Electrophotographic photoreceptor, process cartridge and electrophotographic apparatus

By treating metal oxide particles with a silane coupling agent containing an isocyanate group and combining them with polyol and polyisocyanate compounds, the adhesion and dispersibility issues in electrophotographic photoreceptors are resolved, enhancing image quality and charge transfer.

JP7566680B2Active Publication Date: 2024-10-15CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021063070
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-01
Publication Date
2024-10-15
Estimated Expiration
2041-04-01

AI Technical Summary

Technical Problem

The adhesion between the undercoat layer and the photosensitive layer in electrophotographic photoreceptors is compromised due to the hydrophobicity of metal oxide particles treated with certain silane coupling agents, leading to issues like white spots and reduced charge transfer, which affects image quality.

Method used

Incorporating metal oxide particles surface-treated with a silane coupling agent having an isocyanate group, along with polyol and polyisocyanate compounds, to form a cured film that enhances adhesion and dispersibility in the undercoat layer, using a composition that includes a polyol compound with two or more hydroxy groups and a polyisocyanate compound with two or more isocyanate groups.

Benefits of technology

The solution improves the adhesion between the undercoat and photosensitive layers, ensuring better dispersibility of metal oxide particles, thereby reducing image defects and maintaining charge transfer efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566680000019
    Figure 0007566680000019
  • Figure 0007566680000020
    Figure 0007566680000020
  • Figure 0007566680000021
    Figure 0007566680000021
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor that has good adhesion between an undercoat layer and a photosensitive layer and good dispersion of metal oxide particles in the undercoat layer; a process cartridge; and an electrophotographic device.SOLUTION: An electrophotographic photoreceptor comprises a support, an undercoat layer on the support, and a photosensitive layer on the undercoat layer. The undercoat layer is a cured film of a composition containing a metal oxide surface-treated with a specific silane coupling agent, a polyol compound having two or more hydroxy groups, and a polyisocyanate compound having two or more isocyanate groups.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, and a process cartridge and an electrophotographic apparatus each having the electrophotographic photoreceptor. [Background technology]

[0002] In recent years, undercoat layers containing metal oxide particles have been proposed as undercoat layers for use in organic electrophotographic photoreceptors (hereinafter referred to as "electrophotographic photoreceptors"). In order to improve the dispersibility and electrical properties of the contained metal oxide particles, undercoat layers containing metal oxide particles that have been surface-treated with a silane coupling agent or the like have also been proposed.

[0003] Patent Document 1 discloses a technique for suppressing potential fluctuations by incorporating metal oxide particles surface-treated with a silane coupling agent and a benzophenone compound having a hydroxyl group or an amino group into the undercoat layer. It is presumed that such an organic compound having a substituent interacts with the metal oxide particles to facilitate the transfer of electrons between the metal oxide particles in the undercoat layer or from the photosensitive layer to the undercoat layer.

[0004] Furthermore, Patent Document 2 discloses an undercoat layer containing strontium titanate as a means for improving the potential fluctuation of the electrical properties of the electrophotographic photoreceptor. According to Patent Document 2, an undercoat layer containing strontium titanate particles exerts an excellent effect on residual electricity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-181804 A [Patent Document 2] JP 2019-61219 A Summary of the Invention [Problem to be solved by the invention]

[0006] The inventors have found through their investigations that when an undercoat layer is provided on the support of an electrophotographic photoreceptor, if metal oxide particles that have been surface-treated with a silane coupling agent are used, the combination of the silane coupling agent used for surface treatment and the resin of the undercoat layer can affect the compatibility with the photosensitive layer laminated on top of the undercoat layer, leaving room for improvement in image quality. Specifically, metal oxide particles that have been surface-treated with a silane coupling agent affect the adhesion between the surface of the undercoat layer and the photosensitive layer laminated on the undercoat layer when the undercoat layer is formed into a film, depending on the type of silane coupling agent. It has been known that in order to improve the dispersibility of metal oxide particles in the undercoat layer, it is effective to increase the hydrophobicity of the metal oxide particle surface. On the other hand, metal oxide particles with increased hydrophobicity are one of the causes of reduced adhesion with the photosensitive layer when the undercoat layer is formed into a film. The reduced adhesion between the photosensitive layer and the undercoat layer results in image defects such as white spots.

[0007] As a result of intensive research by the present inventors, it was found that an electrophotographic photoreceptor can be obtained that contains metal oxide particles surface-treated with a silane coupling agent having an isocyanate group, and that contains a polyol compound having two or more hydroxyl groups and a polyisocyanate compound having two or more isocyanate groups, and that contains a cured film of the composition as an undercoat layer, and that has both adhesion between the photosensitive layer and the undercoat layer and dispersibility of the metal oxide particles in the undercoat layer. This is thought to be because, among silane coupling agents, when a silane coupling agent having an isocyanate group is used, hydrophobization of the undercoat layer is suppressed, and therefore adhesion with the photosensitive layer laminated on the undercoat layer can be maintained. In addition, the metal oxide particles surface-treated with a silane coupling agent having an isocyanate group have an isocyanate group on the surface. Therefore, it is believed that when a composition containing a polyol compound and a polyisocyanate compound forms a cured film, the metal oxide particles are incorporated into the cured film, and the metal oxide particles can be dispersible in the undercoat layer. If the metal oxide particles are not sufficiently dispersed in the undercoat layer, the transfer of charges within the undercoat layer is hindered, causing black spots on the image.

[0008] An object of the present invention is to provide an electrophotographic photoreceptor which has an effect of improving the adhesion between an undercoat layer and a photosensitive layer laminated on the undercoat layer, and the dispersibility of metal oxide particles in the undercoat layer, and a process cartridge and an electrophotographic apparatus which have the electrophotographic photoreceptor. [Means for solving the problem]

[0009] Therefore, the present invention provides an electrophotographic photoreceptor having a support, an undercoat layer on the support, and a photosensitive layer on the undercoat layer, wherein the undercoat layer is Metal oxide particles surface-treated with a silane coupling agent represented by the following formula (1): a polyol compound having two or more hydroxy groups, and Polyisocyanate compounds having two or more isocyanate groups The electrophotographic photoreceptor is characterized in that it is a cured film of a composition containing the above. [ka] In formula (1), R 1 and R 2 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 3 R represents a hydroxy group, an alkoxy group having 1 to 4 carbon atoms, or an alkyl group having 1 to 4 carbon atoms. 4 represents an alkylene group having 1 to 4 carbon atoms. Effect of the Invention

[0010] According to the present invention, it is possible to provide an electrophotographic photoreceptor which has good adhesion between an undercoat layer and a photosensitive layer on the undercoat layer and has excellent dispersibility of metal oxide particles in the undercoat layer. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a diagram showing an example of a layer structure of the electrophotographic photoreceptor of the present invention. [Diagram 2]FIG. 1 is a diagram showing an example of an electrophotographic apparatus equipped with a process cartridge having an electrophotographic photosensitive member of the present invention. [Diagram 3] 1A is a top view showing the mold, FIG. 1B is a cross-sectional view of the protrusion taken along line S-S', and FIG. 1C is a cross-sectional view of the protrusion taken along line T-T'. [Figure 4] FIG. 2 is a diagram showing an example of a pressure-contact shape transfer processing device for forming recesses on the peripheral surface of an electrophotographic photosensitive member. [Diagram 5] FIG. 1 is a diagram showing an example of a polishing machine using a polishing sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to an electrophotographic photoreceptor having a support, an undercoat layer on the support, and a photosensitive layer on the undercoat layer, wherein the undercoat layer is a cured film of a composition containing metal oxide particles surface-treated with a silane coupling agent represented by the following formula (1), a polyol compound having two or more hydroxy groups, and a polyisocyanate compound having two or more isocyanate groups: [ka] In formula (1), R 1 and R 2 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 3 R represents a hydroxy group, an alkoxy group, or an alkyl group having 1 to 4 carbon atoms. 4 represents an alkylene group having 1 to 4 carbon atoms.

[0013] The electrophotographic photoreceptor of the present invention will be described in detail below. First, the layer structure of the electrophotographic photoreceptor of the present invention will be described, followed by a description of each layer. Among these, the undercoat layer will be described. After describing each layer, the surface treatment of the electrophotographic photosensitive member will be described, and then a process cartridge and an electrophotographic apparatus that accommodate the electrophotographic photosensitive member will be described.

[0014] [Electrophotographic photoreceptor] 1, the electrophotographic photoreceptor according to the embodiment of the present invention has an undercoat layer 102 directly on a support 101, and further has a photosensitive layer 103 directly on the undercoat layer 102. These layers are laminated. The method for producing the electrophotographic photoreceptor includes a method in which the coating liquids for each layer described later, i.e., the coating liquid for forming the undercoat layer, the coating liquid for forming the charge generating layer, the coating liquid for forming the charge transport layer, and the coating liquid for forming the protective layer, are prepared, coated in order, and dried to obtain the electrophotographic photoreceptor. Coating methods include dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, and the like. Among these, dip coating is preferred from the viewpoints of efficiency and productivity.

[0015] <Support> The support may be non-conductive, but is preferably a conductive support having electrical conductivity. The shape of the support may be cylindrical, belt-like, sheet-like, or the like. Of these, the cylindrical shape is preferred. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, centerless grinding, etc. Among these, cutting is preferred. The material of the support is preferably a metal. Examples of metals include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among them, an aluminum support using aluminum is preferable. The support may have a non-conductive base material such as glass, and the surface on which the undercoat layer is to be disposed may have a conductive film. A conductive layer may be provided on the support. In this case, the conductive layer preferably contains conductive particles and a resin. The conductive particles are preferably metal oxide particles such as titanium oxide, tin oxide, and zinc oxide. The resin is preferably a polycarbonate resin, a phenol resin, or a polyurethane resin.

[0016] <Undercoat layer> The undercoat layer according to the embodiment of the present invention contains metal oxide particles. The primary particle diameter (volume number average) of the metal oxide particles is 1 nm or more and 200 nm or less, and preferably 1 nm or more and 50 nm or less. The metal oxide particles are surface-treated with a compound represented by formula (1). The metal oxide particles are hydrophobized with a compound represented by formula (1), which is a silane coupling agent having an isocyanate group. [ka] In formula (1), R 1 and R 2 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 3 R represents a hydroxy group, an alkoxy group having 1 to 4 carbon atoms, or an alkyl group having 1 to 4 carbon atoms. 4 represents an alkylene group having 1 to 4 carbon atoms.

[0017] In formula (1), R 1 ~R 3 Examples of the alkoxy group having 1 to 4 carbon atoms as R include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an s-butoxy group, a t-butoxy group, and an isobutoxy group. 3 Examples of the alkyl group having 1 to 4 carbon atoms as R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, and an isobutyl group. 4 Examples of the alkylene group having 1 to 4 carbon atoms include a methylene group, an ethylene group, a propylene group, a methylethylene group, a butylene group, a methylpropylene group, a dimethylpropylene group, and an ethylethylene group.

[0018] Specific examples of the compound represented by formula (1) include 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropylmethyldiethoxysilane, 3-isocyanatepropylmethyldiethoxysilane, 3-isocyanatepropylmethyldimethoxysilane, 3-isocyanatemethyltriethoxysilane, and 3-isocyanatemethyltrimethoxysilane. However, the compound represented by formula (1) is not limited to these. In addition, two or more compounds represented by formula (1) may be mixed and used.

[0019] R of the compound represented by formula (1) 1 ~R 3 When is a hydroxy group or an alkoxy group, the hydroxy group or alkoxy group is hydrolyzed to generate a hydroxy group, which undergoes a dehydration reaction with the hydroxy group present on the surface of the metal oxide particle. As a result, the metal oxide particle is surface-treated by bonding with the compound represented by formula (1). In other words, the metal oxide particle is hydrophobized by the compound represented by formula (1).

[0020] The method for surface treating the metal oxide particles with the compound represented by formula (1) may be, for example, a dry method or a wet method. In the dry method, metal oxide particles are stirred in a mixer capable of high-speed stirring such as a Henschel mixer while an alcohol aqueous solution, an organic solvent solution, or an aqueous solution containing the compound represented by formula (1) is added to the metal oxide particles to uniformly disperse them, followed by drying. In the wet method, metal oxide particles and the compound represented by formula (1) are stirred in a solvent or dispersed using a sand mill or the like with glass beads or the like, and after dispersion, the solvent is removed by filtration or distillation under reduced pressure. After removing the solvent, it is preferable to further bake at 100°C or higher.

[0021] Examples of the metal oxide particles include zinc oxide particles, tin oxide particles, titanium oxide particles, aluminum oxide particles, sodium titanate particles, and barium titanate particles. Among these, anatase type titanium oxide particles and strontium titanate particles are preferred.

[0022] In the present invention, only one type of metal oxide particle may be used, or two or more types may be used in combination, such as particles of different types of metal oxide, particles having different types of surface treatments or different specific surface areas.

[0023] The content of the metal oxide in the undercoat layer is preferably 50% by mass or more and 90% by mass or less based on the total mass of the undercoat layer.

[0024] The undercoat layer also contains a binder resin. The binder resin is obtained by polymerizing a composition containing a monomer, oligomer, prepolymer, etc. having a polymerizable functional group by heating or irradiating with an electron beam. In the present invention, the monomer constituting the binder resin by polymerization does not include a structure having an electron transport function.

[0025] Examples of the monomer include compounds having an isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group. The isocyanate group in the present invention includes an isocyanate group (a group represented by -N=C=O) that is not protected with a blocking agent, and a blocked isocyanate group in which an isocyanate group (a group represented by -N=C=O) is protected with a blocking agent. In the present invention, among these monomers, at least a polyol compound having two or more hydroxyl groups and a polyisocyanate compound having two or more isocyanate groups are used.

[0026] Examples of polyisocyanate compounds include, but are not limited to, ethylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate (TDI), 4,4-diphenylmethane diisocyanate (MDI), polymeric diphenylmethane diisocyanate, xylylene diisocyanate, and naphthalene diisocyanate, as well as copolymers and isocyanurates of these isocyanate compounds, as well as compounds having blocked isocyanate groups such as TMP adducts of isocyanate compounds and biuret compounds of isocyanate compounds.

[0027] Examples of the polyol compound include, but are not limited to, polyether polyols, polyester polyols, polycarbonate polyols, polyolefin polyols, polybutadiene polyols, (meth)acrylic polyols, and polysiloxane polyols.

[0028] In a coating solution for forming an undercoat layer, which is made of a composition containing metal oxide particles surface-treated with a silane coupling agent represented by formula (1), a polyol compound having two or more hydroxyl groups, and a polyisocyanate compound having two or more isocyanate groups, the hydroxyl group reacts with the isocyanate group during curing to generate a urethane bond, and the reaction continues to generate a urethane resin. At this time, the coating solution for forming an undercoat layer is cured in a state in which the metal oxide particles are incorporated into the resin by the silane coupling agent represented by formula (1) dispersed in the coating solution for forming an undercoat layer. In a conventional undercoat layer, the resin and the metal oxide particles are not bonded, and as the coating solution for forming an undercoat layer is cured in a fluid manner, the dispersion state of the metal oxide particles changes, and the metal oxide particles may become biased toward the inside of the resin. In contrast, in the present invention, the metal oxide particles are surface-treated with a silane coupling agent represented by formula (1), so that urethane bonds are formed between the isocyanate groups on the surface of the metal oxide particles and the polyol compound, and the metal oxide particles are bonded to the urethane resin serving as a binder resin. As a result, the metal oxide particles are maintained in a dispersed state within the resin while hardening proceeds, and uneven distribution of the metal oxide particles in the undercoat layer can be prevented.

[0029] The undercoat layer of the present invention may further contain an electron transporting material, a metal, a conductive polymer, etc. for the purpose of improving electrical properties. The electron transport material is preferably selected from the group consisting of compounds represented by formula (2). [ka]

[0030] In formula (2), R 11 ~R 15 each independently represents a hydrogen atom, a hydroxyl group, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, or an amino group.

[0031] A 1 represents a hydroxy group, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms.

[0032] In formula (2), R 11 ~R 15 Examples of the alkyl group having 1 to 6 carbon atoms as R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, an isobutyl group, a pentyl group, and a hexyl group. 11 ~R 15 Examples of the alkoxy group having 1 to 8 carbon atoms as the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an s-butoxy group, a t-butoxy group, an isobutoxy group, a pentoxy group, a hexyloxy group, a heptyloxy group, and an octyloxy group.

[0033] In formula (2), A 1 Examples of the alkyl group having 1 to 4 carbon atoms as A include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an s-butyl group, a t-butyl group, and an isobutyl group. 1 Examples of the alkoxy group having 1 to 4 carbon atoms as the aryl group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an s-butoxy group, a t-butoxy group, and an isobutoxy group.

[0034] By incorporating the compound represented by formula (2) in the undercoat layer together with the metal oxide particles, the uniformity of dispersion of the metal oxide particles in the undercoat layer is improved. The inventors believe that the reason for this effect is that the compound represented by formula (2) coordinates with the metal oxide particles or bonds with the isocyanate group provided on the metal oxide surface, so that the metal oxide particles in the coating solution for forming the undercoat layer are kept in a good dispersion state until curing. The content of the compound represented by formula (2) in the undercoat layer is preferably 2.0% by mass relative to the mass of the metal oxide particles.

[0035] The electron transport material may have a polymerizable functional group, and may be copolymerized with the above-mentioned monomer having a polymerizable functional group.

[0036] Specific examples of the compound represented by formula (2) include compounds represented by the following formulas (2-1) to (2-16), but are not limited thereto. [ka] [ka] [ka] [ka]

[0037] Among these, aminosalicylic acid represented by formula (2-15) having a hydroxy group and an amino group highly reactive with an isocyanate group is preferable.

[0038] The average thickness of the undercoat layer is preferably from 0.1 μm to 30 μm, and more preferably from 1.0 μm to 5.0 μm.

[0039] The undercoat layer can be formed by preparing a coating solution for forming the undercoat layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying and / or curing it. Examples of the solvent used in the coating solution for forming the undercoat layer include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0040] The preparation of the coating liquid for forming the undercoat layer is not limited thereto, but may be, for example, the following coating liquid preparation process. First, the metal oxide particles are surface-treated with a silane coupling agent represented by formula (1). Next, the surface-treated metal oxide particles, a polyol compound having two or more hydroxyl groups, and a polyisocyanate compound having two or more isocyanate groups, as well as an electron transport material containing a compound represented by formula (2) as necessary, a metal, a conductive polymer, and the like are mixed in a solvent. Finally, glass beads are added to the mixed liquid, which is stirred with a sand mill or the like, and the glass beads are removed by filtration to obtain a coating liquid for forming the undercoat layer. The coating liquid for forming the undercoat layer contains surface-treated metal oxide particles such that the content of the surface-treated metal oxide particles after drying is 50% by mass or more and 90% by mass or less.

[0041] The obtained coating liquid for forming an undercoat layer is applied onto a support in a coating step to form a coating film of the coating liquid for forming an undercoat layer, and then the coating film is dried at high temperature in a drying step to form an undercoat layer. The electrophotographic photoreceptor of the present invention can be manufactured on the undercoat layer through a known method, for example, a step of forming a photosensitive layer and a step of forming a protective layer, which will be described below.

[0042] <Photosensitive layer> The electrophotographic photoreceptor of the present invention has a photosensitive layer on an undercoat layer. The photosensitive layer of the electrophotographic photoreceptor is mainly classified into (1) a laminated type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The laminated type photosensitive layer has a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer has a photosensitive layer containing both a charge generation material and a charge transport material.

[0043] (1) Laminated photosensitive layer The laminated type photosensitive layer has a charge generating layer and a charge transport layer.

[0044] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin. Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer. The resin is preferably a polyvinyl butyral resin.

[0045] The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds.

[0046] The average thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm.

[0047] The charge generating layer can be formed by preparing a coating solution for forming the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0048] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin.

[0049] Examples of the charge transport material include, but are not limited to, polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these substances. Among these, triarylamine compounds and benzidine compounds are preferred. The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer.

[0050] Examples of the resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10.

[0051] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.

[0052] The average thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm.

[0053] The charge transport layer can be formed by preparing a coating solution for forming the charge transport layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred.

[0054] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for forming a photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming a coating film of this, and drying it. As the charge generating material, the charge transporting material and the resin, polycarbonate resin is preferable, as in the "(1-2) charge transporting layer" in the above "(1) laminated type photosensitive layer".

[0055] <Protective layer> In the present invention, a protective layer may be provided on the photosensitive layer. By providing the protective layer, durability can be improved. The protective layer preferably contains conductive particles and / or a charge transport material, and a resin. The conductive particles include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide. Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred. Examples of the resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among them, polycarbonate resin, polyester resin, and acrylic resin are preferable.

[0056] The protective layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the reaction include thermal polymerization, photopolymerization, and radiation polymerization. Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an acrylic group and a methacrylic group. A material having a charge transport function may be used as the monomer having a polymerizable functional group.

[0057] The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, abrasion resistance improvers, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.

[0058] The average thickness of the protective layer is preferably from 0.5 μm to 10 μm, and more preferably from 1 μm to 7 μm.

[0059] The protective layer can be formed by preparing a coating solution for forming the protective layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying and / or curing it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0060] <Surface treatment of electrophotographic photoreceptor> In the electrophotographic photoreceptor of the present invention, for the purpose of further stabilizing the behavior of a cleaning means that is brought into contact with the electrophotographic photoreceptor, a concave or convex portion may be provided on the surface of the electrophotographic photoreceptor that the cleaning means contacts, or the surface may be roughened by polishing. Examples of the cleaning means include a cleaning blade.

[0061] When forming recesses, a mold having protrusions corresponding to the recesses is pressed against the surface of the electrophotographic photosensitive member to transfer the shape, thereby forming the recesses on the surface of the electrophotographic photosensitive member. When forming convex portions, a mold having concave portions corresponding to the convex portions is pressed against the surface of the electrophotographic photoreceptor to transfer the shape, thereby forming the convex portions on the surface of the electrophotographic photoreceptor. As the mold, for example, a mold having a plurality of convex shapes as shown in FIG. 3 can be used. FIG. 3(a) is a top view showing an outline of the mold, and FIG. 3(b) is a schematic cross-sectional view of the convex portions of the mold in the axial direction of the electrophotographic photoreceptor (cross-sectional view at S-S' section in FIG. 3(a)). FIG. 3(c) is a cross-sectional view of the convex portions of the mold in the circumferential direction of the electrophotographic photoreceptor (cross-sectional view at T-T' section in FIG. 3(a)). The formation of recesses on the surface of an electrophotographic photoreceptor is performed by placing the mold shown in Fig. 3 in a pressure contact shape transfer processing device having a configuration generally shown in Fig. 4, and performing surface processing on the electrophotographic photoreceptor before the recesses are formed. 401 is a processing target (electrophotographic photoreceptor before processing), 402 is a mold type, 403 is a pressure member, and 404 is a support member.

[0062] When the surface of the electrophotographic photoreceptor is polished to impart roughness, an abrasive tool is brought into contact with the electrophotographic photoreceptor and one or both of them are moved relatively to polish the surface of the electrophotographic photoreceptor, thereby imparting roughness. Examples of the abrasive tool include an abrasive member having a layer in which abrasive grains are dispersed in a binder resin provided on a substrate.

[0063] [Process cartridges, electrophotographic devices] The process cartridge of the present invention integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means, a transfer means and a cleaning means, and is detachably attachable to the main body of the electrophotographic apparatus. The electrophotographic apparatus of the present invention also comprises the electrophotographic photosensitive member, charging means, exposure means, developing means and transfer means described above.

[0064] FIG. 2 shows an example of a schematic configuration of an electrophotographic apparatus having a process cartridge 11 equipped with an electrophotographic photosensitive member. A cylindrical electrophotographic photoreceptor 1 is rotated at a predetermined peripheral speed in the direction of the arrow around an axis 2. The surface of the electrophotographic photoreceptor 1 is charged by charging means 3 to a predetermined positive or negative potential.

[0065] 2 shows a roller charging method using a roller-type charging member, but other charging methods such as corona charging, proximity charging, injection charging, etc. In the case of the roller charging method, there is a DC charging method in which the voltage applied to the roller-type charging member is only a DC voltage, and an AC / DC charging method in which an AC voltage is superimposed on a DC voltage, and either may be used. The charged surface of the electrophotographic photosensitive member 1 is irradiated with exposure light 4 from an exposure means (not shown), and an electrostatic latent image corresponding to the target image information is formed. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 1 is developed with toner contained in developing means 5, and a toner image is formed on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor 1 is transferred to a transfer material 7 by transfer means 6. The transfer material 7 onto which the toner image has been transferred is transported to fixing means 8, where the toner image is fixed and printed out from the electrophotographic apparatus. The electrophotographic apparatus may have cleaning means 9 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 1 after transfer. The electrophotographic apparatus may have a charge eliminating mechanism that eliminates charge on the surface of the electrophotographic photosensitive member 1 by pre-exposure light 10 from a pre-exposure means (not shown). In addition, a guide means 12 such as a rail may be provided in order to mount and remove the process cartridge 11 of the present invention to and from the main body of the electrophotographic apparatus.

[0066] The electrophotographic photoreceptor of the present invention can be used in laser beam printers, LED printers, copiers, facsimiles, and multifunction machines thereof.

[0067] (Example) The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited by the following examples without departing from the gist of the present invention. In the following description of the examples, "parts" are based on mass unless otherwise specified.

[0068] [Production of strontium titanate particles S-1] A titanium oxide hydroxide slurry obtained by hydrolysis of an aqueous solution of titanyl sulfate was washed with an aqueous alkali solution. Next, hydrochloric acid was added to the above-mentioned slurry of hydrous titanium oxide to adjust the pH to 0.7, thereby obtaining a titania sol dispersion liquid. To 1.8 moles (titanium oxide equivalent) of the obtained titania sol dispersion, an aqueous solution containing 1.1 times the molar amount of strontium chloride was added and placed in a reaction vessel, and the atmosphere was replaced with nitrogen gas. Furthermore, pure water was added so that the titanium concentration was 0.9 moles / L in terms of titanium oxide. Next, this was stirred and mixed, heated to 80°C, and then 792 mL of 5N sodium hydroxide aqueous solution was added over 40 minutes, and then the reaction was carried out for 20 minutes. The slurry after the reaction was cooled to 30°C or less, and the supernatant liquid was removed. Furthermore, a hydrochloric acid aqueous solution of pH 5.0 was added to the slurry, and the mixture was stirred for 1 hour, and then repeatedly washed with pure water. Furthermore, the mixture was neutralized with sodium hydroxide, filtered through a Nutsche filter, and washed with pure water. The obtained cake was dried to obtain strontium titanate particles S-1. The primary particle size was 35 nm.

[0069] [Example of manufacturing surface-treated metal oxide particles] <Production Example of Metal Oxide Particle S-1A> 100 parts of strontium titanate particles S-1 were mixed with 500 parts of toluene and stirred, and 3.0 parts of 3-isocyanatepropyltriethoxysilane was added as a silane coupling agent and stirred for 6 hours. After that, the toluene was distilled off under reduced pressure, and the mixture was dried by heating at 130°C for 6 hours to obtain surface-treated metal oxide particles S-1A.

[0070] <Production Example of Metal Oxide Particle S-1B> Surface-treated metal oxide particles S-1B were produced in the same manner as in the production example of metal oxide particles S-1A, except that the silane coupling agent in the production example of metal oxide particles S-1A was changed to 3.0 parts of 3-isocyanatepropyltrimethoxysilane.

[0071] <Production example of metal oxide particle S-1C> Surface-treated metal oxide particles S-1C were produced in the same manner as in the production example of metal oxide particles S-1A, except that the silane coupling agent in the production example of metal oxide particles S-1A was changed to 3.0 parts of 3-isocyanatepropylmethyldiethoxysilane.

[0072] <Production example of metal oxide particle S-1D> Surface-treated metal oxide particles S-1D were produced in the same manner as in the production example of metal oxide particles S-1A, except that the silane coupling agent in the production example of metal oxide particles S-1A was changed to 4.0 parts of 3-isocyanatepropylmethyldimethoxysilane.

[0073] <Production Example of Metal Oxide Particles S-1E> Surface-treated metal oxide particles S-1E were produced in the same manner as in the production example of metal oxide particles S-1A, except that the silane coupling agent in the production example of metal oxide particles S-1A was changed to 3.0 parts of 3-isocyanatemethyltriethoxysilane.

[0074] <Production example of metal oxide particle S-1F> Surface-treated metal oxide particles S-1F were produced in the same manner as in the production example of metal oxide particles S-1A, except that the silane coupling agent in the production example of metal oxide particles S-1A was changed to 3.0 parts of 3-isocyanatemethyltrimethoxysilane.

[0075] <Production Example of Metal Oxide Particle T-1A> 100 parts of titanium oxide particles T-1 (product name: TKP101, manufactured by Teika Corporation, primary particle size 6 nm) were mixed with 500 parts of toluene and stirred, and 3.0 parts of 3-isocyanatepropyltriethoxysilane was added as a silane coupling agent and stirred for 2 hours. After that, the toluene was distilled off by reduced pressure distillation, and the mixture was baked at 120°C for 3 hours to obtain surface-treated metal oxide particles T-1A.

[0076] <Production Example of Metal Oxide Particle T-1B> 100 parts of titanium oxide particles T-1 (product name: TKP101, manufactured by Teika Co., Ltd., primary particle size 6 nm) were mixed with 500 parts of toluene and stirred, and 3.0 parts of 3-isocyanatepropyltrimethoxysilane was added as a silane coupling agent and stirred for 2 hours. After that, toluene was distilled off by reduced pressure distillation, and baking was performed at 120°C for 3 hours to obtain surface-treated metal oxide particles T-1B.

[0077] <Production Example of Metal Oxide Particle T-2A> 100 parts of titanium oxide particles T-2 (product name: AMT-600, manufactured by Teika Co., Ltd., primary particle size 30 nm) were mixed with 500 parts of toluene and stirred, and 3.0 parts of 3-isocyanatepropyltriethoxysilane was added as a silane coupling agent and stirred for 2 hours. After that, toluene was distilled off by reduced pressure distillation, and baking was performed at 120°C for 3 hours to obtain surface-treated metal oxide particles T-2A.

[0078] <Production Example of Metal Oxide Particles Z-1A> Zinc oxide particles Z-1 (specific surface area: 19 m 2 100 parts of 1,2-dichlorophenyl ether (1.0 parts by weight, 1 / g, primary particle size 50 nm) was mixed with 500 parts of toluene and stirred, and 1.0 part of 3-isocyanatepropyltriethoxysilane was added as a silane coupling agent and stirred for 2 hours. After that, the toluene was distilled off by reduced pressure distillation, and the mixture was baked at 120°C for 3 hours to obtain surface-treated metal oxide particles Z-1A.

[0079] [Table 1]

[0080] Example 1 The surface of an aluminum cylinder was cut using a lathe under the following cutting conditions to prepare an aluminum blank tube with a length of 370 mm, an outer diameter of 30.6 mm, and a thickness of 1.0 mm. The cutting conditions were a cutting tool with an R0.1, a spindle speed of 10,000 rpm, and a cutting tool feed rate that was continuously changed within the range of 0.03 to 0.06 mm / rpm.

[0081] Next, 15 parts of butyral resin (trade name: BM-1, manufactured by Sekisui Chemical Co., Ltd.) as a polyol compound having two or more hydroxyl groups and 15 parts of blocked isocyanate (trade name: Sumidur BL3175, manufactured by Sumika Bayern Urethane Co., Ltd.) as a polyisocyanate compound having two or more isocyanate groups were dissolved in a mixture of 300 parts of methyl ethyl ketone and 300 parts of 1-butanol. 120 parts of metal oxide particles S-1A and 1.2 parts of 5-aminosalicylic acid (manufactured by Tokyo Kasei Kogyo Co., Ltd.) as a charge transport agent were added to this solution, and this was dispersed in a sand mill device using glass beads with a diameter of 0.8 mm under an atmosphere of 23 ± 3 ° C. for 4 hours. After dispersion, 0.01 parts of silicone oil (trade name: SH28PA, manufactured by Toray Dow Corning Co., Ltd.) was added to the dispersion and stirred to obtain a coating solution for the undercoat layer. The obtained coating liquid for forming an undercoat layer was dip-coated onto the above-mentioned support and then dried at 165° C. for 30 minutes to form an undercoat layer having a thickness of 2 μm.

[0082] Next, 20 parts of hydroxygallium phthalocyanine crystals (charge generating material) having strong peaks at Bragg angles 2θ±0.2° of 7.4° and 28.2° in CuKα characteristic X-ray diffraction, 0.2 parts of a calixarene compound represented by formula (A), 10 parts of polyvinyl butyral resin (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.), and 600 parts of cyclohexanone were placed in a sand mill using glass beads with a diameter of 1 mm, and the mixture was dispersed for 4 hours. Then, 600 parts of ethyl acetate was added to prepare a coating liquid for forming a charge generating layer. This charge generating layer forming coating liquid was dip coated onto the above undercoat layer, and the resulting coating was dried at 80° C. for 15 minutes to form a charge generating layer having a thickness of 0.19 μm. [ka]

[0083] next, 60 parts of a compound represented by the following formula (B) (charge transport material), 30 parts of a compound represented by the following formula (C) (charge transport material), 10 parts of a compound represented by the following formula (D) (charge transport material), Polycarbonate resin (product name: Iupilon Z400, manufactured by Mitsubishi Engineering Plastics Corporation, bisphenol Z type polycarbonate) 100 parts, 0.02 parts of polycarbonate (viscosity average molecular weight Mv: 20,000) represented by the following formula (E), A coating solution for the charge transport layer was prepared by dissolving in a mixed solvent of 600 parts of o-xylene and 200 parts of dimethoxymethane. This charge transport layer coating liquid was dip coated onto the charge generating layer to form a coating film, and the resulting coating film was dried at 100° C. for 30 minutes to form a charge transport layer with a thickness of 18 μm. [ka] [ka]

[0084] next, 1.65 parts of a resin having a repeating structural unit represented by the following formula (F1) and a repeating structural unit represented by the following formula (F2) (weight average molecular weight: 130,000, copolymerization ratio (F1) / (F2)=1 / 1 (molar ratio)), The mixture was dissolved in a mixed solvent of 40 parts of 1,1,2,2,3,3,4-heptafluorocyclopentane (trade name: Zeorola H, manufactured by Zeon Corporation) and 55 parts of 1-propanol. Thereafter, 30 parts of tetrafluoroethylene resin powder (product name: Lubron L-2, manufactured by Daikin Industries, Ltd.) was added to the liquid, and the liquid was passed through a high-pressure disperser (product name: Microfluidizer M-110EH, manufactured by Microfluidics, Inc., USA) to obtain a dispersion liquid. after that, 52.0 parts of a hole transporting compound represented by the following formula (G), 16.0 parts of a compound represented by the following formula (H) (Aronix M-315, manufactured by Toagosei Co., Ltd.), 2.0 parts of a compound represented by the following formula (I) (manufactured by Sigma-Aldrich), Siloxane-modified acrylic compound, 0.75 parts (BYK-3550, manufactured by BYK Japan Co., Ltd.), 35 parts of 1,1,2,2,3,3,4-heptafluorocyclopentane and 15 parts of 1-propanol are added to the above dispersion, The mixture was filtered through a Polyflon filter (product name: PF-040, manufactured by Advantec Toyo Co., Ltd.) to prepare a coating solution for forming a protective layer. This protective layer forming coating solution was dip-coated on the charge transport layer, and the resulting coating film was dried at 40°C for 5 minutes. After drying, the coating film was irradiated with an electron beam for 1.6 seconds under nitrogen atmosphere at an acceleration voltage of 70KV and an absorbed dose of 15kGy. Then, the coating film was heat-treated for 15 seconds under nitrogen atmosphere at a temperature of 135°C. The oxygen concentration from the irradiation of the electron beam to the heat treatment for 15 seconds was 15ppm. Next, a heat treatment was performed for 1 hour in air under conditions where the coating film reached 105° C., forming a protective layer with a film thickness of 5 μm. In this manner, an electrophotographic photoreceptor was manufactured. [ka]

[0085] [Formation of recesses by transferring mold pressure shape] Next, the mold 403 shown in FIG. 3 was placed in a pressure-contact shape transfer processing device shown in FIG. 4, and the surface of the electrophotographic photosensitive member 401 before the formation of the recesses was processed. Specifically, in the mold used in the examples and comparative examples, the maximum width X of the convex shape shown in FIG. 3(b) (the maximum width in the axial direction of the electrophotographic photoreceptor when the convex part on the mold is viewed from above) was 50 μm. Also, the maximum length Y of the convex shape shown in FIG. 3(c) (the maximum length in the circumferential direction of the electrophotographic photoreceptor when the convex part on the mold is viewed from above) was 75 μm. The area ratio of the convex shape in the mold was 56%, and the height H of the convex shape was 4 μm. The area ratio is the ratio of the area of ​​the convex part to the entire surface when the mold is viewed from above. During processing, the temperatures of the electrophotographic photoreceptor and the mold were controlled so that the temperature of the surface of the electrophotographic photoreceptor was 120° C. Then, while pressing the electrophotographic photoreceptor and the pressure member against the mold with a pressure of 7.0 MPa, the electrophotographic photoreceptor was rotated in the circumferential direction to form recesses on the entire surface (peripheral surface) of the electrophotographic photoreceptor. In the manner described above, an electrophotographic photoreceptor for image evaluation in Example 1 was prepared.

[0086] [Image evaluation] As an electrophotographic device for evaluation, a copying machine imagePRESS C800 manufactured by Canon Inc. was used. As a photoreceptor, an electrophotographic photoreceptor prepared by the above-mentioned method was used. As a charging means, a method of applying a superimposed voltage of an AC voltage and a DC voltage to a roller-type contact charging member (charging roller) was used for evaluation. The evaluation device was placed in an environment with a temperature of 25°C and a humidity of 50% RH, and after printing 300,000 sheets using the electrophotographic photoreceptor prepared, it was confirmed whether or not there were any image defects caused by peeling of the photosensitive layer, such as white spots on halftone images. The evaluation results are shown in Table 2.

[0087] [Adhesion evaluation] The adhesion between the undercoat layer and the photosensitive layer was evaluated by the following method. A load was applied to 10 locations of the manufactured electrophotographic photoreceptor using a microhardness measuring device under the following conditions, and then the surface was observed using a laser microscope (product name: VK-200, manufactured by Keyence Corporation) with a 20x lens, and the average area where peeling of the film occurred was calculated. The smaller the area, the higher the adhesion. The measurement was carried out using a FISCHERSCOPE HM2000 (manufactured by Fischer Instruments) as the microhardness measuring device, under normal temperature and humidity conditions of an air temperature of 23°C and a relative humidity of 50%. A peeled area of ​​0 or more and 0.005 μm 2 When the adhesion is less than 0.005 μm, the adhesion is evaluated as (A). 2 More than 0.015μm 2 The adhesion evaluation is (B) when the thickness is less than 0.015 μm. 2 The adhesion in the above case was evaluated as (C), and the evaluation results are shown in Table 2. When the evaluation result is A or B, the effects of the present invention are obtained.

[0088] (Loading conditions) Indenter: A square pyramid-shaped diamond indenter (Vickers indenter) with an opposing angle of 136° Maximum set pressing load: 2,000mN Load application time: 0 seconds

[0089] [Evaluation of dispersibility of metal oxide particles in the undercoat layer] The dispersibility of the metal oxide particles in the undercoat layer was evaluated by the following method. Using a scanning electron microscope, 10 cross-sectional backscattered electron images of the undercoat layer of the electrophotographic photoreceptor were taken at an accelerating voltage of 2.0 kV. The 10 photographed locations were divided into 5 parts in the longitudinal direction of the electrophotographic photoreceptor and 2 parts in the circumferential direction. The scanning electron microscope used was an S-4800 (manufactured by Hitachi, Ltd.). Each of the cross-sectional backscattered electron image screens taken was a square with a side length of 0.9 μm. Each of the 10 cross-sectional backscattered electron image screens obtained was equally divided into 9 (3 × 3) screens, and the following calculations were performed using a total of 90 cross-sectional backscattered electron image screens. When the cross-sectional area of ​​the obtained cross-sectional backscattered electron image is S(α), S(α) is 0.09 μm 2The sum of the cross-sectional areas of the metal oxide particles observed in each of the 90 cross-sectional backscattered electron image segments was defined as S(β) m (m is 1 to 90) μm 2 The cross-sectional area of ​​the metal oxide particles was measured using the image processing software Image-Pro Plus5.1J (Media Cybernetics), with the brightness range set to 140-255 in the "brightness range selection" menu, and the high brightness parts of the image were extracted to obtain the cross-sectional area value. The cross-sectional area of ​​the cross-sectional backscattered electron image split screen was calculated by taking the sum of the cross-sectional areas of the metal oxide particles S(α), S(β), as A m (m is 1 to 90), and in each cross-sectional backscattered electron image division screen, A m Furthermore, A m The average value of A(ave.) and A m The standard deviation A(σ) of the above was calculated, and A(ave.) and A(σ) were compared and evaluated. A(ave.) is an indication of the amount of metal oxide particles contained on average at the measurement point. Therefore, A(ave.) is preferably 0.50 or more and 0.90 or less. It can be said that the smaller the standard deviation A(σ), the less the distribution of metal oxide particles in any cross section of the undercoat layer. Therefore, A(ave.) is preferably 0.15 or less. When A(σ) is 0.1 or less, the dispersibility is evaluated as (A), when it is 0.15 or less, the dispersibility is evaluated as (B), and when it is more than 0.15, the dispersibility is evaluated as (C). The evaluation results are shown in Table 2. When the evaluation result is A or B, the effect of the present invention is obtained.

[0090] (Examples 2 to 6) Except for changing the metal oxide particles S-1A used in the coating solution for the undercoat layer to metal oxide particles S-1B to S-1F, electrophotographic photoreceptors of Examples 2 to 6 were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0091] (Examples 7 to 9) Except for changing the metal oxide particles S-1A used in the coating solution for the undercoat layer to metal oxide particles T-1A, T-1B, and T-2A, respectively, electrophotographic photoreceptors of Examples 7 to 9 were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0092] Example 10 Except for changing the metal oxide particles S-1A used in the coating solution for the undercoat layer to the metal oxide particles Z-1A, an electrophotographic photoreceptor of Example 10 was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0093] Example 11 Except for omitting the silicone oil and 5-aminosalicylic acid used in the coating liquid for the undercoat layer, an electrophotographic photoreceptor of Example 11 was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0094] (Examples 12 to 14) Except for changing the thickness of the undercoat layer from 2.0 μm to 5.0 μm, 1.1 μm, and 0.9 μm, respectively, electrophotographic photoreceptors of Examples 12, 13, and 14 were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0095] Example 15 An electrophotographic photoreceptor of Example 15 was produced and evaluated in the same manner as in Example 1, except that the polyisocyanate compound having two or more isocyanate groups used in the coating liquid for the undercoat layer was changed to a bifunctional isocyanate compound (product name: Duranate D101, manufactured by Asahi Kasei Corporation). The results are shown in Table 2.

[0096] Example 16 An electrophotographic photoreceptor of Example 16 was produced and evaluated in the same manner as in Example 1, except that the surface treatment of the electrophotographic photoreceptor in Example 1 was changed to treatment using a polishing device described below. The results are shown in Table 2. The surface of the electrophotographic photoreceptor before surface polishing was polished. The polishing was performed using the polishing device shown in Fig. 5 under the following conditions. 501 is a polishing sheet, 502a to 502d are guide rollers, 503 is a backup roller, 504 is a processing target (electrophotographic photoreceptor before polishing), 505 is a winding means, and 506 is a hollow shaft. Abrasive sheet feed speed: 400mm / min Rotational speed of electrophotographic photoreceptor: 450 rpm Pressing of electrophotographic photoreceptor onto backup roller: 3.5mm Rotation direction of the abrasive sheet and electrophotographic photoreceptor; With Backup roller; outer diameter 100mm, Asker C hardness 25 The polishing sheet A to be attached to the polishing device was made using GC3000 and GC2000 manufactured by Riken Corundum Co., Ltd. GC3000 (polishing sheet surface roughness Ra0.83μm) GC2000 (abrasive sheet surface roughness Ra1.45μm) Abrasive sheet A (abrasive sheet surface roughness Ra1.12μm) The polishing time using the polishing sheet A was 20 seconds.

[0097] (Example 17) An electrophotographic photoreceptor of Example 17 was produced and evaluated in the same manner as in Example 1, except that in forming the protective layer in Example 1, the protective layer forming coating liquid was prepared by the method described below. The results are shown in Table 2. 95 parts of a compound represented by the following formula (L), 5 parts of a vinyl ester compound represented by the following formula (M) (manufactured by Tokyo Chemical Industry Co., Ltd.), Siloxane-modified acrylic compound (product name: BYK-3550, manufactured by BYK Japan Co., Ltd.) 3.5 parts, 5 parts of a urea compound represented by the following formula (N): 200 parts of 1-propanol, 100 parts of 1,1,2,2,3,3,4-heptafluorocyclopentane (product name: Zeorola H, manufactured by Zeon Corporation) was added and stirred. Thereafter, the solution was filtered through a Polyflon filter (product name: PF-020, manufactured by Advantec Toyo Co., Ltd.) to prepare a coating solution for forming a protective layer. [ka] This protective layer coating solution was dip-coated on the charge transport layer to form a coating film, and the resulting coating film was dried at 50°C for 10 minutes. Thereafter, under a nitrogen atmosphere, the coating film was irradiated with electron beams for 1.6 seconds while rotating the support (irradiated body) at a speed of 200 rpm under the conditions of an acceleration voltage of 70 kV and a beam current of 5.0 mA. The absorbed dose of the electron beam at this time was measured to be 15 kGy. Thereafter, the coating film was heated in a nitrogen atmosphere from 25°C to 117°C over 30 seconds. The oxygen concentration from the electron beam irradiation to the subsequent heat treatment was 15 ppm or less. Next, the coating film was naturally cooled in the atmosphere until the temperature reached 25°C, and then heat-treated for 30 minutes under conditions where the temperature of the coating film reached 105°C, forming a protective layer with a thickness of 5 μm.

[0098] (Example 18) An electrophotographic photoreceptor of Example 18 was produced and evaluated in the same manner as in Example 1, except that a conductive layer was provided between the support and the undercoat layer by the method described below. The results are shown in Table 2. A dispersion was prepared by dispersing 57 parts of titanium oxide particles having a coating layer (product name: Pastran LRS, manufactured by Mitsui Mining & Smelting Co., Ltd.), 35 parts of resol-type phenolic resin (product name: Phenolite J-325CAK, manufactured by DIC Corporation, a methanol solution with a solid content of 60%), and 33 parts of 2-methoxy-1-propanol for 3 hours in a sand mill using glass beads with a diameter of 1 mm. The average particle size of the powder contained in this dispersion was 0.30 μm. To this dispersion was added a liquid in which 8 parts of a silicone resin (product name: Tospearl 120, manufactured by Toshiba Silicones Co., Ltd.) was dispersed in 8 parts of 2-methoxy-1-propanol. Furthermore, 0.008 parts of silicone oil (product name: SH28PA, manufactured by Toray Silicone Co., Ltd.) was added. The dispersion thus prepared was applied onto an aluminum cylinder by dipping, and then heated and cured for 30 minutes in a hot air dryer adjusted to 150°C to harden the coating of the dispersion, thereby forming a conductive layer with a thickness of 30 μm.

[0099] Comparative Example 1 The metal oxide particles S-1A used in the coating solution for the undercoat layer were changed to particles produced by the following method. Except for the above, an electrophotographic photoreceptor of Comparative Example 1 was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2. Zinc oxide particles (specific surface area: 19 m 2 100 parts of zinc oxide (1.0 g, primary particle size 50 nm) were mixed with 500 parts of toluene by stirring. 0.8 parts of N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (product name: KBM602, Shin-Etsu Chemical Co., Ltd.) was added as a silane coupling agent, and the mixture was stirred for 6 hours. Thereafter, the toluene was distilled off under reduced pressure, and the mixture was dried by heating at 130°C for 6 hours to obtain surface-treated zinc oxide particles.

[0100] Comparative Example 2 The metal oxide particles S-1A used in the coating solution for the undercoat layer were changed to particles produced by the following method. Otherwise, an electrophotographic photoreceptor of Comparative Example 2 was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2. 100 parts of strontium titanate particles S-1 were mixed with 500 parts of toluene and stirred, 2.5 parts of dodecyltrimethoxysilane were added, and the mixture was stirred for 2 hours. After that, the toluene was distilled off by reduced pressure distillation, and the mixture was baked at 120°C for 3 hours to obtain surface-treated strontium titanate particles.

[0101] Comparative Example 3 Instead of the polyol compound having two or more hydroxyl groups and the polyisocyanate compound having two or more isocyanate groups used in the coating liquid for the undercoat layer, a phenol resin (product name: Phenolite J325CAK, manufactured by DIC Corporation) was used. Except for this, an electrophotographic photoreceptor of Comparative Example 3 was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0102] [Table 2]

[0103] From the results in Table 2, it is clear that the electrophotographic photoreceptors in the examples are superior in dispersibility and adhesion to the electrophotographic photoreceptors in the comparative examples, and also show improved image evaluation (poking) characteristics. [Explanation of symbols]

[0104] 1. Electrophotographic photoreceptor 2-axis 3. Charging means 4 Exposure light 5. Developing method 6 Transfer Method 7 Transfer material 8 Fixing Method 9 Cleaning Method 10 Pre-exposure light 11 Process cartridge 12 Guidance means 101 Support 102 Undercoat layer 103 Photosensitive layer

Claims

1. An electrophotographic photoreceptor having a support, an undercoat layer on the support, and a photosensitive layer on the undercoat layer, The undercoat layer is Metal oxide particles surface-treated with a silane coupling agent represented by the following formula (1): a polyol compound having two or more hydroxy groups, and Polyisocyanate compound having two or more isocyanate groups 1. An electrophotographic photoreceptor comprising a cured film of a composition comprising: 【Chemistry 1】 (In formula (1), R 1 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 2 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 3 represents a hydroxy group, an alkoxy group, or an alkyl group having 1 to 4 carbon atoms. 4 represents an alkylene group having 1 to 4 carbon atoms.

2. 2. The electrophotographic photoreceptor according to claim 1, wherein the metal oxide particles are anatase type titanium oxide particles.

3. 2. The electrophotographic photoreceptor according to claim 1, wherein the metal oxide particles are strontium titanate particles.

4. 4. The electrophotographic photoreceptor according to claim 1, wherein the undercoat layer contains a compound selected from the group consisting of compounds represented by the following formula (2): 【Chemistry 2】 (In formula (2), R 11 ~R 15 each independently represents a hydrogen atom, a hydroxyl group, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, or an amino group. A 1 represents a hydroxy group, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms.

5. 5. The electrophotographic photoreceptor according to claim 4, wherein the compound represented by the formula (2) is aminosalicylic acid.

6. 6. The electrophotographic photoreceptor according to claim 1, wherein the undercoat layer has a thickness of 1.0 μm or more.

7. 7. The electrophotographic photoreceptor according to claim 6, wherein the undercoat layer has a thickness of 5.0 [mu]m or less.

8. Using a scanning electron microscope, 10 cross-sectional backscattered electron images of the undercoat layer were taken at an accelerating voltage of 2.0 kV to obtain a total of 10 cross-sectional backscattered electron image screens (squares with one side of 0.9 μm). Each of the obtained 10 cross-sectional backscattered electron image screens is equally divided into 9 (3 × 3) to obtain a total of 90 cross-sectional backscattered electron image split screens, The cross-sectional area of ​​the obtained cross-sectional reflected electron image divided screen is defined as S(α) μm 2 (=0.09 μm 2 ), and the sum of the cross-sectional areas of the metal oxide particles observed in each of the 90 cross-sectional backscattered electron image division screens obtained is defined as S(β) m (m is 1 to 90) μm 2 Let S(β) m ÷S(α) to A m (m is 1 to 90), and A m The average value of A (ave.) is A m 8. The electrophotographic photoreceptor according to claim 6, wherein, when the standard deviation of the above is A(σ), A(ave.) is 0.50 or more and 0.90 or less, and A(σ) is 0.1 or less.

9. 9. A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of claims 1 to 8 and at least one means selected from the group consisting of a charging means, a developing means, a transfer means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

10. 9. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging means, an exposing means, a developing means, and a transferring means.

11. A method for producing an electrophotographic photoreceptor having a support, an undercoat layer, and a photosensitive layer, comprising the steps of: Metal oxide particles surface-treated with a silane coupling agent represented by the following formula (1): A polyol compound having two or more hydroxy groups, A polyisocyanate compound having two or more isocyanate groups; Contains a coating liquid preparation step of preparing a coating liquid for forming an undercoat layer, the coating liquid having a content of the surface-treated metal oxide particles of 50% by mass or more and 90% by mass or less after drying; a coating step of coating the undercoat layer-forming coating liquid on the support to form a coating film; A drying step of drying the coating film at a high temperature; Equipped with A method for producing an electrophotographic photoreceptor, comprising the step of forming a photosensitive layer on the undercoat layer. 【Chemistry 3】 (In formula (1), R 1 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 2 R represents a hydroxy group or an alkoxy group having 1 to 4 carbon atoms. 3 is a hydroxy group, an alkoxy group having 1 to 4 carbon atoms, or an alkyl group having 1 to 4 carbon atoms. 4 is an alkylene group having 1 to 4 carbon atoms.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP2012063447A

  • Electrophotographic photoreceptor, process cartridge, electrophotographic device, and method for producing electrophotographic photoreceptor

    JP2017181804A

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP2018010240A

  • Image forming apparatus, process cartridge, and image forming method

    JP2019003131A

  • Electrophotographic photosensitive member, process cartridge and electrophotographic apparatus

    JP2019061051A