Antioxidant low-temperature-resistant soldering tin material and preparation method thereof

By combining rare earth chloride and MXene with SnBi-based solder material to form a composite nanostructure, the problem of insufficient brittleness and oxidation resistance in extremely cold environments is solved, and low-cost and high-performance solder materials are achieved, improving the improvement of the The stability and reliability of the welded joints.

CN119035867AActive Publication Date: 2024-11-29BAODING VICTORY TRAFFIC FACILITIES ENG CO LTD

Patent Information

Application Number
CN202411534055.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-29
Estimated Expiration
2044-10-31

AI Technical Summary

Technical Problem

Traditional solder materials exhibit brittleness and insufficient oxidation resistance in extremely cold environments, resulting in reduced reliability and higher cost of solder joints.

Method used

New materials such as rare earth chloride and MXene are combined with SnBi-based solder materials, and anti-oxidation and low-temperature solder materials are prepared through in-situ synthesis and smelting to form rare earth chloride@MXene composite nanostructures to enhance the mechanical properties and oxidation resistance of solder. sex.

Benefits of technology

It significantly improves the low temperature resistance, oxidation resistance and corrosion resistance of solder materials, reduces production costs, and enhances the stability and reliability of the solder structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035867A_ABST
    Figure CN119035867A_ABST
Patent Text Reader

Abstract

The invention relates to an antioxidant low-temperature-resistant soldering tin material and a preparation method thereof, and belongs to the technical field of low-temperature welding materials. The tin soldering material is composed of the following components of, by weight, 83%-98.9% of SnBi-based eutectic alloy, 0.1%-10% of rare earth modified MXene and 1%-7% of scaling powder. The preparation method comprises the following steps: S1, preparing MXene by a chemical etching method; s2, carrying out in-situ synthesis on XCl3 (at) MXene; and S3, the XCl3-coated MXene enhanced SnBi-based soldering tin material is prepared through a smelting method or a ball milling method. The prepared SnBi-based soldering tin has remarkable low temperature resistance, and good toughness and connection strength can be kept in an extremely low temperature environment. And the mechanical property, wettability, thermal stability and ageing resistance of the soldering tin are also greatly improved. The preparation method is simple, efficient, low in cost and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic circuit welding materials suitable for working under extremely cold conditions, and specifically relates to a circuit welding solder material that is resistant to oxidation and works in a low-temperature environment and a preparation method thereof. Background Art

[0002] With the rapid development of modern electronic technology, the application fields of electronic products are constantly expanding, especially for electronic circuits working in extremely cold environments, which puts forward higher requirements for the low-temperature environment resistance of auxiliary materials for electronic circuit assembly and welding. Among traditional solder materials, tin-lead (SnPb) materials are harmful to the environment and human health. The Restriction of Hazardous Substances Directive (RoHS) issued on July 1, 2006 has banned the use of Pb-based solder in the electronic interconnection and electronic packaging industries. Tin-silver (SnAg) alloy is used in the field of electronic assembly and packaging due to its excellent conductivity and oxidation resistance. Although pure tin (Sn) has good conductivity, it is very easy to oxidize in the air, resulting in reduced reliability of the solder joint. In order to improve the oxidation resistance, silver (Ag) is usually added, but the silver material is expensive, which increases the production cost.

[0003] Tin-bismuth (SnBi) alloys have attracted much attention due to their low melting point and low cost. In particular, the Sn58Bi eutectic alloy, which has a melting point of only 138°C and has similar microstructure and mechanical strength to SnPb alloys, has broad application prospects in the field of electronics. However, SnBi alloys also have some problems that need to be solved, such as poor alloy plasticity caused by the brittleness of the Bi phase, and interfacial embrittlement caused by the segregation of the Bi phase during the thermal aging of the solder joints, which affect the long-term service reliability of the solder joints. In order to improve the performance of SnBi alloys, researchers have conducted a large number of alloying studies to optimize the microstructure and properties of SnBi alloys by adding different alloying elements. For example, the addition of elements such as Ag, Cu, Zn, and In can improve the melting point, wettability, microstructure, and mechanical properties of SnBi alloys to a certain extent.

[0004] In addition, Sn tends to become brittle in low temperature environments, affecting its frost resistance. Whether it is SnAg alloy or SnBi alloy, Sn is one of the important components. When the temperature of Sn drops below 13.2℃, white Sn (βSn) will gradually transform into gray Sn (αSn). This transformation is an allotropic transformation. Gray Sn is in powder form, and its structure is a diamond-type cubic lattice. The relative density is lower than that of white Sn, and the texture is loose and the strength is low, making the originally dense Sn products fragile and brittle, thus losing their normal performance.

[0005] The inventors found that cerium (Ce) and lanthanum (La) rare earth chlorides can refine the solder grains and improve the structural stability of the solder, thereby enhancing the low-temperature resistance of the solder. In a low-temperature environment, rare earth chlorides can inhibit the increase in solder brittleness and improve its toughness and impact resistance. Rare earth chlorides and MXene can also form a dense oxide film on the surface of the solder material to prevent the intrusion of oxygen and other corrosive media, improve the oxidation resistance and corrosion resistance of the solder, which is of great significance for improving the long-term stability and reliability of the welded joint.

[0006] In recent years, the development of nanotechnology has provided new ideas for improving solder performance. By introducing nano-enhanced phases, such as nanoparticles, nanowires or nanosheets, the mechanical properties and reliability of solder can be effectively improved. Among them, MXene, as a new type of two-dimensional nanomaterial, has attracted much attention due to its excellent mechanical and electrical properties. Introducing MXene into SnBi-based solder materials is expected to further improve its mechanical properties and reliability. Combining rare earth chlorides with MXene to form a rare earth chloride @MXene composite nanostructure can not only give play to the nano-enhancement effect of MXene, but also utilize the unique properties of rare earth chlorides to further improve the performance of SnBi-based solders. Summary of the invention

[0007] The purpose of the present invention is to provide an antioxidant and low-temperature resistant solder material and a preparation method thereof, and to obtain a low-cost, antioxidant and antifreeze solder material by introducing new materials such as rare earth chloride and MXene, so as to solve the problems of high cost and insufficient antifreeze of traditional solder materials. The solder material of the present invention not only has a low cost, but also can maintain good physical and chemical stability in an extremely low temperature environment, thereby meeting the demand of modern electronic products for high-performance solder materials.

[0008] Specifically, the present invention provides the following technical solutions: An oxidation-resistant and low-temperature-resistant solder material, the solder material comprising: 83-98.9wt% of SnBi-based eutectic alloy, 0.1-10wt% of rare earth-modified MXene, and 1-7wt% of flux.

[0009] The SnBi-based eutectic alloy is one of Sn58Bi (42wt% Sn, 58wt% Bi), Sn58Bi0.5Ag (41.5wt% Sn, 58wt% Bi, 0.5wt% Ag), Sn58Bi4Cu (38wt% Sn, 58wt% Bi, 4wt% Cu), Sn58Bi0.5In (41.5wt% Sn, 58wt% Bi, 0.5wt% In) and Sn58Bi3Zn (39wt% Sn, 58wt% Bi, 3wt% Zn), the rare earth is one of La and Ce, the flux comprises: 94-98wt% rosin, 1-3wt% activator and 0.5-3wt% surfactant, the activator is at least one of succinic acid, adipic acid, sebacic acid, lauric acid or triethanolamine, and the surfactant is at least one of pentaerythritol oleate or polyethylene glycol 200.

[0010] The preparation process of the solder material is completed according to the following steps: Step S1: preparing MXene by chemical etching; Step S2: in-situ synthesis of XCl3@MXene; Step S3: preparing XCl3@MXene reinforced solder material by melting method or ball milling method.

[0011] The specific process of preparing MXene by chemical etching in step S1 is as follows: adding MAX phase powder to 40wt% HF solution, then transferring to a 40°C water bath for heating reaction for 24 hours, after the reaction is completed, washing the precipitate by centrifugation with deionized water until the pH value is neutral, and finally drying in a 60°C vacuum drying oven for 24 hours to obtain MXene powder.

[0012] In the step S2, X is one of Ce and La.

[0013] The specific process of in-situ synthesis of XCl3@MXene in step S2 is: dispersing the prepared MXene in deionized water to form a uniform suspension, adding X2(CO3)3 and sufficient HCl to the MXene suspension and stirring continuously to make it fully react, and after the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain XCl3@MXene; the weight fraction ratio of MXene to X2(CO3)3 is 2:1-10.

[0014] The specific process of preparing the XCl3@MXene enhanced solder material by the smelting method in step S3 is: the SnBi-based eutectic alloy, rare earth modified MXene, and flux are ball-milled and mixed under argon protection, and then smelted in a smelting furnace at a temperature of 150-250° C. for 15-30 minutes to obtain a composite solder material.

[0015] The specific process of preparing the XCl3@MXene enhanced solder material by the ball milling method in step S3 is: adding the SnBi-based eutectic alloy, rare earth modified MXene, and flux into a ball mill in a certain proportion, filling the ball mill with argon gas, and grinding at a speed of 2000-4000r / min until the solid particle size is ≤40μm to obtain a composite solder material.

[0016] Beneficial effects of the present invention: (1) In the low-temperature resistant solder material of the present invention, the rare earth chlorides of Ce and La can refine the grain structure of the solder, improve the stability of the solder structure, inhibit the increase of brittleness, and improve its toughness and impact resistance, thereby enhancing the low-temperature resistance of the solder material.

[0017] (2) The presence of Ce and La rare earth chlorides reduces the interfacial tension between the solder and the base material, improves the wettability of the solder, and enables the solder to spread more evenly on the welding surface during the welding process, thereby improving the welding quality.

[0018] (3) Ce, La rare earth chlorides, and MXene can also form a dense oxide film on the surface of the solder material to prevent the intrusion of oxygen and other corrosive media, thereby improving the oxidation resistance and corrosion resistance of the solder, which is of great significance for improving the long-term stability and reliability of the solder joint. (4) As a new type of two-dimensional nanomaterial, MXene has excellent mechanical properties. It can work synergistically with Ce and La rare earth chlorides to significantly refine the microstructure of SnBi-based solder materials, reduce problems such as coarse structure and grain boundary segregation, thereby improving the mechanical properties of solder materials such as strength, hardness and fatigue resistance, making it more difficult for solder joints to break when subjected to external forces, thereby enhancing the stability of the welded structure.

[0019] (5) Ce, La rare earth chlorides and MXene do not exist in isolation in solder materials. There is a certain interaction between them. Rare earth chlorides can be adsorbed on the surface of MXene to form stable chemical bonds, thereby enhancing the stability and dispersibility of MXene in solder materials. This synergistic effect not only improves the mechanical properties of the solder material, but also makes the solder material have better thermal stability and anti-aging properties at low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 It is a preparation flow chart of the present invention. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions. Example 1

[0023] An antioxidant and low-temperature resistant solder material, the solder material comprising: 92wt% of Sn58Bi eutectic alloy, 1wt% of rare earth La modified MXene, and 7wt% of flux, wherein the flux comprises 98wt% of rosin, 1wt% of succinic acid activator, and 1wt% of pentaerythritol oleate surfactant.

[0024] The preparation process of the solder material is completed according to the following steps: Step S1: Add the MAX phase powder to a 40wt% HF solution, then transfer it to a 40℃ water bath and heat it for reaction for 24h. After the reaction is completed, the precipitate is centrifuged and washed with deionized water until the pH value is neutral, and finally dried in a 60℃ vacuum drying oven for 24h to obtain MXene powder; Step S2: Disperse 2 parts of the prepared MXene in deionized water to form a uniform suspension, add 1 part of La2(CO3)3 and sufficient HCl to the MXene suspension and stir it continuously to make it fully react. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain LaCl3@MXene; Step S3: The Sn58Bi eutectic alloy, LaCl3@MXene, and flux are ball-milled and mixed under argon protection, and then smelted in a melting furnace at a temperature of 150℃ for 15min to obtain a composite solder material. Example 2

[0025] An antioxidant and low-temperature resistant solder material, the solder material comprising: 95wt% Sn58Bi0.5Ag (41.5wt% Sn, 58wt% Bi, 0.5wt% Ag) eutectic alloy, 0.1wt% rare earth La modified MXene, 4.9wt% soldering flux, wherein the soldering flux comprises 94wt% rosin, 3wt% adipic acid activator, and 3wt% polyethylene glycol 200 surfactant.

[0026] The preparation process of the solder material is completed according to the following steps: Step S1: Add MAX phase powder to 40wt% HF solution, then transfer to a 40℃ water bath for heating reaction for 24h. After the reaction is completed, the precipitate is centrifuged and washed with deionized water until the pH value is neutral, and finally dried in a 60℃ vacuum drying oven for 24h to obtain MXene powder; Step S2: Disperse 2 parts of the prepared MXene in deionized water to form a uniform suspension, add 3 parts of La2(CO3)3 and sufficient HCl to the MXene suspension and stir continuously to make it fully react. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain LaCl3@MXene; Step S3: Add Sn58Bi0.5Ag eutectic alloy, LaCl3@MXene, and flux to a ball mill in a certain proportion, fill the ball mill with argon, and grind at a speed of 3000r / min until the solid particle size is ≤40μm to obtain a composite solder material. Example 3

[0027] An oxidation-resistant and low-temperature-resistant solder material, comprising: 92.5wt% of Sn58Bi4Cu (38wt% Sn, 58wt% Bi, 4wt% Cu) eutectic alloy, 5wt% rare earth Ce-modified MXene, and 2.5wt% soldering flux, wherein the soldering flux comprises 96wt% of rosin, 2wt% of sebacic acid activator, and 2wt% of polyethylene glycol 200 surfactant.

[0028] The preparation process of the solder material is completed according to the following steps: Step S1: Add the MAX phase powder to a 40wt% HF solution, then transfer it to a 40℃ water bath and heat it for reaction for 24h. After the reaction is completed, the precipitate is centrifuged and washed with deionized water until the pH value is neutral, and finally dried in a 60℃ vacuum drying oven for 24h to obtain MXene powder; Step S2: Disperse 2 parts of the prepared MXene in deionized water to form a uniform suspension, add 5 parts of Ce2(CO3)3 and sufficient HCl to the MXene suspension and stir it continuously to make it fully react. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain CeCl3@MXene; Step S3: The Sn58Bi4Cu eutectic alloy, CeCl3@MXene, and flux are ball-milled and mixed under argon protection, and then smelted in a melting furnace at a temperature of 250℃ for 20min to obtain a composite solder material. Example 4

[0029] An antioxidant and low-temperature resistant solder material, the solder material comprising: 89wt% of Sn58Bi3Zn (39wt% Sn, 58wt% Bi, 3wt% Zn) eutectic alloy, 10wt% of rare earth Ce modified MXene, 1wt% of flux, wherein the flux comprises 97wt% of rosin, 1wt% of lauric acid activator, and 2wt% of pentaerythritol oleate surfactant.

[0030] The preparation process of the solder material is completed according to the following steps: Step S1: Add MAX phase powder to 40wt% HF solution, then transfer to a 40℃ water bath for heating reaction for 24h. After the reaction is completed, the precipitate is centrifuged and washed with deionized water until the pH value is neutral, and finally dried in a 60℃ vacuum drying oven for 24h to obtain MXene powder; Step S2: Disperse 2 parts of the prepared MXene in deionized water to form a uniform suspension, add 7 parts of Ce2(CO3)3 and sufficient HCl to the MXene suspension and stir continuously to make it fully react. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain CeCl3@MXene; Step S3: Add Sn58Bi3Zn eutectic alloy gold, CeCl3@MXene, and flux to a ball mill in a certain proportion, fill the ball mill with argon, and grind at a speed of 2000r / min until the solid particle size is ≤40μm to obtain a composite solder material. Example 5

[0031] An oxidation-resistant and low-temperature-resistant solder material, comprising: 87wt% of Sn58Bi0.5In (41.5wt% Sn, 58wt% Bi, 0.5wt% In) eutectic alloy, 7wt% of rare earth Ce-modified MXene, and 6wt% of flux, wherein the flux comprises 98wt% of rosin, 1wt% of succinic acid activator, and 1wt% of polyethylene glycol 200 surfactant.

[0032] The preparation process of the solder material is completed according to the following steps: Step S1: Add the MAX phase powder to a 40wt% HF solution, then transfer it to a 40℃ water bath and heat it for reaction for 24h. After the reaction is completed, the precipitate is centrifuged and washed with deionized water until the pH value is neutral, and finally dried in a 60℃ vacuum drying oven for 24h to obtain MXene powder; Step S2: Disperse 2 parts of the prepared MXene in deionized water to form a uniform suspension, add 10 parts of Ce2(CO3)3 and sufficient HCl to the MXene suspension and stir it continuously to make it fully react. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain CeCl3@MXene; Step S3: The Sn58Bi0.5In eutectic alloy, CeCl3@MXene, and flux are ball-milled and mixed under argon protection, and then smelted in a melting furnace at a temperature of 180℃ for 20min to obtain a composite solder material.

[0033] Comparative Example 1 A Sn58Bi solder alloy has a mass percentage of Sn of 42% and a mass percentage of Bi of 58%. The solder is a binary eutectic alloy with a melting point of 138°C.

[0034] Comparative Example 2 A solder material, comprising: 92wt% of Sn58Bi eutectic alloy, 1wt% of MXene, and 7wt% of flux, wherein the flux comprises 98wt% of rosin, 1wt% of succinic acid activator, and 1wt% of pentaerythritol oleate surfactant.

[0035] The preparation process of the solder material is completed according to the following steps: Step S1: Add the MAX phase powder to a 40wt% HF solution, then transfer it to a 40°C water bath for heating and reaction for 24 hours. After the reaction is completed, the precipitate is centrifuged and washed with deionized water until the pH value is neutral, and finally dried in a 60°C vacuum drying oven for 24 hours to obtain MXene powder; Step S2: The Sn58Bi eutectic alloy, MXene, and flux are ball-milled and mixed under argon protection, and then smelted in a melting furnace at a temperature of 170°C for 15 minutes to obtain a composite solder material.

[0036] Comparative Example 3 A solder material comprises: 92wt% of Sn58Bi eutectic alloy, 1wt% of rare earth LaCl3, and 7wt% of soldering flux, wherein the soldering flux comprises 98wt% of rosin, 1wt% of succinic acid activator, and 1wt% of pentaerythritol oleate surfactant.

[0037] The preparation process of the solder material is completed according to the following steps: Step S1: La2(CO3)3 and sufficient HCl are continuously stirred to fully react. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain LaCl3; Step S2: Sn58Bi eutectic alloy, LaCl3, and flux are ball-milled and mixed under argon protection, and then smelted in a smelting furnace at a temperature of 170°C for 15 minutes to obtain a composite solder material.

[0038] Performance Testing The solder material of the present invention was tested for its low temperature resistance. The samples were placed in different low temperature environments and kept warm for a certain period of time. The samples were taken out of the low temperature test box to check whether the welded parts of the samples had cracks, deformation, desoldering, etc. The test results are as follows:

[0039] The test results of the low temperature resistance of the samples show that the antioxidant low temperature resistant solder material of the present invention has excellent low temperature resistance, can be used normally in an extremely low temperature environment, and has good application prospects.

[0040] The above is only a specific embodiment of the present invention, and cannot be used to limit the scope of the invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the protection scope of the patent of the present invention, should still fall within the scope of this patent. In addition, the technical features of the present invention can be freely combined with each other, with each other and with each other, and with each other.

Claims

1. An oxidation-resistant and low-temperature-resistant solder material, characterized in that: The solder material comprises: 83-98.9wt% of SnBi-based eutectic alloy, 0.1-10wt% of rare earth modified MXene, and 1-7wt% of flux.

2. The oxidation-resistant and low-temperature-resistant solder material according to claim 1, characterized in that: The SnBi-based eutectic alloy is one of Sn58Bi, Sn58Bi0.5Ag, Sn58Bi4Cu, Sn58Bi0.5In and Sn58Bi3Zn, the rare earth is one of La and Ce, the flux includes: 94-98wt% of rosin, 1-3wt% of activator and 0.5-3wt% of surfactant, the activator is at least one of succinic acid, adipic acid, sebacic acid, lauric acid or triethanolamine, and the surfactant is at least one of pentaerythritol oleate or polyethylene glycol 200.

3. A method for preparing an oxidation-resistant and low-temperature-resistant solder material, characterized in that: The preparation process of the solder material is completed according to the following steps: Step S1: preparing MXene by chemical etching; Step S2: in-situ synthesis of XCl3@MXene; Step S3: preparing XCl3@MXene reinforced solder material by melting method or ball milling method.

4. The method for preparing an oxidation-resistant and low-temperature-resistant solder material according to claim 3, characterized in that: The specific process of preparing MXene by chemical etching in step S1 is as follows: adding MAX phase powder to 40wt% HF solution, then transferring to a 40°C water bath for heating reaction for 24 hours, after the reaction is completed, washing the precipitate by centrifugation with deionized water until the pH value is neutral, and finally drying in a 60°C vacuum drying oven for 24 hours to obtain MXene powder.

5. The method for preparing an oxidation-resistant and low-temperature-resistant solder material according to claim 3, characterized in that: In the step S2, X is one of Ce and La.

6. The method for preparing an oxidation-resistant and low-temperature-resistant solder material according to claim 3, characterized in that: The specific process of in-situ synthesis of XCl3@MXene in step S2 is: dispersing the prepared MXene in deionized water to form a uniform suspension, adding X2(CO3)3 and sufficient HCl to the MXene suspension and stirring continuously to make it fully react, and after the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain XCl3@MXene; the weight fraction ratio of MXene to X2(CO3)3 is 2:1-10.

7. The method for preparing an oxidation-resistant and low-temperature-resistant solder material according to claim 3, characterized in that: The specific process of preparing the XCl3@MXene enhanced solder material by the smelting method in step S3 is: the SnBi-based eutectic alloy, rare earth modified MXene, and flux are ball-milled and mixed under argon protection, and then smelted in a smelting furnace at a temperature of 150-250° C. for 15-30 minutes to obtain a composite solder material.

8. The method for preparing an oxidation-resistant and low-temperature-resistant solder material according to claim 3, characterized in that: The specific process of preparing the XCl3@MXene enhanced solder material by the ball milling method in step S3 is: adding the SnBi-based eutectic alloy, rare earth modified MXene, and flux into a ball mill in a certain proportion, filling the ball mill with argon gas, and grinding at a speed of 2000-4000r / min until the solid particle size is ≤40μm to obtain a composite solder material.

Citation Information

Patent Citations

  • Lead-free welding flux alloy suitable for dissimilar metals soldering flux of aluminum and copper

    CN101007374A

  • Tin, zinc and bismuth multi-element eutectic lead-free solder and preparation method

    CN102581507A

  • Two-dimensional carbide-supported rare earth fluoride nanometer powder, preparation method and applications thereof

    CN106563479A

  • Electroless tin-plated solder and solder paste based on graphene, and preparation methods of electroless tin-plated solder and solder paste

    CN110614454A

  • Low-temperature lead-free solder paste and preparation method thereof

    CN111318832A

Cited By

  • Low-hydrogen flux-cored wire based on two-dimensional MXene surface self-assembly modification and preparation method and application of low-hydrogen flux-cored wire

    CN122378320A

  • A low-hydrogen flux-cored wire based on two-dimensional MXene surface self-assembly modification, its preparation method and application

    CN122378320B

  • Nano-metal composite solder and manufacturing method therefor

    WO2026205958A1