Electrophotographic photoreceptor, process cartridge, and electrophotographic apparatus

By controlling the crystal orientation of the support's surface to specific ranges, the photoreceptor addresses peeling issues, ensuring image quality in diverse environments.

JP7566963B2Active Publication Date: 2024-10-15CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052161
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-03-28
Publication Date
2024-10-15
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Electrophotographic photoreceptors face issues with the photosensitive layer peeling off from the support when stored in low-temperature or high-temperature environments, leading to image blurring.

Method used

The photoreceptor features a cylindrical support with a controlled crystal orientation, where the surface of the support is composed of Al and/or Al alloy, with specific crystal grain orientations and area ratios, including {111} orientation of -15° to +15°, to enhance adhesion and resist thermal distortion.

Benefits of technology

This configuration suppresses peeling of the photosensitive layer, maintaining image quality by preventing blurring even in varying temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566963000008
    Figure 0007566963000008
  • Figure 0007566963000009
    Figure 0007566963000009
  • Figure 0007566963000010
    Figure 0007566963000010
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor that can prevent a photosensitive layer from being peeled off from a support and prevent a blur of dots forming an output image even when it is used after storage in a low temperature or high temperature environment.SOLUTION: An electrophotographic photoreceptor has a cylindrical support and a photosensitive layer. A surface of the support is formed of Al and / or an Al alloy. The surface of the support is formed of crystal grains of Al having (α) a surface of -15° or more and less than +15° in the {001} orientation, (β) a surface of -15° or more and less than +15° in the {101} orientation, and (γ) a surface of -15° or more and less than +15° in the {111} orientation. The ratio of the area occupied by the crystal grains of Al having the (α) to the total area of the surface of the support is 10% or less. The ratio of the area occupied by the crystal grains of Al having the (γ) to the total area of the surface of the support exceeds 10%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, a process cartridge having the electrophotographic photoreceptor, and an electrophotographic apparatus having the electrophotographic photoreceptor. [Background technology]

[0002] In recent years, the users of electrophotographic apparatuses have become increasingly diversified, and there is an increasing need for electrophotographic photoreceptors that can withstand a variety of storage conditions and usage environments. Patent Document 1 describes a technique for improving image quality, in which the internal stress value of a conductive support is set in the range of −30 MPa or more and 5 MPa or less. Patent Document 2 describes a technique for improving image quality from the standpoint of precision, in which an aluminum alloy raw tube is heated to 190° C. to 550° C. before cutting. In addition, Patent Document 3 discloses a method for determining the average area of ​​crystal grains of an Al alloy having a specific composition to be 3 μm 2 More than 100μm 2 The following techniques are described: [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 077705 [Patent Document 2] JP 2009-150958 A [Patent Document 3] JP 2017-111409 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the investigations of the present inventors, the electrophotographic photoreceptors described in Patent Documents 1 to 3 have a problem in that the photosensitive layer is easily peeled off from the support when used after storage in a low-temperature or high-temperature environment. Therefore, an object of the present invention is to provide an electrophotographic photoreceptor capable of suppressing peeling of a photosensitive layer from a support even when used after storage in low-temperature or high-temperature environments. [Means for solving the problem]

[0005] The above object can be achieved by the present invention described below. That is, an electrophotographic photoreceptor according to one embodiment of the present invention is an electrophotographic photoreceptor having a cylindrical support and a photosensitive layer, The surface of the support is formed of Al and / or an Al alloy, The surface of the support is (α) {001} orientation: -15° to +15° (β) {101} orientation faces between -15° and +15° (γ) {111} orientation: -15° to +15° The grains of Al have the following structure: The ratio of the area occupied by the Al crystal grains having (α) to the total area of ​​the surface of the support is 10% or less, and the ratio of the area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is greater than 10%.

[0006] Furthermore, a process cartridge according to another aspect of the present invention is characterized in that it integrally supports the above-mentioned electrophotographic photosensitive member and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably attachable to the main body of the electrophotographic apparatus.

[0007] Further, an electrophotographic apparatus according to still another aspect of the present invention comprises the above electrophotographic photoreceptor, as well as a charging means, an exposing means, a developing means, and a transferring means. Effect of the Invention

[0008] According to the present invention, it is possible to provide an electrophotographic photoreceptor which can suppress peeling of a photosensitive layer from a support even when used after storage in low-temperature or high-temperature environments, and as a result, can suppress blurring of dots forming an output image. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram showing the distribution of Al crystal grains. [Diagram 2] FIG. 1 is a diagram showing measurement positions of Al crystal grains. [Diagram 3] FIG. 1 is a diagram showing an example of a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below with reference to preferred embodiments. The present inventors have found through their investigations that in the techniques described in Patent Documents 1 to 3, minute differences in crystal orientation in the conductive support may cause a decrease in adhesion between the support and the photosensitive layer of the electrophotographic photoreceptor during storage in low-temperature or high-temperature environments. This is believed to have caused the coating film to peel off easily after storage in harsh environments. In order to solve the above-mentioned technical problems occurring in the conventional techniques, the present inventors have investigated the crystal orientation of the surface of an aluminum support. As a result of the above-mentioned investigation, it has been found that the above-mentioned technical problems can be solved by using the electrophotographic photoreceptor according to the present invention described below.

[0011] That is, the electrophotographic photoreceptor according to the present invention is an electrophotographic photoreceptor having a cylindrical support and a photosensitive layer, The surface of the support is formed of Al and / or an Al alloy, The surface of the support is (α) {001} orientation: -15° to +15° (β) {101} orientation faces between -15° and +15° (γ) {111} orientation: -15° to +15° The grains of Al have the following structure: The ratio of the area occupied by the Al crystal grains having (α) to the total area of ​​the surface of the support is 10% or less, and the ratio of the area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is greater than 10%. In the present invention, for example, a plane at an angle of −15° or more and less than +15° to the {111} orientation refers to a crystal plane having a deviation of −15° or more and less than +15° from the {111} plane in an aluminum crystal.

[0012] The present inventors consider the mechanism by which the above-mentioned configuration of the present invention can solve the above-mentioned technical problems in the prior art as follows. The crystal orientations of aluminum are roughly divided into three: {101} orientation, {001} orientation, and {111} orientation. As described in "Koberunix" ([No.28] Vol.14 2005.OCT), crystal grains with each crystal orientation are usually randomly distributed, as shown in Figure 1(a). The inventors speculate that since the properties of thermal contraction differ slightly depending on the crystal orientation, the adhesion between the support and the coating resin forming the photosensitive layer differs depending on the crystal orientation, and that crystal grains on the surface of the {111} orientation at -15° or more and less than +15° and crystal grains on the surface of the {101} orientation at -15° or more and less than +15° have higher resin adhesion under a wider range of temperature and humidity conditions than crystal grains on the surface of the {001} orientation at -15° or more and less than +15°. In particular, the inventors speculate that crystal grains on the surface of the {111} orientation at -15° or more and less than +15° have higher resin adhesion under a wider range of temperature and humidity conditions than crystal grains on the surface of the {001} orientation at -15° or more and less than +15° and crystal grains on the surface of the {101} orientation at -15° or more and less than +15°.

[0013] In the aluminum support used in the prior art, crystal grains of three different crystal orientations are randomly present, resulting in minute differences in adhesion at the interface between the support and the coating. This is thought to have caused the coating to peel off, particularly in storage environments with large thermal distortion. Therefore, the surface of the aluminum support is formed in a state where it is rich in crystal grains having faces with an angle of -15° or more and less than +15° in the {111} orientation, which is assumed to have high film adhesion, as shown in Figure 1(b). This is thought to suppress thermal distortion of the surface of the aluminum support and improve minute differences in adhesion, thereby suppressing peeling of the coating film.

[0014] [Electrophotographic photoreceptor] The electrophotographic photoreceptor according to the present invention has a cylindrical support and a photosensitive layer. The method for producing the electrophotographic photoreceptor according to the present invention includes a method in which the coating liquid for each layer described below is prepared, coated in the desired order, and dried. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoint of efficiency and productivity. The support and each layer will be described below.

[0015] <Support> The electrophotographic photoreceptor according to the present invention has a cylindrical support, and the surface of the support is made of at least one selected from Al and Al alloys. The surface of the support may be subjected to a hot water treatment, a blasting treatment, a cutting treatment, or the like.

[0016] (1) Crystal orientation In the present invention, the expression of the crystal orientation of Al in the surface direction of the support surface, for example, the {001} oriented plane, is a representation of the crystal plane of Al in Miller indices. That is, the {001} oriented plane is a comprehensive expression of Miller indices indicating any of the crystal lattice planes (001), (010), (100), (00-1), (0-10), and (-100).

[0017] In the present invention, the surface of the support is (α) {001} orientation: -15° to +15° (β) {101} orientation faces between -15° and +15° (γ) {111} orientation: -15° to +15° The grains of Al have the following structure: The ratio of the area occupied by the Al crystal grains having the (α) to the total area of ​​the surface of the support is 10% or less, and the ratio of the area occupied by the Al crystal grains having the (γ) to the total area of ​​the surface of the support exceeds 10%.

[0018] From the viewpoint of increasing the surface area of ​​the support with small thermal distortion, the ratio of the area occupied by the Al crystal grains having (γ) is preferably 11% or more, more preferably 50% or more. Furthermore, the ratio of the area occupied by the Al crystal grains having (γ) is more preferably 75% or more. In particular, when the ratio of the area occupied by the Al crystal grains having (γ) is 75% or more, the effect of the present invention can be obtained more effectively.

[0019] From the viewpoint of reducing the number of faces that are subject to large thermal distortion, it is preferable that the ratio of the area occupied by Al crystal grains having (α) is 5% or less.

[0020] (Method for measuring crystal orientation of Al crystal grains on the surface of the support) In the present invention, the crystal orientation of Al crystal grains on the surface of the support can be measured, for example, as follows.

[0021] First, the surface of the support is treated with buff polishing and a sodium hydroxide aqueous solution, and the crystal orientation of the Al crystal grains is measured at a point within 20 μm from the surface of the support before treatment. The measurement of the crystal orientation is preferably performed by the SEM-EBSP method.

[0022] Measurements using the SEM-EBSP method use a FE-SEM (Field Emission-Scanning Electron Microscope) equipped with an EBSP (Electron Back Scatter Diffraction Pattern) detector. Here, EBSP refers to the Kikuchi pattern (Kikuchi line) obtained from the reflected electrons generated when an electron beam is incident on the surface of the test piece, and by analyzing this pattern, the crystal orientation of the electron beam incident position can be determined. In addition, the Kikuchi pattern refers to a pattern that appears behind the electron diffraction image as a pair of black and white parallel lines, bands, or arrays when an electron beam hits a crystal and is scattered and diffracted. As an FE-SEM equipped with an EBSP detector, for example, a field emission scanning electron microscope (product name: JSM-6500F, manufactured by JEOL Ltd.) can be used.

[0023] (2) Area of ​​Al crystal grains on the surface of the support In the present invention, the surface of the support is (α) {001} orientation: -15° to +15° (β) {101} orientation faces between -15° and +15° (γ) {111} orientation: -15° to +15° The grains of Al have the following structure: The ratio of the area occupied by the Al crystal grains having the (α) to the total area of ​​the surface of the support is 10% or less, and the ratio of the area occupied by the Al crystal grains having the (γ) to the total area of ​​the surface of the support exceeds 10%.

[0024] The proportion of the area occupied by Al crystal grains having each of the above crystal orientations can be determined as follows. As shown in Figure 2, first, positions are determined in the axial direction from either end of the support, which correspond to 1 / 8, 2 / 8, 3 / 8, 4 / 8, 5 / 8, 6 / 8, and 7 / 8 of the total length. Each position is then divided into four circumferential sections at 90° intervals. At each of the 28 points where the axial and circumferential dividing lines intersect, a 100 μm square region is set so that the intersection of the axial and circumferential dividing lines is at the center, and the crystal orientation is measured in this measurement region using the SEM-EBSP method described above. Next, the area occupied by each orientation is calculated for Al crystal grains having the (α), (β), and (γ) crystal orientations, and the obtained values ​​are multiplied by 10,000 μm. 2 The ratio of the area occupied by Al crystal grains with each crystal orientation in each region is determined by dividing by . Finally, the average value obtained from each of the 28 regions is determined as the ratio of the area occupied by (α), (β), and (γ) of the support. The area occupied by Al crystal grains having each crystal orientation may be calculated using software attached to the microscope. For example, the orientation obtained by measurement may be determined using the hue h of the HSV color space to define the range of (α) as 0≦h<60 and 300≦h<360, the range of (β) as 60≦h<180, and the range of (γ) as 180≦h<300, and the area occupied by Al crystal grains having each crystal orientation may be calculated by performing hue mapping of the region of Al crystal grains having each crystal orientation.

[0025] (3) Aluminum alloy for use as a support From the viewpoint of controlling the crystal orientation, the support is preferably a 3000 series Al alloy, for example, a JIS designated A3003 alloy, or a 6000 series Al alloy, for example, a JIS designated A6063 alloy. Specifically, the JIS designated A3003 alloy is an Al alloy containing 0.6 mass% or less of Si, 0.7 mass% or less of Fe, 0.05 mass% or more and 0.2 mass% or less of Cu, 1.0 mass% or more and 1.5 mass% or less of Mn, and 0.1 mass% or less of Zn. Specifically, the JIS designated A6063 alloy is an Al alloy containing 0.2 mass% or more and 0.6 mass% or less of Si, 0.35 mass% or less of Fe, 0.1 mass% or less of Cu, 0.1 mass% or less of Mn, 0.1 mass% or more and 0.45 mass% or more and 0.9 mass% or less of Mg, 0.1 mass% or less of Cr, 0.1 mass% or less of Zn, and 0.1 mass% or less of Ti.

[0026] (4) Method of manufacturing the support The method for producing the support is not particularly limited as long as it is a method capable of producing a support that satisfies the requirements of the present invention. An example of a method for producing a support includes the following four steps. A first step of preparing a specific Al alloy and performing hot extrusion to obtain a molded body; A second step of cold drawing the molded body obtained in the first step; A third step of annealing after the second step, and The fourth process is to cut the surface after annealing.

[0027] When controlling the crystal orientation by annealing, it is possible to control the crystal orientation by adjusting the heating rate, the annealing temperature, the time for which the annealing temperature is maintained, and the cooling rate. In particular, by setting the cooling rate to 5°C / min or more until the temperature of the support reaches 150°C, the appearance of Al crystal grains having the (α) crystal orientation is suppressed and Al crystal grains having the (γ) crystal orientation are more likely to appear on the surface. As a result, the proportion of the area of ​​the support surface occupied by Al crystal grains having the (α) crystal orientation decreases and the proportion of the area occupied by Al crystal grains having the (γ) crystal orientation increases.

[0028] Furthermore, since changes also occur depending on the heating rate and annealing temperature, it is preferable to control the heating rate to 40°C / min or less and the annealing temperature to 400°C or more and 450°C or less. Moreover, it is preferable that the annealing temperature is maintained for one hour or less.

[0029] In addition, since the thermal history is important in controlling the crystal orientation, it is preferable to anneal the material that has been subjected to the above-mentioned steps of hot extrusion and cold drawing before use.

[0030] <Conductive layer> In the present invention, a conductive layer may be provided on the support. By providing the conductive layer, scratches and irregularities on the surface of the support can be concealed and light reflection on the surface of the support can be controlled. The conductive layer preferably contains conductive particles and a resin.

[0031] The conductive particles may be made of a material such as metal oxide, metal, or carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure having a core particle and a coating layer that covers the core particle. Examples of the core particle include titanium oxide, barium sulfate, zinc oxide, etc. Examples of the coating layer include metal oxides such as tin oxide. When a metal oxide is used as the conductive particles, the volume average particle size is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less.

[0032] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like.

[0033] The thickness of the conductive layer is preferably from 1 μm to 50 μm, and particularly preferably from 3 μm to 40 μm.

[0034] The conductive layer can be formed by preparing a coating solution for the conductive layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the coating solution for the conductive layer include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser.

[0035] <Undercoat layer> In the present invention, an undercoat layer may be provided on the support or the conductive layer. By providing an undercoat layer, the adhesion between layers can be improved and a charge injection blocking function can be imparted. The undercoat layer preferably contains a resin. Alternatively, the undercoat layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group.

[0036] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl phenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin.

[0037] Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.

[0038] For the purpose of improving electrical properties, the undercoat layer may further contain an electron transporting material, a metal oxide, a metal, a conductive polymer, etc. Among these, it is preferable to use an electron transporting material or a metal oxide.

[0039] Examples of the electron transport substance include a quinone compound, an imide compound, a benzimidazole compound, a cyclopentadienylidene compound, a fluorenone compound, a xanthone compound, a benzophenone compound, a cyanovinyl compound, an aryl halide compound, a silole compound, a boron-containing compound, etc. An electron transport substance having a polymerizable functional group may be used as the electron transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the electron transport substance with the monomer having the polymerizable functional group described above.

[0040] Metal oxides include indium tin oxide, tin oxide, indium oxide, titanium oxide, zinc oxide, aluminum oxide, silicon dioxide, etc. Metals include gold, silver, aluminum, etc. The undercoat layer may further contain an additive.

[0041] The thickness of the undercoat layer is preferably from 0.1 μm to 50 μm, more preferably from 0.2 μm to 40 μm, and particularly preferably from 0.3 μm to 30 μm.

[0042] The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0043] <Photosensitive layer> The photosensitive layer of an electrophotographic photoreceptor is mainly classified into (1) a laminated type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The laminated type photosensitive layer is a photosensitive layer having a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer is a photosensitive layer containing both a charge generation material and a charge transport material.

[0044] (1) Laminated photosensitive layer The laminated type photosensitive layer has a charge generating layer and a charge transport layer.

[0045] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin.

[0046] Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer.

[0047] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable.

[0048] The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds.

[0049] The thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm.

[0050] The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming the coating film on a support, a conductive layer, or an undercoat layer, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0051] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin.

[0052] Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred. The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer.

[0053] Examples of the resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10.

[0054] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.

[0055] The thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm.

[0056] The charge transport layer can be formed by preparing a coating solution for the charge transport layer containing the above-mentioned materials and solvent, forming the coating film on the charge generating layer, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred.

[0057] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming the coating film on a support, a conductive layer or an undercoat layer, and drying it. The charge generating material, the charge transporting material and the resin are the same as the examples of materials in "(1) Multi-layer type photosensitive layer" above.

[0058] <Protective layer> In the present invention, a protective layer may be provided on the photosensitive layer. By providing the protective layer, durability can be improved. The protective layer preferably contains conductive particles and / or a charge transport material, and a resin.

[0059] The conductive particles include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide. Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these materials. Among these, triarylamine compounds and benzidine compounds are preferred. Examples of the resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among them, polycarbonate resin, polyester resin, and acrylic resin are preferable.

[0060] The protective layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the reaction include thermal polymerization, photopolymerization, and radiation polymerization. Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an acryloyl group and a methacryloyl group. A material having a charge transport function may be used as the monomer having a polymerizable functional group.

[0061] The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, abrasion resistance improvers, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.

[0062] The thickness of the protective layer is preferably from 0.5 μm to 10 μm, and more preferably from 1 μm to 7 μm.

[0063] The protective layer can be formed by preparing a coating solution for the protective layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0064] [Process cartridges, electrophotographic devices] The process cartridge according to the present invention is characterized in that it integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably attachable to the main body of the electrophotographic apparatus. The electrophotographic apparatus according to the present invention is characterized by having the electrophotographic photosensitive member described above, as well as a charging means, an exposing means, a developing means, and a transferring means.

[0065] FIG. 3 shows an example of a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. A cylindrical electrophotographic photoreceptor 1 is rotated at a predetermined peripheral speed in the direction of the arrow around an axis 2. The surface of the electrophotographic photoreceptor 1 is charged by charging means 3 to a predetermined positive or negative potential. Although FIG. 3 shows a roller charging method using a roller-type charging member, other charging methods such as a corona charging method, a proximity charging method, and an injection charging method may also be used. Exposure light 4 is irradiated from an exposure means (not shown) onto the charged surface of the electrophotographic photoreceptor 1, and an electrostatic latent image corresponding to the target image information is formed. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 1 is developed with toner contained in a development means 5, and a toner image is formed on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor 1 is transferred to a transfer material 7 by a transfer means 6. The transfer material 7 to which the toner image has been transferred is transported to a fixing means 8, where the toner image is fixed, and the resulting image is printed out outside the electrophotographic device. The electrophotographic apparatus may have a cleaning unit 9 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 1 after transfer. Alternatively, a so-called cleanerless system may be used in which the deposits are removed by the developing unit 5 or the like without providing a separate cleaning unit 9. The electrophotographic apparatus may have a charge eliminating mechanism that eliminates charge on the surface of the electrophotographic photosensitive member 1 by pre-exposure light 10 from pre-exposure means (not shown). In addition, in order to mount and remove the process cartridge 11 according to the present invention to the main body of the electrophotographic apparatus, a guide means 12 such as a rail may be provided.

[0066] The electrophotographic photoreceptor according to the present invention can be used in laser beam printers, LED printers, copiers, facsimiles, and multifunction machines thereof. EXAMPLES

[0067] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples without departing from the gist of the present invention. In the following examples, "parts" are based on mass unless otherwise specified.

[0068] [Manufacture of support] The support was prepared in the following manner.

[0069] (Production Example of Support A-1) A hot extruded pipe made of JIS A3003 alloy was cold drawn to obtain a drawn pipe having an outer diameter of 30.8 mm, an inner diameter of 28.5 mm and a length of 370 mm. The drawn tube was then placed in an electric furnace, heated at a rate of 5°C / min, and maintained at 450°C for 1 hour. It was then cooled at a rate of 15°C / min until the drawn tube reached 150°C, and removed from the electric furnace after 24 hours. After annealing, the surface was mirror-finished to obtain "Support A-1" having an outer diameter of 30.5 mm, an inner diameter of 28.5 mm, and a length of 370 mm. The manufacturing conditions for Support A-1 are shown in Table 1. An elemental analysis of the drawn pipe used revealed that it was an Al alloy containing 0.3 mass% Si, 0.4 mass% Fe, 0.1 mass% Cu, 1.2 mass% Mn, and 0.05 mass% Zn.

[0070] (Production Examples of Supports A-2 to A-16) Supports A-2 to A-16 were produced in the same manner as in the production example of Support A-1, except that the same drawn pipe was used and the annealing conditions were changed as shown in Table 1.

[0071] (Production Example of Support A-17) A hot extruded pipe made of JIS A5005 alloy was cold drawn to obtain a drawn pipe having an outer diameter of 30.8 mm, an inner diameter of 28.5 mm and a length of 370 mm. The drawn tube was then placed in an electric furnace, heated at a rate of 5°C / min, and maintained at 450°C for 1 hour. It was then cooled at a rate of 15°C / min until the drawn tube reached 150°C, and removed from the electric furnace after 24 hours. After annealing, the surface was mirror-finished to obtain "Support A-17" having an outer diameter of 30.5 mm, an inner diameter of 28.5 mm, and a length of 370 mm. The manufacturing conditions for Support A-17 are shown in Table 1. Elemental analysis of the drawn pipe used revealed that it was an Al alloy containing 0.25 mass% Si, 0.3 mass% Fe, 0.04 mass% Cu, 0.1 mass% Mn, 0.9 mass% Mg, 0.06 mass% Cr, 0.08 mass% Zn, and 0.06 mass% Ti.

[0072] (Production Example of Support A-18) A hot extruded pipe made of JIS A6063 alloy was cold drawn to obtain a drawn pipe having an outer diameter of 30.8 mm, an inner diameter of 28.5 mm and a length of 370 mm. The drawn tube was then placed in an electric furnace, heated at a rate of 5°C / min, and maintained at 450°C for 30 minutes. It was then cooled at a rate of 15°C / min until the drawn tube reached 150°C, and removed from the electric furnace after 24 hours. After annealing, the surface was mirror-finished to obtain "Support A-18" having an outer diameter of 30.5 mm, an inner diameter of 28.5 mm, and a length of 370 mm. The manufacturing conditions for Support A-18 are shown in Table 1. Elemental analysis of the drawn pipe used revealed that it was an Al alloy containing 0.5 mass% Si, 0.6 mass% Fe, 0.2 mass% Cu, 0.1 mass% Mn, and 0.8 mass% Zn.

[0073] (Production Examples of Supports B-1 to B-12) Substrates B-1 to B-12 were produced in the same manner as in the production example of Substrate A-1, except that the annealing conditions were changed as shown in Table 1 in the production example of Substrate A-1.

[0074] (Production Examples of Support B-13 and Support B-14) A drawn pipe made of an Al-Mg alloy containing 2.5 mass% magnesium, having an outer diameter of 30.8 mm, an inner diameter of 28.5 mm, and a length of 370 mm, was used and annealed under the conditions shown in Table 1. After annealing, the surface was mirror-finished to obtain "supports B-13 and B-14" having an outer diameter of 30.5 mm, an inner diameter of 28.5 mm, and a length of 370 mm. The manufacturing conditions for support B-13 and support B-14 are shown in Table 1.

[0075] [Table 1]

[0076] <Manufacture of electrophotographic photoreceptor> (Production example of photoreceptor A-1) Support A-1 was used as the support. Next, zinc oxide particles (specific surface area: 19 m) were used as a metal oxide. 2 / g, powder resistance: 3.6×10 6 100 parts of the zinc oxide powder (Voltage density: Ω·cm) was mixed with 500 parts of toluene and stirred, to which 0.8 parts of a silane coupling agent was added and stirred for 6 hours. The silane coupling agent used was N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (product name: KBM602, Shin-Etsu Chemical Co., Ltd.). The toluene was then distilled off under reduced pressure, and the mixture was dried by heating at 130°C for 6 hours to obtain surface-treated zinc oxide particles.

[0077] Next, the following materials were prepared: - 15 parts of butyral resin (product name: BM-1, manufactured by Sekisui Chemical Co., Ltd.) as polyol resin Blocked isocyanate (product name: Sumidur 3175, manufactured by Sumika Bayer Urethane Co., Ltd.) 15 parts These were dissolved in a mixed solution of 73.5 parts of methyl ethyl ketone and 73.5 parts of 1-butanol. To this solution, 80.8 parts of the above-mentioned surface-treated zinc oxide particles and 0.8 parts of 2,3,4-trihydroxybenzophenone (manufactured by Tokyo Chemical Industry Co., Ltd.) were added, and the mixture was dispersed in a sand mill using glass beads with a diameter of 0.8 mm under an atmosphere of 23±3°C for 3 hours. Next, the following materials were prepared: Silicone oil (product name: SH28PA, manufactured by Toray Dow Corning Silicone Co., Ltd.) 0.01 part Cross-linked polymethylmethacrylate (PMMA) particles (product name: TECHPOLYMER SSX-102, manufactured by Sekisui Chemical Co., Ltd., average primary particle size 2.5 μm) 5.6 parts These were added to the above-mentioned dispersed solution and stirred to prepare a coating solution for the undercoat layer. This coating liquid for forming an undercoat layer was dip-coated onto the above-mentioned support A-1, and the resulting coating film was dried at 160° C. for 40 minutes to form an undercoat layer with a thickness of 18 μm.

[0078] Next, the following materials were prepared: 20 parts of hydroxygallium phthalocyanine crystal (charge generating material) in a crystal form having peaks at 7.4° and 28.2° of the Bragg angle 2θ±0.2° in CuKα characteristic X-ray diffraction 0.2 parts of a calixarene compound represented by the following formula (A): [ka] Polyvinyl butyral (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.) 10 parts 600 parts cyclohexanone These were placed in a sand mill using 1 mm diameter glass beads and dispersed for 4 hours. Then, 700 parts of ethyl acetate were added to prepare a coating solution for the charge generation layer. This coating solution for the charge generation layer was dip-coated on the undercoat layer, and the resulting coating was dried at 80°C for 15 minutes to form a charge generation layer with a thickness of 0.17 μm.

[0079] Next, the following materials were prepared: 30 parts of a compound represented by the following formula (B) (charge transport material) 60 parts of a compound represented by the following formula (C) (charge transport material) 10 parts of a compound represented by the following formula (D) (charge transport material) [ka] Polycarbonate resin (product name: Iupilon Z400, manufactured by Mitsubishi Engineering Plastics Corporation, bisphenol Z type polycarbonate) 100 parts 0.02 parts of polycarbonate resin having copolymer units of the following structural formula (E-1) and the following structural formula (E-2) (x / y=0.95 / 0.05: viscosity average molecular weight Mv=20,000) [ka] [ka] These were dissolved in a mixed solvent of 600 parts of mixed xylene and 200 parts of dimethoxymethane to prepare a coating solution for the charge transport layer. The coating solution for the charge transport layer was dip-coated onto the charge generating layer to form a coating film, and the resulting coating film was dried at 100° C. for 30 minutes to form a charge transport layer with a thickness of 18 μm.

[0080] Next, a mixed solvent of 20 parts of 1,1,2,2,3,3,4-heptafluorocyclopentane (trade name: Zeorola H, manufactured by Zeon Corporation) and 20 parts of 1-propanol was filtered through a Polyflon filter (trade name: PF-040, manufactured by Advantec Toyo Co., Ltd.). The following materials were also prepared: 90 parts of a hole transporting compound represented by the following formula (F): [ka] 70 parts of 1,1,2,2,3,3,4-heptafluorocyclopentane 70 parts 1-propanol These were added to the mixed solvent. The mixture was filtered with a polyflon filter (product name: PF-020, manufactured by Advantec Toyo) to prepare a coating solution for the second charge transport layer (protective layer). The coating solution for the second charge transport layer was dip-coated on the charge transport layer, and the resulting coating film was dried at 50°C for 6 minutes in air. Thereafter, the coating film was irradiated with an electron beam for 1.6 seconds under conditions of an acceleration voltage of 70 kV and an absorbed dose of 8000 Gy while rotating the support (irradiation target) at 200 rpm in nitrogen. The coating film was then heated from 25°C to 125°C in nitrogen over 30 seconds. The oxygen concentration of the atmosphere during the electron beam irradiation and subsequent heating was 15 ppm. Next, a heat treatment was performed at 100°C in air for 30 minutes to form a second charge transport layer (protective layer) having a thickness of 5 μm that was cured by the electron beam.

[0081] Next, linear grooves were formed on the surface of the protective layer using an abrasive sheet (product name: GC3000, manufactured by Riken Corundum). The feed speed of the abrasive sheet was 40 mm / min, the rotation speed of the workpiece was 240 rpm, and the abrasive sheet pressing pressure against the workpiece was 7.5 N / m. 2 The feed direction of the abrasive sheet and the rotation direction of the workpiece were the same. A backup roller with an outer diameter of 40 cm and an Asker C hardness of 40 was used. Under these conditions, linear grooves were formed on the peripheral surface of the workpiece for 10 seconds. In this manner, photoreceptor A-1 was produced.

[0082] (Production Examples of Photoreceptors A-2 to A-18, and B-1 to B-14) Electrophotographic photoreceptors were produced in the same manner as for photoreceptor A-1, except that the supports shown in Table 2 were used. The obtained electrophotographic photoreceptors are referred to as "Photoreceptor A-2 to Photoreceptor A-18, Photoreceptor B-1 to Photoreceptor B-14."

[0083] [evaluation] Photoreceptor A-1 was prepared and evaluated in a scratch test as follows. First, the photoreceptor A-1 was stored in a high-temperature and high-humidity environment of 40°C / 90%RH for 7 days, and then in a low-temperature and low-humidity environment of 5°C / 20%RH for 7 days. After that, the photoreceptor A-1 was transferred to a normal temperature and normal humidity environment of 23°C / 50%RH, the protective layer was removed with an abrasive sheet, and the photosensitive layer was removed with methyl ethyl ketone to expose the undercoat layer, thereby obtaining a sample for scratch test evaluation. From either end of the evaluation sample, positions corresponding to 1 / 8, 2 / 8, 3 / 8, 4 / 8, 5 / 8, 6 / 8, and 7 / 8 of the total length in the axial direction were determined. Furthermore, positions were determined by dividing each position into four 90° in the circumferential direction. At each of the 28 points where the axial division line and the circumferential division line intersect in this way, a square of 5 mm square was scratched with a cutter so that the intersection of the axial division line and the circumferential division line was the center, and the square was further scratched so that it was divided into 25 squares of 1 mm square. Then, each 1 mm square was rubbed with tweezers to confirm whether the undercoat layer of the 1 mm square peeled off from the support. Within each of the 28 5 mm squares where the axial division line and the circumferential division line intersected, the number of 1 mm squares where the undercoat layer had peeled off from the support was counted among the 25 divided 1 mm squares, and the average of the 28 points was calculated. Depending on the average number, the evaluation rank of the scratch test was determined as follows: A: 0 or more and less than 1 B: 1 or more and less than 5 C: 5 or more but less than 10 D: 10 or more but less than 15 E…15 or more and 25 or less The same evaluation was carried out for the photoreceptors A-2 to A-18 and the photoreceptors B-1 to B-14. The results are shown in Table 2. Next, 28 pieces of 5 mm squares were cut out from the samples evaluated above. The undercoat layer was then removed by buffing to expose the support surface and give it a mirror finish. The samples were then immersed in an aqueous sodium hydroxide solution for 1 minute to obtain samples for crystal orientation observation. The center of the surface of the obtained sample, that is, a 100 μm square region centered on the intersection of the axial parting line and the circumferential parting line of the support, was observed by SEM-EBSP method, and the ratio of the area occupied by Al crystal grains having each crystal orientation was calculated. The results are shown in Table 2.

[0084] [Table 2]

[0085] The disclosure of this embodiment includes the following configuration. (Configuration 1) An electrophotographic photoreceptor having a cylindrical support and a photosensitive layer, The surface of the support is formed of Al and / or an Al alloy, The surface of the support is (α) {001} orientation: -15° to +15° (β) {101} orientation faces between -15° and +15° (γ) {111} orientation: -15° to +15° a ratio of an area occupied by the Al crystal grains having (α) to a total area of ​​the surface of the support is 10% or less, and a ratio of an area occupied by the Al crystal grains having (γ) to a total area of ​​the surface of the support is more than 10%. (Configuration 2) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the ratio of the area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is 11% or more. (Configuration 3) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the ratio of the area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is 50% or more. (Configuration 4) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the ratio of the area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is 75% or more. (Configuration 5) 5. The electrophotographic photoreceptor according to any one of Configurations 1 to 4, wherein the ratio of the area occupied by the Al crystal grains having (α) to the total area of ​​the surface of the support is 5% or less. (Configuration 6) 6. The electrophotographic photoreceptor according to any one of configurations 1 to 5, wherein the Al alloy contains 0.2% by mass or more and 0.6% by mass or less of Si. (Configuration 7) A process cartridge integrally supports the electrophotographic photosensitive member according to any one of configurations 1 to 6 and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus. (Configuration 8) An electrophotographic apparatus comprising the electrophotographic photoreceptor according to any one of configurations 1 to 6, a charging unit, an exposing unit, a developing unit, and a transferring unit. [Explanation of symbols]

[0086] 1. Electrophotographic photoreceptor 2-axis 3. Charging means 4 Exposure light 5. Developing method 6 Transfer Method 7 Transfer material 8 Fixing Method 9 Cleaning Method 10 Pre-exposure light 11 Process cartridge 12 Guidance means

Claims

1. An electrophotographic photoreceptor having a cylindrical support and a photosensitive layer, The surface of the support is formed of Al and / or an Al alloy, The surface of the support is (α) {001} orientation -15° or more and less than +15° (β) {101} orientation -15° or more and less than +15° (γ) {111} orientation -15° or more and less than +15° The crystal grains of Al have the following structure: an area ratio of the Al crystal grains having the (α) to the total area of ​​the surface of the support is 10% or less, and an area ratio of the Al crystal grains having the (γ) to the total area of ​​the surface of the support is more than 10%.

2. 2. The electrophotographic photoreceptor according to claim 1, wherein the ratio of an area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is 11% or more.

3. 2. The electrophotographic photoreceptor according to claim 1, wherein the ratio of an area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is 50% or more.

4. 2. The electrophotographic photoreceptor according to claim 1, wherein the ratio of an area occupied by the Al crystal grains having (γ) to the total area of ​​the surface of the support is 75% or more.

5. 2. The electrophotographic photoreceptor according to claim 1, wherein the ratio of an area occupied by the Al crystal grains having (α) to the total area of ​​the surface of the support is 5% or less.

6. The electrophotographic photoreceptor according to claim 1 , wherein the Al alloy contains 0.2% by mass or more and 0.6% by mass or less of Si.

7. 7. A process cartridge which integrally supports the electrophotographic photosensitive member according to claim 1 and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

8. 7. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging unit, an exposing unit, a developing unit, and a transferring unit.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor substrate and electrophotographic photoreceptor, and image forming device using this electrophotographic receptor

    JP2000047413A

  • Base material for electrophotographic photoreceptor and method for manufacturing same, electrophotographic photoreceptor and method for manufacturing same, as well as electrophotographic device

    JP2004109918A

  • Method of manufacturing support for electrophotographic photoreceptor

    JP2009150958A

  • Conductive support for electrophotographic photoreceptor, electrophotographic photoreceptor, image forming apparatus, and process cartridge

    JP2016004124A

  • Conductive substrate, electrophotographic photoreceptor, process cartridge, image forming apparatus, and manufacturing method of conductive substrate

    JP2017111409A