14, 15 or 16, comprising incorporating said active agent / payload into said nano / microspheres by the method according to any of items 3 to 13.

[18] 17. A method for modulating the release of an active agent / payload comprising incorporating said active agent / payload into nano / microspheres according to item 14, 15 or 16, or incorporating said active agent / payload by the method according to any of items 1 to 13.

Claims

1. A method for producing organosiloxane nano / microspheres comprising the steps of: i0) separately hydrolyzing one or more silica precursors in a hydrolysis medium to provide one or more pre-hydrolyzed silica precursors; i1) combining the pre-hydrolyzed silica precursors of step i0) to provide a dispersed phase comprising the combined pre-hydrolyzed silica precursors; i2) removing some or all of the volatile solvent from the combined pre-hydrolyzed silica precursor to provide a dispersed phase comprising a pre-condensed silica precursor; i3) preparing a dispersed phase comprising a hydrophilic solvent by adding a hydrophilic solvent to said dispersed phase comprising the combined pre-hydrolyzed silica precursors obtained in step i1) or by adding a hydrophilic solvent to said dispersed phase comprising the pre-condensed silica precursors obtained in step i2); i4) emulsifying the dispersed phase of step i1), i2), or i3) in the absence of a surfactant in a continuous phase to provide a water-in-oil emulsion; i5) adding a condensation catalyst to the emulsion of step i4) to provide said organosiloxane nano / microspheres.

2. The silica precursor has the formula R 4-x Si(L) x Or formula (L) 3 Si-R'-Si(L) 3 2. The method of claim 1, comprising: R is a monosilylated residue as an alkyl, alkenyl, alkynyl, cycloaliphatic, aryl, alkylaryl group, which is selected from the group consisting of halogen atoms, glycidyloxy-, -OH, -SH, polyethylene glycol (PEG), -N(R a ) 2 , -N + (R a ) 3 optionally substituted by; L is a halogen or acetoxide -O-C(O)R a , or alkoxide OR a is a group; R' is a disilylated residue as an alkyl, alkenyl, alkynyl, cycloaliphatic, aryl, alkylaryl group, which is a halogen atom, -OH, -SH, -N(R a ) 2 , -N + (R a ) 3 optionally substituted by; R a can be hydrogen, alkyl, alkenyl, alkynyl, cycloaliphatic, aryl, and alkylaryl; and The above method, wherein X is an integer from 1 to 4, or X is an integer from 1 to 3.

3. 2. The method of claim 1, wherein an active agent / payload insoluble in the continuous phase is added to the combined pre-hydrolyzed silica precursor in step (i1).

4. 2. The method of claim 1, wherein an active substance / payload insoluble in the continuous phase is added to the pre-condensed silica precursor in step (i2).

5. 2. The method of claim 1, wherein an active agent / payload that is insoluble in the continuous phase is added to the dispersed phase in step (i3).

6. 2. The method of claim 1, wherein an active agent / payload that is insoluble in the continuous phase is added to the continuous phase in step (i4).

7. 2. The method of claim 1, wherein an active agent / payload that is insoluble in the continuous phase is added to the emulsion in step (i4).

8. 2. The method of claim 1, wherein an active substance / payload insoluble in the continuous phase is added to the condensation catalyst in step (i5).

9. The method according to any one of claims 3 to 8, wherein the active agent / payload that is insoluble in the continuous phase is a hydrophilic molecule in the liquid state.

10. The method of any one of claims 3 to 8, wherein the active agent / payload that is insoluble in the continuous phase is a hydrophilic molecule in the solid state.

11. The method according to any one of claims 3 to 10, wherein the active / payload that is insoluble in the continuous phase is a cosmetic, cosmeceutical or pharmaceutical compound.

12. The method of any one of claims 3 to 10, wherein the active agent / payload that is insoluble in the continuous phase is 5-fluorouracil.

13. The method according to any one of claims 3 to 10, wherein the active substance / payload that is insoluble in the continuous phase is a sugar or derivative.

14. A method for in situ sequestration of an active agent / payload throughout organosiloxane spherical nano / microspheres comprising a network of organosiloxane that are non-calcined, amorphous, surfactant-free, submicron to micron sized particles, comprising incorporating said active agent / payload into said nano / microspheres by a method according to any one of claims 3 to 13.

15. A method for modulating the release of an active agent / payload comprising incorporating the active agent / payload by a method according to any one of claims 3 to 13.

Citation Information

Patent Citations

  • Encapsulated microcapsule and its production

    JP2000225332A

  • Cosmetic formulated with filled fine microcapsule

    JP2001106612A

  • Method for producing silica nanoparticles of core-shell structure, silica nanoparticles of core-shell structure and labeling reagent using the same

    JP2009196829A

  • Synthesis and use of organosilica particles

    US20030124564A1