Bond flux for submerged arc welding

The optimized bond flux composition for submerged arc welding addresses issues of low-temperature toughness and welding workability by improving slag removability and arc stability, resulting in high-quality welds with low hydrogen content and reduced defects.

JP7566660B2Active Publication Date: 2024-10-15NIPPON STEEL WELDING & ENGINEERING CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021025040
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-27
Filing Date
2021-02-19
Publication Date
2024-10-15
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Existing submerged arc welding technologies for high-strength steel face challenges in achieving stable low-temperature toughness, high welding workability, and low diffusible hydrogen content, often resulting in weld defects and unstable arcs.

Method used

A bond flux composition comprising specific percentages of SiO2, CaO, MgO, Al2O3, CaF2, metal carbonates, Si, Al, Na2O, K2O, and Mn, optimized to enhance slag removability, arc stability, and reduce diffusible hydrogen, ensuring stable low-temperature toughness and high tensile strength.

Benefits of technology

The bond flux achieves good welding workability, low diffusible hydrogen content, and defect-free welds with stable low-temperature toughness, enhancing the quality and efficiency of weld metal production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566660000001
    Figure 0007566660000001
  • Figure 0007566660000002
    Figure 0007566660000002
  • Figure 0007566660000003
    Figure 0007566660000003
Patent Text Reader

Abstract

To provide a bond flux for submerged arc welding, favorable in welding workability, low in diffusible hydrogen content of weld metal, causing no weld defect and capable of obtaining the weld metal having stable low-temperature toughness.SOLUTION: A bond flux for submerged arc welding is characterized by including in mass% based on total flux mass, 5-20% of SiO2, 5-20% of CaO, 25-35% of MgO, 5-20% of Al2O3, 20-30% of CaF2, 2.0-8.0% of total of CO2 conversion value of one or more metal carbonates, 0.3-1.0% of Si, 0.1-0.8% of Al, 0.2-0.8% of Mn, and 1.0-4.5% of one or total of Na2O and K2O.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bonded flux for submerged arc welding of 780 MPa class high tensile steel, which provides stable low-temperature toughness of the weld metal, a low amount of diffusible hydrogen in the weld metal, no welding defects, and good welding workability. [Background technology]

[0002] Submerged arc welding is highly efficient and produces weld metal with good welding workability and excellent mechanical properties, and is therefore used in a wide range of fields, such as shipbuilding, steel frame construction, pipe construction, bridges, and vehicles.

[0003] In recent years, with the development of the energy industry, the strength and toughness of steel materials, and the thickness of plates to be increased due to the enlargement of structures, are being considered, and the application rate of submerged arc welding is increasing year by year from the viewpoint of quality and productivity. In the submerged arc welding of such high tensile steel, further quality improvement is required to improve productivity in welding work and ensure safety and durability. In order to satisfy such demands, it is necessary to have strength and low-temperature toughness of the weld metal that matches the steel characteristics, reduce the amount of diffusible hydrogen in the weld metal to prevent low-temperature cracking, and have good welding workability. In the submerged arc welding of high tensile steel, bond fluxes that can freely adjust the chemical composition of the weld metal are applied to ensure the strength and toughness of the weld metal that matches the steel, and various technical developments have been carried out in the past.

[0004] For example, Patent Document 1 discloses a sinterable flux and wire for submerged arc welding that optimizes the composition of the sinterable flux to obtain a weld metal with excellent low-temperature toughness, with a tensile strength of 780 MPa or more and an absorbed energy of 3.5 kgf m or more at -80°C. However, the sinterable flux described in Patent Document 1 had high diffusible hydrogen in the weld metal, resulting in poor resistance to low-temperature cracking. In addition, since it does not contain an arc stabilizer, the arc is unstable and welding workability is also poor.

[0005] Also, Patent Document 2 discloses a sinterable flux and wire for submerged arc welding that, by optimizing the composition of the sinterable flux and the composition of the wire, can obtain a weld metal having excellent low-temperature toughness, with a tensile strength of 780 MPa or more and an absorbed energy of 69 J or more at -60°C. However, the sinterable flux described in Patent Document 2 contains metallic Ca, which causes an unstable arc and a poor bead shape.

[0006] Furthermore, Patent Document 3 discloses a weld metal for multi-layer welding by submerged arc welding, which is obtained by combining a solid wire and a flux, and which has a high strength and stable toughness of the weld metal by optimizing the composition of the weld metal, and is free of welding defects and has good welding workability. However, the flux described in Patent Document 3 has a problem that stable low-temperature toughness cannot be obtained because it contains a small amount of CaF2. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 3-52796 [Patent Document 2] JP 2013-39604 A [Patent Document 3] JP 2007-260696 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a bonded flux for submerged arc welding which has good welding workability, a low amount of diffusible hydrogen in the weld metal, is free of welding defects, and can provide a weld metal with stable low-temperature toughness when performing submerged arc welding of 780 MPa class high tensile steel. [Means for solving the problem]

[0009] The gist of the present invention is a bonded flux for submerged arc welding, which is characterized by containing, in mass % relative to the total mass of the flux, 5-20% SiO2, 5-20% CaO, 25-35% MgO, 5-20% Al2O3, 20-30% CaF2, 2.0-8.0% total of one or more metal carbonates in terms of CO2, 0.3-1.0%, 0.1-0.8% Al, 1.0-4.5% total of one or two of Na2O and K2O, with the remainder being Fe from the iron alloy and impurities.

[0010] The impurities are preferably contained in an amount of 2.0% or less by mass relative to the total mass of the flux.

[0011] The present invention also provides a bonded flux for submerged arc welding, further comprising, in mass % relative to the total mass of the flux, 0.8% or less of Mn as a substitute for a portion of the components. Effect of the Invention

[0012] The bonded flux for submerged arc welding to which the present invention is applied makes it possible to provide high-quality weld metal with high efficiency, such as excellent welding workability, a low amount of diffusible hydrogen in the weld metal, no welding defects, and weld metal with stable low-temperature toughness in submerged arc welding of 780 MPa class high-tensile steel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventors have carried out extensive investigations into the component composition of a bond flux for submerged arc welding that provides good welding workability, a low amount of diffusible hydrogen in the weld metal, no welding defects, and a weld metal with stable low-temperature toughness when performing submerged arc welding of 780 MPa class high tensile steel.

[0014] As a result, it was found that by increasing the basicity of the slag by adding appropriate amounts of CaO, MgO, and CaF2 in the flux, and by adding appropriate amounts of the deoxidizing elements Si and Al, the strength and oxygen content of the weld metal can be optimized, resulting in stable low-temperature toughness. It was also found that the amount of diffusible hydrogen can be reduced by adjusting the amounts of metal carbonate, Na2O, and K2O.

[0015] Furthermore, it was found that the slag removability and bead shape are improved by adding appropriate amounts of SiO2 and Al2O3, and the arc stability is improved by adding appropriate amounts of Na2O, K2O and Al2O3.

[0016] They also found that the tensile strength of the weld metal can be further improved by adding an appropriate amount of Mn.

[0017] The reasons for limiting the composition of the bonded flux for submerged arc welding according to the present invention will be described below. The components are expressed in mass% relative to the total mass of the bonded flux, and when expressing the mass%, they are simply expressed as %.

[0018] [SiO2: 5-20%] SiO2 acts as a slag former and is an important component for obtaining good slag removability and bead shape. If SiO2 is less than 5%, this effect cannot be obtained, resulting in poor slag removability and bead shape. On the other hand, if SiO2 exceeds 20%, the amount of oxygen in the weld metal increases and toughness decreases. Therefore, SiO2 is set to 5-20%. For example, silica sand, water glass, etc. can be used as raw materials for SiO2.

[0019] [CaO: 5-20%] CaO has the effect of increasing the basicity of the slag and reducing the oxygen content of the weld metal. If the CaO content is less than 5%, this effect is not obtained and the toughness of the weld metal decreases. On the other hand, if the CaO content exceeds 20%, the basicity of the slag increases, the arc becomes unstable, and the bead shape and slag removability become poor. Therefore, the CaO content is set to 5 to 20%. CaO includes the CaO content of CaCO3. For example, wollastonite can be used as a raw material for CaO.

[0020] [MgO: 25~35%] MgO, which is made from magnesia clinker or the like, has the effect of increasing the basicity of the slag and reducing the amount of oxygen in the weld metal. If the MgO content is less than 25%, this effect is not obtained and the toughness of the weld metal decreases. On the other hand, if the MgO content exceeds 35%, the melting point of the slag increases and the slag removability becomes poor. In addition, welding defects such as slag inclusion tend to occur. Therefore, the MgO content is set to 25 to 35%. Also, MgO contains the MgO content of MgCO3. For example, magnesia clinker or the like can be used as a raw material for MgO.

[0021] [Al2O3: 5-20%] Al2O3 acts as a slag former and is an important component for obtaining good slag removability and bead shape. Al2O3 also has the effect of increasing arc stability. If Al2O3 is less than 5%, the arc becomes unstable, resulting in poor slag removability and poor bead shape. From the viewpoint of such welding workability, it is necessary to add Al2O3 in an amount of 5% or more, and more preferably, 8% or more. On the other hand, if Al2O3 exceeds 20%, the melting point of the slag becomes high and the slag removability becomes poor. Furthermore, if Al2O3 exceeds 20%, welding defects such as slag inclusion are likely to occur. For this reason, Al2O3 must be 20% or less, and more preferably, 18% or less. Therefore, Al2O3 is set to 5 to 20%. Note that, for example, alumina can be used as a raw material for Al2O3.

[0022] [CaF2: 20~30%] CaF2 has the effect of increasing the basicity of the slag and reducing the amount of oxygen in the weld metal, but because it has a low melting point, if there is too much, pockmarks are likely to occur. If the CaF2 content is less than 20%, this effect cannot be obtained and the toughness of the weld metal decreases. On the other hand, if the CaF2 content exceeds 30%, the arc becomes unstable, and the bead shape and slag removability become poor. Furthermore, if the CaF2 content exceeds 30%, pockmarks are likely to occur. Therefore, the CaF2 content is set to 20 to 30%. Note that fluorite, for example, can be used as a raw material for CaF2.

[0023] [Total of CO2 equivalent value of one or more metal carbonates: 2.0-8.0%] Metal carbonates have the effect of lowering the partial pressure of water vapor in the arc atmosphere by CO or CO2 gas generated by decomposition during welding, and lowering the amount of diffusible hydrogen in the weld metal. If the total of the CO2 equivalent values ​​of one or more metal carbonates is less than 2.0%, the amount of diffusible hydrogen in the weld metal increases, and the low-temperature cracking susceptibility increases. On the other hand, if the total of the CO2 equivalent values ​​of one or more metal carbonates exceeds 8.0%, the amount of oxygen in the weld metal increases, and the toughness deteriorates. If the total of the CO2 equivalent values ​​of one or more metal carbonates exceeds 8.0%, pockmarks are likely to occur on the bead surface. Therefore, the total of the CO2 equivalent values ​​of one or more metal carbonates is 2.0 to 8.0%. For example, CaCO3, MgCO3, Li2CO3, etc. can be used as the metal carbonate, and the CO2 equivalent value is the total amount of CO2 contained therein.

[0024] [Si: 0.3-1.0%] Silicon is a deoxidizing element and reduces the amount of oxygen in the weld metal. If the silicon content is less than 0.3%, the deoxidizing effect is not obtained, and the strength and toughness of the weld metal are reduced. On the other hand, if the silicon content exceeds 1.0%, the yield toughness of the weld metal is excessively deteriorated. Therefore, the silicon content is set to 0.3 to 1.0%. For example, metal silicon, Fe-Si, Fe-Si-Mn, etc. can be used as the raw material for silicon.

[0025] [Al: 0.1-0.8%] Al acts as a deoxidizer, similar to Si, to reduce the amount of oxygen in the weld metal. If Al is less than 0.1%, the deoxidizing effect is not obtained, and the strength and toughness of the weld metal are reduced. On the other hand, if Al exceeds 0.8%, the yield toughness in the weld metal is excessively deteriorated. Therefore, Al is set to 0.1 to 0.8%. For example, metallic Al, Fe-Al, etc. can be used as the raw material for Al.

[0026] [Total of one or both of Na2O and K2O: 1.0-4.5%] Na2O and K2O have the effect of stabilizing the arc. If the total of one or two of Na2O and K2O is less than 1.0%, the arc becomes unstable. On the other hand, if the total of one or two of Na2O and K2O exceeds 4.5%, undercut is likely to occur and the bead shape becomes poor. If the total of one or two of Na2O and K2O exceeds 4.5%, the amount of diffusible hydrogen in the weld metal also increases. Therefore, the total of one or two of Na2O and K2O is set to 1.0 to 4.5%. For example, water glass (sodium silicate, potassium silicate) can be used as the main raw material for Na2O and K2O.

[0027] [Mn:0.8% or less] Mn, which is made from raw materials such as metallic Mn, Fe-Mn, and Fe-Si-Mn, does not need to be added. When added, Mn has the effect of improving the strength of the weld metal, so it should be added according to the required strength. In order to achieve this effect, it is preferable to add 0.2% or more of Mn. On the other hand, if the Mn content exceeds 0.8%, the strength of the weld metal becomes excessively high and the toughness decreases. Therefore, the Mn content is set to 0.8% or less. For example, metallic Mn, Fe-Mn, and Fe-Si-Mn can be used as raw materials for Mn.

[0028] The balance of the bond flux other than the above components is Fe from iron alloys such as Fe-Si, Fe-Al, Fe-Mn, Fe-Si-Mn, etc., and impurities. The higher the strength, the lower the total amount of the balance is, and it is preferable to adjust it to 2.0% or less.

[0029] The impurities include MnO, FeO, B2O3, C, P, S, etc. Among these, P and S both form compounds with low melting points and reduce the toughness of the weld metal, so it is preferable that the contents are as low as possible. EXAMPLES

[0030] The effects of the present invention will now be described in more detail with reference to examples.

[0031] Bond fluxes with various compositions shown in Table 1 were prototyped and combined with the three types of solid wires shown in Table 2, and a 25 mm thick 780 MPa class steel plate with the chemical compositions shown in Table 3 was machined into a groove shape with a groove angle of 30° and root spacing of 13 mm, and a backing metal was applied to carry out a multi-pass welding test under the welding conditions shown in Table 4. In addition, the amount of diffusible hydrogen in the weld metal was measured using a combination of the bond fluxes in Table 1 and the solid wires shown in Table 2.

[0032] The bond flux shown in Table 1 was made by compounding and mixing various mineral raw materials, granulating them with water glass as a binder, and then sintering them at 450 to 500°C for two hours to granulate them to 0.15 x 1.4 mm. The solid wires shown in Table 2 were made by reducing, annealing, and plating the original wires to make strands, which were then drawn to 4.0 mm.

[0033] [Table 1]

[0034] [Table 2]

[0035] [Table 3]

[0036] [Table 4]

[0037] The mechanical performance of the weld metal was evaluated by taking tensile test pieces and impact test pieces in accordance with AWS.5.23 and conducting mechanical tests. In the tensile test, a tensile strength of 760 to 860 MPa was considered good. In the impact test, a Charpy impact test was performed at -40°C, and an average absorbed energy of 80 J or more was considered good for three repeated tests. The amount of diffusible hydrogen in the weld metal was measured in accordance with JIS Z3118. A diffusible hydrogen amount of 5 ml / 100 g or less in the weld metal was considered good. The welding workability was evaluated by examining the arc stability, slag removability, and bead appearance and shape during multi-layer welding except for the first layer, and then examining the presence or absence of welding defects using an X-ray transmission test. The results of these investigations are summarized in Table 5.

[0038] Arc stability was considered good if the welding voltage fluctuation during welding was within ±5V.

[0039] As the slag peels off naturally after welding, it was removed with a brush and the area of ​​the remaining slag that could be visually confirmed was estimated. A slag peeling rate of 98% or more was considered good.

[0040] Bead appearance and shape: The bead width was measured at 10 points from the sound part of the weld bead, and a difference between the minimum and maximum values ​​was 8 mm or less, making it good. Bead appearance was good if it was uniform with no partial discoloration.

[0041] In the X-ray transmission test, the test was performed based on the radiographic test method for steel welded joints shown in JIS Z 3104:1995, and when no flaws were found, the specimen was deemed to be defect-free.

[0042] [Table 5]

[0043] In Tables 1 and 5, flux symbols F1 to F12, F14 to F15, and F26 to F35 are examples of the present invention, and flux symbols F16 to F20 and F36 to F45 are comparative examples. The flux symbols F1 to F12, F14 to F15, and F26 to F35, which are examples of the present invention, have appropriate amounts of SiO2, CaO, MgO, Al2O3, CaF2, the total of one or more of the CO2 equivalent values ​​of metal carbonates, and the total of one or two of Si, Al, Na2O, and K2O, so that good tensile strength and absorbed energy of the weld metal are obtained, the amount of diffusible hydrogen in the weld metal is low, the arc is stable, and the slag removability and bead appearance and shape are good, resulting in extremely satisfactory results.

[0044] In addition, the flux codes F26, F29, and F35 had a large amount of residual, so the absorbed energy of the weld metal tended to be slightly lower, but was within the target range. In addition, the flux codes F3, F6, F10, F12, F26, F28, F30, F33, and F35 had a tensile strength of 810 MPa or more because an appropriate amount of Mn was added.

[0045] In the comparative example, flux symbol F36 had a low Al2O3 content, which resulted in an unstable arc, poor slag removability, and poor bead shape. Also, because it had a high Mn content, the tensile strength of the weld metal was high, but the absorbed energy was low.

[0046] Flux F37 contains a lot of Al2O3, which resulted in poor slag removal and slag inclusion in the weld metal. Also, because it contains little Si, the tensile strength of the weld metal was low, and the absorbed energy was low.

[0047] Flux F38 had a low MgO content, so the absorbed energy of the weld metal was low. Also, the total of the CO2 equivalent values ​​of one or more metal carbonates was low, so the amount of diffusible hydrogen in the weld metal was high.

[0048] Flux F39 had poor slag removability due to its high MgO content, and slag inclusion in the weld metal occurred. In addition, the flux had a high Si content, which resulted in a low absorbed energy of the weld metal.

[0049] Flux F40 had a low CaF2 content, so the absorbed energy of the weld metal was low. Also, because it had a high total of one or both of Na2O and K2O, the bead shape was poor, undercuts occurred, and the amount of diffusible hydrogen in the weld metal was high.

[0050] Flux F41 had poor slag removability and bead shape due to its low SiO2 content. Also, because it had a low Al content, the tensile strength of the weld metal was low and the absorbed energy was low.

[0051] Flux F42 contains a lot of SiO2, so the absorbed energy of the weld metal is low. Also, because it contains a lot of CaF2, the arc is unstable, the slag removability and bead shape are poor, and pockmarks are generated.

[0052] Flux F43 contained a large amount of CaO, which resulted in an unstable arc, poor slag removability, and poor bead shape. In addition, it contained a large amount of Al, which resulted in a low absorbed energy of the weld metal.

[0053] Flux F44 had a low CaO content, so the absorbed energy of the weld metal was low. Also, the total of one or both of Na2O and K2O was low, so the arc was unstable.

[0054] Flux code 45 had a high total CO2 equivalent value of one or more metal carbonates, so the absorbed energy of the weld metal was low. In addition, the bead shape was poor and pockmarks occurred.

[0055] Among the comparative examples, flux symbol F16 contained a large amount of Al, and therefore the absorbed energy of the weld metal was low.

[0056] Flux F17 had a low absorbed energy value for the weld metal because it contained a lot of SiO2. Also, because it contained a lot of CaO, the arc was unstable, and the slag removability and bead shape were poor.

[0057] Flux F18 had a low CaO content, so the absorbed energy of the weld metal was low. Also, because it had a high CaF2 content, the arc was unstable, the slag removability and bead shape were poor, and pockmarks were generated.

[0058] Flux F19 had a low MgO content, so the absorbed energy of the weld metal was low. Also, because it had a high Al2O3 content, the slag removability was poor, and slag inclusion occurred in the weld metal.

[0059] Flux F20 contains a lot of MgO, which resulted in poor slag removal and slag inclusion in the weld metal. In addition, the total CO2 equivalent value of one or more metal carbonates is high, so the absorbed energy of the weld metal is low and pockmarks also occurred.

Claims

1. Mass % relative to the total mass of the flux SiO 2 : 5-20%, CaO: 5-20%, MgO: 25-35%, A 2 O 3 : 5-20%, CaF 2 : 20-30%, One or more metal carbonates 2 Total conversion value: 2.0-8.0%, Si: 0.3-1.0%, Al: 0.1-0.8%, Na 2 O and K 2 One or two types of O in total: 1.0 to 4.5%; A bonded flux for submerged arc welding, the balance of which consists of Fe from the iron alloy and impurities.

2. 2. The bonded flux for submerged arc welding according to claim 1, wherein the balance is 2.0% or less in mass% based on the total mass of the flux.

3. Mass % relative to the total mass of the flux Mn: 0.8% or less 3. The bonded flux for submerged arc welding according to claim 1, further comprising:

Citation Information

Patent Citations

  • Ultralow hydrogen ceramic welding flux for chrome molybdenum heat resistant steel and preparation method thereof

    CN103934594A

  • Baked flux for submerged arc welding

    JP1988013694A

  • Submerged arc welding method for 80-kg / cm2 class high tensile steel

    JP1991052796A

  • Bond flux for submerged arc welding

    JP1994328291A

  • Submerged arc weld metal of high tensile strength steel

    JP2007260696A